Cleaning sheet and method for producing same

JP7551293B2Active Publication Date: 2024-09-17DAIO PAPER CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2019216264
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-11-29
Publication Date
2024-09-17
Estimated Expiration
2039-11-29

AI Technical Summary

Benefits of technology

【0012】 本発明によれば、水解性を損なうことなく接着強度に優れた多層構造の清掃シート及び当該清掃シートの製造方法を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551293000010
    Figure 0007551293000010
  • Figure 0007551293000013
    Figure 0007551293000013
  • Figure 0007551293000014
    Figure 0007551293000014
Patent Text Reader

Abstract

To provide a cleaning sheet having a multilayer structure with excellent bond strength without deteriorating water-disintegrating property and a manufacturing method of the cleaning sheet.SOLUTION: In a manufacturing process of a toilet cleaner S, on two opposing sides of an edge of one face of a raw paper sheet P comprising a water-disintegrable fiber assembly, a cellulose nanofiber of 0.2-2.0 g / m2 is included, or, on a whole area of the one face of the raw paper sheet P, a cellulose nanofiber of 1.0-2.0 g / m2 subjected to a mechanical treatment or an enzyme treatment is included, and another raw paper sheet P is laminated at a bonding part and sufficiently dried upon heat, thereby the toilet cleaner S having excellent bond strength while having similar water-disintegrating property as the case where the raw paper sheets P are bonded to each other by contact embossing can be formed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cleaning sheet and a method for making the cleaning sheet. [Background technology]

[0002] Methods for forming a base paper sheet into a multi-layer structure to produce a water-decomposable cleaning sheet include a method of bonding with a hot melt adhesive (see Patent Document 1) and a method of contact embossing (see Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2002-200726 A [Patent Document 2] JP 2019-103552 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when using hot melt adhesive, there are problems such as a particular odor and the adhesive surface becoming hard. Also, when using contact embossing, holes are made in the paper and it is intertwined, so there is a problem that the cleaning sheet may tear from the holes when force is applied.

[0005] An object of the present invention is to provide a multi-layer cleaning sheet having excellent adhesive strength without impairing water-disintegrability, and a method for producing said cleaning sheet. [Means for solving the problem]

[0006] The invention described in claim 1 is a multi-layered cleaning sheet formed by laminating a plurality of base paper sheets made of a water-decomposable fiber aggregate, The base-paper sheet has an adhesive portion where adjacent base-paper sheets are adhered to each other, The adhesive portion contains cellulose nanofibers, The content of the cellulose nanofiber is 0.2 to 2.0 g / m 2 and The adhesive portion is vs. Toward Two sides Edge only To In succession It is characterized by the fact that

[0008] Claim 2 The invention described in claim 1 to The cleaning sheet according to the present invention, The base paper sheet includes a water-soluble binder, The cleaning sheet is characterized in that it is a wet sheet.

[0009] Claim 3 The invention described in is a method for producing a multi-layered cleaning sheet in which a plurality of base-paper sheets made of a water-decomposable fiber aggregate are laminated, comprising: Cellulose nanofiber solution with a concentration of 2.0% or less Wohara Paper Sheet Continuously on the edges of two opposing sides only A coating step of coating; a lamination step in which the coated surface of the base-paper sheet coated with the cellulose nanofiber solution is placed in contact with another base-paper sheet; a drying step of heat-drying and bonding the superposed base paper sheets; The present invention is characterized by having the following.

[0010] Claim 4 The invention described in claim 3 A method for producing the cleaning sheet according to the present invention, The method for producing the cleaning sheet is characterized by including a chemical impregnation step of impregnating the cleaning sheet with a chemical solution.

[0011] Claim 5 The invention described in claim 3 or 4 A method for producing the cleaning sheet according to the present invention, The applying step is characterized by applying by spraying. Effect of the Invention

[0012] According to the present invention, it is possible to provide a multi-layered cleaning sheet having excellent adhesive strength without impairing water-disintegrability, and a method for producing said cleaning sheet. [Brief description of the drawings]

[0013] [Figure 1] 5A to 5C are diagrams illustrating an example of a manufacturing method of the cleaning sheet according to the embodiment. [Diagram 2] FIG. 2 is a diagram showing an example of a cleaning sheet according to an embodiment. [Diagram 3] FIG. 1(a) is a diagram showing the fiber orientation of conventional paper, and FIG. 1(b) is a diagram showing the fiber orientation of the present invention. [Figure 4] 4A and 4B are an enlarged view and a cross-sectional view of an embossed portion of the toilet cleaner. [Diagram 5] FIG. 4 is an explanatory diagram showing an example of a contact area of ​​an embossment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] A cleaning sheet according to an embodiment of the present invention will be described below with reference to Figures 1 to 5. However, the embodiment described below is subject to various limitations that are technically preferable for carrying out the present invention, but the scope of the present invention is not limited to the following embodiment and illustrated examples. In addition, the cleaning sheet will be described as a toilet cleaner as an example of a water-disintegratable sheet, but the cleaning sheet also includes other cleaning sheets such as wet tissues impregnated with a chemical solution for wiping purposes. For convenience, the following description will be given by defining the X and Y directions as well as the up-down and left-right directions as shown in FIGS.

[0015] [Present embodiment] The toilet cleaner S of the present invention is preferably a wet-type toilet cleaner S impregnated with a specified chemical solution, which is produced, for example, by applying a solution of purified water to one side of multiple base-paper sheets P, layering another base-paper sheet P on the applied surface, and bonding the sheets together by thermal drying to form a multi-layer structure.

[0016] [Base paper sheet] As shown in FIG. 1(a), the base paper sheet P has adhesive parts 1 at opposing edges of its edges and a non-adhesive part 2 at the other edges. The adhesive portion 1 is coated with a CNF solution, and has higher hydrophilicity and hygroscopicity than the non-adhesive portion 2. The non-adhesive portion 2 is a portion to which the CNF solution has not been applied, and is less hydrophilic and less hygroscopic than the adhesive portion 1. Alternatively, the base-paper sheet P may be coated with the CNF solution over substantially the entire surface thereof, and may have only adhesive portions 1, as shown in FIG. 1(b).

[0017] The edge portion here refers to a portion from the sheet edge to the center of the sheet, and the adhesive portion is preferably formed at a distance of 25% to 0% from the sheet edge, and more preferably at a distance of 5% to 1% from the sheet edge. In addition, the application of the CNF solution in this embodiment is not limited to a continuous application form, and may be an intermittent application form. In that case, it is preferable to apply the CNF solution to 70% to 100% of one side or the entire surface, and more preferably to apply the CNF solution to 90% to 100%.

[0018] The CNF content in the adhesive part 1 is 0.2 to 2.0 g / m 2 and more preferably 1.0 to 2.0 g / m 2 It is. Content is 0.2g / m 2 If the content is less than 2.0 g / m, the adhesive strength will be lower than when the material is contact embossed. 2 This is because above this value, the hydrolysis property significantly deteriorates compared to that of a material that does not contain CNF.

[0019] (CNF) Here, CNF refers to fine cellulose fibers obtained by defibrating pulp fibers, and generally refers to cellulose fibers containing cellulose fine fibers with a fiber width of nano-size (1 nm or more and 1000 nm or less), but fibers with an average fiber width of 100 nm or less are preferable. The average fiber width can be calculated, for example, by using a certain number of number averages, medians, mode diameters (mode values), etc.

[0020] The CNF may be uniformly impregnated in the thickness direction of the base-paper sheet P, but it is preferable that the CNF content gradually increases from the center in the thickness direction of the base-paper sheet P toward the front and back surfaces. This makes the toilet cleaner S less likely to tear even when strongly rubbed against the edge of a toilet bowl, compared to conventional products that are uniformly impregnated with the same amount of water-soluble binder.

[0021] (Pulp fibers that can be used for CNF) Pulp fibers that can be used to manufacture CNF include chemical pulps such as hardwood pulp (LBKP) and softwood pulp (NBKP); mechanical pulps such as bleached thermomechanical pulp (BTMP), stone ground pulp (SGP), pressed stone ground pulp (PGW), refiner ground pulp (RGP), chemi-ground pulp (CGP), thermo-ground pulp (TGP), ground pulp (GP), thermomechanical pulp (TMP), chemi-thermomechanical pulp (CTMP), and refiner mechanical pulp (RMP); waste paper pulp produced from brown paper, kraft envelope paper, magazine paper, newspaper paper, flyer paper, office paper, cardboard paper, white waste paper, Kent waste paper, imitation waste paper, land certificate waste paper, and recycled paper; and deinked pulp (DIP) produced by deinking waste paper pulp. These may be used alone or in combination as long as the effects of the present invention are not impaired.

[0022] (CNF defibrillation method) Examples of defibration methods used in the production of CNF include mechanical methods such as the high-pressure homogenizer method, the microfluidizer method, the grinder grinding method, the bead mill freeze-grinding method, and the ultrasonic defibration method, but are not limited to these methods. In addition, CNF that has been subjected to only mechanical treatment (not modified) using the above-mentioned defibration methods, i.e., CNF that has not been modified with functional groups, has higher thermal stability than CNF modified with functional groups such as phosphate groups and carboxymethyl groups, and can be used for a wider range of applications. However, CNF modified with functional groups such as phosphate groups and carboxymethyl groups can also be used in the present invention. In addition, for example, pulp fibers may be mechanically defibrated and then chemically treated, such as carboxymethylation, or may be enzymatically treated. Examples of CNF that have been chemically treated include iCNF (individualized CNF) (single nanocellulose) with a diameter of 3 to 4 nm, such as TEMPO-oxidized CNF, phosphate-esterified CNF, and phosphite-esterified CNF. In addition, CNF that has been subjected to only chemical or enzymatic treatment, or CNF that has been subjected to chemical or enzymatic treatment and then mechanical fiberization treatment may be used.

[0023] The weight of each base paper sheet P is 30 to 150 g / m 2 The basis weight is based on JIS P8124.

[0024] [Fiber assembly] Moreover, in the toilet cleaner S of this embodiment, the base-paper sheet P is made of a water-decomposable fiber aggregate so that it can be disposed of directly in the toilet bowl after cleaning the toilet or the like. The fiber aggregate that is the raw material of the base paper sheet P is suitably a mixture of bleached hardwood kraft pulp (LBKP) and bleached softwood kraft pulp (NBKP) in an appropriate ratio. More preferably, the blending ratio of hardwood bleached kraft pulp exceeds 50 mass%, i.e., the blending ratio of softwood bleached kraft pulp to hardwood bleached kraft pulp is less than 1: 1. By increasing the blending ratio of hardwood bleached kraft pulp to softwood bleached kraft pulp, the interfiber gaps are reduced and moisture evaporation is suppressed, thereby improving the difficulty of the toilet cleaner S drying. It may also be made of a sheet made of pulverized pulp, or a sheet in which pulverized pulp is covered with or sandwiched between water-disintegrable paper.

[0025] [Water-soluble binder] In addition, a water-soluble binder is added to the base paper sheet P to increase the paper strength. Examples of the water-soluble binder include binder components such as carboxymethyl cellulose, polyvinyl alcohol, starch or its derivatives, hydroxypropyl cellulose, sodium alginate, trant gum, guar gum, xanthan gum, gum arabic, carrageenan, galactomannan, gelatin, casein, albumin, purpuran, polyethylene oxide, viscose, polyvinyl ethyl ether, sodium polyacrylate, sodium polymethacrylate, polyacrylamide, hydroxylated derivatives of polyacrylic acid, polyvinylpyrrolidone / vinylpyrrolidone vinyl acetate copolymer, etc.

[0026] In particular, it is preferable to use a water-soluble binder having a carboxyl group, since this binder has good water-decomposability and can exhibit wet strength through a crosslinking reaction. The water-soluble binder having a carboxyl group is an anionic water-soluble binder that easily forms a carboxylate in water. Examples of such binders include polysaccharide derivatives, synthetic polymers, and natural products.

[0027] (Polysaccharide derivative) Examples of the polysaccharide derivative include salts of carboxymethylcellulose, carboxyethylcellulose or a salt thereof, and carboxymethylated starch or a salt thereof, and in particular, alkali metal salts of carboxymethylcellulose (CMC) are preferred.

[0028] (CMC) The degree of etherification of CMC is desirably 0.6 to 2.0, particularly 0.9 to 1.8, and further preferably 1.0 to 1.5, because this results in extremely good water disintegrability and wet paper strength. It is also preferable to use a water-swellable CMC, because the CMC can exhibit the function of binding the fibers constituting the base-paper sheet P together without being swollen by crosslinking with the specific metal ions, which are crosslinking agents in the chemical solution, and can exhibit the strength required for a toilet cleaning sheet that can withstand cleaning and wiping tasks. In the case of the base-paper sheet P of this embodiment, CMC is added as the water-soluble binder.

[0029] The CMC may be uniformly impregnated in the thickness direction of the base-paper sheet P, but it is preferable that the CMC content gradually increases from the center in the thickness direction of the base-paper sheet P toward the front and back surfaces. This makes the toilet cleaner S less likely to tear even when strongly rubbed against the edge of a toilet bowl, compared to conventional products that are uniformly impregnated with the same amount of water-soluble binder.

[0030] (synthetic polymer) Examples of synthetic polymers include salts of polymers or copolymers of unsaturated carboxylic acids, salts of copolymers of unsaturated carboxylic acids and monomers copolymerizable with the unsaturated carboxylic acids, etc. Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic anhydride, maleic acid, fumaric acid, etc. Examples of monomers copolymerizable with these include esters of these unsaturated carboxylic acids, vinyl acetate, ethylene, acrylamide, vinyl ether, etc. Particularly preferred synthetic polymers are those using acrylic acid or methacrylic acid as the unsaturated carboxylic acid, specifically polyacrylic acid, polymethacrylic acid, salts of acrylic acid-methacrylic acid copolymers, and salts of copolymers of acrylic acid or methacrylic acid with alkyl acrylate or alkyl methacrylate.

[0031] (Natural products) Natural products include sodium alginate, xanthan gum, gellan gum, taragacanth gum, and pectin.

[0032] Furthermore, the base paper sheet P may contain CNF. That is, CNF can be added to the water-soluble binder (CMC in this embodiment), and the specific surface area of ​​the base-paper sheet P becomes larger than that of a base-paper sheet composed only of pulp.

[0033] Fiber orientation ratio Furthermore, the ratio of the length to width of the fiber orientation of the toilet cleaner S (length / width) is not particularly limited, but is preferably 0.8 to 2.0, and more preferably 0.8 to 1.2. In the papermaking process, which is a paper manufacturing process, fibers are laid on the wire of a papermaking machine and run in the conveying direction, so paper generally has a characteristic that many fibers are arranged in the vertical direction, which is the conveying direction of the papermaking machine (for example, vertical: horizontal = 2.3: 1, etc., see FIG. 3 (a)). Therefore, the fiber density in the horizontal direction is low and the fibers are easily broken. In other words, it is easy to break depending on the direction when wiping. Therefore, in this embodiment, as shown in FIG. 3 (b), by setting the fiber orientation ratio of the vertical and horizontal directions of the toilet cleaner S to 0.8 to 2.0, preferably 0.8 to 1.2, it is possible to provide a toilet cleaner S that is difficult to break even if wiped from any direction. The ratio of the fiber orientation of the vertical and horizontal directions can be calculated from the ratio of wet strength in the MD and CD directions.

[0034] [Chemical solution] The toilet cleaner S of this embodiment is impregnated with a specific chemical solution containing a cross-linking agent that cross-links with the water-soluble binder (CMC in the case of the toilet cleaner S of this embodiment). The chemical solution also contains other auxiliary agents such as glycol ethers, aqueous detergents, preservatives, disinfectants, and organic solvents. The chemical solution is impregnated into the base-paper sheet P which has been impregnated with the water-soluble binder and then dried. The chemical solution is impregnated in an amount of 100 to 500% by mass, preferably 150 to 300% by mass, based on the mass of the base paper sheet P, which is the substrate of the toilet cleaner S.

[0035] (Crosslinking agent) As the crosslinking agent, boric acid, various metal ions, etc. can be used, but when CMC is used as a water-soluble binder, it is preferable to use polyvalent metal ions. In particular, it is preferable to use one or more polyvalent metal ions selected from the group consisting of alkaline earth metals, manganese, zinc, cobalt, and nickel, because the fibers are sufficiently bonded to each other to develop wet strength that can withstand use, and to have sufficient water decomposability. Among these metal ions, it is particularly preferable to use ions of calcium, strontium, barium, zinc, cobalt, and nickel.

[0036] (Glycol ethers) Glycol ethers are compounds that have a structure in which the hydroxyl groups at one or both ends of glycol, a dihydric alcohol, are etherified, and have hydrophobic alkyl groups and hydrophilic ether and hydroxyl groups in the molecule. They have a smaller molecular weight than surfactants, and have a lower dynamic surface tension than conventional detergents that contain only surfactants, so they can form an interface between the chemical solution and dirt more quickly. Glycol ethers also act as coupling agents that make hydrophobic oils and dirt compatible with water, and can separate dirt and prevent it from reattaching. Therefore, adding glycol ethers to the chemical solution can improve the wiping performance of Toilet Cleaner S.

[0037] The chemical solution in the present invention contains glycol ethers such as propylene glycol monomethyl ether (PGME), diethylene glycol monobutyl ether (DGME), ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, polyethylene glycol monomethyl ether, ethylene glycol isopropyl ether, diethylene glycol monoisopropyl ether, triethylene glycol monomethyl ether, polyethylene glycol monomethyl ether, ethylene glycol isopropyl ether, diethylene glycol monoisopropyl ether, and ethylene glycol monobutyl ether.

[0038] In particular, PGME is usually added as a cleaning ingredient and is known to improve cleaning power, but it also has the effect of directly improving sheet strength and enhances the sheet strength improvement effect of CMC and polyvalent metal ions. As a result, it is thought to have a high deodorizing effect. The amount of PGME added is 20 to 60 g / m 2 and more preferably 26 to 40 g / m 2 20g / m 2 If it is less than 60g / m, the deodorizing effect is not sufficient. 2 Even if more than 60g / m is applied, 2 No greater deodorizing effect can be obtained than when it is added.

[0039] DGME, like PGME, is an auxiliary agent that has the effect of improving sheet strength. The amount of DGME applied is 5 to 30 g / m 2 and more preferably 10 to 20 g / m 2 It is. However, if only DGME, which can improve sheet strength the most, is added, it may wipe away the oils from the user's hands, leading to rough hands. Therefore, in order to prevent rough hands while improving sheet strength, it is necessary to mix glycol ethers such as PGME in addition to DGME in the appropriate ratio.

[0040] (Water-based cleaner) As the aqueous detergent, for example, a surfactant as well as a lower or higher (aliphatic) alcohol can be used.

[0041] (Preservatives) As the preservative, for example, parabens such as methylparaben, ethylparaben, and propylparaben can be used.

[0042] (Disinfectant) Examples of disinfectants that can be used include benzalkonium chloride, chlorhexidine gluconate, povidone-iodine, ethanol, cetyl benzanium oxide, triclosan, chloroxylenol, isopropyl methylphenol, etc. Examples of organic solvents that can be used include polyhydric alcohols such as glycol (dihydric), glycerin (trihydric), and sorbitol (tetrahydric).

[0043] In addition, the above-mentioned auxiliary agents for the components of the drug solution can be appropriately selected, and the drug solution may contain other functional components as necessary. For example, propylene glycol (PG) can be used as an auxiliary agent for solubilizing preservatives and disinfectants.

[0044] [Emboss] In addition, the surface of the toilet cleaner S may be the base paper sheet P as is, but it is preferable that it is embossed. In the case of the toilet cleaner S, for example, as shown in Figure 2, two types of embossing EM11 and EM12 are applied by embossing.

[0045] The shape, number, area ratio, etc. of the embossments are arbitrary, but in the case of the toilet cleaner S, the embossments EM11 are arranged in a diamond lattice, which reduces uneven wiping compared to when the embossments EM11 are arranged in a square lattice or rectangular lattice. Also, the embossments EM12 are arranged between the embossments EM11.

[0046] As shown in FIG. 4(a), the embossment EM11 has a bulging portion PR21 having a curved shape. Moreover, as shown in FIG. 4(b), the embossment EM12 has a bulging portion PR22 having a flat shape.

[0047] Furthermore, since the embossed EM12 is arranged between the embossed EM11, the bulge portion PR21 of the embossed EM11 and the bulge portion PR22 of the embossed EM12 are closely adjacent to each other and adhere to each other, thereby forming the continuous embossed EM21 as shown in Figure 4(c). Moreover, the bulging portion PR21 of the embossed portion EM11 and the bulging portion PR22 of the embossed portion EM12 may simply be adjacent to each other and not connected to each other.

[0048] The two types of embossments EM11 and EM12 thus formed can increase the contact area with the object to be cleaned, etc., thereby reducing the hardness of the toilet cleaner S and improving wiping performance.

[0049] In other words, by forming an embossment EM11 with a curved bulge PR21 and an embossment EM12 with a flat bulge PR22 on the entire surface of the toilet cleaner S, when force is applied to the toilet cleaner S during wiping, each embossment deforms, and the contact area increases for the first time. Therefore, not only is the contact area increased, but the flexibility is also improved due to the deformation of each embossment.

[0050] For example, as shown in Fig. 5(a), in the case of a single embossed EM11, the contact area CN31 generated when the embossed EM11 is deformed by the force applied to the toilet cleaner S during wiping occurs discretely near the embossed EM11. In contrast, when two types of embossed EM11 and EM12 are combined, as shown in Fig. 5(b), the contact area SN32 generated when the embossed EM11 and EM12 are deformed by the force applied to the toilet cleaner S during wiping increases compared to the contact area CN31 in Fig. 5(a).

[0051] The two types of embossed patterns EM11 and EM12 can provide the same effect as normal embossing, and can improve the texture, absorbency, bulkiness, etc. of the toilet cleaner S. Furthermore, the connected embossed patterns EM21 can provide the effect of good appearance due to embossing, just like normal embossing.

[0052] The toilet cleaner S is folded in half at the center in the Y direction by folding. It is stored in a folded state in a plastic case or a wrapping film for storage, and is unfolded as necessary when used. The way in which the toilet cleaner S is folded is not limited to folding in half, and it may be folded in four or eight, for example. EXAMPLES

[0053] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.

[0054] [Sample Creation] First, the weight is 43g / m 2 A base paper sheet P (fiber composition: NBKP: 50% or less, LBKP: 50% or more) measuring 100 mm x 100 mm was prepared. Next, under the conditions of Examples 1-20 and Comparative Examples 1-20, two base paper sheets P were bonded together and left to stand in a thermostatic chamber set at 60° C. for 24 hours for thermal drying to prepare toilet cleaners S. In addition, the base paper sheets P of Examples 17-20 and Comparative Examples 12-20 had a CMC of about 1 g / m as a water-soluble binder in the papermaking process. 2 It has been added. The conditions for Examples 1-20 and Comparative Examples 1-20 are as follows. In each of the following examples and comparative examples, the "CNF solution" is an aqueous solution obtained by mixing only purified water and various types of CNF.

[0055] Example 1 As shown in Figure 1(a), a micropipette (Nichipet EXII00-NPX2-1000) was used to apply 1 g of the mechanically treated CNF solution with a concentration of 0.10% to each of the two opposing edges of a single base paper sheet P, for a total of 2 g (CNF content: 0.2 g / m 2 ).

[0056] Example 2 A total of 2 g of mechanically treated CNF solution with a concentration of 0.25% was applied to each of the two opposing edges of one base paper sheet P (CNF content: 0.5 g / m 2 ). The other conditions were the same as in the first embodiment.

[0057] Example 3 A total of 2 g of mechanically treated CNF solution with a concentration of 0.50% was applied to each of the two opposing edges of one base paper sheet P (CNF content: 1.0 g / m 2 ). The other conditions were the same as in the first embodiment.

[0058] Example 4 A total of 2 g of mechanically treated CNF solution with a concentration of 1.00% was applied to each of the two opposing edges of one base paper sheet P (CNF content: 2.0 g / m 2 ). The other conditions were the same as in the first embodiment.

[0059] (Examples 5-8) The applied solution was an enzyme-treated CNF solution. The other conditions were the same as in Examples 1-4.

[0060] (Examples 9 to 12) The applied solution was a TEMPO-treated CNF solution. The other conditions were the same as in Examples 1-4.

[0061] Example 13 As shown in FIG. 1(b), 2 g of mechanically treated CNF solution with a concentration of 0.50% was sprayed onto the entire surface of one base paper sheet P (CNF content: 1.0 g / m 2 ).

[0062] Example 14 As shown in FIG. 1(b), 2 g of a mechanically treated CNF solution with a concentration of 1.00% was sprayed onto the entire surface of one base paper sheet P (CNF content: 2.0 g / m 2 ).

[0063] (Examples 15-16) The applied solution was an enzyme-treated CNF solution. Other conditions were the same as in Examples 13-14.

[0064] (Examples 17-20) The base paper sheet P has a CMC of approximately 1 g / m during the papermaking process. 2 It has been added. Other conditions were the same as in Examples 13-16.

[0065] Comparative Example 1 The base paper sheets P were bonded together by contact embossing.

[0066] Comparative Example 2 A total of 2 g of mechanically treated CNF solution with a concentration of 0.05% was applied to two opposing edges of one base paper sheet P (CNF content: 0.1 g / m 2 ). The other conditions were the same as in the first embodiment.

[0067] Comparative Example 3 As shown in FIG. 1(b), 2 g of purified water was sprayed onto the entire surface of one base paper sheet P.

[0068] Comparative Example 4 As shown in FIG. 1(b), 2 g of a mechanically treated CNF solution with a concentration of 0.10% was sprayed onto the entire surface of one base paper sheet P (CNF content: 0.2 g / m 2 ).

[0069] Comparative Example 5 As shown in FIG. 1(b), 2 g of mechanically treated CNF solution with a concentration of 1.20% was sprayed onto the entire surface of one base paper sheet P (CNF content: 2.4 g / m 2 ).

[0070] (Comparative Examples 6-7) The applied solution was an enzyme-treated CNF solution. The other conditions were the same as those in Comparative Examples 4-5.

[0071] Comparative Example 8 As shown in FIG. 1(b), 2 g of a TEMPO-treated CNF solution with a concentration of 0.10% was sprayed onto the entire surface of one base paper sheet P (CNF content: 0.2 g / m 2 ).

[0072] Comparative Example 9 As shown in FIG. 1(b), 2 g of a TEMPO-treated CNF solution with a concentration of 0.50% was sprayed onto the entire surface of one base paper sheet P (CNF content: 1.0 g / m 2 ).

[0073] Comparative Example 10 As shown in FIG. 1(b), 2 g of a TEMPO-treated CNF solution with a concentration of 1.00% was sprayed onto the entire surface of one base paper sheet P (CNF content: 2.0 g / m 2 ).

[0074] Comparative Example 11 As shown in FIG. 1(b), 2 g of a TEMPO-treated CNF solution with a concentration of 1.20% was sprayed onto the entire surface of one base paper sheet P (CNF content: 2.4 g / m 2 ).

[0075] (Comparative Examples 12-20) The base paper sheet P has a CMC of approximately 1 g / m during the papermaking process. 2 It has been added. The other conditions were the same as those in Comparative Examples 3-11.

[0076] The following tests 1 to 5 were carried out using the sheets of the above-mentioned examples and comparative examples.

[0077] [Test 1. Adhesive strength test when partially applied and dry] The following tests were carried out for Examples 1-12 and Comparative Examples 1-2.

[0078] [Evaluation method] The samples corresponding to Examples 1-12 and Comparative Examples 1-2 were cut into a width of 25 mm to prepare test pieces. Using a tensile tester (TENSIRON RTG1210 manufactured by A&D), both ends of the bonded test piece were clamped with the chucks of the tensile tester, and the maximum load point at which the sheet materials at each bonded location peeled off was measured under conditions of a chuck distance of 50 mm and a speed of 500 mm / min. This test was performed eight times for each Example and Comparative Example, and the average value of the adhesive strength was calculated.

[0079] [Test 2. Water dissolution test when partially applied and dried] The following tests were carried out for Examples 1-12 and Comparative Examples 1-2.

[0080] [Evaluation method] A stirring bar and 300 ml of purified water at a temperature of about 25°C are added to a 300 ml beaker, and the stirring bar is stirred at 600 rpm. Then, rolled samples corresponding to Examples 1-12 and Comparative Examples 1-2 are placed in the beaker, and the time from when the stirring bar reaches 500 rpm or less to when it reaches 540 rpm or more is measured. Such experiments are carried out four times each, and the average value of the water disintegrability is calculated. At this time, when compared to Comparative Example 1, a time 10 seconds or more slower is indicated as ×, a time 10 to 0 seconds slower is indicated as ◯, and a time equal to or slower than ⊚ is indicated as ⊚.

[0081] The results of tests 1 and 2 are shown in Tables I-III.

[0082] [Table 1]

[0083] [Table 2]

[0084] [Table 3]

[0085] [evaluation] Comparing the Examples and Comparative Examples in Tables I to III, the CNF concentration was 0.2 to 2.0 g / m 2 It can be seen that by adding the above range to two opposing edges of the base-paper sheet P, the adhesive strength between the base-paper sheets P can be increased more than when contact embossing is performed while maintaining the same water-decomposability as when contact embossing is performed. This is thought to be because the raw material for CNF is pulp, just like paper, and CNF is hydrolyzable and highly hygroscopic.

[0086] In addition, comparing the examples in Tables I to III, the CNF content is 0.2 g / m 2 In the case of , the adhesive strength was strongest when the mechanically treated CNF solution was applied, whereas in the other cases, the adhesive strength was strongest when the TEMPO-treated CNF solution was applied. This is thought to be because the fiber length is shorter in the order of mechanically treated CNF, enzyme treated CNF, and TEMPO treated CNF, and the shorter the fiber length, the higher the affinity with pulp. Additionally, regardless of the defibration method, the adhesive strength increases as the CNF content increases.

[0087] [Test 3. Evaluation of adhesive strength when applied over the entire surface and dry] The same test as Test 1 was carried out for the samples corresponding to Examples 13-16 and Comparative Examples 3-11.

[0088] [Test 4. Evaluation of water dissolution when applied to the entire surface and dried] The same test as Test 2 was carried out for the samples corresponding to Examples 13-16 and Comparative Examples 3-11.

[0089] The results of Tests 3-4 are shown in Tables IV-VI.

[0090] [Table 4]

[0091] [Table 5]

[0092] [Table 6]

[0093] [evaluation] Comparing Examples 13-16 in Tables VI-IV with Comparative Example 1 in Table I, the mechanically treated CNF or enzyme-treated CNF was 1.0 to 2.0 g / m 2 It can be seen that by applying the coating to the entire surface of the base-paper sheet P within this range, the adhesive strength between the base-paper sheets P can be increased more than when contact embossing is performed while maintaining the same water disintegrability as when contact embossing is performed. In addition, even when the coating is applied to the entire surface and dry, it can be seen that the adhesive strength increases as the CNF content increases. This is believed to be due to the high moisture absorption of CNF.

[0094] Furthermore, when comparing Comparative Example 1 in Table I, Examples 11-12 in Table III, and Comparative Examples 9-10 in Table VI, it can be seen that when the TEMPO-treated CNF solution is applied, the water-decomposability is equivalent to that when contact embossing is performed only when the solution is applied to two opposing sides of the edge of a single base-paper sheet P. This is thought to be because, when applied to two opposing edges, water can easily seep in everywhere except the adhesive area, and the fiber can be defibrated without any problems. However, when applied to the entire surface, the fiber diameter of the TEMPO-treated CNF is smaller, and it forms a dense intertwining with the pulp fibers of the base paper sheet, making it difficult for water to seep inside the base paper sheet (making it difficult to defibrate).

[0095] [Test 5. Evaluation of tensile strength of wet sheets adhered by full surface coating] For the samples corresponding to Examples 17-20 and Comparative Examples 12-20, a chemical solution containing about 80% purified water, about 4% crosslinking agent, about 15% glycol ethers, about 0.5% aqueous cleaning agent, and about 0.5% disinfectant was impregnated at 200% by mass based on the dry weight of the toilet cleaner S, and using a tensile tester (TENSIRON RTG1210 manufactured by A&D Co., Ltd.), both ends of the bonded test piece were clamped by the chucks of the tensile tester, and the maximum load point at which the toilet cleaner S breaks was measured under the conditions of a chuck distance of 50 mm and a speed of 500 mm / min. Such a test was performed eight times for each Example and Comparative Example, and the average value of tensile strength was calculated.

[0096] The results of Test 5 are shown in Tables VII-IX.

[0097] [Table 7]

[0098] [Table 8]

[0099] [Table 9]

[0100] Comparing the experimental results in Tables VII to IX, the mechanically treated CNF and the TEMPO treated CNF were 0.2 g / m 2 The enzyme-treated CNF is 1.0 g / m 2 It can be seen that by adding the above amount, the tensile strength of Toilet Cleaner S when wet is higher than when purified water is applied. This is believed to be due to the high moisture absorption of CNF.

[0101] Although the present invention has been specifically described based on the embodiment, the present invention is not limited to the above embodiment and can be modified without departing from the gist of the present invention. For example, in the above embodiment, the cleaning sheet is described as being used for cleaning, wiping, etc., but the use is not limited to this. In addition, the components added to the solution may be changed depending on the use.

[0102] In addition, the method of applying the CNF solution to the base-paper sheet P can be changed depending on the application, since as shown in the examples, depending on the CNF content, applying the CNF solution to the entire surface may increase adhesive strength, or applying the solution to the opposing edges may increase adhesive strength. Similarly, Toilet Cleaner S is stronger when used as a wet sheet, but is also strong enough when used as a dry sheet, so it can be changed depending on the application.

[0103] In addition, in the above examples, the CNF solution was applied only to the edges of two opposing sides, but it is sufficient that the CNF solution is applied to at least the opposing edges, and it may be applied to the edges of three sides or four sides.

[0104] In terms of the method of disintegrating the CNF, when applying to the entire surface, using mechanically treated CNF or enzyme-treated CNF will give Toilet Cleaner S excellent water-disintegrability, but this can be changed depending on the application.

[0105] Furthermore, the base paper sheet P in the present invention is not particularly limited in terms of the manufacturing method, composition, and basis weight.

[0106] In addition, the base paper sheet P in the present invention may be provided with perforations for dividing the toilet cleaner S into multiple pieces, but in that case, it is preferable not to apply the CNF solution near the perforations.

[0107] As a method for applying the CNF solution to the base-paper sheet P, spray application is preferred because CNF has thixotropy, can be applied uniformly, and the content can be easily adjusted. However, other methods may be used as long as they do not impair the effects of the present invention, such as application in the form of droplets using a dispenser or the like, roll application in which the solution is applied once to a roll and then brought into contact with the sheet surface to apply the solution, or roll transfer using a flexographic printer or gravure printer.

[0108] As a method for thermally drying the toilet cleaner S, other methods may be used alone or in combination as necessary, such as a method in which the toilet cleaner S is directly brought into contact with the surface of a heated roll such as a Yankee drum and dried, as long as the effects of the present invention are not impaired. Furthermore, the temperature of the thermostatic chamber during thermal drying is not limited to this.

[0109] In the above embodiment, the toilet cleaner S has a two-layer structure, and the CNF solution is applied directly to one side of the base paper sheet P to be bonded, but the present invention is not limited to this. It is also possible to provide a new absorbent material or base paper sheet P as an intermediate layer, apply the CNF solution to both sides of the layer, and laminate the layers to form a three-layer structure. In this way, the toilet cleaner S can be made thicker. In addition, when the toilet cleaner S is a wet sheet and an absorbent material is provided as an intermediate layer, the hygroscopicity of the chemical solution can be further increased.

[0110] Although several embodiments of the present invention have been described, the scope of the present invention is not limited to the above-described embodiments, but includes the scope of the invention described in the claims and its equivalents. [Explanation of symbols]

[0111] S Toilet Cleaner P Base paper sheet 1 Adhesive part 2 Non-adhesive area

Claims

1. A cleaning sheet having a multi-layer structure in which a plurality of base paper sheets made of a water-decomposable fiber aggregate are laminated, The base-paper sheet has an adhesive portion where adjacent base-paper sheets are adhered to each other, The adhesive portion contains cellulose nanofibers, The content of the cellulose nanofiber is 0.2 to 2.0 g / m 2 and The cleaning sheet, wherein the adhesive portion is continuous only along the edges of two opposing sides of the base-paper sheet.

2. The base paper sheet includes a water-soluble binder, 2. The cleaning sheet according to claim 1, wherein the cleaning sheet is a wet sheet.

3. A method for producing a multi-layered cleaning sheet in which a plurality of base paper sheets made of a water-decomposable fiber aggregate are laminated, comprising the steps of: A coating step of continuously coating a cellulose nanofiber solution having a concentration of 2.0% or less only on the edges of two opposing sides of the base-paper sheet; a lamination step in which the coated surface of the base-paper sheet coated with the cellulose nanofiber solution is placed in contact with another base-paper sheet; a drying step of heat-drying and bonding the superposed base paper sheets; A method for producing a cleaning sheet, comprising the steps of:

4. The method for producing the cleaning sheet according to claim 3 , further comprising a step of impregnating the cleaning sheet with a chemical solution.

5. 5. The method for producing a cleaning sheet according to claim 3, wherein the coating step comprises coating by spraying.

Citation Information

Patent Citations

  • Water-disintegrable fiber sheet having multilayered structure

    JP2001288657A

  • Molding processed base paper

    JP2002200726A

  • Method for manufacturing multi-ply paper

    JP2012197544A

  • Wet wipe and method for manufacturing the same

    JP2015190098A

  • Ply adhesive paste and sanitation tissue paper

    JP2016069528A