Semiconductor manufacturing materials
Boron carbide ceramics with titanium compounds address the corrosion issues in semiconductor manufacturing by enhancing resistance to Ar sputtering and CF-based plasma, improving process reliability and component durability.
Patent Information
- Application Number
- JP2021053956
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-26
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2041-03-26
AI Technical Summary
Existing semiconductor manufacturing members face challenges in withstanding the corrosive effects of Ar sputtering, fluorine-based plasma, and oxygen plasma, particularly during advanced etching processes that require high radio frequency power, leading to particle formation and etch stop issues.
The development of boron carbide ceramics containing a titanium compound, such as titanium carbide, which provides enhanced corrosion resistance against Ar sputtering and CF-based plasma, achieved through a specific composition and manufacturing process including hot pressing and thermal spraying.
The boron carbide ceramics with titanium compounds exhibit superior corrosion resistance, reducing particle formation and etch stop occurrences, suitable for use in semiconductor manufacturing components like inner wall members and support structures.
Smart Images

Figure 0007555295000002 
Figure 0007555295000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a member for use in semiconductor manufacturing, which has high corrosion resistance against Ar sputtering (Ar gas plasma), fluorine-based plasma, and oxygen plasma. [Background technology]
[0002] Carbide ceramics such as silicon carbide and boron carbide are resistant to plasma generated during ablation due to laser irradiation, and are therefore used as wafer support members for forming circuits on semiconductor wafers or for etching and other processes in the manufacture of integrated circuit (IC) elements, and as inner wall members for semiconductor manufacturing equipment.
[0003] Before anisotropic processing of IC elements is performed using dry etching technology, a resist pattern is formed using lithography technology. The resolution of a 193 nm ArF immersion system is 38 nm, but a technique called double patterning or multi-patterning has been used to achieve patterns of 10 to 7 nm, exceeding the resolution limit.
[0004] A common method for double patterning is the sidewall process, which utilizes the residues on the sidewalls of the pattern formed after dry etching. For example, an amorphous carbon layer, a SiON layer, and an anti-reflective film layer are first formed on a SiN film substrate on which a line pattern is to be formed, and a resist pattern is then formed by ArF immersion exposure. The resist pattern is then shrunk by isotropic etching using oxygen plasma, and the anti-reflective film, SiON film, and amorphous carbon layer are dry etched in this order to form a carbon pattern. When an atomic layer deposition (ALD) film is deposited on the carbon pattern and then dry etching is performed, a sidewall, which is an etching residue, is generated on the sidewalls of the carbon pattern. When the carbon is removed, only the sidewall remains. This sidewall is masked to perform dry etching of the SiN film, and an extremely fine line pattern is formed when the mask is removed.
[0005] In addition, when used for DRAM capacitors or 3D NAND memory holes, it is necessary to process very deep holes. To form these high aspect ratio micro-holes, a highly accurate anisotropic shape and a high selectivity and mask selectivity between the etching mask and the dielectric material such as SiO2 that serves as the underlayer are required. Fluorocarbon (CF)-based gases are used as etchant gases to meet these requirements, and CF x While the radicals are used to deposit a polymer film as a sidewall protection film on the sidewalls of the holes in the mask and undercoat film, the CF x + Or Ar + A technique is used in which ions such as these are drawn vertically into the holes in the SiO2 film to perform vertical etching.
[0006] If the hole is deep, the reaction products cannot be exhausted well, and metal residues (cuttings) may accumulate at the bottom of the hole, causing etch stop. In such cases, a method called "O2 flash" is used to remove the reaction products by oxygen plasma etching. In order to increase the etching rate of the SiO2 film, it is necessary to increase the amount of ion incidence, increase the total amount of F in the radicals, and use a high-energy ion beam. To achieve this, adjustments are made to the high-frequency power for plasma generation, the flow rate of CF-based gas, and the high-frequency power for ion attraction. Thus, recent dry etching technology uses oxygen plasma, CF-based plasma, and argon sputtering, and also uses very high-frequency power.
[0007] There is a demand for the development of semiconductor manufacturing components that are highly resistant to the recent dry etching techniques described above. A boron carbide (B4C) sintered body with a relative density of 98% or more has been reported as an inner wall member of semiconductor manufacturing equipment that has high corrosion resistance against halogen-based corrosive gases or their plasma, or as a support member for processed objects (Patent Document 1).
[0008] As reported in Patent Document 1, it is known that B4C materials are unlikely to react with oxygen-free fluorine- and chlorine-based corrosive gases or plasmas. However, even B4C materials undergo particle refinement due to etching or sputtering when very high-frequency power is applied. For this reason, there is a growing demand for B4C materials to have improved corrosion resistance to Ar sputtering and CF-based plasmas. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent No. 3500278 Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a boron carbide ceramic or thermal sprayed film containing a titanium compound as a semiconductor manufacturing component having high corrosion resistance against Ar ion bombardment by argon sputtering and CF-based plasma. [Means for solving the problem]
[0011] The semiconductor manufacturing member of the present invention is made of boron carbide ceramics containing a titanium compound and boron carbide. The titanium compound is preferably titanium carbide. In the boron carbide ceramic, the titanium carbide content is preferably 5 to 10%. The boron carbide ceramic is preferably made of a film, and the film is preferably a thermally sprayed film. The membrane is preferably formed on a silicon substrate. Effect of the Invention
[0012] The boron carbide ceramics containing a Ti compound according to the present invention are suitable for use as semiconductor manufacturing members due to their excellent corrosion resistance. In addition, thermal spray coatings made of boron carbide containing the Ti compound also have excellent corrosion resistance. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1(a) shows the etching rate of B4C sintered bodies containing TiC, TiB2, or TiO2 by Ar ion bombardment, compared to B4C sintered bodies not containing Ti compounds. FIG. 1(b) shows the etching rate of B4C sintered bodies containing TiC, TiB2, or TiO2 by O2 plasma, compared to B4C sintered bodies not containing Ti compounds. FIG. 1(c) shows the etching rate of B4C sintered bodies containing TiC, TiB2, or TiO2 by F2 plasma, compared to B4C sintered bodies not containing Ti compounds. In FIG. 1(a)-(c), the rightmost Si 100% in the graph indicates the etching rate of the silicon substrate. [Diagram 2] Figure 2(a) shows the etching rate of B4C coatings containing TiC, TiB2, or TiO2 by Ar ion bombardment in comparison with B4C coatings not containing Ti compounds. Figure 2(b) shows the etching rate of B4C coatings containing TiC, TiB2, or TiO2 by O2 plasma in comparison with B4C coatings not containing Ti compounds. Figure 2(c) shows the etching rate of B4C coatings containing TiC, TiB2, or TiO2 by F2 plasma in comparison with B4C coatings not containing Ti compounds. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The semiconductor manufacturing member of the present invention is made of a boron carbide ceramic containing a titanium compound and boron carbide. The semiconductor manufacturing member will be described in detail below. Boron carbide is used for the ceramics constituting the semiconductor manufacturing members. Even when boron carbide reacts with fluorine or chlorine, it produces a reactant with high vapor pressure, and is released outside the system as a gas without generating particles. In addition, it does not easily react with oxygen-free fluorine-based or chlorine-based corrosive gases or plasmas, and therefore has excellent corrosion resistance, making it suitable as a ceramic material. Boron carbide (B4C) is a powder having an average particle size of 5 μm or less, preferably 0.5 to 2 μm. If the average particle size exceeds 5 μm, the strength of the ceramic decreases, and it may not be suitable for practical use.
[0015] The titanium compound is not limited as long as it contains Ti element, but titanium carbide (TiC), titanium boride (TiB2), titanium(IV) oxide (TiO2), etc. are used because they are easily available.
[0016] In the ceramics, the mixture ratio of B4C and Ti compound is about 90-95:10-5 by weight, preferably 94-92:6-8, and the main component is a mixture of boron carbide-titanium compound, and further, if necessary, a sintering aid, binder, dispersant, etc. are added. Carbonized powder and other organic resins that generate carbon are used as the sintering aid, and can be added in an amount of 0-5% by weight based on the total weight of B4C and Ti compound.
[0017] The ceramics can be manufactured by preparing a slurry by adding a binder, a dispersant, etc. to the B4C and Ti compounds in addition to a sintering aid, and granulating the slurry with a spray dryer. For example, polyvinyl alcohol is used as the binder. For the dispersant, known dispersants such as surfactants and polymers are used. The ceramics can be obtained by filling the granulated powder into a mold and hot pressing the powder in a vacuum at a temperature of 2100 to 2300°C in a non-oxidizing atmosphere by known molding means, for example, hot pressing.
[0018] As a known molding method, in addition to hot pressing, cold isostatic pressing (CIP), injection molding, extrusion molding, etc. may be used. After molding, sintering in an inert atmosphere at a temperature of 1400 to 2250°C under a pressure of 1000 atmospheres or more can produce a densified ceramic with a relative density of 98% or more. If the ceramic has a low density and a large number of pores, the contact area with corrosive gases and plasma increases accordingly, and wear is accelerated. Therefore, the relative density of the ceramic is preferably 99% or more, and more preferably the open porosity is 0.2% or less.
[0019] In addition, as silicon wafers become larger in diameter, the manufacturing equipment and components used in semiconductor manufacturing are also becoming larger. In order to maintain durability as a part, the flexural strength of the ceramics is preferably 300 MPa or more. Flexural strength is an index that indicates the degree of fracture strength and deformation, and is measured by a bending test in accordance with JIS R 1601.
[0020] The ceramics have high resistance to microfabrication (etching reaction) using argon (Ar) sputtering, oxygen (O2) or fluorocarbon (CF) plasma. In the following, test pieces are made from the ceramics, and the surface of the test pieces is irradiated with Ar plasma, F2 plasma, O2 plasma, and CF plasma, respectively, to evaluate the corrosion resistance of the ceramics against plasma.
[0021] Ar sputtering is a process in which Ar is used to physically corrode the test piece. + This refers to the sputtering of ions, and corrosion resistance is related to the strength of atomic bonds. When Ti compounds such as TiC and TiB2, which have greater bond energy than B4C, are added to B4C, superior corrosion resistance is observed (Figure 1(a)). The corrosion resistance improves as the content of Ti compounds increases.
[0022] The corrosion resistance of the test piece against O2 plasma is due to the oxidation reaction between O2 plasma and the test piece. Therefore, as shown in Figure 1(b), as a Ti compound, TiO2, which is an oxide, has a low etching rate and is advantageous against O2 plasma, but TiC and TiB2 also become TiO2 when oxidized, so the corrosion resistance improves when the content of any of these Ti compounds increases.
[0023] When exposed to O2 plasma, the Ti compound and B4C react as follows: TiC+2O2 → TiO2+CO2 2TiB2+5O2→2TiO2+2B2O3 B4C+4O2→2B2O3+CO2
[0024] The corrosion resistance of the test piece to CF plasma is due to the fluorination reaction between the CF plasma and the test piece. When TiC is used as a Ti compound, the corrosion resistance improves as the content increases, but when TiB2 and TiO2 are used, the corrosion resistance decreases as the content increases.
[0025] These principles are within the scope of expectation, but when processing very deep holes for semiconductor memory holes, CF x It is believed that the same phenomenon occurs in this case because the etching method uses radicals to deposit a polymer film on the side walls of the holes as a side wall protective film. As mentioned above, when TiC is used as the Ti compound, the corrosion resistance improves as the content increases, and when TiB2 and TiO2, which do not contain carbon, the corrosion resistance decreases as the content increases.
[0026] When exposed to CF plasma, Ti compounds and B4C react as follows: TiC+8F → TiF4+CF4 TiB2+8F → TiF4+B2F4 TiO2+4F → TiF4+O2 B4C+12F→2B2F4+CF4
[0027] As described above, the corrosion resistance can be improved by selecting a Ti compound depending on the etching plasma to be used. In the etching process, plasma is often mixed and used. When plasma is mixed and used, TiC is the preferred Ti compound. This is because the difference in corrosion resistance is not so great for Ar plasma and oxygen plasma, but is significant for CF-based plasma. In this case, the TiC content is preferably 5-10% in the total of TiC and B4C. If the TiC content is less than 5%, the effect of sputter and plasma corrosion resistance is not obtained, and the performance is almost the same as that of B4C alone. On the other hand, if the TiC content exceeds 10%, the probability of breakage increases as the size and shape become larger due to thermal shock caused by the sudden temperature rise during plasma ignition and plasma exposure. This is thought to be because the thermal conductivity of B4C itself is not very high, and the thermal shock resistance property decreases as the content of TiC, which has a low thermal conductivity, increases.
[0028] The boron carbide ceramics containing a Ti compound may be a film formed on a substrate. The film may be formed by a chemical vapor deposition (CVD) method, a thermal spraying method, or the like. The CVD method can easily form a high-purity film, whereas the thermal spraying method has the advantage of being able to easily form a film on a variety of substrates. A thick film may be formed by these methods, and the substrate may be removed to produce a semiconductor manufacturing equipment component consisting of only the film.
[0029] In the coating process by thermal spraying, the temperature and collision speed of the ceramic raw material particles deposited on the substrate are important factors that determine the density of the coating and its adhesion to the substrate. Therefore, various thermal spraying methods have been developed, such as methods that have excellent heating and acceleration capabilities for the raw material particles, and are used according to the physical properties of the coating material and its application.
[0030] For example, when using TiC, the melting point of B4C is 2763°C and that of TiC is 3160°C, and both are oxidized in an oxygen atmosphere, so low-pressure plasma spraying is preferred. However, it can also be formed by CVD. In general plasma spraying, ceramic powder with a particle size of 10 to 45 μm is used, but since B4C and TiC have high melting points, smaller particle sizes are easier to melt. However, when the particle size is less than 10 μm, the powder fluidity decreases and it is prone to clumping, which can clog the plasma gun.
[0031] The substrate may be any material that is plasma resistant, such as alumina (Al2O3) or silicon (Si). Of these, Si is preferred because it is widely used as a substrate for focus rings and the like, and there is technology for processing high-purity materials with high precision. If a thermal spray layer can be provided on an existing silicon focus ring, it will be easier to obtain the substrate, and the effort required for reshaping the substrate after manufacture can be greatly simplified. EXAMPLES
[0032] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to the following examples.
[0033] [Example 1] B4C ceramics containing TiC, TiB2 or TiO2 as Ti compounds were prepared, and the etching rates by Ar ion bombardment and by O2 plasma and F2 plasma were measured.
[0034] The etching rate due to Ar ion bombardment was measured under the conditions of a high-energy Ar ion beam, a voltage of 3 kV, a beam current of 25 μA, and an irradiation time of 3 hours. After irradiation, the amount of wear of the B4C ceramics was measured.
[0035] As shown in Fig. 1(a), in the B4C ceramics containing TiC and TiB2, the amount of sputtering decreased with increasing TiC and TiB2 content, whereas in the B4C ceramics containing TiO2, the amount of sputtering increased with increasing TiO2 content.
[0036] The etching rate with O2 plasma was measured by exposing the B4C ceramics to oxygen plasma for 3 hours at a reduced pressure of 2.66 Pa, with high frequency power of 800 W on the source side and 300 W on the bias side, and O2 = 20 sccm, using an inductively coupled plasma (ICP) etching device, and measuring the amount of wear after the plasma exposure. As shown in Figure 1(b), the etching rate decreased in both cases as the content of Ti compounds increased.
[0037] The etching rate by F2 plasma was measured by exposing the B4C ceramics to fluorine plasma for 4 hours under a reduced pressure of 2.66 Pa with high frequency power of 800 W on the source side and 100 W on the bias side and CF4 = 100 sccm using the same ICP etching device, and then measuring the amount of wear of the B4C ceramics.
[0038] As shown in Fig. 1(c), for B4C ceramics containing TiC, the etching rate decreased with increasing content, whereas for B4C ceramics containing TiB2 and TiO2, the etching rate increased with increasing content.
[0039] [Example 2] Next, a test similar to that in Example 1 was carried out on a thermal sprayed coating formed by spraying B4C powder containing a Ti compound onto a substrate using a plasma jet.
[0040] In Example 2, as shown in FIGS. 2(a) to (c), the etching rate was several percent to 10% higher than that of the sintered body of Example 1, and the corrosion resistance was inferior. However, the overall tendency was the same as in Example 1.
[0041] The reason why the corrosion resistance was inferior to that of the sintered body is thought to be because it is known that corrosion resistance to plasma is also affected by the density of the tissue or structure, and this effect was apparent. The sintered body was produced by hot pressing, so the porosity was 1-3%, but the sprayed coating had a porosity of around 5%. [Industrial Applicability]
[0042] The semiconductor manufacturing member made of the B4C ceramic containing the Ti compound of the present invention has high corrosion resistance not only to plasma using Ar sputtering or CF-based gas, but also to oxygen-based plasma, and is therefore suitable for use as an inner wall member of semiconductor manufacturing equipment, a support for supporting a workpiece, or other jigs.
Claims
1. The ceramic material is made of boron carbide containing a titanium compound. A member for semiconductor manufacturing, characterized in that the boron carbide ceramic has a titanium carbide content of 5 to 10%.
2. 2. The semiconductor manufacturing member according to claim 1, wherein the boron carbide ceramic is in the form of a film.
3. 3. The member for use in semiconductor manufacturing according to claim 2, wherein the film is a thermally sprayed film.
4. 4. The member for use in semiconductor manufacturing according to claim 2, wherein the film is formed on a silicon substrate.
Citation Information
Patent Citations
Sputtering device and formation of dielectric film
JP1996277461A
Plasma-resistant member and its production
JP2000247743A
Mobile device composed of highly rigid material
JP2001342069A
Boron carbide-based sintered compact and protective member
JP2008273753A
Corrosion-resistant materials for semiconductor manufacturing
JP3500278B2