Lithium secondary battery

A lithium secondary battery with a positive electrode active material layer of single particles and flaky graphite in a tab-less structure addresses high resistance and heat issues, ensuring safety and efficiency in large batteries.

JP2024537149AActive Publication Date: 2024-10-10LG ENERGY SOLUTION LTD

Patent Information

Application Number
JP2024520756
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-23
Filing Date
2022-10-14
Publication Date
2024-10-10
Estimated Expiration
2042-10-14

AI Technical Summary

Technical Problem

Conventional lithium secondary batteries face issues with high resistance, heat generation, and poor current collection efficiency due to concentrated current on strip-shaped electrode tabs, especially in large-sized batteries, leading to safety concerns such as fire and explosion risks.

Method used

The use of a positive electrode active material layer containing single particles and/or pseudo-single particles, along with flaky graphite, in a tab-less structure, to minimize particle cracking and improve thermal stability and charge/discharge efficiency.

Benefits of technology

The solution enhances thermal stability and reduces resistance, achieving excellent safety and capacity in large cylindrical batteries by minimizing gas generation and heat generation, while maintaining high energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537149000001_ABST
    Figure 2024537149000001_ABST
Patent Text Reader

Abstract

The present invention relates to a lithium secondary battery including an electrode assembly in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction, a battery can in which the electrode assembly is housed, and a sealing body that seals an open end of the battery can, wherein the positive electrode plate includes a positive electrode active material layer, and the positive electrode active material layer includes a positive electrode active material powder formed of a single particle, a pseudo-single particle, or a combination thereof, and flake graphite.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0137360 filed on October 15, 2021 and Korean Patent Application No. 10-2022-0121171 filed on September 23, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated as part of this specification.

[0002] The present invention relates to a lithium secondary battery, and more specifically, to a lithium secondary battery having improved battery stability, resistance characteristics, and charge / discharge efficiency by applying a positive electrode active material layer containing a single-particle and / or pseudo-single-particle positive electrode active material and flake graphite. [Background technology]

[0003] 2. Description of the Related Art With technological advances in electric vehicles, portable electronic devices, and the like, the demand for lithium secondary batteries as energy sources is rapidly increasing.

[0004] Lithium secondary batteries are classified into can-type batteries, such as cylindrical or rectangular, and pouch-type batteries, depending on the shape of the battery case. Among them, the can-type battery is formed by stacking a sheet-shaped positive electrode plate, a separator, and a negative electrode plate in sequence in a battery can, and winding the stack in one direction to manufacture a jelly-roll-shaped electrode assembly, and then sealing the battery can by covering the top of the battery can with a cap plate. The positive electrode plate and the negative electrode plate are provided with strip-shaped positive electrode tabs and negative electrode tabs, respectively, and the positive electrode tabs and negative electrode tabs are connected to electrode terminals to be electrically connected to an external power source. For reference, the positive electrode terminal is the cap plate, and the negative electrode terminal is the battery can. However, in the case of a conventional can-type battery having such a structure, current is concentrated in the strip-shaped electrode tabs, resulting in high resistance, a lot of heat generation, and poor current collection efficiency.

[0005] Meanwhile, with the recent development of electric vehicle technology, the need for high-capacity batteries is increasing, and so is the need to develop large-volume batteries. Conventionally, small cylindrical batteries that have been commonly used, i.e., cylindrical batteries with 1865 or 2170 form factors, have a small capacity, so resistance and heat generation do not seriously affect battery performance. However, if the specifications of conventional small cylindrical batteries are directly applied to large batteries, serious problems may occur in the safety of the battery.

[0006] As the size of a battery increases, the amount of heat and gas generated inside the battery also increases, and the heat and gas increase the temperature and pressure inside the battery, which can cause the battery to catch fire or explode. To prevent this, the heat and gas inside the battery must be properly discharged to the outside, and to do so, the cross-sectional area of ​​the battery, which serves as a path for discharging heat to the outside of the battery, must increase in accordance with the increase in volume. However, since the increase in cross-sectional area is usually not enough to match the increase in volume, the larger the battery, the more heat generated inside the battery increases, which increases the risk of explosion and causes problems such as a decrease in output. In addition, when fast charging at a high voltage, a large amount of heat is generated around the electrode tab in a short period of time, which can cause the battery to catch fire.

[0007] On the other hand, the use of a conventional positive electrode active material containing secondary particles can cause particle cracking during electrode production, leading to increased gas generation due to internal cracks during charging and discharging, which can cause problems with battery stability.

[0008] To solve this problem, positive electrode active materials in the form of single particle or pseudo-single particle, in which the primary particle size is relatively large, have been developed. However, when the positive electrode active materials in the form of single particle or pseudo-single particle are applied to a high loading electrode and rolled, there are problems in that the electrode cracks without achieving a target level of electrode porosity, and there are problems in that the resistance characteristics and charge / discharge efficiency of the lithium secondary battery are poor. Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made to solve the above problems, and an object of the present invention is to provide a lithium secondary battery that can achieve excellent thermal stability even when the volume of the battery is increased.

[0010] The present invention has been made to solve the above-mentioned problems, and aims to provide a lithium secondary battery having improved battery stability, resistance characteristics, and charge / discharge efficiency by applying a positive electrode active material layer including a positive electrode active material powder containing flake graphite and single particles and / or pseudo-single particles. [Means for solving the problem]

[0011] According to one embodiment, the present invention provides a lithium secondary battery including an electrode assembly having a structure in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction, a battery can in which the electrode assembly is housed, and a sealing body for sealing an open end of the battery can, wherein the positive electrode plate includes a current collector and a positive electrode active material layer, and the positive electrode active material layer includes a positive electrode active material powder and flake graphite. The positive electrode active material powder includes single particles and / or pseudo-single particles.

[0012] Meanwhile, the negative electrode plate may include a silicon-based negative electrode active material.

[0013] The negative electrode plate may include a silicon-based negative electrode active material and a carbon-based negative electrode active material, and the silicon-based negative electrode active material and the carbon-based negative electrode active material may be included in a weight ratio of 1:99 to 20:80.

[0014] Meanwhile, the secondary battery may be a cylindrical battery with a form factor ratio of 0.4 or more, for example, a 46110 cell, a 4875 cell, a 48110 cell, a 4880 cell, or a 4680 cell. Here, the form factor ratio refers to the value obtained by dividing the diameter of a cylindrical battery by its height, that is, the ratio of the diameter Φ to the height H.

[0015] In addition, the secondary battery according to the present invention may be a battery in which each of the positive and negative electrode plates includes an uncoated portion on which an active material layer is not formed, and at least a portion of the positive or negative electrode plate in the uncoated portion defines an electrode tab.

[0016] The positive plate uncoated portion and the negative plate uncoated portion are located along ends of one side of the positive plate and the negative plate that are parallel to the winding direction of the electrode assembly, respectively, and a current collecting plate is coupled to each of the positive plate uncoated portion and the negative plate uncoated portion, and the current collecting plate may be connected to an electrode terminal.

[0017] Meanwhile, the positive electrode plate uncoated portion and the negative electrode plate uncoated portion may be processed into a plurality of segment pieces that can be bent independently, and at least some of the plurality of segment pieces may define the electrode tab and be bent toward a winding center C of the electrode assembly. Also, at least some of the folded plurality of segment pieces may overlap on upper and lower ends of the electrode assembly, and the current collecting plate may be coupled onto the overlapped plurality of segment pieces.

[0018] Meanwhile, an insulating layer may be further formed on the positive electrode plate, covering a portion of the positive electrode active material layer and a portion of the uncoated portion along a direction parallel to the winding direction.

[0019] According to another embodiment, the present invention provides a battery pack including the lithium secondary battery according to the present invention, and a vehicle including the battery pack. Effect of the Invention

[0020] The lithium secondary battery according to the present invention uses a positive electrode active material including single particles and / or pseudo-single particles as a positive electrode active material, thereby minimizing gas generation due to particle cracking during electrode manufacturing and internal cracking during charging and discharging, thereby achieving excellent safety even in a large battery with an increased volume.

[0021] The lithium secondary battery according to the present invention is also minBy using a positive electrode active material powder having a particle size of 1.0 μm or more, the thermal stability of the battery can be further improved. Research by the present inventors has shown that even if single particles and / or pseudo-single particles are used as the positive electrode active material, the effect of suppressing particle cracking and improving thermal stability after rolling varies depending on the particle size of the positive electrode active material powder. In particular, when particles having a particle size of less than 1.0 μm are contained in the positive electrode active material powder, the voltage increases during the rolling process, particle cracking increases, and thermal stability decreases, making it impossible to ensure sufficient thermal stability when used in large cylindrical batteries. Therefore, in the present invention, min By using positive electrode active material powder with particle size controlled to 1.0 μm or more, the thermal stability improvement effect can be maximized.

[0022] The lithium secondary battery according to the present invention is also 50 , D max By applying positive active material powder with an appropriately controlled particle size distribution (PSD), the increase in resistance caused by the application of single particles can be minimized, resulting in excellent capacity and output characteristics.

[0023] In addition, according to the present invention, since the positive electrode active material layer contains a positive electrode active material and flake graphite, the sliding effect of the flake graphite during rolling prevents the positive electrode plate from being damaged and reduces the porosity of the positive electrode plate to a target value.

[0024] Furthermore, the lithium secondary battery according to the present invention can contain a silicon-based negative electrode active material having a large capacity as the negative electrode active material, and in this case, a higher energy density can be achieved.

[0025] In addition, the lithium secondary battery according to the present invention may have a structure in which the uncoated portions of the positive and negative electrode plates serve as electrode tabs, for example, a tab-less structure. Conventional can-type batteries have a structure in which the electrode plates and electrode leads are connected by electrode tabs, but in this case, a large amount of heat is generated around the electrode tabs due to a large amount of current concentration on the electrode tabs during charging. In particular, this phenomenon becomes severe during fast charging, and there is a risk of the battery catching fire or exploding. In contrast, the lithium secondary battery according to the present invention may have a structure in which uncoated portions on which no active material layer is formed are formed at the ends of the positive and negative electrode plates, and the uncoated portions are connected to electrode terminals by attaching the uncoated portions to current collecting plates having a wide cross-sectional area by a method such as welding. A battery having such a structure has less current concentration than a conventional battery having electrode tabs, and therefore heat generation inside the battery can be effectively reduced, thereby improving the thermal stability of the battery. [Brief description of the drawings]

[0026] [Figure 1] FIG. 4 is a diagram showing a stacked state of an electrode assembly according to the present invention before being wound. [Diagram 2] 2 is a cross-sectional view showing a structure of an electrode plate of an electrode assembly according to an embodiment of the present invention; [Diagram 3] 1 is a cross-sectional view showing the structure of a tabless-type battery according to one embodiment of the present invention; [Figure 4] FIG. 4 is a cross-sectional view showing the structure of a tabless-type battery according to another embodiment of the present invention. [Diagram 5] 2 is a diagram illustrating a structure of an electrode assembly according to an embodiment of the present invention; [Figure 6] 1 is a diagram for explaining a battery pack according to the present invention; [Figure 7] 1 is a diagram for explaining an automobile including a battery pack according to the present invention; [Figure 8] 1 is a graph showing the resistance value versus SOC value for coin half-cells including the positive electrode plates of Example 3 of the present invention, Comparative Example 1, and Comparative Example 2. [Figure 9]1 is a graph showing the capacity retention rate and the resistance increase rate depending on the number of cycles for coin half cells including the positive electrode plates of Example 1, Example 3, and Comparative Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The present invention will now be described in more detail.

[0028] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0029] In the present invention, the term "primary particle" refers to a particle unit that does not have grain boundaries when observed at a magnification of 5,000 to 20,000 using a scanning electron microscope or an electron backscatter diffraction pattern analyzer. The term "average particle size of primary particles" refers to the arithmetic average value calculated after measuring the particle size of primary particles observed using a scanning electron microscope or an EBSD image.

[0030] In the present invention, the "secondary particle" is a particle formed by agglomeration of a plurality of primary particles. In order to distinguish from conventional secondary particles formed by agglomeration of tens to hundreds of primary particles, in the present invention, secondary particles formed by agglomeration of 10 or less primary particles are called pseudo-single particles.

[0031] In the present invention, "D min ", "D 50 " and "D max " is the particle size value of the volume cumulative distribution of the positive electrode active material powder measured using the laser diffraction method. min is the minimum particle size indicated by the cumulative volume distribution, and D 50 is the particle diameter when the cumulative volume is 50%, and D maxis the maximum particle diameter shown in the volume cumulative distribution. The particle size value of the volume cumulative distribution can be measured, for example, by dispersing the positive electrode active material powder in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), irradiating it with ultrasonic waves of about 28 kHz at an output of 60 W, and then obtaining a volume cumulative particle size distribution graph.

[0032] The inventors have conducted extensive research to develop a large-scale battery that achieves high capacity and excellent safety, and as a result have discovered that the safety of large-scale batteries can be significantly improved by using, as a positive electrode active material, a single particle consisting of one primary particle and / or a pseudo-single particle that is an aggregate of 10 or less primary particles, and have thus completed the present invention.

[0033] Specifically, the lithium secondary battery according to the present invention includes an electrode assembly in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction, a battery can in which the electrode assembly is housed, and a seal body that seals an open end of the battery can.

[0034] The configuration of the lithium secondary battery of the present invention will be specifically described below.

[0035] electrode assembly The electrode assembly has a structure in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction, and may be, for example, a jelly roll type electrode assembly.

[0036] FIG. 1 shows a laminated structure of an electrode assembly according to the present invention before being wound, and FIG. 2 shows a cross-sectional structure of an electrode plate (positive or negative electrode plate) according to the present invention.

[0037] Referring to FIG. 1 and FIG. 2, the electrode assembly of the present invention can be manufactured by winding up a laminate formed by stacking a separator 12, a positive electrode plate 10, a separator 12, and a negative electrode plate 11, in that order, at least once, in one direction X.

[0038] Here, the positive electrode plate 10 and the negative electrode plate 11 have a structure in which an active material layer 21 is formed on a long sheet-shaped current collector 20, and may include a blank portion 22 in which the active material layer 21 is not formed in a portion of the current collector 20.

[0039] By using the positive electrode plate 10 and the negative electrode plate 11 including the uncoated portion 22 as described above, a battery having a tabless structure can be realized in which no separate electrode tab is provided, and at least a portion of the uncoated portion of the positive electrode plate 10 and the negative electrode plate 11 define the electrode tab.

[0040] Specifically, the uncoated portion 22 may be formed long along the winding direction X at an end of one side of the current collector 20. A current collecting plate may be bonded to each of the uncoated portions of the positive and negative electrode plates, and the current collecting plates may be connected to electrode terminals, thereby realizing a battery having a tab-less structure.

[0041] For example, a tab-less battery can be manufactured by the following method. First, a separator, a positive plate, a separator, and a negative plate are stacked in order so that the uncoated portions 22 of the positive plate 10 and the negative plate 11 are positioned in the opposite directions, and then the stack is wound in one direction to manufacture an electrode assembly. Then, the uncoated portions 22 of the positive plate and the negative plate are folded in the direction of the winding center C, and current collecting plates are welded to the uncoated portions of the positive plate and the negative plate, respectively, and the current collecting plates are connected to electrode terminals to manufacture a tab-less battery. Meanwhile, the current collecting plates have a larger cross-sectional area than strip-type electrode tabs, and since the resistance is inversely proportional to the cross-sectional area of ​​the path through which the current flows, when a secondary battery is formed in the above-mentioned structure, the cell resistance can be significantly reduced.

[0042] On the other hand, the positive electrode plate and the negative electrode plate uncoated portions may be processed into a plurality of segmented pieces that can be bent independently, and at least a portion of the plurality of segmented pieces may be bent toward the winding center C of the electrode assembly.

[0043] The segments can be formed by processing the current collectors of the positive and negative plates through a metal foil cutting process such as laser notching, ultrasonic cutting, punching, etc.

[0044] When the uncoated portions of the positive and negative electrode plates are processed into multiple segmented pieces, the stress applied to the uncoated portions during bending can be reduced, preventing deformation or damage to the uncoated portions and improving the welding characteristics with the current collecting plates.

[0045] The current collecting plate and the uncoated portion are joined by, for example, welding, and in order to improve the welding characteristics, a strong pressure must be applied to the welded area of ​​the uncoated portion to bend the uncoated portion as flat as possible. However, during this bending process, the shape of the uncoated portion may become irregularly distorted and deformed, and the deformed portion may come into contact with the electrode of the opposite polarity, causing an internal short circuit or causing fine cracks in the uncoated portion. However, if the uncoated portions of the positive and negative electrode plates are processed into multiple segmented pieces that can be bent independently, the stress applied to the uncoated portion during bending is alleviated, and deformation and damage to the uncoated portion can be minimized.

[0046] In addition, when the uncoated portion is processed into segmented pieces as described above, overlaps occur between the segments during folding, which increases the weld strength with the current collecting plate and prevents the laser from penetrating into the electrode assembly and melting the separator or active material when using modern technology such as laser welding. Preferably, at least a portion of the folded segments may overlap on the upper and lower ends of the electrode assembly, and a current collecting plate may be bonded onto the overlapped segments.

[0047] Meanwhile, the electrode assembly according to the present invention may be formed in a structure in which an insulating layer 24 is further formed on the positive electrode plate 10, as shown in Fig. 5. Specifically, the insulating layer 24 may be formed to cover a portion of the positive electrode active material layer and a portion of the uncoated portion in a direction parallel to the winding direction of the electrode assembly.

[0048] In the case of a battery with a tabless structure using the uncoated portion 22c of the positive electrode plate 10 and the uncoated portion 22a of the negative electrode plate 11 as electrode tabs, an electrode assembly is formed such that the positive electrode plate 10 protrudes above the separator 12 and the negative electrode plate 11 protrudes below the separator 12, and the protruding positive electrode plate 10 and / or negative electrode plate 11 are folded and then combined with a current collecting plate. However, when the positive electrode plate 10 or the negative electrode plate 11 is folded as described above, the current collector of the positive electrode plate 10 or the negative electrode plate 11 is positioned adjacent to the electrode of the opposite polarity beyond the separator, which may cause an internal short circuit due to electrical contact between the positive electrode plate and the negative electrode plate. However, when an insulating layer 24 is formed to cover a part of the positive electrode active material layer and the uncoated portion as shown in FIG. 5, the insulating layer 24 can prevent electrical contact between the positive electrode plate 10 and the negative electrode plate 11, thereby preventing a short circuit inside the battery.

[0049] Preferably, the insulating layer 24 is provided on at least one side of the current collector of the positive electrode plate 10, and more preferably, on both sides of the positive electrode plate 10.

[0050] Also, the insulating layer 24 may be formed in a region of the positive electrode plate 10 that may face the active material layer 21a of the negative electrode plate 11. For example, in the uncoated portion 22c of the positive electrode plate 10, the insulating layer 24 may be formed to extend to an end of the uncoated portion 22c on a surface that faces the negative electrode plate 11 after being folded. However, in the case of a surface opposite to the surface that faces the negative electrode plate 11 after being folded, it is preferable that the insulating layer 24 is formed only to a part of the uncoated portion 22c, for example, to a portion in front of the folding point of the uncoated portion 22c. This is because if the insulating layer 24 is formed in the entire region of the uncoated portion on the surface opposite to the surface that faces the negative electrode plate 11, electrical contact with the current collecting plate is not possible, and the insulating layer 24 cannot function as an electrode tab.

[0051] Meanwhile, the insulating layer 24 may be any material or component that can be attached to the positive electrode plate while maintaining insulating performance. For example, the insulating layer may be an insulating coating layer or an insulating tape, and the insulating coating layer may include an organic binder and inorganic particles. Here, the organic binder may be, for example, styrene-butadiene rubber (SBR), and the inorganic particles may be, but are not limited to, alumina oxide.

[0052] Next, each component of the electrode assembly of the present invention will be described in more detail.

[0053] (1) Positive electrode plate The positive electrode plate may have a structure in which a positive electrode active material layer is formed on one or both sides of a sheet-shaped positive electrode current collector, and the positive electrode active material layer may include positive electrode active material powder and flake graphite, and may optionally include a conductive material and / or a binder.

[0054] Specifically, the positive electrode plate may be manufactured by coating one or both sides of a sheet-shaped positive electrode collector with a positive electrode slurry prepared by dispersing a positive electrode active material powder, flake graphite, a conductive material, and / or a binder in a solvent such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and then rolling the coated positive electrode slurry after removing the solvent from the positive electrode slurry by a drying process. Meanwhile, a positive electrode plate including a non-coated portion may be manufactured by not coating a part of the positive electrode collector, for example, one end of the positive electrode collector, with the positive electrode slurry when coating the positive electrode slurry.

[0055] As the positive electrode current collector, various positive electrode current collectors used in the art can be used. For example, as the positive electrode current collector, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used. The positive electrode current collector can usually have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on the surface of the positive electrode current collector to increase the adhesive strength of the positive electrode active material. The positive electrode current collector can be used in various forms, such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0056] In the present invention, the positive electrode plate contains a positive electrode active material powder consisting of a single particle consisting of one primary single particle and / or a quasi-single particle which is an aggregate of 10 or less primary particles.

[0057] Conventionally, it has been common to use spherical secondary particles formed by agglomeration of tens to hundreds of primary particles as the positive electrode active material of a lithium secondary battery. However, in the case of a positive electrode active material in the form of secondary particles formed by agglomeration of many primary particles, there is a problem that the primary particles are easily broken during the rolling process during the manufacture of the positive electrode, and cracks are generated inside the particles during the charge and discharge process. When cracks occur in the particles of the positive electrode active material or inside the particles, the contact area with the electrolyte increases, and the generation of gas due to a side reaction with the electrolyte increases. If the generation of gas increases inside the battery, the pressure inside the battery increases, which may cause the battery to explode. In particular, when the volume of a cylindrical battery is increased, the amount of active material inside the battery increases due to the increase in volume, and the amount of gas generated also increases significantly, which increases the risk of the battery catching fire and / or exploding.

[0058] In contrast, positive electrode active materials in the form of single particles consisting of one primary particle or pseudo-single particles in which 10 or less primary particles are aggregated have higher particle strength than existing positive electrode active materials in the form of secondary particles in which tens to hundreds of primary particles are aggregated, and therefore hardly crack particles during rolling. In addition, in the case of positive electrode active materials in the form of single particles or pseudo-single particles, the number of primary particles constituting the particles is small, so there is little change due to volume expansion and contraction of the primary particles during charging and discharging, and therefore the occurrence of cracks inside the particles is significantly reduced.

[0059] Therefore, when a positive electrode active material consisting of single particles and / or pseudo-single particles is used as in the present invention, the amount of gas generated due to particle breakage and internal cracking can be significantly reduced, thereby realizing excellent safety even in large cylindrical batteries.

[0060] Meanwhile, the monoparticles and / or pseudo-monoparticles are preferably included in an amount of 95% by weight to 100% by weight, preferably 98% by weight to 100% by weight, more preferably 99% by weight to 100% by weight, and even more preferably 100% by weight, based on the weight of the total positive active material powder included in the positive plate. When the content of the monoparticles and / or pseudo-monoparticles satisfies the above range, sufficient safety can be obtained when applied to a large cylindrical battery. When the secondary particle type positive active material is included in an amount exceeding 5% by weight of the total positive active material, the side reaction with the electrolyte increases due to the fraction generated from the secondary particles during the manufacture and charging / discharging of the electrode, thereby reducing the effect of suppressing gas generation, and thus the effect of improving stability may be reduced when applied to a large cylindrical battery.

[0061] On the other hand, the positive electrode active material powder in the form of single particle and / or pseudo-single particle according to the present invention has a D min The diameter of the positive electrode active material powder may be 1.0 μm or more, 1.1 μm or more, 1.15 μm or more, 1.2 μm or more, 1.25 μm or more, 1.3 μm or more, 1.35 μm or more, 1.4 μm or more, 1.45 μm or more, or 1.5 μm or more. minIf the thickness is less than 1.0 μm, the voltage increases during the rolling process of the positive plate, which makes it easy for particles to crack, and the thermal stability decreases, making it difficult to ensure sufficient thermal stability when applied to large cylindrical batteries.

[0062] On the other hand, in terms of output and resistance characteristics, the D of the positive electrode active material powder having a single particle and / or pseudo-single particle form according to the present invention is min may be 3 μm or less, 2.5 μm or less, or 2.0 μm or less. D min If is too large, the number of lithium diffusion paths inside the particles increases, which can result in reduced output and resistance characteristics.

[0063] Specifically, the D of the positive electrode active material powder having a single particle and / or pseudo-single particle form according to the present invention min can be 1.0 μm to 3 μm, 1.0 μm to 2.5 μm, or 1.3 μm to 2.0 μm.

[0064] On the other hand, the positive electrode active material powder is D 50 can be 5 μm or less, 4 μm or less, or 3 μm or less, for example, 0.5 μm to 5 μm, preferably 1 μm to 5 μm, and more preferably 2 μm to 5 μm. A positive electrode active material in the form of a single particle and / or a pseudo-single particle has fewer interfaces between primary particles that serve as diffusion paths for lithium ions inside the particles, so that lithium mobility is lower than in a positive electrode active material in the form of a secondary particle, which causes a problem of increased resistance. Such an increase in resistance becomes more severe as the particle size increases, and the increased resistance has a negative effect on capacity and output characteristics. Therefore, the D of the positive electrode active material powder is 50 By adjusting the diameter to 5 μm or less, the lithium ion diffusion distance inside the positive electrode active material particles can be minimized, thereby suppressing an increase in resistance.

[0065] The positive electrode active material powder is D max The diameter of the positive electrode active material powder may be 12 μm to 17 μm, preferably 12 μm to 16 μm, and more preferably 12 μm to 15 μm. maxWhen the D of the positive electrode active material powder satisfies the above range, the resistance characteristic and the capacitance characteristic are more excellent. max If D is too large, aggregation between single particles occurs, and the lithium migration path inside the aggregated particles becomes longer, which reduces the lithium mobility and increases the resistance. max If is too small, excessive crushing will occur, and excessive crushing will cause D min The particle size distribution (PSD) of the positive electrode active material powder, represented by the following formula (1), may be 3 or less, preferably 2 to 3, and more preferably 2.3 to 3.

[0066] Equation (1): Particle size distribution (PSD) = (D max -D min ) / D 50

[0067] When the positive electrode active material powder has the above particle size distribution, the electrode density of the positive electrode can be appropriately maintained, and particle cracking and an increase in resistance can be effectively suppressed.

[0068] Meanwhile, the positive electrode active material may have an average particle size of 5 μm or less, 4 μm or less, 3 μm or less, or 2 μm or less, for example, 0.5 μm to 5 μm, preferably 1 μm to 5 μm, and more preferably 2 μm to 5 μm. When the average particle size of the primary particles satisfies the above range, a positive electrode active material having excellent electrochemical properties and a single particle and / or pseudo-single particle form may be formed. If the average particle size of the primary particles is too small, the number of agglomerates of the primary particles forming the positive electrode active material increases, and the effect of suppressing the occurrence of particle cracks during rolling decreases. If the average particle size of the primary particles is too large, the lithium diffusion path inside the primary particles becomes long, increasing the resistance and decreasing the output characteristics.

[0069] In the present invention, the positive electrode active material powder preferably has a unimodal particle size distribution. In the past, in order to improve the electrode density of the positive electrode active material layer, bimodal positive electrode active materials have been used in which a large particle size positive electrode active material having a large average particle size and a small particle size positive electrode active material having a small average particle size are mixed. However, in the case of single particle and / or pseudo-single particle positive electrode active materials, as the particle size increases, the lithium migration path becomes longer and the resistance increases significantly, so that when large particle size particles are mixed, the capacity and output characteristics may be reduced. Therefore, in the present invention, the increase in resistance can be minimized by using a positive electrode active material having a unimodal distribution.

[0070] Meanwhile, the positive electrode active material may include a lithium nickel-based oxide, specifically, a lithium nickel-based oxide containing 80 mol% or more of Ni relative to the total moles of transition metals. Preferably, the lithium nickel-based oxide may contain Ni in an amount of 80 mol% or more and less than 100 mol%, 82 mol% or more and less than 100 mol%, or 83 mol% or more and less than 100 mol%. As described above, when a lithium nickel-based oxide with a high Ni content is used, a high capacity can be achieved.

[0071] More specifically, the positive electrode active material may include a lithium nickel-based oxide represented by the following [Chemical Formula 1].

[0072] [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O2

[0073] In the above Chemical Formula 1, M 1 can be Mn, Al or a combination thereof, preferably Mn or Mn and Al.

[0074] Said M 2is one or more selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb, preferably can be one or more selected from the group consisting of Zr, Y, Mg, and Ti, and more preferably can be Zr, Y, or a combination thereof. M 2 The element is not necessarily included, but when included in an appropriate amount, it can play a role in promoting grain growth during firing or improving crystal structure stability.

[0075] Said a represents the lithium molar ratio in the lithium nickel-based oxide, and can be 0.8 ≦ a ≦ 1.2, 0.85 ≦ a ≦ 1.15, or 0.9 ≦ a ≦ 1.2. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium nickel-based oxide can be stably formed.

[0076] Said b represents the molar ratio of nickel among all the metals other than lithium in the lithium nickel-based oxide, and can be 0.8 ≦ b < 1, 0.82 ≦ b < 1, 0.83 ≦ b < 1, 0.85 ≦ b < 1, 0.88 ≦ b < 1, or 0.90 ≦ b < 1. When the molar ratio of nickel satisfies the above range, it shows a high energy density and high capacity can be realized.

[0077] Said c represents the cobalt molar ratio among all the metals other than lithium in the lithium nickel-based oxide, and can be 0 < c < 0.2, 0 < c < 0.18, 0.01 ≦ c ≦ 0.17, 0.01 ≦ c ≦ 0.15, 0.01 ≦ c ≦ 0.12, or 0.01 ≦ c ≦ 0.10. When the molar ratio of cobalt satisfies the above range, good resistance characteristics and output characteristics can be realized.

[0078] Said d represents the molar ratio of the M 1 element among all the metals other than lithium in the lithium nickel-based oxide, and can be 0 < d < 0.2, 0 < d < 0.18, 0.01 ≦ d ≦ 0.17, 0.01 ≦ d ≦ 0.15, 0.01 ≦ d ≦ 0.12, or 0.01 ≦ d ≦ 0.10. M 1 When the molar ratio of the element satisfies the above range, the structure stability of the positive electrode active material is excellent.

[0079] The e is M among all metals other than lithium in the lithium nickel-based oxide. 2 It indicates the molar ratio of the elements and can be 0≦e≦0.1, or 0≦e≦0.05.

[0080] Meanwhile, the positive electrode active material according to the present invention may further include, if necessary, a coating layer on the surface of the lithium nickel-based oxide particles, the coating layer including one or more coating elements selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb, Mo, Sr, Sb, Bi, Si, and S. Preferably, the coating element may be Al, B, Co, or a combination thereof.

[0081] When a coating layer is present on the surface of the lithium nickel-based oxide particles, the coating layer suppresses contact between the electrolyte and the lithium composite transition metal oxide, thereby reducing the elution of the transition metal and the generation of gas due to side reactions with the electrolyte.

[0082] The positive electrode active material can be contained in an amount of 80 to 99% by weight, preferably 85 to 99% by weight, and more preferably 90 to 99% by weight, based on the total weight of the positive electrode active material layer.

[0083] In the present invention, a positive electrode active material layer containing the single-particle and / or quasi-single-particle positive electrode active material and flake graphite is used.

[0084] Flake graphite means graphite having a structure in which a plurality of plate-like graphite layers are laminated, and when a positive electrode active material layer in which flake graphite is added to a single particle or pseudo-single particle positive electrode active material is rolled, the flake graphite provides a slipping effect to the positive electrode active material, improving the rolling characteristics of the electrode and reducing the electrode porosity to a target level. As a result, the lithium secondary battery according to the present invention can have improved battery stability, resistance characteristics, and charge / discharge efficiency.

[0085] Meanwhile, the flake graphite may be included in the positive electrode active material layer in an amount of 0.05 wt% to 5 wt%, and preferably in an amount of 0.1 wt% to 3 wt%. When the content of the flake graphite is within the above range, the rolling characteristics of the positive electrode are improved, and excellent electrode density can be achieved. If the content of the flake graphite is too low, the rolling characteristics are not significantly improved, and if the content is too high, the slurry viscosity may increase and the phase stability may decrease, and the resistance may increase due to the decrease in electrode uniformity caused by binding with the conductive material.

[0086] Meanwhile, the flake graphite used in the present invention may have an average particle size of 1 μm to 20 μm, preferably 2 μm to 10 μm, and more preferably 3 μm to 5 μm, although it is not limited thereto. If the size of the flake graphite is too small, it is difficult to achieve the desired porosity, and the current density may be reduced, resulting in a low capacity. Here, the average particle size of the flake graphite may be measured by a laser diffraction method (ISO 13320).

[0087] The aspect ratio of the flake graphite may be 0.1 to 500, preferably 1 to 100, and more preferably 1 to 30. When the aspect ratio of the flake graphite satisfies the above range, an effect of improving conductivity and reducing electrode resistance is achieved.

[0088] The flake graphite has a density of 2.0 g / cm 3 ~2.5g / cm 3 , preferably 2.1 g / cm 3 ~2.4g / cm 3 , more preferably 2.2 g / cm 3 ~2.3g / cm 3 It can be.

[0089] Meanwhile, in the present invention, the porosity of the positive electrode active material layer may be 15% to 23%, preferably 17% to 23%, and more preferably 18% to 23%. When the porosity of the positive electrode active material layer satisfies the above range, the electrode density increases, excellent capacity can be realized, and resistance decreases. If the porosity is too low, the electrolyte impregnation property decreases, and lithium deposition due to non-impregnation of the electrolyte may occur, and if the porosity is too high, the contact between the electrodes is not good, resistance increases, and the energy density decreases, resulting in little capacity improvement effect.

[0090] The porosity of the positive electrode active material layer can be achieved by i) the positive electrode active material being in a single particle or quasi-single particle form, and ii) adding flake graphite to the positive electrode active material.

[0091] In order to realize a high loading electrode having a relatively high loading amount of the positive electrode active material layer, when a positive electrode active material in the form of a single particle or quasi-single particle is used as in the present invention, cracking of the particles of the active material during rolling is significantly reduced and damage to the positive electrode current collector (aluminum foil) is reduced compared to the conventional positive electrode active material in the form of secondary particles, so that rolling can be performed at a relatively high voltage and the porosity of the positive electrode active material layer can be reduced to the above-mentioned numerical range, thereby increasing the energy density.

[0092] In addition, when flake graphite is added to the positive electrode active material as in the present invention, the flake graphite provides a slipping effect during rolling, improving the rolling characteristics, and the porosity of the positive electrode active material layer may be reduced to the above-mentioned numerical range.

[0093] The positive electrode has a loading of 570 mg / 25 cm 2 More than 600mg / 25cm 2 ~800g / 25m 2 , more preferably 600 mg / 25 cm 2 ~750mg / 25cm 2Specifically, in the case of the lithium secondary battery according to the present invention, the rolling characteristics of the electrode are improved by using the single particle and / or quasi-single particle positive electrode active material and flake graphite, so that the loading amount of the positive electrode can be secured at a relatively high level, thereby realizing high capacity characteristics.

[0094] Next, the conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery that is constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives. Of these, one type alone or a mixture of two or more types can be used. The conductive material can usually be contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.

[0095] The binder plays a role in improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and among these, one type alone or a mixture of two or more types can be used. The binder can be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.

[0096] Meanwhile, an insulating layer may be further formed on the positive electrode plate according to the present invention, covering a portion of the positive electrode active material layer and a portion of the uncoated portion, if necessary, in a direction parallel to the winding direction of the electrode assembly.

[0097] (2) Negative electrode plate The negative electrode plate may have a structure in which a negative electrode active material layer is formed on one or both sides of a long sheet-shaped negative electrode current collector, and the negative electrode active material layer may include a negative electrode active material, a conductive material, and a binder.

[0098] Specifically, the negative electrode plate can be manufactured by applying a negative electrode slurry, which is produced by dispersing a negative electrode active material, a conductive material, and a binder in a solvent such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, onto one or both surfaces of a sheet-like negative electrode current collector, removing the solvent of the negative electrode slurry by a drying process, and then rolling it. On the other hand, when applying the negative electrode slurry, a negative electrode plate including a plain portion can be manufactured by a method of not applying the negative electrode slurry to a partial region of the negative electrode current collector, for example, one end portion of the negative electrode current collector.

[0099] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium can be used. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; silicon-based materials such as Si, Si-Me alloy (where Me is one or more selected from the group consisting of Al, Sn, Mg, Cu, Fe, Pb, Zn, Mn, Cr, Ti, and Ni), SiOy (where 0 < y < 2), and Si-C composite; a thin film of lithium metal; metal materials capable of alloying with lithium such as Sn and Al; and the like. Any one or a mixture of two or more of these can be used.

[0100] Preferably, the negative electrode plate according to the present invention can contain a silicon-based negative electrode active material. The silicon-based negative electrode active material can be Si, Si-Me alloy (where Me is one or more selected from the group consisting of Al, Sn, Mg, Cu, Fe, Pb, Zn, Mn, Cr, Ti, and Ni), SiOy (where 0 < y < 2), Si-C composite, or a combination thereof, and preferably can be SiOy (where 0 < y < 2). Since the silicon-based negative electrode active material has a high theoretical capacity, when the silicon-based negative electrode active material is included, the capacity characteristics can be improved.

[0101] On the other hand, the silicon-based negative electrode active material is M bIt can be doped with a metal, where the M b The metal can be a Group 1 metal element or a Group 2 metal element. Specifically, it can be Li, Mg, etc. Specifically, the silicon negative electrode active material is M b It can be Si doped with a metal, SiOy (where 0 < y < 2), a Si-C composite, etc. In the case of a silicon-based negative electrode active material doped with a metal, the capacity of the active material decreases somewhat depending on the doping element, but since it has high efficiency, a high energy density can be realized.

[0102] In addition, the silicon-based negative electrode active material can further include a carbon coating layer on the surface of the particles. Here, the amount of the carbon coating can be 20% by weight or less, preferably 1 - 20% by weight, based on the total weight of the silicon-based negative electrode active material.

[0103] In addition, the negative electrode plate can further include a carbon-based negative electrode active material as the negative electrode active material, if necessary. The carbon-based negative electrode active material can be, for example, artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, soft carbon, hard carbon, etc., but is not limited thereto.

[0104] On the other hand, when using a mixture of a silicon-based negative electrode active material and a carbon-based negative electrode active material as the negative electrode active material, the mixing ratio of the silicon-based negative electrode active material and the carbon-based negative electrode active material can be 1:99 - 20:80, preferably 1:99 - 15:85, more preferably 1:99 - 10:90 by weight.

[0105] The negative electrode active material can be contained in an amount of 80 - 99% by weight, preferably 85 - 99% by weight, more preferably 90 - 99% by weight, based on the total weight of the negative electrode active material layer.

[0106] Meanwhile, as the negative electrode current collector, a negative electrode current collector generally used in the technical field can be used, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. The negative electrode current collector can usually have a thickness of 3 to 500 μm, and like the positive electrode current collector, the surface of the current collector can be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0107] The conductive material is used to impart electrical conductivity to the negative electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery to be constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives. Of these, one type alone or a mixture of two or more types can be used. The conductive material can usually be contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.

[0108] The binder plays a role in improving the adhesion between the negative electrode active material particles and the adhesive strength between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and among these, one type alone or a mixture of two or more types may be used. The binder may be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.

[0109] (3) Separator The separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. Specifically, the separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, or the like, may be used. In addition, a coated separator containing a ceramic component or a polymeric substance may be used to ensure heat resistance or mechanical strength.

[0110] Lithium secondary battery Next, the lithium secondary battery according to the present invention will be described.

[0111] The lithium secondary battery according to the present invention may include an electrode assembly having a structure in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction, a battery can in which the electrode assembly is housed, and a seal body that seals an open end of the battery can.

[0112] Preferably, the lithium secondary battery according to the present invention can be a cylindrical battery, and more preferably, a large cylindrical battery having a form factor ratio (defined as the value obtained by dividing the diameter of a cylindrical battery by its height, i.e., the ratio of the diameter (Φ) to the height (H)) of 0.4 or more. Here, the form factor refers to values ​​indicating the diameter and height of a cylindrical battery.

[0113] Cylindrical batteries according to the present invention can be, for example, 46110 cells (diameter 46 mm, height 110 mm, form factor ratio 0.418), 4875 cells (diameter 48 mm, height 75 mm, form factor ratio 0.640), 48110 cells (diameter 48 mm, height 110 mm, form factor ratio 0.436), 4880 cells (diameter 48 mm, height 80 mm, form factor ratio 0.600), and 4680 cells (diameter 46 mm, height 80 mm, form factor ratio 0.575). In the form factor numbers, the first two digits indicate the diameter of the cell, and the next two or three digits indicate the height of the cell.

[0114] The lithium secondary battery according to the present invention uses a positive electrode active material in the form of a single particle and / or pseudo-single particle to significantly reduce the amount of gas generated compared to the conventional battery, thereby achieving excellent safety even in a large cylindrical battery having a form factor ratio of 0.4 or more.

[0115] Meanwhile, the lithium secondary battery according to the present invention may preferably be a battery having a tab-less structure that does not include an electrode tab, but is not limited thereto.

[0116] The tabless-structured battery may have a structure in which, for example, each of the positive and negative electrode plates includes an uncoated portion where no active material layer is formed, the uncoated positive and negative electrode plate portions are located at the upper and lower ends of the electrode assembly, respectively, current collecting plates are bonded to the uncoated positive and negative electrode plate portions, and the current collecting plates are connected to electrode terminals.

[0117] Fig. 3 shows a cross-sectional view of a battery having a tabless structure according to one embodiment of the present invention. Hereinafter, a battery according to one embodiment of the present invention will be described with reference to Fig. 3. However, Fig. 3 shows one embodiment of the present invention, and the structure of the battery according to the present invention is not limited to the scope disclosed in Fig. 3.

[0118] A battery 140 according to an embodiment of the present invention includes a jelly-roll type electrode assembly 141, a battery can 142 in which the electrode assembly 141 is housed, and a seal 143 that seals an open end of the battery can 142.

[0119] Here, the positive and negative electrode plates of the electrode assembly may each include an uncoated portion where no active material layer is formed, and may be stacked and wound such that the positive and negative uncoated portions are located at the upper and lower ends of the electrode assembly, respectively. Since the electrode assembly has been described above, only the remaining components other than the electrode assembly will be described below.

[0120] The battery can 142 is a container having an opening at the top and is made of a conductive metal material such as aluminum or steel. The battery can accommodates the electrode assembly 141 in the inner space through the opening at the top, and also accommodates an electrolyte.

[0121] As the electrolyte used in the present invention, various electrolytes that can be used in lithium secondary batteries, such as organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes, can be used, and the type is not particularly limited.

[0122] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0123] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a C2-C20 straight-chain, branched or cyclic hydrocarbon group that can contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of a battery and a low-viscosity straight-chain carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is more preferred.

[0124] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as the lithium salt. The concentration of the lithium salt is preferably within a range of 0.1 to 5.0M, preferably 0.1 to 3.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0125] In addition to the electrolyte components, the electrolyte may further contain additives for the purpose of improving the life characteristics of the battery, suppressing the capacity reduction of the battery, and improving the discharge capacity of the battery. For example, the additives may be haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, which may be used alone or in combination, but are not limited thereto. The additives may be contained in an amount of 0.1 to 10% by weight, preferably 0.1 to 5% by weight, based on the total weight of the electrolyte.

[0126] The battery can 142 is electrically connected to the uncoated portion 146b of the negative plate and functions as a negative terminal that contacts an external power source and transmits a current applied from the external power source to the negative plate.

[0127] If necessary, a beading portion 147 and a crimping portion 148 may be provided at the upper end of the battery can 142. The beading portion 147 may be formed by pressing the periphery of the outer circumferential surface of the battery can 142 up to a distance D1. The beading portion 147 prevents the electrode assembly 141 accommodated inside the battery can 142 from being separated through the upper opening of the battery can 142, and may function as a support on which the sealed body 143 is placed.

[0128] The crimping portion 148 may be formed on the beading portion 147, and has an extended and bent shape so as to enclose the outer circumferential surface of the cap plate 143a disposed on the beading portion 147 and a part of the upper surface of the cap plate 143a.

[0129] Next, the sealing body 143 is for sealing the open end of the battery can 142, and includes a cap plate 143a, a first gasket 143b having insulating properties and providing airtightness between the cap plate 143a and the battery can 142, and may further include a connection plate 143c electrically and mechanically coupled to the cap plate 143a, if necessary. The cap plate 143a may be crimped onto a beading portion 147 formed on the battery can 142 and fixed by a crimping portion 148.

[0130] The cap plate 143a is a part made of a conductive metal material and covers an upper opening of the battery can 142. The cap plate 143a is electrically connected to the positive electrode plate of the electrode assembly 141 and is electrically insulated from the battery can 142 via a first gasket 143b. Thus, the cap plate 143a can function as a positive electrode terminal of the secondary battery. The cap plate 143a may have a protrusion 143d protruding upward from a center C thereof, and the protrusion 143d may come into contact with an external power source so that a current can be applied from the external power source.

[0131] A first gasket 143b may be interposed between the cap plate 143a and the crimping portion 148 to ensure airtightness of the battery can 142 and to electrically insulate the battery can 142 from the cap plate 143a.

[0132] Meanwhile, the battery 140 according to the present invention may further include current collecting plates 144, 145, if necessary. The current collecting plates are joined to the positive plate uncoated portion 146a and the negative plate uncoated portion 146b, and are connected to electrode terminals (i.e., positive and negative terminals).

[0133] Specifically, the battery 140 according to the present invention may include a first current collecting plate 144 coupled to an upper portion of the electrode assembly 141 and a second current collecting plate 145 coupled to a lower portion of the electrode assembly 141 .

[0134] A first current collecting plate 144 and / or a second current collecting plate 145 may further be included.

[0135] The first current collecting plate 144 is coupled to an upper portion of the electrode assembly 141. The first current collecting plate 144 is made of a conductive metal material such as aluminum, copper, or nickel, and is electrically connected to the uncoated portion 146a of the positive electrode plate. A lead 149 may be coupled to the first current collecting plate 144. The lead 149 may extend upwardly of the electrode assembly 141 and be coupled to the connection plate 143c, or may be directly coupled to the lower surface of the cap plate 143a. The coupling of the lead 149 to other components may be performed by welding. Preferably, the first current collecting plate 144 may be formed integrally with the lead 149. In this case, the lead 149 may have a long plate shape extending outward from the center of the first current collecting plate 144.

[0136] Meanwhile, the first current collecting plate 144 is coupled to an end of the uncoated portion 146a of the positive electrode plate, and the coupling may be performed by, for example, laser welding, resistance welding, ultrasonic welding, soldering, or the like.

[0137] The second current collecting plate 145 is coupled to the lower part of the electrode assembly 141. The second current collecting plate 145 is made of a conductive metal material such as aluminum, copper, or nickel, and is electrically connected to the uncoated portion 146b of the negative electrode plate. One surface of the second current collecting plate 145 may be coupled to the uncoated portion 146b of the negative electrode plate, and the opposite surface may be coupled to the inner bottom surface of the battery can 142. Here, the coupling may be performed by a method such as laser welding, resistance welding, ultrasonic welding, soldering, etc.

[0138] Meanwhile, the battery 140 according to the present invention may further include an insulating member (insulator) 146, if necessary. The insulating member 146 may be disposed to cover an upper surface of the first current collecting plate 144. By covering the first current collecting plate 144 with the insulating member 146, it is possible to prevent the first current collecting plate 144 and the inner peripheral surface of the battery can 142 from directly contacting each other.

[0139] The insulating member 146 has a lead hole 151 through which the lead 149 extending upward from the first current collecting plate 144 is pulled out. The lead 149 is pulled out upward through the lead hole 151 and coupled to the lower surface of the connecting plate 143c or the lower surface of the cap plate 143a.

[0140] The insulating member 146 may be made of an insulating polymer resin, such as polyethylene, polypropylene, polyimide, or polybutylene terephthalate.

[0141] Meanwhile, the battery 140 according to the present invention may further include a venting portion 152 formed on the bottom surface of the battery can 142, if necessary. The venting portion 152 corresponds to a region of the bottom surface of the battery can 142 that is thinner than the surrounding region. Since the venting portion 152 is thin, it is structurally weaker than the surrounding region. Therefore, when the pressure inside the battery 140 increases above a predetermined level, the venting portion 152 bursts to release the gas inside the battery can 142 to the outside, thereby preventing the battery from exploding.

[0142] Fig. 4 shows a cross-sectional view of a battery having a tabless structure according to another embodiment of the present invention. Hereinafter, a battery according to another embodiment of the present invention will be described with reference to Fig. 4. However, Fig. 4 shows one embodiment of the present invention, and the structure of the battery according to the present invention is not limited to the scope disclosed in Fig. 4.

[0143] Referring to FIG. 4, a battery 170 according to another embodiment of the present invention has a different structure of the battery can and the sealed body compared to the battery 140 shown in FIG. 3, but the configuration of the electrode assembly and electrolyte is substantially the same.

[0144] Specifically, the battery 170 includes a battery can 171 through which a rivet terminal 172 is installed. The rivet terminal 172 is installed on a partially closed surface (top surface in the drawing) of one end of the battery can 171. The rivet terminal 172 is riveted into a through hole (first opening at a first end) of the battery can 171 with an insulating second gasket 173 interposed therebetween. The rivet terminal 172 is exposed to the outside in the direction opposite to the gravity.

[0145] The rivet terminal 172 includes a terminal exposing portion 172a and a terminal inserting portion 172b. The terminal exposing portion 172a is exposed to the outside of the closed surface of the battery can 171. The terminal exposing portion 172a may be located at an approximately center of the partially closed surface of the battery can 171. The maximum diameter of the terminal exposing portion 172a may be larger than the maximum diameter of the through hole formed in the battery can 171. The terminal inserting portion 172b may penetrate approximately the center of the partially closed surface of the battery can 171 to be electrically connected to the uncoated portion 146a of the positive electrode plate. The terminal inserting portion 172b may be rivet-coupled to the inner surface of the battery can 171. That is, an end of the terminal inserting portion 172b may have a shape that is bent toward the inner surface of the battery can 171. The maximum diameter of the end of the terminal inserting portion 172b may be larger than the maximum diameter of the through hole of the battery can 171.

[0146] A lower end surface of the terminal insertion portion 172b may be welded to the first current collecting plate 144 connected to the uncoated portion 146a of the positive electrode plate. An insulating cap 174 made of an insulating material may be interposed between the first current collecting plate 144 and the inner surface of the battery can 171. The insulating cap 174 covers an upper portion of the first current collecting plate 144 and an upper edge portion of the electrode assembly 141. This prevents the uncoated portion on the outer periphery of the electrode assembly 141 from coming into contact with the inner surface of the battery can 171 having a different polarity, causing a short circuit. The terminal insertion portion 172b of the rivet terminal 172 may be welded to the first current collecting plate 144 by penetrating the insulating cap 174.

[0147] The second gasket 173 is interposed between the battery can 171 and the rivet terminal 172 to prevent electrical contact between the battery can 171 and the rivet terminal 172, which have opposite polarities. This allows the upper surface of the rivet terminal 172, which has a substantially flat shape, to function as a positive terminal of the battery 170.

[0148] The second gasket 173 includes a gasket exposing portion 173a and a gasket inserting portion 173b. The gasket exposing portion 173a is interposed between the terminal exposing portion 172a of the rivet terminal 172 and the battery can 171. The gasket inserting portion 173b is interposed between the terminal inserting portion 172b of the rivet terminal 172 and the battery can 171. The gasket inserting portion 173b is deformed when the terminal inserting portion 172b is riveted, and can be closely attached to the inner surface of the battery can 171. The second gasket 173 may be made of, for example, a polymer resin having insulating properties.

[0149] The gasket exposing portion 173a of the second gasket 173 may extend to cover an outer circumferential surface of the terminal exposing portion 172a of the rivet terminal 172. When the second gasket 173 covers the outer circumferential surface of the rivet terminal 172, it is possible to prevent a short circuit from occurring during the process of connecting an electrical connecting component such as a bus bar to the upper surface of the battery can 171 and / or the rivet terminal 172. Although not shown in the drawings, the gasket exposing portion 173a may extend to cover not only the outer circumferential surface of the terminal exposing portion 172a but also a portion of the upper surface.

[0150] When second gasket 173 is made of a polymer resin, second gasket 173 can be joined to battery can 171 and rivet terminal 172 by thermal fusion. In this case, it is possible to strengthen the airtightness at the joining interface between second gasket 173 and rivet terminal 172 and at the joining interface between second gasket 173 and battery can 171. On the other hand, when gasket exposed portion 173a of second gasket 173 has a form that extends to the upper surface of terminal exposed portion 172a, rivet terminal 172 can be joined integrally with second gasket 173 by insert injection.

[0151] The remaining area 175 of the upper surface of the battery can 171 other than the area occupied by the rivet terminal 172 and the second gasket 173 corresponds to a negative terminal having a polarity opposite to that of the rivet terminal 172 .

[0152] The second current collecting plate 176 is coupled to the lower part of the electrode assembly 141. The second current collecting plate 176 is made of a conductive metal material such as aluminum, steel, copper, or nickel, and is electrically connected to the uncoated portion 146b of the negative electrode plate.

[0153] Preferably, the second current collecting plate 176 is electrically connected to the battery can 171. To this end, the second current collecting plate 176 may be fixed with at least a portion of an edge portion interposed between the inner surface of the battery can 171 and the first gasket 178b. In one example, at least a portion of the edge portion of the second current collecting plate 176 may be fixed to the beading portion 180 by welding while being supported by a lower end surface of the beading portion 180 formed at the lower end of the battery can 171. In a modified example, at least a portion of the edge portion of the second current collecting plate 176 may be directly welded to the inner wall surface of the battery can 171.

[0154] The second current collecting plate 176 may have a plurality of projections and recesses (not shown) formed radially on a surface facing the uncoated portion 146b. When the projections and recesses are formed, the second current collecting plate 176 may be pressed to press the projections and recesses into the uncoated portion 146b.

[0155] Preferably, the end of the second current collecting plate 176 and the uncoated portion 146b may be joined by welding, for example laser welding.

[0156] The sealing body 178 that seals the lower open end of the battery can 171 includes a cap plate 178a and a first gasket 178b. The first gasket 178b electrically separates the cap plate 178a from the battery can 171. A crimping portion 181 fixes the edge of the cap plate 178a and the first gasket 178b together. The cap plate 178a is provided with a vent portion 179. The configuration of the vent portion 179 is substantially the same as that of the above-mentioned embodiment.

[0157] Preferably, the cap plate 178a is made of a conductive metal material. However, the cap plate 178a does not have electrical polarity because the first gasket 178b is interposed between the cap plate 178a and the battery can 171. The seal 178 seals the open end of the lower part of the battery can 171 and functions to discharge gas when the internal pressure of the battery cell 170 increases above a critical value.

[0158] Preferably, the rivet terminal 172 electrically connected to the uncoated portion 146a of the positive electrode plate is used as a positive electrode terminal. Also, a portion 175 of the upper surface of the battery can 171 electrically connected to the uncoated portion 146b of the negative electrode plate via the second current collecting plate 176 other than the rivet terminal 172 is used as a negative electrode terminal. In this way, when two electrode terminals are located on the upper part of the battery, an electrical connection part such as a bus bar can be disposed only on one side of the battery 170. This can simplify the structure of the battery pack and improve the energy density. Also, since the portion 175 used as the negative electrode terminal has a substantially flat shape, a sufficient connection area can be secured when connecting an electrical connection part such as a bus bar. As a result, the battery 170 can reduce the resistance at the connection part of the electrical connection part to a preferable level.

[0159] When a lithium secondary battery is formed in a tabless structure as described above, current concentration is less than in conventional batteries with electrode tabs, so heat generation inside the battery can be effectively reduced, thereby improving the thermal stability of the battery.

[0160] The lithium secondary battery of the present invention as described above may be used to manufacture a battery pack. Fig. 6 is a schematic diagram of a battery pack according to an embodiment of the present invention. Referring to Fig. 6, a battery pack 3 according to an embodiment of the present invention includes an assembly to which secondary batteries 1 are electrically connected and a pack housing 2 that accommodates the assembly. The secondary batteries 1 are the battery cells according to the above-described embodiment. For convenience of illustration, components such as a bus bar for electrically connecting the secondary batteries 1, a cooling unit, and external terminals are omitted in the drawings.

[0161] The battery pack 3 can be mounted on a vehicle. The vehicle can be, for example, an electric vehicle, a hybrid vehicle, or a plug-in hybrid vehicle. The vehicle can include a four-wheeled vehicle or a two-wheeled vehicle.

[0162] FIG. 7 is a diagram for explaining an automobile including the battery pack 3 of FIG.

[0163] Referring to FIG. 7, an automobile 5 according to an embodiment of the present invention includes a battery pack 3 according to an embodiment of the present invention, and is operated by receiving power from the battery pack 3.

[0164] The present invention will now be described in more detail with reference to specific examples.

[0165] Example 1 Unimodal particle size distribution, D min = 1.78 μm, D 50 = 4.23 μm, D max = 13.1 μm, and a positive electrode active material powder (composition: Li[Ni 0.9 Co 0.06 Mn 0.03 Al 0.01 ]O2), flake graphite (SFG6L), conductive material (multi-walled carbon nanotubes), and PVDF binder were mixed in N-methylpyrrolidone in a weight ratio of 96.3:1.5:0.4:1.8 to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector sheet, dried, and rolled at a linear pressure of 3.0 ton / cm to prepare a positive electrode plate. The porosity of the positive electrode active material layer of the positive electrode plate prepared as above was measured and found to be 17.5%.

[0166] Example 2 A positive electrode plate was produced in the same manner as in Example 1, except that the positive electrode active material, flake graphite, conductive material, and binder were mixed in a weight ratio of 97.2:0.6:0.4:1.8, and the porosity of the positive electrode active material layer was measured. The porosity of the positive electrode active material layer was measured to be 19%.

[0167] Example 3 A positive electrode plate was manufactured in the same manner as in Example 1, except that the positive electrode active material, flake graphite, conductive material, and binder were mixed in a weight ratio of 97.4:0.4:0.4:1.8, and the porosity of the positive electrode active material layer was measured. The porosity of the positive electrode active material layer was measured to be 20%.

[0168] Example 4 A positive electrode plate was produced in the same manner as in Example 1, except that the positive electrode active material, flake graphite, conductive material, and binder were mixed in a weight ratio of 97.6:0.2:0.4:1.8, and the porosity of the positive electrode active material layer was measured. The porosity of the positive electrode active material layer was measured to be 21%.

[0169] Comparative Example 1 A positive electrode plate was manufactured in the same manner as in Example 1, except that no flake graphite was added and the positive electrode active material, conductive material, and binder were mixed in N-methylpyrrolidone in a weight ratio of 97.8:0.4:1.8 to prepare a positive electrode slurry, and the porosity of the positive electrode active material layer was measured. The porosity of the positive electrode active material layer was measured to be 24%.

[0170] Comparative Example 2 A positive electrode plate was manufactured in the same manner as in Example 1, except that no flake graphite was added, and the positive electrode active material, conductive material, and binder were mixed in N-methylpyrrolidone in a weight ratio of 97.8:0.4:1.8 to prepare a positive electrode slurry, which was then rolled at a voltage of 2.0 ton / cm, and the porosity of the positive electrode active material layer was measured. The porosity of the positive electrode active material layer was measured to be 30%.

[0171] Experimental Example 1 - Measurement of charge / discharge capacity and charge / discharge efficiency Coin half-cells including positive plates according to Examples 1 to 4 and Comparative Examples 1 and 2 were manufactured, and the charge capacity (mAh / g) and discharge capacity (mAh / g) of each coin half-cell were measured by charging the cells to 4.25 V at a current of 0.2 C and discharging the cells to 2.5 V at a current of 0.2 C. The measurement results are shown in Table 1 below.

[0172] [Table 1]

[0173] Referring to [Table 1], it can be seen that Examples 1 to 4, which use positive electrode plates containing added flake graphite, exhibit lower porosity and superior capacity characteristics compared to Comparative Examples 1 and 2.

[0174] Experimental example 2: Confirmation of resistance characteristics The resistance characteristics according to SOC were measured while charging the coin half-cells including the positive electrode plates according to Example 3, Comparative Example 1, and Comparative Example 2 up to 4.2 V. The measurement results are shown in FIG.

[0175] 8, it can be seen that the resistance value of Example 3, in which flake graphite was added to the positive electrode active material layer, based on an SOC of 10%, was lower than that of Comparative Examples 1 and 2, which did not contain flake graphite. This indicates that the addition of flake graphite to the positive electrode active material layer has the effect of improving the resistance characteristics at a low SOC.

[0176] Experimental Example 3: Measurement of high temperature life characteristics and resistance increase rate A separator was interposed between the positive and negative plates according to Example 1, Example 3, and Comparative Example 1, and the positive and negative plates were laminated in this order of separator / positive plate / separator / negative plate, and then rolled up to prepare a jelly roll type electrode assembly. The electrode assembly prepared as above was inserted into a cylindrical battery can, and an electrolyte was injected to prepare a 4680 cylindrical cell.

[0177] Here, the negative electrode plate was manufactured by mixing the negative active material (a mixture of graphite:SiO = 95:5 by weight), conductive material (super C), styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) in water in a weight ratio of 96:2:1.5:0.5 to prepare a negative electrode slurry, applying the negative electrode slurry to one side of a copper current collector sheet, drying it at 150°C, and rolling it.

[0178] The 4680 cell manufactured as described above was charged at 40° C. at 0.5 C to 4.2 V and then discharged at 0.5 C to 2.5 V, which is defined as one cycle, and then the charge / discharge cycle was repeated 50 times. The capacity retention and the DCIR increase were then measured. The measurement results are shown in FIG.

[0179] 9, in the case of the secondary batteries of Examples 1 and 3, the change in capacity retention rate due to the number of cycles is smaller than that in the secondary battery of Comparative Example 1, and the change in the resistance increase rate due to the number of cycles is also smaller. [Explanation of symbols]

[0180] 10 Positive electrode plate 11 Negative plate 12 Separator 20 Current collector 21, 21a Active material layer 22, 22a, 22c, 146b Plain part 24 insulating layer, 140, 170 batteries 141 Electrode assembly 142, 171 Battery can 143, 178 Sealed body 144 First current collecting plate 145, 176 Second current collecting plate 146 Insulating materials 152 Venting section 172 Rivet terminal 173 Second Gasket 147 Beading Section 148 Crimping section 149 Leads

Claims

1. A secondary battery comprising: an electrode assembly in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction; a battery can in which the electrode assembly is housed; and a sealing body that seals an open end of the battery can, The positive electrode plate includes a positive electrode active material layer, The positive electrode active material layer comprises a positive electrode active material including a single particle, a pseudo-single particle, or a combination thereof, and flake graphite.

2. 2. The lithium secondary battery according to claim 1, wherein the porosity of the positive electrode active material layer is 15% to 23%.

3. 2. The lithium secondary battery according to claim 1, wherein the positive electrode active material layer contains 0.05% by weight to 5% by weight of the flake graphite.

4. The lithium secondary battery according to claim 1 , wherein the positive electrode active material layer further comprises carbon nanotubes.

5. The loading amount of the positive electrode active material layer is 570 mg / 25 cm 2 The lithium secondary battery according to claim 1 .

6. D of the positive electrode active material min The lithium secondary battery according to claim 1 , wherein the average particle diameter is 1.0 μm or more.

7. The positive electrode active material is D 50 The lithium secondary battery according to claim 1 , wherein the thickness of the first electrode is 5 μm or less.

8. The positive electrode active material is D max The lithium secondary battery according to claim 1, wherein the average particle diameter is 12 μm to 17 μm.

9. The lithium secondary battery according to claim 1 , wherein the positive electrode active material has a particle size distribution (PSD) represented by the following formula (1) of 3 or less. Formula (1): Particle size distribution (PSD) = (D max -D min ) / D 50

10. The lithium secondary battery according to claim 1 , wherein the positive electrode active material has a unimodal particle size distribution that shows a single peak in a volume cumulative particle size distribution graph.

11. The lithium secondary battery according to claim 1, wherein the single particle, pseudo-single particle, or a combination thereof is contained in an amount of 95% by weight to 100% by weight based on the total weight of the positive electrode active material contained in the positive electrode plate.

12. 2. The lithium secondary battery according to claim 1, wherein the positive electrode active material contains a lithium nickel-based oxide containing 80 mol % or more of Ni with respect to the total number of moles of transition metals.

13. The lithium secondary battery according to claim 1 , wherein the positive electrode active material comprises a lithium nickel-based oxide represented by the following Chemical Formula 1: [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O 2 In the above Chemical Formula 1, M 1 is Mn, Al or a combination thereof, M 2 are Zr, W, Ti, Mg, Ca, Sr, and Ba, and 0.8≦a≦1.2, 0.83≦b<1, 0<c<0.17, 0<d<0.17, and 0≦e≦0.

1.

14. 2. The lithium secondary battery according to claim 1, wherein the positive electrode active material has an average primary particle size of 0.5 μm to 5 μm.

15. The lithium secondary battery according to claim 1 , wherein the negative electrode plate comprises a silicon-based negative electrode active material.

16. The lithium secondary battery according to claim 1 , wherein the negative electrode plate comprises a silicon-based negative electrode active material and a carbon-based negative electrode active material.

17. The lithium secondary battery according to claim 16, wherein the silicon-based negative electrode active material and the carbon-based negative electrode active material are contained in a weight ratio of 1:99 to 20:

80.

18. The lithium secondary battery according to claim 1 , wherein the lithium secondary battery is a cylindrical battery having a form factor ratio of 0.4 or more.

19. 20. The lithium secondary battery according to claim 18, wherein the cylindrical battery is a 46110 cell, a 4875 cell, a 48110 cell, a 4880 cell or a 4680 cell.

20. each of the positive electrode plate and the negative electrode plate includes a plain portion on which no active material layer is formed; 2. The lithium secondary battery according to claim 1, wherein at least a portion of the uncoated portion of the positive or negative electrode plate defines an electrode tab.

21. the positive plate uncoated portion and the negative plate uncoated portion are formed on one end of one side of the positive plate and the negative plate along a direction in which the electrode assembly is wound, A current collecting plate is coupled to each of the positive electrode uncoated portion and the negative electrode uncoated portion, The lithium secondary battery according to claim 20 , wherein the current collecting plate is connected to an electrode terminal.

22. The positive electrode plate uncoated portion and the negative electrode plate uncoated portion are processed into a plurality of segmented pieces that can be bent independently, The lithium secondary battery according to claim 21 , wherein at least some of the plurality of segment pieces are bent toward the winding center of the electrode assembly.

23. At least a portion of the folded segments overlaps an upper end and a lower end of the electrode assembly, 23. The lithium secondary battery according to claim 22, wherein the current collecting plates are bonded onto the overlapping segments.

24. The lithium secondary battery according to claim 20 , further comprising an insulating layer formed on the positive electrode plate in a direction parallel to the winding direction, the insulating layer covering a portion of the positive electrode active material layer and a portion of the uncoated portion.

25. A battery pack comprising the lithium secondary battery according to any one of claims 1 to 24.

26. 26. A motor vehicle comprising the battery pack of claim 25.

Citation Information

Patent Citations

  • Secondary battery, and battery module, battery pack, and device including same

    CN112563559A

  • Nonaqueous electrolyte secondary battery

    JP1997027344A

  • Positive electrode active material for lithium battery, manufacturing method for the active material, and secondary battery using it

    JP2002075367A

  • Positive electrode and nonaqueous electrolyte secondary battery

    JP2002083601A

  • Nonaqueous secondary battery and nonaqueous secondary battery system

    JP2010009898A

Cited By

  • Lithium secondary battery

    JP2026502007A

  • Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery

    WO2026205266A1