Fully coated gloves with moisture absorbing and sweat absorbing properties
The fully coated glove integrates a polyurethane-based moisture-absorbing ventilation layer and barrier layer to address sweat and bacterial issues, ensuring effective moisture absorption and ventilation for enhanced comfort and safety.
Patent Information
- Application Number
- JP2023518261
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-27
- Filing Date
- 2022-01-06
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2042-01-06
AI Technical Summary
Existing fully coated gloves lack moisture absorption and ventilation functions, leading to discomfort and increased risk of bacterial growth due to sweat accumulation, especially in humid environments.
A fully coated glove design featuring a moisture-absorbing ventilation layer and a barrier layer, both made from polyurethane-based coatings, with the moisture-absorbing layer being foam-coated and the barrier layer non-foamed, utilizing hydrophilic groups and micropores for sweat absorption and bacterial prevention.
The glove provides effective moisture absorption and ventilation, reducing sweat-related discomfort and bacterial risk while maintaining a breathable and protective barrier, enhancing user comfort and safety.
Smart Images

Figure 0007554350000001
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of labor protection equipment, and more particularly to a fully coated glove having moisture absorbing and sweat absorbing functions. [Background technology]
[0002] As we all know, in modern industrial production, safety protection is quite important, and wearing protective gloves is one important component of safety protection. Currently, there are two types of coated safety gloves on the market: full-coated and unlined. Unlined coated labor protective gloves are mainly coated with butyronitrile, natural latex, PVC and polyurethane. Wearing such gloves provides protection, but the back of the hand is not coated, so they are ineffective against the intrusion of liquids and bacteria from the outside. When the working environment is humid, there is oil stains such as lubricating oil, or when touching medical waste, there is a risk of bacteria or viruses invading, it is necessary to apply a coating that firmly blocks and isolates the hands from the outside world, and unlined coated gloves are obviously not suitable, and full-coated gloves should be worn. The main raw materials of the coating of fully coated gloves are butyronitrile, natural latex and PVC. Since it is necessary to block the intrusion of external liquids and bacteria, all such products on the market at present do not have the function of absorbing moisture and breathing, and are hard to the touch, which makes wearing them very uncomfortable. After long-term use, the skin of the hands will become soaked in sweat, which makes the skin prone to wrinkles, and also makes it easy for bacteria to grow, and also increases the fatigue intensity of the work. Summary of the Invention [Problem to be solved by the invention]
[0003] An object of the present invention is to provide a fully coated glove having moisture absorbing and sweat absorbing properties. [Means for solving the problem]
[0004] After conducting research, the inventors have found the following principle of waterproofing and moisture absorption and ventilation of coatings. There are two types of moisture absorption and ventilation methods for films, one is the non-porous hydrophilic method. Water molecules are composed of one oxygen atom and two hydrogen atoms. When water molecules are in gas form, there is almost no force between the molecules, and the water molecules can move freely. When the water molecules in the barrier layer come into contact with the film in gas form, the hydrophilic groups contained in the film adsorb the water molecules, which are then conducted from the high concentration inner layer to the low concentration outer layer through the molecular chain, and then volatilized into the air, completing the complete process of adsorption, migration and desorption. At this time, the barrier layer generates a moisture absorption and ventilation phenomenon, and the difference in concentration and temperature between the water molecules inside and outside the barrier layer is a factor that affects the conduction speed, and the greater the difference, the faster the conduction speed. However, when the water molecules are in liquid form, the binding force between the molecules is relatively large, and there are both van der Waals forces and hydrogen bonds, so the hydrophilic groups in the film are in contact with the liquid water, but the adsorption force between the barrier layer and the water molecules is smaller than the binding force between the water molecules, so the liquid water cannot be transmitted to the other side through the barrier layer, and at this time, the barrier layer plays a waterproofing role. In addition, since the barrier layer is designed without holes, bacteria and viruses cannot pass through the barrier layer, which is the mechanism of the barrier layer that is breathable while being waterproof and anti-virus. The second method of moisture absorption and ventilation of the film is through micropores, and the moisture absorption and ventilation layer of the present invention adopts this method. When the wearer's hand sweats, the volume of the water molecules in gas form is much smaller than the pore size of the micropores, so they can freely contact the barrier layer through the moisture absorption and ventilation layer and can further diffuse to the outside of the glove through the barrier layer. At this time, if the amount of gas generated by sweat is greater than the diffusion speed of the barrier layer, the micropore type moisture absorption and ventilation coating can temporarily adsorb and store the excess gas generated by sweat. In addition, the moisture-absorbing and breathable coating of the present invention itself contains hydrophilic groups, and therefore combines microporous hydrophobicity with hydrophilic moisture absorption function, thereby minimizing or eliminating the stuffy and wet feeling on the hands caused by gas due to sweat.
[0005] According to the above principle, the key is the hydrophilicity and number of micropores of the coating that comes into contact with the skin.The raw materials of the currently available full-coated products are butyronitrile and PVC.When analyzed from the structure of these two raw materials, they have relatively poor hydrophilicity, especially PVC material does not have hydrophilicity.When analyzed from the processing process, these two materials also do not have a foaming process and a foaming step, so the full-coated gloves produced by using these two raw materials have insufficient hydrophilicity and micropores, and even no hydrophilicity and micropores, so that the gloves have no moisture absorption effect and are hard to the touch.
[0006] The present invention uses polyurethane as the raw material for the inner layer, and successfully solves the problems of hydrophilicity and moisture absorption and sweat absorption from the chemical composition and physical structure. First, in terms of chemical composition, polyurethane raw materials currently available on the market are of two types: solvent-based and water-based, and both types contain a certain number of carboxyl, hydroxyl, or amino groups, which are hydrophilic groups that can strongly adsorb gaseous water molecules. In terms of physical structure, for solvent-based polyurethane, a large number of fine pores are formed in the polyurethane film formed by the exchange of solvent and water during the water washing film formation process after dipping, but for water-based polyurethane, a processing process is adopted in which physical foaming is performed before molding, and a large number of fine bubbles are contained in the water-based polyurethane. These fine bubbles have two advantages. The first is that they greatly increase the specific surface area of the coating, that is, increase the contact area between the water molecules and the hydrophilic material. Thus, during the use of the gloves, sweat in gas form can be maximally contacted and adsorbed by the hydrophilic groups of the coating, and can be further led to the outside of the glove through the barrier layer. If sweat is generated faster than it can be discharged, the excess sweat is sucked in by the numerous fine pore capillaries, and is held by the coating and fibers, and is mechanically held in the capillaries between the fibers. The second is that the flexibility of the coating is greatly improved due to the large number of fine pores. This is a fairly important indicator in the actual use process of the gloves, and soft gloves can reduce the fatigue of the hands during work, and can reduce the labor intensity to the maximum extent.
[0007] The present invention is achieved by the following technical solutions:
[0008] The fully coated glove having moisture absorbing and sweat absorbing function includes a knitted glove body, a moisture absorbing and breathable layer dip-coated on the entire inner surface of the glove body, and a barrier layer dip-coated on the entire outer surface of the glove body. The moisture absorbing and sweat absorbing layer and the barrier layer are both manufactured with a paint containing water-based polyurethane or solvent-based polyurethane as the main raw material. The moisture absorbing and sweat absorbing layer is a foamed layer with a thickness of 0.1 to 0.3 mm, and the barrier layer is a non-foamed layer with a thickness of 0.03 to 0.2 mm. The specific manufacturing process of the fully coated glove is as follows: the first layer of the moisture-absorbing and breathable layer has already been cured and baked to form a film, and the surface energy of the barrier layer paint in a liquid state is lower than the surface energy of the moisture-absorbing and breathable layer, so that when the second layer of the barrier layer is dip-coated, the barrier coating material is maximally infiltrated into the surface of the moisture-absorbing and breathable layer and even into the micropores of the surface layer. The low surface energy allows the barrier coating material to maximally infiltrate into the surface of the moisture-absorbing and breathable layer, and even into the micropores in the surface layer, and is adsorbed onto the moisture-absorbing and breathable layer through sufficient interfacial contact. During the subsequent heating process, the dipping material molecules of the barrier layer will bond tightly with the molecules of the moisture-absorbing and breathable layer through the action of Brownian motion, and the two-layer coating will form a stable state through the joint action of van der Waals forces and hydrogen bonds. Therefore, strictly controlling the surface energy of the barrier layer is the key to ensuring high adhesive strength of the two-layer coating.
[0009] Preferably, to achieve a thickness of the blocking layer of 0.03 to 0.2 mm, when the manufacturing material for the blocking layer mainly contains water-based polyurethane resin, the solids content of the paint is controlled to be 20 to 40% and the viscosity is controlled to be between 500 to 2000 centipoise, and when the manufacturing material for the blocking layer mainly contains solvent-based polyurethane resin, the solids content of the paint is controlled to be 12 to 20% and the viscosity is controlled to be between 300 to 1500 centipoise.
[0010] More preferably, when the manufacturing material of the blocking layer mainly comprises an aqueous polyurethane resin, the manufacturing raw material comprises, as components, an aqueous polyurethane emulsion, a defoamer, a thickener, a hardener, and a wetting agent; When the preparation material of the blocking layer mainly comprises a solvent-based polyurethane resin, the preparation raw material comprises, as ingredients, a dry polyurethane resin, DMF, a defoaming agent, a leveling agent, a penetrating agent, and a wetting agent.
[0011] Furthermore, when the production material of the blocking layer mainly contains an aqueous polyurethane resin, the production raw material contains, as components, 1000 parts by mass of an aqueous polyurethane emulsion, 4 to 7 parts by mass of an antifoaming agent, 3 to 8 parts by mass of a thickener, 10 to 30 parts by mass of a curing agent, and 2 to 5 parts by mass of a wetting agent; when the production material of the blocking layer mainly contains a solvent-based polyurethane resin, the production raw material contains, as components, 1000 parts by mass of a dry polyurethane resin, 800 to 2000 parts by mass of DMF, 3 to 10 parts by mass of an antifoaming agent, 3 to 8 parts by mass of a leveling agent, 3 to 8 parts by mass of a penetrating agent, and 2 to 5 parts by mass of a wetting agent.
[0012] Preferably, in order to make the thickness of the moisture-absorbing and breathable layer 0.1-0.3 mm, when the manufacturing material of the moisture-absorbing and breathable layer mainly contains an aqueous polyurethane resin, the solid content of the paint is controlled to 20-40%, the viscosity is controlled to 500-2000 centipoise, and the expansion ratio is controlled to between 1.15-1.8. This is because, in the case of an aqueous polyurethane resin, if the solid content of the paint is 20-40% and the viscosity is 500-2000 centipoise, the thickness of the coating can be controlled to between 0.1-0.3 mm as required; When the material for producing the moisture-absorbing and breathable layer mainly contains solvent-based polyurethane, the solid content of the paint is controlled to 12-18%, and the viscosity is controlled to 500-1500 centipoise. This is because, according to the foaming principle of solvent-based resin, the solid content of the resin can be adjusted and the desired purpose can be achieved by adding a solidification rate regulator and a bubble regulator. By adding a solidification rate regulator, the solidification rate of the resin after being immersed in water can be changed, thereby reducing the resin density of the surface layer. In addition, by adding a bubble regulator, the probability of large-pore bubbles occurring can be reduced. It is appropriate to control the control range of the solid content of the paint to 12-18%, and by controlling the viscosity to between 500-1500 centipoise, the coating thickness can be freely controlled between 0.1-0.3 mm.
[0013] More preferably, when the production material of the moisture-absorbing and breathable layer mainly contains an aqueous polyurethane resin, the production raw material contains, as components, an aqueous polyurethane emulsion, a foaming agent and a thickener, and the amount of the foaming agent added is 5 to 15% by mass of the aqueous polyurethane emulsion; When the manufacturing material of the moisture-absorbing and breathable layer mainly contains solvent-based polyurethane, the manufacturing raw material contains wet polyurethane resin, DMF, defoaming agent, penetrating agent, foaming assistant, and accelerator as components, and the solid content of the paint is controlled to 12-18%. This is because, according to the foaming principle of solvent-based resin, the solid content of the resin can be adjusted and the desired purpose can be achieved by adding a solidification speed regulator and a bubble regulator, and the solidification speed regulator can be added to change the solidification speed of the resin after it is immersed in water, thereby reducing the resin density of the surface layer, and the bubble regulator can be added to reduce the probability of large-pore bubbles, so that it is appropriate to control the control range of the solid content of the paint to 12-18%.
[0014] Furthermore, when the manufacturing material of the moisture-absorbing and breathable layer mainly contains aqueous polyurethane, the manufacturing raw material contains, as components, 1000 parts by mass of an aqueous polyurethane emulsion, 50 to 150 parts by mass of a foaming agent, and 2 to 6 parts by mass of a thickener, When the manufacturing material of the moisture-absorbing and breathable layer mainly contains a solvent-type polyurethane, the manufacturing raw material contains, as ingredients, 1000 parts by mass of wet process polyurethane resin, 800 to 2000 parts by mass of DMF, 3 to 10 parts by mass of an antifoaming agent, 3 to 8 parts by mass of a penetrating agent, 2 to 8 parts by mass of a foaming assistant, and 5 to 15 parts by mass of an accelerator.
[0015] When a fully coated glove is produced, the formulation of the raw materials used for the moisture absorbing and sweat absorbing layer and the barrier layer may be arbitrarily combined as required.
[0016] The reasons for selecting the above parameters are as follows:
[0017] First, there are two points to note regarding the moisture absorption and ventilation layer.
[0018] 1. Size and number of bubbles The number of bubbles in the moisture-absorbing and breathable coating per unit volume is within a reasonable range, and the more bubbles there are, the smaller the pore size becomes, and the larger the specific surface area of the bubbles becomes, which is favorable for moisture absorption and breathability (here, small pore size of the bubbles means that it is greater than the range that inhibits the free passage of water and gas molecules). When the moisture-absorbing and breathable layer is manufactured with water-based polyurethane, the appropriate range of foaming ratio is 1.15 to 1.8, and it is believed that the number of bubbles and pore size can be controlled by the amount of foaming agent added. The amount of foaming agent added is generally 5 to 15% of the amount of resin. When the moisture-absorbing and breathable layer is made of solvent-based polyurethane, the purpose can be achieved by adjusting the solid content of the paint and adding a solidification rate regulator and a bubble regulator according to the foaming principle of the solvent-based resin. Conventional solvent-based urethane glove resins have a very fast solidification rate on the surface after entering water, and the surface of the coating is very dense like the skin of a plastic. By adding a solidification rate regulator, the solidification rate of the resin after entering water can be changed, which can reduce the resin density of the surface layer. In addition, the addition of a bubble regulator can reduce the probability of large-pore bubbles. It is appropriate to control the solid content of the paint to 12-18%. By combining the above three factors, the specific surface area of the entire moisture-absorbing and breathable layer can be controlled within a reasonable range.
[0019] 2. Coating thickness In the moisture-absorbing and breathable layer, there are a large number of fine holes, so the thickness of the coating has some effect on the breathability, because the thicker the thickness, the longer the path that water molecules pass through the coating, which is unfavorable to breathability. Regarding moisture absorption, assuming that the number of bubbles per unit volume is constant, the thicker the coating, the more storage space that can absorb and lock moisture, which is favorable for moisture absorption, but as with the blocking layer, the thicker the coating, the more adversely affects the flexibility and feel of the fingers, so after consideration, it is considered that it is relatively appropriate to control the thickness of the coating between 0.1 to 0.3 mm. When determining the specific manufacturing process, the thickness of the coating can be achieved by adjusting the viscosity and solid content of the paint, and if the viscosity is the same, the higher the solid content of the paint, the thicker the coating will be. If the solid content is the same, the higher the viscosity of the paint, the thicker the coating will be. In the case of water-based polyurethane resin, the coating thickness can be freely controlled between 0.1 and 0.3 mm by controlling the paint solid content between 20 and 40%, the viscosity between 500 and 2000 centipoise, and the expansion ratio between 1.15 and 1.8. In the case of solvent-based polyurethane, the coating thickness can be freely controlled between 0.1 and 0.3 mm by controlling the paint solid content between 12 and 18% and the viscosity between 500 and 1500 centipoise.
[0020] Second, the barrier layer The thickness of the coating must be strictly controlled. A thick coating is advantageous in terms of the barrier effect, but it has the disadvantage that the path through which water molecules pass through the barrier layer is longer, reducing the breathability of the coating, and thick coatings also have a negative effect on the flexibility and feel of the fingers while the wearer is working. A thin coating shortens the path through which water molecules pass through the barrier layer, improving the breathability of the coating and making the tactile sense more sensitive, and the disadvantage is that the continuous barrier effect may be reduced, and it may also have a negative effect on the durability of the gloves. Therefore, it is important to appropriately control the thickness of the coating, and after consideration, it is considered relatively appropriate to control the thickness of the coating to between 0.03 and 0.2 mm. When determining the specific production process, the coating thickness can also be achieved by adjusting the viscosity and solid content of the paint. For water-based polyurethane resin, the paint solid content is 20-40%, and the viscosity is between 500-2000 centipoise. For solvent-based polyurethane, the paint solid content is 12-20%, and the viscosity is between 300-1500 centipoise, so that the coating thickness can be freely controlled between 0.03-0.2 mm.
[0021] 3. Adhesion strength between moisture absorbing and breathable layer and barrier layer The principle of adhesion is that when two layers of adherends come into contact with each other, a force acts between the molecules, and the two adherends are bonded together. Specifically, in the process of the present invention, when the second layer of coating (barrier layer) is dip-coated, the first layer of moisture-absorbing and breathable layer is cured and baked to form a film. In order to improve the bonding strength between the moisture-absorbing and breathable layer and the barrier layer, the surface energy of the barrier layer paint in a liquid state must be lower than that of the moisture-absorbing and breathable layer. Due to the low surface energy, the barrier coating material can maximally infiltrate the surface of the moisture-absorbing and breathable layer and even the micropores of the surface layer, and is adsorbed by the moisture-absorbing and breathable layer through sufficient interface contact. During the subsequent heating process, the dipping material molecules of the barrier layer are tightly bonded with the molecules of the moisture-absorbing and breathable layer through the action of Brownian motion, and the two layers of coating form a stable state through the joint action of van der Waals force and hydrogen bond, so strictly controlling the surface energy of the barrier layer is the key to making the two layers of coating have high adhesive strength. Effect of the Invention
[0022] The beneficial effects of the present invention are as follows:
[0023] The fully coated glove with moisture absorbing and sweat absorbing function of the present invention has an ingenious structure, and in response to the shortcomings of various gloves currently on the market, the present invention creatively realizes that one glove has moisture absorbing and breathable functions and barrier insulation functions by dip-coating the film twice, completely solving the problems of commercially available products. The gloves of the present invention use polyurethane as the coating layer raw material, and effectively combine a foamed coating layer (mainly performing moisture absorbing and breathable functions) with a non-foamed coating layer (mainly performing barrier insulation functions), so that the product has both moisture absorbing and breathable functions and barrier insulation functions, and is soft to the touch, greatly reducing work fatigue, has a wide range of applications, is highly practical, and is worthy of popularization. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The fully coated glove having moisture absorbing and sweat absorbing function includes a knitted glove body, a moisture absorbing and breathable layer dip-coated on the entire inner surface of the glove body, and a barrier layer dip-coated on the entire outer surface of the glove body. The moisture absorbing and sweat absorbing layer and the barrier layer are both manufactured with a paint containing water-based polyurethane or solvent-based polyurethane as the main raw material. The moisture absorbing and sweat absorbing layer is a foamed layer with a thickness of 0.1 to 0.3 mm, and the barrier layer is a non-foamed layer with a thickness of 0.03 to 0.2 mm. The specific manufacturing process of the fully coated glove is as follows: the first layer of the moisture-absorbing and breathable layer has already been cured and baked to form a film, and the surface energy of the barrier layer paint in a liquid state is lower than the surface energy of the moisture-absorbing and breathable layer, so that when the second layer of the barrier layer is dip-coated, the barrier coating material is maximally infiltrated into the surface of the moisture-absorbing and breathable layer and even into the micropores of the surface layer. The low surface energy allows the barrier coating material to maximally infiltrate into the surface of the moisture-absorbing and breathable layer, and even into the micropores in the surface layer, and is adsorbed onto the moisture-absorbing and breathable layer through sufficient interfacial contact. During the subsequent heating process, the dipping material molecules of the barrier layer will bond tightly with the molecules of the moisture-absorbing and breathable layer through the action of Brownian motion, and the two-layer coating will form a stable state through the joint action of van der Waals forces and hydrogen bonds. Therefore, strictly controlling the surface energy of the barrier layer is the key to ensuring high adhesive strength of the two-layer coating.
[0025] To achieve a thickness of 0.03 to 0.2 mm, if the materials used to manufacture the blocking layer mainly contain water-based polyurethane resin, the solids content of the paint is controlled to between 20 and 40% and the viscosity is controlled to between 500 and 2,000 centipoise; if the materials used to manufacture the blocking layer mainly contain solvent-based polyurethane resin, the solids content of the paint is controlled to between 12 and 20% and the viscosity is controlled to between 300 and 1,500 centipoise.
[0026] When the manufacturing material of the blocking layer mainly contains an aqueous polyurethane resin, the manufacturing raw material contains, as components, an aqueous polyurethane emulsion, a defoamer, a thickener, a curing agent, and a wetting agent; When the preparation material of the blocking layer mainly comprises a solvent-based polyurethane resin, the preparation raw material comprises, as ingredients, a dry polyurethane resin, DMF, a defoaming agent, a leveling agent, a penetrating agent, and a wetting agent.
[0027] Specifically, when the production material for the blocking layer mainly contains an aqueous polyurethane resin, the production raw material contains, as ingredients, 1000 parts by mass of an aqueous polyurethane emulsion, 4 to 7 parts by mass of an antifoaming agent, 3 to 8 parts by mass of a thickener, 10 to 30 parts by mass of a curing agent, and 2 to 5 parts by mass of a wetting agent; when the production material for the blocking layer mainly contains a solvent-based polyurethane resin, the production raw material contains, as ingredients, 1000 parts by mass of a dry polyurethane resin, 800 to 2000 parts by mass of DMF, 3 to 10 parts by mass of an antifoaming agent, 3 to 8 parts by mass of a leveling agent, 3 to 8 parts by mass of a penetrating agent, and 2 to 5 parts by mass of a wetting agent.
[0028] In order to make the thickness of the moisture-absorbing and breathable layer 0.1 to 0.3 mm, when the manufacturing material of the moisture-absorbing and breathable layer mainly contains an aqueous polyurethane resin, the solid content of the paint is controlled to 20 to 40%, the viscosity is controlled to 500 to 2000 centipoise, and the expansion ratio is controlled to be between 1.15 and 1.8; When the manufacturing material of the moisture absorbing and breathable layer mainly contains solvent-based polyurethane, the solid content of the paint is controlled to 12 to 18% and the viscosity is controlled to 500 to 1500 centipoise; When the manufacturing material of the moisture-absorbing and breathable layer mainly contains an aqueous polyurethane resin, the manufacturing raw material contains, as components, an aqueous polyurethane emulsion, a foaming agent and a thickener, and the amount of the foaming agent added is 5 to 15% by mass of the aqueous polyurethane emulsion; When the manufacturing material of the moisture-absorbing and breathable layer mainly contains solvent-based polyurethane, the manufacturing raw material contains wet-process polyurethane resin, DMF, antifoaming agent, penetrating agent, foaming assistant, and accelerator as ingredients, and the solid content is controlled to 12 to 18%.
[0029] Specifically, when the manufacturing material of the moisture-absorbing and breathable layer mainly contains aqueous polyurethane, the manufacturing raw material contains, as components, 1000 parts by mass of an aqueous polyurethane emulsion, 50 to 150 parts by mass of a foaming agent, and 2 to 6 parts by mass of a thickener, When the manufacturing material of the moisture-absorbing and breathable layer mainly contains a solvent-type polyurethane, the manufacturing raw material contains, as ingredients, 1000 parts by mass of wet process polyurethane resin, 800 to 2000 parts by mass of DMF, 3 to 10 parts by mass of an antifoaming agent, 3 to 8 parts by mass of a penetrating agent, 2 to 8 parts by mass of a foaming assistant, and 5 to 15 parts by mass of an accelerator.
[0030] When a fully coated glove is produced, the formulation of the raw materials used for the moisture absorbing and sweat absorbing layer and the barrier layer may be arbitrarily combined as required.
[0031] The aqueous polyurethane emulsions, dry process polyurethane resins, and wet process polyurethane resins used are all commercially available materials. Specific Examples
[0032] The basic recipes for producing the moisture-absorbing and sweat-absorbing layer and the barrier layer are shown below, and the recipes of the raw materials used for the moisture-absorbing and sweat-absorbing layer and the barrier layer when producing a fully coated glove may be arbitrarily combined as necessary. In the following, 1 part by mass represents 1 g.
[0033] Basic formulation 1: Formulation of full surface coating barrier layer using aqueous polyurethane emulsion: 1000 parts by weight of aqueous polyurethane emulsion (XWB-7248 manufactured by Asahikawa Chemical Suzhou Co., Ltd.), 4 to 7 parts by weight of defoamer (BYK-016), 3 to 8 parts by weight of thickener (3030 manufactured by TEGO), 10 to 30 parts by weight of hardener (3100 manufactured by Bayer). 2 to 5 parts by weight of wetting agent (Capstone FS-63 manufactured by DuPont)
[0034] Basic formulation 2: Fully coated with aqueous polyurethane emulsion. Formulation for moisture absorbing and breathable layer: 1,000 parts by weight of aqueous polyurethane emulsion (XWB-7510B manufactured by Asahikawa Chemical Suzhou Co., Ltd.), 50 to 150 parts by weight of foaming agent (Glucopon 225DK manufactured by BASF), 2 to 6 parts by weight of thickener (TEGO 3030).
[0035] Basic formulation 3: Formulation for full-surface coating barrier layer using solvent-based polyurethane: 1,000 parts by weight of dry polyurethane resin (XCS-3030L manufactured by Asahikawa Co., Ltd.), 800 to 2,000 parts by weight of DMF (reagent), 3 to 10 parts by weight of defoamer (BYK-016), 3 to 8 parts by weight of leveling agent (TEGO Flow 425), 3 to 8 parts by weight of penetrating agent (AEROSOL OT-75), 2 to 5 parts by weight of wetting agent (Capstone FS~63 manufactured by DuPont).
[0036] Basic formulation 4: Formulation for full surface coating with solvent-based polyurethane. Formulation for moisture-absorbing and breathable layer: 1000 parts by mass of wet-process polyurethane resin (JF-P-2930 manufactured by Hua Feng Group Co., Ltd.), 800 to 2000 parts by mass of DMF (reagent), 3 to 10 parts by mass of defoamer (BYK-016), 3 to 8 parts by mass of penetrating agent (AEROSOL OT-75), 2 to 8 parts by mass of foaming assistant (BYK-L9520), 5 to 15 parts by mass of accelerator (BYK-L9525). Example 1
[0037] The process is to set the raw body in a mold, dip it into coagulant, dipping (foam layer), water washing, baking, dipping (barrier layer), baking, demolding the finished product, and packaging. Formulation of moisture-absorbing and breathable layer: 1000 parts by weight of aqueous polyurethane emulsion (XWB-7510B manufactured by Asahikawa Chemical Suzhou Co., Ltd.), 60 parts by weight of foaming agent (Glucopon 225DK manufactured by BASF), 6 parts by weight of thickener (TEGO 3030). The foaming ratio is 1.2 times. The measured viscosity of the working slurry is 1000 centipoise. Barrier layer formulation: 1000 parts by weight of aqueous polyurethane emulsion (XWB-7248, Asahikawa Chemical Suzhou Co., Ltd.), 5 parts by weight of defoamer (BYK-016), 5 parts by weight of thickener (TEGO 3030), 3 parts by weight of wetting agent (Capstone FS-63, DuPont), 20 parts by weight of hardener (Bayer 3100). The viscosity of the working slurry was measured to be 1000 centipoise. Example 2
[0038] The process involves setting the raw material body in a mold, dipping it in a coagulant, dipping (foam layer), rinsing with water, baking, dipping (barrier layer), baking again, and releasing the finished product into the mold and packaging it. Formulation of moisture-absorbing and breathable layer: 1000 parts by weight of aqueous polyurethane emulsion (XWB-7510B manufactured by Asahikawa Chemical Suzhou Co., Ltd.), 120 parts by weight of foaming agent (Glucopon 225DK manufactured by BASF), 4 parts by weight of thickener (TEGO 3030). The foaming ratio is 1.6 times. The measured viscosity of the working slurry is 980 centipoise. Barrier layer formulation: 1000 parts by weight of aqueous polyurethane emulsion (XWB-7248, Asahikawa Chemical Suzhou Co., Ltd.), 5 parts by weight of defoamer (BYK-016), 5 parts by weight of thickener (TEGO 3030), 3 parts by weight of wetting agent (DuPont Capstone FS-63), 20 parts by weight of hardener (Bayer 3100). The viscosity of the working slurry was measured to be 1020 centipoise. Example 3
[0039] The process involves setting the raw material body in a mold, dipping it in a coagulant, dipping (foam layer), rinsing with water, baking, dipping (barrier layer), baking again, and releasing the finished product into the mold and packaging it. Formulation of moisture-absorbing and breathable layer: 1000 parts by weight of aqueous polyurethane emulsion (XWB-7510B manufactured by Asahikawa Chemical Suzhou Co., Ltd.), 60 parts by weight of foaming agent (Glucopon 225DK manufactured by BASF), 6 parts by weight of thickener (TEGO 3030). The foaming ratio is 1.2 times. The measured viscosity of the working slurry is 980 centipoise. Barrier layer formulation: 1000 parts by weight of dry polyurethane resin (XCS-3030L manufactured by Asahikawa Co., Ltd.), 1000 parts by weight of DMF (reagent), 5 parts by weight of defoamer (BYK-016), 3 parts by weight of leveling agent (TEGO Flow 425), 5 parts by weight of penetrating agent (AEROSOL OT-75), 3 parts by weight of wetting agent (Capstone FS-63 manufactured by DuPont Co., Ltd.). The measured viscosity of the working slurry was 1000 centipoise. Example 4
[0040] The process involves setting the raw material body in a mold, dipping it in a coagulant, dipping (foam layer), rinsing with water, baking, dipping (barrier layer), baking again, and releasing the finished product into the mold and packaging it. Formulation of moisture-absorbing and breathable layer: 1000 parts by mass of aqueous polyurethane emulsion (XWB-7510B manufactured by Asahikawa Chemical Suzhou Co., Ltd.), 120 parts by mass of foaming agent (Glucopon 225DK manufactured by BASF), 4 parts by mass of thickener (TEGO 3030). The foaming ratio is 1.6 times. The measured viscosity of the working slurry is 1010 centipoise. Barrier layer formulation: 1000 parts by weight of dry polyurethane resin (XCS-3030L manufactured by Asahikawa Co., Ltd.), 1000 parts by weight of DMF (reagent), 5 parts by weight of defoamer (BYK-016), 3 parts by weight of leveling agent (TEGO Flow 425), 5 parts by weight of penetrating agent (AEROSOL OT-75), 3 parts by weight of wetting agent (Capstone FS-63 manufactured by DuPont Co., Ltd.). The measured viscosity of the working slurry was 990 centipoise. Example 5
[0041] The process involves setting the raw material body in a mold, dipping (foam layer), rinsing with water, baking, dipping (barrier layer), baking again, and releasing the finished product into the mold and packaging. Formulation of moisture-absorbing and breathable layer: 1000 parts by weight of wet polyurethane resin (JF-P-2930 manufactured by Hua Feng Group Co., Ltd.), 1200 parts by weight of DMF (reagent), 5 parts by weight of defoamer (BYK-016), 5 parts by weight of penetrant (AEROSOL OT-75), 2 parts by weight of foaming assistant (BYK-L9520), 10 parts by weight of accelerator (BYK-L9525). The viscosity of the working slurry measured was 1300 centipoise. Barrier layer formulation: 1000 parts by weight of aqueous polyurethane emulsion (XWB-7248, Asahikawa Chemical Suzhou Co., Ltd.), 5 parts by weight of defoamer (BYK-016), 5 parts by weight of thickener (TEGO 3030), 3 parts by weight of wetting agent (DuPont Capstone FS-63), 20 parts by weight of hardener (Bayer 3100). The viscosity of the working slurry was measured to be 950 centipoise. Example 6
[0042] The process involves setting the raw material body in a mold, dipping (foam layer), rinsing with water, baking, dipping (barrier layer), baking again, and releasing the finished product into the mold and packaging. Formulation of moisture-absorbing and breathable layer: 1000 parts by weight of wet polyurethane resin (JF-P-2930 manufactured by Hua Feng Group Co., Ltd.), 1500 parts by weight of DMF (reagent), 5 parts by weight of defoamer (BYK-016), 5 parts by weight of penetrant (AEROSOL OT-75), 5 parts by weight of foaming assistant (BYK-L9520), 10 parts by weight of accelerator (BYK-L9525). The viscosity of the working slurry measured was 800 centipoise. Barrier layer formulation: 1000 parts by weight of aqueous polyurethane emulsion (XWB-7248, Asahikawa Chemical Suzhou Co., Ltd.), 5 parts by weight of defoamer (BYK-016), 5 parts by weight of thickener (TEGO 3030), 3 parts by weight of wetting agent (DuPont Capstone FS-63), 20 parts by weight of hardener (Bayer 3100). The viscosity of the working slurry was measured to be 1020 centipoise. Example 7
[0043] The process involves setting the raw material body in a mold, dipping (foam layer), rinsing with water, baking, dipping (barrier layer), baking again, and releasing the finished product into the mold and packaging. Formulation of moisture-absorbing and breathable layer: 1000 parts by weight of wet polyurethane resin (JF-P-2930 manufactured by Hua Feng Group Co., Ltd.), 1200 parts by weight of DMF (reagent), 5 parts by weight of defoamer (BYK-016), 5 parts by weight of penetrant (AEROSOL OT-75), 2 parts by weight of foaming assistant (BYK-L9520), 10 parts by weight of accelerator (BYK-L9525). The viscosity of the working slurry measured was 1350 centipoise. Barrier layer formulation: 1000 parts by weight of dry polyurethane resin (XCS-3030L manufactured by Asahikawa Co., Ltd.), 1500 parts by weight of DMF (reagent), 5 parts by weight of defoamer (BYK-016), 3 parts by weight of leveling agent (TEGO Flow 425), 5 parts by weight of penetrating agent (AEROSOL OT-75), 3 parts by weight of wetting agent (Capstone FS-63 manufactured by DuPont Co., Ltd.). The measured viscosity of the working slurry was 800 centipoise. Example 8
[0044] The process involves setting the raw material body in a mold, dipping (foam layer), rinsing with water, baking, dipping (barrier layer), baking again, and releasing the finished product into the mold and packaging. Formulation of moisture-absorbing and breathable layer: 1000 parts by weight of wet polyurethane resin (JF-P-2930 manufactured by Hua Feng Group Co., Ltd.), 1800 parts by weight of DMF (reagent), 5 parts by weight of defoamer (BYK-016), 5 parts by weight of penetrant (AEROSOL OT-75), 5 parts by weight of foaming assistant (BYK-L9520), 10 parts by weight of accelerator (BYK-L9525). The viscosity of the working slurry measured was 850 centipoise. Barrier layer formulation: 1000 parts by weight of dry polyurethane resin (XCS-3030L manufactured by Asahikawa Co., Ltd.), 1500 parts by weight of DMF (reagent), 5 parts by weight of defoamer (BYK-016), 3 parts by weight of leveling agent (TEGO Flow 425), 5 parts by weight of penetrating agent (AEROSOL OT-75), 3 parts by weight of wetting agent (Capstone FS-63 manufactured by DuPont Co., Ltd.). The measured viscosity of the working slurry was 780 centipoise. Example 9
[0045] The process involves setting the raw material body in a mold, dipping it in a coagulant, dipping (foam layer), rinsing with water, baking, dipping (barrier layer), baking again, and releasing the finished product into the mold and packaging it. Formulation of moisture-absorbing and breathable layer: 1000 parts by weight of aqueous polyurethane emulsion (XWB-7510B manufactured by Asahikawa Chemical Suzhou Co., Ltd.), 120 parts by weight of foaming agent (Glucopon 225DK manufactured by BASF), 4 parts by weight of thickener (TEGO 3030). The foaming ratio is 2 times. The measured viscosity of the working slurry is 1010 centipoise. Barrier layer formulation: 1000 parts by weight of dry polyurethane resin (XCS-3030L manufactured by Asahikawa Co., Ltd.), 2000 parts by weight of DMF (reagent), 5 parts by weight of defoamer (BYK-016), 3 parts by weight of leveling agent (TEGO Flow 425), 5 parts by weight of penetrating agent (AEROSOL OT-75), 3 parts by weight of wetting agent (Capstone FS-63 manufactured by DuPont Co., Ltd.). The measured viscosity of the working slurry was 990 centipoise. Example 10
[0046] The process involves setting the raw material body in a mold, dipping (foam layer), rinsing with water, baking, dipping (barrier layer), baking again, and releasing the finished product into the mold and packaging. Formulation of moisture-absorbing and breathable layer: 1000 parts by weight of wet polyurethane resin (JF-P-2930 manufactured by Hua Feng Group Co., Ltd.), 2000 parts by weight of DMF (reagent), 5 parts by weight of defoamer (BYK-016), 5 parts by weight of penetrant (AEROSOL OT-75), 5 parts by weight of foaming assistant (BYK-L9520), 10 parts by weight of accelerator (BYK-L9525). The viscosity of the working slurry measured was 550 centipoise. Barrier layer formulation: 1000 parts by weight of aqueous polyurethane emulsion (XWB-7248, Asahikawa Chemical Suzhou Co., Ltd.), 800 parts by weight of pure water, 5 parts by weight of defoamer (BYK-016), 10 parts by weight of thickener (TEGO 3030), 3 parts by weight of wetting agent (DuPont Capstone FS-63), 20 parts by weight of hardener (Bayer 3100). The viscosity of the working slurry was measured to be 980 centipoise.
[0047] Performance detection standard: Water absorption value: GB / T 1540-2002 Breathability: JIS-L-1096 Moisture permeability: JIS-L-1099 Bacterial penetration rate: EN374-5 Water pressure resistance: GB / T 4744-2013 Abrasion resistance test: EN388-2016. The performance detection results of the fully coated gloves of each example are shown in Table 1. [Table 1]
[0048] As can be seen from the comparison in Table 1, the gloves manufactured in Examples 1 to 6 of the present invention have both moisture absorption and ventilation functions and barrier and isolation functions, and are resistant to abrasion, have low bacterial permeability, and have good protective effects. On the other hand, the effect is insufficient in Example 9 because the foaming ratio of the moisture absorption and ventilation layer is high, and in Example 10 because the coating is too thin, so the effect of the technical solution of the present application is good.
[0049] The above are merely specific embodiments of the present invention, and the scope of protection of the present invention is not limited thereto, and any changes or replacements that can be conceived without creative efforts shall be included in the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be in accordance with the scope of protection defined by the claims.
Claims
1. A method for producing a fully coated glove having moisture absorbing and sweat absorbing functions, comprising: a knitted glove body; a moisture absorbing and breathable layer dip-coated onto the entire inner surface of the glove body; and a blocking layer dip-coated onto the entire outer surface of the glove body, wherein the moisture absorbing and sweat absorbing layer and the blocking layer are both manufactured from a paint containing water-based polyurethane or solvent-based polyurethane as a main raw material, the moisture absorbing and sweat absorbing layer is a foamed layer having a thickness of 0.1 to 0.3 mm, and the blocking layer is a non-foamed layer having a thickness of 0.03 to 0.2 mm, The method includes setting the raw material body in a mold, a first dipping step of dipping to produce a foaming moisture absorbing and breathable layer, washing with water, baking, a second dipping step of dipping to produce a non-foaming barrier layer, baking, demolding the finished product, and packaging. In the second dipping step, the moisture absorption and ventilation layer is already cured and baked to form a film so that the barrier layer paint in a liquid state can infiltrate into the surface and micropores of the surface layer of the moisture absorption and ventilation layer produced in the first dipping step, and the surface energy of the barrier layer paint is lower than that of the moisture absorption and ventilation layer.
2. In order to make the thickness of the barrier layer 0.03 to 0.2 mm, when the manufacturing material of the barrier layer mainly contains an aqueous polyurethane resin, the solid content of the paint is controlled to be 20 to 40%, and the viscosity is controlled to be between 500 and 2000 centipoise; The method for manufacturing a fully coated glove according to claim 1, characterized in that, when the manufacturing material of the barrier layer mainly contains a solvent-based polyurethane resin, the solid content of the paint is controlled to be 12-20%, and the viscosity is controlled to be between 300-1500 centipoise.
3. When the manufacturing material of the blocking layer mainly contains an aqueous polyurethane resin, the manufacturing raw material contains, as components, an aqueous polyurethane emulsion, a defoamer, a thickener, a curing agent, and a wetting agent; The method for producing a fully coated glove according to claim 2, characterized in that when the manufacturing material of the barrier layer mainly comprises a solvent-based polyurethane resin, the manufacturing raw material comprises as components a dry polyurethane resin, DMF, a defoaming agent, a leveling agent, a penetrating agent, and a wetting agent.
4. When the manufacturing material of the blocking layer mainly contains an aqueous polyurethane resin, the manufacturing raw material contains, as components, 1000 parts by weight of an aqueous polyurethane emulsion, 4 to 7 parts by weight of an antifoaming agent, 3 to 8 parts by weight of a thickener, 10 to 30 parts by weight of a curing agent, and 2 to 5 parts by weight of a wetting agent; The manufacturing method of the fully coated glove according to claim 3, characterized in that when the manufacturing material of the blocking layer mainly contains a solvent type polyurethane resin, the manufacturing raw material contains, as components, 1000 parts by weight of dry type polyurethane resin, 800 to 2000 parts by weight of DMF, 3 to 10 parts by weight of a defoaming agent, 3 to 8 parts by weight of a leveling agent, 3 to 8 parts by weight of a penetrating agent, and 2 to 5 parts by weight of a wetting agent.
5. In order to make the thickness of the moisture-absorbing and breathable layer 0.1 to 0.3 mm, when the manufacturing material of the moisture-absorbing and breathable layer mainly contains an aqueous polyurethane resin, the solid content of the paint is controlled to 20 to 40%, the viscosity is controlled to 500 to 2000 centipoise, and the foaming ratio is controlled to be between 1.15 and 1.8; The method for manufacturing a fully coated glove according to claim 1, characterized in that, when the manufacturing material of the moisture absorbing and breathable layer mainly contains solvent-based polyurethane, the solid content of the paint is controlled to 12-18% and the viscosity is controlled to 500-1500 centipoise.
6. When the manufacturing material of the moisture-absorbing and breathable layer mainly contains an aqueous polyurethane resin, the manufacturing raw material contains, as components, an aqueous polyurethane emulsion, a foaming agent and a thickener, and the amount of the foaming agent added is 5 to 15% by mass of the aqueous polyurethane emulsion; The method for producing a fully coated glove according to claim 5, characterized in that when the material for producing the moisture absorbing and breathable layer mainly contains solvent-based polyurethane, the raw material for production contains wet-process polyurethane resin, DMF, a defoaming agent, a penetrating agent, a foaming assistant, and an accelerator as components, and the solid content is controlled to 12-18%.
7. When the manufacturing material of the moisture-absorbing and breathable layer mainly contains aqueous polyurethane, the manufacturing raw material contains, as components, 1000 parts by mass of an aqueous polyurethane emulsion, 50 to 150 parts by mass of a foaming agent, and 2 to 6 parts by mass of a thickener, The manufacturing method of the fully coated glove according to claim 6, characterized in that, when the manufacturing material of the moisture absorption and ventilation layer mainly contains a solvent type polyurethane, the manufacturing raw material contains, as components, 1000 parts by mass of a wet process polyurethane resin, 800 to 2000 parts by mass of DMF, 3 to 10 parts by mass of a defoaming agent, 3 to 8 parts by mass of a penetrating agent, 2 to 8 parts by mass of a foaming assistant, and 5 to 15 parts by mass of an accelerator.
Citation Information
Patent Citations
Preparation method of coated glove with micropores in surface and coated glove
CN113400543A
Gloves
JP1985165416U
Glove having foam lining for sweat management
US20150157072A1
Glove having durable ultra-thin polymeric coating
US20150374052A1
Unidirectional wicking substrate
US20180371665A1