Capacitor, electric circuit, circuit board, and apparatus

The use of a tantalum oxide film with a specific fluorine distribution structure in capacitors addresses the issue of capacity reduction and dielectric loss tangent increase when a solid electrolyte is introduced, achieving high capacitance and low energy loss.

WO2024248112A1PCT designated stage expired Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD

Patent Information

Application Number
PCT/JP2024/019959
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional capacitors using tantalum oxide with fluorine experience capacity reduction when a solid electrolyte is introduced, due to the affinity and contact area changes between the fluorine-containing tantalum oxide film and the solid electrolyte, leading to decreased capacitance and increased dielectric loss tangent.

Method used

A tantalum oxide film with a specific structure is employed, comprising a first part with high fluorine concentration, a second part with lower fluorine concentration closer to the solid electrolyte, and a third part with lower fluorine concentration closer to the metal tantalum, which helps maintain high capacitance and low dielectric loss tangent by controlling fluorine distribution and affinity.

Benefits of technology

The capacitor exhibits a capacitance ratio of 83% or more and a dielectric loss tangent of 0.20 or less at 1 Hz to 10 kHz, effectively suppressing capacity reduction and maintaining high performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019959_05122024_PF_FP_ABST
    Figure JP2024019959_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A capacitor 1a includes metal tantalum 10, a solid electrolyte 20, and a tantalum oxide film 30. The tantalum oxide film 30 is disposed between the metal tantalum 10 and the solid electrolyte 20. A first portion 31 contains fluorine. A second portion 32 is in contact with the first portion 31 at a position that is closer to the solid electrolyte 20 than the first portion 31 in the thickness direction of the tantalum oxide film 30. The concentration of fluorine in the second portion 32 is lower than the concentration of fluorine in the first portion 31.
Need to check novelty before this filing date? Find Prior Art

Description

Capacitors, electric circuits, circuit boards, and devices

[0001] The present disclosure relates to capacitors, electric circuits, circuit boards, and devices.

[0002] It is known that fluorine-containing tantalum oxide is used in capacitors.

[0003] For example, Patent Document 1 describes a solid electrolytic capacitor having a dielectric layer made of fluorine-containing tantalum oxide. The dielectric layer is formed by anodizing a tantalum anode in an aqueous solution containing fluorine ions. An electrolyte layer made of manganese dioxide is formed on the dielectric layer.

[0004] Non-Patent Document 1 describes that the relative dielectric constant of a polycrystalline TaO2F thin film is 60 at 1 MHz.

[0005] Japanese Patent Application Laid-Open No. 2005-294402

[0006] Journal of Materials Chemistry C, (English), 2020, Issue 14, p.4680-4684

[0007] The present disclosure provides a capacitor that uses fluorine-containing tantalum oxide and is advantageous from the viewpoint of suppressing capacity reduction due to a solid electrolyte.

[0008] A capacitor according to the present disclosure comprises: metallic tantalum; a solid electrolyte; and a tantalum oxide film disposed between the metallic tantalum and the solid electrolyte, wherein the tantalum oxide film includes a first portion containing fluorine and a second portion in contact with the first portion at a position closer to the solid electrolyte than the first portion in a thickness direction of the tantalum oxide film, and the fluorine concentration in the second portion is lower than the fluorine concentration in the first portion.

[0009] According to the present disclosure, a capacitor can be provided that uses fluorine-containing tantalum oxide and is advantageous from the viewpoint of suppressing a decrease in capacity due to a solid electrolyte.

[0010] FIG. 1 is a cross-sectional view showing an example of a capacitor according to the present disclosure. FIG. 2 is a cross-sectional view showing another example of a capacitor according to the present disclosure. FIG. 3A is a cross-sectional view showing yet another example of a capacitor according to the present disclosure. FIG. 3B is a cross-sectional view showing yet another example of a capacitor according to the present disclosure. FIG. 4A is a diagram schematically showing an example of an electric circuit according to the present disclosure. FIG. 4B is a diagram schematically showing an example of a circuit board according to the present disclosure. FIG. 4C is a diagram schematically showing an example of an instrument according to the present disclosure. FIG. 6 is a graph showing the relationship between the atomic ratio of fluorine (F), tantalum (Ta), and oxygen (O) and depth in a depth profile obtained by Rutherford backscattering spectroscopy (RBS) of a sample according to Example 1A. FIG. 7 is a graph showing the relationship between the atomic ratio of fluorine (F), tantalum (Ta), and oxygen (O) and depth in a depth profile obtained by time-of-flight secondary ion mass spectrometry (TOF-SIMS) of a sample according to Example 1B. - , TaO 3- , and O - 7 is a graph showing the relationship between the signal intensity and depth of F in the depth profile obtained by TOF-SIMS of the sample according to Comparative Example 1. - , TaO 3- , and O - 8 is a graph showing the relationship between signal intensity and depth in Examples 2A to 2E and Comparative Example 2. FIG. 9 is a graph showing the XRD pattern of the dielectric film of the sample according to Reference Example 1. FIG. 10 is a graph showing the relationship between signal intensity and depth in the depth profile of the sample according to Reference Example 1 by TOF-SIMS. - , TaO 3- , and O - 11 is a graph showing the relationship between the signal intensity and depth of F in the depth profile obtained by TOF-SIMS of the sample according to Comparative Example 3. - , TaO 3- , and O - 12A is a graph showing the relationship between the capacitance of a capacitor and frequency. FIG. 12B is a graph showing the relationship between the capacitance of a capacitor and frequency. FIG. 13A is a graph showing the relationship between the dielectric loss tangent tanδ of a capacitor and frequency. FIG. 13B is a graph showing the relationship between the dielectric loss tangent tanδ of a capacitor and frequency.

[0011] (Knowledge forming the basis of the present disclosure) For example, there is a continuous demand for improving the processing performance of electronic devices. The performance of electronic components such as capacitors has a significant impact on the performance of electronic devices incorporating those electronic components. For this reason, it is expected that there will be an increasing need for capacitors that are small and can exhibit high performance. For example, electrolytic capacitors are known as capacitors. In electrolytic capacitors, a dielectric consisting of a thin oxide film is formed on the surface of metallic aluminum or metallic tantalum by chemical conversion treatment of aluminum or tantalum. In electrolytic capacitors, attempts have been made to increase the capacitance of the capacitor mainly by increasing the specific surface area of ​​the dielectric. However, such attempts have shown limitations, and it is believed that the performance of capacitors can be further improved if a dielectric material with a higher dielectric constant could be developed.

[0012] For example, the polycrystalline TaOF thin film described in Non-Patent Document 1 has a high dielectric constant. It is believed that polycrystalline tantalum oxyfluorides have a different crystalline state from tantalum oxide TaO, resulting in increased polarization and a high dielectric constant. Additionally, the inventors have found that fluorine-containing tantalum oxides, even when amorphous, have a higher dielectric constant than fluorine-free tantalum oxide TaO. Thus, the use of fluorine-containing tantalum oxide in a capacitor is expected to increase the capacitance of the capacitor. Meanwhile, the inventors' studies have revealed that placing a solid electrolyte in contact with a fluorine-containing tantalum oxide film can result in a decrease in the capacitance of the capacitor.

[0013] The reason why the capacitance of a capacitor decreases when a solid electrolyte is placed in contact with a fluorine-containing tantalum oxide film is unclear, but the inventors suspect that the affinity between the fluorine-containing tantalum oxide film and the solid electrolyte affects the contact area between the fluorine-containing tantalum oxide film and the solid electrolyte, resulting in a decrease in the capacitance of the capacitor.

[0014] In light of these circumstances, the present inventors conducted extensive research into the configuration of a capacitor that uses fluorine-containing tantalum oxide and that suppresses capacity loss due to a solid electrolyte. As a result, they discovered that a tantalum oxide film with a specific configuration is advantageous for suppressing capacity loss due to a solid electrolyte. Based on this new finding, the present inventors have completed the capacitor of the present disclosure.

[0015] (Embodiments) Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. The present disclosure is not limited to the following embodiments.

[0016] FIG. 1 is a cross-sectional view showing an example of a capacitor according to the present disclosure. As shown in FIG. 1 , a capacitor 1 a includes metal tantalum 10, a solid electrolyte 20, and a tantalum oxide film 30. The tantalum oxide film 30 is disposed between the metal tantalum 10 and the solid electrolyte 20. The tantalum oxide film 30 includes a first portion 31 and a second portion 32. The tantalum oxide film 30 further includes, for example, a third portion 33. The first portion 31 contains fluorine. The second portion 32 contacts the first portion 31 at a position closer to the solid electrolyte 20 than the first portion 31 in the thickness direction of the tantalum oxide film 30. The third portion 33 contacts the first portion 31 at a position closer to the metal tantalum 10 than the first portion 31 in the thickness direction of the tantalum oxide film 30. In other words, the first portion 31 is disposed, for example, between the second portion 32 and the third portion 33 in the thickness direction of the tantalum oxide film 30. In the tantalum oxide film 30 , the fluorine concentration in the second portion 32 and the fluorine concentration in the third portion 33 are lower than the fluorine concentration in the first portion 31 .

[0017] Because the tantalum oxide film 30 includes the first portion 31 containing fluorine, it is likely to have a high dielectric constant. Therefore, the capacitor 1a is likely to have a high capacitance. Because the tantalum oxide film 30 includes the second portion 32, a decrease in capacitance due to the solid electrolyte 20 is likely to be suppressed. Although the reason for this is not clear, it is thought that this is because the affinity between the tantalum oxide film 30 and the solid electrolyte 20 is likely to be high, and the contact area between the tantalum oxide film 30 and the solid electrolyte 20 is likely to be large.

[0018] The capacitance ratio of the capacitor 1a is, for example, 83% or more. The capacitance ratio is the ratio C1 / C0 of the capacitance C1 of the capacitor 1a to the capacitance C0 before the solid electrolyte 20 is provided on the capacitor 1a. The capacitances C0 and C1 can be determined, for example, according to the method described in the examples.

[0019] According to Patent Document 1, the dielectric layer is formed by anodizing a tantalum anode in an aqueous solution containing fluorine ions. According to Patent Document 1, the dielectric layer is formed of tantalum oxide containing fluorine, thereby reducing the equivalent series resistance (ESR) of the electrolytic capacitor. According to the inventors' research, the dielectric dissipation factor of a film obtained by anodizing tantalum in an aqueous solution containing fluorine ions can be increased. In such a film, the ion diffusion rate of fluoride ions is more than twice the ion diffusion rate of oxide ions. Depending on the anodization conditions, fluorine may accumulate at the interface between the tantalum oxide and elemental tantalum, forming a region with a high fluorine concentration. The formation of a region with a high fluorine concentration at the interface between the tantalum oxide and elemental tantalum is thought to increase the dielectric dissipation factor of the film. Meanwhile, since the tantalum oxide film 30 contains, for example, the third portion 33, the fluorine concentration at the interface between the tantalum oxide film 30 and the metal tantalum 10 is unlikely to increase. This makes the dielectric dissipation factor of the capacitor 1a likely to be low.

[0020] The dielectric loss tangent of the capacitor 1a is, for example, 0.20 or less at frequencies from 1 Hz to 10 kHz.

[0021] As shown in FIG. 1, each of the first region 31, the second region 32, and the third region 33 is, for example, a layer-like region.

[0022] The boundary between the first portion 31 and the second portion 32 and the boundary between the first portion 31 and the third portion 33 in the tantalum oxide film 30 can be determined according to, for example, a depth profile obtained by TOF-SIMS. For example, in the depth profile obtained by TOF-SIMS, fluoride ions (F -) is measured. In addition, a pair of depths corresponding to half of the maximum value are identified in the depth profile. Of the pair of depths, the position corresponding to the depth closest to the metal tantalum 10 is determined as the boundary between the first region 31 and the third region 33, and the position corresponding to the other depth is determined as the boundary between the first region 31 and the second region 32. The boundary between the first region 31 and the second region 32 and the boundary between the first region 31 and the third region 33 in the tantalum oxide film 30 may be determined by Rutherford backscattering spectroscopy (RBS).

[0023] In the capacitor 1a, the boundary between the metal tantalum 10 and the tantalum oxide film 30 can be determined according to, for example, a depth profile obtained by TOF-SIMS. For example, in the depth profile, the boundary between the metal tantalum 10 and the tantalum oxide film 30 can be determined by determining the presence of tantalum oxide ions (TaO 3- The maximum value of the signal of the tantalum metal 10 is identified. The depth corresponding to half the maximum value is identified, and the position corresponding to that depth is determined as the boundary between the tantalum metal 10 and the tantalum oxide film 30. The boundary between the tantalum metal 10 and the tantalum oxide film 30 may be determined by RBS.

[0024] As long as the concentration of fluorine in the second portion 32 is lower than the concentration of fluorine in the first portion 31, the depth profile of the tantalum oxide film 30 by TOF-SIMS and RBS is not limited to a particular embodiment. 31F Average A for 33F Ratio A 33F / A 31F is 0.5 or less. 31F is a fluoride ion (F - ) is the average value of the signal intensities of the 33F is a fluoride ion (F - ) is the average value of the signal intensities of the solid electrolyte 20. With this configuration, the capacity decrease due to the solid electrolyte 20 is more easily suppressed. 33F / A 31F The ratio A may be 0.2 or less, 0.15 or less, or 0.129 or less. 33F / A 31Fis, for example, 0.01 or more, and may be 0.05 or more or 0.1 or more.

[0025] In the depth profile of the tantalum oxide film 30 by TOF-SIMS, the average value A 31F Average value A 32F Ratio A 32F / A 31F is, for example, 0.9 or less. 32F is a fluoride ion (F - ) is the average value of the signal strengths of the capacitors 1a and 1b. With this configuration, the capacitor 1a is more likely to have a low dielectric tangent. 32F / A 31F The ratio A may be 0.5 or less, 0.4 or less, or 0.379 or less. 32F / A 31F is, for example, 0.01 or more, and may be 0.05 or more or 0.1 or more.

[0026] In the depth profile of elements or ions in the tantalum oxide film 30, oxygen (O) or oxygen ions (O - The coefficient of variation of the signal intensity of oxygen ions (O - ) the fluctuation in signal intensity is small, and capacitor 1a is more likely to have a high capacitance. The coefficient of variation may be 0.088 or less, 0.05 or less, or 0.01 or less. The coefficient of variation can be calculated by dividing the standard deviation by the average value.

[0027] Thickness t of the tantalum oxide film 30 30 is not limited to a specific value. 30 is, for example, 1 nm or more and 1 μm or less.

[0028] The first portion 31 may be crystalline or amorphous. Even if the first portion 31 is amorphous, the tantalum oxide film 30 is likely to have a high dielectric constant, and the capacitor 1a is likely to have a high capacitance. For example, the object can be determined to be amorphous when a broad halo pattern is shown in an XRD pattern of the object using Cu-Kα radiation at a diffraction angle 2θ of 10° to 50°.

[0029] The second portion 32 may be crystalline or amorphous, and the third portion 33 may be crystalline or amorphous.

[0030] The composition of the first portion 31 is not limited to a specific composition as long as the concentration of fluorine in the second portion 32 is lower than the concentration of fluorine in the first portion 31. The first portion 31 does not contain, for example, silicon or titanium. The first portion 31 may contain, for example, TaO x1 F y1 This composition satisfies, for example, the conditions 0<x1<2.5 and 0<y1≦0.4. In this case, the tantalum oxide film 30 is likely to have a high relative dielectric constant, and the capacitor 1a is likely to have a high capacitance. Furthermore, the fluorine contained in the tantalum oxide film 30 is likely to be prevented from diffusing toward the metal tantalum 10 due to the influence of an electric field, heat, and the like, and the dielectric loss tangent is likely to be low.

[0031] In the above composition, for example, the condition y1≧0.015 is satisfied. In this case, the tantalum oxide film 30 is more likely to have a high relative dielectric constant, and the capacitor 1a is more likely to have a high capacitance. In the above composition, the condition y1≧0.016, y1≧0.017, y1≧0.018, y1≧0.019, y1≧0.02, or y1≧0.03 may be satisfied. In the above composition, y1≦0.3 or y1≦0.2 may also be satisfied.

[0032] The fluorine concentration in the second region 32 is not limited to a specific value as long as the fluorine concentration in the second region 32 is lower than the fluorine concentration in the first region 31. x2 F y2This composition satisfies, for example, the conditions 0<x2<2.5 and 0≦y2<0.015. In this case, the capacity decrease due to the solid electrolyte is more likely to be suppressed.

[0033] The fluorine concentration in the third region 33 is not limited to a specific value as long as the fluorine concentration in the third region 33 is lower than the fluorine concentration in the first region 31. The third region 33 may be, for example, TaO x3 F y3 This composition satisfies, for example, the conditions 0<x3<2.5 and 0≦y3<0.015. In this case, the fluorine concentration near the metal tantalum 10 in the tantalum oxide film 30 is less likely to become high, and the dielectric loss tangent of the capacitor 1a is more likely to become low.

[0034] The values ​​of x1, y1, x2, y2, x3, and y3 in the above composition can be determined based on the results of RBS, for example. The values ​​of x1, y1, x2, y2, x3, and y3 may also be determined by combining TOF-SIMS with another analytical method such as RBS.

[0035] The solid electrolyte 20 is not limited to a specific solid electrolyte. The solid electrolyte 20 may include, for example, a conductive polymer or a manganese compound such as manganese oxide. Examples of conductive polymers include polypyrrole, polythiophene, polyaniline, and derivatives thereof. The solid electrolyte 20 may be, for example, a layer.

[0036] 1 , the capacitor 1 a further includes, for example, a conductor 40. The solid electrolyte 20 is disposed between the tantalum oxide film 30 and the conductor 40 in the thickness direction of the tantalum oxide film 30. The material of the conductor 40 is not limited to a specific material. The conductor 40 may contain a valve metal such as aluminum, tantalum, niobium, or bismuth, a noble metal such as gold or platinum, or nickel. The conductor 40 may also contain a carbon material such as graphite.

[0037] In the capacitor 1 a, for example, the conductor 40 and the solid electrolyte 20 form a cathode.

[0038] The method for forming the tantalum oxide film 30 is not limited to any particular method. The tantalum oxide film 30 can be formed, for example, by methods including the following (I), (II), and (III): (I) Anodizing the metallic tantalum while the metallic tantalum is in contact with a fluorine-free aqueous solution to form an oxide layer in contact with the metallic tantalum; (II) Anodizing the metallic tantalum while the oxide layer formed in (I) is in contact with a fluorine-containing aqueous solution to obtain an oxide layer; (III) Anodizing the metallic tantalum while the oxide layer formed in (II) is in contact with a fluorine-free aqueous solution to obtain a tantalum oxide film 30 including a first portion 31, a second portion 32, and a third portion 33.

[0039] In anodization, for example, a voltage of several volts [V] to several hundred volts [V] is applied between the anode and cathode with an electrolyte disposed between them. For example, a voltage of 5 volts [V] to 300 volts [V] is applied. When metallic tantalum is used as the anode, anions attracted toward the metallic tantalum combine with ionized tantalum to form a chemical film. Impurities such as ions or atoms derived from the electrolyte present around the anode may be incorporated into the chemical film. For this reason, it is virtually impossible to form a film consisting of only two specific elements, such as tantalum and oxygen, in anodization using metallic tantalum as the anode. Therefore, for example, the second portion 32 and the third portion 33 may contain elements other than tantalum and oxygen, such as fluorine, at a concentration of 0.4% or less by atomic number.

[0040] Fig. 2 is a cross-sectional view showing another example of a capacitor according to the present disclosure. Capacitor 1b shown in Fig. 2 has the same configuration as capacitor 1a, except for portions that will be particularly described. Components of capacitor 1b that are the same as or correspond to components of capacitor 1a are given the same reference numerals, and detailed description thereof will be omitted. The description of capacitor 1a also applies to capacitor 1b, unless technically inconsistent.

[0041] 2, in capacitor 1b, at least a portion of metal tantalum 10 is porous. With this configuration, the surface area of ​​metal tantalum 10 tends to be large, and capacitor 1b tends to have a high capacitance. Such a porous structure can be formed, for example, by etching a metal foil and sintering a powder.

[0042] 2, a tantalum oxide film 30 is disposed on the surface of the porous portion of the metal tantalum 10. The tantalum oxide film 30 is formed, for example, by anodization. A solid electrolyte 20 is disposed so as to fill the voids around the porous portion of the tantalum oxide film 30. In the capacitor 1b, for example, the cathode is formed by a conductor 40 and the solid electrolyte 20. The conductor 40 may include, for example, a solidified silver-containing paste, a carbon material such as graphite, or both the solidified material and a carbon material.

[0043] 3A and 3B are cross-sectional views showing yet another example of a capacitor according to the present disclosure. Capacitor 1c shown in FIG. 3A and capacitor 1d shown in FIG. 3B are configured similarly to capacitors 1a and 1b, respectively, except for portions that are particularly described. Components of capacitor 1c or capacitor 1d that are identical to or correspond to components of capacitor 1a or capacitor 1b are denoted by the same reference numerals, and detailed description thereof will be omitted. The descriptions of capacitors 1a and 1b also apply to capacitors 1c and 1d, unless technically inconsistent.

[0044] 3A and 3B , in capacitors 1c and 1d, the tantalum oxide film 30 includes the first portion 31 and the second portion 32 but does not include the third portion 33. In capacitors 1c and 1d, for example, the first portion 31 is in contact with the metal tantalum 10. Even with this configuration, the tantalum oxide film 30 includes the second portion 32, which makes it easy to suppress a decrease in capacitance due to the solid electrolyte 20. Such a tantalum oxide film 30 can be produced, for example, by adjusting the conditions for anodization (III) in the method including the above-mentioned methods (I), (II), and (III). For example, such a tantalum oxide film 30 can be easily obtained by increasing the voltage applied between the anode and cathode in the anodization (III).

[0045] 4A is a diagram schematically illustrating an example of an electric circuit according to the present disclosure. The electric circuit 3 includes a capacitor 1a. The electric circuit 3 may be an active circuit or a passive circuit. The electric circuit 3 may be a discharge circuit, a smoothing circuit, a decoupling circuit, or a coupling circuit. Because the electric circuit 3 includes the capacitor 1a, the electric circuit 3 is likely to exhibit the desired performance. For example, noise is likely to be reduced in the electric circuit 3. The electric circuit 3 may also include a capacitor 1b.

[0046] 4B is a diagram schematically illustrating an example of a circuit board according to the present disclosure. As shown in FIG. 4B, the circuit board 5 includes a capacitor 1a. For example, an electric circuit 3 including the capacitor 1a is formed on the circuit board 5. Since the circuit board 5 includes the capacitor 1a, the circuit board 5 is likely to exhibit the desired performance. The circuit board 5 may be an embedded board or a motherboard. The circuit board 5 may also include a capacitor 1b.

[0047] FIG. 4C is a schematic diagram illustrating an example of a device according to the present disclosure. As shown in FIG. 4C , the device 7 includes a capacitor 1a. The device 7 includes, for example, a circuit board 5 including the capacitor 1a. Because the device 7 includes the capacitor 1a, the device 7 is likely to exhibit desired performance. The device 7 may be an electronic device, a communication device, a signal processing device, or a power supply. The device 7 may be a server, an AC adapter, an accelerator, or a flat panel display such as a liquid crystal display (LCD). The device 7 may be a USB charger, a solid-state drive (SSD), an information terminal such as a PC, a smartphone, or a tablet PC, or an Ethernet switch. The device 7 may also include a capacitor 1b.

[0048] (Supplementary Note) The above description discloses the following technologies. (Technology 1) A capacitor comprising: metallic tantalum; a solid electrolyte; and a tantalum oxide film disposed between the metallic tantalum and the solid electrolyte, wherein the tantalum oxide film includes a first portion containing fluorine and a second portion in contact with the first portion at a position closer to the solid electrolyte than the first portion in the thickness direction of the tantalum oxide film, and wherein the fluorine concentration in the second portion is lower than the fluorine concentration in the first portion. (Technology 2) The capacitor according to claim 1, wherein the tantalum oxide film further includes a third portion in contact with the first portion at a position closer to the metallic tantalum than the first portion in the thickness direction of the tantalum oxide film, and wherein the fluorine concentration in the third portion is lower than the fluorine concentration in the first portion. (Technology 3) The capacitor according to claim 1, wherein the first portion is amorphous. (Technology 4) The first portion is TaO x1 F y1 The capacitor according to any one of techniques 1 to 3, wherein the second portion has a composition expressed by the formula: x2 F y2The capacitor according to any one of techniques 1 to 4, having a composition expressed by the following formula: wherein the composition satisfies the conditions of 0<x2<2.5 and 0≦y2<0.015. (Technology 6) The third portion is TaO x3 F y3 The capacitor according to Technology 2 has a composition expressed by the following formula: wherein the composition satisfies the conditions of 0<x3<2.5 and 0≦y3<0.015. (Technology 7) In a depth profile of elements or ions in the tantalum oxide film, oxygen (O) or oxygen ions O - The capacitor according to any one of Techniques 1 to 6, wherein the coefficient of variation of signal intensity is 0.09 or less. (Technology 8) An electric circuit comprising the capacitor according to any one of Techniques 1 to 7. (Technology 9) A circuit board comprising the capacitor according to any one of Techniques 1 to 7. (Technology 10) An apparatus comprising the capacitor according to any one of Techniques 1 to 7.

[0049] The present disclosure will be described in more detail below with reference to examples. Note that the following examples are illustrative and the present disclosure is not limited to the following examples.

[0050] Example 1A: A flat tantalum foil was immersed in acetone and subjected to ultrasonic cleaning for 10 minutes to clean the surface of the tantalum foil. The acetone adhering to the tantalum foil surface was then evaporated, and the tantalum foil surface was then washed with pure water. The tantalum foil was then dried in the atmosphere to obtain an anode foil.

[0051] The above anode foil and a platinum foil as a counter electrode were placed at a predetermined distance so that they were immersed in a phosphoric acid aqueous solution. The part of the anode foil not immersed in the aqueous solution was connected to the positive terminal of a power supply, and the part of the platinum foil not immersed in the aqueous solution was connected to the negative terminal of the power supply. A voltage of 97 V was applied between the anode foil and the platinum foil for 30 minutes, forming an oxide layer containing Ta2O5 on the surface of the anode foil. The anode foil was then removed from the aqueous solution, washed with pure water, and then dried in the air.

[0052] Next, the anode foil with the oxide layer formed and a platinum foil as a counter electrode were placed at a predetermined distance so that they were immersed in an NH4HF2 aqueous solution. The part of the anode foil not immersed in the solution was connected to the positive terminal of a power supply, and the part of the platinum foil not immersed in the solution was connected to the negative terminal of the power supply. A voltage of 156 V was applied between the anode foil and the platinum foil for 10 minutes, forming a fluorine-containing tantalum oxide layer. The anode foil was then removed from the solution, washed with pure water, and then dried in the air.

[0053] Next, the anode foil with the fluorine-containing oxide layer formed thereon and a platinum foil as a counter electrode were placed at a predetermined distance so that they were immersed in a phosphoric acid aqueous solution. The portion of the anode foil not immersed in the aqueous solution was connected to the positive terminal of a power supply, and the portion of the platinum foil not immersed in the aqueous solution was connected to the negative terminal of the power supply. A voltage of 187 V was applied between the anode foil and the platinum foil for 30 minutes to form an oxide layer containing Ta2O5. The anode foil was removed from the aqueous solution, washed with pure water, and then dried in the air. In this way, a sample according to Example 1A was obtained, in which a dielectric film was formed on the surface of metallic tantalum.

[0054] Example 1B: A flat tantalum foil was immersed in acetone and subjected to ultrasonic cleaning for 10 minutes to clean the surface of the tantalum foil. The acetone adhering to the tantalum foil surface was then evaporated, and the tantalum foil surface was then washed with pure water. The tantalum foil was then dried in the atmosphere to obtain an anode foil.

[0055] The above anode foil and a platinum foil as a counter electrode were placed at a predetermined distance so that they were immersed in a phosphoric acid aqueous solution. The portion of the anode foil not immersed in the aqueous solution was connected to the positive terminal of a power supply, and the portion of the platinum foil not immersed in the aqueous solution was connected to the negative terminal of the power supply. A voltage of 30 V was applied between the anode foil and the platinum foil for 13 hours, forming an oxide layer containing Ta2O5 on the surface of the anode foil. The anode foil was then removed from the aqueous solution, washed with pure water, and then dried in the air.

[0056] Next, the anode foil with the oxide layer formed thereon and a platinum foil serving as a counter electrode were placed at a predetermined distance so as to be immersed in a mixed aqueous solution of NaF and sodium phosphate buffer. The portion of the anode foil not immersed in the mixed aqueous solution was connected to the positive terminal of a power supply, and the portion of the platinum foil not immersed in the mixed aqueous solution was connected to the negative terminal of the power supply. A voltage of 75 V was applied between the anode foil and the platinum foil for 4 hours to form a fluorine-containing tantalum oxide layer. The concentrations of NaF and sodium phosphate buffer in the mixed aqueous solution were 0.1 mol / L and 0.05 mol / L, respectively. The anode foil was removed from the mixed aqueous solution, washed with pure water, and then dried in the air.

[0057] Next, the anode foil with the fluorine-containing oxide layer formed thereon and a platinum foil as a counter electrode were placed at a predetermined distance so that they were immersed in a phosphoric acid aqueous solution. The portion of the anode foil not immersed in the aqueous solution was connected to the positive terminal of a power supply, and the portion of the platinum foil not immersed in the aqueous solution was connected to the negative terminal of the power supply. A voltage of 90 V was applied between the anode foil and the platinum foil for 4 hours to form an oxide layer containing Ta2O5. The anode foil was removed from the phosphoric acid aqueous solution, washed with pure water, and then dried in the air. In this way, a sample according to Example 1B was obtained, in which a dielectric film was formed on the surface of metallic tantalum.

[0058] Comparative Example 1 A sample according to Comparative Example 1 was obtained in the same manner as in Example 1B, except that the formation of an additional oxide layer using an aqueous phosphoric acid solution on the anode foil on which a fluorine-containing oxide layer had been formed was omitted.

[0059] (RBS) Using a Pelletron 5SDH-2 RBS system, RBS was performed on samples fabricated from the dielectric layers of the samples of Example 1A and Example 1B. In RBS, an ion beam was irradiated onto the sample under specified conditions to obtain RBS spectra. Figure 5 is a graph showing the relationship between the atomic ratio of fluorine (F), tantalum (Ta), and oxygen (O) and depth in the RBS depth profile of the sample of Example 1A. In Figure 5, the vertical axis represents the atomic ratio of fluorine (F), tantalum (Ta), and oxygen (O), and the horizontal axis represents depth. As shown in Figure 5, the dielectric film of the sample of Example 1A included a region a with a relatively high F concentration and regions b and c with relatively low F concentrations. The boundaries between region a and regions b and c were determined by identifying the depth corresponding to half the maximum F concentration in region a. The boundary between region b and region a is understood to be located at a depth of approximately 80 nm. The boundary between the portion c and the portion a is understood to be at a position corresponding to a depth of about 254 nm. Therefore, the thickness of the portion a is understood to be about 174 nm, and the thickness of the portion b is understood to be about 80 nm. The boundary between the dielectric film and the metal tantalum is understood to be the TaO 3- The depth was determined by identifying the depth corresponding to half the maximum value of the signal intensity of the dielectric film. It was suggested that the boundary between the dielectric film and the metallic tantalum was located at a position corresponding to a depth of approximately 300 nm. Therefore, the thickness of portion c is understood to be approximately 46 nm. No increase in fluorine concentration was confirmed at the boundary between the dielectric film and the metallic tantalum. According to the obtained RBS spectra, the compositions of portion a of the dielectric layer of the samples according to Example 1A and Example 1B were TaO 2.33 F 0.19 and TaO 2.27 F 0.03 The composition of the portion b of the dielectric layer of the samples according to Example 1A and Example 1B was TaO 2.47 and TaO 2.48 The elemental concentration of fluorine in the portion b of the samples according to Example 1A and Example 1B was lower than the analytical lower limit of 0.4 mass %, and TaO x2 F y2In the composition represented by the formula (1), y2 was less than 0.015. The elemental concentration of fluorine in the portion c of the samples according to Example 1A and Example 1B was lower than the analytical lower limit of 0.4 mass %, and TaO x3 F y3 In the composition expressed as above, y3<0.015.

[0060] The dielectric films of the samples according to Example 1A and Example 1B have the portion b, and therefore, when comparing Examples 2A to 2E with Comparative Example 2 described later, it is believed that the reduction in capacity due to the solid electrolyte is more easily suppressed than in the sample according to Comparative Example 1. In addition, since the samples according to Example 1A and Example 1B have the portion c, it is believed that the dielectric loss tangent of the capacitor is more easily reduced according to Reference Example 1 described later.

[0061] (TOF-SIMS) Pieces of a predetermined size were cut out from the samples according to Example 1B and Comparative Example 1, and samples for TOF-SIMS were prepared by embedding them in resin. Using a TOF-SIMS device TOF.SIMS5 manufactured by ION-TOF, TOF-SIMS was performed on the samples prepared from the samples according to Example 1B and Comparative Example 1, and composition analysis was performed in the depth direction of the dielectric film. In TOF-SIMS, a Bi beam was used as the primary ion beam. O2 was used as the sputtering ion species. + FIG. 6 shows the fluoride ion (F) in the depth profile of the sample according to Example 1B by TOF-SIMS. - ), tantalate ion (TaO 3- ), and oxygen ions (O - 7 is a graph showing the relationship between the signal intensity of F in the depth profile of the sample according to Comparative Example 1 by TOF-SIMS. - , tantalate ion TaO 3- , and O - 6 and 7 are graphs showing the relationship between the signal intensity of each ion and the depth. In Fig. 6 and Fig. 7, the vertical axis shows the signal intensity of each ion, and the horizontal axis shows the depth in the dielectric film.

[0062] As shown in FIG. 6, the dielectric film of the sample according to Example 1B is F - A region a where the signal intensity of F is relatively high- The boundary between site a and sites b and c is the F - The boundary between the region b and the region a is understood to be located at a position corresponding to a depth of about 43 nm. The boundary between the region c and the region a is understood to be located at a position corresponding to a depth of about 170 nm. Therefore, the thickness of the region a is understood to be about 127 nm, and the thickness of the region b is understood to be about 43 nm. The boundary between the dielectric film and the metal tantalum is understood to be located at a position corresponding to a depth of about 170 nm. 3- The depth was determined by identifying the depth corresponding to half the maximum value of the signal intensity of the dielectric film. It was suggested that the boundary between the dielectric film and the metallic tantalum was located at a position corresponding to a depth of approximately 176 nm. Therefore, the thickness of portion c is understood to be approximately 6 nm. No increase in fluorine concentration was confirmed at the boundary between the dielectric film and the metallic tantalum.

[0063] In the region b and the region a, O - No significant fluctuations were observed in the signal intensity, and the coefficient of variation of the signal intensity was approximately 0.088.

[0064] 7, it is understood that the dielectric film of the sample according to Comparative Example 1 is present from its surface to a depth of about 180 nm. In the sample according to Comparative Example 1, the fluorine concentration was almost constant from the surface of the dielectric film to a depth of about 170 nm.

[0065] Example 2A One longitudinal end of a rod-shaped anode lead made of metallic tantalum was embedded in metallic tantalum powder, and the tantalum powder was molded into a rectangular parallelepiped compact. This compact was sintered to obtain an anode body having a porous structure in which one end of the anode lead was embedded.

[0066] Next, the anode body was immersed in an aqueous phosphoric acid solution, and a voltage of 40 V was applied to the anode body using an anode lead for 13 hours to form an oxide layer containing TaO on the surface of the anode body. The anode body was then removed from the aqueous phosphoric acid solution, washed with pure water, and then dried for 10 minutes in a drying oven adjusted to 100°C.

[0067] Next, the anode body with the oxide layer formed thereon was immersed in an aqueous NHHF solution, and a voltage of 80 V was applied to the anode body for 10 minutes using an anode lead, thereby forming a fluorine-containing tantalum oxide layer on the surface of the anode body.

[0068] Next, the anode body with the fluorine-containing oxide layer formed thereon was immersed in an aqueous phosphoric acid solution, and a voltage of 80 V was applied to the anode body using an anode lead for 30 minutes to form an oxide layer containing TaO. The anode body was removed from the aqueous phosphoric acid solution, washed with pure water, and then dried for 10 minutes in a drying oven adjusted to 100°C. In this manner, 100 anode bodies with a dielectric film according to Example 2A were obtained, each having a dielectric film formed on its surface.

[0069] Next, a solid electrolyte layer containing polythiophene was formed on the surface of the dielectric film of 50 of the dielectric film-coated anode bodies according to Example 2A by chemical polymerization.

[0070] Next, a graphite particle suspension was applied to the solid electrolyte layer and dried in the air to form a carbon-containing layer, and then a silver particle solution was applied to the carbon-containing layer and dried in the air to form a silver-containing layer. In this way, the capacitor according to Example 2A was fabricated.

[0071] Example 2B: An anode body prepared by sintering a compact of tantalum powder in the same manner as in Example 1A was immersed in an aqueous phosphoric acid solution, and a voltage of 30 V was applied to the anode body for 13 hours using an anode lead to form an oxide layer containing TaO on the surface of the anode body. The anode body was removed from the aqueous phosphoric acid solution, washed with pure water, and then dried for 10 minutes in a drying furnace adjusted to 100°C.

[0072] Next, the anode body with the oxide layer formed thereon was immersed in a mixed solution of NaF and sodium phosphate buffer, and a voltage of 83 V was applied to the anode body for 4 hours using an anode lead, thereby forming a fluorine-containing tantalum oxide layer on the surface of the anode body.

[0073] Next, the anode body with the fluorine-containing oxide layer formed thereon was immersed in an aqueous phosphoric acid solution, and a voltage of 88 V was applied to the anode body using an anode lead for 4 hours to form an oxide layer containing TaO. The anode body was removed from the aqueous phosphoric acid solution, washed with pure water, and then dried for 10 minutes in a drying oven adjusted to 100°C. In this manner, 100 anode bodies with a dielectric film according to Example 2B were obtained, each having a dielectric film formed on its surface.

[0074] Next, in the same manner as in Example 2A, a solid electrolyte layer, a carbon-containing layer, and a silver-containing layer were formed on the surfaces of the dielectric films of 50 of the dielectric film-coated anode bodies according to Example 2B, thereby producing capacitors according to Example 2B.

[0075] Examples 2C to 2E Dielectric film-coated anode bodies of Examples 2C, 2D, and 2E were obtained in the same manner as Example 2B, except that the voltage applied to the anode body during the formation of the fluorine-containing oxide layer was changed to 78 V, 73 V, and 68 V. The number of dielectric film-coated anode bodies obtained for each of Examples 2C, 2D, and 2E was 100. Fifty capacitors each of Examples 2C, 2D, and 2E were fabricated in the same manner as Example 2B, except that fifty dielectric film-coated anode bodies each of Examples 2C, 2D, and 2E were used instead of the fifty dielectric film-coated anode bodies of Example 2B.

[0076] <Comparative Example 2> An anode body with a dielectric film according to Comparative Example 2 was obtained in the same manner as in Example 2B, except that the voltage applied to the anode body during the formation of the fluorine-containing oxide layer was changed to 88 V and the subsequent formation of a further oxide layer using an aqueous phosphoric acid solution was omitted. The number of dielectric film-coated anode bodies according to Comparative Example 2 obtained was 100. A capacitor according to Comparative Example 2 was fabricated in the same manner as in Example 2B, except that 50 dielectric film-coated anode bodies according to Comparative Example 2 were used instead of the 50 dielectric film-coated anode bodies according to Example 2B.

[0077] (Capacitance Evaluation) Using an LCR meter for four-terminal measurement, the capacitance at a frequency of 120 Hz was measured for the dielectric film-coated anode bodies and capacitors of Examples 2A, 2B, 2C, 2D, and 2E and Comparative Example 2. The results are shown in Table 1. The results are the arithmetic average of the measurements for 50 dielectric film-coated anode bodies and 50 capacitors. In each Example and Comparative Example 2, the ratio C1 / C0 of the capacitance C1 of the capacitor to the capacitance C0 of the dielectric film-coated anode body was defined as the capacitance ratio. Figure 8 is a graph showing the capacitance ratios for Examples 2A to 2E and Comparative Example 2. The vertical axis in this graph represents the capacitance ratio.

[0078] As shown in Table 1, the capacitances of the capacitors according to Example 2A, Example 2B, Example 2C, Example 2D, Example 2E, and Comparative Example 2 were lower than the capacitances of the dielectric film-coated anode bodies according to Example 2A, Example 2B, Example 2C, Example 2D, Example 2E, and Comparative Example 2. This suggests that the solid electrolyte is not in contact with the entire dielectric film.

[0079] As shown in FIG. 8 , the capacity ratios in Examples 2A to 2E were 83% or higher, which was higher than the capacity ratio in Comparative Example 2. This is thought to be because the further oxide layer formed using an aqueous phosphoric acid solution on the anode body on which the fluorine-containing oxide layer was formed had a high affinity with the solid electrolyte, resulting in a larger contact area between the dielectric film and the solid electrolyte. As shown in FIG. 8 , it was confirmed that the capacity ratio tends to increase when a low voltage is applied to the anode body during the formation of the fluorine-containing oxide layer. It is thought that when a low voltage is applied to the anode body during the formation of the fluorine-containing oxide layer, the thickness of the further oxide layer formed using an aqueous phosphoric acid solution on the anode body on which the fluorine-containing oxide layer was formed accounts for a larger proportion of the thickness of the dielectric film. This suggests that a low voltage applied to the anode body during the formation of the fluorine-containing oxide layer is likely to increase the capacity ratio.

[0080]

[0081] Reference Example 1: A flat plate of metallic tantalum was immersed in acetone and subjected to ultrasonic cleaning for 10 minutes to clean the surface of the metallic tantalum. Thereafter, the acetone adhering to the surface of the metallic tantalum was evaporated, and the surface of the metallic tantalum was washed with pure water, and then the metallic tantalum was dried in the atmosphere.

[0082] Next, the above metal tantalum and a platinum foil as a counter electrode were placed at a predetermined distance so as to be immersed in the phosphoric acid aqueous solution. The part of the metal tantalum not immersed in the aqueous solution was connected to the positive electrode of a power supply, and the part of the platinum foil not immersed in the aqueous solution was connected to the negative electrode of the power supply. A current was applied from the power supply in a constant voltage state, and a voltage of 64 V was applied between the metal tantalum and the counter electrode for 30 minutes. This caused an electrochemical reaction on the surface of the metal tantalum, which was the anode, to form an oxide film. The metal tantalum on which the oxide film had been formed was removed from the aqueous solution, washed with pure water, and dried in the air.

[0083] Next, the above-mentioned metal tantalum with the oxide film formed thereon was used as an anode, and platinum foil was used as a cathode, and they were placed at a predetermined distance so as to be immersed in an NH4HF2 aqueous solution. The portions of the anode and cathode that were not immersed in the aqueous solution were connected to the positive and negative electrodes of a power supply, respectively. A current was applied from the power supply in a constant voltage state, and a voltage of 80 V was applied between the anode and cathode for 10 minutes, thereby performing anodization. Thereafter, the anodized anode was removed from the aqueous solution, washed with pure water, and dried. In this way, a sample according to Reference Example 1, in which a dielectric film was formed on the surface of metal tantalum, was obtained.

[0084] Comparative Example 3: A flat plate of metallic tantalum was immersed in acetone and subjected to ultrasonic cleaning for 10 minutes to clean the surface of the metallic tantalum. Thereafter, the acetone adhering to the surface of the metallic tantalum was evaporated, and the surface of the metallic tantalum was washed with pure water, and then the metallic tantalum was dried in the atmosphere.

[0085] Next, metallic tantalum was used as an anode and platinum foil as a cathode, placed at a predetermined distance so as to be immersed in an NH4HF2 aqueous solution, and the portions of the anode and cathode not immersed in the aqueous solution were connected to the positive and negative terminals of a power supply, respectively. A current was applied from the power supply in a constant voltage state, and a voltage of 80 V was applied between the anode and cathode for 10 minutes, performing anodization. The anodized anode was then removed from the aqueous solution, washed with pure water, and dried. In this way, a sample according to Comparative Example 3 was obtained, in which a dielectric film was formed on the surface of metallic tantalum.

[0086] Comparative Example 4: The surface of metallic tantalum was cleaned by ultrasonic cleaning for 10 minutes while immersed in a container filled with acetone. The acetone adhering to the surface of the metallic tantalum was then evaporated, and the surface of the metallic tantalum was washed with pure water. The metallic tantalum was then dried in the atmosphere.

[0087] Next, the tantalum metal and a platinum foil as a counter electrode were placed at a predetermined distance so as to be immersed in the phosphoric acid aqueous solution. The portion of the tantalum metal not immersed in the aqueous solution was connected to the positive electrode of a power supply, and the portion of the platinum foil not immersed in the aqueous solution was connected to the negative electrode of the power supply. A current was applied from the power supply at a constant voltage, and a voltage of 80 V was applied between the tantalum metal and the counter electrode for 30 minutes. An electrochemical reaction was caused to occur on the surface of the tantalum metal, which served as the anode, to obtain an oxide film. The tantalum metal with the oxide film formed was removed from the aqueous solution, washed with pure water, and dried in the air. In this way, a sample according to Comparative Example 4 was obtained, which had a dielectric film formed from fluorine-free tantalum oxide.

[0088] (X-ray Diffraction Measurement) An XRD pattern was obtained by 2θ / θ scanning of the dielectric film of the sample according to Reference Example 1 using an X-ray diffraction (XRD) device Smartlab manufactured by Rigaku Corporation. Cu-Kα radiation was used as the X-ray source, and the voltage was adjusted to 40 kV, the current to 30 mA, and the scanning speed to 10 deg. / min. FIG. 9 shows the XRD pattern of the dielectric film of the sample according to Reference Example 1. No peaks attributable to a crystalline structure were confirmed in the XRD pattern shown in FIG. 9, indicating that the tantalum oxide film of the sample according to Reference Example 1 was amorphous.

[0089] (TOF-SIMS) Pieces of a predetermined size were cut out from the samples according to Reference Example 1 and Comparative Example 3, and samples for TOF-SIMS were prepared by embedding them in resin. Using a TOF-SIMS device TOF.SIMS5 manufactured by ION-TOF, TOF-SIMS was performed on the samples prepared from the samples according to Reference Example 1 and Comparative Example 3, and composition analysis was performed in the depth direction of the oxide film of the dielectric film. In TOF-SIMS, a Bi beam was used as the primary ion beam. O2 was used as the sputtering ion species. + FIG. 10 shows the F in the depth profile of the sample according to Reference Example 1 by TOF-SIMS. - , TaO 3- , and O - 11 is a graph showing the relationship between the signal intensity and depth of F in the depth profile obtained by TOF-SIMS of the sample according to Comparative Example 3. - , TaO 3- , and O - 10 and 11 are graphs showing the relationship between the signal intensity of each ion and the depth in the dielectric film.

[0090] 10, it can be seen that the dielectric film of the sample according to Reference Example 1 is formed on metal tantalum and includes a region with a high fluorine concentration and a region with a low fluorine concentration. The region with a high fluorine concentration exists from the surface of the dielectric film to a depth of about 60 nm. On the other hand, the region with a low fluorine concentration exists from a depth of about 75 nm to a depth of about 150 nm in the dielectric film. F in the region with a low fluorine concentration of the dielectric film - From the signal intensity, it is understood that the fluorine concentration in this region is 0.4% or less on an atomic number basis. There is little variation in the fluorine concentration between the regions with high and low fluorine concentrations. In FIG. 10, it is understood that a depth of approximately 150 nm or more corresponds to metallic tantalum. No increase in fluorine concentration is observed at the boundary between metallic tantalum and the dielectric film.

[0091] On the other hand, as shown in FIG. 11 , the dielectric film of the sample according to Comparative Example 3 is understood to extend to a depth of approximately 180 nm from the surface. In the sample according to Comparative Example 3, an increased fluorine concentration is observed at the boundary between the metallic tantalum and the dielectric film. This is thought to be due to the fact that the diffusion rate of fluoride ions is much faster than that of oxide ions, causing fluoride ions to diffuse into the metallic tantalum and the generation of tantalum fluoride prior to the formation of a tantalum oxide film by anodization. The tantalum fluoride thus generated has poor electrical insulation properties and may degrade the dielectric properties required for a capacitor. In addition, the presence of such tantalum fluoride near the metallic tantalum may result in non-uniform formation of the tantalum oxide film, potentially causing peeling of the tantalum oxide film. Therefore, a dielectric containing tantalum fluoride near the metallic tantalum is hardly suitable as a dielectric for a capacitor. On the other hand, by performing a chemical conversion treatment using a fluorine-free solution in advance, as in Reference Example 1, a fluorine-containing tantalum oxide film can be easily formed on the metallic tantalum without peeling.

[0092] (Capacitance and Dielectric Loss Tangent) The sample of Reference Example 1 was mounted in an electrochemical cell manufactured by BAS, and the dielectric characteristics of the capacitor of Reference Example 1 were evaluated according to the AC impedance method using a platinum counter electrode. In this evaluation, an AC voltage was applied to the capacitor of Example 1B at an amplitude of 10 to 100 mV and a frequency range of 1 MHz to 0.1 Hz, and the capacitance was calculated from the resistance value at each frequency. FIGS. 12A and 12B are graphs showing the relationship between the capacitance and frequency of the capacitor. In FIGS. 12A and 12B, the vertical axis represents capacitance and the horizontal axis represents frequency. FIG. 12A is an enlarged view of the area surrounded by the two-dot chain line in FIG. 12B. In addition, based on the results of this evaluation, the dielectric loss tangent tanδ at each frequency of the capacitor of Reference Example 1 was calculated. FIGS. 13A and 13B are graphs showing the relationship between the dielectric loss tangent tanδ of the capacitor and frequency. In FIG. 13A, the vertical axis represents tanδ and the horizontal axis represents frequency. FIG. 13A is an enlarged view of the area surrounded by the two-dot chain line in FIG. 13B.

[0093] The sample according to Comparative Example 3 was attached to an electrochemical cell manufactured by BAS, and the capacitance and dielectric loss tangent tanδ of the capacitor according to Comparative Example 3 were determined according to the AC impedance method using platinum as the counter electrode in the same manner as in Reference Example 1. The results are shown in Figures 12A to 13B.

[0094] The sample according to Comparative Example 4 was attached to an electrochemical cell manufactured by BAS, and the capacitance and dielectric loss tangent tanδ of the capacitor according to Comparative Example 4 were determined according to the AC impedance method using platinum as the counter electrode in the same manner as in Reference Example 1. The results are shown in Figures 12A to 13B.

[0095] The dielectric layers of the samples according to Reference Example 1, Comparative Example 3, and Comparative Example 4 were formed on tantalum metal with similar surface conditions, and it was understood that there was little difference in the surface area of ​​the dielectric layers of each sample. As shown in Figures 12A and 12B, the capacitances of the capacitors according to Reference Example 1 and Comparative Example 3 were higher than that of the capacitor according to Comparative Example 4. Although the capacitance of the capacitor according to Comparative Example 3 was high, as shown in Figures 13A and 13B, the dielectric loss tangent tanδ of the capacitor according to Comparative Example 3 was high. Tanδ corresponds to the energy consumed inside the capacitor, and it was understood that the capacitor according to Comparative Example 3 had a large loss of electrical energy. On the other hand, it was understood that the capacitor according to Reference Example 1 not only had a high capacitance, but also a low dielectric loss tangent tanδ, making it superior in terms of low electrical energy loss.

[0096] The correspondence between Example 1A, Example 1B, Examples 2A to 2E, Reference Example 1, and Comparative Examples 1 to 4 is shown in Table 2.

[0097]

[0098] The capacitor according to the present disclosure is advantageous from the viewpoint of suppressing the decrease in capacity due to the solid electrolyte.

Claims

1. A capacitor comprising: metallic tantalum; a solid electrolyte; and a tantalum oxide film disposed between the metallic tantalum and the solid electrolyte, wherein the tantalum oxide film includes a first portion containing fluorine and a second portion in contact with the first portion at a position closer to the solid electrolyte than the first portion in a thickness direction of the tantalum oxide film, and a fluorine concentration in the second portion is lower than a fluorine concentration in the first portion.

2. The capacitor according to claim 1, wherein the tantalum oxide film further includes a third portion in contact with the first portion at a position closer to the metallic tantalum than the first portion in a thickness direction of the tantalum oxide film, and a fluorine concentration in the third portion is lower than a fluorine concentration in the first portion.

3. The capacitor according to claim 1, wherein the first portion is amorphous.

4. The first portion is TaO x1 F y1 The capacitor according to claim 1 , having a composition represented by the following formula: wherein the composition satisfies the conditions: 0<x1<2.5 and 0<y1≦0.

4.

5. The second portion is TaO x2 F y2 The capacitor according to claim 1 , having a composition represented by the following formula: wherein the composition satisfies the conditions: 0<x2<2.5 and 0≦y2<0.

015.

6. The third portion is TaO x3 F y3 The capacitor according to claim 2 , having a composition represented by the following formula: wherein the composition satisfies the conditions: 0<x3<2.5 and 0≦y3<0.

015.

7. In the element or ion depth profile of the tantalum oxide film, oxygen (O) or oxygen ions O - The capacitor according to claim 1 , wherein the coefficient of variation of the signal intensity is 0.09 or less.

8. An electric circuit comprising a capacitor according to any one of claims 1 to 7.

9. A circuit board comprising a capacitor according to any one of claims 1 to 7.

10. An apparatus comprising a capacitor according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Manufacture of solid electrolyte capacitor

    JP1990276215A

  • Solid-state electrolytic capacitor and its manufacture

    JP1998135080A

  • Solid electrolytic capacitor and its manufacturing method

    JP2006270052A

Cited By

  • Capacitor, electric circuit, circuit board, and apparatus

    WO2026018507A1

  • Solid electrolytic capacitor

    WO2026197242A1