Electrode assembly, manufacturing method of electrode assembly, secondary battery, battery pack, and automobile
The electrode assembly design addresses wrinkles and damage issues by using a swelling tape to cover the boundary between coated and uncoated parts, enhancing the stability and performance of secondary batteries.
Patent Information
- Application Number
- JP2024515721
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-07-05
- Filing Date
- 2023-07-05
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2043-07-05
AI Technical Summary
Conventional electrode assemblies face issues with wrinkles and damage during assembly due to the attachment of swelling tapes on uncoated parts of the negative electrode current collector, leading to potential damage and reduced performance of secondary batteries.
The electrode assembly design includes a swelling tape to cover the boundary between the single-sided coated part and the uncoated part of the negative electrode, minimizing wrinkles and ensuring proper contact with the battery can, thereby reducing the risk of damage and enhancing performance.
This design minimizes wrinkles and bubbles, ensuring stable assembly and improved energy density, capacity, and output of secondary batteries by preventing damage during the assembly process.
Smart Images

Figure 2024537650000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode assembly, a manufacturing method for the electrode assembly, a secondary battery, a battery pack, and an automobile. This application claims the benefit of the filing date of Korean Patent Application No. 10-2022-0082557, filed on July 5, 2022 in the Korean Intellectual Property Office, the entire contents of which are incorporated herein by reference. [Background technology]
[0002] Secondary batteries, which have high ease of application depending on the product group and electrical properties such as high energy density, are widely used not only in portable devices but also in electric vehicles (EVs) and hybrid electric vehicles (HEVs) that are driven by electrical sources.
[0003] Such secondary batteries have the primary advantage of dramatically reducing the use of fossil fuels, as well as the advantage of not producing any by-products from the use of energy, and are therefore attracting attention as a new energy source that is environmentally friendly and improves energy efficiency.
[0004] Currently, the types of secondary batteries that are widely used include lithium ion batteries, lithium polymer batteries, nickel cadmium batteries, nickel metal hydride batteries, nickel zinc batteries, etc. The operating voltage of such a unit secondary battery cell is about 2.5 V to 4.5 V. Therefore, when a higher output voltage is required, a battery pack is formed by connecting multiple secondary batteries in series.
[0005] In addition, a battery pack may be configured by connecting a plurality of secondary batteries in parallel according to the charge / discharge capacity required for the battery pack. Therefore, the number and electrical connection form of the secondary batteries included in the battery pack may be variously set according to the required output voltage and / or charge / discharge capacity. Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide an electrode assembly and a method for manufacturing an electrode assembly that can achieve high energy density by providing a swelling tape to cover the boundary between a one-sided coated portion, in which an active material layer is provided only on one side of a negative electrode of an electrode assembly, and an uncoated portion in which no active material layer is provided.
[0007] It is another object of the present invention to provide a secondary battery, a battery pack, and an automobile, each including an electrode assembly having the above-mentioned improved structure.
[0008] However, the technical problems that the present invention aims to solve are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the description of the invention described below. [Means for solving the problem]
[0009] One embodiment of the present invention provides an electrode assembly in which a first electrode, a separator, and a second electrode are stacked, the first electrode including a current collector and a first active material layer and a second active material layer respectively provided on both sides of the current collector, one end of the first electrode including a one-sided coated portion where the first active material layer is provided on one side of the current collector and the second active material layer is not provided on the other side; and an uncoated portion where the first active material layer and the second active material layer are not provided on both sides of the current collector, and a swelling tape provided to cover a boundary between the first active material layer and the uncoated portion of the one-sided coated portion.
[0010] Another embodiment of the present invention provides a method for manufacturing an electrode assembly, the method including the steps of: manufacturing an electrode assembly by stacking a first electrode, a separator, and a second electrode, the first electrode including a current collector, and a first active material layer and a second active material layer respectively provided on both sides of the current collector, one end of the first electrode including a one-sided coated portion where the first active material layer is provided on one side of the current collector and the second active material layer is not provided on the other side, and an uncoated portion where the first active material layer and the second active material layer are not provided on both sides of the current collector; and disposing a swelling tape provided to cover a boundary between the first active material layer and the uncoated portion of the one-sided coated portion.
[0011] Another embodiment of the present invention provides a secondary battery, a battery pack, and a vehicle including the electrode assembly according to the above embodiment. Effect of the Invention
[0012] Due to the trend in the development of secondary batteries requiring high capacity and high output, in order to fit a large number of electrodes into a limited space, optimization is being carried out by changing the thickness of the current collectors and separators, as well as the size and structure of the battery can and top cap.
[0013] When the copper current collector of the negative electrode is used as the outer tab, the outer tab and separator in the conventional electrode assembly are removed, and the current collector is directly abutted against the battery can and electrically connected thereto, so that the amount of separator and outer tab required can be reduced, and the outer diameter of the electrode assembly can be reduced to secure space within the battery can, thereby reducing costs.
[0014] In addition, when the copper current collector of the negative electrode is used as an outer tab, it is possible to secure space within the battery can, thereby improving the capacity realization and output of the secondary battery, and since the area of the copper current collector that contacts the battery can and transfers heat is increased, the heat generation level is improved and the energy density of the electrode can be increased.
[0015] In a conventional electrode assembly, when a swelling tape is applied to an uncoated portion of a negative electrode current collector, rather than to a coated portion on one side, the swelling tape is cut by a winder device and transferred to the negative electrode. In this case, wrinkles are generated due to the characteristics of a thin current collector, and there is a risk that the electrode assembly may be damaged when the electrode assembly is inserted into a battery can in a secondary battery assembly process.
[0016] According to an embodiment of the present invention, an electrode assembly includes a swelling tape provided to cover a boundary between a one-sided coated portion, in which an active material layer is provided on only one side of a negative electrode, and an uncoated portion, in which no active material layer is provided. This minimizes wrinkles in the current collector and air bubbles generated in the swelling tape, thereby controlling the risk of poor appearance, preventing an increase in the outer diameter of the electrode assembly, and eliminating the risk of damage to the electrode assembly when the electrode assembly is inserted into a battery can in the secondary battery assembly process.
[0017] This can eliminate safety problems that may occur due to wrinkles formed on the negative electrode current collector, and can stably increase the current applied to the battery, thereby realizing a high energy density and providing a high-capacity and high-output secondary battery.
[0018] However, the advantageous effects obtained by the present invention are not limited to those described above, and other effects not mentioned will be clearly understood by those skilled in the art from the description of the invention described below. [Brief description of the drawings]
[0019] The following drawings attached to this specification illustrate preferred embodiments of the present invention and, together with the detailed description of the invention described below, serve to further understand the technical ideas of the present invention. Therefore, the present invention should not be interpreted as being limited only to the matters described in the drawings.
[0020] [Figure 1]1 is a schematic diagram illustrating a configuration in which a first electrode and a second electrode face each other in a conventional electrode assembly according to a comparative example of the present invention. [Figure 2(a)] 11 is a photograph showing a case in which wrinkles are formed on a first electrode current collector in a conventional electrode assembly according to a comparative example of the present invention. [Figure 2(b)] 11 is a photograph showing a case in which wrinkles are formed on a first electrode current collector in a conventional electrode assembly according to a comparative example of the present invention. [Figure 3(a)] 11 is a photograph showing a case where wrinkles and bubbles are generated in a first electrode current collector and a swelling tape in a conventional electrode assembly according to a comparative example of the present invention. [Figure 3(b)] 4 is a photograph showing a case where wrinkles and air bubbles in the first electrode current collector and the swelling tape are transferred to a separator. [Figure 4] 2 is a schematic diagram illustrating a configuration in which a first electrode and a second electrode face each other in an electrode assembly according to an embodiment of the present invention. FIG. [Diagram 5] 2 is a perspective view showing a configuration in which a first electrode and a second electrode face each other in an electrode assembly according to an embodiment of the present invention; FIG. [Figure 6] 2 is a plan view showing an end portion perpendicular to a winding axis direction of a jelly roll having an electrode assembly according to an embodiment of the present invention wound thereon; FIG. [Figure 7] 5 is a photograph showing a case where no wrinkles or bubbles are generated in a first electrode current collector and a swelling tape in an electrode assembly according to an embodiment of the present invention. [Figure 8] 6 is a photograph showing a case where a lifting phenomenon of a first electrode collector occurs in an electrode assembly according to a comparative example of the present invention and a portion where the lifting height of the first electrode collector is measured. [Figure 9] 1 is a diagram showing a schematic configuration of a battery pack including a secondary battery according to an embodiment of the present invention; [Figure 10] 1 is a diagram showing a schematic configuration of an automobile including a battery pack according to an embodiment of the present invention. [Explanation of symbols]
[0021] 1, 111...electrode assembly 10, 100...1st electrode 11, 110: First electrode current collector 12, 120: First active material layer of first electrode 13, 130: Second active material layer of first electrode 14, 140: One-sided coating of first electrode 15, 150: Uncoated part of the first electrode 20, 200...2nd electrode 30, 300...Separator 40, 400 ···Swelling Tape 410: A swelling tape provided so as to cover the boundary between the first active material layer and the uncoated portion 420 Length of the swelling tape covering the first active material layer 430 Area of the swelling tape covering the first active material layer 440 Length of swelling tape covering uncoated area 450 Distance between the second active material layer and the swelling tape 460 ···Swelling tape length 470 ···Swelling tape width 50, 500...suction pad 510 Step of suction pad 600...Secondary battery 610 ···Jelly Roll 620 Battery can 630 ···Sealing tape 700 ···Battery pack 710 ···Pack Housing 800 ···Automobiles W Winding direction P: Length direction of the electrode assembly, perpendicular to the winding shaft H: Width direction of the electrode assembly, winding axis direction d Floating height of first electrode current collector DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0023] Throughout this specification, when a part "comprises" a certain element, this means that it may further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.
[0024] Furthermore, the term "unit" or "part" used in the specification means a unit that processes at least one function or operation.
[0025] The embodiment described in this specification and the configurations shown in the drawings are merely the most preferred embodiment of the present invention and do not represent the entire technical idea of the present invention, so it should be understood that there may be various equivalents and modifications that can replace them at the time of filing this application.
[0026] In order to facilitate understanding of the invention, the accompanying drawings may be drawn not to scale, and some dimensions of components may be exaggerated. In addition, the same reference numerals may be used to refer to the same components in different embodiments.
[0027] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0028] In one embodiment of the present invention, there is provided an electrode assembly 111 in which a first electrode 100, a separator 300, and a second electrode 200 are laminated. The first electrode 100 includes a current collector 110, and a first active material layer 120 and a second active material layer 130 respectively provided on both sides of the current collector 110. One end of the first electrode 100 includes a one-sided coated portion 140 in which the first active material layer 120 is provided on one side of the current collector 110 and the second active material layer 130 is not provided on the other side; and an uncoated portion 150 in which the first active material layer 120 and the second active material layer 130 are not provided on both sides of the current collector 110, and a swelling tape 410 provided to cover a boundary between the first active material layer 120 and the uncoated portion 150 of the one-sided coated portion 140.
[0029] The electrode assembly 111 has a swelling tape 410 provided to cover the boundary between a one-sided coated portion 140 in which the first active material layer 120 is provided only on one side of the first electrode collector 110, and an uncoated portion 150 in which the first and second active material layers 120, 130 are not provided. This minimizes the occurrence of wrinkles in the collector 110, thereby controlling the risk of poor appearance and eliminating the risk of damage to the electrode assembly 111 when the electrode assembly 111 is inserted into a battery can 620 during the assembly process of the secondary battery 600.
[0030] FIG. 1 is a diagram illustrating a configuration in which a first electrode 10 and a second electrode 20 face each other in a conventional electrode assembly 1 according to a comparative example of the present invention.
[0031] Referring to FIG. 1, in the case where the swelling tape 40 is attached to the uncoated portion 15 of the first electrode collector 11 instead of the one-sided coated portion 14 in the conventional electrode assembly 1, the swelling tape 40 cut by a winder is transferred to the first electrode 10. In this case, due to the characteristics of the thin collector 11, wrinkles are generated, and there is a risk that the electrode assembly 1 may be damaged when the electrode assembly 1 is inserted into a battery can in the subsequent secondary battery assembly process.
[0032] 2(a) and 2(b) are photographs showing the case where wrinkles and lifting occurred in the first electrode current collector in a conventional electrode assembly according to a comparative example of the present invention, and FIG. 3(a) is a photograph showing the case where wrinkles and air bubbles occurred in the first electrode current collector and swelling tape in a conventional electrode assembly according to a comparative example of the present invention, and FIG. 3(b) is a photograph showing the case where the wrinkles and air bubbles in the first electrode current collector and swelling tape were transferred to the separator.
[0033] 2(a) and 2(b), in a conventional electrode assembly, when the swelling tape 40 is attached to the uncoated portion 15 of the first electrode collector 11 instead of the one-sided coated portion 14, wrinkles and lifting may occur due to the characteristics of the thin collector 11. If wrinkles and lifting occur in the first electrode collector 11, the electrode assembly 1 may be damaged, such as the first electrode collector 11 being torn or broken, when the electrode assembly 1 is inserted into a battery can in a future secondary battery assembly process.
[0034] FIG. 3(a) shows a conventional electrode assembly in which a swelling tape is attached to the uncoated portion of a first electrode current collector instead of the one-sided coated portion. The photograph on the left shows a case in which air bubbles are generated when the swelling tape is attached, causing wrinkles and air bubbles in the swelling tape, and the photograph on the right shows a case in which wrinkles are generated on the first electrode current collector due to the generation of wrinkles and air bubbles when the swelling tape is attached.
[0035] FIG. 3(b) shows a case where wrinkles and air bubbles generated in the first electrode current collector and the swelling tape are transferred to the separator.
[0036] Referring to Figures 3(a) and 3(b), if wrinkles generated in the first electrode collector 11 and the swelling tape 40 are transferred to the separator 30, they may have a direct effect on the electrode, for example, there is a risk of the electrode active material being precipitated.
[0037] Furthermore, if wrinkles occur in the first electrode collector 11, when the electrode assembly 1 including the first electrode collector 11 is inserted into a can, the electrode assembly 1 may be damaged, for example, the outermost collector 11 may break.
[0038] 4 and 5 are a schematic diagram and a perspective view showing a configuration in which a first electrode 100 and a second electrode 200 face each other in an electrode assembly 111 according to an embodiment of the present invention, and FIG. 6 is a schematic plan view showing an end perpendicular to the winding axis direction in a jelly roll 610 in which an electrode assembly 111 according to an embodiment of the present invention is wound up.
[0039] 4 to 6, the electrode assembly 111 has a swelling tape 410 provided to cover the boundary between a one-sided coated portion 140 in which the first active material layer 120 is provided only on one side of the first electrode collector 110, and an uncoated portion 150 in which the first and second active material layers 120, 130 are not provided. This minimizes the occurrence of wrinkles in the first electrode collector 110, thereby controlling the risk of poor appearance, and eliminates the risk of damage to the electrode assembly 111 when the electrode assembly 111 is inserted into a battery can 620 during the secondary battery assembly process.
[0040] According to one embodiment of the present invention, the electrode assembly 111 has a structure in which a first electrode 100, a separator 300, and a second electrode 200 are stacked, and the first electrode includes a current collector 110, and a first active material layer 120 and a second active material layer 130 respectively provided on both sides of the current collector 110.
[0041] One end of the first electrode 100 includes a one-sided coated portion 140 in which the first active material layer 120 is provided on one side of the current collector 110 and the second active material layer 130 is not provided on the other side; and an uncoated portion 150 in which the first active material layer 120 and the second active material layer 130 are not provided on both sides of the current collector 110.
[0042] In addition, the electrode assembly 111 includes a swelling tape 410 provided to cover the boundary between the first active material layer 120 and the uncoated portion 150 of the one-sided coated portion 140 .
[0043] Since the swelling tape 410 is attached from the active material application portion of the first electrode 100, the occurrence of air bubbles and wrinkles in the swelling tape 410 can be suppressed, and thus the occurrence of wrinkles in the first electrode collector 110 can be minimized.
[0044] The first electrode 100 is not particularly limited, and may be manufactured in a form in which the first active material layer 120 and the second active material layer 130 are bonded to the first electrode current collector 110 by a conventional method well known in the art.
[0045] As an example, the first active material layer 120 provided on one side of the current collector 110 in the one-sided coating portion 140 of the first electrode 100 may be an active material coated portion of the first electrode 100, and the uncoated portion 150 in the first electrode 100 in which the first active material layer 120 and the second active material layer 130 are not provided on both sides of the current collector 110 may be a plain portion of the first electrode 100.
[0046] The swelling tape 410 is provided to cover the boundary between the first active material layer 120 and the uncoated portion 150 of the one-sided coated portion 140 of the first electrode 100. When the electrode assembly 111 is subsequently housed in a battery can 620, the swelling tape 410 expands due to the electrolyte, and the wound electrode assembly 111 is pushed from the center of the winding toward the outer side of the winding, so that the first electrode collector 110 abuts against the battery can 620, thereby acting as a tab.
[0047] In this case, the winding center of the wound electrode assembly 111 may be a core portion of the electrode assembly 111 .
[0048] According to an embodiment, the electrode assembly 111 further includes a swelling tape 400 provided on the other surface of the one-sided coating portion 140 on which the second active material layer 130 is not provided.
[0049] When the electrode assembly 111 is repeatedly charged and discharged, one end of the second electrode 200 contracts or expands, and stress is concentrated on the facing first electrode portion, which may cause cracks. However, the occurrence of the cracks can be prevented by further including a swelling tape 400 provided on the other side of the one-sided coating portion 140 where the second active material layer 130 is not provided.
[0050] In addition, when the single-sided coated portion 140 further includes a swelling tape 400 provided on the other side thereof where the second active material layer 130 is not provided, the swelling tape 400 is provided so as not to overlap with the swelling tape 410 provided to cover the boundary between the first active material layer 120 and the uncoated portion 150, and the swelling tape 400 expands to push the first electrode collector 110 from the outer winding portion toward the center of the winding, so that the first electrode collector 110 is closely attached to the battery can 620, thereby reducing resistance and providing a heat dissipation effect.
[0051] According to one embodiment, the first active material layer 120 is disposed on a surface facing the second electrode 200 with the separator 300 interposed therebetween, and is longer than the second electrode 200 in the longitudinal direction (P) of the electrode assembly.
[0052] The electrode assembly 111 may be in the form of a wound jelly roll, and the length direction (P) of the electrode assembly refers to a direction (P) perpendicular to the winding axis of the wound electrode assembly.
[0053] Since the first active material layer 120 is disposed longer than the second electrode 200 in the longitudinal direction (P) of the electrode assembly on the surface facing the second electrode 200 with the separator 300 interposed therebetween, the first active material layer 120 can be positioned to face the second electrode 200 with the separator 300 interposed therebetween even when the electrode assembly 111 is wound up. In this case, damage to the separator 300 can be prevented even when the electrode assembly 111 is charged, and a reduction in the battery life can be prevented.
[0054] According to an embodiment, the second active material layer 130 of the electrode assembly 111 is provided shorter than the second electrode 200 in the length direction (P) of the electrode assembly.
[0055] The electrode assembly 111 may be in the form of a wound jelly roll, and the length direction (P) of the electrode assembly refers to a direction (P) perpendicular to the winding axis of the wound electrode assembly.
[0056] The second active material layer 130 may be shorter than the second electrode 200 in the length direction (P) of the electrode assembly, and may be shorter than the first active material layer 120, which is longer than the second electrode 200 in the length direction (P) of the electrode assembly. Thus, the first and second active material layers 120 and 130 of the first electrode 100 may be provided in a mismatched form, and the first electrode collector 110 provided on the outer circumferential surface of the jelly roll 610 may be exposed toward the outer side when the electrode assembly 111 is wound up.
[0057] According to one embodiment, the electrode assembly 111 is in a wound jelly roll form and the first electrode 100 is the outermost electrode of the wound jelly roll electrode assembly 610.
[0058] The first electrode 100 is the outermost electrode of the wound jelly roll type electrode assembly 610, and a first electrode collector 110 included in the first electrode 100 may be exposed toward the outer side at the outer circumferential surface of the wound jelly roll 610.
[0059] According to one embodiment, the swelling tape 410 provided to cover the boundary between the first active material layer 120 and the uncoated portion 150 is provided on the inner peripheral surface of the first electrode 100 of the jelly roll type electrode assembly 610. Thus, the first electrode current collector 110 is used as an outer tab, and the area of the current collector 110 that contacts the battery can 620 to transfer heat can be increased, improving the heat generation level and increasing the energy density of the electrode.
[0060] The first electrode 100, which is the outermost electrode of the wound jelly roll type electrode assembly 610, includes the swelling tape 410 provided to cover the boundary between the first active material layer 120 and the uncoated portion 150 of the one-sided coated portion 140. When the electrode assembly 111 is subsequently housed in a battery can 620, the swelling tape 410 expands due to an electrolyte, pushing the wound electrode assembly 111 from the center toward the outer side of the winding, so that the first electrode collector 110 abuts against the battery can 620, thereby acting as a tab.
[0061] According to one embodiment, the first electrode collector 110 in the electrode assembly 111 includes copper. The first electrode collector 110 in the electrode assembly 111 may be made of any material known in the art, and non-limiting examples of the first electrode collector 110 include foil made of copper, gold, nickel, or a copper alloy, or a combination thereof.
[0062] According to an example, in the electrode assembly 111, if the first electrode collector 110 contains copper, when the electrode assembly 111 is subsequently housed in a battery can 620, the first electrode collector 110 may abut against the battery can 620 and serve as a tab, and at this time, the first electrode collector 110 may be electrically connected to the battery can 620.
[0063] According to an example, in the electrode assembly 111, the first electrode 100 is a negative electrode and the second electrode 200 is a positive electrode.
[0064] According to one embodiment of the present invention, in the electrode assembly 111, the length (460) of the swelling tape in the longitudinal direction (P) of the electrode assembly is 30 mm or less.
[0065] The electrode assembly 111 may be in the form of a wound jelly roll, and the length direction (P) of the electrode assembly refers to a direction (P) perpendicular to the winding axis of the wound electrode assembly.
[0066] The length (460) of the swelling tape may be 30 mm or less, 28 mm or less, 25 mm or less, 23 mm or less, or 21 mm or less. The length (460) of the swelling tape may be 10 mm or more, 13 mm or more, 15 mm or more, or 17 mm or more.
[0067] If the length of the swelling tape (460) exceeds 30 mm, the area where one long swelling tape is attached to the uncoated portion becomes long, and the first electrode current collector may wrinkle severely. If the length of the swelling tape (460) is less than 10 mm, the force of the swelling tape expanded by the electrolyte when the electrode assembly is housed in a battery can in the future is weak, and the first electrode current collector cannot be used as a tab.
[0068] According to one embodiment, the length (420) of the swelling tape covering the first active material layer in the length direction (P) of the electrode assembly may be 1 mm to 3 mm. The range may be variously set according to the size, length, and ratio of the electrode assembly.
[0069] For example, the length (420) of the swelling tape covering the first active material layer in the length direction (P) of the electrode assembly may be 1 mm or more, 1.3 mm or more, or 1.5 mm or more. For example, the length (420) of the swelling tape covering the first active material layer in the length direction (P) of the electrode assembly may be 3 mm or less, 2.7 mm or less, or 2.5 mm or less.
[0070] When the length (420) of the swelling tape covering the first active material layer satisfies the above range, the generation of air bubbles in the swelling tape 410 can be minimized to control the risk of poor appearance, and the risk of damage to the electrode assembly 111 when the electrode assembly 111 is inserted into the battery can 620 during the assembly process of the secondary battery 600 can be eliminated.
[0071] The length (460) of the swelling tape is equal to the sum of the length (420) of the swelling tape covering the first active material layer in the longitudinal direction (P) of the electrode assembly and the length (440) of the swelling tape covering the uncoated portion.
[0072] According to one embodiment, in the electrode assembly 111, the width (470) of the swelling tape in the width direction (H) of the electrode assembly is 50% or more of the 100% width of the electrode assembly.
[0073] The electrode assembly 111 may be in the form of a wound jelly roll, and the width direction (H) of the electrode assembly refers to the direction of the winding axis (H) of the wound electrode assembly.
[0074] The width (470) of the swelling tape may be 50% or more, 55% or more, 60% or more, 65% or more, or 70% or more of the 100% width of the electrode assembly. The width (470) of the swelling tape may be 100% or less, 98% or less, or 96% or less of the 100% width of the electrode assembly.
[0075] If the width (470) of the swelling tape falls within the above range, when the electrode assembly 111 is subsequently housed in the battery can 620, the swelling tape 410 expands due to the electrolyte, and the first electrode collector 110 abuts against the battery can 620, thereby effectively functioning as a tab.
[0076] According to one embodiment, the swelling tape 410 is arranged to cover an end of the first active material layer 120 of the one-sided coating portion 140, and the area (430) of the swelling tape covering the first active material layer 120 is 5% to 20%.
[0077] The area (430) of the swelling tape covering the first active material layer 120 is 5% or more, 6% or more, 7% or more, or 8% or more. The area (430) of the swelling tape covering the first active material layer 120 is 20% or less, 18% or less, 16% or less, or 14% or less.
[0078] When the area (430) of the swelling tape covering the first active material layer 120 satisfies the above range, the generation of air bubbles in the swelling tape 410 can be minimized to control the risk of poor appearance, and the risk of damage to the electrode assembly 111 when the electrode assembly 111 is inserted into the battery can 620 during the assembly process of the secondary battery 600 can be eliminated.
[0079] In addition, when the electrode assembly 111 is subsequently housed in the battery can 620, the swelling tape 410 expanded by the electrolyte can bring the first electrode collector 110 into contact with the battery can 620, thereby effectively functioning as a tab.
[0080] According to one example, the swelling tape 410 does not overlap the second electrode 200 .
[0081] The swelling tape 410 does not overlap with the second electrode 200 so that lithium ions of the second electrode 200 can be fully utilized, and is provided to cover the boundary between the first active material layer 120 and the uncoated portion 150 of the one-sided coated portion 140 of the first electrode 100 so that it can be effectively attached to the uncoated portion of the first electrode. Thus, the first electrode collector 110, which is the uncoated portion of the first electrode, can be pressed outwardly so as to be in good contact with the battery can 620.
[0082] According to one embodiment, the swelling tape 410 is expanded by an electrolyte. The electrolyte may include an organic solvent, such as ethylene carbonate (EC), dimethyl carbonate (DMC), or ethyl methyl carbonate (EMC). The solvent of the electrolyte may cause the swelling tape 410 to expand.
[0083] The swelling tape 410 may expand through an activation process and a cycle. Whether the swelling tape 410 expands or not can be confirmed by checking whether the direct current resistance (DCR) converges as the cycle progresses after the activation process.
[0084] Specifically, the AC resistance (ACR) may vary depending on the outer diameter of the jelly roll 610 in which the electrode assembly 111 is wound up. That is, when the outer diameter of the jelly roll 610 is large, the first electrode collector 110 can be in sufficient contact with the battery can 620, and the resistance is low, resulting in a small AC resistance (ACR). Conversely, when the outer diameter of the jelly roll 610 is small, the first electrode collector 110 cannot be in sufficient contact with the battery can 620, and the resistance is relatively high, resulting in a large AC resistance (ACR).
[0085] When cycling is performed after the activation process, the performance of the cell can be determined by the direct current resistance (DCR) rather than the alternating current resistance (ACR). The direct current resistance (DCR) varies at the beginning of the cycle, but as the cycle progresses, the swelling tape 410 expands sufficiently, so that the direct current resistance (DCR) can converge to a constant value.
[0086] Therefore, it can be determined that the swelling tape 410 is sufficiently expanded based on the converged value of the DC resistance (DCR). For example, it can be determined that the swelling tape 410 is sufficiently expanded based on the convergence of the DC resistance (DCR) to the same DC resistance (DCR) after 100 cycles following the activation process.
[0087] [Table 1]
[0088] For example, referring to Table 1, it can be seen that cells having different AC resistances (ACR) converge to the same DC resistance (DCR) after 100 cycles, and therefore it can be determined that the swelling tape 410 according to the present invention has been sufficiently expanded. The swelling tape 410 may be immersed in a liquid to expand or become flexible, and may be made of a polymer material.
[0089] The polymer material has a characteristic that the volume of the polymer material can be increased by the penetration of solvent molecules between the chains of the polymer material. Therefore, the swelling tape 410 expands or becomes flexible when it absorbs the electrolyte, so that when the electrode assembly 111 is inserted into the battery can 620, the swelling tape 410 expands due to the electrolyte, and the first electrode collector 110 abuts against the battery can 620, thereby effectively functioning as a tab.
[0090] According to an embodiment, the swelling tape 410 includes polyurethane. The swelling tape 410 expands due to the electrolyte, and at this time, the polyurethane included in the swelling tape 410 may expand due to the solvent of the electrolyte. As the swelling tape 410 expands, the first electrode current collector 110 can abut against the battery can 620 and effectively function as a tab.
[0091] According to one embodiment of the present invention, there is provided a method for manufacturing an electrode assembly 111 by stacking a first electrode 100, a separator 300, and a second electrode 200, the method including the steps of: manufacturing an electrode assembly in which the first electrode 100 includes a current collector 110, and a first active material layer 120 and a second active material layer 130 respectively provided on both sides of the current collector 110, and one end of the first electrode 100 includes a one-sided coated portion 140 in which the first active material layer 120 is provided on one side of the current collector and the second active material layer 130 is not provided on the other side, and an uncoated portion 150 in which the first active material layer 120 and the second active material layer 130 are not provided on both sides of the current collector 110; and disposing a swelling tape 410 provided to cover a boundary between the first active material layer 120 and the uncoated portion 150 of the one-sided coated portion 140.
[0092] The first electrode of the electrode assembly 111 includes a swelling tape 410 provided to cover the boundary between a one-sided coated portion 140 in which the first active material layer 120 is provided only on one side of the current collector 110, and an uncoated portion 150 in which the first and second active material layers 120, 130 are not provided. This minimizes the occurrence of wrinkles in the current collector 110, thereby controlling the risk of poor appearance, and eliminates the risk of damage to the electrode assembly 111 when the electrode assembly 111 is inserted into a battery can 620 during the assembly process of the secondary battery 600.
[0093] According to an example, the electrode assembly 111 is similar to the electrode assembly 111 according to the above-described embodiment.
[0094] According to an embodiment, the method of manufacturing the electrode assembly 111 further includes the step of disposing a swelling tape 400 on the other side of the one-sided coating portion 140 on which the second active material layer 130 is not provided.
[0095] When the electrode assembly 111 is repeatedly charged and discharged, one end of the second electrode 200 contracts or expands, and stress is concentrated in the facing portion of the first electrode 100, which may cause cracks. However, when the electrode assembly 111 further includes a swelling tape 400 provided on the other side where the second active material layer 130 is not provided, the occurrence of the cracks can be prevented.
[0096] In addition, when the single-sided coated portion 140 further includes a swelling tape 400 provided on the other side thereof where the second active material layer 130 is not provided, the swelling tape 400 may be provided so as not to overlap with the swelling tape 410 provided to cover the boundary between the first active material layer 120 and the uncoated portion 150. The swelling tape 400 expands to push the first electrode collector 110 from the outer winding portion toward the center of the winding, so that the first electrode collector 110 is closely attached to the battery can 620, thereby reducing resistance and providing a heat dissipation effect.
[0097] The swelling tape 400 provided on the other surface on which the second active material layer 130 is not provided may be provided spaced apart (a distance 450 between the second active material layer and the swelling tape) from the second active material layer 130 of the electrode assembly 111. By providing the swelling tape 400 spaced apart (a distance 450 between the second active material layer and the swelling tape) from the second active material layer, it is possible to prevent cracks from occurring due to stress concentration when the swelling tape 400 expands due to an electrolyte, and to ensure good adhesion between the first electrode collector 110 and the battery can 620.
[0098] According to one embodiment, the manufacturing method of the electrode assembly 111 further includes a step of providing an adsorption pad 500 on the swelling tape 410 arranged to cover the boundary between the first active material layer 120 and the uncoated portion 150 of the one-sided coated portion 140, and pressing and attaching the swelling tape 410 from the one-sided coated portion 140 of the first electrode toward the uncoated portion 150 using the adsorption pad 500.
[0099] According to an example, the suction pad 500 may have a step portion 510 that is thicker in a direction toward the one-side coated portion 140 than the uncoated portion 150 of the first electrode.
[0100] By using the suction pad 500 having the stepped portion 510, the swelling tape 410, which is provided to cover the boundary between the first active material layer 120 and the uncoated portion 150 of the one-sided coating portion 140 of the first electrode, can be pressed from the one-sided coating portion 140 of the first electrode toward the uncoated portion 150, thereby suppressing the generation of air bubbles and wrinkles in the swelling tape 410 and thereby minimizing the generation of wrinkles in the first electrode collector 110.
[0101] According to one embodiment of the present invention, there is provided an electrode assembly 111 prepared by the manufacturing method of the electrode assembly 111 described above.
[0102] The electrode assembly 111 is similar to the electrode assembly 111 according to the above-described embodiment.
[0103] Figure 6 of For reference, the sealing tape 630 may be attached to both ends of the electrode assembly in the winding axis direction (H), and may be, for example, a PET tape, but is not limited thereto.
[0104] Since the sealing tape 630 is attached to both ends of the electrode assembly in the winding axis direction (H), the first electrode collector 110 at the outermost part of the electrode assembly 111 that is exposed to the outside without the sealing tape 630 attached can directly abut against the battery can 620 and serve as an electrode tab.
[0105] The sealing tape 630 may be attached to 90% or more, 92% or more, or 94% or more of the outer diameter of the electrode assembly 111. The sealing tape 630 may be attached to 100% or less, 99% or less, or 98% or less of the outer diameter of the electrode assembly 111.
[0106] When this range is met, the sealing tape 630 can prevent the outer diameter of the electrode assembly 111 from increasing, prevent the electrode assembly 111 from loosening, and facilitate the electrode assembly 111 being inserted into the battery can 620.
[0107] figure 7 1 is a photograph showing a case where no wrinkles are generated in a first electrode current collector and a swelling tape in an electrode assembly according to an embodiment of the present invention.
[0108] Figure 4 and 7 2, the first electrode of the electrode assembly 111 includes a swelling tape 410 to cover the boundary between a one-sided coated portion 140 in which the first active material layer 120 is provided only on one side of the current collector 110, and an uncoated portion 150 in which the first and second active material layers 120 and 130 are not provided, thereby preventing wrinkles from occurring in the current collector 110 and the swelling tape 410. By preventing wrinkles from occurring in the current collector 110 and the swelling tape 410, the risk of poor appearance of the electrode assembly 111 can be controlled, and the risk of damage to the electrode assembly 111 when the electrode assembly 111 is inserted into a battery can 620 in the assembly process of the secondary battery 600 can be eliminated.
[0109] figure 8 1 is a photograph showing a case where a lifting phenomenon of a first electrode collector occurs in an electrode assembly according to a comparative example of the present invention and a portion where the lifting height of the first electrode collector is measured.
[0110] Figure 4 and 8 Referring to the above, the first electrode of the electrode assembly 111 includes a swelling tape 410 to cover the boundary between a one-sided coated portion 140 in which the first active material layer 120 is provided only on one side of the current collector 110, and an uncoated portion 150 in which the first and second active material layers 120, 130 are not provided, thereby preventing the current collector 110 from floating up.
[0111] A conventional swelling tape 40 is provided on the uncoated portion 15 of the first electrode, but due to the characteristics of the thin current collector, wrinkles are likely to occur when the swelling tape 40 is applied, which may cause lifting of the first electrode current collector 11. The lifting of the first electrode current collector 11 can be confirmed by measuring the lifting height (d) of the first electrode current collector using a 3D shape measuring device.
[0112] At an end of a first electrode collector provided at a winding end of a wound jelly roll type electrode assembly, a space may be formed between the end of the first electrode collector and the first electrode collector wound before the winding end due to the lifting of the first electrode collector. The lifting height (d) of the first electrode collector refers to the height of the highest part in the winding outer direction among the spaces between the wound first electrode collectors, and the degree of lifting of the first electrode collector can be determined by measuring the lifting height.
[0113] The swelling tape 410 provided to cover the boundary of the uncoated portion 150 according to an embodiment of the present invention is located on the inner peripheral surface of the outermost part of the first electrode collector 110 in the wound jelly roll type electrode assembly 610. The portion of the swelling tape 410 covering the boundary between the first active material layer and the uncoated portion prevents the first electrode collector 110 from wrinkling or lifting, thereby controlling the risk of poor appearance of the electrode assembly 111 and eliminating the risk of damage to the electrode assembly 111 when the electrode assembly 111 is inserted into a battery can 620 in the assembly process of the secondary battery 600.
[0114] According to one embodiment of the present invention, there is provided a secondary battery 600 including an electrode assembly 111 according to the above-described embodiment; an electrolyte; and a battery can 620 that contains the electrode assembly 111 and the electrolyte.
[0115] According to an example, the first electrode current collector 110 is electrically connected to the battery can 620 .
[0116] The secondary battery 600 includes an electrode assembly 111 according to the above-described embodiment housed in a battery can 620. At this time, the swelling tape 410 expanded by the electrolyte pushes the first electrode collector 110 from the center of the winding toward the outer side of the winding, so that the first electrode collector 110 is electrically connected to the battery can 620 to serve as a tab.
[0117] The swelling tape 410 is arranged to cover the boundary between the first active material layer 120 and the uncoated portion 150 of the one-sided coated portion 140 of the first electrode 100. When the electrode assembly 111 expands due to the electrolyte when the electrode assembly 111 is housed in the battery can 620, the swelling tape 410 pushes the wound electrode assembly 111 from the center of the winding toward the outer side of the winding, so that the first electrode collector 110 abuts against the battery can 620, thereby acting as a tab.
[0118] The secondary battery 600 may include the electrode assembly 111 according to the above-described embodiment, an electrolyte, a battery can 620 for containing them, and a top cap.
[0119] In the electrode assembly 111, the first electrode 100 may be a negative electrode, and the second electrode 200 may be a positive electrode having a polarity opposite to that of the first electrode 100. The first electrode 100 and the second electrode 200 may have a sheet shape. The electrode assembly 111 may have, for example, a jellyroll shape. That is, the electrode assembly 111 may be manufactured by winding up a stack formed by sequentially stacking the first electrode 100, the separator 300, the second electrode 200, and the separator 300 at least once in a winding direction (W).
[0120] In the present invention, the positive electrode active material coated on the positive electrode plate and the negative electrode active material coated on the negative electrode plate may be any active material known in the art without any limitations.
[0121] Non-limiting examples of the positive electrode active material include conventional positive electrode active materials that can be used for the positive electrodes of conventional electrochemical elements, and in particular, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or a lithium composite oxide that is a combination of these.
[0122] In one example, the positive electrode active material has the general chemical formula A[A x M y ]O 2+z (A includes at least one element selected from Li, Na, and K; M includes at least one element selected from Ni, Co, Mn, Ca, Mg, Al, Ti, Si, Fe, Mo, V, Zr, Zn, Cu, Al, Mo, Sc, Zr, Ru, and Cr; x≧0, 1≦x+y≦2, −0.1≦z≦2; x, y, z, and the stoichiometric coefficients of the components included in M are selected such that the compound remains electrically neutral).
[0123] In another example, the positive electrode active material is an alkali metal compound xLiM disclosed in US Pat. No. 6,677,082, US Pat. No. 6,680,143, etc. 1 O2-(1-x)Li2M 2 O3(M 1 contains at least one element having an average oxidation state of 3; M 2 contains at least one element having an average oxidation state of 4; 0≦x≦1).
[0124] In another embodiment, the positive electrode active material has the general chemical formula Li a M 1 x Fe 1-x M 2 P y1-y M 3 z O 4-z (M 1 contains at least one element selected from Ti, Si, Mn, Co, Fe, V, Cr, Mo, Ni, Nd, Al, Mg, and Al; M 2contains at least one element selected from Ti, Si, Mn, Co, Fe, V, Cr, Mo, Ni, Nd, Al, Mg, Al, As, Sb, Si, Ge, V, and S; M 3 contains halogen elements, optionally including F; <a≦2、0≦x≦1、0≦y<1、0≦z<1;a、x、y、z、M 1 , M 2 , and M. 3 wherein the stoichiometric coefficients of the components included are selected to maintain the compound electrically neutral), or lithium metal phosphate, represented by Li3M2(PO4)3, where M comprises at least one element selected from Ti, Si, Mn, Fe, Co, V, Cr, Mo, Ni, Al, Mg, and Al.
[0125] Preferably, the positive electrode active material may contain primary particles and / or secondary particles formed by agglomeration of the primary particles.
[0126] Non-limiting examples of the negative electrode active material include conventional negative electrode active materials that can be used in the negative electrodes of conventional electrochemical devices, and in particular, lithium metal or lithium alloys, carbon, petroleum coke, activated carbon, graphite, or other carbon-based lithium adsorbent materials, etc.
[0127] In one example, the negative electrode active material may be a carbon material, lithium metal or a lithium metal compound, silicon or a silicon compound, tin or a tin compound, etc. Metal oxides such as TiO2 and SnO2 having a potential of less than 2 V may also be used as the negative electrode active material. The carbon material may be either low-crystalline carbon or high-crystalline carbon.
[0128] Non-limiting examples of positive electrode current collectors include foils made of aluminum, nickel, or a combination thereof.
[0129] As the separator 300, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, etc., can be used alone or in a laminated form. As another example, as the separator 300, a general porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, etc. can be used.
[0130] At least one surface of the separator 300 may include a coating layer of inorganic particles. Alternatively, the separator 300 itself may be made of a coating layer of inorganic particles. The particles constituting the coating layer may have a structure in which they are bound to a binder such that there is an interstitial volume between adjacent particles.
[0131] The inorganic particles may be made of an inorganic material having a dielectric constant of 5 or more. As a non-limiting example, the inorganic particles may be Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT), PB(Mg3Nb 2 / 3 )O3-PbTiO3 (PMN-PT), BaTiO3, hafnia (HfO2), SrTiO3, TiO2, Al2O3, ZrO2, SnO2, CeO2, MgO, CaO, ZnO, and Y2O3.
[0132] The electrolyte is A + B - The salt may have the structure: + Li + , Na + , K + The cations include alkali metal cations such as B - F - , Cl - , Br- , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , AlO4 - , AlCl4 - , PF6 - , SbF6 - , AsF6 - , BF2C2O4 - , BC4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , C4F9SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - The anion includes one or more anions selected from the group consisting of:
[0133] The electrolyte can be dissolved in an organic solvent. Examples of the organic solvent include propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), γ-butyrolactone, and mixtures thereof.
[0134] Another embodiment of the present invention provides a battery pack 700 including at least one of the secondary batteries 600 described above.
[0135] As an example, the secondary battery 600 may be a cylindrical secondary battery.
[0136] The cylindrical secondary battery 600 according to the above-described embodiment can be used to manufacture a battery pack 700.
[0137] figure 9 1 is a diagram showing a schematic configuration of a battery pack 700 including a secondary battery 600 according to an embodiment of the present invention.
[0138] figure 91, a battery pack 700 according to an embodiment of the present invention includes an assembly of electrically connected cylindrical secondary batteries 600 and a pack housing 710 that accommodates the assembly. The cylindrical secondary battery 600 is the secondary battery 600 according to the above-described embodiment. For ease of illustration, components such as a bus bar for electrically connecting the cylindrical secondary batteries, a cooling unit, and external terminals are omitted from the drawings.
[0139] Another embodiment of the present invention provides an automobile 800 including at least one of the battery packs 700 described above. The battery pack 700 may be mounted on the automobile 800. The automobile 800 may be, for example, an electric vehicle, a hybrid vehicle, or a plug-in hybrid vehicle. The automobile may be a four-wheeled vehicle or a two-wheeled vehicle.
[0140] figure 10 The figure 9 1 is a diagram for explaining an automobile 800 including a battery pack 700. FIG.
[0141] figure 10 1, an automobile 800 according to an embodiment of the present invention includes a battery pack 700 according to an embodiment of the present invention. The automobile 800 operates by receiving power from the battery pack 700 according to an embodiment of the present invention.
[0142] Working Example Example 1 (1) Manufacturing of electrode assemblies An electrode assembly was manufactured by sequentially stacking a negative electrode (negative electrode current collector: Cu foil, negative electrode active material: artificial graphite and natural graphite, each 50 parts by weight), a sheet-shaped polyethylene separator, a positive electrode (positive electrode current collector: Al foil, active material: LiCoO2), and the polyethylene separator. The thickness of the negative electrode was 187 μm (Cu foil current collector: 10 μm), the thickness of the positive electrode was 147 μm (Al foil current collector: 15 μm), and two separators, each 13 μm thick, were used.
[0143] The negative electrode includes a one-sided coated portion in which a negative electrode active material layer is provided on the surface of the Cu foil facing the positive electrode and no negative electrode active material layer is provided on the other surface of the Cu foil, and an uncoated portion in which no negative electrode active material layer is provided on either surface of the Cu foil. Therefore, a swelling tape made of polyurethane material was attached to the one-sided coated portion so as to cover the boundary between the negative electrode active material layer provided on the surface facing the positive electrode and the uncoated portion, with the separator interposed therebetween.
[0144] The swelling tape was arranged so that the length of the swelling tape covering the negative electrode active material layer in the length direction (P) of the electrode assembly was 2 mm, and the swelling tape was located on the inner peripheral surface of the outermost part of the Cu foil in the wound jelly roll type electrode assembly. In this case, the area of the swelling tape covering the negative electrode active material layer was set to 5% to 20%. The swelling tape (PU material) used was 20 mm in the length direction (P) of the electrode assembly, 62 mm in the width direction (H) of the electrode assembly, and 52 μm in thickness.
[0145] In addition, in the negative electrode, a swelling tape made of polyurethane material was further attached to the outer peripheral surface of the outermost part of the Cu foil in the wound jelly roll type electrode assembly. At this time, the swelling tape was attached so as to cover the end of the positive electrode. The swelling tape (PU material) used had a length direction (P) of 20 mm, a width direction (H) of 62 mm, and a thickness of 52 μm.
[0146] Next, the laminated electrode assembly including the swelling tape was wound up to manufacture a jelly roll type electrode assembly (end diameter: 20.38 mm to 20.64 mm). At this time, the cross-sectional diameter of the manufactured electrode assembly was 20.4 mm, and the length in the winding axis direction (H) was 66 mm.
[0147] A seal tape made of PET material was attached to both ends of the winding shaft of the wound electrode assembly. The seal tape (PET material) used had a size of 62 mm in the length direction (P) of the electrode assembly, 10 mm in the width direction (H) of the electrode assembly, and a thickness of 22 μm.
[0148] (2) Manufacture of secondary batteries The wound electrode assembly was inserted into a battery can (cross-sectional diameter: 20.95 mm to 21.15 mm), and an electrolyte prepared by mixing ethylene carbonate (EC): ethyl methyl carbonate (EMC) in a volume ratio of 30:70 and dissolving LiPF6 to a concentration of 1.0 M was poured into the battery can. The cylindrical battery can was then sealed with a cap assembly to manufacture a secondary battery.
[0149] Comparative Example 1 An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that a swelling tape was attached onto the negative electrode current collector so as not to cover the end of the negative electrode active material layer provided on the surface facing the positive electrode.
[0150] Experimental Example Experimental Example 1. Number of electrode assemblies A total of 59,200 jelly roll-type electrode assemblies were manufactured and wound in the same manner as in Example 1.
[0151] A total of 1024 jelly-roll type electrode assemblies were manufactured and wound in the same manner as the electrode assembly of Comparative Example 1.
[0152] Experimental Example 2. Wrinkling and lifting of negative electrode current collector The wrinkles on the negative electrode current collector were observed by visual inspection and by the naked eye, as wrinkles formed on the plain part of the current collector due to air bubbles when the swelling tape was applied. In the case of Example 1, 1024 pieces, which is the same number as in Comparative Example 1, were inspected by the naked eye, and the rest were not judged to be defective in the visual inspection, so they were not inspected by the naked eye. In this case, the visual inspection is an inspection in which an example photo of wrinkles is input into the vision, and if a similar case is found, it is judged to be defective.
[0153] The phenomenon of the negative electrode current collector floating when the swelling tape was applied was measured using a 3D shape measuring instrument (Keyence shape measuring instrument, model name: KEYENCE KOREA, One Shot 3D VR3200). In this case, the degree of floating of the negative electrode current collector was determined by measuring the height of the space formed between the end of the negative electrode current collector provided at the winding end of the wound jelly roll type electrode assembly and the negative electrode current collector wound before the winding end due to the floating of the negative electrode current collector. That is, the floating height (d) of the negative electrode current collector was determined by measuring the height of the highest part in the winding outer direction in the space between the wound negative electrode current collectors. When the diameter of the end of the electrode assembly was 20.38 mm to 20.64 mm, if the floating height (d) of the negative electrode current collector was 0.8 mm or more, it was determined to be defective.
[0154] Experimental example 3. Outer diameter defect The outer diameter of the end of the wound jelly roll type electrode assembly perpendicular to the winding axis direction was measured by an outer diameter measuring device of the winder conveyor or by a stop gauge in which holes were previously drilled for each diameter.
[0155] The diameter of the end perpendicular to the winding axis direction of the electrode assembly manufactured in Example 1 was 20.38 mm to 20.64 mm. Therefore, when the diameter of the end perpendicular to the winding axis direction of the electrode assembly exceeds 20.64 mm, it is indicated that there is an outer diameter defect.
[0156] Experimental example 4. Damage caused when inserting into a battery can The outer diameter of the end perpendicular to the winding axis of the wound jelly roll-type electrode assembly (diameter of the end perpendicular to the winding axis of the electrode assembly: 20.38mm to 20.64mm) increases, or the outermost current collector is torn or broken when the wound electrode assembly is inserted into a battery can due to wrinkles and lifting of the current collector. This is called damage.
[0157] That is, when inserting a wound jelly roll type electrode assembly into a battery can, an insertion guide is used to facilitate the insertion of the jelly roll into the can. However, if the electrode assembly does not fit into the insertion guide and is ejected as an error, it is removed from the battery can again and inspected with the naked eye to indicate that damage occurred during insertion into the battery can.
[0158] Experimental example 5. Separator wrinkles If the separator had wrinkles or folds transferred from the wrinkles of the swelling tape, the separator was observed with the naked eye and marked as having wrinkles. In this case, the wrinkles were defined as wrinkles that felt like a foreign object when touched with the hand, not wrinkles that simply had a wavy shape.
[0159] In the case of Example 1, 1024 pieces, which is the same number as in Comparative Example 1, were inspected with the naked eye, and the rest were not inspected with the naked eye because they were not judged to be defective in the appearance vision inspection. In this case, the appearance vision inspection is an inspection in which an example photo of wrinkles is input into the vision, and if a similar case is found, it is judged to be defective.
[0160] [Table 2]
[0161] Referring to Table 2, it can be seen that the electrode assembly manufactured in Example 1 of the present invention has no wrinkles or lifting on the current collector, and therefore no outer diameter defects due to the wrinkles, and therefore no damage when inserted into a can, compared to the electrode assembly manufactured in Comparative Example 1. It can also be seen that the electrode assembly manufactured in Example 1 of the present invention has no wrinkles formed on the current collector that are transferred to the separator as wrinkles, compared to the electrode assembly manufactured in Comparative Example 1. Although the present invention has been described above with reference to limited embodiments and drawings, the present invention is not limited thereto, and various embodiments may be made within the technical spirit of the present invention and the scope of the claims described below by a person having ordinary skill in the art to which the present invention pertains.
Claims
1. An electrode assembly in which a first electrode, a separator, and a second electrode are stacked, the first electrode includes a current collector, and a first active material layer and a second active material layer provided on both sides of the current collector, one end of the first electrode includes a one-sided coated portion in which the first active material layer is provided on one side of the current collector and the second active material layer is not provided on the other side; and an uncoated portion in which the first active material layer and the second active material layer are not provided on both sides of the current collector, an electrode assembly including a swelling tape provided to cover a boundary between the first active material layer of the one-sided coated portion and the uncoated portion;
2. The electrode assembly of claim 1 , further comprising a swelling tape provided on a surface of the one-sided coating portion on which the second active material layer is not provided.
3. The electrode assembly of claim 1 , wherein the first active material layer is provided on a surface facing the second electrode with the separator interposed therebetween.
4. The electrode assembly of claim 3 , wherein the first active material layer is longer than the second electrode in a longitudinal direction of the electrode assembly.
5. The electrode assembly of claim 1 , wherein the second active material layer is shorter than the second electrode in a longitudinal direction of the electrode assembly.
6. The electrode assembly of claim 1 , wherein the electrode assembly is in a wound jelly roll type.
7. The electrode assembly of claim 6 , wherein the first electrode is an outermost electrode of the wound jelly roll type electrode assembly.
8. 8. The electrode assembly of claim 7, wherein the swelling tape covering the boundary between the first active material layer and the uncoated portion is provided on an inner circumferential surface of the first electrode of the jelly roll type electrode assembly.
9. The electrode assembly of claim 1 , wherein the current collector of the first electrode comprises copper.
10. The electrode assembly of claim 1 , wherein the first electrode is a negative electrode and the second electrode is a positive electrode.
11. 2. The electrode assembly according to claim 1, wherein the length of the swelling tape in the longitudinal direction of the electrode assembly is 30 mm or less.
12. The electrode assembly according to claim 1 , wherein a width of the swelling tape in a width direction of the electrode assembly is 50% or more with respect to 100% of a width of the electrode assembly.
13. 2. The electrode assembly of claim 1, wherein an area of the swelling tape covering the first active material layer is 5% to 20% of a total area of the swelling tape provided to cover a boundary between the first active material layer and the uncoated portion of the one-sided coated portion, the total area being 100%.
14. The electrode assembly of claim 1 , wherein the swelling tape does not overlap the second electrode.
15. The electrode assembly of claim 1 , wherein the swelling tape is swelled by an electrolyte.
16. The electrode assembly of claim 15 , wherein the swelling tape comprises polyurethane.
17. manufacturing an electrode assembly by stacking a first electrode, a separator, and a second electrode, the first electrode including a current collector and a first active material layer and a second active material layer respectively provided on both sides of the current collector, one end of the first electrode including a one-sided coated portion where the first active material layer is provided on one side of the current collector and the second active material layer is not provided on the other side, and an uncoated portion where the first active material layer and the second active material layer are not provided on both sides of the current collector; and disposing a swelling tape so as to cover a boundary between the first active material layer of the one-sided coated portion and the uncoated portion; A method for manufacturing an electrode assembly, comprising:
18. The method of claim 17, further comprising disposing a swelling tape on the other side of the one-sided coating unit on which the second active material layer is not provided.
19. a suction pad is provided on the swelling tape arranged to cover the boundary between the first active material layer and the uncoated portion of the one-sided coated portion; The method of claim 17, further comprising the step of pressing and attaching the swelling tape from the coated portion of one side of the first electrode to an uncoated portion of the first electrode using the suction pad.
20. The method of claim 19, wherein the suction pad has a step portion that is thicker in a direction toward the one-side coated portion than in an uncoated portion of the first electrode.
21. An electrode assembly provided by the method for producing an electrode assembly according to any one of claims 17 to 20.
22. An electrode assembly according to any one of claims 1 to 16; Electrolytes; and A secondary battery including the electrode assembly and a battery can housing the electrolyte.
23. The secondary battery of claim 22 , wherein the current collector of the first electrode is electrically connected to the battery can.
24. A battery pack comprising at least one secondary battery according to claim 22.
25. 25. A motor vehicle comprising at least one battery pack according to claim 24.
Citation Information
Patent Citations
Battery part and secondary battery adopting the same
JP2003168417A
Nonaqueous secondary battery
JP2005285691A
Nonaqueous battery
JP2007258050A
Wound nonaqueous electrolyte secondary battery
JP2008277207A
Method and apparatus for manufacturing wound electrode assembly
JP2010198770A