Pattern printing method and printed matter

The use of a coating agent with a water-insoluble solvent and a water-soluble additive solvent in screen and metal mask printing methods addresses the issue of cohesive failure, enabling high aspect ratio patterns with rectangular cross-sections, enhancing accuracy and stability in conductive materials.

JP7552143B2Active Publication Date: 2024-09-18TOPPAN HOLDINGS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020140793
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-24
Publication Date
2024-09-18
Estimated Expiration
2040-08-24

AI Technical Summary

Technical Problem

Conventional printing methods, such as screen printing and metal mask printing, face challenges in forming patterns with a high aspect ratio and rectangular cross-section due to cohesive failure of the ink, resulting in semicircular shapes and limited thickness, which affects the accuracy of resistance calculations and stretchability of conductive materials.

Method used

A pattern printing method using a coating agent composed of a water-insoluble main solvent mixed with a water-soluble additive solvent, applied through screen printing or metal mask printing, reduces shear force and cohesive failure by forming an oil film between the ink and the printing plate, allowing for the formation of patterns with high aspect ratios and rectangular cross-sections.

Benefits of technology

The method enables the formation of patterns with steep edges and high aspect ratios, facilitating accurate resistance calculations and reducing resistance fluctuations in stretchable materials, while maintaining high definition and stability during expansion and contraction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552143000008
    Figure 0007552143000008
  • Figure 0007552143000002
    Figure 0007552143000002
  • Figure 0007552143000003
    Figure 0007552143000003
Patent Text Reader

Abstract

To provide a printing method capable of printing without causing a cohesion failure of an ink, in screen printing and metal mask printing, and capable of forming a high-aspect-ratio pattern being thick and having a sufficient height, with a steep pattern edge and a rectangle cross section.SOLUTION: A pattern is printed on a base plate, using a screen printing plate or a metal mask plate, and using, as a print ink, a coating agent composed of a polymer in which an inorganic filler or an organic filler is dispersed, a solvent and an additive, and in which if the solvent and a main solvent of the additive are non-water soluble, a water soluble solvent is added, and if water soluble, a non-water soluble solvent is added.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pattern printing method, and more particularly to a pattern printing method and printed matter using screen printing and metal mask printing. [Background technology]

[0002] Conventionally, in order to form patterns in the field of printable electronics, for example, attempts have been made to form circuit patterns of conductive or insulating materials using various printing methods such as gravure printing, screen printing, flexographic printing, offset printing, and inkjet printing.

[0003] In such fields, it is desirable to form a print pattern that ideally has a rectangular cross-sectional print shape with a high aspect ratio.

[0004] If a rectangular pattern with a high aspect ratio is possible, for example when printing a wiring pattern using conductive ink, if the cross-sectional shape of the pattern can be made closer to a rectangle, the cross-sectional area can be calculated simply as the base dimension x height dimension, and the wiring resistance value can be easily calculated. Also, a high aspect ratio pattern makes it possible to consolidate dense wiring in an electronic circuit into a small area, and allows more current to flow through the wiring circuit.

[0005] In addition, by using conductive materials such as stretchable silver, carbon, CNT, graphene, and copper as printing inks on stretchable substrates, it is possible to reduce changes in wiring resistance when printed items such as stretchable wiring, circuits, and FPCs are stretched.

[0006] However, with conventional printing methods, the cross-sectional shape of the printed pattern ends up being semicircular (so-called kamaboko-shaped) as shown in the cross-sectional SEM image of Figure 5, and only printing with a low aspect ratio can be achieved.

[0007] Patent Document 1 discloses a method for forming a fine wiring pattern by discharging a coating agent using a coater head for stripe coating or a syringe-based dispenser. However, although this method can form fine patterns, the patterns that can be formed are limited to stripe and line patterns. In addition, printing takes longer than other printing methods, making it difficult to print at high speed. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2018-70854 A Summary of the Invention [Problem to be solved by the invention]

[0009] A feature of the screen printing method is that it can print thicker films than other printing methods, so it can form tall patterns and the printing time is not inferior. Figures 3 and 4 show patterns printed using the conventional screen printing method.

[0010] FIG. 3 is a schematic diagram showing how ink 14 is printed on a substrate 15 using a screen printing plate 10 that is composed of a screen mesh 1 and a mask 16 made of a resin film with mask openings 11 formed therein. A shear force 13 indicated by an arrow is generated between the mask opening 11 and the mask.

[0011] This shear force 13 is a frictional force that occurs at the interface between the side wall surface of the mask opening 11 and the ink 14 when the ink 14 is pushed out onto the substrate 15 to print a pattern, and the shear force 13 acts in the direction of the arrow.

[0012] 4, this shear force 13 causes cohesive failure 41 of the ink during printing, so that a large amount of ink remains on the screen printing plate 10. As a result, the pattern printed on the substrate 15 has a low height and a crumbled edge, resulting in a semi-cylindrical print pattern 42, and no rectangular pattern can be obtained. Therefore, this printing method has the problem that it is not possible to print a thick film pattern with a high aspect ratio.

[0013] Furthermore, in metal mask printing, in which a metal mask is used instead of a screen mesh, the same problem occurs because cohesive failure of the ink occurs.

[0014] Therefore, an object of the present invention is to provide a printing method in screen printing and metal mask printing that can print without causing cohesive failure of the ink, and can form a thick film with sufficient height, steep pattern edges, and a high aspect ratio pattern with a rectangular cross section. [Means for solving the problem]

[0015] As a means for solving the above problems, the present invention provides The above problem was solved by carrying out printing with the screen printing plate or metal mask plate using a coating agent in which an incompatible water-soluble solvent is mixed with an ink material mainly composed of a water-insoluble material.

[0016] That is, the pattern printing method according to the present invention comprises the steps of: Contains silver Inorganic Filler - Dispersed polymer, solvent and additives and, Consists of 、 before Solvents and additives A water-insoluble main solvent is mixed with a water-soluble additive solvent, ethylene glycol monoethyl ether acetate, in an amount of 0.1 to 50 wt % relative to the main solvent. The coating agent is used as printing ink, It is characterized in that a pattern is printed on a substrate using a screen printing plate.

[0017] The pattern printing method according to the present invention further comprises the steps of: Contains silver Inorganic Filler - Dispersed polymer, solvent and additives and, Consists of 、 before Solvents and additives A water-insoluble main solvent is mixed with a water-soluble additive solvent, ethylene glycol monoethyl ether acetate, in an amount of 0.1 to 50 wt % relative to the main solvent. The coating agent is used as printing ink, A metal mask may be used to print a pattern on a substrate.

[0018] The pattern printing method according to the present invention further comprises the steps of: In the pattern printing method described above, After the printing, a baking process may be further carried out.

[0019] In addition, the printed matter according to the present invention is It is characterized in that it is printed by the pattern printing method described above.

[0020] In addition, the printed matter according to the present invention is In the surface shape of the pattern printed by the above-described pattern printing method using the screen printing plate, the portions corresponding to the screen mesh marks may be concave. Effect of the Invention

[0021] According to the pattern printing method of the present invention, since the ink can be printed without causing cohesive failure, a steep pattern perpendicular to the substrate is formed, resulting in a pattern with a high aspect ratio in which the height is large relative to the width. This also makes it possible to print wiring patterns for electronic circuits with the narrowest possible gaps between the wiring. Furthermore, if the cross-sectional shape is rectangular, the cross-sectional area can be calculated simply by multiplying the base dimension by the height dimension, so when a conductive material is used, the wiring resistance value can be calculated easily and accurately. Furthermore, even in the case of a thick film, wiring printing with a high aspect ratio is possible, and a stretchable wiring pattern with high elasticity can be printed, and fluctuations in wiring resistance value after stretching can be reduced. [Brief description of the drawings]

[0022] [Figure 1] FIG. 2 is a schematic diagram illustrating the screen printing of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating the screen printing of the present invention. [Diagram 3] FIG. 1 is a schematic diagram illustrating conventional general screen printing. [Figure 4] FIG. 1 is a schematic diagram illustrating conventional general screen printing. [Diagram 5] SEM image of the cross-sectional shape of a print made using a conventional method. [Figure 6] Observation of the print pattern of Example 1 of the present invention [Figure 7] FIG. 4 is an observation view of a printed pattern of Comparative Example 1. [Figure 8] FIG. 2 is an enlarged surface observation view of the print pattern according to the first embodiment of the present invention. [Figure 9] FIG. 2 is an enlarged surface observation view of the print pattern of Comparative Example 1. [Figure 10] FIG. 11 is an observational view of a printed pattern according to a second embodiment of the present invention. [Figure 11] FIG. 11 is an observation view of a printed pattern of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The printing method of the present invention will now be described in detail.

[0024] In the present invention, screen printing and metal mask printing are used as the printing method, and a coating agent having the composition described in detail below is used as the printing ink.

[0025] The above-mentioned printing method is applicable to the general squeegee method using a urethane rubber plate or ink filling by squeegee sweeping, but it can also be applied to a sealed pressure printing method in which paste is directly inserted into the holes in the printing plate at filling pressure by an actuator provided in the print head. The contact pressure printing method is a new printing method capable of high aspect ratio printing (reference model: Panasonic SP60P), and is primarily used for printing solder paste.

[0026] (Screen printing) The commonly used screen printing method involves attaching a sheet made of woven wire material with a diameter of several tens of microns, called a mesh, made of stainless steel, polyester, or nylon, to a square metal frame with high tension, and then attaching to one side of this mesh a film (made of a resin film or metal film) with holes for the image, wiring pattern, circuits, etc. to be printed, to create a screen printing plate.

[0027] To put it simply, the screen printing process involves placing the screen printing plate on the printing substrate with the film side facing up, and then rubbing a flat plate (squeegee) made of urethane or some other material at an angle of about 60 to 80 degrees to the printing surface, and rubbing the mesh surface from one end of the plate to the other at a constant speed.

[0028] At this time, a mark is printed in the direction of travel from the intersection of the angled plate and the mesh. When the ink to be printed is placed on the plate and moved while rubbing it, the angle of the plate pushes the ink downward, causing it to fall through holes in the film surface for patterns, wiring patterns, circuits, etc. onto the surface of the printing substrate underneath, where it is transferred to the printing substrate.

[0029] After the transfer, the plate is raised upward at a constant speed, causing the printing substrate surface and film surface to separate, and the printing pattern is formed on the printing surface. If a gap of several millimeters is left between the printing surface and the film surface, a cleaner print can be achieved.

[0030] However, as shown in Figure 3 above, commonly used screen printing ink (paste) is pushed out through the screen printing plate, which is made of a mesh of woven stainless steel, polyester, or nylon wires with diameters of tens of microns, and a resin or metal film with holes for the image, wiring pattern, circuits, etc. to be printed, while being subjected to a certain amount of shear by the printing substrate underneath.

[0031] At this time, as shown in Figure 4 above, cohesive failure occurs between the wall of the mesh or film opening and the paste being extruded, causing the paste to split, leaving some paste on the wall of the mesh or film opening in a so-called ``parted'' state, and not all of the paste can be transferred to the printing substrate.As a result, the cross-sectional shape of the pattern is not rectangular but semicircular, making it impossible to create a pattern with a high aspect ratio.

[0032] (Metal mask printing) General metal mask printing is a method of printing a pattern on a substrate by imprinting ink paste using a very thin stainless steel plate with a thickness of 0.2 mm or less called a metal mask, which has a fine opening pattern, as a printing plate. A squeegee is used when printing, just like with screen printing described above.

[0033] When printing using a metal mask, the same phenomenon occurs: shear forces act between the wall of the opening in the metal mask and the extruded paste, causing cohesive failure. As a result, the cross-sectional shape of the printed pattern is not rectangular but semi-cylindrical, making it impossible to create a pattern with a high aspect ratio.

[0034] In the pattern printing method according to the present invention, the coating agent has the following composition, thereby solving the problem of cohesive failure during printing.

[0035] (Composition of coating agent) In other words, the coating agent according to the present invention is configured by mixing a polymer (binder) having an inorganic filler or an organic filler (pigment) dispersed therein, a solvent (organic solvent), and a water-soluble solvent if the main solvent of the additive is water-insoluble, or a non-water-soluble solvent if the main solvent of the additive is water-soluble.

[0036] Specifically, when dispersing fillers such as silver paste, copper paste, and conductive ink developed for filling and printing applications into a polymer (binder) that constitutes a coating material with a filler content of 50 to 99.9%, it is necessary to check whether the dispersing solvent and the main solvent of the additive are water-insoluble or water-soluble, and then a combination of solvents with different polarities that do not destroy the physical properties of the coating agent and the amount of addition are adjusted, and a coating agent in which the filler is dispersed is used.

[0037] The coating agent of the present invention is defined as comprising a polymer (binder), a pigment (for coloring, rust prevention, constitution, other functionality, etc.), a solvent (organic solvent, water, etc.), and additives. Solubility parameters (Solubilit The idea of ​​the y Parameter (SP, or SP value) (hereinafter abbreviated as SP value) is that the force acting between the solvent and the solute is assumed to be an intermolecular force, and the intermolecular force is used as a measure of cohesive force. It is generally believed that two components with a small difference in SP value are easy to mix (high solubility), and two components with a large difference in SP value are difficult to mix (low solubility). Conventionally, based on this idea, coating agents used in general printing applications are commercialized and used by mixing polymers (binders) with a small difference in SP value, solvents (organic solvents, water, etc.), and additives, but the present invention defines a completely different idea. In other words, rather than considering the solubility parameter, it is an idea that emphasizes the main solvent of the coating agent used, and whether the main solvent is a water-insoluble solvent or a water-soluble solvent.

[0038] The coating agent according to the present invention is configured such that it is confirmed whether the organic solvent that is the main solvent of the coating agent to be applied is water-soluble or non-water-soluble, and if the main solvent is water-insoluble, a water-soluble organic solvent is added before use. As an example of how to think about this, let's take the example of mixing rubber (polymer) and oil (solvent). When rubber (polymer) and oil (solvent) are mixed, the rubber swells. This is a phenomenon in which the oil gets between the rubber molecules, and if the oil mixes easily with the rubber, it will swell, and if it does not mix well with the rubber, it will not swell. In other words, if the main solvent of the coating is water-insoluble, adding a water-soluble solvent will result in the water-soluble solvent floating on the surface of the coating, where the main solvent is a water-insoluble solvent, because substances with different polarities (in this case, the water-insoluble solvent and the water-soluble solvent) are difficult to mix with each other.

[0039] (Application to screen printing and metal mask printing) The coating agent having the above-mentioned structure is used as an ink paste and applied to screen printing and metal mask printing, thereby achieving the following effects.

[0040] For example, when performing screen printing, an ink paste made from the coating agent according to the present invention is pushed out through a sheet of woven wire material with a wire diameter of several tens of micrometers, such as stainless steel, polyester, or nylon, called the mesh of the screen printing plate, and through a resin or metal film with holes for the pattern, wiring pattern, circuit, etc. to be printed, while being subjected to a certain amount of shear and onto the printing substrate underneath. At this time, the water-soluble solvent floats on the surface of the coating material between the wall of the mesh or resin film and the ink paste being extruded, forming an oil film. This oil film has the effect of reducing shear force, eliminating or reducing cohesive failure.

[0041] Furthermore, when printing using a metal mask plate, the same procedure is followed as for the screen printing plate described above; an oil film is formed between the wall surface of the opening in the metal mask and the extruded ink paste, reducing the shear force and preventing cohesive failure.

[0042] (Type of solvent) A solvent composition for a coating agent generally used in a filling material, printing method, etc. is a solvent composition containing a solvent and a compound represented by the following formula (1) (excluding monohydroxystearic acid). R 1 -CH 2 -R 2 (1) (In the formula, R 1 represents a monohydroxyalkyl group, and R 2 is a carboxyl group (C(=O)OH) or an amide group (C(=O)NH 2 )

[0043] The solvents include n-heptane (SP value: 7.3), ethylene glycol monoethyl ether acetate (SP value: 8.8), n-propanol (SP value: 11.8), 1,2,5,6-tetrahydrobenzyl alcohol (SP value: 11.3), diethylene glycol ethyl ether (SP value: 10.9), 3-methoxybutanol (SP value: 10.9), triacetin (SP value: 10.2), propylene glycol monomethyl ether (SP value: 10.2), cyclopentanone (SP value: 10.0), γ-butyrolactone (SP value: 9.9 ... Hexanone (SP value: 9.9), propylene glycol n-propyl ether (SP value: 9.8), propylene glycol n-butyl ether (SP value: 9.7), dipropylene glycol methyl ether (SP value: 9.7), 1,4-butanediol diacetate (SP value: 9.6), 3-methoxybutyl acetate (SP value: 8.7), propylene glycol diacetate (SP value: 9.6), ethyl lactate acetate (SP value: 9.6), ε-caprolactone (SP value: 9.6), 1,3-butylene glycol diacetate (SP value: 9.5 ), dipropylene glycol-n-propyl ether (SP value: 9.5), 1,6-hexanediol diacetate (SP value: 9.5), dipropylene glycol-n-butyl ether (SP value: 9.4), tripropylene glycol methyl ether (SP value: 9.4), tripropylene glycol-n-butyl ether (SP value: 9.3), cyclohexanol acetate (SP value: 9.2), diethylene glycol monoethyl ether acetate (SP value: 9.0), ethylene glycol methyl ether acetate (SP value: 9.0), diethylene Glycol monobutyl ether acetate (SP value: 8.9), ethylene glycol monobutyl ether acetate (SP value: 8.9), methyl acetate (SP value: 8.8), ethyl acetate (SP value: 8.7), propylene glycol monomethyl ether acetate (SP value: 8.7), n-propyl acetate (SP value: 8.7), dipropylene glycol methyl ether acetate (SP value: 8.7), 3-methoxybutanol acetate (SP value: 8.7), butyl acetate (SP value: 8.7), isopropyl acetate (SP value: 8.5), tetrahydrofuran (SP value: 8.3), dipropylene glycol methyl-n-butyl ether (SP value: 8.0), dipropylene glycol methyl-n-propyl ether (SP value: 8.0), dipropylene glycol dimethyl ether (SP value: 7.9), propylene glycol methyl-n-butyl ether (SP value: 7.8), propylene glycol methyl-n-propyl ether (SP value: 7.8), etc. can be mentioned.

[0044] The solubility parameters (SP values: Fedors calculated values) of the solvents mentioned here at 25°C are approximately 7.3 to 11.8. However, in the present invention, the SP values ​​are merely used as a reference for selecting a solvent. What is important is to determine whether these solvents are water-insoluble or water-soluble, and to combine them by adding a solvent that is the exact opposite of the main solvent.

[0045] Regarding the definition of water-soluble and water-insoluble solvents, the following is the definition of water-soluble liquids of Class 4 hazardous materials. Class 4 hazardous materials are flammable liquids. They are further divided into (1) those that dissolve in water (water-soluble) and (2) those that do not dissolve in water (water-insoluble). The government ordinance defines them as follows:

[0046] A water-soluble liquid is one that maintains a uniform appearance when mixed with an equal volume of pure water at 1 atmosphere and 20°C, while a water-insoluble liquid is any liquid other than a water-soluble liquid. A water-insoluble liquid separates into two layers when mixed with water. If the specific gravity of the liquid is lower than that of water, a water-insoluble layer will form above the water layer, and if the specific gravity is higher than that of water, a water-insoluble layer will form below the water layer. In the case of water-soluble liquids, when mixed, the layers do not separate and the liquid becomes uniform. Some liquids are slightly soluble in water, such as diethyl ether, a special flammable substance, and ethyl acetate, a first class petroleum product, but by definition they are classified as water-insoluble.

[0047] Therefore, based on the above definitions of water-insoluble and water-soluble, they can be classified as follows: The water-soluble solvents were ethylene glycol monoethyl ether acetate (SP value: 8.8), n-propanol (SP value: 11.8), 1,2,5,6-tetrahydrobenzyl alcohol (SP value: 11.3), diethylene glycol ethyl ether (SP value: 10.9), 3-methoxybutanol (SP value: 10.9), propylene glycol monomethyl ether (SP value: 10.2), γ-butyrolactone (SP value: 9.9), propylene glycol-n-propyl ether (SP value: 9.8), dipropylene glycol methyl ether (SP value: 9.7), lactate ethyl acetate (SP value: 9.6), ε-caprolactone (SP value: 9.6), tripropylene glycol ethyl ether (SP value: 9.6), and ethylene glycol ethyl ether (SP value: 9.6). Examples of the propylene glycol methyl ether include propylene glycol methyl ether (SP value: 9.4), tripropylene glycol-n-butyl ether (SP value: 9.3), diethylene glycol monoethyl ether acetate (SP value: 9.0), ethylene glycol methyl ether acetate (SP value: 9.0), diethyl ether acetate (SP value: 9.0), tetrahydrofuran (SP value: 8.3), dipropylene glycol methyl-n-butyl ether (SP value: 8.0), dipropylene glycol methyl-n-propyl ether (SP value: 8.0), dipropylene glycol dimethyl ether (SP value: 7.9), and propylene glycol methyl-n-propyl ether (SP value: 7.8).

[0048] The non-water-soluble solvents are triacetin (SP value: 10.2), cyclopentanone (SP value: 10.0), cyclohexanone (SP value: 9.9), propylene glycol-n-butyl ether (SP value: 9.7), 1,4-butanediol diacetate (SP value: 9.6), 3-methoxybutyl acetate (SP value: 8.7), propylene glycol diacetate (SP value: 9.6), 1,3-butylene glycol diacetate (SP value: 9.5), dipropylene glycol-n-propyl ether (SP value: 9.5), 1,6-hexanediol diacetate (SP value: 9.5), dipropylene glycol-n-butyl ether (SP value: 9.4), and cyclohexanol acetate. (SP value: 9.2), diethylene glycol monobutyl ether acetate (SP value: 8.9), ethylene glycol monobutyl ether acetate (SP value: 8.9), methyl acetate (SP value: 8.8), ethyl acetate (SP value: 8.7), propylene glycol monomethyl ether acetate (SP value: 8.7), n-propyl acetate (SP value: 8.7), dipropylene glycol methyl ether acetate (SP value: 8.7), 3-methoxybutanol acetate (SP value: 8.7), butyl acetate (SP value: 8.7), isopropyl acetate (SP value: 8.5), propylene glycol methyl-n-butyl ether (SP value: 7.8).

[0049] If the main solvent of the target coating agent is a water-soluble solvent, add a non-water-soluble solvent as an additive and adjust the amount in the range of 0.1wt% to 50wt%. If the main solvent is a non-water-soluble solvent, the opposite is true.

[0050] (Firing of printed matter) The printed matter printed by the above-mentioned method using screen printing or metal mask printing can be cured by baking to volatilize the solvent component of the ink paste. The baking conditions may be appropriately determined depending on the constituent components of the ink paste material, the substrate material, etc. In this way, the printed pattern shrinks in both the height and width directions, resulting in a highly precise pattern. This is particularly useful as a technique for forming wiring patterns of structures such as electronic components, display elements, battery electrodes, sensors, etc. It can also be applied to the cases where an elastic substrate or elastic paste is used in these structures. EXAMPLES

[0051] The following describes an embodiment of the present invention.

[0052] [Example 1] In order to confirm the usefulness of the coating composition according to the present invention, a substrate made of a silicone-based silicone elastomer film having a thickness of 200 μm and a conductive coating material made of a silicone-based stretchable silver paste "Dotite XA-9476" manufactured by Fujikura Chemical Industries, Ltd. were prepared. The coating agent used in Example 1 was the silver paste "Dotite XA-9476" as the main agent. Since the main agent, silicone, is water-insoluble, ethylene glycol monoethyl ether acetate (also known as diethyl acetate), which is a water-soluble solvent, was selected as the additive solvent. Coating agent 1 was prepared by mixing the additive in an amount of 0.1 wt% to 50 wt% of the main agent.

[0053] A 100 μm thick nickel film was then attached to a stainless steel mesh to prepare a screen printing plate with holes for the printing pattern. Next, the above-mentioned silicone elastomer film substrate with a thickness of 200 μm was set on the printing stage, and a screen printing plate with a nickel thickness of 100 μm was placed on top of it so that the nickel film surface and the silicone elastomer film were in close contact with each other. A urethane squeegee was then used to sweep the above-mentioned Coating Agent 1 from the stainless steel mesh side, which is the top surface of the screen plate, at a constant contact angle, sweeping speed and load, and the printing pattern was transferred from the screen printing plate with holes opened onto the silicone elastomer film, thereby producing the printed matter of Example 1. The results are shown in FIG. 6 and FIG.

[0054] [Comparative Example 1] Next, coating agent 2 was prepared using only the silver paste "Dotite XA-9476" as the coating agent of Comparative Example 1. A 100 μm thick nickel film was attached to a stainless steel mesh to prepare a screen printing plate with holes for the printing pattern. Next, the above-mentioned silicone elastomer film substrate with a thickness of 200 μm was set on the printing stage, and a screen printing plate with a nickel thickness of 100 μm was placed on top of it so that the nickel film surface and the silicone elastomer film were in close contact with each other. A urethane squeegee was then used to sweep the above-mentioned Coating Agent 2 from the stainless steel mesh side, which is the top surface of the screen plate, at a constant contact angle, sweeping speed and load, and the printing pattern was transferred from the screen plate, which had holes opened, to the silicone elastomer film, to produce a print of Comparative Example 1. The results are shown in Figures 7 and 9.

[0055] As a result, a clear difference was observed between the printing results of Example 1, in which the coating agent according to the present invention was used, and the printing results of Comparative Example 1, in which only the commercially available Dotite XA-9476 was used.

[0056] FIG. 6 shows the print pattern of Example 1, and FIG. The 100 μm wide coil patterns obtained from these prints had a width of 84.6 μm, a height of 63.76 μm, and an aspect ratio of 0.74 for print result 60 in Example 1, whereas the width of the print pattern in print result 70 in Comparative Example 1, which used only the existing product Dotite XA-9476, was 87.5 μm, a height of 20-92 μm, and an aspect ratio of 0.24.

[0057] Further, FIG. 8 shows an enlarged view of the surface of the printed pattern of Example 1, and FIG. 9 shows an enlarged view of the surface of the printed pattern of Comparative Example 1. In the printed pattern surface 81 of Example 1 shown in Figure 8, the shear force at the interface between the screen mesh and the mask opening with holes in the pattern shape is small due to the effect of the coating agent, and the ink is transferred to the substrate with almost no cohesive failure. As a result, the cross-sectional shape of the part of the transferred ink on the top surface that hits the screen mesh is a concave screen mesh mark 82, and the details of the mask opening are also clear. The fact that the screen mesh mark 82 is concave indicates that the parts that hit other than the mesh were printed thickly without splitting due to cohesive failure of the ink. In other words, it can be seen that the print pattern is printed with a steep rise.

[0058] However, when using only the existing product Dotite XA-9476, the mark of Comparative Example 1 in FIG. As shown in the print pattern surface 91, the cross-sectional shape of the part of the transferred ink surface that comes into contact with the screen mesh is a convex screen mesh mark 92, and the details of the mask opening are coarse, meaning that the rise of the print pattern is rounded. This means that the ink splits due to cohesive failure, resulting in thinner printed areas. The screen mesh marks are a phenomenon in which the areas that come into contact with the mesh during screen printing cause unevenness on the surface of the printed pattern compared to areas other than the mesh.

[0059] The printing result of Example 1 shows that the coating material did not adhere to either the side of the holes formed in the nickel film or the stainless steel mesh, and was transferred 100% to the printing substrate, resulting in sharp details at the pattern edges and concave mesh marks. In contrast, the printing result of Comparative Example 1 was that the pattern adhered to both the sides of the holes formed in the nickel film and the stainless steel mesh and was transferred to the printing substrate with cohesive failure, resulting in blunt details on the pattern edges and convex mesh marks. Therefore, by using the coating agent according to the present invention, a high aspect ratio print pattern could be formed using a screen printing plate.

[0060] [Example 2] Next, as Example 2, a printed matter was produced by metal mask printing using the same coating agent as in Example 1, according to the following procedure. The results are shown in FIG.

[0061] First, a metal mask plate with a film thickness of 100 μm and holes for the printing pattern was prepared. Next, the above-mentioned silicone elastomer film substrate with a thickness of 200 μm was set on the printing stage, and the above-mentioned metal mask plate was placed on top of it so that the mask surface and the silicone elastomer film were in close contact with each other. The urethane squeegee was then swept from the top side of the metal plate at a constant contact angle, at a constant sweeping speed and load, and the coating agent of the present invention was transferred from the metal plate with holes in the printing pattern to the silicone elastomer film, producing the printed matter of Example 2.

[0062] [Comparative Example 2] Next, coating agent 2 was prepared using only the silver paste "Dotite XA-9476" as the coating agent for Comparative Example 1, and this was used to print with a metal printing plate in the same manner to produce a printed matter for Comparative Example 2. The results are shown in Figure 11.

[0063] There was a clear difference between the printing results of Example 2, in which the coating agent according to the present invention was used, and the printing results of Comparative Example 2, in which only the commercially available Dotite XA-9476 was used. The printed patterns compared were pillar patterns with a diameter of 100 μm. The printed pattern surface 101 of Example 2 shown in Figure 10 was a steep pillar pattern, whereas the printed pattern surface 111 of Comparative Example 2 shown in Figure 11 was observed to be a pillar pattern in which cohesive failure had occurred.

[0064] From the above results, the coating agent according to the present invention did not cause cohesive failure even when printing using a metal mask, and was able to print sharp details at the pattern edges, whereas the coating agent of the conventional configuration caused cohesive failure, resulting in dull details. Therefore, the coating agent according to the present invention can be applied to printing using a metal mask. [Industrial Applicability]

[0065] According to the present invention, since a pattern that is perpendicular to the substrate can be formed by screen printing or metal mask printing, a wiring pattern with wiring gaps as narrow as possible can be produced. In addition, since it is possible to print wiring with a high aspect ratio, the surface area in the vertical direction of the wiring can be increased. For example, this is suitable for electrodes that require a large reaction area in the form of stripes. In addition, because it is possible to print stretchable wiring patterns with a high aspect ratio, when using a stretchable substrate, the risk of non-conductivity due to expansion and contraction, which has previously been a problem when using stretchable substrates due to large fluctuations in wiring resistance and resulting in malfunction, and when conductivity is achieved through the contact of metal fillers in the wiring pattern, can be reduced, and a stable current can be passed through. [Explanation of symbols]

[0066] 1…Screen mesh 10…Screen printing plate 11…Mask opening 12...Shear force (of the present invention) 14…Ink 15...Base material 16...Mask 21…High aspect ratio printing pattern 22…Surface recess 41...Cohesive failure 42...Kamaboko-shaped print pattern 51...Kamaboko-shaped (cross-sectional shape) 60...Printing result of Example 1 70…Printing result of Comparative Example 1 81...Printed pattern surface of Example 1 82…Concave screen mesh mark 91...Printed pattern surface of Comparative Example 1 92…Convex screen mesh mark 101...Printed pattern surface of Example 2 111: Printed pattern surface of Comparative Example 2

Claims

1. A coating composition comprising a polymer having a silver-containing inorganic filler dispersed therein, a solvent and an additive, a coating agent obtained by mixing ethylene glycol monoethyl ether acetate, a water-soluble additive solvent, in an amount of 0.1 to 50 wt % relative to the main solvent, with the water-insoluble main solvent of the solvent and additive, to form a printing ink; A pattern printing method, comprising printing a pattern on a substrate using a screen printing plate.

2. A coating composition comprising a polymer having a silver-containing inorganic filler dispersed therein, a solvent and an additive, a coating agent obtained by mixing ethylene glycol monoethyl ether acetate, a water-soluble additive solvent, in an amount of 0.1 to 50 wt % relative to the main solvent, with the water-insoluble main solvent of the solvent and additive, to form a printing ink; A pattern printing method, comprising printing a pattern on a substrate using a metal mask.

3. 3. The pattern printing method according to claim 1, A pattern printing method, further comprising baking the printed material after the printing.

4. A printed matter, characterized in that it is printed by the pattern printing method according to any one of claims 1 to 3.

5. 2. A printed matter, characterized in that in the surface shape of the pattern printed by the pattern printing method according to claim 1, portions corresponding to screen mesh marks are concave.

Citation Information

Patent Citations

  • Screen for thick film paste printing and its manufacture

    JP1998278445A

  • Screen mask and its manufacture

    JP1999348447A

  • Method of manufacturing ceramic substrate

    JP2011077431A

  • Coating agent, discharge, and coating applicator

    JP2018070854A

  • Coating agent, discharged material and coating apparatus

    JP2020105444A