Secondary battery and its manufacturing method, battery module, battery pack and electric device
By using interfacial passivating agents to form a ternary layer on the negative electrode material layer, the cycle and storage performance of secondary batteries are enhanced, addressing the limitations of conventional technologies.
Patent Information
- Application Number
- JP2024523222
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-05-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-05-11
AI Technical Summary
Conventional techniques fail to effectively improve the cycle performance and storage performance of secondary batteries, and there is a challenge in balancing these two performance metrics.
Incorporating an interfacial passivating agent containing elements like lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, or gallium into the negative electrode material layer of secondary batteries, which forms a ternary layer during charging, stabilizing the interface and reducing impedance.
The ternary layer significantly improves cycle life and storage performance by reducing battery impedance and maintaining capacity retention over multiple cycles.
Smart Images

Figure 2024538187000015 
Figure 2024538187000016 
Figure 2024538187000017
Abstract
Description
[Technical field]
[0001] The present application relates to the technical field of lithium batteries, and in particular to a secondary battery and a method for manufacturing the same, a battery module, a battery pack and an electric device including the secondary battery. [Background technology]
[0002] As electric vehicles (EVs) and hybrid vehicles (HEVs) are widely used, people are increasingly paying attention to the usage time and usage costs of vehicles, so the cycle life of secondary batteries as energy storage devices for vehicles is naturally one of the performances that are attracting attention in the field. As expected, secondary batteries have good cycle performance and long battery life, which not only reduces the usage cost for users, but also reduces resource consumption.
[0003] In the prior art, the cycle performance of the secondary battery cannot be effectively improved, and it is difficult to balance the cycle performance and the storage performance of the secondary battery. Therefore, there is a need in the art for a secondary battery having improved cycle and storage performance and a method for manufacturing the same. Summary of the Invention [Problem to be solved by the invention]
[0004] The present application has been made in view of the above problems, and an object of the present invention is to provide a secondary battery having improved cycle and storage performance, and a method for manufacturing the same. [Means for solving the problem]
[0005] In order to achieve the above object, the present application provides a secondary battery and a manufacturing method thereof, a battery module, a battery pack, and an electric device.
[0006] A first aspect of the present application provides a secondary battery, comprising an anode sheet including an anode material layer, a cathode sheet including a cathode material layer, and an electrolyte, wherein at least one of the anode material layer, the cathode material layer, and the electrolyte comprises an interface passivator, the interface passivator being a compound including an element E, the element E being selected from lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, gallium, and germanium. By including the interface passivator, the secondary battery can generate a beneficial ternary layer on the surface of the anode material layer.
[0007] In an optional embodiment, the negative electrode layer has an ADE ternary layer on its surface, A is selected from alkali metal elements and is different from E, and D is silicon or carbon, and the ADE ternary layer is formed by the interfacial passivation agent acting on the surface of the negative electrode layer during at least one charging process of the secondary battery. The secondary battery of the present application has a ternary passivation layer on the surface of the negative electrode layer, which can greatly reduce the battery impedance and improve the cycle life and storage performance of the battery.
[0008] In any embodiment, the interface passivation agent is selected from at least one of beryllium, magnesium, calcium, aluminum and gallium compounds, preferably, the interface passivation agent is selected from at least one of beryllium, magnesium, calcium and aluminum compounds. By selecting the compound containing the above metal element, the stabilizing effect of the ternary layer can be further improved, so that the performance of the secondary battery can be more effectively improved.
[0009] In any embodiment, the interfacial passivation agent is a substituted or unsubstituted C 1-20 carboxylates, and the substituent is C 1-6 Alkyl group, C 2-6 Cycloalkyl group, hydroxyl group, amino group, oxo group, acyl group, C 1-6The compound is one or more selected from alkylthio groups, phenyl groups, benzoylthio groups, phenylthio groups and phenoxy groups, amino acid salts, enoates, phosphates, sulfates, sulfonylimides, sulfonates, benzoates, phthalates, acetylacetonates, inorganic oxyacid salts, and double salts containing at least two of the non-transition metal cations. By selecting the above compounds as the interface passivation agent, the resistance, cycle life, and storage performance of the secondary battery can be more effectively improved.
[0010] In any embodiment, the interface passivator is doped and mixed into at least one of the positive electrode material layer, the negative electrode material layer and the electrolyte. By doping and mixing the interface passivator into the positive electrode material, the negative electrode material and the electrolyte, the performance of the secondary battery can be effectively improved.
[0011] In any embodiment, the ADE ternary layer is selected from Li-Si-Ca, Li-Si-Mg, Li-Si-Be, Li-Si-Al, Li-C-Ca, Li-C-Mg, Li-C-Be, Li-C-Al, Na-Si-Ca, Na-Si-Mg, Na-Si-Be, Na-Si-Al, Na-C-Ca, Na-C-Mg, Na-C-Be, Na-C-Al ternary layers and combinations thereof, preferably, the ADE ternary layer is selected from Li-Si-Ca, Li-Si-Mg, Li-Si-Be, Li-Si-Al, Na-Si-Ca, Na-Si-Mg, Na-Si-Be, Na-Si-Al ternary layers and combinations thereof. The secondary battery includes the ternary layer, which can effectively improve the battery impedance, cycle life and storage performance.
[0012] In any embodiment, prior to the at least one charge, the positive electrode material layer comprises 0.001 wt % to 20 wt %, preferably 1 wt % to 10 wt %, of the interface passivator, based on the total weight of the positive electrode material layer.
[0013] In any embodiment, prior to the at least one charge, the negative electrode material layer comprises 0.001 wt % to 20 wt %, preferably 0.05 wt % to 5 wt %, of the interface passivator, based on the total weight of the negative electrode material layer.
[0014] In any embodiment, prior to the at least one charge, the electrolyte comprises from 0.001% to 20% by weight, preferably from 0.1% to 5% by weight, of the interface passivator, based on the total weight of the electrolyte.
[0015] By controlling the content of the passivator within the above range, the battery performance can be further improved.
[0016] In any embodiment, the negative electrode material layer includes a negative electrode active material, and the negative electrode active material has a D50 of 1 μm to 20 μm, preferably 2 μm to 10 μm. By adopting a negative electrode active material having the above D50, the function of the ternary interface passivation layer of the present application can be effectively exerted, and the performance of the secondary battery can be significantly improved.
[0017] In any embodiment, the negative electrode material layer includes a negative electrode active material, and the negative electrode active material has a Span value of 0.9 to 1.8, preferably 0.9 to 1.2; Where:
number
[0018] A second aspect of the present application provides a secondary battery, the secondary battery comprising: i) providing an anode sheet including an anode material layer, a cathode sheet including a cathode material layer, and an electrolyte to manufacture an uncycled secondary battery, wherein at least one of the anode material layer, the cathode material layer, and the electrolyte includes an interface passivator, the interface passivator being a compound including an element E, the element E being selected from the group consisting of lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, gallium, and germanium; ii) charging and discharging the uncycled secondary battery at least one cycle.
[0019] A third aspect of the present application provides a method for producing a secondary battery, i) providing an anode sheet including an anode material layer, a cathode sheet including a cathode material layer, and an electrolyte to manufacture an uncycled secondary battery, wherein at least one of the anode material layer, the cathode material layer, and the electrolyte includes an interface passivator, the interface passivator being a compound including an element E, the element E being selected from the group consisting of lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, gallium, and germanium; ii) charging and discharging the uncycled secondary battery for at least one cycle to form an ADE ternary layer and obtain the secondary battery, wherein A is selected from an alkali metal element and is different from E, and D is silicon or carbon.
[0020] The above method can provide a secondary battery having a ternary passivation layer on the surface of the negative electrode material layer, which can improve the impedance, cycle life and storage performance of the secondary battery.
[0021] In any embodiment, the interface passivation agent is selected from at least one of beryllium, magnesium, calcium, aluminum and gallium compounds, preferably, the interface passivation agent is selected from at least one of beryllium, magnesium, calcium and aluminum compounds. By selecting the interface passivation agent, a ternary layer can be effectively formed, and the performance of the secondary battery such as cycle and storage can be improved.
[0022] In any embodiment, the interfacial passivation agent is a substituted or unsubstituted C 1-20 carboxylates, and the substituent is C 1-6 Alkyl group, C 2-6 Cycloalkyl group, hydroxyl group, amino group, oxo group, acyl group, C 1-6 The interfacial passivation agent is one or more selected from alkylthio groups, phenyl groups, benzoylthio groups, phenylthio groups and phenoxy groups, amino acid salts, enoates, phosphates, sulfates, sulfonylimides, sulfonates, benzoates, phthalates, acetylacetonates, inorganic oxyacid salts, and double salts containing at least two of the above non-transition metal cations. By selecting the above interfacial passivation agent, a secondary battery having significantly improved resistance, cycle life, and storage performance can be manufactured.
[0023] In any embodiment, in step i), the interfacial passivation agent is doped and mixed into at least one of the positive electrode material layer, the negative electrode material layer, and the electrolyte solution, which facilitates the formation of a ternary layer and can further improve the performance of the secondary battery.
[0024] A fourth aspect of the present application provides a battery module including a secondary battery according to the first or second aspect of the present application or a secondary battery obtained by the method according to the third aspect of the present application.
[0025] A fifth aspect of the present application provides a battery pack including a battery module according to the fourth aspect of the present application.
[0026] A sixth aspect of the present application provides an electric device including at least one selected from the secondary battery according to the first or second aspect of the present application, the secondary battery obtained by the method according to the third aspect of the present application, the battery module according to the fourth aspect, or the battery pack according to the fifth aspect. Effect of the Invention
[0027] The secondary battery of the present application and the secondary battery obtained by the manufacturing method of the present application have balanced cycle performance and storage performance, and low internal resistance. [Brief description of the drawings]
[0028] [Figure 1] FIG. 1 is a schematic diagram showing a secondary battery according to an embodiment of the present application. [Diagram 2] FIG. 2 is an exploded view showing the secondary battery according to the embodiment of the present application shown in FIG. [Diagram 3] FIG. 1 is a schematic diagram illustrating a battery module according to an embodiment of the present application. [Figure 4] FIG. 1 is a schematic diagram illustrating a battery pack according to an embodiment of the present application. [Diagram 5] 5 is an exploded view showing the battery pack according to the embodiment of the present application shown in FIG. 4. [Figure 6] 1 is a schematic diagram showing an electrical device that uses a secondary battery as a power source according to an embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] Hereinafter, with appropriate reference to the drawings, embodiments specifically disclosing the secondary battery, battery module, battery pack, and electric device of the present application will be described in detail. However, unnecessary detailed description may be omitted. For example, detailed description of already well-known matters and duplicated description of the same actual structure may be omitted. This is to avoid the following description becoming unnecessarily long and to facilitate understanding by those skilled in the art. Note that the drawings and the following description are provided to enable those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.
[0030] The "ranges" disclosed herein are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Such defined ranges may be inclusive or exclusive of the limits, and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also contemplated. However, if minimum range values 1 and 2 and maximum range values 3, 4, and 5 are listed, the following ranges are all contemplated: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" refers to a shorthand representation of any combination of real numbers from a to b, where both a and b are real numbers. For example, the numerical range "0-5" refers to all real numbers between "0-5" listed herein, with "0-5" simply being a shorthand for combinations of these numbers. Also, when a parameter refers to an integer ≧2, this is equivalent to disclosing that the parameter is an integer, e.g., 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0031] Unless otherwise specified, all the embodiments and preferred embodiments in this application can be combined with each other to form new technical solutions.
[0032] Unless otherwise specified, all technical features and preferred technical features in this application can be combined with each other to form new technical solutions.
[0033] Unless otherwise stated, all steps in the present application may be performed in sequence or randomly, and preferably in sequence. For example, the method includes steps (a) and (b) indicates that the method may include steps (a) and (b) performed in sequence, or may include steps (b) and (a) performed in sequence. For example, the method mentioned above may include step (c) indicates that step (c) can be added to the method in any order, for example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), or may include steps (c), (a) and (b).
[0034] Unless otherwise specified, the terms "comprising" and "including" used in this application may be open ended or exclusive. For example, the terms "comprising" and "including" may further comprise or include other components not listed, or may comprise or include only the listed components.
[0035] Unless otherwise specified, in this application, the term "or" is inclusive. For example, the word "A or B" indicates "A, B, or both A and B." More specifically, any of the following conditions satisfy the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) but B is true (or exists), or A and B are both true (or exist).
[0036] As electric vehicles (EVs) and hybrid vehicles (HEVs) are widely used, people are increasingly paying attention to the usage time and usage costs of vehicles, so the cycle life of secondary batteries as energy storage devices for vehicles is naturally one of the performances that are attracting attention in the field. As expected, secondary batteries have good cycle performance and long battery life, which not only reduces the usage cost for users, but also reduces resource consumption.
[0037] The solid electrolyte interface (SEI) film on the sheet surface plays an important role in improving the cycling performance of secondary batteries. The formation of the SEI film consumes the electrolyte (or electrolyte ions in the electrolyte, i.e., active ions or charge carrier ions). Therefore, if the SEI film is repeatedly broken and regenerated during cycling, the transport kinetics of the active ions will deteriorate, which may lead to electrolyte depletion and reduced battery cell performance.
[0038] However, the currently commonly used positive and negative active materials undergo different degrees of volume change during cycling, which affects the integrity and stability of the SEI layer and further impairs battery performance.The volume change is particularly obvious for silicon-based negative active materials (the change rate is 100%-300%), and the above problem is more pronounced.
[0039] In this field, the SEI film layer is required to be suitable for the volume change of the material and to be completely maintained, and for this purpose, additives are usually added to the electrolyte, or the active material or the surface of the sheet is coated. However, the SEI layer obtained by these methods is not suitable for the volume change of the material, and therefore the battery performance cannot be significantly improved. As can be seen from the above, the conventional methods cannot effectively solve the interface problem caused by the volume change of the material.
[0040] However, the challenge is also to carefully balance cycle performance and storage performance. As is known in the art, good storage performance and long cycle life have different, even opposite, requirements on the SEI film. For cycle life, a relatively flexible and thin SEI is advantageous because it is suitable for the volume change of the negative electrode material and consumes less during repeated formation, and has a low interfacial impedance. However, for storage life, a non-porous and robust SEI is advantageous because it can prevent electrolyte penetration and current leakage. However, during cycling, such a thick and less flexible SEI will crack and consume additional electrolyte when the volume change of the negative electrode material occurs, and it will also affect ion migration, resulting in a relatively low initial capacity and a somewhat poor performance in terms of the magnification.
[0041] However, a secondary battery expected in this field should have excellent overall performance, that is, excellent cycle performance and storage performance.
[0042] One object of the present application is to provide a secondary battery with balanced overall performance, i.e., excellent cycle performance and storage performance. Another object of the present application is to provide a method for manufacturing a secondary battery. The secondary battery of the present application has excellent overall performance, small battery internal resistance after multiple cycles, longer cycle life, and better storage performance.
[0043] Hereinafter, the secondary battery, the battery module, the battery pack, and the electric device of the present application will be described with appropriate reference to the drawings.
[0044] Secondary battery and its manufacturing method In one embodiment of the present application, the present application proposes a secondary battery, comprising an anode sheet including an anode material layer, a cathode sheet including a cathode material layer, and an electrolyte, wherein at least one of the anode material layer, the cathode material layer, and the electrolyte comprises an interface passivator, the interface passivator being a compound containing an element E, the E being selected from lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, gallium, or germanium. Without being bound by any theory, the inclusion of the interface passivator in at least one of the cathode material layer, the electrolyte, and the anode material layer creates a ternary layer beneficial to the absorption of active ions in the anode material during at least one charging process after the secondary battery is newly manufactured, improving the sheet and the battery performance.
[0045] In this specification, depending on the type of secondary battery, the active ions may be lithium ions or sodium ions, in other words, the active ions of a lithium-ion secondary battery are lithium ions and the active ions of a sodium-ion secondary battery are sodium ions.
[0046] In some embodiments, the negative electrode layer has an ADE ternary layer on its surface, A is selected from an alkali metal element and is different from E, and D is silicon or carbon, and the ADE ternary layer is formed by the interfacial passivation agent acting on the surface of the negative electrode layer during at least one charge of the secondary battery. The secondary battery of the present application has a ternary layer on its surface of its negative electrode layer, which can stabilize the negative electrode interface and adapt to volume changes, thereby improving the performance of the sheet and the battery, particularly achieving a careful balance between cycle performance and storage performance. In addition, with the increase in the number of charge and discharge cycles, the advantages of the secondary battery of the present application become more obvious, especially with significantly reduced battery impedance and improved battery cycle life and storage performance (e.g., improved capacity retention, especially after cycling and storage at high temperatures).
[0047] As used herein, the terms "ternary layer" and similar expressions denote the same or similar meanings and may be used interchangeably.
[0048] In some embodiments, the secondary battery is a lithium ion secondary battery or a sodium ion secondary battery. In this case, the interface passivator or the ternary layer of the present application can significantly improve the cycle performance, impedance, etc. of the battery. In some embodiments, the secondary battery is a lithium ion secondary battery.
[0049] In some embodiments, the interface passivator is a non-transition metal compound with an atomic number of 20 or less. Such a compound may be an organic or inorganic compound. The inventors have discovered that, particularly in lithium-ion secondary batteries, it is ideal to use a compound of a metal element with an atomic number of 20 or less as the interface passivator. In particular, it is desirable to select a compound of a metal with a lower activity than the active ions of the secondary battery as the interface passivator. Without being bound by any theory, such an interface passivator is likely to gain electrons in an electrochemical reaction and to form a ternary layer. In contrast, transition metal compounds can be difficult to improve in performance in some cases, because transition metal atoms contain many vacant orbitals, which are unfavorable to the formation of a ternary layer and may instead promote interface reactions.
[0050] As used herein, the term "transition metal" has its meaning well known in the art and generally refers to metallic elements in the d and ds regions of the periodic table (the elements in the d region include the elements of groups IIIB to VIIB and group VIII of the periodic table, excluding the lanthanide and actinide elements, and the ds region includes the elements of groups IB to IIB of the periodic table).
[0051] In some embodiments, the interfacial passivator has a metal cation moiety with a valence of 2 to 5. In some embodiments, the interfacial passivator can be selected from at least one of lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, gallium, and germanium compounds, and is preferably at least one of beryllium, magnesium, potassium, calcium, aluminum, gallium, and germanium compounds.
[0052] In some embodiments, the interface passivation agent is selected from at least one of beryllium, magnesium, calcium, aluminum, and gallium compounds, and preferably, the interface passivation agent is selected from at least one of beryllium, magnesium, calcium, and aluminum compounds. By selecting a compound containing the above metal element, the effect of the interface passivation layer can be further improved, and the performance of the secondary battery can be more effectively improved.
[0053] In some embodiments, the interfacial passivation agent is selected from a combination of two or three of magnesium, aluminum and calcium compounds. The incorporation of such a combination of interfacial passivation agents can further improve the internal resistance, cycle and storage performance of the battery.
[0054] In some embodiments, the interfacial passivation agent is a substituted or unsubstituted C 1-20 carboxylates, and the substituent is selected from at least one of C 1-6 Alkyl group, C 2-6 Cycloalkyl group, hydroxyl group, amino group, oxo group, acyl group, C 1-6 The salt is one or more selected from an alkylthio group, a phenyl group, a benzoylthio group, a phenylthio group, a phenoxy group, an amino acid salt, an enoate salt, a phosphate salt, a sulfate salt, a sulfonylimide salt, a sulfonate salt, a benzoate salt, a phthalate salt, an acetylacetonate salt, an inorganic oxyacid salt, and a double salt containing at least two of the above non-transition metal cations.
[0055] In some embodiments, preferably, the interfacial passivation agent is selected from the group consisting of calcium propionate, calcium stearate, calcium acetate, calcium cyclohexanebutyrate, calcium formate, calcium DL-malate, calcium glycolate, calcium 3-methyl-2-oxobutyrate, calcium levulinate, calcium 2-ethylhexanoate, calcium 2-hydroxy-4-(methylthio)butyrate, calcium DL-glycerate, aluminum stearate, aluminum monostearate, alkali aluminum acetate, aluminum terephthalate, aluminum acetate, aluminum oxalate, aluminum bis-stearate, aluminum lactate, magnesium stearate, magnesium lactate, magnesium oxalate, magnesium acetate, magnesium citrate, magnesium valproate, magnesium 2-ethylhexanoate, magnesium 2-ethylbutyrate, magnesium phenoxyacetate, calcium bis(nonafluorobutylsulfonyl)imide, calcium bis(fluorosulfonyl)imide, calcium bis(trifluoromethanesulfonyl)imide, and calcium bis(trifluoromethanesulfonyl)imide. sulfonyl)imide, calcium methylsulfonate, calcium 2,5-dihydroxybenzenesulfonate, calcium trifluoromethanesulfonate, calcium dobesilate, magnesium trifluoromethanesulfonate, aluminum tris(trifluorosulfonate), calcium benzoate, calcium phthalate, calcium 4-aminosalicylate, calcium acetylacetonate, calcium hexafluoroacetylacetonate, beryllium acetylacetonate, magnesium acetylacetonate, bis(2,4-pentanedione)magnesium(II), magnesium trifluoroacetylacetonate, magnesium hexafluoroacetylacetonate, aluminum acetylacetonate, aluminum tris(trifluoro-2,4-pentanedionato), calcium metaborate, calcium nitrate, aluminum metaphosphate, aluminum perchlorate, dihydroaluminum phosphate, aluminum hypophosphite, aluminum phosphate, magnesium perchlorate, magnesium metaborate, magnesium nitrate, beryllium sulfate, calcium aluminate, triethylaluminum,Trioctyl aluminum, tri-n-butyl aluminum, isopropyl dimethyl aluminum, tris(hexadecyl) aluminum, diocene magnesium, di-n-butyl magnesium, n-butylethyl magnesium, bis(ethylcyclopentadienyl) magnesium, bis(pentamethylcyclopentene) magnesium, bis(cyclopentadienyl) magnesium, bis(n-propylcyclopentadienyl) magnesium, bis(ethylcyclopentadienyl) magnesium, bis(2-(2-hydroxyphenyl)pyridine) beryllium, bis(pentamethylcyclopentadienyl) tetrahydrofuran calcium, isopropyl alcohol aluminum, ethy. and at least one of aluminum t-butoxy, aluminum t-butoxy, aluminum sec-butyl alcohol, aluminum n-butoxide, hydroxyaluminum bis(2-ethylhexanoate), magnesium methanol, magnesium ethanol, magnesium tert-butoxide, magnesium aluminum silicate, calcium methacrylate, calcium sorbate (2,4-hexadienoic acid), aluminum acrylate, magnesium acrylate, calcium phytate, hemicalcium bis(2-ethylhexyl)phosphate, aluminum diethylphosphinate, magnesium lauryl sulfate, calcium phenylpyruvate, and calcium acetonidioate.
[0056] In some embodiments, the interfacial passivation agent is preferably selected from at least one of fluorosulfonylimide salts, acetylacetone salts, and inorganic oxyacid salts. In some embodiments, the inorganic oxyacid salt is selected from at least one of metaboric acid, nitric acid, metaphosphoric acid, perchloric acid, phosphoric acid, hypophosphorous acid, sulfuric acid, and aluminum acid. In some embodiments, the interfacial passivation agent is selected from at least one of fluorosulfonylimide salts, acetylacetone salts, fluoroacetylacetone salts, nitrates, phosphates, perchlorates, and sulfates.
[0057] In some embodiments, preferably, the interfacial passivation agent is selected from at least one of calcium bis(nonafluorobutylsulfonyl)imide, calcium nitrate, aluminum tris(trifluoro-2,4-pentanedionato), aluminum phosphate, magnesium hexafluoroacetylacetonate, magnesium perchlorate, beryllium acetylacetonate, and beryllium sulfate.
[0058] By selecting the above interfacial passivation agents, it is possible to reduce the resistance of the secondary battery and achieve a careful balance between cycle life and storage performance.
[0059] In some embodiments, the interfacial passivation agent is doped and mixed into at least one of the positive electrode material layer (or positive electrode slurry), the negative electrode material layer (or negative electrode slurry), and the electrolyte solution. By doping and mixing, the interfacial passivation agent is directly added to the battery system, which is more advantageous for the formation of the ternary layer.
[0060] As used herein, "dope mixing" means that the interfacial passivation agent is directly doped and mixed and sprinkled (or dispersed) into the slurry or electrolyte. Dope mixing does not include coating.
[0061] In some embodiments, the ADE ternary layer is selected from Li-Si-Ca, Li-Si-Mg, Li-Si-Be, Li-Si-Al, Li-C-Ca, Li-C-Mg, Li-C-Be, Li-C-Al, Na-Si-Ca, Na-Si-Mg, Na-Si-Be, Na-Si-Al, Na-C-Ca, Na-C-Mg, Na-C-Be, Na-C-Al ternary layers and combinations thereof. In some embodiments, the ADE ternary layer is preferably selected from Li-Si-Ca, Li-Si-Mg, Li-Si-Be, Li-Si-Al, Na-Si-Ca, Na-Si-Mg, Na-Si-Be, Na-Si-Al ternary layers and combinations thereof. The inclusion of the ternary interface passivation layer in the secondary battery can effectively improve the battery impedance, cycle life and storage performance.
[0062] In some embodiments, the ternary layer is formed by the action of an interfacial passivator on the surface of the negative electrode material during at least one charging cycle of the secondary battery, hi some embodiments, the ternary layer is formed during 1-3, preferably 1-2, more preferably 1 charging cycle of the secondary battery.
[0063] In some embodiments, prior to the at least one charge, the positive electrode material layer comprises 0.001 wt % to 20 wt %, preferably 1 wt % to 10 wt %, of the interface passivator, based on the total weight of the positive electrode material layer.
[0064] In some embodiments, prior to the at least one charge, the negative electrode material layer comprises 0.001 wt % to 20 wt %, preferably 0.05 wt % to 5 wt %, of the interface passivator, based on the total weight of the negative electrode material layer.
[0065] In some embodiments, the electrolyte comprises 0.001 wt % to 20 wt %, preferably 0.1 wt % to 5 wt %, of the interface passivator, based on the total weight of the electrolyte, prior to the at least one charge. In some embodiments, the electrolyte preferably comprises 0.2 wt % to 5 wt %, preferably 0.3 wt % to 5 wt %, of the interface passivator, based on the total weight of the electrolyte, prior to the at least one charge.
[0066] The content of the passivation agent can be controlled within the above range to further improve the battery performance: if the content is too low, an effective ternary interface passivation layer cannot be formed, and if the content is too high, a ternary phase will also be generated in the bulk phase of the sheet material layer, reducing the energy density of the battery cell.
[0067] In some embodiments, it is advantageous for the anode material layer to include the interfacial passivator, whereby the interfacial passivator can be added in small amounts to achieve the desired purpose while reducing the impact on electrolyte components or performance.
[0068] In some embodiments, the anode active material layer comprises a silicon-based anode active material or a carbon-based anode active material. In particular, in some embodiments, the anode material layer comprises a silicon-based anode active material. When using an anode material with a large volume change, the advantage of including the ternary layer of the present invention in the secondary battery is particularly significant. When the anode material layer comprises a silicon-based anode material (and thus consists of a silicon-based anode active material), it is particularly advantageous to add the interface passivator of the present application to such a secondary battery system.
[0069] In some embodiments, the negative electrode active material has a D50 of 1 μm to 20 μm, preferably 2 μm to 10 μm. By adopting a material having the above D50, the interface passivation effect of the ternary layer of the present application can be effectively exerted, and the performance of the secondary battery can be significantly improved, and the ease of sheet production and the superiority of performance can be balanced. By adopting a material having a D50 within the above range, it is possible to avoid the interface activity being too high due to the specific surface area of the material being too large, which is advantageous for the interface passivation layer to effectively realize the desired performance improvement, and at the same time, it is advantageous for the inhibition of the movement of active ions to be avoided, which is advantageous for the improvement of the overall battery performance.
[0070] In some embodiments, the negative electrode active material has a Span value of 0.9 to 1.8, preferably 0.9 to 1.2. Where:
number
[0071] In this specification, the "Span value" characterizes the particle size distribution width of a material. The Span value is a dimensionless quantity as defined above. By selecting a negative electrode active material having a Span value within the above range, it is advantageous for the material to have relative interface stability, which contributes to realizing the effect of improving battery performance.
[0072] In some embodiments, the negative electrode active material has a D50 of 1 μm-20 μm and a Span value of 0.9-1.8. In other embodiments, the negative electrode active material has a D50 of preferably 3 μm-10 μm and a Span value of preferably 0.9-1.2.
[0073] A second aspect of the present application provides a secondary battery, the secondary battery comprising: i) providing an anode sheet including an anode material layer, a cathode sheet including a cathode material layer, and an electrolyte to manufacture an uncycled secondary battery, wherein at least one of the anode material layer, the cathode material layer, and the electrolyte includes an interface passivator, the interface passivator being a compound including an element E, the element E being selected from the group consisting of lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, gallium, and germanium; ii) charging and discharging the uncycled secondary battery at least one cycle.
[0074] A third aspect of the present application provides a method for producing a secondary battery, i) providing an anode sheet including an anode material layer, a cathode sheet including a cathode material layer, and an electrolyte to manufacture an uncycled secondary battery, wherein at least one of the anode material layer, the cathode material layer, and the electrolyte includes an interface passivator, the interface passivator being a compound including an element E, the element E being selected from the group consisting of lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, gallium, and germanium; ii) charging and discharging the uncycled secondary battery for at least one cycle to form an ADE ternary layer and obtain the secondary battery, wherein A is selected from an alkali metal element and is different from E, and D is silicon or carbon.
[0075] The secondary battery finally manufactured by the above method is a secondary battery having a ternary passivation layer on the surface of the negative electrode material layer, and has improved impedance, cycle life and storage performance.
[0076] In some embodiments, step i) comprises: a) providing a cathode slurry, an anode slurry, and an electrolyte, wherein at least one of the cathode slurry, the anode slurry, and the electrolyte is doped and mixed with an interfacial passivation agent.
[0077] In some embodiments, step i) includes b) applying the positive electrode slurry and the negative electrode slurry to at least one surface of a positive electrode current collector and a negative electrode current collector, respectively, to obtain a positive electrode sheet and a negative electrode sheet, and assembling the positive electrode sheet, the negative electrode slurry, and the electrolyte as the uncycled secondary battery.
[0078] Regardless of any theory, when the negative electrode sheet material layer contains an interfacial passivation agent, the interfacial passivation agent acts directly on the negative electrode sheet material layer to form a ternary layer during at least one charge-discharge cycle, whereas when the positive electrode sheet material layer and / or the electrolyte contains an interfacial passivation agent, the interfacial passivation agent migrates to the surface of the negative electrode sheet material layer under the action of voltage to form a ternary layer during at least one charge-discharge cycle. For example, the interfacial passivation agent, the active ions of the secondary battery, and the negative electrode active material form the ternary layer under the action of voltage. The present application realizes improvement of battery performance by forming a ternary layer on the surface of the negative electrode sheet material layer.
[0079] In some embodiments, the at least one cycle described in step ii) is performed at a voltage between 3V and 4.3V.
[0080] In some embodiments, step ii) is a conversion step.
[0081] As used herein, the term "formation" has a meaning well known in the art, and generally refers to a first charge of a newly manufactured secondary battery, during which absorption and desorption of lithium ions occurs, activating the negative electrode active material and forming a passivation layer, e.g., a solid electrolyte interface film (SEI film), on the surface of the negative electrode material layer.
[0082] In some embodiments, the interfacial passivator is selected from at least one of compounds of beryllium, magnesium, calcium, aluminum, and gallium, and preferably, the interfacial passivator is selected from at least one of compounds of beryllium, magnesium, calcium, and aluminum.
[0083] In some embodiments, prior to the at least one charge, the positive electrode material layer comprises 0.001 wt % to 20 wt %, preferably 1 wt % to 10 wt %, of the interface passivator, based on the total weight of the positive electrode material layer.
[0084] In some embodiments, prior to the at least one charge, the negative electrode material layer comprises 0.001 wt % to 20 wt %, preferably 0.05 wt % to 5 wt %, of the interface passivator, based on the total weight of the negative electrode material layer.
[0085] In some embodiments, prior to the at least one charge, the electrolyte comprises from 0.001 wt % to 20 wt %, preferably from 0.1 wt % to 5 wt %, of the interface passivator, based on the total weight of the electrolyte.
[0086] In some embodiments, the interfacial passivation agent is added to the positive electrode sheet material slurry, the negative electrode sheet material slurry, or the electrolyte by doping (or mixing).
[0087] The cathode material slurry includes an active cathode material, an interfacial passivator, a solvent, and optional additives. In some embodiments, the cathode material slurry includes 0.001% to 20% by weight, preferably 1% to 10% by weight, of an interfacial passivator, based on the dry weight of the cathode material slurry.
[0088] The negative electrode material slurry includes a negative electrode active material, an interfacial passivator, a solvent, and optional additives. In some embodiments, the negative electrode material slurry includes 0.001 wt % to 20 wt %, preferably 0.05 wt % to 5 wt %, of the interfacial passivator, based on the dry weight of the negative electrode material slurry.
[0089] By using the interface passivator in the above content range, a ternary layer can be effectively formed on the surface of the negative electrode sheet material layer, thereby passivating and protecting the interface and improving the performance of the secondary battery.
[0090] In some embodiments, the anode slurry includes an anode active material. The anode active material includes a silicon-based anode active material or a carbon-based anode active material. In particular, in some embodiments, the anode slurry includes a silicon-based anode active material. When using anode materials with large volume changes, the advantages of the interface passivator of the present invention and the ternary layer formed therewith are particularly prominent.
[0091] In addition, the components other than the interface passivation agent in each component of the secondary battery will be described below.
[0092] [Positive electrode sheet] The positive electrode sheet includes a positive electrode current collector and a positive electrode material layer provided on at least one surface of the positive electrode current collector, the positive electrode material layer including a positive electrode active material.
[0093] For example, the positive electrode current collector has two surfaces opposing each other in the thickness direction of the positive electrode current collector, and the positive electrode film layer is provided on either one or both of the two opposing surfaces of the positive electrode current collector.
[0094] In some embodiments, the positive electrode current collector may be a metal foil sheet or a composite current collector. For example, an aluminum foil may be used as the metal foil sheet. The composite current collector includes a polymeric substrate layer and a metal layer formed on at least one surface of the polymeric substrate layer. The composite current collector may be formed by forming a metal material (such as aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymeric substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0095] In some embodiments, the positive electrode active material may be a battery positive electrode active material known in the art. For example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphate with an olivine structure, lithium transition metal oxide, and modified compounds thereof. The present application is not limited to these materials, and other conventional materials that can be used as a battery positive electrode active material may be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides include lithium cobalt oxide (e.g., LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, and lithium nickel cobalt manganese oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM 333 (can also be abbreviated as LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM 523 (can also be abbreviated as LiNi 0.5 Co 0.25 Mn 0.25 O2(NCM 211 (can also be abbreviated as LiNi 0.6 Co 0.2 Mn 0.2O2(NCM 622 (can also be abbreviated as LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM 811 Lithium nickel cobalt aluminum oxide (e.g. LiNi 0.85 Co 0.15 Al 0.05 Examples of the lithium-containing phosphate having an olivine structure include, but are not limited to, at least one of lithium iron phosphate (e.g., LiFePO4 (which can also be abbreviated as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (e.g., LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon.
[0096] In the secondary battery according to the present invention, the positive electrode active material is preferably selected from materials in which a volume change occurs during the absorption-desorption of battery active ions (such as lithium ions, sodium ions, or potassium ions) and / or the material interface has a catalytic effect on the electrolyte. In some embodiments, the positive electrode active material is selected from one or more of lithium iron phosphate (LFP), lithium manganese iron phosphate (LFMP), lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium-rich materials, sodium acid compounds or potassium acid compounds, and compounds obtained by adding other metals to the above compounds, and the other metals are selected from one or more of transition metals and / or non-transition metals other than beryllium, magnesium, calcium, and aluminum. However, those skilled in the art will understand that the present invention is not limited to these materials.
[0097] In some embodiments, the positive electrode membrane layer preferably further includes a binder. The type and content of the binder are not specifically limited and can be selected according to actual needs. For example, the binder can include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0098] In some embodiments, the positive electrode layer preferably further comprises a conductive agent. The type and content of the conductive agent are not specifically limited and can be selected according to actual needs. For example, the conductive agent can include at least one of superconducting carbon, acetylene black, carbon black, cochin black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0099] In some embodiments, the positive electrode sheet can be manufactured as follows: the above-mentioned components for manufacturing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder, and any other components, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry, and the positive electrode slurry is coated onto a positive electrode current collector. After processes such as drying and cold pressing, the positive electrode sheet can be obtained.
[0100] [Negative electrode sheet] The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer provided on at least one surface of the negative electrode current collector, the negative electrode material layer including a negative electrode active material.
[0101] For example, the negative electrode current collector has two surfaces opposing each other in the thickness direction of the negative electrode current collector, and the negative electrode film layer is provided on either one or both of the two opposing surfaces of the negative electrode current collector.
[0102] In some embodiments, the negative electrode current collector may be a metal foil sheet or a composite current collector. For example, the metal foil sheet may be a copper foil. The composite current collector may include a polymeric substrate layer and a metal layer formed on at least one surface of the polymeric substrate layer. The composite current collector may be formed by forming a metal material (such as copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymeric substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0103] In some embodiments, the negative electrode active material may be a positive electrode active material for a battery known in the art. For example, the negative electrode active material may include at least one of artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based material, tin-based material, and lithium titanate. The silicon-based material may be selected from at least one of silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy. The tin-based material may be selected from at least one of tin, tin oxide, and tin alloy. However, the present application is not limited to these materials, and other conventional materials that can be used as a negative electrode active material for a battery may be used. These negative electrode active materials may be used alone or in combination of two or more.
[0104] In the secondary battery according to the present invention, the negative electrode active material is preferably selected from materials in which a volume change occurs during the absorption-desorption of battery active ions (e.g., sodium ions, lithium ions, or potassium ions, etc.) and / or the material interface has a catalytic effect on the electrolyte. In some embodiments, the negative electrode active material is selected from silicon-based negative electrode materials or silicon-based negative electrode materials. In some embodiments, the negative electrode active material is preferably selected from one or more of graphite, soft carbon, hard carbon, mesocarbon microbeads, carbon fibers, carbon nanotubes, elemental silicon, silicone compounds, silicon carbon composites, and compounds obtained by adding other metals to the above materials, and the other metals are selected from one or more of transition metals and / or non-transition metals other than beryllium, magnesium, calcium, and aluminum. However, those skilled in the art will understand that the present invention is not limited to these materials.
[0105] In some embodiments, the anode active material is selected from silicon-based anode materials, hi some embodiments, the anode active material is selected from one or more of elemental silicon, silicone compounds, and silicon carbon composites.
[0106] In some embodiments, the negative electrode membrane layer preferably further includes a binder. The type and content of the binder are not specifically limited and can be selected according to actual needs. The binder can be selected from at least one of styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0107] In some embodiments, the negative electrode film layer preferably further comprises a conductive agent. The type and content of the conductive agent are not specifically limited and can be selected according to actual needs. The conductive agent can be selected from at least one of superconducting carbon, acetylene black, carbon black, cochin black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0108] In some embodiments, the negative electrode membrane layer preferably further comprises other auxiliary agents, such as a thickening agent (eg, sodium carboxymethylcellulose (CMC-Na)).
[0109] In some embodiments, the negative electrode sheet can be manufactured as follows: the above-mentioned components for manufacturing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder, and any other components, are dispersed in a solvent (e.g., deionized water) to form a negative electrode slurry, and the negative electrode slurry is coated onto a negative electrode current collector. After undergoing processes such as drying and cold pressing, the negative electrode sheet can be obtained.
[0110] [Electrolytes] The electrolyte plays a role in conducting ions between the positive and negative electrode pieces. The present application is not specifically limited to the type of electrolyte, and it can be selected as needed. For example, the electrolytes commonly seen in this decomposition can be liquid, gelled, or all solid. In this application, it mainly refers to liquid electrolytes.
[0111] In some embodiments, the electrolyte is an electrolytic solution, the electrolytic solution including an electrolyte salt and a solvent.
[0112] In the present application, the type of electrolyte salt is not specifically limited, and can be selected as necessary. In some embodiments, the electrolyte salt is lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiCF3SO3), lithium difluorophosphate, lithium difluorooxalate borate, lithium bis(oxalate)borate (LiBOB), lithium difluorooxalate phosphate, lithium tetrafluorooxalate phosphate, and LiN(C x F 2x +1SO2)(C y F 2y +1SO2) (where x and y are natural numbers). Although only electrolyte salts used in lithium ion secondary batteries have been exemplified above, the present invention is not limited thereto. For secondary batteries having other active ions, the corresponding electrolyte salts are not specifically limited and can be selected as necessary.
[0113] In the present application, the type of organic solvent of the electrolyte is not specifically limited, and may be selected as necessary. In some embodiments, the organic solvent includes one or more of a chain carbonate ester, a cyclic carbonate ester, a carboxylate ester, and an ether. In the present application, the type of the chain carbonate ester, the cyclic carbonate ester, the carboxylate ester, and the ether is not specifically limited, and may be selected as necessary. In some embodiments, the organic solvent may preferably include one or more of diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, methyl formate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, tetrahydrofuran, dimethyl ether, diethyl ether, and ethylene glycol dimethyl ether.
[0114] In some embodiments, the electrolyte solution preferably further includes an additive. For example, the additive may include a negative electrode film-forming additive, a positive electrode film-forming additive, and may include an additive that can improve certain performance of the battery, such as an additive that improves the overcharge performance of the battery, or an additive that improves the high-temperature or low-temperature performance of the battery.
[0115] In some embodiments, the electrolyte additive is selected from at least one of a cyclic carbonate compound having an unsaturated bond, a halogen-substituted cyclic carbonate compound, a sulfate compound, a sulfite compound, a sultonic acid ester compound, a disulfonic acid compound, a nitrile compound, an aromatic compound, an isocyanate compound, a phosphazene compound, a cyclic acid anhydride compound, a phosphite compound, a phosphate compound, a borate ester compound, and a carboxylate compound.
[0116] [Separator] In some embodiments, the secondary battery further includes a separator. The present application is not particularly limited to the type of separator, and any known porous separator having excellent chemical stability and mechanical stability can be selected.
[0117] In some embodiments, the material of the separator may be at least one selected from glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator is not particularly limited and may be a single-layered thin film or a multi-layered composite thin film. When the separator is a multi-layered composite thin film, the material of each layer is not particularly limited and may be the same or different.
[0118] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be manufactured into an electrode assembly by a winding process or a lamination process.
[0119] In some embodiments, the secondary battery may include an outer casing, which can be used to enclose the electrode assembly and electrolyte.
[0120] In some embodiments, the exterior of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The exterior of the secondary battery may be a soft bag, such as a pouch soft bag, etc. The material of the soft bag may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0121] The present application is not particularly limited to the shape of the secondary battery, and the secondary battery may be cylindrical, rectangular, or any other shape. For example, FIG. 1 shows an example of a secondary battery 5 having a rectangular structure.
[0122] In some embodiments, referring to FIG. 2, the exterior may include a housing 51 and a cover plate 53. The housing 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate may be enclosed to form a storage chamber. The housing 51 has an opening communicating with the storage chamber, and the cover plate 53 may be covered by the opening to close the storage chamber. The positive electrode sheet, the negative electrode sheet and the separator may form an electrode assembly 52 by a winding process or a lamination process. The electrode assembly 52 is sealed in the storage chamber. An electrolyte is infiltrated into the electrode assembly 52. The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and may be selected by those skilled in the art according to specific practical needs.
[0123] In some embodiments, the secondary batteries can be assembled into a battery module, and the number of secondary batteries included in the battery module can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0124] Fig. 3 is an example of a battery module 4. Referring to Fig. 3, in the battery module 4, a plurality of secondary batteries 5 are arranged in sequence along the length direction of the battery module 4. Of course, they may be distributed in any other manner. Furthermore, the plurality of secondary batteries 5 may be fixed by a fastener.
[0125] Preferably, the battery module 4 may further include an outer case having a storage space, and the multiple secondary batteries 5 are stored in the storage space.
[0126] In some embodiments, the battery modules may be further assembled into a battery pack, and the number of battery modules included in the battery pack may be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0127] 4 and 5 show an example of a battery pack 1. Referring to Fig. 4 and Fig. 5, the battery pack 1 may include a battery box and a plurality of battery modules 4 provided in the battery box. The battery box includes an upper box body 2 and a lower box body 3, and the upper box body 2 may be covered by the lower box body 3 to form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 may be distributed in the battery box in any manner.
[0128] The present application further provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided by the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device includes, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), trains, ships, satellites, energy storage systems, etc.
[0129] The electric device may be a secondary battery, a battery module or a battery pack depending on the usage requirements.
[0130] 6 is an example of an electric device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the high power and high energy density demands of the secondary battery of the electric device, a battery pack or a battery module can be used.
[0131] Other examples of the device may be a mobile phone, a tablet, a notebook computer, etc. Such devices are usually required to be thin and can use a secondary battery as a power source.
[0132] Working Example
[0133] The following examples of the present application are described. The following examples are merely illustrative and are used only to interpret the present application, and should not be understood as limiting the present application. If no specific techniques or conditions are shown in the examples, they should be carried out according to the techniques or conditions described in the literature of the field, or according to the product specifications. If no manufacturer is shown for the reagents or equipment used, they are conventional products that can be purchased commercially.
[0134] The secondary batteries of the present invention and the comparative examples are both manufactured according to the following method.
[0135] 1. Manufacturing of positive electrode sheet According to Table 1 below, the positive electrode active material, acetylene black as a conductive agent, and polyvinylidene fluoride (PVDF) as a binder are dissolved in a solvent N-methylpyrrolidone (NMP) in a weight ratio of 90:5:5, and the interface passivation agent of the present application is added thereto (if any), and then thoroughly stirred to mix uniformly, to obtain a positive electrode slurry. 2 The positive electrode current collector aluminum foil was uniformly coated with the amount of the coating, dried, cold pressed, and then cut into 57,000 mm 2 Cut into positive electrode sheets.
[0136] In each of the tables below, if the positive or negative electrode material layer includes an interfacial passivator, the content of the interfacial passivator is in weight percent (wt%) on a dry basis of the positive or negative electrode material layer, respectively, and if the electrolyte includes an interfacial passivator, the content of the interfacial passivator is in weight percent of the total weight of the electrolyte.
[0137] [Table 1]
[0138] 2. Manufacturing of negative electrode sheet According to Table 2 below, each negative electrode active material, acetylene black as a conductive agent, styrene butadiene rubber (SBR) as a binder, and sodium carboxymethylcellulose (CMC) as a thickener are dissolved in deionized water as a solvent in a weight ratio of 90:4:4:2, and the interface passivation agent of the present application is added thereto (if any), and then thoroughly stirred to mix uniformly to obtain a negative electrode slurry. Next, the negative electrode slurry is added once or multiple times to obtain 0.12 mg / mm 2 The negative electrode current collector copper foil is coated uniformly with a loading amount of 60,000 mm. 2 A negative electrode sheet of
[0139] [Table 2] Here, " / " indicates "and", i.e. "calcium bis(nonafluorobutylsulfonyl)imide / magnesium perchlorate" indicates "calcium bis(nonafluorobutylsulfonyl)imide and magnesium perchlorate". In the following, similar expressions have the same meaning.
[0140] 3. Electrolyte production According to Table 3 below, in an argon gas atmosphere (H2O<0.1ppm, O2<0.1ppm) glove box, ethylene carbonate (EC) and ethyl methyl carbonate (EMC) as organic solvents are mixed uniformly in a volume ratio of 3 / 7, 12.5% by weight of lithium hexafluorophosphate (LiPF6) is added to the mixed organic solvent to dissolve it as an electrolyte salt, 1% by weight of 1,3-propanesulfonic acid lactone (PS), 0.5% by weight of ethylene sulfate (DTD), 0.5% by weight of vinylene carbonate (VC) and 2% by weight of fluoroethylene carbonate (FEC) are added as additives, and the interface passivation agent of the present application (if any) is added, and the mixture is stirred uniformly to obtain an electrolyte solution. The weight percentage obtained is calculated based on the total weight of the electrolyte solution.
[0141] [Table 3]
[0142] 4. Secondary battery manufacturing (1) As shown in Table 4 below, a positive electrode sheet, a separator, and a negative sheet are stacked in order, and a separator is placed between the positive and negative sheets to tightly adhere them and play the role of isolation. Then, the separator is wound up to obtain an electrode assembly. The electrode assembly is placed into a battery housing, dried, and then an electrolyte solution is injected in an amount of 2.4 g / Ah to obtain a newly manufactured secondary battery. (2) The secondary battery is formed by sealing the battery under normal pressure at a formation temperature of 45° C., a current of 0.1 C, and a voltage of 3 to 4.3 V, and then allowed to stand to produce the secondary batteries of the present invention and the comparative examples.
[0143] [Table 4-1] [Table 4-2]
[0144] 5. Testing 5.1 Ternary layer detection The ternary layer can be detected by means conventional in the art, such as solid-state nuclear magnetism, X-ray powder diffraction (XRD), X-ray photoelectron spectroscopy (XPS), Raman spectroscopy, or a combination of the above means.
[0145] 5.2 Internal resistance of the initial secondary battery and the internal resistance of the secondary battery after 1000 cycles (1) The secondary battery (hereinafter referred to as "new battery") prepared in the above steps is charged at a constant current of 1C to 4.3V at 45℃, then charged at a constant voltage of 4.3V until the current is less than 0.05C, and the lithium-ion battery is discharged at a constant current of 1C to 3.0V, thus completing one charge-discharge process (i.e., one cycle). The above cycle is repeated 1000 times to obtain a secondary battery cycled 1000 times at 45℃ (hereinafter referred to as "battery with 1000 cycles at 45℃"). (2) At 25℃, the above newly manufactured batteries and the batteries after 1000 cycles at 45℃ are charged at a constant current of 1C to 4.3V, then charged at a constant voltage of 4.3V until the current is less than 0.05C, and discharged at 1C for 30min, i.e., the charge amount of the secondary battery is adjusted to 50% battery state of charge (SOC). Next, the positive and negative pens of the TH2523A AC internal resistance tester (Tonghui Electronics) are respectively contacted with the positive and negative poles of the two secondary batteries under test, and the internal resistance value of the battery is read through the internal resistance tester, which are the internal resistance of the initial secondary battery and the internal resistance of the secondary battery after 1000 cycles, respectively.
[0146] 5.3 Capacity retention after 1000 cycles at 45℃ The test uses Wuhan Blue-Electric. At 45℃, the secondary battery is charged at 1C to 4.3V at constant current, then charged at 4.3V at constant voltage until the current is less than 0.05C, and the lithium-ion battery is discharged at 1C to 3.0V at constant current, which is one charge-discharge process (i.e., one cycle, or the first cycle), and the discharge capacity of the first cycle is recorded. This is repeated for 1000 cycles, and the discharge capacity of the 1000th cycle is recorded. The capacity retention rate of the secondary battery when it is cycled 1000 times is calculated according to the following formula: Capacity retention (%) of a lithium-ion battery after 1000 cycles at 45°C = (discharge capacity at 1000th cycle / discharge capacity at first cycle) x 100%.
[0147] 5.4 Capacity retention after 300 days storage at 60℃ At 25℃, charge at a constant current of 1C until the voltage reaches 4.3V, then charge at a constant voltage of 4.3V until the current reaches 0.05C, and discharge the lithium-ion battery at a constant current of 1C until the voltage reaches 3.0V, completing one charge-discharge process (i.e., one cycle, or the first cycle), at which point the discharge capacity of the first cycle of the secondary battery is tested. Next, place the fully charged secondary battery in a thermostatic box at 60℃ and store it for 300 days, and test the discharge capacity after 300 days of storage. Capacity retention (%) after storing a lithium-ion battery for 300 days at 60°C = (discharge capacity after 300 days storage / discharge capacity of the first cycle) x 100%.
[0148] The above test results are recorded in Table 5-9 below.
[0149] [Table 5]
[0150] As can be seen from the above table, in Comparative Example 1, the secondary battery in which the positive active material is LFP and the negative active material is a silicon carbon composite material does not contain the interface passivator of the present application, and the cycle life of the secondary battery is short. In contrast, the secondary batteries in Examples 1-2 and 4-5 contain the interface passivator of the present application, which can effectively improve the capacity retention rate, reduce the battery impedance, and improve the battery performance.
[0151] Regardless of any theory, in Comparative Example 1, such a poor cycle life is mainly due to the silicon carbon composite material contained in the negative electrode undergoing a large volume change during the lithium release-lithium absorption process of the charge-discharge cycle, which leads to cracking and regeneration of the interface component. After multiple cycles, the interface component becomes thicker. Therefore, the internal resistance of the secondary battery of Comparative Example 1 after 1000 cycles is high, and active lithium is consumed due to cracking and regeneration of the interface, so the capacity retention rate drops rapidly during the cycle process. In addition, the fully charged silicon-based negative electrode has high interface activity and consumes excessive electrolyte, so the capacity retention rate after 300 days of storage at 60°C is low. However, in the secondary battery of the present application, the included interface passivator forms a ternary interface passivation layer at the interface between the negative electrode material layer and the electrolyte during the charge-discharge cycle, which reduces the reaction activity of the negative electrode interface. In addition, with an increase in the number of cycles, the above-mentioned advantages of the secondary battery of the present application become more prominent.
[0152] In addition, from the data in the above table, it can be seen that the secondary battery of Example 3 contains a cobalt salt, and the secondary battery of Example 6 contains a manganese salt, which does not achieve the beneficial effects of Examples 1-2 and 4-5, but rather deteriorates the battery performance.
[0153] [Table 6]
[0154] As can be seen from the above table, the secondary battery in Comparative Example 2, in which the positive electrode active material is NCM811 and the negative electrode active material is a silicon carbon composite material, has a poor cycle life. However, the secondary batteries in Examples 7-8 (in which the negative electrode material layer contains an interface passivator) and 10-11 (in which the electrolyte contains an interface passivator) have significantly improved cycle performance.
[0155] Regardless of the theory, the reason why the secondary battery of Comparative Example 2 has such a poor cycle life is that in addition to the large volume change of the silicon-carbon material itself and the instability of the NCM811 structure, the migration and catalysis of transition metal ions are also important influencing factors that lead to interfacial instability.
[0156] In Examples 7-8 and 10-11 of the present application, by including an interface passivation agent, such a multivalent salt can form an interface passivation layer with silicon to stabilize the electrode-electrolyte interface. The secondary battery of the present application can effectively improve the capacity retention rate, reduce the impedance of the secondary battery, and improve the performance of the secondary battery.
[0157] The inclusion of a cobalt salt in the negative electrode of Example 9 and a manganese salt in the electrolyte of Example 12 do not improve cycle performance.
[0158] [Table 7]
[0159] In Comparative Example 2, the positive electrode of the secondary battery made of NCM811 uses a non-modified silicon carbon composite material, and the cycle life of the secondary battery is poor.
[0160] The secondary batteries of Examples 13, 15-16 and 18-19 contain calcium, magnesium, aluminum and beryllium interface passivation agents, which can effectively improve the capacity retention rate, reduce the battery impedance and improve the battery performance.
[0161] The inclusion of nickel, cobalt, and manganese salts in Examples 14, 17, and 20 deteriorates the performance of the secondary battery.
[0162] [Table 8]
[0163] In Comparative Example 2, the secondary battery in which the positive electrode material is NCM811 does not use the interface passivator of the present invention, and the cycle life of the secondary battery is poor.
[0164] The secondary batteries of Examples 21-22 contain organic or inorganic salts of calcium, magnesium, aluminum, and beryllium, and thus have significantly improved cycle performance. The secondary batteries of Examples 23-27 contain salts of nickel, cobalt, and manganese, and thus have a significant effect of deteriorating the performance of the secondary batteries. In Examples 24 and 25, although the negative electrode contains cobalt, which deteriorates the performance, the positive electrode and electrolyte contain beryllium, magnesium, or aluminum, and thus the degree of deterioration can be slightly reduced.
[0165] [Table 9]
[0166] In Example 28, the negative active material is surface-coated with aluminum phosphate, which has a certain effect on improving the battery performance compared with Comparative Example 2, but the degree of improvement is small. It is not easy for such a coating layer structure to be stable and to react with the negative active material to form the ternary layer described in the present application, and it is difficult to avoid cracking of the interface layer even after the coating layer is cycled multiple times, so the performance improvement effect is very limited.
[0167] The interface passivation agent calcium salt is introduced into the negative electrode material of Example 7, which can significantly improve the overall performance of the secondary battery compared with Comparative Example 2, and the degree of improvement is much higher than that of Example 28. The materials of Examples 29 and 30 are introduced with two kinds of multivalent salts, which can significantly improve the performance of the secondary battery compared with the case of introducing one kind of multivalent salt into Example 7. It shows that the effect of the combined additive is better than the improvement effect of a single salt.
[0168] [Table 10]
[0169] Compared with Example 2, Examples 31-50 investigated the addition of different amounts of multivalent salt additives to the positive electrode, negative electrode, and electrolyte, respectively. The results show that, compared with Comparative Example 2, which does not contain additives, the secondary batteries of Examples 31-50 contain organic or inorganic salts of calcium, magnesium, aluminum, and beryllium, which greatly improves the battery cell performance.
[0170] The present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and any embodiment having substantially the same configuration as the technical idea within the scope of the technical solution of the present application and having similar effects is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can conceive of in the embodiment, and other forms constructed by combining some of the components of the embodiment, are also included in the scope of the present application, within the scope of the present application, without departing from the gist of the present application. [Explanation of symbols]
[0171] 1 Battery pack 2 Upper box 3 Lower box 4 Battery Module 5 Secondary battery 51 Housing 52 Electrode Assembly 53 Top cover assembly
Claims
1. 1. A secondary battery comprising: a negative electrode sheet including a negative electrode material layer, a positive electrode sheet including a positive electrode material layer, and an electrolyte, wherein at least one of the negative electrode material layer, the positive electrode material layer, and the electrolyte comprises an interface passivator, the interface passivator being a compound containing an element E, the element E being selected from the group consisting of lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, gallium, and germanium.
2. 2. The secondary battery according to claim 1, wherein the surface of the negative electrode material layer has an A-D-E ternary layer, A is selected from alkali metal elements and is different from E, and D is silicon or carbon, and the A-D-E ternary layer is formed by the action of the interface passivation agent on the surface of the negative electrode material layer during at least one charging process of the secondary battery.
3. 3. The secondary battery according to claim 1 or 2, wherein the interface passivation agent is selected from at least one of compounds of beryllium, magnesium, calcium, aluminum and gallium, preferably, the interface passivation agent is selected from at least one of compounds of beryllium, magnesium, calcium and aluminum.
4. The interfacial passivation agent may be a substituted or unsubstituted C 1-20 and the substituent is selected from at least one of C 1-6 Alkyl group, C 2-6 Cycloalkyl group, hydroxyl group, amino group, oxo group, acyl group, C 1-6 The secondary battery according to any one of claims 1 to 3, wherein the E is one or more selected from an alkylthio group, a phenyl group, a benzoylthio group, a phenylthio group, a phenoxy group, an amino acid salt, an enoate salt, a phosphate salt, a sulfate salt, a sulfonylimide salt, a sulfonate salt, a benzoate salt, a phthalate salt, an acetylacetonate salt, an inorganic oxyacid salt, and a double salt of a cation containing at least two of the E.
5. 5. The secondary battery according to claim 1, wherein the interface passivator is doped and mixed into at least one of the positive electrode material layer, the negative electrode material layer, and the electrolyte.
6. The ADE ternary layer is Li-Si-Ca, Li-Si-Mg, Li-Si-Be, Li-Si-Al, Li-C-Ca, Li-C-Mg, Li-C-Be, Li-C-Al, Na- selected from Si-Ca, Na-Si-Mg, Na-Si-Be, Na-Si-Al, Na-C-Ca, Na-C-Mg, Na-C-Be, Na-C-Al ternary layer and combinations thereof; Preferably, the A-D-E ternary layer is selected from Li-Si-Ca, Li-Si-Mg, Li-Si-Be, Li-Si-Al, Na-Si-Ca, Na-Si-Mg, Na-Si-Be, Na-Si-Al ternary layers and combinations thereof. The secondary battery according to any one of claims 1 to 5.
7. 7. The secondary battery according to claim 2, wherein the positive electrode material layer comprises 0.001% by weight to 20% by weight, preferably 1% by weight to 10% by weight, of the interface passivator, based on the total weight of the positive electrode material layer, before the at least one charging.
8. The secondary battery according to any one of claims 2 to 7, wherein the negative electrode material layer comprises 0.001 wt % to 20 wt %, preferably 0.05 wt % to 5 wt %, of the interface passivator, based on the total weight of the negative electrode material layer, before the at least one charging.
9. 9. The secondary battery according to claim 2, wherein the electrolyte comprises, based on the total weight of the electrolyte, 0.001% by weight to 20% by weight, preferably 0.1% by weight to 5% by weight of the interface passivator, before the at least one charging.
10. The secondary battery according to any one of claims 1 to 9, wherein the negative electrode material layer contains a negative electrode active material, and the negative electrode active material has a D50 of 1 µm to 20 µm, preferably 1 µm to 10 µm.
11. the negative electrode material layer includes a negative electrode active material, and the negative electrode active material has a Span value of 0.9 to 1.8, preferably 0.9 to 1.2; Where: [0030] and 11. The secondary battery according to claim 1, wherein D90, D10 and D50 represent particle sizes corresponding to cumulative distribution rates of 90%, 10% and 50%, respectively.
12. A secondary battery, comprising: i) providing an anode sheet including an anode material layer, a cathode sheet including a cathode material layer, and an electrolyte to manufacture an uncycled secondary battery, wherein at least one of the anode material layer, the cathode material layer, and the electrolyte includes an interface passivator, the interface passivator being a compound including an element E, the element E being selected from the group consisting of lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, gallium, and germanium; ii) charging and discharging the uncycled secondary battery for at least one cycle.
13. A method for manufacturing a secondary battery, comprising the steps of: i) providing an anode sheet including an anode material layer, a cathode sheet including a cathode material layer, and an electrolyte to manufacture an uncycled secondary battery, wherein at least one of the anode material layer, the cathode material layer, and the electrolyte includes an interface passivator, the interface passivator being a compound including an element E, the element E being selected from the group consisting of lithium, sodium, beryllium, magnesium, potassium, calcium, aluminum, gallium, and germanium; ii) charging and discharging the uncycled secondary battery for at least one cycle to form an A-D-E ternary layer to obtain the secondary battery, wherein A is selected from an alkali metal element and is different from E, and D is silicon or carbon.
14. 14. The method of claim 13, wherein the interfacial passivator is selected from at least one of compounds of beryllium, magnesium, calcium, aluminum and gallium, preferably, the interfacial passivator is selected from at least one of compounds of beryllium, magnesium, calcium and aluminum.
15. The interfacial passivation agent may be a substituted or unsubstituted C 1-20 and the substituent is selected from at least one of C 1-6 Alkyl group, C 2-6 Cycloalkyl group, hydroxyl group, amino group, oxo group, acyl group, C 1-6 15. The method according to claim 13 or 14, wherein the non-transition metal cation is one or more selected from the group consisting of alkylthio groups, phenyl groups, benzoylthio groups, phenylthio groups and phenoxy groups, amino acid salts, enoates, phosphates, sulfates, sulfonylimides, sulfonates, benzoates, phthalates, acetylacetonates, inorganic oxyacid salts, and double salts containing at least two of the non-transition metal cations.
16. 16. The method of any one of claims 13 to 15, wherein in step i), the interfacial passivation agent is doped and mixed into at least one of the positive electrode material layer, the negative electrode material layer and the electrolyte.
17. A battery module comprising the secondary battery according to any one of claims 1 to 12 or a secondary battery obtained by the method according to any one of claims 13 to 16.
18. A battery pack comprising the battery module according to claim 17.
19. An electric device comprising at least one selected from the group consisting of the secondary battery according to any one of claims 1 to 12, the secondary battery obtained by the method according to any one of claims 13 to 16, the battery module according to claim 17, and the battery pack according to claim 18.
Citation Information
Patent Citations
Electrochemical device and electronic device
CN114388811A
Nonaqueous system electrolyte battery
JP1995192760A
Nonaqueous electrolyte secondary battery
JP2005085589A
Lithium secondary battery and its producing method
JP2006278185A
Nonaqueous electrolytic secondary battery
JP2008288112A