Method for producing heterophasic binder pitch and heterophasic binder pitch produced therefrom
The method of producing heterophase binder pitch by hydrotreating, polymerizing, and solvent extracting medium oil components addresses the low density and strength of graphite blocks, achieving higher carbonization yield and density in graphite blocks with improved physical properties.
Patent Information
- Application Number
- JP2022107030
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-07-01
- Filing Date
- 2022-07-01
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2042-07-01
AI Technical Summary
Existing binder pitches produced from petroleum medium oil result in graphite blocks with low density and low strength due to low carbonization yield, posing a significant challenge in the production of high-quality graphite molded bodies.
A method involving hydrotreating medium oil to obtain a hydrogenation feedstock, thermally polymerizing, thin film distillation to enrich mesogenic components, solvent extraction to separate mesogenic components, and mixing with basic isotropic pitch to create a heterophase binder pitch with anisotropic texture uniformly dispersed within an isotropic matrix.
The method produces a heterophase binder pitch with increased carbonization yield, resulting in graphite blocks with higher density and improved physical properties, offering economic benefits and wide application potential.
Smart Images

Figure 0007555374000001 
Figure 0007555374000002 
Figure 0007555374000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a heterophase binder pitch having a heterophase texture in which an anisotropic texture is uniformly dispersed in an isotropic matrix, and which does not significantly change the softening point and selectively increases only the carbonization yield, and to a heterophase binder pitch produced thereby. [Background technology]
[0002] Pitch is a residue resulting from the thermal decomposition of organic substances or tar distillation that is solid at room temperature. It consists of numerous highly directional hydrocarbon compounds and heterocyclic compounds and does not have a constant melting point but rather shows a wide softening range.
[0003] The pitch has the property that when it melts and cools, it solidifies without going through a crystallization step.
[0004] Binder pitch is a secondary material used together with the primary material, coke, in producing artificial graphite compacts such as isotropic graphite blocks and electrode rods.
[0005] Typically, a method for producing binder pitch involves heat treating medium oil in an inert atmosphere at a temperature of 300 to 500°C for a certain period of time to remove volatile components and induce a polycondensation reaction of the remaining components to produce a binder pitch having optical isotropy.
[0006] The biggest problem with the petroleum-based binder pitch produced by these production methods is the low density and low strength of the graphite block due to the low carbonization yield, which is known to be the most difficult problem to solve.
[0007] Through various studies, the applicant has developed a technology for producing binder pitch from medium petroleum oil, which has a heterophase structure in which anisotropic texture is uniformly dispersed in an isotropic matrix.
[0008] As a result, the applicant has produced a pitch whose softening point does not change significantly and whose carbonization yield only increases selectively. When the pitch is used as a binder pitch in the production of graphite molded bodies, the applicant has acquired a manufacturing process technology for the binder pitch, which significantly increases the density of the molded bodies, and has thus completed the present invention. [Prior art documents] [Patent documents]
[0009] Korean Patent Publication No. 1993-0005525 (Patent Publication Date: June 22, 1993) Summary of the Invention [Problem to be solved by the invention]
[0010] Therefore, an object of the present invention is to provide a method for producing a heterophase binder pitch that can solve the problem of low density / low strength of a graphite block due to a low carbonization yield of the binder pitch by producing a heterophase binder pitch with a high carbonization yield and, when a graphite block is produced using the heterophase binder pitch, can produce a molded product having a high density.
[0011] Another object of the present invention is to provide a heterophase binder pitch having a heterophase texture in which anisotropic texture is uniformly dispersed in an isotropic matrix, and which does not significantly change the softening point and selectively increases only the carbonization yield.
[0012] The problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0013] In order to solve the above problems, according to one aspect of the present invention, A method for producing a heterophase binder pitch having an anisotropic texture uniformly dispersed in an isotropic matrix, comprising: hydrotreating the middle oil to obtain a hydrotreated feed; thermally polymerizing the resulting hydrogenated feedstock to produce a primary pitch; thin-film distillation of the produced primary pitch to remove low boiling point components and obtain an anisotropic pitch enriched in mesogen components; A step of extracting the anisotropic pitch with a solvent, filtering and drying the anisotropic pitch to separate only the mesogen component in the anisotropic pitch; mixing the separated mesogenic component with a basic isotropic pitch.
[0014] According to one embodiment of the present invention, the basic isotropic pitch is Thermally polymerizing the medium oil under normal and elevated pressure to produce an isotropic pitch; and subjecting the isotropic pitch to thin film distillation.
[0015] According to one embodiment of the present invention, the hydrotreatment comprises: Reaction temperature of 350℃~500℃; A reaction time of 10 minutes to 10 hours; or The mixing ratio (weight ratio) of medium oil:organic solvent can be 1:0.5 to 1:4.
[0016] According to one embodiment of the present invention, the organic solvent may include a hydrogen donor solvent including tetralin or tetrahydroquinoline.
[0017] According to one embodiment of the present invention, the thermal polymerization is Reaction temperature of 400℃~500℃; A reaction time of 10 minutes to 10 hours; or The inert gas flow rate can be set to 100 mL / min / kg to 5000 mL / min / kg.
[0018] According to one embodiment of the present invention, the thin film distillation comprises: Processing temperature: 250℃~400℃; Processing time of 5 to 60 minutes, or It can be performed under pressure conditions of 1 hPa to 100 hPa.
[0019] According to one embodiment of the present invention, the anisotropic pitch obtained from the thin film distillation has Softening point 250℃~350℃; Anisotropic content 70% to 100%, or The production yield may be 15% to 25%.
[0020] According to one embodiment of the invention, the extraction of the solvent comprises: Anisotropic pitch:solvent mixing ratio (weight ratio) = 1:2 to 1:40; Extraction time: 5 minutes to 24 hours; or This can be done using the extraction solvent THF (tetrahydrofuran).
[0021] According to one embodiment of the present invention, the step of mixing the basic isotropic pitch and the mesogen comprises: Basic isotropic pitch:mesogen mixing ratio = 95:5~60:40; Mixing temperature 200℃~400℃; or The mixing time can be set to 5 minutes to 2 hours.
[0022] According to another aspect of the present invention, The present invention provides a heterophase binder pitch produced by the method for producing a heterophase binder pitch.
[0023] According to an embodiment of the present invention, the microstructure of the heterophase binder pitch may have a morphology in which anisotropic globules are uniformly dispersed in an isotropic matrix.
[0024] According to an embodiment of the present invention, the softening point of the heterophase binder pitch may be 50°C to 200°C.
[0025] According to an embodiment of the present invention, the anisotropic content of the heterophase binder pitch may be 0% to 30%.
[0026] According to an embodiment of the present invention, the carbonization yield of the hetero-phase binder pitch may be 25% to 50%. Effect of the Invention
[0027] According to the present invention, the problem of low density / low strength of graphite blocks due to low carbonization yield is solved by producing a heterophase binder pitch with a high carbonization yield, and when a graphite block is produced using the heterophase binder pitch, a method for producing a heterophase binder pitch capable of producing a molded body having a high density is provided, which has excellent process stability and low production cost, and is therefore economical.
[0028] In addition, the present invention provides a heterophase texture in which anisotropic texture is uniformly dispersed within an isotropic matrix, and the softening point does not change significantly, and the heterophase binder pitch selectively increases only the carbonization yield. This has the advantages of excellent physical properties and a wide range of applications.
[0029] It should be understood that the effects of the present invention are not limited to the above effects, but include all effects that can be inferred from the configuration of the invention described in the detailed description of the present invention or the claims. [Brief description of the drawings]
[0030] [Figure 1] 1 is a process flow diagram for a heterophase binder pitch according to one embodiment of the present invention. [Diagram 2] 1 is a polarized microscope image of FCC-DO basic isotropic pitch according to one embodiment of the present invention. [Diagram 3] 1 is a polarizing microscope image of FCC-DO pitch containing up to 20% anisotropic globules in an isotropic matrix according to one embodiment of the present invention. [Figure 4] 4 is a polarizing microscope image of FCC-DO pitch containing up to 20% anisotropic globules in an isotropic matrix according to another embodiment of the present invention. [Diagram 5] 1 is a polarized microscope image of hydrogenated FCC-D anisotropic pitch according to one embodiment of the present invention. [Figure 6] 3 is a polarizing microscope image of a binder pitch obtained by mixing an FCC-DO basic isotropic pitch according to an embodiment of the present invention with THFI, a mesogen component, in a weight ratio of 9:1. [Figure 7] 3 is a polarizing microscope image of a binder pitch obtained by mixing an FCC-DO basic isotropic pitch according to an embodiment of the present invention with THFI, a mesogen component, in a weight ratio of 8:2. [Figure 8] 3 is a polarizing microscope image of a binder pitch obtained by mixing an FCC-DO basic isotropic pitch according to an embodiment of the present invention with THFI, a mesogen component, in a weight ratio of 7:3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] In the following, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0032] The advantages and features of the present invention, as well as the manner in which it is achieved, will become apparent from the following detailed description of the embodiments taken in conjunction with the accompanying drawings.
[0033] However, the present invention is not limited to the embodiments disclosed below, and may be embodied in various different forms, but the embodiments are provided to fully disclose the present invention and fully inform those skilled in the art of the scope of the invention, and the present invention is defined only by the scope of the claims.
[0034] Furthermore, in describing the present invention, if it is determined that related publicly known techniques may obscure the gist of the present invention, detailed description thereof will be omitted.
[0035] The present invention will be described in detail below.
[0036] <Method for producing heterophase binder pitch> The present invention provides a method for producing a heterophase binder pitch with a high carbonization yield, which solves the problem of low density / low strength of a graphite block due to a low carbonization yield, and a method for producing a heterophase binder pitch that can produce a molded product having a high density when a graphite block is produced using the heterophase binder pitch.
[0037] The method for producing the heterophase binder pitch of the present invention comprises the steps of: A method for producing a heterophase binder pitch having an anisotropic texture uniformly dispersed in an isotropic matrix, comprising: hydrotreating the middle oil to obtain a hydrotreated feed; thermally polymerizing the resulting hydrogenated feedstock to produce a primary pitch; thin-film distillation of the produced primary pitch to remove low boiling point components and obtain an anisotropic pitch enriched in mesogen components; A step of extracting the anisotropic pitch with a solvent, filtering and drying the anisotropic pitch to separate only the mesogen component in the anisotropic pitch; mixing the separated mesogenic component with a basic isotropic pitch.
[0038] Here, the heterophase binder pitch may have a heterophase texture in which an anisotropic texture is uniformly dispersed in an isotropic matrix.
[0039] The medium oil is a medium oil or residual oil generated in a crude oil refining process, and examples of the medium oil that can be used include FCC-DO (fluidized catalytic cracking-decant oil), which is the residual oil of a fluidized bed reactor, PFO (pyrolysis fuel oil) and EBO (ethylene bottom oil), which are the residual oils of a naphtha cracker, VR (vacuum residue), which is the residue of a vacuum distillation tower, and other petroleum-based raw materials such as DAO (de-asphalted oil) obtained by removing asphaltene from these medium oils, and coal-based raw materials such as coal tar, which is a by-product of a coal carbonization process.
[0040] Here, the basic isotropic pitch is Thermally polymerizing the medium oil under normal and elevated pressure to produce an isotropic pitch; and subjecting the isotropic pitch to thin film distillation.
[0041] Here, the thin film distillation may be a thin-film evaporation (TFE) or a thin-layer evaporation (TLE).
[0042] The hydrotreatment is also Reaction temperature of 350℃~500℃; A reaction time of 10 minutes to 10 hours; or The mixing ratio (weight ratio) of medium oil:organic solvent can be 1:0.5 to 1:4.
[0043] Here, if the reaction temperature of the hydrotreating is less than 350° C., the efficiency of the hydrotreating is reduced, and if the reaction temperature of the hydrotreating is more than 500° C., the economic efficiency is reduced.
[0044] In addition, if the reaction time of the hydrogenation treatment is less than 10 minutes, the efficiency of the hydrogenation treatment may be negligible, and if the reaction time of the hydrogenation treatment is more than 10 hours, there may be a problem of reduced economic efficiency.
[0045] If the mixing ratio (weight ratio) of the medium oil to the organic solvent during the hydrotreatment is less than 1:0.5, the efficiency of the hydrotreatment decreases, and if the mixing ratio (weight ratio) of the medium oil to the organic solvent during the hydrotreatment exceeds 1:4, there may be a problem that the production cost increases.
[0046] And, the organic solvent can include a hydrogen donor solvent, including tetralin or tetrahydroquinoline.
[0047] Here, the organic solvent is not limited thereto, and any hydrogen donor solvent can be used.
[0048] The thermal polymerization is Reaction temperature of 400℃~500℃; A reaction time of 10 minutes to 10 hours; or The inert gas flow rate can be set to 100 mL / min / kg to 5000 mL / min / kg.
[0049] Here, if the reaction temperature of the thermal polymerization is less than 400° C., the efficiency of the thermal polymerization decreases, and if the reaction temperature of the thermal polymerization is more than 500° C., the economic efficiency decreases.
[0050] In addition, if the reaction time of the thermal polymerization is less than 10 minutes, the efficiency of the thermal polymerization may be insignificant, and if the reaction time of the thermal polymerization is more than 10 hours, there may be a problem of reduced economic efficiency.
[0051] If the flow rate of the inert gas during the thermal polymerization is less than 100 mL / min / kg, the thermal polymerization efficiency decreases, and if the flow rate of the inert gas during the thermal polymerization is more than 5000 mL / min / kg, there may be a problem of increased production costs.
[0052] The thin film distillation further comprises: Processing temperature: 250℃~400℃; A processing time of 5 to 60 minutes; or It can be performed under pressure conditions of 1 hPa to 100 hPa.
[0053] Here, the thin film distillation is a method for separating a desired substance with high purity by forming a thin film and then performing evaporation. This method is suitable for separating heat-sensitive substances and substances with high boiling points.
[0054] Here, if the treatment temperature of the thin film distillation is less than 250° C., the thin film distillation efficiency decreases, and if the treatment temperature of the thin film distillation is more than 400° C., a problem of producing a non-uniform heterophase binder pitch may occur.
[0055] Furthermore, if the processing time of the thin film distillation is less than 5 minutes, the thin film distillation efficiency may be negligible, and if the processing time of the thin film distillation is more than 60 minutes, a problem of reduced economic efficiency may occur.
[0056] If the pressure during the thin film distillation exceeds 100 hPa, the thin film distillation efficiency decreases, and if the pressure during the thin film distillation is less than 1 hPa, a problem may occur in that a non-uniform hetero-phase binder pitch is produced.
[0057] The anisotropic pitch obtained by the thin film distillation is Softening point 250℃~350℃; Anisotropic content between 70% and 100%; or The production yield may be 15% to 25%.
[0058] Here, the extraction of the solvent is Anisotropic pitch:solvent mixing ratio (weight ratio) = 1:2 to 1:40; Extraction time: 5 minutes to 24 hours; or This can be done using the extraction solvent THF (tetrahydrofuran).
[0059] Here, if the mixing ratio (weight ratio) of the anisotropic pitch to the solvent during the solvent extraction is less than 1:2, the efficiency of the solvent extraction decreases, and if the mixing ratio (weight ratio) of the anisotropic pitch to the solvent exceeds 1:40, a problem of reduced economic efficiency may occur.
[0060] In addition, if the treatment time for the solvent extraction is less than 5 minutes, the efficiency of the solvent extraction may be negligible, and if the treatment time for the solvent extraction is more than 24 hours, there may be a problem of reduced economic efficiency.
[0061] The extraction solvent may be ethers including diethyl ether or ketones including MEK.
[0062] The mixing step of the basic isotropic pitch and the mesogen comprises: Basic isotropic pitch:mesogen mixing ratio = 95:5~60:40; Mixing temperature 200℃~400℃; or The mixing time can be set to 5 minutes to 2 hours.
[0063] Here, in the step of mixing the separated mesogen component with the basic isotropic pitch, if the mixing ratio of the basic isotropic pitch to the mesogen is less than 95:5, the production efficiency of the binder pitch decreases, and if the mixing ratio of the basic isotropic pitch to the mesogen exceeds 60:40, a problem of producing a non-uniform heterophase binder pitch may occur.
[0064] In addition, in the step of mixing the separated mesogen component with the basic isotropic pitch, if the mixing temperature is less than 200°C, the production efficiency of the anisotropic pitch may be negligible, and if the mixing temperature is more than 400°C, a problem of producing a non-uniform heterophase binder pitch may occur.
[0065] In addition, in the step of mixing the separated mesogen component with the basic isotropic pitch, if the mixing time is less than 5 minutes, the production efficiency of the binder pitch decreases, and if the mixing time exceeds 2 hours, a problem of producing a non-uniform heterophase binder pitch may occur.
[0066] The carbonization yield of the hetero-phase binder pitch may be 25% to 50%.
[0067] FIG. 1 is a process flow diagram of a heterophase binder pitch according to one embodiment of the present invention.
[0068] Referring to FIG. 1, the raw material medium oil (S100) is thermally polymerized (S110) and then undergoes thin-film evaporation (TFE) or thin-layer evaporation (TLE) (S120) to produce basic isotropic pitch (S125).
[0069] Then, the raw material, medium oil (S100), is hydrogenated (S130), thermally polymerized (S140), and then undergoes thin-film evaporation (TFE) or thin-layer evaporation (TLE) (S150) to produce anisotropic pitch (S160).
[0070] Then, the anisotropic pitch (S160) is subjected to solvent extraction (S170) with THF (tetrahydrofuran) solvent to produce THFI (S180), which is a mesogen component insoluble in THF.
[0071] Finally, the mesogenic component THFI (S180), which is insoluble in THF, can be mixed (S190) with the basic isotropic pitch (S125) to produce the binder pitch (S200).
[0072] <Heterophase binder pitch> The present invention provides a heterophase binder pitch produced by the above-mentioned method for producing a heterophase binder pitch.
[0073] In particular, the present invention provides a heterophase binder pitch having a uniformly dispersed anisotropic texture in an isotropic matrix, which does not significantly change the softening point and selectively increases only the carbonization yield.
[0074] Here, the microstructure of the heterophase binder pitch may have a morphology in which anisotropic globules are uniformly dispersed in an isotropic matrix.
[0075] The softening point of the heterophase binder pitch may be from 50°C to 200°C.
[0076] The heterophase binder pitch may have an anisotropic content of 0% to 30%.
[0077] The carbonization yield of the hetero-phase binder pitch may be 25% to 50%.
[0078] The present invention will be described in more detail below with reference to examples. However, the following examples are provided to more specifically explain the present invention, and the scope of the present invention is not limited to the following examples. The following examples may be appropriately modified or altered by those skilled in the art within the scope of the present invention.
[0079] <Preparation Example> Manufacturing of FCC-DO isotropic pitch 1) Thermal polymerization 100g of FCC-DO, the raw material, was placed in an autoclave reactor (volume 150mL) and completely sealed. Then, the temperature was raised to 390°C at a rate of 10°C / min while stirring at 100 rpm, and thermal polymerization was carried out by maintaining the temperature for 6 hours. Then, heating was stopped and the internal temperature of the reactor was allowed to drop to room temperature, after which the reaction product, the thermally polymerized FCC-DO, was collected.
[0080] 2) Thin-film evaporation The FCC-DO thermal polymer obtained by thermal polymerization was placed in a rotary thin-film evaporator, heated to 300°C under a reduced pressure of 10 hPa, and then subjected to thin-film distillation for 30 minutes to obtain FCC-DO basic isotropic pitch.
[0081] The softening point of the FCC-DO basic isotropic pitch obtained by thin-film distillation was 97°C, and the carbonization yield was 23.2%. The microstructure of the FCC-DO basic isotropic pitch was observed under a polarizing microscope, and it showed a 100% isotropic structure. The polarizing microscope image is shown in Figure 2.
[0082] <Example> <Comparative Example 1> 410℃ thermal polymerization, 20% anisotropy, production of FCC-DO pitch Thermal polymerization and thin-film distillation were performed under the same conditions as in the preparation example, but only the thermal polymerization temperature was changed to 410°C, and an FCC-DO pitch in which anisotropic spheres were contained within 20% in an isotropic matrix (410°C thermal polymerization, 20% anisotropy, FCC-DO pitch) was produced.
[0083] The resulting 410°C thermally polymerized, 20% anisotropic, FCC-DO pitch had a softening point of 100°C and a carbonization yield of 30.0%. Observation under a polarizing microscope showed that the microstructure contained within 20% anisotropic globules in an isotropic matrix, with some of the globules being uniformly dispersed, but most of them exhibiting an aggregated morphology. The polarizing microscope image is shown in Figure 3.
[0084] <Comparative Example 2> 430℃ thermal polymerization, 20% anisotropy, production of FCC-DO pitch Thermal polymerization and thin-film distillation were performed under the same conditions as in the preparation example, but only the thermal polymerization temperature was changed to 430°C, and an FCC-DO pitch in which anisotropic spheres were contained within 20% in an isotropic matrix (430°C thermal polymerization, 20% anisotropy, FCC-DO pitch) was produced.
[0085] The resulting 430°C thermally polymerized, 20% anisotropic, FCC-DO pitch had a softening point of 110°C and a carbonization yield of 39.2%. Observation under a polarizing microscope showed that the microstructure was an isotropic matrix containing anisotropic globules at a ratio of 20% or less, and the globules were not uniformly dispersed but mostly existed in agglomerates. The polarizing microscope image is shown in Figure 4.
[0086] Example 1: Preparation of 9:1 mixed heterophase binder pitch 1) Hydrogenation 50g of FCC-DO and 50g of tetralin were put into an autoclave reactor (volume 150mL) and then completely sealed. Then, the temperature was raised to 370°C at a rate of 10°C / min while stirring at a speed of 100 rpm, and the hydrogenation reaction was carried out by maintaining the temperature for 1 hour. Then, heating was stopped and the internal temperature of the reactor was allowed to drop to room temperature, and the reaction product, FCC-DO and tetralin hydride, were collected.
[0087] In order to separate tetralin from the reaction products FCC-DO and tetralin hydride, the FCC-DO and tetralin hydride were placed in a rotary evaporator and treated at 150°C for 1 hour. As a result, 50g of hydrogenated FCC-DO from which tetralin had been removed was obtained. The above procedure was repeated once more to prepare a total of 100g of hydrogenated FCC-DO from which tetralin had been removed for the subsequent steps.
[0088] 2) Thermal polymerization 100g of hydrogenated FCC-DO from which tetralin had been removed was added to an autoclave reactor (volume 150mL), and nitrogen gas was introduced at a rate of 200mL / min. The temperature was raised to 390°C at a rate of 5°C / min while stirring at a rate of 100rpm, and thermal polymerization was carried out by maintaining the temperature for 6 hours. After that, heating was stopped and the internal temperature of the reactor was allowed to drop to room temperature. Then, the introduction of nitrogen gas and stirring were stopped, and the reaction product, the hydrogenated FCC-DO thermal polymer, was collected.
[0089] 3) Thin-film distillation The hydrogenated FCC-DO thermal polymer obtained by thermal polymerization was placed in a rotary thin-film distillation apparatus, heated to 390°C under a reduced pressure of 10 hPa, and maintained at that temperature for 30 minutes to obtain a hydrogenated FCC-DO anisotropic pitch.
[0090] The hydrogenated FCC-DO anisotropic pitch obtained by thin film distillation had a softening point of 284°C, and its microstructure was observed under a polarizing microscope and showed an anisotropic structure of about 93%. The polarizing microscope image is shown in Figure 5.
[0091] 4) Solvent extraction To separate the mesogen component, the 93% hydrogenated FCC-DO anisotropic pitch was mixed with an organic solvent, THF (tetrahydrofuran), in a weight ratio of 1:9, and then stirred at a temperature of 50° C. for 24 hours.
[0092] Thereafter, the components that were not soluble in the THF solvent (insoluble matter) were filtered by filtration under reduced pressure, and the insoluble matter was collected and then dried for 12 hours in a convection oven at 60° C. The dried insoluble matter corresponds to the mesogen component and was named THFI.
[0093] The component dissolved in THF solvent was named THFS.
[0094] 5) Mixing The basic isotropic pitch obtained in Preparation Example and the mesogen component THFI were mixed in a weight ratio of 9:1, and the mixture was heated to 350° C. at a heating rate of 5° C. / min, and then stirred for 30 minutes.
[0095] The softening point of the heterophase binder pitch obtained from the 9:1 mixture was 106°C, and the carbonization yield was 35.5%. Observation under a polarizing microscope showed that it contained 7.7% anisotropic structure, and showed a uniformly dispersed morphology in the form of small spheres without aggregation. The polarizing microscope image is shown in Figure 6.
[0096] Example 2: Preparation of 8:2 mixed heterophase binder pitch The basic isotropic pitch obtained from Preparation Example and the THFI obtained from Example 1 were mixed in a weight ratio of 8:2, and the mixture was heated to 350° C. at a heating rate of 5° C. / min, and then stirred for 30 minutes.
[0097] The softening point of the heterophase binder pitch obtained from the 8:2 mixture was 118°C, and the carbonization yield was 38.7%. Observation under a polarizing microscope showed that it contained 10.3% anisotropic structure, and showed a uniformly dispersed morphology in the form of small spheres without aggregation. The polarizing microscope image is shown in Figure 7.
[0098] Example 3: Preparation of heterophase binder pitch mixed at 7:3 ratio The basic isotropic pitch obtained from Preparation Example and the THFI obtained from Example 1 were mixed in a weight ratio of 7:3, and the mixture was heated to 350° C. at a heating rate of 5° C. / min, and then stirred for 30 minutes.
[0099] The softening point of the heterophase binder pitch obtained from the 7:3 mixture was 122°C, and the carbonization yield was 40.8%. Observation under a polarizing microscope showed that it contained 16.8% anisotropic structure, and showed a uniformly dispersed morphology in the form of small spheres without aggregation. The polarizing microscope image is shown in Figure 8.
[0100] <Example 4> Production of graphite block compact 1 The binder pitch obtained from the present invention was applied to the production of graphite blocks. The FCC-DO basic isotropic pitch obtained from the preparation example was mixed with needle coke (particle size 0.1 to 2 mm) in a weight ratio of 25:75, and then kneaded at 180°C for 2 hours.
[0101] The kneaded sample was then placed in a cylindrical mold with a diameter of 1 cm, and pressed with a weight of 1 ton for 10 minutes at 150°C. A cylindrical molded body with a press diameter of 1 cm was obtained, and in order to perform carbonization heat treatment, the temperature was raised to 800°C at a rate of 1°C / min in a furnace under a nitrogen atmosphere, and then maintained at that temperature for 30 minutes.
[0102] Then, the graphitization heat treatment was performed at 2,800° C. The graphitization heat treatment conditions were as follows: after reaching 2,800° C., the maintenance time was 10 minutes, the temperature increase rate was 10° C. / min, and the gas used to maintain the inert atmosphere was argon gas.
[0103] After graphitization, the final compact obtained showed perfect patterning without any breaks or cracks and had a measured density of 1.16 g / cm 3 It was.
[0104] <Example 5> Production of graphite block compact 2 The molded body was produced in the same manner as in Example 4, but the binder pitch used was the pitch obtained in Example 1. Carbonization and graphitization were also carried out under the same conditions. After graphitization, the final molded body obtained showed a perfect pattern without any breaks or cracks, and the measured density was 1.22 g / cm 3 It was.
[0105] <Example 6> Production of graphite block compact 3 The molded body was produced in the same manner as in Example 4, but the binder pitch used was the pitch obtained in Example 2. Carbonization and graphitization were also carried out under the same conditions. After graphitization, the final molded body obtained showed a perfect pattern without any breaks or cracks, and the measured density was 1.24 g / cm3 It was.
[0106] <Example 7> Production of graphite block compact 4 The molded body was produced in the same manner as in Example 4, but the binder pitch used was the pitch obtained in Example 3. Carbonization and graphitization were also carried out under the same conditions. After graphitization, the final molded body obtained showed a perfect pattern without any breaks or cracks, and the measured density was 1.19 g / cm 3 It was.
[0107] As can be seen from the results of Examples 4 to 7, the binder pitch prepared according to the present invention not only exhibits a higher carbonization yield than the existing binder pitch, but also realizes a higher density of the compact when used to prepare a graphite compact compared to the existing binder pitch.
[0108] Thus far, specific examples of the method for producing a heterophase binder pitch according to the present invention and the heterophase binder pitch produced therefrom have been described. However, it is obvious that various modifications are possible within the scope of the present invention.
[0109] Therefore, the scope of the present invention should not be limited to the described embodiments, but should be defined not only by the claims set forth below, but also by equivalents to these claims.
[0110] In other words, it should be understood that the above-described embodiments are illustrative in all respects and not limiting, and the scope of the present invention is indicated by the claims set forth below rather than the detailed description, and all modifications and variations that come within the meaning and scope of the claims and their equivalents should be interpreted as being included in the scope of the present invention.
Claims
1. A method for producing a heterophase binder pitch having a heterophase texture in which an anisotropic texture is uniformly dispersed in an isotropic matrix, comprising: hydrotreating the middle oil to obtain a hydrotreated feed; thermally polymerizing the resulting hydrogenated feedstock to produce a primary pitch; thin-film distillation of the produced primary pitch to remove low boiling point components and obtain an anisotropic pitch enriched in mesogen components; A step of extracting the anisotropic pitch with a solvent, filtering and drying the anisotropic pitch to separate only the mesogen component in the anisotropic pitch; and homogeneously mixing the separated mesogenic component with an isotropic pitch. Method for producing heterophase binder pitch.
2. The isotropic pitch is Thermally polymerizing the medium oil under normal and elevated pressure to produce an isotropic pitch; and subjecting the isotropic pitch to thin-film distillation. A method for producing the heterophase binder pitch according to claim 1.
3. The hydrotreatment is Reaction temperature of 350°C to 500°C; A reaction time of 10 minutes to 10 hours; and The mixing ratio (weight ratio) of medium oil to organic solvent is 1:0.5 to 1:
4. A method for producing the heterophase binder pitch according to claim 1.
4. The organic solvent contains a hydrogen donor solvent containing tetralin or tetrahydroquinoline. A method for producing the heterophase binder pitch according to claim 3.
5. The thermal polymerization is A reaction temperature of 400°C to 500°C; A reaction time of 10 minutes to 10 hours; and The inert gas flow rate is 100 mL / min / kg to 5000 mL / min / kg. A method for producing the heterophase binder pitch according to claim 1.
6. The thin film distillation comprises: A treatment temperature of 250°C to 400°C; A treatment time of 5 to 60 minutes; and It is characterized by being carried out under pressure conditions of 1 hPa to 100 hPa; A method for producing the heterophase binder pitch according to claim 1.
7. The anisotropic pitch obtained from the thin film distillation is Softening point 250℃~350℃; anisotropic content of 70% to 100%; and The production yield is 15% to 25%. A method for producing the heterophase binder pitch according to claim 1.
8. The solvent extraction is Mixing ratio (weight ratio) of anisotropic pitch:solvent=1:2 to 1:40; Extraction time: 5 minutes to 24 hours; and The extraction is carried out under the condition of an extraction solvent of THF (tetrahydrofuran), A method for producing the heterophase binder pitch according to claim 1.
9. The step of mixing the isotropic pitch with the mesogen comprises: Mixing ratio of isotropic pitch:mesogen=95:5 to 60:40; A mixing temperature of 200°C to 400°C; and The mixing time is 5 minutes to 2 hours. A method for producing the heterophase binder pitch according to claim 1.
Citation Information
Patent Citations
Mesophase pitch-based carbon fiber with mixed structure and preparation method of mesophase pitch-based carbon fiber
CN115369520A
Production of mesophase pitch
JP1987270685A
Production of both pitch for producing high-performance carbon fiber and pitch for producing widely useful carbon fiber
JP1990058596A
Production of active carbon fiber
JP1994272117A
Production of carbonic microsphere
JP1998095982A