Membrane
The membrane material with a triaxial fabric surface layer adjusts light transmittance by varying void area ratios, addressing labor-intensive and costly manufacturing issues, enhancing flexibility and cost-effectiveness.
Patent Information
- Application Number
- JP2020048951
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-19
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-03-19
AI Technical Summary
Existing membrane materials require different densities and thicknesses of glass fiber fabrics to achieve varying light transmittance, leading to labor-intensive and costly manufacturing processes, especially in spaces with varying distances from light sources.
A membrane material comprising a base material with a triaxial fabric surface layer having a void area ratio between 5% and 50%, which allows adjusting light transmittance by varying the void area ratio of the surface material, using glass fiber or glass nonwoven fabric with specific thickness and density.
Enables easy adjustment of light transmittance by altering the void area ratio in the surface material, reducing labor intensity and costs while maintaining rigidity and non-flammability, suitable for diverse lighting applications.
Smart Images

Figure 0007552044000001 
Figure 0007552044000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a film material having optical transparency. [Background technology]
[0002] For example, currently, light-transmitting ceiling materials mainly use membrane materials containing glass fiber fabric, which are lightweight and non-flammable (for example, see Patent Document 1 below). In ceiling materials using such light-transmitting membrane materials (light membrane ceiling materials), the light from a light source located inside is diffused and transmitted, thereby reducing glare. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-214177 A Summary of the Invention [Problem to be solved by the invention]
[0004] The light membrane ceiling material as described above has different light transmittance requirements for small spaces that are relatively close to the light source, such as the interior of a house, an office conference room, or a waiting room in a train station, and for large spaces that are relatively far from the light source, such as a gymnasium or a commercial facility. The light membrane ceiling material required to have such different light transmittances requires the use of glass fiber fabrics with different densities and thicknesses, which is troublesome and costly to manufacture.
[0005] This type of problem is not limited to membrane materials used in the light membrane ceiling materials described above, but can also occur in membrane materials used for wall surfaces such as building materials and waist-high walls, lighting furniture such as three-sided mirrors, and indirect lighting that houses lighting fixtures inside, such as footlights and guide lights.
[0006] In view of the above, an object of the present invention is to provide a film material that can easily provide a desired light transmittance. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems, the film material according to the present invention is a light-transmitting film material, comprising: a light-transmitting base material; and a surface material having a triaxial woven fabric laid on one side of the base material, the surface material having an area ratio of voids being 5% or more and 50% or less; The substrate includes a glass cloth or a glass nonwoven fabric. Characterized by 。 Effect of the Invention
[0008] With the film material of the present invention, the light transmittance can be set by the area proportion of the voids in the surface material. Therefore, even if the light transmittance of the base material is the same, the light transmittance can be changed by applying a surface material with a different light transmittance, so that the required light transmittance can be easily obtained. [Brief description of the drawings]
[0009] [Figure 1] 1 is a cross-sectional view showing a schematic configuration of a main embodiment of a membrane material according to the present invention. [Diagram 2] 2 is a plan view showing a schematic configuration of a surface material of the membrane material of FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] An embodiment of the membrane material according to the present invention will be described with reference to the drawings, however, the present invention is not limited to only the embodiment described with reference to the drawings.
[0011] <Main embodiment> A main embodiment of the membrane material according to the present invention will be described with reference to FIGS.
[0012] As shown in Fig. 1, a surface material 12 having a triaxial fabric is laid on one surface (the upper surface in Fig. 1) of a light-transmitting base material 11. An adhesive layer 13 is interposed between the base material 11 and the surface material 12.
[0013] The substrate 11 includes a glass cloth or a glass nonwoven fabric made of glass fibers and has a mass of 500 g / m 2 It is preferable that the thickness is 0.5% or less, since it is possible to reduce the weight. In the case of glass cloth, it is preferable that the glass cloth is woven with warp and weft threads of glass fibers so that the opening ratio is 0.5% or more and 1.0% or less and the thickness is 100 μm or more and 1 mm or less. On the other hand, in the case of glass nonwoven fabric, it is preferable that the thickness is 50 μm or more and 150 μm or less.
[0014] Furthermore, the base material 11 satisfies the non-combustibility standard. Specifically, for example, in a heat generation test using a cone calorimeter tester in accordance with ISO5660-1 and in accordance with the fire resistance test method and performance evaluation standard based on Article 2, Paragraph 9 of the Building Standards Act and Article 108, Paragraph 2 of the Enforcement Order of the Building Standards Act, the base material 11 satisfies the non-combustibility standard. (1) The total heat generation amount (MJ / m) for 20 minutes after the start of heating 2 ) is 4MJ / m 2 (2) The maximum heat generation rate during the first 20 minutes after heating begins is 200 kW / m or less for 10 seconds or more. 2 and (3) there are no cracks or holes that penetrate to the back surface and are harmful to fire safety for 20 minutes after heating begins.
[0015] As shown in Figures 1 and 2, the surface material 12 includes a triaxial fabric in which glass fiber threads 12a are woven in three axial directions so as to have voids 12b penetrating between one side and the other side, and the area ratio of the voids 12b is adjusted to a range of 5% or more and 50% or less.
[0016] The triaxial fabric has a thickness of 100 μm to 1 mm and a mass of 500 g / m 2The thickness of the surface material 12 is preferably less than 1 mm because it can be made lighter. The surface material 12 is made of a resin that is impregnated between the glass fibers of the woven threads 12a and hardened, and has high rigidity. Examples of the impregnated resin include thermoplastic resin, thermosetting resin, and ultraviolet-curable resin.
[0017] Examples of the thermoplastic resin include polyester resins such as polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, polytrimethylene terephthalate (PTT) resin, polyethylene naphthalate (PEN) resin, and liquid crystal polyester resin; polyolefin resins such as polyethylene (PE) resin, polypropylene (PP) resin, and polybutylene resin; styrene-based resins; polyoxymethylene (POM) resin, polyamide (PA) resin, polycarbonate (PC) resin, polymethylene methacrylate (PMMA) resin, polyvinyl chloride (PVC) resin, polyphenylene sulfide (PPS) resin, polyphenylene ether (PPE) resin, modified PPE resin, thermoplastic polyimide (PI) resin, and polyamide-imide (PAI). Examples of fluororesins such as polyetherimide (PEI) resin, polysulfone (PSU) resin, modified PSU resin, polyethersulfone (PES) resin, polyketone (PK) resin, polyetherketone (PEK) resin, polyetheretherketone (PEEK) resin, polyetherketoneketone (PEKK) resin, polyarylate (PAR) resin, polyethernitrile (PEN) resin, thermoplastic phenolic resin, phenoxy resin, and polytetrafluoroethylene resin, as well as thermoplastic elastomers such as polystyrene resin, polyolefin resin, polyurethane resin, polyester resin, polyamide resin, polybutadiene resin, polyisoprene resin, and fluororesins, as well as copolymers, modified products, and blends of two or more of these resins.
[0018] Examples of the thermosetting resin include phenolic resin (PF), epoxy resin (EP), melamine resin (MF), urea resin (UF), unsaturated polyester resin (UP), alkyd resin, polyurethane (PUR), and thermosetting polyimide (PI).
[0019] Examples of the ultraviolet-curable resin include acrylic and epoxy resins.
[0020] The adhesive layer 13 bonds the substrate 11 and the surface material 12, and may be, for example, a hot melt adhesive with a solid content of 100%, a moisture-curing adhesive with a solid content of 100% (e.g., polyurethane (PUR)-based resin), a high-viscosity rubber-based adhesive, or a high-viscosity urethane resin-based adhesive. Examples of hot melt adhesives include ethylene-vinyl acetate copolymer resin (EVA resin), polyamide resin, etc.
[0021] It is highly preferable to use the above-mentioned adhesive in the adhesive layer 13, since this prevents the adhesive from penetrating into the pores of the substrate 11 or the surface material 12, or into the voids 12b of the surface material 12, thereby preventing a decrease in the adhesive strength between the substrate 11 and the surface material 12. Note that it is preferable to use a high-viscosity rubber-based adhesive or a high-viscosity urethane resin-based adhesive having a viscosity of, for example, 40 Pa s or more, more preferably 50 Pa s or more.
[0022] A method for manufacturing the membrane material 10 according to this embodiment will now be described. First, the above-mentioned resin (e.g., a thermosetting resin) is dissolved or dispersed in a solvent such as water to prepare an impregnation liquid, and the surface material 12 is immersed in the impregnation liquid to impregnate the resin between the glass fibers of the yarns 12a of the fabric of the surface material 12.
[0023] Examples of the method for impregnating the resin include a method in which the sheet-like surface material 12 is directly immersed in the impregnation liquid in a container, and a method in which a web-like surface material is run between a pair of rolls to which the impregnation liquid is applied to impregnate the surface material with the impregnation liquid, and then the web is cut.
[0024] Next, a mesh-like (or sheet-like) adhesive layer (e.g., hot melt adhesive) 13 is laminated on one side of the base material 11, and then a resin-impregnated surface material 12 is laminated. This is then heated (e.g., at about 100°C for about 30 seconds) to harden the resin and melt the adhesive. As a result, the surface material 12 hardens and the base material 11 and the surface material 12 are bonded together by the adhesive layer 13, and the membrane material 10 is obtained.
[0025] In the membrane material 10 of this embodiment, a surface material 12 including a triaxial fabric having voids 12b formed by weaving glass fiber threads 12a in triaxial directions is laid on a substrate 11 including a glass cloth containing glass fibers or a glass nonwoven fabric, so that the light transmittance can be set by the area proportion of the voids 12b of the surface material 12.
[0026] That is, if the light transmittance of the base material 11 is Pb, the light transmittance of the surface material 12 is Ps, and the light transmittance of the adhesive layer 13 is Pg, the light transmittance Pf of the film material 10 can be expressed by the following formula (1).
[0027] Pf = Pb × Ps × Pg (1)
[0028] Here, since the light transmittance Pg of the adhesive layer 13 can be practically ignored, the above formula (1) essentially consists of only the first and second terms.
[0029] Therefore, even if the light transmittance Pb of the base material 11 is the same, the light transmittance Pf of the film material 10 can be set to a value as required by applying a surface material 12 with a different light transmittance Ps.
[0030] Specifically, for example, when the width W of the glass fiber threads 12a is 4 mm and the weave angle θ is 60°, the area ratio of the voids 12b in the surface material 12 can be approximately 30%. In this case, by decreasing the width W of the threads 12a or increasing the weave angle θ, the area ratio of the voids 12b in the surface material 12 can be increased. On the other hand, by increasing the width W of the threads 12a or decreasing the weave angle θ, the area ratio of the voids 12b in the surface material 12 can be decreased.
[0031] In this way, the area ratio of the void portion 12b is adjusted to be in the range of 5% or more and 50% or less. In other words, by laying the surface material 12 with adjusted light transmittance Ps on the base material 11 with light transmittance Pb, it is possible to easily make the film material 10 have the light transmittance Pf required.
[0032] Specifically, for example, when used as a light membrane ceiling material in a large space such as a commercial facility or gymnasium where the distance to the light source is relatively far, the light transmittance Pf of the film material 10 is set to 50% or more and 90% or less; when used as a light membrane ceiling material in a small space such as the interior of a house, an office conference room, or a waiting room in a station where the distance to the light source is relatively close, the light transmittance Pf of the film material 10 is set to 30% or more and 70% or less; and when used for applications that do not require a relatively large amount of light, such as indirect lighting for footlights and guide lights, the light transmittance Ps of the film material 10 is set to 10% or more and 50% or less. In this way, the surface material 12 with the adjusted area proportion of the void portion 12b is laid on the base material 11 with light transmittance Pb.
[0033] In other words, a series of surface materials 12 are available with multiple surface area ratios of void portions 12b in the range of 5% or more and 50% or less.In other words, a series of surface materials 12 with different light transmittances Ps are available, and by combining them with a substrate 11 with a single light transmittance Pb, a combination series can be created to obtain a film material 10 with the desired light transmittance Pf.
[0034] Therefore, according to the film material 10 of this embodiment, the required light transmittance Pf can be easily obtained.
[0035] Furthermore, since it is necessary to keep the light transmittance Pb of the base material 11 as high as possible, the density and thickness of the base material 11 become relatively small, and the rigidity of the base material 11 becomes low. However, the rigidity of the surface material 12 is increased by impregnating the glass fibers of the woven threads 12a of the surface material 12 with resin and hardening the resin, so that the surface material 12 can be used as a core material and has sufficient rigidity.
[0036] If the surface material is made of a biaxial (warp, weft) fabric, the directionality is vertical and horizontal, so when the resin is impregnated and cured, it tends to bend vertically or horizontally. In contrast, the membrane material 10 according to this embodiment has a surface material 12 made of a triaxial (axial, right-up bias yarn, left-up bias yarn) fabric, so the directionality is diagonal, and it can maintain its rigidity when the resin is impregnated and cured.
[0037] Other Embodiments In the above-mentioned embodiment, the description was centered on the case where the present invention is applied to a light-transmitting membrane ceiling material, but the present invention is not limited to this. As another embodiment, the present invention can be applied in the same manner as the above-mentioned embodiment, if the present invention is used as a light-transmitting membrane material, such as a membrane material used for wall surfaces such as fittings and waist-high walls, lighting furniture such as a three-way mirror, or indirect lighting such as footlights and guide lights that house lighting fixtures inside. [Industrial Applicability]
[0038] The film material according to the present invention can be easily obtained with the required light transmittance, and therefore can be used industrially with great advantage. [Explanation of symbols]
[0039] 10 Membrane material 11 Base material 12 Surface material 12a Yarn 12b Cavity 13 Adhesive layer
Claims
1. A light-transmitting film material, A substrate having optical transparency; A surface material having a triaxial woven fabric laid on one surface of the base material; Equipped with The surface material has an area ratio of voids of 5% or more and 50% or less, The substrate includes a glass cloth or a glass nonwoven fabric. A membrane material characterized by:
2. The fibers of the triaxial fabric are hardened by a resin. The membrane material according to claim 1 .
3. The triaxial fabric contains glass fibers.
3. The membrane material according to claim 1 or 2.
4. An adhesive layer is interposed between the substrate and the surface material. The membrane material according to any one of claims 1 to 3.
5. The adhesive layer contains at least one of a hot melt adhesive having a solid content of 100%, a moisture-curing adhesive having a solid content of 100%, a high-viscosity rubber-based adhesive, and a high-viscosity urethane resin-based adhesive. The membrane material according to claim 4 .
Citation Information
Patent Citations
High frequency fusible polyolefinic resin film material
JP2002046237A
Incombustible membrane material
JP2014040034A
Membrane material and membrane roof using the same
JP2019214177A