Modified composite separator and manufacturing method thereof
Patent Information
- Application Number
- JP2024547814
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-02-11
- Filing Date
- 2022-10-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-10-20
AI Technical Summary
Traditional lithium-ion battery separators made of polyolefin materials face issues with thermal shrinkage at high temperatures, leading to potential short circuits and poor wettability with electrolytes, which affect safety and performance.
A modified composite separator is developed with a coating comprising high-temperature-resistant polymer microspheres, nanofibers, and inorganic particles, forming a network structure that enhances thermal stability and electrolyte retention.
The modified separator improves heat resistance, reduces weight, and increases energy density while maintaining excellent electrolyte absorption and retention, thereby enhancing battery safety and performance.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of battery separators, and in particular to modified composite separators and methods for making the same. [Background technology]
[0002] Lithium-ion batteries are a new type of green secondary battery that was successfully developed and commercialized in 1990. Compared with traditional lead-acid batteries, cadmium-nickel batteries, etc., lithium-ion batteries have the advantages of high energy density, high working voltage, long cycle life, small size, no memory effect, rapid charging and discharging, and environmental protection. Lithium-ion batteries are widely used in 3C products such as mobile phones, laptop computers, and power tools, and have become the main development direction of secondary batteries at the present stage. In recent years, as new energy strategies are implemented around the world, the development of high energy density lithium-ion batteries has progressed rapidly, and the energy density has improved to a level of 300Wh / kg, and its application has rapidly expanded from the traditional small 3C electronic field to large power equipment fields such as new energy electric vehicles, energy storage, large unmanned aerial vehicles, ships, and pure electric aircraft. With the rapid development of 3C products and large power equipment, especially new energy electric vehicles, the requirements for the specific capacity, safety, etc. of lithium-ion batteries are also increasing.
[0003] Lithium-ion batteries are mainly composed of positive / negative electrode materials, electrolyte, and separator. The separator is an important part of the lithium-ion battery, which separates the positive electrode from the negative electrode, prevents the battery from shorting, and allows lithium ions to pass freely. The separator plays an important role in improving the overall performance of the battery, and is known in the battery industry as the "third electrode" of the battery. Although the separator does not participate in the battery reaction, its structure and performance have an important impact on the manufacture, performance, service life, reliability, and safety of the battery. Conventional lithium-ion battery separators generally use polyolefin materials represented by polyethylene and polypropylene, which are manufactured through wet, dry uniaxial stretching, dry biaxial stretching, and other processes, and have good tensile properties, pore size distribution, etc. At present, conventional polyolefin microporous separators are commonly used as separators for lithium-ion batteries due to their excellent chemical stability, thickness, and mechanical strength. However, these separators undergo severe thermal shrinkage at high temperatures. This problem is fatal to the safety of the battery, as it may lead to contact and short circuit of the positive and negative electrodes inside the battery, and eventually to fire or explosion. Also, the polarity of the separator is totally different from that of the electrolyte. Since the separator is a non-polar material and the electrolyte is polar, the separator is difficult to wet with the electrolyte, resulting in poor wettability of the separator. The insufficient wettability and low porosity of the separator greatly hinder the conductivity of lithium ions, and as a result, affect the overall performance of the lithium-ion battery. These problems of polyolefin-based separators have become a significant obstacle in the development of safe and high-power lithium-ion batteries.
[0004] Therefore, the development of new separator materials with high temperature resistance and good wettability is an important problem that the lithium battery industry urgently needs to solve, and has become one of the most important research directions, especially for the development of large-capacity and high-energy density lithium-ion batteries.
[0005] In view of the above situation, the current modification methods mainly include compound modification, composite modification, coating modification, ion modification, and other modification methods. Surface coating is one of the most important and commonly used methods. The surface of polyolefin membrane is usually coated with ceramic coating such as aluminum oxide (Al2O3), silicon dioxide (SiO2), titanium dioxide (TiO2), etc. The coating can significantly improve the wettability of the separator by the electrolyte and the heat resistance of the separator. However, ceramic-coated modified polyolefin separators continue to face some challenges. For example, inorganic ceramics have poor compatibility with the substrate, and the ceramic coating is easy to peel off. In addition, the density of the ceramic layer increases in weight, especially when the base membrane becomes thin or melts, and the insulation of the ceramic becomes poor, resulting in poor dielectric properties. Another problem is that the inorganic coating is a powder-like aggregate structure of particles and cannot form a continuous self-supporting structure by itself. Therefore, inorganic coating usually shows the problem that the powder is easily lost and the coating is easily peeled off during use. More importantly, the inorganic particle layer of the inorganic coated separator at high temperature will generally shatter and break, leading to the destruction of the separator. It cannot suppress the occurrence of thermal runaway and cannot meet the requirements of high heat resistance and high thermal dimensional stability of the separator of lithium ion battery.
[0006] Considering the above problems, there are more and more studies on using high temperature resistant polymers as coating materials, and commonly used polymers include PVDF, PMMA, PEI, etc. For example, patent CN104993089 reports an aramid-coated lithium ion battery separator and its manufacturing method. According to the patent, the aramid solution, emulsifier solution, and binder are uniformly mixed to obtain an aramid slurry, and then the resulting polymer colloid fluid is applied to the surface of the polyolefin separator. The thermal dimensional stability of the separator is improved to a certain extent, and the safety and reliability of the lithium ion battery are improved. However, the organic polymer in this method has insufficient heat resistance and insufficient improvement in thermal dimensional stability.
[0007] Considering the above shortcomings, it is necessary to innovate the existing coatings and develop new coating technologies to solve the problem of crushing and breaking of inorganic particle coatings at high temperatures, thereby improving the heat resistance of the separator, and producing new separator materials with high heat resistance and high thermal dimensional stability, thus meeting the urgent needs of high-energy density lithium-ion batteries for high-temperature resistant separators and high safety. Summary of the Invention
[0008] Contents of the invention The present invention provides a modified composite separator, in which the coated modified composite separator includes a base membrane and a coating, the coating is coated on one or both sides of the base membrane, and the coating includes at least two of the following three components: high temperature resistant polymer microspheres, high temperature resistant polymer nanofibers, and inorganic particles. When the high temperature resistant polymer is incorporated into the coating, the separator exhibits excellent thermal protection effect and high temperature thermal dimensional stability, since the polymer is an organic material and is more closely bonded with the binder, etc., and at the same time, the high temperature resistant polymer has a low density, which can increase the electrolyte retention rate of the separator and improve the cycle performance and heat resistance of the battery.
[0009] The base membrane is a polymer base membrane or a polymer base membrane coated with inorganic particles. The particle size of the high temperature resistant polymer microspheres is 3 to 20000 nm, preferably 5 to 18000 nm, more preferably 8 to 15000 nm; more preferably, the particle size of the high temperature resistant polymer microspheres is 3 to 5000 nm, preferably 5 to 3000 nm, more preferably 8 to 2000 nm. The diameter of the high temperature resistant polymer nanofibers is 5 to 1500 nm, preferably 6 to 1450 nm, more preferably 8 to 1350 nm. The length of the high temperature resistant polymer nanofibers is 0.5 to 1000 μm, preferably 0.6 to 950 μm, more preferably 1.0 to 900 μm. The thickness of the base membrane is 1.5 to 40 μm, preferably 2.0 to 35 μm, more preferably 3.5 to 30 μm. The coating has a thickness of 0.2 to 10 μm, preferably 0.3 to 9 μm, and more preferably 0.5 to 8 μm. The total thickness of the modified composite separator is 2.0 to 45 μm, preferably 2.5 to 40 μm, and most preferably 3 to 36 μm.
[0010] The present invention relates to a method for producing a method for manufacturing a semiconductor device comprising the steps of: (1) The following: High temperature resistant polymer microspheres, High temperature resistant polymer nanofibers, and inorganic particles; formulating a coating slurry comprising at least two of: (2) Coating one or both sides of the base membrane with a coating slurry. Also provided is a method for making a coated modified composite separator, comprising:
[0011] In one aspect, the present invention also provides a coating slurry comprising a slurry solvent and at least two of the following: high temperature resistant polymeric microspheres, high temperature resistant polymeric nanofibers, and inorganic particles, which is used to produce a coated modified composite separator by a coating method.
[0012] In one aspect, the present invention also provides a lithium ion battery, characterized in that the lithium ion battery includes a positive electrode, a negative electrode, an electrolyte, and a coated modified composite separator.
[0013] The coated modified composite separator and method of making the same of the present invention have one, several, or all of the following beneficial effects:
[0014] The present invention provides a modified composite separator coated with a high temperature resistant polymer, in which the coating of the modified composite separator is made of high temperature resistant polymer microspheres, high temperature resistant polymer microspheres and high temperature resistant polymer nanofibers, or high temperature resistant polymer microspheres or high temperature resistant polymer nanofibers and inorganic particles. The high temperature resistant polymer has good adhesion to binders, etc., and therefore provides the separator with good thermal protection effect, which can significantly improve the heat resistance of the separator and the safety of the battery.
[0015] The density of high temperature resistant polymers is much lower than that of inorganic particles, which greatly reduces the weight of the coating and the weight per unit area of the separator, which is beneficial for increasing the energy density of the battery.
[0016] The modified composite separator produced by the present invention has a high electrolyte absorption rate and retention rate because the high temperature resistant polymer and the electrolyte are both organic substances with polar structures, and can improve the rate capability and cycle life of the battery.
[0017] The coating technology provided by the present invention can be applied to any substrate separator to achieve coating formation, and has a wide range of applications. The forming process is simple and can be realized by any one of electrostatic spraying, blade coating, extrusion coating, transfer coating, dip coating, wire rod coating, gravure or microgravure coating, which is easy to implement on an industrial scale and has great industrialization prospects.
[0018] The present invention uses template method, spray drying technique, electrospinning technique, blow spinning technique, or blow assisted electrospinning to produce high temperature resistant polymer with composite morphology of fiber / microsphere. The production process is simple and efficient.
[0019] The incorporation of high temperature resistant polymer nanofibers can form a network structure, enhance the integrity of the coating, and avoid the shattering problem of pure microsphere structures caused by the breakdown of the binder at high temperatures.
[0020] High temperature resistant polymers can enhance the thermal stability of polyolefin separators. Moreover, at high temperatures, polyolefins can be thermally melted, effectively achieving heat sealing / thermal pore closure, greatly improving the safety of the battery.
[0021] When high temperature resistant polymer nanofibers and inorganic particles are mixed to form a coating of modified composite separator, a "reinforced concrete" structure is formed after mixing high temperature resistant polymer nanofibers and ceramics, and the nanofibers form a network so that the whole mixed coating has continuous self-supporting properties, so that the inorganic coating can maintain good integrity without breakage and shattering even when the base membrane is melted at high temperature, and shows excellent thermal protection effect, which can solve the problem of shattering and breakage of pure inorganic particle coating at high temperature, and greatly improve the heat resistance of the separator and the safety of the battery.
[0022] When the modified composite separator has high temperature resistant polymer nanofibers, the high temperature thermal dimensional stability is significantly improved, the incorporation of high temperature resistant polymer nanofibers significantly improves the overall strength of the mixed coating, and at the same time, the weight of the coating and the weight of the separator per unit area are greatly reduced because the density of the high temperature resistant polymer nanofibers is significantly lower than that of the inorganic particles. The modified composite separator has the characteristic of being lightweight, which facilitates the improvement of the energy density of the battery.
[0023] When the modified composite separator has high temperature resistant polymer nanofibers, the separator can have higher electrolyte absorption rate and electrolyte retention rate, and improve the rate capability and cycle life of the battery, because the high temperature resistant polymer nanofibers form a network structure in the mixed coating. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a scanning electron microscope image at 5000x magnification of the polyimide with a composite fiber / microsphere morphology prepared according to Example 1.1. [Diagram 2] FIG. 2 is a scanning electron microscope image at 2000x magnification of the polyolefin composite separator modified by coating with the polyimide prepared in Example 1.1. [Diagram 3] FIG. 3 is a scanning electron microscope image at 5000x magnification of the polyimide having a fiber / microsphere composite morphology prepared according to Example 1.2. [Figure 4] FIG. 4 is a scanning electron microscope image at 2000x magnification of the polyolefin composite separator modified by coating with the polyimide prepared according to Example 1.2. [Diagram 5] FIG. 5 is a scanning electron microscope image at 5000x magnification of the polyimide having a composite fiber / microsphere morphology produced according to Example 1.3. [Figure 6] FIG. 6 is a scanning electron microscope image at 2000x magnification of a polyolefin composite separator modified by coating with a polyimide prepared according to Example 1.3. [Figure 7] FIG. 7 is a comparison photograph of the heat shrinkage at different temperatures of a polyolefin composite separator which is modified by coating with the polyimide prepared according to Example 1.3. [Figure 8] FIG. 8 is a scanning electron microscope image of the 7+4CP+4CP modified composite separator provided in Example 2.1 of the present invention. [Figure 9]FIG. 9 is a scanning electron microscope image of the 7+4C+4C modified composite separator provided in Example 2.1 of the present invention. [Figure 10] FIG. 10 is a scanning electron microscope image of the modified composite separator provided in Example 2.15 of the present invention. [Figure 11] FIG. 11 is a scanning electron microscope image of the modified composite separator provided in Example 3.1 of the present invention. [Figure 12] FIG. 12 is a scanning electron microscope image of the modified composite separator provided in Example 3.2 of the present invention. [Figure 13] FIG. 13 is a scanning electron microscope image of the modified composite separator provided in Example 3.3 of the present invention. [Figure 14] FIG. 14 is a scanning electron microscope image of the modified composite separator provided in Example 3.4 of the present invention. [Figure 15] FIG. 15 is a scanning electron microscope image of the modified composite separator provided in Example 3.5 of the present invention. [Figure 16] FIG. 16 is a scanning electron microscope image of the modified composite separator provided in Example 4.1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Detailed Description Hereinafter, specific embodiments of the present invention will be described in detail. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not intended to limit the present invention.
[0026] 1. The coated modified composite separator includes a base membrane and a coating; The coating covers either one or both sides of the base membrane; Coatings include: b2.1 High temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles A coated modified composite separator comprising at least two of the following:
[0027] 2. The coated modified composite separator of embodiment 1, wherein the high temperature resistant polymer comprises a polyimide.
[0028] 3. The coated modified composite separator according to embodiment 1, characterized in that the particle size of the high temperature resistant polymeric microspheres is 3-20000nm, preferably 5-18000nm, more preferably 8-15000nm; more preferably, the particle size of the high temperature resistant polymeric microspheres is 3-5000nm, preferably 5-3000nm, more preferably 8-2000nm.
[0029] 4. The coated modified composite separator according to embodiment 1, wherein the thickness of the base membrane is 1.5 to 40 μm, preferably 2.0 to 35 μm, more preferably 3.5 to 30 μm.
[0030] 5. The coated modified composite separator according to embodiment 1, characterized in that the total thickness of the modified composite separator is 2.0 to 45 μm, preferably 2.5 to 40 μm, and most preferably 3 to 36 μm.
[0031] 6. The coated modified composite separator according to embodiment 1, characterized in that the coating has a thickness of 0.2-10 μm, preferably 0.3-9 μm, more preferably 0.5-8 μm.
[0032] 7. The coated modified composite separator of embodiment 1 or 2, wherein the base membrane is a polyolefin-based membrane or a polyolefin-based membrane coated with inorganic particles.
[0033] 8. The coated modified composite separator of embodiment 2, wherein the coating comprises polyimide nanofibers / polyimide microspheres.
[0034] 9. The coated modified composite separator according to embodiment 7, wherein the thickness of the polyolefin-based membrane coated with inorganic particles is 3-40 μm.
[0035] 10. The coated modified composite separator according to embodiment 8, wherein the diameter of the polyimide nanofibers in the polyimide coating is 20-1000 nm.
[0036] 11. The coated modified composite separator according to embodiment 1, wherein the coating comprises high temperature resistant polymeric microspheres and inorganic particles, and the weight ratio of the high temperature resistant polymeric microspheres to the inorganic particles is 0.1-100:99.9-0, preferably 0.1-99.9:99.9-0.1.
[0037] 12. The coated modified composite separator according to embodiment 11, wherein the weight ratio of the high temperature resistant polymeric microspheres to the inorganic particles in the coating is 1-100:99-0, preferably 5-100:95-0, most preferably 30-100:70-0, and even more preferably, the weight ratio of the high temperature resistant polymeric microspheres to the inorganic particles in the coating is 1-99.9:99-0.1, preferably 5-99.9:95-0.1, most preferably 30-99.9:70-0.1.
[0038] 13. The base membrane is at least one of a polymer base membrane and a base membrane coated with inorganic particles; Preferably, the coated modified composite separator of embodiment 11, wherein the polymer-based membrane comprises at least one of a polyolefin-based membrane, a cellulose-based membrane, a polyester-based membrane, an aramid-based membrane, a polyimide-based membrane, and an organic-inorganic hybrid-based membrane.
[0039] 14. The coated modified composite separator of embodiment 13, wherein the polymer-based membrane comprises a monolayer membrane, a bilayer membrane, or a multilayer membrane, and the polymer-based membranes contained in each layer are the same or different.
[0040] 15. The coated modified composite separator of any one of embodiments 11-14, wherein the high temperature resistant polymeric microspheres comprise at least one of the following: unmodified high temperature resistant polymeric microspheres, surface-modified high temperature resistant polymeric microspheres, and inorganic hybrid high temperature resistant polymeric microspheres.
[0041] 16. The coated modified composite separator of embodiment 15, wherein the polymer in the unmodified, surface-modified, and inorganic hybrid high temperature resistant polymer microspheres comprises at least one of P84, polyetherimide, polyphosphazene, polyacrylonitrile, polystyrene, polyvinylidene fluoride, polyvinylidene fluoride copolymer, polyvinylidene fluoride-hexafluoropropylene, polymethyl methacrylate, polytetrafluoroethylene, polyimide, polyester, cellulose, polyether ether ketone, polyaryl ether, polyamide, and polybenzimidazole.
[0042] 17. The coated modified composite separator of embodiment 16, wherein the surface-modified high temperature resistant polymeric microspheres comprise at least one of inorganic surface-modified high temperature resistant polymeric microspheres, high temperature resistant polymeric microspheres having polar groups after surface treatment, or high temperature resistant polymeric microspheres surface-coated with a functionalized polymer layer containing polar groups.
[0043] 18. The coated modified composite separator of embodiment 15, wherein the inorganic hybrid high temperature resistant polymer microspheres comprise at least one of polyimide / silica microspheres, polyimide / titanium dioxide microspheres, polyimide / zirconia microspheres, polyimide / zinc oxide microspheres, polyimide / magnesium oxide microspheres, polyimide / magnesium hydroxide microspheres, and polyimide / boehmite microspheres.
[0044] 19. The inorganic particles in the coating include at least one of ceramic, metal oxide, metal hydroxide, metal carbonate, silicate, kaolin, talc, mineral, and glass; preferably at least one of boehmite, alumina, silica, barium titanate, titanium dioxide, zinc oxide, magnesium oxide, magnesium hydroxide, zirconia, or an oxide solid electrolyte; Preferably, the oxide solid electrolyte comprises at least one of a perovskite type, a NASICON type, a LISICON type, a garnet type, and a LiPON type electrolyte; Preferably, the coated modified composite separator according to any one of embodiments 10 to 13, characterized in that the inorganic particles have an average particle size of 3 nm to 5 μm, preferably 7 nm to 4.9 μm, and most preferably 10 nm to 4.5 μm.
[0045] 20. The coating further comprises at least one of a binder, a surfactant, a dispersant, a wetting agent, and an antifoaming agent; 15. The coated modified composite separator of any one of embodiments 11-14, wherein the amount of binder is 0.3-10.5 parts by weight; the amount of surfactant is 0.05-7 parts by weight; the amount of dispersant is 0.05-9 parts by weight; the amount of wetting agent is 0.02-7 parts by weight; and the amount of antifoaming agent is 0.04-4 parts by weight.
[0046] 21. The coated modified composite separator according to embodiment 1, wherein the coating comprises high temperature resistant polymer nanofibers and inorganic particles, and the weight ratio of the high temperature resistant polymer nanofibers to the inorganic particles is (0.4-65):(99.6-35).
[0047] 22. The coated modified composite separator according to embodiment 21, wherein the weight ratio of the high temperature resistant polymer nanofibers to the inorganic particles in the coating is (1-64):(99-36), preferably (3-62):(97-38), and most preferably (5-59):(95-41).
[0048] 23. The base membrane is at least one of a polymer base membrane and a base membrane coated with inorganic particles; 23. The coated modified composite separator of any one of embodiments 21-22, wherein the polymer-based membrane comprises at least one of a polyolefin-based membrane, a cellulose-based membrane, a polyester-based membrane, and an aramid-based membrane.
[0049] 24. The coated modified composite separator of any one of embodiments 21-23, wherein the polymer-based membrane comprises a monolayer membrane, a bilayer membrane, or a multilayer membrane, and the polymer-based membranes contained in each layer are the same or different.
[0050] 25. The coated modified composite separator of any one of embodiments 21-24, wherein the high temperature resistant polymer nanofibers comprise at least one of the following: unmodified high temperature resistant polymer nanofibers, surface modified high temperature resistant polymer nanofibers, and inorganic hybrid high temperature resistant polymer nanofibers.
[0051] 26. The diameter of the high temperature resistant polymer nanofiber is 5 to 1500 nm, preferably 6 to 1450 nm, more preferably 8 to 1350 nm; and / or 26. The coated modified composite separator according to any one of embodiments 21 to 25, wherein the high temperature resistant polymer nanofibers have a length of 0.5 to 1000 μm, preferably 0.6 to 950 μm, more preferably 1.0 to 900 μm.
[0052] 27. The coated modified composite separator according to any one of embodiments 21 to 26, wherein the unmodified high temperature resistant polymer nanofibers and the high temperature resistant polymer nanofibers used for surface modification and inorganic hybridization comprise at least one of P84 nanofibers, polyetherimide nanofibers, polyvinylidene fluoride and its copolymer nanofibers, polyvinylidene fluoride-hexafluoropropylene nanofibers, polytetrafluoroethylene nanofibers, polyphosphazene nanofibers, polyacrylonitrile nanofibers, polyimide nanofibers, polyester nanofibers, cellulose nanofibers, polyetheretherketone nanofibers, polyarylether nanofibers, polyamide nanofibers, and polybenzimidazole nanofibers.
[0053] 28. The coated modified composite separator of any one of embodiments 21-27, wherein the surface-modified high temperature resistant polymer nanofibers comprise at least one of inorganic surface-modified high temperature resistant polymer nanofibers, high temperature resistant polymer nanofibers having polar groups after surface treatment, or high temperature resistant polymer nanofibers surface-coated with a functionalized polymer layer containing polar groups.
[0054] 29. The inorganic particles in the coating include at least one of ceramic, metal oxide, metal hydroxide, metal carbonate, silicate, kaolin, talc, mineral, and glass; preferably at least one of boehmite, alumina, silica, barium titanate, titanium dioxide, zinc oxide, magnesium oxide, magnesium hydroxide, zirconia, or an oxide solid electrolyte; Preferably, the oxide solid electrolyte comprises at least one of a perovskite type, a NASICON type, a LISICON type, a garnet type, and a LiPON type electrolyte; Preferably, the coated modified composite separator according to any one of embodiments 21 to 28, characterized in that the inorganic particles have an average particle size of 10 nm to 5 μm, preferably 11 nm to 4.9 μm, most preferably 15 nm to 4.5 μm.
[0055] 30. The coated modified composite separator of any one of embodiments 21-29, wherein the coating further comprises at least one of a binder, a surfactant, a dispersant, a wetting agent, and an antifoaming agent.
[0056] 31. The amount of binder is 0.5 to 12.5 parts by weight, preferably 0.6 to 12 parts by weight, more preferably 1.0 to 9 parts by weight; and / or the amount of the surfactant is 0.1 to 5 parts by weight, preferably 0.2 to 4.9 parts by weight, more preferably 0.4 to 4.7 parts by weight; and / or the amount of dispersant is 0.1 to 7 parts by weight, preferably 0.2 to 6.9 parts by weight, more preferably 0.4 to 6.4 parts by weight; and / or the amount of wetting agent is 0.05 to 5 parts by weight, preferably 0.06 to 4.9 parts by weight, more preferably 0.09 to 4.7 parts by weight; and / or 31. The coated modified composite separator according to any one of embodiments 21 to 30, wherein the amount of antifoaming agent is 0.1 to 4 parts by weight, preferably 0.2 to 3.9 parts by weight, more preferably 0.4 to 3.5 parts by weight.
[0057] 32. The process of: (1) The following: b2.1 High temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles formulating a coating slurry comprising at least two of: (2) Coating one or both sides of the base membrane with a coating slurry. 31. A method for producing a coated modified composite separator according to any one of embodiments 21 to 30, comprising:
[0058] 33. The method of manufacturing of embodiment 32, wherein the coating slurry comprises high temperature resistant polymeric microspheres and high temperature resistant polymeric nanofibers, the high temperature resistant polymer being a polyimide, the method comprising the steps of: A: Producing a polyamic acid solution with an intrinsic viscosity controlled at 0.01-1 dl / g by low-temperature condensation polymerization using dianhydride and diamine as monomers in an aprotic polar solvent; and, if necessary, adjusting the spinning parameters to produce a polyamic acid material with a composite morphology of nanofibers / microspheres by using a template method, a spray-drying technique, an electrospinning technique, a blow-spinning technique, or a blow-assisted electrospinning; B: subjecting the polyamic acid material produced in step A to high-temperature heat treatment to thermally imidize the polyamic acid material into a polyimide material; C: Formulating a coating slurry: dispersing the polyimide material prepared in step B in a dispersion, for example, dispersing it in the dispersion by ultrasonic waves, and stirring uniformly, for example, in a homogenizer; adding a binder such as a polymer binder to the polyimide dispersion, and stirring uniformly, for example, in a homogenizer at a stirring speed of 500 to 30,000 rpm; D: uniformly applying the coating slurry obtained in step C onto the surface of the base membrane; E: Drying the composite separator obtained by the treatment of step D, wherein the drying temperature is 50 to 100°C and the drying time is 0.1 minutes to 12 hours or 2 minutes to 12 hours. A manufacturing method comprising:
[0059] 34. For the polyamic acid solution used in step A, the dianhydride may be pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (α-BPDA), 4,4'-diphenylether dianhydride (ODPA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), hexafluorodianhydride (6F DA), bisphenol A diether dianhydride (BPADA), 3,3,4,4-diphenylsulfonetetracarboxylic dianhydride (DSDA), or a mixture of two or more thereof, and the diamine is 4,4'-diaminodiphenyl ether (ODA), p-phenylenediamine (p-PDA), 3,4'-diaminodiphenylmethane (3,4'-MDA), 4,4'-diaminodiphenylmethane (4,4'-MDA), 2, 34. The method according to embodiment 33, characterized in that the polyamic acid is one of 2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB), 1,3-bis(4-aminophenoxy)benzene (1,3,4-APB), 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether (6FODA), 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), or a mixture of two or more thereof; or is prepared by blending at least two polyamic acid solutions; the solid content of the polyamic acid solution is 5-40 wt%; and the electrospinning parameters are as follows: spinning voltage 15-100 kV, preferably 16-80 kV, more preferably 17-75 kV, or 15-55 kV, and receiving distance 10-30 cm.
[0060] 35. The method according to embodiment 33, wherein the thermal imidization process used in step B has a maximum temperature of 250-450°C, preferably 300-450°C, and a residence time of 0.1-30 minutes or 1-30 minutes.
[0061] 36. The manufacturing method of embodiment 33, wherein the binder in step C is one or more of an aqueous PVDF emulsion, polyvinyl alcohol, polyethylene oxide, an acrylic water-soluble adhesive, styrene-butadiene rubber, sodium carboxymethylcellulose, and polyvinylpyrrolidone; the weight parts of each component of the coating slurry are as follows: 1-3 parts binder, 89-52 parts solvent, and 10-45 parts polyimide; and the dispersion is water.
[0062] 37. The method of claim 33, wherein in step D, the polyolefin separator is coated on one or both sides with polyimide, and the coating method is one of electrostatic spraying, blade coating, extrusion coating, transfer coating, wire rod coating, dip coating, gravure or microgravure coating.
[0063] 38. The method of claim 32, wherein the coating slurry comprises high temperature resistant polymeric microspheres, or high temperature resistant polymeric microspheres and inorganic particles, the method comprising the steps of: (1) formulating a mixed coating slurry containing high temperature resistant polymeric microspheres or high temperature resistant polymeric microspheres and inorganic particles; (2) Coating one or both sides of the base membrane with a coating slurry. A manufacturing method comprising the steps of:
[0064] 39. The solid content of the coating slurry is 2-71.4 wt%, preferably 4-70 wt%, more preferably 10-62 wt%; The method according to embodiment 38, wherein the viscosity of the coating slurry is 20 to 7000 cP, preferably 100 to 6000 cP, and more preferably 150 to 5500 cP.
[0065] 40. The slurry solvent is one of an aqueous solvent or an organic solvent; Preferably, the aqueous solvent comprises pure water or a mixed solution of water and at least one of ethanol, ethylene glycol, glycerol, isopropyl alcohol, propylene glycol, butanol, and acetic acid; Preferably, the method according to any one of embodiments 38 to 39, wherein the organic solvent comprises at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethylsulfoxide, acetone, ethanol, isopropanol, ethylene carbonate, and dimethyl carbonate.
[0066] 41. The method of any one of embodiments 38-39, wherein the coating method of the coating comprises at least one of electrostatic spraying, blade coating, rotary spraying, extrusion coating, transfer coating, dip coating, wire rod coating, gravure or microgravure coating.
[0067] 42. The manufacturing method of embodiment 32, wherein the coating slurry comprises high temperature resistant polymer nanofibers and inorganic particles, and the method comprises the following steps: (1) formulating a coating slurry containing high temperature resistant polymer nanofibers and inorganic particles; (2) Coating one or both sides of the base membrane with a coating slurry. A manufacturing method comprising the steps of:
[0068] 43. The method of manufacturing according to embodiment 42, wherein the coating slurry comprises the following components by weight: 0.4 to 65 parts of high temperature resistant polymer nanofibers, 35 to 99.6 parts of inorganic particles, and 100 to 5000 parts of slurry solvent; the sum of the parts by weight of the high temperature resistant polymer nanofibers and inorganic particles is 100.
[0069] 44. The solid content of the coating slurry is 2 to 50 wt%, preferably 6 to 48 wt%, more preferably 10 to 43 wt%; and / or The method according to any one of embodiments 42 to 43, wherein the viscosity of the coating slurry is 50 to 4000 cP, preferably 100 to 3500 cP, more preferably 200 to 3000 cP.
[0070] 45. The slurry solvent is one of an aqueous solvent or an organic solvent; Preferably, the aqueous solvent comprises pure water or a mixed solution of water and at least one of ethanol, ethylene glycol, glycerol, isopropyl alcohol, and butanol; The method according to any one of embodiments 42 to 44, wherein the organic solvent comprises at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethylsulfoxide, acetone, ethanol, isopropanol, ethylene carbonate, and dimethyl carbonate.
[0071] 46. The method according to any one of embodiments 42-43, wherein the coating slurry further comprises an additive selected from at least one of a binder, a surfactant, a dispersant, a wetting agent, an antifoaming agent, and the like.
[0072] 47. The amount of the slurry solvent is 100 to 5000 parts by weight, preferably 120 to 4000 parts by weight, and most preferably 150 to 2900 parts by weight; and / or the amount of binder is 0.5 to 12.5 parts by weight, preferably 0.6 to 12 parts by weight, more preferably 1.0 to 9 parts by weight; and / or the amount of the surfactant is 0.1 to 5 parts by weight, preferably 0.2 to 4.9 parts by weight, more preferably 0.4 to 4.7 parts by weight; and / or the amount of dispersant is 0.1 to 7 parts by weight, preferably 0.2 to 6.9 parts by weight, more preferably 0.4 to 6.4 parts by weight; and / or the amount of wetting agent is 0.05 to 5 parts by weight, preferably 0.06 to 4.9 parts by weight, more preferably 0.09 to 4.7 parts by weight; and / or The method according to any one of embodiments 42 to 44, wherein the amount of the antifoaming agent is from 0.1 to 4 parts by weight, preferably from 0.2 to 3.9 parts by weight, and more preferably from 0.4 to 3.5 parts by weight.
[0073] 48. The method of any one of embodiments 42-45, wherein the coating method of the coating comprises at least one of electrostatic spraying, blade coating, rotary spraying, extrusion coating, transfer coating, dip coating, wire rod coating, gravure or microgravure coating.
[0074] 49. A slurry solvent and: b2.1 High temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles and a coating slurry comprising at least two of:
[0075] 50. The coating slurry according to embodiment 49, wherein the coating slurry comprises high-temperature resistant polymer nanofibers, inorganic particles, and a slurry solvent, the high-temperature resistant polymer nanofibers are 0.4 to 65 parts by weight, the inorganic particles are 35 to 99.6 parts by weight, and the sum of the parts by weight of the high-temperature resistant polymer nanofibers and the inorganic particles is 100.
[0076] 51. The solid content of the coating slurry is 2 to 50 wt%, preferably 6 to 48 wt%, more preferably 10 to 43 wt%; and / or The coating slurry according to any one of embodiments 49 to 50, wherein the viscosity of the coating slurry is 50 to 4000 cP, preferably 100 to 3500 cP, more preferably 200 to 3000 cP.
[0077] 52. The slurry solvent is one of an aqueous solvent or an organic solvent; Preferably, the aqueous solvent comprises pure water or a mixed solution of water and at least one of ethanol, ethylene glycol, glycerol, isopropyl alcohol, and butanol; Preferably, the coating slurry according to any one of embodiments 49 to 50, wherein the organic solvent comprises at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethylsulfoxide, acetone, ethanol, isopropanol, ethylene carbonate, and dimethyl carbonate.
[0078] 53. The coating slurry according to any one of embodiments 49 to 51, wherein the coating slurry further comprises an additive selected from at least one of a binder, a surfactant, a dispersant, a wetting agent, an antifoaming agent, and the like.
[0079] 54. The amount of the slurry solvent is 100 to 5000 parts by weight, preferably 120 to 4000 parts by weight, and most preferably 150 to 2900 parts by weight; and / or the amount of binder is 0.5 to 12.5 parts by weight, preferably 0.6 to 12 parts by weight, more preferably 1.0 to 9 parts by weight; and / or the amount of the surfactant is 0.1 to 5 parts by weight, preferably 0.2 to 4.9 parts by weight, more preferably 0.4 to 4.7 parts by weight; and / or the amount of dispersant is 0.1 to 7 parts by weight, preferably 0.2 to 6.9 parts by weight, more preferably 0.4 to 6.4 parts by weight; and / or the amount of wetting agent is 0.05 to 5 parts by weight, preferably 0.06 to 4.9 parts by weight, more preferably 0.09 to 4.7 parts by weight; and / or 52. The coating slurry according to any one of embodiments 49 to 51, wherein the amount of the antifoaming agent is 0.1 to 4 parts by weight, preferably 0.2 to 3.9 parts by weight, more preferably 0.4 to 3.5 parts by weight.
[0080] 55. A lithium ion battery comprising a positive electrode, a negative electrode, an electrolyte, and a separator, wherein the separator is a coated modified composite separator according to any one of embodiments 1 to 31, or a coated modified composite separator produced by the method according to any one of embodiments 32 to 48.
[0081] 56. A coated modified composite separator comprising a base membrane and a coating; The coating covers either one or both sides of the base membrane; The coating comprises high temperature resistant polymer nanofibers and: b2.1 High temperature resistant polymer microspheres, and b2.3 Inorganic particles and at least one of the above.
[0082] 57. The following process: (1) High-temperature resistant polymer nanofibers: b2.1 High temperature resistant polymer microspheres, and b2.3 Inorganic particles; and formulating a coating slurry comprising at least one of: (2) Coating one or both sides of the base membrane with a coating slurry. 57. A method for producing the coated modified composite separator of embodiment 56, comprising:
[0083] 58. A slurry solvent and high temperature resistant polymer nanofibers: b2.1 High temperature resistant polymer microspheres, and b2.3 Inorganic particles and a coating slurry comprising at least one of:
[0084] 59. A coated modified composite separator comprising a base membrane and a coating; The coating covers either one or both sides of the base membrane; The coating, b2.1 High temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles 1. A coated modified composite separator comprising:
[0085] 60. The following process: (1)b2.1 High temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles formulating a coating slurry containing; (2) Coating one or both sides of the base membrane with a coating slurry. 60. A method for producing the coated modified composite separator of embodiment 59, comprising:
[0086] 61. Slurry solvent, as well as: b2.1 High temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles 1. A coating slurry comprising:
[0087] General Explanations and Definitions of Terms The range endpoints and any values disclosed herein are not intended to be limited to the exact ranges or values, but should be understood to include values close to such ranges or values. For numerical ranges, the endpoints of each range, and the individual values and individual point values can be combined with each other to obtain one or more new numerical ranges, which numerical ranges are to be considered specifically disclosed herein.
[0088] The foregoing description of the embodiments has been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the present disclosure. Individual elements or features of a particular embodiment are generally not limited to that particular embodiment, but where applicable, even if not explicitly shown or described, they can be interchanged and used in other selected embodiments. It can also be modified in many respects. Such modifications should not be considered as departures from the present disclosure, and all such modifications are intended to be included within the scope of the present application.
[0089] A. Base membrane The type of base membrane in the present application is not particularly limited, and it can be any kind of base membrane; the base membrane is a polymer base membrane or a base membrane coated with inorganic particles, such as a ceramic base membrane, and the ceramic base membrane is the same as the conventional ceramic base membrane in this field, and includes both a polymer base membrane and a ceramic layer coated on at least one side of the polymer base membrane. In some embodiments, the thickness of the base membrane is 1.5 to 40 μm; preferably 2.0 to 35 μm, more preferably 3.5 to 30 μm. The thickness of the base membrane is preferably 2 μm or more, 3 μm or more, 4 μm or more, 5 μm or more, 7 μm or more, 9 μm or more, or 12 μm or more, and the thickness of the base membrane is preferably 37 μm or less, 35 μm or less, 33 μm or less, 30 μm or less, 28 μm or less, or 26 μm or less.
[0090] The polymer base film may include, but is not limited to, at least one of, for example, polyolefin base film, cellulose base film, polyester base film, aramid base film, polyimide base film, and organic-inorganic hybrid base film. In some embodiments, the polymer base film includes a single layer film, a bilayer film, or a multilayer film, and the polymer base film included in each layer may be the same or different. In some embodiments, for a bilayer polymer base film or a multilayer polymer base film, the thickness of each layer may be the same or different from that of the other layers. In some embodiments, for a bilayer polymer base film or a multilayer polymer base film, each layer may be manufactured using the same or different processes, such as coextrusion and / or lamination together. In some embodiments, the polymer base film includes a polyolefin base film, and the polyolefin may include, but is not limited to, polyethylene, polypropylene, polybutylene, copolymers of the above polyolefins, and blends thereof.
[0091] In some embodiments, the polyolefin may be an ultra-low molecular weight, low molecular weight, medium molecular weight, high molecular weight, or ultra-high molecular weight polyolefin. For example, the ultra-high molecular weight polyolefin may have a molecular weight of 450,000 (450k) or more, such as 500k or more, 600k or more, 700k or more, 800k or more, 1 million or more, 2 million or more, 3 million or more, etc. The high molecular weight polyolefin may have a molecular weight in the range of 250k to 450k, such as 250k to 400k, 250k to 350k, or 250k to 300k. The medium molecular weight polyolefin may have a molecular weight of 150k to 250k, such as 150k to 225k, 150k to 200k, 150k to 200, etc. The low molecular weight polyolefin may have a molecular weight in the range of 100k to 150k, such as 100k to 125k. The ultra-low molecular weight polyolefin may have a molecular weight of less than 100k. The above numbers are weight average molecular weights. The polyolefin separator may have the following non-limiting structures: PP, PE, PP / PP, PP / PE, PE / PP, PE / PE, PE / PP / PE, etc.
[0092] According to the present invention, in the inorganic particle coated base film, there is no special requirement for inorganic particle coating such as ceramic layer, and ceramic layer generally used in this field can be selected.The ceramic particles in the ceramic layer can include, but are not limited to, at least one of Al2O3 (including α, β, γ type), SiO2, BaSO4, BaO, titanium dioxide (TiO2, rutile or anatase), CuO, MgO, Mg(OH)2, LiAlO2, ZrO2, carbon nanotube (CNT), BN, SiC, Si3N4, WC, BC, AlN, Fe2O3, BaTiO3, MoS2, V2O5, PbTiO3, TiB2, CaSiO3, molecular sieve (ZSM-5), clay, boehmite, and kaolin, preferably at least one of Al2O3, SiO2, and BaSO4.
[0093] The separator disclosed in the present invention may further contain fillers, elastomers, wetting agents, lubricants, flame retardants, nucleating agents, antioxidants, colorants, and / or other additional components not inconsistent with the objectives of the present invention. For example, the substrate may contain fillers such as calcium carbonate, zinc oxide, diatomaceous earth, talc, kaolin, synthetic silica, mica, clay, boron nitride, silicon dioxide, titanium dioxide, barium sulfate, aluminum hydroxide, magnesium hydroxide, or combinations thereof. Elastomers may include ethylene-propylene (EPR), ethylene-propylene-diene (EPDM), styrene-butadiene (SBR), styrene isoprene (SIR), ethylidene norbornene (ENB), epoxy resins, and polyurethanes, or combinations thereof. Wetting agents may include ethoxylated alcohols, primary polymeric carboxylic acids, glycols (e.g., polypropylene glycol and polyethylene glycol), functionalized polyolefins, and the like. The lubricants may include silicones, fluoropolymers, oleamide, stearamide, erucamide, calcium stearate, lithium stearate, or other metal stearates.The flame retardants may include brominated flame retardants, ammonium phosphate, magnesium hydroxide, aluminum oxide trihydrate, and phosphate esters.The nucleating agents may include any nucleating agent not inconsistent with the objectives of the present invention.
[0094] B. Coatings and Coating Slurries The coating of the present invention comprises at least two of the following: high temperature resistant polymeric microspheres, high temperature resistant polymeric nanofibers, and inorganic particles.
[0095] In some embodiments, the coating thickness is 0.2 to 10 μm, and the coating thickness is preferably 0.3 μm or more, 0.4 μm or more, 0.5 μm or more, 0.7 μm or more, 1 μm or more, or 1.2 μm or more, and the coating layer thickness is preferably 9 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, or 5 μm or less. If the coating thickness is less than 0.2 μm, the thermal dimensional stability, electrolyte retention and capacity retention of the modified separator will decrease; if the coating thickness is more than 10 μm, the difficulty of coating will increase and at the same time the electrolyte retention of the electrolyte will increase, resulting in a decrease in the energy density of the battery.
[0096] In some embodiments, the coating and / or coating slurry comprises high temperature resistant polymer nanofibers and inorganic particles. The coating comprises, by weight, 0.4-65 parts high temperature resistant polymer nanofibers, 35-99.6 parts inorganic particles, and the sum of the parts by weight of the high temperature resistant polymer nanofibers and inorganic particles is 100. In some embodiments, the parts by weight of the high temperature resistant polymer nanofibers in the coating are preferably 1-64, 2-63, 3-62, 4-61, 5-59, or 7-58. In some embodiments, the parts by weight of the inorganic particles in the coating are preferably 36-99, 37-98, 38-97, 39-96, 41-95, or 42-93.
[0097] In some embodiments, the coating and / or coating slurry comprises high temperature resistant polymeric microspheres and inorganic particles. The coating comprises, in parts by weight, 0.1-100 parts high temperature resistant polymeric microspheres, 99.9-0 parts inorganic particles, preferably 0.1-99.9 parts high temperature resistant polymeric microspheres, and 99.9-0.1 parts inorganic particles, and the sum of the parts by weight of the high temperature resistant polymeric microspheres and inorganic particles is 100. In some embodiments, the parts by weight of the high temperature resistant microspheres in the coating are preferably 0.3-100, 1-100, 3-100, 5-100, 7-100, or 10-100. In some embodiments, the parts by weight of the inorganic particles in the coating are preferably 99.7-0, 99-0, 97-0, 95-0, 93-0, or 90-0.
[0098] In some embodiments, the coating and / or coating slurry comprises high temperature resistant polymeric microspheres, or high temperature resistant polymeric microspheres and high temperature resistant polymeric nanofibers.
[0099] In some embodiments, the coating and / or coating slurry comprises high temperature resistant polymer nanofibers and at least one of high temperature resistant polymer microspheres and inorganic particles. In some embodiments, the coating and / or coating slurry comprises high temperature resistant polymer microspheres, high temperature resistant polymer nanofibers, and inorganic particles. The incorporation of high temperature resistant polymer nanofibers can form a network structure and enhance the integrity of the coating, avoiding the problem of crushing of single components of the microsphere structure caused by the breakdown of the binder at high temperatures.
[0100] In some embodiments, the coating slurry comprises high temperature resistant polymeric microspheres and high temperature resistant polymeric nanofibers, in which the high temperature resistant polymer in the high temperature resistant polymeric microspheres and high temperature resistant polymeric nanofibers is polyimide. In the above embodiments, the method for producing a polyolefin composite separator modified by coating with polyimide includes: A: Producing a polyamic acid solution with an intrinsic viscosity controlled at 0.01-1 dl / g by low-temperature condensation polymerization using dianhydride and diamine as monomers in an aprotic polar solvent; then, adjusting spinning parameters as necessary, producing a polyamic acid material with a composite morphology of nanofibers / microspheres by using template method, spray drying technique, electrospinning technique, blow spinning technique, or blow-assisted electrospinning; B: subjecting the polyamic acid material produced in step A to high-temperature heat treatment to thermally imidize the polyamic acid material into a polyimide material; C: Formulating the coating slurry: dispersing the polyimide material prepared in step B in the dispersion and stirring uniformly; adding the binder to the polyimide dispersion and stirring uniformly at a stirring speed of 500-30000 rpm; D: uniformly applying the coating slurry obtained in step C onto the surface of the base membrane; E: Drying the composite separator obtained by the treatment of step D, wherein the drying temperature is 50 to 100°C and the drying time is 0.1 minutes to 12 hours or 2 minutes to 12 hours. The process includes the steps of:
[0101] For the polyamic acid solution used in step A, the dianhydride is one or a mixture of two or more of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (α-BPDA), 4,4'-diphenylether dianhydride (ODPA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), hexafluorodianhydride (6FDA), bisphenol A diether dianhydride (BPADA), 3,3,4,4-diphenylsulfonetetracarboxylic dianhydride (DSDA); and the diamine is one or a mixture of two or more of 4,4'-diaminodiphenylether (ODA), p-phenylenediamine (p-PDA), 3,4'-diaminodiphenylmethane (3,4'-MDA), 4,4'-diaminodiphenylmethane (4, 4'-MDA), 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB), 1,3-bis(4-aminophenoxy)benzene (1,3,4-APB), 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether (6FODA), 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), or a mixture of two or more thereof; or is prepared by blending at least two polyamic acid solutions; the solid content of the polyamic acid solution is 5-40 wt%; and the electrospinning parameters are as follows: spinning voltage 15-100 kV, preferably 16-80 kV, more preferably 17-75 kV, or 15-55 kV, and receiving distance 10-30 cm.
[0102] The thermal imidization process used in step B has a maximum temperature of 250-450° C., preferably 300-450° C., and a residence time of 0.1-30 minutes or 1-30 minutes.
[0103] The binder in step C is one or more of aqueous PVDF emulsion, polyvinyl alcohol, polyethylene oxide, acrylic water-soluble adhesive, styrene-butadiene rubber, sodium carboxymethyl cellulose, and polyvinylpyrrolidone; the parts by weight of each component in the coating slurry are as follows: 1-3 parts binder, 89-52 parts solvent, and 10-45 parts polyimide; the dispersion is water.
[0104] In step D, the polyolefin separator is coated on one or both sides with the polyimide, and the coating method is one of electrostatic spray, blade coating, extrusion coating, transfer coating, wire rod coating, dip coating, gravure or microgravure coating.
[0105] In some embodiments, the coating and / or coating slurry further comprises an additive selected from at least one of a binder, a surfactant, a dispersant, a wetting agent, an antifoaming agent, and the like.
[0106] The binder includes, but is not limited to, at least one of polyvinylidene fluoride and its copolymers, polyvinyl alcohol, polyacrylate, styrene-butadiene rubber, carboxymethyl cellulose and its salts, polyvinylpyrrolidone, and polyimide. The amount of the binder is 0.5 to 12.5 parts by weight. In some embodiments, the amount of the binder is preferably 0.6 to 12, 0.7 to 11, 0.8 to 10, or 1.0 to 9 parts by weight.
[0107] The surfactant may be at least one of fluorocarbon surfactants, nonionic surfactants, cationic surfactants, and anionic surfactants, preferably perfluoroalkyl ether alcohol amine salts, perfluoroalkyl ether quaternary ammonium salts, perfluoroalkyl ether potassium carboxylate fluorocarbon surfactants, as well as polyethylene glycol type, polyol type, block copolyether, and special polyether nonionic surfactants, but is not limited thereto. The amount of surfactant is 0.1 to 5 parts by weight. In some embodiments, the surfactant is preferably used in an amount of 0.2 to 4.9, 0.3 to 4.8, 0.4 to 4.7, or 0.6 to 4.5 parts by weight.
[0108] Dispersants include, but are not limited to, at least one of tris(2-ethylhexyl)phosphate, sodium lauryl sulfate, methylpentanol, cellulose derivatives, polyacrylamides, guar gum, fatty acid polyethylene glycol esters, and cellulose ethers, preferably hydroxypropylmethylcellulose or polyacrylamide. The amount of dispersant is 0.1 to 7 parts by weight. In some embodiments, the dispersant is preferably used in an amount of 0.2 to 6.9, 0.3 to 6.8, 0.4 to 6.4, or 0.6 to 6.0 parts by weight.
[0109] The humectant includes, but is not limited to, at least one of monohydric alcohol, dihydric alcohol, and trihydric alcohol; preferably at least one of ethanol, ethylene glycol, glycerol, isopropyl alcohol, and butanol. The amount of the humectant is 0.05 to 5 parts by weight. In some embodiments, the amount of the humectant is preferably 0.06 to 4.9, 0.07 to 4.8, 0.09 to 4.7, or 0.11 to 4.3 parts by weight.
[0110] The antifoaming agent includes, but is not limited to, at least one of alcohol, fatty acid and fatty acid ester, amide, phosphate ester, silicone, polyether, and polyether-modified polysiloxane antifoaming agent; preferably at least one of monoalkyl, dialkyl phosphate, and fluorinated alkyl phosphate, and polyether-modified silicone antifoaming agent. The amount of the antifoaming agent is 0.1 to 4 parts by weight. In some embodiments, the amount of the antifoaming agent is preferably 0.2 to 3.9, 0.3 to 3.7, 0.4 to 3.5, or 0.6 to 3.3 parts by weight.
[0111] The coating method of the coating is not particularly limited, and includes at least one of electrostatic spraying, blade coating, rotary spraying, extrusion coating, transfer coating, dip coating, wire rod coating, gravure or microgravure coating; preferably, extrusion coating, gravure coating, or microgravure coating, but is not limited thereto.
[0112] In some embodiments, the base film coated with the coating slurry is dried. The drying temperature is 40 to 210° C., preferably 50 to 200° C.; and the drying time is 0.1 to 60 minutes, or 1 to 60 minutes, or 5 to 50 minutes. The drying method is preferably oven drying.
[0113] b.1 High temperature resistant polymer microspheres The high temperature resistant polymeric microspheres include unmodified high temperature resistant polymeric microspheres, surface modified high temperature resistant polymeric microspheres, and / or inorganic hybrid high temperature resistant polymeric microspheres.
[0114] The particle size of the high temperature resistant polymeric microspheres is 3 to 20,000 nm, preferably 5 nm or more, 7 nm or more, 9 nm or more, 12 nm or more, 15 nm or more, 20 nm or more, and preferably 50 nm or less, 11,000 nm or less, 13,000 nm or less, 15,000 nm or less, or 18,000 nm or less.
[0115] The method for producing high-temperature resistant polymeric microspheres is not particularly limited, and includes at least one of the following: electrostatic spraying, phase separation, template, precipitation, blowing, blow-assisted electrospinning, centrifugal, self-assembly, solution spinning, in-situ synthesis, and reprecipitation. In some embodiments, the electrostatic spraying method is used to produce high-temperature resistant polymeric microspheres. The concentration of the spinning polymer in the polymer solution used for electrostatic spraying is 3-30 wt%, more preferably 8-20 wt%. When the relative molecular weight of the polymer is fixed and other conditions are constant, the concentration of the spinning solution is a decisive factor that affects the entanglement of molecular chains in the solution.
[0116] The polymer in the unmodified, surface-modified, and inorganic hybrid high temperature resistant polymeric microspheres includes, but is not limited to, at least one of P84, polyetherimide, polyphosphazene, polyacrylonitrile, polystyrene, polyvinylidene fluoride, polyvinylidene fluoride copolymers, polyvinylidene fluoride-hexafluoropropylene, polymethyl methacrylate, polytetrafluoroethylene, polyimide, polyester, cellulose, polyether ether ketone, polyaryl ether, polyamide, and polybenzimidazole.
[0117] Polyimide microspheres are preferred. The polyimide in the polyimide microspheres is produced by homopolycondensation and copolycondensation of a raw material mixture containing a polybasic acid anhydride and a polyamine.
[0118] The surface-modified high-temperature-resistant polymeric microspheres include, but are not limited to, inorganic surface-modified high-temperature-resistant polymeric microspheres, high-temperature-resistant polymeric microspheres with polar groups after surface treatment, or high-temperature-resistant polymeric microspheres surface-coated with a functionalized organic layer containing polar groups. The polar groups include, but are not limited to, at least one of hydroxyl, carboxyl, sulfonic acid group, amino, phosphate ester group, halogen, and nitro. The functionalized organics containing polar groups include, but are not limited to, polymers such as at least one of polyphosphazene, polyacrylonitrile, polyphosphoric acid, polysiloxane, polyester polymer, polyetherimide, polyetheretherketone, polyarylether, and polybenzimidazole, as well as aromatic sulfonic acid derivatives such as 8-aminopyrene-1,3,6-trisulfonic acid and its salts. It should be noted that the above surface modification is not grafted onto the original particles to produce a core-shell structure. Compared with the core-shell structure particles, which are difficult and costly to produce, the surface modification of the present invention is simple to produce, has fewer components, and has a low process cost.
[0119] The inorganic hybrid high temperature resistant polymeric microspheres contain an inorganic material. The inorganic material used for surface modification and for the inorganic hybrid high temperature resistant polymeric microspheres includes, but is not limited to, at least one of alumina, boehmite, magnesium oxide, zirconia, barium titanate, titanium dioxide, silica, magnesium hydroxide, and zinc oxide.
[0120] The inorganic particles in the coating include, but are not limited to, at least one of ceramic, boehmite, metal oxide, metal hydroxide, metal carbonate, silicate, kaolin, talc, mineral, and glass. In some embodiments, the inorganic particles include at least one of boehmite, alumina, silica, barium titanate, titanium dioxide, zinc oxide, magnesium oxide, magnesium hydroxide, zirconia, or oxide solid electrolytes. Also, the oxide solid electrolytes include at least one of perovskite type, NASICON type, LISICON type, garnet type, and LiPON type electrolytes.
[0121] b.2 High temperature resistant polymer nanofiber The high temperature resistant polymer nanofibers include unmodified high temperature resistant polymer nanofibers, surface modified high temperature resistant polymer nanofibers, and / or inorganic hybrid high temperature resistant polymer nanofibers.
[0122] The diameter of the high-temperature resistant polymer nanofiber is 5 to 1500 nm, preferably 6 nm or more, 7 nm or more, 8 nm or more, 10 nm or more, 15 nm or more, or 20 nm or more, and preferably 1450 nm or less, 1400 nm or less, 1350 nm or less, 1300 nm or less, or 1200 nm or less. The length of the high-temperature resistant polymer nanofiber is 0.5 to 1000 μm, preferably 0.6 μm or more, 1.0 μm or more, 3.0 μm or more, 5.0 μm or more, 7.0 μm or more, or 10.0 μm or more, and preferably 950 μm or less, 900 μm or less, 800 μm or less, 700 μm or less, or 600 μm or less. The aspect ratio of the high-temperature resistant polymer nanofiber is 5 to 2000, preferably 10 to 1500, more preferably 20 to 500.
[0123] The method for producing high-temperature resistant polymer nanofibers is not particularly limited, and includes at least one of electrospinning, phase separation, template, precipitation, blowing, blow-assisted electrospinning, centrifugation, self-assembly, solution spinning, and in situ synthesis, but is not limited thereto. In some embodiments, electrospinning is used to produce high-temperature resistant polymer nanofibers. The concentration of the spinning polymer in the polymer solution used for electrospinning is 3-30 wt%, more preferably 8-20 wt%. When the relative molecular weight of the polymer is fixed and other conditions are constant, the concentration of the spinning solution is a decisive factor that affects the entanglement of molecular chains in the solution. In the present invention, when the concentration of the spinning solution is within the above range, the spinning performance can be effectively ensured. In addition, when the concentration of the spinning solution is increased, the degree of entanglement of the polymer increases, resulting in good spinning performance. In the present invention, when electrospinning is performed using spinning solutions containing different polymers, the concentration of each spinning solution is independently selected from the above concentration range.
[0124] The unmodified, surface-modified, and inorganic hybrid high temperature resistant polymer nanofibers include, but are not limited to, at least one of P84 nanofibers, polyetherimide nanofibers, polyvinylidene fluoride and its copolymer nanofibers, polyvinylidene fluoride-hexafluoropropylene nanofibers, polytetrafluoroethylene nanofibers, polyphosphazene nanofibers, polyacrylonitrile nanofibers, polyimide nanofibers, polyester nanofibers, cellulose nanofibers, polyetheretherketone nanofibers, polyarylether nanofibers, polyamide nanofibers, and polybenzimidazole nanofibers.
[0125] The polyimide in the polyimide nanofibers is produced by homopolycondensation and copolycondensation of a raw material mixture containing a polybasic acid anhydride and a polyamine.
[0126] Surface-modified high-temperature-resistant polymer nanofibers include, but are not limited to, inorganic surface-modified high-temperature-resistant polymer nanofibers, high-temperature-resistant polymer nanofibers with polar groups after surface treatment, or high-temperature-resistant polymer nanofibers surface-coated with a functionalized organic layer containing polar groups. Polar groups include, but are not limited to, at least one of hydroxyl, carboxyl, sulfonic acid group, amino, phosphate ester group, halogen, and nitro. Compounds used for surface treatment include, but are not limited to, oxidizing agents such as potassium permanganate, chlorate, and potassium dichromate, acidic compounds such as sulfuric acid, nitric acid, phosphoric acid, and hydrochloric acid, alkaline compounds such as sodium hydroxide, potassium hydroxide, calcium hydroxide, lithium hydroxide, barium hydroxide, strontium hydroxide, rubidium hydroxide, aqueous ammonia, methylamine, ethylamine, dimethylamine, diethylamine, ethylenediamine, triethylamine, hydrazine hydrate, DMAB, and salts of strong and weak acids. Functionalized organics containing polar groups include, but are not limited to, polymers such as at least one of polyphosphazenes, polyacrylonitriles, polyphosphoric acids, polysiloxanes, polyester polymers, polyetherimides, polyetheretherketones, polyarylethers, and polybenzimidazoles, and aromatic sulfonic acid derivatives such as 8-aminopyrene-1,3,6-trisulfonic acid and its salts.
[0127] The inorganic hybrid high temperature resistant polymer nanofiber contains an inorganic material. The inorganic material used for surface modification and for the inorganic hybrid high temperature resistant polymer nanofiber includes, but is not limited to, at least one of alumina, boehmite, magnesium oxide, zirconia, barium titanate, titanium dioxide, silica, magnesium hydroxide, and zinc oxide.
[0128] b.3 Inorganic particles In the coating according to the present invention, the inorganic particles are selected from inorganic particles commonly used in this field. The inorganic particles in the coating include, but are not limited to, at least one of ceramics, metal oxides, metal hydroxides, metal carbonates, silicates, kaolin, talc, minerals, and glasses. In some embodiments, the inorganic particles in the coating include, but are not limited to, at least one of Al2O3 (including α, β, γ types), SiO2, BaSO4, BaO, titanium dioxide (TiO2, rutile or anatase), CuO, MgO, Mg(OH)2, LiAlO2, ZrO2, BN, SiC, Si3N4, WC, BC, AlN, Fe2O3, BaTiO3, MoS2, VO5, PbTiO3, TiB2, CaSiO3, molecular sieve (ZSM-5), clay, boehmite, and kaolin, preferably at least one of Al2O3, boehmite, MgO, Mg(OH)2, titanium dioxide (TiO2, rutile or anatase), SiO2, and BaSO4. In some embodiments, the inorganic particles include at least one of boehmite, alumina, silica, barium titanate, titanium dioxide, zinc oxide, magnesium oxide, magnesium hydroxide, zirconia, or oxide solid electrolytes, including at least one of perovskite, NASICON, LISICON, garnet, and LiPON type electrolytes.
[0129] The inorganic particles have an average particle size of 10 nm to 5 μm, preferably 11 nm or more, 13 nm or more, 15 nm or more, 20 nm or more, 25 nm or more, or 30 nm or more, and preferably 4.9 μm or less, 4.7 μm or less, 4.5 μm or less, 4.3 μm or less, or 4.0 μm or less. In some embodiments, the inorganic particles have an average particle size of 10 nm to 5 μm, preferably 11 nm to 4.9 μm, and most preferably 15 nm to 4.5 μm.
[0130] C. Lithium-ion battery The present invention further provides a lithium ion battery comprising a positive electrode, a negative electrode, an electrolyte, and a separator, wherein the separator is said coated modified composite separator.
[0131] The positive electrode is made from the positive electrode material, conductive agent, and binder for lithium-ion batteries. Positive electrode materials used include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), lithium iron phosphate (LiFePO4), lithium manganese iron phosphate (LiFe x Mn 1-x PO4), Lithium manganate-nickel-cobalt (LiNi 1-x-y Co y Mn x O2), lithium aluminate-nickel-cobalt (LiNi 1-x-y Co y Al x O 2e ) and any positive electrode material that can be used in a lithium ion battery.
[0132] The negative electrode is made from a negative electrode material for a lithium ion battery, a conductive agent, and a binder. The negative electrode material used includes any negative electrode material that can be used in a lithium ion battery, such as at least one of graphite, soft carbon, hard carbon, silicon carbon, silicon oxide carbon, etc.
[0133] Examples of binders include, but are not limited to, at least one of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resins, polyamic acids, polyimides, and aramid fibers.
[0134] The conductive material is used to improve the conductivity of the electrode, and includes, but is not limited to, at least one of natural graphite, artificial graphite, carbon black, carbon fiber, carbon nanotube, graphene, carbon nanofiber, metal powder, metal fiber, etc. Metallic copper, nickel, aluminum, silver, etc. may be used as the metal powder and metal fiber.
[0135] The main improvement of the lithium ion battery provided by the present invention is the use of the above-mentioned coated modified composite separator, and the arrangement (connection mode) of the positive electrode, negative electrode, separator, and electrolyte can be similar to that of the prior art, which is known to those skilled in the art and will not be described in detail herein.
[0136] The manufacturing method of a lithium ion battery provided by the present invention includes stacking or winding a positive electrode, a separator, and a negative electrode in order into a cell, and then injecting and sealing an electrolyte into the cell, in which the separator is said coated modified composite separator. EXAMPLES
[0137] In order to make the objectives, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described below with reference to the figures in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, but not all of the embodiments. Based on the embodiments of the present invention, all other embodiments that can be obtained by those skilled in the art without creative work are included in the protection scope of the present invention.
[0138] In the following examples of the present invention, the abbreviation C represents inorganic particles, the abbreviation P represents high temperature resistant polymer nanofibers and / or microspheres, and the abbreviation CP represents a composite of inorganic particles and high temperature resistant polymer nanofibers and / or microspheres.
[0139] The number before the abbreviation represents the thickness of the coating, for example, 4C represents an inorganic coating having a thickness of 4 μm, and 4CP represents a composite coating of inorganic particles and high temperature resistant polymer nanofibers and / or microspheres having a thickness of 4 μm. The coating thickness in the examples of the present invention refers to the thickness after drying.
[0140] Shrinkage rate The modified composite separator is cut into separators of 5cm x 5cm size, and placed in an oven and kept at 150℃ or 200℃ for 30 minutes. The test method for heat shrinkage refers to Chinese standard GB / T 36363-2018. The heat shrinkage of the separator is measured in the longitudinal direction (MD) and transverse direction (TD), and the higher value of the heat shrinkage in MD and TD is defined as the heat shrinkage of the separator.
[0141] Tensile strength measurement The measurement method of the tensile strength of the modified composite separator is in accordance with Chinese standard GB / T 36363-2018. The measurement is carried out on a type 2 sample with a width of (15±0.1)mm under the condition of an initial distance between the clamps of (100±5)mm and a test speed of (250±10)mm / min, and the maximum strength value during the tensile process of the sample is recorded as the tensile strength and compared. The tensile strength is measured in the longitudinal direction (MD) and transverse direction (TD) respectively, and the lower value of the tensile strength in MD and TD is defined as the tensile strength of the modified composite separator.
[0142] Here, the 200° C. tensile strength refers to the tensile strength tested by the above-mentioned method on a sample cut from the modified composite separator after maintaining it at 200° C. for 30 minutes and measuring the thermal shrinkage rate.
[0143] Measurement of air permeability The measurement method of the air permeability of the modified composite separator is in accordance with Chinese standard GB / T 36363-2018. Three pieces of modified composite separator with size of 100mm×100mm are taken for measurement. The modified composite separator is put into Labthink Company's BTY-B2P type air permeability tester for air permeability test. The average value of the three test results is the air permeability of the modified composite separator.
[0144] porosity The modified composite separator is cut into a sample of 2 cm × 2 cm. The mass of the sample is W a The membrane is then placed in a vacuum oven and heated at 60°C for 2 hours to remove the moisture. The dried fiber membrane is then completely immersed in n-butanol for at least 2 hours. The solvent on the membrane surface is completely absorbed through the filter paper. The mass of the membrane is then calculated as W b The porosity is calculated using the following formula:
[0145]
number
[0146] During the ceremony: ρ p : Density of modified composite separator ρ b : Density of n-butanol, 0.81 g / mL.
[0147] Ionic Conductivity The modified composite separator is cut into disks of corresponding specifications. Their thickness is measured. It is placed in a vacuum oven with the temperature set at 80°C and kept at that temperature for 10 hours. The button cell is assembled in a glove box, the atmosphere in the box is argon, and the order is shell, gasket, electrolyte-containing separator, gasket, shell. After the battery is installed, it is left for 12 hours. The AC impedance is measured with a chemical workstation. Its amplitude is set to 5mV, the time is 2 seconds, and the test range is 1-10. 5 Hz. The internal resistance of the separator R dcan be obtained from the AC impedance diagram and the ionic conductivity can be calculated by: δ = d / (R d ×S) (In the formula, R d is the internal resistance of the modified composite gasket, S is the area of the stainless steel gasket, and d is the thickness of the modified composite gasket).
[0148] Battery capacity retention rate A complete battery is fabricated using nickel-rich 8 series NCM ternary material (S85E) and anode silicon oxide carbon 450: the mass ratio of the positive plate active material (S85E): binder (PVDF): conductive agent (SP) = 95: 1.8: 3.2, the solid content is 65 wt%, and the solvent is NMP; the mass ratio of the negative plate active material (silicon oxide carbon 450): binder (SBR: CMC = 2.5: 1.5): conductive agent (SP) = 95: 4.0: 1.0, the solid content is 45 wt%, and the solvent is water. A 2 Ah soft-pack laminated battery is fabricated using the above electrode plates and cycle tested at 1C, and the ratio of the discharge capacity at the 100th cycle to the discharge capacity at the 1st cycle is taken as the capacity retention rate.
[0149] Experiment Series 1 Example 1.1 Preparation of PMDA / ODA-based polyimide (PI) with fiber / microsphere composite morphology: Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed in a molar ratio of 1:1 and reacted in a solvent N,N-dimethylformamide (DMF) in an ice-water bath at 0 °C for 10 h to obtain a clear and transparent polyamic acid solution with a mass concentration of 12%. The polyamic acid solution was electrospun in an electric field with an electric field strength of 1 kV / cm. The polyamic acid film was collected in a stainless steel drum, and then the polyamic acid film was peeled off from the drum and placed in a high-temperature furnace for imidization treatment. The heating program was: from room temperature to 300 °C at a heating rate of 5 °C / min, maintained at 300 °C for 1 h, opened the furnace, and naturally cooled to room temperature.
[0150] Coating slurry formulation: A polymer binder, a mixed solvent of water and ethanol, and a polyimide film were mixed in a weight ratio of 1:79:20 to produce a coating slurry. First, 0.8 g of polyimide film was weighed and dispersed in 3.16 g of a mixed solvent of water and ethanol to obtain a polyimide dispersion. Then, 0.04 g of CMC was weighed and added to the polyimide dispersion, and the mixture was stirred with a high-speed homogenizer at a rotation speed of 1000 rpm for 10 minutes.
[0151] Coating: The stirred PI slurry was placed in a vacuum oven for 1 hour for degassing treatment. The slurry was then uniformly applied to the PE separator and one side of the single-sided ceramic PE separator using microgravure coating. The thickness of the base membrane was 7 μm and 7+2 μm (denoted as 7 and 7+2C, respectively). After coating, the thickness of the coating was 3 μm and the thickness of the membrane was 10 μm and 12 μm (denoted as 7+3P and 7+2C+3P, respectively).
[0152] Drying: The separator coated with the PI slurry was placed in a constant temperature oven and dried. The drying temperature was 50-100°C, and the drying time was 0.5-12 hours. The resulting polyimide with a fiber / microsphere composite morphology is shown in Figure 1, and the morphology of the resulting polyolefin composite separator coated with PI with a fiber / microsphere composite structure is shown in Figure 2.
[0153] After being maintained at 150°C for 30 min, the heat shrinkage of the PE-based membrane was 85%, the heat shrinkage of the PE / PI composite membrane was 4%; the heat shrinkage of the single-sided ceramic PE separator was 6%, and the heat shrinkage of the PI / PE / ceramic composite membrane was 0%.
[0154] After being maintained at 200°C for 30 min, the thermal shrinkage of the PE-based membrane was 87%, the thermal shrinkage of the PE / PI composite membrane was 4.5%; the thermal shrinkage of the single-sided ceramic PE separator was 7%, and the thermal shrinkage of the PI / PE / ceramic composite membrane was 0%.
[0155] Example 1.2 Preparation of PMDA / 4,4'-MDA-based polyimide with fiber / microsphere composite morphology: Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (MDA) were weighed in a molar ratio of 1:1 and reacted in a solvent N,N-dimethylformamide (DMF) in an ice-water bath at 0 °C for 10 h to obtain a clear and transparent polyamic acid solution with a mass concentration of 12%. The polyamic acid solution was electrospun in an electric field with an electric field strength of 1 kV / cm. The polyamic acid film was collected in a stainless steel drum, and then the polyamic acid film was peeled off from the drum and placed in a high-temperature furnace for imidization treatment. The heating program was: from room temperature to 300 °C at a heating rate of 5 °C / min, maintained at 300 °C for 1 h, opened the furnace, and naturally cooled to room temperature.
[0156] Coating slurry formulation: A polymer binder, a mixed solvent of water and ethanol, and a polyimide film were mixed in a weight ratio of 1:79:20 to produce a coating slurry. First, 0.8 g of polyimide film was weighed and dispersed in 3.16 g of a mixed solvent of water and ethanol to obtain a polyimide dispersion. Then, 0.04 g of CMC was weighed and added to the polyimide dispersion, and the mixture was stirred with a high-speed homogenizer at a rotation speed of 1000 rpm for 10 minutes.
[0157] Coating: The stirred PI slurry was placed in a vacuum oven for 1 hour for degassing treatment.The slurry was then uniformly applied onto the PE separator and one side of the single-sided ceramic PE separator using microgravure coating.
[0158] Drying: The separator coated with PI slurry was placed in a constant temperature oven to dry. The drying temperature was 50-100°C, and the drying time was 0.5-12 hours. The thickness of the base film was 7 μm and 7+2 μm (denoted as 7 and 7+2C, respectively). After coating, the thickness of the coating was 3 μm, and the thickness of the film was 10 μm and 12 μm (denoted as 7+3P and 7+2C+3P, respectively). The obtained polyimide with fiber / microsphere composite morphology is shown in Figure 3, and the morphology of the obtained polyolefin composite separator coated with PI with fiber / microsphere composite structure is shown in Figure 4.
[0159] After being maintained at 150°C for 30 min, the heat shrinkage of the PE-based membrane was 85%, the heat shrinkage of the PE / PI composite membrane was 3.5%; the heat shrinkage of the single-sided ceramic PE separator was 6%, and the heat shrinkage of the PI / PE / ceramic composite membrane was 0%.
[0160] After being maintained at 200°C for 30 min, the thermal shrinkage of the PE-based membrane was 87%, the thermal shrinkage of the PE / PI composite membrane was 4%; the thermal shrinkage of the single-sided ceramic PE separator was 7%, and the thermal shrinkage of the PI / PE / ceramic composite membrane was 0%.
[0161] Example 1.3 Preparation of PMDA / p-PDA-based polyimide with fiber / microsphere composite morphology: Monomer pyromellitic dianhydride (PMDA) and monomer p-phenylenediamine (p-PDA) were weighed in a molar ratio of 1:1 and reacted in a solvent N,N-dimethylformamide (DMF) in an ice-water bath at 0 °C for 10 h to obtain a clear and transparent polyamic acid solution with a mass concentration of 12%. The polyamic acid solution was electrospun in an electric field with an electric field strength of 1 kV / cm. The polyamic acid film was collected in a stainless steel drum, and then the polyamic acid film was peeled off from the drum and placed in a high-temperature furnace for imidization treatment. The heating program was: from room temperature to 300 °C at a heating rate of 5 °C / min, maintained at 300 °C for 1 h, opened the furnace, and naturally cooled to room temperature.
[0162] Coating slurry formulation: A polymer binder, a mixed solvent of water and ethanol, and a polyimide film were mixed in a weight ratio of 1:79:20 to produce a coating slurry. First, 0.8 g of polyimide film was weighed and dispersed in 3.16 g of a mixed solvent of water and ethanol to obtain a polyimide dispersion. Then, 0.04 g of CMC was weighed and added to the polyimide dispersion, and the mixture was stirred with a high-speed homogenizer at a rotation speed of 1000 rpm for 10 minutes.
[0163] Coating: The stirred PI slurry was placed in a vacuum oven for 1 hour for degassing treatment.The slurry was then uniformly applied onto the PE separator and one side of the single-sided ceramic PE separator using microgravure coating.
[0164] Drying: The separator coated with PI slurry was placed in a constant temperature oven to dry. The drying temperature was 50-100°C, and the drying time was 0.5-12 hours. The thickness of the base film was 7μm and 7+2μm (denoted as 7 and 7+2C, respectively). After coating, the thickness of the coating was 3μm, and the thickness of the film was 10μm and 12μm (denoted as 7+3P and 7+2C+3P, respectively). The polyimide with the obtained fiber / microsphere composite morphology is shown in Figure 5, the morphology of the obtained polyolefin composite separator coated with PI of the fiber / microsphere composite structure is shown in Figure 6, and the comparative photograph of the thermal shrinkage at different temperatures of the obtained polyolefin composite separator coated with PI of the fiber / microsphere composite structure is shown in Figure 7.
[0165] After being maintained at 150°C for 30 min, the heat shrinkage of the PE-based membrane was 85%, the heat shrinkage of the PE / PI composite membrane was 3%; the heat shrinkage of the single-sided ceramic PE separator was 6%, and the heat shrinkage of the PI / PE / ceramic composite membrane was 0%.
[0166] After being maintained at 200°C for 30 min, the thermal shrinkage of the PE-based membrane was 87%, the thermal shrinkage of the PE / PI composite membrane was 3.2%; the thermal shrinkage of the single-sided ceramic PE separator was 7%, and the thermal shrinkage of the PI / PE / ceramic composite membrane was 0%.
[0167] Experiment Series 2 Example 2.1 Polyimide microspheres / ceramic coated polyethylene separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed in a molar ratio of 1:1 and reacted in the solvent N,N-dimethylformamide (DMF) to obtain a clear and transparent polyamic acid solution with a mass concentration of 6%. Then, electrostatic spraying method was used to fabricate PAA microspheres. The obtained microspheres were imidized in a high-temperature furnace. The heating program was: from room temperature to 300°C at a heating rate of 5°C / min and maintained for 1 hour to obtain polyimide microspheres.
[0168] (2) 10 g of polyimide microspheres (average particle size 800 nm), 90 g of ceramic, 1.5 g of binder sodium carboxymethylcellulose, 200 g of a mixed solvent of water and ethanol (ethanol 5 wt%), 0.3 g of surfactant perfluoroalkyl ether quaternary ammonium salt, 0.3 g of dispersant hydroxypropylmethylcellulose, 0.06 g of wetting agent glycerol, and 0.3 g of defoaming agent fluorinated alkyl phosphate were weighed; the components were dissolved and uniformly dispersed by stirring to obtain a coating slurry.
[0169] (3) The stirred coating slurry was placed in a vacuum oven for 1 hour for degassing treatment, and then uniformly coated on one or both sides of a 7 μm polyethylene separator using microgravure coating to obtain coated polyethylene separator (denoted as 7+4CP and 7+4CP+4CP); the non-ceramic side of the 7+4 μm single-sided ceramic polyethylene separator was denoted as 7+4C+4P, which indicates a base membrane thickness of 7 μm, and a ceramic coating thickness of 4 μm, the coating thickness of which is 4 μm obtained from the coating slurry in (2).
[0170] (4) Drying: The coated polyethylene separator was placed in a thermostatic oven and dried. The drying temperature was 60°C and the drying time was 0.5 hours. The shape of the obtained modified composite polyethylene separator is shown in Figure 8.
[0171] Each of the above separators was tested for performance, the results of which are shown in Table 1 below:
[0172] [Table 1]
[0173] Example 2.2 Polyimide Microspheres / Boehmite Coated Polypropylene Separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed in a molar ratio of 1:1 and reacted in the solvent N,N-dimethylformamide (DMF) to obtain a clear and transparent polyamic acid solution with a mass concentration of 20%. Polyamic acid microspheres were then produced by blow electrostatic spraying. The microspheres were imidized in a high-temperature furnace. The heating program was: from room temperature to 300°C at a heating rate of 5°C / min and maintained for 1 hour to obtain polyimide microspheres.
[0174] (2) 80 g of boehmite, 20 g of polyimide microspheres (average particle size of the microspheres: 200 nm), and 6.4 g of PVDF were weighed and dispersed in 450 g of NMP to obtain a coating slurry.
[0175] (3) The stirred coating slurry was placed in a vacuum oven for 1 h for degassing treatment, and then uniformly coated on one or both sides of a 12 μm polypropylene separator using microgravure coating to obtain two types of coated polypropylene separators.
[0176] (4) The coated polypropylene separator was placed in a constant temperature oven to dry. The drying temperature was 60°C, and the drying time was 1 hour. The modified composite separators coated on one side and both sides obtained in step (3) were denoted as 12+3CP and 12+3CP+3CP, respectively. The non-ceramic side of the 12+3μm single-sided ceramic polypropylene separator was uniformly coated by the coating method according to step (3), which was denoted as 12+3C+3CP, which indicates a base film thickness of 12μm, a ceramic coating film thickness of 3μm, and a coating thickness of 3μm obtained from the coating slurry in (2).
[0177] Each of the above separators was tested for performance and the results are shown in Table 2 below.
[0178] [Table 2]
[0179] Example 2.3 Hybrid polyimide microsphere / ceramic coated polyethylene separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed in a molar ratio of 1:1 and added to the solvent N,N-dimethylformamide (DMF) to synthesize a clear and transparent polyamic acid solution (PAA) with a mass concentration of 10%. 100 nm of LATP solid electrolyte was dispersed in the PAA solution to obtain a dispersion of LATP and polyamic acid. The dispersion was electrostatically sprayed to obtain LATP / PAA hybrid microspheres. The microspheres were placed in a high-temperature furnace for imidization treatment. The heating program was: from room temperature to 300 °C at a heating rate of 5 °C / min and maintained for 1 h to obtain LATP / PI hybrid microspheres.
[0180] (2) 50 g of LATP / PI hybrid microspheres (average particle size of the microspheres: 300 nm), 50 g of ceramic, 5.0 g of PVDF binder, 390 g of a mixed solvent of water and ethanol (ethanol 10 wt%), 2.5 g of perfluoroalkyl ether quaternary ammonium salt surfactant, 2.5 g of hydroxypropylmethylcellulose dispersant, and 0.1 g of glycerol wetting agent were weighed and uniformly stirred to obtain a coating slurry.
[0181] (3) The stirred coating slurry was placed in a vacuum oven for 1 hour for degassing treatment, and then uniformly coated on both sides of a 7 μm polyethylene separator using extrusion coating to obtain a coated polyethylene separator.
[0182] (4) The coated polyethylene separator was placed in a thermostatic oven and dried. The drying temperature was 60° C. and the drying time was 1 hour. The separator was designated as 7+2CP+2CP.
[0183] The above separators were tested for performance and the results are shown in Table 3 below.
[0184] [Table 3]
[0185] Example 2.4 Polyacrylonitrile (PAN) microspheres / magnesium oxide coated polypropylene separator (1) 7.3 g of polyacrylonitrile was dissolved in 92.7 g of N-methylpyrrolidone (NMP) and stirred to obtain a clear and transparent PAN solution with a mass concentration of 7.3%. PAN microspheres were produced by a blow electrostatic spray method.
[0186] (2) 5 g of PAN microspheres (average particle size of microspheres: 1000 nm) and 95 g of magnesium oxide were weighed, dispersed in 240 g of water, and stirred at high speed to obtain a PAN microsphere / magnesium oxide dispersion. Then, 5.0 g of sodium carboxymethylcellulose was weighed and dissolved in 150 g of water until it was completely dissolved. The above two slurries were mixed and stirred uniformly to obtain a coating slurry.
[0187] (3) The stirred coating slurry was placed in a vacuum oven for 1 hour for degassing treatment, and then uniformly coated on both sides of a 12 μm polypropylene separator using microgravure coating to obtain a coated polypropylene separator.
[0188] (4) The coated polypropylene separator was placed in a constant temperature oven to dry. The drying temperature was 60°C and the drying time was 1 hour. The thickness of the dried coating was 3 μm, and the separator was designated as 12+3CP+3CP.
[0189] Each of the above separators was tested for performance, the results of which are shown in Table 4 below:
[0190] [Table 4]
[0191] Example 2.5 Polyimide / Silica microspheres / Li7La3Zr2O 12(LLZO) Garnet-type solid oxide electrolyte coated polyethylene separator (1) 90g of monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed in a molar ratio of 1:1 and added to the solvent N,N-dimethylformamide (DMF) to synthesize a clear and transparent polyamic acid solution with a mass concentration of 12%. 10g of TEOS was added and stirred uniformly. Then polyamic acid microspheres were produced by electrostatic spraying. The microspheres were placed in a high-temperature furnace for imidization treatment. The heating program was: from room temperature to 300°C at a heating rate of 5°C / min, and maintained at 300°C for 1 hour to obtain polyimide / silica microspheres containing silica on the surface and inside.
[0192] (2) 1 g of polyimide / silica microspheres (average particle size of the microspheres: 1300 nm), 99 g of LLZO, 5 g of polyacrylamide, 1.8 g of a perfluoroalkyl ether quaternary ammonium salt surfactant, 0.5 g of a hydroxypropyl methylcellulose dispersant, 0.5 g of a glycerol wetting agent, and 0.2 g of an antifoaming agent were dissolved in 140 g of water and thoroughly stirred to dissolve the mixture, thereby obtaining a coating slurry.
[0193] (3) The stirred coating slurry was placed in a vacuum oven for 1 hour for degassing treatment. The slurry was then uniformly coated on both sides of a 7 μm polyethylene separator using a microgravure coating method.
[0194] (4) The coated polyethylene separator was placed in a thermostatic oven and dried at a temperature of 55° C. for 0.5 hours.
[0195] The above separators were tested for performance and the results are shown in Table 5 below.
[0196] [Table 5]
[0197] Example 2.6 Polyimide nanospheres / boehmite-coated polyethylene composite separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and reacted in the solvent N,N-dimethylformamide (DMF) to obtain a clear and transparent polyamic acid solution with a mass concentration of 10%. Polyamic acid (PAA) microspheres were then fabricated by electrostatic blowing. The temperature of the obtained microspheres was increased from room temperature to 300 °C at a heating rate of 5 °C / min and maintained for 1 h to obtain polyimide microspheres.
[0198] (2) 20 g of polyimide microspheres (average particle size of the microspheres: 750 nm), 80 g of boehmite (average particle size of 500 nm), 1.5 g of sodium carboxymethylcellulose, 175 g of a mixed solvent of water and ethanol (ethanol 5 wt%), 0.3 g of a perfluoroalkyl ether quaternary ammonium salt surfactant, 0.3 g of a hydroxypropylmethylcellulose dispersant, and 0.06 g of glycerol wetting agent were weighed out and stirred uniformly to obtain a coating slurry.
[0199] (3) The coating slurry was placed in a vacuum oven for 1 hour for degassing treatment, and then uniformly coated on both sides of a 7 μm polyethylene separator using a microgravure coating method to obtain a coated modified separator.
[0200] (4) The coated modified separator was placed in a constant temperature oven and dried. The drying temperature was 55°C and the drying time was 1 hour. The obtained modified composite polyethylene separator was designated as 7+2CP+2CP.
[0201] The manufacturing processes of Examples 2.7-2.14 were similar to that of Example 2.6, except that the inorganic particles and / or high temperature resistant microspheres used in the coating were different.
[0202] Table 6 shows the test results of the test performance of Examples 2.6 to 2.14.
[0203] [Table 6]
[0204] Example 2.15 Polyimide hybrid microspheres / barium titanate polyolefin composite separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and reacted in the solvent N,N-dimethylformamide (DMF) to obtain a polyamic acid solution with a mass concentration of 10%. Nano-titanium dioxide (PAA:titanium dioxide mass ratio 95:5) was added to this and thoroughly stirred. Then PAA hybrid microspheres were produced by electrostatic spraying. The obtained microspheres were imidized in a high-temperature furnace. The heating program was: from room temperature to 300°C at a heating rate of 5°C / min, and maintained at 300°C for 1 hour to obtain polyimide / titanium dioxide microspheres.
[0205] Steps (2) to (4) were the same as those in Example 2.6, except that the inorganic particles were changed to barium titanate.
[0206] Example 2.16 Polyetherimide microspheres / zinc oxide polyolefin composite separator (CP / PE / CP) (1) 7.5 g of polyetherimide was dissolved in 92.5 g of N-methylpyrrolidone (NMP) and stirred to obtain a polyetherimide solution with a mass concentration of 7.5%, from which polyetherimide microspheres were produced by electrostatic spraying. Steps (2) to (4) were similar to those in Example 2.6.
[0207] Example 2.17 Polyacrylonitrile (PAN) microspheres / silica polyolefin composite separator (CP / PE / CP) (1) 7.5 g of polyacrylonitrile was dissolved in 92.5 g of N-methylpyrrolidone (NMP) and stirred to obtain a PAN solution with a mass concentration of 7.5%, from which polyacrylonitrile microspheres were produced by electrostatic spraying. Steps (2) to (4) were similar to those in Example 2.6.
[0208] Example 2.18 P84 microsphere / zirconia polyolefin composite separator (CP / PE / CP) (1) 7.5 g of P84 was dissolved in 92.5 g of N-methylpyrrolidone (NMP) and stirred to obtain a P84 solution with a mass concentration of 7.5%, from which P84 microspheres were produced by blow-spraying. Steps (2) to (4) were similar to those in Example 2.6.
[0209] Example 2.19 Polyester (polyethylene terephthalate, PET) microspheres / kaolin polyolefin composite separator (CP / PE / CP) (1) 7.5 g of PET was dissolved in 92.5 g of xylenol and stirred to obtain a PET solution with a mass concentration of 7.5%, and then PET microspheres were produced by electrostatic spraying. Steps (2) to (4) were similar to those in Example 2.6.
[0210] Example 2.20 Polyimide nanosphere-coated polyethylene composite separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and reacted in the solvent N,N-dimethylformamide (DMF) to obtain a polyamic acid solution with a mass concentration of 10%. PAA microspheres were then produced by electrostatic blowing. The temperature of the obtained microspheres was increased from room temperature to 300 °C at a heating rate of 5 °C / min and maintained for 1 h to obtain polyimide microspheres.
[0211] (2) 100 g of polyimide microspheres (average particle size of the microspheres: 750 nm), 1.5 g of sodium carboxymethylcellulose, 175 g of a mixed solvent of water and ethanol (ethanol 5 wt %), 0.3 g of a perfluoroalkyl ether quaternary ammonium salt surfactant, 0.3 g of a hydroxypropylmethylcellulose dispersant, and 0.06 g of glycerol wetting agent were weighed out and stirred uniformly to obtain a coating slurry.
[0212] (3) The stirred coating slurry was placed in a vacuum oven for 1 h for degassing treatment, and then uniformly coated on both sides of a 7 μm polyethylene separator using a microgravure coating method to obtain a coated modified separator.
[0213] (4) The coated modified separator was placed in a constant temperature oven and dried. The drying temperature was 55°C and the drying time was 1 hour. The obtained modified composite polyethylene separator was designated as 7+2P+2P.
[0214] [Table 7]
[0215] Experiment Series 3 Example 3.1 Polyimide nanofiber / ceramic coated polyethylene separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and reacted in a solvent N,N-dimethylformamide (DMF) to obtain a polyamic acid solution with a mass concentration of 6% in this example. PAA nanofibers were produced by electrospinning. The obtained fibers were imidized in a high-temperature furnace. The heating program was: from room temperature to 300°C at a heating rate of 5°C / min, and maintained for 1 hour to obtain polyimide nanofibers.
[0216] (2) 10 g of polyimide nanofibers (average fiber diameter 800 nm, aspect ratio in the range of 10 to 200), 90 g of ceramic, 1.5 g of binder sodium carboxymethylcellulose, 200 g of a mixed solvent of water and ethanol (ethanol 5 wt%), 0.3 g of surfactant perfluoroalkyl ether quaternary ammonium salt, 0.3 g of dispersant hydroxypropylmethylcellulose, 0.06 g of wetting agent glycerol, and 0.3 g of defoaming agent fluorinated alkyl phosphate were weighed; the components were dissolved and uniformly dispersed by stirring to obtain a coating slurry.
[0217] (3) The stirred coating slurry was placed in a vacuum oven for 1 hour for degassing treatment, and then uniformly coated on one or both sides of a 7μm polyethylene separator using a microgravure coating method to obtain coated polyethylene separators (denoted as 7+4CP and 7+4CP+4CP); the non-ceramic side of the 7+4μm single-sided ceramic polyethylene separator was denoted as 7+4C+4P. The thickness of the base membrane was 7μm.
[0218] (4) Drying: The coated polyethylene separator was placed in a thermostatic oven and dried. The drying temperature was 60°C and the drying time was 0.5 hours. The shape of the obtained modified composite polyethylene separator is shown in Figure 11.
[0219] Each of the above separators was tested for performance and the results are shown in Table 8 below.
[0220] [Table 8]
[0221] Example 3.2 Polyimide nanofiber / boehmite coated polypropylene separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and added to a solvent N,N-dimethylformamide (DMF) to obtain a polyamic acid solution with a mass concentration of 20% in this example. Polyamic acid nanofibers were produced by blow electrospinning. The nanofibers were imidized in a high-temperature furnace. The heating program was: from room temperature to 300°C at a heating rate of 5°C / min, and maintained for 1 hour to obtain polyimide nanofibers.
[0222] (2) 80 g of boehmite, 20 g of polyimide nanofibers (average fiber diameter 200 nm, aspect ratio in the range of 10 to 200), and 6.4 g of PVDF were weighed and dispersed in 450 g of NMP to obtain a coating slurry.
[0223] (3) The stirred coating slurry was placed in a vacuum oven for 1 hour for degassing treatment, and then uniformly coated on one or both sides of a 12 μm polypropylene separator using a microgravure coating method to obtain two types of coated polypropylene separators.
[0224] (4) The coated polypropylene separator was placed in a constant temperature oven to dry. The drying temperature was 60°C, and the drying time was 1 hour. The modified composite separators coated on one side and both sides obtained in step (3) were denoted as 12+4CP and 12+4CP+4CP, respectively. The non-ceramic side of the 12+4μm single-sided ceramic polypropylene separator was uniformly coated by the coating method according to step (3), which was denoted as 12+4C+4CP, which indicates a base film thickness of 12μm, a ceramic coating thickness of 4μm, and a coating thickness of 4μm obtained from the coating slurry in (2).
[0225] The coating morphology of the obtained modified composite polypropylene separator is shown in FIG. Each of the above separators was tested for performance and the results are shown in Table 9 below.
[0226] [Table 9]
[0227] Example 3.3 Hybrid polyimide nanofiber / ceramic coated polyethylene separator (1) P84 was dissolved in a solvent, N,N-dimethylacetamide (DMAc), to obtain a polyamic acid solution with a mass concentration of 10% in this example. A 100 nm LATP solid electrolyte was dispersed in the P84 solution to obtain a LATP and P84 dispersion. The dispersion was electrospun to obtain LATP / P84 hybrid nanofibers.
[0228] (2) 50 g of LATP / P84 hybrid nanofibers (average fiber diameter: 300 nm, aspect ratio in the range of 20 to 400), 50 g of ceramic, 5.0 g of binder PVDF, 390 g of a mixed solvent of water and ethanol (ethanol 10 wt%), 2.5 g of surfactant perfluoroalkyl ether quaternary ammonium salt, 2.5 g of dispersant hydroxypropyl methylcellulose, and 0.1 g of wetting agent glycerol were weighed and uniformly stirred to obtain a coating slurry.
[0229] (3) The stirred coating slurry was placed in a vacuum oven for 1 hour for degassing treatment, and then uniformly coated on both sides of a 7 μm polyethylene separator using an extrusion coating method to obtain a coated polyethylene separator.
[0230] (4) The coated polyethylene separator was placed in a thermostatic oven and dried. The drying temperature was 60° C. and the drying time was 1 hour. The separator was designated as 7+2CP+2CP.
[0231] The coating morphology of the obtained modified composite polyethylene separator is shown in FIG.
[0232] [Table 10]
[0233] Example 3.4 Polyacrylonitrile (PAN) nanofiber / magnesium oxide coated polypropylene separator (1) 8 g of polyacrylonitrile was dissolved in 92 g of N-methylpyrrolidone (NMP) and stirred to obtain a PAN solution with a mass concentration of 8% in this example, from which PAN nanofibers were produced by electrospinning.
[0234] (2) 5 g of PAN nanofibers (average nanofiber diameter: 400 nm, aspect ratio in the range of 10 to 300) and 95 g of magnesium oxide were weighed, dispersed in 240 g of water, and stirred at high speed to obtain a PAN nanofiber / magnesium oxide dispersion. Next, 5.0 g of sodium carboxymethylcellulose was weighed and dissolved in 150 g of water until it was completely dissolved. The above two slurries were mixed and stirred uniformly to obtain a coating slurry.
[0235] (3) The stirred coating slurry was placed in a vacuum oven for 1 hour for degassing treatment, and then uniformly coated on both sides of a 12 μm polypropylene separator using a microgravure coating method to obtain a coated polypropylene separator.
[0236] (4) The coated polypropylene separator was placed in a constant temperature oven to dry. The drying temperature was 60°C and the drying time was 1 hour. The thickness of the dried coating was 3 μm, and the separator was designated as 12+3CP+3CP.
[0237] The coating morphology of the obtained modified composite polypropylene separator is shown in FIG.
[0238] [Table 11]
[0239] Example 3.5 Polyimide / Silica nanofiber / Li7La3Zr2O 12 (LLZO) Garnet-type solid oxide electrolyte coated polyethylene separator (1) 90 g of monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and added to the solvent N,N-dimethylformamide (DMF) to obtain a polyamic acid solution with a mass concentration of 12% in this example. 10 g of TEOS was added and stirred uniformly. Then polyamic acid nanofibers were produced by electrospinning. The nanofibers were placed in a high-temperature furnace for imidization treatment. The heating program was: from room temperature to 300°C at a heating rate of 5°C / min, and maintained at 300°C for 1 hour, to obtain polyimide / silica nanofibers containing silica on the surface and inside of the fiber.
[0240] (2) 1 g of polyimide / silica nanofibers (average fiber diameter: 350 nm, aspect ratio in the range of 15 to 450), 99 g of LLZO, 5 g of polyacrylamide, 1.8 g of a surfactant perfluoroalkyl ether quaternary ammonium salt, 0.5 g of a dispersant hydroxypropyl methylcellulose, 0.5 g of a wetting agent glycerol, and 0.2 g of an antifoaming agent were dissolved in 140 g of water and thoroughly stirred to dissolve, thereby obtaining a coating slurry.
[0241] (3) The stirred coating slurry was placed in a vacuum oven for 1 hour for degassing treatment. The slurry was then uniformly coated on both sides of a 7 μm polyethylene separator using a microgravure coating method.
[0242] (4) The coated polyethylene separator was placed in a thermostatic oven and dried at 55° C. for 0.5 hours.
[0243] The shape of the resulting modified composite polyethylene separator is shown in FIG.
[0244] [Table 12]
[0245] Example 3.6 Polyimide nanofiber / boehmite-coated polyethylene composite separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and reacted in a solvent N,N-dimethylformamide (DMF) to obtain a polyamic acid solution with a mass concentration of 10% in this example. PAA nanofibers were then produced by electrospinning. The temperature of the obtained fiber was increased from room temperature to 300°C at a heating rate of 5°C / min and maintained for 1 hour to obtain polyimide nanofibers.
[0246] (2) 20 g of polyimide nanofibers (nanofiber average diameter: 270 nm, aspect ratio in the range of 10 to 280), 80 g of boehmite (average particle size 500 nm), 1.5 g of sodium carboxymethylcellulose, 175 g of a mixed solvent of water and ethanol (ethanol 5 wt%), 0.3 g of a surfactant perfluoroalkyl ether quaternary ammonium salt, 0.3 g of a dispersant hydroxypropylmethylcellulose, and 0.06 g of a wetting agent glycerol were weighed out and uniformly stirred to obtain a coating slurry.
[0247] (3) The stirred coating slurry was placed in a vacuum oven for 1 h for degassing treatment, and then uniformly coated on both sides of a 7 μm polyethylene separator using a microgravure coating method to obtain a coated modified separator.
[0248] (4) The coated modified separator was placed in a constant temperature oven and dried. The drying temperature was 55°C and the drying time was 1 hour. The obtained modified composite polyethylene separator was designated as 7+2CP+2CP.
[0249] The manufacturing process of Examples 3.7-3.8 was similar to that of Example 2.6, except that the inorganic particles used in the coating were different.
[0250] Example 3.9 Polyvinylidene fluoride (PVDF) nanofiber / boehmite-coated polyolefin composite separator (1) PVDF was dissolved in a solvent, N,N-dimethylacetamide (DMAc), to obtain a PVDF solution with a mass concentration of 8% in this example, from which PVDF nanofibers were produced by blow electrospinning. Steps (2) to (4) were similar to those in Example 3.6.
[0251] Example 3.10 Polyimide hybrid nanofiber / barium titanate polyolefin composite separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and reacted in a solvent N,N-dimethylformamide (DMF) to obtain a polyamic acid solution with a mass concentration of 10% in this example. Nano-titanium dioxide was added thereto (mass ratio of PAA:titanium dioxide 95:5) and thoroughly stirred. Then, PAA hybrid nanofibers were produced by electrospinning. The obtained nanofibers were imidized in a high-temperature furnace. The heating program was: from room temperature to 300°C at a heating rate of 5°C / min, and maintained at 300°C for 1 hour to obtain polyimide / titanium dioxide hybrid nanofibers.
[0252] Steps (2) to (4) were the same as those in Example 3.6, except that the inorganic particles were changed to barium titanate.
[0253] Example 3.11 Polyetherimide nanofiber / zinc oxide polyolefin composite separator (CP / PE / CP) (1) 7.5 g of polyetherimide was dissolved in 92.5 g of N-methylpyrrolidone (NMP) and stirred to obtain a polyetherimide solution having a mass concentration of 8% in this example, from which polyetherimide nanofibers were produced by blow spinning. Steps (2) to (4) were similar to those in Example 3.6.
[0254] Example 3.12 Polyacrylonitrile (PAN) nanofiber / silica polyolefin composite separator (CP / PE / CP) (1) 7.5 g of polyacrylonitrile was dissolved in 92.5 g of N-methylpyrrolidone (NMP) and stirred to obtain a PAN solution with a mass concentration of 7.5% in this example, from which polyacrylonitrile nanofibers were produced by blow spinning. Steps (2) to (4) were similar to those in Example 3.6.
[0255] Example 3.13 P84 nanofiber / zirconia polyolefin composite separator (CP / PE / CP) (1) 7.5 g of P84 was dissolved in 92.5 g of N-methylpyrrolidone (NMP) and stirred to obtain a P84 solution with a mass concentration of 7.5% in this example, and then P84 nanofibers were produced by blow spinning. Steps (2) to (4) were similar to those in Example 3.6.
[0256] Example 3.14 Polyester (polyethylene terephthalate, PET) nanofiber / kaolin polyolefin composite separator (CP / PE / CP) (1) 7.5 g of PET was dissolved in 92.5 g of xylenol and stirred to obtain a PET solution with a mass concentration of 7.5% in this example, from which PET nanofibers were produced by blow spinning. Steps (2) to (4) were similar to those in Example 3.6.
[0257] Example 3.15 Hydroxypropyl methylcellulose nanofiber / calcium silicate polyolefin composite separator (CP / PE / CP) (1) 3.5 g of cellulose was dissolved in 96.5 g of xylenol and stirred to obtain a cellulose solution with a mass concentration of 3.5% in this example, from which cellulose nanofibers were produced by blow spinning. Steps (2) to (4) were similar to those in Example 3.6.
[0258] Table 13 shows the test performance test results for Examples 3.6 to 3.15.
[0259] [Table 13]
[0260] Example 3.16 Double-sided coated polyimide nanofiber / boehmite polyolefin composite separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and reacted in a solvent N,N-dimethylformamide (DMF) to obtain a polyamic acid solution with a mass concentration of 10% in this example. Then, PAA nanofibers were produced by electrospinning. The fibers were imidized in a high-temperature furnace. The heating program was; from room temperature to 300°C at a heating rate of 5°C / min, and maintained for 1 hour to obtain polyimide nanofibers.
[0261] (2) 0.4 g of polyimide nanofibers, 99.6 g of boehmite (average particle size 500 nm), 1.5 g of sodium carboxymethylcellulose, 175 g of a mixed solvent of water and ethanol (ethanol 5 wt%), 0.3 g of a surfactant perfluoroalkyl ether quaternary ammonium salt, 0.3 g of a dispersant hydroxypropylmethylcellulose, and 0.06 g of a wetting agent glycerol were weighed and thoroughly stirred to obtain a coating slurry.
[0262] (3) The coating slurry was placed in a vacuum oven for 1 hour for degassing treatment, and then uniformly coated on both sides of a 9μm polyethylene separator using a microgravure coating method to obtain a coated modified separator. The coating thickness after drying was 2μm.
[0263] (4) The coated modified separator was placed in a constant temperature oven and dried. The drying temperature was 55°C and the drying time was 1 hour. The obtained modified composite separators were denoted as 9+2CP+2CP. The thickness of the modified composite polyethylene separator was 13 μm.
[0264] The manufacturing processes of Examples 3.17 to 3.24, Comparative Example 1 (3.C1), and Comparative Example 2 (3.C2) were similar to that of Example 3.16, except that the amounts of polyimide nanofiber and boehmite were different. Specific compositions and test results are shown in Table 14.
[0265] [Table 14]
[0266] Example 4.1 Double-sided coated polyimide nanofiber / boehmite polyolefin composite separator (1) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and reacted in a solvent N,N-dimethylformamide (DMF) to obtain a polyamic acid solution with a mass concentration of 10% in this example. Then PAA nanofibers were produced by electrospinning. The fibers were imidized in a high-temperature furnace. The heating program was: from room temperature to 300°C at a heating rate of 5°C / min, and maintained for 1 hour to obtain polyimide nanofibers.
[0267] (2) Monomer pyromellitic dianhydride (PMDA) and monomer 4,4'-diaminodiphenyl ether (ODA) were weighed out in a molar ratio of 1:1 and reacted in the solvent N,N-dimethylformamide (DMF) to obtain a clear and transparent polyamic acid solution with a mass concentration of 10%. PAA microspheres were then fabricated by electrostatic blowing. The temperature of the obtained microspheres was increased from room temperature to 300 °C at a heating rate of 5 °C / min and maintained for 1 h to obtain polyimide microspheres.
[0268] (3) 35 g of polyimide microspheres (average particle size of the microspheres: 750 nm), 5.4 g of polyimide nanofibers, 59.6 g of silica (average particle size of 500 nm), 1.5 g of sodium carboxymethylcellulose, 175 g of a mixed solvent of water and ethanol (ethanol 5 wt%), 0.3 g of a perfluoroalkyl ether quaternary ammonium salt surfactant, 0.3 g of a hydroxypropylmethylcellulose dispersant, and 0.06 g of glycerol wetting agent were weighed out and stirred uniformly to obtain a coating slurry.
[0269] (4) The coating slurry was placed in a vacuum oven for 1 hour for degassing treatment, and then uniformly coated on both sides of a 7μm polyethylene separator using a microgravure coating method to obtain a coated modified separator. The coating thickness after drying was 2μm.
[0270] (5) The coated modified separator was placed in a constant temperature oven and dried. The drying temperature was 55°C and the drying time was 1 hour. The obtained modified composite polyethylene separator was designated as 7+2CP+2CP. The thickness of the modified composite polyethylene separator was 11 μm. The performance test results are shown in Table 15.
[0271] [Table 15]
Claims
1. The coated modified composite separator includes a base membrane and a coating, The coating covers either one or both sides of the base membrane; The coating is: b2.1 high temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles A coated modified composite separator comprising at least two of:
2. 2. The coated modified composite separator of claim 1, wherein the high temperature resistant polymer comprises polyimide and the coating preferably comprises polyimide nanofibers / polyimide microspheres.
3. The particle size of the high temperature resistant polymeric microspheres is between 3 and 5000 nm, preferably between 5 and 3000 nm, more preferably between 8 and 2000 nm; and / or The diameter of the high temperature resistant polymer nanofibers is 5 to 1500 nm, preferably 6 to 1450 nm, more preferably 8 to 1350 nm; and / or The length of the high temperature resistant polymer nanofiber is 0.5 to 1000 μm, preferably 0.6 to 950 μm, more preferably 1.0 to 900 μm; and / or The inorganic particles have an average particle size of 3 nm to 5 μm, preferably 7 nm to 4.9 μm, and most preferably 10 nm to 4.5 μm; and / or the thickness of the base membrane is between 1.5 and 40 μm, preferably between 2.0 and 35 μm, more preferably between 3.5 and 30 μm; and / or The total thickness of the coated modified composite separator is from 2.0 to 45 μm, preferably from 2.5 to 40 μm, and most preferably from 3 to 36 μm; and / or The coated modified composite separator according to claim 1, characterized in that the thickness of the coating is 0.2-10 μm, preferably 0.3-9 μm, more preferably 0.5-8 μm.
4. the base membrane is a polymer-based membrane or a polymer-based membrane coated with inorganic particles; 3. The coated modified composite separator according to claim 1 or 2, characterized in that the polymer-based membrane preferably comprises at least one of polyolefin-based membrane, cellulose-based membrane, polyester-based membrane, aramid fiber-based membrane, polyimide-based membrane, and organic-inorganic hybrid-based membrane.
5. the coating comprises high temperature resistant polymeric microspheres and inorganic particles; and The coated modified composite separator according to claim 1, characterized in that the weight ratio of high temperature resistant polymeric microspheres to inorganic particles is 0.1-99.9:99.9-0.1, preferably 1-99.9:99-0.1, more preferably 5-99.9:95-0.1, and most preferably 30-99.9:70-0.
1.
6. 2. The coated modified composite separator of claim 1, wherein the polymer-based membrane comprises a single layer membrane, a bilayer membrane, or a multilayer membrane, and the polymer-based membranes contained in each layer are the same or different.
7. the high temperature resistant polymeric microspheres include at least one of the following: unmodified high temperature resistant polymeric microspheres, surface modified high temperature resistant polymeric microspheres, and inorganic hybrid high temperature resistant polymeric microspheres; Preferably, the polymer in the unmodified high temperature resistant polymeric microspheres, the surface modified high temperature resistant polymeric microspheres, and the inorganic hybrid high temperature resistant polymeric microspheres comprises at least one of P84, polyetherimide, polyphosphazene, polyacrylonitrile, polystyrene, polyvinylidene fluoride, polyvinylidene fluoride copolymers, polyvinylidene fluoride-hexafluoropropylene, polymethylmethacrylate, polytetrafluoroethylene, polyimide, polyester, cellulose, polyetheretherketone, polyarylether, polyamide, and polybenzimidazole; Preferably, the surface-modified high temperature resistant polymeric microspheres include at least one of inorganic surface-modified high temperature resistant polymeric microspheres, high temperature resistant polymeric microspheres having polar groups after surface treatment, or high temperature resistant polymeric microspheres surface-coated with a functionalized polymer layer containing polar groups; 7. The coated modified composite separator according to any one of claims 5 to 6, characterized in that the inorganic hybrid high temperature resistant polymer microspheres preferably comprise at least one of polyimide / silica microspheres, polyimide / titanium dioxide microspheres, polyimide / zirconia microspheres, polyimide / zinc oxide microspheres, polyimide / magnesium oxide microspheres, polyimide / magnesium hydroxide microspheres, polyimide / alumina microspheres, polyimide / boehmite microspheres, polyimide / cerium oxide microspheres, polyimide / scandium oxide microspheres, polyimide / vanadium pentoxide microspheres.
8. 2. The coated modified composite separator of claim 1, wherein the coating comprises high temperature resistant polymer nanofibers and inorganic particles, and the weight ratio of high temperature resistant polymer nanofibers to inorganic particles is (0.4-65):(99.6-35), preferably (1-64):(99-36), more preferably (3-62):(97-38), and most preferably (5-59):(95-41).
9. the high temperature resistant polymer nanofibers include at least one of the following: unmodified high temperature resistant polymer nanofibers, surface modified high temperature resistant polymer nanofibers, and inorganic hybrid high temperature resistant polymer nanofibers; Preferably, the unmodified high temperature resistant polymer nanofibers and the high temperature resistant polymer nanofibers used for surface modification and inorganic hybridization include at least one of P84 nanofibers, polyetherimide nanofibers, polyvinylidene fluoride and its copolymer nanofibers, polyvinylidene fluoride-hexafluoropropylene nanofibers, polytetrafluoroethylene nanofibers, polyphosphazene nanofibers, polyacrylonitrile nanofibers, polyimide nanofibers, polyester nanofibers, cellulose nanofibers, polyetheretherketone nanofibers, polyarylether nanofibers, polyamide nanofibers, and polybenzimidazole nanofibers; Preferably, the surface-modified high temperature resistant polymer nanofibers include at least one of inorganic surface-modified high temperature resistant polymer nanofibers, high temperature resistant polymer nanofibers having polar groups after surface treatment, or high temperature resistant polymer nanofibers surface-coated with a functionalized polymer layer containing polar groups.
10. the inorganic particles in the coating include at least one of ceramic, metal oxide, metal hydroxide, metal carbonate, silicate, kaolin, talc, mineral, and glass; preferably at least one of boehmite, alumina, silica, barium titanate, titanium dioxide, zinc oxide, magnesium oxide, magnesium hydroxide, zirconia, or an oxide solid electrolyte; Preferably, the oxide solid electrolyte comprises at least one of a perovskite type, a NASICON type, a LISICON type, a garnet type, and a LiPON type electrolyte; The coated modified composite separator according to claim 5, characterized in that the inorganic particles preferably have an average particle size of 10 nm to 5 μm, preferably 11 nm to 4.9 μm, most preferably 15 nm to 4.5 μm.
11. the coating further comprises at least one of a binder, a surfactant, a dispersant, a wetting agent, and an antifoaming agent; Preferably, the amount of binder is from 0.3 to 10.5 parts by weight, preferably from 0.5 to 12.5 parts by weight, more preferably from 0.6 to 12 parts by weight, more preferably from 1.0 to 9 parts by weight; and / or and / or the amount of surfactant is from 0.05 to 7 parts by weight, preferably from 0.1 to 5 parts by weight, more preferably from 0.2 to 4.9 parts by weight, more preferably from 0.4 to 4.7 parts by weight; and / or and / or the amount of dispersant is from 0.05 to 9 parts by weight, preferably from 0.1 to 7 parts by weight, more preferably from 0.2 to 6.9 parts by weight, more preferably from 0.4 to 6.4 parts by weight; and / or and / or the amount of wetting agent is from 0.02 to 7 parts by weight, preferably from 0.05 to 5 parts by weight, more preferably from 0.06 to 4.9 parts by weight, more preferably from 0.09 to 4.7 parts by weight; and / or 6. The coated modified composite separator of claim 5, wherein the amount of the antifoaming agent is 0.04-4 parts by weight, preferably 0.1-4 parts by weight, more preferably 0.2-3.9 parts by weight, more preferably 0.4-3.5 parts by weight.
12. The following steps: (1) The following: b2.1 high temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles formulating a coating slurry comprising at least two of: (2) Applying the coating slurry to either one or both sides of the base membrane.
2. The method of claim 1, comprising:
13. the coating slurry further comprises a slurry solvent, and the slurry solvent is one of an aqueous solvent or an organic solvent; Preferably, the aqueous solvent comprises pure water or a mixed solution of pure water and at least one of ethanol, ethylene glycol, glycerol, isopropyl alcohol, propylene glycol, butanol, and acetic acid; The method according to claim 12, wherein the organic solvent preferably comprises at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethylsulfoxide, acetone, ethanol, isopropanol, ethylene carbonate, and dimethyl carbonate.
14. 13. The method of claim 12, wherein the coating method comprises at least one of electrostatic spraying, blade coating, rotary spraying, extrusion coating, transfer coating, dip coating, wire rod coating, gravure or microgravure coating.
15. 13. The method of claim 12, wherein the coating slurry comprises high temperature resistant polymer microspheres and high temperature resistant polymer nanofibers, the high temperature resistant polymer is polyimide, and the method comprises the steps of: A: preparing a polyamic acid solution with an intrinsic viscosity controlled at 0.01-1 dl / g by low-temperature condensation polymerization using dianhydride and diamine as monomers in an aprotic polar solvent; and, if necessary, adjusting spinning parameters to prepare a polyamic acid material with a composite morphology of nanofibers / microspheres by using a template method, a spray-drying technique, an electrospinning technique, a blow-spinning technique, or a blow-assisted electrospinning; B: subjecting the polyamic acid material produced in step A to high-temperature heat treatment and thermally imidizing the polyamic acid material into a polyimide material; C: Formulating the coating slurry: dispersing the polyimide material prepared in step B in the dispersion and stirring uniformly; adding the binder into the polyimide dispersion and stirring uniformly at a stirring speed of 500-30000 rpm; D: uniformly applying the coating slurry obtained in step C onto the surface of the base film; E: Drying the composite separator obtained by the treatment of step D, in which the drying temperature is 50 to 100°C and the drying time is 0.1 minutes to 12 hours. A manufacturing method comprising:
16. For the polyamic acid solution used in step A, the dianhydride is one or a mixture of two or more of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (α-BPDA), 4,4'-diphenyl ether dianhydride (ODPA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), hexafluoro dianhydride (6FDA), bisphenol A diether dianhydride (BPADA), 3,3,4,4-diphenylsulfonetetracarboxylic dianhydride (DSDA), and the diamine is 4,4'-diaminodiphenyl ether (ODA), p-phenylenediamine (p-PDA), 3,4'-diaminodiphenyl ether (DSDA ... p-phenylenediamine (p-PDA), p-phenylenediamine (p-PDA), p-phenylenediamine (p-PDA), p-phenylenediamine (p-PDA), p-phenylenediamine (p-PDA), p-phenylenediamine (p-PDA), p-phenylenediamine (p-PDA), p-phenylenediamine (p-PDA), p-phenylenediamine ( diphenylmethane (3,4'-MDA), 4,4'-diaminodiphenylmethane (4,4'-MDA), 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB), 1,3-bis(4-aminophenoxy)benzene (1,3,4-APB), 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether (6FODA), 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), or a mixture of two or more thereof; or is prepared by blending at least two polyamic acid solutions; the solids content of the polyamic acid solution is 5-40 wt %; and / or the thermal imidization process used in step B has a maximum temperature of 250-450° C. and a residence time of 0.1-30 minutes; and / or the binder in step C is one or more of an aqueous PVDF emulsion, polyvinyl alcohol, polyethylene oxide, an acrylic water-soluble adhesive, styrene-butadiene rubber, sodium carboxymethyl cellulose, and polyvinylpyrrolidone; the parts by weight of each component of the coating slurry are as follows: 1-3 parts binder, 89-52 parts solvent, and 10-45 parts polyimide; the dispersion is water; and / or 16. The method of claim 15, wherein in step D, the polyolefin separator is coated on one or both sides with the polyimide, and the coating method is one of electrostatic spraying, blade coating, extrusion coating, wire rod coating, transfer coating, dip coating, gravure or microgravure coating.
17. 13. The method of claim 12, wherein the coating slurry comprises high temperature resistant polymeric microspheres, or high temperature resistant polymeric microspheres and inorganic particles, the method comprising the steps of: (1) formulating a mixed coating slurry containing high temperature resistant polymeric microspheres or high temperature resistant polymeric microspheres and inorganic particles; (2) Applying the coating slurry to one or both sides of the base membrane. A manufacturing method comprising the steps of:
18. The solids content of the coating slurry is 2-71.4 wt %, preferably 4-70 wt %, more preferably 10-62 wt %; The method according to claim 17, characterized in that the viscosity of the coating slurry is from 20 to 7000 cP, preferably from 100 to 6000 cP, more preferably from 150 to 5500 cP.
19. 13. The method of claim 12, wherein the coating slurry comprises high temperature resistant polymer nanofibers and inorganic particles, and the method comprises the steps of: (1) formulating a coating slurry containing high temperature resistant polymer nanofibers and inorganic particles; (2) Applying the coating slurry to one or both sides of the base membrane. A manufacturing method comprising the steps of:
20. 20. The method of claim 19, wherein the coating slurry comprises the following components in parts by weight: 0.4 to 65 parts of high temperature resistant polymer nanofibers, 35 to 99.6 parts of inorganic particles, and 100 to 5000 parts of slurry solvent; the sum of the parts by weight of the high temperature resistant polymer nanofibers and inorganic particles is 100.
21. The solids content of the coating slurry is 2-50 wt %, preferably 6-48 wt %, more preferably 10-43 wt %; and / or The method according to claim 19, wherein the viscosity of the coating slurry is 50 to 4000 cP, preferably 100 to 3500 cP, more preferably 200 to 3000 cP.
22. The coating slurry further comprises an additive selected from at least one of a binder, a surfactant, a dispersant, a wetting agent, and a defoamer; Preferably, the amount of slurry solvent is from 100 to 5000 parts by weight, preferably from 120 to 4000 parts by weight, most preferably from 150 to 2900 parts by weight; and / or the amount of binder is from 0.5 to 12.5 parts by weight, preferably from 0.6 to 12 parts by weight, more preferably from 1.0 to 9 parts by weight; and / or The amount of surfactant is from 0.1 to 5 parts by weight, preferably from 0.2 to 4.9 parts by weight, more preferably from 0.4 to 4.7 parts by weight; and / or the amount of dispersant is from 0.1 to 7 parts by weight, preferably from 0.2 to 6.9 parts by weight, more preferably from 0.4 to 6.4 parts by weight; and / or the amount of wetting agent is from 0.05 to 5 parts by weight, preferably from 0.06 to 4.9 parts by weight, more preferably from 0.09 to 4.7 parts by weight; and / or The process according to claim 12, wherein the amount of the antifoaming agent is 0.1 to 4 parts by weight, preferably 0.2 to 3.9 parts by weight, more preferably 0.4 to 3.5 parts by weight.
23. a slurry solvent and: b2.1 high temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles and a coating slurry comprising at least two of the above.
24. The coating slurry according to claim 23, characterized in that the coating slurry contains high temperature resistant polymer nanofibers, inorganic particles, and a slurry solvent, the coating slurry comprises 0.4 to 65 parts by weight of high temperature resistant polymer nanofibers and 35 to 99.6 parts by weight of inorganic particles, and the sum of the parts by weight of the high temperature resistant polymer nanofibers and the inorganic particles is 100.
25. The coating slurry according to claim 23, characterized in that the coating slurry comprises high temperature resistant polymer microspheres, inorganic particles and a slurry solvent, and the weight ratio of the high temperature resistant polymer microspheres to the inorganic particles is 0.1-99.9:99.9-0.1, preferably 1-99.9:99-0.1, more preferably 5-99.9:95-0.1, and most preferably 30-99.9:70-0.
1.
26. 24. The coating slurry of claim 23, wherein the coating slurry contains high temperature resistant polymer nanofibers, high temperature resistant polymer microspheres, and a slurry solvent, the high temperature resistant polymer is a polyimide, and the weight parts of each component of the coating slurry are 1-3 parts binder, 89-52 parts solvent, and 10-45 parts polyimide.
27. The solids content of the coating slurry is 2-50 wt %, preferably 6-48 wt %, more preferably 10-43 wt %; and / or The coating slurry according to any one of claims 23 to 26, wherein the viscosity of the coating slurry is from 50 to 4000 cP, preferably from 100 to 3500 cP, more preferably from 200 to 3000 cP.
28. the slurry solvent is one of an aqueous solvent or an organic solvent; Preferably, the aqueous solvent comprises pure water or a mixed solution of water and at least one of ethanol, ethylene glycol, glycerol, isopropyl alcohol, and butanol; The coating slurry according to any one of claims 23 to 26, wherein the organic solvent comprises at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethylsulfoxide, acetone, ethanol, isopropanol, ethylene carbonate, and dimethyl carbonate.
29. the coating slurry further comprises an additive selected from at least one of a binder, a surfactant, a dispersant, a wetting agent, and an antifoaming agent; the amount of slurry solvent is from 100 to 5000 parts by weight, preferably from 120 to 4000 parts by weight, most preferably from 150 to 2900 parts by weight; and / or the amount of binder is from 0.5 to 12.5 parts by weight, preferably from 0.6 to 12 parts by weight, more preferably from 1.0 to 9 parts by weight; and / or The amount of surfactant is from 0.1 to 5 parts by weight, preferably from 0.2 to 4.9 parts by weight, more preferably from 0.4 to 4.7 parts by weight; and / or the amount of dispersant is from 0.1 to 7 parts by weight, preferably from 0.2 to 6.9 parts by weight, more preferably from 0.4 to 6.4 parts by weight; and / or the amount of wetting agent is from 0.05 to 5 parts by weight, preferably from 0.06 to 4.9 parts by weight, more preferably from 0.09 to 4.7 parts by weight; and / or 27. Coating slurry according to any one of claims 23 to 26, wherein the amount of antifoaming agent is from 0.1 to 4 parts by weight, preferably from 0.2 to 3.9 parts by weight, more preferably from 0.4 to 3.5 parts by weight.
30. A lithium ion battery comprising a positive electrode, a negative electrode, an electrolyte, and a separator, the separator being the coated modified composite separator of claim 1 or the coated modified composite separator produced by the method of claim 12.
31. The coated modified composite separator includes a base membrane and a coating, a coating covers either one or both sides of the base membrane; Coating: b2.1 high temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles 1. A coated modified composite separator comprising:
32. The following steps: (1) b2.1 High temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles; formulating a coating slurry containing (2) Coating one or both sides of the base membrane with a coating slurry.
32. The method of claim 31 , comprising:
33. a slurry solvent, as well as: b2.1 high temperature resistant polymer microspheres, b2.2 High temperature resistant polymer nanofibers, and b2.3 Inorganic particles 1. A coating slurry comprising: