Electrolytic copper foil for secondary battery current collector
An electrolytic copper foil with tailored crystal orientation and additives addresses production costs and adhesion issues, enhancing mechanical properties and contact with active materials, resulting in improved battery stability and performance.
Patent Information
- Application Number
- JP2024525745
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-29
- Filing Date
- 2022-10-07
- Publication Date
- 2024-10-18
AI Technical Summary
Existing electrolytic copper foils for secondary battery current collectors face challenges such as high production costs, contamination from lubricating oil, reduced adhesion to active materials, volume changes and heat generation during lithium battery use, uneven surface roughness affecting battery characteristics, and poor contact with active materials, leading to reduced cycle life and performance.
The development of an electrolytic copper foil with specific crystal orientation and additives to achieve high mechanical strength, elongation, and uniform coating on both sides, ensuring good contact with active materials, and maintaining surface roughness consistency.
The solution provides a copper foil with high mechanical strength and elongation across various temperatures, enabling stable and uniform active material coating, improving battery performance and lifespan by preventing cracks and wrinkles.
Smart Images

Figure 2024538308000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolytic copper foil, and more particularly to an electrolytic copper foil for use as a current collector for a secondary battery. [Background technology]
[0002] Copper foil is generally used as a current collector for secondary batteries. The copper foil is mainly rolled copper foil produced by rolling, but the manufacturing cost is high and it is difficult to produce wide copper foil. In addition, rolled copper foil requires the use of lubricating oil during rolling, and the adhesion to the active material decreases due to contamination of the lubricating oil, which may result in a decrease in the charge / discharge cycle characteristics of the battery.
[0003] Lithium batteries undergo volumetric changes during charging and discharging and heat generation due to overcharging. In addition, the surface roughness of the copper foil must be low so that it can improve adhesion with the electrode active material, and has a relatively small effect on the copper foil base material in relation to the expansion and contraction of the active material layer due to the charge and discharge cycle, and prevents the copper foil as a current collector from wrinkling or breaking. Therefore, a copper foil that can withstand the volumetric changes and heat generation phenomenon of lithium batteries and has excellent adhesion with the active material, high elongation, high strength, and low roughness is required. In addition, when used as an anode current collector for secondary batteries, both sides of the copper foil are coated with electrode active material. In this case, if the roughness of both sides of the electrolytic copper foil is different, the battery characteristics will differ, so it is necessary to maintain the roughness of both sides of the electrolytic copper foil at the same or similar level.
[0004] In the manufacturing process of a secondary battery using such an electrolytic copper foil, the copper foil is vacuum-dried. However, since vacuum drying is a process that is performed at high temperature for a long time, the adhesive strength and stress between the copper foil and the active material coating surface change during the vacuum drying of the copper foil, which may shorten the life of the battery or cause cracks.
[0005] When electrolytic copper foil is used as an anode current collector for a secondary battery, both sides of the copper foil are coated with an electrode active material. Therefore, it is preferable that the surface of the electrolytic copper foil provides good contact with the active material. However, conventional approaches to provide good contact with the active material are limited to controlling the surface roughness of the electrolytic copper foil.
[0006] Therefore, there is a demand for electrolytic copper foils for use as current collectors for secondary batteries that have high mechanical properties over a wide range of temperatures and, at the same time, can provide good contact properties with active materials.
[0007] Good contact properties between the electrolytic copper foil and the active material may be related to the surface energy of the electrolytic copper foil and may be determined by the orientation of the crystal plane of the copper foil. The crystal orientation of the copper foil may also affect the tensile strength and elongation rate, so it is necessary to design the crystal orientation of the electrolytic copper foil for high strength, high elongation rate, and / or good contact properties. Summary of the Invention [Problem to be solved by the invention]
[0008] In order to solve the above-mentioned problems of the prior art, an object of the present invention is to provide an electrodeposited copper foil having high mechanical strength and high elongation in a wide temperature range.
[0009] Another object of the present invention is to provide an electrolytic copper foil having high mechanical strength and high elongation even when a high-temperature drying process is applied.
[0010] Another object of the present invention is to provide an electrolytic copper foil for a current collector of a secondary battery, which can provide good contact performance with an active material coating containing a water-based binder.
[0011] Another object of the present invention is to provide an electrolytic copper foil for use as a current collector for a secondary battery, which enables uniform coating of an active material on both sides of the electrolytic copper foil.
[0012] Another object of the present invention is to provide an electrolytic copper foil having a crystal orientation designed for high strength, high elongation, and / or good contact properties. [Means for solving the problem]
[0013] In order to achieve the above technical objectives, the present invention provides an electrodeposited copper foil, characterized in that the stretch ratio relative to thickness at room temperature is 1.3 to 2.0% / μm, and in an XRD spectrum of a deposit surface at room temperature, I(200) / I(111), which is the ratio of the diffraction peak intensity I(200) for the (200) crystal plane to the diffraction peak intensity I(111) for the (111) crystal plane, is 0.4 to 0.5.
[0014] The electrolytic copper foil of the present invention has a tensile strength of 40 kgf / mm 2 In the XRD spectrum for the deposition surface at room temperature, the ratio I(200) / I(111), which is the ratio of the diffraction peak intensity I(200) for the (200) crystal plane to the diffraction peak intensity I(111) for the (111) crystal plane, may be 0.4 to 0.5.
[0015] In the electrodeposited copper foil of the present invention, when A is the ratio of the diffraction peak intensity I(200) of the (200) crystal plane to the diffraction peak intensity I(111) of the (111) crystal plane in the XRD spectrum of the deposit side at room temperature, and B is the ratio I(200) / I(111) of the diffraction peak intensity I(200) of the (200) crystal plane to the diffraction peak intensity I(111) of the (111) crystal plane in the XRD spectrum of the deposit side after heat treatment at 200° C. for 1 hour, A>B. In this case, A and B may have a relationship of -0.3<(BA) / A<-0.1.
[0016] In addition, in the XRD spectrum of the deposition surface of the electrodeposited copper foil of the present invention at room temperature, the ratio of the orientation index M(200) for the (200) crystal plane to the orientation index M(111) for the (111) crystal plane, M(200) / M(111), may be 0.5 to 1.
[0017] In the electrodeposited copper foil of the present invention, C may be greater than D, where C is the ratio of the orientation index M(200) to the (200) crystal plane and the orientation index M(111) to the (111) crystal plane in an XRD spectrum of the deposit side at room temperature, and D is the ratio of the orientation index M(200) to the (200) crystal plane and the orientation index M(111) to the (111) crystal plane in an XRD spectrum of the deposit side after heat treatment at 200° C. for 1 hour. In this case, C and D may have a relationship of -0.3<(DC) / C<-0.1.
[0018] The electrodeposited copper foil of the present invention may have a TOC content of 5 to 8 ppm.
[0019] Moreover, the electrolytic copper foil of the present invention may have a thickness-to-thickness elongation ratio after heat treatment at 200° C. for 1 hour of 1.4 to 2.4% / μm.
[0020] In addition, the electrodeposited copper foil of the present invention may have a ratio of the elongation rate relative to the thickness after heat treatment at 200° C. for 1 hour to the elongation rate relative to the thickness at room temperature of 1.05 to 1.25. Effect of the Invention
[0021] According to the present invention, it is possible to provide an electrolytic copper foil having high mechanical strength and a high elongation rate in various temperature ranges.
[0022] Furthermore, according to the present invention, it is possible to provide a current collector that can provide good contact performance to an active material coating that contains a water-based binder.
[0023] Furthermore, according to the present invention, it is possible to provide a secondary battery current collector that enables uniform coating of active material on both sides of the electrolytic copper foil. [Brief description of the drawings]
[0024] [Figure 1A]1A and 1B are diagrams showing XRD analysis results of copper foil test pieces at room temperature and high temperature, respectively, according to an embodiment of the present invention. [Figure 1B] 1A and 1B are diagrams showing XRD analysis results of copper foil test pieces at room temperature and high temperature, respectively, according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The embodiments described in this specification and the configurations shown in the drawings are merely the most preferred embodiments of the present invention and do not represent all of the technical ideas of the present invention, so it should be understood that there are various equivalents and modifications that can replace them at the time of filing this application. Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0026] In the present specification, the S side refers to the side that comes into contact with the drum during the production process of the electrodeposited copper foil and is generally referred to as the gloss side, and the M side refers to the opposite side, which is generally referred to as the deposit side or matte side. These terms do not express the roughness of the respective sides, and it goes without saying that the S side may have a lower gloss or a higher surface roughness than the M side.
[0027] In the present invention, the electrodeposited copper foil has a tensile strength at room temperature (hereinafter referred to as "room temperature tensile strength") of 40 kgf / mm 2 The electrolytic copper foil preferably has a room temperature tensile strength of 50 kgf / mm 2 Less than or equal to 45kgf / mm 2 It is preferable that:
[0028] The room temperature tensile strength of copper foil is 40kgf / mm 2 If it is less than 50 kgf / mm, there is a high possibility that defects such as wrinkles, distortions, and bending may occur due to plastic deformation when the negative electrode active material is coated on the copper foil at high speed in the process of forming the anode in the lithium secondary battery. 2If the temperature exceeds 100° C., the occurrence of distortion or wrinkles may be reduced, but there is a high possibility that a high tension imbalance may occur during high-speed coating of the negative active material, and the brittleness of the copper foil itself may increase, which may cause cracks and breaks.
[0029] The electrolytic copper foil of the present invention has high tensile strength even after high-temperature heat treatment. The electrolytic copper foil of the present invention has a tensile strength of 36 kgf / mm after heat treatment at 200° C. for 1 hour (hereinafter referred to as "high-temperature tensile strength"). 2 The electrolytic copper foil preferably has a high-temperature tensile strength of 45 kgf / mm 2 Less than or equal to 42kgf / mm 2 It is preferable that:
[0030] In the present specification, the high-temperature tensile strength is a measured value that imitates the process of high-temperature processes such as coating dry and vacuum dry during the process of forming the anode of a lithium secondary battery. The high-temperature tensile strength of copper foil is 36 kgf / mm 2 If it is less than 45kgf / mm, deformation occurs due to the stress caused by the volume expansion of the negative electrode during charging and discharging of the lithium secondary battery, causing a decrease in lifespan during charging and discharging. 2 If it exceeds this value, the deformation due to stress caused by volume expansion decreases, but the brittleness of the copper foil increases, and cracks and electrode detachment due to accumulation of stress occur, shortening the life of the electrode. Electrodeposited copper foil is required to have a high elongation rate with appropriate strength.
[0031] In the present invention, the ratio of the high-temperature tensile strength to the room-temperature tensile strength is preferably 0.9 or more, and the tensile strength ratio is less than 1, preferably less than 0.95. In the present invention, the electrodeposited copper foil is characterized in that the deterioration of the tensile strength due to high-temperature heat treatment is suppressed as much as possible.
[0032] In the present invention, the electrolytic copper foil has a high elongation. Specifically, the electrolytic copper foil of the present invention has a higher value obtained by dividing the elongation by the thickness (hereinafter referred to as "elongation per unit thickness") than conventional electrolytic copper foils. For example, the elongation per unit thickness at room temperature (hereinafter referred to as "elongation per unit thickness at room temperature") may be 1.3% / μm or more, or 1.5% / μm or more. In addition, the elongation per unit thickness at room temperature may be 2.0% / μm or less, 1.9% / μm or less, or 1.8% / μm or less. In addition, in the present invention, the electrolytic copper foil exhibits a high elongation even after high-temperature heat treatment. The electrolytic copper foil of the present invention may have a thickness-to-thickness elongation ratio after heat treatment at 200° C. for 1 hour (hereinafter referred to as “high-temperature thickness-to-thickness elongation ratio”) of 1.4% / μm or more, 1.5% / μm or more, or 1.6% / μm or more. The high-temperature thickness-to-thickness elongation ratio of the electrolytic copper foil may be 2.4% / μm or less, 2.2% / μm or less, or 2.0% / μm or less.
[0033] In order to improve the energy density of a lithium secondary battery, the content of active materials must be increased and the thickness of non-active materials such as copper foil, aluminum foil, and separator must be reduced. Therefore, the higher the energy density of a lithium secondary battery, the thinner the required copper foil thickness. However, as the copper foil becomes thinner, the physical energy content of the foil decreases. Therefore, the thinner the thickness, the more likely it is to break or crack even when a small external stress is applied. Therefore, only if the copper foil has a certain or higher elongation rate per thickness can a stable product be manufactured in a copper foil manufacturing process or a secondary battery electrode manufacturing process using the copper foil, and a stable life performance can be realized during charging and discharging of the secondary battery. As described below, the electrolytic copper foil of the present invention has a high elongation rate per thickness even at a thin thickness.
[0034] In the present invention, the electrodeposited copper foil exhibits a high elongation ratio relative to thickness even at a thickness as small as 2 μm or 4 μm. For example, the thickness range in which the copper foil of the present invention exhibits the above-mentioned elongation ratio relative to thickness may be in the range of 2 to 12 μm, 4 to 12 μm, 2 to 10 μm, or 4 to 10 μm.
[0035] In addition, in the present invention, the elongation ratio relative to thickness of the electrolytic copper foil shows a narrow deviation over the range of copper foil thicknesses. For example, an electrolytic copper foil having a thickness of 4 μm may have a similar elongation ratio relative to thickness value to an electrolytic copper foil having a thickness of 12 μm.
[0036] In addition, the electrodeposited copper foil of the present invention has a ratio of the high-temperature elongation rate to the room-temperature elongation rate (elongation rate ratio) of 1 or more, or 1.05 or more. In addition, the ratio of the high-temperature elongation rate to the room-temperature elongation rate (elongation rate ratio) may be 1.25 or less, or 1.2 or less.
[0037] The electrodeposited copper foil of the present invention has the following relationship between the peak intensities of specific crystal planes on the XRD spectrum and the orientation index (M) calculated from the XRD spectrum, as described below.
[0038] Here, the orientation index is a value measured using the orientation index (M) proposed by S. Yoshimura, S. Yoshihara, T. Shirakashi, and E. Sato, Electrochim, Acta 39, 589 (1994).
[0039] For example, for a specimen having a (111) surface, the orientation index (M) is calculated as follows:
[0040] IFR(111)=IF(111) / {IF(111)+IF(200)+IF(220)+IF(311)}
[0041] IR(111)=I(111) / {I(111)+I(200)+I(220)+I(311)}
[0042] M(111)=IR(111) / IFR(111)
[0043] IF(111) is the XRD intensity in the JCPDS cards, and I(111) is the experimental value. If M(111) is greater than 1, it means that the material has a preferred orientation parallel to the (111) plane, and if M is less than 1, the preferred orientation decreases.
[0044] (blank paragraph)
[0045] The electrodeposited copper foil of the present invention may have the following room temperature XRD spectrum characteristics for the M plane:
[0046] In the XRD spectrum, I(200) / I(111) may have a value of 0.5 or less, or 0.45 or less. In the present invention, in the XRD spectrum of the copper foil deposit side, I(200) / I(111) may be 0.35 or more, or 0.40 or more.
[0047] (blank paragraph)
[0048] In addition, the electrodeposited copper foil of the present invention may have a crystal plane orientation index (M), M(200) / M(111), of 1 or less, 0.95 or less, or 0.93 or less. Also, M(200) / M(111) may have a value of 0.8 or more, or 0.85 or more.
[0049] (blank paragraph)
[0050] On the other hand, the electrodeposited copper foil of the present invention has a reduced I(200) / I(111) in the XRD spectrum after heat treatment at 200°C for 1 hour (hereinafter referred to as "high temperature"). For example, I(200) / I(111) may have a value of 0.4 or less, or 0.35 or less. Also, at high temperatures, I(200) / I(111) may have a value of 0.2 or more, or 0.25 or more.
[0051] In addition, the electrodeposited copper foil of the present invention has a decreased M(200) / M(111) in the XRD spectrum after heat treatment at 200°C for 1 hour (hereinafter referred to as "high temperature"). For example, at high temperature, M(200) / M(111) may have a value of 0.8 or less, 0.75 or less, or 0.7 or less. In addition, M(200) / M(111) may have a value of 0.6 or more, or 0.65 or more.
[0052] The present invention may be manufactured using an electrolyte containing a combination of additives selected from the following additives A to C so that the electrolytic copper thin film has high strength and high elongation at room temperature and has a specific orientation of the crystal plane of the electrolytic copper thin film.
[0053] (blank paragraph)
[0054] Additive A
[0055] Additive A is a thiourea compound, a compound in which a thiol group is linked to a nitrogen-containing heterocycle, or a mixture thereof.
[0056] Here, the thiourea compound is ethylenethiourea, diethylthiourea, acetylenethiourea, dipropylthiourea, dibutylthiourea, N-trifluoroacetylthiourea, N-ethylthiourea, N-cyanoacetylthiourea, N-allylthiourea, o-tolylthiourea, N,N'-butylene ... The thiourea compound may be at least one selected from the group consisting of 4-thiourea, thiazolidinethiol, 4-thiazolinethiol, 4-methyl-2-pyrimidinethiol, and 2-thiouracil, but is not necessarily limited thereto, and various thiourea compounds that can be used as additives in the field of the art may be used.
[0057] The compound having a thiol group linked to a nitrogen-containing heterocycle of the additive A may be at least one selected from the group consisting of 2-mercapto-5-benzoimidazole sulfonic acid sodium salt, sodium 3-(5-mercapto-1-tetrazolyl)benzene sulfonate, and 2-mercapto benzothiazole, but is not necessarily limited thereto. Any compound having a thiol group linked to a nitrogen-containing heterocycle that can be used as an additive in the field of the art may be used.
[0058] In the present invention, the additive A is preferably added to the electrolyte solution at a concentration of less than 2 ppm, and more preferably, the additive A is added at 0.5 to 1.9 ppm.
[0059] Additive A can improve the strength of the electrolytic copper foil. If the content of Additive A exceeds 1.9 ppm, the surface roughness of the deposit side increases, making it difficult to produce an electrolytic copper foil with low roughness, and the elongation rate may decrease.
[0060] (blank paragraph)
[0061] Additive B
[0062] Additive B is a sulfonic acid or a metal salt thereof, which is a compound containing a sulfur atom.
[0063] For example, sulfonic acids or metal salts thereof of compounds containing sulfur atoms include bis-(3-sulfopropyl)-disulfide disodium salt (SPS), 3-mercapto-1-propanesulfonic acid (MPS), 3-(N,N-dimethylthiocarbamoyl)-thiopropanesulfonate sodium salt (DPS), 3-[(amino-iminomethyl)thio]-1-propanesulfonate sodium salt (UPS), o-ethyldithiocarbonate-S-(3-sulfopropyl)-ester sodium salt (OPX), 3-(benzothiazolyl-2-mercapto)-propylsulfonic acid sodium salt (ZPS), ethylenedithiodipropylsulfonic acid sodium salt, thioglycolic acid, thiophosphoric acid-o-ethyl-bis-(ω-sulfopropyl)ester disodium salt, The sulfonic acid may be at least one selected from the group consisting of thiophosphoric acid-tris-(ω-sulfopropyl)ester trisodium salt, and thiophosphoric acid-tris-(ω-sulfopropyl)ester trisodium salt, but is not necessarily limited thereto, and any sulfonic acid or metal salt thereof of a compound containing a sulfur atom that can be used as an additive in the field of the art may be used.
[0064] In the present invention, the additive B is preferably added to the electrolytic solution in an amount of 20 to 80 ppm.
[0065] Additive B can improve the surface gloss of the electrolytic copper foil. If the content of Additive B is less than 20 ppm, the gloss of the electrolytic copper foil may be reduced, and if the content of Additive B is more than 80 ppm, the surface roughness of the deposit surface increases, making it difficult to manufacture an electrolytic copper foil with low roughness, and the tensile strength of the electrolytic copper foil may be reduced.
[0066] (blank paragraph)
[0067] Additive C
[0068] Additive C is a non-ionic water-soluble polymer.
[0069] The nonionic water-soluble polymer may be polyethylene glycol, polyglycerin, nonylphenol polyglycol ether, octanediol-bis-(polyalkylene glycol ether), octanol polyalkylene glycol ether, oleic acid polyglycol ether, polyethylene propylene glycol, polyethylene glycol dimethyl ether, polyoxypropylene glycol, polyvinyl alcohol, β-naphthol polyglycol ether, stearic acid polyglycol ether, and stearyl alcohol polyglycol ether. However, the present invention is not limited thereto, and any water-soluble polymer usable as an additive in the field of the art may be used. For example, the molecular weight of the polyethylene glycol may be 100 to 20,000.
[0070] The nonionic water-soluble polymer may be at least one selected from the group consisting of hydroxyethyl cellulose and carboxymethyl cellulose, but is not necessarily limited thereto.
[0071] The nonionic water-soluble polymer is a water-soluble proteinaceous gelatin such as gelatin and collagen, and has a structure in which glycine, hydroxylysine, and hydroxyproline are repeated, and there are six or more types including type I, type II, and type V. A chain in which three types of amino acids are repeated is called an alpha chain, and a triple helix is formed when three alpha chains are wound around each other. In general, the complex structure of collagen is formed by cross-linking the triple helices. The nonionic water-soluble polymer of the present invention may be one or more selected from the group consisting of collagen and gelatin, but is not necessarily limited thereto.
[0072] In the present invention, the additive C is preferably added to the electrolytic solution in an amount of 5 to 10 ppm.
[0073] In the copper electrolyte, the additive C can reduce the surface roughness of the electrolytic copper foil and improve the surface gloss. If the content of the additive C is less than 5 ppm, the surface roughness of the deposit surface increases, making it difficult to manufacture an electrolytic copper foil with a low roughness, and the gloss of the electrolytic copper foil may decrease. If the content of the additive C is more than 10 ppm, the high-temperature strength and high-temperature hardness of the electrolytic copper foil may decrease.
[0074] The effects of the additives A, B, and C in the electrolyte on the physical properties of the electrolytic copper foil have been described above, but the above description is merely illustrative. It is understood that the type, content, or combination of each additive of the present invention may affect other physical properties of the electrolytic copper foil produced by the present invention through unknown mechanisms.
[0075] Although it cannot be clearly defined, in the present invention, the XRD spectrum may change depending on the type, content, and / or relative ratio of the additives. For example, when the concentration of additive C increases or the relative ratio of additive C to additives A and B increases, the (200) plane of the electrolytic copper film tends to decrease. EXAMPLES
[0076] <Electrolytic copper foil manufacturing example 1>
[0077] (Examples 1 to 5)
[0078] In an electrolyte solution containing 200-452g / L CuSO45H2O, 30-250g / L sulfuric acid, and 10-30ppm chloride ion concentration, at 50-60℃ and 50-70A / dm 2 Electrolytic plating was performed at a current density of 100000 (ASD). 0.5 to 1.9 ppm of ETU (ethylene thiourea) was added as additive A, and 20 to 80 ppm of DPS (3-(N,N-dimethylthiocarbamoyl)-thiopropanesulfonate sodium salt) and 5 to 10 ppm of PEG (polyethylene glycol, molecular weight Mw: 500 to 4000) were added as additive B to the electrolyte. The composition of the electrolyte used in each example is shown in Table 1. The thickness of the plating film was varied depending on the example.
[0079] (blank paragraph)
[0080] Comparative Example 1
[0081] In an electrolyte solution of Cu 100g / L, sulfuric acid 150g / L, and chloride ion concentration 20ppm, at 50-60℃, 50-70A / dm 2 Electrolytic plating was performed at a current density of 100000 (ASD) to produce a plating film with a thickness of 18 μm. 2 ppm of DET (diethylthiourea) was added as additive A, 45 ppm of SPS (bis-(3-sulfopropyl)-disulfide disodium salt) and 10 ppm of ZPS (3-(benzothiazolyl-2-mercapto)-propylsulfonic acid sodium salt) were added as additive B, 20 ppm of PEG (polyethylene glycol, molecular weight Mw: 500-4000) was added as additive C, and 3 ppm of JGB (Janus Green B) was added as additive D to the electrolyte.
[0082] (blank paragraph)
[0083] Comparative Example 2
[0084] In an electrolyte solution of Cu 90g / L, sulfuric acid 120g / L, and chloride ion concentration 30ppm, 50-60℃, 50-70A / dm 2 Electrolytic plating was performed at a current density of 10000 ppm (ASD) to produce a 4 μm-thick plating film. The electrolyte contained 3 ppm DET (diethylthiourea) as additive A, 60 ppm SPS (bis-(3-sulfopropyl)-disulfide disodium salt) and 40 ppm ZPS (3-(benzothiazolyl-2-mercapto)-propylsulfonic acid sodium salt) as additive B, and 20 ppm PEG (polyethylene glycol, molecular weight Mw: 500-4000) as additive C, 10 ppm PGL (polyglycerin), 375 ppm Zn, and 75 ppm Fe.
[0085] (blank paragraph)
[0086] Comparative Example 3
[0087] In an electrolyte solution of Cu 100g / L, sulfuric acid 130g / L, and chloride ion concentration 30ppm, 50-60℃, 50-70A / dm 2 Electrolytic plating was performed at a current density of 10000 (ASD) to produce a plating film with a thickness of 6 μm. The electrolyte contained 26 ppm DET (diethylthiourea) as additive A, 80 ppm SPS (bis-(3-sulfopropyl)-disulfide disodium salt) and 40 ppm ZPS (3-(benzothiazolyl-2-mercapto)-propylsulfonic acid sodium salt) as additive B, and 20 ppm PEG (polyethylene glycol, molecular weight Mw: 500-4000) and 10 ppm PGL (polyglycerin) as additive C.
[0088] (blank paragraph)
[0089] Comparative Example 4
[0090] In an electrolyte solution of Cu 80g / L, sulfuric acid 140g / L, and chloride ion concentration 10ppm, at 50-60℃, 50-70A / dm 2Electrolytic plating was performed at a current density of ASD to produce a plating film with a thickness of 12 μm. 5 ppm of MPS (3-mercapto-1-propanesulfonic acid) as additive B and DDAC (diallyldimethylammonium chloride) as additive E were added to the electrolyte.
[0091] (blank paragraph)
[0092] Comparative Example 5
[0093] In an electrolyte solution of Cu 80g / L, sulfuric acid 140g / L, and chloride ion concentration 10ppm, at 50-60℃, 50-70A / dm 2 Electrolytic plating was performed at a current density of ASD to produce a plating film with a thickness of 12 μm. 5 ppm of MPS (3-mercapto-1-propanesulfonic acid) as additive B and DDAC (diallyldimethylammonium chloride) as additive E were added to the electrolyte.
[0094] The plating solution compositions for each example are shown in Table 1 below.
[0095] [Table 1]
[0096] (blank paragraph)
[0097] <Physical property evaluation>
[0098] The physical properties of each surface-treated foil specimen prepared in the Examples and Comparative Examples were measured and are shown in Tables 1 and 2. The physical property evaluation items and measurement methods are as follows.
[0099] (blank paragraph)
[0100] a. Tensile strength / elongation rate
[0101] Tensile test pieces were taken from the electrolytic copper foil with a width of 12.7 mm and a gauge length of 50 mm, and a tensile test was carried out at a crosshead speed of 50.8 mm / min according to the IPC-TM-650 2.4.18B standard, and the maximum load of the measured tensile strength was taken as the tensile strength, and the elongation at break was taken as the elongation. The tensile strength and elongation of each test piece were measured at room temperature, and after heat treatment at a high temperature of 200°C for 1 hour, the tensile strength and elongation were measured, and the results are shown in Table 2 below.
[0102] (blank paragraph)
[0103] b. TOC measurement of electrolytic copper foil
[0104] The TOC content in the electrodeposited copper foil was analyzed by dissolving the electrodeposited copper foil obtained in the examples and comparative examples in 60 ml of hydrochloric acid (35%) and 40 ml of hydrogen peroxide solution (30%) using a Shimadzu TOC-V WP. The results are shown in Table 2 below.
[0105] (blank paragraph)
[0106] c.XRD analysis
[0107] XRD analysis was performed on the M side of the copper foil specimens manufactured in the examples and comparative examples. XRD analysis was performed on the specimens that were not heat-treated (room temperature) and the specimens that were heat-treated at 200°C for 1 hour (high temperature). Figures 1A and 1B show the XRD analysis results for the room temperature and high temperature specimens of Example 1, respectively.
[0108] (blank paragraph)
[0109] From the measured XRD data, Ir(200) / Ir(111), M(200) / M(111), and the rate of change of Ir and M between room temperature and high temperature calculated based on the room temperature value (i.e., (high temperature value - room temperature value) / room temperature value) are shown in Table 3.
[0110] (blank paragraph)
[0111] [Table 2]
[0112] As listed in Table 2, the test pieces of Examples 1 to 5 had a compressive strength of 40 kgf / mm at room temperature. 2 It can be seen that the high strength characteristics are exhibited, and that high strength is maintained even after high-temperature heat treatment at 200° C. Furthermore, as shown in Table 2, Examples 1 to 5 exhibit high values of thickness-to-thickness elongation ratio at room temperature of 1.3 to 1.97% / μm. Furthermore, it can be seen that even in Example 1 with a thickness of 4 μm, the thickness-to-thickness elongation ratio is 1.3% / μm, while the comparative examples exhibit values of 1.2 or less.
[0113] (blank paragraph)
[0114] [Table 3]
[0115] As shown in Table 3, in the examples of the present invention, the I(200) / I(111) ratio at room temperature is 0.4 to 0.5. In addition, in the examples of the present invention, the I(200) / I(111) ratio at high temperatures is reduced compared to the I(200) / I(111) ratio at room temperature. This tendency is also seen in M(200) / M(111). In contrast, in Comparative Examples 1 to 5, the I(200) / I(111) ratio increases at high temperatures. The above-mentioned examples and comparative examples show that the orientation of the crystal planes of electrolytic copper thin films can change depending on the type, content, and / or relative ratio of additives. For example, Comparative Examples 1 to 3, in which 20 ppm or more of additive C is added, show a tendency for the (200) plane to decrease. In addition, Comparative Examples 4 and 5, in which additive C is not present, show that the (200) plane develops.
[0116] (blank paragraph)
[0117] Although the preferred embodiment of the present invention has been described in detail above, those skilled in the art will understand that various modifications can be made to the above-described embodiment without departing from the scope of the present invention. Therefore, the scope of the present invention should not be limited to the described embodiment, but should be determined by the following claims and their equivalents.
[0118] (blank paragraph) [Industrial Applicability]
[0119] The present invention is applicable to electrolytic copper foils.
Claims
1. The thickness-to-thickness elongation ratio at room temperature is 1.3 to 2.0% / μm; The electrolytic copper foil is characterized in that, in an XRD spectrum of a deposit surface at room temperature, the ratio I(200) / I(111), which is the ratio of the diffraction peak intensity I(200) of a (200) crystal plane to the diffraction peak intensity I(111) of a (111) crystal plane, is 0.4 to 0.
5.
2. Tensile strength at room temperature is 40 kgf / mm 2 That's all. The electrolytic copper foil is characterized in that, in an XRD spectrum of a deposit surface at room temperature, the ratio I(200) / I(111), which is the ratio of the diffraction peak intensity I(200) of a (200) crystal plane to the diffraction peak intensity I(111) of a (111) crystal plane, is 0.4 to 0.
5.
3. In the XRD spectrum for the deposition surface at room temperature, the ratio of the diffraction peak intensity I(200) for the (200) crystal plane to the diffraction peak intensity I(111) for the (111) crystal plane, I(200) / I(111), is defined as A; In the XRD spectrum of the precipitate surface after heat treatment at 200° C. for 1 hour, the ratio of the diffraction peak intensity I(200) of the (200) crystal plane to the diffraction peak intensity I(111) of the (111) crystal plane, I(200) / I(111), is defined as B. The electrolytic copper foil according to claim 1 or 2, wherein A>B.
4. The electrolytic copper foil according to claim 3, characterized in that -0.3<(B-A) / A<-0.
1.
5. 3. The electrodeposited copper foil according to claim 1, characterized in that in an XRD spectrum of a deposit surface at room temperature, the ratio of the orientation index M(200) to the (200) crystal plane M(200) / M(111) is 0.5 to 1.
6. In the XRD spectrum for the deposition surface at room temperature, C is defined as M(200) / M(111), which is the ratio of the orientation index M(200) for the (200) crystal plane to the orientation index M(111) for the (111) crystal plane; In the XRD spectrum of the precipitate surface after heat treatment at 200° C. for 1 hour, when the ratio of the orientation index M(200) to the (200) crystal plane and the orientation index M(111) to the (111) crystal plane, M(200) / M(111), is D, The electrolytic copper foil according to claim 5, wherein C>D.
7. The electrolytic copper foil according to claim 6, characterized in that -0.3<(D-C) / C<-0.
1.
8. The electrolytic copper foil according to claim 1 or 2, characterized in that the TOC content is 5 to 8 ppm.
9. The electrolytic copper foil according to claim 1 or 2, characterized in that the elongation rate relative to the thickness after heat treatment at 200° C. for 1 hour is 1.4 to 2.4% / μm.
10. The electrolytic copper foil according to claim 9, wherein the ratio of the thickness-to-thickness elongation rate after heat treatment at 200° C. for 1 hour to the thickness-to-thickness elongation rate at room temperature is 1.05 to 1.25.
Citation Information
Patent Citations
Electrodeposited copper, and electrical component and battery comprising same
CN105705329A
Electrolytic copper foil, electrical parts and batteries containing it
JP2016537514A
Electrolytic copper foil, current collector containing same, negative electrode and lithium battery
JP2017517637A
Electrolytic copper foil of high tensile strength, electrode comprising the same, secondary battery comprising the same, and method of producing the same
JP2019026878A
Electrolytic copper foil for secondary batteries and its manufacturing method
JP2019536209A