High temperature composites and methods for preparing high temperature composites - Patents.com

PAEK copolymers with controlled pyrolysis conditions address the inefficiencies of traditional methods, achieving high char yields and reduced cycle times for high temperature composites, enhancing production efficiency and quality.

JP2024544967APending Publication Date: 2024-12-05ARKEMA FRANCE SA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024527821
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-19
Filing Date
2022-11-15
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The pyrolysis process for producing high temperature composites like carbon-carbon, carbon-ceramic matrix, and carbon-silica composites is time-consuming and labor-intensive, often requiring multiple cycles with potential defects and dimensional changes, leading to long lead times and reduced quality.

Method used

The use of poly(aryletherketone) (PAEK) copolymers with specific repeating unit ratios and reinforcing materials allows for automated processing, increasing char yield from 70% to 95%, reducing the number of pyrolysis cycles, and minimizing dimensional changes through controlled pyrolysis conditions.

Benefits of technology

This approach significantly reduces production time, improves quality, and enhances char yield, resulting in high-performance composites with fewer defects and dimensional issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544967000001
    Figure 2024544967000001
  • Figure 2024544967000002
    Figure 2024544967000002
  • Figure 2024544967000003
    Figure 2024544967000003
Patent Text Reader

Abstract

The present invention relates to a method for making a high temperature composite, which is a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite, comprising the steps of: a. making a precursor part from a resin comprising a poly(aryl ether ketone) (PAEK) copolymer comprising at least two different repeat units, one of the repeat units being present in an amount of 50-78 mol % relative to the total amount of repeat units constituting the copolymer, and at least one reinforcing material; b. pyrolyzing the precursor part to form a pyrolyzed part; c. injecting a liquid second resin into the pyrolyzed part to form an infused part; and d. pyrolyzing the infused part to form a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite, optionally repeating steps c. through d. one or more times.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to high temperature composites such as carbon-carbon composites, carbon-ceramic matrix composites and carbon-silica composites. The present invention also relates to methods for preparing high temperature composites such as carbon-carbon composites, carbon-ceramic matrix composites and carbon-silica composites. [Background technology]

[0002] High temperature composites such as carbon-carbon composites, carbon-ceramic matrix composites, and carbon-silica composites can be useful in areas such as hypersonics, solid / liquid rocket propulsion, and other defense / aerospace applications where very high temperature properties are required. Industrial applications can include metal and glass processing, and concentrated solar power.

[0003] High temperature composite materials, including carbon composites, carbon ceramic matrix composites, and carbon silica composites, have traditionally been fabricated utilizing thermosetting resins such as pitch or phenolic resins (e.g., Hexion Durite SC1008) or epoxies. Precursor parts utilizing these thermosetting composites are fabricated by "hand layup," which requires significant manual labor to press the thermosetting prepregs. This manual labor also introduces human error and reduced quality in the precursor parts, in addition to the time and expense of such labor. Thermoplastic composite materials have the advantage that they can be processed by automated methods, including automated tape placement and 3D printing. Thermoplastic tapes have an additional advantage over thermosetting prepregs in that they do not typically require refrigerated shipping and storage.

[0004] Pyrolysis processes (heat treatments) can be used to produce carbon-carbon composites, carbon-ceramic matrix composites, and carbon-silica composites. Pyrolysis can be carried out to preserve the carbon elements while removing volatiles and / or non-carbon organic elements in the composite (such as in a polymer matrix). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] US 10,669,659 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the pyrolysis step can sometimes take hundreds of hours, with additional days for graphitization. The process is then repeated several times, resulting in long lead times for the part to be completed. Each additional reinjection and pyrolysis cycle is labor intensive and time consuming. Furthermore, with each cycle, there is a possibility that defects or imperfections may result in an unacceptable final object. It is therefore desirable to reduce the number of cycles required to achieve a fully dense part. A higher char yield allows this process to be shortened, since the part is closer to being completely solid after the first pyrolysis cycle, thereby reducing the number of cycles required. Typically, only phenolic resin-based solutions can provide char yields of 50-70%. Many other (non-PAEK) thermoplastic solutions provide char yields of less than 65%.

[0007] Among other defects to be avoided during the pyrolysis process are dimensional changes of the pyrolyzed parts, in particular the expansion of the parts and / or the appearance of cracks inside the parts.

[0008] The invention described herein, utilizing selected poly(aryl ether ketone) (PAEK) copolymers, unexpectedly overcomes at least some of the problems noted above.

[0009] PAEK polymers are high performance semi-crystalline polymers with high melting points, extremely high thermal properties, exceptional chemical and flame resistance, and high modulus and strength. By following embodiments of the present invention, it is possible to use thermoplastic resins to make carbon-carbon composites, carbon-ceramic matrix composites, and carbon-silica composites. Thermoplastic resins allow for the preparation of precursor parts by automated methods, which reduces time and cost while improving quality, and have unexpectedly high char yields, such as char yields of 70%-80%, up to 85%, up to 90%, and even up to 95% or more. Pyrolysis cycles can be speeded up since PAEK materials exhibit a single decomposition point, which alleviates the need for long hold cycles at multiple temperatures often observed with thermosets. The surprisingly high char yields also allow for fewer pyrolysis / injection steps than other methods, which reduces days and even weeks of production time. In certain embodiments, carbon-carbon composites, carbon-ceramic matrix composites, and carbon-silica composites can be made with total processing times of less than about 50 hours, 60 hours, 70 hours, 80 hours, 90 hours, 100 hours, 110 hours, 120 hours, 130 hours, 140 hours, 150 hours, 160 hours, 170 hours, 180 hours, 190 hours, 200 hours, or any range between the specified values.

[0010] Applicants have also surprisingly discovered that, inter alia, thanks to the selection of poly(aryl ether ketone) (PAEK) copolymers, it is possible to utilize carbon-carbon composite, carbon-ceramic matrix composite and carbon-silica composite precursors that combine the advantages of the high mechanical performance of PAEK polymers with high char yields and low dimensional changes of the pyrolyzed parts. [Means for solving the problem]

[0011] The present invention relates to a method for making a high temperature composite, which is a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite, comprising: a. preparing a precursor part from a resin comprising a poly(aryl ether ketone) (PAEK) copolymer having at least two different repeat units, one of the repeat units being present in an amount of 50-78 mol % relative to the total amount of repeat units constituting the copolymer, and at least one reinforcing material; b. pyrolyzing the precursor parts into pyrolyzed parts; c. injecting a liquid second resin into the pyrolyzed part to produce an infused part; d. pyrolyzing the injected component to produce a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite; and optionally repeating steps c. through d. one or more times.

[0012] In certain embodiments, the PAEK copolymer consists essentially of or consists of two repeat units. In certain embodiments, the PAEK copolymer is a polyetherketoneketone (PEKK) having a T:I ratio of 50:50 to 78:22, preferably 55:45 to 75:25. In certain embodiments, the PEKK has a T:I ratio of about 55:45 to about 65:35. In certain embodiments, the PEKK has a T:I ratio of about 65:35 to about 75:25.

[0013] In one particular embodiment, during pyrolysis, the temperature within the chamber is increased to a peak temperature of about 1000° C. or greater.

[0014] In certain embodiments, the temperature within the chamber is increased one or more times during the pyrolysis at a rate of between 1° C. / hr and about 20° C. / hr, and optionally, the pyrolysis is maintained at one or more temperatures for a period of time.

[0015] In certain embodiments, during pyrolysis, the temperature within the chamber is increased to a peak temperature of about 1000° C. or greater, the temperature within the chamber is increased one or more times during said pyrolysis at a rate of about 1° C. / hr to about 20° C. / hr, and optionally, said pyrolysis is maintained at one or more temperatures for a period of time.

[0016] In one particular embodiment, during pyrolysis of the precursor part, the temperature in the chamber is increased one or more times between 450° C. and 600° C. at a rate of less than 10° C. / hour and optionally maintained at one or more temperatures between 450° C. and 600° C., inclusive, for a period of time.

[0017] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10° C. / hour or greater below 400° C. and / or above 650° C.

[0018] In certain embodiments, the liquid second resin comprises one or more of pitch, benzoxazine, furfural, polyester, vinyl ester, acrylic, and phenolic resins.

[0019] In certain embodiments, the precursor part is made by melt processing a resin including poly(aryl ether ketone) and at least one reinforcing material, hi certain embodiments, the melt processing includes one or more of injection molding, extrusion, rotational molding, compression molding, pultrusion, filament winding, and fused filament manufacturing printing.

[0020] In certain embodiments, the precursor part of step (a) comprises: a1) impregnating a continuous fiber tape or fabric with a resin comprising a poly(aryl ether ketone) (PAEK) copolymer comprising at least two different repeat units, one of which is present in an amount of 50-78 mol % based on the total amount of repeat units constituting the copolymer, and at least one reinforcing additive, to produce a filled PAEK tape or fabric, or co-weaving the continuous fiber or fabric with a PAEK fiber comprising PAEK and at least one reinforcing additive to produce a filled co-woven PAEK fiber or fabric; and a2) processing the filled PAEK tape or fabric, or co-woven PAEK fiber or fabric, by one or more of the following methods: hand layup, automated tape placement, 3D printing, filament winding, needle punching and other methods of Z-axis consolidation followed by one or more of compression molding, vacuum bag consolidation, autoclave consolidation and in situ consolidation to create a precursor part. It is made by.

[0021] In certain embodiments, the precursor part of step (a) comprises: a1) processing an aligned reinforcement material with a resin comprising a PAEK copolymer comprising at least two different repeat units, one of which is present in an amount of 50-78 mol % based on the total amount of repeat units constituting the copolymer, to produce an aligned reinforcement material PAEK composition to produce a fabric, prepreg or tape comprising the aligned reinforcement material and the impregnated PAEK; a2) processing the aligned reinforcement material and impregnated PAEK-containing fabric, prepreg or tape by hand layup, automated tape placement, 3D printing, filament winding or needle punching, or other methods of Z-axis consolidation followed by compression molding, vacuum bag consolidation, autoclave consolidation, in situ consolidation to create a precursor object. It is made by.

[0022] In certain embodiments, the reinforcing material comprises one or more reinforcing additives selected from carbon-based additives, chopped fibers, inorganic additives, or mixtures thereof; fibrous materials including long fibers, continuous fibers, or mixtures thereof; or mixtures thereof.

[0023] In certain embodiments, the reinforcing material comprises a carbon-based additive that is one or more of carbon fiber, carbon nanotubes, graphite, graphene, carbon whiskers, fullerenes, carbon black, carbon flakes, buckyballs, and mixtures thereof.

[0024] In certain embodiments, the reinforcing material comprises chopped, long or continuous fibers that are one or more of carbon, glass, silica, boron, natural fibers, polymeric fibers, and mixtures thereof.

[0025] In one particular embodiment, the reinforcing material is chopped carbon fiber or chopped glass fiber.

[0026] In certain embodiments, the reinforcing material is long or continuous carbon fiber or long or continuous glass fiber.

[0027] In certain embodiments, the reinforcement material includes an inorganic additive that is one or more of a Group IV, V, or VI carbide, silicide, boride, or nitride, and / or ceramic whiskers.

[0028] In certain embodiments, the precursor part includes a dispersing agent that is an organosilicate, an organozirconate, an organoaluminate, or an organotitanate.

[0029] In one particular embodiment, the reinforcing material is a mixture of chopped fibers and long or continuous fibers.

[0030] In certain embodiments, the precursor part of step (a) is made by processing a tape or fabric, or a co-woven PAEK fiber or fabric, made from a PAEK copolymer comprising at least two different repeat units, one of the repeat units being present in an amount of 50-78 mol % relative to the total amount of repeat units making up the copolymer, and at least one reinforcing material, by one or more of the following methods: hand layup, automated tape placement, 3D printing, filament winding, needle punching and other methods of Z-axis consolidation followed by one or more of compression molding, vacuum bag consolidation, autoclave consolidation and in situ consolidation.

[0031] The present invention is also directed to a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite made by the method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] Embodiments of the present disclosure relate to methods for preparing high temperature composites, such as carbon-carbon, carbon-ceramic matrix and carbon-silica composites. Embodiments of the present disclosure also relate to carbon-carbon, carbon-ceramic matrix and carbon-silica composites made by the disclosed methods.

[0033] As used herein, the term "about" means ±10% of the specified value. By way of example only, at least "about 50 percent" can include at least 45 percent to at least 55 percent (and inclusive).

[0034] The word "comprising" is used consistent with its open-ended meaning, i.e., meaning that a given product or process can optionally have additional features or elements other than those explicitly recited. Even when an embodiment is described with the phrase "comprising," it is understood that other similar embodiments described in terms of "consisting of" and / or "consisting essentially of" are also contemplated and within the scope of the present disclosure.

[0035] As used herein, the term "aligned" means that greater than 75% of the objects have at least one of their major axes oriented in the same direction (±5°) as measured using an image from an optical microscope of a cross-section of the composite.

[0036] As used herein, the term "char yield" refers to the residual carbon content as measured by the mass remaining after pyrolysis, and can be determined as described in the Examples herein.

[0037] As used herein, in the context of composites, the term "% solid" refers to the percent (%) of density of a pyrolyzed part compared to a theoretically fully dense part containing no pores or voids. The density of a fully dense part can be calculated by the formula for a mixture of matrix material (carbon or ceramic) and fiber material (glass or carbon). D = d1a + d2 (1-a) In the above formula, D = density of fully dense parts d1 = density of fiber material (glass or carbon) a = mass fraction of fiber material (glass or carbon) d2=density of the matrix material (carbon or ceramic). The density of a pyrolyzed part can be experimentally determined by dividing its mass by its volume.

[0038] As used herein, the term "composite" refers to a material that includes at least two different and / or separate components. For example, and without limitation, a carbon-carbon composite can include a carbon matrix (e.g., graphite-based) that includes carbon fibers. A carbon ceramic matrix composite can include a ceramic matrix (e.g., SiC) that includes carbon. A carbon silica composite can include a carbon (usually graphite-based) matrix that includes glass / silica fibers.

[0039] As used herein, the term "high temperature," when used in reference to high temperature composites, means and refers to temperatures of about 1000° C. or greater, at which the composite may be used without deleterious decomposition.

[0040] As used herein, the term "pyrolyzing" refers to the application of heat to effect a chemical change in a material, causing the volatilization removal of some, substantially all, or all non-carbon or non-inorganic elements of the material. In the present invention, the chemical change of the precursor generally occurs at a temperature of at least 250°C, particularly at least 400°C.

[0041] As used herein, the term "infusion" (or "infusing") means the permeation of a matrix with a liquid resin, which can fill voids or pores.

[0042] As used herein, the term "chopped" refers to fibers that are not continuous and have a length of less than about 20 mm, preferably less than about 15 mm, preferably less than about 10 mm, and most preferably less than about 5 mm.

[0043] As used herein, the term "polyaryletherketone", commonly referred to by its acronym "PAEK", refers to a polymer having the following formula: (-Ar-X-) and (-Ar1-Y-) (In the formula, Ar and Ar1 each represent a divalent aromatic radical, Ar and Ar1 may preferably be selected from 1,3-phenylene, 1,4-phenylene, 1,1'-biphenylene divalent in the 3,3' positions, 1,1'-biphenyl divalent in the 3,4' positions, 1,4-naphthylene, 1,5-naphthylene and 2,6-naphthylene, X represents an electron-withdrawing group, which may preferably be chosen from carbonyl and sulfonyl groups, - Y represents an oxygen atom, a sulfur atom or a group selected from alkylene groups such as -(CH2)- and isopropylidene. In these units X and Y, at least 50%, preferably at least 70% and more particularly at least 80% of the X groups are carbonyl groups and at least 50%, preferably at least 70% and more particularly at least 80% of the Y groups represent oxygen atoms.

[0044] According to a preferred embodiment, 100% of the X groups may represent a carbonyl group and 100% of the Y groups may represent an oxygen atom.

[0045] PAEK Copolymer The PAEK used in the present invention is a copolymer, which means that it has at least two repeat units of different chemical structure. One of the repeat units is present in an amount of 50 mol% to 78 mol% based on the total moles of repeat units that make up the copolymer. In fact, the inventors have recognized that the presence of two different repeat units in the PAEK structure is responsible for minimizing the dimensional change of the PAEK during pyrolysis.

[0046] In some embodiments, the PAEK copolymer consists essentially of or consists of two repeat units of different chemical structures. As used herein, the term "consisting essentially of repeat units" means that the repeat units represent 95% to 99.9% of the molar ratio in the polymer. Furthermore, the term "consisting of repeat units" means that the repeat units represent at least 99.9%, ideally 100% of the molar ratio in the polymer.

[0047] In some embodiments, the repeating units predominantly present in the copolymer structure represent 55 mol % to 75 mol % of the total number of moles of repeating units constituting the copolymer.

[0048] Advantageously, the PAEK copolymer comprises: - polyetherketoneketone copolymers, also known as PEKK, consisting essentially of or consisting of one or more repeat units of the formula: -Ph-O-Ph-C(O)-Ph-C(O)-; - polyetheretherketone copolymers, also known as PEEK, consisting essentially of or consisting of one or more repeat units of the formula: -Ph-O-Ph-O-Ph-C(O)-; - polyetherketone copolymers, also known as PEK, consisting essentially of or consisting of one or more repeat units of the formula: -Ph-O-Ph-C(O)-; - polyetheretherketoneketone copolymers, also known as PEEKK, consisting essentially of or consisting of one or more repeat units of the formula: -Ph-O-Ph-O-Ph-C(O)-Ph-C(O)-; - polyetheretheretherketone copolymers, also known as PEEEK, consisting essentially of or consisting of one or more repeat units of the formula: -Ph-O-Ph-O-Ph-O-Ph-C(O)- - polyether diphenyl ether ketone copolymers, also known as PEDEK, consisting essentially of or consisting of one or more repeat units of the formula: -Ph-O-Ph-Ph-O-Ph-C(O)- - and mixtures thereof; and - a copolymer comprising at least two of the repeating units mentioned above, Ph represents a phenylene group, -C(O)- represents a carbonyl group, and each phenylene may independently be of the ortho (1-2), meta (1-3) or para- (1-4) type, preferentially of the meta or para type.

[0049] In certain embodiments, the PAEK can be a PEKK consisting essentially of, or consisting of, terephthalic acid repeat units and isophthalic acid repeat units, the terephthalic acid repeat units having the formula ("T units"): [ka] and the isophthalic acid repeat unit has the formula ("I unit"): [ka]

[0050] has.

[0051] A "T unit" may also be written as -AC(=O)-BC(=O)-, and an "I unit" may also be written as -AC(=O)-DC(=O)-, where A is a p,p'-Ph-O-Ph- group, Ph is a phenylene radical, B is p-phenylene, and D is m-phenylene.

[0052] According to the invention, when the PAEK is PEKK, the isomer ratio of formula I:formula II (T:I) in the polyetherketoneketone is advantageously in the range of 50:50 to 78:22. The isomer ratio can be easily varied, for example by varying the relative amounts of the different monomers used to make the polyetherketoneketone, as may be desired to achieve a particular set of properties. These T:I isomer ratios allow both maximization of the char yield of the pyrolyzed parts and minimization of dimensional deformation of the precursor parts.

[0053] In preferred embodiments, the polyetherketoneketone copolymers can have a T:I isomer ratio of 55:45 to 75:25. In some embodiments, the polyetherketoneketones can have a T:I isomer ratio of about 55:45 to about 65:35, more particularly about 60:40. In some other embodiments, the polyetherketoneketones can have a T:I isomer ratio of about 65:35 to about 75:25, more particularly about 70:30.

[0054] A suitable polyetherketoneketone is sold under the trade name KEPSTAN® supplied by Arkema.

[0055] In certain embodiments, the PAEK is: formula: [ka] Repeating units and repeating units of: [ka] The polymer may consist essentially of, or even consist of,

[0056] In certain embodiments, the PAEK copolymer can have a molar ratio of units (III) to units (IV) of from 55:45 to 75:25.

[0057] In certain embodiments, the PAEK copolymer can have a molar ratio of units (IV) to units (III) of from 55:45 to 75:25.

[0058] In certain embodiments, the PAEK is: formula: [ka] and a repeating unit of the formula: [ka]

[0059] The polymer may consist essentially of, or consist of, repeat units of

[0060] In certain embodiments, the PAEK copolymer can have a molar ratio of units (III) to units (V) of from 55:45 to 75:25.

[0061] In certain embodiments, the PAEK copolymer can have a molar ratio of units (V) to units (III) of from 55:45 to 75:25.

[0062] reinforcement material The reinforcing material of the present invention may be an additive, a fibrous material or a mixture thereof.

[0063] In certain embodiments, the reinforcing material can be present in an amount of about 0.1%, 0.5%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 80%, or any range between the specified values, based on the weight of the total resin composition of the precursor part after melt processing.

[0064] When the reinforcing material is a reinforcing additive, it is meant in the present invention as a separate entity. The reinforcing material does not include in particular long fibers, continuous fibers, or other materials considered as fibrous materials. Among the fibers, the reinforcing additive does not include in particular fibers having a length of more than 20 mm, or in some embodiments, fibers having a length of more than 15 mm, or more than 10 mm, or more than 5 mm. The advantage of using a reinforcing additive to make a precursor part is that the reinforcing additive can increase the char content of the pyrolyzed part, improving its mechanical properties compared to a comparable part made only from polyaryletherketone. At the same time, a precursor part comprising PAEK and at least one reinforcing additive is easier to process than a precursor part made from PAEK containing long fibers, continuous fibers, or other materials considered as fibrous materials.

[0065] In certain embodiments, the reinforcing material is a toughening additive. The toughening material can be present in an amount of about 0.1% to about 70% by weight of the total resin composition. In certain embodiments, the toughening additive can be present in an amount of about 1% to about 60% by weight of the total resin composition. In certain embodiments, the toughening material can be present in an amount of about 5% to about 50% by weight of the total resin composition of the precursor part after melt processing.

[0066] In a preferred embodiment, the toughening additive may be present in an amount between 20% and 45%, especially between 25% and 40%, based on the weight of the total composition of the resin of the precursor part after melt processing.

[0067] In certain advantageous embodiments, the reinforcing additive may be one or more of a carbon-based additive, chopped fibers, a dispersant, and an inorganic additive, or a mixture thereof.

[0068] In certain embodiments, the carbon-based additive may be one or more of carbon fibers, carbon nanotubes, graphite, graphene, carbon whiskers, fullerenes, carbon black, carbon flakes, and buckyballs, and mixtures thereof. In certain embodiments, the carbon-based additive may be aligned by shear from melt processing.

[0069] In certain embodiments, the carbon-based additive can have a length of about 0.1 mm to 10 mm, about 0.5 mm to 9 mm, or about 1 mm to 8 mm. In certain embodiments, the carbon-based additive can have a length of about 0.1 mm, 0.5 mm, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, and any range between the specified values. In certain embodiments, the carbon-based additive can have a diameter of about 0.1 μm to 10 μm, about 0.5 μm to 9 μm, or about 1 μm to 8 μm. In certain embodiments, the carbon-based additive can have a diameter of about 0.1 μm, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, and any range between the specified values. The length of the additive can be measured by optical microscopy before melt compounding. The diameter of the additive can be measured by scanning electron microscopy.

[0070] In certain embodiments, the reinforcing additive can be chopped fibers. In certain embodiments, the chopped fibers include one or more of carbon, glass, silica, boron, natural fibers, and polymer fibers, and mixtures thereof. In certain embodiments, the natural fibers can be one or more of cellulose, bamboo, hemp, and jute. In certain embodiments, the polymer fibers can be one or more of polyamide, polyimide, polyaramid, polyurethane, polyester, and polyurethane, and mixtures thereof.

[0071] In certain embodiments, the chopped fibers are chopped carbon fibers. The one or more carbon fibers can have a fiber length of about 0.1 mm to 10 mm, about 0.5 mm to 9 mm, or about 1 mm to 8 mm. In certain embodiments, the chopped carbon fibers can have a fiber length of about 0.1 mm, 0.5 mm, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, and any range between the specified values. In certain embodiments, the chopped carbon fibers can have a diameter of about 0.1 μm to 10 μm, about 0.5 μm to 9 μm, or about 1 μm to 8 μm. In certain embodiments, the chopped carbon fibers can have a diameter of about 0.1 μm, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, and any range between the specified values. The length of the additive can be measured by optical microscopy prior to melt compounding, and the diameter of the additive can be measured by scanning electron microscopy.

[0072] A preferred embodiment is directed to a loading level of chopped carbon fiber of 10-45%, or 15-40%, or 20-35%, measured by weight, in a PEKK matrix having a T:I ratio of 50:50 to 78:22.

[0073] More preferred embodiments are directed to a loading level of chopped carbon fiber between 20% to 45%, more particularly 25% to 40%, as measured by weight, in a PEKK matrix having a T:I ratio of 50:50 to 78:22, more particularly a T:I ratio of about 60:40 or about 70:30.

[0074] In certain embodiments, the chopped fibers are chopped glass fibers. The one or more glass fibers can have a fiber length of about 0.1 mm to 10 mm, about 0.5 mm to 9 mm, or about 1 mm to 8 mm. In certain embodiments, the chopped glass fibers can have a fiber length of about 0.1 mm, 0.5 mm, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, and any range between the specified values. In certain embodiments, the chopped glass fibers can have a diameter of about 0.1 μm to 10 μm, about 0.5 μm to 9 μm, or about 1 μm to 8 μm. In certain embodiments, the chopped glass fibers can have a diameter of about 0.1 μm, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, and any range between the specified values. The length of the additive can be measured by optical microscopy prior to melt compounding, and the diameter of the additive can be measured by scanning electron microscopy.

[0075] A preferred embodiment is directed to a loading level of chopped glass fibers of 10-45%, or 15-40%, or 20-35%, measured by weight, in a PEKK matrix having a T:I ratio of 50:50 to 78:22.

[0076] More preferred embodiments are directed to loading levels of chopped glass fibers between 20% to 45%, more particularly 25% to 40%, as measured by weight, in a PEKK matrix having a T:I ratio of 50:50 to 78:22, more particularly a T:I ratio of about 60:40 or about 70:30.

[0077] In certain embodiments, the inorganic additive can be one or more of Group IV, V, or VI carbides, silicids, borides, and nitrides. In certain embodiments, the inorganic additive can be in powder form. In certain embodiments, the powder can have an average particle size of about 0.01 μm to 500 μm, about 0.1 μm to 250 μm, about 1 μm to 100 μm, or about 2 μm to 50 μm. In certain embodiments, the powder can have an average particle size of 0.01 μm, 0.1 μm, 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 40 μm, 50 μm, 75 μm, 100 μm, 250 μm, 500 μm, or any range between the specified values.

[0078] In certain embodiments, the toughening additive can include a dispersant. By dispersant, we mean any moiety that improves additive / particle separation and / or prevents agglomeration or settling. In certain embodiments, the dispersant can be an organosilicate, an organozirconate, an organoaluminate, or an organotitanate. In certain embodiments, the dispersant can have an average particle size of about 1 nm to 500 nm, about 2 nm to 250 nm, or about 3 nm to 100 nm. In certain embodiments, the dispersant can have an average particle size of about 1 nm, 2 nm, 3 nm, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 40 nm, 50 nm, 75 nm, 100 nm, 250 nm, 500 nm, or any range between the specified values. The particle size can be determined by scanning electron microscopy of the dispersion prior to melt compounding.

[0079] With regard to the reinforcing materials considered as fibrous materials, mention may be made of several fibers, unidirectional rovings or continuous filament mats, fabrics, felts, or nonwovens that may be in the form of strips, wraps, braids, tufts or pieces. The fibrous materials can have various forms and dimensions, either in one, two or three dimensions. They generally comprise an assembly of one or more long or continuous fibers. When the fibers are continuous, the assembly forms a fabric.

[0080] The unidirectional form corresponds to linear long fibers. The fibers may be discontinuous or continuous. The fibers may be randomly aligned or aligned parallel to each other in the form of continuous filaments. A fiber is defined by its aspect ratio, which is the ratio between the length and the diameter of the fiber. The fibers of the fibrous material are long or continuous fibers. These fibers generally have an aspect ratio of at least 1000, preferably at least 1500, more preferably at least 2000, advantageously at least 3000 and more advantageously at least 5000, even more advantageously at least 6000, even more advantageously at least 7500 and most advantageously at least 10 000.

[0081] The two-dimensional forms correspond to non-woven or woven fiber mats, or fiber reinforcements or bundles, which may also be knitted. Even if the two-dimensional form has a certain thickness and therefore in principle has a third dimension, it is still considered two-dimensional according to the invention.

[0082] The three-dimensional form corresponds to an assembly of two-dimensional forms in a third dimension, for example a non-woven fiber mat or reinforcement, or a stacked or folded bundle of fibers, or a mixture thereof.

[0083] In certain embodiments, the long or continuous fibers may be one or more of carbon, glass, silica, boron, natural fibers, and polymeric fibers, and mixtures thereof. In certain embodiments, the natural fibers may be one or more of cellulose, bamboo, hemp, and jute. In certain embodiments, the polymeric fibers may be one or more of polyamide, polyimide, polyaramid, polyurethane, polyester, and polyurethane, and mixtures thereof.

[0084] Preferably, the fibrous material is selected from inorganic fibers, more preferably, the fibrous substrate is selected from glass fibers or carbon fibers.

[0085] The fibres of the fibre material may have a diameter between 0.005 μm and 100 μm, preferably between 1 μm and 50 μm, more preferably between 5 μm and 30 μm and advantageously between 10 μm and 25 μm.

[0086] The fibers of the fibrous material have a fiber length of more than 5 mm. In some embodiments, the fibers of the fibrous material have a fiber length of more than 10 mm, or more than 15 mm, or more than 20 mm. In most cases, the fibers of the fibrous material have a fiber length of more than 20 mm.

[0087] In certain embodiments, the fiber material can be present in an amount of about 40% to about 80% by weight of the total resin composition. In certain embodiments, the fiber material can be present in an amount of about 45% to about 75% by weight of the total resin composition. In certain embodiments, the fiber material can be present in an amount of about 50% to about 70% by weight of the total resin composition of the precursor part.

[0088] A preferred embodiment is directed to long or continuous glass fibers present in an amount of 40-80%, or 45-75%, or 50-70%, measured by weight of the total composition of the resin of the precursor part, and the resin is PEKK having a T:I ratio of 50:50 to 78:22, especially a T:I ratio of about 60:40 or about 70:30.

[0089] One other preferred embodiment is directed to long or continuous glass fibers present in an amount of 40-80%, or 45-75%, or 50-70%, measured by weight of the total composition of the resin of the precursor part, and the resin is PEKK having a T:I ratio of 50:50 to 78:22, especially a T:I ratio of about 60:40 or about 70:30.

[0090] Method for manufacturing high temperature composites The present disclosure is directed to a method for preparing a carbon-carbon, carbon-ceramic matrix, or carbon-silica composite.

[0091] In certain embodiments, a method for preparing a carbon-carbon composite, a carbon ceramic matrix composite, or a carbon silica composite comprises the steps of: a. preparing a precursor part from a resin comprising a poly(aryl ether ketone) (PAEK) copolymer comprising at least two different repeat units, one of which is present in an amount of 50-78 mol % relative to the total amount of repeat units constituting the copolymer, and at least one reinforcing material; b. pyrolyzing the precursor part to produce a pyrolyzed part; c. injecting a liquid second resin into the pyrolyzed part to produce an infused part; d. pyrolyzing the injected component to produce a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite; e. optionally repeating steps (c) through (d) one or more times. Includes.

[0092] In certain embodiments, the present disclosure is directed to a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite made by the above method.

[0093] Methods involving melt processing In certain embodiments, the method may include fabricating the precursor part by melt processing.

[0094] In certain embodiments, the melt processing can be one or more of injection molding, extrusion, rotational molding, compression molding, pultrusion, filament winding, and fused filament manufacturing printing. In certain embodiments, the melt processing can optionally be followed by melt forming, such as thermoforming or rod bending.

[0095] Reinforcing materials may be added to the polyetherketoneketone as additives and / or as fibrous materials.

[0096] According to the present invention, during pyrolysis, the temperature within the chamber is increased at a rate of about 1° C. / hour to about 20° C. / hour to a peak temperature of about 1000° C.

[0097] In certain embodiments, during pyrolysis, the temperature in the chamber may be increased at a rate of about 3° C. / hr to about 17° C. / hr. In certain embodiments, during pyrolysis, the temperature in the chamber may be increased at a rate of about 5° C. / hr to about 15° C. / hr. In certain embodiments, the pyrolysis conditions during pyrolysis step b. are the same as the pyrolysis conditions during pyrolysis step d. In certain embodiments, the pyrolysis conditions during pyrolysis step b. are different from the pyrolysis conditions during pyrolysis step d.

[0098] In certain embodiments, during pyrolysis, the temperature within the chamber may be increased at a rate of about 1° C. / hr, 2° C. / hr, 3° C. / hr, 4° C. / hr, 5° C. / hr, 6° C. / hr, 7° C. / hr, 8° C. / hr, 9° C. / hr, 10° C. / hr, 11° C. / hr, 12° C. / hr, 13° C. / hr, 14° C. / hr, 15° C. / hr, 16° C. / hr, 17° C. / hr, 18° C. / hr, 19° C. / hr, 20° C. / hr, or any range between the specified values.

[0099] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10° C. / hour or greater to a temperature below 450° C. or below 400° C.

[0100] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10° C. / hour or greater to a temperature above 600° C. or above 650° C. or higher.

[0101] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of less than 10° C. / hour between 400° C. and 650° C. or between 450° C. and 600° C. In particular, the temperature in the chamber may be increased at a rate of about 1° C. / hour, 2° C. / hour, 3° C. / hour, 4° C. / hour, 5° C. / hour, 6° C. / hour, 7° C. / hour, 8° C. / hour, 9° C. / hour, 10° C. / hour between 400° C. and 650° C. or between 450° C. and 600° C.

[0102] In a preferred embodiment, during pyrolysis of the precursor part, the temperature in the chamber is increased one or more times at a rate of 10°C / hour or more at temperatures below 400°C, at a rate of less than 10°C / hour between 450°C and 600°C, and at a rate of 10°C / hour or more at temperatures above 650°C.

[0103] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10°C / hr to 15°C / hr at temperatures below 400°C, at a rate of 2°C / hr to 5°C / hr at temperatures between 450°C and 600°C, and at a rate of 10°C / hr to 15°C / hr at temperatures above 650°C.

[0104] In certain embodiments, pyrolysis can optionally include a temperature hold during pyrolysis at a temperature between 120°C and 1000°C, or between 200°C and 1000°C, or between 400°C and 1000°C. In certain embodiments, pyrolysis can be performed under nitrogen, argon, or forming gas (a mixture of hydrogen and nitrogen). In certain embodiments, pyrolysis is performed on a graphite bed. In certain embodiments, the temperature hold during pyrolysis can be about 1 hour to 72 hours, about 2 hours to 48 hours, or about 3 hours to 24 hours. In certain embodiments, the temperature hold (i.e., maintained) during pyrolysis can be about 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours, 16 hours, 20 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 ​​hours, 54 hours, 60 hours, 66 hours, 72 hours, or any range between the specified values.

[0105] In certain embodiments, pyrolysis of the precursor part can include one or more temperature holds between 400° C. and 650° C. or between 450° C. and 600° C. (inclusive) during pyrolysis. In certain embodiments, pyrolysis of the precursor part can be performed under nitrogen, argon, or forming gas (a mixture of hydrogen and nitrogen). In certain embodiments, pyrolysis of the precursor part is performed on a graphite bed. In certain embodiments, the temperature hold during pyrolysis can be about 1 hour to 72 hours, about 2 hours to 48 hours, or about 3 hours to 24 hours. In certain embodiments, the temperature hold (i.e., maintained) during pyrolysis of the precursor part can be about 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours, 16 hours, 20 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 ​​hours, 54 hours, 60 hours, 66 hours, 72 hours, or any range between the specified values.

[0106] In certain embodiments, the liquid second resin comprises, consists essentially of, or consists of one or more of pitch, benzoxazine, furfural, polyester, vinyl ester, acrylic, and phenolic resins, In certain embodiments, the liquid second resin comprises, consists essentially of, or consists of pitch, phenolic resin, or combinations thereof.

[0107] In certain embodiments, the method includes repeating the injection step c. and the pyrolysis step d. at least once. In certain embodiments, the method includes repeating the injection step c. and the pyrolysis step d. at least 2, 3, 4, 5 or more times. In certain embodiments, the char yield after the first pyrolysis cycle, or after 2, 3, 4, 5 or more cycles, can be greater than 65%, greater than 70%, greater than 75%, greater than 80%, greater than 85%, greater than 90%, or greater than 95% or higher.

[0108] In certain embodiments, the method includes repeating the infusion step c. and the pyrolysis step d. until the carbon-carbon composite, carbon-ceramic matrix composite, or carbon-silica composite is at least about 75% solid, 80% solid, 85% solid, 90% solid, 95% solid, or 99% solid, as measured according to the Examples.

[0109] In certain embodiments, the method comprises repeating steps c. through d. one or more times.

[0110] Processing of PAEK tapes or fabrics or co-woven PAEK fibres or fabrics In certain embodiments, the precursor part of step (a) is made by processing a tape or fabric, or a co-woven fiber or fabric, made from a PAEK copolymer comprising at least two different repeat units, one of the repeat units being present in an amount of 50-78 mol % relative to the total amount of repeat units constituting the copolymer, and at least one reinforcing material, by one or more of the following methods: hand layup, automated tape placement, 3D printing, filament winding, needle punching and other methods of Z-axis consolidation followed by one or more of compression molding, vacuum bag consolidation, autoclave consolidation and in situ consolidation.

[0111] In these embodiments, the reinforcing material is generally a fibrous material.

[0112] According to the present invention, during pyrolysis, the temperature within the chamber is increased at a rate of about 1° C. / hour to about 20° C. / hour to a peak temperature of about 1000° C.

[0113] In certain embodiments, during pyrolysis, the temperature in the chamber may be increased at a rate of about 3° C. / hr to about 17° C. / hr. In certain embodiments, during pyrolysis, the temperature in the chamber may be increased at a rate of about 5° C. / hr to about 15° C. / hr. In certain embodiments, the pyrolysis conditions during pyrolysis step b. are the same as the pyrolysis conditions during pyrolysis step d. In certain embodiments, the pyrolysis conditions during pyrolysis step b. are different from the pyrolysis conditions during pyrolysis step d.

[0114] In certain embodiments, during pyrolysis, the temperature within the chamber may be increased at a rate of about 1° C. / hr, 2° C. / hr, 3° C. / hr, 4° C. / hr, 5° C. / hr, 6° C. / hr, 7° C. / hr, 8° C. / hr, 9° C. / hr, 10° C. / hr, 11° C. / hr, 12° C. / hr, 13° C. / hr, 14° C. / hr, 15° C. / hr, 16° C. / hr, 17° C. / hr, 18° C. / hr, 19° C. / hr, 20° C. / hr, or any range between the specified values.

[0115] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10° C. / hour or greater to a temperature below 450° C. or below 400° C.

[0116] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10° C. / hour or greater to a temperature above 600° C. or above 650° C. or higher.

[0117] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of less than 10° C. / hour between 400° C. and 650° C. or between 450° C. and 600° C. In particular, the temperature in the chamber may be increased at a rate of about 1° C. / hour, 2° C. / hour, 3° C. / hour, 4° C. / hour, 5° C. / hour, 6° C. / hour, 7° C. / hour, 8° C. / hour, 9° C. / hour, 10° C. / hour between 400° C. and 650° C. or between 450° C. and 600° C.

[0118] In a preferred embodiment, during pyrolysis of the precursor part, the temperature in the chamber is increased one or more times at a rate of 10°C / hour or more at temperatures below 400°C, at a rate of less than 10°C / hour between 450°C and 600°C, and at a rate of 10°C / hour or more at temperatures above 650°C.

[0119] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10°C / hr to 15°C / hr at temperatures below 400°C, at a rate of 2°C / hr to 5°C / hr at temperatures between 450°C and 600°C, and at a rate of 10°C / hr to 15°C / hr at temperatures above 650°C.

[0120] In certain embodiments, pyrolysis can optionally include a temperature hold during pyrolysis at a temperature between 120°C and 1000°C, or between 200°C and 1000°C, or between 400°C and 1000°C. In certain embodiments, pyrolysis can be performed under nitrogen, argon, or forming gas (a mixture of hydrogen and nitrogen). In certain embodiments, pyrolysis is performed on a graphite bed. In certain embodiments, the temperature hold during pyrolysis can be about 1 hour to 72 hours, about 2 hours to 48 hours, or about 3 hours to 24 hours. In certain embodiments, the temperature hold (i.e., maintained) during pyrolysis can be about 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours, 16 hours, 20 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 ​​hours, 54 hours, 60 hours, 66 hours, 72 hours, or any range between the specified values.

[0121] In certain embodiments, pyrolysis of the precursor part can include one or more temperature holds between 400° C. and 650° C. or between 450° C. and 600° C. (inclusive) during pyrolysis. In certain embodiments, pyrolysis of the precursor part can be performed under nitrogen, argon, or forming gas (a mixture of hydrogen and nitrogen). In certain embodiments, pyrolysis of the precursor part is performed on a graphite bed. In certain embodiments, the temperature hold during pyrolysis can be about 1 hour to 72 hours, about 2 hours to 48 hours, or about 3 hours to 24 hours. In certain embodiments, the temperature hold (i.e., maintained) during pyrolysis of the precursor part can be about 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours, 16 hours, 20 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 ​​hours, 54 hours, 60 hours, 66 hours, 72 hours, or any range between the specified values.

[0122] In certain embodiments, the liquid second resin comprises, consists essentially of, or consists of one or more of pitch, benzoxazine, furfural, polyester, vinyl ester, acrylic, and phenolic resins, In certain embodiments, the liquid second resin comprises, consists essentially of, or consists of pitch, phenolic resin, or combinations thereof.

[0123] In certain embodiments, the method includes repeating the injection step c. and the pyrolysis step d. at least once. In certain embodiments, the method includes repeating the injection step c. and the pyrolysis step d. at least 2, 3, 4, 5 or more times. In certain embodiments, the char yield after the first pyrolysis cycle, or after 2, 3, 4, 5 or more cycles, can be greater than 65%, greater than 70%, greater than 75%, greater than 80%, greater than 85%, greater than 90%, or greater than 95% or higher.

[0124] In certain embodiments, the method includes repeating the infusion step c. and the pyrolysis step d. until the carbon-carbon composite, carbon-ceramic matrix composite, or carbon-silica composite is at least about 75% solid, 80% solid, 85% solid, 90% solid, 95% solid, or 99% solid, as measured according to the Examples.

[0125] In certain embodiments, the method comprises repeating steps c. through d. one or more times.

[0126] Methods involving aligned materials In one particular embodiment, a method for preparing a carbon-carbon composite, a carbon ceramic matrix composite, or a carbon silica composite comprises the following steps: a1) processing an aligned reinforcement material with a resin comprising a PAEK copolymer having at least two different repeat units, one of which is present in an amount of 50-78 mol % based on the total amount of repeat units constituting the copolymer, to produce an aligned reinforcement material PAEK composition and a fabric, prepreg or tape comprising the aligned reinforcement material and the impregnated PAEK; a2) processing the aligned reinforcement material and impregnated PAEK-containing fabric, prepreg or tape by hand layup, automated tape placement, 3D printing, filament winding or needle punching or other methods of Z-axis consolidation followed by compression molding, vacuum bag consolidation, autoclave consolidation, in situ consolidation to create a precursor object; c. pyrolyzing the object to produce a pyrolyzed object; d. infusing a liquid second resin into the pyrolyzed body to create an infused body; e. pyrolyzing the infused mass to produce a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite; f. Optionally, repeating steps c. through d. one or more times. Includes.

[0127] In certain embodiments, the present disclosure is directed to a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite made by the above method.

[0128] In certain embodiments, the reinforcing material is a 1-2 dimensional flake material or an aligned 1-2 dimensional platelet material. The reinforcing material can be graphite, graphene or whiskers, among others.

[0129] In certain embodiments, the 1-2D flake material or 1-2D platelet material can have a diameter of about 0.1 mm to 10 mm, about 0.5 mm to 9 mm, or about 1 mm to 8 mm. In certain embodiments, the 1-2D flake material or 1-2D platelet material can have a diameter of about 0.1 mm, 0.5 mm, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, and any range between the specified values. In certain embodiments, the 1-2D flake material or 1-2D platelet material can have a thickness of about 0.001 mm to 0.1 mm, about 0.005 mm to 0.09 mm, or about 0.01 mm to 0.08 mm. In certain embodiments, the 1-2D flake material or 1-2D platelet material can have a thickness of about 0.001 mm, 0.005 mm, 0.01 mm, 0.02 mm, 0.03 mm, 0.04 mm, 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm, 0.1 mm, and any range between the specified values. Measurements can be obtained from optical or scanning electron microscope imaging prior to melt compounding.

[0130] In certain embodiments, the process can produce a fabric comprising the aligned reinforcing material and the impregnated PAEK. In certain embodiments, the process can produce a prepreg comprising the aligned reinforcing material and the impregnated PAEK. In certain embodiments, the process can produce a tape comprising the aligned reinforcing material and the impregnated PAEK.

[0131] In certain embodiments, the aligned reinforcing additive can be produced by stretching a unidirectional tape until the fibers break and subjecting the fibers to a fluid flow to align the fibers or subjecting the fibers to an electromagnetic field to align the fibers. In certain embodiments, the aligned reinforcing additive can be produced by stretching a unidirectional tape until the fibers break (either before or after impregnation with the PAEK resin). In a preferred embodiment, the fibers are aligned by a fluid flow on a porous belt to produce a mat of aligned fibers as described in US 10,669,659.

[0132] In certain embodiments, the aligned reinforcing material can be one or more of carbon, glass, silica, boron, natural fibers, polymeric fibers, carbon nanotubes, graphite, graphene, and carbon or ceramic whiskers. In certain embodiments, the natural fibers can be one or more of cellulose, bamboo, hemp, and jute. In certain embodiments, the polymeric fibers can be one or more of polyamide, polyimide, polyaramid, polyurethane, polyester, and polyurethane.

[0133] In certain embodiments, the aligned reinforcing material can have a length of about 0.1 mm to 10 mm, about 0.5 mm to 9 mm, or about 1 mm to 8 mm. In certain embodiments, the aligned reinforcing additive can have a fiber length of about 0.1 mm, 0.5 mm, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, and any range between the specified values.

[0134] In certain embodiments, in situ consolidation can include rolling to apply pressure and / or heat.

[0135] In certain embodiments, during pyrolysis, the temperature in the chamber may be increased at a rate of about 1° C. / hr to about 20° C. / hr to a peak temperature of about 1000° C. In certain embodiments, during pyrolysis, the temperature in the chamber may be increased at a rate of about 3° C. / hr to about 17° C. / hr. In certain embodiments, during pyrolysis, the temperature in the chamber may be increased at a rate of about 5° C. / hr to about 15° C. / hr. In certain embodiments, the pyrolysis conditions during pyrolysis step c. are the same as the pyrolysis conditions during pyrolysis step e. In certain embodiments, the pyrolysis conditions during pyrolysis step c. are different from the pyrolysis conditions during pyrolysis step e.

[0136] In certain embodiments, during pyrolysis, the temperature within the chamber may be increased at a rate of about 1° C. / hr, 2° C. / hr, 3° C. / hr, 4° C. / hr, 5° C. / hr, 6° C. / hr, 7° C. / hr, 8° C. / hr, 9° C. / hr, 10° C. / hr, 11° C. / hr, 12° C. / hr, 13° C. / hr, 14° C. / hr, 15° C. / hr, 16° C. / hr, 17° C. / hr, 18° C. / hr, 19° C. / hr, 20° C. / hr, or any range between the specified values.

[0137] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10° C. / hour or greater to a temperature below 450° C. or below 400° C.

[0138] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10° C. / hour or greater to a temperature above 600° C. or above 650° C. or higher.

[0139] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of less than 10° C. / hour between 400° C. and 650° C. or between 450° C. and 600° C. In particular, the temperature in the chamber may be increased at a rate of about 1° C. / hour, 2° C. / hour, 3° C. / hour, 4° C. / hour, 5° C. / hour, 6° C. / hour, 7° C. / hour, 8° C. / hour, 9° C. / hour, 10° C. / hour between 400° C. and 650° C. or between 450° C. and 600° C.

[0140] In a preferred embodiment, during pyrolysis of the precursor part, the temperature in the chamber is increased one or more times at a rate of 10°C / hour or more at temperatures below 400°C, at a rate of less than 10°C / hour between 450°C and 600°C, and at a rate of 10°C / hour or more at temperatures above 650°C.

[0141] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10°C / hr to 15°C / hr at temperatures below 400°C, at a rate of 2°C / hr to 5°C / hr at temperatures between 450°C and 600°C, and at a rate of 10°C / hr to 15°C / hr at temperatures above 650°C.

[0142] In certain embodiments, pyrolysis can optionally include a temperature hold during pyrolysis. In certain embodiments, pyrolysis can be performed under nitrogen, argon, or forming gas. In certain embodiments, pyrolysis is performed on a graphite bed. In certain embodiments, the temperature hold during pyrolysis can be about 1 hour to 72 hours, about 2 hours to 48 hours, or about 3 hours to 24 hours. In certain embodiments, the temperature hold during pyrolysis can be about 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours, 16 hours, 20 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 ​​hours, 54 hours, 60 hours, 66 hours, 72 hours, or any range between the specified values.

[0143] In certain embodiments, pyrolysis of the precursor part can include one or more temperature holds between 400° C. and 650° C. or between 450° C. and 600° C. (inclusive) during pyrolysis. In certain embodiments, pyrolysis of the precursor part can be performed under nitrogen, argon, or forming gas (a mixture of hydrogen and nitrogen). In certain embodiments, pyrolysis of the precursor part is performed on a graphite bed. In certain embodiments, the temperature hold during pyrolysis can be about 1 hour to 72 hours, about 2 hours to 48 hours, or about 3 hours to 24 hours. In certain embodiments, the temperature hold (i.e., maintained) during pyrolysis of the precursor part can be about 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours, 16 hours, 20 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 ​​hours, 54 hours, 60 hours, 66 hours, 72 hours, or any range between the specified values.

[0144] In certain embodiments, the precursor bodies may be melt-formed after processing step a. but before pyrolysis step c.

[0145] In certain embodiments, the liquid second resin can be one or more of pitch, benzoxazine, furfural, polyester, vinyl ester, acrylic, and phenolic resins, with pitch, phenolic resins, or combinations thereof being preferred in certain embodiments.

[0146] In certain embodiments, the method includes repeating the injection step d. and the pyrolysis step e. at least once. In certain embodiments, the method includes repeating the injection step d. and the pyrolysis step e. at least 2, 3, 4, or 5 times. In certain embodiments, the char yield after the first pyrolysis cycle, or after 2, 3, 4, 5, or more cycles, can be greater than 65%, 70%, 75%, 80%, 85%, 90%, or 95% or higher.

[0147] In certain embodiments, the method includes repeating the infusion step d. and the pyrolysis step e. until the carbon-carbon composite, carbon-ceramic matrix composite, or carbon-silica composite is at least about 75% solid, 80% solid, 85% solid, 90% solid, 95% solid, or 99% solid.

[0148] In certain embodiments, steps c. to d. are repeated one or more times.

[0149] Processes involving impregnation or co-weaving steps in the presence of one reinforcing additive In certain embodiments, the present disclosure is directed to a method of making a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite.

[0150] In one particular embodiment, a method for making a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite includes the following: a1) impregnating a continuous fiber tape or fabric with a resin comprising a poly(aryl ether ketone) (PAEK) copolymer containing at least two different repeat units, one of which is present in an amount of 50-78 mol % relative to the total amount of repeat units constituting the copolymer, and at least one reinforcing additive, to produce a filled PEKK tape or fabric; a2) processing the filled PEKK tape or fabric or co-woven PEKK / fiber material to create a precursor part by hand layup, automated tape placement, 3D printing, filament winding or needle punching or other methods of Z-axis consolidation followed by compression molding, vacuum bag consolidation, autoclave consolidation or in situ consolidation; c. pyrolyzing the precursor part to produce a pyrolyzed part; d. injecting a liquid second resin into the pyrolyzed part to produce an infused part; e. pyrolyzing the injected component to produce a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite; Includes.

[0151] In certain embodiments, the present disclosure is directed to a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite made by the above method.

[0152] In certain embodiments, the method includes impregnating a continuous fiber tape or fabric with a resin comprising PAEK and at least one additive to create a filled PAEK tape, hi certain embodiments, the method includes co-weaving a continuous fiber or fabric with PAEK fibers comprising PAEK and at least one additive to create a filled PAEK tape or fabric.

[0153] In one particular embodiment, the continuous fibers or fabric may be carbon fibers.

[0154] In certain embodiments, the reinforcing additive may be one or more of a carbon-based additive, a chopped fiber, a dispersant, and an inorganic additive.

[0155] In certain embodiments, the additive may be present in an amount of about 0.01% to about 30% by weight of the total resin composition. In certain embodiments, the additive may be present in an amount of about 0.1% to about 25% by weight of the total resin composition. In certain embodiments, the additive may be present in an amount of about 1% to about 20% by weight of the total resin composition.

[0156] In certain embodiments, the additives can be present in an amount of about 0.01%, 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 15%, 20%, 25%, 30% by weight of the total resin composition, or any range between the specified values.

[0157] In certain embodiments, the additive can be a carbon-based additive. In certain embodiments, the carbon-based additive can be one or more of carbon fiber, carbon nanotube, graphite, graphene, carbon whisker, fullerene, carbon black, carbon flake, and buckyball. In certain embodiments, the carbon-based additive can be aligned by shear from melt processing.

[0158] In certain embodiments, the carbon-based additive can have a length of about 0.1 mm to 10 mm, about 0.5 mm to 9 mm, or about 1 mm to 8 mm. In certain embodiments, the carbon-based additive can have a length of about 0.1 mm, 0.5 mm, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, and any range between the specified values. In certain embodiments, the carbon-based additive can have a diameter of about 0.1 μm to 10 μm, about 0.5 μm to 9 μm, or about 1 μm to 8 μm. In certain embodiments, the carbon-based additive can have a diameter of about 0.1 μm, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, and any range between the specified values.

[0159] In certain embodiments, the additive can be chopped fibers. In certain embodiments, the chopped fibers include one or more of carbon, glass, silica, boron, natural fibers, and polymer fibers. In certain embodiments, the natural fibers can be one or more of cellulose, bamboo, hemp, and jute. In certain embodiments, the polymer fibers can be one or more of polyamide, polyimide, polyaramid, polyurethane, polyester, and polyurethane.

[0160] In certain embodiments, the chopped fibers are chopped carbon fibers. The one or more carbon fibers can have a fiber length of about 0.1 mm to 10 mm, about 0.5 mm to 9 mm, or about 1 mm to 8 mm. In certain embodiments, the chopped carbon fibers can have a fiber length of about 0.1 mm, 0.5 mm, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, and any range between the specified values. In certain embodiments, the chopped carbon fibers can have a diameter of about 0.1 μm to 10 μm, about 0.5 μm to 9 μm, or about 1 μm to 8 μm. In certain embodiments, the chopped carbon fibers can have a diameter of about 0.1 μm, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, and any range between the specified values.

[0161] In certain embodiments, the additive can be an inorganic additive. In certain embodiments, the inorganic additive can be one or more of carbides, silicides, borides, and nitrides of Group IV, V, or VI. Carbides and silicides are preferred, with silicon carbide being most preferred. In certain embodiments, the inorganic additive can be in powder form. In certain embodiments, the powder can have an average particle size of about 0.01 μm to 500 μm, about 0.1 μm to 250 μm, about 1 μm to 100 μm, or about 2 μm to 50 μm. In certain embodiments, the average particle size of the powder can be 0.01 μm, 0.1 μm, 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 40 μm, 50 μm, 75 μm, 100 μm, 250 μm, 500 μm, or any range between the specified values.

[0162] In certain embodiments, the additive can include a dispersant. In certain embodiments, the dispersant can be an organosilicate, an organozirconate, an organoaluminate, or an organotitanate, with organosilicates and organotitanates being preferred, and organosilicates being most preferred. In certain embodiments, the dispersant can have an average pore size of about 1 nm to 500 nm, about 2 nm to 250 nm, or about 3 nm to 100 nm. In certain embodiments, the dispersant can have an average pore size of about 1 nm, 2 nm, 3 nm, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 40 nm, 50 nm, 75 nm, 100 nm, 250 nm, 500 nm, or any range between the specified values.

[0163] In certain embodiments, in situ consolidation can include rolling to apply pressure and / or heat.

[0164] In certain embodiments, during pyrolysis, the temperature in the chamber may be increased at a rate of about 1° C. / hr to about 20° C. / hr to a peak temperature of about 1000° C. In certain embodiments, during pyrolysis, the temperature in the chamber may be increased at a rate of about 3° C. / hr to about 17° C. / hr. In certain embodiments, during pyrolysis, the temperature in the chamber may be increased at a rate of about 5° C. / hr to about 15° C. / hr. In certain embodiments, the pyrolysis conditions during pyrolysis step c. are the same as the pyrolysis conditions during pyrolysis step e. In certain embodiments, the pyrolysis conditions during pyrolysis step c. are different from the pyrolysis conditions during pyrolysis step e.

[0165] In certain embodiments, during pyrolysis, the temperature within the chamber may be increased at a rate of about 1° C. / hr, 2° C. / hr, 3° C. / hr, 4° C. / hr, 5° C. / hr, 6° C. / hr, 7° C. / hr, 8° C. / hr, 9° C. / hr, 10° C. / hr, 11° C. / hr, 12° C. / hr, 13° C. / hr, 14° C. / hr, 15° C. / hr, 16° C. / hr, 17° C. / hr, 18° C. / hr, 19° C. / hr, 20° C. / hr, or any range between the specified values.

[0166] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10° C. / hour or greater to a temperature below 450° C. or below 400° C.

[0167] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10° C. / hour or greater to a temperature above 600° C. or above 650° C. or higher.

[0168] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased at a rate of less than 10° C. / hour one or more times between 400° C. and 650° C. or between 450° C. and 600° C. In particular, the temperature in the chamber may be increased at a rate of about 1° C. / hour, 2° C. / hour, 3° C. / hour, 4° C. / hour, 5° C. / hour, 6° C. / hour, 7° C. / hour, 8° C. / hour, 9° C. / hour, 10° C. / hour between 400° C. and 650° C. or between 450° C. and 600° C.

[0169] In a preferred embodiment, during pyrolysis of the precursor part, the temperature in the chamber is increased one or more times at a rate of 10°C / hour or more at temperatures below 400°C, at a rate of less than 10°C / hour between 450°C and 600°C, and at a rate of 10°C / hour or more at temperatures above 650°C.

[0170] In certain embodiments, during pyrolysis of the precursor parts, the temperature in the chamber is increased one or more times at a rate of 10°C / hr to 15°C / hr at temperatures below 400°C, at a rate of 2°C / hr to 5°C / hr at temperatures between 450°C and 600°C, and at a rate of 10°C / hr to 15°C / hr at temperatures above 650°C.

[0171] In certain embodiments, pyrolysis can optionally include a temperature hold during pyrolysis. In certain embodiments, pyrolysis can be performed under nitrogen, argon, or forming gas. In certain embodiments, pyrolysis is performed on a graphite bed. In certain embodiments, the temperature hold during pyrolysis can be about 1 hour to 72 hours, about 2 hours to 48 hours, or about 3 hours to 24 hours. In certain embodiments, the temperature hold during pyrolysis can be about 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours, 16 hours, 20 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 ​​hours, 54 hours, 60 hours, 66 hours, 72 hours, or any range between the specified values.

[0172] In certain embodiments, pyrolysis of the precursor part can include one or more temperature holds between 450° C. and 600° C. (inclusive) during pyrolysis. In certain embodiments, pyrolysis of the precursor part can be performed under nitrogen, argon, or forming gas (a mixture of hydrogen and nitrogen). In certain embodiments, pyrolysis of the precursor part is performed on a graphite bed. In certain embodiments, the temperature hold during pyrolysis can be about 1 hour to 72 hours, about 2 hours to 48 hours, or about 3 hours to 24 hours. In certain embodiments, the temperature hold (i.e., maintained) during pyrolysis of the precursor part can be about 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours, 16 hours, 20 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 ​​hours, 54 hours, 60 hours, 66 hours, 72 hours, or any range between the specified values.

[0173] In certain embodiments, the precursor bodies may be melt-formed after processing step b. but before pyrolysis step c.

[0174] In certain embodiments, the liquid second resin can be one or more of pitch, benzoxazine, furfural, polyester, vinyl ester, acrylic, and phenolic resins.

[0175] In certain embodiments, the method includes repeating the injection step d. and the pyrolysis step e. at least once. In certain embodiments, the method includes repeating the injection step d. and the pyrolysis step e. at least 2, 3, 4, or 5 or more times. In certain embodiments, the char yield after the first pyrolysis cycle, or after 2, 3, 4, 5 or more cycles, can be greater than 65%, greater than 70%, greater than 75%, greater than 80%, greater than 85%, greater than 90%, or greater than 95% or higher.

[0176] In certain embodiments, the method includes repeating the infusion step d. and the pyrolysis step e. until the carbon-carbon composite, carbon-ceramic matrix composite, or carbon-silica composite is at least about 75% solid, 80% solid, 85% solid, 90% solid, 95% solid, or 99% solid. EXAMPLES

[0177] The methods and products described herein will now be further described with reference to the following examples. These examples are presented for illustrative purposes only, and the embodiments described herein should in no way be construed as being limited to these examples. Rather, the embodiments should be construed to encompass any and all variations that become evident as a result of the teachings presented herein.

[0178] Example 1 Effect of T / I ratio on PEKK samples PEKK with various T / I ratios (60 / 40; 80 / 20) and 30% chopped fibers (either glass or carbon), as well as neat PEKK or PEEK samples ("Table 1") were produced by injection molding, pyrolyzed in quartz crucibles in a muffle furnace under inert environment, and subjected to the pyrolysis cycle described in Table 2. Their initial dimensions were all approximately 5.1 cm x 1.3 cm x 0.3 cm. PEEK was a homopolymer made from repeating units of formula (III).

[0179] [Table 1]

[0180] [Table 2]

[0181] Samples A and B were weighed, their thickness (t) was measured before and after pyrolysis, the char yield was calculated, and the dimensional change (Table 3) was determined.

[0182] The char yield was calculated from the mass of each sample before and after pyrolysis ("Equation 1"):

[0183]

number

[0184] (In the formula, w b and w a are the masses of the sample before and after pyrolysis, respectively).

[0185] The parameter Δt was calculated by the difference between the thickness after pyrolysis and the thickness at 25° C. before pyrolysis divided by the thickness at 25° C. before pyrolysis (expressed as a percentage).

[0186] [Table 3]

[0187] Neat PEKK (Sample C) exhibited significantly higher char yields upon pyrolysis compared to neat PEEK (Sample D), thus favoring the PEKK repeat unit compared to the PEEK repeat unit.

[0188] PEKK with a T:I ratio of 60:40 and filled with chopped fiber (Sample A) showed a slight improvement in char yield and an almost 3x reduction in sample expansion as measured by dimensional change in thickness when compared to PEKK with a T:I ratio of 80:20 and filled with chopped fiber (Sample B), indicating that there is an optimum in the PAEK copolymer repeat unit ratio that minimizes expansion while still obtaining similar char yields.

Claims

1. 1. A method for making a high temperature composite, which is a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite, comprising: a. preparing a precursor part from a resin comprising a poly(aryl ether ketone) (PAEK) copolymer comprising at least two different repeat units, one of the repeat units being present in an amount of 50-78 mol % relative to the total amount of repeat units constituting the copolymer, and at least one reinforcing material; b. pyrolyzing the precursor parts into pyrolyzed parts; c. injecting a liquid second resin into the pyrolyzed part to produce an infused part; d. pyrolyzing the injected component to produce a carbon-carbon composite, a carbon-ceramic matrix composite, or a carbon-silica composite; and optionally repeating steps c. through d. one or more times.

2. 2. The method of claim 1, wherein the PAEK copolymer consists essentially of, or consists of, two repeat units.

3. 3. The method of claim 2, wherein the PAEK copolymer is a polyetherketoneketone (PEKK) having a T:I ratio of 50:50 to 78:22, preferably 55:45 to 75:

25.

4. 3. The method of claim 2, wherein the PEKK has a T:I ratio of about 55:45 to about 65:

35.

5. 3. The method of claim 2, wherein the PEKK has a T:I ratio of about 65:35 to about 75:

25.

6. During pyrolysis, the temperature within the chamber is increased to a peak temperature of about 1000° C. or greater; the temperature in the chamber is increased one or more times during the pyrolysis at a rate of between 1° C. / hr and about 20° C. / hr, and optionally the pyrolysis is maintained at one or more temperatures for a period of time; 6. The method according to any one of claims 1 to 5.

7. 7. The method of any one of claims 1 to 6, wherein during pyrolysis of the precursor part, the temperature in the chamber is increased one or more times between 450°C and 600°C at a rate of less than 10°C / h, and optionally maintained for a period of time at one or more temperatures between 450°C and 600°C, inclusive.

8. 8. The method according to claim 1, wherein during pyrolysis of the precursor part, the temperature in the chamber is increased one or more times at a rate of 10° C. / h or more at a temperature below 400° C. and / or above 650° C.

9. 9. The method of any one of claims 1 to 8, wherein the liquid second resin comprises one or more of pitch, benzoxazine, furfural, polyester, vinyl ester, acrylic and phenolic resins.

10. 10. The method of claim 1, wherein the precursor part is made by melt processing a resin comprising poly(aryl ether ketone) and at least one reinforcing material.

11. 11. The method of claim 10, wherein melt processing comprises one or more of injection molding, extrusion, rotational molding, compression molding, pultrusion, filament winding, and fused filament manufacturing printing.

12. The precursor part of step (a) comprises: a1) impregnating a continuous fiber tape or fabric with a resin comprising a poly(aryl ether ketone) (PAEK) copolymer comprising at least two different repeat units, one of which is present in an amount of 50-78 mol % based on the total amount of repeat units constituting the copolymer, and at least one reinforcing additive, to produce a filled PAEK tape or fabric, or co-weaving the continuous fiber or fabric with a PAEK fiber comprising PAEK and at least one reinforcing additive to produce a filled co-woven PAEK fiber or fabric; and a2) processing the filled PAEK tape or fabric, or co-woven PAEK fiber or fabric, by one or more of the following methods: hand layup, automated tape placement, 3D printing, filament winding, needle punching and other methods of Z-axis consolidation followed by one or more of compression molding, vacuum bag consolidation, autoclave consolidation and in situ consolidation to create a precursor part. The method of any one of claims 1 to 10, wherein the compound is produced by

13. The precursor part of step (a) comprises: a1) processing an aligned reinforcement material with a resin comprising a PAEK copolymer comprising at least two different repeat units, one of the repeat units being present in an amount of 50-78 mol % based on the total amount of repeat units making up the copolymer, to produce an aligned reinforcement material PAEK composition to produce a fabric, prepreg or tape comprising the aligned reinforcement material and impregnated PAEK; a2) processing the aligned reinforcement material and impregnated PAEK-containing fabric, prepreg or tape by hand layup, automated tape placement, 3D printing, filament winding or needle punching, or other methods of Z-axis consolidation followed by compression molding, vacuum bag consolidation, autoclave consolidation, in situ consolidation to create a precursor object. The method of any one of claims 1 to 10, wherein the compound is produced by

14. 14. The method according to any one of claims 1 to 13, wherein the reinforcing material comprises one or more reinforcing additives selected from carbon-based additives, chopped fibers, inorganic additives or mixtures thereof; fibrous materials comprising long fibers, continuous fibers or mixtures thereof; or mixtures thereof.

15. 15. The method of any one of claims 1 to 14, wherein the reinforcing material comprises a carbon-based additive that is one or more of carbon fibers, carbon nanotubes, graphite, graphene, carbon whiskers, fullerenes, carbon black, carbon flakes, buckyballs, and mixtures thereof.

16. 16. The method of any one of claims 1 to 15, wherein the reinforcing material comprises chopped, long or continuous fibers that are one or more of carbon, glass, silica, boron, natural fibers, polymeric fibers and mixtures thereof.

17. 17. The method of any one of claims 1 to 16, wherein the reinforcing material comprises an inorganic additive which is one or more of a Group IV, V or VI carbide, silicide, boride or nitride, and / or ceramic whiskers.

18. 18. The method of any one of claims 1 to 17, wherein the precursor part comprises a dispersing agent which is an organosilicate, an organozirconate, an organoaluminate or an organotitanate.

19. 14. The method according to any one of claims 1 to 13, wherein the reinforcing material is chopped carbon fibre or chopped glass fibre.

20. 14. The method according to any one of claims 1 to 13, wherein the reinforcing material is long or continuous carbon fibres or long or continuous glass fibres.

21. 14. The method according to any one of claims 1 to 13, wherein the reinforcing material is a mixture of chopped fibres and long or continuous fibres.

22. 11. The method of any one of claims 1 to 10, wherein the precursor part of step (a) is made by processing a tape or fabric, or a co-woven PAEK fiber or fabric, made from a PAEK copolymer comprising at least two different repeat units, one of the repeat units being present in an amount of 50-78 mol % with respect to the total amount of repeat units constituting the copolymer, and at least one reinforcing material, by one or more of the following methods: hand layup, automated tape placement, 3D printing, filament winding, needle punching and other methods of Z-axis consolidation followed by one or more of compression molding, vacuum bag consolidation, autoclave consolidation and in situ consolidation.

23. 23. A carbon-carbon, carbon-ceramic matrix or carbon-silica composite made by the method of any one of claims 1 to 22.