Metal-Ligand Complexes
Metal-ligand complexes, particularly those with titanium, zirconium, or hafnium centers, form bimodal catalyst systems to overcome limitations of existing metallocene catalysts, resulting in polyolefin polymers with enhanced properties like reduced melt index, increased melting temperature, and improved molecular weight.
Patent Information
- Application Number
- JP2021564703
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-17
- Filing Date
- 2020-04-27
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-04-27
AI Technical Summary
Existing asymmetric non-bridged metallocene polymerization catalysts are inadequate in achieving desired properties such as reduced melt index, increased melting temperature, and improved molecular weight distribution in polyolefin polymers.
Development of metal-ligand complexes, specifically those with titanium, zirconium, or hafnium centers, which form bimodal catalyst systems when activated, allowing for the production of polyolefin polymers with improved properties through controlled polymerization processes.
The metal-ligand complexes enhance polymerization outcomes by reducing melt index, increasing melting temperature, and improving molecular weight, leading to superior polyolefin polymers with tailored properties.
Smart Images

Figure 0007555352000007 
Figure 0007555352000009 
Figure 0007555352000010
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE Embodiments of the present disclosure relate to metal-ligand complexes, and more particularly, to metal-ligand complexes that may be used to make olefin polymerization catalysts. [Background technology]
[0002] Polymers may be used in many products such as films, fibers, nonwoven and / or woven fabrics, extruded articles, and / or molded articles, among others. Polymers may be formed by reacting one or more monomers in a polymerization reaction in the presence of a polymerization catalyst. Summary of the Invention [Problem to be solved by the invention]
[0003] The present disclosure provides various embodiments, including:
[0004] A metal-ligand complex of formula I, [ka]
[0005] In the formula, M is titanium, zirconium or hafnium, R is hydrogen or (C1-C4) alkyl, and R 1 is (C1-C4) alkyl, R 2 , R 3 , R 4 , R 5 Any one or two of the following can be independently selected: 20 ) alkyl, R 2 , R 3 , R 4 , R 5 Three or two of the X's are H, and each X is independently a halide, (C1-C 20 ) Alkyl, (C7-C 20 )Aralkyl, (C1-C6)Alkyl-substituted (C6-C 12) aryl, (C1-C6) alkyl substituted benzyl or silicon-containing alkyl.
[0006] A bimodal catalyst system comprising a metal-ligand complex of formula I and a bis(2-(pentamethylphenylamido)ethyl)-amine zirconium complex of formula III, [ka] In the formula, M is Zr, and each R 1 are independently Cl, Br, (C1-C 20 )Alkyl, (C1-C6)Alkyl-substituted (C6-C 12 ) aryl, benzyl, or (C1-C6) alkyl substituted benzyl, a bimodal catalyst system.
[0007] 1. A method of making a polymerization catalyst comprising contacting a metal-ligand complex or a bimodal catalyst system of formula I with an activating agent under activating conditions to activate the metal-ligand complex or the bimodal catalyst system, thereby making the polymerization catalyst.
[0008] A method of making a polyolefin polymer, comprising contacting an olefin with a polymerization catalyst under polymerization conditions to polymerize the olefin to make the polyolefin polymer.
[0009] A polyolefin polymer made using the same manufacturing method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The metal-ligand complexes disclosed herein may be represented by Formula I: [ka]
[0011] In the formula, M is titanium, zirconium or hafnium, R is hydrogen or (C1-C4) alkyl, and R 1 is (C1-C4) alkyl, R2 , R 3 , R 4 , R 5 Any one or two of the following can be independently selected: 20 ) alkyl, R 2 , R 3 , R 4 , R 5 Three or two of the X's are H, and each X is independently a halide, (C1-C 20 ) Alkyl, (C7-C 20 )Aralkyl, (C1-C6)Alkyl-substituted (C6-C 12 ) aryl, (C1-C6) alkyl substituted benzyl or silicon-containing alkyl.
[0012] The metal-ligand complex can be used to make a polymerization catalyst, for example, an asymmetric unbridged metallocene polymerization catalyst. For example, the metal-ligand complex can be made into a polymerization catalyst by contacting with an activator under activating conditions to activate the metal-ligand complex. An embodiment provides a method of making a polymerization catalyst, comprising contacting with a metal-ligand complex or a bimodal catalyst system of formula I with an activator under activating conditions to activate the metal-ligand complex or the bimodal catalyst system to make a polymerization catalyst. A polymerization catalyst made from only one metal-ligand complex is useful for making polyolefin polymers characterized by a monomodal molecular weight distribution. A polymerization catalyst made from a bimodal catalyst system is useful for making polyolefin polymers characterized by a bimodal molecular weight distribution.
[0013] Surprisingly, polymerization catalysts made from metal-ligand complexes can be useful for providing polymers having improved, i.e., reduced, melt index ((I2); D1238-13 (190°C, 2.16 kg load)) compared to polymers formed using other asymmetric unbridged metallocene (non-invention) polymerization catalysts under similar polymerization conditions. In some applications, a reduced melt index is desirable.
[0014] Additionally, polymerization catalysts made from the metal-ligand complexes can surprisingly provide polymers having improved, i.e., elevated, melting temperatures, as compared to polymers formed using other asymmetric unbridged metallocene polymerization catalysts under similar polymerization conditions. In some applications, elevated melting temperatures are desirable.
[0015] Additionally, polymerization catalysts made from the metal-ligand complexes can be useful in providing polymers having improved, i.e., increased, molecular weights (Mn, Mw, and / or Mz) as compared to polymers formed using other asymmetric unbridged metallocene polymerization catalysts under similar polymerization conditions. In some applications, increased molecular weights (Mn, Mw, and / or Mz) are desirable.
[0016] Additionally, polymerization catalysts made from the metal-ligand complexes can be useful in providing polymers having improved, i.e., increased, density, as compared to polymers formed with other asymmetric unbridged metallocene polymerization catalysts under similar polymerization conditions. In some applications, increased density is desirable.
[0017] As stated above, R is hydrogen or (C1-C4) alkyl. One or more embodiments provide that R is (C1-C3) alkyl. One or more embodiments provide that R is (C1-C2) alkyl. One or more embodiments provide that R is C1 alkyl. One or more embodiments provide that R is C2 alkyl. One or more embodiments provide that R is C3 alkyl. One or more embodiments provide that R is C4 alkyl.
[0018] As mentioned above, R 1 is (C1-C4) alkyl. One or more embodiments include 1 is (C1-C3) alkyl. One or more embodiments provide that R 1 is (C1-C2) alkyl. One or more embodiments provide that R 1 is C alkyl. One or more embodiments provide that R1 is C alkyl. One or more embodiments provide that R 1 is C alkyl. One or more embodiments provide that R 1 is a C4 alkyl.
[0019] As mentioned above, R 2 , R 3 , R 4 , R 5 One or two of the following can be independently selected (C1 to C 20 ) alkyl, R 2 , R 3 , R 4 , R 5 are H. One or more embodiments provide that any three or two of R 2 , R 3 , R 4 , R 5 One or two of the following can be independently selected (C1 to C 10 ) alkyl, R 2 , R 3 , R 4 , R 5 are H. One or more embodiments provide that R 2 , R 3 , R 4 , R 5 One or two of R are independently (C1-C6) alkyl; 2 , R 3 , R 4 , R 5 are H. One or more embodiments provide that R 2 , R 3 , R 4 , R 5 One or two of the following are independently (C1-C3) alkyl: 2 , R 3 , R 4 , R 5 are H. One or more embodiments provide that R 2 , R 3 , R 4 , R 5one or two of the following are independently (C1-C2) alkyl; R 2 , R 3 , R 4 , R 5 are H. One or more embodiments provide that R 2 , R 3 , R 4 , R 5 any one or two of are independently C alkyl; R 2 , R 3 , R 4 , R 5 Provide that three or two of are H.
[0020] As previously mentioned, each X is independently a halide, (C1-C 20 ) Alkyl, (C7-C 20 )Aralkyl, (C1-C6)Alkyl-substituted (C6-C 12 )aryl, (C1-C6)alkyl-substituted benzyl, or silicon-containing alkyl. One or more embodiments provide that each X is independently Cl. One or more embodiments provide that each X is independently (C1-C 20 One or more embodiments provide that each X is independently (C1-C 15 One or more embodiments provide that each X is independently (C1-C 10 )alkyl. One or more embodiments provide that each X is independently (C1-C5)alkyl. One or more embodiments provide that each X is independently C1alkyl. One or more embodiments provide that each X is independently silicon-containing alkyl. One or more embodiments provide that each X is independently trihydrocarbylsilylmethyl. One or more embodiments provide that each X is independently trimethylsilylmethyl.
[0021] The metal-ligand complex of formula I may be referred to as a metallocene complex. Examples of metal-ligand complexes of formula I include cyclopentadienyl(1,4,7-trimethylindenyl)zirconium dichloride, cyclopentadienyl(1,5,7-trimethylindenyl)zirconium dichloride, methylcyclopentadienyl(1,4-dimethylindenyl)zirconium dichloride, methylcyclopentadienyl(1,6-dimethylindenyl)zirconium dichloride, methylcyclopentadienyl(1,7-dimethylindenyl)zirconium dichloride, methylcyclopentadienyl(1,4,7-trimethylindenyl)zirconium dichloride, methylcyclopentadienyl(1,5,7-trimethylindenyl)zirconium dichloride, and propylcyclopentadienyl(1,5-dimethylindenyl)zirconium dichloride. , propyl cyclopentadienyl(1,6-dimethylindenyl)zirconium dichloride, propyl cyclopentadienyl(1,7-dimethylindenyl)zirconium dichloride, propyl cyclopentadienyl(1,4,7-trimethylindenyl)zirconium dichloride, propyl cyclopentadienyl(1,5,7-trimethylindenyl)zirconium dichloride, cyclopentadienyl(1,5-dimethylindenyl)zirconium dichloride, methyl cyclopentadienyl(1,5-dimethylindenyl)zirconium dichloride, cyclopentadienyl(1,5-dimethylindenyl)zirconium dimethyl, and methyl cyclopentadienyl(1,5-dimethylindenyl)zirconium dimethyl.
[0022] One or more embodiments provide that the metal-ligand complex of formula I comprises a disubstituted indenyl group, for example, where each indenyl substitution is independently (C1-C4) alkyl. For example, the metal-ligand complex can comprise a disubstituted indenyl, a 1,5-disubstituted indenyl, a 1,6-disubstituted indenyl, or a 1,7-disubstituted indenyl. As used herein, the following indenyl numbering is used: [ka]
[0023] As mentioned above, R 1 is a (C1-C4) alkyl, as shown in FIG. 1. Additionally, as shown in FIG. 1, the 2- and 3-positions of the indenyl 5-membered ring are each substituted with hydrogen. Thus, the metal-ligand complex of formula I may be referred to as an asymmetric non-bridged metal-ligand complex. The asymmetric non-bridged metal-ligand complex is a particular class of metal-ligand complex that is desirable for a variety of applications. As known in the art, the asymmetric non-bridged metal-ligand complex can advantageously have excellent stability when activated and stored as a supported catalyst formulation, can be used to produce polyethylene polymers with zero, undetectable, or extremely low levels of long chain branching, and can be operated in gas phase reactors such that the incidence of fouling and / or sheeting is reduced and / or can be controlled by known methods, as compared to other catalysts.
[0024] One or more embodiments provide that the metal-ligand complexes disclosed herein can be represented by Formula II: [ka]
[0025] wherein R is hydrogen or (C1-C2) alkyl, M is titanium, zirconium or hafnium, and each X is independently a halide, (C1-C 20 ) Alkyl, (C7-C 20 )Aralkyl, (C1-C6)Alkyl-substituted (C6-C 12 ) aryl, (C1-C6) alkyl substituted benzyl, or silicon-containing alkyl. 1 is C alkyl, and R 2 is hydrogen, and R 3 is hydrogen, and R 4 is C alkyl, and R 5 is hydrogen.
[0026] The metal-ligand complex of formula II may be referred to as cyclopentadienyl(1,5-dimethylindenyl)zirconium dimethyl, for example, when R is hydrogen, M is zirconium, and each X is a C alkyl, or the metal-ligand complex of formula II may be referred to as methylcyclopentadienyl(1,5-dimethylindenyl)zirconium dimethyl, for example, when R is a C alkyl, M is zirconium, and each X is a C alkyl.
[0027] As shown in Formula I and Formula II, R can be hydrogen or (C1-C4) alkyl. One or more embodiments provide that R is hydrogen. One or more embodiments provide that R is C1-C4 alkyl. For example, R can be a C1 alkyl (e.g., methyl), a C2 alkyl, a C3 alkyl (e.g., propyl) or a C4 alkyl (e.g., butyl). An "alkyl" can be linear, branched, if there are sufficient carbon atoms, or a cyclic paraffin radical that is missing one hydrogen, if there are sufficient carbon atoms. Thus, for example, a CH3 group ("methyl") and a CH3CH2 group ("ethyl") are examples of alkyl.
[0028] As shown in Formula I and Formula II, M can be titanium, zirconium, or hafnium. One or more embodiments provide that M is titanium. One or more embodiments provide that M is zirconium. One or more embodiments provide that M is hafnium.
[0029] As previously mentioned, each X may independently be a halide, (C1-C 20 ) Alkyl, (C7-C 20 )Aralkyl, (C1-C6)Alkyl-substituted (C6-C 12)aryl, (C1-C6)alkyl-substituted benzyl, or silicon-containing alkyl. One or more embodiments provide that each X is a halide, e.g., Cl. One or more embodiments provide that each X is a (C1-C3)alkyl, e.g., C1 alkyl, C2 alkyl, or C3 alkyl. One or more embodiments provide that each X is benzyl.
[0030] As used herein, "substituted" indicates that the group following the term has at least one moiety in place of one or more hydrogens at any position, the moiety being a halogen radical, a hydroxyl group, a carbonyl group, a carboxyl group, an amine group, a phosphine group, an alkoxy group, a phenyl group, a naphthyl group, a C1-C 20 Alkyl groups, C2-C 10 alkenyl groups, and combinations thereof.
[0031] Metal-ligand complexes of formula I, including those of formula II, can be made using the reactants described herein. Metal-ligand complexes of formula I can be made by a number of processes using, for example, conventional solvents, reaction conditions, reaction times, and isolation procedures used to make known metallocenes.
[0032] One or more embodiments provide a polymerization catalyst. The polymerization catalyst can be made by contacting a metal-ligand complex of the complex of formula I with an activator under activation conditions to provide a polymerization catalyst, for example, an activated metal-ligand complex (formula I). Activation conditions are well known in the art.
[0033] As used herein, "activator" refers to any compound or combination of compounds, supported or unsupported, that can activate a complex or catalyst component, for example, by generating a cationic species of the catalyst component. For example, this can include abstraction of at least one leaving group, such as an "X" group as described herein, from the metal center of the complex / catalyst component, for example, a metal complex of formula I. An activator can also be referred to as a "cocatalyst." As used herein, "leaving group" refers to one or more chemical moieties that are bonded to a metal atom and capable of abstraction by an activator, thus generating a species active for olefin polymerization.
[0034] Activators can include Lewis acids or non-coordinating ionic activators or ionizing activators, or any other compounds including Lewis bases, aluminum alkyls, and / or conventional cocatalysts. In addition to the methylaluminoxanes ("MAO") and modified methylaluminoxanes ("MMAO") mentioned above, exemplary activators include, but are not limited to, aluminoxanes or modified aluminoxanes, and / or ionizing compounds, neutral or ionic, such as dimethylanilinium tetrakis(pentafluorophenyl)borate, triphenylcarbenium tetrakis(pentafluorophenyl)borate, dimethylanilinium tetrakis(3,5-(CF3)2phenyl)borate, triphenylcarbenium tetrakis(3,5-(CF3)2phenyl)borate, dimethylanilinium tetrakis(perfluoronaphthalene)borate, triphenylcarben ...
[0033] Examples of the perfluorophenyl tetrakis(perfluoronaphthyl)borate include triphenylcarbenium tetrakis(perfluoronaphthyl)borate, dimethylanilinium tetrakis(pentafluoronaphthyl)aluminate, triphenylcarbenium tetrakis(pentafluoronaphthyl)aluminate, dimethylanilinium tetrakis(perfluoronaphthyl)aluminate, triphenylcarbenium tetrakis(perfluoronaphthyl)aluminate, tris(perfluorophenyl)boron, tris(perfluoronaphthyl)boron, tris(perfluorophenyl)aluminum, tris(perfluoronaphthyl)aluminum, or any combination thereof.
[0035] Aluminoxanes can be described as oligomeric aluminum compounds having -A1(R)-O- subunits, where R is an alkyl group. Examples of aluminoxanes include, but are not limited to, methylaluminoxane ("MAO"), modified methylaluminoxane ("MMAO"), ethylaluminoxane, isobutylaluminoxane, or combinations thereof. Aluminoxanes can be produced by hydrolysis of the respective trialkylaluminum compounds. MMAO can be produced by hydrolysis of trimethylaluminum and higher trialkylaluminums, such as triisobutylaluminum. There are various known methods for preparing aluminoxanes and modified aluminoxanes. Aluminoxanes can include modified methylaluminoxane ("MMAO") type 3A (commercially available from Akzo Chemicals, Inc. under the trade name Modified Methylaluminoxane Type 3A, described in U.S. Pat. No. 5,041,584). The MAO source can be, for example, a solution having about 1% to about 50% MAO by weight. Commercially available MAO solutions include 10% and 30% by weight MAO solutions available from Albemarle Corporation (Baton Rouge, La.).
[0036] One or more organoaluminum compounds, such as one or more alkylaluminum compounds, can be used in combination with the aluminoxane. Examples of alkylaluminum compounds include, but are not limited to, diethylaluminum ethoxide, diethylaluminum chloride, diisobutylaluminum hydride, and combinations thereof. Examples of other alkylaluminum compounds, such as trialkylaluminum compounds, include, but are not limited to, trimethylaluminum, triethylaluminum ("TEAL"), triisobutylaluminum ("TiBAl"), tri-n-hexylaluminum, tri-n-octylaluminum, tripropylaluminum, tributylaluminum, and combinations thereof.
[0037] Polymerization catalysts made from metal-ligand complexes of formula I can be used to make polymers. For example, a polymerization catalyst and an olefin can be contacted under polymerization conditions to form a polymer, such as a polyolefin polymer.
[0038] As used herein, a "polymer" has two or more of the same or different polymer units derived from one or more different monomers, e.g., homopolymer, copolymer, terpolymer, etc. A "homopolymer" is a polymer having the same polymer units. A "copolymer" is a polymer having two or more polymer units that are different from each other. A "terpolymer" is a polymer having three polymer units that are different from each other. When referring to polymer units, "different" indicates that the polymer units differ from each other by at least one atom or are isomerically different. Thus, the definition of a copolymer as used herein includes terpolymers, etc. As used herein, a "polymerization process" is a process used to form a polymer.
[0039] An embodiment provides that the polymer may be a polyolefin polymer. As used herein, "olefin," which may be referred to as "alkene," refers to a linear, branched, or cyclic compound that contains carbon and hydrogen and has at least one double bond. As used herein, when a polymer or copolymer is said to contain (e.g., made from) an olefin, the olefin present in such polymer or copolymer is the polymerized form of the olefin. For example, when a copolymer is said to have an ethylene content of 75% to 85% by weight, it is understood that the polymer units in the copolymer are derived from ethylene in a polymerization reaction, and the derived units are present at 75% to 85% by weight based on the total weight of the polymer. By higher α-olefin is meant an α-olefin with 3 or more carbon atoms.
[0040] Polyolefins include polymers made from olefin monomers such as ethylene, i.e., polyethylene, and linear or branched higher α-olefin monomers containing 3 to 20 carbon atoms. Examples of higher α-olefin monomers include, but are not limited to, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 3,5,5-trimethyl-1-hexene. Examples of polyolefins include, among others, ethylene-1-butene, ethylene-1-hexene, and ethylene-1-octene copolymers, and other ethylene-based polymers having at least 50% by weight ethylene. Other olefins that may be used include, for example, ethylenically unsaturated monomers, diolefins having 4 to 18 carbon atoms, conjugated or non-conjugated dienes, polyenes, vinyl monomers, and cyclic olefins. Examples of monomers include, but are not limited to, norbornene, norbornadiene, isobutylene, isoprene, vinylbenzocyclobutane, styrene, alkyl-substituted styrenes, ethylidene norbornene, dicyclopentadiene, and cyclopentene. In many embodiments, copolymers of ethylene are produced, in which ethylene and a comonomer having at least one α-olefin having 4 to 15 carbon atoms, preferably 4 to 12 carbon atoms, and most preferably 4 to 8 carbon atoms, can be polymerized in a solution process. In another embodiment, ethylene and / or propylene can be polymerized with at least two different comonomers, optionally one of which can be a diene, to form a terpolymer.
[0041] One or more embodiments provide that the polymer can include 50 to 99.9 weight percent ethylene derived units, based on the total weight of the polymer. All individual values and subranges between 50 and 99.9 weight percent are included, for example, the polymer can include a lower limit of 50, 60, 70, 80, or 90 weight percent ethylene derived units, based on the total weight of the polymer, to an upper limit of 99.9, 99.7, 99.4, 99, 96, 93, 90, or 85 weight percent ethylene derived units, based on the total weight of the polymer. The polymer can include 0.1 to 50 weight percent comonomer derived units, based on the total weight of the polymer.
[0042] As discussed above, surprisingly, polymerization catalysts made from the metal-ligand complexes of formula I can be useful for providing polymers having an improved, i.e., reduced, melt index ((I2); D1238-13 (190° C., 2.16 kg load)) compared to polymers formed using other polymerization catalysts under similar polymerization conditions. For example, polymerization catalysts made from the metal-ligand complexes can be useful for providing polymers having a reduced melt index ((I2); D1238-13 (190° C., 2.16 kg load)) compared to polymers formed using other polymerization catalysts when both polymerizations occur at the same polymerization temperature, the same hydrogen concentration, and / or the same comonomer to monomer ratio.
[0043] Additionally, as previously discussed, polymerization catalysts made from the metal-ligand complexes of formula I can surprisingly be useful in providing polymers having improved, i.e., elevated, melting temperatures, as compared to polymers formed using other polymerization catalysts under similar polymerization conditions. For example, polymerization catalysts made from the metal-ligand complexes can be useful in providing polymers having elevated melting temperatures, as compared to polymers formed using other polymerization catalysts, when both polymerizations occur at the same polymerization temperature, the same hydrogen concentration, and / or the same comonomer to monomer ratio.
[0044] Embodiments provide that the polymer can have a melt index (I2) measured by D1238-13 (190°C, 2.16 kg load) in the range of 0.001 g / 10 min to 1000 g / 10 min. For example, the polymer can have a melt index of 0.001 g / 10 min to 500 g / 10 min, or 0.1 g / 10 min to 320 g / 10 min. Some embodiments provide that the melt index is less than 310, less than 300, less than 290, less than 280, less than 270, less than 260, less than 250, less than 240, less than 230, or less than 220.
[0045] An embodiment provides that the polymer may have a Mn (number average molecular weight) of 5,000 to 75,000. All individual values and subranges between 5,000 and 75,000 are included, for example, the polymer may have a Mn from a lower limit of 5,000, 6,000, 7,000, 7,500, 8,000 or 8,500 to an upper limit of 75,000, 65,000, 55,000, 45,000, 35,000, 25,000, 24,000, 23,000 or 22,000. Mn may be determined by gel permeation chromatography (GPC), as known in the art.
[0046] An embodiment provides that the polymer may have a Mw (weight average molecular weight) of 15,000 to 110,000. All individual values and subranges between 15,000 and 110,000 are included, for example, the polymer may have a Mw from a lower limit of 15,000, 20,000, 22,000, 24,000, 24,500, or 25,000 to an upper limit of 110,000, 100,000, 80,000, 60,000, or 40,000. As is known in the art, Mw can be determined by GPC.
[0047] An embodiment provides that the polymer may have an Mz (z-average molecular weight) of 40,000 to 400,000. All individual values and subranges between 40,000 and 400,000 are included, for example, the polymer may have an Mz of 40,000, 44,000, 46,000, 47,000, 48,000, 48,500, or 49,000 at lower limits to 400,000, 300,000, 200,000, 100,000, or 65,000 at upper limits. As is known in the art, Mz can be determined by GPC.
[0048] An embodiment provides that the polymer may have a molecular weight distribution, determined as Mw / Mn (weight average molecular weight / number average molecular weight), of 2.50 to 8.00. All individual values and subranges between 2.50 and 8.00 are included, for example, the polymer may have a Mw / Mn with a lower limit of 2.50, 2.80, 2.90, 3.00, or 3.10 to an upper limit of 8.00, 7.50, 7.00, or 6.50. Mw / Mn may be determined by GPC analysis, as known in the art.
[0049] An embodiment provides that the polymer may have a melting temperature of 100-165° C. All individual values and subranges between 100-165° C. are included, for example, the polymer may have a melting temperature of lower limits of 100, 110, 120, 125, 128, 129, 130° C. to upper limits of 165, 160, 155, 150, 140, 135° C. The melting temperature may be determined by differential scanning calorimetry according to ASTM D3418-08.
[0050] In an embodiment, the polymer has a viscosity of 0.890 g / cm 3 ~0.970g / cm 3 It is provided to obtain a concentration of 0.890 to 0.970 g / cm 3 All individual values and subranges of 0.890, 0.900, 0.910, 0.920, 0.930, 0.940, 0.950, 0.957, 0.958, 0.959, or 0.960 g / cm are included, for example, the polymer may have a molecular weight of 0.890, 0.900, 0.910, 0.920, 0.930, 0.940, 0.950, 0.957, 0.958, 0.959, or 0.960 g / cm 3from the lower limit of 0.970, 0.966, 0.966, or 0.963 g / cm 3 Density can be determined according to ASTM D-792-13, Standard Test Method for Density and Specific Gravity (Relative Density) of Plastics by Displacement, Method B (for testing solid plastics in liquids other than water, e.g., liquid 2-propanol). Results are reported in units of grams per cubic centimeter (g / cm 3 )
[0051] One or more embodiments provide that the polymer can be a bimodal polymer. For example, the bimodal polymer can include a low molecular weight component, for example, as described herein.
[0052] Gel Permeation Chromatography (GPC) Test Method: Weight-average molecular weight test method: Using a chromatogram obtained with a high-temperature gel permeation chromatography device (HTGPC, Polymer Laboratories), M w , number average molecular weight (M n ), and M w / M nThe HTGPC is equipped with a transfer line, a differential refractive index detector (DRI), and three Polymer Laboratories PLgel 10 μm Mixed-B columns, all housed in an oven maintained at 160 °C. The method uses a solvent consisting of BHT-treated TCB at a nominal flow rate of 1.0 milliliters per minute (mL / min) and a nominal injection volume of 300 microliters (μL). The solvent is prepared by dissolving 6 grams of butylated hydroxytoluene (BHT, an antioxidant) in 4 liters (L) of reagent-grade 1,2,4-trichlorobenzene (TCB) and filtering the resulting solution through a 0.1 micrometer (μm) Teflon filter to obtain the solvent. The solvent is degassed with an in-line degasser before it enters the HTGPC instrument. The column is calibrated with a series of monodisperse polystyrene (PS) standards. Separately, prepare a known concentration of the test polymer dissolved in a known amount of solvent by heating a known amount of it in the solvent at 160 °C for 2 h with continuous shaking. (All amounts are measured gravimetrically.) The target solution concentration c of the test polymer is 0.5 to 2.0 milligrams polymer per milliliter solution (mg / mL), with lower concentrations of c being used for higher molecular weight polymers. Before running each sample, purge the DRI detector. Then, increase the flow rate in the instrument to 1.0 mL / min and allow the DRI detector to stabilize for 8 h before injecting the first sample. Using the general calibration relationship for column calibration, determine the M w and M. n Calculate the MW at each elution volume using the following formula:
number
[0334] -
[0341] . GPC chromatograms are obtained by plotting dW / dLog(MW) on the y-axis and Log(MW) on the x-axis (Log(MW) and dW / dLog(MW) are as defined above).
[0053] The polymers may be used in many articles such as films, fibers, nonwoven and / or woven fabrics, extruded articles, and / or molded articles, among others.
[0054] A bimodal catalyst system is provided that includes a metal-ligand complex of formula I and a bis(2-(pentamethylphenylamido)ethyl)-amine zirconium complex of formula III: [ka]
[0055] Also provided is a bimodal catalyst system comprising a metal-ligand complex of formula I or an activated reaction product thereof and at least one olefin polymerization catalyst (second catalyst) that is not a metal-ligand complex of formula I or formula III or an activated reaction product thereof. Such second catalyst can be a Ziegler-Natta catalyst, a chromium-based catalyst (e.g., a so-called Phillips catalyst), a metallocene catalyst that does not contain an indenyl ring (e.g., a metallocene catalyst that contains an unsubstituted and / or alkyl-substituted cyclopentadienyl ring), a Group 15 metal-containing catalyst compound as described in paragraphs
[0041] to
[0046] of WO 2018 / 064038A1, or a biphenylphenol-based catalyst compound as described in paragraphs
[0036] to
[0080] of U.S. Patent Application Publication No. 20180002464.
[0056] The metal-ligand complexes of formula I and other components discussed herein, such as activators and / or additional polymerization components, may be used with a support. "Support," also called a carrier, refers to any support material, including porous support materials such as talc, inorganic oxides, and inorganic chlorides.
[0057] The metal-ligand complex of formula I, as well as other components discussed herein, can be supported on the same or separate supports, or one or more components can be used in unsupported form. Using a support can be accomplished by any technique used in the art. One or more embodiments provide that a spray drying process is used. Spray drying processes are well known in the art. The support can be functionalized.
[0058] The support may be a porous support material, such as talc, an inorganic oxide, or an inorganic chloride. Other support materials include resin support materials, functionalized or crosslinked organic supports, such as polystyrene, polystyrene divinylbenzene polyolefins or polymeric compounds, zeolites, clays, or any other organic or inorganic support material, or mixtures thereof.
[0059] Support materials include inorganic oxides, including metal oxides of groups 2, 3, 4, 5, 13, or 14. Some preferred supports include silica, fumed silica, alumina, silica-alumina, and mixtures thereof. Some other supports include magnesia, titania, zirconia, magnesium chloride, montmorillonite, phyllosilicates, zeolites, talc, clay, and the like. Also, combinations of these support materials can be used, such as silica-chrome, silica-alumina, silica-titania, and the like. Additional support materials include porous acrylic polymers, nanocomposites, aerogels, spherulites, and polymer beads.
[0060] One example of a support is fumed silica available under the trade name Cabosil™ TS-610, or other TS or TG series supports available from Cabot Corporation. Fumed silica is typically silica having particles 7 to 30 nanometers in size that have been treated with dimethylsilyl dichloride so that most of the surface hydroxyl groups are capped.
[0061] The support material has a surface area ranging from about 10 to about 700 m / g, and a surface area ranging from about 0.1 to about 4.0 g / cm 3 and an average particle size in the range of about 5 to about 500 μm. More preferably, the surface area of the support material is in the range of about 50 to about 500 m / g and about 0.5 to about 3.5 g / cm. 3 and an average particle size of about 10 to about 200 μm. Most preferably, the surface area of the support material ranges from about 100 to about 400 m / g and from about 0.8 to about 3.0 g / cm. 3 and an average particle size of about 5 to about 100 μm. The average pore diameter of the support is typically in the range of 10 to 1000 A, preferably 50 to about 500 A, and most preferably 75 to about 350 A.
[0062] The metal-ligand complex of formula I and other components discussed herein, such as an activator and / or additional polymerization components, can be slurried. Slurries are well known in the art. The slurry can include, for example, the metal-ligand complex of formula I, an activator, and a support.
[0063] The molar ratio of the metal in the activator to the metal in the metal-ligand complex of formula I and / or additional polymerization components in the slurry can be 1000:1 to 0.5:1, 300:1 to 1:1, or 150:1 to 1:1. One or more diluents, e.g., fluids, can be used to facilitate the combination of any two or more components in the slurry. For example, the metal-ligand complex of formula I and the activator can be combined together in the presence of toluene or another non-reactive hydrocarbon or mixture of hydrocarbons. In addition to toluene, other suitable diluents include, but are not limited to, ethylbenzene, xylene, pentane, hexane, heptane, octane, other hydrocarbons, or any combination thereof. The support, either dried or mixed with toluene, can then be added to the mixture, or the metal-ligand complex / activator can be added to the support. The slurry can be fed to a reactor for a polymerization process, and / or the slurry can be dried (e.g., spray dried) before being fed to a reactor for a polymerization process.
[0064] The polymerization process may be a suspension polymerization process, a slurry polymerization process, and / or a gas phase polymerization process. The polymerization process may be used using known equipment and reaction conditions, such as known polymerization conditions. The polymerization process is not limited to any particular type of polymerization system. By way of example, the polymerization temperature may range from about 0° C. to about 300° C. at atmospheric, subatmospheric, or superatmospheric pressures. In particular, slurry or solution polymerization systems may use subatmospheric or superatmospheric pressures and temperatures ranging from about 40° C. to about 300° C. An embodiment provides a method of making a polyolefin polymer, comprising contacting an olefin with a polymerization catalyst under polymerization conditions to polymerize the olefin to make a polyolefin polymer.
[0065] One or more embodiments provide that the polymer may be formed via a gas phase polymerization system at pressures above atmospheric ranging from 0.07 to 68.9 bar, 3.45 to 27.6 bar, or 6.89 to 24.1 bar, and temperatures ranging from 30 to 130° C., 65 to 110° C., 75 to 120° C., or 80 to 120° C. In one or more embodiments, the operating temperature may be less than 112° C. Stirred and / or fluidized bed gas phase polymerization systems may be used.
[0066] In general, a conventional gas-phase fluidized bed polymerization process can be carried out by continuously passing a stream containing one or more olefin monomers through a fluidized bed reactor at a rate sufficient to maintain a bed of solid particles in suspension under reactive conditions and in the presence of a catalyst composition, such as a composition comprising a metal complex of formula I and an activator. A stream containing unreacted monomers can be continuously withdrawn from the reactor, compressed, cooled, optionally partially or completely condensed, and recycled to the reactor. The product, i.e., polymer, can be removed from the reactor and a replacement monomer can be added to the recycle stream. Gases inert to the catalyst composition and reactants can also be present in the gas stream. The polymerization system can include, for example, a single reactor or two or more reactors in series.
[0067] The feed stream of the polymerization process may include olefin monomers, non-olefin gases such as nitrogen and / or hydrogen, and may further include one or more non-reactive alkanes that are condensable in the polymerization process and can be used to remove heat of reaction. Exemplary non-reactive alkanes include, but are not limited to, propane, butane, isobutane, pentane, isopentane, hexane, their isomers and their derivatives. The feed may enter the reactor at a single or multiple different locations.
[0068] In the polymerization process, the polymerization catalyst may be continuously fed to the reactor. A gas that is inert to the polymerization catalyst, such as nitrogen or argon, may be used to carry the polymerization catalyst to the reactor bed. In one embodiment, the polymerization catalyst may be provided as a slurry in mineral oil or a liquid hydrocarbon or mixture, such as, for example, propane, butane, isopentane, hexane, heptane or octane. The slurry may be delivered to the reactor with a carrier fluid, such as, for example, nitrogen or argon, or a liquid, such as, for example, isopentane or other C3-C8 alkanes.
[0069] In the polymerization process, hydrogen may be used in a gas molar ratio of hydrogen to ethylene in the reactor that may range from lower limits of 0.0002, 0.0006, 0.001, 0.0016, 0.002, 0.004 to upper limits of 0.1, 0.05, 0.01, 0.008, 0.006. Many embodiments use hydrogen gas.
[0070] The polymerization process can use a gas phase polymerization (GPP) reactor, such as a stirred bed gas phase polymerization reactor (SB-GPP reactor) or a fluidized bed gas phase polymerization reactor (FB-GPP reactor), to make the polymer. Such reactors and processes are generally well known. The gas phase polymerization reactor / process can be a fluidized bed reactor / process, such as those described in US 3,709,853, US 4,003,712, US 4,011,382, US 4,302,566, US 4,543,399, US 4,882,400, US 5,352,749, US 5,541,270, EP-A-0802202, and Belgian Patent No. 839,380. These SB-GPP and FB-GPP polymerization reactors and processes are either mechanically stirred or fluidized by a continuous flow of the polymerization medium of gaseous monomer and diluent inside the reactor, respectively. Other useful reactors / processes contemplated include continuous or multi-stage polymerization processes such as those described in US 5,627,242, US 5,665,818, US 5,677,375, EP-A-0794200, EP-B1-0649992, EP-A-0802202, and EP-B-634421.
[0071] Polymerization operating conditions are any variable or combination of variables that can affect the polymerization reaction in the GPP reactor or the composition or properties of the polymer produced thereby. Variables include reactor design and dimensions, composition and amounts of components, molar ratios of different reactants, presence or absence of feed gases such as H2 and / or O2, molar ratio of feed gas to reactants, absence or concentration of interfering substances (e.g., H2O), presence or absence of induced condensing agents (ICAs), average residence time of polymer in the reactor, partial pressures of components, feed rate of monomer, reactor bed temperature (e.g., fluidized bed temperature), nature or sequence of process steps, transition periods between steps. Variables other than those described or changed by the method or use may be kept constant.
[0072] In the polymerization process, a fixed comonomer to ethylene monomer gas ratio (C) equal to a stated value (e.g., 0.00500) is used. X / C2, e.g., C6 / C2), ethylene ("C2"), hydrogen ("H2") and 1-hexene ("C6" or "C X ", where x is 6), a constant hydrogen to ethylene gas molar ratio ("H2 / C2") equal to the stated value (0.00200), and a constant ethylene ("C2") partial pressure equal to the stated value (e.g., 1,000 kPa) can be controlled individually. The concentrations of the gases can be measured by an in-line gas chromatograph to understand and maintain the composition in the recycle gas stream. The reaction bed of growing polymer particles can be maintained in a fluidized state by continuously flowing the make-up feed and recycle gas through the reaction zone. A superficial gas velocity of 0.49 to 0.67 meters per second (m / s) (1.6 to 2.2 feet per second (ft / s)) can be used. The FB-GPP reactor can be operated at a total pressure of about 2344 to about 2413 kilopascals (kPa) (about 340 to about 350 pounds per square inch gauge (psig)), and the desired first reactor bed temperature. The fluidized bed can be maintained at a constant height by withdrawing a portion of the bed at a rate equal to the production rate of the particulate form of the bimodal ethylene-co-1-hexene copolymer composition, which can be 10 to 20 kilograms per hour (kg / hr). The product, e.g., a polymer such as the bimodal ethylene-co-1-hexene copolymer composition, is removed semi-continuously through a series of valves into a fixed volume chamber, and the removed bimodal ethylene-co-1-hexene copolymer composition is purged to remove entrained hydrocarbons and treated with a stream of humidified nitrogen (N2) gas to deactivate traces of residual catalyst.
[0073] The catalyst system may be fed to the polymerization reactor(s) in "dry mode" or "wet mode", or in dry mode, or in wet mode. Dry mode is as a dry powder or granules. Wet mode is as a suspension in an inert liquid such as mineral oil.
[0074] Induction condensing agents (ICAs), such as inert liquids useful for cooling materials in gas phase polymerization reactor(s), may be used. ICAs are generally classified into four groups: (C5-C 20) an alkane, such as 2-methylbutane (i.e., isopentane). An embodiment of the process using ICA may be referred to as being inductively condensed mode operation (ICMO). ICMO is described in US 4,453,399, US 4,588,790, US 4,994,534, US 5,352,749, US 5,462,999, and US 6,489,408. Gas chromatography can be used to measure the concentration of ICA in the gas phase by calibrating the peak area percentage to mole percent (mol%) with gas mixture standards of known gas phase component concentrations. The concentration of ICA can be from 1 to 10 mol%.
[0075] The polymerization process may further include one or more additives such as chain transfer agents or accelerators. Chain transfer agents are well known and may be alkyl metals such as diethyl zinc. Accelerators are known such as in US 4,988,783 and may include chloroform, CFCl3, trichloroethane, and difluorotetrachloroethane. A scavenger may be used to react with moisture prior to reactor start-up and may be used to react with excess activator during reactor transition. The scavenger may be trialkylaluminum. Gas phase polymerization may be operated without a scavenger (without intentionally being added). The polymerization conditions of the gas phase polymerization reactor / method may further include an amount (e.g., 0.5-200 ppm based on all feeds to the reactor) of a static charge control agent and / or a continuity additive such as aluminum stearate or polyethyleneimine. A static charge control agent may be added to the FB-GPP to inhibit the formation or accumulation of static charge on the FB-GPP.
[0076] The polymerization process may employ a pilot-scale fluidized bed gas-phase polymerization reactor (pilot reactor) including a reaction vessel containing a fluidized bed of powder of the bimodal ethylene-co-1-hexene copolymer composition and a distribution plate disposed above the bottom head, defining a bottom gas inlet and having an expansion section or cyclone system at the top of the reaction vessel to reduce the amount of resin fines that may escape the fluidized bed. The expansion section may define a gas outlet. The pilot reactor may further include a compressor blower of sufficient power to continuously circulate or loop gas from the gas outlet of the expansion section at the top of the reaction vessel to the bottom gas inlet of the pilot reactor and through the distribution plate and the fluidized bed. The pilot reactor may further include a cooling system to remove the heat of polymerization and maintain the fluidized bed at a target temperature. The composition of the gases, such as ethylene, alpha-olefins (e.g., 1-hexene), and hydrogen, fed to the pilot reactor may be monitored by an in-line gas chromatograph in a cycle loop to maintain specific concentrations that can define and control the properties of the polymer. The catalyst system can be fed to the pilot reactor from the high pressure device as a slurry or dry powder, with the slurry being fed via a syringe pump and the dry powder being fed via a metering disk. The catalyst system usually enters the fluidized bed at less than 1 / 3 of its bed height. The pilot reactor can further include a method for weighing the fluidized bed and an isolation port (product discharge system) for discharging the bimodal ethylene-co-1-hexene copolymer composition powder from the reactor vessel in response to the increase in fluidized bed weight as the polymerization reaction proceeds.
[0077] In some embodiments, the FB-GPP reactor is a commercial-scale reactor, such as a UNIPOL™ reactor or a UNIPOL™ II reactor, available from Univation Technologies, LLC, a subsidiary of The Dow Chemical Company, Midland, Michigan, USA.
[0078] Some aspects of the present disclosure are provided as follows.
[0079] Aspect 1 is a metal-ligand complex of formula I, [ka] In the formula, M is titanium, zirconium or hafnium, R is hydrogen or (C1-C4) alkyl, and R 1 is (C1-C4) alkyl, R 2 , R 3 , R 4 , R 5 Any one or two of the following can be independently selected: 20 ) alkyl, R 2 , R 3 , R 4 , R 5 Three or two of the X's are H, and each X is independently a halide, (C1-C 20 ) Alkyl, (C7-C 20 )Aralkyl, (C1-C6)Alkyl-substituted (C6-C 12 ) aryl, (C1-C6) alkyl substituted benzyl or silicon-containing alkyl.
[0080] Aspect 2 is a metal-ligand complex of formula II: [ka] wherein R is hydrogen or (C1-C2) alkyl, M is titanium, zirconium or hafnium, and each X is independently a halide, (C1-C 20 ) Alkyl, (C7-C 20 )Aralkyl, (C1-C6)Alkyl-substituted (C6-C 12 ) aryl, (C1-C6) alkyl substituted benzyl, or silicon-containing alkyl.
[0081] Aspect 3 provides a metal-ligand complex according to aspect 1 or aspect 2, wherein R is hydrogen.
[0082] Aspect 4 provides a metal-ligand complex according to aspect 1 or aspect 2, wherein R is (C1-C2) alkyl.
[0083] Embodiment 5 provides a metal-ligand complex according to any one of embodiments 1 and 4, wherein R is methyl.
[0084] Aspect 6 provides a metal-ligand complex according to any one of aspects 1 and 4, wherein R is ethyl.
[0085] Example 7 provides a metal-ligand complex according to any one of Examples 1 to 6, wherein M is Zr.
[0086] Example 8 provides a metal-ligand complex according to any one of Examples 1 to 7, wherein each X is independently Cl, (C1-C3) alkyl, or benzyl.
[0087] Embodiment 9 provides a metal-ligand complex according to embodiment 1 or embodiment 2, selected from: where R is hydrogen, M is zirconium, and each X is Cl. where R is methyl, M is zirconium, and each X is Cl. where R is ethyl, M is zirconium, and each X is Cl. where R is hydrogen, M is zirconium, and each X is methyl. where R is methyl, M is zirconium, each X is methyl, and where R is ethyl, M is zirconium, and each X is methyl.
[0088] Aspect 10 is a bimodal catalyst system comprising a metal-ligand complex according to any one of aspects 1-9 and a bis(2-(pentamethylphenylamido)ethyl)-amine zirconium complex of formula III, [ka] In the formula, M is Zr, and each R 1are independently Cl, Br, (C1-C 20 )Alkyl, (C1-C6)Alkyl-substituted (C6-C 12 ) aryl, benzyl, or (C1-C6) alkyl substituted benzyl.
[0089] Example 11 provides a method of making a polymerization catalyst, the method including contacting a metal-ligand complex of any one of Examples 1-9 or a bimodal catalyst system of Example 10 with an activating agent under activating conditions to activate the metal-ligand complex or the bimodal catalyst system, thereby making the polymerization catalyst.
[0090] Example 12 provides the method of example 11, wherein the activator is methylaluminoxane.
[0091] Example 14 provides a polymerization catalyst made by the method of any one of Examples 11-12.
[0092] Example 14 is a method of making a polyolefin polymer, comprising: A method is provided that includes contacting an olefin with the polymerization catalyst of embodiment 13 under polymerization conditions to polymerize the olefin and thereby make a polyolefin polymer.
[0093] Example 15 provides a polyolefin polymer made by the method of example 14.
[0094] Example 16 provides a metal-ligand complex according to any one of Examples 1 to 6, wherein M is zirconium or hafnium. The present invention includes the following aspects. Section 1. A metal-ligand complex of formula I, [ka] In the formula, M is titanium, zirconium or hafnium, R is hydrogen or (C1-C4) alkyl, and R 1is (C1-C4) alkyl, R 2 , R 3 , R 4 , R 5 Any one or two of the following can be independently selected: 20 ) alkyl, R 2 , R 3 , R 4 , R 5 Three or two of the X's are H, and each X is independently a halide, (C1-C 20 ) Alkyl, (C7-C 20 )Aralkyl, (C1-C6)Alkyl-substituted (C6-C 12 ) aryl, (C1-C6) alkyl substituted benzyl or silicon-containing alkyl. Section 2. A metal-ligand complex of formula I, wherein R 1 is C1 alkyl, R 2 is hydrogen, and R 3 is C1 alkyl, R 4 is hydrogen, and R 5 is hydrogen; [ka] wherein R is hydrogen or (C1-C2) alkyl, M is titanium, zirconium or hafnium, and each X is independently a halide, (C1-C 20 ) Alkyl, (C7-C 20 )Aralkyl, (C1-C6)Alkyl-substituted (C6-C 12 ) aryl, (C1-C6) alkyl substituted benzyl, or silicon-containing alkyl. Section 3. Item 3. The metal-ligand complex according to item 1 or 2, wherein R is hydrogen. Section 4. Item 3. The metal-ligand complex according to item 1 or 2, wherein R is (C1-C2) alkyl. Section 5. 5. The metal-ligand complex of any one of claims 1, 2, and 4, wherein R is methyl. Section 6. 5. The metal-ligand complex according to any one of claims 1, 2 and 4, wherein R is ethyl. Section 7. Item 7. The metal-ligand complex according to any one of items 1 to 6, wherein M is Zr. Section 8. 8. The metal-ligand complex according to any one of claims 1 to 7, wherein each X is independently Cl, (C1-C3) alkyl, or benzyl. Section 9. below, A metal-ligand complex of formula I, wherein R is hydrogen, M is zirconium, and each X is Cl; A metal-ligand complex of formula I, wherein R is methyl, M is zirconium, and each X is Cl; A metal-ligand complex of formula I, wherein R is ethyl, M is zirconium, and each X is Cl; A metal-ligand complex of formula I, wherein R is hydrogen, M is zirconium, and each X is methyl; A metal-ligand complex of formula I, wherein R is methyl, M is zirconium, and each X is methyl; and Item 3. The metal-ligand complex according to item 1 or 2, selected from the group consisting of metal-ligand complexes of formula I, in which R is ethyl, M is zirconium, and each X is methyl. Section 10. A bimodal catalyst system comprising the metal-ligand complex according to any one of claims 1 to 9 and a bis(2-(pentamethylphenylamido)ethyl)-amine zirconium complex of formula III, [ka] In the formula, M is Zr, and each R 1 are independently Cl, Br, (C1-C 20 )Alkyl, (C1-C6)Alkyl-substituted (C6-C 12 ) aryl, benzyl, or (C1-C6) alkyl substituted benzyl, a bimodal catalyst system. Section 11. A method for preparing a polymerization catalyst, the method comprising contacting the metal-ligand complex of any one of claims 1 to 9 or the bimodal catalyst system of claim 10 with an activating agent under activating conditions to activate the metal-ligand complex or the bimodal catalyst system, thereby preparing a polymerization catalyst. Section 12. Item 12. The method of item 11, wherein the activating agent is methylaluminoxane. Section 13. Item 13. A polymerization catalyst produced by the method according to any one of items 11 to 12. Section 14. 1. A method of making a polyolefin polymer, the method comprising: 14. A method of making a polyolefin polymer by contacting an olefin with the polymerization catalyst of claim 13 under polymerization conditions to polymerize the olefin. Section 15. Item 15. A polyolefin polymer produced by the method according to item 14. EXAMPLES
[0095] 3,6-Dimethyl-1H-indene represented by the following formula, [ka]
[0096] Prepared as follows: 3,6-Dimethyl-1H-indene can be deprotonated to form the anion that can be referred to as 1,5-dimethyl-indenyl. In a glove box, a 250 mL two-neck vessel equipped with a thermometer (side port) and a solid addition funnel was charged with tetrahydrofuran (25 mL) and methylmagnesium bromide (2 equiv., 18.24 mL, 54.72 mmol). The contents of the vessel were cooled in a freezer set at -35°C for 40 minutes and upon removal from the freezer, the contents of the vessel were measured to be -12°C. With stirring, indanone [5-methyl-2,3-dihydro-1H-inden-1-one (catalog #HC-2282)] (1 equiv., 4.000 g, 27.36 mmol) was added in small portions as a solid to the vessel, causing an exothermic reaction to increase in temperature. The addition was controlled to maintain the temperature at or below room temperature. Once the addition was complete, the funnel was removed and the vessel was sealed (SUBA). The sealed vessel was transferred into a fume hood (contents were already at room temperature), placed under a nitrogen purge, and stirred for 3 hours. The nitrogen purge was removed and diethyl ether (25 mL) was added to the vessel to replace the evaporated solvent, then the reactants were cooled using an acetone / ice bath. HCl (15% by volume) solution (9 equiv., 50.67 mL, 246.3 mmol) was added very slowly to the vessel contents using an addition funnel, maintaining the temperature below 10° C. The vessel contents were then allowed to warm slowly (bath installed) for approximately 12 hours. The vessel contents were then transferred to a separatory funnel and the phases were separated. The aqueous phase was washed with diethyl ether (3×25 mL). The combined organic phase was then washed with sodium bicarbonate (50 mL, saturated aqueous solution), water (50 mL), and brine (50 mL). The organic phase was dried over magnesium sulfate, filtered, and the solvent removed on a rotary evaporator. The resulting dark oil, confirmed as product by NMR, was dissolved in pentane (25 mL) and filtered through a short silica plug (pre-wetted with pentane) capped with sodium sulfate. Additional pentane (25-35 mL) was used to rinse the plug, then combined with the initial pentane. The solution was dried on a rotary evaporator to give 2.87 g (74% yield) of 3,6-dimethyl-1H-indene, confirmed as product by NMR.1 H NMR (C6D6): δ7.18(d,1H), 7.09(s,1H), 7.08(d,1H), 5.93(mult,1H), 3.07(mult,2H), 2.27(s,3H), 2.01(q,3H).
[0097] Example 1, cyclopentadienyl(1,5-dimethylindenyl)zirconium dimethyl, was prepared as follows: In a glove box, 3,6-dimethyl-1H-indene (1.000 g, 6.94 moles) in dimethoxyethane (10 mL) was added to a 4 ounce container, the container was capped, and the contents of the container were cooled to -35°C. Butyllithium (1.6 M in hexane, 4.3 mL, 0.0069 moles) was added to the container and the contents were stirred for approximately 3 hours while removing heat to maintain the contents near -35°C. 1 The progress of the reaction was monitored by dissolving small aliquots in d8-THF for H NMR analysis. Upon completion of the reaction, solid cyclopentadienyl zirconium trichloride (CpZrCl3) (1.821 g) was added portionwise to the contents of the vessel with stirring. 1 The progress of the reaction was monitored by dissolving a small aliquot in d8-THF for H NMR analysis. The reaction was complete after about 3 hours, and the contents of the vessel were stirred for about an additional 12 hours. Methylmagnesium bromide (3.0 M in ether, 4.6 mL) was then added to the contents of the vessel, and after the addition, the contents of the vessel were stirred for about 12 hours. The solvent was then removed in vacuo, and the product was extracted into hexane (40 mL), filtered through Celite, washed with additional hexane (30 mL), and then dried under vacuum to give cyclopentadienyl(1,5-dimethylindenyl)zirconium dimethyl. 1 H NMR analysis confirmed the identity of cyclopentadienyl(1,5-dimethylindenyl)zirconium dimethyl. 1 H NMR(C6D6): δ7.26(d,1H),6.92(d,1H),6.83(dd,1H),5.69(d,1H),5.65(mu lt,1H),5.64(s,5H),2.18(s,3H),2.16(s,3H),-0.34(s,3H),-0.62(s,3H).
[0098] Example 2, cyclopentadienyl(1,5-dimethylindenyl)zirconium dichloride, was prepared as follows: In a glove box, 3,6-dimethyl-1H-indene (5.00 g, 34.7 mmol) and hexane (100 mL) were placed in a vessel. While stirring with a magnetic stir bar, n-butyllithium (1.6 M in hexane, 23.8 mL, 38.1 mmol) was added slowly to the contents of the vessel, then stirred for about 12 hours to give a precipitate that was observed to be solid and white. The precipitate was collected by filtration, washed with hexane (3×20 mL), and dried under vacuum to give 1,5-dimethylindenyllithium (4.88 g, 93.7% yield), observed to be a white solid.
[0099] Next, in a glove box, a portion of 1,5-dimethylindenyllithium (2.315 g, 15.42 mmol) was dissolved in dimethoxyethane (60 mL) in a vessel, then CpZrCl3 (4.05 g, 15.42 mmol) was added portionwise as a solid. After stirring for approximately 12 hours, the solvent was removed in vacuo and the contents of the vessel were taken up in toluene (110 mL) at 60 °C and filtered. NMR analysis of an aliquot then showed the desired product. To purify the product, the volume of the filtrate was reduced to 40 mL in vacuo and the temperature was raised to 80 °C to dissolve. The solution was then slowly cooled to room temperature and then kept in a glove box freezer (−32° C.) to precipitate the recrystallized product, which was collected by filtration, washed with hexanes (2×10 mL), and then dried under vacuum to give cyclopentadienyl(1,5-dimethylindenyl)zirconium dichloride, which was observed to be a light yellow solid (4.09 g, 71.6%). 1 H NMR (C6D6): d7.32(m,1H), 6.90(dt,1H), 6.75(dd,1H), 6.19(dq,1H), 5.76(s,5H), 5.73(m,1H), 2.35(d,3H), 2.08(d,3H).
[0100] Example 3, methylcyclopentadienyl(1,5-dimethylindenyl)zirconium dichloride, was prepared as follows: 1,5-dimethylindenyllithium was prepared as described in Example 2. In a glove box, 1,5-dimethylindenyllithium (0.500 g, 3.33 mmol) was dissolved in dimethoxyethane (30 mL) in a vessel and MeCpZrCl3 (0.921 g, 3.33 mmol) was added portionwise as a solid. After stirring for approximately 12 hours, the solvent was removed in vacuo and the vessel contents were taken up in dichloromethane (40 mL) and filtered. NMR analysis of an aliquot showed the desired product. To purify the product, the volume of the filtrate was reduced to 20 mL in vacuo and hexane (20 mL) was added. The solution was then kept in a glove box freezer (−32° C.) to precipitate the recrystallized product, which was collected by filtration, washed with hexane (3×5 mL), and then dried in vacuum to give methylcyclopentadienyl(1,5-dimethylindenyl)zirconium dichloride (0.527 g, 41.1%). 1 H NMR(C6D6): δ7.32(m,1H), 6.93(m,1H), 6.75(dd,1H), 6.25(dd,1H), 5.76(m,2H) , 5.58(m,1H), 5.52(m,1H), 5.38(td,1H), 2.37(d,3H), 2.09(d,3H), 2.01(s,3H).
[0101] Example 4, propylcyclopentadienyl(1,5-dimethylindenyl)zirconium dichloride, was prepared as follows: 1,5-dimethylindenyllithium was prepared as described in Example 2. In a glove box, 1,5-dimethylindenyllithium (0.500 g, 3.33 mmol) was dissolved in dimethoxyethane (30 mL) in a vessel and PrCpZrCl3(DME) (1.315 g, 3.33 mmol) was added portionwise as a solid. After stirring for approximately 12 hours, the solvent was removed in vacuo and the contents of the vessel were taken up in toluene (50 mL) and filtered. NMR analysis of an aliquot showed the desired product. To purify the product, the volume of the filtrate was reduced to 25 mL in vacuo and hexane (25 mL) was added. The resulting mixture was heated to 60° C. to dissolve and then kept in a glove box freezer (−32° C.) to precipitate the recrystallized product, which was collected by filtration, washed with hexane (3×5 mL), and then dried in vacuum to give propylcyclopentadienyl(1,5-dimethylindenyl)zirconium dichloride (0.893 g, 65.0%). 1 H NMR(C6D6): δ7.34(m,1H), 6.96(m,1H), 6.77(dd,1H), 6.27(dd,1H), 5.85(m,1H), 5.81(dd,1H), 5.68(d t,1H), 5.57(td,1H), 5.46(td,1H), 2.47(td,2H), 2.39(d,3H), 2.11(d,3H), 1.36(m,2H), 0.75(t,3H).
[0102] 4,7-Dimethyl-1H-indene was prepared by one of two methods (Method A or Method B).
[0103] Method A
[0104] A 500 mL two-neck round-bottom vessel equipped with a magnetic stir bar, a powder addition funnel containing aluminum chloride (16.04 g, 120.3 mmol), a nitrogen inlet, and an outlet purging to a NaOH scrubber was flushed with dry nitrogen gas. The vessel was charged with anhydrous dichloromethane (70 mL), followed by p-xylene (14.91 g, 140.5 mmol) and 3-chloropropionyl chloride (13.35 g, 105.1 mmol), then cooled using an ice-water bath. Excess aluminum chloride was then added via the powder addition funnel over 90 minutes, then the vessel was warmed to 10 °C, then stirred for approximately 2 hours. The contents of the vessel were then poured onto ice, resulting in a color change from red to yellow. The organic layer was separated, washed three times with water, dried over anhydrous magnesium sulfate, filtered, and condensed under vacuum to form the intermediate, which was observed to be a yellow liquid. Sulfuric acid (60 mL) was then added to the vessel, the intermediate was added to the vessel via syringe over 30 minutes, and the vessel contents were slowly heated to 65° C. and held at this temperature for 2 hours. The vessel contents were cooled to room temperature, poured onto ice, and extracted with diethyl ether (100 mL). The organic layer was washed with sodium bicarbonate solution and water, dried over anhydrous magnesium sulfate, and condensed under vacuum to give the crude product, which was observed to be a tan solid. Purification by column chromatography (SiO2, hexane:ethyl acetate=90:10) gave 4,7-dimethylindan-1-one, which was observed to be a light yellow / tan solid (11.82 g, 70.43%).
[0105] 4,7-Dimethylindan-1-one (8.040 g, 50.18 mmol), methanol (150 mL) and THF (50 mL) were added to a 500 mL two-neck round-bottom vessel equipped with a magnetic stir bar, removable cap, and reflux condenser fitted with a nitrogen inlet. The contents of the vessel were cooled in an ice bath to a temperature of 5° C. Sodium borohydride (1.96 g, 51.81 mmol) was added to the vessel in small portions through the removable cap over a period of 60 minutes with stirring, allowing gas evolution to cease between each addition. The contents of the vessel were allowed to warm to room temperature and stirred for approximately 17 hours. The contents of the vessel were quenched by the addition of ice, concentrated under vacuum and extracted with ethyl acetate. The organic layer was separated, dried over anhydrous magnesium sulfate, filtered and concentrated to give 4,7-dimethylindan-1-ol, observed to be a tan solid (7.56 g, 93.3%).
[0106] 4,7-Dimethylindan-1-ol (8.56 g, 52.8 mmol), toluene (800 mL), and p-toluenesulfonic acid (p-TSA) (0.188 g, 0.99 mmol) were added to a 1000 mL two-neck round-bottom vessel equipped with a magnetic stir bar and a reflux condenser fitted with a nitrogen inlet. The contents of the vessel were heated at 45° C. and the progress of the reaction was monitored by GC / MS. After 4 hours, molecular sieves were added to the vessel and heating was continued. After 6 hours, the reaction was quenched with saturated sodium bicarbonate solution. The organic layer was separated, dried over anhydrous magnesium sulfate, filtered, and concentrated to give the crude product, which was observed to be a pale yellow liquid. Purification by column chromatography (SiO2, hexane) gave 4,7-dimethyl-1H-indene, which was observed to be a colorless liquid (5.68 g, 74.7%).
[0107] Method B
[0108] A solution of sodium methoxide in methanol (5M, 170.5 mL, 852.5 mmol) was placed in a three-necked round-bottom vessel and the contents of the vessel were cooled to 0° C. Freshly cracked and distilled cyclopentadiene (34.3 mL, 511.5 mmol) was added to the vessel over 20 minutes. The contents of the vessel were stirred at a temperature of 0° C. under a nitrogen atmosphere for approximately 2 hours. 2,5-hexanedione (40 mL, 340.9 mmol) was added using an addition funnel over 30 minutes. The contents of the vessel were stirred at ambient temperature for approximately 12 hours. The volatiles were removed in vacuo and water (150 mL) and ether (250 mL) were added. The organic and aqueous layers were separated and the aqueous layer was extracted twice with diethyl ether (50 mL). The organic layer was washed with saturated sodium chloride, dried over magnesium sulfate and the solvent was removed in vacuo. Purification by distillation (bp 65° C., 0.01 mmHg) afforded 4,7-dimethyl-1H-indene, which was observed to be a pale yellow oil (35 g, 71% yield). Further synthetic steps discussed herein can be carried out using 4,7-dimethyl-1H-indene obtained via either Method A or Method B.
[0109] Comparative Example A, cyclopentadienyl(4,7-dimethylindenyl)zirconium dimethyl, was prepared as follows.
[0110] 4,7-Dimethyl-1H-indene (5.60 g, 39.4 mmol) was dissolved in hexane (100 mL) in a 200 mL glass vessel equipped with a stir bar. A solution of n-butyllithium in hexane (2.5 M, 17 mL, 43 mmol) was slowly added to the vessel at room temperature. The contents of the vessel were stirred at room temperature for approximately 17 hours, and the resulting white precipitate was collected by vacuum filtration, washed with hexane, and dried under vacuum to give 4,7-dimethylindenyllithium (5.27 g, 90.4%), which was determined to be an off-white solid.
[0111] 4,7-Dimethylindenyllithium (2.33 g, 15.5 mmol) in diethyl ether (100 mL) was added to a glass vessel (110 mL) equipped with a stir bar. CpZrCl3·DME (5.50 g, 15.6 mmol) and diethyl ether (20 mL) were added to the vessel, and the formation of a light yellow solution and a precipitate was observed immediately. The contents of the vessel were stirred for approximately 17 hours, then diluted with dichloromethane (80 mL) and filtered. The filtrate was concentrated under vacuum to give cyclopentadienyl(4,7-dimethylindenyl)zirconium dichloride, observed to be a light yellow solid (3.72 g, 65.1%).
[0112] Comparative Example B, methylcyclopentadienyl(4,7-dimethylindenyl)zirconium dimethyl, was prepared as follows.
[0113] 4,7-Dimethylindenyllithium was prepared as previously described. 4,7-Dimethylindenyllithium (0.800 g, 5.33 mmol) in diethyl ether (100 mL) was added to a glass vessel (200 mL) equipped with a stir bar. MeCpZrCl3·DME (1.95 g, 5.34 mmol) was added to the vessel, and the formation of a light yellow solution and a precipitate was observed immediately. The contents of the vessel were stirred for approximately 17 hours, then diluted with dichloromethane (20 mL) and filtered. The filtrate was concentrated under vacuum, and the resulting yellow solid was suspended in hexane (100 mL) and collected by vacuum filtration. The crude residue was recrystallized first from diethyl ether (20 mL) and dichloromethane (10 mL), then from toluene (40 mL) and hexane (10 mL). The crystals were collected and dried under vacuum to give methylcyclopentadienyl(4,7-dimethylindenyl)zirconium dichloride, observed as a light yellow solid (0.471 g, 23.1%).
[0114] Example 1-CAT, a polymerization catalyst, was prepared as follows: Treated fumed silica (Cabosil TS-610, 1.33 grams) was slurried in toluene (38 grams), followed by the addition of a 10 wt. % solution of methylaluminoxane (MAO) in toluene (11 g). Example 1 (0.42 grams) was then added, and the mixture was stirred for about 45 minutes before being introduced into the atomizer. The atomizer produced droplets that were then contacted with a hot nitrogen gas stream to evaporate the liquid and form a powder. The powder was separated from the gas mixture in a cyclone separator and discharged into a vessel. The spray dryer temperature was set at 140° C., and the outlet temperature was set at 75° C. Example 1-CAT was recovered as a fine powder. The loading was maintained at a constant 50 μmol / g, corresponding to an Al:Zr ratio of about 100.
[0115] Example 2-CAT is a polymerization catalyst and was prepared similarly to Example 1-CAT, with the change that Example 2 was used instead of Example 1.
[0116] Example 3-CAT is a polymerization catalyst and was prepared similarly to Example 1-CAT, with the change that Example 3 was used instead of Example 1.
[0117] Example 4-CAT was prepared similarly to Example 1-CAT, with the change that Example 4 was used instead of Example 1.
[0118] Comparative Example A-CAT was prepared similarly to Example 1-CAT, with the difference that Example A was used instead of Example 1.
[0119] Comp. B-CAT was prepared as Ex. 1-CAT, except that Comp. B was used instead of Ex. 1.
[0120] Polymerizations using Comparative Example B-CAT were carried out using a gas-phase pilot reactor operating at 105°C, C6 / C2 ratio of 0.0050, H2 / C2 ratio of 0.0020, 9 mole percent isopentane and 220 psi ethylene partial pressure. Several polymer properties were then determined, such as melt index (I2) determined according to ASTM D1238-13 (190°C, 2.16 kg loading), catalyst activity (grams of polymer / grams of catalyst / hour) determined as the ratio of polymer yield to the amount of catalyst added to the reactor, melting temperature (Tm) determined by differential scanning calorimetry according to ASTM D 3418-08, density according to ASTM D 792-13, and Mn, Mw, Mz and Mw / Mn determined by gel permeation chromatography (GPC). The results are reported in Table 1.
[0121] Based on the Comparative Example B-CAT polymerization, Ex. 1-CAT, Ex. 2-CAT and Comparative Example A-CAT were expected to have the melt index, catalyst activity, melting temperature, density, Mn, Mw, Mz and Mw / Mn as reported in Table 1. [Table 1]
[0122] The data in Table 1 show that the polymers formed using Ex. 1-CAT and Ex. 2-CAT, respectively, are expected to have surprising and improved, i.e., reduced, melt index (I2) compared to the polymers formed using Comp. A-CAT and Comp. B-CAT, respectively.
[0123] The data in Table 1 also show that the polymers formed using each of Ex. 1-CAT and Ex. 2-CAT are expected to have surprising and improved, i.e., elevated, melting temperatures compared to the polymers formed using each of Comparative Examples A-CAT and Comparative Example B-CAT.
[0124] The data in Table 1 also show that the polymers formed using each of Ex. 1-CAT and Ex. 2-CAT are expected to have surprising and improved, i.e., increased, molecular weights (Mn, Mw, and / or Mz) compared to the polymers formed using each of Comparative Examples A-CAT and Comparative Example B-CAT.
[0125] The data in Table 1 also show that the polymers formed using each of Ex. 1-CAT and Ex. 2-CAT are expected to have surprising and improved, i.e., increased, density compared to the polymers formed using each of Comparative Examples A-CAT and B-CAT.
[0126] 1,4-Dimethylindenyllithium was synthesized as follows: A solution of 4-methyl-1-indanone (5.00 g, 34.2 mmol) in THF (20 mL) was added to a vessel containing a solution of methylmagnesium bromide (3.0 M in ether, 22.8 mL, 68 mmol) in THF (50 mL) at a temperature of approximately 0° C. over a period of 15 minutes. The contents of the vessel were stirred at room temperature for 3 hours, then cooled in a dry ice / acetone bath and 15% HCl (100 mL) was added slowly in a fume hood under a nitrogen purge. The contents of the vessel were stirred while warming to room temperature. Ether (40 mL) was added and the organic layer was separated. The aqueous fraction was extracted with ether (3×40 mL) and the combined organic fractions were washed with saturated sodium bicarbonate, water, and brine, then dried over magnesium sulfate. After filtration and evaporation of volatiles from the filtrate, the crude dimethylindene was dissolved in hexane (~60 mL), passed through silica gel, and treated with BuLi (21 mL, 33.6 mmol). After stirring for ~12 h, 1,4-dimethylindenyllithium was collected by filtration, washed with hexane, and dried in vacuum. Yield = 4.441 g (86.5%) of a white solid. 1H NMR(400MHz,THF-d8)δ7.14(dq,J=8.1,0.8Hz,1H),6.42(dd,J=8.1,6.5Hz,1H),6.30(dd,J=3.1,0.7Hz,1 H),6.28(dp,J=6.5,0.9Hz,1H),5.73(dd,J=3.2,0.8Hz,1H),2.41(d,J=0.6Hz,3H),2.40(d,J=0.7Hz,4H).
[0127] 1,6-Dimethylindenyllithium was synthesized as follows: 6-Methyl-1-indanone (3.00 g, 20.52 mmol) was dissolved in toluene (20 mL) under nitrogen atmosphere and cooled to about -35°C. Trimethylaluminum (2.0 M in toluene, 21.6 mL, 43.1 mmol) was added and the resulting mixture was stirred overnight, then diluted with ether (100 mL), cooled in an ice bath, and quenched by adding 6 M HCl (30 mL) under a stream of nitrogen. The resulting biphasic mixture was stirred for about 2 hours to convert to dimethylindene. The organic layer was separated, washed with water (2 x 40 mL), saturated sodium bicarbonate (40 mL), and brine (40 mL), dried over magnesium sulfate, and filtered. The resulting mixture was concentrated on a rotary evaporator at 100 Torr for about 1 hour, then placed in a glove box, diluted with hexane (80 mL), and filtered through silica. n-Butyllithium (1.6 M in hexanes, 12.8 mL, 20.5 mmol) was added and the mixture was stirred for about 3 days. The white precipitate was collected by filtration, washed thoroughly with hexanes (3×20 mL), and dried in vacuum to give 1,6-dimethylindenyllithium (2.561 g). 1 H NMR(400MHz,THF-d8)δ7.16(dd,J=8.1,0.7Hz,1H),7.03(dq,J=1.8,0.9Hz,1H),6.30(dd,J=8.1,1. 7Hz,1H),6.26(d,J=3.2,1H),5.65(dd,J=3.2,0.8Hz,1H),2.40-2.37(m,3H),2.32(d,J=0.9Hz,3H).
[0128] 1,7-Dimethylindenyllithium was synthesized as follows: The synthesis described for 1,6-dimethylindenyllithium was repeated except that 7-methyl-1-indanone (4.795 g, 32.80 mmol) was used. The yield of 1,7-dimethylindenyllithium was 4.152 g (84.31%). 1 H NMR(400MHz,THF-d8)δ7.07(d,J=8.1Hz,1H),6.28(dd,J=8.1,6.5Hz,1H),6.24-6.18(m,1H),6 .12(dp,J=6.5,1.0Hz,1H),5.66(d,J=3.1Hz,1H),2.68(d,J=0.7Hz,3H),2.66(t,J=0.7Hz,3H).
[0129] 1,5,7-Trimethylindenyllithium was synthesized as follows: The synthesis described for 1,6-dimethylindenyllithium was repeated except that 5,7-dimethyl-1-indanone (5.00 g, 31.2 mmol) was used and ether (ca. 1 mL) was added to the reaction mixture after the n-BuLi addition step. 1,5,7-Trimethylindenyllithium was obtained as a white solid. Yield=4,133 g (80.7%). 1 H NMR(400MHz,THF-d8)δ6.84(s,1H),6.14(d,J=3.0Hz,1H),6.00(s,1H),5.56(d,J=3.1Hz,1H),2.66-2.64(m,3H),2.62(s,3H),2.21(d,J=0.8Hz,3H).
[0130] 1-Ethyl-5-methyl-indenyllithium was synthesized as follows: The synthesis of 1,4-dimethyl-indenyllithium was repeated except that 5-methyl-1-indanone (5.00 g, 34.2 mmol) and ethylmagnesium bromide (3.0 M in ether, 22.8 mL, 68 mmol) were used. 1-Ethyl-5-methyl-indenyllithium was obtained as a pale orange solid (Yield=4.192 g). 1H NMR(400MHz,THF-d8)δ7.22(dt,J=8.1,0.9Hz,1H),7.04(dq,J=1.8,0.9Hz,1H),6.33-6.29(m,2H),5 .62(dd,J=3.1,0.8Hz,1H),2.84(qd,J=7.5,0.6Hz,2H),2.29(d,J=0.9Hz,4H),1.26(t,J=7.5Hz,3H).
[0131] Example 5, cyclopentadienyl(1,4-dimethylindenyl)zirconium dichloride, was synthesized as follows: In a glove box, 1,4-dimethylindenyl lithium (0.500 g, 3.33 mmol) was dissolved in dimethoxyethane (30 mL) and added to the vessel. Cyclopentadienyl zirconium trichloride (0.875 g, 3.33 mmol) was added to the vessel as a solid in portions. The vessel contents were stirred for approximately 48 hours. The solvent was then removed in vacuo and the residue was taken up in toluene (80 mL), filtered through Celite, and washed with additional toluene (2X10 mL). The solvent was removed from the filtrate in vacuo and the residue was recrystallized from a dichloromethane solution (approximately 7 mL) by overlaying with hexane (approximately 20 mL). The product was isolated by decantation, rinsing with hexane, and drying under vacuum to give a light yellow solid. Yield=0.686 g (65.3%). 1 H NMR (400MHz, benzene-d6) δ7.28(dq,J=8.5,0.8Hz,1H),6.92(dd,J=8.6,6.7Hz,1H),6.73(dp,J =6.7,1.1Hz,1H),6.09-5.97(m,1H),5.83(dd,J=3.2,0.9Hz,1H),5.78(s,5H),2.21(s,6H).
[0132] Example 6, cyclopentadienyl(1,6-dimethylindenyl)zirconium dichloride, was synthesized as follows: Cyclopentadienyl zirconium trichloride (0.875 g, 3.33 mmol) was dissolved in dimethoxyethane (40 mL) and added to the vessel. 1,6-dimethylindenyl lithium (0.500 g, 3.33 mmol) was added to the vessel as a solid in portions. The contents of the vessel were stirred for approximately 48 hours. The solvent was then removed in vacuum and the residue was taken up in a mixture of dichloromethane (40 mL) and hexanes (30 mL) and filtered. The volume of the filtrate was reduced in vacuum to 55 mL and kept in a freezer. The product crystallized at low temperature and was collected as a yellow solid by filtration, washed with hexanes (3X5 mL) and dried under vacuum. Yield=0.681 g (55.2%). 1 H NMR (400MHz, benzene-d6) δ7.24(tq,J=2.1,1.0Hz,1H),7.03(dt,J=8.5,0.6Hz,1H),6.72(dd,J=8.6,1.5Hz,1H),6. 21(dd,J=3.2,0.7Hz,1H),5.77(s,5H),5.75(dd,J=3.2,0.9Hz,1H),2.37(d,J=0.6Hz,3H),2.11(d,J=1.1Hz,3H).
[0133] Example 7, cyclopentadienyl(1,7-dimethylindenyl)zirconium dichloride, was synthesized as follows: Cyclopentadienyl zirconium trichloride (0.875 g, 3.33 mmol) was dissolved in dimethoxyethane (40 mL) and added to the vessel. 1,7-dimethylindenyl lithium (0.500 g, 3.33 mmol) was added to the vessel in portions as a solid. The contents of the vessel were stirred for approximately 4 hours. The solvent was then removed in vacuum and the residue was taken up in toluene (50 mL) and filtered. The solvent was removed in vacuum and the product was recrystallized from a mixture of toluene (approximately 40 mL) and hexane (approximately 10 mL) by dissolving at 55° C. and cooling to −35° C. to give the product as a light yellow solid (0.844 g (68.4%)). 1H NMR (400MHz, benzene-d6) δ6.95-6.89(m,1H),6.73(dd,J=8.5,6.8Hz,1H),6.60(dp,J=6.8,1.1Hz,1H),6.17 (dd,J=3.2,0.7Hz,1H),5.77(s,5H),5.63(d,J=3.2Hz,1H),2.55(d,J=0.6Hz,3H),2.52(d,J=1.0Hz,3H).
[0134] Example 8, cyclopentadienyl(1,5,7-trimethylindenyl)zirconium dichloride, was synthesized as follows: 1,5,7-trimethylindenyl lithium (0.150 g, 0.914 mmol) was dissolved in dimethoxyethane (20 mL) and added to the vessel. Cyclopentadienyl zirconium trichloride (0.240 g, 0.914 mmol) was added to the vessel as a solid in portions. The vessel contents were stirred for approximately 12 hours. The solvent was then removed in vacuum and the residue was taken up in toluene (approximately 60 mL) and filtered. The volume of the filtrate was reduced in vacuum to 30 mL, heated to 50° C. to dissolve, filtered again to remove traces of white solid, and recrystallized at low temperature from a solvent mixture of toluene (15 mL) and hexane (7 mL) to give the product as a light yellow solid. Yield=0.097 g (27.7%). 1 H NMR (400 MHz, chloroform-d) δ 7.19 (s, 1H), 6.79 (t, J = 1.3 Hz, 1H), 6.47 (d, J = 3.2 Hz, 1H), 6.20 (d, J = 3.2 Hz, 1H), 6.17 (s, 5H), 2.70 (d, J = 0.5 Hz, 3H), 2.66 (t, J = 0.8 Hz, 3H), 2.40 (d, J = 1.0 Hz, 3H).
[0135] Example 9, cyclopentadienyl(1-ethyl-5-methylindenyl)zirconium dichloride, was synthesized as follows: 1-Ethyl-5-methylindenyl lithium (0.600 g, 3.33 mmol) was dissolved in dimethoxyethane (30 mL) and added to the vessel. Cyclopentadienyl zirconium trichloride (0.960 g, 3.33 mmol) was added portionwise as a solid to the vessel. The vessel contents were stirred for approximately 12 hours. The solvent was then removed in vacuo and the residue was taken up in dichloromethane (30 mL), filtered through Celite, and washed with additional dichloromethane (3X10 mL). The volume of the filtrate was reduced in vacuo to 20 mL, hexane (10 mL) was added, and the product was crystallized at low temperature, collected by filtration, washed with hexane (2X10 mL), and dried under vacuum to give 0.761 g. 1 H NMR (400 MHz, chloroform-d) δ 7.53 (d, J = 8.7 Hz, 1H), 7.39 (m, 1H), 7.11 (dd, J = 8.7, 1.5 Hz, 1H), 6.62 (d, J = 3.2 Hz, 1H), 6.32 (dd, J = 3.2, 0.8 Hz, 1H), 6.13 (s, 5H), 3.11-2.79 (m, 2H), 2.47 (d, J = 1.2 Hz, 3H), 1.28 (t, J = 7.5 Hz, 4H).
[0136] Example 10, methylcyclopentadienyl(1,4-dimethylindenyl)zirconium dichloride, was synthesized as follows: 1,4-dimethylindenyl lithium (0.500 g, 3.33 mmol) was dissolved in dimethoxyethane (30 mL) and added to the vessel. Methylcyclopentadienyl zirconium trichloride (0.921 g, 3.33 mmol) was added to the vessel in portions as a solid. The vessel contents were stirred for approximately 12 hours. The solvent was then removed in vacuo and the residue was taken up in toluene (50 mL), filtered at room temperature, and washed with more toluene (2X15 mL). The product was crystallized at low temperature from a solvent mixture of toluene (20 mL) and hexane (20 mL), collected by filtration, and washed with hexane to give 1.027 g of product at approximately 94% purity (by NMR). For further purification, it was dissolved in dichloromethane (10 mL) and hexane (25 mL) was carefully added as the top layer. After about 12 hours, the precipitated crystalline product was collected by decantation, washed with hexane, and dried in vacuum to give 0.569 g (44.4%) of product. 1 H NMR (400MHz, chloroform-d) δ7.49(dq,J=8.6,0.8Hz,1H),7.22(dd,J=8.6,6.7Hz,1H) ,7.05(dp,J=6.7,1.0Hz,1H),6.62(d,J=3.3Hz,1H),6.38(dd,J=3.2,0.9Hz,1H),6 .00(q,J=2.6Hz,1H),5.97(q,J=3.8,3.2Hz,1H),5.94(td,J=3.1,2.4Hz,1H),5.87 (td,J=3.1,2.3Hz,1H),2.46(d,J=1.0Hz,3H),2.46(d,J=0.6Hz,3H),2.18(s,3H).
[0137] Example 11, methylcyclopentadienyl(1,6-dimethylindenyl)zirconium dichloride, was synthesized as follows: Methylcyclopentadienyl zirconium trichloride (0.921 g, 3.33 mmol) was dissolved in dimethoxyethane (30 mL) and added to the vessel. 1,6-dimethylindenyl lithium (0.500 g, 3.33 mmol) was added to the vessel as a solid in portions. The vessel contents were stirred for approximately 1.5 hours, then filtered to remove some salts, and the solvent was removed from the filtrate in vacuum. The residue was taken up in hexanes (35 mL) and dichloromethane (30 mL), warmed to 40° C., and filtered again. The clear filtrate was concentrated to 45 mL and kept in the freezer to produce a yellow crystalline solid, which was collected by filtration, washed with hexanes (3×5 mL), and dried under vacuum. Yield=0.646 g (50.5%). 1 H NMR (400MHz, benzene-d6) δ7.24(tt,J=2.0,1.0Hz,1H),7.09(dd,J=8.7,0.9Hz,1H),6.74(dd ,J=8.7,1.6Hz,1H),6.26(dd,J=3.3,0.7Hz,1H),5.81(dd,J=3.2,0.9Hz,1H),5.75(dtd,J= 2.9,2.3,0.6Hz,1H),5.59(dtd,J=2.9,2.3,0.6Hz,1H),5.51(td,J=3.1,2.3Hz,1H),5.40( td,J=3.1,2.3Hz,1H),2.38(d,J=0.6Hz,3H),2.11(d,J=1.0Hz,3H),2.02(d,J=0.6Hz,3H).
[0138] Example 12, methylcyclopentadienyl(1,7-dimethylindenyl)zirconium dichloride, was synthesized as follows: Methylcyclopentadienyl zirconium trichloride (0.921 g, 3.33 mmol) was dissolved in dimethoxyethane (40 mL) and added to the vessel. 1,7-dimethylindenyl lithium (0.500 g, 3.33 mmol) was added to the vessel in portions as a solid. The contents of the vessel were stirred for about 16 hours. The solvent was then removed in vacuum and the residue was taken up in toluene (60 mL), warmed to about 60° C., and filtered. The solvent was removed from the filtrate in vacuum to give the product as a yellow solid (1.250 g). The product was recrystallized at low temperature from a solvent mixture of toluene (45 mL) and hexane (12 mL). Yield=0.985 g (77.0%). 1 H NMR (400MHz, chloroform-d) δ7.43(dp,J=8.5,0.8Hz,1H),7.11(dd,J=8.5,6.8Hz,1H) ,6.92(dp,J=6.8,1.1Hz,1H),6.53(dd,J=3.2,0.7Hz,1H),6.28(d,J=3.2Hz,1H), 6.12-6.07(m,1H),5.96(td,J=3.1,2.3Hz,1H),5.87-5.82(m,1H),5.80(td,J=3. 1,2.3Hz,1H),2.74(d,J=0.6Hz,3H),2.70(d,J=0.9Hz,3H),2.17(d,J=0.6Hz,3H).
[0139] Example 13, methylcyclopentadienyl(1,5,7-trimethylindenyl)zirconium dichloride, was synthesized as follows: Methylcyclopentadienyl zirconium trichloride (0.914 g, 3.30 mmol) was dissolved in dimethoxyethane (20 mL) and added to the vessel. 1,5,7-trimethylindenyl lithium (0.543 g, 3.30 mmol) was added to the vessel as a solid in portions. The vessel contents were stirred for approximately 12 hours. The solvent was then removed in vacuum and the residue was taken up in dichloromethane (20 mL) at 35° C. and filtered. The solvent was removed from the filtrate in vacuum to give the product (1.377 g). The product was recrystallized at low temperature from a mixture of dichloromethane (25 mL) and hexane (25 mL) to give a light yellow solid. The yield was 0.793 g (60.2%). 1 H NMR (400MHz, chloroform-d) δ7.18(td,J=1.7,0.8Hz,1H),6.77(q,J=1.3Hz,1H),6. 46(dd,J=3.1,0.7Hz,1H),6.16(d,J=3.1Hz,1H),6.11-6.06(m,1H),5.96(td,J =3.1,2.3Hz,1H),5.85(qd,J=2.6,1.4Hz,1H),5.77(td,J=3.1,2.3Hz,1H),2.7 0(d,J=0.6Hz,3H),2.66(t,J=0.9Hz,3H),2.39(d,J=1.1Hz,3H),2.16(d,J=0.6 z,3H).
[0140] Example 14, Propylcyclopentadienyl(1,5-dimethylindenyl)zirconium dichloride, was synthesized as follows: Propylcyclopentadienyl zirconium trichloride, DME adduct (1.315 g, 3.33 mmol) was dissolved in dimethoxyethane (40 mL) and added to the vessel. 1,5,7-trimethylindenyl lithium (0.500 g, 3.33 mmol) was added portionwise as a solid to the vessel. The vessel contents were stirred for approximately 7 hours. The solvent was then removed in vacuum and the residue was taken up in toluene (50 mL) and filtered. The volume of the filtrate was reduced to 25 mL, hexane (25 mL) was added and the product recrystallized at low temperature as a yellow solid which was collected by filtration, washed with hexane (3X5 mL) and dried in vacuum. Yield=0.893 g (65.0%). 1 H NMR (400MHz, benzene-d6) δ 7.35 (dd, J = 8.7, 1.0Hz, 1H), 6.96 (h, J = 1.0Hz, 1H), 6.77 (dd, J = 8.8, 1.5Hz, 1H), 6.27 (dd, J = 3.1, 0.7Hz, 1H), 5.85 (dt, J = 3.0, 2.3Hz, 1H), 5.81 (dd, J = 3.1, 0.9Hz, 1H), 5.68 ( dt,J=3.0,2.3Hz,1H),5.57(td,J=3.1,2.3Hz,1H),5.46(td,J=3.1,2.3Hz,1H),2.47(td,J=7.5,3 .6Hz,2H),2.39(d,J=0.6Hz,3H),2.11(d,J=1.2Hz,3H),1.43-1.30(m,2H),0.75(t,J=7.4Hz,3H).
[0141] Example 15, Propylcyclopentadienyl(1,6-dimethylindenyl)zirconium dichloride, was synthesized as follows: Propylcyclopentadienyl zirconium trichloride, DME adduct (1.315 g, 3.33 mmol) was dissolved in dimethoxyethane (40 mL) and added to the vessel. 1,6-Dimethylindenyl lithium (0.500 g, 3.33 mmol) was added to the vessel as a solid in portions. The vessel contents were stirred for approximately 12 hours. The solvent was then removed in vacuum and the residue was taken up in toluene (50 mL) and filtered. The toluene was removed from the filtrate in vacuum to give 1.310 g of product, which was recrystallized at low temperature from a solvent mixture of dichloromethane (15 mL) and hexane (30 mL) as a yellow solid, which was collected by filtration, washed with hexane (3X5 mL) and dried under vacuum. Yield=0.6621 g (48.2%). 1 H NMR (400MHz, benzene-d6) δ7.26(tt,J=2.0,1.0Hz,1H),7.09(dd,J=8.6,0.9Hz,1H),6.75(dd ,J=8.7,1.5Hz,1H),6.27(dd,J=3.2,0.7Hz,1H),5.83(td,J=3.0,0.8Hz,2H),5.66(dt,J= 3.0,2.3Hz,1H),5.54(td,J=3.1,2.3Hz,1H),5.46(td,J=3.1,2.3Hz,1H),2.53-2.44(m,2 H),2.39(d,J=0.6Hz,3H),2.11(d,J=1.1Hz,3H),1.43-1.30(m,2H),0.75(t,J=7.3Hz,3H).
[0142] Example 16, propylcyclopentadienyl(1,7-dimethylindenyl)zirconium dichloride, was synthesized as follows: Propylcyclopentadienyl zirconium trichloride, DME adduct (1.315 g, 3.33 mmol) was dissolved in dimethoxyethane (40 mL) and added to the vessel. 1,7-dimethylindenyl lithium (0.500 g, 3.33 mmol) was added to the vessel as a solid in portions. The vessel contents were stirred for approximately 16 hours. The solvent was then removed in vacuo and the residue was taken up in toluene (50 mL) and filtered. The solvent was removed from the filtrate in vacuo to give the product as a high purity yellow solid. Yield=1.316 g (95.8%). 1 H NMR (400MHz, benzene-d6) δ 6.99 (dp, J = 8.5, 0.8Hz, 1H), 6.77 (dd, J = 8.5, 6.8Hz, 1H), 6.61 (dp, J = 6.8, 1.1Hz, 1H), 6.24 (dd, J = 3.2, 0.7Hz, 1H), 5.87 (dt, J = 3.0, 2.3Hz, 1H), 5.70 (d, J = 3.2Hz, 1H), 5.65 (dt, J =2.9,2.3Hz,1H),5.57(td,J=3.1,2.3Hz,1H),5.43(td,J=3.1,2.3Hz,1H),2.58(d,J=0.6Hz,3H),2. 54(t,J=1.0Hz,3H),2.49(td,J=7.5,3.3Hz,2H),1.37(dt,J=7.9,7.3Hz,2H),0.75(t,J=7.3Hz,3H).
[0143] Example 17, Propylcyclopentadienyl(1,5,7-trimethylindenyl)zirconium dichloride, was synthesized as follows: Propylcyclopentadienyl zirconium trichloride, DME adduct (1.203 g, 3.05 mmol) was dissolved in dimethoxyethane (40 mL) and added to the vessel. 1,5,7-trimethylindenyl lithium (0.500 g, 3.05 mmol) was added portionwise as a solid to the vessel. The vessel contents were stirred for approximately 48 hours. The solvent was then removed in vacuum and the residue was taken up in toluene (60 mL) and filtered. The volume of the filtrate was reduced in vacuum to 25 mL, hexane (25 mL) was added, and the product was crystallized at low temperature. The product was collected by filtration, washed with hexane (3X5 mL), and then dried under vacuum. Yield=0.895 g (68.9%). 1 H NMR (400 MHz, chloroform-d) δ 7.21-7.15 (m, 1H), 6.77 (t, J = 1.3 Hz, 1H), 6.45 (dd, J = 3.2, 0.7 Hz, 1H), 6.16 (d, J = 3.2 Hz, 1H), 6.13-6.08 (m, 1H), 5.94 (td, J = 3.1, 2.3 Hz, 1H), 5.90-5.85 ( m,1H),5.81(td,J=3.1,2.3Hz,1H),2.70(d,J=0.6Hz,3H),2.65(t,J=0.9Hz,3H),2.48(t d,J=7.5,5.5Hz,2H),2.39(d,J=1.1Hz,3H),1.51(q,J=7.5Hz,2H),0.89(t,J=7.3Hz,3H).
[0144] It is expected that the polymers formed using the polymerization catalysts produced from each of Examples 5-17, respectively, may have surprising and improved, i.e., reduced, melt index (I2) compared to the polymers formed using each of Comparative Examples A-CAT and B-CAT.
[0145] It is expected that the polymers formed using the polymerization catalysts produced from each of Examples 5-17, respectively, may have surprising and improved, i.e., elevated, melting temperatures as compared to the polymers formed using each of Comparative Examples A-CAT and B-CAT.
[0146] It is expected that the polymers formed using the polymerization catalysts produced respectively from each of Examples 5-17 may have surprising and improved, i.e., increased, molecular weights (Mn, Mw, and / or Mz) as compared to the polymers formed using each of Comparative Examples A-CAT and Comparative Example B-CAT.
[0147] It is expected that the polymers formed using the polymerization catalysts produced from each of Examples 5-17, respectively, may have surprising and improved, i.e., increased, density compared to the polymers formed using each of Comparative Examples A-CAT and B-CAT.
Claims
1. A metal-ligand complex of formula I, 【Chemistry 1】 In the formula, M is titanium, zirconium or hafnium, and R is hydrogen or (C 1 ~C 4 ) alkyl, R 1 (C 1 ~C 4 ) alkyl, R 2 , R 3 , R 4 , R 5 Any one or two of are independently (C 1 -C 3 ) alkyl; R 2 , R 3 , R 4 , R 5 three or two of are H, and each X is independently a halide, (C 1 ~C 20 ) alkyl, (C 7 ~C 20 ) aralkyl, (C 1 ~C 6 ) Alkyl-substituted (C 6 ~C 12 ) aryl, (C 1 ~C 6 ) Alkyl-substituted benzyl, or silicon-containing alkyl metal-ligand complexes.
2. A metal-ligand complex represented by formula II, 【Chemistry 2】 In the formula, M is titanium, zirconium or hafnium, and R is hydrogen or (C 1 ~C 2 ) alkyl, and each X is independently a halide, (C 1 ~C 20 ) alkyl, (C 7 ~C 20 ) aralkyl, (C 1 ~C 6 ) Alkyl-substituted (C 6 ~C 12 ) aryl, (C 1 ~C 6 ) Alkyl-substituted benzyl, or silicon-containing alkyl metal-ligand complexes.
3. 3. The metal-ligand complex of claim 1 or claim 2, wherein R is hydrogen, methyl, or ethyl, and M is Zr.
4. Each X is independently Cl, (C 1 ~C 3 4. The metal-ligand complex of claim 1, wherein R is 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30
5. below, A metal-ligand complex of formula I, wherein R is hydrogen, M is zirconium, and each X is Cl; A metal-ligand complex of formula I, wherein R is methyl, M is zirconium, and each X is Cl; A metal-ligand complex of formula I, wherein R is ethyl, M is zirconium, and each X is Cl; A metal-ligand complex of formula I, wherein R is hydrogen, M is zirconium, and each X is methyl; A metal-ligand complex of formula I, wherein R is methyl, M is zirconium, and each X is methyl; and 3. The metal-ligand complex of claim 1 or claim 2, selected from a metal-ligand complex of formula I, wherein R is ethyl, M is zirconium, and each X is methyl.
6. A bimodal catalyst system comprising a metal-ligand complex according to any one of claims 1 to 5 and a bis(2-(pentamethylphenylamido)ethyl)-amine zirconium complex of formula III, 【Chemistry 3】 In the formula, M is Zr, and each R 1 are independently Cl, Br, (C 1 ~C 20 ) alkyl, (C 1 ~C 6 ) Alkyl-substituted (C 6 ~C 12 ) aryl, benzyl, or (C 1 ~C 6 ) alkyl substituted benzyl, a bimodal catalyst system.
7. 13. A method of making a polymerization catalyst, the method comprising contacting a metal-ligand complex of any one of claims 1 to 5 or a bimodal catalyst system of claim 6 with an activating agent under activating conditions to activate the metal-ligand complex or the bimodal catalyst system, thereby making a polymerization catalyst.
8. The method of claim 7, wherein the activator is methylaluminoxane.
9. 1. A method of making a polyolefin polymer, the method comprising:
9. A process comprising contacting an olefin with a polymerization catalyst made by the process of claim 7 or 8 under polymerization conditions to polymerize the olefin to produce a polyolefin polymer.
Citation Information
Patent Citations
Polymerization catalyst and method for producing a two-mode polymer in a single reaction vessel.
JP2009508980A
Producing polyolefin products
WO2016168700A1
Polymerization catalysts
WO2018064038A1