Secondary battery including sealing tape

JP2024542116A5Active Publication Date: 2024-12-06LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024526704
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-07-19
Filing Date
2023-07-19
Publication Date
2024-12-06
Estimated Expiration
2043-07-19

AI Technical Summary

Technical Problem

The existing secondary batteries with jelly-roll type electrode assemblies face issues of increased resistance due to the sealing tape inducing the electrode assembly to unravel after electrolyte injection, leading to poor contact between the negative electrode and the can, which is exacerbated by the limited space within the battery can.

Method used

A sealing tape with an adhesive layer that expands upon contact with the electrolyte is applied to the outer peripheral surface of the electrode assembly, allowing it to detach and increase the contact area between the negative electrode and the can, thereby reducing resistance.

Benefits of technology

The expanded adhesive layer effectively increases the contact area between the negative electrode and the can, reducing battery resistance and ensuring stable electrode assembly insertion, while maintaining structural integrity and preventing disconnection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present specification relates to a secondary battery including a sealing tape.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a secondary battery including a sealing tape.

[0002] This application claims the benefit of the filing date of Korean Patent Application No. 10-2022-0088822 filed with the Korean Intellectual Property Office on July 19, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference. [Background technology]

[0003] In recent years, the demand for portable electronic products such as notebook computers, video cameras, and mobile phones has increased dramatically, and the development of electric vehicles, energy storage batteries, robots, satellites, and the like has progressed in earnest. As a result, much research has been conducted on secondary batteries to be used as the driving power source for these products.

[0004] Such secondary batteries include, for example, nickel-cadmium batteries, nickel-metal hydride batteries, nickel-zinc batteries, lithium secondary batteries, etc. Among these, lithium secondary batteries are widely used in the field of cutting-edge electronic devices due to the advantages that they can be freely charged and discharged since they hardly have a memory effect compared to nickel-based secondary batteries, have a very low self-discharge rate, a high operating voltage, and a high energy density per unit weight.

[0005] In general, a lithium secondary battery is constructed by incorporating an electrode assembly, which is made up of a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, in a laminated or wound structure and then injecting or impregnating an electrolyte into the case.

[0006] Electrode assemblies with a positive electrode / separator / negative electrode structure that constitute secondary batteries are roughly classified into a jelly roll type (wound type) and a stack type (laminated type) according to their structure. The jelly roll type has a structure in which a long sheet-like positive electrode and negative electrode coated with an active material are wound with a separator interposed between them, while the stack type has a structure in which a large number of positive electrodes and negative electrodes of a given size are stacked in sequence with a separator interposed between them. Among these, the jelly roll type electrode assembly has the advantages of being easy to manufacture, having a high energy density per weight, and being structurally stable.

[0007] Since cylindrical batteries including such jelly-roll type electrode assemblies are standardized, there is a demand for maximizing performance within a limited space. Summary of the Invention [Problem to be solved by the invention]

[0008] In this specification, in a secondary battery including a jelly-roll type electrode assembly having a negative electrode provided on its outer peripheral surface, a sealing tape that absorbs an electrolyte and then expands is attached to the outer peripheral surface of the electrode assembly, thereby inducing unraveling of the electrode assembly from the sealing tape after the electrolyte is injected into a can, thereby increasing the contact area between the negative electrode located on the outer peripheral surface of the electrode assembly and the inside of the can, thereby providing a secondary battery with low battery resistance. [Means for solving the problem]

[0009] One embodiment of the present invention provides a secondary battery including an electrode assembly having a structure in which a positive electrode, a negative electrode, and a separator are wound; an electrolyte; and a can containing the electrode assembly and the electrolyte, wherein the negative electrode is located on an outer circumferential surface of the electrode assembly, and a sealing tape is provided on the outer circumferential surface of the electrode assembly, the sealing tape includes a substrate and an adhesive layer provided on one surface of the substrate, and the adhesive layer has an expansion property in response to the electrolyte. Effect of the Invention

[0010] In the present invention, a sealing tape that expands in response to an electrolyte is attached to the negative electrode located on the outer peripheral surface of the electrode assembly. When electrolyte is injected into the battery can, the adhesive layer of the sealing tape absorbs the electrolyte and expands, causing the sealing tape to detach from the electrode assembly. As a result, the wound-up electrode assembly is partially unwound, increasing the contact area between the negative electrode on the outer peripheral surface of the electrode assembly and the inside of the battery can, thereby providing low resistance characteristics for the battery. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a diagram illustrating a secondary battery according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram illustrating a secondary battery according to an embodiment of the present invention. [Diagram 3] 1 shows CT images of batteries produced in Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present specification will be explained in further detail below.

[0013] In this specification, when a part is said to "comprise" a certain component, this means that it may further include other components, rather than excluding other components, unless specifically stated to the contrary.

[0014] In this specification, when a member is said to be located "on" another member, this includes not only the case where the member is in contact with the other member, but also the case where another member exists between the two members.

[0015] In this specification, when a certain portion is said to be connected to another portion, this includes not only the case where the portion is directly connected to another portion, but also the case where the portion is indirectly connected via another element between the portions.

[0016] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the embodiments of the present invention may be modified in various ways, and the scope of the present invention is not limited to the embodiments described below. However, in describing the operation principle of the preferred embodiments of the present invention in detail, if it is determined that a detailed description of related known functions or configurations may unnecessarily obscure the gist of the present invention, the detailed description will be omitted. Furthermore, the same reference numerals are used throughout the drawings to refer to parts having similar functions and actions.

[0017] One embodiment of the present invention provides a secondary battery including: an electrode assembly having a structure in which a positive electrode, a negative electrode, and a separator are wound; an electrolyte; and a can in which the electrode assembly and the electrolyte are stored, the negative electrode being located on an outer circumferential surface of the electrode assembly, a sealing tape being provided on the outer circumferential surface of the electrode assembly, the sealing tape including a substrate and an adhesive layer provided on one surface of the substrate, and the adhesive layer having an expansion property in response to the electrolyte.

[0018] In general, a cylindrical battery including a jelly-roll type electrode assembly has a separator positioned on the outer periphery of the electrode assembly. Since the electrode assembly is standardized, it is required to maximize performance within a limited space, and generally, the performance of the secondary battery is improved by maximizing capacity and reducing resistance. In this case, the content of the electrode inserted must be increased to maximize the capacity of the battery, and the number of negative electrode tabs must be increased to reduce resistance. However, it is difficult to infinitely increase the number of negative electrode tabs in the internal space of the battery, and the increase in the number of tabs reduces weldability with the battery can. In addition, when the content of the electrode is increased to maximize the capacity of the battery, the internal space of the battery becomes small, and it is not easy to add electrode tabs.

[0019] To address this issue, a method was developed to reduce resistance by positioning the negative electrode on the outer periphery of the electrode assembly to increase the contact area between the negative electrode and the inside of the can. In this case, in order to maintain stable contact between the negative electrode and the inside of the can, the internal gap between the negative electrode and the inside of the can must be minimized.

[0020] However, before the jelly-roll type electrode assembly is inserted into the can, a seal tape must be attached to the outer periphery of the electrode assembly to prevent the electrode assembly from coming loose, and a certain amount of internal gap must exist between the can and the electrode assembly for smooth insertion. If the gap is insufficient, the appearance of the electrode assembly may be damaged during insertion, and problems such as poor insertion may occur.

[0021] In this case, if existing sealing tape is used, the electrode assembly is tightly fixed, and stress caused by the contraction / expansion of the electrodes due to the charge / discharge of the secondary battery cannot be relieved, which can cause problems such as electrode breakage, cracks, and metal elution.

[0022] The present invention is characterized in that a negative electrode is located on the outer peripheral surface of an electrode assembly, and a sealing tape that has an expansion property in response to an electrolyte and absorbs and expands in the electrolyte is used on the outer peripheral surface of the electrode assembly. When the electrode assembly is inserted into a can and the electrolyte is poured in, the adhesive layer of the sealing tape absorbs the electrolyte, loses its adhesiveness, and expands, thereby inducing unraveling of the electrode assembly.

[0023] Therefore, the electrode assembly that was wound is loosened due to the removal of the sealing tape and the contraction / expansion of the electrodes, and the contact area between the negative electrode located on the outer surface of the electrode assembly and the can becomes larger, which has the effect of lowering the resistance of the battery.

[0024] In addition, before the electrode assembly is inserted into the can, the sealing tape stably fixes the jelly roll, thereby preventing the electrode assembly from coming undone and facilitating the insertion of the electrode assembly.

[0025] In one embodiment of the present invention, the sealing tape includes a substrate; and an adhesive layer provided on one surface of the substrate.

[0026] The adhesive layer included in the sealing tape will be specifically described below.

[0027] In one embodiment of the present invention, the adhesive layer has swelling properties due to the electrolyte. Having swelling properties due to the electrolyte means that the adhesive layer is deformed in structure by the electrolyte, for example, it absorbs the electrolyte after contacting with the electrolyte and expands. That is, the adhesive layer may be in a state in which it absorbs the electrolyte and expands.

[0028] The sealing tape can absorb the electrolyte and expand to form a three-dimensional structure. Specifically, the adhesive layer can absorb the electrolyte and expand to form a three-dimensional structure. For example, the adhesive layer can expand in the thickness direction and / or length direction of the adhesive layer when in contact with the electrolyte, thereby forming a three-dimensional structure. In the above, the "three-dimensional structure" of the sealing tape is formed by the action of the expansion force of the adhesive layer of the sealing tape in contact with the electrolyte and the peeling force with the substrate, and can be a concept including all structures that can allow the adhesive layer to be detached from the electrode assembly.

[0029] According to one example, the three-dimensional structure may include a plurality of shapes protruding in a direction perpendicular to the length direction of the adhesive layer. In the above, the "length direction" may mean a direction perpendicular to the thickness direction of the adhesive layer when the adhesive layer is held flat. In addition, the "vertical" or "horizontal" means substantially vertical or horizontal within a range that does not impair the intended effect, and may include an error of, for example, about ±10 degrees, ±5 degrees, or ±3 degrees.

[0030] In one embodiment of the present invention, the adhesive layer may have a center line average roughness value of 100 μm to 250 μm, measured 24 hours after contact with the electrolyte solution.

[0031] Specifically, the center line average roughness (Ra) after contact with the electrolyte may be 150 μm to 240 μm, or 155 μm to 230 μm. The center line average roughness (Ra) may be a value measured on the surface of the adhesive layer 24 hours after contact with the electrolyte.

[0032] In the present invention, when the center line average roughness of the three-dimensional structure formed by the adhesive layer is adjusted within the above-mentioned range, the sealing tape can be efficiently detached from the outer circumferential surface of the electrode assembly.

[0033] The "center line average roughness" means, for example, a value calculated from the following formula 1 in micrometers when a cross section of an adhesive layer forming a three-dimensional structure is photographed, the cross section of the three-dimensional structure is mathematically remodeled through the photograph to obtain a roughness curve, a reference length L is extracted from the roughness curve in the direction of the mean line, the mean line direction is the x-axis, and the height direction is the y-axis, and the roughness curve is expressed as y=f(x).

[0034]

number

[0035] The center line average roughness can be measured according to the standard of ASTM D4417, or can be determined as defined in JIS B0031 or JIS B0601.

[0036] In one embodiment of the present invention, the pressure-sensitive adhesive layer may include a cured product of a pressure-sensitive adhesive composition, or may include a polymer contained in the pressure-sensitive adhesive composition in a crosslinked form.

[0037] In one embodiment of the present invention, the pressure-sensitive adhesive composition may include a polymer including polymerization units derived from a (meth)acrylic acid ester monomer, a monomer having a polar functional group, and a crosslinkable monomer containing a crosslinkable functional group.

[0038] In one example, in the case of a secondary battery manufactured by attaching a sealing tape including an adhesive layer formed from the adhesive composition to an electrode assembly via the adhesive layer and inserting the electrode assembly into a battery can, the adhesive layer deforms, for example, swells or expands due to the polar functional groups present in the adhesive layer when it comes into contact with an electrolyte injected into the secondary battery. In this case, the sealing tape forms a three-dimensional structure, and the surface of the adhesive layer has a surface roughness value within a specific range, thereby reducing the adhesive force or peel force between the electrode assembly and the adhesive layer, and the adhesive layer may detach from the electrode assembly.

[0039] The pressure-sensitive adhesive composition includes a polymer having a polymerization unit. According to one example, the polymer may include, in a polymerized form, a (meth)acrylic acid ester monomer, a monomer having a polar functional group, and a crosslinkable monomer having a crosslinkable functional group.

[0040] As the (meth)acrylic acid ester monomer contained in the polymerized unit of the polymer, for example, an alkyl (meth)acrylate can be used, and taking into consideration the cohesive force, glass transition temperature, or adhesiveness of the adhesive, an alkyl (meth)acrylate having an alkyl group having 1 to 14 carbon atoms can be used. Examples of such monomers include one or more of methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, sec-butyl (meth)acrylate, pentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate, and tetradecyl (meth)acrylate, but are not limited thereto.

[0041] In the above, "(meth)acrylate" means either acrylate or methacrylate, and similarly other terms in which "(meth)" is used.

[0042] The monomer having a polar functional group is a monomer having excellent affinity with an electrolyte, and is included in the polymer of the adhesive composition as a polymerization unit so that an adhesive layer manufactured from the adhesive composition deforms, for example, swells, when it comes into contact with an electrolyte, thereby reducing the adhesive force or peeling force between the electrode assembly and the adhesive layer. In addition, in the present application, a monomer having a specific structure is used as the monomer having a polar functional group, so that the sealing tape can form a three-dimensional structure having a specific surface roughness when it comes into contact with an electrolyte, and thus the sealing tape can be detached from the electrode assembly with excellent efficiency, thereby inducing isotropic volume expansion and contraction of the electrode assembly, and efficiently preventing disconnection of the electrode.

[0043] In one embodiment of the present invention, the monomer having a polar functional group is represented by the following chemical formula 1.

[0044] [ka]

[0045] In the above formula 1, R1 represents hydrogen or an alkyl group having 1 to 12 carbon atoms; R2 represents an alkylene group having 1 to 6 carbon atoms; R3 represents hydrogen, an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 24 carbon atoms, or an arylalkyl group having 6 to 48 carbon atoms; n is 0 or greater.

[0046] In the above Chemical Formula 1, the alkyl group having 1 to 12 carbon atoms may be a straight-chain or branched-chain alkyl group.

[0047] In the above Chemical Formula 1, R1 is hydrogen or an alkyl group having 1 to 12 carbon atoms, 1 to 8 carbon atoms or 1 to 4 carbon atoms, and examples thereof include hydrogen, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and preferably hydrogen or a methyl group, but is not limited thereto.

[0048] In addition, in the above Chemical Formula 1, R2 is an alkylene group having 1 to 6, 1 to 4, or 1 to 2 carbon atoms, and may be, for example, ethylene or propylene, but is not limited thereto.

[0049] R3 represents hydrogen, an alkyl group having 1 to 12, 1 to 8, 1 to 6, or 1 to 4 carbon atoms; an aryl group having 6 to 24, 6 to 20, 6 to 18, or 6 to 12 carbon atoms; or an arylalkyl group having 6 to 48, 6 to 30, 6 to 24, or 6 to 18 carbon atoms. Examples of R3 include hydrogen, a methyl group, an ethyl group, a propyl group, a phenyl group, a naphthalic group, a butylphenol group, a pentylphenol group, a hexylphenol group, a heptylphenol group, an octylphenol group, and a nonylphenol group, but are not limited to these.

[0050] Moreover, the n may be 0 or more, for example, 1 or more, and preferably 2 or more.

[0051] In one embodiment of the present invention, the monomer represented by Chemical Formula 1 may be a monomer represented by Chemical Formula 2 below.

[0052] [ka]

[0053] In the above formula 2, R1 and R3 are as defined above; p+q is equal to or greater than 1, p is a number from 0 to 100, and q is a number from 0 to 100.

[0054] Examples of the monomer represented by Chemical Formula 1 or Chemical Formula 2 include methoxyethyl (meth)acrylate, methoxyethoxyethyl (meth)acrylate, ethoxyethoxyethyl (meth)acrylate, ethoxytriethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol methyl ether (meth)acrylate, ethoxylated nonylphenol (meth)acrylate, propoxylated nonylphenol (meth)acrylate, ethoxylated phenol (meth)acrylate, and polypropylene glycol (meth)acrylate. Preferred examples include methoxyethyl (meth)acrylate, methoxyethoxyethyl (meth)acrylate, ethoxyethoxyethyl (meth)acrylate, ethoxytriethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, and polyethylene glycol methyl ether (meth)acrylate, but are not limited thereto.

[0055] The monomer represented by Formula 1 or Formula 2 contains at least one oxygen atom, and the monomer has a high polarity due to the high electronegativity of the oxygen atom, so that the adhesive layer containing the monomer has a high affinity with a polar electrolyte solution and can expand when contacted with the electrolyte solution. Meanwhile, the term "electrolyte solution" in the above may refer to an ion-conducting medium used in, for example, a secondary battery. For example, the electrolyte solution may be an electrolyte solution that is a liquid medium, but is not limited thereto. In the present specification, the electrolyte solution may be referred to as an electrolyte.

[0056] The polymer may contain 30 to 300 parts by weight, for example, 40 to 280 parts by weight or 44 to 250 parts by weight of the monomer represented by Formula 1, based on 100 parts by weight of the (meth)acrylic acid ester monomer, in a polymerized form, but is not limited thereto. Also, the monomer represented by Formula 1 may be contained in an amount of 25 to 80 parts by weight, for example, 25 to 75 parts by weight or 30 to 70 parts by weight, based on 100 parts by weight of the total monomers contained in the polymer as polymerization units. If the monomer represented by Formula 1 is contained in too little amount, it is difficult for the adhesive layer to expand sufficiently to be detached from the electrode assembly when contacting the electrolyte, and if it is contained in too much amount, gelation occurs excessively during the polymerization reaction of the polymer, making it difficult to realize the adhesive properties of the adhesive. In consideration of this, the content of the monomer having a polar functional group may be adjusted within the above range. In this specification, unless otherwise specified, "parts by weight" means relative "weight ratio".

[0057] The crosslinkable monomer having a crosslinkable functional group is a monomer that can be copolymerized with the (meth)acrylic acid ester monomer or other monomers contained in the polymer, and can provide a crosslinking point in the main chain of the polymer that can react with a multifunctional crosslinking agent after copolymerization. The crosslinkable functional group may be a hydroxyl group, a carboxyl group, an isocyanate group, a glycidyl group, an amide group, or the like, and may be a photocrosslinkable functional group such as an acryloyl group or a methacryloyl group in some cases. In the case of a photocrosslinkable functional group, it can be introduced by reacting a compound having a photocrosslinkable functional group with the crosslinkable functional group provided by the copolymerizable monomer. The crosslinkable monomer containing a hydroxyl group may be, for example, a monomer containing a hydroxyl group such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxyethylene glycol (meth)acrylate, glycerol (meth)acrylate, or hydroxypropylene glycol (meth)acrylate, or a monomer containing one or more of these may be used, but is not limited thereto. The carboxyl group-containing monomer may be, for example, (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, etc., but is not limited thereto. In addition, the crosslinkable monomer containing a glycidyl group may be, for example, glycidyl (meth)acrylate, epoxyalkyl (meth)acrylate, or epoxycycloalkylalkyl (meth)acrylate such as epoxycyclohexylmethyl (meth)acrylate, but is not limited thereto.Examples of the crosslinkable monomer containing an isocyanate group include, but are not limited to, 2-isocyanate ethyl (meth)acrylate, 1,1-bis(acryloyloxymethyl)ethyl isocyanate, (meth)acryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, methacryloyl isocyanate or allyl isocyanate; an acryloyl monoisocyanate compound obtained by reacting a diisocyanate compound or a polyisocyanate compound with 2-hydroxyethyl (meth)acrylate; and an acryloyl monoisocyanate compound obtained by reacting a diisocyanate compound or a polyisocyanate compound, a polyol compound and 2-hydroxyethyl (meth)acrylate. Examples of the amide group-containing monomer include, but are not limited to, (meth)acrylamide, diethylacrylamide, N-vinylpyrrolidone, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N'-methylenebisacrylamide, N,N-dimethylaminopropylacrylamide, N,N-dimethylaminopropylmethacrylamide, and diacetone(meth)acrylamide. Examples of the amino group-containing monomer include, but are not limited to, aminoethyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, and N,N-dimethylaminopropyl(meth)acrylate. Examples of the alkoxysilyl group-containing monomer include, but are not limited to, trimethoxysilylpropyl(meth)acrylate or allyloxyethyl(meth)acrylate.

[0058] The polymer may contain, in a polymerized form, 0.1 to 10 parts by weight, for example, 2.5 to 10 parts by weight, 2.9 to 9 parts by weight, or 2.9 to 8 parts by weight of the crosslinkable monomer relative to 100 parts by weight of the (meth)acrylic acid ester monomer, but is not limited thereto. Also, the crosslinkable monomer may be contained in an amount of 0.1 to 5 parts by weight, for example, 0.5 to 3 parts by weight, or 1 to 2 parts by weight, relative to 100 parts by weight of the total monomers contained in the polymerized units in the polymer. If the crosslinkable monomer is contained in too much amount, the peel strength may be too low, which may cause a problem that the adhesive layer is difficult to fix the electrode assembly, and if the crosslinkable monomer is contained in too little amount, the adhesive layer is difficult to expand sufficiently to be detached from the electrode assembly when it comes into contact with the electrolyte. Therefore, taking these points into consideration, the content of the crosslinkable monomer may be adjusted within the above-mentioned range.

[0059] In one embodiment of the present invention, the adhesive layer may include a cured product of an adhesive composition including a polymer having polymerization units derived from a (meth)acrylic acid ester monomer, a monomer represented by Chemical Formula 1, and a crosslinkable monomer containing a crosslinkable functional group.

[0060] The polymer may further include other functional comonomers in a polymerized form as necessary, and examples of such comonomers include the monomer represented by the following Formula 3:

[0061] [ka]

[0062] In the above formula 3, R6 to R8 each independently represent a hydrogen atom or an alkyl group, and R9 represents a cyano group; a phenyl group substituted or unsubstituted with an alkyl group; an acetyloxy group; or a COR 10 where R 10 represents an amino group or a glycidyloxy group which may be unsubstituted or substituted with an alkyl group or an alkoxyalkyl group.

[0063] R6 to R 10In the definition, the alkyl group or alkoxy group means an alkyl group or alkoxy group having 1 to 8 carbon atoms, and is preferably a methyl group, an ethyl group, a methoxy group, an ethoxy group, a propoxy group or a butoxy group.

[0064] Specific examples of the monomer of Formula 3 include nitrogen-containing monomers such as (meth)acrylamide, N-butoxymethyl(meth)acrylamide, N-methyl(meth)acrylamide, (meth)acrylonitrile, N-vinylpyrrolidone, and N-vinylcaprolactam; styrene-based monomers such as styrene and methylstyrene; glycidyl(meth)acrylate; caprolactone; and vinyl esters of carboxylic acids such as vinyl acetate, but are not limited thereto.

[0065] The polymer may be included in the composition in a crosslinked form with a multifunctional crosslinking agent. When the polymer is included in a crosslinked form, the adhesive layer prepared from the composition may have a property of expanding or swelling when contacted with an electrolyte, thereby preventing disconnection of the electrode. In addition, since the polymer is included in a crosslinked form, the adhesive layer prepared from the adhesive composition may have an appropriate cohesive force.

[0066] The type of the polyfunctional crosslinking agent crosslinking the polymer is not particularly limited, and an appropriate crosslinking agent can be selected according to the type of crosslinkable functional group present in the polymer from known crosslinking agents such as isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, metal chelate crosslinking agents, photocrosslinking agents, etc. Examples of the isocyanate crosslinking agent include diisocyanates such as tolylene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isoboron diisocyanate, tetramethylxylene diisocyanate, and naphthalene diisocyanate, and reaction products of the diisocyanates with polyols, and trimethylolpropane can be used as the polyol. Examples of the epoxy crosslinking agent that can be used include ethylene glycol diglycidyl ether, triglycidyl ether, trimethylolpropane triglycidyl ether, N,N,N',N'-tetraglycidylethylenediamine, and glycerin diglycidyl ether. Examples of the aziridine crosslinking agent include N,N'-toluene-2,4-bis(1-aziridinecarboxamide), N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), triethylenemelamine, bisisoprotoyl-1-(2-methylaziridine), and tri-1-aziridinylphosphine oxide. Examples of the metal chelate crosslinking agent include compounds in which a polyvalent metal is coordinated to a compound such as acetylacetone or ethyl acetoacetate. In the above, examples of the polyvalent metal include aluminum, iron, zinc, tin, titanium, antimony, magnesium, and vanadium. Examples of the photocrosslinking agent that can be used include polyfunctional acrylates. In the above, one or more crosslinking agents may be used, taking into consideration the type of crosslinkable functional group contained in the polymer.

[0067] The weight ratio of the multifunctional crosslinking agent in the adhesive composition can be adjusted to a range that can secure the desired peel strength or gel fraction described below. For example, the crosslinking agent can be included in an amount of 0.001 to 10 parts by weight, for example, 0.1 to 5 parts by weight or 0.5 to 4 parts by weight, based on 100 parts by weight of the total composition, but is not limited thereto. If the ratio of the multifunctional crosslinking agent is too low, the cohesive strength of the adhesive layer cannot be adequately secured, and if it is too high, the adhesive properties may be reduced, so an appropriate range can be selected taking this into consideration.

[0068] The polymer contained in the pressure-sensitive adhesive composition can be prepared by subjecting a mixture of the monomers described above to a polymerization process such as solution polymerization, photo polymerization, bulk polymerization, suspension polymerization, or emulsion polymerization.

[0069] The polymer may have a weight average molecular weight (Mw) of about 300,000 to 2.5 million, 400,000 to 2 million, 500,000 to 2 million, 800,000 to 1.8 million, 600,000 to 1.2 million, 700,000 to 1.4 million, or 600,000 to 800,000. In this specification, the weight average molecular weight may mean a converted value relative to standard polystyrene measured by GPC (Gel Preparation Chromatograph), and unless otherwise specified, the molecular weight may mean the weight average molecular weight. If the molecular weight of the polymer is too low, the cohesive force of the adhesive layer may decrease, and if it is too high, the adhesive properties may decrease, so an appropriate molecular weight can be selected in consideration of these points.

[0070] In addition to the above components, the adhesive composition may further include various additives known in this field as necessary. For example, the adhesive composition may further include a tackifier. As the tackifier, for example, a rosin ester-based or styrene-based tackifier can be used, but the tackifier is not limited thereto, and an appropriate type can be selected and used as necessary. The content of the tackifier is also not particularly limited, and can be adjusted in consideration of the peel strength with the electrode assembly. For example, the tackifier may be used in a ratio of 1 to 25 parts by weight with respect to 100 parts by weight of the polymer.

[0071] The pressure-sensitive adhesive composition may further contain additives such as an initiator, such as a thermal initiator or a photoinitiator; an epoxy resin; a curing agent; an ultraviolet stabilizer; an antioxidant; a color-matching agent; a reinforcing agent; a filler; an antifoaming agent; a surfactant; a photopolymerizable compound, such as a multifunctional acrylate; or a plasticizer, within a range that does not affect the intended effect.

[0072] For example, the polymer contained in the pressure-sensitive adhesive composition may be prepared through a photopolymerization method by selecting a suitable photoinitiator that is generally known. The photoinitiator may be, for example, an organic peroxide such as benzoyl peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-triethylcyclohexane, tert-butyl peroxyacetate, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisopropyl carbonate, di-2-ethylhexyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-3-methoxybutyl peroxydicarbonate, di-3,3,5-trimethylhexanoyl peroxide, di-tert-butyl peroxide, lauroyl peroxide, dicumyl peroxide, or methyl ether ketone peroxide; butyl hydroperoxide; the photopolymerization method may be applied by, but is not limited to, hydroperoxides such as ammonium peroxide and cumyl hydroperoxide; oxidizing agents such as hydrogen peroxide, ammonium peroxydisulfate, nitric acid and its salts, perchloric acid and its salts, sulfuric acid and its salts, hypochloric acid and its salts, permanganic acid and its salts, chromic acid and its salts, lead dioxide, manganese dioxide, copper oxide, iron chloride, fluorine, chlorine, bromine, iodine; reducing agents such as sodium borohydride, formaldehyde, acetaldehyde, amines, hydrazine; azo compounds such as azobisisobutyronitrile (hereinafter referred to as AIBN); means of irradiating with heat, light, ultraviolet light, or high-energy wavelengths; electron transfer in an electrolyte;

[0073] The content of the photoinitiator is not particularly limited, but may be 0.01 to 5 parts by weight, for example, 0.01 to 1 part by weight, or 0.01 to 0.5 parts by weight, based on 100 parts by weight of the total monomer mixture.

[0074] The adhesive layer can be formed, for example, by coating a coating liquid containing the polymer and a multifunctional crosslinking agent on the substrate, and inducing a crosslinking reaction between the polymer and the multifunctional crosslinking agent under appropriate conditions.

[0075] The thickness of the adhesive layer is not particularly limited and can be appropriately selected depending on the application, for example, the desired peel strength, etc. The adhesive layer can be formed to have a thickness of, for example, about 2 μm to 100 μm, 3 μm to 50 μm, 4 μm to 25 μm, 4 μm to 15 μm, 4 μm to 10 μm, 4 μm to 9 μm, 4 μm to 7 μm, or 5 μm to 7 μm, but this can be changed depending on the purpose.

[0076] The adhesive layer may be provided on one side of the substrate in a form including a pattern. Specifically, the pattern may be a closed figure pattern, a linear pattern, or a combination of a closed figure pattern and a linear pattern. In one example, the pattern may be a lattice pattern or an S-shaped pattern, but is not limited thereto, and may be applied by adopting a suitable pattern known in the art.

[0077] In addition, the pattern may include, but is not limited to, a wave pattern, a lattice pattern, or a relief embossed pattern, and any suitable pattern known in the art may be adopted and applied.

[0078] The wavy pattern may refer to a pattern formed by wavy curves. In this case, the wavy curves may have convex or concave portions, and the uneven surface included in the adhesive layer may include such a pattern, thereby improving the adhesive strength of the adhesive layer.

[0079] The lattice pattern may refer to a pattern formed by convex portions formed by the intersection of linear concave portions. Alternatively, it may refer to a pattern formed by concave portions formed by the intersection of linear convex portions. In this case, the formed convex portions or concave portions form a lattice, and the shape of each lattice may be any of a square, a rectangle, a parallelogram, and a rhombus. The uneven surface included in the adhesive layer includes such a pattern, thereby improving the adhesion of the adhesive layer.

[0080] The embossed pattern of the relief may be, for example, a pattern in which spherical projections and recesses are protruded in relief.

[0081] As described above, when the adhesive layer is provided (coated) in a patterned form, the contact area with the electrolyte increases, and the diffusion rate of the electrolyte into the adhesive layer can be increased. When the diffusion rate of the electrolyte increases, the adhesive layer absorbs and expands the electrolyte at a higher rate, and the sealing tape detaches from the electrode assembly more quickly. Therefore, the sealing tape detaches immediately after the electrolyte is injected into the battery can, which induces the electrode assembly to break apart, and the contact area between the negative electrode and the inside of the can can be more stably expanded. In addition, the detachment time is shortened, which is advantageous in that mass production quality can be ensured after battery production. However, if the detachment time is delayed and the adhesion of the sealing tape continues, there is a problem that the resistance deviation of the battery increases when checking the mass production quality.

[0082] The sealing tape may be a sealing tape attached to an outer circumferential surface of an electrode assembly in a secondary battery. In addition, in the sealing tape according to an embodiment of the present invention, the initial peel strength of the adhesive layer is not too high, and the sealing tape includes an adhesive layer including a monomer having a polar functional group as described above, so that when the sealing tape comes into contact with an electrolyte in a secondary battery, the adhesive layer absorbs the electrolyte and expands, so that the peel strength of the adhesive layer can be adjusted to a level low enough to be detached from the electrode assembly.

[0083] In one embodiment of the present invention, the sealing tape may have an initial peel strength sufficient to detach from the electrode assembly when it contacts the electrolyte while fixing the electrode assembly. If the initial peel strength of the electrode assembly is too high, the adhesive layer may be difficult to detach from the electrode assembly even after contacting the electrolyte. For example, the adhesive layer may have a peel strength of 370 gf / 25 mm or less, e.g., 350 gf / 25 mm or less, 315 gf / 25 mm or less, or 312 gf / 25 mm or less, measured at a peel speed of 5 mm / sec and a peel angle of 180 degrees against glass at room temperature. The lower limit of the peel strength of the adhesive layer against glass is not particularly limited, and for example, if the adhesive layer has a very low initial peel strength, the adhesive layer will lose its adhesive strength when it contacts the electrolyte, and the sealing tape will detach from the electrode assembly, thereby preventing disconnection of the electrode. However, if the initial peel strength of the adhesive layer is too low, the adhesive layer may come loose before the electrode assembly is housed in a can without coming into contact with the electrolyte, and in consideration of this, the lower limit of the peel strength of the adhesive layer against glass may be adjusted to 5 gf / 25 mm or more, for example, 10 gf / 25 mm or more, 20 gf / 25 mm or more, 30 gf / 25 mm or more, 40 gf / 25 mm or more, 50 gf / 25 mm or more, 60 gf / 25 mm or more, 70 gf / 25 mm or more, 80 gf / 25 mm or more, 85 gf / 25 mm or more, or 88 gf / 25 mm or more. When the adhesive layer has a peel strength in the above range against glass, even if the adhesive layer is attached to the outer peripheral surface of the electrode assembly, it can exhibit an appropriate initial peel strength for detachment when it comes into contact with the electrolyte, and when the sealing tape comes into contact with the electrolyte, a three-dimensional structure having a specific surface roughness can be formed.

[0084] In one embodiment of the present invention, the sealing tape may be detached from the outer peripheral surface of the electrode assembly, i.e., it may not be attached to the outer peripheral surface and may have lost its adhesive force.

[0085] The adhesive strength of the sealing tape after the electrolyte injection is reduced by 80% or more based on the adhesive strength of the sealing tape before the electrolyte injection, specifically, by 90% or more, 95% or more, or 99% or more.

[0086] In one embodiment of the present invention, the adhesive layer of the sealing tape absorbs the electrolyte and expands to form a three-dimensional structure, and the peeling force of the adhesive layer may be adjusted to be low enough to be detached from the electrode assembly, so that the adhesive layer can be detached from the outer peripheral surface of the electrode assembly. According to one example, the sealing tape can be detached from the outer peripheral surface of the electrode assembly after contacting with the electrolyte, and preferably, 50% or more, for example, 60% or more, 70% or more, or 80% or more of the area of ​​the sealing tape attached to the outer peripheral surface of the electrode assembly can be detached.

[0087] The thickness of the sealing tape can be appropriately selected according to the desired peeling force and is not particularly limited. The sealing tape can be formed to have a thickness of, for example, about 10 μm to 100 μm, 15 μm to 75 μm, 20 μm to 45 μm, 15 μm to 40 μm, 20 μm to 40 μm, or 20 μm to 30 μm, but this may be changed according to the purpose. If the thickness of the sealing tape is too thin, the effect of the expansion of the adhesive layer of the sealing tape may not be exhibited easily, and conversely, if the thickness is too thick, the thickness of the electrode assembly increases accordingly, which may cause significant damage to the electrode assembly due to a decrease in processability when inserting it into a battery case, or may cause a decrease in capacity at the same standard size.

[0088] The sealing tape may further include a release sheet attached to the adhesive layer to protect the adhesive layer before the sealing tape is used.

[0089] The base material contained in the sealing tape will be specifically described below.

[0090] In one embodiment of the present invention, the substrate may include one or more films selected from the group consisting of a polypropylene film, a polyimide film, an acrylic film, a polyolefin film, a polyamide film, a polycarbonate film, a polyurethane film, a cellulose acetate film, and a polyester film, but is not limited thereto.

[0091] When the substrate includes a polyester film, it may include at least one selected from the group consisting of a polyethylene terephthalate film, a polyethylene nitrate film, and a polybutylene terephthalate film. When the substrate includes a cellulose-based substrate, it may include at least one selected from the group consisting of a cellulose acetate resin and a cellulose alkylate resin, and may be manufactured by applying a mixture containing the resin to an extrusion or casting process. For example, cellulose acetate propionate or cellulose acetate butylate may be used as the cellulose alkylate.

[0092] In order to shorten the removal time, the following base materials can be used as the base material of the sealing tape.

[0093] In one embodiment of the present invention, the substrate may have a property of expanding in response to an electrolyte. Specifically, the substrate may absorb the electrolyte after contacting the electrolyte. Specifically, the substrate may absorb the electrolyte and change its structure. For example, the substrate may change its shape in the length direction after contacting the electrolyte.

[0094] When a substrate that absorbs the electrolyte after contacting the electrolyte is used as described above, the electrolyte can move more freely through the substrate, and the electrolyte absorption rate of the adhesive layer is further increased. Therefore, the sealing tape is detached faster than when a general substrate is used, and the sealing tape is detached immediately after the electrolyte is poured into the battery can, which induces the loosening of the electrode assembly and more stably increases the contact area between the negative electrode and the inside of the can. In addition, the detachment time is shortened, which is advantageous in that mass production quality can be ensured after battery production. However, if the detachment time is delayed and the sealing tape continues to adhere, there is a problem that the resistance deviation of the battery increases when checking the mass production quality.

[0095] In the present specification, the term "length direction" may mean a direction perpendicular to the thickness direction of the substrate when the substrate is held flat. In addition, in the present specification, the term "vertical" or "horizontal" means substantially vertical or horizontal within a range that does not impair the intended effect, and may include an error of, for example, within ±10 degrees, within ±5 degrees, or within ±3 degrees.

[0096] The substrate may be one that is capable of deforming, e.g., expanding, in any direction, including horizontal or vertical, or diagonal, in the plane of the substrate, so long as it has the property of deforming, e.g., expanding, in the length direction.

[0097] In one embodiment of the present invention, the substrate may have a longitudinal distortion rate according to the following formula 2 of 10% or more.

[0098] [Formula 2] Distortion rate in the longitudinal direction of the substrate = (L2-L1) / L1×100 In the formula 2, L1 is the initial length of the substrate before contacting with a fluid, and L2 is the length of the substrate measured after contacting the substrate with a fluid for 24 hours at room temperature or at 60°C.

[0099] When calculating the formula 2, the specific type of fluid that the substrate comes into contact with is not particularly limited. According to one example, the fluid may be a liquid electrolyte that is injected into the can. The term "electrolyte" may mean, for example, an ion-conducting medium used in batteries. Furthermore, the term "room temperature" may mean a natural temperature that is not heated or cooled, and may mean, for example, a temperature of about 10°C to about 30°C, about 20°C to about 30°C, or about 25°C.

[0100] The distortion rate in the longitudinal direction of the substrate may be 30% or more, 40% or more, 50% or more, 60% or more, 70% or more, 80% or more, or 90% or more. The upper limit of the distortion rate in the longitudinal direction of the substrate is not particularly limited. That is, the larger the distortion rate value, the easier it is to induce detachment of the sealing tape. For example, the upper limit of the distortion rate of the substrate may be 500%.

[0101] In the formula 2, L1 and L2 are the lengths of the substrate before and after contact with the fluid. The lengths are measured in a predetermined direction relative to the substrate, and the specific direction in which the lengths are measured is not particularly limited, as long as the directions are equally applied when measuring L1 and L2.

[0102] For example, when the substrate is a rectangular sheet, the length of the substrate may be the horizontal, vertical, or diagonal length of the sheet, or the length in any direction on a plane. However, since the direction in which the lengths are measured is similarly applied when measuring L1 and L2, for example, when the horizontal length of the substrate is adopted as L1, the horizontal length of the substrate is also adopted as L2.

[0103] The shape of the substrate is not particularly limited and may be, for example, a film or sheet. The film or sheet substrate may have a rectangular, circular, triangular, or amorphous shape.

[0104] The substrate may have a Shore A hardness of 70A or more according to ASTM D2240. The substrate may have a Shore D hardness of 40D or more according to JIS K-7311. The upper limit of the hardness of the substrate is not particularly limited, but for example, the upper limit of the Shore A hardness may be 100A or 95A, and the upper limit of the Shore D hardness may be 100D or 85D.

[0105] The substrate may include a thermoplastic polyurethane film (TPU film). The substrate may be a single-layer structure of a thermoplastic polyurethane film, or a multilayer structure, for example a two-layer structure, including at least one polyurethane film. The thermoplastic polyurethane film may be a uniaxially or biaxially stretched film, or a non-stretched film.

[0106] The thermoplastic polyurethane film may be a polyester TPU film, a polyether TPU film, or a polycaprolactone TPU film, and may be selected from among these films. The use of a polyester TPU film may be appropriate. The thermoplastic polyurethane film may be an aromatic or aliphatic thermoplastic polyurethane film. When the thermoplastic polyurethane film is used, a release layer may be further included to ensure peel strength by adjusting the adhesive strength.

[0107] The thermoplastic polyurethane film may be a reaction product of a mixture containing a polyol compound, such as a polyester polyol compound, a chain extender, and an isocyanate compound, such as an aromatic or aliphatic diisocyanate compound, and the ratio and type of the polyol compound forming a soft chain and the chain extender and isocyanate compound forming a hard chain may be adjusted to provide a thermoplastic polyurethane film with desired physical properties. As an example, the substrate may include a polyester-based thermoplastic polyurethane film, and if necessary, a film in which the weight ratio of the unit derived from the polyester polyol and the unit derived from the isocyanate compound and / or the chain extender in the polyurethane is adjusted to an appropriate range may be used.

[0108] When a thermoplastic polyurethane film is used as the substrate as described above, the electrolyte can move more freely through the substrate, and therefore the electrolyte absorption rate of the adhesive layer becomes even faster.

[0109] When the substrate includes another film in addition to the thermoplastic polyurethane film, the other film may be a polymer film or sheet manufactured to exhibit the above-mentioned deformation, e.g., expansion properties, when it comes into contact with a fluid due to the stretching or shrinking processing conditions in the manufacturing process.

[0110] According to one example, the other film may be a film containing an ester bond or an ether bond, or a cellulose ester compound, such as an acrylate-based film, an epoxy-based film, or a cellulose-based film.

[0111] In another embodiment, the substrate may include a film having a porous structure. Specifically, a separation membrane, a nonwoven fabric, a fiber, or a paper may be used as the film having a porous structure, but is not limited thereto, and any structure known in the art may be appropriately adopted.

[0112] When a film including a porous structure is used as the substrate, the electrolyte can move more freely through the substrate, and the electrolyte absorption rate of the adhesive layer is further increased. Therefore, the sealing tape is detached faster than when a general substrate is used, and the sealing tape is detached immediately after the electrolyte is poured into the battery can, which induces the loosening of the electrode assembly and more stably increases the contact area between the negative electrode and the inside of the can. In addition, the detachment time is shortened, which is advantageous in that mass production quality can be ensured after battery production. However, if the detachment time is delayed and the adhesion of the sealing tape continues, there is a problem that the resistance deviation of the battery increases when checking the mass production quality.

[0113] The method for producing the substrate is not particularly limited, and for example, a typical film or sheet molding method such as extrusion or casting of the raw material containing the resin can be used. In this case, the raw material containing the resin can be used by adding known additives, if necessary.

[0114] When the substrate is in the form of a sheet or film, the thickness of the substrate is not particularly limited and may be, for example, about 10 μm to 200 μm, 10 μm to 100 μm, 10 μm to 50 μm, 15 μm to 30 μm, or 15 μm to 20 μm.

[0115] According to an embodiment of the present invention, a secondary battery includes an electrode assembly having a structure in which a positive electrode, a negative electrode, and a separator are wound up; an electrolyte; and a can containing the electrode assembly and the electrolyte, the negative electrode being positioned on an outer circumferential surface of the electrode assembly and a sealing tape being provided on the outer circumferential surface. In this case, the sealing tape includes a substrate and an adhesive layer provided on one surface of the substrate, the adhesive layer having an expansion property in response to the electrolyte and capable of absorbing the electrolyte and expanding after contacting the electrolyte.

[0116] The electrode assembly may have a structure in which a positive electrode, a negative electrode, and a separator provided between the positive electrode and the negative electrode are wound, and the negative electrode may be located on an outer periphery of the electrode assembly.

[0117] The sealing tape may be attached to the outer circumferential surface of the electrode assembly via the adhesive layer. The electrode assembly may be wound in a jelly roll shape.

[0118] In one embodiment of the present invention, the negative electrode may include a negative electrode coating portion and a negative electrode uncoated portion, and the negative electrode uncoated portion may be located on an outer circumferential surface of the electrode assembly. That is, the negative electrode uncoated portion may be located on the outer circumferential surface of the electrode assembly, and a sealing tape may be provided on the negative electrode uncoated portion.

[0119] In one embodiment of the present invention, the negative electrode may include a negative electrode coating portion and a negative electrode uncoated portion, and the negative electrode covering portion may be located on an outer circumferential surface of the electrode assembly. That is, a negative electrode coating portion may be located on an outer circumferential surface of the electrode assembly, and a seal tape may be provided on the negative electrode coating portion.

[0120] In one embodiment of the present invention, the negative electrode may include a negative electrode coating portion and a negative electrode uncoated portion, and the negative electrode coating portion and the negative electrode uncoated portion may both be located on the outer circumferential surface of the electrode assembly. That is, a negative electrode coating portion coated with a negative electrode active material and a negative electrode uncoated portion not coated with a negative electrode active material may both be located on the outer circumferential surface of the electrode assembly, and sealing tape may be provided on the negative electrode coating portion and the negative electrode uncoated portion.

[0121] The positive electrode may include a positive electrode current collector and a positive electrode active material coated on the positive electrode current collector. Specifically, the positive electrode includes a positive electrode current collector, and includes a positive electrode coating portion in which a positive electrode active material layer is provided on the positive electrode current collector; and a positive electrode uncoated portion in which the positive electrode active material layer is not provided on the positive electrode current collector. Specifically, the positive electrode coating portion may be formed by coating a positive electrode active material on one or both sides of the positive electrode current collector, and the positive electrode current collector may be exposed in the positive electrode uncoated portion in which the positive electrode active material is not coated. Here, the positive electrode current collector may be made of, for example, an aluminum (Al) foil. In this case, the positive electrode active material may be, for example, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron phosphate, or a compound or mixture containing at least one of them.

[0122] The negative electrode may include a negative electrode current collector and a negative electrode active material coated on the negative electrode current collector. Specifically, the negative electrode includes a negative electrode current collector, and includes a negative electrode coating portion having a negative electrode active material layer on the negative electrode current collector; and a negative electrode uncoated portion on which the negative electrode active material layer is not provided. Specifically, the negative electrode coating portion may be formed by coating a negative electrode active material on one or both sides of the negative electrode current collector, and the negative electrode current collector may be exposed in the negative electrode uncoated portion where the negative electrode active material is not coated. Here, the negative electrode current collector may be made of a foil made of, for example, copper (Cu) or nickel (Ni). In this case, the negative electrode active material may be made of a material including, for example, artificial graphite. In addition, the negative electrode active material may be made of, for example, lithium metal, lithium alloy, carbon, petroleum coke, activated carbon, graphite, silicon compound, tin compound, titanium compound, or an alloy thereof.

[0123] The separator separates and electrically insulates the positive electrode and the negative electrode. Here, the positive electrode and the negative electrode may be wound together with the separator to form a jelly roll type electrode assembly, or may be formed as a stack type or a stack and folding type.

[0124] The separator may be made of an insulating material and may be laminated alternately with the positive and negative electrodes, where the separator may be located between the positive and negative electrodes and on the outer surfaces of the positive and negative electrodes.

[0125] There are no particular limitations on the separator membrane that may be used as long as it is normally used as a separator membrane in a secondary battery. In particular, it is preferable for the separator membrane to have low resistance to the ion transfer of the electrolyte and excellent electrolyte moisture-absorbing capacity.

[0126] The separator may be made of a ductile material. In this case, the separator may be made of a polyolefin resin film such as polyethylene or polypropylene having microporosity. As another example, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high melting point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material may be used to ensure heat resistance or mechanical strength, and may be used selectively in a single layer or multilayer structure.

[0127] In the above, the type of electrolyte, which is a fluid that deforms, for example expands, the adhesive layer of the sealing tape, is not particularly limited, and any electrolyte known in this field may be used depending on the type of battery.

[0128] In one example, the electrolytic solution may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, or the like that can be used in manufacturing a secondary battery, but is not limited thereto.

[0129] Specifically, the electrolyte may contain a non-aqueous organic solvent and a metal salt.

[0130] Examples of the non-aqueous organic solvent include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0131] In particular, among the carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are preferably used because they are high-viscosity organic solvents with high dielectric constants and can dissociate lithium salts well. When such cyclic carbonates are mixed with low-viscosity, low-dielectric-constant linear carbonates such as dimethyl carbonate and diethyl carbonate in an appropriate ratio, an electrolyte solution having high electrical conductivity can be produced, and these can be used more preferably.

[0132] The metal salt may be a lithium salt, which is a substance that is easily dissolved in the non-aqueous electrolyte. For example, the anion of the lithium salt may be F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3- , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - It is possible to use one or more selected from the group consisting of: The concentration of the lithium salt in the electrolyte can vary depending on the application, and can usually be within the range of 0.1M to 2.0M.

[0133] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, and aluminum trichloride for the purposes of improving the life characteristics of the battery, suppressing a decrease in battery capacity, and improving the discharge capacity of the battery.

[0134] The can in which the electrode assembly and the electrolyte are contained may be, but is not limited to, a cylindrical can.

[0135] The secondary battery may be manufactured by attaching the sealing tape to an electrode assembly, placing the electrode assembly in a can, injecting an electrolyte into the can, and then sealing the can.

[0136] The sealing tape is inserted into the can while being fixed to the electrode assembly, and then absorbs the electrolyte injected into the can and expands, thereby reducing the peel strength between the adhesive layer and the electrode assembly, thereby allowing the adhesive layer of the sealing tape to be detached from the electrode assembly. Therefore, the secondary battery according to one embodiment of the present invention may have a structure including a region where the electrode assembly is loosened to a certain extent and the outer circumferential surface of the electrode assembly is in contact with the inside of the can.

[0137] FIG. 1 is a diagram illustrating a secondary battery according to an embodiment of the present invention.

[0138] Referring to FIG. 1, the secondary battery includes an electrode assembly 11 and a sealing tape 12 attached to the outer circumferential surface of the electrode assembly 11 .

[0139] FIG. 1-1 is a schematic diagram of a secondary battery from the process of attaching the sealing tape 12 to the electrode assembly 11 until it is stored inside a can. The sealing tape 12 is attached to the outer peripheral surface of the electrode assembly 11 to fix the electrode assembly 11, and a certain amount of gap is formed between the inside of the can 10 and the electrode assembly 11.

[0140] 1-2 is a schematic diagram of a secondary battery after an electrolyte is injected into the inside of the can 10, in which the sealing tape 12 absorbs the electrolyte and its peeling strength decreases, causing it to detach from the electrode assembly 11, causing the wound electrode assembly 11 to unravel to some extent, reducing the gap between the inside of the can 10 and the electrode assembly 11. At this time, although not clearly shown in FIG. 1-2, the outer circumferential surface of the electrode assembly can come into contact with the inside of the can.

[0141] That is, the secondary battery according to an embodiment of the present invention includes a region where the inside of the can and the outer periphery of the electrode assembly are in contact with each other. In this case, the contact area between the inside of the can and the outer periphery of the electrode assembly may be 5% or more based on the total area of ​​the outer periphery of the electrode assembly. Alternatively, the contact area may be 10% or more, 20% or more, 30% or more, 40% or more, or 50% or more, or may be 100% or less, 90% or less, 80% or less, 70% or less, or 60% or less.

[0142] 2 is a schematic diagram of a secondary battery according to an embodiment of the present invention. Referring to FIG. 2, the sealing tape 12 may be attached to surround an outer circumferential surface of the electrode assembly 11.

[0143] Specifically, the sealing tape 12 may be provided to surround the outer circumferential surface, including a finishing portion 21 where the outermost end of the outer circumferential surface of the electrode assembly 11 is located. That is, the sealing tape 12 may be provided to surround the outer circumferential surface in the width direction (direction perpendicular to the height direction) of the electrode assembly 11. In this case, the sealing tape being provided to surround the outer circumferential surface means that the sealing tape is provided continuously without being broken along the outer circumferential surface of the electrode assembly.

[0144] Specifically, the sealing tape 12 may be provided on the upper portion 31 and the lower portion 33 of the outer peripheral surface of the electrode assembly 11. That is, the sealing tape may be attached to the outer peripheral surface of the electrode assembly in a total of two rows. In this case, the upper portion 31 and the lower portion 33 refer to the upper region and the lower region, respectively, based on the center portion 32 of the outer peripheral surface. In addition, the upper end portion 41 and the lower end portion 42 of the outer peripheral surface of the electrode assembly may be provided so that the electrode assembly is exposed as it is. However, the present invention is not limited thereto, and the sealing tape may be attached to an appropriate position depending on the size and type of the battery so that the detachment time can be appropriately adjusted.

[0145] The sealing tape 12 may be provided in an area not including the central portion 32 of the outer circumferential surface when the height of the electrode assembly 11 is taken as a reference. In this case, the central portion 32 may refer to an area within ±1% (height basis) above and below the center of the outer circumferential surface.

[0146] If the sealing tape is attached including the center of the outer periphery, it is difficult to induce unraveling of the electrode assembly even if the sealing tape absorbs the electrolyte and deforms, and there is a problem that the contact area between the negative electrode and the inside of the can is not secured. On the other hand, if the sealing tape is attached to the upper and lower parts of the outer periphery without including the center of the outer periphery as in the present invention, it is easy to induce unraveling of the electrode assembly, and it is possible to increase the contact area between the negative electrode and the inside of the can and easily realize low resistance characteristics.

[0147] The area where the sealing tape is attached to the outer peripheral surface of the electrode assembly may be adjusted according to the size and type of the battery so that the detachment time can be appropriately adjusted. In one example, the area where the sealing tape is attached may be less than 80%, less than 70%, less than 60%, less than 50%, less than 40%, or less than 30% of the total area of ​​the outer peripheral surface of the electrode assembly, and may be 5% or more, 10% or more, or 20% or more, but is not limited thereto.

[0148] In another embodiment, the sealing tape may be provided on a finishing portion where an outermost end of an outer peripheral surface of the electrode assembly is located. Specifically, although not shown in the drawings, the sealing tape may be attached in a height direction on the finishing portion where an outermost end of an outer peripheral surface of the electrode assembly is located. That is, the sealing tape may be attached in a line so as to cover the finishing portion where an outermost end of an outer peripheral surface of the electrode assembly is located. However, the present invention is not limited thereto, and the sealing tape may be attached at an appropriate position depending on the size and type of the battery so that the unraveling of the electrode assembly can be appropriately controlled.

[0149] When the sealing tape is attached in the height direction on the finishing portion of the electrode assembly, it can be attached in a form that continuously covers the finishing portion of the electrode, thereby preventing damage to the electrode assembly, and increasing the contact area between the negative electrode and the inside of the cylindrical can, thereby easily implementing low resistance characteristics.

[0150] In one embodiment of the present invention, the average gap between the inside of the can and the outer peripheral surface of the electrode assembly before the sealing tape is removed, i.e., the difference between the average inner diameter of the can and the average outer diameter of the electrode assembly, may be more than 0.9% and not more than 2% based on the inner diameter of the can, specifically, not more than 1.5%, not more than 1.3%, not more than 1.2%, not more than 1.1%, or not more than 1%.

[0151] In one embodiment of the present invention, after the sealing tape is removed, the average gap between the inside of the can and the outer peripheral surface of the electrode assembly, i.e., the difference between the average inner diameter of the can and the average outer diameter of the electrode assembly, may be 0.9% or less based on the inner diameter of the can, specifically, 0.8% or less, 0.7% or less, 0.6% or less, 0.5% or less, 0.4% or less, 0.3% or less, or 0.2% or less, or may be 0% or more, more than 0%, or 0.1% or more.

[0152] In one embodiment of the present invention, the electrode assembly may include one negative electrode tab. Generally, an electrode assembly in which a separator is located on an outer periphery includes a plurality of negative electrode tabs to realize low resistance, but in this case, it is difficult to weld the negative electrode tabs and to secure the internal space of the can. On the other hand, in the present invention, the negative electrode is located on the outer periphery of the electrode assembly, and the contact area between the negative electrode and the inside of the can is increased to realize low resistance, so that even if one negative electrode tab is included, high low resistance characteristics can be realized, and at the same time, costs can be reduced, the internal space of the can can be secured, and the weldability of the negative electrode tab can be secured.

[0153] [Example] Hereinafter, the present specification will be described in detail with reference to examples in order to specifically explain the present specification. However, the examples according to the present specification can be modified into various other forms, and the scope of the present application is not to be construed as being limited to the examples detailed below. The examples of the present application are provided to more completely explain the present specification to those having average knowledge in the art.

[0154] <Example 1> (1) Manufacturing of sealing tapes In a 1000cc reactor equipped with a cooling device for easy temperature control and refluxing with nitrogen gas, 68 parts by weight of n-butyl acrylate (n-BA), 30 parts by weight of methoxyethyl acrylate (MEA), and 2 parts by weight of hydroxybutyl acrylate (HBA) were added to the monomer mixture, 0.02 parts by weight of n-dodecanethiol as a chain transfer agent, and 150 parts by weight of ethyl acetate (EAc) were added as a solvent. Then, in order to remove oxygen, nitrogen gas was purged at 60°C for 60 minutes, and the temperature was maintained at 60°C. After the mixture was homogenized, 0.04 parts by weight of azobisisobutyronitrile (AIBN) was added as a reaction initiator. The mixture was reacted for 8 hours to produce a polymer having a weight average molecular weight of 780,000. In the above, parts by weight means wt%.

[0155] For 100 parts by weight of the polymer prepared as above, 0.3 parts by weight of a trimethylolpropane tolylene diisocyanate adduct as a multifunctional isocyanate-based crosslinking agent was added to an ethyl acetate solution, and then diluted to an appropriate concentration in consideration of coating properties and mixed uniformly.

[0156] The adhesive composition prepared as above was coated on one side of a PET (poly(ethylene terephthalate)) film (thickness: 12 μm) and dried to form a uniform adhesive layer with a thickness of 5 μm. Then, a release film was laminated on the coating layer, and the adhesive layer was aged for 3 days under constant temperature (25°C) and humidity conditions to prepare a sealing tape.

[0157] (2) Manufacture of secondary batteries A seal tape was applied to cover approximately 30% of the outer peripheral surface of a jelly-roll-shaped electrode assembly (cross-sectional diameter: 20.5 mm) in which the negative electrode, positive electrode, and separator were wound and the negative electrode was provided on the outer peripheral surface, and the assembly was inserted into a cylindrical can (cross-sectional diameter: 21.05 mm). Next, a carbonate-based electrolyte solution was poured into the can and sealed to prepare a secondary battery.

[0158] <Example 2> A secondary battery was manufactured in the same manner as in Example 1, except that a non-stretched PU film (thickness: 40 μm) made of thermoplastic polyurethane (TPU) was used as a substrate instead of the PET film in Example 1.

[0159] <Comparative Example 1> A secondary battery was manufactured in the same manner as in Example 1, except that a monomer mixture consisting of 98 parts by weight of n-butyl acrylate and 2 parts by weight of hydroxybutyl acrylate was used instead of the monomer mixture in Example 1.

[0160] <Experimental Example> For the secondary batteries manufactured in the examples and comparative examples, the ACIR was measured at room temperature using a charge / discharge measuring device (P&E Solutions) by bringing the probes of the measuring device into contact with the positive and negative electrodes. In addition, the expansion of the adhesive layer of the sealing tape and the time it took for the sealing tape to detach from the electrode assembly were measured, and the results are shown in Table 1 below.

[0161] FIG. 3 shows CT images of the batteries prepared in Example 1 and Comparative Example 1. In the case of Comparative Example 1, the sealing tape did not come off, creating a gap between the negative electrode and the inside of the can. In the case of Example 1, it was confirmed that the sealing tape absorbed the electrolyte and expanded, inducing the unraveling of the electrode assembly, resulting in almost no gap between the negative electrode and the inside of the can.

[0162] [Table 1]

[0163] In Table 1, it was confirmed that in Examples 1 and 2, the adhesive layer of the sealing tape includes a sealing tape having an expandable property in response to an electrolyte, and after the electrolyte is injected into the can, the electrode assembly is unraveled, so that the contact area between the negative electrode and the can is increased and the internal resistance is reduced.

[0164] Moreover, it was confirmed that in Example 2, the electrolyte solution diffused through the base material, and the electrolyte solution had a high diffusion rate, so that the removal time of the sealing tape was faster.

[0165] Meanwhile, in the case of Comparative Example 1, since the adhesive layer did not have the ability to expand in response to the electrolyte, it was difficult to induce the electrode assembly to unravel, and the contact area between the negative electrode and the inside of the can could not be secured, resulting in high internal resistance.

[0166] While the present invention has been described above with reference to preferred embodiments, it will be understood that those skilled in the art can make various modifications and variations to the present invention without departing from the spirit and scope of the present invention as set forth in the following claims. [Explanation of symbols]

[0167] 10 Cylindrical can 11...electrode assembly 12 Sealing tape 21 Finishing section 31 ...Upper part of outer periphery 32...Center of outer periphery 33 Lower part of outer periphery 41: Upper end of outer periphery 42: Lower end of outer periphery

Claims

1. A secondary battery comprising: an electrode assembly having a structure in which a positive electrode, a negative electrode, and a separator are wound; an electrolyte; and a can in which the electrode assembly and the electrolyte are contained, the negative electrode is located on an outer circumferential surface of the electrode assembly, A seal tape is provided on the outer circumferential surface of the electrode assembly, The sealing tape includes a base material and an adhesive layer provided on one surface of the base material, The adhesive layer has an expansion property in response to the electrolyte solution, The sealing tape is detached from the outer peripheral surface of the electrode assembly.

2. The secondary battery according to claim 1 , wherein the adhesive layer is in a swollen state after absorbing the electrolyte.

3. The secondary battery according to claim 1 , further comprising a region where the inside of the can and the outer circumferential surface of the electrode assembly are in contact with each other.

4. The secondary battery according to claim 1 , wherein the sealing tape is provided to surround the outer circumferential surface of the electrode assembly, including a finishing portion where an outermost end of the outer circumferential surface of the electrode assembly is located.

5. The secondary battery according to claim 1 , wherein the sealing tapes are provided on both upper and lower parts of an outer circumferential surface of the electrode assembly.

6. The secondary battery according to claim 1 , wherein the sealing tape is provided in an area that does not include a center portion of the outer circumferential surface when a height of the electrode assembly is taken as a reference.

7. The secondary battery of claim 1 , wherein the negative electrode includes a negative electrode coating portion and a negative electrode uncoated portion, the negative electrode uncoated portion being located on an outer circumferential surface of the electrode assembly.

8. The secondary battery of claim 1 , wherein the negative electrode includes a negative electrode coating portion and a negative electrode uncoated portion, the negative electrode coating portion being located on an outer circumferential surface of the electrode assembly.

9. The secondary battery according to claim 1, wherein the adhesive layer has a center line average roughness value of 100 μm to 250 μm measured 24 hours after contact with the electrolyte.

10. The secondary battery according to claim 1, wherein the adhesive layer comprises a cured product of an adhesive composition including a polymer having polymerization units derived from a (meth)acrylic acid ester monomer, a monomer represented by the following Chemical Formula 1, and a crosslinkable monomer having a crosslinkable functional group: 【Chemistry 1】 In the above Chemical Formula 1, R 1 is hydrogen; or an alkyl group having 1 to 12 carbon atoms; R 2 is an alkylene group having 1 to 6 carbon atoms, R 3 is hydrogen; an alkyl group having 1 to 12 carbon atoms; an aryl group having 6 to 24 carbon atoms; or an arylalkyl group having 6 to 48 carbon atoms, n is 0 or greater.

11. The secondary battery according to claim 1 , wherein the adhesive layer is provided on one surface of the substrate in a pattern.

12. The secondary battery according to claim 1 , wherein the substrate has an expansion property with respect to the electrolyte.

13. The secondary battery according to claim 1, wherein the substrate has a longitudinal distortion rate of 10% or more according to the following formula 2: [Formula 2] Distortion rate in the longitudinal direction of the substrate = (L2 - L1) / L1 x 100 In the formula 2, L1 is the initial length of the substrate before contact with a fluid, and L2 is the length of the substrate measured after contacting the substrate with a fluid for 24 hours at room temperature or at 60°C.

14. The secondary battery according to any one of claims 1 to 13, wherein the substrate comprises a thermoplastic polyurethane film.

15. The secondary battery according to claim 1 , wherein the substrate comprises a polyester thermoplastic polyurethane film (polyester TPU film).

16. The secondary battery according to claim 1 , wherein the substrate comprises a film including a porous structure.

17. The secondary battery according to claim 1 , wherein the electrode assembly includes one negative electrode tab.