Ophthalmic lenses and their manufacture by in-mold transformation

The method of using a dual-initiator reactive monomer mixture in a mold assembly allows for spatial integration of functional moieties in ophthalmic lenses, addressing the limitations of existing customization techniques by enhancing refractive and light management properties.

JP2024537047APending Publication Date: 2024-10-10JOHNSON & JOHNSON VISION CARE INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024519331
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-22
Filing Date
2022-09-15
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for manufacturing ophthalmic lenses, such as those described in U.S. Pat. No. 8,317,505, while allowing for customizable lenses, do not effectively incorporate functional features like refractive index properties, apodization, or spatially controlled dyes, limiting the customization and functionality of these lenses.

Method used

A method involving a mold assembly with a base curve and a front curve, using a reactive monomer mixture containing a first and second polymerization initiator, where the first initiator is activated by a specific wavelength to incorporate functional moieties spatially, and the second initiator completes polymerization, allowing for selective integration of refractive index and light-absorbing properties into the lens.

Benefits of technology

Enables the production of ophthalmic lenses with spatially controlled functional properties, such as refractive index and light management, enhancing customization and functionality, including improved vision correction and cosmetic features.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537047000001_ABST
    Figure 2024537047000001_ABST
Patent Text Reader

Abstract

Methods of forming ophthalmic lenses and lenses formed by such methods are provided, the methods including curing a reactive monomer mixture in a mold assembly under conditions that allow for the incorporation of functional features into selective portions of the ophthalmic lens.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to U.S. Patent Application No. 17 / 821,311, filed August 22, 2022, and U.S. Provisional Patent Application No. 63 / 249,643, filed September 29, 2021, both of which are incorporated by reference in their entireties.

[0002] FIELD OF THEINVENTION The present invention relates generally to the field of ophthalmic lenses, and more specifically to new and improved methods for imparting various properties and attributes to ophthalmic lenses formed using mold-molding techniques. [Background technology]

[0003] In today's world, it is common to use ophthalmic lenses to correct vision. The traditional and most common method for producing soft contact lenses is by the casting technique, where a polymerizable liquid is placed between two mold halves that together form the shape of the desired lens, and the entire liquid is cured between the mold halves. The lens is then removed from the mold and undergoes certain post-processing steps.

[0004] Recently, a novel system and method for manufacturing contact lenses has been disclosed that can easily produce an unlimited number of truly custom lenses in a cost-effective manner. U.S. Patent No. 8,317,505, the entire contents of which are incorporated herein by reference, discloses a method for growing a "Lens Precursor Form" voxel-by-voxel on a single male mold or optical mandrel by selectively projecting actinic radiation through the optical mandrel into a vat or bath of photocurable reactive monomer mixture. The optical mandrel and Lens Precursor Form are then removed from the vat and inverted so that the convex side of the optical mandrel is upright. After a dwell period during which any residual uncured liquid from the bath that remains on the Lens Precursor Form flows by gravity or otherwise over the Lens Precursor Form, the liquid is cured by applying a fixed radiation to form the final lens. As described therein, the system utilizes a single mold rather than two mold halves as in conventional casting, and allows true custom lenses to be manufactured by simply "reprogramming" software instructions rather than changing equipment or parts.

[0005] As described in the '505 patent, actinic radiation is projected through the male mold and into the reactive mixture at an array of discrete locations, each of which is selectively controllable, to selectively cure the reactive mixture to a predetermined depth at any point in the array ("voxel by voxel"), thereby "growing" a lens from the convex side of the male mold. The term "voxel" as used herein is the same as in the '505 patent and refers to a volume element that represents a value on a regular grid in three-dimensional space. Voxels can be viewed as three-dimensional pixels, with each voxel associated with a particular point in the selectively controllable array. Summary of the Invention [Problem to be solved by the invention]

[0006] While the '505 represents a significant advancement in lens manufacturing capabilities, further development remains needed, for example, to expand options for creating customizable lenses that incorporate functional features to further enhance the lens wearer's experience. [Means for solving the problem]

[0007] The present invention utilizes the technology detailed in the '505 patent for new systems, methods and compositions for spatially incorporating functional moieties, geometries and / or physical properties into molded ophthalmic lenses. The invention has particular application for spatially controlling and imparting various properties to molded lenses without costly process modifications. The invention allows, for example, to impart various refractive index properties to lenses to provide individualized patient solutions for conditions such as presbyopia. The invention described herein also allows for the spatial incorporation of dyes into ophthalmic lenses to create lenses with generic or custom apodization properties that improve the patient's vision, or the incorporation of cosmetic or other visual properties or designs into lenses.

[0008] Thus, in one aspect, the present invention provides a method for forming an ophthalmic lens, comprising: (a) providing a mold assembly comprised of a base curve and a front curve, the base curve and the front curve defining and enclosing a cavity therebetween, the cavity containing a reactive monomer mixture, the reactive monomer mixture including a monomer suitable for making an ophthalmic lens, a first polymerization initiator activatable at a first wavelength, a first functional moiety chemically bonded to the first polymerization initiator, and a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator; at least one of the curves is optically transparent; (b) exposing one or more selected areas of the reactive monomer mixture to a source of actinic radiation at a first wavelength, thereby selectively polymerizing a portion of the reactive monomer mixture, wherein the selectively polymerized portions incorporate a first functional moiety; (c) exposing the reactive monomer mixture to a second activation to activate a second polymerization initiator and harden the reactive monomer mixture; (d) removing the ophthalmic lens from the mold assembly; and (e) extracting unreacted first polymerization initiator from the ophthalmic lens.

[0009] In another aspect, the present invention provides a reactive monomer mixture for making an ophthalmic lens, the reactive monomer mixture comprising a monomer suitable for making an ophthalmic lens, a first polymerization initiator activatable at a first wavelength, a first functional moiety chemically bonded to the first polymerization initiator, and a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator.

[0010] In yet a further aspect, the present invention provides a polymerization initiator having a functional moiety attached thereto, for example, as set forth in Table A. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 illustrates a prior art apparatus for forming custom contact lenses. [Diagram 2]FIG. 2 is an enlarged view of the molding optics portion of the prior art device of FIG. [Diagram 3] 1 illustrates an exemplary curing apparatus including a mold in an exposure jig that may be used to form a lens in accordance with the systems and methods described herein. [Figure 4] 500 MHz 1H-NMR spectrum of MAPO-PVP in deuterium oxide. [Diagram 5] SEC-MALS chromatograms of MAPO-PVP, PVP K30, and PVP K12 are shown. [Figure 6] 500 MHz 1H-NMR spectrum of MAPO-PDMA in deuterated methanol. [Figure 7] 1 shows the UV-VIS spectra of PI-Dye1 and PI-Dye2 in 0.2 mM solution. [Figure 8] USAF 1951 test chart shown. [Figure 9] 1 shows a USAF 1951 test chart image applied onto a contact lens. [Figure 10] Spherical / defocused and cylindrical projection images as well as the measured wavefront are shown. [Figure 11] An apodized image and a pupil-only image are shown, along with the corresponding lens. [Figure 12] 1 shows images of a contact lens as a function of energy and exposure time. [Figure 13] Apodized, pupil-only, and jack-o-lantern images and corresponding lenses are shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. All publications, patent applications, patents, and other references mentioned herein are incorporated herein by reference.

[0013] Unless otherwise stated, numerical ranges, such as in "from 2 to 10" or "between 2 and 10," are inclusive of the numbers defining the range (e.g., 2 and 10).

[0014] Unless otherwise stated, ratios, percentages, parts, etc. are by weight.

[0015] The phrase "number average molecular weight" refers to the number average molecular weight (M n The phrase "weight average molecular weight" refers to the weight average molecular weight (M w The term "polydispersity index" (PDI) refers to the M w M n "Molecular weight" refers to the ratio of the molecular weight (Mw) divided by the molecular weight (Mw) and represents the molecular weight distribution of a sample. If no type of "molecular weight" is indicated or is not clear from the context, it is intended to mean number average molecular weight.

[0016] As used herein, the term "about" refers to a range of plus or minus ten percent of the modified number. For example, the phrase "about 10" would include both 9 and 11.

[0017] As used herein, the term "(meth)" refers to optional methyl substitution. Thus, a term such as "(meth)acrylate" refers to both methacrylate and acrylate.

[0018] Wherever a chemical structure is depicted, it should be understood that the disclosed options for the substituents in the structure may be combined in any combination. * and R ** and each of these contains a list of three possible groups, then nine combinations are disclosed. The same is true for combinations of features.

[0019] The average number of repeating units in a polymer sample is known as the "degree of polymerization." The general chemical formula of a polymer sample, e.g., *** ] n When used, "n" refers to the degree of polymerization of the sample, and the formula should be interpreted as representing the number average molecular weight of the polymer sample.

[0020] As used herein, the term "individual" includes humans and vertebrate animals.

[0021] As used herein, the term "ophthalmic device" refers to any device that resides in or on the eye, or any part of the eye, including the surface of the eye. These devices can provide optical correction, appearance enhancement, vision enhancement, therapeutic effects (e.g., as a dressing), or delivery of active ingredients such as pharmaceutical and nutraceutical ingredients, or any combination of the foregoing. Preferred ophthalmic devices are ophthalmic lenses, including soft contact lenses, hard contact lenses (including rigid gas permeable lenses), hybrid contact lenses, intraocular lenses, and inlay and overlay lenses. Ophthalmic devices may preferably include contact lenses.

[0022] As used herein, the term "contact lens" refers to an ophthalmic device that can be placed on the cornea of ​​an individual's eye. Contact lenses can correct refractive errors, thereby improving vision, absorb ultraviolet or visible light, thereby providing protection or color enhancement, and can also provide cosmetic benefits, such as changing the color and pattern of the wearer's iris. Contact lenses can be of any suitable material known in the art, and can be soft lenses, hard lenses, or hybrid lenses that contain at least two distinct portions with different physical, mechanical, or optical properties, such as modulus of elasticity, water content, light transmission, or a combination thereof.

[0023] The ophthalmic devices, ophthalmic lenses, and contact lenses of the present invention may be composed of silicone hydrogels. These silicone hydrogels typically contain at least one hydrophilic component and at least one silicone-containing component covalently bonded to each other in a curing device. The ophthalmic devices, ophthalmic lenses, and contact lenses of the present invention may also be composed of conventional hydrogels, or a combination of conventional hydrogels and silicone hydrogels.

[0024] A "polymer" is an organic compound having a number average molecular weight greater than 1500 and may be reactive or non-reactive.

[0025] As used herein, a "target macromolecule" is a macromolecule of interest that has been synthesized from reactive compositions that include monomers, macromers, prepolymers, crosslinkers, initiators, additives, diluents, and the like.

[0026] As used herein, a "monomer" is a monofunctional molecule capable of undergoing chain growth polymerization, particularly free radical polymerization, to create repeat units within the chemical structure of a target macromolecule. Some monomers have difunctional impurities that can act as crosslinkers. A "hydrophilic monomer" is also a monomer that, when mixed with deionized water at a concentration of 5% by weight at 25°C, gives a clear, single-phase solution. A "hydrophilic component" is a monomer, macromer, prepolymer, initiator, crosslinker, additive, or polymer that, when mixed with deionized water at a concentration of 5% by weight at 25°C, gives a clear, single-phase solution. The hydrophilic component may contain at least one polymerizable group. It may be preferred that the hydrophilic component consists of one polymerizable group.

[0027] As used herein, a "macromonomer" or "macromer" is a linear or branched macromolecule having at least one polymerizable group capable of undergoing chain growth polymerization, specifically free radical polymerization.

[0028] As used herein, the term "polymerizable" means that the compound contains at least one polymerizable group. A "polymerizable group" is a group capable of undergoing free radical and / or cationic polymerization, e.g., chain growth polymerization, such as a carbon-carbon double bond group that can polymerize when subjected to radical polymerization initiation conditions. Non-limiting examples of polymerizable groups include (meth)acrylates, styrenes, vinyl ethers, (meth)acrylamides, N-vinyl lactams, N-vinyl amides, O-vinyl carbamates, O-vinyl carbonates, and other vinyl groups. Preferably, the polymerizable group comprises (meth)acrylates, (meth)acrylamides, and mixtures thereof. Preferably, the polymerizable group comprises (meth)acrylates, (meth)acrylamides, N-vinyl lactams, N-vinyl amides, styryl functional groups, or mixtures of any of the foregoing. The polymerizable group may be unsubstituted or substituted. For example, the nitrogen atom in (meth)acrylamide may be bonded to a hydrogen or the hydrogen may be replaced by an alkyl or cycloalkyl (which itself may be further substituted). In contrast to "polymerizable," the term "non-polymerizable" means that the compound does not contain such free-radically polymerizable groups.

[0029] Examples of the foregoing include substituted or unsubstituted C 1~6 Alkyl (meth)acrylate, C 1~6 Alkyl (meth)acrylamide, C 2~12 Alkenyl, C 2~12 Alkenylphenyl, C 2~12 Alkenyl naphthyl, C 2~6 Alkenyl Phenyl C 1~6 Alkyl is an example of the C 1~6 Suitable substituents on an alkyl include ether, hydroxyl, carboxyl, halogen, and combinations thereof.

[0030] Any type of free radical polymerization can be used, including but not limited to bulk, solution, suspension, and emulsion, as well as any of the controlled radical polymerization techniques, such as stable free radical polymerization, nitric oxide mediated living polymerization, atom transfer radical polymerization, reversible addition-fragmentation chain transfer polymerization, organotellurium mediated living radical polymerization, etc.

[0031] In free radical polymerization, in the absence of chain transfer reactions, a growing chain can be terminated by radical coupling or disproportionation. In coupling, two growing chains simply join to form a single bond, and the resulting polymer has an end group composed of the initiator fragment. In disproportionation, one growing chain radical extracts a proton from another growing chain adjacent to the free radical, which then forms a terminal double bond. Chain transfer reactions can occur with any component in the reaction mixture, such as chain transfer to a monomer, chain transfer to a polymer resulting in branching, chain transfer to an initiator, etc., as well as chain transfer to any chain transfer agent intentionally added to reduce and control molecular weight. In most chain transfer reactions, the growing chain abstracts a proton from another molecule, thereby terminating the chain growth and simultaneously generating another radical. The term "chain terminating group" refers to a chemical group that terminates the chain growth and becomes one end group of the final polymer. In most cases the chain terminating group is a proton, but others are known or believed to exist, such as chain transfer to a peroxide initiator where the chain terminating group is dependent on the peroxide, e.g., in the case of benzoyl peroxide, the chain terminating group is a benzoate.

[0032] As used herein, a "silicone-containing component" or "silicone component" is a monomer, macromer, prepolymer, crosslinker, initiator, additive, or polymer in a reactive composition that has at least one silicon-oxygen bond, usually in the form of a siloxy group, a siloxane group, a carbosiloxane group, and mixtures thereof. Examples of silicone-containing components useful in the present invention are disclosed in U.S. Pat. Nos. 3,808,178, 4,120,570, 4,136,250, 4,153,641, 4,740,533, 5,034,461, 5,070,215, 5,244,981, 5,314,960, 5,331,067, 5,371,147, 5,760,100, 5,849,811, 5,96 2,548, 5,965,631, 5,998,498, 6,367,929, 6,822,016, 6,943,203, 6,951,894, 7,052,131, No. 7,247,692, No. 7,396,890, No. 7,461,937, No. 7,468,398, No. 7,538,146, No. 7,553,880, No. 7,572,841, No. 7,666,921 , No. 7,691,916, No. 7,786,185, No. 7,825,170, No. 7,915,323, No. 7,994,356, No. 8,022,158, No. 8,163,206, No. 8,273, No. 802, No. 8,399,538, No. 8,415,404, No. 8,420,711, No. 8,450,387, No. 8,487,058, No. 8,568,626, No. 8,937,110, No. 8,9 37,111, 8,940,812, 8,980,972, 9,056,878, 9,125,808, 9,140,825, 9,156,934, 9,170,349, 9,217,813, 9,244,196, 9,244,197, 9,260,544, 9,297,928, 9,297,929, and European Patent No. 080539. These patents are incorporated herein by reference in their entirety.The silicone-containing component may also contain at least one polymerizable group. The silicone-containing component may preferably consist of one or two polymerizable groups.

[0033] A "polymer" is a target macromolecule composed of repeating units of monomers and macromers used during polymerization.

[0034] A "homopolymer" is a polymer made from one monomer, a "copolymer" is a polymer made from two or more monomers, and a "terpolymer" is a polymer made from three monomers. A "block copolymer" consists of compositionally distinct blocks or segments. A diblock copolymer has two blocks. A triblock copolymer has three blocks. A "comb or graft copolymer" is made from at least one macromer.

[0035] A "repeating unit" is the smallest grouping of atoms in a polymer that corresponds to the polymerization of a particular monomer or macromer.

[0036] An "initiator" is a molecule capable of decomposing into free radical groups capable of reacting with monomers to initiate a free radical polymerization reaction. Thermal initiators decompose at a specific rate depending on the temperature, and typical examples are azo compounds such as azobisisobutyronitrile and 4,4'-aobis(4-cyanovaleric acid), peroxides such as benzoyl peroxide, tert-butyl peroxide, tert-butyl hydroperoxide, tert-butyl peroxybenzoate, dicumyl peroxide, and lauroyl peroxide, peracids such as peracetic acid and potassium persulfate, and various redox systems. Photoinitiators decompose by a photochemical process, and typical examples are derivatives of benzil, benzoin, acetophenone, benzophenone, camphorquinone, and mixtures thereof, as well as various monoacyl and bisacylphosphine oxides, and combinations thereof.

[0037] A "free radical group" is a molecule that has an unpaired valence electron that can react with a polymerizable group to initiate a free radical polymerization reaction.

[0038] A "cross-linking agent" (or crosslinker) is a di- or polyfunctional monomer capable of undergoing free radical polymerization at two or more locations in the molecule, thereby creating branch points and polymer networks. The two or more polymerizable functional groups present in the cross-linker can be the same or different and can be independently selected from, for example, vinyl groups (including allyl), (meth)acrylate groups, and (meth)acrylamide groups. Common examples are ethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, methylene bisacrylamide, triallyl cyanurate, and the like.

[0039] A "prepolymer" is a reaction product of monomers (or macromers) that contain remaining polymerizable groups that can be further reacted to form a polymer.

[0040] A "polymer network" is a type of polymer in the form of cross-linked macromolecules. Generally, a polymer network may swell but cannot dissolve in a solvent. For example, the cross-linked substrate network of the present invention is a material that can swell without dissolving.

[0041] A "hydrogel" is a polymer network that typically swells in water or an aqueous solution while absorbing at least 10% by weight (at 25° C.). A "silicone hydrogel" is a hydrogel made from at least one silicone-containing component along with at least one hydrophilic component. The hydrophilic component may also include a non-reactive polymer.

[0042] "Conventional hydrogel" refers to a polymer network made from monomers that do not have any siloxy, siloxane, or carbosiloxane groups. Conventional hydrogels are prepared from reactive compositions that primarily include hydrophilic monomers such as 2-hydroxyethyl methacrylate ("HEMA"), N-vinylpyrrolidone ("NVP"), N,N-dimethylacrylamide ("DMA"), or vinyl acetate.

[0043] As used herein, the term "reactive composition" refers to a composition containing one or more reactive components (and optionally non-reactive components) that form a polymeric composition when mixed together (if more than one is present) and subjected to polymerization conditions. When more than one component is present, the reactive composition may also be referred to herein as a "reactive mixture" or "reactive monomer mixture" (or RMM). The reactive composition includes reactive components such as monomers, macromers, prepolymers, crosslinkers, and initiators, as well as optional additives such as wetting agents, release agents, dyes, light absorbing compounds (e.g., UV-VIS absorbers), pigments, dyes, and photochromic compounds (any of which may be reactive or non-reactive, but are preferably capable of being retained within the resulting polymeric composition, as well as pharmaceutical and nutraceutical compounds), and optional diluents. It will be understood that a wide range of additives may be added based on the final product to be made and its intended use. The concentrations of the components of the reactive composition are expressed as a weight percentage of all components in the reactive composition, excluding the diluent. When a diluent is used, concentrations are expressed as weight percentages based on the amount of all components and diluent in the reaction composition.

[0044] "Reactive components" are components of the reactive composition that become part of the chemical structure of the resulting material through covalent bonds, hydrogen bonds, electrostatic interactions, the formation of interpenetrating polymer networks, or in any other manner. Examples include, but are not limited to, silicone reactive components (e.g., silicone-containing components described below) and hydrophilic reactive components (e.g., hydrophilic monomers described below).

[0045] As used herein, the term "silicone hydrogel contact lenses" refers to contact lenses that contain at least one silicone hydrogel.Silicone hydrogel contact lenses generally have increased oxygen permeability compared to conventional hydrogels.Silicone hydrogel contact lenses utilize both their water content and polymer content to deliver oxygen to the eye.

[0046] "DMD" refers to a Digital Micromirror Device, which may be a bistable spatial light modulator consisting of an array of movable micromirrors functionally implemented across a CMOS SRAM. Each mirror may be independently controlled by loading data into memory cells, which may be under the mirror, to direct reflected light, spatially mapping pixels of video data to pixels on the display. The data electrostatically controls the tilt angle of the mirror in a binary manner, where the mirror state is either +X degrees (on) or -X degrees (off). Light reflected by the (on) mirror may then pass through a projection lens onto a screen. The light may be reflected off to produce a dark field, defining the black level floor of the image. Images may be produced by grayscale modulation between on and off levels at a rate fast enough to be integrated by an observer. DMD (Digital Micromirror Device) may include DLP projection systems.

[0047] "DMD script" refers to the control protocol for the spatial light modulator, and also refers to the control signals for any system components, such as the light source or filter wheel, either of which may contain a series of command sequences at any given time.

[0048] The term "multifunctional" refers to a component having two or more polymerizable groups. The term "monofunctional" refers to a component having one polymerizable group.

[0049] The terms "halogen" or "halo" refer to fluorine, chlorine, bromine, and iodine.

[0050] As used herein, the term "alkyl" refers to an unsubstituted or substituted straight or branched chain alkyl group containing the indicated number of carbon atoms. If no number is indicated, the alkyl (optionally including any substituents on the alkyl) may contain 1-16 carbon atoms. Preferably, the alkyl group contains 1-10 carbon atoms, alternatively 1-7 carbon atoms, or alternatively 1-4 carbon atoms. Examples of alkyl include methyl, ethyl, propyl, isopropyl, butyl, iso-, sec- and tert-butyl, pentyl, hexyl, heptyl, 3-ethylbutyl, and the like. Examples of substituents on the alkyl include one, two, or three groups independently selected from hydroxy, amino, amido, oxa, carboxy, alkylcarboxy, carbonyl, alkoxy, amido, carbamate, carbonate, halogen, phenyl, benzyl, and combinations thereof. "Alkylene" means a divalent alkyl group, e.g., -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2CH(CH3)CH2-, and -CH2CH2CH2CH2-.

[0051] "Haloalkyl" refers to an alkyl group, as defined above, substituted with one or more halogen atoms, each halogen being independently F, Cl, Br, or I. A preferred halogen is F. Preferred haloalkyl groups contain 1 to 6 carbons, more preferably 1 to 4 carbons, and even more preferably 1 to 2 carbons. "Haloalkyl" includes perhaloalkyl groups such as -CF3- or -CF2CF3-. "Haloalkylene" refers to a divalent haloalkyl group, such as -CH2CF2-.

[0052] "Cycloalkyl" refers to an unsubstituted or substituted cyclic hydrocarbon containing the indicated number of ring carbon atoms. If no number is indicated, the cycloalkyl may contain 3 to 12 ring carbon atoms. Preferably, it is a C3-C8 cycloalkyl group, more preferably a C4-C7 cycloalkyl, and even more preferably a C5-C6 cycloalkyl. Examples of cycloalkyl include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl. Examples of substituents on cycloalkyl include one, two, or three groups independently selected from alkyl, hydroxy, amino, amido, oxa, carbonyl, alkoxy, amido, carbamate, carbonate, halo, phenyl, benzyl, and combinations thereof. "Cycloalkylene" refers to a divalent cycloalkyl group, such as 1,2-cyclohexylene, 1,3-cyclohexylene, or 1,4-cyclohexylene.

[0053] "Heterocycloalkyl" refers to a cycloalkyl ring or ring system as defined above in which at least one ring carbon is replaced by a heteroatom selected from nitrogen, oxygen, and sulfur. The heterocycloalkyl ring is optionally fused or otherwise attached to other heterocycloalkyl rings and / or non-aromatic hydrocarbon rings and / or phenyl rings. Preferred heterocycloalkyl groups have 5 to 7 members. More preferred heterocycloalkyl groups have 5 or 6 members. Heterocycloalkylene refers to a divalent heterocycloalkyl group.

[0054] "Aryl" refers to an unsubstituted or substituted aromatic hydrocarbon ring system containing at least one aromatic ring. The aryl group contains the indicated number of ring carbon atoms. If no number is indicated, the aryl may contain 6 to 14 ring carbon atoms. The aromatic ring may be optionally fused or otherwise attached to other aromatic or non-aromatic hydrocarbon rings. Examples of aryl groups include phenyl, naphthyl, and biphenyl. Preferred examples of aryl groups include phenyl. Examples of substituents on an aryl include one, two, or three groups independently selected from alkyl, hydroxy, amino, amido, oxa, carboxy, alkylcarboxy, carbonyl, alkoxy, amido, carbamate, carbonate, halo, phenyl, benzyl, and combinations thereof. "Arylene" refers to a divalent aryl group, such as 1,2-phenylene, 1,3-phenylene, or 1,4-phenylene.

[0055] "Heteroaryl" refers to an aryl ring or ring system, as defined above, in which at least one ring carbon atom is replaced by a heteroatom selected from nitrogen, oxygen, and sulfur. The heteroaryl ring may be fused or otherwise bonded to one or more heteroaryl rings, aromatic or non-aromatic hydrocarbon rings, or heterocycloalkyl rings. Examples of heteroaryl groups include pyridyl, furyl, and thienyl. "Heteroarylene" refers to a divalent heteroaryl group.

[0056] "Alkoxy" refers to an alkyl group attached to the parent molecular moiety through an oxygen bridge. Examples of alkoxy groups include, for example, methoxy, ethoxy, propoxy, and isopropoxy. "Aryloxy" refers to an aryl group attached to the parent molecular moiety through an oxygen bridge. Examples include phenoxy. "Cyclic alkoxy" refers to a cycloalkyl group attached to the parent moiety through an oxygen bridge.

[0057] "Alkylamine" refers to an alkyl group attached to the parent molecular moiety through an -NH bridge. Alkyleneamine refers to a divalent alkylamine group, such as -CHCHNH-.

[0058] "Siloxanyl" refers to a structure having at least one Si-O-Si bond. Thus, for example, a siloxanyl group refers to a group having at least one Si-O-Si group (i.e., a siloxane group), and a siloxanyl compound refers to a compound having at least one Si-O-Si group. "Siloxanyl" refers to monomeric (e.g., Si-O-Si) as well as oligomeric / polymeric structures (e.g., -[Si-O] n -, where n is 2 or greater. Each silicon atom in the siloxanyl group is independently selected to complete their valence. A Group(R A is replaced by (as defined in options (b) to (i) of formula A).

[0059] "Silyl" refers to a structure of formula RSi- and "siloxy" refers to a structure of formula RSi-O-, where each R in silyl or siloxy is independently selected from trimethylsiloxy, C1-C8 alkyl (preferably C1-C3 alkyl, more preferably ethyl or methyl), and C3-C8 cycloalkyl.

[0060] "Alkyleneoxy" refers to a group having the general formula -(alkylene-O-) p -or-(O-alkylene) p-, where alkylene is as defined above, p is 1-200, or 1-100, or 1-50, or 1-25, or 1-20, or 1-10, and each alkylene is independently optionally substituted with one or more groups independently selected from hydroxyl, halo (e.g., fluoro), amino, amido, ether, carbonyl, carboxyl, and combinations thereof. When p is greater than 1, each alkylene may be the same or different, and the alkyleneoxy may be in a block or random configuration. When the alkyleneoxy forms a terminal group in a molecule, the terminus of the alkyleneoxy may be, for example, a hydroxyl or alkoxy (e.g., HO-[CH2CHO] p - or CH3O-[CH2CH2O] p Examples of alkyleneoxy include polymethyleneoxy, polyethyleneoxy, polypropyleneoxy, polybutyleneoxy, and poly(ethyleneoxy-co-propyleneoxy).

[0061] "Oxaalkylene" refers to an alkylene group as defined above in which one or more non-adjacent CH groups are replaced by an oxygen atom, such as, for example, -CHCHOCH(CH)CH-. "Thiaalkylene" refers to an alkylene group as defined above in which one or more non-adjacent CH groups are replaced by a sulfur atom, such as, -CHCHSCH(CH)CH-.

[0062] The term "linking group" refers to a moiety that attaches a polymerizable group to a parent molecule. The linking group may be any moiety that does not unnecessarily interfere with the polymerization of the compound of which it is a part. For example, the linking group may be a bond or may comprise one or more alkylene, haloalkylene, amide, amine, alkyleneamine, carbamate, carboxylate (-CO2-), arylene, heteroarylene, cycloalkylene, heterocycloalkylene, alkyleneoxy, oxaalkylene, thiaalkylene, haloalkyleneoxy (alkyleneoxy substituted with one or more halo groups (e.g., -OCF2-, -OCF2CF2-, -OCF2CH2-), siloxanyl, alkylenesiloxanyl, or combinations thereof. The linking group may be optionally substituted with one or more substituents. Suitable substituents may include those independently selected from alkyl, halo (e.g., fluoro), hydroxyl, HO-alkyleneoxy, MeO-alkyleneoxy, siloxanyl, siloxy, siloxy-alkyleneoxy-, siloxy-alkylene-alkyleneoxy- (wherein there may be more than one alkyleneoxy group, and each methylene in the alkylene and alkyleneoxy is independently optionally substituted with hydroxyl), ether, amine, carbonyl, carbamate, and combinations thereof. The linking group may also be substituted with a polymerizable group, such as (meth)acrylate.

[0063] Preferred linking groups include C1-C8 alkylene (preferably C2-C6 alkylene) and C1-C8 oxaalkylene (preferably C2-C6 oxaalkylene), each of which is optionally substituted with one or two groups independently selected from hydroxyl and siloxy. Preferred linking groups also include carboxylate, amide, C1-C8 alkylene carboxylate-C1-C8 alkylene, or C1-C8 alkylene amide-C1-C8 alkylene.

[0064] When the linking group is composed of a combination of moieties as described above (e.g., alkylene and cycloalkylene), the moieties may be present in any order. For example, in formula E below, when L (the linking group) is shown to be -alkylene-cycloalkylene-, Rg-L may be either Rg-alkylene-cycloalkylene- or Rg-cycloalkylene-alkylene-. Regardless, the order listed represents the preferred order in which the moieties appear in the compound, starting from the terminal polymerizable group (Rg) to which the linking group is attached. For example, two linking groups, L and L 2 and -L are preferably Rg-alkylene-cycloalkylene-, where -L 2 -Rg is preferably -cycloalkylene-alkylene-Rg.

[0065] As noted above, in one aspect, the present invention provides a method for forming an ophthalmic lens, the method comprising: (a) providing a mold assembly comprised of a base curve and a front curve, the base curve and the front curve defining and enclosing a cavity therebetween, the cavity containing a reactive monomer mixture, the reactive monomer mixture including a monomer suitable for making an ophthalmic lens, a first polymerization initiator activatable at a first wavelength, a first functional moiety chemically bonded to the first polymerization initiator, and a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, and (b) providing a mold assembly comprising a base curve and a front curve defining and enclosing a cavity therebetween, the cavity containing a reactive monomer mixture comprising a monomer suitable for making an ophthalmic lens, a first polymerization initiator activatable at a first wavelength, a first functional moiety chemically bonded to the first polymerization initiator, and a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, and a second polymerization initiator activating the first polymerization initiator ... is optically transparent; (b) exposing one or more selected areas of the reactive monomer mixture to a source of actinic radiation at a first wavelength, thereby selectively polymerizing a portion of the reactive monomer mixture, where the selectively polymerized portions incorporate a first functional moiety; (c) exposing the reactive monomer mixture to a second activation to activate a second polymerization initiator and harden the reactive monomer mixture; (d) removing the ophthalmic lens from the mold assembly; and (e) extracting unreacted first polymerization initiator (having the first functional moiety chemically bound thereto) from the ophthalmic lens.

[0066] In accordance with the present invention, the reactive monomer mixture is formed into an ophthalmic lens, such as a soft contact lens, by dispensing the mixture into a mold assembly and subsequently curing the mixture. The mold assembly is comprised of a base curve, which is a mold half that contacts the posterior surface of the lens, and a front curve that contacts the anterior surface. When brought together, the front curve and base curve define and surround a cavity therebetween which, in accordance with the present invention, contains the reactive monomer mixture.

[0067] The mold components (front curve and base curve) that make up the mold assembly used in the present invention may be made from a variety of materials, including disposable or reusable materials. For example, the mold may be a thermoplastic optical mold made from any suitable material, including, but not limited to, polyethylene, polypropylene, other polyolefins including homopolymers, copolymers, and terpolymers, polystyrene, polystyrene copolymers, polyesters such as poly(ethylene terephthalate) and poly(butylene terephthalate), polyamides, poly(vinyl alcohol) and its derivatives, hydrogenated styrene butadiene block copolymers such as Tuftec, cyclic olefin polymers such as Zeonor and Topas resins, and combinations thereof. The mold may be selected to be transparent or nearly transparent to the wavelengths that activate the first polymerization initiator, thus allowing irradiation through the front curve, the base curve, or both the front curve and the base curve. The materials may be the same or different for the front curve and the base curve. A preferred material for the front curve of the mold assembly is a 90:10 (w / w) blend of a cyclic olefin polymer and a hydrogenated styrene butadiene block copolymer, respectively. A preferred material for the base curve of the mold assembly is a 90:10 (w / w) blend of cyclic olefin polymer and polypropylene. Other exemplary materials include blends of Zeonor and Tuftec for either or both of the base curve and front curve. The thickness of the base curve or front curve mold can vary, but is typically between 100 and 1500 microns, preferably between 600 and 800 microns, as measured at the center of the optical zone of the target lens mold design. Other mold materials that can be used include reusable molds made of, for example, glass, quartz, or ceramics such as aluminum oxide. BK270 and RB 270 are examples of materials suitable for molding the transmissive mold halves. They may be shaped or polished to achieve acceptable optical profile and surface roughness characteristics. In addition, coatings may be applied to such reusable molds to aid in the release of the cured lens.These mold coatings are typically siloxane or silane based and may be partially or fully fluorinated.

[0068] The reactive monomer mix of the present invention contains a first polymerization initiator having a first functional moiety chemically bonded thereto. The first polymerization initiator is activatable with a first wavelength (which may be in the range of wavelengths that activate the first polymerization initiator). As described above, when activated by the first wavelength, the polymerization initiator breaks down into free radical groups that can react with monomers in the reactive monomer mix to initiate a free radical polymerization reaction. When polymerization is initiated, the initiator adds monomer units to grow a polymer chain, and as a result, also becomes a covalently bonded part of the polymer. As a result, the first functional moiety that is chemically bonded to the initiator also becomes part of the polymer. As a result, the functional moiety is incorporated into the lens. And because the method of the present invention employs a selective polymerization approach, it is possible to place the functional moiety at a specific location in the ophthalmic lens. Such selective positioning of functional features allows for the production of lenses that incorporate a wide variety of capabilities, including, for example, light filtering, light apodization, modified refractive index, and the like.

[0069] The first polymerization initiator can absorb (and be activated by) various wavelengths of light, such as UV and / or visible wavelengths. Preferably, the first polymerization initiator can absorb within the visible range of the electromagnetic spectrum (about 380 nm to about 780 nm). Visible light initiators that can function as the first polymerization initiator are known in the art and include, but are not limited to, aromatic α-hydroxyketones, alkoxyoxybenzoins, acetophenones, acylphosphine oxides, bisacylphosphine oxides, and tertiary amines and diketones, mixtures thereof, and the like. Illustrative examples of initiators further include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, bis(2,6-dimethoxybenzoyl)-2,4-4-trimethylpentylphosphine oxide (DMBAPO), bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Irgacure 819), 2,4,6-trimethylbenzyldiphenylphosphine oxide, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide, benzoin methyl ester, and a combination of camphorquinone and ethyl 4-(N,N-dimethylamino)benzoate. Commercially available visible light initiator systems that can function as the first polymerization initiator include Irgacure 819, Irgacure 1700, Irgacure 1800, Irgacure 819, Irgacure 1850 (all from Ciba Specialty Chemicals) and Lucirin TPO initiator (sold by BASF). These and other photoinitiators that can be used are disclosed in Volume III, Photoinitiators for Free Radical Cationic & Anionic Photopolymerization, 2nd Edition by JV Crivello & K. Dietliker; edited by G. Bradley; John Wiley and Sons; New York; 1998.

[0070] Particularly preferred visible light initiators that can function as the first polymerization initiator include α-hydroxyketones such as Irgacure® available from CIBA (e.g., Irgacure 1700 or 1800); various organic phosphine oxides such as monoacylphosphine oxides and bisacylphosphine oxides; diethoxyacetophenone, 1-hydroxycyclohexylphenyl ketone, 2,2-dimethoxy-2-phenylacetophenone, phenothiazine, diisopropylxanthogen disulfide, benzoin or benzoin derivatives, etc. Preferably, the first polymerization initiator is activated at wavelengths including the ranges of 200 to 600 nm, or 300 to 500 nm, or 350 to 450 nm, or 380 to 450 nm.

[0071] The reactive monomer mixture of the present invention contains a first functional moiety chemically bonded to a first polymerization initiator. As described above, the present invention allows the incorporation of the first functional moiety at selective locations in ophthalmic lenses. A wide variety of functional moieties can be incorporated. Thus, as described in detail in U.S. Pat. No. 8,317,505, the entirety of which is incorporated herein by reference, the first wavelength, as well as its intensity and pattern, can be selectively selected to interact with the spectral absorbance of the monomer mixture so that the desired two-dimensional or three-dimensional incorporation of the first functional moiety is achieved by Beer's law effect.

[0072] The first functional moiety may be designed to affect an overall change in optical path length, with or without a concomitant change in the absorption spectrum in the region of the hydrated lens formed by the first polymerization initiator. In this way, the entire optics of the lens can be deterministically altered. The optical path length (OPL) is calculated by the following formula:

[0073]

number

[0074] The first functional moiety may be, for example, a refractive index moiety, a light absorbing moiety, or a combination thereof. The light absorbing moiety may be used to provide an ophthalmic lens with various functions, including, for example, cosmetic properties, or absorption of specific wavelengths of light (e.g., absorption of high energy visible (HEV) light and / or other wavelengths). The first functional moiety may provide two or more functionalities. For example, the light absorbing moiety may also modify the refractive index of the lens in a desired manner. Thus, the incorporated moiety may achieve multiple effects.

[0075] Light absorbing moieties can be used to provide lenses with general or custom apodization properties to improve the vision of the lens wearer. Examples of light absorbing moieties include, for example, static dyes, photochromic dyes, thermochromic dyes, leuco dyes, and combinations thereof. More specific examples include, but are not limited to, azo dyes; anthraquinone dyes; nitro dyes; phthalocyanine dyes; quinoneimine dyes; quinoline dyes; carbonyl dyes; triarylmethane dyes; methine dyes; naphthopyrans; spiro(indoline)quinopyrans and spiro(indoline)pyrans; oxazines such as spiro(indoline)naphthoxazine, spiro(indoline)pyridobenzoxazine, spiro(benzoindoline)pyridabenzoxazine, spiro(benzoindoline)naphthoxazine and spiro(indoline)benzoxazine; mercury dithizonates; fulgides; fulgimides, acridine dyes, arylmethane dyes, indamines, xanthenes, acridones, or combinations thereof.

[0076] The first functional moiety may be a refractive index moiety. The refractive index moiety changes the OPL of the lens in the area in which it is incorporated relative to the bulk lens. The change in refractive properties throughout the lens can be used to impart images or other visual features to the lens, for example to create bifocal or multifocal lenses, or to impart features that affect visual function. A preferred class of refractive index moieties is polyamides. Exemplary polyamides include, but are not limited to, polyvinylpyrrolidone (PVP), polyvinylmethylacetamide (PVMA), polydimethylacrylamide (PDMA), polyvinylacetamide (PNVA), poly(hydroxyethyl(meth)acrylamide), polyacrylamide, and copolymers of two or more thereof.

[0077] Exemplary first polymerization initiators that include a chemically attached first functional moiety are shown in Table A:

[0078] [Table 1-1]

[0079] [Table 1-2]

[0080] [Table 1-3]

[0081] [Table 1-4]

[0082] The first polymerization initiator (containing a chemically bonded first functional moiety) may be present in the reactive monomer mixture in an effective amount, for example, from 0.01% to 20% by weight, based on all components in the reactive monomer mixture excluding the diluent.

[0083] The reactive monomer mixture of the present invention contains a second polymerization initiator. The second polymerization initiator can be activated by a second activation that does not substantially activate the first polymerization initiator (e.g., activation of less than 50 mole percent, preferably less than 20 mole percent, more preferably less than 5 mole percent, even more preferably less than 1 mole percent). For example, the second polymerization initiator can be activated by either photon energy or thermal energy that does not substantially activate the first polymerization initiator. Preferably, the second polymerization initiator is a thermal initiator. Examples of thermal initiators include, but are not limited to, azo compounds such as azobisisobutyronitrile and 4,4'-azobis(4-cyanovaleric acid), peroxides such as benzoyl peroxide, tert-butyl peroxide, tert-butyl hydroperoxide, tert-butyl peroxybenzoate, dicumyl peroxide, and lauroyl peroxide, peracids such as peracetic acid and potassium persulfate, and various redox systems. A preferred thermal initiator is azobisisobutyronitrile (AIBN). Optionally, the second polymerization initiator may contain a chemically bound second functional moiety that may be the same as or different from the first functional moiety. The second polymerization initiator is used in the reactive monomer mixture in an amount effective to initiate photopolymerization of the reactive monomer mixture, for example, from about 0.1 to about 2 parts by weight per 100 parts of the reactive monomer mixture.

[0084] According to the process of the present invention, one or more selected regions of the reactive monomer mixture (within the cavity of the mold assembly) are exposed to a source of actinic radiation of a first wavelength, thereby selectively activating a first polymerization initiator, thereby selectively polymerizing a portion of the reactive monomer mixture. Advantageously, the first polymerization initiator has a first functional moiety chemically bonded to it, such that the selectively polymerized portion of the reactive monomer mixture incorporates the first functional moiety.

[0085] For selective activation of the first polymerization initiator, various techniques can be used.Preferred technique is voxel-based lithography, which is generally described in, for example, US Patent Application Publication No. 20150146159, US Patent No. 9075186, and US Patent No. 8317505, each of which is incorporated herein by reference in its entirety.Further references include US Patent No. 7905594, US Patent No. 8157373, US Patent No. 8240849, US Patent No. 8313828, US Patent No. 8318055, US Patent No. 8795558, US Patent No. 9180633, US Patent No. 9180634, US Patent No. 9417464, US Patent No. 9610742, and US Patent No. 9857607, each of which is incorporated herein by reference in its entirety.

[0086] FIG. 1 shows an exemplary prior art apparatus described in U.S. Pat. No. 8,317,505 ("the '505 patent") that can be used to selectively control an array of individual beams of actinic radiation to cure or partially cure reactive monomer mixtures such as those used to form ophthalmic lenses. Light is generated by a source of actinic radiation or light source 120 and occurs as light that is at a wavelength within a defined band, but has spatial variations in intensity and direction. Element 130, a spatial intensity controller or collimator, focuses, diffuses, and in some embodiments collimates the light to produce a light beam 140 that is highly uniform in intensity and preferably centered around a predetermined wavelength. Furthermore, in some embodiments, beam 140 impinges on a digital mirror device ("DMD") 110, which includes an array of selectively controllable mirrors that split the beam into intensity pixel elements, each of which can be assigned a digital on or off value. In effect, each pixel mirror simply reflects the light down one of two paths. The "on" path, item 150, is the path that directs the photons traveling toward the reactive chemical medium. The "off" path is light that is reflected along a different path between the paths shown as items 116 and 117. This "off" path directs photons to strike a beam dump 115 that is carefully crafted to absorb and capture any photons that are directed at it. Returning to reference to the "on" path 150, the light shown on this path actually comprises many different potential pixel values ​​that are set to "on" values ​​and spatially directed along appropriate individual paths corresponding to their pixel locations. The time-averaged intensity of each of the pixel elements along their respective paths 150 can be shown as a spatial intensity profile 160 across the spatial grid defined by the DMD 110. Alternatively, with a constant intensity striking each mirror, item 160 can show a spatial-temporal exposure profile. The computer program that selectively controls the array of mirrors (on / off times) is referred to herein as a "script."

[0087] The '505 patent describes a beam that is normally incident on an optically transmissive molding optic 180 and enters a volume of reactive monomer mixture 302 (FIG. 2), where a selectively controllable beam of actinic radiation causes selective curing of the reactive monomers in the vat, voxel by voxel, through the molding optic according to a script.

[0088] The present invention may utilize the apparatus of Figures 1 and 2, but replace the molded optic (male mold) with a conventional two-part mold, such as the exemplary one shown in Figure 3. As shown in Figure 3, the curing apparatus 200 includes a first mold half 201 and a second mold half 202 that together form the shape of the cured contact lens to be formed, at least one of which is light-transmitting, and a reactive monomer mixture 204 fills the entire space between them. The first and second mold halves are fixed in place within the curing apparatus 200, which includes a first portion 210a and a second portion 210b, at least a portion of which (i.e., 210b in Figure 3) is also light-transmitting. A selectively controllable actinic radiation source 205, as described above, is directed to selectively impinge on the light-transmitting mold half and the exposure jig portion, as shown. The apparatus may further include a light absorber 212, designed to capture stray light after it has passed through the light-transmitting jig portion, the mold half, and the reactive monomer mixture. Alternatively, the opposing mold section and / or jig section may be non-transparent or otherwise light absorbing, such as when the mold section or jig section is constructed from a carbon black filled thermoplastic such as styrene or polymethylmethacrylate (PMMA).

[0089] Using the invention described herein, functional moieties (two- or three-dimensional), geometric shapes, or physical properties can be spatially incorporated into the ophthalmic lens formed between the two mold halves. As mentioned above, this can be accomplished by incorporating in the reactive monomer mix a first polymerization initiator attached to a first functional moiety that is activated by a first predetermined wavelength or range of wavelengths, and a second polymerization initiator attached or not attached to a second functional moiety. The second polymerization initiator can be activated by a second activation that does not substantially activate the first polymerization initiator. The second activation can be, for example, by application of light energy and / or heat energy. Thus, light energy and / or heat energy can be selectively applied by a curing device to selectively and differentially cure and / or otherwise selectively activate the functional chemistry.

[0090] As an example, the reactive monomer mixture may first be exposed to a first wavelength or range of wavelengths of light via the actinic radiation source 205 according to a predefined digital script as described above. The first wavelength of light activates a first polymerization initiator to cause free radical polymerization. The desired degree and depth of polymerization at each point in the array of beams of actinic radiation is defined by the preprogrammed script and wavelength of the actinic radiation, as the actinic radiation may interact lightly or heavily with the spectral absorption of the reactive monomer mixture in a manner consistent with Beer's Law. The first functional moiety attached to the first polymerization initiator is incorporated into the polymer chains of the selectively polymerized reactive monomer mixture. After exposure to actinic radiation, the mold assembly may be exposed to a second energy, preferably thermal energy, that does not substantially activate the first photoinitiator again. To accomplish this, the mold assembly shown in FIG. 3 may simply be placed in a thermally controlled environment, such as an oven, until the reactive monomer mixture is cured, for example, at about 90° C. for about 2-3 hours.

[0091] Alternatively, following exposure to the first actinic radiation, the mold halves and exposure jig assembly are placed in a thermal apparatus for about 20 minutes to allow sufficient gelation of the reactive monomer mixture to prevent undesired relative movement of the BC mold to the FC mold, at which point it is removed from the thermal apparatus and the exposure jig is removed from the mold halves. The mold halves are then immediately placed back into the thermal apparatus for the time for final curing. This allows the exposure jig to be reused as needed during the remainder of the final lens curing step. The formed lens object is then removed from the mold halves 202 and 203 and can undergo an extraction process to remove unreacted first polymerization initiator. The extraction process to remove unreacted first polymerization initiator can be complete or incomplete. In some cases, removal of all unreacted first polymerization initiator is not required to create the desired feature or optical effect. In other cases, the extraction process removes only a portion of the unreacted first polymerization initiator, allowing for an optional irradiation step using a lower concentration of first polymerization initiator. After removal of unreacted first polymerization initiator, standard post-processing steps of lens extraction and lens hydration to remove other reactive monomer components can be performed to form the final ophthalmic lens. In some instances, standard post-processing steps of lens extraction and hydration using aqueous alcohol, water, and buffers can also extract unreacted first polymerization initiator, thereby combining two or more extraction steps into one operation.

[0092] The resulting lens object has a variety of properties spatially integrated therein as determined by the different curing methods applied to each portion. The first functional moieties may be, for example, refractive index moieties, light absorbing moieties, or a combination thereof. The first wavelength, as well as its intensity and pattern, are selectively selected to interact with the spectral absorbance of the reactive monomer mixture, such that the desired two- or three-dimensional integration is achieved via Beer's Law effects, as described in detail in the '505 patent.

[0093] One application of the invention described herein involves incorporating functional chemistries within a lens that can change the refractive properties, which can be used to impart images or other visual features to the lens, for example for the purpose of producing bifocal or multifocal lenses, or to impart features that affect visual function.

[0094] Another application of the invention described herein is to incorporate dyes for cosmetic and / or light management purposes utilizing selected functional moieties. With regard to light management, current technology uses monomer dyes and a single initiator-based curing process. This process has no inherent spatial control and results in lenses with uniform properties throughout. Furthermore, when dyes are incorporated for light management purposes, the transmission profile of the lens is highly dependent on the thickness profile of the lens, and the concentration of the dye is typically selected to represent a compromise to achieve an average desired transmission across the optical zone of the lens over the range of optical power produced. The present invention can improve light management in lenses with selected patterns of dyes incorporated into the lens to achieve a desired transmission profile that varies throughout the lens, as opposed to a mostly thickness-defined profile as in the prior art. This can be achieved to some extent by pad printing onto the surface of the lens, but cannot currently be incorporated into the lens itself by known techniques. Pad printing also has the disadvantage that known pad printing techniques involve heavy dyes, dye-pigment combinations, or pigment-containing compounds applied in a thin printed layer that results in a non-uniform transmission profile due to small variations in the thickness of the printed layer typical of pad printing capabilities. Furthermore, there is a high probability of undesirable optical effects due to printing layers within the optical zone that have index matching / thickness variation issues.

[0095] While voxel-based lithography, as described above, is a preferred technique for selective activation of the first polymerization initiator, other techniques may also be utilized. For example, selective activation may be provided by photomasking from a first wavelength those areas of the reactive monomer mixture where polymerization is not desired. The unmasked areas of the reactive monomer mixture may then undergo activation and selective polymerization. The photomask may be binary in nature, but is more preferably grayscale. The specification and fabrication of photomasks of this type are known to those skilled in the art of grayscale photolithography.

[0096] Preferably, the reactive monomer mixture has sufficient viscosity so that the polymerized portion does not undesirably diffuse during or immediately after the first selective polymerization. Various options are available to provide such viscosity. For example, a reactive monomer mixture containing a viscous component such as a macromer or prepolymer can be used. Diluents can also be omitted or at least used at low concentrations to avoid significantly reducing the viscosity of the reactive monomer mixture.

[0097] A preferred approach is to perform a limited pre-cure of the reactive monomer mixture through a brief activation of a second polymerization initiator prior to or simultaneously with the first activation. Thus, for example, if the second polymerization initiator is a thermal initiator, the reactive monomer mixture in the mold assembly can be heated to briefly activate the thermal initiator and thus initiate some polymerization of the reactive monomer mixture. Initiation and polymerization can then be stopped once the desired viscosity has been achieved. By way of example, if the thermal initiator is AIBN, such pre-cure can be achieved by heating the reactive monomer mixture to a temperature in the range of, for example, 40-150°C for about 0.1-120 minutes. Preferably, the pre-cure step is performed prior to the selective activation of the first polymerization initiator.

[0098] According to the invention, the selective polymerization is followed by a complete cure of the reactive monomer mixture, using a second polymerization initiator present in the reactive monomer mixture, in particular, the second polymerization initiator is activated, thereby initiating the polymerization of the remaining reactive components in the reactive monomer mixture.

[0099] As discussed above, the reactive monomer mix of the present invention contains monomers suitable for making the desired ophthalmic lens. By way of further example, the reactive monomer mix may include one or more of a hydrophilic component, a hydrophobic component, a silicone-containing component, a wetting agent such as a polyamide, a crosslinker, and additional components such as a diluent and an initiator.

[0100] hydrophilic component Examples of suitable families of hydrophilic monomers that may be present in the reactive monomer mixture include (meth)acrylates, styrenes, vinyl ethers, (meth)acrylamides, N-vinyl lactams, N-vinyl amides, N-vinyl imides, N-vinyl ureas, O-vinyl carbamates, O-vinyl carbonates, other hydrophilic vinyl compounds, and mixtures thereof.

[0101] Non-limiting examples of hydrophilic (meth)acrylate and (meth)acrylamide monomers include acrylamide, N-isopropylacrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N,N-dimethylacrylamide (DMA), 2-hydroxyethyl methacrylate (HEMA), 2-hydroxypropyl(meth)acrylate, 3-hydroxypropyl(meth)acrylate, 2,3-dihydroxypropyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, 3-hydroxybutyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, N-(2-hydroxyethyl)(meth)acrylamide, N,N-bis(2-hydroxyethyl)(meth)acrylamide, N-(2-hydroxypropyl)(meth)acrylamide, N,N-bis(2-hydroxypropyl)(meth)acrylamide, N-(3 ... N-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, N-(4-hydroxybutyl)(meth)acrylamide, 2-aminoethyl(meth)acrylate, 3-aminopropyl(meth)acrylate, 2-aminopropyl(meth)acrylate, N-2-aminoethyl(meth)acrylamide), N-3-aminopropyl(meth)acrylamide, N-2-aminopropyl(meth)acrylamide, N,N-bis-2-aminoethyl(meth)acrylamide, N,N-bis-3-aminopropyl(meth)acrylamide), N,N-bis-2-aminopropyl(meth)acrylamide, glycerol methacrylate, polyethylene glycol monomethacrylate, (meth)acrylic acid, vinyl acetate, acrylonitrile, and mixtures thereof.

[0102] The hydrophilic monomers may also be ionic, such as anionic, cationic, zwitterionic, betaine, and mixtures thereof. Non-limiting examples of such charged monomers include (meth)acrylic acid, N-[(ethenyloxy)carbonyl]-β-alanine (VINAL), 3-acrylamidopropanoic acid (ACA1), 5-acrylamidopropanoic acid (ACA2), 3-acrylamido-3-methylbutanoic acid (AMBA), 2-(methacryloyloxy)ethyltrimethylammonium chloride (Q salt or METAC), 2-acrylamido-2-methylpropanesulfonic acid (AMPS), 1-propanaminium, N-(2-carboxyethyl)-N,N-dimethyl-3-[(1-oxo-2-propen-1-yl)amino]-, inner salt (CBT), 1-propanaminium, N,N-dimethyl-N-[3-[(1-oxo-2-propen-1-yl)amino]propyl]-3-sulfo-, inner salt (SBT), 3,5 dioxa- 8-Aza-4-phosphanedec-10-en-1-aminium, 4-hydroxy-N,N,N-trimethyl-9-oxo-, inner salt, 4-oxide (9CI) (PBT), 2-methacryloyloxyethyl phosphorylcholine, 3-(dimethyl(4-vinylbenzyl)ammonio)propane-1-sulfonate (DMVBAPS), 3-((3-acrylamidopropyl)dimethylammonio)propane-1-sulfonate (AMPDAPS), 3-((3-methacrylamidopropyl)dimethylammonio)propane-1-sulfonate (MAMPDAPS), 3-((3-(acryloyloxy)propyl)dimethylammonio)propane-1-sulfonate (APDAPS), and methacryloyloxy)propyl)dimethylammonio)propane-1-sulfonate (MAPDAPS).

[0103] Non-limiting examples of hydrophilic N-vinyl lactam and N-vinyl amide monomers include N-vinyl pyrrolidone (NVP), N-vinyl-2-piperidone, N-vinyl-2-caprolactam, N-vinyl-3-methyl-2-caprolactam, N-vinyl-3-methyl-2-piperidone, N-vinyl-4-methyl-2-piperidone, N-vinyl-4-methyl-2-caprolactam, N-vinyl-3-ethyl-2-pyrrolidone, N-vinyl-4,5-dimethyl-2-pyrrolidone, N-vinyl acetamide (NVA), N-vinyl-N-methyl acetamide (VMA), N-vinyl-N-ethyl acetamide, N-vinyl-N-ethyl formamide, N-vinyl formamide, N-vinyl-N-methyl propionamide, N-vinyl-N-methyl-2-methyl propionamide, N-vinyl ... N-methylpropionamide, N-vinyl-N,N'-dimethylurea, 1-methyl-3-methylene-2-pyrrolidone, 1-methyl-5-methylene-2-pyrrolidone, 5-methyl-3-methylene-2-pyrrolidone, 1-ethyl-5-methylene-2-pyrrolidone, N-methyl-3-methylene-2-pyrrolidone, 5-ethyl-3-methylene-2-pyrrolidone, 1-N-propyl-3-methylene-2-pyrrolidone, 1-N-propyl-5-methylene-2-pyrrolidone, 1-isopropyl-3-methylene-2-pyrrolidone, 1-isopropyl-5-methylene-2-pyrrolidone, N-vinyl-N-ethylacetamide, N-vinyl-N-ethylformamide, N-vinylformamide, N-vinylisopropylamide, N-vinylcaprolactam, N-vinylimidazole, and mixtures thereof.

[0104] Non-limiting examples of hydrophilic O-vinyl carbamate and O-vinyl carbonate monomers include N-2-hydroxyethyl vinyl carbamate and N-carboxy-β-alanine N-vinyl ester. Further examples of hydrophilic vinyl carbonate or vinyl carbamate monomers are disclosed in U.S. Patent No. 5,070,215. Hydrophilic oxazolone monomers are disclosed in U.S. Patent No. 4,910,277.

[0105] Other hydrophilic vinyl compounds include ethylene glycol vinyl ether (EGVE), di(ethylene glycol) vinyl ether (DEGVE), allyl alcohol, and 2-ethyloxazoline.

[0106] The hydrophilic monomer may also be a macromer or prepolymer of linear or branched poly(ethylene glycol), poly(propylene glycol), or statistical random or block copolymers of ethylene oxide and propylene oxide, having polymerizable moieties such as (meth)acrylates, styrenes, vinyl ethers, (meth)acrylamides, N-vinyl amides, etc. Macromers of these polyethers have one polymerizable group and prepolymers may have two or more polymerizable groups.

[0107] Preferred hydrophilic monomers of the present invention are DMA, NVP, HEMA, VMA, NVA, and mixtures thereof. Preferred hydrophilic monomers include mixtures of DMA and HEMA. Other suitable hydrophilic monomers will be apparent to those skilled in the art.

[0108] Generally, there is no particular limitation regarding the amount of hydrophilic monomer present in the reactive monomer mixture. The amount of hydrophilic monomer can be selected based on the desired properties of the resulting hydrogel, including water content, transparency, wettability, protein uptake, and the like. Wettability can be measured by contact angle, with desirable contact angles being less than about 100°, less than about 80°, and less than about 60°. The hydrophilic monomer can be present in an amount ranging from about 0.1 to about 100% by weight, alternatively from about 1 to about 80% by weight, alternatively from about 5 to about 65% by weight, alternatively from about 40 to about 60% by weight, alternatively from about 55 to about 60% by weight, based on the total weight of the reactive components in the reactive monomer mixture.

[0109] Silicone-containing ingredients Silicone-containing components suitable for use in the reactive monomer mixture of the present invention include one or more polymerizable compounds, each compound independently including at least one polymerizable group, at least one siloxane group, and one or more linking groups connecting the polymerizable group(s) to the siloxane group(s). The silicone-containing component may contain, for example, 1 to 220 siloxane repeat units, such as those defined below. The silicone-containing component may also contain at least one fluorine atom.

[0110] The silicone-containing component may include one or more polymerizable groups as defined above; one or more optionally repeating siloxane units; and one or more linking groups connecting the polymerizable groups to the siloxane units. The silicone-containing component may include one or more polymerizable groups that are independently (meth)acrylate, styryl, vinyl ether, (meth)acrylamide, N-vinyl lactam, N-vinyl amide, O-vinyl carbamate, O-vinyl carbonate, vinyl groups, or mixtures thereof; one or more optionally repeating siloxane units; and one or more linking groups connecting the polymerizable groups to the siloxane units.

[0111] The silicone-containing component may include, independently, one or more polymerizable groups that are (meth)acrylate, (meth)acrylamide, N-vinyl lactam, N-vinyl amide, styryl, or mixtures of the foregoing; one or more optionally repeating siloxane units; and one or more linking groups connecting the polymerizable groups to the siloxane units.

[0112] The silicone-containing component may include, independently, one or more polymerizable groups that are (meth)acrylate, (meth)acrylamide, or a mixture of the foregoing; one or more optionally repeating siloxane units; and one or more linking groups connecting the polymerizable groups to the siloxane units.

[0113] The silicone-containing component has the formula A:

[0114] [ka] During the ceremony, At least one R A is the formula R g -L-, where R g is a polymerizable group, L is a linking group, and the remaining R A are, independently: (a)R g -L-, (b) C1-C optionally substituted with one or more hydroxy, amino, amido, oxa, carboxy, alkylcarboxy, carbonyl, alkoxy, amido, carbamate, carbonate, halo, phenyl, benzyl, or combinations thereof. 16 Alkyl, (c) C-C optionally substituted with one or more alkyl, hydroxy, amino, amido, oxa, carbonyl, alkoxy, amido, carbamate, carbonate, halo, phenyl, benzyl, or combinations thereof. 12 Cycloalkyl, (d) C-C optionally substituted with one or more alkyl, hydroxy, amino, amido, oxa, carboxy, alkylcarboxy, carbonyl, alkoxy, amido, carbamate, carbonate, halo, phenyl, benzyl, or combinations thereof. 14 Aryl groups, (e) halo, (f) alkoxy, cyclic alkoxy, or aryloxy, (g) siloxy, (h) alkyleneoxy-alkyl or alkoxy-alkyleneoxy-alkyl, such as polyethyleneoxyalkyl, polypropyleneoxyalkyl, or poly(ethyleneoxy-co-propyleneoxyalkyl); or (i) a monovalent siloxane chain comprising 1 to 100 siloxane repeat units optionally substituted with alkyl, alkoxy, hydroxy, amino, oxa, carboxy, alkylcarboxy, alkoxy, amido, carbamate, halo, or combinations thereof; (n is 0 to 500, or 0 to 200, or 0 to 100, or 0 to 20, and when n is other than 0, it is understood that n is a distribution having a mode equivalent to the indicated value). When n is 2 or more, the SiO units may contain one or more polymerizable compounds of the same or different R A may carry substituents, different R A When substituents are present, the n groups may be in a random or block configuration.

[0115] In formula A, three R A may each contain a polymerizable group, alternatively two R A may each contain a polymerizable group, or alternatively one R A may contain a polymerizable group.

[0116] Examples of silicone-containing components suitable for use in the present invention include, but are not limited to, the compounds listed in Table B. When the compounds in Table B contain polysiloxane groups, the number of SiO repeat units in such compounds is preferably 3 to 100, more preferably 3 to 40, or even more preferably 3 to 20, unless otherwise specified.

[0117] [Table 2-1]

[0118] [Table 2-2]

[0119] Additional non-limiting examples of suitable silicone-containing components are listed in Table C. Unless otherwise stated, where applicable, j2 is preferably 1-100, more preferably 3-40, or even more preferably 3-15. In compounds containing j1 or j2, the sum of j1 and j2 is preferably 2-100, more preferably 3-40, or even more preferably 3-15.

[0120] [Table 3-1]

[0121] [Table 3-2]

[0122] Mixtures of silicone-containing components may also be used.For example, suitable mixtures may include, but are not limited to, mixtures of mono-(2-hydroxy-3-methacryloxypropyloxy)-propyl-terminated mono-n-butyl-terminated polydimethylsiloxanes (OH-MPDMS) with different molecular weights, such as mixtures of OH-mPDMS containing 4 and 15 repeating SiO units; mixtures of OH-mPDMS with different molecular weights (e.g., containing 4 and 15 repeating SiO units) and silicone-based crosslinkers, such as bis-3-acryloxy-2-hydroxypropyloxypropyl polydimethylsiloxanes (ac-PDMS); mixtures of 2-hydroxy-3-[3-methyl-3,3-di(trimethylsiloxy)silylpropoxy]-propyl methacrylate (SiMAA) and mono-methacryloxypropyl-terminated mono-n-butyl-terminated polydimethylsiloxanes (mPDMS), such as mPDMS1000.

[0123] The silicone-containing component used in the present invention can have an average molecular weight of from about 400 to about 4000 Daltons.

[0124] The silicone-containing component(s) may be present in an amount up to about 95%, or from about 10 to about 80%, or from about 20 to about 70% by weight of the reactive monomer mixture (excluding diluent), based on all reactive components.

[0125] polyamide The reactive monomer mixture may include at least one polyamide. As used herein, the term "polyamide" refers to polymers and copolymers that include repeating units that contain amide groups. The polyamide may include cyclic amide groups, non-cyclic amide groups, and combinations thereof, and may be any polyamide known to those skilled in the art. Non-cyclic polyamides include pendant non-cyclic amide groups and are capable of association with hydroxyl groups. Cyclic polyamides include cyclic amide groups and are capable of association with hydroxyl groups.

[0126] Examples of suitable acyclic polyamides include polymers and copolymers comprising repeat units of the formulae G1 and G2:

[0127] [ka] In the formula, X is a direct bond, -(CO)-, or -(CONHR 44 )-, where R 44 is a C1-C3 alkyl group; R 40 is selected from H, linear or branched, substituted or unsubstituted C1-C4 alkyl groups; R 41 is selected from H, linear or branched, substituted or unsubstituted C1-C4 alkyl groups, amino groups having up to 2 carbon atoms, amido groups having up to 4 carbon atoms, and alkoxy groups having up to 2 carbon atoms; R 42 is selected from H, linear or branched, substituted or unsubstituted C1-C4 alkyl groups; or selected from methyl, ethoxy, hydroxyethyl, and hydroxymethyl; R 43 is selected from H, linear or branched, substituted or unsubstituted C1-C4 alkyl groups; or selected from methyl, ethoxy, hydroxyethyl, and hydroxymethyl; R 40 and R 41 The total number of carbon atoms in R is 8 or less, including 7, 6, 5, 4, 3, or less; 42 and R 43 The total number of carbon atoms in R is 8 or less, including 7, 6, 5, 4, 3, or less. 40 and R 41The total number of carbon atoms in R may be 6 or less, or 4 or less. 42 and R 43 The total number of carbon atoms in may be up to 6. As used herein, a substituted alkyl group includes an alkyl group substituted with an amine group, an amide group, an ether group, a hydroxyl group, a carbonyl group, or a carboxyl group, or combinations thereof.

[0128] R 40 and R 41 may be independently selected from H, a substituted or unsubstituted C1-C2 alkyl group; X may be a direct bond, and R 40 and R 41 may be independently selected from H, a substituted or unsubstituted C1-C2 alkyl group. 42 and R 43 may be independently selected from H, a substituted or unsubstituted C1-C2 alkyl group, methyl, ethoxy, hydroxyethyl, and hydroxymethyl.

[0129] The acyclic polyamides of the present invention may comprise a majority of repeat units of formula LV or formula LVI, or the acyclic polyamides may comprise at least 50 mol % of repeat units of formula G or formula G1, such as at least about 70 mol %, and at least 80 mol %. Specific examples of repeat units of formula G and formula G1 include repeat units derived from N-vinyl-N-methylacetamide, N-vinylacetamide, N-vinyl-N-methylpropionamide, N-vinyl-N-methyl-2-methylpropionamide, N-vinyl-2-methyl-propionamide, N-vinyl-N,N'-dimethylurea, N,N-dimethylacrylamide, methacrylamide, and acyclic amides of formulas G2 and G3,

[0130] [ka]

[0131] Examples of suitable cyclic amides that can be used to form the cyclic polyamides include α-lactams, β-lactams, γ-lactams, δ-lactams, and ε-lactams. Examples of suitable cyclic polyamides include those represented by formula G4:

[0132] [ka] (In the formula, R 45 is a hydrogen atom or a methyl group; f is a number from 1 to 10; X is a direct bond, -(CO)-, or -(CONHR 46 )- and R 46 is a C1-C3 alkyl group). In formula LIX, f can be 8 or less, including 7, 6, 5, 4, 3, 2, or 1. In formula G4, f can be 6 or less, including 5, 4, 3, 2, or 1. In formula G4, f can be 2 to 8, including 2, 3, 4, 5, 6, 7, or 8. In formula LIX, f can be 2 or 3. When X is a direct bond, f can be 2. In such cases, the cyclic polyamide can be polyvinylpyrrolidone (PVP).

[0133] The cyclic polyamides of the present invention may comprise 50 mol % or more of repeat units of formula G4, or the cyclic polyamides may comprise at least 50 mol % of repeat units of formula G4, such as at least 70 mol %, and at least 80 mol %.

[0134] Polyamides may also be copolymers containing both cyclic and non-cyclic amide repeat units. The additional repeat units may be formed from monomers selected from hydroxyalkyl (meth)acrylates, alkyl (meth)acrylates, other hydrophilic monomers, and siloxane-substituted (meth)acrylates. Any of the monomers listed as suitable hydrophilic monomers may be used as comonomers to form the additional repeat units. Specific examples of additional monomers that may be used to form polyamides include 2-hydroxyethyl (meth)acrylate, vinyl acetate, acrylonitrile, hydroxypropyl (meth)acrylate, methyl (meth)acrylate and hydroxybutyl (meth)acrylate, dihydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, and the like, and mixtures thereof. Ionic monomers may also be included.Examples of ionic monomers include (meth)acrylic acid, N-[(ethenyloxy)carbonyl]-β-alanine (VINAL, CAS#148969-96-4), 3-acrylamidopropanoic acid (ACA1), 5-acrylamidopropanoic acid (ACA2), 3-acrylamido-3-methylbutanoic acid (AMBA), 2-(methacryloyloxy)ethyltrimethylammonium chloride (Q salt or METAC), 2-acrylamido-2-methylpropanesulfonic acid (AMPS), 1-propanaminium, N-(2-carboxyethyl)-N,N-dimethyl-3-[(1-oxo-2-propen-1-yl)amino]-, inner salt (CBT, carboxybetaine; CAS 79704-35-1), 1-propanaminium, N,N-dimethyl-N-[3-[(1-oxo-2-propen-1-yl)amino]propyl]-3-sulfo-, inner salt (SBT, sulfobetaine, CAS 80293-60-3), 3,5-dioxa-8-aza-4-phosphanundeca-10-ene-1-aminium, 4-hydroxy-N,N,N-trimethyl-9-oxo-, inner salt, 4-oxide (9CI) (PBT, phosphobetaine, CAS 163674-35-9, 2-methacryloyloxyethyl phosphorylcholine, 3-(dimethyl(4-vinylbenzyl)ammonio)propane-1-sulfonate (DMVBAPS), 3-((3-acrylamidopropyl)dimethylammonio)propane-1-sulfonate (AMPDAPS), 3-((3-methacrylamidopropyl)dimethylammonio)propane-1-sulfonate (MAMPDAPS), 3-((3-(acryloyloxy)propyl)dimethylammonio)propane-1-sulfonate (APDAPS), methacryloyloxy)propyl)dimethylammonio)propane-1-sulfonate (MAPDAPS).

[0135] The reactive monomer mixture may include both acyclic and cyclic polyamides or copolymers thereof. The acyclic polyamide may be any of the acyclic polyamides or copolymers thereof described herein, and the cyclic polyamide may be any of the cyclic polyamides or copolymers thereof described herein. The polyamide may be selected from the group of polyvinylpyrrolidone (PVP), polyvinylmethylacetamide (PVMA), polydimethylacrylamide (PDMA), polyvinylacetamide (PNVA), poly(hydroxyethyl(meth)acrylamide), polyacrylamide, and copolymers and mixtures thereof. The polyamide may be a combination of PVP (e.g., PVP K90) and PVMA (e.g., PVMA with an M of about 570 KDa). w The mixture may be

[0136] The total amount of all polyamides in the reactive monomer mix can be in the range of 1% to about 35% by weight, such as in the range of 1% to about 15% by weight, and such as in the range of about 5% to about 15% by weight, in all cases based on the total weight of the reactive components of the reactive monomer mix.

[0137] Without being bound by theory, when used with silicone hydrogels, polyamides function as internal wetting agents. The polyamides of the present invention may be non-polymeric, in which case they are incorporated into the silicone hydrogel as a semi-interpenetrating network. The polyamides are encapsulated or physically held within the silicone hydrogel. Alternatively, the polyamides of the present invention may be polymeric, for example as polyamide macromers or prepolymers, in which case they are covalently incorporated into the silicone hydrogel. Mixtures of polymeric and non-polymeric polyamides may also be used.

[0138] When a polyamide is incorporated within the reactive monomer mixture, the polyamide may have a weight average molecular weight of at least 100,000 Daltons, greater than about 150,000, from about 150,000 to about 2,000,000 Daltons, from about 300,000 Daltons to about 1,800,000 Daltons. Higher molecular weight polyamides can be used if compatible with the reactive monomer mixture.

[0139] Crosslinking Agent Generally, it is desirable to add one or more crosslinking agents, also referred to as crosslinking monomers, multifunctional macromers, and prepolymers, to the reactive monomer mixture. The crosslinking agents may be selected from difunctional crosslinkers, trifunctional crosslinkers, tetrafunctional crosslinkers, and mixtures thereof, including silicone-containing and non-silicone-containing crosslinkers. Non-silicone-containing crosslinkers include ethylene glycol dimethacrylate (EGDMA), tetraethylene glycol dimethacrylate (TEGDMA), trimethylolpropane trimethacrylate (TMPTMA), triallyl cyanurate (TAC), glycerol trimethacrylate, methacryloxyethyl vinyl carbonate (HEMAVc), allyl methacrylate, methylene bisacrylamide (MBA), and polyethylene glycol dimethacrylate, where the polyethylene glycol has a molecular weight of up to about 5000 Daltons. The crosslinking agents are used in the reactive monomer mixture in conventional amounts, for example, from about 0.000415 to about 0.0156 moles per 100 grams of reactive formulation. Alternatively, if hydrophilic monomer and / or silicone-containing component is multifunctional due to molecular design or impurities, adding crosslinker to reactive monomer mixture is optional. Examples of hydrophilic monomer and macromer that can act as crosslinker and do not require additional crosslinker to be added to reactive monomer mixture when present include (meth)acrylate and (meth)acrylamide end-capped polyether. Other crosslinkers will be known to those skilled in the art and can be used to make the silicone hydrogel of the present invention.

[0140] It may be desirable to select a crosslinker that has a similar reactivity to one or more of the other reactive components in the formulation. In some cases, it may be desirable to select a mixture of crosslinkers with different reactivities to control some physical, mechanical, or biological properties of the resulting silicone hydrogel. The structure and morphology of the silicone hydrogel may also be affected by the diluent(s) and curing conditions used.

[0141] Multifunctional silicone-containing components, including macromers, crosslinkers, and prepolymers, may also be included to further increase modulus and maintain tensile strength. Silicone-containing crosslinkers may be used alone or in combination with other crosslinkers. An example of a silicone-containing component that can act as a crosslinker and does not require the addition of a crosslinking monomer to the reactive monomer mixture when present includes α,ω-bismethacryloylpropyl polydimethylsiloxane. Another example is bis-3-acryloxy-2-hydroxypropyloxypropyl polydimethylsiloxane (ac-PDMS).

[0142] Crosslinkers with hard chemical structures and polymerizable groups that undergo free radical polymerization may also be used. Non-limiting examples of suitable hard structures include crosslinkers containing phenyl and benzyl rings, such as 1,4-phenylenediacrylate, 1,4-phenylenedimethacrylate, 2,2-bis(4-methacryloxyphenyl)-propane, 2,2-bis[4-(2-acryloxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxy-3-methacryloxypropoxy)phenyl]propane, and 4-vinylbenzyl methacrylate, and combinations thereof. Hard crosslinkers may be included in an amount of about 0.5 to about 15, or about 2 to 10, 3 to 7, based on the total weight of all reactive components. The physical and mechanical properties of the silicone hydrogels of the present invention may be optimized for a particular application by adjusting the components in the reactive monomer mixture.

[0143] Non-limiting examples of silicone crosslinkers also include the multifunctional silicone-containing components set forth in Table C above.

[0144] Further components The reactive monomer mixture may contain additional components such as, but not limited to, diluents, initiators, UV absorbers, visible light absorbers, photochromic compounds, pharmaceuticals, nutritional supplements, antimicrobial substances, colorants, pigments, copolymerizable dyes, non-polymerizable dyes, release agents, and combinations thereof.

[0145] Suitable types of diluents for the silicone hydrogel reactive monomer mixture include alcohols having 2 to 20 carbon atoms, amides derived from primary amines having 10 to 20 carbon atoms, and carboxylic acids having 8 to 20 carbon atoms. The diluents can be primary, secondary, and tertiary alcohols.

[0146] Generally, the reactive components are mixed in a diluent to form a reactive monomer mixture. Suitable diluents are known in the art. For silicone hydrogels, suitable diluents are disclosed in WO 03 / 022321 and US 6,020,445, the disclosures of which are incorporated herein by reference.

[0147] Suitable diluent classes for the silicone hydrogel reactive monomer mixture include alcohols having 2-20 carbons, amides having 10-20 carbon atoms derived from primary amines, and carboxylic acids having 8-20 carbon atoms. Primary and tertiary alcohols may be used. Preferred classes include alcohols having 5-20 carbons and carboxylic acids having 10-20 carbon atoms.

[0148] Specific diluents that may be used include 1-ethoxy-2-propanol, diisopropylaminoethanol, isopropanol, 3,7-dimethyl-3-octanol, 1-decanol, 1-dodecanol, 1-octanol, 1-pentanol, 2-pentanol, 1-hexanol, 2-hexanol, 2-octanol, 3-methyl-3-pentanol, tert-amyl alcohol, tert-butanol, 2-butanol, 1-butanol, 2-methyl-2 ... Examples of diluents include ethanol, 2-propanol, 1-propanol, ethanol, 2-ethyl-1-butanol, (3-acetoxy-2-hydroxypropyloxy)-propylbis(trimethylsiloxy)methylsilane, 1-tert-butoxy-2-propanol, 3,3-dimethyl-2-butanol, tert-butoxyethanol, 2-octyl-1-dodecanol, decanoic acid, octanoic acid, dodecanoic acid, 2-(diisopropylamino)ethanol, mixtures thereof, and the like. Examples of amide diluents include N,N-dimethylpropionamide and dimethylacetamide.

[0149] Preferred diluents include 3,7-dimethyl-3-octanol, 1-dodecanol, 1-decanol, 1-octanol, 1-pentanol, 1-hexanol, 2-hexanol, 2-octanol, 3-methyl-3-pentanol, 2-pentanol, t-amyl alcohol, tert-butanol, 2-butanol, 1-butanol, 2-methyl-2-pentanol, 2-ethyl-1-butanol, ethanol, 3,3-dimethyl-2-butanol, 2-octyl-1-dodecanol, decanoic acid, octanoic acid, dodecanoic acid, mixtures thereof, and the like.

[0150] More preferred diluents include 3,7-dimethyl-3-octanol, 1-dodecanol, 1-decanol, 1-octanol, 1-pentanol, 1-hexanol, 2-hexanol, 2-octanol, 1-dodecanol, 3-methyl-3-pentanol, 1-pentanol, 2-pentanol, t-amyl alcohol, tert-butanol, 2-butanol, 1-butanol, 2-methyl-2-pentanol, 2-ethyl-1-butanol, 3,3-dimethyl-2-butanol, 2-octyl-1-dodecanol, mixtures thereof, and the like.

[0151] When a diluent is present, there is generally no particular limit as to the amount of diluent present. When a diluent is used, it may be present in an amount ranging from about 2 to about 70% by weight, such as from about 5 to about 50% by weight and from about 15 to about 40% by weight, based on the total weight of the reactive monomer mixture (including reactive and non-reactive compounds). Mixtures of diluents may also be used.

[0152] The reactive monomer mixture for producing the ophthalmic lens of the present invention may contain, in addition to the first and second polymerization initiators, any of the polymerizable compounds and optional components described above.

[0153] The reactive monomer mixture may include a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, and a hydrophilic component.

[0154] The reactive monomer mixture may include a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, a hydrophilic component, and a hydrophilic component selected from DMA, NVP, HEMA, VMA, NVA, methacrylic acid, and mixtures thereof, with mixtures of HEMA and methacrylic acid being preferred.

[0155] The reactive monomer mixture may include a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, a hydrophilic component, a hydrophilic component, and a silicone-containing component.

[0156] The reactive monomer mixture may include a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, a hydrophilic component selected from DMA, HEMA, and mixtures thereof. It may include a silicone-containing component selected from 2-hydroxy-3-[3-methyl-3,3-di(trimethylsiloxy)silylpropoxy]-propyl methacrylate (SiMAA), mono-methacryloxypropyl terminated mono-n-butyl terminated polydimethylsiloxane (mPDMS), mono-(2-hydroxy-3-methacryloxypropyl)-propyl ether terminated mono-n-butyl terminated polydimethylsiloxane (OH-mPDMS), and mixtures thereof, and a wetting agent (preferably PVP or PVMA). For the hydrophilic component, a mixture of DMA and HEMA is preferred. For the silicone-containing component, a mixture of SiMAA and mPDMS is preferred.

[0157] The reactive monomer mixture may include a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, a hydrophilic component, a hydrophilic component comprising a mixture of DMA and HEMA, and a silicone-containing component comprising a mixture of OH-mPDMS having 2-20 repeat units (preferably a mixture of 4 and 15 repeat units). Preferably, the reactive monomer mixture further comprises a silicone-containing crosslinker such as ac-PDMS. Also preferably, the reactive monomer mixture contains a wetting agent (preferably DMA, PVP, PVMA, or a mixture thereof).

[0158] The reactive monomer mixture comprises a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, and a hydrophilic component; from about 1 to about 15 weight percent of at least one polyamide (e.g., acyclic polyamide, cyclic polyamide, or mixtures thereof), at least one first monofunctional hydroxyl-substituted poly(disubstituted siloxane) having 4 to 8 siloxane repeat units (e.g., OH-mPDMS, where n is 4 to 8, preferably n is 4), and at least one second hydroxyl-substituted poly(disubstituted siloxane) that is a monofunctional hydroxyl-substituted poly(disubstituted siloxane) having 10 to 200, or 10 to 100, or 10 to 50, or 10 to 20 siloxane repeat units. and from about 5 to about 35 weight percent of at least one hydrophilic monomer, and optionally a multifunctional hydroxyl-substituted poly(disubstituted siloxane) having 10 to 200 or 10 to 100 siloxane repeat units (e.g., ac-PDMS). Preferably, the first monofunctional hydroxyl-substituted poly(disubstituted siloxane) and the second hydroxyl-substituted poly(disubstituted siloxane) are present in concentrations to provide a ratio of the weight percent of the first monofunctional hydroxyl-substituted poly(disubstituted siloxane) to the weight percent of the second hydroxyl-substituted poly(disubstituted siloxane) of 0.4 to 1.3 or 0.4 to 1.0.

[0159] The reactive monomer mixture may include a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, a hydrophilic component, such as DMA, a silicone-containing component such as compound 8 (TRIS) of Table B, a silicone macromer such as compound 42 of Table C.

[0160] The reactive monomer mixture may include a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, a hydrophilic component, such as DMA and / or NVP; a silicone-containing component, such as compound 14 (TRIS-Am) in Table B, a silicone macromer, such as compound 43 (IEM-PDMS-IPDI-PDMS-IPDI-PDMS-IEM) in Table C.

[0161] The reactive monomer mixture may include a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, a hydrophilic component, such as VMA, and a silicone macromer, such as compound 35 of Table C.

[0162] The reactive monomer mixture may include a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, a hydrophilic component, such as VMA and / or NVP; a silicone-containing component, such as compound 28 of Table C (e.g., where j2 is about 16), a silicone macromer, such as compound 35 of Table C.

[0163] The reactive monomer mixture may include a first polymerization initiator having a first functional moiety chemically bonded thereto, a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, a hydrophilic component, such as VMA and / or NVP; a silicone-containing component, such as compound 18 of Table B (e.g., where j2 is about 4), a silicone macromer, such as compound 41 of Table C.

[0164] The reactive monomer mixture may contain optional components such as, but not limited to, internal wetting agents, crosslinkers, other UV or HEV absorbers, and diluents. Additionally, ophthalmic lenses made from the reactive monomer mixture may be subjected to further processing, including, but not limited to, plasma treatment, application of coatings (such as in-package coatings (IPC) as described in U.S. Pat. No. 8,480,227), and the like.

[0165] The formed lens object may then be removed from the mold halves by mechanical means, solvent swelling, or a combination thereof, and then undergo an extraction process to remove unreacted first polymerization initiator. The extraction process to remove unreacted first polymerization initiator may be complete or incomplete. In some cases, removal of all unreacted first polymerization initiator is not required to create the desired feature or optical effect. In other cases, the extraction process removes only a portion of the unreacted first polymerization initiator, allowing for an optional irradiation step using a lower concentration of first polymerization initiator. Alternatively, the extraction process may remove substantially all of the unreacted first polymerization initiator. After removal of the unreacted first polymerization initiator, standard post-processing steps of lens extraction and lens hydration to remove other reactive monomer components may be performed to form the final ophthalmic lens. In some instances, standard post-processing steps of lens extraction and hydration using aqueous alcohol, water, and buffers may also extract unreacted first polymerization initiator, thereby combining two or more extraction steps into one operation.

[0166] An aqueous solution is a solution that contains water. The aqueous solution of the present invention may contain at least about 20% water by weight, or at least about 50% water by weight, or at least about 70% water by weight, or at least about 95% water by weight. The aqueous solution may also contain additional water-soluble ingredients, such as inorganic salts or release agents, wetting agents, slip agents, pharmaceutical ingredients and nutritional supplements, combinations thereof. A release agent is a compound or mixture of compounds that, when combined with water, reduces the time required to remove a contact lens from a mold when compared to the time required to remove a contact lens using an aqueous solution that does not contain a release agent. The aqueous solution may not require special handling, such as purification, recycling, or special waste disposal.

[0167] Extraction may occur, for example, via immersion of the lens in an aqueous solution or exposure of the lens to a stream of an aqueous solution. Extraction may also include, for example, one or more of heating the aqueous solution, agitating the aqueous solution, increasing the concentration of a release agent in the aqueous solution to a level sufficient to cause release of the lens, mechanical or ultrasonic agitation of the lens, and incorporating at least one leaching or extraction aid into the aqueous solution to a sufficient concentration to facilitate adequate removal of unreacted components from the lens. The foregoing may be performed in a batch or continuous process, with or without the addition of heat, vibration, or both.

[0168] To facilitate leaching and demolding, it may be desirable to apply physical agitation. For example, the lens mold part to which the lens is attached can be vibrated or moved back and forth in the aqueous solution. Other methods may include passing ultrasound through the aqueous solution.

[0169] The lenses may be sterilized by known means, such as, but not limited to, high pressure steam treatment.

[0170] As mentioned above, the preferred ophthalmic lens is a contact lens, more preferably a soft hydrogel contact lens. The silicone hydrogel ophthalmic lens (e.g., contact lens) according to the present invention may preferably exhibit the following characteristics. All values ​​are preceded by "about", and the device may have any combination of the listed properties. The characteristics can be determined by methods known to those skilled in the art, for example, as described in U.S. Pre-grant Publication No. 20180037690, which is incorporated herein by reference.

[0171] Water concentration %: at least 20%, or at least 25% and at most 80%, or at most 70% Haze: 30% or less, or 10% or less Advancing dynamic contact angle (Wilhelmy plate method): 100° or less, or 80° or less, or 50° or less Tensile modulus (psi): 120 or less, or 80-120 Oxygen permeability (Dk, Barrer): at least 80, or at least 100, or at least 150, or at least 200 Elongation at break: at least 100

[0172] With respect to ionic silicone hydrogels, the following properties may also be preferred (in addition to those mentioned above): Lysozyme uptake (μg / lens): at least 100, or at least 150, or at least 500, or at least 700 Polyquaternium 1 (PQ1) uptake (%): 15 or less, or 10 or less, or 5 or less Some embodiments of the present invention are described in detail in the following examples. EXAMPLES

[0173] The following abbreviations are used throughout the examples and figures and have the following meanings: DMA: N,N-dimethylacrylamide (Jarchem) HEMA: 2-hydroxyethyl methacrylate (Bimax) PVP K12, PVP K30, PVP K90: Poly(N-vinylpyrrolidone) (ISP Ashland) TEGDMA: Tetraethylene glycol dimethacrylate (Esstech) Omnirad 819: Bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) AIBN: Azobisisobutyronitrile [CAS 78-67-1] SiMAA: 2-Propenoic acid, 2-methyl-2-hydroxy-3-[3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]disiloxanyl]propoxy]propyl ester (Toray), or 3-(3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propoxy)-2-hydroxypropyl methacrylate HO-mPDMS: mono-n-butyl terminated mono-(2-hydroxy-3-methacryloxypropyloxy)-propyl terminated polydimethylsiloxane (M n = 1400 Daltons, n = 15) (Ortec or DSM-Polymer Technology Group)

[0174] [ka] Norbloc: 2-(2'-hydroxy-5-methacrylyloxyethylphenyl)-2H-benzotriazole (Janssen) Blue HEMA: 1-amino-4-[3-(4-(2-methacryloyloxy-ethoxy)-6-chlorotriazin-2-ylamino)-4-sulfophenylamino]anthraquinone-2-sulfonic acid (described in U.S. Pat. No. 5,944,853) Boric Acid Buffer Filling Solution: 18.52 grams (300 mmol) of boric acid, 3.7 grams (9.7 mmol) of sodium borate decahydrate, and 28 grams (197 mmol) of sodium sulfate were dissolved in enough deionized water to fill a 2 liter volumetric flask. D3O: 3,7-dimethyl-3-octanol (Vigon) HCl: Hydrochloric acid IPA: 2-propanol ACN: Acetonitrile THF: tetrahydrofuran PEO: Polyethylene oxide DMF: Dimethylformamide DCM: dichloromethane PP: Polypropylene, a homopolymer of propylene TT: Tuftec (Asahi Kasei Chemicals), a hydrogenated styrene butadiene block copolymer Z: Zeonor (Nippon Zeon Co Ltd), a polycycloolefin thermoplastic polymer LED: Light Emitting Diode 1 N NMR: Proton nuclear magnetic resonance spectroscopy UV-VIS: Ultraviolet-visible spectroscopy TLC: Thin Layer Chromatography ID: Inner diameter L: Liters mL: milliliter mM: millimolar M: mole Equiv. or eq.: equivalent kg: kilogram g: grams mg: milligram mol: mole mmol: millimolar min:minutes mm: millimeters cm: centimeters μm: micrometer nm: nanometer mW: milliwatt mJ: millijoule Pa: Pascal PSI: Pounds per square inch Abs: Absorption amount %T: Transmittance percentage MAPO: monoacylphosphine oxide DMD: Digital micromirror device

[0175] Working Example Preparation 1 - Synthesis of monoacylphosphine oxide monoterminated poly(N-vinylpyrrolidone) (MAPO-PVP) as shown in Scheme A.

[0176] A three-necked round-bottom flask fitted with a reflux condenser was charged with N-vinylpyrrolidone (20.0 grams), ethanol (41.0 grams), and Omnirad 819 (1.0 grams) under yellow light, degassed, and heated to 65° C. under nitrogen. The resulting mixture was then cooled to approximately 1.22 mW / cm. 2 The reaction mixture was irradiated with 435 nm LED light with an intensity of 1000 Hz for 30 minutes. The reaction mixture was quenched in air and cooled to room temperature. The solvent was removed under reduced pressure, followed by precipitation in cold diethyl ether and filtration to give a white solid. The white solid was suspended in diethyl ether (50 mL), stirred for 30 minutes, and refiltered. The product ("MAPO-PVP") was then washed with diethyl ether (3 x 50 mL) and air-dried to give a white powder (16.0 grams, 80% yield). The polymer structure was purified by 500 MHz NMR in deuterium oxide. 1 The product was characterized by H-NMR spectroscopy. See FIG. 4. The molecular weight and its distribution were determined by viscosity comparison and size-exclusion multi-angle light scattering (SEC-MALS) for commercial samples of PVP K12-K90. Note that the product "MAPO-PVP" is a mixture of monoacylphosphine oxide-terminated PVP and monoacyl-terminated PVP, as shown in Scheme A. The type of monoacyl group depends on the type of bisacylphosphine oxide initiator used for copolymerization; if the initiator has two different acyl groups, then "MAPO-PVP" is a mixture of two monoacylphosphine oxide-terminated PVP and two monoacyl-terminated PVP. It is important to protect these materials from ambient light during storage. MAPO-PVP is an example of the first formula in Table A.

[0177] [ka]

[0178] Viscosity measurements were performed on an Anton-Paar rheometer using a CP50-1 cone and plate at 1 s -1 ~500 seconds -1 The shear rate was 0.01, and the run time was 400 seconds, at room temperature, with data collected every 10 seconds. Measurements were performed in duplicate and averaged. The viscosity results are shown in Table 1. The viscosity data showed that MAPO-PVP exhibited a viscosity slightly greater than that of PVP K30.

[0179] [Table 4]

[0180] Polymer molecular weights were determined by size-exclusion chromatography with multi-angle light scattering (SEC-MALS) against the molecular weights of commercial samples of PVP K12 and PVP K30. The SEC-MALS setup used 20% ACN (containing 50 mM Na2SO4) in deionized water (v / v) as the mobile phase at a flow rate of 0.3 mL / min at 40 °C, and three Tosoh Biosciences TSK gel columns in series (SuperAW3000 4 μm, 6.0 mm ID x 15 cm (PEO / DMF exclusion limit = 60,000 g / mol), SuperAW4000 6 μm, 6.0 mm ID x 15 cm (PEO / DMF exclusion limit = 400,000 g / mol) and SuperAW5000 7 μm, 6.0 mm ID x 15 cm (PEO / DMF exclusion limit = 4,000,000 g / mol)) were monitored using an online Agilent 1200 UV / VIS diode array detector, a Wyatt Optilab rEX interference refractometer and a Wyatt mini-DAWN A Treos multi-angle laser scattering (MALS) detector (λ=658 nm) was used. Molecular weight and polydispersity data were calculated using the Wyatt ASTRA 6.1.1.17 SEC / LS software package. Figure 5 shows the SEC-MALS chromatograms of PVP K12, PVP K30, and MAPO-PVP. Since the chromatograms of PVP K30 and MAPO-PVP are similar, it was inferred that PVP K30 and MAPO-PVP have similar molecular weight distributions.

[0181] Preparation Example 2 - Synthesis of monoacylphosphine oxide monoterminated poly(N,N-dimethylacrylamide) (MAPO-PDMA): A three-necked round bottom flask fitted with a reflux condenser was charged with N,N-dimethylacrylamide (11.0 grams), ethanol (11.0 grams) and Omnirad 819 (400 milligrams) under yellow light, degassed and heated at 75°C under nitrogen. Then, approximately 1.22 mW / cm 2The reaction mixture was irradiated for 20 min with 435 nm LED light with an intensity of 100 Hz. The reaction was then quenched in air, cooled to room temperature, and precipitated in cold diethyl ether to give a white solid, which was redissolved in methanol and precipitated with diethyl ether. This precipitation process was repeated once more to give a white solid (65% yield). MAPO-PDMA was purified by 500 MHz NMR in deuterated methanol. 1 Characterized by H-NMR spectroscopy, see Figure 6.

[0182] Polymer molecular weights were determined by size-exclusion chromatography with multi-angle light scattering (SEC-MALS). The SEC-MALS setup used methanol (containing 10 mM LiBr) as the mobile phase at a flow rate of 0.6 mL / min at 50° C. and three Tosoh Biosciences TSK gel columns in series (SuperAW3000 4 μm, 6.0 mm ID×15 cm (PEO / DMF exclusion limit=60,000 g / mol), SuperAW4000 6 μm, 6.0 mm ID×15 cm (PEO / DMF exclusion limit=400,000 g / mol) and SuperAW5000 7 μm, 6.0 mm ID×15 cm (PEO / DMF exclusion limit=4,000,000 g / mol)) with an online Agilent 1200 UV / VIS diode array detector, a Wyatt Optilab rEX interference refractometer and a Wyatt mini-DAWN Treos multi-angle laser scattering (MALS) detector (λ=658 nm). A dη / dc value of 0.183 mL / g at 30° C. (λ=658 nm) was used for the absolute molecular weight determination. Absolute molecular weight and polydispersity data were calculated using the Wyatt ASTRA 6.1.1.17 SEC / LS software package. The number average molecular weight was determined to be 56,500 grams / mole; the weight average molecular weight was determined to be 96,100 grams / mole; resulting in a polydispersity index [M w / M n ] was obtained.

[0183] Preparative Example 3 (Prophetic) - Synthesis of monoacylphosphine oxide mono-terminated poly(N-vinylpyrrolidone-co-N,N-dimethylacrylamide): A three-necked round bottom flask fitted with a reflux condenser is charged with N-vinylpyrrolidone (10.0 grams), N,N-dimethylacrylamide (10.0 grams), ethanol (41.0 grams) and Omnirad 819 (1.0 grams) under yellow light, degassed and heated at 65°C under nitrogen. Then approximately 1.22 mW / cm 2 The reaction mixture is irradiated for 30 min with 435 nm LED light with an intensity of 1000 nm. The reaction mixture is quenched in air and cooled to room temperature. The solvent is removed under reduced pressure, followed by precipitation in cold diethyl ether and filtration to give a white solid. The white solid is suspended in diethyl ether (50 mL), stirred for 30 min, and refiltered. The product ("MAPO-poly[NVP-co-DMA]") is then washed with diethyl ether (3 x 50 mL) and air-dried to give a white powder.

[0184] Example 4 - Synthesis of the photoinitiator-dye ("PI-Dye1") shown in Scheme B.

[0185] Synthesis of 1-(3-(benzyloxy)phenyl)-N,N,N',N'-tetraethylphosphanediamine: 2.5 M n-butyllithium in hexanes (42.0 mL, 105.0 mmol, 1.05 equiv.) was added dropwise to a solution of 1-(benzyloxy)-3-bromobenzene (26.3 grams, 100.0 mmol, 1.00 equiv.) in THF (200 mL) at -78°C. After stirring for 2 hours, 1-chloro-N,N,N',N'-tetraethyl-phosphanediamine (22 mL, 105.0 mmol, 1.05 equiv.) was added dropwise to the reaction mixture, maintaining the reaction temperature below -70°C. The reaction was allowed to warm to room temperature and stirred overnight. The reaction mixture was cooled to 0°C and diluted with water (20 mL). The reaction mixture was concentrated under reduced pressure to a volume of approximately 50 mL. The residual material was diluted with methyl tert-butyl ether (350 mL) and water (100 mL). The layers were separated and the aqueous layer was extracted with methyl tert-butyl ether (2×250 mL). The combined organic layers were washed with water (2×150 mL), dried over sodium sulfate, filtered, and concentrated under reduced pressure to provide 1-(3-(benzyloxy)phenyl)-N,N,N′,N′-tetraethylphosphanediamine (36.0 grams, quantitative yield) as a colorless oil, which was used in the next step without further purification.

[0186] Synthesis of (3-(benzyloxy)phenyl)dichlorophosphane: 2.0 M HCl in diethyl ether (200 mL, 400.0 mmol, 4.0 equiv.) was added to a solution of 1-(3-(benzyloxy)phenyl)-N,N,N',N'-tetraethylphosphanediamine (36.0 grams, 100.0 mmol, 1.0 equiv.) in anhydrous diethyl ether (400 mL) at 0° C. The reaction mixture was allowed to warm slowly to room temperature and stirred overnight. The resulting suspension was filtered under nitrogen through a plug of Celite (80.0 grams), which was then washed with anhydrous diethyl ether (2×100 mL). The filtrate was concentrated under reduced pressure and blanketed with nitrogen to give (3-(benzyloxy)phenyl)dichlorophosphane (22.0 grams, 77% yield) as a yellow oil, which was used subsequently without further purification. Note: Anhydrous diethyl ether (250 mL) and NMR solvents were sparged with nitrogen for 15 min before use.

[0187] Synthesis of ((3-(benzyloxy)phenyl)phosphoryl)bis(mesitylmethanone): 2,4,6-trimethylbenzoyl chloride (31.0 mL, 185.0 mmol, 2.4 equiv.) was added to a suspension of zinc dust (12.1 grams, 185.0 mmol, 2.4 equiv.) in anhydrous ethyl acetate (150 mL) at room temperature. The reaction mixture was shielded from ambient light exposure. A solution of (3-(benzyloxy)phenyl)dichlorophosphane (22.0 grams, 77.0 mmol, 1.0 equiv.) in anhydrous ethyl acetate (100 mL) was added dropwise to the reaction mixture at room temperature. After stirring at room temperature for 24 hours, the reaction was cooled to 0° C. and sodium bicarbonate (15.6 grams, 185.0 mmol, 2.4 equiv.) was added in one portion, followed by the dropwise addition of 30% aqueous hydrogen peroxide (11.0 mL, 93.0 mmol, 1.2 equiv.) over 40 minutes while maintaining the reaction temperature below 5° C. The reaction mixture was stirred for 1 hour and diluted with water (100 mL). Insoluble material was removed by filtration through a plug of sand (50.0 grams), which was washed with ethyl acetate (300 mL). The layers were separated and the aqueous layer was extracted with ethyl acetate (3×300 mL). The combined organic layers were dried over sodium sulfate, filtered, and concentrated under reduced pressure. The crude product was redissolved in dichloromethane (150 mL), absorbed onto Celite (80 grams), and purified on a Biotage automated chromatography system (2 x 200 gram Biotage silica gel columns), eluting with a gradient of 0 to 50% ethyl acetate in heptane each time, to give (3-(benzyloxy)phenyl)phosphoryl)bis(mesitylmethanone) (10.3 grams, 25% yield) as a yellow semi-solid. Note: Anhydrous ethyl acetate (250 mL) was sparged with nitrogen for 30 minutes before use.

[0188] Synthesis of ((3-hydroxyphenyl)phosphoryl)bis(mesitylmethanone): A solution of (3-(benzyloxy)phenyl)phosphoryl)bis(mesitylmethanone) (7.7 grams, 15.0 mmol, 1 equiv.) in a mixture of methanol (180 mL) and ethyl acetate (720 mL) was added to a suspension of palladium on charcoal (10 wt. % loading, 2.2 grams, 2.1 mmol, 0.15 equiv.) in methanol (10 mL). The reaction mixture was hydrogenated in a Parr shaking reactor at 25 psi for 24 hours. The reaction mixture was filtered through a pad of Celite (100 grams) and the Celite was washed with ethyl acetate (2×500 mL). The filtrate was concentrated under reduced pressure, redissolved in dichloromethane (150 mL), absorbed onto Celite (80 grams), and purified on a Biotage automated chromatography system (200 gram, Biotage silica gel column, followed by a 50 gram Biotage high performance silica gel column), eluting with a gradient of 10-50% ethyl acetate in heptane each time, to give ((3-hydroxyphenyl)phosphoryl)bis(mesitylmethanone): (3.7 grams, 58% yield) as a pale yellow solid. 1 H-NMR (400MHz, CDCl3): δ9.01 (brs, 1H), 7.80 (ddd, J=1.4, 2.3, 12.7Hz, 1H), 7.22-7.16 (m, 1H), 7.15-7.09(m, 1H), 6.99-6.95(m, 1H), 6.77(s, 4H), 2.24(s, 6H), 2.10(s, 12H). 31 P NMR (162MHz, CDCl3) δ 6.82(s, 1P).

[0189] Synthesis of N,N'-(9,10-dioxo-9,10-dihydroanthracene-1,4-diyl)bis(3-chloropropanamide): To a cooled solution (0°C, ice bath) of 1,4-diaminoanthracene-9,10-dione (1.2 grams, 5.04 mmol, 1.0 equiv.) in 40 mL of toluene, a solution of 3-chloropropionyl chloride (4.8 mL, 50.37 mmol, 10.0 equiv.) in toluene (50 mL) and triethylamine (1.55 mL, 11.09 mmol, 2.2 equiv.) was added while stirring the solution at room temperature for 15 hours, followed by refluxing for 1 hour (reaction completion was monitored by TLC). The solids were removed by filtration and the residue was washed with toluene. The filtrate was extracted with 3% aqueous sodium chloride solution and the organics were concentrated under reduced pressure. The product was precipitated with ethyl acetate-n-hexane as a red solid (98% yield). 1 H-NMR (500MHz, CDCl3): δ12.8 (m, 2H), 9.2 (m, 2H), 8.3 (m, 2H), 7.8 (m, 2H), 3.9 (t, J=6.0Hz, 4H), 3.0 (t, J=6.0Hz, 4H).

[0190] Synthesis of N,N'-(9,10-dioxo-9,10-dihydroanthracene-1,4-diyl)bis(3-(3-(bis(2,4,6-trimethylbenzoyl)phosphoryl)phenoxy)propanamide) ("PI-dye 1"): (3-hydroxyphenyl)phosphoryl)bis(mesitylmethanone) (0.21 grams, 0.48 mmol, 2.0 equiv.) and N,N'-(9,10-dioxo-9,10-dihydroanthracene-1,4-diyl)bis(3-chloropropanamide) (0.10 grams, 0.24 mmol, 1.0 equiv.) were dissolved in dimethylsulfoxide (5 mL). Potassium carbonate (0.07 grams, 0.50 mmol, 2.1 equiv.) was added and the reaction mixture was heated at 80° C. for 6 hours (protected from light exposure and monitored for reaction completion by TLC). The reaction mixture was cooled to room temperature, water (15 mL) was added, extracted with dichloromethane (2×25 mL), and the combined organic extracts were washed with water (1×15 mL), brine (1×15 mL), dried over sodium sulfate, filtered, and evaporated under reduced pressure. The residue was purified on a silica gel column and eluted with 40% ethyl acetate in n-hexane to give N,N′-(9,10-dioxo-9,10-dihydroanthracene-1,4-diyl)bis(3-(3-(bis(2,4,6-trimethylbenzoyl)phosphoryl)phenoxy)propanamide) ("PI-dye 1") as a red semi-solid (25% yield). 1 H-NMR (500MHz, CDCl3): δ12.31(m, 2H), 9.21(m, 2H), 8.33(m, 2H), 7.81(m, 4H), 7.20-7.18(m, 2H), 7.14-7.01(m , 2H), 6.90~6.95(m, 2H), 6.68(s, 8H), 3.8(t, J=6.0Hz, 4H), 3.0(t, J=6.0Hz, 4H), 2.22(s), 12H), 2.10(s, 24H). 31 P-NMR (202MHz, CDCl3): δ 7.01(s).

[0191] Example 5 - Synthesis of the photoinitiator-dye shown in Scheme B ("PI-Dye2").

[0192] Synthesis of 3-((9,10-dioxo-9,10-dihydroanthracen-1-yl)amino)propanoic acid: To a stirred solution of 1-aminoanthracene-9,10-dione (22.3 grams, 75.52 mmol, 1.0 equiv.) and boric acid (6.2 grams, 100.0 mmol, 1.3 equiv.) in 120 mL of 100% sulfuric acid. Acrylic acid (15.0 grams, 208.15 mmol, 2.75 equiv.) was added slowly while maintaining the temperature at 30° C.-35° C. The mixture was then stirred at 90° C.-95° C. for 12 hours. The reaction mixture was cooled and poured into 400 grams of ice, thereby precipitating a solid, which was filtered, washed with water, and dried. The red solid was suspended in dichloromethane (500 mL) and filtered to remove insoluble material. The filtrate was concentrated under reduced pressure to give 3-((9,10-dioxo-9,10-dihydroanthracen-1-yl)amino)propanoic acid as a red solid (quantitative yield). 1 H-NMR(500MHz,CDCl3):δ 12.28(br s,1H),8.32-7.85(m,4H),7.45(m,1H),7.27(m,1H),7.11(m,1H),6.79(br s,1H),3.44(t,J=6.2Hz,2H),2.80(t,J=6.2Hz,2H).

[0193] Synthesis of 3-(bis(2,4,6-trimethylbenzoyl)phosphoryl)phenyl 3-((9,10-dioxo-9,10-dihydroanthracen-1-yl)amino)propanoate ("PI-Dye2"): ((3-hydroxyphenyl)phosphoryl)-bis(mesitylmethanone) (0.25 grams, 0.58 mmol, 1.0 equiv.), 3-((9,10-dioxo-9,10-dihydroanthracen-1-yl)amino)propanoic acid (0.21 grams, 0.64 mmol, 1.1 equiv.) and N,N-dimethylaminopyridine (catalyst) were dissolved in anhydrous tetrahydrofuran (10 mL) and cooled to 0° C. (ice bath). N-(3-Dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (EDC-HCl, 0.13 grams, 0.67 mmol, 1.15 equiv.) was added in one portion and stirred while maintaining the temperature at 0°C, after which the system was stirred at room temperature under nitrogen for 12 hours. Upon completion of the reaction, the solvent was removed under reduced pressure and the crude product was passed through a silica gel column eluting with 30-40% ethyl acetate in n-hexane to give the title compound ("PI-Dye2") as a red solid (95% yield). 1 H-NMR(500MHz, CDCl3):δ9.91(br s,1H),8.30-8.24(m,2H),7.75-7.60(m,6H),7.45-7.43(m,1H),7.37-7.35(m,1H),7.16-7.1 4(m,1H),6.79(s,4H),3.81(t,J=6.0Hz,2H),3.0(t,J=6.0Hz,2H),2.25(s,6H),2.14(s,12H). 31 P NMR(202MHz, CDCl3)δ 4.79(s,1P).

[0194] The UV-visible spectra of the compounds in solution were measured on a Perkin Elmer Lambda 45 or Agilent Cary 6000i UV / VIS scanning spectrometer. The instruments were allowed to thermally equilibrate for at least 30 minutes before use. For the Perkin Elmer instrument, the scan range was 200-800 nm, the scan speed was 960 nm per minute, the slit width was 4 nm, the mode was set to transmission or absorbance, and baseline correction was selected. For the Cary instrument, the scan range was 200-800 nm, the scan speed was 600 nm / min, the slit width was 2 nm, the mode was transmission or absorbance, and baseline correction was selected. Baseline correction was performed before analyzing the samples using the autozero function.

[0195] The UV-visible spectra of contact lenses partially formed from the claimed compositions were measured using packing solutions on a Perkin Elmer Lambda 45 UV / VIS or Agilent Cary 6000i UV / VIS scanning spectrometer. Prior to use, the instruments were allowed to thermally equilibrate for at least 30 minutes. For the Perkin Elmer instruments, the scan range was 200-800 nm, the scan speed was 960 nm per minute, the slit width was 4 nm, the mode was set to transmission, and baseline correction was selected. Baseline correction was performed using a plastic two-piece lens holder and a cuvette containing the same solvent. These two-piece contact lens holders were designed to hold the sample in the quartz cuvette at a position traversed by the incident light beam. A reference cuvette also housed the two-piece holder. To ensure that the thickness of the samples was consistent, all lenses were made using the same mold. The center thickness of the contact lenses was measured using an electronic thickness gauge. The center thickness and transmission spectra reported are obtained by averaging three individual lens data.

[0196] It is important to ensure that the exterior of the cuvette is completely clean and dry and that there are no air bubbles within the cuvette. Measurement reproducibility is improved when the reference cuvette and its lens holder remain constant and all samples use the same sample cuvette and its lens holder, ensuring that both cuvettes are properly inserted into the instrument.

[0197] The UV-VIS absorption spectra of PI-Dye1 in 0.2 mM DCM and PI-Dye2 in 0.2 mM methanol are shown in FIG.

[0198] [ka]

[0199] Example 6 - Synthesis of polymeric photoinitiator-dye ("PolyPI-Dye") shown in Scheme C (Prophetic).

[0200] A mixture of 2-((9,10-dioxo-9,10-dihydroanthracen-1-yl)amino)ethyl methacrylate, 3-(bis(2,4,6-trimethylbenzoyl)phosphoryl)phenyl methacrylate, and optionally another vinyl monomer (CH2=CXY) are copolymerized in a solvent using a thermal initiator such as azobisisobutyronitrile (AIBN) under yellow illumination or in the dark. The optional vinyl monomer may be any monomer or macromer and may be used to adjust the solubility of the terpolymer in the reactive monomer mixture and / or to distribute the pendant dye and initiator moieties. The monomer shown in Scheme C as CH2=CXY may represent any 1,1-disubstituted monomer or macromer. However, CH2=CXY is preferably a hydrophilic monomer as defined herein, including, but not limited to, (meth)acrylate, styrene, vinyl ether, vinyl ester, (meth)acrylamide, N-vinyl lactam, N-vinyl amide, N-vinyl imide, N-vinyl urea, O-vinyl carbamate, O-vinyl carbonate, and mixtures thereof. The resulting copolymer is then isolated by precipitation, washed, and dried under yellow lighting to reduce exposure to ambient light. The resulting solid is protected from exposure until use.

[0201] [ka]

[0202] Example 1 (changing the optical path length) A reactive monomer mix was formed having the formulation set forth in Table 2. The reactive monomer mix was degassed by applying a vacuum for approximately 15 minutes. Approximately 100 microliters of the reactive monomer mix was then dispensed onto a Zeonor base curve mold, after which a Zeonor front curve mold was placed onto the base curve mold. The resulting mold assembly was transferred to the irradiation jig shown in FIG. 3, which was then irradiated with 47.5 mW / cm. 2A 365 nm LED light source with an intensity of 1000 nm was directed into separate volumes within the mold cavity and connected to a computer-controlled light projector that was modulated by a digital light processing chip or a digital micromirror device.

[0203] [Table 5]

[0204] A computer controlled light projector was programmed to illuminate or irradiate the USAF 1951 test object shown in Figure 8. The USAF 1951 test chart is a widely known image that encompasses a wide range of spatial frequencies and recognizable digits, and is therefore a good standard for objectively measuring the overall quality of an imparted image profile. The reactive monomer mixture in the mold cavity was exposed to 700 mJ / cm2. 2 The contact lenses were irradiated by a computer-controlled light projector using a maximum energy of 100000 and an exposure time of 31.6 seconds to impart a USAF 1951 test chart image profile to the contact lenses, and then heated to 90°C for 2 hours and 45 minutes to thermally cure the remainder of the reactive monomer mixture into contact lenses. The resulting lenses were removed using 70% (v / v) aqueous IPA (approximately 1 hour immersion), extracted twice for 30 minutes with 70% (v / v) aqueous IPA, hydrated for 30 minutes with deionized water, and then equilibrated with packing solution. An optical micrograph of the final hydrated lens is shown in Figure 9. Note: The exact conditions of the computer-controlled light projector usually need to be optimized based on the composition of the reactive monomer mixture and the projected image. This optimization usually involves varying the energy [energy = LED intensity x DMD attenuation x exposure time] delivered to the reactive monomer mixture in the mold cavity and the exposure time. Preferably, the optimization uses the highest possible intensity with the shortest exposure time.

[0205] To improve spatial resolution, the above experiment was repeated using a thermal pre-cure step at 90°C for 5, 10, and 15 minutes prior to light projector exposure. The pre-cure step improves image quality by increasing the viscosity of the reactive monomer mixture prior to light projector exposure, thereby reducing molecular motion. Based on these data, a 10 minute pre-cure step appeared to improve the imparted profile image quality and repeatability.

[0206] Example 2 (Optical Characteristics) Example 1 was repeated using a 10 minute pre-cure, but instead of projecting an image, a computer-controlled light projector illuminated a pattern of circular dots, each of which was exposed to a different energy level, thereby generating pillars of different optical paths due to local changes in volume and refractive index after the lens was demolded, extracted, hydrated, and equilibrated as described in Example 1. In this way, a calibration curve was generated by plotting the applied energy (mJ) versus delta path length effect (wavefront measurement of the wave after conversion from the filling solution to air) versus wavefront values ​​of an untreated lens of the same design for each pillar position for energy exposures of less than about 100 mJ, and the calibration curve was reasonably linear and deterministic. Such a relationship allows for the creation of optical features in a predictable manner, such as adding spherical power or defocus or cylindrical power to a lens made in a mold cavity designed to exhibit only a fixed spherical power. Based on this information, a 3.6 second exposure time and 86 mJ / cm 2 Using an energy level of 0.01, a computer-controlled projector projected a spherical or cylindrical power image into the lens cavity. A projected image and a two-dimensional representation of the measured delta wavefront obtained from a perfectly equilibrated lens are shown in FIG. 10. The estimated change in spherical power by adding some defocus was about 0.7 diopters, and the estimated addition of cylindrical power was about 0.12 diopters.

[0207] A calibrated dual interferometry method was used to measure contact lens parameters in the packaging solution. These parameters include equivalent spherical power (diopters or D) at multiple apertures, cylindrical power (diopters or D) at multiple apertures, diameter (millimeters or mm), central thickness (millimeters or mm), sagittal height (millimeters or mm), and root-mean-square (RMS) optical path wavefront deviation from lens design targets in micrometers or micrometers (μm), sometimes expressed as a wave with spherical / cylinder power and removed coma aberration when measured using a 6.5 mm aperture. The instrument consists of a custom proprietary interferometer for measurement of wavefront parameters and a Lumetrics OptiGauge™ II low coherence interferometer for measurement of dimensional parameters of sagittal height and central thickness. The two individual instruments combined are similar to the Lumetrics Clearwave™ Plus and the software is similar to the Lumetrics OptiGauge Control Center v7.0 or later. The Clearwave™ Plus uses a camera to find the lens edge and then calculates the lens center, which is then used to align a 1310 nanometer interferometer probe to the lens center to measure sagittal height and central thickness. The transmitted wavefront is also continuously collected using a wavefront sensor (Shack-Hartmann sensor). Multiple parameters from the transmitted wavefront of the contact lens are measured and other parameters are calculated from these measurements.

[0208] From the collected data, difference terms are calculated by comparing the measurements from the targets. These include the root mean square path wavefront deviation (RMS_65) from the lens design target (spherical / cylindrical power and removed coma) in μm when measured using a 6.5 mm aperture, the second equivalent spherical power deviation (PW2EQD) from the lens design target in diopters (D) when measured using a 5 mm aperture, the deviation from the lens design target diameter (DMD) in mm, the deviation from the lens design target base curve radius and lens diameter (BCD) in mm, and the deviation from the lens design target center thickness (CTD) in mm, calculated from the sagittal height measured by ISO 18369-3. The amount of additional spherical or cylindrical power generated by the modulated and localized photopolymerization was calculated using such data after subtracting the spherical power designed based on the mold design.

[0209] Example 3 (Light Absorbing Zone) A reactive monomer mixture was formed having the formulation set forth in Table 3. The reactive monomer mixture was degassed by applying a vacuum for approximately 15 minutes. Approximately 100 microliters of the reactive monomer mixture was then dispensed onto a Zeonor base curve mold, after which a Zeonor front curve mold was placed onto the base curve mold. The resulting mold assembly was transferred to the irradiation jig shown in FIG. 3, which was then irradiated with 47.5 mW / cm. 2 A 365 nm LED light source with an intensity of 1000 nm was directed into separate volumes within the mold cavity and connected to a computer-controlled light projector that was modulated by a digital light processing chip or a digital micromirror device.

[0210] [Table 6]

[0211] A computer-controlled light projector was programmed to illuminate or irradiate the apodized lens image or pupil-only lens image shown in Figure 11. The reactive monomer mixture in the mold cavity was then injected with 6000 mJ / cm2 The lenses were illuminated by a computer-controlled light projector using a maximum energy of 1000 uL to produce an apodized image or an image of the pupil only, and then heated to 90° C. for 2 hours and 45 minutes to thermally cure the remainder of the reactive monomer mixture into contact lenses. The resulting lenses were removed using 70% (v / v) aqueous IPA (approximately 1 hour immersion), extracted twice with 70% (v / v) aqueous IPA for 30 minutes, hydrated with deionized water for 30 minutes, and then equilibrated with packing solution. An optical micrograph of the final hydrated lens is also shown in FIG. 11. Although very faint, the image appears to be replicated on the contact lens. However, the level of light absorption is low.

[0212] Example 4 Example 3 was repeated, except that PI-Dye2 was used instead of PI-Dye1 in the reactive monomer mixture and the project image was changed to the calibration segment image shown in Figure 12. Different energy levels and exposure times were used, i.e., 230 mJ / cm 2 (3.6 seconds), 461mJ / cm 2 (7.2 seconds), 1150mJ / cm 2 (18.0 seconds), and 2300 mJ / cm 2 Contact lenses were made using a 18 second exposure time of 1150 mJ / cm2. Optical micrographs of these contact lenses are also shown in FIG. 12. By comparing these micrographs, it is clear that an exposure time of 18 seconds is sufficient to produce 1150 mJ / cm2. 2 Using energy levels of 100 nm appears to be sufficient to generate images with PI-Dye2.

[0213] Example 5 Example 4 was repeated using the 9.5 mm diameter apodized image, the 9.0 mm diameter pupil-only image, and the Jack-o'-Lantern image shown in Figure 13. The corresponding contact lenses were then irradiated with 1150 mJ / cm 2 The LED light source was 63 mW / cm and had an exposure time of 18 seconds. 2Optical micrographs of these contact lenses are also shown in Figure 13. The images appear to have been accurately replicated under these conditions using the reactive monomer mixture containing PI-dye 2.

[0214] [Embodiment] (1) A reactive monomer mixture for making an ophthalmic lens, said reactive monomer mixture comprising: a monomer suitable for making said ophthalmic lens; a first polymerization initiator activatable at a first wavelength; a first functional moiety chemically bonded to the first polymerization initiator; a second polymerization initiator activatable by a second activation agent that does not substantially activate the first polymerization initiator. (2) The mixture of embodiment 1, further comprising a second functional moiety chemically bonded to the second polymerization initiator. (3) The mixture of any one of the preceding claims, wherein the first wavelength is 435 nanometers or less. (4) The mixture of embodiment 1, wherein the second polymerization initiator is a thermal initiator. (5) The mixture of embodiment 4, wherein the thermal initiator is azobisisobutyronitrile.

[0215] 6. The mixture of claim 1, wherein the first functional moiety is selected from a refractive index moiety, a light absorbing moiety, and combinations thereof. 7. The mixture of claim 6, wherein the refractive index portion is a polyamide. (8) The blend of claim 7, wherein the polyamide comprises polyvinylpyrrolidone (PVP), polyvinylmethylacetamide (PVMA), polydimethylacrylamide (PDMA), polyvinylacetamide (PNVA), poly(hydroxyethyl(meth)acrylamide), polyacrylamide, a copolymer of two or more thereof, or a combination of two or more thereof. 9. The mixture of claim 6, wherein the light absorbing moiety absorbs ultraviolet light, visible light, or a combination thereof. 10. The mixture of claim 9, wherein the light absorbing moiety comprises a static dye, a photochromic dye, a thermochromic dye, a leuco dye, or a combination of two or more thereof.

[0216] 11. The mixture of claim 1, wherein the first polymerization initiator is a copolymer having pendant monoacylphosphine oxide groups, bisacylphosphine oxide groups, or a combination thereof. 12. The mixture of claim 11, wherein the copolymer further comprises a refractive index moiety, a light absorbing moiety, or a combination thereof. (13) The first polymerization initiator having a first functional moiety chemically bonded thereto, [ka] wherein n is an integer ranging from 10 to 4000 and T is a chain terminating group; [ka] wherein n is an integer ranging from 10 to 4000 and T is a chain terminating group; [ka] wherein x and y are independently integers ranging from 10 to 4000, and T is a chain terminating group; [ka] wherein m is an integer ranging from 10 to 3000, n is an integer ranging from 1 to 100, and T is independently a chain terminating group; [ka] wherein m is an integer ranging from 10 to 3000 and T is a chain terminating group; [ka] wherein a is an integer ranging from 1 to 100, b is an integer ranging from 1 to 100, c is an integer ranging from 1 to 250, T is independently a chain terminator or initiator fragment, and Q is derived from hydrophilic monomers such as N,N-dimethylacrylamide, N-vinylpyrrolidone, 2-hydroxyethyl methacrylate, N-vinyl-N-methylacetamide, N-vinylacetamide, and the like; The mixture of embodiment 1 selected from a combination of two or more thereof. (14) A method of forming an ophthalmic lens, the method comprising: (a) providing a mold assembly comprised of a base curve and a front curve, the base curve and the front curve defining and enclosing a cavity therebetween, the cavity containing a reactive monomer mixture comprising a monomer suitable for making the ophthalmic lens, a first polymerization initiator activatable at a first wavelength, a first functional moiety chemically bonded to the first polymerization initiator, and a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, and at least one of the base curve or the front curve is optically transparent; (b) exposing one or more selected areas of the reactive monomer mixture to a source of actinic radiation at the first wavelength, thereby selectively polymerizing a portion of the reactive monomer mixture, wherein the selectively polymerized portions incorporate the first functional moiety; and (c) exposing the reactive monomer mixture to a second activation to activate the second polymerization initiator and cure the reactive monomer mixture; (d) removing the ophthalmic lens from the mold assembly; (e) extracting unreacted first polymerization initiator from said ophthalmic lens. 15. The method of claim 14, wherein the reactive monomer mixture contains a second functional moiety chemically bonded to the second polymerization initiator.

[0217] (16) The method of any one of claims 14 to 15, further comprising, prior to step (b), exposing the reactive monomer mixture to a second activation to partially activate the second polymerization initiator and partially cure the reactive monomer mixture. 17. The method of claim 14, wherein the second polymerization initiator is a thermal initiator. 18. The method of claim 17, wherein the thermal initiator is azobisisobutyronitrile. 19. The method of claim 17, wherein the thermal initiator is initiated at a temperature between 60° C. and 100° C. 20. The method of claim 14, wherein the source of actinic radiation in step (b) comprises a plurality of selectively controllable beams of actinic radiation, and the exposure is performed according to a predetermined script to cause selective polymerization of the reactive monomer mixture in a predetermined pattern within the cavities of the mold assembly.

[0218] (21) The method of embodiment 14, wherein the multiple beams of actinic radiation in step (b) are selectively controlled by a digital micromirror device according to a predetermined script. (22) The method of embodiment 21, wherein the digital micromirror device comprises an illumination source including at least one light emitting diode. (23) The method of embodiment 14, wherein the first wavelength comprises one or more wavelengths in the range of 380 to 450 nm. 24. The method of claim 14, wherein the first functional moiety is selected from a refractive index moiety, a light absorbing moiety, and combinations thereof. 25. The method of claim 24, wherein the refractive index portion is a polyamide.

[0219] 26. The method of claim 25, wherein the polyamide comprises polyvinylpyrrolidone (PVP), polyvinylmethylacetamide (PVMA), polydimethylacrylamide (PDMA), polyvinylacetamide (PNVA), poly(hydroxyethyl(meth)acrylamide), polyacrylamide, a copolymer of two or more thereof, or a combination of two or more thereof. 27. The method of claim 24, wherein the light absorbing moiety absorbs ultraviolet light, visible light, or a combination thereof. 28. The method of claim 27, wherein the light absorbing moiety comprises a static dye, a photochromic dye, a thermochromic dye, a leuco dye, or a combination of two or more thereof. 29. The method of claim 14, wherein the first polymerization initiator is a copolymer having pendant monoacylphosphine oxide groups, bisacylphosphine oxide groups, or a combination thereof. 30. The method of claim 29, wherein the copolymer further comprises a refractive index moiety, a light absorbing moiety, or a combination thereof.

[0220] (31) The first polymerization initiator having a first functional moiety chemically bonded thereto, [ka] wherein n is an integer ranging from 10 to 4000 and T is a chain terminating group; [ka] wherein n is an integer ranging from 10 to 4000 and T is a chain terminating group; [ka] wherein x and y are independently integers ranging from 10 to 4000, and T is a chain terminating group; [ka] wherein m is an integer ranging from 10 to 3000, n is an integer ranging from 1 to 100, and T is independently a chain terminating group; [ka] wherein m is an integer ranging from 10 to 3000 and T is a chain terminating group; [ka] wherein a is an integer ranging from 1 to 100, b is an integer ranging from 1 to 100, c is an integer ranging from 1 to 250, T is independently a chain terminator or initiator fragment, and Q is derived from hydrophilic monomers such as N,N-dimethylacrylamide, N-vinylpyrrolidone, 2-hydroxyethyl methacrylate, N-vinyl-N-methylacetamide, N-vinylacetamide, and the like; The method of embodiment 14, wherein the compound is selected from a combination of two or more of these. 32. The method of claim 14, wherein step (d) is accomplished by mechanically releasing the ophthalmic lens from the mold assembly. 33. The method of claim 14, wherein step (d) comprises a solvent swell of the ophthalmic lens. 34. The method of claim 14, wherein step (e) extracts a portion of the unreacted first polymerization initiator. (35) The method of embodiment 14, further comprising a lens extraction step to remove other components of the reactive monomer mixture, and a lens hydration step following extraction step (e) to remove unreacted first polymerization initiator.

[0221] 36. The method of claim 14, wherein the ophthalmic lens is a hard contact lens, a soft contact lens, a hybrid contact lens, a rigid gas permeable contact lens, or an intraocular lens.

Claims

1. 1. A reactive monomer mixture for making an ophthalmic lens, said reactive monomer mixture comprising: a monomer suitable for making said ophthalmic lens; a first polymerization initiator activatable at a first wavelength; a first functional moiety chemically bonded to the first polymerization initiator; a second polymerization initiator activatable by a second activation agent that does not substantially activate the first polymerization initiator.

2. 10. The mixture of claim 1 further comprising a second functional moiety chemically bonded to the second polymerization initiator.

3. 3. The mixture of claim 1 or 2, wherein the first wavelength is less than or equal to 435 nanometers.

4. The mixture of claim 1 , wherein the second polymerization initiator is a thermal initiator.

5. 5. The mixture of claim 4, wherein the thermal initiator is azobisisobutyronitrile.

6. 10. The mixture of claim 1, wherein the first functional moiety is selected from a refractive index moiety, a light absorbing moiety, and combinations thereof.

7. 7. The mixture of claim 6, wherein the refractive index portion is a polyamide.

8. 8. The blend of claim 7, wherein the polyamide comprises polyvinylpyrrolidone (PVP), polyvinylmethylacetamide (PVMA), polydimethylacrylamide (PDMA), polyvinylacetamide (PNVA), poly(hydroxyethyl(meth)acrylamide), polyacrylamide, copolymers of two or more thereof, or combinations of two or more thereof.

9. 7. The mixture of claim 6, wherein the light absorbing moiety absorbs ultraviolet light, visible light, or a combination thereof.

10. 10. The mixture of claim 9, wherein the light absorbing moiety comprises a static dye, a photochromic dye, a thermochromic dye, a leuco dye, or a combination of two or more thereof.

11. 2. The mixture of claim 1, wherein the first polymerization initiator is a copolymer having pendant monoacylphosphine oxide groups, bisacylphosphine oxide groups, or a combination thereof.

12. The mixture of claim 11 , wherein the copolymer further comprises a refractive index moiety, a light absorbing moiety, or a combination thereof.

13. The first polymerization initiator having a first functional moiety chemically attached thereto is 【Chemistry 1】 wherein n is an integer ranging from 10 to 4000 and T is a chain terminating group; 【Chemistry 2】 wherein n is an integer ranging from 10 to 4000 and T is a chain terminating group; 【Chemistry 3】 wherein x and y are independently integers ranging from 10 to 4000, and T is a chain terminating group; 【Chemistry 4】 wherein m is an integer ranging from 10 to 3000, n is an integer ranging from 1 to 100, and T is independently a chain terminating group; 【Chemistry 5】 wherein m is an integer ranging from 10 to 3000 and T is a chain terminating group; 【Chemistry 6】 wherein a is an integer ranging from 1 to 100, b is an integer ranging from 1 to 100, c is an integer ranging from 1 to 250, T is independently a chain terminator or initiator fragment, and Q is derived from hydrophilic monomers such as N,N-dimethylacrylamide, N-vinylpyrrolidone, 2-hydroxyethyl methacrylate, N-vinyl-N-methylacetamide, N-vinylacetamide, and the like; The mixture of claim 1 selected from a combination of two or more thereof.

14. 1. A method of forming an ophthalmic lens, the method comprising: (a) providing a mold assembly comprised of a base curve and a front curve, the base curve and the front curve defining and enclosing a cavity therebetween, the cavity containing a reactive monomer mixture comprising a monomer suitable for making the ophthalmic lens, a first polymerization initiator activatable at a first wavelength, a first functional moiety chemically bonded to the first polymerization initiator, and a second polymerization initiator activatable by a second activation that does not substantially activate the first polymerization initiator, and at least one of the base curve or the front curve is optically transparent; (b) exposing one or more selected areas of the reactive monomer mixture to a source of actinic radiation at the first wavelength, thereby selectively polymerizing a portion of the reactive monomer mixture, wherein the selectively polymerized portions incorporate the first functional moiety; and (c) exposing the reactive monomer mixture to a second activation to activate the second polymerization initiator and cure the reactive monomer mixture; (d) removing the ophthalmic lens from the mold assembly; (e) extracting unreacted first polymerization initiator from said ophthalmic lens.

15. 15. The method of claim 14, wherein the reactive monomer mixture contains a second functional moiety chemically bonded to the second polymerization initiator.

16. 16. The method of claim 14 or 15, further comprising exposing the reactive monomer mixture to a second activation prior to step (b) to partially activate the second polymerization initiator and partially cure the reactive monomer mixture.

17. The method of claim 14 , wherein the second polymerization initiator is a thermal initiator.

18. 18. The method of claim 17, wherein the thermal initiator is azobisisobutyronitrile.

19. The method of claim 17, wherein the thermal initiator is initiated at a temperature of from 60° C. to 100° C.

20. 15. The method of claim 14, wherein the source of actinic radiation in step (b) comprises a plurality of selectively controllable beams of actinic radiation, and the exposure is performed according to a predetermined script to cause selective polymerization of the reactive monomer mixture in a predetermined pattern within the cavities of the mold assembly.

21. 15. The method of claim 14, wherein the multiple beams of actinic radiation in step (b) are selectively controlled by a digital micromirror device according to a predetermined script.

22. The method of claim 21 , wherein the digital micromirror device comprises an illumination source that includes at least one light emitting diode.

23. The method of claim 14, wherein the first wavelength comprises one or more wavelengths in a range of 380 to 450 nm.

24. The method of claim 14 , wherein the first functional moiety is selected from a refractive index moiety, a light absorbing moiety, and combinations thereof.

25. 25. The method of claim 24, wherein the refractive index portion is a polyamide.

26. 26. The method of claim 25, wherein the polyamide comprises polyvinylpyrrolidone (PVP), polyvinylmethylacetamide (PVMA), polydimethylacrylamide (PDMA), polyvinylacetamide (PNVA), poly(hydroxyethyl(meth)acrylamide), polyacrylamide, copolymers of two or more thereof, or combinations of two or more thereof.

27. 25. The method of claim 24, wherein the light absorbing moiety absorbs ultraviolet light, visible light, or a combination thereof.

28. 28. The method of claim 27, wherein the light absorbing moiety comprises a static dye, a photochromic dye, a thermochromic dye, a leuco dye, or a combination of two or more thereof.

29. 15. The method of claim 14, wherein the first polymerization initiator is a copolymer having pendant monoacylphosphine oxide groups, bisacylphosphine oxide groups, or a combination thereof.

30. 30. The method of claim 29, wherein the copolymer further comprises a refractive index moiety, a light absorbing moiety, or a combination thereof.

31. The first polymerization initiator having a first functional moiety chemically attached thereto is 【Chemistry 7】 wherein n is an integer ranging from 10 to 4000 and T is a chain terminating group; 【Chemistry 8】 wherein n is an integer ranging from 10 to 4000 and T is a chain terminating group; 【Chemistry 9】 wherein x and y are independently integers ranging from 10 to 4000, and T is a chain terminating group; 【Chemistry 10】 wherein m is an integer ranging from 10 to 3000, n is an integer ranging from 1 to 100, and T is independently a chain terminating group; 【Chemistry 11】 wherein m is an integer ranging from 10 to 3000 and T is a chain terminating group; 【Chemistry 12】 wherein a is an integer ranging from 1 to 100, b is an integer ranging from 1 to 100, c is an integer ranging from 1 to 250, T is independently a chain terminator or initiator fragment, and Q is derived from hydrophilic monomers such as N,N-dimethylacrylamide, N-vinylpyrrolidone, 2-hydroxyethyl methacrylate, N-vinyl-N-methylacetamide, N-vinylacetamide, and the like; The method of claim 14 selected from a combination of two or more of these.

32. The method of claim 14 , wherein step (d) is accomplished by mechanically releasing the ophthalmic lens from the mold assembly.

33. The method of claim 14 , wherein step (d) comprises a solvent swell of the ophthalmic lens.

34. The method of claim 14, wherein step (e) extracts a portion of the unreacted first polymerization initiator.

35. 15. The method of claim 14, further comprising a lens extraction step to remove other components of the reactive monomer mixture, and a lens hydration step following extraction step (e) to remove unreacted first polymerization initiator.

36. 15. The method of claim 14, wherein the ophthalmic lens is a hard contact lens, a soft contact lens, a hybrid contact lens, a rigid gas permeable contact lens, or an intraocular lens.

Citation Information

Patent Citations

  • Lens for soft eye and its manufacture

    JP1998024097A

  • Composition capable of forming hydrogels in the eye

    JP2004535511A

  • A method for creating visible marks on lenses using leuco dyes.

    JP2014535067A

  • shape memory polymer intraocular lens

    JP2016536436A

  • Ophthalmic devices containing locally grafted networks and processes for their preparation and use - Patent Application 20070122997