Rapid charging negative electrode active material and method for producing the same, negative electrode sheet, secondary battery, and power consumption device

A carbon-based negative electrode active material with a conductive carbon and ferroelectric coating layer addresses the limitations of graphite in secondary batteries, enabling rapid charging and maintaining high energy density by lowering kinetic barriers and improving ion transfer.

JP2024537572AActive Publication Date: 2024-10-11CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024521843
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-06-24
Publication Date
2024-10-11
Estimated Expiration
2042-06-24

AI Technical Summary

Technical Problem

Existing negative electrode active materials in secondary batteries, particularly graphite, face limitations in fast charging capacity, leading to issues such as increased kinetic energy barriers, lithium dendrite formation, and reduced energy density during rapid charging.

Method used

A fast-charging negative electrode active material is developed, comprising carbon-based material particles with a coating layer containing a conductive carbon material and dispersed ferroelectric material, which lowers kinetic energy barriers and enhances lithium ion transfer, allowing for high energy density and rapid charging capabilities.

Benefits of technology

The solution improves the rapid charging ability and cycle performance of secondary batteries without compromising their energy density, reducing lithium dendrite formation and enhancing ion transport and electron conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537572000001_ABST
    Figure 2024537572000001_ABST
Patent Text Reader

Abstract

The present application provides a rapid charging negative electrode active material and a method for preparing the same, a negative electrode sheet, a secondary battery, and a power consumption device. The rapid charging negative electrode active material includes carbon-based material particles, a coating layer located on at least a part of the surface of the carbon-based material particles, and a ferroelectric material dispersed in the coating layer, the coating layer including a conductive carbon material, and at least a part of the ferroelectric material protruding from the surface of the coating layer. The rapid charging negative electrode active material according to the present application has good dynamic performance, can withstand high charging rates, and improves the rapid charging ability of the secondary battery without impairing the high energy density of the secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the technical field of batteries, and in particular to a fast-charging negative electrode active material and a method for preparing the same, a negative electrode sheet, a secondary battery, and a power consuming device. [Background technology]

[0002] In recent years, secondary batteries have been widely used in many fields, such as energy storage power systems such as hydroelectric, thermal, wind and solar power plants, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. With the application and popularity of secondary batteries, the requirements for the fast charging ability of secondary batteries are becoming higher and higher, and the negative electrode active material, as an important component of secondary batteries, has a great influence on the charging ability of secondary batteries. At present, graphite is one of the most commonly used negative electrode active materials for secondary batteries, but the fast charging ability of conventional graphite has already approached a bottleneck and cannot meet the requirements for higher fast charging ability of secondary batteries. Summary of the Invention

[0003] The objective of the present application is to provide a rapid-charge negative electrode active material and a method for preparing the same, a negative electrode sheet, a secondary battery, and a power consumption device, which can significantly improve the rapid charging capability of a secondary battery on the premise that the secondary battery has a high energy density.

[0004] A first aspect of the present application provides a fast-charging negative electrode active material comprising: carbon-based material particles; a coating layer located on at least a portion of the surfaces of the carbon-based material particles; and a ferroelectric material dispersed in the coating layer, wherein the coating layer comprises a conductive carbon material, and at least a portion of the ferroelectric material protrudes from a surface of the coating layer.

[0005] The negative electrode active material of the present application, on the premise of containing a small amount of inactive components, can lower the kinetic energy barrier of the desolvation process, increase the speed at which lithium ions reach the surface of the carbon-based material particles, and reduce the insertion resistance of lithium ions into the negative electrode. The negative electrode active material of the present application can also increase the rate at which the lithium insertion product diffuses from the particle surface to the inside of the particles in a solid phase. Therefore, the negative electrode active material of the present application has good dynamic performance without compromising the high energy density of the secondary battery, can withstand high-power charging, and can improve the rapid charging ability of the secondary battery.

[0006] In any embodiment of the present application, the average thickness of the coating layer is H nm, and the volume average particle size Dv50 of the ferroelectric material is d 1 nm, and the fast charging negative electrode active material has a H / d 1 ≦1.1, preferably 0.25≦H / d 1 ≦0.5. This is advantageous for the secondary battery to have high fast charging capability, high energy density and good cycle performance at the same time.

[0007] In any embodiment of the present application, the volume average particle diameter Dv50 of the ferroelectric material is d 1 nm, 0 <d 1 ≦200, preferably 0 <d 1 ≦100. This allows less ferroelectric material to be used for the same specific surface area, thereby reducing the energy density loss of the secondary battery.

[0008] In any embodiment of the present application, the average thickness of the coating layer is H nm, and 20≦H≦100, preferably 20≦H≦50. This allows the secondary battery to simultaneously have a high rapid charging capability, a high energy density, and a high cycle capacity retention rate.

[0009] In any embodiment of the present application, the mass ratio of the ferroelectric material to the carbon-based material particles is α 1 and α 1is (0.5 to 10): 100, and preferably (1 to 3): 100. This is advantageous in that the secondary battery simultaneously has high rapid charging capability and high energy density.

[0010] In any embodiment of the present application, the mass ratio of the coating layer to the carbon-based material particles is α 2 and α 2 is (2-10):100, preferably (2 to 5):100. This is advantageous in that the negative electrode active material has high fast charging capability, high capacity per gram, high initial coulombic efficiency, and high compaction density.

[0011] In any embodiment of the present application, the mass ratio of the ferroelectric material to the carbon-based material particles is α 1 and the mass ratio of the coating layer to the carbon-based material particles is α 2 and α 1 :α 2 is 1:6 to 4:1, and preferably 1:4 to 2:1. This allows the secondary battery to have a high rapid charging capability, a high energy density, and a high cycle capacity retention rate at the same time.

[0012] In any embodiment of the present application, the coating layer has a graphitization degree of 45 to 80%.

[0013] In any embodiment of the present application, the conductive carbon material in the coating layer includes amorphous carbon, and preferably hard carbon, which can further improve the rapid charging capability of the secondary battery.

[0014] In any embodiment of the present application, the graphitization degree of the carbon-based material particles is 88% to 96%.

[0015] In any embodiment of the present application, the volume average particle diameter Dv50 of the carbon-based material particles is d 2 μm, 5≦d 2 ≦20, preferably 8≦d 2≦15. This allows the secondary battery to have a higher rapid charging capability.

[0016] In any embodiment of the present application, the carbon-based material particles are in the form of primary particles, secondary particles, or a combination thereof, and preferably, in the carbon-based material particles in the form of secondary particles, the ratio of the volume average particle diameter Dv50 of the primary particles to the volume average particle diameter Dv50 of the secondary particles formed therefrom is 0.2 to 0.5, which is advantageous in that the carbon-based material particles have good ion transport and electron transport performance as well as high structural stability.

[0017] In any embodiment of the present application, the carbon-based material particles include one or a combination of a plurality of types selected from graphite, mesocarbon microbeads, hard carbon, and soft carbon, and are preferably selected from graphite, which can provide the secondary battery with high energy density and high cycle stability.

[0018] In any embodiment of the present application, the dielectric constant of the ferroelectric material is greater than 100, and preferably between 100 and 100,000, which can better reduce the kinetic energy barrier in the desolvation process and improve the rapid charging ability of the secondary battery.

[0019] In any embodiment of the present application, the ferroelectric material has a Curie temperature of 80° C. or more, which can better reduce the kinetic energy barrier in the desolvation process and improve the fast charging ability of the secondary battery.

[0020] In any embodiment of the present application, the ferroelectric material includes one or a combination of a plurality of materials selected from a perovskite structure oxide, a tungsten bronze type compound, a bismuth oxide type layer structure compound, lithium niobate, and lithium tantalate.

[0021] In any embodiment of the present application, the volume average particle diameter Dv50 of the fast charging negative electrode active material is 5 μm to 20 μm, preferably 8 μm to 15 μm, which is advantageous for the negative electrode active material to have better ion transport and electron transport performance and fast charging performance.

[0022] In any embodiment of the present application, the specific surface area of ​​the fast charging negative electrode active material is 0.8 m 2 / g~1.3m 2 / g, preferably 0.9m 2 / g~1.2m 2 / g. This allows the secondary battery to have a higher rapid charging capability.

[0023] In any embodiment of the present application, the powder compression density of the fast charging negative electrode active material at an applied force of 20000 N is 1.5 g / cm 3 ~1.9g / cm 3 and preferably 1.5 g / cm 3 ~1.7g / cm 3 This allows the secondary battery to have high energy density and improved cycle performance.

[0024] A second aspect of the present application provides a method for preparing a rapid-charging negative electrode active material, the method including: step S10 of supplying carbon-based material particles, a carbon source, and a ferroelectric material, preferably the carbon source including one or a combination of a plurality of types selected from asphalt, resin, and biomass material; and step S20 of uniformly mixing the carbon-based material particles, the carbon source, and the ferroelectric material, and forming a coating layer including a conductive carbon material on at least a portion of the surface of the carbon-based material particles by a carbonization sintering treatment, the ferroelectric material being dispersed in the coating layer, and at least a portion of the ferroelectric material protruding from the surface of the coating layer.

[0025] In any embodiment of the present application, the carbonization sintering temperature in S20 is 700°C to 1800°C, and preferably 1000°C to 1300°C.

[0026] In any embodiment of the present application, the carbonization sintering time in S20 is 1 h to 15 h, preferably 6 h to 14 h.

[0027] In any embodiment of the present application, the carbon-based material particles are prepared by a method including: S101 supplying coke powder and placing the coke powder in a reaction vessel; and S102 graphitizing the coke powder to obtain carbon-based material particles.

[0028] A third aspect of the present application provides a negative electrode sheet including a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, the negative electrode film layer including the fast-charging negative electrode active material of the first aspect of the present application or the fast-charging negative electrode active material produced by the method of the second aspect of the present application.

[0029] A fourth aspect of the present application provides a secondary battery including the negative electrode sheet of the third aspect of the present application.

[0030] A fifth aspect of the present application provides a power consuming device including the secondary battery of the fourth aspect of the present application.

[0031] The fast-charging negative electrode active material of the present application has good dynamic performance, can withstand high charging rates, and can improve the fast-charging ability of the secondary battery without compromising the high energy density of the secondary battery. The power consumption device of the present application includes the secondary battery of the present application, and thus has at least the same advantages as the secondary battery. [Brief description of the drawings]

[0032] In order to more clearly explain the technical solutions of the embodiments of the present application, the following briefly introduces drawings required in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can also obtain other drawings based on the drawings without any creative efforts. [Figure 1] FIG. 1 is a schematic diagram of one embodiment of a fast-charging negative electrode active material of the present application. [Diagram 2]FIG. 1 is a schematic diagram of one embodiment of a secondary battery of the present application. [Diagram 3] 3 is an exploded schematic view of the embodiment of the secondary battery of FIG. 2. [Figure 4] FIG. 1 is a schematic diagram of one embodiment of a battery module of the present application. [Diagram 5] FIG. 1 is a schematic diagram of one embodiment of a battery pack of the present application. [Figure 6] 6 is an exploded schematic view of the embodiment of the battery pack shown in FIG. 5. [Figure 7] 1 is a schematic diagram of one embodiment of a power consuming device including a secondary battery of the present application as a power source.

[0033] In the drawings, the drawings are not necessarily drawn to scale.

[0034] The symbols are explained as follows: 1 Battery pack 2 Upper case 3 Lower housing 4 Battery Module 5 Secondary battery 51 cases 52 Electrode Assembly 53 Cover plate 10 Fast charging negative electrode active material 101 Carbon-based material particles 102 Covering layer 103 Ferroelectric Materials DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] Hereinafter, the embodiments specifically disclosing the fast charging negative electrode active material and its preparation method, the negative electrode sheet, the secondary battery, and the power consumption device of the present application will be described in detail with reference to the drawings as appropriate. However, unnecessary detailed description may be omitted. For example, detailed description of already well-known matters and duplicated description of substantially the same configuration may be omitted. This is to avoid the following description becoming unnecessarily redundant and to facilitate understanding by those skilled in the art. Note that the attached drawings and the following description are provided to enable those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.

[0036] The "ranges" disclosed herein are defined in the form of lower and upper limits, where a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits specifically define the boundaries of the range. Ranges defined in this manner may or may not include the endpoints and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, by reciting ranges of 60-120 and 80-110 for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also contemplated. Also, by reciting minimum range values ​​1 and 2 and maximum range values ​​3, 4 and 5, the ranges 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5 are all contemplated. In this application, unless otherwise stated, a numerical range "a-b" refers to a contraction of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0 to 5" indicates that all real numbers between "0 and 5" are listed herein, and "0 to 5" is a contraction of combinations of these numerical values. In addition, when a parameter is expressed as an integer ≧2, this is equivalent to disclosing that the parameter is an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0037] Unless otherwise stated, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure content of the present application.

[0038] Unless otherwise stated, all technical features and optional technical features of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure content of the present application.

[0039] Unless otherwise stated, all steps in the present application may be performed in sequence, may be performed randomly, and are preferably performed in sequence. For example, when the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed in sequence, or may include steps (b) and (a) performed in sequence. For example, when the method may further include step (c), it means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b), and (c), may include steps (a), (c), and (b), and may further include steps (c), (a), and (b), etc.

[0040] Unless otherwise specified, the terms "comprise" and "include" referred to in this application may be open-ended or closed-ended. For example, the terms "comprise" and "include" indicate that the term may comprise or include other components not further recited, or may comprise or include only the recited components.

[0041] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, any of the following conditions satisfy the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), or A and B are both true (or exist).

[0042] As used herein, the terms "plurality" and "multiple types" refer to two or more than two types.

[0043] In this application, the use of "about" a certain numerical value indicates a range, indicating that the numerical value falls within a range of ±10%.

[0044] The key to improving the fast charging ability of secondary batteries is to improve the performance of the negative electrode active material and the negative electrode sheet. In the charging process of secondary batteries, taking graphite as an example, the electrode kinetics process usually includes several steps: (1) Liquid phase mass transfer step in the electrolyte phase: The solvated lithium ions in the electrolyte are diffused and transferred to the graphite particle surface. (2) Surface conversion step: During the first charge, the solvated lithium ions are adsorbed on the graphite particle surface and react to form a solid electrolyte interface (SEI) film, and during the subsequent charge process, the solvated lithium ions are adsorbed on the SEI film surface, and the lithium ions reach the graphite particle surface through a desolvation process. (3) Charge exchange step: The lithium ions obtain electrons from the graphite particle surface to form lithium insertion products. (4) Lithium insertion product solid phase mass transfer step: The lithium insertion product diffuses in the solid phase from the graphite particle surface to the inside, completing the charging process.

[0045] In the conventional research, the solid-phase diffusion rate of the lithium intercalation product is considered to be relatively slow, so the above step (4) is a step for controlling the dynamic process of the negative electrode, and further, the conventional research is considered to have mainly focused on how to increase the solid-phase diffusion rate of the lithium intercalation product and how to shorten the solid-phase diffusion distance. For example, in order to improve the fast charging ability of graphite, the conventional technology mainly uses a method including (1) etching voids on the graphite surface to increase the surface active sites and the intercalation paths of lithium ions, thereby shortening the lithium ion diffusion distance, and (2) coating the graphite with amorphous carbon to increase the layer spacing of the graphite surface layer and increase the diffusion rate of lithium ions. However, the above method has a limited effect on improving the fast charging ability of secondary batteries.

[0046] The inventors of the present application have studied the electrode dynamics process during charging of a secondary battery in detail and found that one important factor affecting the improvement of the fast charging ability of graphite is the effect of electrolyte solvation. An electrolyte is usually obtained by uniformly mixing a lithium salt and a solvent molecule, and thus the electrolyte usually contains three components: a solvent molecule, an anion, and a solvated lithium ion. Before the lithium ion reaches the graphite particle surface and is inserted into the graphite particle during the charging process, the solvated lithium ion needs to go through a desolvation process to release the solvent molecule, and in this process there is a high kinetic energy barrier, for example about 50 kJ / mol to 70 kJ / mol.

[0047] In addition, the occurrence of "lithium dendrites" and "dead lithium" is another important factor that affects the improvement of the rapid charging ability of secondary batteries. During the charging process of secondary batteries, if the lithium insertion space of the negative electrode is insufficient, the insertion resistance of lithium ions into the negative electrode is too large, and lithium ions are too quickly removed from the positive electrode but cannot be inserted into the negative electrode in equal amounts, the lithium ions that are not inserted into the negative electrode can only obtain electrons on the surface of the negative electrode, and silver-white metallic lithium elements, i.e., "lithium dendrites", are formed. The formation of lithium dendrites not only reduces the performance of secondary batteries, such as shortening the cycle life, but also forms sharp shapes in severe cases, piercing the separator and shorting the inside of the secondary battery, which can cause catastrophic results such as combustion and explosion. At the same time, the metallic lithium elements that are constantly accumulating fall off the surface of the negative electrode, forming "dead lithium" that cannot participate in the reaction, which reduces the energy density of the secondary battery.

[0048] As a result of studying the electrode dynamics process during charging of a secondary battery, the inventors of the present application further discovered that the presence of a high kinetic energy barrier in the desolvation process limits the speed at which lithium ions reach the graphite particle surface, increases the insertion resistance of lithium ions into the negative electrode, and is particularly likely to induce "lithium dendrites" and "dead lithium" when the secondary battery is rapidly charged at a large rate.

[0049] Through extensive research, the inventors of the present application have proposed a new type of fast-charging negative electrode active material that can greatly improve the fast charging capability of secondary batteries on the premise that they have high energy density. negative electrode active material

[0050] Specifically, a first aspect of an embodiment of the present application provides a fast-rechargeable negative electrode active material.

[0051] The fast-charging negative electrode active material includes carbon-based material particles, a coating layer located on at least a portion of the surfaces of the carbon-based material particles, and a ferroelectric material dispersed in the coating layer, the coating layer including a conductive carbon material, and at least a portion of the ferroelectric material protruding from a surface of the coating layer.

[0052] The negative electrode active material of the present application has good dynamic performance without compromising the high energy density of the secondary battery, and can improve the fast charging ability of the secondary battery. Although the mechanism is unclear, the following points are considered as possible causes.

[0053] First, the negative electrode active material of the present application has a ferroelectric material with spontaneous polarization strength on the surface, and the spontaneous polarization strength is reversed when the external electric field is reversed, thereby reducing the kinetic energy barrier in the desolvation process of solvated lithium ions, accelerating the speed at which lithium ions reach the surface of carbonaceous material particles, and reducing the insertion resistance of lithium ions into the negative electrode. As a result, the negative electrode active material of the present application has good dynamic performance, can withstand high-power charging, and can improve the rapid charging ability of secondary batteries.

[0054] Secondly, in the negative electrode active material of the present application, at least a part of the ferroelectric material protrudes from the surface of the coating layer, so that the part of the ferroelectric material can contact the carbon-based material particles while directly contacting the electrolyte. The surface of the ferroelectric material that contacts the electrolyte is negatively induced, and the surface that contacts the carbon-based material particles is positively induced, so that the kinetic energy barrier of the desolvation process can be better reduced, the speed at which the lithium ions reach the surface of the carbon-based material particles can be increased, and the insertion resistance of the lithium ions into the negative electrode can be reduced, so that the negative electrode active material of the present application has good dynamic performance, can withstand high-power charging, and can improve the rapid charging ability of the secondary battery.

[0055] Thirdly, as the charging process progresses, the amount of lithium inserted into the negative electrode gradually increases, and the activation energy that needs to be overcome when the lithium insertion product diffuses from the particle surface to the inside of the particle increases, making the solid-state diffusion more difficult. In the negative electrode active material of the present application, the coating layer includes a conductive carbon material with good conductivity, which can increase the rate at which the lithium insertion product diffuses from the particle surface to the inside of the particle, and provide the negative electrode active material with good dynamic performance.

[0056] Fourth, in the negative electrode active material of the present application, the conductive carbon material and the carbon-based material particles in the coating layer are both active components and can contribute to the capacity, while the ferroelectric material is an inactive component and cannot contribute to the capacity, but it can lower the kinetic energy barrier in the desolvation process, increase the speed at which lithium ions reach the surface of the carbon-based material particles, and reduce the insertion resistance of lithium ions into the negative electrode. In the negative electrode active material of the present application, the ferroelectric material is dispersed in the coating layer, and at least a part of the ferroelectric material is protruded from the surface of the coating layer, thereby increasing the exposed surface area of ​​the ferroelectric material, increasing the contact area with the electrolyte, and reducing the kinetic energy barrier in the desolvation process when the amount of use is small. Therefore, the secondary battery using the negative electrode active material of the present application has a high rapid charging ability and does not lose its high energy density.

[0057] The negative electrode active material of the present application, on the premise of containing a small amount of inactive components, can lower the kinetic energy barrier of the desolvation process, increase the speed at which lithium ions reach the surface of the carbon-based material particles, and reduce the insertion resistance of lithium ions into the negative electrode. The negative electrode active material of the present application can also increase the rate at which the lithium insertion product diffuses from the particle surface to the inside of the particles in a solid phase. Therefore, the negative electrode active material of the present application has good dynamic performance without compromising the high energy density of the secondary battery, can withstand high-power charging, and can improve the rapid charging ability of the secondary battery.

[0058] In some embodiments, preferably, all of the ferroelectric material protrudes from the surface of the coating layer, which increases the exposed surface area of ​​the ferroelectric material, increases the contact area with the electrolyte, and reduces the kinetic energy barrier of the desolvation process when used in smaller amounts.

[0059] In some embodiments, the average thickness of the coating layer is H nm, and the volume average particle size Dv50 of the ferroelectric material is d 1 nm, and the fast charging negative electrode active material has a H / d 1 H / d≦1.1 1 When H / d is less than 1.1, at least a part of the ferroelectric material can be protruded from the surface of the coating layer, which increases the contact area with the electrolyte and reduces the kinetic energy barrier in the desolvation process when the amount of electrolyte used is small. 1 If H / d is less than 0.25, the contact area between the ferroelectric material and the electrolyte is large, and the effect of lowering the kinetic energy barrier in the desolvation process can be better achieved. However, in this case, the entire negative electrode active material is difficult to compact, and the ion conduction ability and electron conduction ability of the negative electrode sheet are deteriorated, which may affect the rapid charging ability, energy density and cycle performance of the secondary battery. Therefore, 1 When H / d is within an appropriate range, it is advantageous for the secondary battery to have high rapid charging capability, high energy density, and good cycle performance at the same time. 1≦1.0, 0.25≦H / d 1 ≦0.9, 0.25≦H / d 1 ≦0.8, 0.25≦H / d 1 ≦0.7, 0.25≦H / d 1 ≦0.6, 0.25≦H / d 1 ≦0.5, 0.25≦H / d 1 ≦0.4, 0.30≦H / d 1 ≦0.9, 0.30≦H / d 1 ≦0.8, 0.30≦H / d 1 ≦0.7, 0.30≦H / d 1 ≦0.6, 0.30≦H / d 1 ≦0.5, 0.30≦H / d 1 ≦0.4, 0.35≦H / d 1 ≦0.9, 0.35≦H / d 1 ≦0.8, 0.35≦H / d 1 ≦0.7, 0.35≦H / d 1 ≦0.6 or 0.35≦H / d 1 ≦0.5.

[0060] In some embodiments, the volume average particle size Dv50 of the ferroelectric material is d 1 nm, 0 <d 1 ≦200. Preferably, 0 <d 1 ≦180, 0 <d 1 <= 160, 0 <d 1 <= 140, 0 <d 1 <= 120, 0 <d 1 <= 100, 0 <d 1 ≦80, 0 <d 1 ≦60, 0 <d 1 ≦40, 20≦d 1 ≦180, 20≦d 1 ≦160, 20≦d 1 ≦140, 20≦d 1 ≦120, 20≦d 1 ≦100, 20≦d 1 ≦80, 20≦d 1 ≦60, 20≦d 1 ≦40, 30≦d 1 ≦180, 30≦d 1 ≦160, 30≦d 1 ≦140, 30≦d 1≦120, 30≦d 1 ≦100, 30≦d 1 ≦80 or ≦30 d 1 ≦60. The smaller the volume average particle diameter Dv50 of the ferroelectric material, the larger the specific surface area, so that less ferroelectric material can be used with the same specific surface area, and the energy density loss of the secondary battery can be reduced.

[0061] In some embodiments, the average thickness of the coating layer is H nm, and 20≦H≦100. The coating layer contains a conductive carbon material with good conductivity, which increases the rate of solid-phase diffusion of lithium insertion products from the particle surface to the inside, and allows the negative electrode active material to have good dynamic performance. Therefore, when the coating layer is thick, the rapid charging ability of the secondary battery can be improved, but because the conductive carbon material in the coating layer has many voids, many surface defects, and a large specific surface area, when the coating layer is thick, there are many interfacial side reactions between the negative electrode active material and the electrolyte, the initial coulombic efficiency of the negative electrode active material is low, and the capacity decay is fast. Therefore, when the average thickness of the coating layer is within an appropriate range, it is advantageous for the negative electrode active material to have a high rapid charging ability, a high capacity per gram, and a high initial coulombic efficiency, and further, the secondary battery can have a high rapid charging ability, a high energy density, and a high cycle capacity retention rate at the same time. Preferably, 20≦H≦95, 20≦H≦90, 20≦H≦85, 20≦H≦80, 20≦H≦75, 20≦H≦70, 20≦H≦65, 20≦H≦60, 20≦H≦55, 20≦H≦50, 20≦H≦45, or 20≦H≦40.

[0062] In some embodiments, the dielectric constant of the ferroelectric material is preferably 100 or more. When the ferroelectric material has a high dielectric constant, its surface can provide a new route for the desolvation process of solvated lithium ions, and the higher the dielectric constant of the ferroelectric material, the better the effect of reducing the kinetic energy barrier in the desolvation process, but the effect is not always increasing. At the same time, the higher the dielectric constant, the higher the requirements for the fabrication process of the ferroelectric material, which increases the production cost. In some embodiments, the dielectric constant of the ferroelectric material is preferably 100 to 100,000, for example, 100 to 50,000, 100 to 25,000, 100 to 10,000, 100 to 5,000, 100 to 4,000, 100 to 3,000, 100 to 2,000, 100 to 1,000, 100 to 500, 150 to 50,000, 150 to 25 000, 150-10000, 150-5000, 150-4000, 150-3000, 150-2000, 150-1000, 150-500, 200-50000, 200-25000, 200-10000, 200-5000, 200-4000, 200-3000, 200-2000, or 200-1000.

[0063] In this application, the dielectric constant of a ferroelectric material refers to the dielectric constant at room temperature (25±5°C), and has a meaning known in the art, and can be tested by devices and methods known in the art. For example, after preparing a circular sample of the ferroelectric material, the capacitance C is tested using an LCR meter, and the dielectric constant ε=(C×d) / (ε 0 × A), where C is the capacitance in farads (F), d is the thickness of the sample in cm, and A is the area of ​​the sample in cm. 2 and ε 0 denotes the vacuum dielectric constant, and ε 0 =8.854×10 -14F / cm. In this application, the test conditions may be 1KHz, 1.0V, 25±5℃. The test standard may be in accordance with GB / T11297.11-2015. When preparing the sample, reference may be made to Chinese patent application CN114217139A.

[0064] In some embodiments, the dielectric constant of the ferroelectric material is preferably higher than that of the electrolyte, so as to better reduce the kinetic energy barrier of the desolvation process and improve the fast charging capability of the secondary battery.

[0065] In some embodiments, the ferroelectric material is insoluble in water and has a high Curie temperature, typically above 80° C., so that the effect of the ferroelectric material can be better exerted during the use of the secondary battery.

[0066] In some embodiments, the ferroelectric material is preferably a perovskite structure oxide, a tungsten bronze type compound, a bismuth oxide type layer structure compound, or lithium niobate (LiNbO 3 ) and lithium tantalate (LiTaO 3 ) More preferably, the ferroelectric material is selected from perovskite structure oxides.

[0067] Preferably, the perovskite oxide has the molecular formula Ba 1-x A x Ti 1-y B y O 3 A includes one or a combination of elements selected from Pb, Sr, Ca, K, Na, and Cd, and B includes one or a combination of elements selected from Sn, Hf, Zr, Ce, Nb, and Th, and 0≦x≦1, 0≦y≦1. For example, the perovskite oxide is BaTiO 3 , B.A. 1-x1 Sr x1 TiO 3 (0≦x1≦1), SrTiO 3 , PbTiO3 , PbZr y1 Ti 1-y1 O 3 (0 ≦ y1 ≦ 1), BaZr y2 Ti 1-y2 O 3 (0 < y2 < 1), KNbO 3 , NaNbO 3 and may contain one or more combinations selected therefrom.

[0068] Further, the tungsten bronze type compound may have the molecular formula M z WO 3 . M contains one or more combinations selected from Na, K, Rb, and Cs, and 0 < z < 1. For example, the tungsten bronze type compound may contain one or more combinations selected from Na z1 WO 3 (0 < z1 < 1), K z2 WO 3 (0 < z2 < 1).

[0069] Preferably, the bismuth oxide type layered structure compound has the molecular formula (Bi 2 O 2 )(C n-1 D n O 3n+1 ). C contains one or more combinations selected from Na, K, Ba, Sr, Pb, Ca, Ln, and Bi, D contains one or more combinations selected from Zr, Cr, Nb, Ta, Mo, W, Fe, Ti, and V, and 2 ≦ n ≦ 5. For example, the bismuth oxide type layered structure compound may be one or more combinations of SrBi 2 Nb 2 O 9 , SrBi 2 Ta 2 O 9 , SrBi 2 Nb 2 O 9 , Bi 4 Ti 3 O 12 .

[0070] In some embodiments, the mass ratio of the ferroelectric material to the carbon-based material particles is α 1 and α 1 is (0.5 to 10):100. Preferably, α 1 are (0.5~9):100, (0.5~8):100, (0.5~7):100, (0.5~6):100, (0.5~5):100, (0.5~4):100, (0.5~3):100, (1~9):100, (1~8):100, (1~7):100, (1~6):100, (1~5):100, (1~4):100 or (1~3):100.

[0071] α 1 When α is within an appropriate range, it is advantageous for the secondary battery to have high rapid charging capability and high energy density at the same time. Furthermore, the following situation can be effectively avoided. 1 When α is large, the content of inactive components in the negative electrode active material particles increases and the content of active components decreases, which can impair the energy density of the secondary battery. 1 When α is large, the ferroelectric material covers many surfaces of the negative electrode active material, which may reduce the surface active sites of the negative electrode active material and deteriorate the fast charging capability and cycle performance of the secondary battery. 1 When the content of the ferroelectric material is small, the effect of lowering the kinetic energy barrier in the desolvation process is not obvious, which is disadvantageous to improving the rapid charging ability of the secondary battery.

[0072] In some embodiments, the mass ratio of the coating layer to the carbon-based material particles is α 2 and α 2 is (2-10):100. Preferably, α 2 is (2~9):100, (2~8):100, (2~7):100, (2~6):100, (2~5):100, (3~9):100, (3~8):100, (3~7):100, (3~6):100 or (3~5):100.

[0073] α 2When is within an appropriate range, the negative electrode active material has a high fast charging ability, a high capacity per gram, a high initial coulombic efficiency, and a high compression density, and the secondary battery has a high fast charging ability, a high energy density, and a high cycle capacity retention rate at the same time. Furthermore, the following situation can be effectively avoided. 2 When α is large, the coating layer is thick, the content of conductive carbon material is high, the conductive carbon material has many voids, and the specific surface area is large, so there are many interfacial side reactions between the negative electrode active material and the electrolyte. At the same time, 2 When α is large, the surface morphology of the conductive carbon material is rough and there are many surface defects, which makes it difficult to compact the negative electrode active material, and the surface defect structure of the conductive carbon material is unstable, which results in low initial Coulomb efficiency of the negative electrode active material, rapid capacity decay, and poor capacity development and cycle performance of the secondary battery. 2 If the value is small, it is disadvantageous for rapid insertion and desorption of lithium ions, and is disadvantageous for improving the rapid charging ability of the secondary battery.

[0074] In some embodiments, the mass ratio of the ferroelectric material to the carbon-based material particles is α 1 and the mass ratio of the coating layer to the carbon-based material particles is α 2 and α 1 :α 2 is between 1:6 and 4:1, preferably between 1:4 and 2:1.

[0075] α 1 :α 2 When is within an appropriate range, the negative electrode active material has a high fast charging ability, a high capacity per gram, a high initial coulombic efficiency, and a high compression density, and the secondary battery has a high fast charging ability, a high energy density, and a high cycle capacity retention rate at the same time. Furthermore, the following situation can be effectively avoided. 1 :α 2 When α is large, the content of inactive components in the negative electrode active material particles increases, and the content of active components decreases, which causes a large loss of energy density in the secondary battery and is unfavorable to the rapid insertion and desorption of lithium ions.1 :α 2 When the amount of the ferroelectric material is small, the content of the ferroelectric material is small, and the effect of reducing the kinetic energy barrier of the desolvation process is not obvious, which deteriorates the fast charging ability of the secondary battery, and at the same time, the initial Coulombic efficiency of the negative electrode active material is low, and the capacity fade is easily accelerated.

[0076] The coating layer includes a conductive carbon material. Preferably, the conductive carbon material includes amorphous carbon. Amorphous carbon is a carbon material with low graphitization crystallinity and in a transition state close to an amorphous form (or amorphous and periodic structural order), which is obtained by carbonization and sintering with a carbon source (e.g., asphalt, resin, biomass material, etc.). The layer spacing of amorphous carbon is large, and does not cause volume shrinkage and expansion effects during the process of lithium ion desorption and insertion, so that the crystal structure is more stable, and the negative electrode active material has good dynamic performance, can withstand high-power charging, and can improve the rapid charging ability of the secondary battery. The amorphous carbon includes soft carbon, hard carbon, or a combination thereof. Preferably, in some embodiments, the conductive carbon material includes hard carbon, which can further improve the rapid charging ability of the secondary battery.

[0077] In some embodiments, the carbon-based material particles include one or more combinations selected from graphite (e.g., artificial graphite, natural graphite, graphite oxide, etc.), mesocarbon microbeads, hard carbon, and soft carbon, and are preferably selected from graphite. Graphite has the advantages of stable cycle performance and high capacity per gram, which can provide the secondary battery with high energy density and high cycle stability.

[0078] In some embodiments, the coating layer has a graphitization degree of 45-80%.

[0079] In some embodiments, the carbon-based material particles have a degree of graphitization of 88% to 96%.

[0080] Through research, the inventors have discovered that when the coating layer and the carbon-based material particles further satisfy the requirement that the graphitization degree is within the above range, this contributes to a rational matching of the crystal structures of the coating layer and the carbon-based material particles, thereby effectively improving the solid-phase diffusion rate of lithium ions and improving the fast charging capability and cycle performance of the secondary battery.

[0081] In some embodiments, the carbon-based material particles are in the form of primary particles, secondary particles, or a combination thereof. Secondary particles are usually obtained by agglomeration of primary particles. Preferably, in the carbon-based material particles in the form of secondary particles, the ratio of the volume average particle diameter Dv50 of the primary particles to the volume average particle diameter Dv50 of the secondary particles is 0.2 to 0.5. When the carbon-based material particles are in the form of secondary particles and the ratio of the volume average particle diameter Dv50 of the primary particles to the volume average particle diameter Dv50 of the secondary particles is adjusted within an appropriate range, it is advantageous for the carbon-based material particles to have a good secondary particle size, and the carbon-based material particles can have high structural stability while having good ion transport and electron transport performance.

[0082] In some embodiments, the volume average particle size Dv50 of the carbon-based material particles is d 2 μm, 5≦d 2 ≦20, preferably 8≦d 2≦15. When the volume average particle diameter Dv50 of the carbon-based material particles is within an appropriate range, it is advantageous for the negative electrode active material of the present application to have high electrochemical activity, which allows the secondary battery to have a higher rapid charging ability. In addition, the following situation can be effectively avoided. When the volume average particle diameter Dv50 of the carbon-based material particles is small, the capacity per gram of the negative electrode active material is low and the compressed density is low, which is disadvantageous for designing a battery with a high energy density. When the volume average particle diameter Dv50 of the carbon-based material particles is small, the specific surface area is large and the reaction activity is high, which increases the interfacial side reaction between the negative electrode active material and the electrolyte, and further increases the irreversible consumption of active lithium ions, which may deteriorate the capacity and energy density of the secondary battery. When the volume average particle diameter Dv50 of the carbon-based material particles is large, the surface active sites on the particle surface are reduced, and the path for the lithium insertion product to diffuse into the solid phase from the particle surface to the inside is lengthened, which is disadvantageous for improving the rapid charging ability of the secondary battery.

[0083] In some embodiments, the volume average particle diameter Dv50 of the fast charging negative electrode active material is 5 μm to 20 μm, preferably 8 μm to 15 μm. By adjusting the volume average particle diameter Dv50 of the negative electrode active material within a suitable range, it is advantageous for the negative electrode active material to have better ion transport and electron transport performance and fast charging performance, and to have high powder compaction density.

[0084] In some embodiments, the specific surface area of ​​the fast charging negative electrode active material is 0.8 m 2 / g~1.3m 2 / g, preferably 0.9m 2 / g~1.2m 2 By adjusting the specific surface area of ​​the negative electrode active material within an appropriate range, it is possible to reduce the interfacial side reaction between the negative electrode sheet using the material and the electrolyte, and to impart an appropriate electrochemical reaction activity to the negative electrode sheet using the material, thereby enabling the secondary battery to have a higher rapid charging capability.

[0085] In some embodiments, the powder compression density of the fast charging negative electrode active material at an applied force of 20000 N is 1.5 g / cm 3 ~1.9g / cm 3 and preferably 1.5 g / cm 3 ~1.7g / cm 3 By adjusting the compressed density of the powder of the negative electrode active material within a suitable range, the negative electrode film layer has a high compressed density, and the secondary battery has a high energy density. In addition, by adjusting the compressed density of the powder of the negative electrode active material within a suitable range, the negative electrode film layer has the ability to maintain a strong channel structure during the cycle process, which improves the wettability of the electrolyte of the negative electrode sheet, and can better improve the cycle performance of the secondary battery.

[0086] In the present application, the average thickness of the coating layer has a meaning known in the art, and can be tested using equipment and methods known in the art; for example, a TEM (Transmission Electron Microscope) picture can be obtained using a transmission electron microscope, and then the thicknesses of multiple (e.g., 30 or more) different positions in the TEM picture can be measured, and the average value can be taken as the average thickness of the coating layer.

[0087] In this application, the volume average particle size Dv50 of a material has a meaning known in the art, and indicates the particle size corresponding to the material cumulative volume distribution percentage reaching 50%, and can be tested by instruments and methods known in the art, for example, GB / T19077-2016 Particle Size Distribution Laser Diffraction Method, and can be easily tested by using a laser particle size analyzer, for example, the Mastersizer2000E type laser particle size analyzer of Malvern Company, UK.

[0088] In the present application, the graphitization degree of a material has a meaning known in the art and can be tested by an apparatus and method known in the art. For example, the graphitization degree of a material can be tested by using an X-ray diffractometer (e.g., Bruker D8 Discover) with reference to JIS K0131-1996 and JB / T4220-2011. 002After obtaining the formula g=(0.344-d 002 The graphitization degree of the material was calculated from d / (0.344-0.3354)×100%. 002 is the layer spacing of the (002) crystal plane in the crystal structure of the material, expressed in nanometers (nm).

[0089] In this application, the specific surface area of ​​a material has a meaning known in the art, and can be tested using instruments and methods known in the art. For example, the nitrogen adsorption specific surface area analysis test method can be used with reference to GB / T19587-2017, and the nitrogen adsorption specific surface area analysis test can be calculated by the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis test can be performed by a Tri-Star3020 type specific surface area pore size analysis tester manufactured by Micromeritics, USA.

[0090] In this application, the powder compaction density of a material has a meaning known in the art and can be tested by equipment and methods known in the art, for example, by an electronic pressure test machine (e.g., UTM7305 type) with reference to standard GB / T24533-2009. One exemplary test method is to weigh 1 g of material and measure the surface area of ​​the material to be 1.327 cm2. 2 The method includes the steps of placing the powder in a mold, pressurizing the powder to 2000 kg (equivalent to 20,000 N), holding the pressure for 30 seconds, releasing the pressure, holding for 10 s, and then recording and calculating the compressed density of the powder at the applied force of 20,000 N of the material.

[0091] In addition, the above-mentioned tests for various parameters of the negative electrode active material may be performed by sampling before coating, or by sampling from the negative electrode film layer after cold pressing. When the test sample of the negative electrode active material is sampled from the negative electrode film layer after cold pressing, the sampling can be performed, for example, by the following steps. The negative electrode film layer after cold pressing is arbitrarily selected, and the negative electrode active material is sampled (for example, the powder may be scraped off using a blade for sampling). The collected negative electrode active material powder is put into deionized water, and then suction filtered and dried. The dried negative electrode active material is sintered at a certain temperature and time (for example, 400 ° C, 2 h) to remove the adhesive and conductive agent, and a test sample of the negative electrode active material is obtained.

[0092] Hereinafter, the fast charging negative electrode active material of the present application will be described with reference to the drawings. FIG. 1 is a schematic diagram of one embodiment of the fast charging negative electrode active material 10 of the present application. As shown in FIG. 1, the fast charging negative electrode active material 10 includes carbon-based material particles 101, a coating layer 102 located on at least a part of the surface of the carbon-based material particles 101, and a ferroelectric material 103 dispersed in the coating layer 102, the coating layer 102 includes a conductive carbon material, and at least a part of the ferroelectric material 103 protrudes from the surface of the coating layer 102. Method of preparation

[0093] A second aspect of the embodiment of the present application provides a method for preparing a fast-charging negative electrode active material of the first aspect of the present application, the method including: a step S10 of supplying carbon-based material particles, a carbon source, and a ferroelectric material; and a step S20 of uniformly mixing the carbon-based material particles, the carbon source, and the ferroelectric material, and forming a coating layer containing a conductive carbon material on at least a part of the surface of the carbon-based material particles by a carbonization sintering process, wherein the ferroelectric material is dispersed in the coating layer, and at least a part of the ferroelectric material protrudes from the surface of the coating layer.

[0094] In the present application, the term "carbon source" refers to a compound capable of forming a conductive carbon material. The carbon source includes one or a combination of organic carbon sources and inorganic carbon sources. Preferably, the carbon source is an organic carbon source.

[0095] In some embodiments, the carbon source preferably includes one or more combinations selected from asphalt, resin, and biomass material. For example, the asphalt includes one or more combinations selected from coal asphalt and petroleum asphalt, and is preferably petroleum asphalt. For example, the resin includes one or more combinations selected from phenolic resin and epoxy resin. For example, the biomass material refers to a material derived from a living organism such as an animal, a plant, or a microorganism, and is mainly composed of organic polymeric substances, and mainly consists of three elements, carbon, hydrogen, and oxygen, in its chemical composition, and may be, for example, a polysaccharide (e.g., starch, sucrose polymer, glucose polymer, cellulose, etc.).

[0096] In some embodiments, the carbonization sintering temperature in S20 is preferably 700°C to 1800°C, more preferably 1000°C to 1300°C.

[0097] In some embodiments, the carbonization sintering time in S20 is preferably 1 h to 15 h, and more preferably 6 h to 14 h.

[0098] In S20, by controlling the carbonization sintering temperature and the carbonization sintering time within the above ranges, the carbon source is carbonized to form a coating layer containing a conductive carbon material on at least a part of the surface of the carbon-based material particles, and the coating layer can have an appropriate thickness and graphitization degree.

[0099] In some embodiments, the carbon-based material particles may be a commercially available product, or preferably, are prepared by the following method: In S101, provide coke powder and put the coke powder into a reaction vessel; In S102, the coke powder is graphitized to obtain carbon-based material particles.

[0100] In some embodiments, the coke powder may be a commercially available product, or is preferably prepared by the following method: In S1011, a coke raw material is coked to obtain coke, and in S1012, the obtained coke is crushed, shaped, and classified to obtain coke powder.

[0101] In this application, the term "coke raw material" refers to a component that can be processed to obtain "coke", i.e., a raw material for producing coke, and "coke" is a product of the coking process of the coke raw material. "Coke powder" and "coke" have exactly the same composition, and the difference between them is that "coke powder" is "coke" that exists as a powder of a certain particle size, i.e., "coke powder" is obtained after "coke" is subjected to processing such as crushing.

[0102] Preferably, the coke raw material can include one or a combination of a petroleum-based raw material and a coal-based raw material. As an example, the petroleum-based raw material includes one or a combination of a heavy oil, a residual oil, and a vacuum residual oil, and the coal-based raw material mainly includes coal asphalt. The heavy oil, the residual oil, and the vacuum residual oil are usually generated in a petroleum refining process, and the coal asphalt is usually generated in a coal carbonization process.

[0103] Preferably, the coke obtained in S1011 includes one or more combinations selected from petroleum-based non-needle coke, petroleum-based needle coke, coal-based non-needle coke, and coal-based needle coke. More preferably, the coke obtained in S1011 includes one or more combinations of petroleum-based non-needle coke (e.g., petroleum calcined coke, petroleum-based raw coke) and petroleum-based needle coke. In particular, the coke obtained in S1011 is petroleum-based raw coke. By adopting an appropriate coke, the produced carbon-based material particles have an appropriate number of end faces and defects, and further have good ion transport and electron transport performance and high structural stability, which can improve the rapid charging ability and cycle performance of the secondary battery.

[0104] Preferably, the coking process of the coke feedstock in S1011 is carried out in a delayed coking unit, which includes a heating furnace and a coke tower, and the delayed coking process means that the coke feedstock is first rapidly heated to a desired coking temperature in the heating furnace, and then enters the coke tower, where it undergoes processes such as preheating, cold coking, etc. to produce coke.

[0105] Preferably, in S1012, the resulting coke can be crushed using equipment and methods known in the art, for example, jet mills, mechanical milling, roll presses or other crushing equipment can be employed.

[0106] The morphology of the coke powder obtained after crushing can include one or a combination of agglomerated, spherical, and near-spherical. After crushing is completed, the corners of the coke powder are ground by shaping. The greater the degree of shaping, the closer the powder particles are to a sphere, thus increasing the active sites on the surface of the carbon-based material particles. The shaping process also contributes to the subsequent granulation process, and provides high structural stability to the secondary particle portion in the obtained carbon-based material particles. The shaping process can be carried out using equipment and methods known in the art, such as a shaping machine or other shaping equipment.

[0107] In the process of crushing and shaping, many undersized particles are often generated, and oversized particles may also be present, so that classification can be performed as necessary to remove the undersized and oversized particles in the powder. After classification, coke powder having a good particle size distribution suitable for the subsequent granulation process can be obtained. Classification can be performed using equipment and methods known in the art, such as a classification sieve, a gravity classifier, or a centrifugal classifier.

[0108] In some embodiments, preferably, S101 further includes adding an adhesive to a reaction vessel, uniformly mixing the adhesive and the coke powder, and then granulating the mixture. By adding the adhesive, the obtained carbon-based material particles can have excellent secondary particle size, which is advantageous for improving the ion transport and electron transport performance of the negative electrode active material and also having high structural stability.

[0109] Preferably, the mass percentage content of the adhesive is 3% to 12%, more preferably 5% to 8%, calculated based on the total mass of the coke powder. When the content of the adhesive is within an appropriate range, excessive aggregation of particles can be avoided.

[0110] Preferably, the adhesive comprises one or a combination of a plurality of materials selected from coal asphalt, petroleum asphalt, mesophase asphalt, phenolic resin, epoxy resin, and petroleum resin.

[0111] The granulation process can be carried out using equipment and methods known in the art, such as a granulator. The granulator usually includes a stirring reaction vessel and a module for controlling the temperature of the reaction vessel. By adjusting the stirring rotation speed, the temperature increase rate, the granulation temperature, the temperature decrease rate, and the like in the granulation process, the degree of granulation and the structural strength of the particles can be adjusted, and the volume average particle size Dv50 of the finally produced carbon-based material particles can be within a desired range.

[0112] In some embodiments, the graphitization temperature in S102 may be preferably 2400°C to 3200°C, and more preferably 2800°C to 3200°C or 2900°C to 3100°C.

[0113] In some embodiments, the graphitization treatment time in S102 may be preferably 20 hours to 48 hours.

[0114] The graphitization treatment can provide the carbon-based material particles with an appropriate graphitization degree to increase the capacity per gram of the negative electrode active material; the graphitization treatment can reduce the lattice expansion coefficient of the carbon-based material particles to improve the structural stability; the graphitization treatment can effectively remove the phase structural defects in the carbon-based material particles to improve the cycle stability of the secondary battery.

[0115] The graphitization process can be carried out using equipment and methods known in the art, such as a graphitization furnace, particularly an Acheson graphitization furnace. After the graphitization process is completed, a small amount of excessively large particles formed by agglomeration during the graphitization process can be removed by sieving, thereby preventing the excessively large particles from affecting the processing performance of the obtained negative electrode active material, such as the stability and coating performance of the negative electrode slurry.

[0116] In some embodiments, the method for preparing the fast charging negative electrode active material includes the steps of: putting coke powder and an adhesive into a reaction vessel, uniformly mixing them, and then granulating them; graphitizing the resulting granulated product to obtain carbon-based material particles; uniformly mixing the resulting carbon-based material particles with a carbon source and a ferroelectric material, and forming a coating layer containing a conductive carbon material on at least a portion of the surface of the carbon-based material particles by a carbonization sintering process, wherein the ferroelectric material is dispersed in the coating layer, and at least a portion of the ferroelectric material protrudes from the surface of the coating layer.

[0117] The method for preparing the fast-charging negative electrode active material of the present application has a simple process, low production cost, and is compatible with the current process for preparing carbon-based material particles, especially artificial graphite, and does not require additional production equipment and process steps. When preparing the fast-charging negative electrode active material by the method of the present application, the ferroelectric material is less likely to aggregate, so that the desolvation effect of the solvated lithium ions can be exerted on the entire negative electrode active material, which is favorable for the negative electrode active material to have a higher fast-charging ability and a longer service life.

[0118] Some raw materials used in the method for preparing the fast charging negative electrode active material of the present application and their contents, etc., can be referred to the fast charging negative electrode active material of the first aspect of the embodiment of the present application, and the description thereof is omitted here. Negative electrode sheet

[0119] A third aspect of the present embodiment provides a negative electrode sheet including a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, the negative electrode film layer including the fast-charging negative electrode active material according to the first aspect of the present embodiment or the fast-charging negative electrode active material produced by the method according to the second aspect of the present embodiment. For example, the negative electrode current collector has opposite surfaces in a thickness direction thereof, and the negative electrode film layer is provided on one or both of the two opposite surfaces of the negative electrode current collector.

[0120] In some embodiments, the negative electrode film layer may further include other negative electrode active materials used in secondary batteries known in the art. For example, the other negative electrode active materials may include one or more combinations selected from natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based materials may include one or more combinations selected from elemental silicon, silicon oxide, silicon carbon composites, silicon nitrogen composites, and silicon alloy materials. The tin-based materials may include one or more combinations selected from elemental tin, tin oxide, and tin alloy materials.

[0121] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent, if necessary. In the present application, the type of the negative electrode conductive agent is not particularly limited, and as an example, the negative electrode conductive agent may include one or a combination of a plurality of types selected from superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage content of the negative electrode conductive agent is 5% or less with respect to the total mass of the negative electrode film layer.

[0122] In some embodiments, the negative electrode film layer may further include a negative electrode adhesive, if necessary. In the present application, the type of the negative electrode adhesive is not particularly limited, but as an example, the negative electrode adhesive may include one or a combination of a plurality of types selected from styrene butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-soluble acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage content of the negative electrode adhesive is 5% or less with respect to the total mass of the negative electrode film layer.

[0123] In some embodiments, the negative electrode membrane layer may further include other auxiliary agents as necessary. For example, the other auxiliary agents may include thickeners such as sodium carboxymethylcellulose (CMC-Na) and PTC thermistor materials. In some embodiments, the mass percentage content of the other auxiliary agents is 2% or less based on the total mass of the negative electrode membrane layer.

[0124] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. Examples of the metal foil include copper foil and copper alloy foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material may include one or more combinations selected from copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, and the polymeric material base layer may include one or more combinations selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0125] The negative electrode film layer is typically formed by applying a negative electrode slurry to a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is typically formed by dispersing a negative electrode active material, an optional conductive agent, an optional adhesive, and other optional auxiliary agents in a solvent, and stirring the mixture uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.

[0126] The negative electrode sheet does not exclude any additional functional layers other than the negative electrode film layer. For example, in some embodiments, the negative electrode sheet described herein further includes a conductive primer layer (e.g., made of a conductive agent and an adhesive) sandwiched between the negative electrode collector and the negative electrode film layer and provided on the surface of the negative electrode collector. In some other embodiments, the negative electrode sheet described herein further includes a protective layer covering the surface of the negative electrode film layer. secondary battery

[0127] A secondary battery, also called a rechargeable battery or storage battery, is a battery that can continue to be used after discharging by activating the active material through charging. The secondary battery includes an electrode assembly and an electrolyte, and the electrode assembly usually includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is provided between the positive electrode sheet and the negative electrode sheet, and mainly serves to prevent short circuits between the positive electrode and the negative electrode, and at the same time allows metal ions to pass through. The electrolyte serves to conduct metal ions between the positive electrode sheet and the negative electrode sheet. The secondary battery of the present application may be a lithium-containing secondary battery, etc., and in particular may be a lithium-ion secondary battery. [Negative electrode sheet]

[0128] The negative electrode sheet used in the secondary battery of the present application is the negative electrode sheet of any of the embodiments of the third aspect of the present application. [Positive electrode sheet]

[0129] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, for example, the positive electrode current collector has two surfaces opposed to each other in a thickness direction of the positive electrode current collector, and the positive electrode film layer is disposed on one or both of the two opposed surfaces of the positive electrode current collector.

[0130] The positive electrode film layer contains a positive electrode active material, and the positive electrode active material may employ a positive electrode active material known in the art for secondary batteries. For example, the positive electrode active material may include one or a combination of multiple types selected from lithium transition metal oxides, lithium-containing phosphates with an olivine structure, and their respective modified compounds. Examples of the lithium transition metal oxide may include one or a combination of multiple types selected from lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of the lithium-containing phosphate with an olivine structure may include one or a combination of multiple types selected from lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, a composite material of lithium manganese iron phosphate and carbon, and their modified compounds.

[0131] In some embodiments, in order to further increase the energy density of the secondary battery, the positive electrode active material may include one or a combination of multiple types of the lithium transition metal oxides and their modified compounds represented by Formula 1.

[0132] Li a Ni b Co c M d O e A f Formula 1

[0133] In Formula 1, 0.8 ≦ a ≦ 1.2, 0.5 ≦ b < 1, 0 < c < 1, 0 < d < 1, 1 ≦ e ≦ 2, 0 ≦ f ≦ 1, M includes one or a combination of multiple types selected from Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, and B, and A includes one or a combination of multiple types selected from N, F, S, and Cl.

[0134] In the present application, the modified compound of each of the positive electrode active materials may perform doping modification and / or surface coating modification on the positive electrode active materials.

[0135] In some embodiments, the positive electrode film layer may contain a positive electrode conductive agent as necessary. In the present application, the type of the positive electrode conductive agent is not particularly limited, but as an example, the positive electrode conductive agent may include one or a combination of a plurality of types selected from superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage content of the positive electrode conductive agent is 5% or less with respect to the total mass of the positive electrode film layer.

[0136] In some embodiments, the positive electrode film layer may include a positive electrode adhesive, if necessary. In the present application, the type of the positive electrode adhesive is not particularly limited, but as an example, the positive electrode adhesive may include one or a combination of a plurality of types selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. In some embodiments, the mass percentage content of the positive electrode adhesive is 5% or less with respect to the total mass of the positive electrode film layer.

[0137] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. Examples of the metal foil include aluminum foil or aluminum alloy foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material may include one or more combinations selected from aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, and the polymeric material base layer may include one or more combinations selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0138] The positive electrode membrane layer is usually formed by applying a positive electrode slurry to a positive electrode current collector, drying, and cold pressing. The positive electrode slurry is usually formed by dispersing a positive electrode active material, an optional conductive agent, an optional adhesive, and any other components in a solvent, and stirring the mixture uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP).

[0139] [Electrolyte]

[0140] The electrolyte of the present application may be any electrolyte for secondary batteries known in the art, and includes a lithium salt and an organic solvent.

[0141] As an example, the lithium salt is lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium perchlorate (LiClO 4 ), lithium hexafluoroarsenate (LiAsF 6 ), lithium bisfluorosulfonylimide (LiFSI), lithium bistrifluoromethanesulfonylimide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium bis(oxalatoborate) (LiBOB), lithium difluorophosphate (LiPO2 F 2 ), lithium difluorobisoxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP), or a combination of two or more of these.

[0142] By way of example, the organic solvent may include at least one or a combination of more than one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE). [Separator]

[0143] In the present application, the type of the separator is not particularly limited, and any known porous structure separator having good chemical stability and mechanical stability can be selected.

[0144] In some embodiments, the separator may be made of at least one material selected from the group consisting of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of the layers may be the same or different.

[0145] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly by a winding process or a stacking process.

[0146] In some embodiments, the secondary battery can include an exterior case that can be used to seal the electrode assembly and the electrolyte.

[0147] In some embodiments, the exterior of the secondary battery may be a hard case, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior of the secondary battery may be a soft package, such as a bag-type soft package. The material of the soft package may be, for example, plastic, such as one or a combination of multiple types of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0148] In the present application, the shape of the secondary battery is not particularly limited, and may be cylindrical, rectangular, or any other shape. For example, FIG. 2 shows a secondary battery 5 having a rectangular structure as an example.

[0149] In some embodiments, as shown in FIG. 3, the exterior may include a case 51 and a cover plate 53. The case 51 includes a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are surrounded to form a chamber. The case 51 has an opening communicating with the chamber, and the cover plate 53 covers the opening to close the chamber. The positive electrode sheet, the negative electrode sheet and the separator may form an electrode assembly 52 by a winding process or a lamination process. The electrode assembly 52 is sealed in the chamber. The electrode assembly 52 is infiltrated with an electrolyte. The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and may be adjusted according to needs.

[0150] The method of fabricating the secondary battery of the present application is known. In some embodiments, a secondary battery can be formed by assembling a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte. For example, a positive electrode sheet, a separator, and a negative electrode sheet can be formed into an electrode assembly by a winding process or a lamination process, and the electrode assembly can be placed in an outer casing, dried, and then an electrolyte can be injected, and a secondary battery can be obtained through processes such as vacuum sealing, standing, chemical formation, and shaping.

[0151] In some embodiments of the present application, the secondary battery of the present application may be assembled into a battery module, and the number of secondary batteries included in the battery module may be multiple, and the specific number may be adjusted according to the application and capacity of the battery module.

[0152] Fig. 4 is a schematic diagram of an example battery module 4. As shown in Fig. 4, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed by a fastener.

[0153] Preferably, the battery module 4 further includes a housing having an accommodation space, and the multiple secondary batteries 5 are accommodated in the accommodation space.

[0154] In some embodiments, the battery modules may be assembled into a battery pack, and the number of battery modules included in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0155] 5 and 6 are schematic diagrams of an example battery pack 1. As shown in Fig. 5 and 6, the battery pack 1 may include a battery box and a plurality of battery modules 4 provided in the battery box. The battery box includes an upper housing 2 and a lower housing 3, and the upper housing 2 is covered by the lower housing 3 to form an enclosed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner. power consumption equipment

[0156] A fifth aspect of the present embodiment provides a power consumption device including at least one of the secondary battery, battery module, and battery pack of the present application. The secondary battery, battery module, and battery pack may be used as a power source for the power consumption device, or may be used as an energy storage unit for the power consumption device. The power consumption device may be, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0157] The power consumption device can select a secondary battery, a battery module or a battery pack according to its usage demand.

[0158] 7 is a schematic diagram of an example power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. A battery pack or battery module may be employed to meet the high power and high energy density demands of the power consuming device.

[0159] Other examples of power consuming devices may be mobile phones, tablet computers, notebook computers, etc. Such power consuming devices are usually required to be thin and may employ secondary batteries as their power source. Working Example

[0160] The following examples are provided to more specifically describe the contents of the present application, and these examples are merely used for explanatory purposes, and it is obvious to those skilled in the art that various modifications and changes can be made within the scope of the contents of the present application. Unless otherwise specified, all parts, percentages, and ratios described in the following examples are calculated based on mass, and all reagents used in the examples can be purchased or synthesized according to conventional methods and can be used directly without further processing, and all devices used in the examples can be purchased. Example 1

[0161] Step (1): Preparation of negative electrode active material

[0162] In S10, the petroleum residual oil is subjected to delayed coking treatment under conditions of 490°C to 510°C to obtain petroleum non-needle coke. The raw coke is crushed, shaped, and classified to obtain coke powder. The obtained coke powder is mixed with coal asphalt as an adhesive, and then granulated. The obtained granulated product is placed in a graphite crucible, and then the graphite crucible is placed in an Acheson graphitization furnace, an electric resistance material is placed around the graphite crucible, and an electric current is passed through the electric resistance material to generate thermal energy, and graphitization is performed at about 3000°C for about 30 hours to obtain artificial graphite particles. The volume average particle size Dv50 of the artificial graphite particles is about 9.8 μm, and the graphitization degree is about 92%.

[0163] In S20, the obtained artificial graphite particles, the petroleum asphalt as a carbon source (the added mass was calculated based on the residual carbon value), and the ferroelectric material BaTiO 3 (Volume average particle size Dv50 is 200 nm, dielectric constant is 2000) are uniformly mixed in a mass ratio of 100:3:3, and then carbonization sintering is performed in a roller hearth kiln. The temperature in the maximum temperature range is about 1150°C, and the operation time in the maximum temperature range is about 12 hours. An amorphous carbon coating layer is formed on at least a part of the surface of the artificial graphite particles, and a negative electrode active material is obtained. In the obtained negative electrode active material, BaTiO 3 is dispersed in the coating layer, and at least a part of BaTiO 3 protrudes from the surface of the coating layer.

[0164] Step (2): Preparation of negative electrode sheet

[0165] The negative electrode active material prepared above, styrene butadiene rubber (SBR) as an adhesive, sodium carboxymethylcellulose (CMC-Na) as a thickener, and carbon black as a conductive agent are thoroughly mixed in a mass ratio of 96.8:1.2:1.2:0.8 in an appropriate amount of deionized water as a solvent to form a uniform negative electrode slurry. The negative electrode slurry is uniformly applied to the surface of copper foil as a negative electrode current collector, and then dried and cold pressed to obtain a negative electrode sheet. The application amount is 0.162 kg / m 2 , compressed density is 1.65g / cm 3 It is.

[0166] Step (3): Preparation of the positive electrode sheet

[0167] Positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3 O 2 (NCM523), carbon black as a conductive agent, and polyvinylidene fluoride (PVDF) as an adhesive are thoroughly mixed in a mass ratio of 96.2:1.8:2 in an appropriate amount of NMP solvent, and a uniform positive electrode slurry is formed. The positive electrode slurry is uniformly applied to the surface of aluminum foil as a positive electrode current collector, and after drying and cold pressing, a positive electrode sheet is obtained. The amount of application is 0.256 kg / m 2 , compressed density is 3.4g / cm 3 It is.

[0168] Step (4): Preparation of electrolyte

[0169] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain an organic solvent, which was then thoroughly dried and then cooled to 100°C. 6 is dissolved in the above organic solvent to prepare an electrolyte solution with a concentration of 1 mol / L.

[0170] Step (5): Making the separator

[0171] The separator is a porous polyethylene film.

[0172] Step (6): Preparation of secondary battery

[0173] A positive electrode sheet, a separator, and a negative electrode sheet are stacked in that order and wound up to obtain an electrode assembly. The electrode assembly is then placed in an outer casing and dried. After that, an electrolyte is injected, and the assembly goes through processes such as vacuum sealing, leaving it to stand, chemical formation, and shaping to obtain a secondary battery. (Examples 2 to 16)

[0174] The secondary batteries of Examples 2 to 16 are prepared in a similar manner to that of Example 1, except that the relevant parameters in "Preparation of negative electrode active material" are adjusted. See Table 2 for specific parameters. Comparative Example 1

[0175] The secondary battery of Comparative Example 1 was produced in a similar manner to Example 1, except that a conventional artificial graphite without a coating layer was used as the negative electrode active material. Specifically, the artificial graphite was produced by the following method.

[0176] Petroleum residual oil is subjected to delayed coking treatment at 490°C to 510°C to obtain petroleum non-needle coke raw coke. The raw coke is crushed, shaped, and classified to obtain coke powder. The obtained coke powder is mixed with coal asphalt as an adhesive, and then granulated. The obtained granulated product is placed in a graphite crucible, which is then placed in an Acheson graphitization furnace, an electrical resistance material is placed around the graphite crucible, and electricity is passed through the electrical resistance material to generate thermal energy, and graphitization is performed at about 3000°C for about 30 hours to obtain artificial graphite particles. The volume average particle size Dv50 of the artificial graphite particles is about 9.8 μm, and the graphitization degree is about 92%. Comparative Example 2

[0177] The secondary battery of Comparative Example 2 was fabricated in a similar manner to that of Example 1, except that the negative electrode active material was prepared in the following manner.

[0178] In S10, the petroleum residual oil is subjected to delayed coking treatment under conditions of 490°C to 510°C to obtain petroleum non-needle coke raw coke. The raw coke is crushed, shaped, and classified to obtain coke powder. The obtained coke powder is mixed with coal asphalt as an adhesive, and then granulated. The obtained granulated product is placed in a graphite crucible, and then the graphite crucible is placed in an Acheson graphitization furnace, an electric resistance material is placed around the graphite crucible, and an electric current is passed through the electric resistance material to generate thermal energy, and graphitization is performed at about 3000°C for about 30 hours to obtain artificial graphite particles. The volume average particle size Dv50 of the artificial graphite particles is about 9.8 μm, and the graphitization degree is about 92%.

[0179] In S20, the obtained artificial graphite particles are mixed with petroleum asphalt as a carbon source, and then carbonization sintering is carried out in a roller hearth kiln, the temperature in the maximum temperature region is about 1150°C, and the operation time in the maximum temperature region is about 12 hours, and an amorphous carbon coating layer is formed on at least a part of the surface of the artificial graphite particles to obtain a negative electrode active material. Comparative Example 3

[0180] The secondary battery of Comparative Example 3 was fabricated in a similar manner to that of Example 1, except that the negative electrode active material and the negative electrode sheet were prepared in the following manner.

[0181] Step (1): Preparation of negative electrode active material

[0182] In S10, the petroleum residual oil is subjected to delayed coking treatment under conditions of 490°C to 510°C to obtain petroleum non-needle coke raw coke. The raw coke is crushed, shaped, and classified to obtain coke powder. The obtained coke powder is mixed with coal asphalt as an adhesive, and then granulated. The obtained granulated product is placed in a graphite crucible, and then the graphite crucible is placed in an Acheson graphitization furnace, an electric resistance material is placed around the graphite crucible, and an electric current is passed through the electric resistance material to generate thermal energy, and graphitization is performed at about 3000°C for about 30 hours to obtain artificial graphite particles. The volume average particle size Dv50 of the artificial graphite particles is about 9.8 μm, and the graphitization degree is about 92%.

[0183] In S20, the obtained artificial graphite particles are mixed with petroleum asphalt as a carbon source, and then carbonization sintering is carried out in a roller hearth kiln, the temperature in the maximum temperature region is about 1150°C, and the operation time in the maximum temperature region is about 12 hours, and an amorphous carbon coating layer is formed on at least a part of the surface of the artificial graphite particles to obtain a negative electrode active material.

[0184] Step (2): Preparation of negative electrode sheet

[0185] The negative electrode active material prepared above, ferroelectric material BaTiO 3 (Volume average particle size Dv50 is 85 nm), styrene butadiene rubber (SBR) as an adhesive, sodium carboxymethylcellulose (CMC-Na) as a thickener, and carbon black as a conductive agent are thoroughly mixed in a mass ratio of 93.8:3:1.2:1.2:0.8 in an appropriate amount of deionized water as a solvent to form a uniform negative electrode slurry. The negative electrode slurry is uniformly applied to the surface of copper foil as a negative electrode current collector, and after drying and cold pressing, a negative electrode sheet is obtained. Comparative Example 4

[0186] The secondary battery of Comparative Example 4 was fabricated in a similar manner to that of Example 1, except that the negative electrode active material was prepared in the following manner.

[0187] In S10, the petroleum residual oil is subjected to delayed coking treatment under conditions of 490°C to 510°C to obtain petroleum non-needle coke raw coke. The raw coke is crushed, shaped, and classified to obtain coke powder. The obtained coke powder is mixed with coal asphalt as an adhesive, and then granulated. The obtained granulated product is placed in a graphite crucible, and then the graphite crucible is placed in an Acheson graphitization furnace, an electric resistance material is placed around the graphite crucible, and an electric current is passed through the electric resistance material to generate thermal energy, and graphitization is performed at about 3000°C for about 30 hours to obtain artificial graphite particles. The volume average particle size Dv50 of the artificial graphite particles is about 9.8 μm, and the graphitization degree is about 92%.

[0188] In S20, the obtained artificial graphite particles are mixed with petroleum asphalt, which is a carbon source, and then a carbonization sintering process is carried out in a roller hearth kiln, the temperature in the maximum temperature region is about 1150°C, and the operating time in the maximum temperature region is about 12 hours, and an amorphous carbon coating layer is formed on at least a portion of the surface of the artificial graphite particles.

[0189] In S30, the obtained artificial graphite particles with the amorphous carbon coating layer and the ferroelectric material BaTiO 3 (Volume average particle size Dv50 is 85 nm) are ball milled in a mass ratio of 97:3 to mix uniformly, then placed in a planetary ball mill and ball milled at an ambient temperature of 25°C and a rotation speed of 300 rpm for 2 hours, and then removed to obtain the negative electrode active material. Test part

[0190] (1) Volume average particle size Dv50 test

[0191] A certain amount of the prepared negative active material sample was taken and tested for the volume average particle size Dv50 by Mastersizer2000E type laser particle size analyzer. The test standard is in accordance with GB / T19077-2016.

[0192] (2) Specific surface area test

[0193] A certain amount of the negative electrode active material sample prepared above was taken and the specific surface area was tested using a Tri-Star 3020 specific surface area pore size analysis tester from Micromeritics, USA. The specific surface area was calculated using the BET (Brunauer Emmett Teller) method. The test standard was in accordance with GB / T19587-2017.

[0194] (3) Powder compression density test

[0195] A certain amount of the negative electrode active material sample was taken and measured with a UTM7305 electronic pressure tester so that the bottom area of ​​the sample was 1.327 cm 2The powder was then pressed to 2000 kg (equivalent to 20000 N) after 30 seconds of pressure retention, and the pressure was released and held for 10 s, and then recorded to calculate the powder compression density of the negative active material at a force of 20000 N. The test standard was in accordance with GB / T24533-2009.

[0196] (4) Graphitization degree test

[0197] A certain amount of the negative electrode active material sample prepared above was taken and tested using a Bruker D8Discover X-ray diffractometer to measure the interlayer distance d between the coating layer and the (002) crystal plane of the carbon-based material particles. 002 After obtaining each of these, the formula g=(0.344-d 002 ) / (0.344-0.3354)×100%, the graphitization degree of the coating layer g 1 and the degree of graphitization of carbon-based material particles g 2 The test standards are in accordance with JIS K0131-1996 and JB / T4220-2011.

[0198] (5) (Average coating thickness test)

[0199] A certain amount of the negative electrode active material sample prepared above is taken, and a thin slice of about 100 nm is cut out from the middle of a single particle. Then, a transmission electron microscope analysis test is performed on the thin slice to obtain a TEM picture, and the thickness is measured at multiple (e.g., five or more) different positions on the TEM picture. At least six negative electrode active material samples are tested, and the average value of the test results is the average thickness of the coating layer.

[0200] (6) Initial Capacity per Gram Test

[0201] The negative electrode active material prepared above, carbon black as a conductive agent, and polyvinylidene fluoride (PVDF) as an adhesive were mixed uniformly in a mass ratio of 91.6:1.8:6.6 with N-methylpyrrolidone (NMP) as a solvent to make a slurry. The prepared slurry was applied to copper foil and dried in an oven to make a backup. Then, a piece of metallic lithium was used as the counter electrode, a polyethylene (PE) film was used as the separator, and a few drops of the same electrolyte as the secondary battery were dropped into it, and the battery was assembled as a CR2430 button battery in a glove box protected by argon gas.

[0202] The obtained button battery was left to stand for 12 hours, then discharged at a constant current of 0.05C to 0.005V at 25°C, left to stand for 10min, discharged at a constant current of 50μA to 0.005V, left to stand for 10min, discharged at a constant current of 10μA to 0.005V, and then charged at a constant current of 0.1C to 2V, and the charge capacity was recorded. The ratio of the charge capacity to the mass of the negative electrode active material is the initial capacity per gram of the negative electrode active material.

[0203] (7) Testing the rapid charging performance of secondary batteries

[0204] At 25°C, the secondary battery prepared above was charged at a constant current of 0.33 C up to a charge cut-off voltage of 4.4 V, then charged at a constant voltage of 0.05 C, allowed to stand for 5 minutes, and further discharged at a constant current of 0.33 C up to a discharge cut-off voltage of 2.8 V, and the actual capacity was recorded as C0.

[0205] After that, the secondary battery was charged at a constant current of 0.5C0, 1C0, 1.5C0, 2C0, 2.5C0, 3C0, 3.5C0, 4C0, and 4.5C0 in that order to a total battery charge cut-off voltage of 4.4V or a negative electrode cut-off potential of 0V (whichever reached first), and after each charge was completed, it was discharged at 1C0 to a total battery discharge cut-off voltage of 2.8V, and then measured at different charge rates of 10%, 20%, 30%, ... 80% SOC (State of Charge). The negative electrode potential corresponding to the charging up to 0 V was recorded, and the charge rate vs. negative electrode potential curves at different SOC states were plotted and linearly fitted to obtain the charge rate corresponding to the negative electrode potential of 0 V at different SOC states. The charge rate was the charge window at the SOC state, which was C10% SOC, C20% SOC, C30% SOC, C40% SOC, C50% SOC, C60% SOC, C70% SOC, and C80% SOC, and the charging time T for the secondary battery to be charged from 10% SOC to 80% SOC was calculated from the formula (60 / C20% SOC+60 / C30% SOC+60 / C40% SOC+60 / C50% SOC+60 / C60% SOC+60 / C70% SOC+60 / C80% SOC)×10%. The shorter the charging time T, the more excellent the rapid charging performance of the secondary battery.

[0206] (8) (Cycle performance test)

[0207] At 25°C, the secondary battery prepared above was charged at a constant current of 0.33C to a charge cut-off voltage of 4.4V, then charged at a constant voltage of 0.05C, left to stand for 5min, and discharged at a constant current of 0.33C to a discharge cut-off voltage of 2.8V, and the initial capacity was recorded as C0. Thereafter, charging was performed according to the policy shown in Table 1, and discharging was performed at 0.33C, and the discharge capacity Cn per cycle was recorded until the cycle capacity retention rate (i.e., Cn / C0×100%) reached 80%, and the number of cycles was recorded. The higher the number of cycles, the better the cycle performance of the secondary battery. [Table 1]

[0208] Table 2 shows the preparation parameters of the negative electrode active materials of Examples 1-16.

[0209] Table 3 shows the test results obtained for Examples 1 to 16 and Comparative Examples 1 to 4 according to the above performance test methods. [Table 2] [Table 3]

[0210] To summarize the test results in Table 3, it can be seen that the negative electrode active material of the present invention has good dynamic performance, shortens the fast charging time of the secondary battery, and extends the cycle life of the secondary battery without compromising the high capacity per gram of the negative electrode active material.

[0211] Compared with Comparative Example 1, Comparative Example 2 employs artificial graphite coated with amorphous carbon as the negative electrode active material, which can improve the fast charging performance and cycle performance of the secondary battery to a certain extent, but the improvement effect is limited and cannot meet the requirements for higher fast charging capability and longer cycle life for the secondary battery.

[0212] In comparison with Comparative Example 2, Comparative Example 3 further adds a ferroelectric material to the negative electrode slurry, which can further improve the fast charging performance and cycle performance of the secondary battery, but the improvement effect is limited and the secondary battery cannot meet the requirements for higher fast charging ability and longer cycle life. Possible reasons are that by physically mixing and adding the ferroelectric material to the negative electrode slurry, the density of the ferroelectric material is high, so it is easy to settle in the negative electrode slurry, making it difficult to form a stable negative electrode slurry, which affects the productivity and the quality of the negative electrode sheet, while the addition of the ferroelectric material by physical mixing causes some of the ferroelectric material and the negative electrode active material to not form physical contact in the negative electrode sheet, and furthermore, the function of the ferroelectric material cannot be exerted, so that the improvement effect of the fast charging performance and cycle performance of the secondary battery is limited.

[0213] In comparison with Comparative Example 1, Comparative Example 4 employs artificial graphite coated with barium titanate as the negative electrode active material. However, the negative electrode active material is obtained by a direct ball milling method, and although the fast charging performance and cycle performance of the secondary battery are improved to a certain extent compared with Comparative Example 1, the improvement effect is limited, and the demand for higher fast charging ability and longer cycle life for the secondary battery cannot be met. Possible reasons are that in the direct ball milling method, artificial graphite particles and ferroelectric material particles are collided and polished to combine them to form the negative electrode active material, but the high-energy ball mill destroys the morphology of the already formed artificial graphite particles, causing the amorphous carbon coating layer on the surface to fall off, which may affect the fast charging performance of the negative electrode active material, while after the surface of the negative electrode active material is destroyed, the electrolyte (especially the solvent) is inserted into the negative electrode active material, increasing the irreversible consumption of active lithium ions, thereby deteriorating the cycle performance of the secondary battery.

[0214] The present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and any embodiment having substantially the same configuration as the technical idea within the technical scope of the present application and having similar effects is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can conceive of may be added to the embodiment within the scope of the present application, and other forms constructed by combining some of the components in the embodiment are also included in the scope of the present application.

Claims

1. A fast charging negative electrode active material comprising: carbon-based material particles; a coating layer located on at least a portion of the surface of the carbon-based material particles; and a ferroelectric material dispersed in the coating layer, The coating layer includes a conductive carbon material, and at least a portion of the ferroelectric material protrudes from a surface of the coating layer.

2. The average thickness of the coating layer is H nm, and the volume average particle diameter Dv50 of the ferroelectric material is d 1 nm, and the fast charging negative electrode active material has a H / d 1 ≦1.1, preferably 0.25≦H / d 1 2. The fast charging negative electrode active material of claim 1, which satisfies ≦0.

5.

3. The volume average particle diameter Dv50 of the ferroelectric material is d 1 nm, 0<d 1 ≦200, preferably 0<d 1 ≦100, and / or 3. The fast-charging negative electrode active material according to claim 1, wherein the coating layer has an average thickness of H nm, 20≦H≦100, preferably 20≦H≦50.

4. The mass ratio of the ferroelectric material to the carbon-based material particles is α 1 and α 1 is (0.5-10):100, preferably (1-3):100; and / or The mass ratio of the coating layer to the carbon-based material particles is α 2 and α 2 The fast-charging negative electrode active material according to any one of claims 1 to 3, wherein the ratio of the charge / discharge ratio to the charge / discharge ratio is (2-10):100, preferably (2-5):

100.

5. The mass ratio of the ferroelectric material to the carbon-based material particles is α 1 and the mass ratio of the coating layer to the carbon-based material particles is α 2 and α 1 :α 25. The fast-charging negative electrode active material according to claim 1, wherein the ratio of the ionic charge to the total charge is 1:6 to 4:1, preferably 1:4 to 2:

1.

6. The graphitization degree of the coating layer is between 45% and 80%; and / or 6. The rapid charging negative electrode active material according to claim 1, wherein the graphitization degree of the carbon-based material particles is 88% to 96%.

7. The volume average particle diameter Dv50 of the carbon-based material particles is d 2 μm, and 5≦d 2 ≦20, preferably 8≦d 2 7. The fast charging negative electrode active material of claim 1, wherein the R2 is ≦15.

8. The carbon-based material particles are in the form of primary particles, secondary particles, or a combination thereof; Preferably, in the secondary particle form of the carbon-based material particles, the ratio of the volume average particle diameter Dv50 of the primary particles to the volume average particle diameter Dv50 of the secondary particles composed of the primary particles is 0.2 to 0.

5. The rapid charging negative electrode active material according to any one of claims 1 to 7.

9. the dielectric constant of the ferroelectric material is greater than or equal to 100, preferably between 100 and 100,000; and / or The fast charging negative electrode active material according to any one of claims 1 to 8, wherein the ferroelectric material has a Curie temperature of 80°C or higher.

10. The carbon-based material particles include one or a combination of a plurality of types selected from graphite, mesocarbon microbeads, hard carbon, and soft carbon, and are preferably selected from graphite, and / or The conductive carbon material in the coating layer includes amorphous carbon, preferably hard carbon, and / or The fast charging negative electrode active material according to any one of claims 1 to 9, wherein the ferroelectric material comprises one or more combinations selected from the group consisting of perovskite structure oxides, tungsten bronze type compounds, bismuth oxide type layered structure compounds, lithium niobate and lithium tantalate.

11. The fast charging negative electrode active material according to any one of claims 1 to 10, wherein the fast charging negative electrode active material satisfies at least one of the following conditions (1) to (3): (1) The volume average particle size Dv50 of the rapid charging negative electrode active material is 5 μm to 20 μm, preferably 8 μm to 15 μm. (2) The specific surface area of ​​the fast charging negative electrode active material is 0.8 m 2 / g to 1.3 m 2 / g, preferably 0.9m 2 / g to 1.2 m 2 / g. (3) The powder compression density of the rapid charging negative electrode active material at a force of 20,000 N is 1.5 g / cm 3 ~1.9g / cm 3 and preferably 1.5 g / cm 3 ~1.7g / cm 3 It is.

12. Step S10 of supplying carbonaceous material particles, a carbon source, and a ferroelectric material, preferably the carbon source including one or a combination of a plurality of types selected from asphalt, resin, and biomass material; a step S20 of uniformly mixing the carbon-based material particles, the carbon source, and the ferroelectric material, and forming a coating layer containing a conductive carbon material on at least a part of the surface of the carbon-based material particles by a carbonization sintering process, the ferroelectric material being dispersed in the coating layer, and at least a part of the ferroelectric material protruding from the surface of the coating layer; A method for making a fast-charging negative electrode active material comprising:

13. The carbonization sintering temperature in S20 is 700°C to 1800°C, preferably 1000°C to 1300°C, and / or The method according to claim 12, wherein the carbonization sintering time in S20 is 1h to 15h, preferably 6h to 14h.

14. 14. The method of claim 12, wherein the carbon-based material particles are made by a method comprising: S101 supplying coke powder and placing the coke powder in a reaction vessel; and S102 graphitizing the coke powder to obtain the carbon-based material particles.

15. A negative electrode sheet comprising: a negative electrode current collector; and a negative electrode film layer provided on at least one surface of the negative electrode current collector, the negative electrode film layer comprising the fast-charging negative electrode active material according to any one of claims 1 to 11, or the fast-charging negative electrode active material produced by the method according to any one of claims 12 to 14.

16. A secondary battery comprising the negative electrode sheet according to claim 15.

17. A power consuming device comprising the secondary battery of claim 16.

Citation Information

Patent Citations

  • Core-shell type anode active material for lithium secondary batteries, method for preparing the same and lithium secondary batteries comprising the same

    CN101855756A

  • Negative electrode active material composite, negative electrode pole piece, secondary battery, battery module, battery pack and electric device

    CN117154022A

  • Nonaqueous electrolyte secondary battery

    JP2009176597A

  • Core-shell type negative electrode active material for lithium secondary batteries, method for manufacturing the same, negative electrode for lithium secondary batteries and lithium secondary battery containing the same

    JP2011515012A

  • Nonaqueous electrolyte secondary battery

    JP2016039114A