Solar cell, solar cell manufacturing method, multi-junction solar cell, solar cell module, and solar power generation system

By controlling the brightness profile and converting the Cu phase to cuprous oxide through a specific heating process, the solar cell achieves enhanced Voc and conversion efficiency by minimizing recombination at the p-type and n-type layer interface.

JP7551892B2Active Publication Date: 2024-09-17KK TOSHIBA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023501619
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-09
Publication Date
2024-09-17
Estimated Expiration
2041-07-09

AI Technical Summary

Technical Problem

Existing solar cells using cuprous oxide (Cu2O) face challenges in achieving high conversion efficiency due to the formation of a Cu phase at the boundary between the p-type and n-type layers, which increases recombination rates and decreases Voc and overall efficiency.

Method used

The solar cell design includes a p-type light absorption layer made of cuprous oxide with a controlled brightness profile in the HAADF-STEM image, where the maximum brightness of a specific region near the boundary is maintained within a certain percentage of the average brightness, and a heating process in a non-oxidizing atmosphere is used to convert the Cu phase into cuprous oxide, improving the interface quality.

Benefits of technology

This approach enhances Voc and conversion efficiency by reducing carrier recombination and maintaining transparency, resulting in improved performance of the solar cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551892000013
    Figure 0007551892000013
  • Figure 0007551892000011
    Figure 0007551892000011
  • Figure 0007551892000008
    Figure 0007551892000008
Patent Text Reader

Abstract

The problem to be solved by the present invention is to provide a solar cell, a solar cell manufacturing method, a multi-junction solar cell, a solar cell module, and a photovoltaic power generation system having excellent conversion efficiency. A solar cell according to one embodiment includes: a p electrode; a p-type light absorption layer containing cuprous oxide and / or a composite oxide of cuprous oxide on the p electrode; an n-type layer on the p-type light absorption layer; and an n electrode on the n-type layer. The p-type light absorption layer is such that, when defining a region from a position of a boundary between the p-type light absorption layer and the n-type layer to a position up to a depth of 10 nm toward the p electrode side as a first region, and a region other than the first region from a region from the position of the of the p-type light absorption layer at the boundary between the p-type light absorption layer and the n-type layer to a position up to a depth of 100 nm toward the p electrode side as a second region, the maximum luminance of the luminance profile of a HAADF-STEM image of the first region is 95-105% of the average luminance of the luminance profile of a HAADF-STEM image of the second region.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solar cell, a method for manufacturing a solar cell, a multi-junction solar cell, a solar cell module, and a solar power generation system. [Background technology]

[0002] One of the new solar cells is one that uses cuprous oxide (Cu2O) in the light absorption layer. Cu2O is a wide-gap semiconductor. Cu2O is a safe and inexpensive material made from copper and oxygen, which are abundant on Earth, and is therefore expected to realize highly efficient, low-cost solar cells. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2019 / 146119 Summary of the Invention [Problem to be solved by the invention]

[0004] The problem to be solved by the present invention is a solar cell having excellent conversion efficiency, a method for manufacturing a solar cell, a multi-junction solar cell, a solar cell module, and a solar power generation system. [Means for solving the problem]

[0005] A solar cell according to an embodiment has a p-electrode, a p-type light absorbing layer containing cuprous oxide and / or a composite oxide of cuprous oxide on the p-electrode, an n-type layer on the p-type light absorbing layer, and an n-electrode on the n-type layer, in which a first region of the p-type light absorbing layer is a region from a boundary between the p-type light absorbing layer and the n-type layer to a depth of 10 nm toward the p-electrode side, and a second region is a region of the p-type light absorbing layer from a boundary between the p-type light absorbing layer and the n-type layer to a depth of 100 nm toward the p-electrode side excluding the first region, the maximum luminance of the luminance profile of a HAADF-STEM image of the first region is 95% or more and 105% or less of the average luminance of the luminance profile of a HAADF-STEM image of the second region. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a cross-sectional view of a solar cell according to an embodiment. [Diagram 2] FIG. 2 is a diagram for explaining analysis spots of a solar cell according to an embodiment. [Diagram 3] Figure 3 shows an example HAADF-STEM image and brightness profile. [Figure 4] Figure 4 shows an example HAADF-STEM image and brightness profile. [Diagram 5] FIG. 5 is a flowchart of a method for manufacturing a laminated thin film and a solar cell according to an embodiment. [Figure 6] FIG. 6 is a cross-sectional view of a multi-junction solar cell according to an embodiment. [Figure 7] FIG. 7 is a perspective view of a solar cell module according to an embodiment. [Figure 8] FIG. 8 is a cross-sectional view of a solar cell module according to an embodiment. [Figure 9] FIG. 9 is a configuration diagram of a solar power generation system according to an embodiment. [Figure 10] FIG. 10 is a conceptual diagram of a vehicle according to an embodiment. [Figure 11] FIG. 11 is a conceptual diagram of a flying object according to an embodiment. [Figure 12] FIG. 12 is a table relating to an embodiment. [Figure 13] FIG. 13 is a table relating to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] A preferred embodiment of the present invention will be described in detail below with reference to the drawings. Unless otherwise specified, values ​​are shown at 25° C. and 1 atmospheric pressure (atmosphere). Also, the average is an arithmetic mean value. (First embodiment) The first embodiment relates to a solar cell and a method for manufacturing the solar cell. A cross-sectional view of a solar cell 100 of the first embodiment is shown. As shown in FIG. 1, the solar cell 100 according to this embodiment has a substrate 1, a p-electrode 2 as a first electrode, a p-type light absorbing layer 3, an n-type layer 4, and an n-electrode 5 as a second electrode. An intermediate layer (not shown) may be included between the n-type layer 4 and the n-electrode 5. Sunlight may be incident from either the n-electrode 5 side or the p-electrode 2 side, but it is more preferable that it is incident from the n-electrode 5 side. The solar cell 100 of the embodiment is a transparent solar cell, so it is preferable to use it as a top cell (light incident side) of a multi-junction solar cell. In FIG. 1, the substrate 1 is provided on the opposite side of the p-electrode 2 from the p-type light absorbing layer 3 side. In the solar cell 100 of the embodiment, light is incident from the n-electrode 5 side toward the p-electrode 2 side.

[0008] The substrate 1 is a transparent substrate. For the substrate 1, organic substrates such as light-transmitting acrylic, polyimide, polycarbonate, polyethylene terephthalate (PET), polypropylene (PP), fluorine-based resin (polytetrafluoroethylene (PTFE), perfluoroethylene propene copolymer (FEP), ethylene tetrafluoroethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), perfluoroalkoxyalkane (PFA), etc.), polyarylate, polysulfone, polyethersulfone, polyetherimide, etc., or inorganic substrates such as soda-lime glass, white plate glass, chemically strengthened glass, and quartz, etc., can be used. The substrate 1 may be a laminate of the substrates listed above. The solar cell 100 in which the substrate 1 is omitted is also included in the embodiment.

[0009] The p-electrode 2 is provided on the substrate 1 and is disposed between the substrate 1 and the p-type light absorbing layer 3. The p-electrode 2 is a conductive layer having optical transparency provided on the p-type light absorbing layer 3 side. The thickness of the p-electrode 2 is typically 100 nm or more and 2,000 nm or less. In FIG. 1, the p-electrode 2 is in direct contact with the p-type light absorbing layer 3. In the case of a transparent solar cell 100, the p-electrode 2 preferably includes one or more oxide transparent conductive films (semiconductor conductive films). In the case of a non-transparent solar cell 100, a metal film that does not transmit light, such as Au or Ag, having a thickness of 100 nm or more can be used as the p-electrode 2. Examples of the oxide transparent conductive film include, but are not limited to, indium tin oxide (ITO), aluminum doped zinc oxide (AZO), boron doped zinc oxide (BZO), gallium doped zinc oxide (GZO), doped tin oxide, titanium doped indium oxide (ITiO), indium zinc oxide (IZO), indium gallium zinc oxide (IGZO), and hydrogen doped indium oxide (IOH). The oxide transparent conductive film may be a laminated film having a plurality of films.

[0010] The dopant for the film such as tin oxide is not particularly limited as long as it is one or more selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, Cl, etc. The p electrode 2 preferably contains doped tin oxide. When the p electrode 2 contains doped tin oxide, it is preferable that the doped tin oxide is in direct contact with the p-type light absorbing layer 3. When the p electrode 2 contains a doped tin oxide film, it is preferable that the doped tin oxide film is provided on the surface of the p electrode 2 facing the p-type light absorbing layer 3, and it is preferable that the doped tin oxide film is in direct contact with the p-type light absorbing layer 3. The p electrode 2 preferably contains a tin oxide film doped with one or more elements selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, Cl, etc. In the doped tin oxide film, one or more elements selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, Cl, etc. are preferably contained in an amount of 10 atomic % or less relative to the tin contained in the tin oxide film.

[0011] A laminated film in which an oxide transparent conductive film and a metal film are laminated can be used as the p electrode 2. The metal film preferably has a thickness of 10 nm or less, and the metal (including alloy) contained in the metal film is not particularly limited, such as Mo, Au, Cu, Ag, Al, Ta, or W. In addition, the p electrode 2 preferably includes a dot-shaped, line-shaped, or mesh-shaped electrode (one or more selected from the group consisting of metal, alloy, graphene, conductive nitride, and conductive oxide) between the oxide transparent conductive film and the substrate 1, or between the oxide transparent conductive film and the p-type light absorbing layer 3. The dot-shaped, line-shaped, or mesh-shaped metal preferably has an aperture ratio of 50% or more with respect to the transparent conductive film. The dot-shaped, line-shaped, or mesh-shaped metal is not particularly limited, such as Mo, Au, Cu, Ag, Al, Ta, or W. When a metal film is used for the p electrode 2, it is preferable to set the film thickness to about 5 nm or less from the viewpoint of transparency. When a line-shaped or mesh-shaped metal film is used, transparency is ensured at the openings, so the film thickness of the metal film is not limited to this.

[0012] The method for forming the p-electrode 2 on the substrate 1 is, for example, to form a transparent conductive oxide film on the substrate 1 by, for example, sputtering. When a metal film, a mesh-shaped metal, or a line-shaped metal is included in the p-electrode 2, the metal is formed and patterned as necessary.

[0013] The p-type light absorbing layer 3 is a p-type semiconductor layer. The p-type light absorbing layer 3 may be in direct contact with the p-electrode 2, or other layers may be present as long as the contact with the p-electrode 2 can be ensured. The p-type light absorbing layer 3 is disposed between the p-electrode 2 and the n-type layer 4. The p-type light absorbing layer 3 is in direct contact with the n-type layer 4. The p-type light absorbing layer 3 is a semiconductor layer of a metal oxide mainly composed of Cu. The metal oxide mainly composed of Cu is cuprous oxide and / or a composite oxide of cuprous oxide. In other words, the p-type light absorbing layer 3 is a layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide. The p-type light absorbing layer 3 is preferably a polycrystal of cuprous oxide and / or a composite oxide of cuprous oxide. The cuprous oxide and / or a composite oxide of cuprous oxide is preferably a polycrystal of cuprous oxide and / or a composite oxide of cuprous oxide. a M1 b O cIt is an oxide represented by the formula: M1 is preferably one or more elements selected from the group consisting of Sn, Sb, Ag, Li, Na, K, Cs, Rb, Al, In, Zn, Mg, and Ca. It is preferable that a, b, and c satisfy 1.80≦a≦2.01, 0.00≦b≦0.20, and 0.98≦c≦1.02. It is preferable that 90 wt% or more of the p-type light absorbing layer 3 is cuprous oxide and / or a composite oxide of cuprous oxide. It is more preferable that 95 wt% or more of the p-type light absorbing layer 3 is cuprous oxide and / or a composite oxide of cuprous oxide. It is even more preferable that 98 wt% or more of the p-type light absorbing layer 3 is cuprous oxide and / or a composite oxide of cuprous oxide. It is preferable that the p-type light absorbing layer 3 contains almost no Cu and / or CuO, which are heterophases. It is preferable that the p-type light absorbing layer 3 contains few heterophases and has good crystallinity, because the transmittance of the p-type light absorbing layer 3 is high. When the p-type light absorbing layer 3 contains an element M2, the band gap of the p-type light absorbing layer 3 can be adjusted. The band gap of the p-type light absorbing layer 3 is preferably 2.0 eV or more and 2.2 eV or less. With a band gap in this range, in a multi-junction solar cell in which a solar cell using Si as a light absorbing layer is used as a bottom cell and the solar cell of the embodiment is used as a top cell, sunlight can be efficiently utilized in both the top cell and the bottom cell. The p-type light absorbing layer 3 preferably contains Sn and / or Sb. The Sn and Sb in the p-type light absorbing layer 3 may be added to the p-type light absorbing layer 3 or may be derived from the p-electrode 2. Hereinafter, in the places where cuprous oxide is described, a composite oxide of cuprous oxide is also included in the description.

[0014] Elements such as Cu and M1 contained in the p-type light absorbing layer 3 and elements such as Ga and M2 contained in the n-type layer 4 may be partially diffused near the boundary between the p-type light absorbing layer 3 and the n-type layer 4.

[0015] The above composition ratio of the p-type light absorbing layer 3 is the composition ratio of the entire p-type light absorbing layer 3. It is preferable that the above compound composition ratio of the p-type light absorbing layer 3 is satisfied throughout the p-type light absorbing layer 3. If the concentrations of Sn and Sb in the p-type light absorbing layer 3 are high, defects increase, leading to increased carrier recombination. Therefore, the total volume concentration of Sb and Sn in the p-type light absorbing layer 3 is set to 1.5x10 19 atoms / cm 3 The following is preferred:

[0016] The composition of the p-type light absorbing layer 3 is the average value of the composition at depths of 0.2d3, 0.5d3, and 0.8d3 from the surface of the p-type light absorbing layer 3 on the p-electrode 2 side, assuming that the thickness of the p-type light absorbing layer 3 is d3. Except for the condition that the element composition ratio of the compound of the p-type light absorbing layer 3 is inclined, the p-type light absorbing layer 3 preferably satisfies the above and following suitable compositions at each depth. The analysis is performed by analyzing the analysis spots (A1 to A9) distributed at each distance from the surface of the n-type layer as equally spaced as possible as shown in the diagram explaining the analysis spots in FIG. 2 by, for example, secondary ion mass spectrometry (SIMS). FIG. 2 is a schematic diagram of the solar cell 100 as seen from the light incident side. When analyzing the composition of the p-type light absorbing layer 3, D1 is the length in the width direction of the p-type light absorbing layer 3, and D2 is the length in the depth direction of the p-type light absorbing layer 3.

[0017] The thickness of the p-type light absorbing layer 3 is determined by cross-sectional observation using an electron microscope or a step gauge, and is preferably 1,000 nm or more and 10,000 nm or less.

[0018] The n-type layer 4 is an n-type semiconductor layer. The n-type layer 4 is disposed between the p-type light absorbing layer 3 and the n-electrode 5. The n-type layer 4 is in direct contact with the surface of the p-type light absorbing layer 3 opposite to the surface in contact with the p-electrode 2. The n-type layer 4 is a semiconductor layer containing an oxide or a sulfide. The n-type layer 4 preferably contains at least one of an oxide or a sulfide. The n-type layer 4 preferably contains an oxide containing Ga as a main component. The n-type layer 4 preferably contains an oxide or a sulfide containing one or more elements selected from the group consisting of Ga, Al, B, In, Ti, Zn, Hf, Zr, Cd, Sn, Si, and Ge.

[0019] The n-type layer 4 is a single layer or a multilayer. The n-type layer 4 preferably contains a single layer or a multilayer of oxide, or a single layer or a multilayer of sulfide. The n-type layer 4 may have a gradient composition in a single layer, or each layer of the n-type layer 4 may have a gradient composition. When the n-type layer 4 is a multilayer, the layers are a first n-type layer and a second n-type layer in this order from the p-type light absorbing layer 3 side. For example, when the n-type layer 4 is a three-layered layer, the n-type layer 4 is stacked in the order of a first n-type layer, a second n-type layer, and a third n-type layer from the p-type light absorbing layer 3 side. The surface of the first n-type layer facing the p-type light absorbing layer 3 side is in direct contact with the p-type light absorbing layer 3. When the n-type layer 4 is a multilayered layer, it is preferable that all layers are oxide layers or all layers are sulfide layers.

[0020] When the n-type layer 4 contains an oxide, the oxide of the n-type layer 4 is preferably an oxide containing one or more elements selected from the group consisting of Ga, Al, B, In, Ti, Zn, Hf, Zr, Sn, Si and Ge. The oxide of the n-type layer 4 easily extracts oxygen bonded to Cu in the cuprous oxide and / or the composite oxide of cuprous oxide when the n-type layer 4 is formed. The sulfide of the n-type layer 4 may contain Cu and M1 elements diffused from the cuprous oxide and / or the composite oxide of cuprous oxide. When the n-type layer 4 is a multi-layer n-type semiconductor layer containing an oxide, it is preferable that the ratio of Ga to the metal elements of the oxide in at least one layer is 50 atom % or more. When the n-type layer 4 is a multi-layer n-type semiconductor layer containing an oxide, it is preferable that the ratio of Ga to the metal elements of the oxide in at least the first n-type layer is 50 atom % or more.

[0021] When the n-type layer 4 contains a sulfide, the sulfide of the n-type layer 4 is preferably a sulfide containing one or more elements selected from the group consisting of Ga, In, Zn, and Cd. The sulfide of the n-type layer 4 is more preferably a sulfide containing Zn and In, a sulfide containing Cd and Zn, and a sulfide containing In and Ga. The sulfide of the n-type layer 4 easily extracts oxygen bonded to Cu in the cuprous oxide and / or the composite oxide of cuprous oxide when the n-type layer 4 is formed. The sulfide of the n-type layer 4 may contain Cu, M1, and O diffused from the cuprous oxide and / or the composite oxide of cuprous oxide.

[0022] The composition of the compound in the n-type layer 4 is the average composition of the entire n-type layer 4 unless otherwise specified. The composition of the n-type layer 4 is the average value of the composition at depths of 0.2d4, 0.5d4, and 0.8d4 from the surface of the n-type layer 4 on the p-type light absorbing layer 3 side (the boundary between the p-type light absorbing layer 3 and the n-type layer 4) when the thickness of the n-type layer 4 is d4. When the n-type layer 4 is very thin (for example, 5 nm or less), the composition at a depth of 0.5d from the p-type light absorbing layer 3 side and the surface of the n-type layer 4 can be regarded as the composition of the entire n-type layer 4. The analysis is performed by analyzing the analysis spots (A1 to A9) that are distributed as closely as possible at equal intervals at each distance from the surface of the n-type layer 4 as shown in the diagram explaining the analysis spots in FIG. 2, for example, by secondary ion mass spectrometry (SIMS). FIG. 2 is a schematic diagram of a solar cell 100 viewed from the light incident side. When analyzing the composition of the n-type layer 4, D1 is the length of the n-type layer 4 in the width direction, and D2 is the length of the n-type layer 4 in the depth direction.

[0023] It is preferable that the boundary between the p-type light absorbing layer 3 and the n-type layer 4 contains little Cu phase, which is a different phase of cuprous oxide. Examples of different phases of cuprous oxide and complex oxide of cuprous oxide that may exist at the boundary between the p-type light absorbing layer 3 and the n-type layer 4 include Cu phase and CuO phase. Even if the Cu phase does not exist on the surface of the p-type light absorbing layer 3 before the n-type layer 4 is formed, after the n-type layer 4 is formed, when the oxide or sulfide of the n-type layer 4 is formed, the oxygen of Cu2O is extracted by the element M2 contained in the oxide and sulfide, and Cu2O is reduced, and Cu is likely to precipitate near the boundary between the p-type light absorbing layer 3 and the n-type layer 4. If a Cu phase exists near the boundary between the p-type light absorbing layer 3 and the n-type layer 4, the recombination rate in the p-type light absorbing layer 3 increases, Voc decreases, and it is considered that this causes a decrease in conversion efficiency. Since the amount of Cu present near the boundary between the p-type light absorbing layer 3 and the n-type layer 4 after the formation of the n-type layer 4 is very small, it is difficult to directly measure the position and amount of the Cu phase. Until now, it has been difficult to quantitatively evaluate the Cu phase near the boundary between the p-type light absorbing layer 3 and the n-type layer 4.

[0024] The inventors have noticed that the brightness of the p-type light absorbing layer 3 near the boundary between the p-type light absorbing layer 3 and the n-type layer 4 is high from the brightness profile of a high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image, and have discovered that the high brightness region contains a Cu phase. FIG. 3 shows a HAADF-STEM image and brightness profile of a solar cell of a reference example. From the HAADF-STEM image and brightness profile of FIG. 3, it can be seen that a high brightness region exists near the surface of the p-type light absorbing layer 3 on the n-type layer 4 side. Analysis of this revealed that it was a Cu phase. Even if a member in which a Cu phase was not confirmed on the surface of the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide was used before the n-type layer 4 was formed, a Cu phase was confirmed after the n-type layer 4 was formed. The inventors have found a method for reducing or eliminating this Cu phase. Comparing the Voc and conversion efficiency of a solar cell in which a Cu phase remains (reference example) and the solar cell 100 of the embodiment, it was confirmed that the solar cell 100 of the embodiment had a tendency to have improved Voc and conversion efficiency.

[0025] From the above results, the inventors have found the following evaluation method, which is correlated with Voc and conversion efficiency, for the Cu phase in the p-type light absorbing layer 3 near the boundary between the p-type light absorbing layer 3 and the n-type layer 4. Since it is difficult to directly measure the amount of the Cu phase, the amount of the Cu phase is evaluated from the brightness profile of the HAADF-STEM image.

[0026] FIG. 4 shows the HAADF-STEM image and the luminance profile of the solar cell 100 of the embodiment. In the luminance profile of FIG. 4, no clear high luminance peak is confirmed in the region of the p-type light absorbing layer 3 on the n-type layer 4 side. In the p-type light absorbing layer 3, the region from the boundary between the p-type light absorbing layer 3 and the n-type layer 4 to a depth of 10 nm toward the p-electrode 2 side is defined as the first region. In addition, the region from the boundary between the p-type light absorbing layer 3 and the n-type layer 4 to a depth of 100 nm toward the p-electrode 2 side of the p-type light absorbing layer 3, excluding the first region, is defined as the second region. Note that the region (bulk) of the p-type light absorbing layer 3 excluding the first and second regions is defined as the third region, and it is preferable that the third region also satisfies the same luminance profile conditions as the second region described below.

[0027] The boundary between the p-type light absorbing layer 3 and the n-type layer 4 may not be clear. When the boundary between the p-type light absorbing layer 3 and the n-type layer 4 is not clear, the boundary between the p-type light absorbing layer 3 and the n-type layer 4 can be found from the brightness profile of the HAADF-STEM image. In the vicinity of the boundary between the p-type light absorbing layer 3 and the n-type layer 4, the position shifted 1 nm toward the p-electrode 2 from the position where the brightness is lowest can be regarded as the boundary between the p-type light absorbing layer 3 and the n-type layer 4. The boundary between the p-type light absorbing layer 3 and the n-type layer 4 may not be flat but may be uneven. The interface between the p-type light absorbing layer 3 and the n-type layer 4 can be identified by observing the cross section of the p-type light absorbing layer 3 and the n-type layer 4.

[0028] The maximum brightness of the brightness profile of the HAADF-STEM image of the first region is preferably 95% or more and 105% or less of the average brightness of the brightness profile of the HAADF-STEM image of the second region. If the maximum brightness of the brightness profile of the HAADF-STEM image of the first region is less than 95% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, a large amount of CuO phase is present, and an appropriate pn interface cannot be formed, which causes a decrease in Voc. If the maximum brightness of the brightness profile of the HAADF-STEM image of the first region is greater than 105% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, the first region contains a Cu phase, and the recombination speed in the p-type light absorbing layer 3 is high, resulting in a decrease in Voc. It is more preferable that the maximum brightness of the brightness profile of the HAADF-STEM image of the first region is 97% or more and 103% or less of the average brightness of the brightness profile of the HAADF-STEM image of the second region. It is preferable that the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide before forming the n-type layer 4 also satisfies the same preferable conditions of the brightness profile of the HAADF-STEM image as the p-type light absorbing layer 3. In the brightness profile shown in FIG. 4, the maximum brightness of the brightness profile of the HAADF-STEM image of the first region is 102% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, and the above condition is satisfied. In the brightness profile shown in FIG. 3, the maximum brightness of the brightness profile of the HAADF-STEM image of the first region is 115% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, and the above condition is not satisfied. Similarly, the maximum brightness of the brightness profile of the HAADF-STEM image of the first region is preferably 95% to 105% of the average brightness of the brightness profile of the HAADF-STEM image of the third region, and more preferably 97% to 103%.

[0029] The brightness profile of the HAADF-STEM image is obtained by the following method. After the sample is processed with a focused ion beam (FIB), HAADF-STEM observation is performed at an acceleration voltage of 120 kV using an atomic resolution analytical electron microscope JEM-ARM200F Dual-X (manufactured by JEOL). The brightness profile is detected, and contrast correction is performed in the range of 20 nm to 40 nm from the boundary between the p-type light absorbing layer 3 and the n-type layer 4 toward the p-electrode 2 side, and the maximum brightness is calculated based on the intensity in that range. It is preferable to perform the contrast correction so that the low brightness (brightness of the n-type layer 4 on the n-electrode side) and the high brightness (average brightness of the second region of the p-type light absorbing layer 3) of the solar cell that has been subjected to the heating treatment of the embodiment and the solar cell that has not been subjected to the heating treatment of the embodiment are approximately the same.

[0030] The average brightness of the brightness profile of the HAADF-STEM image of the first region is preferably 85% to 95% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, and more preferably 87% to 93%. In the brightness profile shown in FIG. 4, the average brightness of the brightness profile of the HAADF-STEM image of the first region is 91% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, and the above condition is satisfied. In the brightness profile shown in FIG. 3, the average brightness of the brightness profile of the HAADF-STEM image of the first region is 98% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, and the above condition is not satisfied. In the brightness profile of the reference example in FIG. 3, the average brightness of the second region is not low, but the above condition is not satisfied due to the high peak and high average brightness of the first region. Similarly, the average brightness of the brightness profile of the HAADF-STEM image of the first region is preferably 85% to 95%, and more preferably 87% to 93%, of the average brightness of the brightness profile of the HAADF-STEM image of the third region.

[0031] The minimum brightness of the brightness profile of the HAADF-STEM image of the first region from the boundary between the p-type light absorbing layer 3 and the n-type layer 4 toward the p-electrode 2 side to the depth position of 5 nm to 10 nm is preferably 85% to 95% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, and more preferably 87% to 93%. In the brightness profile shown in Fig. 4, the minimum brightness of the brightness profile of the HAADF-STEM image of the first region from the boundary between the p-type light absorbing layer 3 and the n-type layer 4 toward the p-electrode 2 side to the depth position of 5 nm to 10 nm is 89% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, which satisfies the above condition. In the brightness profile shown in FIG. 3, the minimum brightness of the brightness profile of the HAADF-STEM image of the region from the boundary position between the p-type light absorbing layer 3 and the n-type layer 4 in the first region toward the p-electrode 2 side to the depth position of 5 nm to 10 nm is 93% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, and the above condition is satisfied. In the brightness profile of the reference example in FIG. 3, the difference between the minimum brightness of the region from the boundary position between the p-type light absorbing layer 3 and the n-type layer 4 in the first region toward the p-electrode 2 side to the depth position of 5 nm to 10 nm is small compared to the average brightness of the second region, and the above condition is satisfied. Similarly, the minimum brightness of the brightness profile of the HAADF-STEM image of the region from the boundary position between the p-type light absorbing layer 3 and the n-type layer 4 in the first region toward the p-electrode 2 side to the depth position of 5 nm to 10 nm is preferably 85% to 95% of the average brightness of the brightness profile of the HAADF-STEM image of the third region, and more preferably 87% to 93%.

[0032] The minimum brightness of the brightness profile of the HAADF-STEM image of the first region is preferably 78% to 85% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, and more preferably 80% to 83%. In the brightness profile of FIG. 4, the minimum brightness of the brightness profile of the HAADF-STEM image of the first region is 81% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, which satisfies the above condition. In the brightness profile of FIG. 3, the minimum brightness of the brightness profile of the HAADF-STEM image of the first region is 80% of the average brightness of the brightness profile of the HAADF-STEM image of the second region, which satisfies the above condition. In the brightness profile of the reference example of FIG. 3, there is no clear peak in the second region, but the bottom of the peak in the first region is low, so the above condition is not met. Similarly, the minimum brightness of the brightness profile of the HAADF-STEM image of the first region is preferably 78% or more and 85% or less of the average brightness of the brightness profile of the HAADF-STEM image of the third region, and more preferably 80% or more and 83% or less.

[0033] The average brightness of the brightness profile of the HAADF-STEM image of the first region is preferably 85% to 95% of the maximum brightness of the brightness profile of the HAADF-STEM image of the first region, more preferably 87% to 93%, and is preferably 110% to 120% of the minimum brightness of the brightness profile of the HAADF-STEM image of the first region, more preferably 112% to 118%. In the brightness profile shown in FIG. 4, the average brightness of the brightness profile of the HAADF-STEM image of the first region is 90% of the maximum brightness of the brightness profile of the HAADF-STEM image of the first region, and is 113% of the minimum brightness of the brightness profile of the HAADF-STEM image of the first region, satisfying the above condition. In the brightness profile shown in FIG. 3, the average brightness of the brightness profile of the HAADF-STEM image of the first region is 79% of the maximum brightness of the brightness profile of the HAADF-STEM image of the first region, not satisfying the above condition. In the luminance profile of the reference example in FIG. 3, the bottom of the peak in the first region is low and the top is high, so that the above condition is not satisfied.

[0034] The average brightness of the brightness profile of the HAADF-STEM image of the second region is preferably 90% to 99% of the maximum brightness of the brightness profile of the HAADF-STEM image of the second region, more preferably 92% to 97%, and is preferably 101% to 110% of the minimum brightness of the brightness profile of the HAADF-STEM image of the second region, more preferably 103% to 108%. In the brightness profile shown in FIG. 4, the average brightness of the brightness profile of the HAADF-STEM image of the second region is 95% of the maximum brightness of the brightness profile of the HAADF-STEM image of the second region and 108% of the minimum brightness of the brightness profile of the HAADF-STEM image of the second region, satisfying the above condition. In the brightness profile shown in FIG. 3, the average brightness of the brightness profile of the HAADF-STEM image of the second region is 97% of the maximum brightness of the brightness profile of the HAADF-STEM image of the second region and 103% of the minimum brightness of the brightness profile of the HAADF-STEM image of the second region, satisfying the above condition. In the reference example of Fig. 3, the crystallinity of the p-type light absorbing layer 3 in the bulk (second region) is good and there are few heterogeneous phases, so the brightness profile of the reference example in Fig. 3 also satisfies the above conditions. Similarly, the average brightness of the brightness profile of the HAADF-STEM image of the third region is preferably 90% to 99% of the maximum brightness, and more preferably 92% to 97%, and is preferably 101% to 110% of the minimum brightness, and more preferably 103% to 108%.

[0035] The n-electrode 5 is preferably an electrode on the n-type layer 4 side, which has optical transparency to visible light. The n-type layer 4 is sandwiched between the n-electrode 5 and the p-type light absorbing layer 3. An intermediate layer (not shown) can be provided between the n-type layer 4 and the n-electrode 5. This intermediate layer can include a mesh or line-shaped electrode. The n-electrode 5 is preferably made of an oxide transparent conductive film (semiconductor conductive film). The oxide transparent conductive film used in the n-electrode 5 is preferably one or more transparent conductive films selected from the group consisting of indium tin oxide, aluminum-doped zinc oxide, boron-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, titanium-doped indium oxide, indium gallium zinc oxide, and hydrogen-doped indium oxide. Graphene can also be used in the n-electrode 5. Graphene is preferably laminated with silver nanowires. In the case where the solar cell 100 is not made optically transparent and the p-electrode 2 has optical transparency to visible light, the n-electrode 5 can be made of a metal film having a thickness of 100 nm or more, similar to the p-electrode 2.

[0036] The thickness of n-electrode 5 is determined by cross-sectional observation using an electron microscope or a step gauge, and is not particularly limited, but is typically 1 nm or more and 2 μm or less.

[0037] Next, a method for manufacturing the solar cell 100 will be described. A flowchart of the method for manufacturing the solar cell 100 of the embodiment is shown in Fig. 5. The method for manufacturing the solar cell 100 of the embodiment includes the steps of forming an n-type layer 4 on a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide, forming an n-electrode 5 on the n-type layer 4, and heating the member on which the n-type layer is formed after the step of forming the n-type layer and before the step of forming the n-electrode, or during the step of forming the n-type layer.

[0038] The layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide is a precursor of the p-type light absorbing layer 3. The layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide becomes the p-type light absorbing layer 3 by forming a part or all of the n-type layer 4 and then heating it. In the step of forming the n-type layer 4 on the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide, the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide provided on the p-electrode 2 on the substrate 1, the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide provided on the p-electrode 2, or the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide is a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide.

[0039] The layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide provided on p-electrode 2 on substrate 1 is obtained by forming p-electrode 2 on substrate 1, and further forming a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide on p-electrode 2. When substrate 1 is not used, a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide may be formed on p-electrode 2, or the p-electrode may be formed on a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide.

[0040] As a method for forming a layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide on the p-electrode 2, a layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide is formed on the p-electrode 2. The layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide is preferably formed by sputtering. It is preferable to form a layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide with few heterogeneous phases. Sputtering is preferably performed by heating a member having the p-electrode 2 formed on the substrate 1 to 300°C or higher and 600°C or lower, and at an oxygen partial pressure of 0.01 [Pa] or higher and 4.8 [Pa] or lower, and at a speed of 0.02 μm / min or higher and 20 μm / min or lower. The temperature of the member having the p-electrode 2 formed on the substrate 1 is considered to be equal to the temperature of the stage. From the viewpoint of forming a polycrystalline film having high transparency and large grain size, when the deposition rate is d, the oxygen partial pressure is more preferably 0.55xd [Pa] or more and 1.00xd [Pa] or less. In addition, the heating temperature of the p-electrode 2 is more preferably 350° C. or more and 500° C. or less. An element M1 can be added during the formation of the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide.

[0041] In addition to sputtering, a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide can be formed by heating a Cu plate in an oxygen atmosphere to oxidize Cu to Cu2O to obtain a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide. The cuprous oxide layer can be doped with an element M1 by, for example, implanting ions into the cuprous oxide layer.

[0042] The process of forming the n-type layer 4 on the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide includes forming the n-type layer 4 on the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide provided on the p-electrode 2 on the substrate 1 described above, the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide provided on the p-electrode 2, or a member made of a single layer of a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide. The n-type layer 4 may be formed by depositing the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide by atomic layer deposition or the like, or by transferring the n-type layer 4 to the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide and heating it. By heating after the transfer, the n-type layer 4 and the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide are bonded to each other. It is believed that when n-type layer 4 is deposited or heated after transfer, that is, when and after the oxide or sulfide crystals of n-type layer 4 are bonded with cuprous oxide and / or composite oxide of cuprous oxide by heating, a Cu phase precipitates in the first region on the side of the layer mainly composed of cuprous oxide and / or composite oxide of cuprous oxide on which n-type layer 4 is formed.

[0043] The temperature of the layer mainly composed of cuprous oxide or a composite oxide of cuprous oxide when depositing the n-type layer 4 is, for example, 100° C. or higher and 150° C. or lower. It is preferable to deposit the n-type layer 4 on the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide in a sulfiding or oxidizing atmosphere.

[0044] The step of heating the member on which the n-type layer is formed after the step of forming the n-type layer 4 and before the step of forming the n-electrode, or during the step of forming the n-type layer, is a step of oxidizing the precipitated Cu phase. The heat treatment is performed after the formation of the single-layer n-type layer 4 and before the formation of the n-electrode 5, or after the formation of one or more layers of the multi-layer n-type layer 4 and before the formation of the n-electrode 5. The heat treatment oxidizes the Cu phase, but if the heat treatment is performed in an oxidizing atmosphere, the cuprous oxide is further oxidized to become CuO. If the CuO phase exists, the transmittance and power generation characteristics of the p-type light absorbing layer 3 are greatly reduced. Therefore, the heating step is preferably performed in a non-oxidizing atmosphere. When the heating step is performed, the p-electrode 2 may be formed, but the n-electrode 5 is not formed.

[0045] The heating step is performed by placing the member in which the n-type layer 4 is formed on the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide in a sealed container, for example, in a glove box in which an inert gas is flowed, or on a stage in a vacuum chamber. Note that a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide may be formed, and a treatment such as oxidizing the surface of the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide may be performed before forming the n-type layer 4. Even if this oxidation treatment is performed, Cu precipitates when forming the n-type layer 4, so it is effective to perform the heating step.

[0046] It is to be noted that, since the atmosphere is changed from that in which the n-type layer 4 was formed to that in the heating step, it takes a certain amount of time until the atmosphere meets the following conditions. If the temperature is high at this time under a high oxygen partial pressure, the Cu phase will be excessively oxidized. Therefore, it is preferable to first lower the temperature of the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide to a temperature above room temperature and below 100°C, and then adjust the atmosphere in the container to a suitable oxygen concentration. Alternatively, the member on which the n-type layer 4 has been formed may be moved into a container adjusted to a suitable oxygen concentration.

[0047] The temperature of the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide in the heating step is preferably 150°C or more and 250°C or less. If the temperature is too low, a large amount of Cu phase remains, and the heating step is substantially ineffective. If the temperature is too high, not only the Cu phase becomes a CuO phase, but also the cuprous oxide of the cuprous oxide and / or composite oxide of cuprous oxide becomes copper oxide. Furthermore, metal elements contained in the n-type layer 4 diffuse into the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide, and metal elements contained in the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide diffuse into the n-type layer 4, which may deteriorate the characteristics of the p-type light absorbing layer 3 and the n-type layer 4. For these reasons, the temperature of the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide in the heating step is more preferably 160°C or more and 230°C or less, and even more preferably 170°C or more and 220°C or less.

[0048] The treatment time of the heating step is preferably 5 minutes or more and 60 minutes or less. If the heating treatment is too short, the conversion of the Cu phase to cuprous oxide does not proceed sufficiently. If the heating treatment is too long, not only the Cu phase becomes a CuO phase, but also the cuprous oxide of the cuprous oxide and / or cuprous oxide composite oxide becomes copper oxide. Furthermore, a long treatment time is not economical. Therefore, the treatment time of the heating step is more preferably 15 minutes or more and 50 minutes or less, and even more preferably 15 minutes or more and 45 minutes or less. When the temperature of the layer mainly composed of cuprous oxide and / or cuprous oxide composite oxide in the heating step is 150°C or more and 180°C or less, the treatment time is preferably 20 minutes or more and 60 minutes or less, and more preferably 30 minutes or more and 60 minutes or less. When the temperature of the layer mainly composed of cuprous oxide and / or cuprous oxide composite oxide in the heating step is 170°C or more and 220°C or less, the treatment time is preferably 10 minutes or more and 50 minutes or less, and more preferably 10 minutes or more and 40 minutes or less. When the temperature of the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide in the heating step is 210° C. or higher and 250° C. or lower, the treatment time is preferably 5 minutes or higher and 40 minutes or lower, more preferably 5 minutes or higher and 30 minutes or lower. When the temperature of the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide in the heating step is 150° C. or higher and 220° C. or lower, the treatment time is preferably 10 minutes or higher and 60 minutes or lower, more preferably 20 minutes or higher and 50 minutes or lower. When the temperature of the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide in the heating step is 210° C. or higher and 250° C. or lower, the treatment time is preferably 5 minutes or higher and 50 minutes or lower, more preferably 5 minutes or higher and 40 minutes or lower.

[0049] The atmosphere during the heating process has an oxygen concentration (mass [g] / volume [L]) of 8.0×10 -4 [g / L] or less. In the heating step, in an environment with a very low oxygen partial pressure, it is considered that the oxygen contained in the atmosphere in the heating step is unlikely to oxidize the Cu phase. If the oxygen concentration is high, not only will the Cu phase turn into a CuO phase, but the cuprous oxide and / or cuprous oxide composite oxide will turn into copper oxide. Therefore, the oxygen concentration in the atmosphere during heating is set to 5.0×10 -8 [g / L] or more 8.0×10 -4It is more preferable that the oxygen concentration is 5.0×10 -8 [g / L] or more 2.0×10 -4 It is even more preferable that the oxygen concentration is 5.0×10 -8 [g / L] or more 1.0×10 -4 From the same viewpoint, the ozone concentration in the atmosphere during heating (mass [g] / volume [L]) is preferably 0.0 [g / L] or more and 5.0×10 -4 [g / L] or less is preferable, and 0.0 [g / L] or more 2.0 × 10 -4 [g / L] or less is more preferable, and 0.0 [g / L] or more and 1.4 × 10 -4 [g / L] or less. The ozone concentration is preferably lower than the oxygen concentration, and more preferably 1 / 10 or less of the oxygen concentration. From the same viewpoint, the water vapor degree (mass [g] / volume [L]) of the atmosphere during heating is preferably 8.0×10 -4 [g / L] or less is preferable, and 5.0×10 -8 [g / L] or more 8.0×10 -4 [g / L] or less is more preferable, and 5.0×10 -8 [g / L] or more 2.0×10 -4 [g / L] or less is even more preferred.

[0050] The total pressure of the non-oxidizing atmosphere in the heating step is not particularly limited, but is preferably 100 Pa or more and 200,000 Pa or less. The non-oxidizing atmosphere contains an inert gas such as Ar. The non-oxidizing atmosphere in the heating step may contain a trace amount of reducing gas. The reducing gas is preferably at a level that does not substantially affect the oxidation of the Cu phase. The partial pressure of the reducing gas is preferably lower than the partial pressure of oxygen and the partial pressure of ozone.

[0051] It is preferable to carry out the heating step before forming the n-electrode 5. If heating is carried out after the n-electrode 5 is formed, the metal elements contained in the n-type layer 4 will diffuse into the n-electrode 5, and the metal elements contained in the n-electrode 5 will diffuse into the n-type layer 4, degrading the characteristics of the n-type layer 4 and the n-electrode 5. Therefore, it is preferable to carry out the heating step before forming the n-electrode 5.

[0052] Here, the heating step will be described with reference to an example. First, the case where the n-type layer 4 is a single layer will be described. After the single n-type layer 4 is formed on a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide, a heating step is performed.

[0053] A case where the n-type layer 4 is multi-layered will be described. When the n-type layer 4 is multi-layered, the continuity of the connection of the conduction band bottom between the p-type light absorbing layer 3 and the n-type layer 4 and the connectivity of the conduction band bottom between the n-type layer 4 and the n-electrode 5 are likely to be improved. When the connectivity of the conduction band bottom between the p-type light absorbing layer 3 and the n-electrode 5 is improved, the short-circuit current density is improved, which contributes to improving the conversion efficiency. Therefore, the difference between the conduction band bottom of the p-type light absorbing layer 3 and the conduction band bottom of the n-type layer 4 ([the conduction band bottom of the p-type light absorbing layer 3]-[the conduction band bottom of the n-type layer 4]) is preferably 0.0 eV or more and 0.5 eV or less, more preferably 0.0 eV or more and 0.4 eV or less.

[0054] An example will be described in which the n-type layer 4 is two-layered, including a first n-type layer and a second n-type layer. The first n-type layer is formed on a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide. The first time is the time after the first n-type layer is formed and before the second n-type layer is formed. The second time is the time after the first n-type layer is formed and before the n-electrode 5 is formed. The heating step can be performed at the first time and / or the second time. When the heating step is performed at the first time, the Cu phase precipitated near the boundary between the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide and the first n-type layer can be oxidized and changed to cuprous oxide. When the heating step is performed at the second time, the Cu phase precipitated near the boundary between the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide and the first n-type layer can be oxidized and changed to cuprous oxide, and the metal element contained in the first n-type layer can be diffused to the second n-type layer and the metal element contained in the second n-type layer can be diffused to the first n-type layer. When it is desired to prevent diffusion, it is preferable to perform the heating step only at the first time. By performing the heating step at a plurality of times, even if a Cu phase is formed during the formation of the second n-type layer, this Cu phase can be oxidized. When the heating step is performed at the first time and the second time, the conditions of the two heating steps may be the same or different.

[0055] Another example will be described in which the n-type layer 4 is multi-layered. An example will be described in which the n-type layer 4 is two-layered, including a first n-type layer and a second n-type layer. The first n-type layer is Ga2O3, and the second n-type layer is ZTO. The first n-type layer is formed on a layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide. The first time is the time after the first n-type layer is formed and before the second n-type layer is formed. The second time is the time after the first n-type layer is formed and before the n-electrode 5 is formed. The heating step can be performed at the first time and / or the second time. When the heating step is performed at the first time, the Cu phase precipitated near the boundary between the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide and the first n-type layer can be oxidized and changed to cuprous oxide. When the heating step is performed at the second time, the Cu phase precipitated near the boundary between the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide and the first n-type layer can be oxidized and changed to cuprous oxide, and the metal elements contained in the first n-type layer can be diffused into the second n-type layer and the metal elements contained in the second n-type layer can be diffused into the first n-type layer. When Ga diffuses into the second n-type layer, Ga is present on the first n-type layer side of the second n-type layer, and when Zn and Sn diffuse into the first n-type layer, Zn and Sn are present on the second n-type layer side of the first n-type layer. Then, the composition of the first n-type layer and the second n-type layer changes gradually, improving the continuity of the connection at the bottom of the conduction band. Improving the continuity of the connection at the bottom of the conduction band increases the short-circuit current density of the solar cell 100, contributing to improving the conversion efficiency. Under the above-mentioned heating conditions, elements can be diffused so as to improve the connectivity at the bottom of the conduction band between the p-type light absorbing layer 3 and the n-electrode 5. When the heating step is performed at the first time and the second time, the conditions for the two heating steps may be the same or different.

[0056] Similarly, when the n-type layer 4 has a multi-layer structure of three or more layers, a heating step can be carried out after (during and / or after) forming each layer of the n-type layer 4 and before forming the n-electrode 5.

[0057] In the step of forming an n-electrode on the n-type layer 4, the n-electrode 5 is formed on the n-type layer 4 by sputtering or the like. When an intermediate layer is provided between the n-type layer 4 and the n-electrode 5, the intermediate layer is formed before forming the n-electrode 5. Through the above steps, a solar cell 100 is manufactured, which has the substrate 1, the p-electrode 2, the p-type light absorbing layer 3 mainly made of cuprous oxide and / or a composite oxide of cuprous oxide whose surface has been oxidized, the n-type layer 4, and the n-electrode 5.

[0058] Second embodiment The second embodiment relates to a multijunction solar cell. Fig. 6 shows a cross-sectional conceptual diagram of a multijunction solar cell of the second embodiment. The multijunction solar cell 200 of Fig. 6 has a solar cell (first solar cell) 100 of the first embodiment and a second solar cell 201 on the light incident side. The first solar cell 100 is the solar cell of the first embodiment. The band gap of the light absorption layer of the second solar cell 201 is smaller than the band gap of the p-type light absorption layer 3 of the multijunction solar cell 200 of the second embodiment. The multijunction solar cell of the embodiment also includes a solar cell in which three or more solar cells are joined together.

[0059] Since the band gap of the p-type light absorbing layer 3 of the solar cell 100 of the first embodiment is about 2.0 eV to 2.2 eV, the band gap of the light absorbing layer of the second solar cell 201 is preferably 1.0 eV or more and 1.6 eV or less. The light absorbing layer of the second solar cell is preferably one selected from the group consisting of one or more compound semiconductor layers selected from the group consisting of CIGS and CdTe with a high In content, crystalline silicon, and a perovskite compound.

[0060] Third embodiment The third embodiment relates to a solar cell module. Fig. 7 shows a perspective view of a solar cell module 300 of the third embodiment. The solar cell module 300 in Fig. 7 is a solar cell module in which a first solar cell module 301 and a second solar cell module 302 are stacked. The first solar cell module 301 is on the light incident side, and uses the solar cell 100 of the first embodiment. It is preferable to use a second solar cell 201 for the second solar cell module 302.

[0061] FIG. 8 shows a cross-sectional view of a solar cell module 300. FIG. 8 shows the structure of the first solar cell module 301 in detail, but does not show the structure of the second solar cell module 302. For the second solar cell module 302, the structure of the solar cell module is appropriately selected depending on the light absorption layer of the solar cell to be used. The solar cell module 300 in FIG. 8 includes a plurality of submodules 303 surrounded by dashed lines in which a plurality of solar cells 100 (solar cells) are arranged in the horizontal direction and electrically connected in series by wiring 304, and the plurality of submodules 303 are electrically connected in parallel or in series. Adjacent submodules 303 are electrically connected by bus bars 305.

[0062] Adjacent solar cells 100 have their n-electrodes 5 on the upper side and p-electrodes 2 on the lower side connected by wiring 304. Both ends of the solar cells 100 in the submodule 303 are preferably connected to a bus bar 305, which electrically connects the multiple submodules 303 in parallel or series to adjust the output voltage with the second solar cell module 302. Note that the connection form of the solar cells 100 shown in the third embodiment is just one example, and a solar cell module can be configured using other connection forms.

[0063] (Fourth embodiment) The fourth embodiment relates to a solar power generation system. The solar cell module of the third embodiment can be used as a generator that generates power in the solar power generation system of the fourth embodiment. The solar power generation system of the embodiment generates power using a solar cell module, and specifically includes a solar cell module that generates power, a means for converting the generated electricity, and a storage means for storing the generated electricity or a load for consuming the generated electricity. FIG. 9 shows a configuration diagram of a solar power generation system 400 of the embodiment. The solar power generation system of FIG. 9 includes a solar cell module 401 (300), a converter 402, a storage battery 403, and a load 404. Either the storage battery 403 or the load 404 may be omitted. The load 404 may be configured to be able to utilize the electrical energy stored in the storage battery 403. The converter 402 is a device including a circuit or element that performs power conversion such as voltage transformation and DC-AC conversion, such as a DC-DC converter, a DC-AC converter, or an AC-AC converter. The converter 402 may have a suitable configuration depending on the generated voltage and the configurations of the storage battery 403 and the load 404 .

[0064] The solar cell included in the solar cell module 300 generates electricity, and the electric energy is converted by the converter 402 and stored in the storage battery 403 or consumed by the load 404. It is preferable to provide the solar cell module 401 with a solar tracking drive device for always directing the solar cell module 401 toward the sun, a collector for collecting sunlight, or other devices for improving power generation efficiency.

[0065] The solar power generation system 400 is preferably used in real estate such as residences, commercial facilities, and factories, and in movable property such as vehicles, aircraft, and electronic devices. By using the photoelectric conversion element having excellent conversion efficiency according to the embodiment in a solar cell module, an increase in the amount of power generation is expected.

[0066] A vehicle is shown as an example of use of the solar power generation system 400. FIG. 10 shows a schematic diagram of the vehicle 500. The vehicle 500 in FIG. 8 has a vehicle body 501, a solar cell module 502, a power converter 503, a storage battery 504, a motor 505, and tires (wheels) 506. The power generated by the solar cell module 502 provided on the upper part of the vehicle body 501 is converted by the power converter 503 and charged in the storage battery 504, or the power is consumed by a load such as the motor 505. The vehicle 500 can be moved by rotating the tires (wheels) 506 with the motor 505 using the power supplied from the solar cell module 502 or the storage battery 504. The solar cell module 502 may not be of a multi-junction type, but may be composed of only a first solar cell module equipped with the solar cell 100 of the first embodiment. When a transparent solar cell module 502 is adopted, it is also preferable to use the solar cell module 502 as a window for generating power on the side of the vehicle body 501 in addition to the upper part of the vehicle body 501.

[0067] An air vehicle (drone) is shown as an example of use of the solar power generation system 400. The air vehicle uses a solar cell module 300. The configuration of the air vehicle according to this embodiment will be briefly described using a schematic diagram of an air vehicle (quadcopter) 600 in FIG. 11. The air vehicle 600 has a solar cell module 300, a frame 601, a motor 602, a rotor 603, and a control unit 604. The solar cell module 300, the motor 602, the rotor 603, and the control unit 604 are arranged on the frame 601. The control unit 604 converts the power output from the solar cell module 300 and adjusts the output. The control unit 604 may further include a storage battery that stores the power generated by the solar cell module 300. The motor 602 rotates the rotor 603 using the power output from the solar cell module 300. By configuring the flying object 600 to have the solar cell module 300 of the embodiment, a flying object that can fly using more electric power is provided. The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0068] Example 1 On the glass substrate, ITO (In:Sn=80:20, 20 nm thick) and ATO (Sn:Sb=98:2, 150 μm thick) are deposited on the top surface of the glass substrate as a p-electrode on the back side. A Cu2O light absorbing layer is formed on the transparent p-electrode ATO by sputtering in an oxygen and argon gas atmosphere at 500°C. Next, Ga is deposited as an n-type layer by ALD. 2.0 O 3.0 After that, the n-type layer is returned to room temperature and then cooled to a temperature of 2.0×10 -4 The temperature of the Cu2O light absorbing layer of the member on which the n-type layer is deposited is adjusted to 200°C in an atmosphere of 100°C [g / L]. The temperature of the Cu2O light absorbing layer of the member on which the n-type layer is deposited is considered to be 200°C when the temperature of the hot plate reaches 200°C. In this state, the member on which the n-type layer is formed is treated for 30 minutes. After that, an AZO transparent conductive film is deposited on the n-type layer as an n-electrode. Then, a MgF2 film is formed as an anti-reflective film to obtain a solar cell. The short-circuit current (Jsc), open circuit voltage (Voc), fill factor (FF), conversion efficiency, and transmittance of the obtained solar cell are evaluated. Figure 12 shows the n-type layer, the treatment temperature (Temp [°C]), treatment time (Time [min]), and oxygen concentration ([g / L]) in the heating process. In the case of a single n-type layer, the composition, etc. are shown in the column for the first n-type layer. The circle to the right of the composition of the n-type layer indicates that the heating process was carried out after the n-type layer of that composition was formed. Note that, since ozone and water vapor were not introduced into the container during the heating process, the ozone concentration and water vapor concentration were 5.0×10 -8 [g / L] or less.

[0069] (Examples 2 to 34, Comparative Examples 1 to 10) In Examples 2-34 and Comparative Examples 1-10, solar cells were fabricated in the same manner as in Example 1, except that an n-type layer was formed and heated under the conditions shown in the table of FIG. 12. The short-circuit current (Jsc), open-circuit voltage (Voc), conversion efficiency, and transmittance of the obtained solar cells were evaluated. In the table of FIG. 12, the columns in which the temperature, etc. are marked with "-" indicate that the heating process was not carried out.

[0070] (Example 35, Comparative Example 11) The Cu plate is heated in an oxidizing atmosphere to obtain a Cu2O light absorbing layer. Then, a Ga 2.0 O 3.0 A 10 nm thick layer is deposited on the CuO light absorbing layer, and then a heating step is performed. After forming an n-electrode, an Au electrode film is formed on the surface of the CuO light absorbing layer opposite to the n-type layer. A solar cell is fabricated under the same conditions as in Example 1 except for the above. The short circuit current (Jsc), open circuit voltage (Voc), conversion efficiency, and transmittance of the obtained solar cell are evaluated.

[0071] A solar simulator simulating an AM1.5G light source is used, and the amount of light is adjusted to 1 sun using a reference Si cell under that light source. Measurements are performed under atmospheric pressure with the temperature in the measurement room at 25°C. The voltage is swept and the current density (current divided by cell area) is measured. With the horizontal axis representing voltage and the vertical axis representing current density, the point where the horizontal axis intersects the horizontal axis is the open voltage Voc, and the point where the vertical axis intersects the horizontal axis is the short-circuit current density Jsc. On the measurement curve, the voltage and current density are multiplied together, and the maximum points are Vmpp and Jmpp (maximum power point), respectively. FF = (Vmpp * Jmpp) / (Voc * Jsc), and the conversion efficiency Eff. is calculated as Eff. = Voc * Jsc * FF. After measurement, the sample is cleaved and the brightness profile of the HAADF-STEM images of the first and second regions is calculated.

[0072] The table relating to the examples in FIG. 13 summarizes the evaluation of the brightness profiles of the HAADF-STEM images of the examples and comparative examples, together with the short-circuit current (Jsc), open-circuit voltage (Voc), conversion efficiency, and light transmittance.

[0073] The brightness profile of the HAADF-STEM image is evaluated as follows: A: when the maximum brightness of the brightness profile of the HAADF-STEM image of the first region is 97% or more and 103% or less than the maximum brightness of the brightness profile of the HAADF-STEM image of the second region; B: when the maximum brightness of the brightness profile of the HAADF-STEM image of the first region is greater than 103% and less than 105%, or greater than 95% and less than 97% of the maximum brightness; and C: when the maximum brightness of the brightness profile of the HAADF-STEM image of the first region is 105% or more and 95% or less than the maximum brightness of the brightness profile of the HAADF-STEM image of the second region.

[0074] Regarding transmittance, when the transmittance of light in the wavelength band of 700 nm or more and 1200 nm or less is 70% or more, it is evaluated as A, when the transmittance of light in the wavelength band of 700 nm or more and 1200 nm or less is 60% or more and less than 70%, it is evaluated as B, and when the transmittance of light in the wavelength band of 700 nm or more and 1200 nm or less is less than 60%, it is evaluated as C.

[0075] When the Voc is 1.1 times or more compared to the Voc of Comparative Example 2, it is evaluated as A. When it is 1.0 times or more but less than 1.1 times compared to the Voc of Comparative Example 2, it is evaluated as B. When it is less than 1.0 times compared to the Voc of Comparative Example 2, it is evaluated as C.

[0076] Conversion efficiency is rated as A when it is 1.1 times or more compared to the conversion efficiency of Comparative Example 2, rated as B when it is 1.0 times or more but less than 1.1 times compared to the conversion efficiency of Comparative Example 2, and rated as C when it is less than 1.0 times compared to the conversion efficiency of Comparative Example 2.

[0077] For the evaluation of Voc and conversion efficiency, Examples 1 to 17 and Comparative Examples 1, 3 to 7 are compared with Comparative Example 2. For the evaluation of Voc and conversion efficiency, Examples 18 to 20 are compared with Comparative Example 8. For the evaluation of Voc and conversion efficiency, Examples 21 to 27 are compared with Comparative Example 9. For the evaluation of Voc and conversion efficiency, Examples 28 to 34 are compared with Comparative Example 10. For the evaluation of Voc and conversion efficiency, Example 35 is compared with Comparative Example 11. The contrast correction of the brightness profile of the HAADF-STEM image is performed so that the low brightness (brightness of the n-type layer on the n-electrode side) and high brightness (average brightness of the second region of the p-type light absorption layer) are approximately the same as those of the comparative examples, and then the evaluation is performed.

[0078] As can be seen from the tables of Figures 12 and 13, under appropriate heating conditions in an atmosphere with an appropriate oxygen concentration, the Cu phase precipitated near the boundary between the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide and the first n-type layer can be oxidized and changed to cuprous oxide, improving the brightness profile of the HAADF-STEM image. By oxidizing the Cu phase precipitated near the boundary between the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide and the first n-type layer and changing it to cuprous oxide, the recombination of carriers at the interface is reduced, Voc is increased, and the conversion efficiency is improved accordingly. The presence of a Cu phase reduces the transmittance, but by oxidizing the Cu phase precipitated near the boundary between the layer mainly made of cuprous oxide and / or a composite oxide of cuprous oxide and the first n-type layer and changing it to cuprous oxide, the transmittance is improved. If heating is performed under extreme conditions, copper oxide is formed, which reduces the transmittance and also reduces Voc and conversion efficiency. The conversion efficiency is also improved in a multi-junction solar cell in which the solar cell of the embodiment is used as the top cell and a solar cell using Si in the light absorption layer is used as the bottom cell. In the present specification, some elements are shown only by their element symbols. The technical solutions of the embodiments are described below. Technical proposal 1 A p-electrode; a p-type light absorbing layer containing cuprous oxide and / or a composite oxide of cuprous oxide on the p-electrode; an n-type layer on the p-type light absorbing layer; an n-electrode on the n-type layer, a first region of the p-type light absorbing layer extends from a boundary between the p-type light absorbing layer and the n-type layer to a depth of 10 nm toward the p-electrode; When a second region is a region of the p-type light absorbing layer from a boundary between the p-type light absorbing layer and the n-type layer to a depth of 100 nm toward the p-electrode side, excluding the first region, A solar cell in which the maximum brightness of the brightness profile of the HAADF-STEM image of the first region is 95% or more and 105% or less of the average brightness of the brightness profile of the HAADF-STEM image of the second region. Technical proposal 2 The solar cell according to Technical Scheme 1, wherein the n-type layer contains at least one of an oxide or a sulfide. Technical proposal 3 The solar cell according to Technical Proposal 1 or 2, wherein the n-type layer contains the oxide or the sulfide containing one or more elements selected from the group consisting of Ga, Al, B, In, Ti, Zn, Hf, Zr, Cd, Sn, Si and Ge. Technical proposal 4 The solar cell according to any one of Technical Solutions 1 to 3, wherein the n-type layer includes a single layer or multiple layers of the oxide, or a single layer or multiple layers of the sulfide. Technical proposal 5 A solar cell described in any one of technical proposals 1 to 4, wherein the average brightness of the brightness profile of the HAADF-STEM image of the first region is 85% or more and 95% or less of the average brightness of the brightness profile of the HAADF-STEM image of the second region. Technical proposal 6 A solar cell described in any one of technical proposals 1 to 5, wherein the minimum brightness of a brightness profile of an HAADF-STEM image of the region of the first region from a depth position of 5 nm to a depth position of 10 nm toward the p-electrode side from the position of the boundary between the p-type light absorption layer and the n-type layer is 87% or more and 93% or less of the average brightness of the brightness profile of the HAADF-STEM image of the second region. Technical proposal 7 A solar cell described in any one of technical proposals 1 to 6, wherein the minimum brightness of the brightness profile of the HAADF-STEM image of the first region is 78% or more and 85% or less of the average brightness of the brightness profile of the HAADF-STEM image of the second region. Technical proposal 8 A solar cell described in any one of technical proposals 1 to 7, wherein the average brightness of the brightness profile of the HAADF-STEM image of the first region is 85% or more and 95% or less of the maximum brightness of the brightness profile of the HAADF-STEM image of the first region, and 110% or more and 120% or less of the minimum brightness of the brightness profile of the HAADF-STEM image of the first region. Technical proposal 9 A solar cell described in any one of technical proposals 1 to 8, wherein the average brightness of the brightness profile of the HAADF-STEM image of the second region is 90% or more and 99% or less of the maximum brightness of the brightness profile of the HAADF-STEM image of the second region, and 101% or more and 110% or less of the minimum brightness of the brightness profile of the HAADF-STEM image of the second region. Technical proposal 10 forming an n-type layer on the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide; forming an n-electrode on the n-type layer; a step of heating the member on which the n-type layer is formed, after the step of forming the n-type layer and before the step of forming the n-electrode, or during the step of forming the n-type layer; A method for manufacturing a solar cell comprising the steps of: Technical proposal 11 The manufacturing method described in Technical Proposal 10, wherein the heating step is carried out in a non-oxidizing atmosphere. Technical proposal 12 The manufacturing method according to Technical Scheme 10 or 11, wherein the temperature of the layer mainly composed of the cuprous oxide and / or the composite oxide of cuprous oxide in the heating step is 150°C or higher and 250°C or lower. Technical proposal 13 The manufacturing method according to any one of Technical Schemes 11 to 13, wherein the temperature of the layer mainly composed of the cuprous oxide and / or the composite oxide of cuprous oxide in the heating step is 160°C or higher and 230°C or lower. Technical proposal 14 The manufacturing method according to any one of technical proposals 11 to 14, wherein the temperature of the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide in the heating step is 170°C or higher and 220°C or lower. Technical proposal 15 A manufacturing method described in any one of technical proposals 11 to 15, wherein the processing time in the heating step is 5 minutes or more and 60 minutes or less. Technical proposal 16 The atmosphere in the heating step has an oxygen concentration of 5.0×10 -8 [g / L] or more 8.0×10 -4 The manufacturing method according to any one of technical proposals 11 to 16, wherein the amount of the manufacturing method is less than or equal to [g / L]. Technical proposal 17 A manufacturing method according to any one of technical proposals 11 to 17, wherein the ozone concentration in the atmosphere during the heating step is 1 / 10 or less of the oxygen concentration. Technical proposal 18 The water vapor concentration in the atmosphere during the heating step is 5.0×10 -8 [g / L] or more 8.0×10 -4 The manufacturing method according to any one of technical proposals 11 to 18, wherein the amount of the manufacturing method is less than or equal to [g / L]. Technical proposal 19 A manufacturing method described in any one of technical proposals 11 to 19, wherein the total pressure of the atmosphere in the heating step is 100 Pa or more and 200,000 Pa or less. Technical proposal 20 A solar cell according to any one of technical proposals 1 to 10; A multi-junction solar cell having a solar cell having a light absorption layer with a band gap smaller than that of the p-type light absorption layer of the solar cell described in any one of Technical Solutions 1 to 10. Technical proposal 21 A solar cell module using a solar cell according to any one of technical proposals 1 to 15. Technical proposal 22 A solar power generation system that generates solar power using the solar cell module described in Technical Proposal 21.

[0079] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and the components can be modified and embodied in the implementation stage without departing from the gist of the invention. In addition, various inventions can be formed by appropriately combining the multiple components disclosed in the above embodiment. For example, components from different embodiments may be appropriately combined as in the modified examples. [Explanation of symbols]

[0080] 100, 101... solar cell (first solar cell), 1... substrate, 2... p-electrode, 3... p-type light absorbing layer, 4... n-type layer, 5... n-electrode 200...multijunction solar cell, 201...second solar cell, 300... solar cell module, 301 first solar cell module, 302... second solar cell module, 303... submodule, 304... bus bar, 400... solar power generation system, 401... solar cell module, 402... converter, 403... storage battery, 404... load 500...vehicle, 501...vehicle body, 502...solar cell module, 503...power conversion device, 504...storage battery, 505...motor, 506...tire (wheel) 600: flying object, 601: aircraft frame, 602: motor, 603: rotor, 604: control unit

Claims

1. A p-electrode; a p-type light absorbing layer containing cuprous oxide and / or a composite oxide of cuprous oxide on the p-electrode; an n-type layer on the p-type light absorbing layer; an n-electrode on the n-type layer; a first region of the p-type light absorbing layer is a region extending from a boundary between the p-type light absorbing layer and the n-type layer to a depth of 10 nm toward the p-electrode side; When a second region is a region of the p-type light absorbing layer from a boundary between the p-type light absorbing layer and the n-type layer to a depth of 100 nm toward the p-electrode side, excluding the first region, A solar cell, wherein the maximum brightness of a brightness profile of a HAADF-STEM image of the first region is 95% or more and 105% or less of the average brightness of a brightness profile of a HAADF-STEM image of the second region.

2. The solar cell according to claim 1 , wherein the n-type layer contains at least one of an oxide or a sulfide.

3. 3. The solar cell according to claim 2, wherein the n-type layer contains the oxide or the sulfide containing one or more elements selected from the group consisting of Ga, Al, B, In, Ti, Zn, Hf, Zr, Cd, Sn, Si, and Ge.

4. The solar cell according to claim 2 , wherein the n-type layer comprises a single layer or multiple layers of the oxide, or a single layer or multiple layers of the sulfide.

5. The solar cell according to any one of claims 1 to 4, wherein the average brightness of the brightness profile of the HAADF-STEM image of the first region is 85% or more and 95% or less of the average brightness of the brightness profile of the HAADF-STEM image of the second region.

6. 6. The solar cell according to claim 1, wherein a minimum brightness of a brightness profile of a HAADF-STEM image of the first region from a position at a depth of 5 nm to a position at a depth of 10 nm toward the p-electrode side from the position of the boundary between the p-type light absorption layer and the n-type layer is 87% or more and 93% or less of an average brightness of a brightness profile of a HAADF-STEM image of the second region.

7. The solar cell according to any one of claims 1 to 6, wherein the minimum brightness of the brightness profile of the HAADF-STEM image of the first region is 78% or more and 85% or less of the average brightness of the brightness profile of the HAADF-STEM image of the second region.

8. The solar cell according to any one of claims 1 to 7, wherein an average brightness of the brightness profile of the HAADF-STEM image of the first region is 85% or more and 95% or less of the maximum brightness of the brightness profile of the HAADF-STEM image of the first region, and 110% or more and 120% or less of the minimum brightness of the brightness profile of the HAADF-STEM image of the first region.

9. The solar cell described in any one of claims 1 to 8, wherein the average brightness of the brightness profile of the HAADF-STEM image of the second region is 90% or more and 99% or less of the maximum brightness of the brightness profile of the HAADF-STEM image of the second region, and 101% or more and 110% or less of the minimum brightness of the brightness profile of the HAADF-STEM image of the second region.

10. forming an n-type layer on the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide; forming an n-electrode on the n-type layer; a step of heating the member on which the n-type layer is formed, after the step of forming the n-type layer and before the step of forming the n-electrode, or during the step of forming the n-type layer; Including, When the n-type layer is a single layer, in the step of heating a member on which the n-type layer is formed, heating is performed after the single layer n-type layer is formed and before the step of forming the n-electrode, When the n-type layer is multi-layered, in the step of heating a member on which the n-type layer is formed, heating is performed after the multi-layered n-type layer is formed and before the step of forming the n-electrode, or in the middle of the step of forming the n-type layer, heating is performed after the step of forming one layer that constitutes the multi-layered n-type layer and before the step of forming the next layer of the one layer that constitutes the multi-layered n-type layer.

11. The method according to claim 10, wherein the heating step is carried out in a non-oxidizing atmosphere.

12. The method according to claim 10 or 11, wherein the temperature of the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide in the heating step is 150° C. or higher and 250° C. or lower.

13. 13. The method according to claim 10, wherein the temperature of the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide in the heating step is 160° C. or higher and 230° C. or lower.

14. 14. The method according to claim 10, wherein the temperature of the layer mainly composed of cuprous oxide and / or a composite oxide of cuprous oxide in the heating step is 170° C. or higher and 220° C. or lower.

15. 15. The method according to claim 10, wherein the heating step is performed for a treatment time of 5 minutes or more and 60 minutes or less.

16. The atmosphere in the heating step has an oxygen concentration of 5.0×10 -8 [g / L] or more 8.0×10 -4 The method according to any one of claims 10 to 15, wherein the concentration is 0.01 to 0.1 g / L or less.

17. 17. The method according to claim 10, wherein the ozone concentration in the atmosphere during the heating step is 1 / 10 or less of the oxygen concentration.

18. The water vapor concentration in the atmosphere during the heating step is 5.0×10 -8 [g / L] or more 8.0×10 -4 The method according to any one of claims 10 to 17, wherein the concentration is 0.01 to 0.1 g / L or less.

19. 19. The method according to claim 10, wherein a total pressure of the atmosphere in the heating step is 100 Pa or more and 200,000 Pa or less.

20. A solar cell according to any one of claims 1 to 9; 10. A multijunction solar cell comprising: a solar cell having a light absorbing layer having a band gap smaller than that of the p-type light absorbing layer of the solar cell according to claim 1.

21. A solar cell module using the solar cell according to claim 1 .

22. A solar power generation system that generates solar power using the solar cell module according to claim 21.

Citation Information

Patent Citations

  • Ultrathin MgO layer modified Cu2O planar heterojunction solar cell

    CN109309136A

  • Photoelectric conversion element

    JP2000243994A

  • Oxide thin film solar cell

    JP2006332373A

  • Thin film solar cell

    JP2011258858A

  • Solar battery, multi-junction type solar battery, solar battery module and photovoltaic power generation system

    JP2019169545A