Engine air filter media

The air filter medium with an electrically charged meltblown polyester layer addresses the inefficiencies of nanofiber layers by enhancing filtration efficiency and dust retention, facilitating cost-effective and stable engine air filtration.

JP7555342B2Active Publication Date: 2024-09-24NEENAH GESSNER GMBH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021540337
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-10
Filing Date
2020-01-10
Publication Date
2024-09-24
Estimated Expiration
2040-01-10

AI Technical Summary

Technical Problem

Existing engine air filters face challenges in achieving high filtration efficiency and dust retention capacity while being cost-effective and easily producible using standard manufacturing methods, with nanofiber layers being expensive and mechanically unstable.

Method used

An air filter medium comprising a support layer and a meltblown layer made of polyester fibers, which are electrically charged, allowing for larger fiber diameters and improved efficiency and dust retention capacity.

Benefits of technology

The charged filter medium exhibits enhanced filtration efficiency and dust holding capacity, enabling cheaper production and longer replacement intervals due to improved mechanical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555342000001
    Figure 0007555342000001
Patent Text Reader

Abstract

The engine air filter medium has a support layer and a meltblown layer containing polyester fibers. The filter medium is electrically charged.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an engine air filter medium, the filter medium having a support layer and a meltblown layer, and a filter element including such a filter medium. [Background technology]

[0002] Important quality criteria for air filter media include high filtering efficiency, i.e. separation of large and small particles, as well as a sufficiently high dust retention capacity. For engine air filter media, it is worth noting that the dust retention capacity is 200 m3 per hour when the engine is at full load, depending on the cylinder volume. 3 ~500m 3 The problem is that the filter element draws in a lot of air, which contains polluting and dust particles. If the filter element does not allow enough air to pass through, the engine cannot develop its full potential.

[0003] Engine air filter elements are responsible for supplying the engine with the clean air required for a flawless combustion process. Engine air filter media have the following additional functions in terms of air management within a vehicle: filtering the engine intake air, improving airflow for optimal combustion and engine acoustics, such as attenuating intake noise, and protecting downstream engine components, such as turbochargers, from particle impact.

[0004] To increase the filtration efficiency, nanofiber layers (i.e., fiber diameters less than 1.5 μm) are used. However, such nanofiber layers require complex manufacturing methods and are therefore expensive. A further drawback is the low mechanical stability of nanofiber layers.

[0005] In addition, the engine air filter must be changed at intervals suggested by the vehicle manufacturer. This is carried out within the framework of inspection work. If there is a high dust content in the air (or for a given total mileage), it is recommended to change the filter earlier. Therefore, it is ideal for the filter material (or filter) to be as cheap as possible. Summary of the Invention [Problem to be solved by the invention]

[0006] The object of the present invention is therefore to provide a filter medium and a filter element, which are particularly suitable for engine air filters, have very good efficiency and dust holding capacity, and can be easily produced by standard manufacturing methods and correspondingly inexpensively manufactured. [Means for solving the problem]

[0007] The present invention relates to an engine air filter medium, the engine air filter medium having a support layer and a meltblown layer containing polyester fibers, the filter medium being electrically charged. Effect of the Invention

[0008] The filter medium is particularly suitable for engine air filters. Previously, engine air filter medium was not charged because high dust generation would cause rapid discharge, and thus no difference in filtration efficiency was observed with respect to non-charged filter medium. Surprisingly, it was found that the charged filter medium of the present invention has better efficiency and dust retention capacity than non-charged filter medium. Therefore, the meltblown layer can be manufactured with a larger fiber diameter. This allows for a cheaper production of filter medium and a higher efficiency and dust retention capacity, assuming the same pressure loss.

[0009] Advantageously, the polyester fibers contain polybutylene terephthalate or consist of polybutylene terephthalate fibers.

[0010] The average diameter of such meltblown fibers is specifically 2 to 8 μm, preferably 2 to 5 μm, and particularly preferably 3 to 4 μm. The average diameter is measured by the method described herein.

[0011] The thickness of the meltblown layer according to the invention is in particular 0.05 to 0.90 mm, preferably 0.10 to 0.80 mm, particularly preferably 0.15 to 0.70 mm, at a contact pressure of 0.005 bar.

[0012] The mass per unit area of ​​the meltblown layer is specifically 5 to 90 g / m 2 , advantageously 10 to 60 g / m 2 , particularly preferably 15 to 25 g / m 2 It is.

[0013] The air permeability of the meltblown layer according to the present invention is specifically 50 to 3000 l / m 2 s, advantageously 300-2000 l / m 2 s, and particularly preferably from 800 to 1300 l / m 2 It is s.

[0014] To produce the meltblown nonwoven fabric according to the invention, the meltblown method known to those skilled in the art is used. Suitable polymers, in particular polyesters, are, for example, polyethylene terephthalate or polybutylene terephthalate. The meltblown layer preferably comprises polybutylene terephthalate fibers. The meltblown layer is particularly preferably made of polybutylene terephthalate fibers. If necessary, the polymer can be mixed with further additives, such as hydrophilizing agents, hydrophobizing agents, crystallization promoters or pigments. The meltblown layer can be charged during production or together with the support layer. Charging methods include all known methods, such as corona charging methods.

[0015] In order to enhance the electrostatic stability, additives known to those skilled in the art, such as bis-stearoyl-ethylenediamide, may be mixed in.

[0016] The support layer may be a wet layer or a dry layer.

[0017] The wet layer or paper layer in the sense of the present invention is any layer that can be formed by wet methods known to those skilled in the art to produce filter paper. The wet layer can contain natural fibers, synthetic fibers, or a mixture thereof. Examples of natural fibers are cellulose, cotton, wool and hemp. The cellulose materials used can include wood-free cellulose and / or wood-containing cellulose from softwoods and / or hardwoods, regenerated cellulose, and fibrillated cellulose.

[0018] Suitable synthetic fibres are, for example, polyester fibres (eg polyethylene terephthalate fibres, polybutylene terephthalate fibres, PLA fibres), polyolefin fibres, polyamide fibres, polyacrylonitrile fibres and also multicomponent fibres whose individual components have different melting points.

[0019] The average fiber diameter of the synthetic fibers in the wet layer is in particular 3 μm (0.1 dtex) to 30 μm (10 dtex), preferably 7 to 20 μm, and the cut length is preferably 3 mm to 20 mm, particularly preferably 4 mm to 12 mm.

[0020] The support layer may comprise 100% by weight natural fibres (based on total fibre content). The support layer may comprise 30-45% by weight synthetic fibres and 70-55% by weight natural fibres, or may comprise 100% by weight synthetic fibres. Advantageously, the support layer comprises 100% by weight natural fibres.

[0021] The thickness of the wet support layer at a contact pressure of 0.005 bar is in particular 0.1 mm to 1.2 mm, preferably 0.2 mm to 0.9 mm, particularly preferably 0.3 mm to 0.8 mm.

[0022] The dry support layer is a layer that can be formed by dry processes known to those skilled in the art for producing nonwoven layers. Advantageously, the nonwoven layer is a spunbonded or carded nonwoven fabric with only synthetic fibers. Advantageously, the dry support layer consists of a spunbonded nonwoven layer. The thickness of the dry support layer is advantageously between 1 mm and 3.0 mm, in particular at a contact pressure of 0.005 bar. Particularly advantageously, the thickness of the dry support layer is between 1.2 mm and 2.5 mm, in particular between 1.3 mm and 2.1 mm.

[0023] The dry support layer comprises monocomponent or bicomponent synthetic fibers. The dry support layer preferably comprises (or consists of) monocomponent polyester fibers, particularly preferably polyethylene terephthalate fibers. Suitable synthetic fibers are, for example, polyester fibers (e.g. polyethylene terephthalate fibers, polybutylene terephthalate fibers, PLA fibers), polyolefin fibers, polyamide fibers, polyacrylonitrile fibers, and multicomponent fibers whose individual components have different melting points.

[0024] Bicomponent fibers are comprised of at least one fiber portion having a higher melting point and a second fiber portion having a lower melting point thermoplastic material. The physical form of such fibers is known to those skilled in the art and typically comprises a side-by-side or sheath-core structure.

[0025] Bicomponent fibers can be made from a number of thermoplastic materials including polyolefins (e.g., polyethylene and polypropylene), polyesters (e.g., polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyamides including nylon 6, nylon 6.6, nylon 6.12, and the like). Advantageously, the bicomponent fibers are made from polyesters. Particularly advantageously, the bicomponent fibers are made from PET / coPET.

[0026] The specific average diameter of the monocomponent or bicomponent fibers of the dry support layer is 10 to 50 μm, preferably 12 to 40 μm, and particularly preferably 14 to 35 μm.

[0027] The support layer can be impregnated. The type of impregnating agent is selected by the skilled artisan depending on the intended use of the filter material according to the invention. The proportion of dry impregnating agent in the total weight of the paper is typically 0.5% to 50% by weight, preferably 5% to 40% by weight. As impregnating agents, substances known for filter paper are used, for example phenolic or epoxy resins from alcoholic solutions, but also for example aqueous dispersions of acrylates, phenolic resins, polyvinyl chloride, polyvinyl acetate. Other possible types of impregnating agents are, for example, aqueous solutions of polyvinyl alcohol, melamine resins, urea resins. To improve the wettability and thus the flow-through rate, the impregnation can be adjusted to be hydrophilic or oleophilic by suitable additives, for example surface-active substances or fluorocarbon resins.

[0028] The mass per unit area of ​​the support layer (i.e., wet layer or dry layer) is specifically 50 to 350 g / m 2 , advantageously 70 to 250 g / m 2 , and particularly preferably from 80 to 200 g / m 2 It is.

[0029] The air permeability of the support layer (i.e., the wet layer or the dry layer) is specifically 50 to 4000 l / m 2 s, advantageously from 100 to 3000 l / m 2 s, and particularly preferably from 200 to 2800 l / m 2 It is s.

[0030] The filter media may consist solely of the support layer and meltblown layer combination described herein, or it may include one or more additional layers.

[0031] To produce the filter medium, the meltblown layer can be bonded to the support layer. For this purpose, any method known to those skilled in the art can be used, such as needling, water jet needling, thermal (i.e. calendar fixing and ultrasonic fixing) and chemical (i.e. adhesive fixing). Advantageously, the meltblown layer is bonded to the support layer by point calendaring or adhesive. The amount of adhesive applied is 2-10 g / m 2 , advantageously 4 to 8 g / m 2 It is.

[0032] The mass per unit area of ​​the filter medium according to the invention is preferably 55 g / m 2 ~440g / m 2 , advantageously 80 to 300 g / m 2 , and particularly preferably from 90 to 200 g / m 2 Advantageously, the air permeability of the filter medium is between 50 and 1200 l / m 2 s, advantageously between 100 and 1000 l / m 2 s, and particularly preferably from 200 to 900 l / m 2 It is s.

[0033] Preferably, the thickness of the filter medium is between 0.4 and 2.5 mm, particularly preferably between 0.45 and 2 mm, and most preferably between 0.45 and 1 mm, at a contact pressure of 0.005 bar.

[0034] The maximum pore diameter (or maximum pore size) of the filter medium according to the present invention is specifically 30 to 120 μm, preferably 35 to 110 μm. The diameter of most of the pores of the filter medium according to the present invention is specifically 20 to 80 μm, preferably 25 to 65 μm.

[0035] The H value of the filter medium is specifically 1.00 to 2.50, preferably 1.00 to 2.00, and particularly preferably 1.00 to 1.80. H value = maximum pore diameter / diameter of most pores It is calculated from: When the H value is within the above range, it shows very good homogeneity, so that the filter medium can ensure very high efficiency and dust holding capacity for a longer period of time.

[0036] The efficiency of the filter medium according to the invention is in particular at least 99.00%, preferably at least 99.70%, particularly preferably at least 99.90%. The efficiency indicated here corresponds to the total efficiency after a pressure increase of up to 2000 Pa. This should be distinguished from the initial efficiency.

[0037] The dust retention capacity of the filter medium according to the present invention is specifically 70 to 350 g / m 2 , advantageously 100 to 300 g / m 2 , particularly preferably 125 to 300 g / m 2 It is.

[0038] Due to the excellent breaking strength of the filter medium according to the invention, the filter medium only needs to be renewed after longer time intervals.

[0039] The breaking strength in the machine direction (MD) of a filter medium also containing natural fibers is in particular 60-200 N, preferably 70-180 N, particularly preferably 75-100 N. The breaking strength in the machine direction (MD) of a filter medium containing only synthetic fibers (no natural fibers) is in particular 250-600 N, preferably in particular 350-600 N, particularly preferably 400-600 N.

[0040] The flow direction is advantageously from the side of the support layer, but can also be from the side of the meltblown layer.

[0041] The invention also relates to a filter element comprising a filter medium, which may additionally comprise other filter media which are distinct from the filter medium according to the invention, i.e. have other properties.

[0042] A particularly advantageous field of application for the filter medium according to the invention is engine air filters.

[0043] Test Method Mass per unit area according to DIN EN ISO 536:2012-11.

[0044] Thickness: Test area 2500mm at contact pressure 0.5kPa 2 (diameter 56.42 mm) in accordance with DIN EN ISO 9073-2 (1997-02).

[0045] Air permeability according to DIN EN ISO 9237 (1995-12) at a pressure difference of 200 Pa.

[0046] Pore ​​size Based on measurements on flat test specimens according to DIN ISO 4003 (1990-10). Reagent: denatured ethanol (= 100 L ethanol with 1 L MEK (Methyl-Ethyl-Ketone) as denaturant). The nonwoven fabric is clamped airtight above a cavity equipped with an air conduit and a connection to a manometer (U-tube in mm).

[0047] Denatured ethanol is added through the edge of the upper sample holder (do not spray directly onto the sample / approximately 4 mm height) and simultaneously a slight positive pressure is created. Slowly increase the positive pressure (approximately 5 mm WC / sec) until the first bubbles are visible.

[0048] The pressure required for this is read on a manometer (mm WC) and the maximum pore size "Max Hole" is calculated according to the surface tension of ethanol (23°C). 2 If the positive pressure is increased until air penetrates through the entire pore (air bubbles are distributed almost uniformly, but no foam formation occurs), the value for "multiple pores" is obtained. In addition to this, the positive pressure for the "multiple pores" is measured again, and the corresponding pore size is calculated.

[0049] [Breaking strength] - For the entire filter medium (support + meltblown, filter medium contains natural fibres) according to DIN EN ISO 1924-2 (2009-05) (100 mm long, 15 mm wide measuring strip, drawing speed 15 mm / min). - For the entire filter medium (support + meltblown, filter medium does not contain natural fibres) according to DIN EN ISO 29073 Part 3 (1992-08) (100 mm long, 50 mm wide measuring strip, drawing speed 100 mm / min).

[0050] [Efficiency and dust holding capacity] The efficiency values ​​shown are based on flat sample measurements according to ISO 5011:2014. The test conditions are: - Test dust ISO 12103-A2 (ISO Fine) - Mass concentration: 1g / m 3 - Inflow velocity 11.1cm / s - Filter area: 100cm 2

[0051] Once a final pressure of 2000 Pa is reached, the total efficiency and dust holding capacity are measured.

[0052] Fiber diameter Measurement principle: Images are taken at defined magnifications by a scanning electron microscope. These images are measured by automatic software. Measurement points that capture fiber crossovers and therefore do not represent the fiber diameter are manually removed. The fiber bundle is evaluated as a single fiber as a whole.

[0053] Device: Scanning electron microscope Phenom Fei with software Fibermetric V2.1.

[0054] Testing Sampling: Nonwoven material at 5 locations across the web width (approximately 1.8 m)

[0055] photograph: a. Sputter the sample. b. Photograph the area based on the optical image at will. Photograph the area found in this way by SEM at 1000x magnification. c. The "one click" method determines the fiber diameter. One capture must be made for each fiber. d. The data obtained from Fibermetric is used to evaluate the average value and fiber diameter distribution using Excel. This will result in the detection of the average fiber diameter at at least 5 locations per nonwoven. The 5 average values ​​are combined into one average value. Such a value is called the average fiber diameter of the nonwoven. At least 500 fibers are evaluated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0056] Working Example Example 1 Thickness 0.22mm, air permeability 650 l / m 2 s, and 20 g / m with an average fiber diameter of 3.5 μm 2 PBT (polybutylene terephthalate) meltblown is cut into 135g / m2 with a thickness of 0.68mm by point calendaring. 2 and subjected to a corona charge. The paper layer utilized here consisted of cellulose and had been previously impregnated with resin.

[0057] The resulting filter medium has a thickness of 0.75 mm and an air permeability of 365 l / m 2 s, and mass per unit area of ​​155 g / m 2 The maximum pore size of the filter medium is about 39 μm, with most pores having a diameter of about 27 μm.

[0058] Example 2 Thickness 0.66mm, air permeability 1200 l / m 2 s, and 60 g / m 2 The PBT meltblown is cut by point calendaring to a thickness of 1.47 mm at 130 g / m 2 The nonwoven fabric was bonded to a PET / CoPET spunbond nonwoven fabric of 1000g each, and was subjected to a corona charging.

[0059] The filter medium thus obtained has a thickness of 2.00 mm and an air permeability of 900 l / m 2 s, and mass per unit area of ​​190 g / m 2 The maximum pore size of the filter medium is about 100 μm, with most pores having a diameter of about 58 μm.

[0060] Comparative Example 1 It corresponds to the same filter medium as in Example 1, but was not subjected to corona charging.

[0061] Comparative Example 2 It corresponds to the same filter medium as in Example 2, but was not subjected to corona charging.

[0062] Some advantages of the filter media according to the present invention are shown in Table 1. [Table 1] The following are some aspects of the embodiment of the present invention. [Aspect 1] An engine air filter medium, comprising a support layer and a meltblown layer containing polyester fibers, the filter medium being electrically charged. [Aspect 2] 2. The filter medium of claim 1, wherein the polyester fibers comprise polybutylene terephthalate. [Aspect 3] 3. The filter medium according to aspect 1 or 2, wherein the polyester fibers have an average diameter of 2 to 8 μm. [Aspect 4] The mass per unit area of ​​the meltblown layer is 5 to 90 g / m 2 4. The filter medium according to any one of claims 1 to 3, wherein [Aspect 5] 5. The filter medium of any one of the preceding embodiments, wherein the filter medium has an overall efficiency of at least 99.00%. [Aspect 6] 6. The filter medium of any one of the preceding aspects, wherein the support layer comprises a paper layer or a spunbond nonwoven fabric layer. [Aspect 7] 7. The filter medium of claim 6, wherein the spunbond nonwoven layer contains monocomponent or bicomponent polyester fibers. [Aspect 8] 8. The filter medium of claim 7, wherein the bicomponent fibers comprise PET / CoPET. [Aspect 9] 9. The filter medium of any one of the preceding claims, wherein the filter medium comprises a support layer and a meltblown layer. [Aspect 10] A filter element comprising the filter medium of any one of the first to ninth embodiments.

Claims

1. An air filter medium for an engine, comprising a support layer and a meltblown layer containing polyester fibers, the air filter medium being electrically charged, the maximum pore size, measured according to DIN ISO 4003 (1990-10), is between 30 and 120 μm and the majority of the pores have a diameter, measured according to DIN ISO 4003 (1990-10), between 20 and 80 μm; The H value calculated from the following formula is 1.00 to 2.50, H value = maximum pore diameter / diameter of most pores: An engine air filter medium having an efficiency of 99.00% or more as measured under the following test conditions in accordance with ISO 5011:2014. - Test dust ISO 12103-A2 (ISO Fine) - Mass concentration: 1g / m3 - Inflow speed: 11.1cm / s - Filter area: 100 cm2 Final pressure reached: 2000 Pa

2. 2. The air filter medium according to claim 1, wherein the polyester fibers contain polybutylene terephthalate.

3. 3. The air filter medium according to claim 1, wherein the polyester fibers have an average diameter of 2 to 8 μm.

4. The mass per unit area of ​​the meltblown layer is 5 to 90 g / m 2 4. The air filter medium according to claim 1, wherein the air filter medium is

5. 5. The air filter medium according to claim 1, wherein the support layer comprises a paper layer or a spunbond nonwoven fabric layer.

6. 6. The air filter medium of claim 5, wherein the spunbond nonwoven layer contains monocomponent or bicomponent polyester fibers.

7. 7. The air filter media of claim 6, wherein the bicomponent polyester fibers comprise PET / CoPET.

8. 8. The air filter medium according to claim 1, wherein the air filter medium comprises the support layer and the meltblown layer.

9. A filter element comprising an air filter medium according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Cleanable gas filter

    DE4443158A1

  • Nonwoven fabric for filter

    JP2007125546A

  • Manufacturing method for unwoven fabric filter medium

    JP2017080708A