Biaxially oriented polyester film for packaging

A biaxially oriented polyester film with specific PET and PBT resin ratios and orientation achieves improved puncture strength and transparency, addressing the limitations of conventional films in packaging applications.

JP7554387B2Active Publication Date: 2024-09-20TOYOBO CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020144812
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-28
Publication Date
2024-09-20
Estimated Expiration
2040-08-28

AI Technical Summary

Technical Problem

Existing polyester films used in packaging lack sufficient puncture strength and transparency, especially when used for heavy or sharp contents, and often require laminating with materials like nylon to improve tear resistance, which can lead to crystallization and reduced transparency.

Method used

A biaxially oriented polyester film composed of 80-100% PET resin and 0-20% PBT resin, with specific plane orientation and film forming conditions, achieving a puncture strength of 0.76 to 1.00 N/μm and a haze value of 2% or less, ensuring excellent transparency and mechanical properties.

Benefits of technology

The film provides enhanced bag breakage resistance and transparency, suitable for packaging heavy or sharp contents, while maintaining cost-effectiveness and environmental friendliness by using a high PET content and controlled resin blending.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554387000002
    Figure 0007554387000002
  • Figure 0007554387000001
    Figure 0007554387000001
Patent Text Reader

Abstract

To provide a biaxially oriented polyester film for packaging which is excellent in bag-tearing resistance even if the film is thin, and is excellent in transparency.SOLUTION: A biaxially oriented polyester film for packaging contains 80-100 mass% of a polyethylene terephthalate resin (A), and 0-20 mass% of a polyester resin (B) other than the polyethylene terephthalate resin (A), and has a plane orientation degree of 0.17 to 0.20 and a piercing strength of 0.76-1.00 N / μm, and a ratio a / b of tensile elongation at break (a) in a longitudinal direction of a film to tensile elongation at break (b) in a width direction thereof of 0.65-1.50.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester film used in the field of packaging food, medicines, industrial products, etc. More specifically, it relates to a biaxially oriented polyester film which is thin but has excellent bag rupture resistance and is environmentally friendly. [Background technology]

[0002] Polyethylene terephthalate (hereinafter sometimes abbreviated as PET) is used in a wide range of fields, such as food packaging and industrial products, due to its excellent transparency, dimensional stability, mechanical properties, electrical properties, chemical resistance, etc. However, there are cases where the mechanical strength, such as puncture strength and pinhole resistance, is insufficient. For example, in packaging for relatively heavy food products or packaging for sharp contents, it has sometimes been used in combination with a nylon film, which has excellent puncture strength and pinhole resistance.

[0003] Polybutylene terephthalate (hereinafter sometimes abbreviated as PBT) has been used as an engineering plastic because of its excellent mechanical properties, impact resistance, gas barrier properties, and chemical resistance. PBT has been used as a useful material as an engineering plastic because of its good productivity due to its fast crystallization rate, but when used as a stretched film, for example, crystallization causes deterioration in stretchability and transparency.

[0004] For example, Patent Document 1 discloses a polyester film for inner bags of cans, characterized in that the weight ratio (a / b) of PET resin (a) to PBT resin (b) is 20-60 / 80-40, and the tensile modulus of elasticity in the longitudinal and transverse directions of the film is 2.3-3.5 GPa.

[0005] However, since the stretch ratio of the polyester film is relatively low, it is expected that the puncture strength is insufficient, and therefore, for example, when used for packaging relatively heavy food products or packaging for sharp contents, the bag is likely to be easily torn.

[0006] Patent Document 2 discloses a biaxially oriented polyester film roll characterized in that the weight ratio (a / b) of a polyester resin other than PBT resin (a) to a PBT resin (b) is 0-40 / 60-100, and the winding hardness of the surface layer of the film roll is 20 or more and 80 or less.

[0007] It has high puncture strength, and is expected to be suitable for use, for example, in packaging for relatively heavy foods or packaging for sharp contents, as the bags are unlikely to tear. However, the PBT resin composition in the film is high, and it is thought that crystallization is likely to occur during film formation. Therefore, there is a high possibility that the transparency of the film will deteriorate and its printability will deteriorate. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 6195765 [Patent Document 2] Patent Publication No. 2020-12086 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0009] The present invention has been made against the background of the problems of the conventional technology. That is, the object of the present invention is to provide a polyester film for use in packaging of foods, medicines, industrial products, etc. More specifically, the object of the present invention is to provide a biaxially oriented polyester film for packaging that is thin but has excellent bag-breaking resistance and excellent transparency. [Means for solving the problem]

[0010] As a result of extensive research to achieve this objective, the inventors have discovered that by setting the blending ratio of PET resin to PBT resin in the film within a specified range and setting the planar orientation within a specified range, it is possible to obtain a biaxially oriented polyester film for packaging that is thin but has excellent bag rupture resistance and excellent transparency.

[0011] The present invention comprises the following configurations. [1] A biaxially oriented polyester film for packaging, comprising 80 to 100% by mass of a polyethylene terephthalate resin (A) and 0 to 20% by mass of a polyester resin (B) other than the polyethylene terephthalate resin (A), having a degree of planar orientation of 0.17 to 0.20, a puncture strength measured in a puncture test in accordance with JIS-Z1707 of 0.76 to 1.00 N / μm, and a ratio a / b of the tensile breaking elongation in the longitudinal direction (a) to the tensile breaking elongation in the transverse direction (b) of 0.65 to 1.50. [2] The biaxially oriented polyester film for packaging according to [1], characterized in that the film thickness is 6 to 10 μm. [3] The biaxially oriented polyester film for packaging according to [1] or [2], characterized in that the haze value is 2% or less, and the dynamic friction coefficient when the front and back surfaces of the film are brought into contact and slid is 0.25 to 0.95. [4] A laminated film obtained by laminating a sealant film to the biaxially oriented polyester film for packaging according to any one of [1] to [3]. [5] The laminated film according to [4], wherein the sealant film is a polyolefin film. [6] A packaging material using the laminated film described in [4] or [5]. Effect of the Invention

[0012] The biaxially oriented polyester film for packaging of the present invention is obtained by adjusting the compounding ratio of PET resin and PBT resin in the film and setting the film surface orientation within a specified range under specific film-forming conditions, thereby obtaining a biaxially oriented polyester film for packaging that is thin but has excellent bag rupture resistance and excellent transparency. [Brief description of the drawings]

[0013] [Figure 1] Schematic diagram of four-sided sealed bag for evaluating ease of opening DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described in detail below. The biaxially oriented polyester film for packaging of the present invention is mainly composed of PET resin, and the content of PET resin is 80% by mass or more, preferably 85% by mass, and more preferably 90% by mass. By making the content 80% by mass or more, the transparency of the biaxially oriented polyester film obtained becomes good and it can be suitably used for printing, and since the relatively inexpensive PET resin is the main component, it is also inexpensive in terms of cost.

[0015] The polyester resin (B) other than the PET resin (A) used in the biaxially oriented packaging polyester film of the present invention can be contained for the purpose of adjusting the mechanical properties and stretchability of the biaxially oriented polyester film. Examples of the polyester resin (B) other than the PET resin (A) include polyester resins such as PBT, polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), and polypropylene terephthalate (PPT); polyester resins copolymerized with dicarboxylic acids such as isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, biphenyl dicarboxylic acid, cyclohexane dicarboxylic acid, adipic acid, azelaic acid, and sebacic acid; and polyester resins copolymerized with diol components such as ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, cyclohexanediol, polyethylene glycol, polytetramethylene glycol, and polycarbonate diol. Among them, PBT is preferred because it has excellent mechanical properties, and the addition of a small amount of it improves stretchability. It also has good compatibility with PET resin and is excellent in transparency.

[0016] The amount of polyester resin (B) other than the PET resin (A) is 20% by mass or less, preferably 15% by mass or less, and more preferably 10% by mass or less. By making it 20% by mass or less, the transparency of the biaxially oriented polyester film obtained becomes good, and it can be suitably used for printing. In addition, as described above, by adding a small amount, the stretchability is improved, and stable film formation is possible even when stretched at a high ratio.

[0017] The lower limit of the intrinsic viscosity of the PET resin (A) is preferably 0.45 dl / g, more preferably 0.50 dl / g, and most preferably 0.55 dl / g. By making it 0.45 dl / g or more, the intrinsic viscosity of the obtained biaxially oriented polyester film can be kept high, and mechanical properties such as puncture strength can be improved. The upper limit of the intrinsic viscosity of the PET resin (A) is preferably 0.80 dl / g, more preferably 0.75 dl / g, and most preferably 0.70 dl / g. By setting it to 0.80 dl / g or less, it is possible to prevent the stress during film stretching from becoming too high, and to obtain good film formability.

[0018] The biaxially oriented polyester film for packaging of the present invention may contain, in addition to the polyester resin composition, conventionally known additives such as lubricants, stabilizers, colorants, antioxidants, antistatic agents, and ultraviolet absorbers.

[0019] When the entire biaxially oriented polyester film for packaging of the present invention is taken as 100% by mass, the content of the polyester resin composition is preferably 99.5% by mass or more, more preferably 99.6% by mass, and most preferably 99.7% by mass.

[0020] The lubricant can adjust the dynamic friction coefficient of the film, and examples of the lubricant include inorganic lubricants such as silica, calcium carbonate, alumina, and organic lubricants. Silica and calcium carbonate are preferred, and from the viewpoint of achieving both transparency and lubricity, porous silica is the most preferred.

[0021] The lower limit of the lubricant content in the biaxially oriented polyester film for packaging of the present invention is preferably 100 ppm by mass, more preferably 300 ppm by mass, and most preferably 500 ppm by mass. By making it 100 ppm by mass or more, the slipperiness of the film can be improved. The upper limit of the lubricant content in the biaxially oriented polyester film for packaging of the present invention is preferably 10000 mass ppm, more preferably 6000 mass ppm, and most preferably 2000 mass ppm. By setting it to 10000 mass ppm or less, the transparency of the film can be made good.

[0022] The method for obtaining the biaxially oriented polyester film for packaging of the present invention is not particularly limited, but the T-die method is preferred from the viewpoint of thickness accuracy. In the inflation method, the stretch ratio is difficult to increase due to the manufacturing method, and thickness defects in the width direction may occur.

[0023] The upper limit of the resin melting temperature in the extruder is preferably 310° C., and more preferably 300° C. When the temperature is 300° C. or less, decomposition of the resin can be suppressed, and the film can be prevented from becoming brittle, and deterioration of the film quality due to heat degradation products can also be prevented. The lower limit of the resin melting temperature in the extruder is preferably 230° C., and more preferably 240° C. When the temperature is 230° C. or higher, the resin can be extruded, and the extrusion is stable, resulting in good thickness accuracy.

[0024] The upper limit of the cooling roll temperature is preferably 40° C., and more preferably not more than 20° C. When the temperature is 40° C. or less, the crystallinity of the molten polyester resin composition when cooled and solidified is not too high, making it easier to stretch the composition, and also making it possible to suppress a decrease in transparency due to crystallization. The lower limit of the cooling roll temperature is preferably 0° C. If the temperature is 0° C. or higher, the crystallization suppression effect when the molten polyester resin composition is cooled and solidified can be sufficiently exhibited. In addition, when the temperature of the cooling roll is in the above range, it is preferable to lower the humidity of the environment near the cooling roll to prevent condensation.

[0025] The thickness of the unstretched sheet is preferably in the range of 15 to 2500 μm, more preferably 500 μm or less, and most preferably 300 μm or less.

[0026] The stretching method will now be described. The stretching method may be simultaneous biaxial stretching or sequential biaxial stretching, but in order to increase the puncture strength, it is necessary to increase the degree of planar orientation, and in that respect sequential biaxial stretching is preferred.

[0027] The lower limit of the stretching temperature in the machine direction (hereinafter also referred to as MD direction) is preferably 90° C., more preferably 95° C., and particularly preferably 100° C. When it is 90° C. or higher, breakage can be further suppressed. The upper limit of the MD stretching temperature is preferably 140° C., more preferably 135° C., and particularly preferably 130° C. When the temperature is 140° C. or less, the degree of planar orientation can be increased, and the puncture strength can be increased.

[0028] The lower limit of the stretching ratio in the MD direction is preferably 2.8 times, more preferably 2.9 times, and particularly preferably 3.0 times. If it is 2.8 times or more, the degree of planar orientation can be increased, and the puncture strength can be increased. Also, if it is 2.8 times or more, thickness unevenness can be suppressed, and slackness of the film roll can be prevented. The upper limit of the stretching ratio in the MD direction is preferably 4.5 times, more preferably 4.4 times, and particularly preferably 4.3 times. When it is 4.5 times or less, the effect of improving the mechanical strength and thickness unevenness can be sufficiently obtained.

[0029] The lower limit of the stretching temperature in the width direction (hereinafter also referred to as TD direction) is preferably 100° C., more preferably 105° C., and particularly preferably 110° C. If it is 100° C. or higher, breakage can be made less likely to occur. The upper limit of the stretching temperature in the TD direction is preferably 140° C., more preferably 135° C., and particularly preferably 130° C. When the temperature is 140° C. or less, the degree of planar orientation can be increased, and the puncture strength can be increased.

[0030] The lower limit of the stretching ratio in the TD direction is preferably 3.8 times, more preferably 3.9 times, and particularly preferably 4.0 times. When it is 3.8 times or more, the degree of planar orientation can be increased, and the puncture strength can be increased. The upper limit of the stretching ratio in the TD direction is preferably 5.0, more preferably 4.9, and particularly preferably 4.8. When it is 5.0 or less, the effect of improving the mechanical strength and thickness unevenness can be sufficiently obtained.

[0031] The lower limit of the heat setting temperature is preferably 170° C., more preferably 180° C., and particularly preferably 190° C. If the temperature is 170° C. or higher, the heat shrinkage rate can be made smaller. The upper limit of the heat setting temperature is preferably 240° C., more preferably 225° C., and particularly preferably 210° C. When the temperature is 240° C. or lower, melting of the film can be suppressed, and the degree of planar orientation can be increased, thereby increasing the puncture strength.

[0032] The lower limit of the relaxation rate is preferably 0.5%, more preferably 1.0%, and particularly preferably 2.0%. If it is 0.5% or more, the thermal shrinkage rate in the TD direction can be kept low. The upper limit of the relaxation rate is preferably 10%, more preferably 8%, and particularly preferably 6%. If it is 10% or less, loosening can be prevented, and flatness can be improved.

[0033] The lower limit of the thickness of the biaxially oriented polyester film for packaging of the present invention is preferably 3 μm, more preferably 5 μm, and particularly preferably 7 μm. By making it 3 μm or more, the strength of the film can be maintained. The upper limit of the thickness of the biaxially oriented polyester film for packaging of the present invention is preferably 40 μm, more preferably 20 μm, and particularly preferably 10 μm. By making it 40 μm or less, it can be used as a packaging material as intended by the present invention. The biaxially oriented polyester film for packaging of the present invention can be made to an appropriate thickness depending on the type of packaging material, but can be made thinner than conventional polyester films.

[0034] The lower limit of the planar orientation degree of the biaxially oriented polyester film for packaging of the present invention is preferably 0.170, more preferably 0.173, and particularly preferably 0.175. By making it 0.170 or more, the puncture strength of the film can be increased, and it can be suitably used, for example, for packaging of relatively heavy food products or packaging of sharp contents. The upper limit of the planar orientation degree of the biaxially oriented polyester film for packaging of the present invention is preferably 0.200, more preferably 0.190. By making it 0.200 or less, heat shrinkage can be suppressed, and processing troubles due to film shrinkage in processes such as deposition and printing can be reduced.

[0035] The lower limit of the puncture strength of the biaxially oriented polyester film for packaging of the present invention is 0.76 N / μm, preferably 0.78 N / μm, and more preferably 0.80 N / μm. By setting it to 0.76 N / μm or more, it can be suitably used for packaging of relatively heavy foods or packaging of sharp contents, for example. The upper limit of the puncture strength of the biaxially oriented polyester film for packaging of the present invention is preferably 1.00 N / μm, more preferably 0.97 N / μm, and particularly preferably 0.94 N / μm. By setting it to 1.00 N / μm or less, heat shrinkage can be suppressed, and processing troubles due to film shrinkage in processes such as deposition and printing can be reduced.

[0036] The lower limit of the ratio a / b of the longitudinal tensile elongation at break (a) to the transverse tensile elongation at break (b) of the biaxially oriented polyester film for packaging of the present invention is 0.65, preferably 0.75, and more preferably 0.85. By making it 0.65 or more, for example, when opening a bag from a notch, the straightness of the tear is improved, and spillage of the contents can be prevented. The upper limit of the ratio a / b of the tensile elongation at break of the biaxially oriented polyester film for packaging of the present invention is 1.50. By making it 1.50 or less, for example, when opening a bag from a notch, the straightness of the tear is good, and spillage of the contents can be prevented.

[0037] The upper limit of the haze of the biaxially oriented polyester film for packaging of the present invention is preferably 2.0%, more preferably 1.5%, and particularly preferably 1.0%. By setting it to 2.0% or less, the contents can be clearly seen and the print can be clearly seen when it is used as a package, which is preferable.

[0038] The lower limit of the dynamic friction coefficient of the biaxially oriented polyester film for packaging of the present invention is preferably 0.2, more preferably 0.35. By making it 0.25 or more, the film has appropriate slippage and the winding quality of the film roll is good. The upper limit of the dynamic friction coefficient of the biaxially oriented polyester film for packaging of the present invention is preferably 0.55, more preferably 0.53, and particularly preferably 0.51. By making it 0.90 or less, the transparency can be increased and the appearance can be improved.

[0039] The lower limit of the heat shrinkage rate in the MD direction of the biaxially oriented polyester film for packaging of the present invention is preferably 1.0%, more preferably 1.2%, and particularly preferably 1.4%. By making it 1.0% or more, the puncture strength can be increased. The upper limit of the heat shrinkage rate in the MD direction of the biaxially oriented polyester film for packaging of the present invention is preferably 5.0%, more preferably 4.8%, and particularly preferably 4.6%. By keeping it at 5.0% or less, processing troubles due to shrinkage of the film in steps such as deposition and printing can be reduced.

[0040] The lower limit of the heat shrinkage rate in the TD direction of the biaxially oriented polyester film for packaging of the present invention is preferably -1.0%, more preferably -0.8%, and particularly preferably -0.6%. By making it -1.0% or more, the puncture strength can be increased. The upper limit of the heat shrinkage rate in the TD direction of the biaxially oriented polyester film for packaging of the present invention is preferably 4.0%, more preferably 3.8%, and particularly preferably 3.6%. By keeping it at 4.0% or less, processing troubles due to shrinkage of the film in steps such as deposition and printing can be reduced.

[0041] The biaxially oriented polyester film for packaging of the present invention may be laminated with a printed layer. As the printing ink for forming the printed layer, water-based and solvent-based resin-containing printing inks can be preferably used. Here, examples of the resin used in the printing ink include acrylic resins, urethane resins, polyester resins, vinyl chloride resins, vinyl acetate copolymer resins, and mixtures thereof. The printing ink may contain known additives such as antistatic agents, light blocking agents, ultraviolet absorbing agents, plasticizers, lubricants, fillers, colorants, stabilizers, lubricants, defoamers, crosslinking agents, antiblocking agents, and antioxidants.

[0042] The printing method for providing the printed layer is not particularly limited, and known printing methods such as offset printing, gravure printing, screen printing, etc. can be used. For drying the solvent after printing, known drying methods such as hot air drying, hot roll drying, infrared drying, etc. can be used.

[0043] The biaxially oriented polyester film for packaging of the present invention may be subjected to corona discharge treatment, glow discharge treatment, flame treatment, or surface roughening treatment, as long as the purpose of the present invention is not impaired, and may also be subjected to known anchor coat treatment, printing, decoration, etc.

[0044] The biaxially oriented polyester film for packaging of the present invention may be provided with a gas barrier layer such as an inorganic thin film layer or a metal foil such as aluminum foil, so long as the object of the present invention is not impaired.

[0045] When an inorganic thin film layer is used as a gas barrier layer, the inorganic thin film layer is a thin film made of a metal or an inorganic oxide. There are no particular limitations on the material forming the inorganic thin film layer as long as it can be made into a thin film, but from the viewpoint of gas barrier properties, inorganic oxides such as silicon oxide (silica), aluminum oxide (alumina), and a mixture of silicon oxide and aluminum oxide are preferred. In particular, a composite oxide of silicon oxide and aluminum oxide is preferred from the viewpoint of achieving both flexibility and denseness of the thin film layer.

[0046] In this composite oxide, the mixing ratio of silicon oxide and aluminum oxide is preferably in the range of 20 to 70% Al by mass ratio of the metal content. On the other hand, if it is 70% or less, the inorganic thin film layer can be softened, and the thin film can be prevented from being destroyed during secondary processing such as printing and lamination, resulting in a decrease in gas barrier properties. Note that silicon oxide here refers to various silicon oxides such as SiO and SiO2, or mixtures thereof, and aluminum oxide refers to various aluminum oxides such as AlO and AL2O3, or mixtures thereof.

[0047] The inorganic thin film layer has a thickness of usually 1 to 100 nm, preferably 5 to 50 nm. When the inorganic thin film layer has a thickness of 1 nm or less, more satisfactory gas barrier properties are easily obtained. On the other hand, when the inorganic thin film layer has a thickness of 100 nm or less, it is advantageous in terms of bending resistance and production costs.

[0048] The method for forming the inorganic thin film layer is not particularly limited, and any known deposition method such as physical deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, or chemical deposition (CVD) may be appropriately adopted. A typical method for forming the inorganic thin film layer will be described below using a silicon oxide / aluminum oxide thin film as an example. For example, when the vacuum deposition method is adopted, a mixture of SiO2 and Al2O3, or a mixture of SiO2 and Al, is preferably used as the deposition raw material. Particles are usually used as these deposition raw materials, and in this case, it is desirable that the size of each particle is such that the pressure during deposition does not change, and the preferred particle diameter is 1 to 5 mm. Heating can be performed by resistance heating, high-frequency induction heating, electron beam heating, laser heating, or other methods. It is also possible to introduce oxygen, nitrogen, hydrogen, argon, carbon dioxide, water vapor, or other reactive gases as reaction gases, or to adopt reactive deposition using means such as ozone addition and ion assist. Furthermore, the film formation conditions can be changed arbitrarily, such as applying a bias to the deposition target (laminated film to be subjected to deposition), or heating or cooling the deposition target. The deposition material, reactive gas, bias of the deposition target, heating / cooling, etc. can be changed in the same manner when the sputtering method or CVD method is adopted. Furthermore, a print layer may be laminated on the inorganic thin film layer.

[0049] In this embodiment, it is preferable to provide a protective layer on the gas barrier layer. The gas barrier layer made of a metal oxide is not a completely dense film, but has minute defects scattered therein. By forming a protective layer by applying a specific resin composition for a protective layer described later on the metal oxide layer, the resin in the protective compatible resin composition penetrates into the defective parts of the metal oxide layer, resulting in an effect of stabilizing the gas barrier properties. In addition, by using a material having gas barrier properties for the protective layer itself, the gas barrier performance of the laminated film is also greatly improved.

[0050] Examples of the protective layer include resins such as urethane-based, polyester-based, acrylic-based, titanium-based, isocyanate-based, imine-based, and polybutadiene-based resins to which curing agents such as epoxy-based, isocyanate-based, and melamine-based curing agents have been added. Examples of the solvent used in forming the protective layer include aromatic solvents such as benzene and toluene; alcohol-based solvents such as methanol and ethanol; ketone-based solvents such as acetone and methyl ethyl ketone; ester-based solvents such as ethyl acetate and butyl acetate; and polyhydric alcohol derivatives such as ethylene glycol monomethyl ether.

[0051] The biaxially oriented polyester film for packaging of the present invention may be laminated with a layer of another material. The method for laminating the layer may be either lamination after the biaxially oriented polyester film is produced or lamination during film production.

[0052] The biaxially oriented polyester film for packaging of the present invention can be used as a packaging material by forming a heat-sealable resin layer (also called a sealant layer) on the biaxially oriented polyester film. The heat-sealable resin layer is usually formed by extrusion lamination or dry lamination. The thermoplastic copolymer forming the heat-sealable resin layer may be any one that can fully exhibit the sealant adhesiveness, and may be polyethylene resins such as HDPE, LDPE, and LLDPE, polypropylene resins, ethylene-vinyl acetate copolymers, ethylene-α-olefin random copolymers, ionomer resins, etc.

[0053] The sealant layer may be a single layer film or a multilayer film, and may be selected according to the required function. For example, in order to provide moisture resistance, a multilayer film containing a resin such as an ethylene-cyclic olefin copolymer or polymethylpentene may be used. In addition, the sealant layer may contain various additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, and a tackifier. The thickness of the sealant layer is preferably from 10 to 100 μm, and more preferably from 20 to 60 μm.

[0054] The biaxially oriented polyester film for packaging of the present invention can be used in the packaging field of food, medicine, industrial products, etc. In particular, it can be used as a base film (base layer) of a laminated film for packaging. The layer structure of the laminated film for packaging, where the boundary of layers is represented by / , is, for example, base layer / sealant layer, base layer / gas barrier layer / protective layer, base layer / gas barrier layer / protective layer / adhesive layer / sealant layer, base layer / gas barrier layer / protective layer / adhesive layer / resin layer / adhesive layer / sealant layer, base layer / adhesive layer / resin layer / gas barrier layer / protective layer / adhesive layer / sealant layer, base layer / gas barrier layer / protective layer / printed layer / adhesive layer / sealant layer, and base layer / printed layer / gas barrier layer / protective layer / adhesive layer / sealant layer. Examples include substrate layer / gas barrier layer / protective layer / adhesive layer / resin layer / printing layer / adhesive layer / sealant layer, substrate layer / adhesive layer / resin layer / printing layer / gas barrier layer / protective layer / adhesive layer / sealant layer, substrate layer / printing layer / gas barrier layer / protective layer / adhesive layer / resin layer / adhesive layer / sealant layer, substrate layer / printing layer / adhesive layer / resin layer / gas barrier layer / protective layer / adhesive layer / sealant layer, substrate ...printing layer / adhesive layer / sealant layer, and the like.

[0055] The laminated film obtained by laminating a sealant film on the biaxially oriented polyester film for packaging of the present invention can be suitably used for packaging materials such as packaging products, various label materials, lid materials, sheet molded products, and laminated tubes. It is particularly used for packaging bags (for example, pillow bags, standing pouches, four-sided pouches, and other pouches). The thickness of the laminated film can be appropriately determined depending on the application. For example, it is used in the form of a filmless sheet having a thickness of about 5 to 500 μm, preferably about 10 to 300 μm. EXAMPLES

[0056] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following examples. [Film thickness] The measurement was performed using a dial gauge in accordance with JIS K7130-1999 Method A.

[0057] [Film plane orientation] According to JIS K 7142-1996 A method, the refractive index in the longitudinal direction (Nx), the refractive index in the width direction (Ny), and the refractive index in the thickness direction (Nz) of the film were measured with an Abbe refractometer using sodium D line as a light source and diiodomethane as a contact liquid, and ΔP was calculated using the following formula. Planar orientation = [(Nx+Ny) / 2]-Nz

[0058] [Film puncture strength] The values ​​measured using a test method conforming to JIS-Z1707 were converted to 1 μm using the following formula. Puncture strength (N / μm) = measured puncture strength / film thickness

[0059] [Film tensile elongation at break] A sample with a width of 15 mm and a length of 180 mm was cut out from the film. The cut sample was left in an atmosphere of 23°C and 65% RH for 12 hours, and then measured under the conditions of 23°C, 65% RH, chuck distance of 100 mm, and tensile speed of 200 mm / min. The average value of five measurement results was used. The measurement device used was Shimadzu Autograph AG-1.

[0060] [Film Haze] In accordance with JIS K7361-1, the film was cut into a square shape with each side being 10 cm long, and the haze was measured using a haze meter NDH2000 manufactured by Nippon Denshoku Co., Ltd. Measurements were performed at three locations, and the average value was regarded as the actual haze measurement value.

[0061] [Dynamic friction coefficient of film] In accordance with JIS K-7125, a tensile tester (A&D Tensilon RTG-1210) was used to determine the dynamic friction coefficient when the front and back surfaces of the film were joined together in an environment of 23°C and 65% RH. The weight of the thread (weight) on which the upper film was wrapped was 1.5 kg, and the size of the base area of ​​the thread was 39.7 mm 2 The pulling speed in measuring the friction coefficient was 200 mm / min.

[0062] [Film heat shrinkage rate] The thermal shrinkage rate was measured using a dimensional change test method in accordance with JIS-C-2318, except that the test temperature was 150°C and the heating time was 15 minutes.

[0063] [Evaluation of bag tear resistance] A urethane-based two-component curing adhesive (Mitsui Chemicals' "Takelac (registered trademark) A525S" and "Takenate (registered trademark) A50" were mixed in a ratio of 13.5:1.0 (mass ratio) on a polyester film, and a 70 μm thick unstretched polypropylene film (Toyobo Co., Ltd.'s "P1147") was attached as a heat sealable resin by dry lamination, and aging was performed at 40°C for 4 days to obtain a laminate. Note that the thickness of the adhesive layer formed with the urethane-based two-component curing adhesive after drying was approximately 4 μm in all cases. The laminate was cut to a size of 15 cm square, two sheets were stacked together with the sealant on the inside, and three sides were heat sealed at a sealing temperature of 160°C with a seal width of 1.0 cm to obtain a three-sided sealed bag with an inner dimension of 13 cm. The resulting three-side sealed bag was filled with 250 mL of water, and the fourth side was then closed by heat sealing to prepare a four-side sealed bag filled with water. The resulting four-sided sealed bags were subjected to a moist heat treatment by placing them in hot water at 130°C for 30 minutes, after which they were dropped onto a concrete slab from a height of 100 cm in an environment of room temperature of 5°C and humidity of 35% RH, and the number of times they were dropped until they broke was counted. Falls 30 or more times: Yes Fewer than 30 drops: ×

[0064] [Evaluation of openability] The laminate was cut to a size of 15 cm square, two sheets were stacked together with the sealant on the inside, and the four sides were heat sealed at a sealing temperature of 160°C with a seal width of 1.0 cm to obtain a four-sided sealed bag with an inner dimension of 13 cm. As shown in Figure 1, two types of four-sided sealed bags were cut in the lengthwise and widthwise directions of the film, and each was manually opened 10 times. The straight line extending from the tip of the cut was used as the reference line, and if all tears were within 4 cm of the reference line when opened, they were marked as ◯, and if even one tear was more than 4 cm away, they were marked as ×.

[0065] [Example 1] Using a single screw extruder, PET resin (intrinsic viscosity 0.62 dl / g, silica particle blended) was melted at 280°C, cast from a T-die at 280°C, and adhered to a cooling roll at 10°C by electrostatic adhesion to obtain an unstretched sheet. The content of silica particles in the resin composition was 0.1% by mass in terms of silica concentration. The unstretched sheet was then stretched 4.0 times in the MD direction at a temperature of 115°C, then passed through a tenter to stretch 4.2 times in the TD direction at 110°C, and subjected to heat setting treatment at 200°C for 3 seconds and relaxation treatment of 5% for 1 second to obtain a biaxially oriented polyester film with a thickness of 9 μm. The resin composition of the biaxially oriented polyester film and the film formation conditions are shown in Table 1. The physical properties and evaluation results of the obtained film are also shown in Table 1.

[0066] [Examples 2 to 5] A biaxially oriented polyester film having a thickness of 9 μm was obtained by film production in the same manner as in Example 1, except that the raw material composition, stretching conditions, and heat treatment conditions in Example 1 were changed as shown in Table 1. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0067] [Comparative Example 1] The same procedure as in Example 1 was carried out except that the raw material composition and stretching conditions in Example 1 were changed as shown in Table 1. The obtained film had low puncture strength and was therefore insufficient in resistance to bag breakage.

[0068] Comparative Example 2 The same procedure as in Example 1 was repeated, except that the raw material composition and stretching conditions were changed to a biaxially oriented polyester film as shown in Table 1. The obtained film had low puncture strength and was therefore insufficient in terms of bag breakage resistance.

[0069] Comparative Example 3 The same procedure as in Example 1 was repeated, except that the raw material composition and stretching conditions were changed to a biaxially oriented polyester film as shown in Table 1. The obtained film had low puncture strength and was therefore insufficient in terms of bag breakage resistance.

[0070] Comparative Example 4 The same procedure as in Example 1 was carried out except that the raw material composition and stretching conditions were changed to the biaxially oriented polyester film shown in Table 1. The obtained film had low puncture strength and therefore insufficient bag break resistance. In addition, the ratio of the tensile breaking elongation in the MD direction to the TD direction was high, so the straight tearing property was insufficient.

[0071] Comparative Example 5 The same procedure as in Example 1 was carried out except that the raw material composition and stretching conditions were changed to the biaxially oriented polyester film shown in Table 1. The obtained film had low puncture strength and therefore insufficient bag break resistance. In addition, the ratio of the tensile breaking elongation in the MD direction to the TD direction was high, so the straight tearing property was insufficient. [Table 1] [Industrial Applicability]

[0072] The biaxially oriented polyester film for packaging of the present invention has excellent puncture strength and bag-breaking resistance even though it is thin, so it can be used as a base material for various packaging materials. It is useful because it can be used in packaging in fields where conventional PET films could not be used because of their insufficient bag-breaking resistance. In addition, the use of thinner films can save resources and reduce the burden on the environment.

Claims

1. A biaxially oriented polyester film for packaging, comprising 80-100% by mass of a polyethylene terephthalate resin (A) and 0-20% by mass of a polyester resin (B) other than the polyethylene terephthalate resin (A), having a degree of planar orientation of 0.17-0.20, a puncture strength measured in a puncture test in accordance with JIS-Z1707 of 0.76-1.00 N / μm, and a ratio a / b of the tensile breaking elongation (a) in the longitudinal direction of the film to the tensile breaking elongation (b) in the transverse direction perpendicular thereto, of 1.33-1.

50.

2. 2. The biaxially oriented polyester film for packaging according to claim 1, characterized in that the film thickness is 6 to 10 μm.

3. 3. The biaxially oriented polyester film for packaging according to claim 1 or 2, characterized in that the haze value is 2% or less, and the dynamic friction coefficient when the front and back surfaces of the film are in contact and slid is 0.25 to 0.

95.

4. A laminated film comprising the biaxially oriented polyester film for packaging according to any one of claims 1 to 3 and a sealant film laminated thereon.

5. 5. The laminated film according to claim 4, wherein the sealant film is a polyolefin film.

6. A packaging material using the laminated film according to claim 4 or 5.

Citation Information

Patent Citations

  • Device for supplying molten aluminum

    JP1986095765A

  • Polyester film

    JP1995018163A

  • Laminated body for packing snack confection and packing bag composed of the same

    JP2007144918A

  • Biaxially orientated polyester film for packaging and package using this film

    JP2009202390A

  • Polyester film

    JP2019194339A