Optical film set, optical laminate

The optical film set addresses the issue of glass film cracking in liquid crystal cells by using a specific adhesive layer thickness to enhance durability and impact resistance.

JP7553174B2Active Publication Date: 2024-09-18NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021511342
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-11
Publication Date
2024-09-18
Estimated Expiration
2040-03-11

AI Technical Summary

Technical Problem

Thin glass films used as front plates in liquid crystal cells are prone to cracking due to their thinness, which limits their durability and resistance to impact.

Method used

An optical film set is designed with a first adhesive layer and a first optical film on the viewing side, and a second adhesive layer and a second optical film on the back side, where the second adhesive layer has a thickness of 50 μm or more and 200 μm or less, enhancing the resistance to cracking of the glass film.

Benefits of technology

The optical film set significantly improves the resistance to cracking of the glass film on the viewing side of optical elements, providing enhanced durability and protection against impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553174000006
    Figure 0007553174000006
  • Figure 0007553174000001
    Figure 0007553174000001
  • Figure 0007553174000002
    Figure 0007553174000002
Patent Text Reader

Abstract

This optical film set has a first optical film which is provided with a first adhesive layer and which is disposed on the visible side of an optical element via the first adhesive layer, and a second optical film which is provided with a second adhesive layer and which is disposed on the back surface side of the optical element via the second adhesive layer, a first glass film having a thickness of 50 µm to 150 µm being provided on the visible-side surface of the first optical film, and the thickness of the second adhesive layer being 50 µm to 200 µm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical film set and an optical laminate. [Background technology]

[0002] In recent years, liquid crystal cells equipped with a touch sensor function on the screen have come to be used in a wide range of fields, from mobile phones to information displays.

[0003] One example is a display panel in which a film or glass having a sensor function is laminated on a polarizing plate, and a reinforced glass called a front plate is placed on the outermost layer via an adhesive layer to fill in the steps on the sensor surface. Recently, liquid crystal panels called in-cell have appeared, in which a touch sensor is incorporated into the glass substrate of the liquid crystal cell, in order to reduce thickness and weight.

[0004] On the other hand, tempered glass is becoming thinner, but there is a limit to how thin it can be because tempered glass self-destructs due to compressive stress when it is 300μm or thinner. Under these circumstances, efforts are being made to increase the hardness of the front panel by using resin, but the reality is that sufficient hardness cannot be obtained.

[0005] In view of this, a thin glass film has been attracting attention as a front panel for a liquid crystal cell. This glass film is integrated with a polarizing plate, for example, via an adhesive layer. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2013 / 175767 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the glass film disposed on the viewing side surface of an optical element such as a liquid crystal cell has a very thin thickness of about 50 μm to 150 μm, and therefore has a problem of being easily broken when subjected to impact.

[0008] The present invention has been made in view of the above-mentioned points, and has an object to provide an optical film set capable of improving the resistance to cracking of a glass film arranged on the viewing side of an optical element. [Means for solving the problem]

[0009] This optical film set comprises a first optical film having a first adhesive layer and arranged on the viewing side of an optical element via the first adhesive layer, and a second optical film having a second adhesive layer and arranged on the back side of the optical element via the second adhesive layer, wherein a first glass film having a thickness of 50 μm or more and 150 μm or less is provided on the viewing side surface of the first optical film, and the second adhesive layer has a thickness of 50 μm or more and 200 μm or less. Effect of the Invention

[0010] According to the disclosed technique, it is possible to provide an optical film set capable of improving the resistance to cracking of a glass film disposed on the viewing side of an optical element. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a cross-sectional view illustrating an optical film set according to the first embodiment. [Diagram 2] FIG. 11 is a cross-sectional view illustrating an optical film set according to a second embodiment. [Diagram 3] FIG. 11 is a cross-sectional view illustrating an optical laminate according to a third embodiment. [Figure 4] FIG. 11 is a cross-sectional view illustrating an optical laminate according to a fourth embodiment. [Diagram 5] FIG. 1 is a diagram illustrating a ball drop test. [Figure 6] FIG. 1 is a diagram for explaining an embodiment. [Figure 7] FIG. 13 is a diagram illustrating a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, the same components are denoted by the same reference numerals, and duplicated explanations may be omitted.

[0013] First Embodiment 1 is a cross-sectional view illustrating an optical film set according to Embodiment 1. Referring to FIG. 1, the optical film set 1 includes a first optical film 10 and a second optical film 20.

[0014] The first optical film 10 includes, in this order, a first glass film 11, a first adhesive layer 12, a first polarizing plate 13, a first retardation layer 14, a first pressure-sensitive adhesive layer 18, and a first release film 19. However, the first retardation layer 14 is not an essential component and is provided as necessary.

[0015] In this specification, the pressure-sensitive adhesive layer refers to a layer that has adhesiveness at room temperature and adheres to an adherend with light pressure. Therefore, even when an adherend attached to the pressure-sensitive adhesive layer is peeled off, the pressure-sensitive adhesive layer retains practical adhesive strength. On the other hand, the adhesive layer refers to a layer that can bond substances by being interposed between substances. Therefore, when an adherend attached to the adhesive layer is peeled off, the adhesive layer does not have practical adhesive strength.

[0016] The first polarizing plate 13 has a first polarizer 131 and a first protective film 132. The first protective film 132 is disposed on at least one side of the first polarizer 131. The first protective film 132 is preferably disposed at least on the first adhesive layer 12 side of the first polarizer 131, but may be disposed on both sides of the first polarizer as necessary.

[0017] The first retardation layer 14 is disposed on the opposite side of the first polarizing plate 13 from the first adhesive layer 12. The first retardation layer 14 can be laminated to the first polarizing plate 13 via any suitable pressure-sensitive adhesive layer or adhesive layer (not shown).

[0018] The first release film 19 is disposed on the opposite side of the first retardation layer 14 from the first polarizing plate 13 with the first pressure-sensitive adhesive layer 18 interposed therebetween.

[0019] The second optical film 20 includes, in this order, a second release film 29, a second pressure-sensitive adhesive layer 28, a second retardation layer 24, a second polarizing plate 23, and an optical layer 25. However, the second retardation layer 24 and the optical layer 25 are not essential components and are provided as necessary.

[0020] The second polarizing plate 23 has a second polarizer 231. The second polarizing plate 23 may include a second protective film 232 disposed on one side or both sides of the second polarizer 231, as necessary.

[0021] The second retardation layer 24 can be laminated to the second polarizing plate 23 via any appropriate pressure-sensitive adhesive layer or adhesive layer (not shown).

[0022] The optical layer 25 may be disposed on both sides of the second polarizing plate 23, if necessary. When the second polarizing plate 23 includes a second protective film 232, the optical layer 25 is preferably disposed on the side of the second protective film 232 opposite to the second polarizer 231. The optical layer 25 can be laminated to the second polarizing plate 23 via any suitable pressure-sensitive adhesive layer or adhesive layer (not shown).

[0023] Each component of the optical film set 1 will now be described in more detail.

[0024] (First Optical Film) [First Glass Film] The first glass film 11 is not particularly limited, and an appropriate one can be adopted depending on the purpose. The first glass film 11 can be classified according to composition, for example, soda-lime glass, borate glass, aluminosilicate glass, quartz glass, etc. Also, according to alkali components, it can be non-alkali glass or low-alkali glass. The content of alkali metal components (for example, Na2O, K2O, Li2O) in the above glass is preferably 15 wt% or less, more preferably 10 wt% or less.

[0025] The thickness of the first glass film 11 is preferably 50 μm to 150 μm, more preferably 60 μm to 140 μm, further preferably 70 μm to 130 μm, and particularly preferably 80 μm to 120 μm. Within such a range, the first optical film 10 can be obtained which is excellent in flexibility, can be processed by a roll-to-roll process, is less likely to break, and has excellent productivity.

[0026] The first glass film 11 preferably has a light transmittance of 85% or more at a wavelength of 550 nm.The first glass film 11 preferably has a refractive index of 1.4 to 1.65 at a wavelength of 550 nm.

[0027] The density of the first glass film 11 is preferably 2.3 g / cm 3 ~3.0g / cm 3 and more preferably 2.3 g / cm 3 ~2.7g / cm 3 If the glass film falls within the above range, it is possible to provide the optical film set 1 that can contribute to reducing the weight of the image display.

[0028] The method for forming the first glass film 11 is not particularly limited, and an appropriate method can be adopted depending on the purpose. Typically, the first glass film 11 can be produced by melting a mixture containing a main raw material such as silica or alumina, an antifoaming agent such as mirabilite or antimony oxide, and a reducing agent such as carbon at a temperature of about 1400°C to 1600°C, forming the mixture into a thin plate, and then cooling the mixture. Examples of the method for forming the first glass film 11 include a slot downdraw method, a fusion method, and a float method. The glass film formed into a plate by these methods may be chemically polished with a solvent such as hydrofluoric acid as necessary to make the glass film thinner or to improve the smoothness.

[0029] [First adhesive layer] The first adhesive layer 12 is not particularly limited, and an appropriate adhesive can be used depending on the purpose. Examples of the adhesive include polyester adhesives, polyurethane adhesives, polyvinyl alcohol adhesives, and epoxy adhesives. Among these, epoxy adhesives are preferred because they provide particularly good adhesion.

[0030] If the first adhesive layer 12 is a thermosetting adhesive, it can be heated to harden (solidify) and thereby exert its peel resistance. If the first adhesive layer 12 is a photocurable adhesive such as an ultraviolet-curable adhesive, it can be hardened by irradiating it with ultraviolet light or other light and thus exert its peel resistance. If the first adhesive layer 12 is a moisture-curable adhesive, it can be hardened by reacting with moisture in the air and therefore can be hardened by being left to stand and exert its peel resistance.

[0031] The first adhesive layer 12 may be, for example, a commercially available adhesive, or may be prepared as an adhesive solution (or dispersion) by dissolving or dispersing various curable resins in a solvent.

[0032] The thickness of the first adhesive layer 12 is preferably 10 μm or less, more preferably 0.1 μm to 10 μm, further preferably 0.5 μm to 8 μm, and particularly preferably 1 μm to 6 μm. Within such a range, the first optical film 10 has excellent flexibility and excellent puncture resistance.

[0033] The elastic modulus of the first adhesive layer 12 is preferably 0.5 GPa to 15 GPa, more preferably 0.8 GPa to 10 GPa, and even more preferably 1 GPa to 5 GPa. Within such ranges, the first optical film 10 having excellent flexibility and excellent puncture resistance can be obtained. In this specification, the elastic modulus can be measured using an autograph under the following conditions.

[0034] [Elasticity measurement method] Measurement temperature: 23℃ Sample size: width 2cm, length 15cm Chuck distance: 10cm Tensile speed: 10mm / min.

[0035] [First polarizing plate] The thickness of the first polarizing plate 13 is preferably 5 μm to 300 μm, more preferably 10 μm to 250 μm, further preferably 25 μm to 200 μm, and particularly preferably 25 μm to 100 μm.

[0036] The elastic modulus of the first polarizing plate 13 is preferably 1 GPa or more, more preferably 1 GPa to 10 GPa, still more preferably 2 GPa to 7 GPa, and particularly preferably 2 GPa to 5 GPa. Within such a range, the first optical film 10 having excellent puncture resistance can be obtained.

[0037] The shape of the first polarizing plate 13 is not particularly limited and may be any suitable shape depending on the purpose, and an example thereof is a rectangular shape having long and short sides. When the first polarizing plate 13 has a rectangular shape, it is preferable that the absorption axis direction of the first polarizer 131 of the first polarizing plate 13 is substantially parallel to the long or short side of the first polarizing plate 13. In this specification, the term "substantially parallel" refers not only to the case where the lines are strictly parallel, but also to the case where the angle between the lines is within ±10° (preferably ±5°).

[0038] [First polarizer] The thickness of the first polarizer 131 is not particularly limited, and an appropriate thickness can be adopted depending on the purpose. The thickness of the first polarizer 131 is typically about 1 μm to 80 μm. A thin polarizer may be used as the first polarizer 131. In this case, the thickness of the first polarizer 131 is preferably 20 μm or less, more preferably 15 μm or less, further preferably 10 μm or less, and particularly preferably 6 μm or less.

[0039] The first polarizer 131 preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is preferably 40.0% or more, more preferably 41.0% or more, even more preferably 42.0% or more, and particularly preferably 43.0% or more. The degree of polarization of the first polarizer 131 is preferably 99.8% or more, more preferably 99.9% or more, and even more preferably 99.95% or more.

[0040] The first polarizer 131 is preferably an iodine-based polarizer. More specifically, the polarizer can be made of a polyvinyl alcohol-based resin (hereinafter, referred to as a "PVA-based resin") film containing iodine.

[0041] The PVA-based resin that forms the PVA-based resin film is not particularly limited, and an appropriate resin can be used depending on the purpose. Examples of the resin include polyvinyl alcohol and ethylene-vinyl alcohol copolymer.

[0042] Polyvinyl alcohol is obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymer is obtained by saponifying ethylene-vinyl acetate copolymer. The saponification degree of the PVA resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, and more preferably 99.0 mol% to 99.93 mol%. The saponification degree is determined in accordance with JIS K 6726-1994. By using a PVA resin having such a saponification degree, a polarizer having excellent durability can be obtained. If the saponification degree is too high, gelation may occur.

[0043] The average degree of polymerization of the PVA-based resin is not particularly limited and can be appropriately selected depending on the purpose. The average degree of polymerization of the PVA-based resin is, for example, 1000 to 10000, preferably 1200 to 5000, and more preferably 1500 to 4500. The average degree of polymerization is determined in accordance with JIS K 6726-1994.

[0044] Examples of the method for producing the first polarizer 131 include a method (I) in which a PVA-based resin film alone is stretched and dyed, and a method (II) in which a laminate (i) having a resin substrate and a polyvinyl alcohol-based resin layer is stretched and dyed, etc. The method (I) is a well-known and commonly used method in the art, and therefore a detailed description thereof will be omitted.

[0045] The method (II) preferably includes a step of stretching and dyeing a laminate (i) having a resin substrate and a polyvinyl alcohol-based resin layer formed on one side of the resin substrate to produce a polarizer on the resin substrate. The laminate (i) can be formed by applying a coating liquid containing a polyvinyl alcohol-based resin onto a resin substrate and drying the coating liquid. Alternatively, the laminate (i) may be formed by transferring a polyvinyl alcohol-based resin layer onto the resin substrate. Details of the above-mentioned manufacturing method (II) are described, for example, in JP 2012-73580 A, which is incorporated herein by reference.

[0046] [First protective film] There is no particular limitation on the first protective film 132, and an appropriate resin film can be used depending on the purpose. Examples of materials for forming the first protective film 132 include polyester-based resins such as polyethylene terephthalate (PET), cellulose-based resins such as triacetyl cellulose (TAC), cycloolefin-based resins such as norbornene-based resins, olefin-based resins such as polyethylene and polypropylene, and (meth)acrylic resins. Among these, polyethylene terephthalate (PET) is preferable. Note that "(meth)acrylic resin" refers to acrylic resin and / or methacrylic resin.

[0047] As the (meth)acrylic resin, for example, a (meth)acrylic resin having a glutarimide structure is used. The (meth)acrylic resin having a glutarimide structure (hereinafter also referred to as glutarimide resin) is described in, for example, JP 2006-309033 A, JP 2006-317560 A, JP 2006-328329 A, JP 2006-328334 A, JP 2006-337491 A, JP 2006-337492 A, JP 2006-337493 A, JP 2006-337569 A, JP 2007-009182 A, JP 2009-161744 A, and JP 2010-284840 A. These descriptions are incorporated herein by reference.

[0048] The first protective film 132 and the first polarizer 131 can be laminated via any appropriate adhesive layer. The resin base material used in producing the first polarizer 131 is peeled off before or after the first protective film 132 and the first polarizer 131 are laminated.

[0049] The thickness of the first protective film 132 is preferably 4 μm to 250 μm, more preferably 5 μm to 150 μm, still more preferably 10 μm to 100 μm, and particularly preferably 10 μm to 50 μm.

[0050] The elastic modulus of the first protective film 132 is 1 GPa or more, preferably 1 GPa to 10 GPa, more preferably 1.8 GPa to 7 GPa, and even more preferably 2 GPa to 5 GPa. Within such a range, the first optical film 10 having excellent puncture resistance can be obtained.

[0051] [First retardation layer] The first retardation layer 14 is not particularly limited and may have any suitable optical and / or mechanical properties depending on the purpose. The first retardation layer 14 typically has a slow axis. The optical and / or mechanical properties of the first retardation layer 14 can be appropriately selected depending on the alignment mode of the liquid crystal cell.

[0052] The first retardation layer 14 may exhibit an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the retardation value hardly changes depending on the wavelength of the measurement light.

[0053] The thickness of the first retardation layer 14 is preferably 60 μm or less, more preferably 30 μm to 55 μm, and further preferably 30 μm or less.

[0054] The first retardation layer 14 can be made of any appropriate resin film that can satisfy the above characteristics. Representative examples of such resins include cyclic olefin resins, polycarbonate resins, cellulose resins, polyester resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyether resins, polystyrene resins, acrylic resins, and polymer liquid crystal resins.

[0055] [First adhesive layer] The first adhesive layer 18 can be formed from any appropriate adhesive. For example, adhesives having an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyether, a fluorine-based polymer, a rubber-based polymer, or the like as a base polymer are used. An acrylic adhesive is preferably used. This is because an acrylic adhesive has excellent optical transparency and exhibits adhesive properties such as appropriate wettability, cohesion, and adhesion, and can have excellent weather resistance, heat resistance, and the like. In particular, an acrylic adhesive made of an acrylic polymer having 4 to 12 carbon atoms is preferred.

[0056] The first pressure-sensitive adhesive layer 18 is formed from the pressure-sensitive adhesive. The thickness of the first pressure-sensitive adhesive layer 18 is not particularly limited, and is, for example, about 1 to 400 μm. The thickness of the first pressure-sensitive adhesive layer 18 can be appropriately set in a preferred range depending on the manufacturing method of the (meth)acrylic polymer used for the pressure-sensitive adhesive. For example, when the (meth)acrylic polymer is manufactured by solution polymerization or the like, the thickness of the first pressure-sensitive adhesive layer 18 is preferably 1 to 100 μm, more preferably 2 to 50 μm, even more preferably 2 to 40 μm, and particularly preferably 5 to 35 μm. When the (meth)acrylic polymer is manufactured by radiation polymerization or the like, the thickness of the first pressure-sensitive adhesive layer 18 is preferably 50 to 400 μm, more preferably 75 to 300 μm, and even more preferably 100 to 200 μm.

[0057] When producing an acrylic polymer having such a thickness, solution polymerization is preferable.

[0058] [First release film] The first release film 19 can be formed of, for example, a polyethylene terephthalate (PET) resin. The thickness of the first release film 19 is preferably 5 μm to 200 μm, more preferably 10 μm to 100 μm, and even more preferably 30 μm to 50 μm. The first release film 19 is peeled off at the interface with the first pressure-sensitive adhesive layer 18 before the first optical film 10 is attached to an optical element such as a liquid crystal cell.

[0059] (Second Optical Film) The second optical film 20 preferably has a dimensional change of 0.5% or less, and more preferably 0% to 0.2%. The optical film set 1 combines the first optical film 10 including the first glass film 11 with the second optical film 20 exhibiting the above-mentioned dimensional change. Therefore, by disposing the first optical film 10 and the second optical film 20 on either side of the liquid crystal cell, respectively, an optical laminate (first optical film / liquid crystal cell / second optical film) with little warping can be obtained.

[0060] The dimensional change is the dimensional change rate (|length in the absorption axis direction before test X0-length in the absorption axis direction after test X1| / length in the absorption axis direction before test X0) x 100 when a rectangular sample having a length of X0 (e.g., 20 cm) in the absorption axis direction of the second polarizer 231 is left standing for 150 hours in an environment at a temperature of 80° C. The dimensional change can be measured by a two-axis planar measuring device, for example, Quick Vision (manufactured by Mitutoyo Corporation).

[0061] [Second release film] The second release film 29 can be formed of, for example, a polyethylene terephthalate (PET) resin. The thickness of the second release film 29 is preferably 5 μm to 200 μm, more preferably 10 μm to 100 μm, and even more preferably 30 μm to 50 μm. The second release film 29 is peeled off at the interface with the second pressure-sensitive adhesive layer 28 before the second optical film 20 is attached to an optical element such as a liquid crystal cell.

[0062] [Second adhesive layer] The second adhesive layer 28 can be formed from any suitable adhesive. The adhesive may be similar to the first adhesive layer 18 except for the thickness.

[0063] The thickness of the second pressure-sensitive adhesive layer 28 is 50 μm or more and 200 μm or less. If the thickness of the second pressure-sensitive adhesive layer 28 is 50 μm or more and 200 μm or less, the crack resistance of the first glass film 11 can be improved when the optical laminate 3 described below is formed. In particular, when the thickness of the first glass film 11 is 50 μm or more and 150 μm or less, the first glass film 11 is thin and easily cracked. Therefore, it is very significant to set the thickness of the second pressure-sensitive adhesive layer 28 to 50 μm or more and 200 μm or less to improve the crack resistance of the first glass film 11.

[0064] Radiation polymerization is suitable for producing an acrylic polymer having such a thickness.

[0065] [Second polarizing plate] The thickness of the second polarizing plate 23 is preferably 5 μm to 250 μm, more preferably 10 μm to 200 μm, further preferably 25 μm to 200 μm, and particularly preferably 25 μm to 100 μm.

[0066] The shape of the second polarizing plate 23 is not particularly limited and may be any suitable shape depending on the purpose, but an example thereof is a rectangular shape having long and short sides. When the second polarizing plate 23 has a rectangular shape, it is preferable that the absorption axis direction of the second polarizer 231 of the second polarizing plate 23 is approximately parallel to the long or short side of the second polarizing plate 23.

[0067] As an example of the relationship between the second polarizing plate 23 and the first polarizing plate 13, the absorption axis direction of the first polarizer 131 is approximately parallel to the short side of the first polarizing plate 13, and the absorption axis of the second polarizing plate 231 is approximately parallel to the long side of the second polarizing plate 23.

[0068] As another example of the relationship between the second polarizing plate 23 and the first polarizing plate 13, the absorption axis direction of the first polarizer 131 is approximately parallel to the long side of the first polarizing plate 13, and the absorption axis of the second polarizing plate 231 is approximately parallel to the short side of the second polarizing plate 23.

[0069] [Second polarizer] The thickness of the second polarizer 231 is 1 μm to 10 μm, and preferably 2 μm to 7 μm. Within this range, the second optical film 20 with little dimensional change can be obtained. By disposing the first optical film 10 and the second optical film 20 on both sides of the liquid crystal cell, respectively, an optical laminate (first optical film / liquid crystal cell / second optical film) with little warping can be obtained.

[0070] The single transmittance, material, manufacturing method, and the like of the second polarizer 231 can be exemplified by the same items as those of the first polarizer 131 described above.

[0071] [Second protective film] As the second protective film 232, for example, a protective film similar to the above-mentioned first protective film 132 is used.

[0072] [Second retardation layer] As the second retardation layer 24, for example, a retardation layer similar to the above-mentioned first retardation layer 14 is used.

[0073] [Optical layer] Examples of the optical layer 25 include an anti-reflection layer, an anti-glare layer, etc. The optical layer has a thickness of, for example, 1 μm to 200 μm.

[0074] In the optical film set 1, the first optical film 10 is a thin glass integrated polarizing plate including the first glass film 11, and therefore has high hardness. In addition, the first optical film 10 has the first polarizing plate 13 on one side of the first glass film 11, which can prevent damage to the first glass film 11 and provides excellent puncture resistance. Point compression applied to the surfaces of the first optical film 10 and the first glass film 11 can be effectively released to the first polarizing plate 13 side, resulting in excellent puncture resistance as described above.

[0075] The first optical film 10 functions as described above, but when constructing a liquid crystal panel, if the first optical film 10 is used as a viewing-side polarizing plate and a conventional polarizing plate is used on the back side, the laminate composed of the liquid crystal cell and the polarizing plate (first optical film 10 / liquid crystal cell / conventional polarizing plate) tends to be prone to warping.

[0076] On the other hand, by using an optical film set 1 including a first optical film 10 and a second optical film 20 and arranging the first optical film 10 and the second optical film 20 on either side of a liquid crystal cell, an optical laminate (first optical film 10 / liquid crystal cell / second optical film 20) with little warping can be obtained.

[0077] This effect is achieved by using the second optical film 20 as an optical film to be combined with the first optical film 10, which is equipped with the first glass film 11 and therefore has little dimensional change due to moist heat, thereby reducing the difference in dimensional change between the first optical film 10 and the second optical film 20.

[0078] As described below, the first optical film 10 is disposed on the viewing side of a liquid crystal cell and can function as a front plate of a liquid crystal panel. On the other hand, the second optical film 20 is disposed on the rear side of a liquid crystal cell. The viewing side refers to the side facing the viewer when a specific member is applied to an image display device. The rear side refers to the side opposite to the viewing side.

[0079] The optical film set 1 is preferably used in, for example, an in-cell type liquid crystal element. The in-cell type liquid crystal element is a liquid crystal element including a liquid crystal cell having a substrate with a built-in touch sensor, and the first optical film 10 is disposed, for example, on the viewing side of the liquid crystal cell, and the second optical film 20 is disposed, for example, on the back side of the liquid crystal cell. The optical film set 1 is also suitable for image display devices that require chemical resistance. In this case, in the optical film set 1, the first optical film 10 is used, for example, with the first glass film 11 facing outward.

[0080] Second Embodiment The second embodiment shows an example of an optical film set having a layer structure different from that of the first embodiment. Note that in the second embodiment, the description of the same components as those in the already described embodiments may be omitted.

[0081] Fig. 2 is a cross-sectional view illustrating an optical film set according to a second embodiment. Referring to Fig. 2, the optical film set 2 includes a first optical film 10 and a second optical film 20A. That is, the optical film set 2 differs from the optical film set 1 (see Fig. 1) in that the second optical film 20 is replaced with the second optical film 20A.

[0082] The second optical film 20A includes, in this order, a second release film 29, a second pressure-sensitive adhesive layer 28, a second retardation layer 24, a second polarizing plate 23, a second adhesive layer 22, a second glass film 21, and an optical layer 25. However, the second retardation layer 24 and the optical layer 25 are not essential components and are provided as necessary.

[0083] The elastic modulus of the second adhesive layer 22 is preferably 1 GPa or more, more preferably 1 GPa to 10 GPa, further preferably 2 GPa to 8 GPa, and particularly preferably 2 GPa to 5 GPa. Within such a range, dimensional changes can be suppressed while maintaining flexibility.

[0084] The material, thickness, and the like of the second adhesive layer 22 can be exemplified by the same items as those described above for the first adhesive layer 12.

[0085] The thickness of the second glass film 21 is preferably 20 μm to 150 μm, more preferably 40 μm to 130 μm, and further preferably 60 μm to 110 μm. Within such a range, the second optical film 20A having excellent flexibility can be obtained.

[0086] The second glass film 21 may be, for example, thinner than the first glass film 11. This is because the first glass film 11 is required to have a certain degree of strength since it is in direct contact with the outside, whereas the second glass film 21 only needs to be able to suppress dimensional changes in the resin and be processable by a roll-to-roll process.

[0087] The material, transmittance, refractive index, density, forming method, and the like of the second glass film 21 can be exemplified by the same items as those described above for the first glass film 11.

[0088] Thus, in the optical film set 2, the second optical film 20A has the second adhesive layer 22 and the second glass film 21 in addition to the configuration of the second optical film 20. By using the optical film set 2 including the first optical film 10 and the second optical film 20A and arranging the first optical film 10 and the second optical film 20A on both sides of the liquid crystal cell, respectively, an optical laminate (first optical film 10 / liquid crystal cell / second optical film 20A) with less warping can be obtained.

[0089] Similarly to the optical film set 1, the optical film set 2 is suitable for use in liquid crystal cells and image display devices that require chemical resistance. Third embodiment In the third embodiment, an example of an optical laminate having the optical film set according to the first embodiment will be described. Note that in the third embodiment, the description of the same components as those in the already described embodiments may be omitted.

[0090] Fig. 3 is a cross-sectional view illustrating an optical laminate according to a third embodiment. Referring to Fig. 3, the optical laminate 3 includes, in this order from the viewing side, a first optical film 10 from which a first release film 19 has been peeled off, a liquid crystal cell 30, and a second optical film 20 from which a second release film 29 has been peeled off.

[0091] That is, in the optical laminate 3, the first optical film 10 is laminated on the viewing side of the liquid crystal cell 30, and the second optical film 20 is laminated on the side opposite the viewing side of the liquid crystal cell 30 (rear side).

[0092] The first optical film 10 can be arranged, for example, from the viewing side, with a first glass film 11, a first adhesive layer 12, a first polarizing plate 13, a first retardation layer 14, and a first pressure-sensitive adhesive layer 18. The second optical film 20 can be arranged, for example, from the viewing side, with a second pressure-sensitive adhesive layer 28, a second retardation layer 24, a second polarizing plate 23, and an optical layer 25. However, as described above, the first retardation layer 14, the second retardation layer 24, and the optical layer 25 may be provided as necessary.

[0093] In this manner, the first optical film 10 and the second optical film 20 are disposed on either side of the liquid crystal cell 30, respectively, to obtain the optical laminate 3.

[0094] As described above, the thickness of the second pressure-sensitive adhesive layer 28 is 50 μm or more and 200 μm or less. This can improve the resistance to cracking of the first glass film 11 in the optical laminate 3. In particular, when the thickness of the first glass film 11 is 50 μm or more and 150 μm or less, the first glass film 11 is thin and easily cracked. Therefore, it is very significant to set the thickness of the second pressure-sensitive adhesive layer 28 to 50 μm or more and 200 μm or less to improve the resistance to cracking of the first glass film 11.

[0095] The optical laminate 3 is preferably configured so that the absorption axis of the first polarizer 131 and the absorption axis of the second polarizer 231 are substantially perpendicular to each other. With such a configuration, an optical laminate 3 that is less likely to warp can be obtained. Note that the term "substantially perpendicular" is a concept that includes not only the case where the axes are strictly perpendicular to each other, but also the case where the angle between the two lines is 90°±10° (preferably 90°±5°).

[0096] Fourth embodiment In the fourth embodiment, an example of an optical laminate having the optical film set according to the second embodiment is shown. Note that in the fourth embodiment, the description of the same components as those in the already described embodiments may be omitted.

[0097] Fig. 4 is a cross-sectional view illustrating an optical laminate according to a fourth embodiment. Referring to Fig. 4, the optical laminate 4 includes, in this order from the viewing side, a first optical film 10 from which a first release film 19 has been peeled off, a liquid crystal cell 30, and a second optical film 20A from which a second release film 29 has been peeled off.

[0098] That is, the optical laminate 4 differs from the optical laminate 3 (see FIG. 3) in that the second optical film 20 is replaced with a second optical film 20A.

[0099] The first optical film 10 can be arranged, for example, in the order from the viewing side, of the first glass film 11, the first adhesive layer 12, the first polarizing plate 13, the first retardation layer 14, and the first pressure-sensitive adhesive layer 18. The second optical film 20A can be arranged, for example, in the order from the viewing side, of the second adhesive layer 28, the second retardation layer 24, the second polarizing plate 23, the second adhesive layer 22, the second glass film 21, and the optical layer 25. However, as described above, the first retardation layer 14, the second retardation layer 24, and the optical layer 25 may be provided as necessary.

[0100] In this manner, the first optical film 10 and the second optical film 20A are disposed on either side of the liquid crystal cell 30, respectively, to obtain the optical laminate 4.

[0101] As described above, the thickness of the second pressure-sensitive adhesive layer 28 is 50 μm or more and 200 μm or less. This can improve the resistance to cracking of the first glass film 11 in the optical laminate 4. In particular, when the thickness of the first glass film 11 is 50 μm or more and 150 μm or less, the first glass film 11 is thin and easily cracked. Therefore, it is very significant to set the thickness of the second pressure-sensitive adhesive layer 28 to 50 μm or more and 200 μm or less to improve the resistance to cracking of the first glass film 11.

[0102] In addition, the optical laminate 4 is preferably configured so that the absorption axis of the first polarizer 131 and the absorption axis of the second polarizer 231 are substantially perpendicular to each other. With such a configuration, an optical laminate 4 that is less likely to warp can be obtained.

[0103] [Example] The optical film set and the optical laminate will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0104] [Manufacturing Example 1] Preparation of Polarizing Plate A A 100 μm thick polyvinyl alcohol film (PVA) was stretched to 3 times while dyeing in a 0.3% concentration iodine solution at 30° C. for 1 minute between rolls with different speed ratios. Then, the film was stretched to 6 times the total stretch ratio while immersing in an aqueous solution containing 4% concentration boric acid and 10% concentration potassium iodide at 60° C. for 0.5 minutes. Next, the film was washed by immersing in an aqueous solution containing 1.5% concentration potassium iodide at 30° C. for 10 seconds, and then dried at 50° C. for 4 minutes to obtain a polarizer with a thickness of 28 μm. A saponified triacetyl cellulose film (TAC) with a thickness of 40 μm and a modulus of elasticity of 3.6 GPa was attached to one side of the polarizer, and an acrylic resin film with a thickness of 30 μm and a modulus of elasticity of 2.5 GPa was attached to the other side of the polarizer with a polyvinyl alcohol adhesive, respectively, to obtain a polarizing plate A (thickness: 98 μm).

[0105] [Manufacturing Example 2] Preparation of Polarizing Plate B (Preparation of polarizer) First, a laminate having a 9 μm-thick PVA layer formed on an amorphous PET substrate was subjected to an air-assisted stretching at a stretching temperature of 130° C. to produce a stretched laminate. Next, the stretched laminate was dyed to produce a colored laminate, and the colored laminate was further stretched in boric acid water at a stretching temperature of 65° C. to produce an optical film laminate including a 4 μm-thick PVA layer stretched integrally with the amorphous PET substrate to a total stretch ratio of 5.94 times.

[0106] This two-stage stretching process enabled the production of an optical film laminate including a 4 μm-thick PVA layer that constitutes a high-performance polarizer in which the PVA molecules in the PVA layer formed on the amorphous PET substrate were highly oriented in one direction, and the iodine adsorbed by dyeing was highly oriented in one direction as a polyiodine ion complex.

[0107] (Preparation of acrylic film) Methacrylic resin pellets having glutarimide ring units were dried at 100.5 kPa and 100° C. for 12 hours, and extruded from a T-die of a single-screw extruder at a die temperature of 270° C. to form a film. This film was stretched in the conveying direction (MD) in an atmosphere 10° C. higher than the Tg of the resin, and then stretched in the direction perpendicular to the film conveying direction (TD) in an atmosphere 7° C. higher than the Tg of the resin, to obtain an acrylic film with a thickness of 40 μm and an elastic modulus of 2.5 GPa.

[0108] (Preparing the curing adhesive) A curable adhesive was obtained by mixing 35 parts by weight of N-hydroxyethylacrylamide HEAA (manufactured by Kojinsha), 45 parts by weight of N-acryloylmorpholine ACMO (manufactured by Kojinsha), 25 parts by weight of polypropylene glycol diacrylate TPGDA (manufactured by Toa Goseisha, product name Aronix M-220), 3 parts by weight of a photopolymerization initiator (manufactured by Chiba Specialty Chemicals, product name Irgacure 184), and 1.5 parts by weight of another photopolymerization initiator (manufactured by Nippon Kayakusha, product name KAYACUREDETX-S).

[0109] (Preparation of polarizing plate) The above-mentioned curable adhesive was applied to the polarizer prepared on the PET film to a thickness of about 1 μm. Then, the above-mentioned 40 μm acrylic film was laminated to the adhesive layer. The adhesive was cured by irradiating ultraviolet rays from the PET film side using a conveyor-type UV irradiation device (manufactured by Fusion Co., Ltd.) with a peak UV illuminance of 1600 mW / cm2 and an accumulated UV light amount of 1000 mJ / cm2 (wavelength 380 to 440 nm), and was further dried at 70 ° C for 2 minutes. Finally, the PET film was peeled off from the laminate in which the acrylic film, polarizer, and PET film were laminated to obtain a laminate of the acrylic film (protective film) and the polarizer (polarizing plate B with a thickness of 44 μm).

[0110] [Production Example 3] Preparation of adhesive (Preparation of Acrylic Polymer) In a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser, 100 parts by weight of butyl acrylate, 5 parts by weight of acrylic acid, 0.075 parts by weight of 2-hydroxyethyl acrylate, 0.2 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator, and 200 parts by weight of ethyl acetate as a polymerization solvent were charged, and after sufficient nitrogen replacement, the liquid temperature in the flask was kept at around 55°C while stirring under a nitrogen stream for 10 hours to prepare an acrylic polymer solution. The weight average molecular weight of the acrylic polymer was 2.2 million.

[0111] (Preparation of Pressure-Sensitive Adhesive Composition) 100 parts by weight of the solid content of the acrylic polymer solution was mixed and stirred uniformly with 0.2 parts by weight of dibenzoyl peroxide (Niper BMT, manufactured by Nippon Oil & Fats Co., Ltd.) as a peroxide, 0.05 parts by weight of diglycidylaminomethylcyclohexane (Tetrad C, manufactured by Mitsubishi Gas Chemical Co., Ltd.) as an epoxy crosslinking agent, 0.1 parts by weight of an adduct of trimethylolpropane / tolylene diisocyanate (Coronate L, manufactured by Nippon Polyurethane Industry Co., Ltd.) as an isocyanate crosslinking agent, and 0.075 parts by weight of a silane coupling agent (KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.) to prepare an acrylic adhesive (solid content 10.9% by weight).

[0112] [Production Example 4] Preparation of adhesive (Preparation of monomer components for UV polymerization) A monomer mixture was prepared by adding 61 parts by weight of 2-ethylhexyl acrylate (2EHA), 14 parts by weight of N-vinyl-2-pyrrolidone (NVP), 0.05 parts by weight of two kinds of photopolymerization initiators (trade name: Irgacure 184, manufactured by BASF) and 0.05 parts by weight of a photopolymerization initiator (trade name: Irgacure 651, manufactured by BASF) to a four-neck flask. The monomer mixture was then partially photopolymerized by exposing it to ultraviolet light under a nitrogen atmosphere to obtain a partially polymerized product (acrylic polymer syrup) with a polymerization rate of about 10% by weight.

[0113] To the total amount (75.1 parts by weight) of the obtained acrylic polymer syrup, 3 parts by weight of 2-hydroxyethyl acrylate (2HEA), 22 parts by weight of 4-hydroxybutyl acrylate (HBA), and 0.06 parts by weight of dipentaerythritol pentaacrylate (product name "KAYARAD DPHA", manufactured by Nippon Kayaku Co., Ltd.) were added, and then these were mixed uniformly to prepare a monomer component.

[0114] [Production Example 5] Preparation of adhesive (Preparing the epoxy adhesive) An epoxy adhesive was prepared by mixing 70 parts by weight of Celloxide 2021P (manufactured by Daicel Chemical Industries, Ltd.), 5 parts by weight of EHPE3150, 19 parts by weight of Aron Oxetane OXT-221 (manufactured by Toa Gosei Co., Ltd.), 4 parts by weight of KBM-403 (manufactured by Shin-Etsu Chemical Co., Ltd.), and 2 parts by weight of CPI101A (manufactured by San-Afro Co., Ltd.). [Example 1] (Preparation of First Optical Film A) A glass film (manufactured by Nippon Electric Glass Co., Ltd., product name "OA-10G", thickness: 100 μm) and the polarizing plate A produced in Production Example 1 were bonded together via an adhesive layer made of the adhesive prepared in Production Example 5. At this time, the polarizing plate A was placed so that the acrylic film was on the glass film side. Next, the adhesive layer was irradiated with ultraviolet light (500 mJ / cm 2 ) from a high-pressure mercury lamp. 2 ) and the adhesive layer was cured to obtain a first optical film A. The adhesive layer had a thickness of 5 μm and an elastic modulus of 1.8 GPa. (Preparation of Second Optical Film A) The polarizing plate B produced in Production Example 2 was prepared as a second optical film B. (Preparation of Laminate A for Evaluation) A glass plate (13.3 inches, 296 mm x 168 mm, thickness: 0.4 mm) was prepared to serve as a glass cell.

[0115] The first optical film A was cut to a size of 295 mm×163 mm such that the absorption axis direction of the polarizer was parallel to the short side.

[0116] The second optical film B was cut to a size of 295 mm×163 mm such that the absorption axis direction of the polarizer was parallel to the long side.

[0117] The first optical film A was laminated on one surface of the above glass plate such that the short sides of the glass plate and the first optical film A were parallel to each other and the polarizing plate A (polarizer) was on the glass plate side.

[0118] The second optical film B was laminated on the other surface of the above glass plate such that the short sides of the glass plate and the second optical film A were parallel to each other and the polarizer was on the glass plate side.

[0119] The first optical film A was laminated on a glass plate via an adhesive layer (thickness: 20 μm) composed of the adhesive prepared in Production Example 3. This adhesive layer was formed as follows: (i) it was applied onto a silicone-treated polyethylene terephthalate film (manufactured by Mitsubishi Chemical Polyester Film Corporation, thickness: 38 μm) and heated at 155° C. for 1 minute to form an adhesive layer having a thickness of 20 μm after drying, and (ii) the adhesive layer was transferred from the polyethylene terephthalate film to the polarizing plate A to form an adhesive layer.

[0120] The second optical film B was laminated on a glass plate via an adhesive layer (thickness 50 μm) composed of the adhesive prepared in Production Example 4. The adhesive layer was formed by applying the monomer component prepared in Production Example 4 and the release-treated surface of a polyester film (trade name: Diafoil MRF, manufactured by Mitsubishi Plastics, Inc.) having a thickness of 38 μm, one side of which had been subjected to a release treatment with silicone, to a final thickness of 100 μm to form a coating layer. Next, the surface of the applied monomer component was covered with a polyester film (trade name: Diafoil MRE, manufactured by Mitsubishi Plastics, Inc.) having a thickness of 38 μm, one side of which had been subjected to a release treatment with silicone, so that the release-treated surface of the film was on the coating layer side. This blocked the coating layer of the monomer component from oxygen. The sheet having the coating layer thus obtained was irradiated with a chemical light lamp (manufactured by Toshiba Corporation) at an illuminance of 5 mW / cm. 2 The adhesive layer was cured by irradiating it with ultraviolet light (measured with a Topcon UVR-T1 with maximum sensitivity at about 350 nm) for 360 seconds to form an adhesive layer, and an adhesive sheet was produced. The polyester film coated on both sides of the adhesive layer functions as a release film.

[0121] Next, the polyester film on one side was peeled off and laminated onto optical film B, and then the other polyester film was peeled off.

[0122] In the manner described above, a laminate A for evaluation was prepared.

[0123] [Example 2] A laminate B for evaluation was produced in the same manner as in Example 1, except that the pressure-sensitive adhesive layer composed of the pressure-sensitive adhesive prepared in Production Example 4 had a thickness of 150 μm.

[0124] [Example 3] A laminate C for evaluation was produced in the same manner as in Example 1, except that the pressure-sensitive adhesive layer composed of the pressure-sensitive adhesive prepared in Production Example 4 had a thickness of 200 μm.

[0125] [Example 4] A laminate D for evaluation was produced in the same manner as in Example 1, except that the thickness of the glass film was 50 μm.

[0126] [Example 5] A laminate E for evaluation was produced in the same manner as in Example 1, except that the glass film had a thickness of 50 μm and the pressure-sensitive adhesive layer composed of the pressure-sensitive adhesive prepared in Production Example 4 had a thickness of 150 μm.

[0127] [Example 6] A laminate F for evaluation was produced in the same manner as in Example 1, except that the glass film had a thickness of 50 μm and the pressure-sensitive adhesive layer composed of the pressure-sensitive adhesive prepared in Production Example 4 had a thickness of 200 μm.

[0128] [Comparative Example 1] The second optical film B was laminated on a glass plate via an adhesive layer (thickness: 20 μm) composed of the adhesive prepared in Production Example 3. The adhesive layer was formed as follows: (i) the adhesive was applied onto a silicone-treated polyethylene terephthalate film (manufactured by Mitsubishi Chemical Polyester Film Corporation, thickness: 38 μm) and heated at 155° C. for 1 minute to form an adhesive layer having a thickness of 20 μm after drying, and (ii) the adhesive layer was transferred from the polyethylene terephthalate film to the optical film B to form an adhesive layer. Except for this, the evaluation laminate G was produced in the same manner as in Example 1.

[0129] [Comparative Example 2] Evaluation laminate H was prepared in the same manner as in Example 1, except that the glass film was 50 μm thick and the adhesive layer used in the second optical film B was an adhesive layer (thickness 20 μm) composed of the adhesive prepared in Manufacturing Example 3.

[0130] [Comparative Example 3] A laminate I for evaluation was produced in the same manner as in Example 1, except that the pressure-sensitive adhesive layer composed of the pressure-sensitive adhesive prepared in Production Example 4 had a thickness of 250 μm.

[0131] (evaluation) The evaluation laminates obtained in Examples 1 to 6 and Comparative Examples 1 to 3 were subjected to a ball drop test.

[0132] 5, the ball drop test is a test in which an evaluation laminate S (a collective term for evaluation laminates A to I) is placed on a 10 mm-thick glass plate 820 placed on a measurement table 810, and a 130 g iron ball B is dropped vertically onto the evaluation laminate S from a height L to measure the height L at which the glass film of the evaluation laminate S breaks. The evaluation laminate S was placed on the glass plate 820 with the second optical film B facing the glass plate 820.

[0133] The ball drop test was performed three times for each of the evaluation laminates A to I, and the height L at which the glass film broke was calculated as an average of the three measurements. If the average of the three measurements was less than 17 mm, it was evaluated as × (fail), if it was 17 mm or more and less than 34 mm, it was evaluated as ◯ (pass), and if it was 34 mm or more, it was evaluated as ⊚ (pass). These criteria were set based on the inventors' experience. The results of the ball drop test are shown in Figs. 6 and 7. The maximum height L was set to 100 mm, and tests beyond this were not performed.

[0134] As shown in Figures 6 and 7, it was found that the pass / fail result of the ball drop test depends greatly on the thickness of the adhesive layer on the B side of the second optical film (the adhesive layer made of the adhesive prepared in Production Example 4), and the influence of the thicknesses of the other layers is small. It was also found that the adhesive layer on the B side of the second optical film should not be too thin or too thick, and that there is an optimum value (50 µm or more and 200 µm or less). These were facts that were not known before and were newly discovered by the inventors.

[0135] Thus, it was confirmed that when the thickness of the pressure-sensitive adhesive layer on the second optical film B side is 50 μm or more and 200 μm or less, cracking of the glass film can be prevented regardless of whether the thickness of the glass film is 50 μm or 100 μm.

[0136] Although the preferred embodiments have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims.

[0137] For example, in the optical laminate 3 etc., the liquid crystal cell 30 is exemplified, but an organic EL (Organic Electro-Luminescence) cell, a micro LED (Light Emitting Diode) cell, etc. may be used instead of the liquid crystal cell 30. For example, in the case of an optical laminate including an organic EL cell, an anti-reflection film (for anti-glare or anti-glare) may be provided instead of the first polarizing plate 13, and a base material made of resin may be provided instead of the second polarizing plate 23.

[0138] This international application claims priority based on Japanese Patent Application No. 2019-066163, filed on March 29, 2019, the entire contents of which are incorporated herein by reference. [Explanation of symbols]

[0139] 1, 2 Optical film set 3, 4 Optical laminate 10 First Optical Film 11 First Glass Film 12 First adhesive layer 13 First polarizing plate 14 First retardation layer 18 First adhesive layer 19 First release film 20, 20A Second optical film 21 Second Glass Film 22 Second adhesive layer 23 Second polarizing plate 24 Second retardation layer 25 Optical layer 28 Second adhesive layer 29 Second release film 30 Liquid crystal cell 131 First polarizer 132 First protective film 231 Second Polarizer 232 Second Protective Film

Claims

1. a first optical film including a first pressure-sensitive adhesive layer and disposed on a viewing side of an optical element via the first pressure-sensitive adhesive layer; a second optical film provided with a second pressure-sensitive adhesive layer and disposed on a back surface side of the optical element via the second pressure-sensitive adhesive layer; a first glass film having a thickness of 50 μm or more and 150 μm or less is provided on the viewing side surface of the first optical film; The optical film set, wherein the thickness of the second pressure-sensitive adhesive layer is 50 μm or more and 200 μm or less.

2. the first optical film comprises a first adhesive layer, and a first polarizing plate having a first polarizer and a first protective film, which are sequentially arranged on the optical element side of the first glass film; The optical film set of claim 1 , wherein the second optical film comprises a second polarizing plate having a second polarizer.

3. The optical film set according to claim 2 , wherein the first protective film is disposed on a side of the first polarizer facing the first adhesive layer.

4. The optical film set according to claim 2 , wherein the first optical film further comprises a first retardation layer.

5. The optical film set according to claim 4 , wherein the first retardation layer is disposed on a side of the first polarizing plate opposite the first adhesive layer.

6. The optical film set of claim 2 , wherein the second optical film comprises a second adhesive layer and a second glass film arranged in sequence on the side of the second polarizing plate opposite the optical element.

7. The optical film set of claim 6 , wherein the second optical film comprises an optical layer disposed on an opposite side of the second glass film from the second adhesive layer.

8. The optical film set according to claim 2 , wherein the second optical film further comprises a second retardation layer.

9. The optical film set of claim 6 , wherein the second optical film further comprises an optical layer disposed on at least one side of the second polarizer.

10. the first polarizing plate has a rectangular shape having long sides and short sides, The optical film set according to claim 2 , wherein an angle between an absorption axis direction of the first polarizer and the short side of the first polarizer is within a range of ±10°.

11. the second polarizing plate has a rectangular shape having long sides and short sides, The optical film set according to claim 10 , wherein an angle between the absorption axis direction of the second polarizer and the long side of the second polarizer is within a range of ±10°.

12. the first polarizing plate has a rectangular shape having long sides and short sides, The optical film set according to claim 2 , wherein an angle between an absorption axis direction of the first polarizer and the long side of the first polarizer is within a range of ±10°.

13. the second polarizing plate has a rectangular shape having long sides and short sides, The optical film set according to claim 12 , wherein an angle between the absorption axis direction of the second polarizer and the short side of the second polarizer is within a range of ±10°.

14. 14. An optical laminate comprising, in this order from the viewing side, the first optical film of the optical film set described in any one of claims 1 to 13, an optical element, and the second optical film of the optical film set described in any one of claims 1 to 13.

15. The optical laminate according to claim 14 , wherein the optical element is an in-cell type liquid crystal element.

16. The optical laminate according to claim 14, which is used in an image display device that requires chemical resistance.

Citation Information

Patent Citations

  • Adhesive layer, optical film, and image display device

    JP2016148848A

  • Polarizing plate, fabrication method for polarizing plate, and image display device

    WO2013175767A1

  • Polarizing film with double-sided adhesive layers and image display device

    WO2017216886A1

  • Polarization plate set, liquid crystal display panel, and liquid crystal display device

    WO2018016216A1

  • Organic el display device

    WO2018062183A1