Polypropylene Composition for Retort Packaging Applications
A polypropylene composition with specific ratios of homopolypropylene, random copolymer polypropylene, and propylene-ethylene copolymer addresses seal contamination and speed issues in retort packaging by providing high seal strength at lower temperatures, improving manufacturing efficiency and reducing waste.
Patent Information
- Application Number
- JP2019133575
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-12
- Filing Date
- 2019-07-19
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2039-07-19
AI Technical Summary
Current retort packaging processes face issues with slow manufacturing speeds due to manual cleaning, human errors, and seal contamination during high-pressure sterilization, leading to packaging waste and food waste, with existing solutions focusing on increasing seal initiation temperatures or altering resin polarity.
A polypropylene composition comprising 50-76% homopolypropylene, 12-25% random copolymer polypropylene with 2-10% ethylene-derived units, and 12-25% propylene-ethylene copolymer with 10-25% ethylene-derived units, optimized for low seal initiation temperatures and improved mechanical properties, reducing seal contamination.
The composition achieves high seal strength with lower initiation temperatures, preventing food leakage and seal contamination during sterilization, enhancing production efficiency and reducing waste.
Smart Images

Figure 0007551283000007 
Figure 0007551283000013 
Figure 0007551283000009
Abstract
Description
[Technical field]
[0001] Various embodiments relate to the polypropylene composition, a method of making molded articles using the polypropylene composition, molded articles made with the polypropylene composition, and the use of the molded articles in retort packaging applications. [Background technology]
[0002] A retort package (also known as a retort pouch or retortable pouch) is a type of packaging made of a laminate of flexible plastic and metal foil that is used to aseptically package a wide variety of foods and pharmaceuticals in aseptic processing, as an alternative to traditional industrial canning, to aseptically package heat-sterilized products in sterile containers, and to produce stable products that do not require refrigeration.
[0003] Generally, retort packaging includes multiple layers of laminated film to meet various demands from users. For example, the multi-layered laminated film can include a first outer layer intended for direct contact with the external environment, a second outer layer disposed on the opposite side of the multi-layered laminated film intended for direct contact with the packaged product, and one or more middle layers disposed between the first and second outer layers. The first outer layer is on the outside of the package and is visible to the user. Therefore, the first outer layer of the package can generally be designed to have printable properties. Thus, the first outer layer can serve an important function in terms of aesthetics or appearance of the packaged product. In addition, the first outer layer can act as a protective layer to maintain the integrity of the retort package against puncture forces. One or more of the middle layers can function as a barrier layer to prevent the penetration of moisture and / or oxygen through the package. In addition, one or more of the middle layers can function as a sealant layer to bond or join the various layers of the package using heat and pressure to form a laminated film. Meanwhile, the second outer layer, which is in direct contact with the packaged product, can also function as a sealant layer, acting alone or in conjunction with a middle sealant layer to enable the package contents to be sealed upon heating.
[0004] Currently, each retort package is manually cleaned after packaging, slowing down the production rate of the packaged product and introducing human error into the cleaning process. It is therefore desirable to improve the cleaning speed of retort packages to increase the production rate of the packaged product and prevent human error. This can be done industrially using high pressure processing conditions or thermal pasteurization (also called sterilization), but it is necessary that the seal provided by the retort package remain intact during these harsh conditions to prevent the contents of the retort package from leaking and contaminating the seal.
[0005] Currently, this leakage problem remains unsolved in the production line, resulting in a lot of packaging waste and food waste. Therefore, the film layers that make up the retort packaging must meet requirements such as good mechanical properties and strong adhesion between the layers of the package to ensure a good seal and avoid contamination of the seal.
[0006] Furthermore, for the sealing process of retort packages, especially in the use of retort packages for food products, it is desirable to have a packaging process carried out at a lower or at least lower seal initiation temperature compared to the state of the art methods. As used herein, the seal initiation temperature (SIT), also called the seal initial temperature, is the lowest temperature at which a seal is formed with a certain seal strength. Considering that the food product is in direct contact with the package, this is advantageous for the quality preservation of the food product. Furthermore, a lower seal initiation temperature means that a lower temperature can be set at the sealing bar, which leads to an improvement in speed in the production of retort packages.
[0007] Previous attempts to prevent or substantially avoid seal contamination have included (1) increasing the seal initiation temperature of the polypropylene resin to form a completely sealed polypropylene film layer, and / or (2) improving the polarity of the polypropylene resin to make the food more fluid relative to the resulting polypropylene film.
[0008] Notwithstanding the above, there remains a need for an improved sealant layer that overcomes or at least mitigates one or more of the above-mentioned problems. This may be in the form of an improved material for forming the sealant layer (e.g., the polypropylene composition disclosed herein) and a molded article made therefrom. This allows for high seal strength, preferably low seal initiation temperature, and has been demonstrated to reduce seal contamination. Summary of the Invention
[0009] In a first aspect, there is provided a polypropylene composition comprising: (a) 50-76% by weight homopolypropylene; (b) 12% to 25% by weight of a random copolymer polypropylene having 2% by mole to 10% by mole of units derived from ethylene; and (c) 12% to 25% by weight of a propylene-ethylene copolymer having 10% to 25% by weight of units derived from ethylene.
[0010] In a second aspect, there is provided a method of producing a molded article, the method comprising providing a polypropylene composition comprising 50% to 76% by weight of a homopolypropylene, 12% to 25% by weight of a random copolymer polypropylene having 2% to 10% by mole of units derived from ethylene, and 12% to 25% by weight of a propylene-ethylene copolymer having 10% to 25% by weight of units derived from ethylene, and molding the polypropylene composition into a molded article.
[0011] In a third aspect, there is provided a shaped article obtainable by the method of the second aspect.
[0012] In a fourth aspect, there is provided a molded article comprising a polypropylene composition comprising 50% by weight to 76% by weight of a homopolypropylene, 12% by weight to 25% by weight of a random copolymer polypropylene having 2 mol% to 10 mol% of units derived from ethylene, and 12% by weight to 25% by weight of a propylene-ethylene copolymer having 10% by weight to 25% by weight of units derived from ethylene.
[0013] In a fifth aspect, there is provided the use of the molded article in a retort packaging application.
[0014] Further advantages and features of the subject matter of the present application are illustrated below by way of example with accompanying drawings. [Brief description of the drawings]
[0015] [Figure 1A]FIG. 1A shows the seal strength (N / 15 mm) versus seal temperature (° C.) for Comparative Sample 1A and Samples 2A, 3A, and 4A. [Figure 1B] FIG. 1B shows the seal strength (N / 15 mm) versus seal temperature (° C.) for Comparative Sample 1A and Samples 2A, 5A and 6A. [Figure 2A] FIG. 2A shows the seal strength of films (obtained for polypropylene compositions according to samples 2A, 3A and 4A) measured by hot tack test, shown as force (N / 25.4 mm) versus temperature (° C.). [Figure 2B] FIG. 2B shows the seal strength of films (obtained for polypropylene compositions according to samples 2A, 5A and 6A) measured by hot tack test, shown as force (N / 25.4 mm) versus temperature (° C.). [Diagram 3] Figure 3 shows a comparison of the seal strength of films (obtained for polypropylene compositions according to Comparative Sample 1A and Samples 2A and 3A) before and after retort treatment. The seal strength after retort treatment was measured on the side of the food-containing retort package. No contamination was observed. [Figure 4A] 4A is a photograph showing a retort pouch of Comparative Sample 1A, showing food leakage and contamination of the seal as indicated by the circled area in the figure. [Figure 4B] Figure 4B is a photograph showing the retort pouch of Sample 2A. No food leakage or contamination of the seal was observed. [Figure 4C] Figure 4C is a photograph showing the retort pouch of Sample 3A. No food leakage or contamination of the seal was observed. [Figure 4D] Figure 4D is a photograph showing the retort pouch of Sample 4A. No food leakage or contamination of the seal was observed. [Figure 4E] Figure 4E is a photograph showing the retort pouch of Sample 5A. No food leakage or contamination of the seal was observed. [Figure 4F]Figure 4F is a photograph showing the retort pouch of Sample 6A. No food leakage or contamination of the seal was observed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] In a first aspect, a polypropylene composition is provided that includes: (a) 50% to 76% by weight of homopolypropylene; (b) 12% to 25% by weight of random copolymer polypropylene having 2% to 10% by mole of ethylene-derived units; and (c) 12% to 25% by weight of propylene-ethylene copolymer having 10% to 25% by weight of ethylene-derived units. For simplicity, the homopolypropylene, random copolymer polypropylene, and propylene-ethylene copolymer contained in the polypropylene composition may be referred to herein as component (a), component (b), and component (c), respectively. The weight percentages of components (a), (b), and (c) in the propylene composition are calculated based on the total weight of the polypropylene composition. In various embodiments, the polypropylene composition consists of components (a), (b), and (c), i.e., the weight percentages of components (a), (b), and (c) total 100% by weight.
[0017] Advantageously, the polypropylene composition of the present disclosure or the molded article produced therefrom has good seal and low seal initiation temperature throughout performance. For example, retort packaging formed from the film produced from the polypropylene composition disclosed herein does not leak food during sterilization and packaging process, which makes the polypropylene composition suitable for use in retort packaging applications. The polypropylene composition provided according to the embodiments disclosed herein can substantially avoid the seal contamination problem caused by the use of polypropylene. The selection and relative amount of polymers included in the polypropylene composition disclosed herein have been demonstrated to exhibit synergy to obtain target properties between mechanical properties and seal performance, which may be due to factors such as polymer chain entanglement, seal initiation temperature and seal contamination.
[0018] In particular, it has been demonstrated that the incorporation of random copolymer polypropylene and propylene-ethylene copolymer into a polypropylene composition in an amount of at least 12% by weight and no more than 25% by weight of the polypropylene composition, respectively, can improve the mechanical properties, such as the strength, of the film prepared using the composition.For example, the addition of random copolymer polypropylene can act as a compatibilizer to improve the diffusion of the propylene-ethylene copolymer phase in a homopolypropylene matrix, which can result in improved mechanical properties of the molded article, such as a monolayer film, a multilayer film, or a retort package, prepared using the polypropylene composition.
[0019] Also, careful consideration should be given to the melt flow rate and melting point of each of components (a), (b) and (c), which can be controlled by the comonomers of components (b) and (c). Propylene-ethylene copolymers can function to reduce the seal initiation temperature of the polypropylene composition, since the propylene-ethylene copolymer can be melted at a lower temperature. Advantageously, the formulation of the polypropylene composition disclosed herein can be adjusted within the claimed ranges to provide an optimized balance between mechanical and sealing properties, so that the resulting retort package can be tailored depending on the intended use, such as, for example, the contents and size of the retort package. In an embodiment, both components (b) and (c) are propylene-based copolymers, which means that each of components (b) and (c) contains at least 50% by weight of propylene-derived repeat units. Components (b) and (c) may have sufficiently low melting points based on their particular comonomer content, provided that they are in at least 12 wt.% polypropylene composition, an amount sufficient to lower the overall melting point of the composition, which is advantageous for lowering the seal initiation temperature. Furthermore, the compositions of the present disclosure according to various embodiments exhibit substantially retained seal strength even after the harsh conditions of sterilization, including heating to 121° C., due to the respective amounts and distribution of comonomers in components (b) and (c).
[0020] The term "composition" as used herein refers to a blend of polymers, such as homopolymers, random copolymers, block polymers, terpolymers, or combinations thereof, where the polymers are already polymerized and do not participate in further polymerization during blending. In this context, a polypropylene composition includes a physical blend of homopolypropylene, random copolymer polypropylene, and propylene-ethylene copolymer. This composition is also referred to as a "resin blend."
[0021] As used herein, the term "homopolypropylene" refers to a polymer consisting essentially of or consisting of repeat units derived from propylene. Homopolypropylene can, for example, contain at least 99.0% by weight of repeat units derived from propylene, more preferably at least 99.5% by weight, even more preferably at least 99.95% by weight, even more preferably at least 99.99% by weight, or 100% by weight.
[0022] According to various embodiments, the homopolypropylene may be present in the polypropylene composition in an amount of 50% to 76% by weight, such as an amount of 60% to 76% by weight, or an amount of 60% to 70% by weight. In some aspects, the homopolypropylene comprises at least 60% by weight of the polypropylene composition. According to various embodiments, the homopolypropylene may have a melt flow rate of 1 g / 10 min to 10 g / 10 min at 230° C., 2.16 kg per ASTM D 1238-13, or 2 g / 10 min to 5 g / 10 min at 230° C., 2.16 kg, or 2 g / 10 min to 4 g / 10 min, 2.16 kg per ASTM D 1238-13. The homopolypropylene may have a molecular weight distribution (Mw / Mn) of 4 g / mol to 15 g / mol, more preferably 5 g / mol to 10 g / mol. The concentration of the homopolypropylene is 0.88 g / cm 3 ~0.92g / cm 3 , more preferably 0.89 g / cm 3 ~0.91g / cm 3 It is.
[0023] The homopolypropylene may have a melting point, as measured by differential scanning calorimetry (DSC), in the range of 150° C. to 170° C., more preferably in the range of 160° C. to 165° C. If the melting point is below this range, for example below 160° C., the resulting molded article may have low heat resistance and may not be suitable for retort packaging applications.
[0024] In addition to homopolypropylene, the polypropylene composition also includes random copolymer polypropylene. The term "random copolymer polypropylene" as used herein means a polymer containing repeat units derived from propylene and at least one other comonomer, for example, 2, 3, 4 or 5 other comonomers. The random copolymer polypropylene may contain at least 50% by weight of propylene-derived units, or more than 50% by weight of propylene-derived units, and at least 0.05% by weight, more preferably at least 0.1% by weight, and even more preferably at least 0.4% by weight of repeat units derived from at least one other comonomer. According to various embodiments, the repeat units derived from at least one other comonomer in the random copolymer polypropylene are 15% by weight or less. The other comonomer may be selected from any α-olefin except propylene, and may be, for example, C2- 12 C2- such as alkylene 20 The other comonomer may be an alkylene. Thus, the other comonomer may be selected from the group consisting of ethylene, butylene, pentylene, hexylene, heptylene, octylene, nonylene, decylene, and combinations thereof.
[0025] In various embodiments, the other comonomer is an ethylene-derived unit. Thus, the random copolymer polypropylene can contain up to 10 mol% of ethylene-derived units, for example, 2 mol% to 10 mol% of ethylene-derived units, 3 mol% to 9 mol% of ethylene-derived units, 4 mol% to 8 mol% of ethylene-derived units, 2 mol% to 7 mol% of ethylene-derived units, 2 mol% to 5 mol% of ethylene-derived units, or 2 mol% to 4 mol% of ethylene-derived units, or about 3 mol% of ethylene-derived units.
[0026] According to various embodiments, the random copolymer polypropylene may be present in an amount of 12% to 25% by weight, or the random copolymer polypropylene may be present in an amount of 15% to 25% by weight, or the random copolymer polypropylene may be present in an amount of 15% to 20% by weight. Alternatively, the random copolymer polypropylene may be present in an amount of 25% by weight. Advantageously, when the random copolymer polypropylene is present in an amount of 25% by weight, the resulting polypropylene composition has a viscosity of 287 kg / cm 2 It can exhibit an extremely high tensile strength at break of 726% and an extremely high elongation at break of 726%.
[0027] Preferably, the random copolymer polypropylene has a melt flow rate (MFR) according to ASTM D 1238-13 of 5 g / 10 min to 10 g / 10 min at 230° C. and 2.16 kg, more preferably an MFR of 6.5 g / 10 min to 7.5 g / 10 min, even more preferably an MFR of 7.0 g / 10 min to 7.5 g / 10 min.
[0028] In various embodiments, the random copolymer polypropylene may have a melting point in the range of 140° C. to 165° C., such as in the range of 145° C. to 155° C. or 150° C. to 160° C., as measured by differential scanning calorimetry.
[0029] The polypropylene composition disclosed herein also includes a propylene-ethylene copolymer. The term "propylene-ethylene copolymer" as used herein refers to a copolymer comprising repeat units derived from propylene and ethylene. In various embodiments, the propylene-ethylene copolymer comprises at least 50% by weight of propylene-derived units, for example, at least 60% by weight or at least 70% by weight of propylene-derived units. In addition to the repeat units derived from propylene and ethylene, the copolymer may be further derived from additional comonomers such as butylene and / or other α-olefins having 5 to 18 carbon atoms. Alternatively, it may consist essentially or completely of repeat units derived from propylene and ethylene.
[0030] According to various embodiments, the propylene-ethylene copolymer may have 10% to 25% by weight of ethylene derived units, such as 15% to 20% by weight of ethylene derived units, or about 16% by weight of ethylene derived units. The ethylene units may be randomly distributed in the propylene polymer, which may be isotactic. In the context of the present disclosure, the low crystalline copolymer of propylene / α-olefin has a melt flow rate of about 0.2 dg / min to about 20 dg / min, a melting point of about 80° C. to about 150° C., and a viscosity of about 0.88 g / cm. 3 ~Approx. 0.92g / cm 3 has a concentration of
[0031] The inclusion of a propylene-ethylene copolymer in the polypropylene composition advantageously improved the mechanical strength of the resulting polypropylene composition according to the embodiments disclosed herein. According to various embodiments, the propylene-ethylene copolymer may be present in an amount of 12% to 25% by weight, or 15% to 25% by weight, or 15% to 20% by weight. Alternatively, the propylene-ethylene copolymer may be present in the polypropylene composition in an amount of 20% to 25% by weight. Advantageously, when the propylene-ethylene copolymer is present in the polypropylene composition at least 20% by weight, the resulting polypropylene composition has a mechanical strength of 261 kg / cm. 2 or 244kg / cm 2 and very high elongation at break of 664% and 676%.
[0032] According to various embodiments, the propylene-ethylene copolymer has a MFR of 0.1 g / 10 min to 15 g / 10 min, measured according to ASTM D1238 at 230° C. and 2.16 kg. All individual values and subranges from 0.1 g / 10 min to 15 g / 10 min are included herein and disclosed herein; for example, the propylene-ethylene copolymer can have a melt flow rate of 0.1 g / 10 min to 10 g / 10 min, e.g., 0.2 g / 10 min to 10 g / 10 min, 0.5 g / 10 min to 10 g / 10 min, 1 g / 10 min to 10 g / 10 min, 2 g / 10 min to 10 g / 10 min, 2.5 g / 10 min to 10 g / 10 min. In some embodiments, the propylene-ethylene copolymer has a MFR of 2.5 g / 10 min to 15 g / 10 min.
[0033] Preferably, the propylene-ethylene copolymer may have a molecular weight distribution (Mw / Mn) of 3.5 g / mol or less, preferably 3.0 g / mol or less, more preferably from 1.8 g / mol to 3.0 g / mol.
[0034] In one embodiment, components (a), (b) and (c) of the polypropylene composition have a melting point from 145°C to 165°C.
[0035] Homopolypropylene and random copolymer polypropylene can be prepared by any conventional method known in the art. For example, homopolypropylene and random copolymer polypropylene can be produced in a reactor or multi-reactor in the presence of a catalyst system. The catalyst system can include a Ziegler-Natta catalyst or a metallocene catalyst. In certain embodiments, the catalyst system includes a Ziegler-Natta catalyst.
[0036] The polypropylene compositions of the present disclosure can be prepared using any method known in the art, including, but not limited to, mechanical mixing using a Banbury-type high shear internal mixer or direct mixing in a twin screw extruder.
[0037] According to various embodiments, the composition may have a melt flow rate of 0.1 g / 10 min to 4.0 g / 10 min at 230° C. and 2.16 kg per ASTM D 1238-13.
[0038] Preferred polypropylene compositions of the present disclosure may include at least two, and more preferably all, of the following characteristics: (i) MFR between 0.1 g / 10 min and 4.0 g / 10 min; (ii) Sealing strength of 15N / 15mm~30N / 15mm (iii) A seal initiation temperature of 165°C for a seal strength of at least 15N / 15mm.
[0039] The polypropylene compositions of the present disclosure and the molded articles prepared therefrom may contain various additives that can impart specific properties to the molded articles. Additives known to those skilled in the art that can be used in these blends include, but are not limited to, fillers such as talc and calcium carbonate, pigments, antioxidants, stabilizers, corrosion inhibitors, slip agents, and antiblocking agents.
[0040] The polypropylene compositions of the present disclosure are particularly well suited for use in blown film processing and / or coextrusion casting to prepare molded articles, which may be, for example, films, layers, or sheets.
[0041] Thus, in a second aspect, there is provided a method for producing a molded article, the method comprising the steps of providing a polypropylene composition comprising 50% to 76% by weight of homopolypropylene, 12% to 25% by weight of random copolymer polypropylene having 2% to 10% by mole of units derived from ethylene, and 12% to 25% by weight of a propylene-ethylene copolymer having 10% to 25% by weight of units derived from ethylene, and molding the polypropylene composition into a molded article. The homopolypropylene, random copolymer polypropylene and propylene-ethylene copolymers that can be used have already been discussed above.
[0042] In various embodiments, forming the polypropylene composition into a molded article includes blown film processing, film casting, and / or co-extrusion of the polypropylene composition. The blown film processing, film casting, and / or co-extrusion can be performed according to methods known in the art. Furthermore, the film or sheet material of the present disclosure may be laminated with other materials after each blown film processing, film casting, and / or extrusion. Also, known techniques for laminating sheets and films can be applied to form these laminates.
[0043] Thus, in a third aspect, there is provided a moulded article obtainable by the method as described above.
[0044] In a fourth aspect, there is provided a molded article comprising a polypropylene composition comprising 50% by weight to 76% by weight of a homopolypropylene, 12% by weight to 25% by weight of a random copolymer polypropylene having 2 mol% to 10 mol% of units derived from ethylene, and 12% by weight to 25% by weight of a propylene-ethylene copolymer having 10% by weight to 25% by weight of units derived from ethylene.
[0045] According to various embodiments, the molded article may be a monolayer film or a monolayer sheet. The polypropylene composition of the first aspect may act as a sealant layer, for example as one or more middle layers, or as an outer layer that contacts the packaged contents, such as food products in retort packages.
[0046] According to various embodiments, the molded article is one or more sheets of a multilayer film or sheet. For example, one or more of the monolayer films or sheets described above may be part of a multilayer film or sheet. The polypropylene composition disclosed herein may be used to form a multilayer polypropylene film by cast coextrusion. The multilayer film may have any number of layers, for example, 2, 3, 4, 5, 10, 15, or 20 layers. The multilayer film or sheet may constitute a pouch or bag. The inner layer of the pouch or bag may be a monolayer film or sheet.
[0047] In a particular embodiment, the molded article may be a retort pouch for food. The molded article may advantageously have a seal strength of at least 15 N / 15 mm according to ASTM F 88-15. Preferably, the molded article comprising the polypropylene composition may have a seal strength in the range of 15 N / 15 mm to 30 N / 15 mm, more preferably 20 N / 15 mm to 27 N / 15 mm, even more preferably 22 N / 15 mm to 25 N / 15 mm according to ASTM F 88-15. At a seal strength of at least 15 N / 15 mm, the seal initiation temperature may be 165° C. Advantageously, these sealing properties of the polypropylene composition of the present disclosure may provide good and / or improved protection from contamination for the sealing of the molded article.
[0048] Other mechanical properties such as elongation at break, tensile at yield, tensile at break, and / or 2% secant modulus can also be improved by using the polypropylene composition of the present disclosure. For example, the elongation at break can be in the range of about 400% to about 800%, such as about 450% to about 750%, or about 500% to about 700%. Meanwhile, the yield tensile can be in the range of about 100 kg / cm. 2 ~About 300kg / cm 2 , for example, about 100 kg / cm 2 ~About 250kg / cm 2 , or about 100 kg / cm2 ~About 200kg / cm 2 The breaking tensile strength is about 100kg / cm 2 ~About 300kg / cm 2 , for example, about 150 kg / cm 2 ~About 250kg / cm 2 The 2% secant elastic modulus is approximately 3,000 kg / cm 2 ~Approx. 5,000kg / cm 2 , for example, about 3,500 kg / cm 2 ~Approx. 4,500kg / cm 2 , or about 3,500 kg / cm 2 ~Approx. 4,000kg / cm 2 It is.
[0049] According to various advantages offered by the present invention, in a fifth aspect there is provided the use of the shaped article described herein in a retort packaging application.
[0050] The present invention illustratively described herein may be suitably practiced in the absence of any element, limitation, or restriction not specifically disclosed herein. Thus, for example, the terms "comprising", "including", "containing", etc., should be understood broadly and without limitation. Furthermore, the terms and expressions used herein are used as terms of description and not as terms of limitation, and there is no intention in the use of such terms and expressions to exclude any equivalents or portions of the features shown and described, and it is recognized that various modifications are possible within the scope described in the claims. Thus, although the present invention has been specifically disclosed by preferred embodiments and optional features, it should be understood that modifications and variations of the present invention disclosed herein may depend on those skilled in the art, and such modifications and variations are considered to be within the scope of the present invention.
[0051] The present disclosure will now be described more fully with reference to the accompanying drawings, in which exemplary embodiments of the present invention are shown. However, the present invention may be embodied in many different forms and should not be construed as being limited to the exemplary embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. In the drawings, the lengths and sizes of layers and regions may be exaggerated for clarity. EXAMPLES
[0052] (Experimental section) Example 1: Measurement method
[0053] The following describes the property tests of the polypropylene composition of the present disclosure. The test methods and equipment used are conventional and are not intended to limit the scope of the present disclosure.
[0054] (1) Melt flow rate (MFR): Melt flow rate (MFR) was measured at 230° C. and 2.16 kg in accordance with ASTM D 1238-13.
[0055] (2) Density: Density was measured in accordance with ASTM D 1505-10.
[0056] (3) Tensile strength of film: The tensile strength, elongation and secant modulus of elasticity of the film were measured according to ASTM D 882-12.
[0057] (4) Seal Strength: The seal strength was measured in accordance with ASTM F88-15.
[0058] (5) Hot tack test: The sealing initiation temperature of the film was measured using a hot tack device in accordance with ASTM F1921-12.
[0059] (6) Sealed through contamination test (6.1) Sample Preparation: Flat retortable pouches were used to evaluate sealing for the contamination properties of the polypropylene films disclosed herein. The pouches were prepared in the form of three-sided sealed packaging pouches using a high temperature sealing bar instrument with a thermostatic sealing bar at 180° C., 2 bar pressure, and 1 second hold time. The three-sided sealed packaging pouches had an inner diameter of 12.0 cm by 15.0 cm. The three-sided sealed packaging pouches formed small bags containing 200 mL of food simulant each. The remaining sides of the pouch were sealed to close the retortable pouch and in a fixed position to control the volume and headspace within each filled pouch.
[0060] (6.2) Food simulant preparation: The food simulant used was a mixture of white vinegar, tomato sauce, and soil bean oil in a 1:1:1 weight ratio.
[0061] (6.3) Retort treatment: Retort treatment was carried out using a 40 liter capacity high pressure autoclave machine (single basket type) manufactured by Vertical Floor-Standing Autoclaves SYSTEC V-Series. Water was used as the pressure transfer liquid. First, the filled pouches were preheated to an initial temperature of 100°C before autoclaving. Then, the temperature was increased to 121°C and the pressure to 2.2MPa, and the pouches were kept in this state for 30 to 35 minutes. Depending on factors such as the type of food and the size of the pouch, different conditions than those mentioned above may be used. Generally, in retort pouch packaging, the free space available in the package is controlled to optimize the pressure inside the package. After the temperature and pressure controlled sterilization process, the filled pouches were cooled and the autoclave pressure was released. The filled pouches were removed from the chamber and tested for general appearance, leakage of the seals, and seal strength after retort treatment.
[0062] Example 2: P Preparation of polypropylene compositions All starting materials were commercially available.
[0063] Homopolypropylene (hPP) has a MFR of 2.5 g / 10 min at 230°C, a weight of 2.16 kg, a molecular weight distribution of 7.5 g / mol, and a concentration of 0.910 g / cm 3 Random copolymer polypropylene (rPP) contains 3 mol% ethylene units and has a viscosity of 0.910 g / cm 3 The propylene-ethylene copolymer contained isotactic polypropylene with 16% by weight of randomly distributed ethylene units.
[0064] Homopolypropylene, random copolymer polypropylene and propylene-ethylene copolymer were blended in various ratios as shown in Table 1 using a twin screw extruder.
[0065] The resulting blended polypropylene composition was formed into a film having a thickness of 70 μm by coextrusion. The film obtained from the polypropylene composition was then analyzed as described above. The results are shown in Table 1.
[0066] [Table 1]
[0067] Comparing the samples having the same amount of propylene-ethylene copolymer at 15 wt%, i.e., Samples 2A, 3A and 4A, Sample 4A having the highest random copolymer polypropylene content at 25 wt% exhibited the highest tensile strength at break and elongation at break, as shown in Table 1. The tensile strength at break and elongation at break of Sample 4A were also higher than those of Comparative Sample 1A. For example, the tensile strength at break obtained was 287 kg / cm 2 However, the comparative sample 1A had a strength of 202 kg / cm 2 In terms of elongation to break, Sample 4A exhibited an elongation to break of 726%, compared to Comparative Sample 1A, which had an elongation to break of only 569%.
[0068] Without wishing to be bound by theory, it is believed that the random copolymer polypropylene acts as a compatibilizer that improves the diffusion of the propylene-ethylene copolymer phase in the homopolypropylene matrix, thereby resulting in better mechanical properties of the film.
[0069] Comparing samples with the same amount (15 wt%) of random copolymer polypropylene but with different amounts of propylene-ethylene copolymer, i.e., Samples 2A, 5A and 6A, it was found that the amount of propylene-ethylene copolymer did not significantly affect the yield tensile strength of the film. Sample 2A showed slightly higher yield tensile strength than Samples 5A and 6A. This may be due to the higher homopolypropylene content of Sample 2A. However, Samples 5A and 6A, which had at least 20 wt% propylene-ethylene copolymer, showed better tensile strength at break and elongation at break compared to Sample 2A. The effect of propylene-ethylene copolymer content on the properties of the polypropylene compositions was compared.
[0070] The seal strength was measured at various temperatures for Comparative Sample 1A and Samples 2A, 3A and 4A, and the results are shown in Figure 1A. Sample 3A showed the lowest seal initiation temperature and higher seal strength in the transition stage of film sealing between 145°C and 165°C. This is advantageous compared to Comparative Sample 1A, which showed a high seal initiation temperature, sealed only between 160°C and 170°C, and had a seal strength of less than about 10N / 15mm at 165°C. Without wishing to be bound by theory, it is believed that the polypropylene composition containing homopolypropylene, random copolymer polypropylene and propylene-ethylene copolymer in various ratios as claimed provides a synergistic effect to obtain the target properties between mechanical properties and seal performance.
[0071] FIG. 1B shows the seal strength measured for Comparative Sample 1A and Samples 2, 5 and 6 at various temperatures. It is shown that in the low temperature range around 140°C to 155°C, the seal strength of the film is significantly enhanced by increasing the propylene-ethylene copolymer content. However, the polypropylene (PP) matrix shows a dominant effect in the high temperature range (160°C to 200°C) because the PP matrix can completely melt and fuse between the film layers in this temperature range. In other words, the seal strength of the film in the high temperature range depends on the strength of homopolypropylene because it can completely melt and fuse between the layers, whereas the random copolymer polypropylene and propylene-ethylene copolymer perform the film fusion in the low temperature range. Therefore, the optimization of the formulation should be a balance between the easy sealing function and the mechanical properties of the film.
[0072] In order to ensure the seal initiation temperature of the film, hot tack measurements were also performed to measure the seal strength of the film during the melting stage. Corresponding to Figures 1A and 1B, there was no significant effect of random copolymer polypropylene on the seal performance, but the results in Figures 2A and 2B showed that there was a part of the film that was melted and sealed between the layers. This suggests that the seal initiation temperature of the film was reduced by blending random copolymer polypropylene and propylene-ethylene copolymer in homopolypropylene. With the increase in propylene-ethylene copolymer content, the seal initiation temperature of the film shifted to a lower temperature range.
[0073] Comparative sample 1A and samples 2A-6A were laminated with a 12 mm thick polyethylene terephthalate (PET) film (where the PET film was on the top and bottom, i.e., both ends, of the sample). The laminate film was sealed on three sides to form a pouch for filling the food sample.
[0074] A second sample of Comparative Sample 1A and Sample 5A were used to prepare laminated retortable packages (identified herein as Comparative Sample 1B and Sample 5B, respectively). For Comparative Sample 1B and Sample 5B, a dry lamination process was used to form a polyethylene terephthalate / aluminum / nylon / Comparative Sample 1B or polyethylene terephthalate / aluminum / nylon / Sample 5B film structure to form a pouch, which was then filled with the food sample using the process described above.
[0075] Food samples were prepared by mixing commercial tomato sauce, vinegar and vegetable oil in an equal weight ratio of 1:1:1. 200 ml of food samples were filled into comparative samples 1A, 1B, samples 2A, 3A, 4A, 5A, 5B and 6A. The pouches were heat sealed at 180°C and a pressure of 4 bar was applied for 4 seconds to close the pouches. After sealing, the pouches were autoclaved under overpressure conditions and at a temperature of 121°C for 30 minutes. Observations for the presence or absence of food leakage were carried out and reported in Table 2.
[0076] The inventive example shows perfect pouch sealing as there was no leakage of food from the pouch and no food contamination at the seal, whereas both comparative samples 1A and 1B showed leakage and food contamination at the seal.
[0077] The sealing performance after autoclaving was examined, and the results are shown in Figure 3. The sealing strength of Samples 2A and 3A after autoclaving was maintained, in contrast to Comparative Sample 1A, which showed a dramatic decrease in sealing strength after autoclaving.
[0078] [Table 2]
[0079] 4A-4F are photographs showing the retouched pouches of Comparative Sample 1A (FIG. 4A) and Samples 2A-6A (FIGS. 4B-4F). As can be seen from the figures, food leakage and contamination of the seal were observed in Comparative Sample 1A, but not in Samples 2A-6A.
[0080] Although the present invention has been particularly shown and described with reference to exemplary embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the invention as defined by the following claims.
Claims
1. A polypropylene composition comprising: (a) 60% to 76% by weight of homopolypropylene; (b) 12% to 25% by weight of a random copolymer polypropylene having 2% to 10% by mole of units derived from ethylene; and (c) 12% to 25% by weight of a propylene-ethylene copolymer having 10% to 25% by weight of units derived from ethylene. wherein components (a), (b) and (c) have a melting point in the range of 145°C to 165°C.
2. 2. The polypropylene composition of claim 1, wherein the homopolypropylene, the random copolymer polypropylene, and the propylene-ethylene copolymer in the polypropylene composition total 100% by weight.
3. 3. The polypropylene composition of claim 1 or 2, wherein the random copolymer polypropylene comprises at least 50% by weight of propylene derived units.
4. The polypropylene composition according to any one of claims 1 to 3, wherein the random copolymer polypropylene has 2 mol% to 5 mol% of units derived from ethylene.
5. The polypropylene composition according to any one of claims 1 to 4, wherein the random copolymer polypropylene is present in an amount of 25 wt%.
6. The polypropylene composition according to any one of claims 1 to 5, wherein the propylene-ethylene copolymer comprises at least 50% by weight of propylene derived units.
7. The polypropylene composition according to any one of claims 1 to 6, wherein the propylene-ethylene copolymer has 15% to 20% by weight of units derived from ethylene.
8. The polypropylene composition of any one of claims 1, 2, 3, 4, 6, or 7, wherein the propylene-ethylene copolymer is present in an amount of from 20% to 25% by weight.
9. The polypropylene composition according to any one of claims 1 to 8, wherein the homopolypropylene has a melt flow rate according to ASTM D 1238-13 of 1 g / 10 min to 10 g / 10 min at 230°C and 2.16 kg.
10. Polypropylene composition according to any one of the preceding claims, wherein said composition has a melt flow rate according to ASTM D 1238-13 of 0.1 g / 10 min to 4.0 g / 10 min at 230°C and 2.16 kg.
11. A method of producing a molded article, comprising the steps of providing a polypropylene composition according to any one of claims 1 to 10 and molding said polypropylene composition into a molded article.
12. A molded article obtainable by the method according to claim 11.
13. A molded article comprising the polypropylene composition according to any one of claims 1 to 10.
14. The molded article according to claim 12 or 13, which is a monolayer film or a monolayer sheet.
15. 14. The molded article of claim 12 or 13, wherein the molded article is one or more sheets of a multilayer film or sheet.
16. 16. The article of claim 15, wherein the multilayer film or sheet constitutes a pouch or bag.
17. The molded article according to any one of claims 12 to 16, having a seal strength of at least 15 N / 15 mm at a seal initiation temperature of 165°C.
18. Use of the molded article according to any one of claims 12 to 17 in retort packaging applications.
Citation Information
Patent Citations
Polypropylene resin composition
JP1979039453A
Water dispersion type adhesive
JP1989174579A