Manufacturing method for PTP packaging sheets

By adjusting the heat-resistant coating layer's hardness to match the post-printing layer's hardness through controlled mixing ratios and heating, the method addresses adhesion issues in PTP packaging sheets, enabling flexible use of various ultraviolet curable inks without equipment modifications.

JP7553113B2Active Publication Date: 2024-09-18SHOHOKU LAMINATE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021203326
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-15
Publication Date
2024-09-18
Estimated Expiration
2041-12-15

AI Technical Summary

Technical Problem

Existing PTP packaging sheets face issues with the post-printing layer peeling off or cracking due to poor adhesion between the ultraviolet curable ink and the heat-resistant coating layer, requiring modifications to packaging equipment and limiting the type of ultraviolet curing ink usable in PTP packaging assembly factories.

Method used

A method for producing a packaging sheet with a heat-resistant coating layer adjusted to match the hardness of the post-printing layer by controlling the mixing ratio of epoxy resin and volatile solvent, and specific heating conditions to ensure stable adhesion, allowing for various ultraviolet curable inks to be used without equipment modifications.

Benefits of technology

The method enables consistent high adhesion between the post-printing layer and the heat-resistant coating layer, facilitating easy production of packaging sheets suitable for different ultraviolet curable inks, enhancing manufacturing flexibility and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553113000005
    Figure 0007553113000005
  • Figure 0007553113000002
    Figure 0007553113000002
  • Figure 0007553113000007
    Figure 0007553113000007
Patent Text Reader

Abstract

To provide a manufacturing method of a PTP packaging sheet which can easily produce a packaging sheet having high adhesion to a post-applied printing layer made of an ultraviolet curable ink.SOLUTION: A manufacturing method of a PTP packaging sheet includes the steps of: preparing a heat-resistant coating agent 28x that is a liquid substance obtained by mixing a solid component containing an epoxy resin as a main component and a volatile solvent, in which when a mixing ratio of the solid component is changed in the range of 30 to 45 mass%, the solid component has a kinematic viscosity within the range of 37.3 to 74.8 mm2 / s, the solid component being contained at a constant mixing ratio within the range of 30 to 45 mass% (step KK2); applying the heat-resistant coating agent 28x to a first surface 22a side of an aluminum foil 22 (step KK3); heating the solid component to an extent that the solid component is not thermally cured so as to volatilize the volatile solvent (process KK4, KK5); then heating the heat-resistant coating agent 28x and thermally curing the solid component (step KK6); and adjusting a heating temperature of a first heating step KK4 so that a hardness of a heat-resistant coat layer 28 corresponds to the hardness of a post-applied printed layer 18.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a packaging sheet for PTP, which is thermally bonded to a container sheet to form a lid material for a PTP package and has a post-applied printed layer made of ultraviolet-curable ink on its outer surface. [Background technology]

[0002] A press through package (PTP) is a packaging form in which a small solid object 14 is placed in a storage section 12a formed in a resin container sheet 12, as in the PTP packaging body 10 shown in FIG. 7, and the storage section 12a is closed by adhering a packaging sheet 16 to the flat section 12b of the container sheet 12. The PTP has traditionally been widely used for packaging solid objects such as medicinal tablets and capsules.

[0003] When opening the PTP package 10, the contained solid matter 14 is pressed strongly from the outside of the containing portion 12a against the inner surface of the packaging sheet 16, and is taken out by breaking through the packaging sheet 16, and aluminum foil is generally used as the base material of the packaging sheet 16. When attaching the packaging sheet 16 to the container sheet 12, a method is used in which a heat seal layer provided on one side of the packaging sheet 16 is abutted against the flat portion 12b of the container sheet 12, and heating is applied from the side of the heat-resistant coating layer provided on the other side of the packaging sheet 16, thereby fusing the heat seal layer to the flat portion 12b.

[0004] In many cases, a pre-printed layer (not shown) is provided on the packaging sheet, and information whose contents do not change frequently (such as product name, price, dosage, efficacy, effect, etc.) is displayed on the pre-printed layer. Furthermore, in recent years, when the packaging sheet 16 is assembled into a PTP package, a post-printed layer 18 of ultraviolet-curable ink is added by an inkjet method to the outer surface side of the packaging sheet 16 to display information whose contents change frequently (such as manufacturing date, lot number, expiration date, etc.).

[0005] The post-applied printing layer 18 is formed on the outer surface of the heat-resistant coating layer of the packaging sheet 16, but problems have been pointed out in that the post-applied printing layer 18 is prone to peeling off at the interface from the heat-resistant coating layer, or cracks occur in the post-applied printing layer 18, causing partial fall-off, and the challenge is to improve the adhesion between the post-applied printing layer 18 and the heat-resistant coating layer.

[0006] Conventionally, as a technique for solving this problem, there has been a technique disclosed in Patent Document 1 by the applicants of the present application, in which the composition of the ultraviolet-curable ink that forms the post-applied printed layer is limited, a packaging sheet is prepared in which a first undercoat layer (heat-resistant coating layer) is laminated on an aluminum foil base material, a second undercoat layer made of a specific material is provided on the first undercoat layer of the packaging sheet, and a post-applied printed layer is formed on the second undercoat layer. The second undercoat layer is a layer that functions to improve the adhesion between the post-applied printed layer and the first undercoat layer (heat-resistant coating layer). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2020-1189 A Summary of the Invention [Problem to be solved by the invention]

[0008] Generally, in PTP packaging assembly factories (factories where solid materials are packaged into PTP packaging), components such as packaging sheets, flat resin sheets that will become container sheets, and ultraviolet-curing ink are prepared, and these are then fed into a fully automated packaging machine to assemble the PTP packaging.

[0009] Therefore, when implementing the technology of Patent Document 1, the type of ultraviolet-curable ink to form the post-applied printing layer is limited in the PTP packaging assembly factory, and furthermore, the existing packaging equipment must be modified to add a mechanism for forming the second undercoat layer. Therefore, it is desirable for the PTP packaging assembly factory to solve the above problems at the stage of purchasing the packaging sheet. However, it is difficult for the packaging sheet manufacturer to realize a heat-resistant coating layer that can always obtain high adhesion to various types of ultraviolet-curable ink.

[0010] The present invention has been made in consideration of the above-mentioned background art, and has an object to provide a method for manufacturing a packaging sheet for PTP, which can easily produce a packaging sheet that has high adhesion to a post-applied printed layer made of ultraviolet-curable ink. [Means for solving the problem]

[0011] The present invention provides a heat-sealing film comprising an aluminum foil as a base material, a heat-resistant coating layer located on a surface layer of a first surface side of the aluminum foil, and a heat seal layer located on a surface layer of a second surface side of the aluminum foil, A method for producing a packaging sheet for PTP, the method comprising the steps of: heating an outer surface of the heat-resistant coating layer; heat-sealing the heat-sealing layer to a mating container sheet to form a lid material for a PTP package; and providing a post-applied printing layer using an ultraviolet-curable ink on the outer surface of the heat-resistant coating layer, a hardness information acquiring step of acquiring hardness information of the post-applied printing layer; and a liquid material obtained by mixing a solid component having an epoxy resin as a main component with a volatile solvent, the liquid material having a kinetic viscosity of 37.3 to 74.8 mm at 25° C. when the mixing ratio of the solid component is changed in a range of 30 to 45 mass %. 2a heat-resistant coating agent preparation step of preparing a heat-resistant coating agent containing the solid components falling within the range of 30 to 45 mass % in a constant mixing ratio within the range of 30 to 45 mass %; a heat-resistant coating agent application step of applying a predetermined amount of the heat-resistant coating agent to the first surface side of the aluminum foil so that the finished thickness of the heat-resistant coating layer is a specified value; a solvent volatilization step of heating the heat-resistant coating agent applied in the heat-resistant coating agent application step to an extent that the solid components are not thermally cured to volatilize the volatile solvent; and a solid component thermal curing step of heating the heat-resistant coating agent after the solvent volatilization step to thermally cure the solid components and form the heat-resistant coating layer. This is a method for producing a packaging sheet for PTP, in which the heating temperature in the solvent evaporation step is adjusted so that the hardness of the heat-resistant coating layer corresponds to the hardness of the post-applied printed layer.

[0012] The solvent evaporation process includes a first heating process in which the heat-resistant coating agent applied in the heat-resistant coating agent application process is heated under certain conditions within a range of 215 to 275°C and 1.2±0.2 seconds, and the heating temperature in the first heating process is adjusted so that the hardness of the heat-resistant coating layer corresponds to the hardness of the post-applied printing layer. of The method may further include a second heating step in which the other coating agent applied after the heating step is heated at 270±5° C. for 1.2±0.2 seconds. In the solid component heat curing step, the heat-resistant coating agent and the other coating agent that have been subjected to the second heating step are preferably heated under specific conditions within the range of 175 to 255° C. and 5.7 to 7.5 seconds. Effect of the Invention

[0013] The manufacturing method of the packaging sheet for PTP of the present invention was invented with the aim of improving the adhesion between the post-applied printed layer provided during assembly of the PTP package and the heat-resistant coating layer of the packaging sheet by making the hardness of the heat-resistant coating layer approximately the same as that of the post-applied printed layer. By devising the contents of the heat-resistant coating agent preparation process and the heating conditions of the solvent evaporation process, it is possible to widely change the hardness of the heat-resistant coating layer, so that a heat-resistant coating layer of a hardness corresponding to the hardness information of the other party's post-applied printed layer can be easily formed. Therefore, it is possible to easily and stably manufacture and provide a packaging sheet that matches the user's post-applied printed layer to the user (such as a PTP package assembly factory). [Brief description of the drawings]

[0014] [Figure 1] FIG. 1A is an enlarged cross-sectional view showing an example of the structure of a packaging sheet for a PTP, and FIG. 1B is an enlarged cross-sectional view showing the structure of a PTP package assembled using this packaging sheet. [Diagram 2] 2 is a flowchart showing the relationship between a general manufacturing flow of the packaging sheet in FIG. 1(a) and one embodiment of a manufacturing method of a packaging sheet for PTP of the present invention. [Diagram 3] FIG. 2 is a schematic diagram illustrating an example of a packaging sheet manufacturing apparatus. [Figure 4] 1A is a diagram showing the heating conditions in each pre-heating step, and FIG. 1B is a diagram showing the heating conditions in the main heating step. [Diagram 5] Graph (a) shows the relationship between the kinetic viscosity of the heat-resistant coating agent (solid components A and B) and the workability of the heat-resistant coating agent application process K17, and graph (b) shows the characteristics of heat-resistant coating agent prototypes A30 to A45 and comparison products B15 and B20. [Figure 6] FIG. 1A shows the evaluation results of the heat resistance and adhesion of the heat-resistant coating layer of each packaging sheet produced using prototypes A30 to A45 and comparison products B15 and B20, and FIG. 1B shows a graph conceptually showing the relationship between the heating temperature in the first heating process and the hardness of the heat-resistant coating layer. [Figure 7] FIG. 1 is a cross-sectional view showing the structure of a typical PTP package. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the manufacturing method of a PTP packaging sheet of the present invention will be described with reference to the drawings. First, the structure of a general packaging sheet 16 to which the manufacturing method of this embodiment can be applied, the manufacturing flow (steps K11 to K24) of the packaging sheet 16, and the configuration of a packaging sheet manufacturing apparatus 20 that sequentially executes steps K13 to K24 in the manufacturing flow will be briefly described with reference to Figs. 1 to 3.

[0016] The packaging sheet 16 is manufactured as a single continuous sheet and shipped to an assembly factory for the PTP package 10 in a rolled state. As shown in the enlarged cross-sectional view of FIG. 1(a), the packaging sheet 16 has an aluminum foil 22 as a base material, and on the first surface 22a side of the aluminum foil 22, a milky white printed layer 24 covering the first surface 22a, a first pre-printed layer 26 for displaying information provided on the outer surface of the milky white printed layer 24, and a heat-resistant coating layer 28 covering the outer surfaces of the milky white printed layer 24 and the first pre-printed layer 26 are laminated in this order. In addition, on the second surface 22b side of the aluminum foil 22, a second pre-printed layer 30 and a third pre-printed layer 32 for displaying information provided on the second surface 22b, and a heat seal layer 34 covering the second surface 22b and the outer surfaces of each pre-printed layer 30, 32 are laminated in this order.

[0017] The aluminum foil 22 is made of a hard or soft aluminum material having a thickness of about 10 to 30 μm so that it can be easily torn when the solid matter 14 in the storage section 12a is taken out. The aluminum foil 22 is prepared in a member preparation step K12 in FIG. 2, and is set in the packaging sheet manufacturing apparatus 20 in a rolled state as shown in FIG.

[0018] The opaque white printing layer 24 is formed by preparing a liquid opaque white printing agent 24x, which is a coating resin obtained by mixing a medium and an ink containing a white pigment (component preparation step K12), applying the liquid opaque white printing agent 24x to the first surface 22a of the aluminum foil 22 by the application device Ts13 of the packaging sheet manufacturing device 20 (opaque white printing agent application step K13), heating and pre-drying in a heating furnace Kr14 (pre-heating step K14), and heating and drying / hardening in the final heating furnace Kr24 (main heating step K24). The medium is, for example, a solid component obtained by mixing vinyl chloride resin, which is the main component, with an amino resin for promoting molecular cross-linking, diluted with an appropriate amount of a solvent such as thinner. The ink containing a white pigment is a solid component obtained by mixing titanium oxide, which is a white pigment, with the same composition as the solid component of the medium, diluted with an appropriate amount of a solvent such as thinner.

[0019] The first pre-printed layer 26 is formed by preparing a liquid first pre-printed ink 26x by mixing a pigment of an appropriate color with a base material such as polyvinyl chloride resin and an appropriate amount of volatile solvent (component preparation process K12), applying it to the outer surface of the opaque white printing agent 24x using an application device Ts15 of the packaging sheet manufacturing apparatus 20 (first pre-printed ink application process K15), heating and pre-drying in a heating furnace Kr16 (pre-heating process K16), and heating and drying / hardening in the final stage heating furnace Kr24 (main heating process K24).

[0020] The heat-resistant coating layer 28 is formed by preparing a liquid heat-resistant coating agent 28x, which is a mixture of a solid component mainly made of epoxy resin and a volatile solvent (component preparation step K12), applying it to the outer surfaces of the opaque printing agent 24x and the first pre-printed ink 26x by the application device Ts17 of the packaging sheet manufacturing device 20 (heat-resistant coating agent application step K17), heating and pre-drying it in a heating furnace Kr18 (pre-heating step K18), and heating and drying / hardening it in the final heating furnace Kr24 (main heating step K24). The heat-resistant coating agent may have a solid component mainly made of nitrocellulose or acrylic resin, but epoxy resin is the most commonly used material.

[0021] Here, the heat-resistant coating layer 28 is transparent or semi-transparent so that the information displayed on the first pre-printed layer 26 can be seen from the outside. The opaque white printed layer 24 is a layer that suppresses reflection from the glossy surface of the aluminum foil 22 when the first pre-printed layer 26 is viewed, and serves to improve the visibility of the first pre-printed layer 26, and may be a opaque white color or a clear white color.

[0022] The second pre-printed layer 30 is formed by preparing a liquid second pre-printed ink 30x by mixing a pigment of an appropriate color with a base material such as polyvinyl chloride resin and an appropriate amount of volatile solvent (component preparation process K12), applying it to the second surface 22b of the aluminum foil 22 using an application device Ts19 of the packaging sheet manufacturing apparatus 20 (second pre-printed ink application process K19), heating and pre-drying in a heating furnace Kr20 (pre-heating process K20), and heating and drying / curing in the final stage heating furnace Kr24 (main heating process K24).

[0023] The third pre-printed layer 32 is formed by preparing a liquid third pre-printed ink 32x by mixing a pigment of a different color from the second pre-printed layer 30 with a base material such as polyvinyl chloride resin, mixing it with an appropriate amount of volatile solvent (component preparation process K12), applying it to the second surface 22b of the aluminum foil 22 using an application device Ts21 of the packaging sheet manufacturing apparatus 20 (third pre-printed ink application process K21), heating and pre-drying in a heating furnace Kr22 (pre-heating process K22), and heating and drying / hardening in the final stage heating furnace Kr24 (main heating process K24).

[0024] The heat seal layer 34 is formed by preparing a liquid heat seal agent 34x mainly made of a mixture of polyvinyl chloride resin and polyester-based resin, a mixture of polyvinyl chloride resin and acrylic-based resin, or polypropylene resin (component preparation process K12), applying it to the second surface 22b of the aluminum foil 22 and the outer surfaces of each pre-printed ink 30x, 32x using an application device Ts23 of the packaging sheet manufacturing apparatus 20 (heat seal agent application process K23), and heating and drying / curing it in the final stage heating furnace Kr24 (main heating process K24).

[0025] The packaging sheet 16 is manufactured through the above-mentioned process, wound up on a roll, and shipped to an assembly factory for the PTP packages 10. Note that the process design step K11 in Fig. 2 is a step for determining what materials will be prepared in the material preparation step K12 and the specific contents of steps K13 to K24 performed by the packaging sheet manufacturing apparatus 20 (e.g., heating conditions for each heating furnace, etc.).

[0026] In the assembly factory of the PTP package 10, the incoming package sheet 16 is put into a dedicated packaging device (not shown), and ultraviolet-curable ink is applied to the outer surface of the heat-resistant coating layer 28 by a method such as an inkjet method, and then dried and cured to form the post-applied printed layer 18. Then, after the solid matter 14 is placed in the storage section 12a of the container sheet 12, the outer surface of the heat-resistant coating layer 28 is heated and pressurized to thermally bond the heat seal layer 34 to the container sheet 12 in order to close the opening of the storage section 12a with the package sheet 16 (lid material). This forms the PTP package 10 in the assembled state shown in FIG. 1(b).

[0027] Next, one embodiment of the method for producing a packaging sheet of the present invention will be described assuming that the method is applied to the production flow of the packaging sheet 16 described above (steps K11 to K24).

[0028] The manufacturing method of the packaging sheet of this embodiment, as shown in the right column of Figure 2, is composed of a hardness information acquisition process KK1, a heat-resistant coating agent preparation process KK2, a heat-resistant coating agent application process KK3, a solvent evaporation process (first and second heating processes KK4, KK5) and a solid component thermal curing process KK6.

[0029] The hardness information acquisition process KK1 is a process for acquiring hardness information of the post-additional printing layer 18, and is performed as a part of the process design process K11 described above. The hardness information means information on the hardness of the post-additional printing layer 18 in the finished state or on the physical property value corresponding to the hardness, and may be obtained from, for example, a user's assembly plant for PTP packages, or may be obtained as a sample on which the user's post-additional printing layer 18 is formed, and the hardness may be measured.

[0030] The concept of the present invention is to "make the hardness of the heat-resistant coating layer approximately the same as that of the post-applied printed layer in order to improve adhesion between the post-applied printed layer and the heat-resistant coating layer," so it is important to obtain hardness information of the other party's post-applied printed layer 18 before starting production of the packaging sheet 16.

[0031] The heat-resistant coating agent preparation process KK2 is a liquid mixture of a solid component mainly composed of an epoxy resin and a volatile solvent, and when the mixture ratio of the solid component is changed in the range of 30 to 45 mass%, the kinetic viscosity at 25 ° C. is 37.3 to 74.8 mm 2 This is a process for preparing a heat-resistant coating agent 28x containing solid components falling within the range of 30 to 45 mass % in terms of viscosity / s, at a constant mixing ratio within the range of 30 to 45 mass %, and is performed as part of the component preparation process K12 described above. The meanings of the solid component mixing ratio and the kinetic viscosity values ​​will be explained in detail later, but these values ​​specify the type of heat-resistant coating agent that can be used (the type of epoxy resin that is the main agent of the solid components). The heat-resistant coating agent 28x may be prepared in the manufacturing plant of the packaging sheet 16, or may be purchased by ordering from a heat-resistant coating agent manufacturer.

[0032] The heat-resistant coating agent application process KK3 is a process of applying a predetermined amount of heat-resistant coating agent 28x to the first surface 22a side of the aluminum foil 22 so that the finished thickness of the heat-resistant coating layer 28 becomes a specified value, and corresponds to the heat-resistant coating agent application process K17 described above.

[0033] The solvent evaporation process is a process in which the heat-resistant coating agent 28x applied in the heat-resistant coating agent application process KK3 is heated to a degree that does not thermally harden the solid components, and volatile solvents are evaporated, and is composed of first and second heating processes KK4 and KK5. The first heating process KK4 is a process in which the heat-resistant coating agent 28x applied in the heat-resistant coating agent application process KK3 is heated under certain conditions, and corresponds to the pre-heating process K18 described above. The second heating process KK5 is a process in which the heat-resistant coating agent 28x that has been subjected to the first heating process KK4 and the first ofThis is a process for heating the other coating materials (second and third pre-printing inks 30x, 32x) applied after the heating process KK4 under certain conditions, and corresponds to the pre-heating processes K20 and K22 described above. Here, the second heating process KK5 is performed twice. The specific heating conditions will be described later.

[0034] The solid component thermal curing step KK6 is a step of heating the heat-resistant coating agent 28x after the solvent evaporation step to thermally cure the solid components and form the heat-resistant coating layer 28, and corresponds to the main heating step K24 described above. Specific heating conditions will be described later.

[0035] The specific contents of steps KK2 to KK6 are determined in the initial process design step K11. Among these, items to be determined based on the hardness information of the post-applied printing layer 18 acquired in the hardness information acquisition step KK1 are the heating conditions in the preliminary heating step K18 (first heating step KK4), etc.

[0036] 4(a) and (b) show the preferred heating conditions for each heating step. The heating conditions for the pre-heating steps K14 and K16 are 270±5°C and 1.2±0.2 seconds, respectively. The pre-heating steps K14 and K16 are performed before the application of the heat-resistant coating agent 28x, and the heating conditions for these steps have almost no effect on the hardness of the finished heat-resistant coating layer 28.

[0037] The heating conditions of the pre-heating step K18 (first heating step KK4) are set to constant conditions within the ranges of 215 to 275°C and 1.2±0.2 seconds. The pre-heating step K18 (first heating step KK4) is a step in which the applied heat-resistant coating agent 28x is first heated to volatilize the volatile solvent, and since the heating conditions of this step greatly affect the hardness of the finished state of the heat-resistant coating layer 28, the heating temperature t18 is determined to a specific value within the range of 215 to 275°C based on the hardness information of the post-applied printing layer 18. How this is determined will be explained later.

[0038] The heating conditions for the pre-heating steps K20 and K22 (second heating step KK5) are 270±5°C and 1.2±0.2 seconds, respectively. Since the pre-heating steps K20 and K22 (second heating step KK5) are steps for heating the heat-resistant coating agent 28x, the heating conditions affect to some extent the hardness of the finished state of the heat-resistant coating layer 28. However, since the heating conditions for the pre-heating step K18 (first heating step KK4) have a greater influence, the heating conditions for this step are fixed to a certain condition regardless of the hardness information of the post-applied printing layer 18.

[0039] The heating conditions for this heating step K24 (solid component heat curing step KK6) are specific conditions within the range of 175 to 255°C and 5.7 to 7.5 seconds. For example, a continuous furnace with three zones is used as the heating furnace Kr24, with the first zone at 180±5°C and 2.2±0.3 seconds, the second zone at 250±5°C and 2.2±0.3 seconds, and the third zone at 250±5°C and 2.2±0.3 seconds.

[0040] Since the main heating step K24 (solid component heat curing step KK6) is a step for heating and heat curing the heat-resistant coating agent 28x, the heating conditions affect the hardness of the finished state of the heat-resistant coating layer 28, but also affect the finished states of the other coating layers, and therefore cannot be easily changed. Therefore, the hardness of the heat-resistant coating layer 28 is adjusted by the heating temperature t18 of the preliminary heating step K18 (first heating step KK4), and the heating conditions of this step are fixed to certain conditions regardless of the hardness information of the post-applied printing layer 18.

[0041] Next, the meaning of the mixing ratio and the kinetic viscosity of the heat-resistant coating agent 28x prepared in the heat-resistant coating agent preparation step KK2, and the method of setting the heating temperature t18 in the preliminary heating step K18 (first heating step KK4) will be explained. These are important matters for achieving the objective of "setting the hardness of the finished heat-resistant coating layer 28 to a value corresponding to (almost the same as) the hardness of the finished post-applied printing layer 18."

[0042] First, the contents of the tests and evaluations carried out by the inventors in the process of considering the present invention will be described. The inventors prepared two types of solid components A and B, which are different types of epoxy resin as the main component, and a volatile solvent, to produce heat-resistant coating agents 28x with various mixing ratios, and measured the kinetic viscosity at 25°C (FIG. 5(a)). The heat-resistant coating agent 28x using solid component B is a general-purpose heat-resistant coating agent that the inventors have been using for some time.

[0043] In the general-purpose packaging sheet manufacturing apparatus 20, in order to perform the heat-resistant coating agent application step K17 and the temporary drying step K18 without any problems (to ensure good coating properties), the kinetic viscosity is set to 37.3 to 74.8 mm. 2 / s. Therefore, as shown in Fig. 5(a), when the heat-resistant coating layer 28x is produced using solid component A, the mixing ratio of solid component A needs to be set in the range of 30 to 45%, and when the heat-resistant coating layer 28x is produced using solid component B, the mixing ratio of solid component B needs to be set in the range of 15 to 20%. In other words, in the case of solid component A, the ratio of the volatile solvent can be low, and in the case of solid component B, the ratio of the volatile solvent must be significantly high.

[0044] Next, the inventors produced packaging sheets 16 using heat-resistant coating agents 28x (trial products A30, A35, A40, A45) in which the mixing ratio of solid component A was set to 30, 35, 40, 45 mass% and heat-resistant coating agents 28x (comparison products B15, B20) in which the mixing ratio of solid component B was set to 15, 20 mass%, and evaluated the heat resistance and adhesion of the finished heat-resistant coating layer 28. The application amount of the heat-resistant coating agent 28x was appropriately adjusted so that the thickness of the heat-resistant coating layer 28 in the finished state was a specified value, the heating conditions of each heating furnace when producing the packaging sheet 16 were the conditions shown in Figures 4(a) and (b), and the heating temperature t18 in the provisional heating process K18 (first heating process KK4) was set to three values, 220, 245, and 270°C (setting accuracy ±5°C).

[0045] Heat resistance was evaluated by applying stress to the heat-resistant coating layer 28 equivalent to the heating and pressurization by a heat seal bar when welding the packaging sheet 16 to the mating container sheet 12, and observing whether discoloration, carbonization, or other abnormalities occurred in the heat-resistant coating layer 28. Adhesion was also evaluated by performing a test in which a specified adhesive tape was attached to the surface of the heat-resistant coating layer 28, folded back 180 degrees, and peeled off (a so-called 180-degree peel test), and the result was judged to be good or bad.

[0046] Figure 6(a) shows the evaluation results of heat resistance and adhesion. The heat-resistant coating layer 28 made of prototypes A30 to A45 was OK at heating temperatures t18 = 220, 245, and 270°C, but the heat-resistant coating layer 28 made of comparison products B15 and B20 was NG at heating temperatures t18 = 220 and 245°C, and was OK only at t18 = 270°C.

[0047] The evaluation results of the heat-resistant coating layer 28 made of the comparative products B15 and B20 are thought to be influenced by the fact that the mixture ratio of the volatile solvent in the comparative products B15 and B20 is very high (80-85%). In other words, when the heating temperature t18 was set to 270°C, it was OK because a specific amount of the volatile solvent could be evaporated in the preliminary drying step K18 (first heating step KK4), but when the heating temperature t18 was set to 220, 245°C, it was NG because a specific amount of the volatile solvent could not be evaporated in the preliminary drying step K18 (first heating step KK4).

[0048] Similarly, the evaluation results of the heat-resistant coating layer 28 made of prototypes A30 to A45 are thought to be influenced by the fact that the mixture ratio of the volatile solvent is relatively low (55 to 70%) in prototypes A30 to A45. In other words, even when the heating temperature t18 was set to a low temperature of 220°C, it was possible to volatilize a specific amount of the volatile solvent in the preliminary drying step K18 (first heating step KK4), and it is presumed that all of the heating temperatures in the range of t18 = 220, 245, and 270°C were OK.

[0049] FIG. 6(b) conceptually shows the relationship between the hardness of the heat-resistant coating layer 28 made of the prototypes A30, A35, A40, and A45) and the heating temperature t18 in the preliminary drying step K18 (first heating step KK4), and the hardness of the heat-resistant coating layer 28 tends to decrease as the heating temperature t18 decreases. This characteristic is almost unchanged even if the mixing ratio of the solid components is changed. This is considered to be because the thermal curing speed of the solid components changes depending on the amount of volatile solvent remaining in the heat-resistant coating agent 28 at the time when it is introduced into the final main heating step K24 (solid component thermal curing step KK6). In other words, it is presumed that the lower the heating temperature t18 in the preliminary heating step K18 (first heating step KK4), the more the amount of volatile solvent remaining in the heat-resistant coating agent 28, and the slower the thermal curing speed of the solid components in the main heating step K24 (solid component thermal curing step KK6), resulting in a decrease in the hardness of the heat-resistant coating layer 28.

[0050] As can be seen from Figs. 6(a) and (b), when the heat-resistant coating layer 28 is formed using the prototypes A30 to A45, the heating temperature t18 can be set in a wide range of 215 to 275°C, so the hardness of the finished heat-resistant coating layer 28 can be changed significantly by adjusting the heating temperature t18. Therefore, the heat-resistant coating agent 28x using the solid component A is suitable for the manufacturing method of the packaging sheet of the present invention. On the other hand, when the heat-resistant coating layer 28 is formed using the comparative products B15 and B20, the heating temperature t18 can only be set in a narrow range of around 270°C, so the hardness of the finished heat-resistant coating layer 28 cannot be changed significantly. Therefore, the heat-resistant coating agent 28x using the solid component B cannot be used for the manufacturing method of the packaging sheet of the present invention.

[0051] Based on the results of the above experiments and evaluations, the meaning of the mixing ratio and the dynamic viscosity of the heat-resistant coating agent 28x prepared in the heat-resistant coating agent preparation process KK2, and the method of setting the heating temperature t18 in the preliminary heating process K18 (first heating process KK4) will be explained.

[0052] As described above, in the heat-resistant coating agent preparation process KK2, a liquid mixture of a solid component mainly composed of an epoxy resin and a volatile solvent is prepared. When the mixture ratio of the solid component is changed in the range of 30 to 45 mass%, the kinetic viscosity at 25°C is 37.3 to 74.8 mmHg. 2 A heat-resistant coating agent 28x is prepared by mixing a solid component falling within the range of 30 to 45 mass % in the range of 100 / s. This allows the subsequent heat-resistant coating agent application step K17 and pre-drying step K18 to be carried out without any problems, and allows the heating temperature t18 of the pre-heating step K18 (first heating step KK4) to be set within a wide range of 215 to 275°C.

[0053] Furthermore, the heating temperature t18 in the pre-heating step K18 (first heating step KK4) is adjusted to a specific temperature within the range of 215 to 275°C based on the hardness information of the post-applied printed layer 18 acquired in the hardness information acquisition step KK1. This makes it possible to easily and stably achieve the objective of "adjusting the hardness of the finished heat-resistant coating layer 28 to a value corresponding to (almost the same as) the hardness of the finished post-applied printed layer 18."

[0054] The optimum value of the heating temperature t18 varies somewhat depending on the heating conditions of other heating steps that affect the hardness of the finished state of the heat-resistant coating layer 28, i.e., the other preliminary heating steps K20 and K22 (second heating step KK5) in which the heat-resistant coating agent 28x is heated, and the main heating step K24 (solid component thermal curing step KK6). However, since the heating conditions of the other heating steps also affect the finished state of coating layers other than the heat-resistant coating layer 28, it is preferable to fix them to general heating conditions as shown in Figures 4(a) and (b). Then, by fixing the heating conditions of the other heating steps, the optimum value of the heating temperature t18 can be easily derived based on the hardness information.

[0055] As described above, the manufacturing method of the PTP packaging sheet of this embodiment makes it possible to widely change the hardness of the heat-resistant coating layer 28 by devising the heating conditions in the heat-resistant coating agent preparation step KK2 and the solvent evaporation step (first heating step KK4), and therefore, based on the hardness information of the other party's post-applied printed layer 18, it is possible to easily form the heat-resistant coating layer 28 with a hardness corresponding to this. Therefore, it is possible to easily and stably manufacture and provide the packaging sheet 16 that matches the user's post-applied printed layer 18 to the user (such as an assembly plant for the PTP package 10).

[0056] The manufacturing method of the PTP packaging sheet of the present invention is not limited to the above embodiment. For example, the PTP packaging sheet manufacturing method (steps K13 to K24 / steps KK1 to KK6) shown in Fig. 2 corresponds to the configuration of the packaging sheet 16 shown in Fig. 1(a), but even if a part of the configuration of the packaging sheet 16 is changed, it can be handled by changing a part of the steps in accordance with the change.

[0057] For example, when manufacturing a packaging sheet 16 that does not have the opaque white printed layer 24 or the first pre-printed layer 26 between the aluminum foil 22 and the heat-resistant coating layer 28, the steps related to the opaque white printed layer 24 and the first pre-printed layer 26 (steps K13 to K16) in the manufacturing flow of Figure 2 can be simply omitted, and the content of the other steps (steps K11, K12, K17 to K24 / steps KK1 to KK6) does not need to be changed much.

[0058] In addition, when manufacturing a packaging sheet 16 without the second pre-printed layer 30 or the third pre-printed layer 32 between the aluminum foil 22 and the heat seal layer 34, the steps related to the second pre-printed layer 30 or the third pre-printed layer 32 in the manufacturing flow of FIG. 2 (steps K19 to K22 / step KK5) can be omitted, and the contents of the other steps (steps K11 to K18, K23, K24 / steps KK1 to KK4, KK6) do not need to be significantly changed. However, since the preliminary drying steps K20 and K22 (second heating step KK5), which have some effect on the hardness of the heat-resistant coating layer 28, are omitted, there is a possibility that the way in which the hardness of the heat-resistant coating layer 28 changes when the heating temperature t18 of the preliminary heating step K18 (first heating step KK4) is changed may be slightly different. Therefore, in the process design step K11, the heating temperature t18 is determined taking this point into consideration.

[0059] The heating conditions in this heating step K24 (solid component thermal curing step KK6) are not changed for the purpose of adjusting the hardness of the heat-resistant coating layer 28, and are preferably fixed at specific conditions within the ranges of 175 to 255° C. and 5.7 to 7.5 seconds.

[0060] In addition, the type of ultraviolet-curing ink that forms the counterpart post-applied printed layer is not particularly limited, and various ultraviolet-curing inks can be used. [Explanation of symbols]

[0061] 10 PTP packaging 12 Container Sheet Packaging sheet for 16 PTP 18 Post-printing layer using UV-curable ink 20 Packaging sheet manufacturing equipment 22 Aluminum foil 22a Front page 22b Second side 28 Heat-resistant coating layer 28x Heat-resistant coating agent 34 Heat seal layer 34x Heat sealant KK1 Hardness information acquisition process KK2 Heat-resistant coating preparation process KK3 Heat-resistant coating process KK4 First heating process (solvent evaporation process) KK5 Second heating process (solvent evaporation process) KK6 Solid component heat curing process

Claims

1. The present invention comprises an aluminum foil as a base material, a heat-resistant coating layer located on a surface layer of a first surface side of the aluminum foil, and a heat seal layer located on a surface layer of a second surface side of the aluminum foil, In a method for producing a packaging sheet for a PTP, an outer surface of the heat-resistant coating layer is heated, and the heat seal layer is thermally bonded to a mating container sheet to form a lid material for a PTP package, and a post-applied printing layer using an ultraviolet-curable ink is provided on the outer surface of the heat-resistant coating layer, a hardness information acquisition step of acquiring hardness information of the post-applied printing layer; and a liquid mixture of a solid component having an epoxy resin as a main component and a volatile solvent, the liquid mixture having a kinetic viscosity of 37.3 to 74.8 mm at 25° C. when the mixture ratio of the solid component is changed in a range of 30 to 45 mass %. 2 a heat-resistant coating agent preparation step of preparing a heat-resistant coating agent containing the solid components falling within the range of 30 to 45 mass % in a constant mixing ratio within the range of 30 to 45 mass %; a heat-resistant coating agent application step of applying a predetermined amount of the heat-resistant coating agent to the first surface side of the aluminum foil so that the thickness of the finished heat-resistant coating layer becomes a specified value; a solvent volatilization step of heating the heat-resistant coating agent applied in the heat-resistant coating agent application step to an extent that the solid components are not thermally cured to volatilize the volatile solvent; and a solid component thermal curing step of heating the heat-resistant coating agent after the solvent volatilization step to thermally cure the solid components and form the heat-resistant coating layer. A method for manufacturing a packaging sheet for PTP, characterized in that the heating temperature in the solvent evaporation process is adjusted so that the hardness of the heat-resistant coating layer corresponds to the hardness of the post-applied printed layer.

2. 2. The method for manufacturing a packaging sheet for a PTP according to claim 1, wherein the solvent evaporation process includes a first heating process for heating the heat-resistant coating agent applied in the heat-resistant coating agent application process under constant conditions within a range of 215 to 275° C. and 1.2±0.2 seconds, and the heating temperature in the first heating process is adjusted so that the hardness of the heat-resistant coating layer corresponds to the hardness of the post-applied printing layer.

3. 3. The method for manufacturing a packaging sheet for a PTP according to claim 2, wherein the solvent evaporation process includes a second heating process in which the heat-resistant coating agent that has undergone the first heating process and another coating agent that has been applied after the first heating process are heated under conditions of 270±5°C and 1.2±0.2 seconds.

4. The method for manufacturing a packaging sheet for PTP according to claim 3, wherein in the solid component heat curing process, the heat-resistant coating agent and other coating agents that have been subjected to the second heating process are heated under specific conditions within the range of 175 to 255°C and 5.7 to 7.5 seconds.

Citation Information

Patent Citations

  • Fluorine-containing polymer and method for producing the same

    JP2014001369A

  • Inkjet recording method, and method for producing laminated printed matter

    JP2020001189A

  • Method for manufacturing hard coat film

    JP2021159795A