Separator for aluminum electrolytic capacitor and aluminum electrolytic capacitor
The use of a synthetic fiber and binder-based separator with controlled bursting strength and tensile modulus addresses the mechanical weaknesses of conventional separators, achieving low ESR and preventing short-circuit defects in conductive polymer capacitors.
Patent Information
- Application Number
- JP2020139532
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-20
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-08-20
AI Technical Summary
Conventional separators for conductive polymer capacitors face challenges in maintaining low ESR while improving withstand voltage and suppressing short-circuit defects, as they often suffer from mechanical weakness and uneven impregnation due to applied forces during capacitor winding.
A separator composed of synthetic fibers and a binder, with specific bursting strength and tensile modulus ranges, ensuring stability against various forces and maintaining impregnation and retention properties, thereby preventing partial defects and enhancing short-circuit resistance.
The proposed separator structure achieves low ESR and suppresses short-circuit defects, contributing to increased withstand voltage in conductive polymer capacitors by maintaining stability and uniform impregnation of polymer solutions.
Smart Images

Figure 0007554599000001 
Figure 0007554599000002 
Figure 0007554599000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a separator for an aluminum electrolytic capacitor and an aluminum electrolytic capacitor using the separator. [Background technology]
[0002] In recent years, electronic devices and automotive electrical equipment have become more and more sophisticated. This has created a demand for faster computers used in these devices. The key to making computers faster is to increase the processing speed of the CPU. This increase in CPU processing speed has led to a further increase in operating frequencies. This has created a demand for capacitors used in power supply circuits to have improved characteristics at high frequencies.
[0003] It is difficult to improve the high frequency characteristics of aluminum electrolytic capacitors that use an electrolyte for the cathode material (hereafter referred to as "non-solid electrolytic capacitors"). For this reason, aluminum electrolytic capacitors that use a conductive polymer for the cathode material (hereafter referred to as "solid electrolytic capacitors") have been marketed. Solid electrolytic capacitors have the characteristics of lower ESR (equivalent series resistance) and superior high frequency characteristics compared to non-solid electrolytic capacitors. In recent years, aluminum electrolytic capacitors that use both conductive polymers and electrolytes as cathode materials (hereafter referred to as "hybrid electrolytic capacitors") have been released onto the market. Hybrid electrolytic capacitors have the characteristics of both non-solid electrolytic capacitors and solid electrolytic capacitors. In other words, they have the capacitance characteristics of non-solid electrolytic capacitors, while also having the low ESR of solid electrolytic capacitors.
[0004] The conduction mechanism of conductive polymers is electronic conduction, which provides higher conductivity than electrolytes, whose conduction mechanism is ionic conduction. Therefore, solid electrolytic capacitors and hybrid electrolytic capacitors that use conductive polymers as the cathode material (hereinafter, solid electrolytic capacitors and hybrid electrolytic capacitors will be collectively referred to as "conductive polymer capacitors") can achieve a lower ESR than non-solid electrolytic capacitors.
[0005] Unlike non-solid electrolytic capacitors, solid electrolytic capacitors do not use electrolyte in the cathode material and electrolyte does not evaporate from the sealing part, which allows for a long life.Solid electrolytic capacitors are being widely adopted in applications where less frequent maintenance is required, such as wireless communication base stations and data center servers. Hybrid electrolytic capacitors are also used in a variety of applications from the viewpoints of reducing the number of parts, saving space, and reducing weight. In particular, in automotive applications such as electric power steering and advanced driver assistance systems, safety and reliability are emphasized for the parts used. Therefore, the loaded parts are required to safely end their lifespan in the event of a failure. Hybrid electrolytic capacitors are being increasingly adopted for automotive applications because their failure mode is open.
[0006] There are two methods for forming the conductive polymer layer of a conductive polymer capacitor. One is a method in which an element made by rolling up an electrode foil and a separator is impregnated with a polymerization liquid of a conductive polymer (a solution of a monomer and an oxidizer), and then polymerization is carried out inside the element to form a conductive polymer layer (hereinafter referred to as the "polymerization liquid type"). The other is a method in which a rolled element is impregnated with a dispersion liquid of a conductive polymer (a dispersion liquid with a conductive polymer as a dispersoid), and then dried to remove the dispersion medium to form a conductive polymer layer (hereinafter referred to as the "dispersion liquid type"). Dispersion liquid type conductive polymer capacitors are said to have better withstand voltage characteristics than polymerization liquid type conductive polymer capacitors, and are used in applications that require a rated voltage of around 50 to 60 V. However, there are circuits in which both polymerization liquid type and dispersion liquid type capacitors cannot be used due to insufficient withstand voltage, and so there is a demand for conductive polymer capacitors with a higher rated voltage than before. For these reasons, conductive polymer capacitors are required to improve their voltage resistance characteristics, in other words, to suppress the occurrence of short-circuit defects, while maintaining the low ESR that is a feature compared to non-solid electrolytic capacitors.The separators used are also required to improve short-circuit resistance while having good impregnation and retention of the conductive polymer polymerization liquid and dispersion liquid.
[0007] One type of separator used in conductive polymer capacitors is a cellulose separator. Generally, cellulose separators are carbonized after element fabrication before use. There are two main purposes for this. The first is to suppress the reaction between the hydroxyl groups of cellulose and oxidizing agents by carbonizing the cellulose separator. The second is to improve the impregnation and retention of conductive polymer polymerization liquid and dispersion liquid by increasing the voids between the fibers that make up the separator through carbonization.
[0008] While carbonization of cellulose separators has the above-mentioned effects, the heat generated during the carbonization process causes thermal decomposition of cellulose, which reduces the mechanical strength of the separator. Furthermore, since cellulose molecules are gradually decomposed under acidic conditions, the mechanical strength of the separator is also significantly reduced by impregnating the element with an acidic polymerization solution or dispersion solution of a conductive polymer.
[0009] In order to avoid such problems with cellulose separators, separators containing synthetic fibers have been used, and the techniques disclosed in Patent Documents 1 to 4, for example, are disclosed. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2004-235293 A [Patent Document 2] JP 2018-73895 A [Patent Document 3] JP 2019-176074 A [Patent Document 4] JP 2004-146137 A Summary of the Invention [Problem to be solved by the invention]
[0011] Patent Document 1 discloses a separator that contains non-fibrillated organic fibers as synthetic fibers and a fibrillated polymer with a melting point or thermal decomposition temperature of 250° C. or higher, and has a water absorption rate of 5 mm / min or higher. It is said that the use of this separator makes the conductive polymer in the solid electrolytic capacitor uniform, thereby reducing the ESR of the solid electrolytic capacitor.
[0012] The separator in Patent Document 1 uses a fibrillated polymer that is very thin and has a large aspect ratio, and therefore the number of fibers in the separator can be significantly increased to increase the frequency with which the fibrillated polymers are entangled with each other and with other fibers, thereby making the separator denser.
[0013] However, even in a dense separator like that in Patent Document 1, the mechanical strength such as tensile strength and tear strength is weak, and there are cases where the occurrence of short circuit defects cannot be suppressed. If the content of the fibrillated polymer is increased to improve the short circuit resistance of the separator in Patent Document 1, the density of the separator becomes excessively high, which deteriorates the impregnation of the polymerization solution or dispersion solution of the conductive polymer, making it impossible to reduce the ESR.
[0014] Patent Document 2 discloses a wetlaid nonwoven fabric made of synthetic fibers having an average pore size in the range of 0.5 to 15 μm and a wet tensile strength of 0.30 kN / m or more after immersion in ion-exchanged water at 70° C. for 30 minutes. By controlling the average pore size to within the range of 0.5 to 15 μm and setting the wet tensile strength to 0.3 kN / m or more after immersion in ion-exchanged water at 70° C. for 30 minutes, it is said that the denseness of the separator is guaranteed and the shape of the separator can be maintained in the re-chemical conversion process. Therefore, the occurrence of short circuit defects in aluminum electrolytic capacitors can be suppressed.
[0015] Patent Document 3 discloses a wet-laid nonwoven fabric that contains polyester main fibers, polyester binder, and polyvinyl alcohol binder, and has an average pore size of 5.0 to 20.0 μm, a pore size frequency of 5.0 to 15.0 μm being 70% or more of the total pore size, and a pore size frequency of 20.0 μm or more being 10% or less. This configuration is said to homogenize the gaps between the fibers that make up the separator, thereby improving the short-circuit resistance of the separator and improving the impregnation of the conductive polymer polymerization solution or dispersion liquid. Therefore, it is said that an aluminum electrolytic capacitor using this separator can simultaneously achieve an improvement in capacitance and a reduction in the short-circuit defect rate.
[0016] The separators described in Patent Documents 2 and 3 are capable of suppressing the occurrence of short-circuit defects by controlling the average pore size of the separator. However, even with these separators, it is difficult to suppress the occurrence of short-circuit defects while suppressing deterioration of ESR.
[0017] The separators described in Patent Documents 2 and 3 are said to be highly dense and homogeneous, and contribute to reducing short-circuit defects in capacitors, but the separators may have weak mechanical strength such as tensile strength and tear strength, or may have narrow voids for impregnating and retaining the polymerization liquid or dispersion liquid of the conductive polymer. Therefore, it has been found that it is not possible to achieve both impregnation and retention of the polymerization liquid or dispersion liquid of the conductive polymer and short-circuit resistance at the same time by simply controlling the average pore size of the separator.
[0018] Patent Document 4 describes a nonwoven fabric containing a fibrillated polymer having a melting point or thermal decomposition temperature of 250° C. or higher, at least a portion of which has a fiber diameter of 1 μm or less and a weight average fiber length in the range of 0.2 to 2 mm, and organic fibers with a fineness of 3.3 dtex or less, and a volume resistivity of 1×10 11The paper discloses a separator for electrochemical elements with a resistivity of Ω·cm or more. It states that this structure allows for a separator that is dense and has a high volume resistivity. It also states that an aluminum electrolytic capacitor using this separator has low internal resistance and excellent high-speed charge / discharge characteristics.
[0019] However, even a separator that is dense and can reduce the internal resistance of a capacitor, such as the separator described in Patent Document 4, has low mechanical strength such as tensile strength and tear strength, and cannot suppress the occurrence of short circuit defects while achieving a low ESR.
[0020] When winding elements of aluminum electrolytic capacitors, including conductive polymer capacitors, and inside the wound element, various forces are applied to the separator in various directions. For example, there is a force applied in the longitudinal direction of the separator (MD direction: when papermaking with a papermaking machine, the direction of the separator parallel to the direction of travel), a force that spreads from the center of the wound element toward the outer edge, and a compressive force from irregularities such as tabs and electrode foil burrs. Here, it is known that a method for increasing the withstand voltage of aluminum electrolytic capacitors is to increase the thickness of the oxide film formed on the surface of the anode foil. As the oxide film becomes thicker, the thickness of the anode foil itself becomes thicker, and the above-mentioned forces applied to the separator become greater.
[0021] In conventional separators, the application of these various forces from various directions can cause problems such as the bonds between the fibers that make up the separator being broken, or the fibers moving, causing uneven density, and partial defects such as the disappearance of fibers where there should have been fibers. It was found that these defects can cause partial insufficient isolation between the anode foil and cathode foil, resulting in short circuit defects.
[0022] In order to prevent the above-mentioned partial defects in the separator, if the separator is made denser or the bonding area between the fibers is increased, the gaps between the fibers that make up the separator will become narrower. As a result, even if the occurrence of short circuits in the capacitor can be prevented, the impregnation and retention of the conductive polymer polymerization solution and dispersion liquid deteriorates, and the deterioration of the ESR cannot be prevented.
[0023] As a result of intensive research, the inventors of the present invention have found that in order to simultaneously maintain the impregnation and retention of the conductive polymer polymerization solution or dispersion liquid and improve the short-circuit resistance of the separator, it is important to increase the stability of the separator against various forces in various directions applied to the separator during and inside the element winding after winding. In other words, by increasing the stability against various forces in various directions, it is possible to suppress the occurrence of partial defects.
[0024] The present invention has been made in consideration of the above problems, and aims to suppress partial damage to the separator and improve the short-circuit resistance of the separator by improving stability against various forces in various directions applied to the separator during and inside the element winding after winding while maintaining the impregnation and retention of the conductive polymer polymerization solution or dispersion solution. Another aim is to suppress the occurrence of short-circuit defects without deteriorating the ESR of a conductive polymer capacitor using this separator compared to conventional conductive polymer capacitors. [Means for solving the problem]
[0025] The separator according to the present invention has been made with the aim of solving the above problems, and has, for example, the following configuration. That is, a separator for an aluminum electrolytic capacitor is interposed between a pair of electrodes and is used in an aluminum electrolytic capacitor having a conductive polymer as a cathode material, the separator being made of synthetic fibers and a binder, The synthetic fibers are composed of fibrillated synthetic fibers and non-fibrillated synthetic fibers. The separator contains 70 to 95% by mass of synthetic fibers and 5 to 30% by mass of binder, and the separator contains 20 to 70% by mass of fibrillated synthetic fibers and 10 to 75% by mass of non-fibrillated synthetic fibers based on the total mass of the separator. The separator has a thickness of 20 to 100 μm and a density of 0.2 to 0.6 g / cm. 3 The fibrillated synthetic fibers contain only fibers selected from one or more of polyamide fibers, acrylic fibers, polyester fibers, and vinylon fibers, and the non-fibrillated synthetic fibers contain only fibers selected from one or more of nylon fibers, acrylic fibers, polyester fibers, and vinylon fibers, Burst strength: 40~180kPa, specific burst strength: 3.5~7.5kPa / (g / m 2 ) , tensile modulus is 500-1710MPa It is characterized by being do.
[0027] The aluminum electrolytic capacitor of the present invention is characterized in that it uses a conductive polymer as a cathode material and the separator of the present invention as a separator. Effect of the Invention
[0028] According to the present invention, by being provided with a configuration that solves the above-mentioned problems, a separator can be obtained that maintains the impregnation and retention of a polymerization liquid or dispersion liquid of a conductive polymer, while having stability against various forces in various directions applied to the separator during and inside the wound element after winding. A conductive polymer capacitor using the separator of the present invention can suppress the occurrence of short circuit defects while having a low ESR, and can also contribute to increasing the withstand voltage of the conductive polymer capacitor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] Hereinafter, an embodiment of the present invention will be described in detail. In the present invention, attention is focused on partial damage to the separator that occurs during winding of the element and inside the element winding after winding, and synthetic fibers and a binder are used to improve the stability of the separator against various forces in various directions applied to it during winding of the element and inside the element winding after winding.
[0030] Conventional separators have improved short-circuit resistance by improving the density and homogeneity of the separator, but there was a limit to achieving both low ESR and suppression of short-circuit defects. The separator of the present invention can achieve improved short-circuit resistance by improving stability against various forces applied to the separator from various directions, without impregnating or impregnating the conductive polymer polymerization solution or dispersion solution.
[0031] As a result of intensive research, the inventors of the present invention found that by controlling the burst strength and burst strength ratio of the separator within a certain range, it is possible to improve short-circuit resistance without the occurrence of partial defects while maintaining the impregnation and retention of the conductive polymer polymerization solution or dispersion liquid. In addition, they found that a conductive polymer capacitor using the separator of the present invention can simultaneously achieve low ESR and suppress the occurrence of short-circuit defects, leading to the present invention.
[0032] In the embodiment for implementing the present invention, the burst strength and the specific burst strength, which is the burst strength divided by the basis weight of the separator, are used as indicators of stability against various forces in various directions applied to the separator during and inside the element winding after winding.
[0033] Unlike mechanical strength when a force is applied in a certain direction, such as tensile strength or tear strength, bursting strength can measure resistance when a force is applied from multiple directions at the same time. Even if a separator has strong mechanical strength in a certain direction, such as tensile strength or tear strength, it does not necessarily have strong bursting strength. When a force is applied from another direction, partial damage may occur due to the bonds between the fibers that make up the separator being broken, or the fibers moving from where they should be, etc.
[0034] In addition to burst strength, burst strength index can be used as an index of the strength of the bond between the fibers that make up the separator. Since burst strength index indicates burst strength per basis weight, the degree of entanglement between the fibers that make up the separator and the size of the bonded area can be compared by comparing burst strength indexes. If the burst strength index is within a certain range, it can be seen that the degree of entanglement between the fibers that make up the separator and the bonded area are controlled. The less the fibers are entangled or the smaller the bond area, the more likely the bonds between the fibers constituting the separator will break, and partial defects may occur due to the fibers moving from where they should be. Conversely, the more the fibers are entangled or the larger the bond area, the more difficult it becomes for the conductive polymer polymerization solution or dispersion liquid to penetrate into the separator.
[0035] From the above, by controlling the burst strength and burst strength index within certain ranges, it is possible to provide a separator that maintains the impregnation and retention of the conductive polymer polymerization solution and dispersion solution, while improving stability against various forces in various directions applied to the separator during and inside the element winding after winding.
[0036] The separator according to the embodiment of the present invention is, for example, a separator for an aluminum electrolytic capacitor, which is interposed between a pair of electrodes and used in an aluminum electrolytic capacitor having a conductive polymer as a cathode material, and the separator has a burst strength of 40 to 180 kPa and a specific burst strength of 3.5 to 7.5 kPa / (g / m 2 Preferably, the burst strength is 50 to 160 kPa, and the specific burst strength is 4.0 to 7.0 kPa / (g / m 2 )
[0037] In the separator according to the embodiment of the present invention, the burst strength is 40 to 180 kPa, and the specific burst strength is 3.5 to 7.5 kPa / (g / m 2 ) can improve the stability against various forces in various directions applied to the separator during and inside the element winding after winding. Also, it is possible to provide voids between the fibers constituting the separator, which are necessary for impregnating and retaining the polymerization solution or dispersion solution of the conductive polymer. This makes it possible to maintain the impregnation and retention of the conductive polymer polymerization solution or dispersion liquid while improving short-circuit resistance, without causing partial damage to the separator.
[0038] If the burst strength is less than 40 kPa, the separator cannot withstand the various forces acting in various directions on the separator during and after winding, causing the bonds between the fibers constituting the separator to break, the fibers to move and cause unevenness in density, etc. This causes partial damage to the separator, resulting in insufficient isolation between the anode foil and the cathode foil, and for example, burrs on the electrode foil may penetrate the separator, or the tab may compress and break the separator, causing a short circuit. Judging from the thickness and density of the separator that can be used in conductive polymer capacitors, the upper limit of the burst strength is 180 kPa. If the burst strength exceeds 180 kPa, the ESR tends to become higher.
[0039] Specific burst strength is 3.5kPa / (g / m 2 ), the specific burst strength is 3.5 kPa / (g / m 2 ) or above, the bonds between the fibers that make up the separator are weaker. This means that the fibers are less entangled or the bonding area between the fibers is smaller. As a result, the separator cannot withstand the various forces acting from various directions on the separator during and inside the winding of the element after winding, and the fibers that make up the separator move, causing the fibers to disappear from where they were originally located, resulting in partial defects in the separator. This results in insufficient isolation between the anode foil and cathode foil, causing short circuits.
[0040] Specific burst strength is 7.5kPa / (g / m 2 ), the specific burst strength is 7.5kPa / (g / m 2 ) The bonds between the fibers that make up the separator are excessively strong compared to separators below this grade. This means that the fibers are entangled and excessively dense, or that the bonding area between the fibers is large. This causes the conductive polymer polymerization solution or dispersion liquid to be impregnated non-uniformly, worsening the ESR.
[0041] The separator according to the embodiment of the present invention contains synthetic fibers from the viewpoint of chemical stability, and also contains a binder from the viewpoint of mechanical strength.
[0042] As the synthetic fiber of the embodiment of the present invention, any synthetic fiber can be selected as long as it satisfies the burst strength and burst strength ratio. From the viewpoints of acid resistance, oxidation resistance, and impregnation with the polymerization solution or dispersion solution of the conductive polymer, examples of the synthetic fiber to be used include polyamide fiber, acrylic fiber, polyester fiber, vinylon fiber, etc.
[0043] In addition, the synthetic fibers in the embodiment of the present invention are preferably made of fibrillated synthetic fibers and non-fibrillated synthetic fibers in order to increase the density and mechanical strength of the separator and further to improve the impregnation and retention of the polymerization liquid and dispersion liquid of the conductive polymer.
[0044] Fibrillated synthetic fibers are synthetic fibers that have been processed by beating or other methods to produce fine, branch-like fibrils from the main part of the fiber, or that have been produced in a state with branch-like fibrils like pulp. From the viewpoints of heat resistance and chemical resistance, the fibrillated synthetic fiber is preferably a fibrillated polyamide fiber, more specifically, a fibrillated aramid fiber.
[0045] Non-fibrillated synthetic fibers are synthetic fibers that do not have branched fibrils. Non-fibrillated synthetic fibers may be fibers made of a single component or fibers made of multiple components, or may have a structure such as a composite fiber. As non-fibrillated synthetic fibers, polyamide fibers, acrylic fibers, polyester fibers, vinylon fibers, etc. can be used. From the viewpoint of chemical resistance and impregnation with a polymerization solution or dispersion liquid of a conductive polymer, polyamide fibers, acrylic fibers, and polyester fibers are preferred.
[0046] The binder according to the embodiment of the present invention is used to bond the fibers constituting the separator. Any binder can be selected as long as the burst strength and burst strength ratio are satisfied. Furthermore, the binder forms a film, which makes it difficult for the burrs of the electrode foil to penetrate the separator, or for the tab to compress the separator and cause damage, and improves the short-circuit resistance of the separator. The film here refers to a film-like substance formed by the binder under moist and hot conditions at the intertwining points of the fibers constituting the separator and between the fibers. It is preferable to use polyvinyl alcohol or a vinyl alcohol copolymer as the binder, since this improves the mechanical strength and allows easy formation of a film.
[0047] In addition, the separator according to the embodiment of the present invention preferably contains 70 to 95% by mass of synthetic fibers and 5 to 30% by mass of binder, and of the total mass of the separator, it preferably contains 20 to 70% by mass of fibrillated synthetic fibers and 10 to 75% by mass of non-fibrillated synthetic fibers.
[0048] If the synthetic fiber is less than 70% by mass and the binder is more than 30% by mass, the ESR of the conductive polymer capacitor may deteriorate. This is thought to be because the increased binder increases the area of the film that is formed, causing the gaps between the fibers that make up the separator to be filled excessively, resulting in a deterioration in the impregnation and retention of the conductive polymer polymerization liquid and dispersion liquid. If the synthetic fiber content exceeds 95% by mass and the binder content is less than 5% by mass, the separator will have low mechanical strength and short-circuit resistance will not be improved, and the occurrence of short-circuit defects in the conductive polymer capacitor may not be suppressed.
[0049] If the fibrillated synthetic fiber is less than 20% by mass and the non-fibrillated synthetic fiber is more than 75% by mass, the separator tends to have low density, making it difficult to suppress the occurrence of short circuits in the separator. In addition, the low density tends to reduce the amount of conductive polymer retained, making it difficult to reduce the ESR. On the other hand, if the amount of fibrillated synthetic fibers exceeds 70% by mass and the amount of non-fibrillated synthetic fibers is less than 10% by mass, the separator tends to be highly dense, and the impregnation of the conductive polymer polymerization solution or dispersion liquid tends to become non-uniform, which tends to cause variation in the ESR characteristics.
[0050] For example, by containing 20 to 70 mass% fibrillated synthetic fibers with a length-weighted average fiber length in the range of 0.3 to 2.0 mm, 10 to 75 mass% non-fibrillated synthetic fibers with a fiber length in the range of 1.5 to 6.5 mm, and 5 to 30 mass% binder, the burst strength and burst strength index can be kept within a certain range, and a separator of the present invention can be produced. If the fiber length is shorter than the above value, there is a concern that the tensile strength may be insufficient, whereas if the fiber length is longer than the above value, there is a concern that the uniformity of the separator, such as the texture, may be impaired.
[0051] In the present invention, the tensile modulus is used as an index of the elasticity of the separator. The tensile modulus can indicate the ease of deformation in the elastic deformation region, and the lower the tensile modulus, the weaker the force required for the separator to stretch and deform. Also, the higher the tensile modulus, the stronger the force required to deform the separator.
[0052] The tensile modulus of the separator of the present invention is preferably 500 to 2000 MPa. If the tensile modulus is within the range of 500 to 2000 MPa, the separator has appropriate elasticity and can exhibit flexible responsiveness to various forces in various directions applied to the separator during and inside the element winding after winding. This improves the conformability to the electrode foil, and the separator can have high adhesion to the electrode foil. As a result, the continuity of the conductive polymer formed at the interface between the electrode foil and the separator can be maintained, and the ESR of the conductive polymer capacitor can be reduced.
[0053] If the tensile modulus is less than 500 MPa, the separator is easily deformed due to various forces acting in various directions on the separator during and inside the element winding after winding. As a result, the electrode foil and the separator are in excessively close contact with each other, and the separator acts as a sealant, which can cause uneven impregnation with the conductive polymer polymerization solution or dispersion liquid, and may prevent the conductive polymer capacitor from achieving the ESR reduction effect. If the tensile modulus exceeds 2000 MPa, the separator has low elasticity and poor adhesion to the electrode foil, which may impair the continuity of the conductive polymer at the interface between the electrode foil and the separator, resulting in the conductive polymer capacitor failing to achieve the ESR reduction effect.
[0054] The thickness and density of the separator according to the embodiment of the present invention are not particularly limited as long as they satisfy the desired characteristics of the conductive polymer capacitor. Generally, separators for conductive polymer capacitors have a thickness of 20 to 100 μm and a density of 0.20 to 0.60 g / cm. 3 Separators of thickness and density in the range have been used, but are not limited to this range.
[0055] There is no particular limitation on the method for producing the separator, but a papermaking method in which fibers dispersed in water are deposited on a wire, dehydrated, dried and papered is preferred from the viewpoint of uniformity of the separator's texture. In the embodiment of the present invention, the separator is a wet nonwoven fabric formed by a papermaking method. The separator may be made in any manner as long as it satisfies the burst strength and burst strength ratio, and may be made by combining a plurality of layers formed by these papermaking methods. In addition, additives such as dispersants, defoamers, and paper strength enhancers may be added during the papermaking process as long as the impurity content is at a level that does not affect the separator for conductive polymer capacitors, and post-processing such as paper strength enhancement, lyophilicity, calendaring, and embossing may be performed after the paper layer is formed.
[0056] By adopting the above configuration, the separator of the embodiment for carrying out the present invention can maintain good impregnation and retention of the polymerization solution or dispersion solution of the conductive polymer, while having stability against various forces in various directions applied to the separator during and inside the element winding after winding, and can have improved short-circuit resistance without causing partial damage to the separator. Furthermore, by using this separator in a conductive polymer capacitor, it is possible to suppress the occurrence of short-circuit defects while maintaining a low ESR. This can also contribute to increasing the withstand voltage of the conductive polymer capacitor.
[0057] [Method of measuring the characteristics of separators and conductive polymer capacitors] Specific measurements of the characteristics of the separator and conductive polymer capacitor of the present embodiment were performed under the following conditions and by the following method.
[0058] [Thickness] The thickness of the separator was measured using the micrometer specified in "JIS C 2300-2 'Cellulose paper for electrical purposes - Part 2: Test methods' 5.1 Thickness" in "5.1.1 Measuring instruments and measurement methods a When using an outside micrometer" and the method of folding the paper into 10 sheets in "5.1.3 When measuring thickness by folding the paper"
[0059] 〔density〕 The density of the separator in an absolute dry state was measured according to the method specified in "JIS C 2300-2 'Cellulose paper for electrical use - Part 2: Test method' 7.0A Density" Method B.
[0060] [Burst strength] The burst strength of the separator was measured according to the method specified in "JIS C 2300-2 'Cellulose paper for electrical use - Part 2: Test methods' 11. Burst strength".
[0061] [Specific burst strength] The burst strength index was calculated by dividing the burst strength measured by the above test method by the basis weight of the separator measured by the method specified in "JIS C 2300-2 'Cellulose paper for electrical use - Part 2: Test methods' 6. Basis weight."
[0062] [Tensile modulus] The tensile modulus of the separator in the machine direction (MD) was measured according to the method specified in "JIS P 8113 'Paper and paperboard -- Test methods for tensile properties -- Part 2: Constant speed extension method'".
[0063] [Length-weighted average fiber length of fibrillated synthetic fibers] The measurement was performed using a device described in "JIS P 8226-2 'Pulps-Determination of Fibre length by automated optical analysis-Part 2: Unpolarized light method'" (ISO16065-2 'Pulps-Determination of Fibre length by automated optical analysis-Part 2: Unpolarized light method'), in this case a Fiber Tester PLUS (manufactured by Lorentzen & Wettre), and the length-weighted average fiber length was taken as the fiber length of the fibrillated synthetic fiber.
[0064] [Non-fibrillated synthetic fiber length] Various commercially available non-fibrillated synthetic fibers were purchased, and the cut length was taken as the fiber length of the non-fibrillated synthetic fiber.
[0065] [Fabrication process of solid electrolytic capacitor] Using the separators of each of the examples, comparative examples, and conventional examples shown below, two types of solid electrolytic capacitors were fabricated: one with a diameter of 10.0 mm and a height of 10.0 mm, a rated voltage of 35 V, and a capacitance of 150 μF, and the other with a rated voltage of 80 V and a capacitance of 22 μF. The specific manufacturing method is as follows.
[0066] The 115 μm thick anode foil and the 50 μm thick cathode foil, which had been subjected to etching and oxide film formation, were wound with a separator between them so that they would not come into contact with each other, and the outer periphery of the element winding was fixed with tape to prepare a capacitor element. The prepared capacitor element was then re-chemically treated and dried.
[0067] The solid electrolytic capacitor with a rated voltage of 35V was made by impregnating the capacitor element with a conductive polymer polymerization solution, heating and polymerizing it, and then drying the solvent to form a conductive polymer layer. The conductive polymer polymerization solution used 3,4-ethylenedioxythiophene as the monomer, and iron paratoluenesulfonate solution as the oxidizer solution. A conductive polymer layer was formed on the solid electrolytic capacitor with a rated voltage of 80 V by impregnating the capacitor element with a conductive polymer dispersion, then heating and drying it. The conductive polymer dispersion used was a dispersion with PEDOT / PSS (a composite of poly(3,4-ethylenedioxythiophene) and polystyrene sulfonic acid) as the dispersoid. Next, the capacitor element was placed in a prescribed case, the opening was sealed, and then aging was carried out to obtain each solid electrolytic capacitor.
[0068] [Production process of hybrid electrolytic capacitor] Using the separators of each of the Examples, Comparative Examples, and Conventional Examples, two types of hybrid electrolytic capacitors were fabricated: one with a diameter of 10.0 mm and a height of 10.5 mm, a rated voltage of 35 V, and a capacitance of 270 μF, and the other with a rated voltage of 160 V and a capacitance of 6.8 μF. The specific manufacturing method is as follows.
[0069] The 115 μm thick anode foil and the 50 μm thick cathode foil, which had been subjected to etching and oxide film formation, were wound with a separator between them so that they would not come into contact with each other, and the outer periphery of the element winding was fixed with tape to prepare a capacitor element. The prepared capacitor element was then re-chemically treated and dried.
[0070] The hybrid electrolytic capacitor with a rated voltage of 35V was made by impregnating the capacitor element with a conductive polymer polymerization liquid, heating and polymerizing it, and then drying the solvent to form a conductive polymer layer. The conductive polymer polymerization liquid used 3,4-ethylenedioxythiophene as the monomer, and iron paratoluenesulfonate solution as the oxidizer solution. The hybrid electrolytic capacitor with a rated voltage of 160 V was fabricated by impregnating the capacitor element with a conductive polymer dispersion, then heating and drying to form a conductive polymer layer. The conductive polymer dispersion used was a dispersion with PEDOT / PSS (a composite of poly(3,4-ethylenedioxythiophene) and polystyrene sulfonic acid) as the dispersoid. Next, the capacitor element was impregnated with a driving electrolyte, the capacitor element was placed in a predetermined case, the opening was sealed, and then aging was performed to obtain each hybrid electrolytic capacitor.
[0071] [Evaluation method of conductive polymer capacitors] Specific performance evaluation of the conductive polymer capacitor of the present embodiment was carried out under the following conditions and by the following method.
[0072] [Short circuit failure rate] 1,000 wound capacitor elements were prepared, and the number of short circuits that occurred during aging was counted. The number of elements that became short circuits was divided by the number of capacitor elements that had been aged to obtain the short circuit defect rate as a percentage.
[0073] [ESR] The ESR of the fabricated capacitor element was measured using an LCR meter at a temperature of 20°C and a frequency of 100 kHz.
[0074] [Example] Hereinafter, specific examples of the separator according to the embodiment of the present invention will be described.
[0075] Example 1 A separator of Example 1 was obtained by cylinder-type papermaking using a raw material that was a mixture of 60 mass % of fibrillated acrylic fibers (weighted average fiber length 0.8 mm), 30 mass % of aramid fibers (fiber length 2.0 mm), and 10 mass % of polyvinyl alcohol. The completed separator of Example 1 had a thickness of 50 μm and a density of 0.55 g / cm 3 , burst strength is 120kPa, specific burst strength is 4.4kPa / (g / m 2 ) and the tensile modulus was 2030 MPa.
[0076] Example 2 A separator of Example 2 was obtained by cylinder-type papermaking using a raw material that was a mixture of 45 mass% of fibrillated polyester fiber (weighted average fiber length 0.5 mm), 50 mass% of vinylon fiber (fiber length 5.0 mm), and 5 mass% of ethylene-vinyl alcohol copolymer. The completed separator of Example 2 had a thickness of 20 μm and a density of 0.45 g / cm 3 , burst strength is 52kPa, specific burst strength is 5.8kPa / (g / m 2 ) and the tensile modulus was 480 MPa.
[0077] Example 3 A separator of Example 3 was obtained by cylinder-type papermaking using a raw material that was a mixture of 60 mass % of fibrillated aramid fibers (weighted average fiber length 0.4 mm), 10 mass % of acrylic fibers (fiber length 5.0 mm), and 30 mass % of polyvinyl alcohol. The completed separator of Example 3 had a thickness of 50 μm and a density of 0.60 g / cm 3 , burst strength is 178kPa, specific burst strength is 5.9kPa / (g / m 2 ) and the tensile modulus was 1320 MPa.
[0078] Example 4 A separator of Example 4 was obtained by cylinder-type papermaking using a raw material that was a mixture of 70 mass % of fibrillated aramid fibers (weighted average fiber length 0.8 mm), 10 mass % of nylon fibers (fiber length 3.0 mm), and 20 mass % of polyvinyl alcohol. The completed separator of Example 4 had a thickness of 40 μm and a density of 0.50 g / cm 3 , burst strength is 135kPa, specific burst strength is 6.8kPa / (g / m 2 ) and the tensile modulus was 1710 MPa.
[0079] Example 5 A separator of Example 5 was obtained by cylinder-type papermaking using a raw material that was a mixture of 45 mass % of fibrillated acrylic fibers (weighted average fiber length 1.2 mm), 30 mass % of nylon fibers (fiber length 3.0 mm), and 25 mass % of polyvinyl alcohol. The completed separator of Example 5 had a thickness of 80 μm and a density of 0.40 g / cm 3 , burst strength is 155kPa, specific burst strength is 4.8kPa / (g / m 2 ) and the tensile modulus was 1620 MPa.
[0080] Example 6 A separator of Example 6 was obtained by cylinder-type papermaking using a raw material that was a mixture of 30 mass % of fibrillated aramid fibers (weighted average fiber length 1.8 mm), 40 mass % of polyester fibers (fiber length 3.0 mm), and 30 mass % of polyvinyl alcohol. The completed separator of Example 6 had a thickness of 100 μm and a density of 0.45 g / cm 3 , burst strength is 163kPa, specific burst strength is 3.6kPa / (g / m 2 ) and the tensile modulus was 870 MPa.
[0081] Example 7 A separator of Example 7 was obtained by cylinder-type papermaking using a raw material that was a mixture of 45 mass % of fibrillated aramid fibers (weighted average fiber length 0.6 mm), 40 mass % of acrylic fibers (fiber length 3.0 mm), and 15 mass % of polyvinyl alcohol. The completed separator of Example 7 had a thickness of 50 μm and a density of 0.35 g / cm 3 , burst strength is 100kPa, specific burst strength is 5.7kPa / (g / m 2 ) and the tensile modulus was 1270 MPa.
[0082] Example 8 A separator of Example 8 was obtained by cylinder-type papermaking using a raw material that was a mixture of 20 mass% of fibrillated aramid fibers (weighted average fiber length 0.3 mm), 50 mass% of acrylic fibers (fiber length 2.0 mm), and 30 mass% of ethylene-vinyl alcohol copolymer. The completed separator of Example 8 had a thickness of 45 μm and a density of 0.35 g / cm 3 , burst strength is 116kPa, specific burst strength is 7.4kPa / (g / m 2 ) and the tensile modulus was 1112 MPa.
[0083] Example 9 A separator of Example 9 was obtained by cylinder-type papermaking using a mixture of 30 mass% fibrillated acrylic fiber (weighted average fiber length 1.4 mm), 50 mass% aramid fiber (fiber length 4.0 mm), and 20 mass% ethylene-vinyl alcohol copolymer. The completed separator of Example 9 had a thickness of 70 μm and a density of 0.40 g / cm 3 , burst strength is 117kPa, specific burst strength is 4.2kPa / (g / m 2 ) and the tensile modulus was 1960 MPa.
[0084] Example 10 A separator of Example 10 was obtained by cylinder-type papermaking using a raw material that was a mixture of 20 mass % of fibrillated polyester fibers (weighted average fiber length 1.6 mm), 75 mass % of acrylic fibers (fiber length 6.0 mm), and 5 mass % of polyvinyl alcohol. The completed separator of Example 10 had a thickness of 40 μm and a density of 0.20 g / cm 3 , burst strength is 41kPa, specific burst strength is 5.1kPa / (g / m 2 ) and the tensile modulus was 533 MPa.
[0085] Comparative Example 1 A separator of Comparative Example 1 was obtained by cylinder-type papermaking using a raw material that was a mixture of 65 mass % of fibrillated aramid fibers (weighted average fiber length 0.4 mm), 5 mass % of acrylic fibers (fiber length 5.0 mm), and 30 mass % of polyvinyl alcohol. The completed separator of Comparative Example 1 had a thickness of 40 μm and a density of 0.50 g / cm 3 , burst strength is 158kPa, specific burst strength is 7.9kPa / (g / m 2 ) and the tensile modulus was 1420 MPa.
[0086] Comparative Example 2 A separator of Comparative Example 2 was obtained by cylinder-type papermaking using a raw material that was a mixture of 75 mass % of fibrillated aramid fibers (weighted average fiber length 0.3 mm), 10 mass % of nylon fibers (fiber length 2.0 mm), and 15 mass % of polyvinyl alcohol. The completed separator of Comparative Example 2 had a thickness of 60 μm and a density of 0.60 g / cm 3 , burst strength is 121kPa, specific burst strength is 3.4kPa / (g / m 2 ) and the tensile modulus was 1750 MPa.
[0087] Comparative Example 3 A separator of Comparative Example 3 was obtained by cylinder-type papermaking using a raw material that was a mixture of 25 mass % of fibrillated acrylic fibers (weighted average fiber length 1.9 mm), 40 mass % of polyester fibers (fiber length 3.0 mm), and 35 mass % of polyvinyl alcohol. The completed separator of Comparative Example 3 had a thickness of 80 μm and a density of 0.35 g / cm 3 , burst strength is 187kPa, specific burst strength is 6.7kPa / (g / m 2 ) and the tensile modulus was 570 MPa.
[0088] Comparative Example 4 A separator of Comparative Example 4 was obtained by cylinder-type papermaking using a raw material that was a mixture of 15 mass% of fibrillated aramid fibers (weighted average fiber length 0.5 mm), 60 mass% of acrylic fibers (fiber length 2.0 mm), and 25 mass% of ethylene-vinyl alcohol copolymer. The completed separator of Comparative Example 4 had a thickness of 35 μm and a density of 0.35 g / cm 3 , burst strength is 94kPa, specific burst strength is 7.7kPa / (g / m 2 ) and the tensile modulus was 980 MPa.
[0089] Comparative Example 5 A separator of Comparative Example 5 was obtained by cylinder-type papermaking using a raw material that was a mixture of 15 mass % of fibrillated acrylic fibers (weighted average fiber length 0.9 mm), 80 mass % of acrylic fibers (fiber length 6.0 mm), and 5 mass % of polyvinyl alcohol. The completed separator of Comparative Example 5 had a thickness of 50 μm and a density of 0.30 g / cm 3 , burst strength is 43kPa, specific burst strength is 2.9kPa / (g / m 2 ) and the tensile modulus was 2060 MPa.
[0090] Comparative Example 6 A separator for Comparative Example 6 was obtained by cylinder-type papermaking using a raw material that was a mixture of 45 mass% of fibrillated polyester fiber (weighted average fiber length 0.4 mm), 52 mass% of vinylon fiber (fiber length 3.0 mm), and 3 mass% of ethylene-vinyl alcohol copolymer. The completed separator of Comparative Example 6 had a thickness of 20 μm and a density of 0.45 g / cm 3 , burst strength is 35kPa, specific burst strength is 3.9kPa / (g / m 2 ) and the tensile modulus was 460 MPa.
[0091] [Conventional Example 1] A separator was produced in the same manner as in Example 1 of Patent Document 1, and a separator of Conventional Example 1 was obtained. The thickness of the separator in Conventional Example 1 was 45 μm and the density was 0.36 g / cm 3 , burst strength is 46kPa, specific burst strength is 2.8kPa / (g / m 2 ) and the tensile modulus was 720 MPa.
[0092] [Conventional Example 2] A separator was produced in the same manner as in Example 1 of Patent Document 2, and a separator of Conventional Example 2 was obtained. The thickness of the separator in Conventional Example 2 is 30 μm and the density is 0.55 g / cm 3 , burst strength is 54kPa, specific burst strength is 3.3kPa / (g / m 2 ) and the tensile modulus was 1560 MPa.
[0093] [Conventional Example 3] A separator was produced in the same manner as in Example 1 of Patent Document 3, and a separator of Conventional Example 3 was obtained. The separator of Conventional Example 3 has a thickness of 60 μm and a density of 0.20 g / cm 3 , burst strength is 94kPa, specific burst strength is 7.8kPa / (g / m 2 ) and the tensile modulus was 540 MPa.
[0094] [Conventional Example 4] A separator was produced in the same manner as in Example 1 of Patent Document 4, and a separator of Conventional Example 4 was obtained. The separator of Conventional Example 4 has a thickness of 55 μm and a density of 0.33 g / cm 3 , burst strength is 37kPa, specific burst strength is 2.0kPa / (g / m 2 ) and the tensile modulus was 630 MPa.
[0095] Table 1 shows the raw materials and compositions of each of the separators of Examples 1 to 10, Comparative Examples 1 to 6, and Conventional Examples 1 to 4 described above.
[0096] [Table 1]
[0097] Table 2 shows the evaluation results of each of the separators of Examples 1 to 10, Comparative Examples 1 to 6, and Conventional Examples 1 to 4 described above.
[0098] [Table 2]
[0099] Conductive polymer capacitors produced using the separators of each Example, Comparative Example, and Conventional Example are described below. Solid electrolytic capacitors with a rated voltage of 35V, a capacitance of 150μF, a rated voltage of 80V, and a capacitance of 22μF, and hybrid electrolytic capacitors with a rated voltage of 35V, a capacitance of 270μF, a rated voltage of 160V, and a capacitance of 6.8μF were produced using the separators of each Example, Comparative Example, and Conventional Example. The performance evaluation results of each capacitor are shown in Table 3.
[0100] [Table 3]
[0101] The evaluation results of the conductive polymer capacitors using the separators of each of the Examples, Comparative Examples, and Conventional Examples will be described in detail below.
[0102] The capacitors using the separators of Examples 1 and 2 have the same ESR as the capacitors using the separators of Conventional Examples 1 to 4, but have a lower short circuit defect rate.
[0103] Furthermore, the capacitors using the separators of Examples 3 to 10 have a similar short circuit defect rate to the capacitors using the separators of Examples 1 and 2, but have a lower ESR.
[0104] The reason why the ESR of the separators in Examples 3 to 10 was low is believed to be that the separators had a tensile modulus of elasticity of 533 to 1960 MPa, had good adhesion to the electrode foil, and were able to maintain the continuity of the conductive polymer at the interface between the electrode foil and the separator. This shows that the ESR can be reduced by providing a separator with appropriate elasticity. In other words, it was made clear that a low ESR can be achieved in conductive polymer capacitors if the separator has a tensile modulus of elasticity in the range of 500 to 2000 MPa.
[0105] The separator of Comparative Example 1 has the same levels of thickness, density, and burst strength as the other examples, but the specific burst strength is 7.9 kPa / (g / m 2 ), which is higher than that of each of the Examples. The capacitor using the separator of Comparative Example 1 has a higher ESR than that of each of the Examples.
[0106] The ESR of the capacitor using the separator of Comparative Example 1 was high because the burst strength of the separator was 7.9 kPa / (g / m 2), which is believed to be due to excessively strong bonding between the fibers that make up the separator. The separator of Comparative Example 1 contains 5% by mass of non-fibrillated synthetic fibers, which is believed to have made it excessively dense, resulting in an excessively high burst strength ratio and non-uniform impregnation of the conductive polymer polymerization solution and dispersion solution. From this, the burst strength of the separator is 7.5 kPa / (g / m 2 ) or less, it is possible to achieve a low ESR for the conductive polymer capacitor. It is also clear that by making the content of non-fibrillated synthetic fibers 10 mass % or more, it is possible to maintain the impregnation of the conductive polymer polymerization solution or dispersion solution.
[0107] The separator of Comparative Example 2 has the same levels of thickness, density, and burst strength as the other Examples, but the specific burst strength is 3.4 kPa / (g / m 2 ), which is lower than the other Examples. The capacitor using the separator of Comparative Example 2 has a higher short-circuit defect rate than the other Examples. Also, the ESR is slightly higher than that of the conventional example.
[0108] The short-circuit defect rate of the capacitor using the separator of Comparative Example 2 was high because the burst strength of the separator was 3.4 kPa / (g / m 2 ), which is believed to be due to the weak bonds between the fibers that make up the separator. Because the bursting strength is low, the separator cannot withstand the various forces applied in various directions during and after winding of the element, which is believed to cause partial damage to the separator and short circuit defects. Also, the ESR of the capacitor using the separator of Comparative Example 2 is high due to the fibrillation. Aramid fiber This is thought to be because the content is 75% by mass. From this, the specific burst strength is 3.5 kPa / (g / m 2 ) or more, it was found that the occurrence of short circuit defects in conductive polymer capacitors can be suppressed. It was also found that the deterioration of ESR can be suppressed by setting the content of fibrillated synthetic fibers to 70 mass % or less.
[0109] The separator of Comparative Example 3 has the same thickness, density, and specific burst strength as the other Examples, but has a burst strength of 187 kPa, which is higher than the other Examples. The capacitor using the separator of Comparative Example 3 has a higher ESR than the other Examples.
[0110] The reason why the ESR of the capacitor using the separator of Comparative Example 3 was high is believed to be that the separator had a high burst strength of 187 kPa. The separator of Comparative Example 3 had an excessively high burst strength because the polyvinyl alcohol content was 35 mass %, and the gaps between the fibers constituting the separator were filled. Therefore, the separator of Comparative Example 3 was considered to have poor impregnation and retention of the polymerization solution and dispersion solution of the conductive polymer. This shows that if the burst strength exceeds 180 kPa, the ESR deteriorates. In other words, it became clear that if the burst strength is 180 kPa or less, the separator can be applied to conductive polymer capacitors and can have a low ESR. It was also found that by setting the binder content to 30 mass% or less, it is possible to provide voids between the fibers that make up the separator, which are necessary for impregnating and retaining the polymerization liquid or dispersion liquid of the conductive polymer, and to achieve a low ESR.
[0111] The separator of Comparative Example 4 has the same levels of thickness, density, and burst strength as the other Examples, but the specific burst strength is 7.7 kPa / (g / m 2 ) is high. The capacitor using the separator of Comparative Example 4 has a higher ESR than the other Examples. In addition, the short-circuit defect rate is high for the solid electrolytic capacitor with a rated voltage of 80V and the hybrid electrolytic capacitor with a rated voltage of 160V.
[0112] The ESR of the capacitor using the separator of Comparative Example 4 was high because the burst strength of the separator was 7.7 kPa / (g / m 2 ), which is thought to be due to the excessively strong bonds between the fibers that make up the separator. The high burst strength indicates that the bonding area between the fibers that make up the separator is large, and the conductive polymer polymerization liquid and Impregnation of dispersionIn addition, since the content of fibrillated aramid in the separator of Comparative Example 4 was 15 mass %, the density of the separator was low, and it is considered that the short circuit defect rate in the capacitor with a high rated voltage was high.
[0113] In addition to the evaluation of the capacitor using the separator of Comparative Example 1, the evaluation of the capacitor using the separator of Comparative Example 4 also showed that the burst strength of the separator was 7.5 kPa / (g / m 2 ) or less, it is possible to achieve a low ESR for the conductive polymer capacitor. It is also clear that if the content of fibrillated synthetic fibers is 20 mass% or more, the density of the separator can be increased, and the occurrence of short circuit defects can be suppressed.
[0114] The separator of Comparative Example 5 has the same levels of thickness, density, and burst strength as the other Examples, but the specific burst strength is 2.9 kPa / (g / m 2 The capacitor using the separator of Comparative Example 5 has a high short-circuit defect rate and ESR compared to the other Examples.
[0115] The short-circuit defect rate of the capacitor using the separator of Comparative Example 5 was high because the burst strength of the separator was 2.9 kPa / (g / m 2 ), which is believed to be due to weak bonding between the fibers that make up the separator. In addition, the separator of Comparative Example 5 has a fibrillated aramid content of 15 mass % and an acrylic content of 80 mass %, which is believed to have resulted in an excessively low density of the separator and a high rate of short-circuit defects. Furthermore, it is believed that the low density of the separator reduces the amount of conductive polymer retained, resulting in a high ESR.
[0116] In addition to the evaluation of the capacitor using the separator of Comparative Example 2, the evaluation of the capacitor using the separator of Comparative Example 5 also showed that the burst strength of the separator was 3.5 kPa / (g / m 2) or more, it was found that the occurrence of short circuit defects in conductive polymer capacitors can be suppressed. In addition, it was found that if the content of fibrillated synthetic fibers is 20 mass% or more and the content of non-fibrillated synthetic fibers is 75 mass% or less, the density of the separator can be increased, and the occurrence of short circuit defects can be suppressed without deteriorating the ESR of the capacitor.
[0117] The separator of Comparative Example 6 has the same thickness, density, and specific burst strength as the other Examples, but has a low burst strength of 35 kPa. The capacitor using the separator of Comparative Example 6 has a higher short circuit defect rate than the other Examples.
[0118] The short-circuit failure rate of the capacitor using the separator of Comparative Example 6 was high because the separator had a low burst strength of 35 kPa and could not withstand the various forces applied to the separator from various directions during and inside the winding of the element, causing partial damage to the separator and insufficient isolation between the anode foil and the cathode foil. Also, the separator of Comparative Example 6 had an ethylene-vinyl alcohol copolymer content of 3 mass%, which is thought to have reduced the burst strength of the separator. This shows that if the separator has a burst strength of 40 kPa or more, it is possible to suppress the occurrence of short-circuit defects in conductive polymer capacitors. It is also clear that if the binder content is 5 mass% or more, the separator's burst strength can be increased, and the separator's short-circuit resistance can be improved.
[0119] The separator of Conventional Example 1 is similar to the separator described in Example 1 of Patent Document 1. The separator of Conventional Example 1 has a specific burst strength of 2.8 kPa / (g / m 2 ) is low. For this reason, the short circuit defect rate is also high in the capacitor evaluation results.
[0120] The separator of Conventional Example 2 is similar to the separator described in Example 1 of Patent Document 2. The separator of Conventional Example 2 has a specific burst strength of 3.3 kPa / (g / m 2) is low. For this reason, the short circuit defect rate is also high in the capacitor evaluation results.
[0121] From the evaluation results of the capacitors using the separators of Conventional Examples 1 and 2 and a comparison with each of the Examples, it is found that the occurrence of short circuit defects cannot be suppressed by only containing 20 to 70 mass% of fibrillated synthetic fibers and 10 to 75 mass% of non-fibrillated synthetic fibers in the separator, and it is necessary to contain a binder. In addition, when the burst strength of the separator is 3.5 kPa / (g / m 2 ) or more, it has become clear that the occurrence of short circuit defects can be suppressed.
[0122] Furthermore, the separator of Conventional Example 2 is a separator with controlled wet tensile strength, and although it has resistance to forces from one direction, it has low resistance to various forces from various directions, and it is believed that it was unable to suppress the occurrence of short circuits. From this, it can be seen that by setting the burst strength and burst strength index within a certain range, it is possible to increase stability against various forces from various directions, and to suppress the occurrence of short circuits.
[0123] The separator of Conventional Example 3 is similar to the separator described in Example 1 of Patent Document 3. The separator of Conventional Example 3 has a burst strength of 7.8 kPa / (g / m 2 The evaluation results for the capacitor using the separator of Conventional Example 3 showed a high short-circuit failure rate and a high ESR.
[0124] The separator of Conventional Example 3 is composed of non-fibrillated synthetic fibers and polyvinyl alcohol, which is thought to have led to a low density of the separator and a high rate of short-circuit defects in the capacitors. In addition, the ESR of each capacitor using the separator of Conventional Example 3 was high because the burst strength was 7.8 kPa / (g / m 2 ) is thought to be the cause.
[0125] From the capacitor evaluation results of Conventional Examples 2 and 3 and a comparison with each Example, it became clear that the occurrence of short circuit defects in conductive polymer capacitors cannot be suppressed by merely controlling the average pore size of the separator, and that it is necessary to improve the stability against various forces in various directions applied to the separator during winding of the element and inside the element winding. In other words, it became clear that it is necessary to set the burst strength and burst strength ratio of the separator within a certain range.
[0126] The separator of Conventional Example 4 is similar to the separator described in Example 1 of Patent Document 4. Evaluation results of a capacitor using the separator of Conventional Example 4 showed a high short-circuit defect rate and a high ESR.
[0127] The short-circuit defect rate of the capacitor using the separator of Conventional Example 4 was high because the separator of Conventional Example 4 had a burst strength of 37 kPa and a burst strength ratio of 2.0 kPa / (g / m 2 ), which is believed to be due to the separator being unable to withstand the various forces in various directions applied to it during and inside the winding of the element. In addition, the separator of Conventional Example 4 has a cellulose content of 15 mass%, and it is believed that the separator's burst strength was reduced and the short circuit defect rate was further increased by impregnating and retaining the conductive polymer polymerization liquid and dispersion liquid. Furthermore, it is believed that the inclusion of cellulose reduced the impregnation and retention of the conductive polymer polymerization liquid and dispersion liquid, resulting in the high ESR.
[0128] From a comparison of the capacitor evaluation results of Conventional Example 4 with each of the Examples, it is found that a separator containing cellulose cannot improve short-circuit resistance while maintaining the impregnation and retention of the conductive polymer polymerization solution or dispersion liquid, and therefore needs to be composed of only synthetic fibers and binders.
[0129] As described above, according to the embodiment of the present invention, the separator made of synthetic fibers and a binder has a burst strength of 40 to 180 kPa and a specific burst strength of 3.5 to 7.5 kPa / (g / m 2), it is possible to improve the stability against various forces in various directions applied to the separator during and inside the element winding after winding, while maintaining the impregnation and retention of the conductive polymer polymerization solution or dispersion liquid. Therefore, it is possible to suppress the occurrence of partial damage to the separator. And it is possible to suppress the occurrence of short circuit defects without deteriorating the ESR of the conductive polymer capacitor using the separator of the present invention.
[0130] Furthermore, by setting the tensile modulus of the separator to be in the range of 500 to 2000 MPa, the adhesion between the electrode foil and the separator can be controlled, making it possible to achieve a low ESR for the conductive polymer capacitor.
[0131] As described above, the conductive polymer capacitor using the separator of the present embodiment can suppress the occurrence of short circuit defects without deteriorating the ESR, and can also contribute to increasing the withstand voltage of the conductive polymer capacitor.
Claims
1. A separator for an aluminum electrolytic capacitor, which is interposed between a pair of electrodes and is used in an aluminum electrolytic capacitor having a conductive polymer as a cathode material, comprising: The separator is made of synthetic fibers and a binder, the synthetic fibers are comprised of fibrillated synthetic fibers and non-fibrillated synthetic fibers; The separator contains 70 to 95% by mass of the synthetic fiber and 5 to 30% by mass of the binder, and contains 20 to 70% by mass of the fibrillated synthetic fiber and 10 to 75% by mass of the non-fibrillated synthetic fiber based on the total mass of the separator; The thickness is 20 to 100 μm and the density is 0.2 to 0.6 g / cm 3 ; The fibrillated synthetic fiber contains only one or more fibers selected from the group consisting of polyamide fiber, acrylic fiber, polyester fiber, and vinylon fiber, The non-fibrillated synthetic fibers contain only fibers selected from one or more of nylon fibers, acrylic fibers, polyester fibers, and vinylon fibers, Burst strength: 40-180 kPa, specific burst strength: 3.5-7.5 kPa / (g / m 2 ), the tensile modulus is 500 to 1710 MPa 1. A separator for an aluminum electrolytic capacitor comprising:
2. An aluminum electrolytic capacitor using a conductive polymer as a cathode material, 2. An aluminum electrolytic capacitor comprising the separator according to claim 1.
Citation Information
Patent Citations
Separator for electrochemical element
JP2004146137A
Separator for solid-state electrolytic capacitor
JP2004235293A
Evaluation method of alkaline dry cell and separator for alkaline dry cell
JP2006019094A
Separator for capacitor, and capacitor arranged by use thereof
JP2014183235A
Separator for aluminum electrolytic capacitors and aluminum electrolytic capacitor