Aluminum Brazing Sheet
The aluminum brazing sheet with a multilayer structure and specific additive elements addresses the issue of coarse Si particles, ensuring stable and effective brazing joints by suppressing their formation.
Patent Information
- Application Number
- JP2020065306
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-31
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-03-31
AI Technical Summary
Existing aluminum brazing sheets face issues with coarse Si crystallized particles that lower the melting point and cause erosion during brazing, leading to poor bonding properties.
An aluminum brazing sheet with a multilayer structure containing specific Si and additive elements like Ni, Mo, and others, formulated to suppress the activity of P and reduce coarse Si particles, ensuring stable brazing joints.
The solution results in fewer coarse Si particles, enabling good and stable brazing joints with improved bonding properties.
Smart Images

Figure 0007555722000005 
Figure 0007555722000006 
Figure 0007555722000007
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum brazing sheet suitable for brazing and the like. [Background technology]
[0002] In the field of aluminum heat exchangers for automobiles, such as radiators, efforts are being made to reduce the size and weight while at the same time making the aluminum materials thinner and stronger. In the manufacture of aluminum heat exchangers, brazing is used to join joints.
[0003] As a prior art example of a method for manufacturing a brazing filler metal for an aluminum brazing sheet, a method is known in which Na, Sr, or Sb is contained in an Al-Si based brazing filler metal to suppress the generation of coarse Si particles (see Patent Document 1). In aluminum brazing sheets, the remaining coarse Si crystal particles diffuse into the Al during brazing and increase the Si concentration, lowering the melting point of the Al and causing erosion due to localized melting during brazing. Therefore, it is desirable to prevent the crystallization of coarse Si in the brazing material. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 4636520 [Patent Document 2] JP 2014-50861 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors have studied coarse Si crystals in Al-Si brazing filler metals and found that even in the hypoeutectic composition of the Al-Si system, coarse Si crystals like primary Si crystals may crystallize, and that these coarse Si crystals grow from AlP compounds as nuclei. It is believed that P is contained as an inevitable impurity, albeit in trace amounts, in the molten aluminum alloy used in manufacturing aluminum brazing sheets. In order to eliminate the effect of P contained in the molten aluminum alloy, the present inventors have attempted to add an element that reduces the activity of P in the molten aluminum alloy, and have arrived at the present invention.
[0006] The present invention has been made in consideration of the background described above, and has an object to provide an aluminum brazing sheet for brazing that can provide good joinability during brazing. [Means for solving the problem]
[0007] (1) The aluminum brazing sheet according to the present embodiment is an aluminum brazing sheet having a multi-layer structure of at least two layers, which contains, by mass%, 1.5 to 14.0% Si, and further satisfies the following formula (1) in a thermodynamic calculation, contains 0.01 to 0.5% of at least one additive element other than Cr and Cu, and the total content of the one or more additive elements, including other unavoidable impurity elements, is in the range of 0.05 to 1.5%. The remainder is made up of aluminum. The Al-Si brazing material is located on one or both sides of the core material and on the outermost surface of the brazing sheet, and the Al-Si brazing material contains coarse Si particles having a long side length of 50 μm or more when observed in the surface layer (RD-TD) direction, and the number of coarse Si particles having a long side length of 50 μm or more is 1,000,000 μm or more. 2 10 or less per one aluminum brazing sheet. Gamma x <γ0 and γ 3x <γ x ...Formula (1) In the formula (1), γ x indicates the activity coefficient of P when an additive element is added at a target concentration of 0.01 to 0.5 mass%, γ0 indicates the activity coefficient of P when no element is added, and γ3x indicates the activity coefficient of P when each added element is three times the target concentration.
[0008] (2) In the aluminum brazing sheet according to the present embodiment, the additive element is Ni, Mo Either one of the following or 2 types It is preferable that there is. Effect of the Invention
[0009] According to the present invention, the number of coarse precipitated Si particles that cause erosion is reduced, and good and stable brazing can be performed. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a diagram showing a brazing sheet for brazing in one embodiment of the present invention. [Diagram 2] 1 is a perspective view showing an aluminum heat exchanger for an automobile according to an embodiment of the present invention; [Diagram 3] FIG. 2 is a diagram showing a brazing evaluation model in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the present invention will be described in detail based on embodiments. The brazing sheet of the first embodiment is an aluminum brazing sheet having a multi-layer structure of at least two layers, and includes a core material and an Al-Si brazing material clad on one or both sides of the core material and positioned on the outermost surface. Alternatively, the brazing sheet may be a three-layer structure brazing sheet having an Al-Si brazing material clad on one side of the core material and a sacrificial material clad on the other side of the core material. The Al-Si brazing material contains, by mass%, 1.5 to 14.0% Si, and further contains 0.01 to 0.5% of at least one additive element that satisfies the following formula (1) in thermodynamic calculation. It may contain inevitable impurities, which will be described later.
[0012] Gamma x <γ0 and γ 3x <γ x ...Formula (1) In the formula (1), γ x indicates the activity coefficient of P when the additive element is added at the target concentration (0.01 to 0.5 mass%), γ0 indicates the activity coefficient of P when no element is added, and γ 3x indicates the activity coefficient of P when each added element is three times the target concentration.
[0013] The total content of the one or more additive elements contained in the Al-Si brazing filler metal is in the range of 0.05 to 1.5%, including other inevitable impurity elements, and the number of coarse Si particles having a long side length of 50 μm or more when observed in the surface layer (RD-TD) direction of the Al-Si brazing filler metal is 1,000,000 μm or more. 2 There are 10 or less per
[0014] The composition and the like specified in the brazing sheet of this embodiment will be described below. The contents are all indicated as mass ratios, and when the range of mass ratios is expressed using "~", the expression includes the lower and upper limits unless otherwise specified. Thus, as an example, 0.01-2.0% means a content of 0.01% or more and 2.0% or less.
[0015] "Brazing material" Si: 1.5-14.0% Silicon forms a molten brazing material during brazing and forms a fillet at the joint. However, if the Si content is too low, there will be insufficient molten brazing material to form the fillet. On the other hand, if the Si content is too high, not only will the effect saturate, but the material will become hard and brittle, making it difficult to manufacture the material. For this reason, the Si content of the brazing material of this embodiment is set to the above range. For the same reason, the lower limit of the Si content is preferably 3.0% and the upper limit is preferably 12.0%.
[0016] Ca: 100 mass ppm or less Ca is usually contained as an inevitable impurity at about several hundred ppm by mass or less, but since it forms high melting point compounds with other elements and may deteriorate brazing properties, it is preferable to set the upper limit at 100 ppm by mass. For the same reason, it is even more preferable to set the Ca content in the brazing filler metal of this embodiment at 10 ppm by mass or less.
[0017] Zn: 0.1-9.0% Zn can provide a sacrificial anticorrosive effect by making the potential of the material more base, so it is included in the brazing material as desired. However, when Zn is included, if the content is too small, the sacrificial anticorrosive effect becomes insufficient, while if the content is too large, the effect becomes saturated. Therefore, when Zn is included in the brazing material of this embodiment, the content is set to the above range. For the same reason, the Zn content is preferably set at a lower limit of 0.5% and an upper limit of 7.0%. Even if Zn is not actively added, it may contain less than 0.1% Zn as an impurity.
[0018] "Elements that decrease the activity of P" The brazing filler metal of this embodiment contains one or more of Cr, Ni, Cu and Mo as elements that reduce the activity of P in the molten aluminum alloy. For example, in a molten aluminum alloy with a target composition of Al: 87.959%, Si: 12%, P: 0.001%, and the balance 0.004%, the activity coefficient of P in the absence of the above-mentioned additive elements is 1.37 × 10 -3 It is. In contrast, among Cr, Ni, Cu, and Mo, Cr has a large effect of decreasing the activity coefficient of P, and the effect of decreasing the activity coefficient of P gradually decreases in the order from Cr to Ni, Cu, and Mo.
[0019] Therefore, by preparing a molten aluminum alloy containing the above-mentioned additive elements constituting the brazing material and adding these elements to the molten aluminum alloy, AlP compounds are less likely to precipitate during casting if the molten aluminum alloy contains a trace amount of P. If a large amount of AlP compounds precipitate during casting, a large amount of primary crystal Si will precipitate with the AlP compounds as nuclei. Therefore, when a slab that serves as a base for a brazing material is produced by casting an aluminum alloy melt containing the above-mentioned elements, the precipitation of AlP compounds in the slab can be suppressed. Therefore, when the cast piece is rolled to the required thickness to form a brazing sheet as the clad material, and the core material and the brazing sheet are then clad rolled to produce a brazing sheet, no coarse primary Si crystals are precipitated in the brazing material, or even if they are precipitated, the number of precipitates is small.
[0020] "Example of calculation of activity coefficient" The activity and activity coefficient of P at 900°C were calculated for an aluminum alloy with a composition of Al: 87.959%, Si: 12%, and P: 0.001% when 0.04% of elements was added. The thermodynamic calculation software Fact Stage 7,X (database SGTEb: Computational Mechanics Research Center, Inc.) was used for the calculation. The results are set forth in Table 1 below.
[0021] [Table 1]
[0022] The calculation example shown in Table 1 shows the results of calculating the difference in activity coefficients between an aluminum alloy having a composition of Al: 87.959%, Si: 12%, and P: 0.001%, with 0.04% of the target composition of elements being added and an aluminum alloy having three times the target composition, that is, 0.12% of the elements being added.
[0023] As shown in Table 1, the calculation results suggest that Cr, Ni, Cu, and Mo are elements with large drag when suppressing the activity of P. Based on these results, by using an aluminum alloy brazing filler metal containing one or more of Cr, Ni, Cu, and Mo in an Al-Si alloy, with the remainder being Al and unavoidable impurities, it is possible to provide a brazing sheet equipped with a brazing filler metal with a low number of precipitated coarse Si particles with a long side length of 50 μm or more.
[0024] "Distribution of Si particles on the surface of brazing filler metal" Coarse Si particles: Coarse Si particles with a long side length of 50 μm or more are 1,000,000 μm 2 10 or less per Coarse silicon particles resulting from casting remain in the brazing sheet in the form of lumps or plates without being crushed even during hot rolling. These coarse silicon particles cause local melting called erosion during brazing, which causes holes during brazing. Furthermore, these coarse Si particles are generated during casting, and for example, solidification conditions differ between the surface side and the center side during DC casting, which may result in differences in distribution. Furthermore, brazing sheets are usually cut out in both width and length directions from a coil before being supplied. Therefore, in order to confirm that they are not generated under different casting conditions, observations were made so that each particle would be included when the sheet was divided into three in the width direction during casting, and also so that each particle would be included when the sheet was divided into three in the height direction during casting (length direction in the case of horizontal continuous casting), with an observation field of 1,000,000 μm 2 It is preferable to configure a field of view (1000 μm square).
[0025] "Heartwood" The composition of the core material in this embodiment is not limited to a specific one, but the following components are preferably shown. As an example, the core material can be composed of an aluminum alloy containing, by mass%, one or more of the following: Si: 0.05-1.2%, Mg: 0.01-2.0%, Mn: 0.1-2.5%, Cu: 0.01-2.5%, Fe: 0.05-1.5%, Zr: 0.01-0.3%, Ti: 0.01-0.3%, Cr: 0.01-0.5%, Bi: 0.005-1.5%, and Zn: 0.1-9.0%, with the remainder being Al and unavoidable impurities. As another example, the core material can be composed of an aluminum alloy containing, by mass%, Si: 0.05-1.2%, Mg: 0.01-2.0%, and one or more of Mn: 0.1-2.5%, Cu: 0.01-2.5%, Fe: 0.05-1.5%, Zr: 0.01-0.3%, Ti: 0.01-0.3%, Cr: 0.01-0.5%, Bi: 0.005-1.5%, and Zn: 0.1-9.0%, with the remainder being Al and unavoidable impurities.
[0026] Silicon: 0.05 to 1.2% Si not only improves the strength of the material by solid solution, but also has the effect of improving the strength of the material by precipitating as Mg2Si or Al-Mn-Si compounds. However, if the content is too small, the effect is insufficient. On the other hand, if the content is too large, the solidus temperature of the core material decreases and it melts during brazing. For these reasons, when Si is contained in the core material, the Si content is set to the above range. For the same reason, it is desirable to set the Si content to a lower limit of 0.1% and an upper limit of 1.0%. Even if Si is not intentionally contained, the core material may contain, for example, 0.05% or less as an inevitable impurity.
[0027] Mg: 0.01-2.0% Mg improves the strength of the material by precipitating compounds with Si and other elements. However, if the content is too low, the effect is insufficient, while if the content is too high, not only the effect saturates but the material becomes hard and brittle, making it difficult to manufacture. For these reasons, if Mg is contained in the core material, the Mg content is set to the above range. For the same reason, it is preferable that the Mg content be 0.05% at the lower limit and 1.0% at the upper limit. Even if Mg is not intentionally contained, the core material may contain, for example, 0.01% or less as an unavoidable impurity.
[0028] Mn: 0.1-2.5% Mn precipitates as an intermetallic compound to improve the strength of the material. Furthermore, by dissolving in solid solution, it makes the potential of the material more noble, improving the corrosion resistance. However, if the content is too small, the effect is insufficient, while if it is too large, the material becomes hard and the material rollability decreases. For these reasons, when Mn is contained in the core material, the Mn content is set to the above range. For the same reason, it is preferable that the Mn content be 0.3% at the lower limit and 1.8% at the upper limit. Even if Mn is not intentionally added, the core material may contain, for example, 0.1% or less as an unavoidable impurity.
[0029] Cu: 0.01-2.5% Cu dissolves in the material to improve its strength. However, if the content is too low, the effect is insufficient, while if the content is too high, the solidus temperature of the core material drops and the core material melts during brazing. For these reasons, when Cu is contained in the core material, the Cu content is set to the above range. For the same reason, it is preferable that the Cu content be limited to a lower limit of 0.02% and an upper limit of 1.2%. Even if Cu is not intentionally contained, the core material may contain, for example, 0.01% or less of Cu as an unavoidable impurity.
[0030] Fe: 0.05 to 1.5% Fe precipitates as an intermetallic compound to improve material strength. It also promotes recrystallization during brazing and inhibits brazing erosion. However, if the content is below the lower limit, the effect is insufficient, while if it is too high, the corrosion rate after brazing increases. For these reasons, when Fe is contained in the core material, the Fe content is set to the above range. For the same reason, it is preferable that the Fe content be 0.1% at the lower limit and 0.6% at the upper limit. Even if Fe is not intentionally contained, the core material may contain, for example, 0.05% or less Fe as an unavoidable impurity.
[0031] Zr: 0.01 to 0.3% Zr forms fine intermetallic compounds to improve the strength of the material. However, if the content is below the lower limit, the effect is insufficient, while if the content is too high, the material becomes hard and the workability decreases. For these reasons, when Zr is contained in the core material, the Zr content is set to the above range. For the same reason, the Zr content is preferably set at 0.05% at the lower limit and 0.2% at the upper limit. Even if Zr is not intentionally contained, the core material may contain, for example, 0.01% or less as an unavoidable impurity.
[0032] Ti: 0.01 to 0.3% Ti forms fine intermetallic compounds and improves material strength. However, if the content is less than the lower limit, the effect is insufficient, while if it is too high, the material becomes hard and the workability decreases. For these reasons, when Ti is contained in the core material, the Ti content is set to the above range. For the same reason, it is preferable that the Ti content be set to a lower limit of 0.05% and an upper limit of 0.2%. Even if Ti is not intentionally contained, the core material may contain, for example, 0.01% or less as an unavoidable impurity.
[0033] Cr: 0.01~0.5% Cr forms fine intermetallic compounds and improves material strength. However, if the content is less than the lower limit, the effect is insufficient, while if it is too high, the material becomes hard and its workability decreases. For these reasons, when Cr is contained in the core material, the Cr content is set to the above range. For the same reason, it is preferable that the Cr content be set to a lower limit of 0.05% and an upper limit of 0.3%. Even if Cr is not intentionally contained, the core material may contain, for example, 0.01% or less as an unavoidable impurity.
[0034] Bi: 0.005 to 1.5% Bi reduces the surface tension of the molten brazing filler metal by partially diffusing into the brazing filler metal layer. It also suppresses the growth of a dense oxide film on the material surface. However, if the content is below the lower limit, the effect is insufficient, while if it is too high, the effect saturates and Bi oxides are easily generated on the material surface, hindering joining. For these reasons, when Bi is contained in the core material, the Bi content is set to the above range. For the same reason, it is preferable that the Bi content be set at a lower limit of 0.05% and an upper limit of 0.5%. Even if Bi is not intentionally contained, the core material may contain, for example, 0.005% or less as an unavoidable impurity.
[0035] Zn: 0.1-9.0% Zn makes the pitting potential of the material more base than other materials, and exerts a sacrificial corrosion protection effect. However, if the content is below the lower limit, the effect is insufficient, while if it is too high, the effect saturates. For these reasons, when Zn is contained in the core material, the Zn content is set to the above range. For the same reason, it is preferable that the Zn content be 0.5% at the lower limit and 7.0% at the upper limit. Even if Zn is not intentionally contained, the core material may contain, for example, 0.1% or less as an unavoidable impurity.
[0036] "Sacrificial material" In this embodiment, the aluminum brazing sheet may be an aluminum brazing sheet having a core material clad with a sacrificial material. The composition of the sacrificial material in this embodiment is not limited to a specific one, but the following components are preferably shown. Zn: 0.1-9.0% Zn is added to the sacrificial material to make the natural potential of the material more base than other materials, to exert a sacrificial anticorrosive effect, and to improve the pitting corrosion resistance of the clad material. If the content is less than the lower limit, the effect is insufficient, and if the content is more than the upper limit, the potential becomes too base, the corrosion wear rate of the sacrificial material increases, and the pitting corrosion resistance of the clad material decreases due to the early disappearance of the sacrificial material. For the same reason, it is preferable that the amount of Zn contained in the sacrificial material is 1.0% at the lower limit and 8.0% at the upper limit.
[0037] Silicon: 0.05 to 1.2% Silicon is added to the sacrificial material as desired, because it precipitates as an intermetallic compound such as Al-Mn-Si or Al-Mn-Si-Fe, dispersing the starting points of corrosion and improving the pitting corrosion resistance of the clad material. If the content is less than the lower limit, the effect is insufficient, and if the content is more than the upper limit, the corrosion rate increases, and the pitting corrosion resistance of the clad material decreases due to the early disappearance of the sacrificial material. For the same reason, it is preferable that the amount of silicon contained in the sacrificial material is 0.3% at the lower limit and 1.0% at the upper limit.
[0038] Mg: 0.01-2.0% Mg is added to the sacrificial material as desired to strengthen the oxide film and thereby improve corrosion resistance. If the content is less than the lower limit, the effect is insufficient, and if the content is more than the upper limit, the material becomes too hard and rolling manufacturability decreases. For the same reason, it is preferable that the amount of Mg contained in the sacrificial material is 0.05% at the lower limit and 1.5% at the upper limit.
[0039] Mn: 0.1-2.5% Mn is added to the sacrificial material as desired, because it precipitates as intermetallic compounds such as Al-Mn, Al-Mn-Si, Al-Mn-Fe, and Al-Mn-Si-Fe, dispersing the starting points of corrosion and improving the pitting corrosion resistance of the clad material. If the content is less than the lower limit, the effect is insufficient, and if the content is more than the upper limit, the corrosion rate increases and the pitting corrosion resistance of the clad material decreases due to the early disappearance of the sacrificial material. For the same reason, it is preferable that the amount of Mn contained in the sacrificial material is 0.4% at the lower limit and 1.8% at the upper limit.
[0040] Fe: 0.05 to 1.5% Fe is added to the sacrificial material as desired, because it precipitates as an intermetallic compound such as Al-Mn-Fe or Al-Mn-Si-Fe, dispersing the starting points of corrosion and improving the pitting corrosion resistance of the clad material. If the content is less than the lower limit, the effect is insufficient, and if the content is more than the upper limit, the corrosion rate increases and the pitting corrosion resistance of the clad material decreases due to the early disappearance of the sacrificial material. For the same reason, it is preferable to set the Fe content in the sacrificial material to 0.1% at the lower limit and 0.7% at the upper limit.
[0041] Zr: 0.01 to 0.3% Zr is added to the sacrificial material as desired to improve the pitting corrosion resistance of the clad material by precipitating as an Al-Zr intermetallic compound to disperse the starting point of corrosion, and by forming a layered corrosion form by forming a shaded area of solid-solubilized Zr. If the content is below the lower limit, the effect is insufficient, and if it exceeds the upper limit, a huge intermetallic compound is formed during casting, resulting in a decrease in rollability. For the same reason, it is preferable that the amount of Zr contained in the sacrificial material is 0.05% at the lower limit and 0.25% at the upper limit.
[0042] Ti: 0.01 to 0.3% Ti is added to the sacrificial material as desired to improve the pitting corrosion resistance of the clad material by precipitating as an Al-Ti intermetallic compound to disperse the starting point of corrosion, and by forming a layered corrosion form by forming a shading area of solid solution Ti. If the content is below the lower limit, the effect is insufficient, and if it exceeds the upper limit, a huge intermetallic compound is formed during casting, resulting in a decrease in rollability. For the same reason, it is preferable that the amount of Ti contained in the sacrificial material is 0.05% at the lower limit and 0.25% at the upper limit.
[0043] Cr: 0.01~0.5% Cr is added to the sacrificial material as desired to improve the pitting corrosion resistance of the clad material by precipitating as an Al-Cr intermetallic compound to disperse the starting point of corrosion or by forming a layered corrosion form by forming a dark and light area of solid-solubilized Cr. If the content is below the lower limit, the effect is insufficient, and if it exceeds the upper limit, a huge intermetallic compound is formed during casting, resulting in a decrease in rollability. For the same reason, it is preferable that the amount of Cr contained in the sacrificial material is 0.1% at the lower limit and 0.4% at the upper limit.
[0044] Bi: 0.005 to 1.5% Bi is added to the sacrificial material as desired because it diffuses into the molten brazing filler metal when the molten brazing filler metal comes into contact with the surface of the sacrificial material, thereby reducing the surface tension of the molten brazing filler metal and suppressing the growth of a dense oxide film on the surface of the material. However, if the content is less than the lower limit, the effect is insufficient, while if the content is too high, the effect is saturated and Bi oxide is easily generated on the surface of the material, hindering bonding. For these reasons, the Bi content in the sacrificial material is set to the above range. For the same reason, it is preferable that the Bi content be 0.05% at the lower limit and 0.5% at the upper limit. However, even if Bi is not intentionally added, the sacrificial material may contain, for example, 0.005% or less Bi as an inevitable impurity.
[0045] In the aluminum brazing sheet according to this embodiment, the core material is clad with a sacrificial material, and the sacrificial material contains, by mass%, Zn: 0.1-9.0%, and further contains one or more of Si: 0.05-1.2%, Mg: 0.01-2.0%, Mn: 0.1-2.5%, Fe: 0.05-1.5%, Zr: 0.01-0.3%, Ti: 0.01-0.3%, Cr: 0.01-0.5%, and Bi: 0.005-1.5%.
[0046] "Brazing sheet manufacturing method" The aluminum alloy is prepared to have the composition of the present invention and produced by melting. The melting can be carried out by a semi-continuous casting method. The resulting aluminum alloy ingot is subjected to homogenization treatment under prescribed conditions. If the homogenization treatment temperature is low, coarse intermetallic compounds may precipitate, so the treatment temperature is 400°C or higher for 1 to 10 hours.
[0047] A sheet-shaped brazing filler metal can be obtained by hot rolling and cold rolling an aluminum alloy ingot. In aluminum alloy ingots, normal eutectic Si crystallizes in needle-like shapes and is easily crushed during hot rolling, but coarse Si particles that crystallize as primary crystals are less likely to be crushed because they are lumpy or plate-like. Therefore, coarse Si particles that are not needle-like often remain embedded in the clad material from the brazing material even when the reduction rate is increased. Therefore, the crystallization of coarse Si particles must be prevented, but as described below, the crystallization of coarse Si particles can be suppressed by adding an element that reduces the activity of P.
[0048] Next, the brazing filler metal is assembled with a core material or the like and subjected to hot clad rolling. At this time, in this embodiment, it is desirable to control the rolling time at a predetermined temperature during hot rolling, the equivalent strain from the start to the end of hot rolling, the hot rolling finish temperature, and the cooling rate after hot rolling. Specifically, the condition can be exemplified as follows: the material temperature during hot rolling is between 400 and 500° C. and the rolling time is 10 minutes or longer.
[0049] In addition, the equivalent strain from the start to the end of hot rolling can be controlled. Specifically, the slab thickness and the finishing thickness can be adjusted so that the equivalent strain ε shown in the following formula (2) is ε>5.0. ε=(2 / √3)ln(t0 / t) …Equation (2) In formula (2), t0: hot rolling start thickness (slab thickness), t: hot rolling finish thickness.
[0050] Furthermore, if the hot rolling finishing temperature is high and a state without dynamic strain is maintained, and if the cooling rate after hot rolling is slow, coarse compounds will precipitate at grain boundaries, etc., so it is desirable to lower the hot rolling finishing temperature to a predetermined temperature and ensure a cooling rate above a certain level. Specifically, as an example, the hot rolling finish temperature can be set to 250 to 350° C., and the cooling rate from the finish temperature to 200° C. can be controlled to be faster than 20° C. / hr.
[0051] Thereafter, the brazing sheet of this embodiment is obtained through cold rolling and the like. In the cold rolling, for example, cold rolling is performed at a total reduction of 75% or more, intermediate annealing is performed at a temperature of 300 to 400°C, and then final rolling at a rolling reduction of 40% is performed, but the conditions are not particularly limited. Also, intermediate annealing may not be performed.
[0052] By carrying out hot rolling and cold rolling, a clad material can be obtained in which a brazing material is superimposed and bonded to one or both surfaces of a core material. Through the above steps, an aluminum brazing sheet 1 for a heat exchanger is obtained in which an aluminum alloy brazing material 3 is clad on one side of an aluminum alloy core material 2, as shown in Fig. 1. Although Fig. 1 shows an aluminum brazing sheet 1 in which one side of the core material is clad with brazing material, an aluminum brazing sheet in which both sides of the core material are clad with brazing material may also be used. Alternatively, an aluminum brazing sheet in which a sacrificial material or the like is clad on the other side of the core material may also be used.
[0053] For example, an aluminum alloy containing, by mass, 0.1-0.8% Mg, 0.1-1.2% Si, and the remainder consisting of Al and unavoidable impurities is prepared as the brazing target member 4, and processed into an appropriate shape such as a fin material. Note that, in this embodiment, the composition of the brazing target member is not particularly limited. When a fin material for a heat exchanger is obtained by the above-mentioned cold rolling or the like, it is then subjected to corrugating processing or the like as necessary. The corrugating processing can be performed by passing the material between two rotating dies, which enables good processing and shows excellent formability.
[0054] The fin material obtained in the above process is used as a component of a heat exchanger, and is combined with other components (tubes, headers, etc.) to form an assembly which is then subjected to brazing.
[0055] The assembled body is heated at a temperature increase rate of, for example, 10 to 200°C / min, and brazing is performed under heat treatment conditions such that the assembled body reaches a temperature of 559 to 630°C. In terms of brazing conditions, the faster the heating rate, the shorter the brazing time, which suppresses the growth of an oxide film on the material surface and improves brazing properties. Brazing is possible if the temperature reached is at least the solidus temperature of the brazing material, but by bringing the temperature closer to the liquidus temperature, the amount of flowing brazing material increases, making it easier to obtain a good joint condition in joints with open parts. However, if the temperature is too high, brazing material erosion will progress and the structural dimensional accuracy of the assembled body after brazing will decrease, which is not preferable.
[0056] At this time, the eutectic temperature of the Al-Si system is 577°C, and the eutectic portion melts under the above brazing conditions. At this time, if coarse Si particles are present, local melting occurs, which is not preferable, especially when the plate thickness is thin, so it is preferable to add an element that reduces the activity coefficient of P to the brazing material as described above.
[0057] 2 shows an aluminum heat exchanger 5 in which fins 6 are formed using the aluminum brazing sheet 1 and an aluminum alloy tube 7 is used as the material to be brazed. The fins 6 and tubes 7 are assembled with a reinforcing material 8 and a header plate 9, and then brazed to obtain the aluminum heat exchanger 5 for use in automobiles, etc.
[0058] FIG. 3 shows the width W of the joint 10 consisting of a fillet formed between the curved portion of the fin 6 and the tube 7 (the total width of the fillet along the length of the tube 7 so as to sandwich the contact point between the apex of the curved portion of the fin 6 and the tube 7). FIG. 3 shows, on the left and right, an example in which the width W of the joint 10 is large and an example in which it is small. If the width W of the joint 10 is large as shown in FIG. 3, then a good brazing joint has been formed. If a heat exchanger 5 is manufactured by brazing using a fin 6 made of the brazing sheet 1 of this embodiment, a sufficiently large fret can be formed at the brazed joint, so that a heat exchanger 5 having a good brazed joint can be provided.
[0059] In addition, the number of coarse silicon particles generated in the brazing material can be suppressed to 10 or less, making it possible to achieve brazing joints with low likelihood of causing erosion during brazing. In addition, the coarse Si particles are 100,000 μm 2 In the case of a brazing sheet having a brazing filler metal with 10 or less Si particles per square meter, strictly speaking, there is a possibility that erosion may occur at the locations where the coarse Si particles exist. However, the proportion of the joint 10 consisting of the fillet shown in Figure 3 relative to the total area of the brazing sheet is extremely low. For this reason, 2 If the number of particles per square inch is 10 or less, it is unlikely that any substantial problems will occur in the joint 10, and it can be determined that sufficiently excellent brazing performance can be obtained. EXAMPLES
[0060] Various brazing sheets using brazing filler metals with the compositions shown in Tables 2 and 3 (balance: Al and unavoidable impurities) were produced from hot-rolled sheets obtained under the casting and hot-rolling conditions shown in Table 4. The cladding ratio was 10% brazing filler metal to the core material. Thereafter, cold rolling including intermediate annealing was performed to produce a 0.30 mm thick cold rolled sheet with an H14 equivalent temper.
[0061] <Number of coarse Si particles with a long side length of 50 μm or more on the surface of the brazing material layer> For the aluminum clad materials produced, the outermost surface of the brazing material was polished with abrasive grains of about 0.1 μm, and fully automatic particle analysis was performed from the surface direction using an EPMA (electron beam microanalyzer) at 10,000 μm for each sample. 2 The purpose of polishing with the above abrasive grains is to remove rolling marks (surface irregularities) and make the brazing material surface smoother, thereby improving the accuracy of particle analysis. In the measurement, the number of Si particles having a long side length of 50 μm or more was calculated. The measurement results are shown in Tables 2 and 3.
[0062] [Table 2]
[0063] [Table 3]
[0064] [Table 4]
[0065] As shown in Tables 2 and 3, Examples 1 to 34 are brazing sheets in which an Al-Si-based brazing material containing, by mass%, 1.5 to 14.0% Si and, in addition, 0.01 to 0.5 mass% of at least one additive element that satisfies the above-mentioned formula (1) in thermodynamic calculations, with the total content of the additive elements being 0.05 to 1.5 mass% including other unavoidable impurities, is clad on one side of a core material and positioned as the outermost surface. The brazing sheets of these examples are made of Al-Si brazing materials, and the amount of coarse Si particles having a long side length of 50 μm or more when observed in the surface layer (RD-TD) direction is 1,000,000 μm or more. 2 There are 10 or less per Therefore, when brazing is performed using the above-mentioned brazing sheet, it is possible to obtain a brazing object such as a heat exchanger that is less susceptible to erosion, has excellent corrosion resistance, and has excellent brazing joinability.
[0066] When the Si content was low, as in Comparative Example 35 shown in Table 3, the molten brazing material was insufficient during brazing, while when the Si content was high, as in Comparative Example 36, the brazing material layer became hard and brittle, causing cracks during rolling and making production impossible.
[0067] Comparative Examples 37 to 44 shown in Table 3 did not contain any elements that reduce the activity coefficient of P, or the content was insufficient, resulting in a large number of coarse Si particles of 50 μm or more, and causing problems with erosion resistance.
[0068] In Comparative Examples 45 to 47 shown in Table 3, the content of elements that reduce the activity coefficient of P was too high, so coarse compounds were generated, which caused breakage during rolling and made production impossible. [Industrial Applicability]
[0069] The brazing sheet of the present invention can be widely used in heat exchangers such as indoor and outdoor units of air conditioning equipment, and heat exchangers for automobiles. [Explanation of symbols]
[0070] 1...aluminum brazing sheet, 2...aluminum alloy core material, 3...aluminum alloy brazing material, 4...target component, 5...aluminum heat exchanger, 6...fin, 7...tube, 10...joint.
Claims
1. An aluminum brazing sheet having a multi-layer structure of at least two layers, Contains 1.5 to 14.0% Si by mass%, Furthermore, an Al-Si based brazing material that satisfies the following formula (1) in a thermodynamic calculation, contains at least one additive element excluding Cr and Cu in an amount of 0.01 to 0.5%, the total content of the one or more additive elements including other unavoidable impurity elements is in the range of 0.05 to 1.5%, and the balance is aluminum, is located on one or both sides of the core material and on the outermost surface of the brazing sheet, The Al-Si brazing material contains coarse Si particles having a long side length of 50 μm or more when observed in the surface layer (RD-TD) direction, and the Si particles are 1,000,000 μm or more in length. 2 10 or less defects per one aluminum brazing sheet. Gamma x <γ 0 , and γ 3x <γ x ...Formula (1) However, in formula (1), γ x indicates the activity coefficient of P when the additive element is added at a target concentration of 0.01 to 0.5 mass%, and γ 0 indicates the activity coefficient of P when no element is added, and γ 3x indicates the activity coefficient of P when each added element is three times the target concentration.
2. 2. The aluminum brazing sheet according to claim 1, wherein the additional element is one or both of Ni and Mo.
Citation Information
Patent Citations
Aluminum alloy brazing filler metal for brazing heat exchanger and aluminum alloy brazing sheet for heat exchanger
JP1994182581A
Aluminum alloy brazing filler metal for brazing heat exchanger and aluminum alloy brazing sheet for heat exchanger
JP1994182582A
Aluminum alloy brazing fin material for heat exchanger
JP2005060790A
Aluminum brazing filler alloy excellent in brazing filler metal filling property, brazing sheet using the same, header pipe for heat exchanger, and heat exchanger
JP2010064080A
Brazing sheet excelling in brazing property, and method of manufacturing brazed article
JP2012250272A