Cookware that realizes anti-stick effect by pure inorganic structure layer and its manufacturing method
A cooking utensil with a layered inorganic structure addresses the limitations of existing non-stick materials by using inorganic particles to create a void structure for oil storage and self-lubrication, achieving effective non-stick performance and durability.
Patent Information
- Application Number
- JP2024522395
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-09
- Filing Date
- 2023-06-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-13
AI Technical Summary
Existing non-stick cookware materials, such as fluorinated organic compounds and silica sol resin, suffer from high-temperature degradation, poor heat resistance, and environmental safety concerns, while ceramic and enamel materials lack non-stick properties and require complex manufacturing processes.
A cooking utensil with a pure inorganic structural layer formed by spraying inorganic particles onto a base layer, creating a communicating void structure with three sub-layers of varying particle sizes to achieve non-stick functionality through oil storage and self-lubrication.
The inorganic structural layer provides high bonding strength, toughness, and non-stick properties with easy cleaning, maintaining a non-stick effect by boiling oil and fat to separate food, and is resistant to high temperatures and scratches.
Smart Images

Figure 2024545389000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of kitchenware, and in particular to a cookware having a non-stick layer and a method for manufacturing the same. [Background technology]
[0002] Non-stick cookware, especially non-stick pans, is the mainstream cookware product currently on the market, and is mainly realized by forming a layer of non-stick material on the surface of the pan base material.
[0003] In the prior art, the main component of a general non-stick material is a fluoro-organic compound such as polytetrafluoroethylene, and the non-wetting property of the fluoro-organic compound can be used to provide a non-stick function to cooking utensils. However, the decomposition of the fluoro-organic compound under high temperature conditions (for example, polytetrafluoroethylene exceeds 250°C) can damage the fluoro-organic compound coating, causing the cooking utensil to lose its non-stick function, and also generating toxic substances after the decomposition of the fluoro-organic compound coating, which may be harmful to human health.
[0004] The main component of another non-sticky material is silica sol resin, which, like fluorine-based organic compound materials, has excellent non-stick properties. However, due to the characteristics of the material itself, it has severe limitations in terms of heat resistance, hardness, durability, and environmental safety, and is unable to fully meet the demands of the market and consumers.
[0005] It has also been proposed to use ceramics and enamel as non-stick materials to manufacture non-stick cookware. Although ceramics and enamel have characteristics such as good appearance, super heat resistance, high hardness, durability and environmental protection, the materials themselves do not have any non-stick properties and have low non-stick effects whether oiled or not. Therefore, they are generally used in products such as soup pots and stew pots and cannot be mass-produced.
[0006] At present, anti-stick structures with many fine grooves or capillary pores formed on the inner surface of cooking utensils have been released on the market, which can reduce the contact area between the food ingredients and the inner surface of the cooking utensil during cooking, and can adsorb oil and fat into the grooves and capillary pores on the inner surface of the cooking utensil. During cooking, the oil and fat in the grooves and capillary pores expands and is released from the grooves and capillary pores, forming a layer of oil film on the bottom of the cooking utensil, thus producing the effect of "anti-sticking". After heating is stopped, the edible oil is cooled and stored in the grooves and capillary pores on the inner surface of the cooking utensil. Therefore, cooking utensils with the above structure can maintain a certain function for a long time, but the structure of such small grooves or capillary pores has a significant effect on the anti-sticking properties of the cooking utensil, and a specific structure is required to achieve a good anti-sticking effect, so there are high requirements for the manufacturing process, etc. Summary of the Invention
[0007] To solve the above problems, the present invention provides a cookware and a manufacturing method thereof that realizes the anti-stick effect by using a pure inorganic structural layer.
[0008] According to one aspect of the present invention, the cooking utensil includes a base layer and a pure inorganic structural layer, and the pure inorganic structural layer is formed by spraying inorganic particles onto an inner surface of the base layer, and a communicating void structure is formed between the inorganic particles of the pure inorganic structural layer, and the inorganic particles sprayed onto the inner surface of the base layer are pure inorganic particles to which no organic solvent is added, The purely inorganic structural layer includes at least three sub-inorganic structural layers, which are stacked on the inner surface of the substrate layer in order according to the particle size of the inorganic particles, wherein the particle size of the inorganic particles in the sub-inorganic structural layer adjacent to the substrate layer is the largest, and the particle sizes of the inorganic particles in the multiple sub-inorganic structural layers become smaller in order in the direction away from the substrate layer, whereby the voids in the multiple sub-inorganic structural layers become smaller in order in the direction away from the substrate layer.
[0009] In one embodiment, the particle size of the inorganic particles is 100 nm-60 μm, the inorganic particles are plasma sprayed, supersonic sprayed, cold sprayed, laser cladding or airless sprayed onto the inner surface of the substrate layer, and the thickness of the pure inorganic structural layer is 61-130 μm.
[0010] In one embodiment, the inorganic particulate material is a metal particle, a ceramic particle, or a carbon powder, the metal particle being one or more of titanium, a titanium alloy, zirconium, a zirconium alloy, stainless steel, low carbon steel, high carbon steel, and zinc, the ceramic particle being one or more of zirconium oxide, zirconium nitride, titanium oxide, titanium nitride, titanium carbide, aluminum oxide, magnesium oxide, iron oxide, iron sesquioxide, boron nitride, calcium oxide, silicon oxide, and silicon nitride, and the carbon powder being one or more of natural graphite, polycrystalline graphite, pyrolytic graphite, highly oriented pyrolytic graphite, and carbon quantum dots.
[0011] In one embodiment, the three sub-inorganic structural layers are an oil reservoir layer, a sustained release hardening layer and a dispersion surface layer, and the oil reservoir layer, the sustained release hardening layer and the dispersion surface layer are arranged in order in a direction away from the substrate layer.
[0012] In one embodiment, the oil reservoir layer, the sustained release curing layer and the dispersing surface layer are layered in sequence.
[0013] In one embodiment, the particle size of the inorganic particles in the oil reservoir layer is 15-60 μm, the layer thickness of the oil reservoir layer is 40-70 μm, and the porosity is 15-25%; the particle size of the inorganic particles in the sustained release hardened layer is 1-15 μm, the layer thickness of the sustained release hardened layer is 20-40 μm, and the porosity is 5-15%; the particle size of the inorganic particles in the dispersed surface layer is 100 nm-1 μm, and the layer thickness of the dispersed surface layer is 1-20 μm.
[0014] In one embodiment, the weight ratio of ceramic particles in the oil reservoir layer is 70% or more, the weight ratio of metal particles in the sustained release hardened layer is 60% or more, and the weight ratio of carbon powder in the dispersed surface layer is 50% or more.
[0015] According to another aspect of the present invention, a method for manufacturing the cookware includes the steps of: A metal substrate is formed by drawing or die casting, and then burrs are removed, and the surface is polished and cleaned to form a substrate layer having a thickness of 1 mm or more; spraying inorganic particles onto an inner surface of a substrate layer by cold spraying, plasma spraying, supersonic spraying, laser cladding or airless spraying to form a purely inorganic structural layer; Includes.
[0016] Beneficial Effects of the Invention In the cookware having a pure inorganic structure layer of the present invention, the pure inorganic structure layer includes at least three sub-inorganic structure layers, which are stacked on the inner surface of the base layer in order according to the particle size of the inorganic particles, and the particle size of the inorganic particles in the sub-inorganic structure layers decreases in order away from the base layer, so that the void structure in the sub-inorganic structure layers decreases in order away from the base layer, and the pure inorganic structure layer has high bonding strength and toughness, high surface hardness, scratch resistance, and wear resistance, and when there is oil in the pan, it can absorb the oil on its surface, and has the functions of oil storage and self-lubrication. After heating, the voids can perform heating and breathing of the pores, thereby achieving the effects of anti-sticking and easy cleaning. [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 is a cross-sectional view of a container wall of a cooking utensil having a purely inorganic structural layer as proposed in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] In order to make the objectives, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below with reference to specific embodiments and drawings. Those skilled in the art can understand that the present invention is not limited to the drawings and the following embodiments.
[0019] As used herein, the term "including" and various variations thereof may be understood as open terms, meaning "including but not limited to." The term "based on" and similar expressions may be understood as "based at least on." The terms "first," "second," "third," and the like, are merely used to distinguish different features and have no substantive meaning. The terms "left," "right," "middle," and the like, are merely used to indicate the positional relationship between relative objects.
[0020] According to one embodiment of the present invention, a cooking utensil that realizes a non-stick effect by a pure inorganic structural layer is provided. The cooking utensil includes a base layer 1 and a pure inorganic structural layer 2. The pure inorganic structural layer 2 is formed by spraying inorganic particles on the inner surface of the base layer 1. A void structure is formed between the inorganic particles of the pure inorganic structural layer 2. The inorganic particles sprayed on the inner surface of the base layer are pure inorganic particles to which no organic solvent is added. The pure inorganic structural layer 2 includes at least three sub-inorganic structural layers. The at least three sub-inorganic structural layers are stacked on the inner surface of the base layer 1 in order according to the particle size of the inorganic particles. The particle size of the inorganic particles of the sub-inorganic structural layer adjacent to the base layer 1 is the largest, and the particle size of the inorganic particles of the multiple sub-inorganic structural layers becomes smaller in the direction away from the base layer 1, so that the voids in the multiple sub-inorganic structural layers become smaller in the direction away from the base layer 1.
[0021] Specifically, Fig. 1 shows a cross-sectional view of the container wall of a cooking utensil. The cooking utensil in Fig. 1 is preferably a frying pan, depending on the conditions and effects of use. The cooking utensil includes a base layer 1 and a pure inorganic structural layer 2.
[0022] The base layer 1 is the base of the cookware and is usually made of a metal material such as an aluminum alloy, stainless steel or iron, and its thickness is usually 1 mm or more.
[0023] The pure inorganic structural layer 2 according to the embodiment of the present invention is formed by spraying inorganic particle material on the inner surface of the substrate layer 1. The particle size of the inorganic particles is 100nm-60μm. The spraying can be realized by plasma spraying, supersonic spraying, cold spraying, laser cladding technology, airless spraying, etc. The thickness of the pure inorganic structural layer 2 is 61-130μm.
[0024] The inorganic particle material may be metal particles, ceramic particles or carbon powder. The metal particles may be one or more of titanium, titanium alloy, zirconium, zirconium alloy, stainless steel, low carbon steel, high carbon steel and zinc. The ceramic particles may be one or more of zirconium oxide, zirconium nitride, titanium oxide, titanium nitride, titanium carbide, aluminum oxide, magnesium oxide, iron oxide, iron sesquioxide, boron nitride, calcium oxide, silicon oxide and silicon nitride. The carbon powder may be one or more of natural graphite, polycrystalline graphite, pyrolytic graphite, highly oriented pyrolytic graphite and carbon quantum dots. Because a spray process is used, the inorganic particles of the pure inorganic structural layer 2 do not adhere to each other, and a void structure is formed between the inorganic particles.
[0025] The purely inorganic structural layer 2 includes at least three sub-inorganic structural layers stacked in order according to the particle size of the inorganic particles. The particle size of the inorganic particles in the sub-inorganic structural layer adjacent to the base layer 1 is the largest. In the direction away from the base layer 1, the particle sizes of the inorganic particles in the multiple sub-inorganic structural layers become smaller in order.
[0026] In this embodiment, the three sub-inorganic structure layers are an oil reservoir layer 21, a sustained release hardened layer 22 and a dispersion surface layer 23, which are stacked in order. The particle size of the inorganic particles of the oil reservoir layer 21 is 15-60 μm. The inorganic particles may be one or more of the metal particles, ceramic particles or carbon powder. The layer thickness of the oil reservoir layer 21 is 40-70 μm, and the porosity is 15-25%. The particle size of the inorganic particles of the sustained release hardened layer 22 is 1-15 μm. The inorganic particles may be one or more of the metal particles, ceramic particles or carbon powder. The layer thickness of the sustained release hardened layer 22 is 20-40 μm, and the porosity is 5-15%. The particle size of the inorganic particles of the dispersion surface layer 23 is 100 nm-1 μm. The inorganic particles may be one or more of the metal particles, ceramic particles or carbon powder. The layer thickness of the dispersion surface layer 23 is 1-20 μm. The "dispersed" surface layer in the present invention refers to inorganic particles not completely covering the sustained-release cured layer 22. For example, the inorganic particles cover the sustained-release cured layer 22 evenly dispersedly as independent particles, and / or form a plurality of sub-regions of the surface layer uniformly distributed in the form of cracks on the sustained-release cured layer 22, so that the dispersed surface layer 23 does not block the sustained-release cured layer 22, and the surface of the dispersed surface layer 23 has an uneven matte state.
[0027] In the three sub-inorganic structure layers, i.e., the oil reservoir layer 21, the sustained release hardened layer 22 and the dispersion surface layer 23, the particle size of the inorganic particles increases in the order of the oil reservoir layer 21, the sustained release hardened layer 22 and the dispersion surface layer 23, and therefore the voids formed between the inorganic particles also increase in the order of the oil reservoir layer 21, the sustained release hardened layer 22 and the dispersion surface layer 23.
[0028] In addition, in this embodiment, the particle size of the inorganic particles in the dispersion surface layer 23 is 100nm-1μm, which is much smaller than the particle size (15-60μm) of the inorganic particles in the oil reservoir layer 21 and the particle size (1-15μm) of the inorganic particles in the sustained release hardened layer 22, so the voids in the oil reservoir layer 21 are relatively large and are used to store fats and oils. The voids in the dispersion surface layer 23 are very small and relatively dense and uniform, which can improve the hardness of the dispersion surface layer 23 and facilitate the uniform penetration or precipitation of fats and oils. In addition, the sustained release hardened layer 22, whose inorganic particles have a medium particle size, is provided between the oil reservoir layer 21 and the dispersion surface layer 23. This layer is a transition layer, which has the effect of hardening the coating layer, effectively bonding the oil storage layer 21 and the dispersion surface layer 23, improving the bonding strength and toughness of the pure inorganic structure layer 2, and playing the role of assisting oil storage. When the cookware starts to heat up, as the temperature of the cookware increases, the oil and gas mixture needs to fill the sustained-release hardened layer 22 before it precipitates from the dispersion surface layer 23, and the degree of heating of the cookware can be estimated by the amount of oil and fat precipitated from the bottom of the cookware.
[0029] Preferably, the main component of the oil storage layer 21 is ceramic particles, and the weight ratio of the ceramic particles is 70% or more. The main component of the sustained release hardened layer 22 is metal particles, and the weight ratio of the metal particles is 60% or more. The main component of the dispersed surface layer 23 is carbon powder, and the weight ratio of the carbon powder is 50% or more. As a result, the lower layer is a ceramic layer mainly composed of ceramic particles as the oil storage layer, and this layer is mainly a porous layer with stable structure, high strength and high hardness. The second layer is a composite metal layer mainly composed of metal particles as the sustained release layer, and this layer improves the toughness of the lower ceramic layer, optimizes the pore structure, improves the pore density, reduces the pore size, improves the stability of the stored oil, and gives the surface a relatively high metallic texture. The third layer is a surface layer mainly made of carbon powder-like material, which provides a self-lubricating functional layer with a self-lubricating effect, the surface friction coefficient of the dispersed surface layer 23 is small, and in the presence of oil, the dynamic friction coefficient is small, making it easy to clean the surface of the pure inorganic structure layer 2, and having high physical anti-stick properties.
[0030] As a result of the deposition of materials, the purely inorganic structure layer 2 has a three-dimensional structure with voids that is capable of storing oil, and an uneven structure is formed on the surface of the purely inorganic structure layer 2. Due to the uneven structure, parts of the food ingredients float up, and the heated oil and fat in the food ingredients and the voids on the surface boil slightly, generating a large amount of hot gas, which pushes the food ingredients further up, separating the food ingredients from the surface and achieving a certain degree of physical anti-stick effect.
[0031] The invention will now be described using a non-stick frying pan as an example.
[0032] During the cooking process, when the non-stick frying pan is heated, the voids / pores in the pure inorganic structure layer 2 expand due to heat, so that it has a very strong adsorption power for fats and oils. After oil is added to the non-stick frying pan, the oil completely wets and fills the pores. When it is further heated, the fats and oils in the voids will boil slightly and generate hot gas, so that during the cooking process, the slightly boiled fats and oils and hot gases are located between the food and the pure inorganic structure layer 2, and push up the food, thereby realizing the separation of the food and the pure inorganic structure layer 2. After the cooking is completed, as the fats and oils are taken by the food and the temperature of the non-stick frying pan decreases, the temperature of the fats and oils in the voids of the pure inorganic structure layer 2 decreases, the volume shrinks, and the fats and oils remain. Even if the surface of the non-stick frying pan is washed, some fats and oils are still retained in the voids of the coating layer 2, especially in the voids of the oil reservoir layer 21. When it is heated again, the fats and oils are precipitated from the voids, so that the oil-wet state of the pan bottom is maintained. Therefore, the working principle of the non-stick frying pan of this embodiment is as follows: when the non-stick frying pan is continuously heated, the fats and oils in the pores of the pure inorganic structure layer 2 are continuously kept boiling and generate a large amount of hot gas, so that the cooked ingredients are pushed up to the bottom of the non-stick frying pan so that they partially float, thereby realizing the technical effect of "non-stick". In addition, for the non-stick frying pan of this embodiment, the fats and oils remaining in the pores can be replaced by boiling and cleaning the non-stick frying pan in hot water after cooking, so that the non-stick frying pan can be thoroughly cleaned.
[0033] Although this embodiment only shows three sub-inorganic structural layers stacked in sequence, those skilled in the art can understand that in order to further improve the bonding strength and toughness of the pure inorganic structural layer 2, one or more sustained release hardening layers with different inorganic particle size may be included between the oil reservoir layer 21 and the dispersion surface layer 23, which is within the protection scope of the present invention.
[0034] According to another embodiment of the present invention, there is provided a method for manufacturing the cookware, comprising the following steps S1 and S2. S1: Forming the base layer A metal substrate such as an aluminum alloy, stainless steel, or iron is formed by drawing or die casting, and then burrs are removed, and the surface is polished and cleaned to form a substrate layer 1 having a thickness of 1 mm or more. S2: The substrate layer 1 is sprayed to form a purely inorganic structural layer 2.
[0035] Inorganic particles are applied to the inner surface of the substrate layer 1 by cold spraying, plasma spraying, supersonic spraying, laser cladding or airless spraying to form a purely inorganic structural layer 2. Note that the laser cladding referred to here is a type of hot spraying.
[0036] In a preferred embodiment of the present invention, the substrate is preheated to 80-120°C, and inorganic particles, the main component of which is ceramic particles (70% by weight or more), are sprayed on the inner surface of the substrate layer 1 by plasma spraying or supersonic spraying to form an oil reservoir layer 21. Preferably, for example, plasma spraying is performed under conditions of voltage 55-65V, current 500-600A, adjusting the supply amount of inorganic particles to 4-8mg / s, and using hydrogen gas with a flow rate of 4-8L / m to spray inorganic particles on the inner surface of the substrate layer 1 at a spray distance of 10-15mm to form an oil reservoir layer 21 with a coating thickness of 40-70μm and porosity of 15-25%. For a 30cm frying pan, it is necessary to spray for 50-90s. This layer serves as a base coating layer to ensure the hardness and strength of the pure inorganic structural layer 2, and builds a base void layer with a thickness of 40-70μm.
[0037] Then, the inorganic particles, the main component of which is metal particles (60% by weight or more), are sprayed on the outer surface of the oil reservoir 21 by cold spraying process and supersonic spraying process to form a sustained release hardened layer 22. Preferably, for cold spraying, nitrogen gas with a temperature of 200-400°C is used as the propellant gas, the spray pressure is controlled to 2.0-3.5MPa, and the gas flow rate is controlled to 500-900m / s. Metal particle powder is sent into the gas along the axial direction of the propellant gas to form a gas-solid two-phase flow, and spraying is performed at a position 10-25mm from the outer surface of the oil reservoir 21 to form a sustained release hardened layer 22 with a spray thickness of 2-40μm and a porosity of 5-15%. For a 30cm frying pan, it is necessary to spray for 30-60s. In the spraying process, the oil reservoir 21 is subjected to appropriate hole filling, secondary deposition and surface improvement to form a fine micro-nano morphology, and the voids become finer and finer.
[0038] Finally, the inorganic particles, the main component of which is carbon powder (50% by weight or more), are sprayed on the outer surface of the sustained-release hardened layer 22 by laser cladding or spraying process to form the dispersion surface layer 23. Preferably, the spraying process is exemplified by spraying carbon powder resin at a pressure of 0.4-0.6 MPa at a position 10-25 mm away from the outer surface of the sustained-release hardened layer 22, and then sintering and hardening is performed at a temperature of 330°C for 8-12 minutes, forming a dispersion surface layer 23 with a thickness of 1-20 μm and a self-lubricating function on the surface of the sustained-release hardened layer 22, and the surface of the dispersion surface layer 23 is in an uneven matte state.
[0039] The non-stick frying pan according to the embodiment of the present invention is manufactured by the above manufacturing method. Here, the material of the substrate layer is stainless steel, and the thickness of the substrate layer is 1.2 mm. The pure inorganic structure layer is composed of three sub-inorganic structure layers, namely, the oil reservoir layer 21, the sustained release hardening layer 22, and the dispersion surface layer 23. The oil reservoir layer 21 contains 72% by weight of ceramic particles, the inorganic particles have a particle size of 35 μm, the layer thickness is 60 μm, and the porosity is 20%. The sustained release hardening layer 22 contains 64% by weight of metal particles, the inorganic particles have a particle size of 10 μm, the layer thickness is 30 μm, and the porosity is 15%. The dispersion surface layer 23 contains 50% by weight of carbon powder, the inorganic particles have a particle size of 300 nm, and the layer thickness is 5 μm.
[0040] Physical Indicator Detection 1. Hardness: The pencil hardness is over 9H, and it cannot be scratched by a steak knife, shovel or steel wool. 2. Extreme heat resistance: Even when placed in a 500°C oven and heated continuously for one hour, there was no cracking or discoloration on the surface, and no weight loss or other phenomena occurred. 3. Thermal shock: After heating the workpiece to 400°C, it was placed in water at 20°C and subjected to 50 consecutive shocks. No cracks, discoloration or other changes were observed on the surface. 4. Test method for non-stick properties 1. Fried egg After seasoning according to the standard method, it was washed thoroughly. The pan was heated to 150℃, sprayed with oil spray three times (about 5g of oil), heated to 160℃, and eggs were added. It was observed that the eggs were prevented from burning. No more oil was used and the eggs were continued to be fried. This product was able to fry six eggs consecutively without burning under continuous heating conditions without adding oil. 2. Stir-fried shredded pork (two methods) Hot frying pan / cold oil: Heat a pan to 200℃ and add oil. Immediately after adding the oil, add marinated shredded pork and stir fry. No burning was observed. Hot frying pan and hot oil: Heat a pan to 200℃, add oil, and heat until the oil starts to smoke slightly. After adding marinated shredded pork and frying, it was observed that the food did not burn.
[0041] In the present description, reference to terms such as "one embodiment," "some embodiments," "examples," "particular examples," or "some examples" means that the specific features, structures, materials, or characteristics described with reference to the embodiment or example are included in at least one embodiment or example of the present invention. In the present description, schematic expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.
[0042] The above is a description of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention should be included within the scope of protection of the present invention.
Claims
1. A cookware that achieves a non-stick effect by a purely inorganic structural layer, The cooking utensil includes a base layer (1) and a purely inorganic structural layer (2), the purely inorganic structural layer (2) is formed by spraying inorganic particles on the inner surface of the base layer (1), and a void structure that communicates between the inorganic particles of the purely inorganic structural layer (2) is formed; The purely inorganic structural layer (2) includes at least three sub-inorganic structural layers, which are stacked on the inner surface of the base layer (1) in order according to the particle size of the inorganic particles, and wherein the particle size of the inorganic particles in the sub-inorganic structural layer adjacent to the base layer (1) is the largest, and the particle sizes of the inorganic particles in the multiple sub-inorganic structural layers become smaller in order in the direction away from the base layer (1), thereby causing the voids in the multiple sub-inorganic structural layers to become smaller in order in the direction away from the base layer (1).
2. The cookware of claim 1, characterized in that the inorganic particles have a particle size of 100nm-60μm, the inorganic particles are plasma sprayed, supersonic sprayed, cold sprayed, laser cladding or airless sprayed on the inner surface of the substrate layer (1), and the thickness of the pure inorganic structural layer (2) is 61-130μm.
3. 2. The cookware of claim 1, wherein the inorganic particulate material is metal particles, ceramic particles or carbon powder, the metal particles are one or more of titanium, titanium alloy, zirconium, zirconium alloy, stainless steel, low carbon steel, high carbon steel and zinc, the ceramic particles are one or more of zirconium oxide, zirconium nitride, titanium oxide, titanium nitride, titanium carbide, aluminum oxide, magnesium oxide, iron tetraoxide, iron sesquioxide, boron nitride, calcium oxide, silicon oxide and silicon nitride, and the carbon powder is one or more of natural graphite, polycrystalline graphite, pyrolytic graphite, highly oriented pyrolytic graphite and carbon quantum dots.
4. The cooking utensil according to claim 1, characterized in that the three sub-inorganic structural layers are an oil storage layer (21), a sustained-release hardening layer (22) and a dispersion surface layer (23), and the oil storage layer (21), the sustained-release hardening layer (22) and the dispersion surface layer (23) are arranged in order in a direction away from the base layer (1).
5. The cooking utensil according to claim 4, characterized in that the oil storage layer (21), the slow-release hardening layer (22) and the dispersing surface layer (23) are laminated in order.
6. The cooking utensil according to claim 5, characterized in that the diameter of the inorganic particles in the oil reservoir layer (21) is 15-60 μm, the layer thickness of the oil reservoir layer (21) is 40-70 μm, and the porosity is 15-25%; the diameter of the inorganic particles in the sustained-release hardened layer (22) is 1-15 μm, the layer thickness of the sustained-release hardened layer (22) is 20-40 μm, and the porosity is 5-15%; the diameter of the inorganic particles in the dispersion surface layer (23) is 100 nm-1 μm, and the layer thickness of the dispersion surface layer (23) is 1-20 μm.
7. The cooking utensil according to claim 5, characterized in that the weight ratio of ceramic particles in the oil storage layer (21) is more than 70%, the weight ratio of metal particles in the sustained release hardening layer (22) is more than 60%, and the weight ratio of carbon powder in the dispersed surface layer (23) is more than 50%.
8. A method for manufacturing a cookware according to any one of claims 1 to 7, comprising the steps of: A step of forming a metal substrate by drawing or die casting, removing burrs, polishing the surface and cleaning the substrate to form a substrate layer (1) having a thickness of 1 mm or more; Spraying inorganic particles onto the inner surface of the substrate layer (1) by cold spraying, plasma spraying, supersonic spraying, laser cladding or airless spraying to form a purely inorganic structural layer (2); A manufacturing method comprising the steps of:
Citation Information
Patent Citations
Composite material and preparation method thereof, cooking device and household electrical appliance
CN110757915A
Heating cooker
JP1998174654A
Non-stick cook surface
US20050208272A1