Aluminum alloy bare material and brazing sheet with excellent thermal conductivity and strength
The aluminum alloy composition with optimized Fe, Si, Cu, and Mn content, along with controlled compound particle distribution, addresses the trade-off between conductivity and strength in heat exchangers, providing enhanced performance for miniaturized automotive applications.
Patent Information
- Application Number
- JP2020151358
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-09
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-09-09
AI Technical Summary
Existing aluminum alloys used in automotive heat exchangers face a trade-off between thermal conductivity and structural strength, with Al-Mn alloys compromising electrical conductivity and 1000 series alloys lacking sufficient strength, making it difficult to achieve both high heat dissipation and structural integrity.
An aluminum alloy composition with controlled amounts of Fe, Si, Cu, and Mn, along with optimized particle size and distribution of Al-Fe and Al-Fe-Si compounds, enhances electrical conductivity and strength through solid solution strengthening and particle dispersion, while minimizing corrosion risks.
The alloy achieves high electrical conductivity and structural strength, suitable for miniaturized heat exchangers with improved heat dissipation performance and corrosion resistance.
Smart Images

Figure 0007555765000005 
Figure 0007555765000006 
Figure 0007555765000007
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum alloy bare material and a brazing sheet having excellent thermal conductivity and strength. [Background technology]
[0002] In recent years, new heat exchangers such as inverter coolers have been installed in automobiles due to the shift to electric vehicles. In order to reduce the size and weight of inverter coolers, it is necessary to improve the heat dissipation performance of the heat exchanger. For example, in inverter coolers that have a structure with a high density of bonding between components, the higher the thermal conductivity of the aluminum material used, the better the heat dissipation performance of the inverter cooler. Aluminum alloys used in automotive heat exchangers are generally Al-Mn alloys due to their strength and corrosion resistance. However, Mn added to Al tends to significantly reduce electrical conductivity when dissolved in the Al matrix. The thermal conductivity and electrical conductivity of Al are proportional, and a decrease in electrical conductivity leads to a decrease in thermal conductivity. Therefore, there is a limit to the improvement of heat dissipation performance in automotive heat exchangers that use Al-Mn alloys with poor electrical conductivity. On the other hand, if 1000 series alloys that do not contain Mn are used with an emphasis on heat dissipation, they have high electrical conductivity, but their strength is low as a component of automotive heat exchangers and they cannot maintain the structural strength of the heat exchanger. For this reason, in order to improve the heat dissipation performance while ensuring the structural strength and corrosion resistance of automotive heat exchangers, it is necessary to ensure strength and improve thermal conductivity by using aluminum alloys other than Al-Mn alloys.
[0003] Conventionally, an aluminum alloy material having a composition of 2.0 to 3.0 mass% Fe, 0.5 to 1.5 mass% Si, 0.05 mass% or less Ti, with the balance being Al and unavoidable impurities, has been known as an aluminum alloy material exhibiting high strength and high thermal conductivity (see Patent Document 1). In addition, an aluminum alloy fin material for heat exchangers is provided, which is composed of 0.010 to 0.4 mass% Fe, less than 0.005 mass% Cu, the balance being Al and impurities, has an Al purity of 99.30 mass% or more, has an average grain size of subgrains of 2.5 μm or less, and has an intermetallic compound content of 2000 particles / mm2 with a maximum length exceeding 3 μm. 2 The following aluminum fin material is known (see Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-256365 A [Patent Document 2] JP 2014-074198 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in recent years, with the demand for further miniaturization and high heat dissipation performance of heat exchangers, there is a demand for aluminum alloys with high electrical conductivity (= high thermal conductivity). Therefore, the inventors have been developing various Al alloys of systems other than Al-Mn alloys. In connection with the development of this material, the inventors conducted research into a composition system in which Fe, Si, and Cu were added to Al. As a result, they discovered that it is possible to improve the electrical conductivity dramatically compared to Al-Mn alloys by adding Fe, which hardly forms a solid solution in aluminum base material, and Si, and by taking a step of optimizing the particle size of the Al-Fe compound present in the Al matrix, or the particle size and density of the Al-Fe-Si compound.
[0006] However, it was found that the structural strength of the heat exchanger cannot be maintained after molding into the target component only by the dispersed particle strengthening mechanism of these compounds in the Al alloy. Therefore, the inventors considered adding Cu, which does not affect the distribution state of the compound particles, to Al to improve the strength of the Al alloy. In this Al alloy system, Cu was actively added because the material strength can be improved by solid solution strengthening by adding Cu. In addition, although the strength can be improved by solid solution strengthening by adding Si in a similar manner, it was also found that it is effective to suppress the amount of Si added to the Al alloy because the melting point of the Al alloy decreases when a large amount of Si is added, and the Al alloy may be severely eroded by brazing during brazing. Based on the research results described above, it was discovered that by making the material stronger than conventional Al-Fe alloys while maintaining excellent electrical conductivity, it is possible to maintain the structural strength of automotive heat exchangers, which require excellent thermal conductivity and strength, and thus the present invention was arrived at.
[0007] The present invention has been made in view of the above background, and has an object to provide an aluminum alloy bare material and an aluminum alloy brazing sheet that have high electrical conductivity and excellent strength. [Means for solving the problem]
[0008] (1) The aluminum alloy bare material of the present embodiment contains, by mass%, Fe: 0.6% or more and 0.8% or less, Si: 0.4% or less, Cu: 0.6% or more and 1.0% or less, Mn: 0.2% or less, Zn: 0.3% or less, and the balance being Al and unavoidable impurities. The aluminum alloy bare material has an electrical conductivity of 54% IACS or more, and the number of Al-Fe based compound particles or Al-Fe-Si based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in a matrix is 0.3 × 10 4 ~2.4×10 4 pieces / mm 2 It is characterized in that:
[0009] (2) In the present embodiment of the aluminum alloy bare material, Heat to 600℃ and hold for 5 minutes, then cool to 300℃ at 60℃ / min.The material has an electrical conductivity of 43% IACS or more after heat treatment equivalent to that of heat exchanger brazing, and the number of Al-Fe compound particles or Al-Fe-Si compound particles with a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is 0.3 × 10 4 ~2.4×10 4 pieces / mm 2 It is preferable that:
[0010] (3) The aluminum alloy brazing sheet of this embodiment is characterized in that a core material is an alloy having the same composition as the aluminum alloy bare material for heat exchangers described in (1) or (2), and an aluminum alloy layer containing 3.0 to 12.0% by mass of Si as a brazing material, with the remainder being Al and unavoidable impurities, is bonded to one or both surfaces of the core material.
[0011] (4) In the aluminum alloy brazing sheet of the present embodiment, the brazing filler metal preferably further contains, by mass %, Zn: 2.5 to 5.0%. (5) In the aluminum alloy brazing sheet according to (3) or (4) of the present invention, the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having an equivalent circle diameter of 0.5 to 2.0 μm distributed in the core matrix is 0.3×10 4 ~2.4×10 4 pieces / mm 2 It is preferable that:
[0012] (6) In the aluminum alloy brazing sheet according to any one of (3) to (5) of the present invention, Heat to 600℃ and hold for 5 minutes, then cool to 300℃ at 60℃ / min. After heat treatment equivalent to brazing a heat exchanger, the core material has an electrical conductivity of 43% IACS or more, and the number of Al-Fe compound particles or Al-Fe-Si compound particles with a circle equivalent diameter of 0.5 to 2.0 μm distributed in the core material matrix is 0.3 × 10 4 ~2.4×10 4 pieces / mm 2 It is preferable that:
[0013] (7) In the aluminum alloy brazing sheet according to any one of (3) to (6) of the present invention, Heat to 600℃ and hold for 5 minutes, then cool to 300℃ at 60℃ / min. It is preferable that the pitting potential difference between the surface of the core material and the surface of the brazing material after the heat treatment equivalent to that of heat exchanger brazing is 80 mV or more. Effect of the Invention
[0014] The present invention can provide an aluminum alloy bare material or an aluminum alloy brazing sheet for heat exchangers that has excellent electrical conductivity and high strength. The aluminum alloy bare material or brazing sheet according to the present invention has excellent electrical conductivity and strength, and can therefore be used as an aluminum alloy bare material or brazing sheet suitable for use in automotive heat exchangers, which have been required to be further miniaturized and have high heat dissipation performance in recent years. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view showing an example of an aluminum alloy bare material according to the present invention. [Diagram 2] 1 is a partial cross-sectional view showing an example of a brazing sheet according to the present invention. [Diagram 3] FIG. 4 is a partial cross-sectional view showing another example of the brazing sheet according to the present invention. [Figure 4] FIG. 2 is a side view for explaining a joining state between the brazing sheet according to the present invention and a member to be brazed. [Diagram 5] 1 is a perspective view showing a heat exchanger configured to which a brazing sheet according to the present invention is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. Note that the drawings used in the following description may show characteristic portions in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand.
[0017] Fig. 1 shows an example of an aluminum alloy bare material according to the present invention, and Fig. 2 shows a cross-sectional structure of an aluminum alloy brazing sheet for heat exchangers of a first embodiment having a core material of the same composition as the aluminum alloy bare material shown in Fig. 1. The aluminum alloy brazing sheet A of this embodiment is in the form of a plate or sheet, and has a three-layer structure in which a first brazing material layer 2 is laminated on both the top and bottom surfaces of a core material 1 made of the same composition as the aluminum alloy bare material M shown in Fig. 1. The brazing material layer 2 may be laminated on only one side of the core material 1 as in other embodiments described later.
[0018] "Aluminum alloy bare material and core material" The core material 1 is made of an aluminum alloy bare material M containing, by mass%, Fe: 0.6% or more and 0.8% or less, Si: 0.4% or less, Cu: more than 0.6% and 1.0% or less, Mn: 0.2% or less, Zn: 0.3% or less, and the remainder being Al and unavoidable impurities. The aluminum alloy bare material M can be rolled into a plate shape as shown in Fig. 1 and used as a fin for a heat exchanger, or the aluminum alloy and the double-sided clad material can be processed into a cup shape and used as a component to be brazed by stacking them alternately. One example of the use of the aluminum alloy bare material M of this embodiment is the brazing sheet A shown in Fig. 2, which uses an alloy of the same composition as the core material 1, but it is of course possible to use it for other purposes.
[0019] The reasons for limiting the composition of the component elements contained in the aluminum alloy constituting the aluminum alloy bare material M and the core material 1 will be explained below. Fe: 0.6% or more and 0.8% or less Adding Fe to Al causes Al-Fe or Al-Fe-Si compound particles to precipitate in the aluminum alloy matrix, improving the material strength through particle dispersion strengthening. Fe also dissolves in the matrix in small amounts, improving strength through solid solution strengthening. If the Fe content is below the lower limit, the Al-Fe compound particles or Al-Fe-Si compound particles do not achieve the desired dispersion state (required number per unit area), and strength is not obtained. If the Fe content exceeds the upper limit, the number of dispersed Al-Fe compound particles or Al-Fe-Si compound particles increases more than necessary, promoting the cathodic reaction on the material surface and reducing the self-corrosion resistance of the bare material and core material.
[0020] Si: 0.4% or less Si improves the material strength of Al by dissolving in Al or by precipitating in the aluminum alloy matrix as compound particles such as Al-Fe-Si. If the Si content exceeds the upper limit, the melting point of the aluminum alloy will be lower than necessary, which may cause the bare material or core material to melt during brazing, resulting in poor brazing joints. If the Si content exceeds the upper limit, the electrical conductivity after brazing may decrease. In addition, the number of dispersed compound particles such as Al-Fe-Si particles will increase and become coarser, promoting the cathodic reaction, which may decrease the self-corrosion resistance.
[0021] Cu: More than 0.6% and not more than 1.0% Cu is added to improve the material strength of Al by dissolving in Al. If the Cu content is less than the lower limit, the desired strength cannot be obtained. If the Cu content exceeds the upper limit, the electrical conductivity after brazing decreases. If the Cu content exceeds the upper limit, a large amount of Cu is redeposited on the bare material surface or the core material surface during corrosion of the Al alloy, and the self-corrosion resistance decreases. In addition, when used as a brazing sheet, the diffusion of Cu from the core material to the brazing material becomes significant during brazing, which increases the potential of the brazing material and reduces the potential difference between the core material and the brazing material, which may reduce the sacrificial corrosion protection effect of the brazing material.
[0022] Mn: 0.2% or less It is difficult to completely eliminate Mn from the aluminum alloy when manufacturing it, so a small amount is included for manufacturing convenience. Even if a small amount of Mn is included, it significantly reduces the electrical conductivity when it dissolves in Al. However, if the Mn content is 0.2% or less, the amount of Mn dissolved in Al can be minimized by carrying out a predetermined homogenization treatment, thereby suppressing the reduction in electrical conductivity. The Mn content is preferably 0.1% or less. Zn: 0.3% or less Zn is an element that contributes to ensuring corrosion resistance, and if the Zn content exceeds 0.3%, the self-corrosion resistance of the bare material and the core material decreases. The Zn content is more preferably 0.2% or less.
[0023] "Brazing material" The reasons for limiting the composition of the component elements contained in the brazing material 2 will be explained below. Si: 3.0-12.0% Silicon is added to form a molten braze during brazing and to form a fillet at the brazed joint. If the Si content is below the lower limit, the molten brazing filler metal will be insufficient, resulting in poor brazing joinability, whereas if the Si content is above the upper limit, the molten brazing filler metal generated during brazing will be excessive, causing the core material 1 or the brazing target material to melt violently, making it impossible to maintain the shape of the heat exchanger, resulting in poor performance and impaired appearance. In addition, when a mass% range or a numerical range is expressed using "~", the lower and upper limits are included unless otherwise specified. For example, 3.0-12.0% means that the content is 3.0 mass% or more and 12.0 mass% or less.
[0024] Zn: 2.5-5.0% Zn is added to brazing filler metal to obtain the sacrificial corrosion protection effect of the core material. If more than 5.0% Zn is added, the corrosion rate of the brazing filler metal increases, and the brazing filler metal corrodes early, so the core material cannot be protected from corrosion and the corrosion resistance decreases.
[0025] "Particle size of Al-Fe compound particles or Al-Fe-Si compound particles" 0.5~2.0μm (0.5μm or more and 2.0μm or less) If the particle size (circle equivalent diameter) of the compound particles is less than 0.5 μm, the compound will re-dissolve in the matrix during brazing, lowering the electrical conductivity of the material after brazing. If the particle size is 2.0 μm or more, effective particle dispersion strengthening cannot be achieved, and the material strength will decrease, so the structural strength as a heat exchanger cannot be maintained. In addition, if there are many compound particles of 2.0 μm or more, the compounds will cause the oxide film on the aluminum surface to lose continuity, and the potential difference between the compound and the Al parent phase will increase, lowering the self-corrosion resistance.
[0026] Number of Al-Fe compound particles or Al-Fe-Si compound particles: 0.3×10 4 ~2.4×10 4 pieces / mm 2 (0.3×10 4 pieces / mm 2 More than 2.4 x 10 4 pieces / mm 2 below)" The number of compound particles is 0.3×10 4 If the number of elements is less than 1, when the amount of the element added to the material is large, most of the added element will be in a solid solution state in the matrix, and the electrical conductivity will be significantly reduced. Conversely, when the amount of the element added is small, the solid solubility is low and the number of compound particles is also small, so the material strength is low and the structural strength for applications such as heat exchangers cannot be maintained. The number of compound particles is 2.4×10 4 When the number of particles exceeds 1, the number of compounds exposed to the surface increases. The increase in the number of compound particles increases the cathodic reaction occurring on the material surface, and the self-corrosion resistance of the aluminum alloy decreases. The number of Al-Fe compound particles or Al-Fe-Si compound particles is 0.3 × 10 4 ~2.4×10 4 pieces / mm 2 The range is more preferable.
[0027] Number of Al-Fe compound particles or Al-Fe-Si compound particles after brazing: 0.3×10 4~2.4×10 4 pieces / mm 2 (0.3×10 4 pieces / mm 2 More than 2.4 x 10 4 pieces / mm 2 below)"
[0028] "Potential difference between core potential and brazing material potential" When the potential difference between the core material potential and the brazing material potential is 80 mV or more, the brazing material improves the sacrificial corrosion protection (corrosion resistance) of the core material. When the potential difference is 80 mV or less, the brazing material does not provide effective sacrificial corrosion protection, and the brazing material and the core material corrode. The fact that corrosion resistance improves when the potential difference is 80 mV or more can be confirmed, for example, by the corrosion test described below.
[0029] The corrosion test is carried out by immersing a brazed test sample, in which the brazing material and the core material are overlapped so that the core material is exposed, in OY water. The composition of OY water is 195 ppm Cl. - , 60ppmSO4 2- , 1ppmCu 2+ , 30 ppm Fe 3+ It is an aqueous solution containing The test cycle is 88°C for 8 hours, followed by 16 hours at room temperature. When heating to 88°C, the corrosive solution is stirred using a magnetic stirrer. The specific liquid volume is 16.7ml / cm 2 The sample size is adjusted so that For those with a potential difference of 80 mV or more, after four weeks of OY water testing, the core material had 0.1 pits / mm2 or less in depth. 2 The number is less than this, and the corrosion resistance is good. Therefore, if the potential difference between the core material and the brazing material is 80 mV or more, the brazing sheet is less susceptible to pitting corrosion and can be provided as a brazing sheet with excellent corrosion resistance.
[0030] "Manufacturing method" For example, aluminum alloys for bare materials, core materials, and brazing materials are cast by semi-continuous casting. An aluminum alloy that can be used for bare material and core material has a composition restricted to the following, by mass percentage: Fe: 0.6% or more and 0.8% or less, Si: 0.4% or less, Cu: 0.6% or more and 1.0% or less, Mn: 0.2% or less, Zn: 0.3% or less, with the remainder being Al and unavoidable impurities, and bare material and core material can be manufactured using this aluminum alloy. An aluminum alloy for brazing filler metal can contain, by mass%, 3.0 to 12.0% Si, and optionally 2.5 to 5.0% Zn, with the remainder being Al and unavoidable impurities. Brazing filler metal can be produced from this aluminum alloy.
[0031] "Homogenization treatment" The obtained bare material and aluminum alloy for core material can be subjected to homogenization treatment at 400°C to 600°C for 3 to 12 hours. By selecting the appropriate temperature and time, it is possible to obtain the desired properties of high electrical conductivity and optimal dispersion of compound particles in the matrix.
[0032] For the brazing material, in order to improve machinability, a homogenization treatment may be performed under conditions selected from the ranges of 400° C. to 500° C. and a treatment time of 1 to 10 hours.
[0033] "Pasting" When used as a brazing sheet, it can be produced by combining it appropriately on one or both sides of a sheet-shaped or plate-shaped core material with a cladding ratio of brazing material:core material=5-15%:85-95%.When used on both sides, the brazing sheet can be produced by combining it with a cladding ratio of skin material:core material:skin material=5-15%:70-90%:5-15%. There are no particular limitations on the preparation of the brazing material, and it can be prepared under the conditions for preparing the brazing material when manufacturing a general brazing sheet. After homogenization, the surface is machined, rolled to the desired thickness by hot rolling, cut to a specified length, and bonded to the core material.
[0034] "Hot rolling, cold rolling, annealing" Bare aluminum alloys and materials combining core and skin materials can be hot rolled (or clad rolled) using a hot rolling mill to produce bare materials and brazing sheets. After hot rolling, cold rolling can be performed to a predetermined thickness. In this case, annealing may be performed during cold rolling to continue rolling. The thickness of the bare material and the final material as the brazing sheet is not particularly limited, but the reduction ratio from the thickness finished by hot rolling and the thickness annealed for continuing rolling to the final thickness is preferably 20 to 99%. In addition, annealing may be performed after cold rolling to achieve O temper. Annealing may be performed by performing heat treatment at 200°C to 500°C for 1 to 10 hours using a batch annealing furnace, for example.
[0035] The aluminum alloy bare material M produced according to the steps described above or the aluminum alloy brazing sheet A having the configuration shown in FIG. 2 is used for the purpose of brazing by placing it for about 1 to 30 minutes in an inert gas atmosphere at a brazing temperature in the range of, for example, about 590 to 620°C when producing a heat exchanger or the like. For example, it is used in assembling heat exchangers by laminating it with brazing target components such as fins and tubes of various heat exchangers or cup-shaped bodies, and after assembling the fins, tubes, or cup-shaped bodies, the whole is heated to the brazing temperature to melt the brazing material 2 of the aluminum alloy brazing sheet A, and then cooled to room temperature to form a fillet and complete the brazing. Alternatively, components such as fins and tubes of a heat exchanger can be directly formed with the brazing sheet and used for brazing. The workpiece to be brazed may be a bare aluminum alloy material M shown in FIG.
[0036] FIG. 3 shows a brazing sheet B obtained by cladding and rolling a brazing material 2 on only one side of a core material 1, and FIG. 4 is an explanatory diagram showing the state in which this brazing sheet B is used to braze a brazing target member 3 such as a fin. Brazing is completed by brazing the brazing sheet B and the brazing target member 3 shown in FIG. 4 under the brazing conditions described above.
[0037] The bare material M and brazing sheets A and B have high electrical conductivity, and are strong enough to maintain the structure of heat exchangers, which require high strength, and are also corrosion resistant. Therefore, they can be provided as bare materials and brazing sheets suitable for use in automotive heat exchangers, which have been required to be further miniaturized and have higher heat dissipation performance in recent years. The brazing material 2 may have a multi-layer structure, such as a two-layer structure including a first brazing material 2A and a second brazing material 2B as shown by the two-dot chain line in FIG. 4, or another multi-layer structure.
[0038] 5 shows an aluminum heat exchanger 5 in which fins 6 are formed using the brazing sheet A or brazing sheet B, and an aluminum alloy tube 7 is used as the brazing target component. The fins 6 and tubes 7 can be combined with a reinforcing material 8 and a header plate 9, and brazed to obtain the aluminum heat exchanger 5 for automotive use, etc. The bare material M and the brazing sheets A and B described above have excellent electrical conductivity and high strength, and therefore can be used in automotive heat exchangers, which have been required to be further miniaturized and have high heat dissipation performance in recent years, and can provide automotive heat exchangers, which are being made smaller and have high heat dissipation performance.
[0039] The brazing sheet can be used for various purposes such as forming fins of heat exchangers, forming tubes, forming header pipes, and other heat exchanger components. In such cases, various laminated structures can be adopted depending on the application, such as a single-sided brazing material type, a double-sided brazing material type, a structure combined with a sacrificial material, or a multi-layer structure combined with an intermediate material. EXAMPLES
[0040] Each aluminum alloy was produced by semi-continuous casting so as to have the composition of Alloy No. A1 to A28 shown in Tables 1 and 2. The obtained aluminum alloy ingots were subjected to homogenization annealing (homogenization treatment) under the conditions (temperature (°C) x time (h)) shown in Tables 1 and 2, and then hot rolled and cold rolled to a thickness of 1.0 mm so as to have a rolling reduction of 85%. Then, annealing was performed at 350°C for 5 hours to produce the target aluminum alloy bare samples. Additionally, sample brazing sheets were prepared by combining the aluminum alloys of each alloy number listed in Tables 1 and 2 as core materials with the brazing filler metals of the compositions shown in Tables 3 and 4 by clad rolling. At this time, the brazing filler metal was laminated to one side of the core material by clad rolling so that the clad ratio was 10%, and then hot-rolled and cold-rolled to a thickness of 1.0 mm so that the reduction ratio was 85%, and annealed at 350°C for 5 hours to prepare brazing sheet samples of each number.
[0041] "Heat treatment equivalent to brazing" In order to evaluate the aluminum alloy bare material or brazing sheet used in the brazed heat exchanger alone, the bare material or brazing sheet sample was subjected to a brazing-equivalent heat treatment in a batch furnace. The conditions of the brazing-equivalent heat treatment were, although not limited to this example, heating from room temperature to 600°C, holding at 600°C for 5 minutes, and then cooling to 300°C at 60°C / min. After reaching 300°C, each sample was quickly cooled to room temperature using a fan. The obtained brazing sheet sample was subjected to the evaluation described below.
[0042] "Evaluation Method" <Electrical conductivity> The measurement was performed by a four-terminal method. A current of 500 mA was applied to the sample in a room temperature environment of 20 to 25° C., and the resistance was calculated from the voltage value, and then the electrical conductivity was calculated. <Compound particle distribution state> The cross sections parallel to the rolling direction were observed for the manufactured aluminum alloy bare material and brazing sheet core material, and for the aluminum alloy bare material and brazing sheet core material that had been subjected to heat treatment equivalent to brazing. The cross sections that had been subjected to CP processing (cross-section polishing) based on the ion milling method were observed using a field emission scanning electron microscope (FE-SEM). The circle equivalent diameter and distribution density of the compound particles were calculated based on the observed images by image analysis.
[0043] <Electrochemical polarization measurement> A 2.67% AlCl3 aqueous solution that had been thoroughly degassed with high-purity N2 gas and an electrochemical measurement cell were used, Pt was used as the working counter electrode, and the Luggin capillary and reference electrode Ag / AgCl were bypassed. The liquid temperature during the measurement was kept at 40°C. The measurement area of the brazing material surface and core material of the sample that was subjected to heat treatment equivalent to brazing was 10 mm 2 The test area was exposed to light, and the rest was masked with insulating paint. As pretreatment for the measurement area, it was immersed in 5% NaOH at 50°C for 30 seconds, washed with water, and then immersed in 30% HNO3 at room temperature for 1 minute and washed with water. After holding the specimen at the natural potential for about 5 minutes, the potential was swept from the natural potential at a rate of 0.5 mV / s. The bending point (the region where the current suddenly stops flowing (passivation region) and the region where the current suddenly starts flowing) observed after a constant sweep of the polarization curve was determined as the pitting potential. In addition, since no bending point was observed in specimens containing a large amount of Zn, a bending potential of 0.1 mA / cm was used. 2 The potential was determined as the pitting potential.
[0044] "Strength" After brazing, JIS No. 5 test pieces were prepared from the aluminum alloy bare material and brazing sheet parallel to the rolling direction, and tensile tests were carried out on three samples of each. The average strength was judged as excellent (◎) for ultimate tensile strength (TS) of 130 MPa or more, good (○) for 115 MPa or more and less than 130 MPa, and passable (△) for less than 115 MPa.
[0045] Tables 1 and 2 show the composition of the bare aluminum alloy materials No. A1 to A28 used in the evaluation of each test, the temperature (℃) and time (h) of the homogenization treatment, the electrical conductivity (%IACS) before and after brazing, and the number of compound particles (×10 4 pieces / mm 2 ), strength after brazing (MPa), and the results of the strength evaluation after brazing are shown. Tables 3 and 4 show the brazing sheets of alloys B1 to B29 used in the evaluation of each test, the core alloy numbers used (corresponding to the aluminum alloy numbers shown in Tables 1 and 2), the results of measuring the electrical conductivity of the brazing sheets before and after brazing, the results of measuring the number of compound particles before and after brazing, the strength after brazing, the results of the strength evaluation after brazing, the core material potential after brazing, the brazing material potential after brazing, and the potential difference after brazing. In addition, in each column of Tables 1 and 2, the notation "-" indicates that the corresponding component is not contained (less than the measurement limit).
[0046] [Table 1]
[0047] [Table 2]
[0048] [Table 3]
[0049] [Table 4]
[0050] The aluminum alloy bare materials of alloy Nos. A1 to A18 shown in Table 1 contain, by mass%, Fe: 0.6% or more and 0.8% or less, Si: 0.4% or less, Cu: 0.6% or more and 1.0% or less, Mn: 0.2% or less, Zn: 0.3% or less, and the balance being Al and unavoidable impurities. They have an electrical conductivity of 54% IACS or more, and the number of Al-Fe compound particles or Al-Fe-Si compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is 0.3 × 10 4 ~2.4×10 4 pieces / mm 2 The aluminum alloy bare material is characterized in that
[0051] The aluminum alloy bare materials of alloy Nos. A1 to A18 shown in Table 1 showed excellent electrical conductivity of 54% IACS or more (54 to 62% IACS) before brazing and 43% IACS or more (43 to 57% IACS) after brazing. The bare aluminum alloys of alloy No. A1 to A18 had a compound particle count of 0.4×10 4 ~2.1×10 4 pieces / mm 2 The range in which the number of compound particles after brazing is 0.3×10 4 ~2.1×10 4 pieces / mm 2 The range was shown. The aluminum alloy bare materials of Alloy Nos. A1 to A18 exhibited strength after brazing in the range of 118 to 155 MPa, and thus exhibited sufficiently high brazing strength.
[0052] The aluminum alloy bare material of alloy No. A19 shown in Table 2 has a low Fe content, so the number of compound particles before and after brazing is small, and the desired strength cannot be obtained.
[0053] The aluminum alloy bare material of alloy No. A20 has too much Fe content, which makes it easy to form huge compounds during casting, resulting in reduced self-corrosion resistance.
[0054] The aluminum alloy bare material of alloy No. A21 had a high Si content and a low melting point, so the bare material was severely corroded by the brazing material during brazing, resulting in poor molding of the heat exchanger.
[0055] The aluminum alloy bare material of alloy No. A22 has a low Cu content, and therefore has a post-brazing strength of 113 MPa, which is not sufficient to obtain the desired strength. The bare aluminum alloy No. A23 had too much Cu, so cracks occurred during casting and a satisfactory ingot could not be obtained, and the target aluminum alloy could not be manufactured. Therefore, the evaluation results shown in Table 1 could not be obtained. The aluminum alloy bare material of alloy No. A24 had too much Mn and Zn content, so its electrical conductivity was low both before and after brazing. The aluminum alloy bare material of alloy No. A25 had a low Cu content, so its strength after brazing was low.
[0056] In the case of the bare aluminum alloy material of Alloy No. A26, the homogenization temperature was too low, so the number of compound particles was small both before and after brazing, and the strength after brazing was slightly reduced. In the case of the bare aluminum alloy material of alloy No. A27, the homogenization treatment time was too short, so the number of compound particles was reduced both before and after brazing, and the strength after brazing was reduced. In the case of the bare aluminum alloy material of Alloy No. A28, the homogenization temperature was too high, so the number of compound particles decreased both before and after brazing, and the strength after brazing decreased.
[0057] The aluminum alloy bare materials No. A1 to A18 shown in Table 1 contain, by mass%, Fe: 0.6% or more and 0.8% or less, Si: 0.4% or less, Cu: 0.6% or more and 1.0% or less, Mn: 0.2% or less, Zn: 0.3% or less, and the balance is Al and unavoidable impurities. They have an electrical conductivity of 54% IACS or more, and the number of Al-Fe compound particles or Al-Fe-Si compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is 0.3 × 10 4 ~2.4×104 pieces / mm 2 The aluminum alloy bare material is characterized in that
[0058] The brazing sheets No. B1 to B23 shown in Table 3 showed excellent electrical conductivity of 54% IACS or more (54 to 60% IACS) before brazing and 43% IACS or more (43 to 54% IACS) after brazing. The brazing sheets No. B1 to B23 had a compound particle count of 0.3 × 10 4 ~2.4×10 4 pieces / mm 2 Range (0.4×10 4 ~2.1×10 4 pieces / mm 2 ), and the number of compound particles after brazing was 0.3×10 4 ~2.4×10 4 pieces / mm 2 (0.3×10 4 ~2.1×10 4 pieces / mm 2 ) range is shown. The aluminum alloys Nos. B1 to B23 exhibited high strength after brazing, with strengths in the range of 119 to 152 MPa.
[0059] The brazing sheet No. B24 shown in Table 4 has a core material of the aluminum alloy bare material No. A19 with a low Fe content, so the number of compound particles before brazing is small and the desired strength cannot be obtained.
[0060] The brazing sheet No. B25 shown in Table 4 has a core of the aluminum alloy bare material No. A20, which has too much Fe content. The bare material has a compound particle count of 2.4 × 10 4 Therefore, when the core material is exposed to a corrosive environment, the cathodic reaction occurring on the material surface increases, and the self-corrosion resistance of the core material decreases.
[0061] The brazing sheet No. B26 shown in Table 4 has a core of the aluminum alloy bare material No. A21, which has a high Si content, so the core was severely corroded by the brazing material during brazing, resulting in poor molding of the heat exchanger.
[0062] The brazing sheet No. B27 shown in Table 4 has a core material of the aluminum alloy bare material No. A22 with a low Cu content, and therefore has a post-braze strength of 114 MPa, which is not the desired strength. The brazing sheet No. B28 shown in Table 4 has a core of the aluminum alloy bare material No. A24, which has too high a Mn and Zn content, so that the electrical conductivity both before and after brazing was low. The brazing sheet No. B29 shown in Table 4 had a core of the aluminum alloy bare material No. A25 with a low Cu content, and therefore had low strength after brazing.
[0063] Therefore, according to the present invention, it is possible to provide an aluminum alloy bare material or an aluminum alloy brazing sheet for heat exchangers which has excellent electrical conductivity and high strength. Furthermore, the aluminum alloy bare material or brazing sheet according to the present invention has excellent electrical conductivity and strength, and therefore can be used as an aluminum alloy and brazing sheet suitable for use in automotive heat exchangers, which have been required to be further miniaturized and have high heat dissipation performance in recent years. [Explanation of symbols]
[0064] A, B...aluminum alloy brazing sheet, M...aluminum alloy bare material, 1...core material, 2...filler material, 3...part to be brazed (fin), 5...heat exchanger, 6...fin, 7...tube.
Claims
1. The composition contains, by mass%, Fe: 0.6% or more and 0.8% or less, Si: 0.4% or less, Cu: more than 0.6% and 1.0% or less, Mn: 0.2% or less, Zn: 0.3% or less, and the balance is Al and unavoidable impurities. The composition has an electrical conductivity of 54% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is 0.3×10 4 ~2.4 x 10 4 pieces / mm 2 1. An aluminum alloy bare material for a heat exchanger, comprising:
2. After subjecting a heat treatment equivalent to that for brazing a heat exchanger, which involves heating to 600°C, holding for 5 minutes, and then cooling to 300°C at 60°C / min, the material has an electrical conductivity of 43% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is 0.3 × 10 4 ~2.4 x 10 4 pieces / mm 2 2. The aluminum alloy bare material for heat exchangers according to claim 1,
3. 3. An aluminum alloy brazing sheet for heat exchangers, comprising the aluminum alloy for heat exchangers according to claim 1 or 2 as a core material, and an aluminum alloy layer containing, as a brazing material, 3.0 to 12.0% by mass of Si, the remainder being Al and unavoidable impurities, laminated on one or both surfaces of the core material.
4. 4. The aluminum alloy brazing sheet for heat exchangers according to claim 3, characterized in that the brazing material further contains, by mass%, Zn: 2.5 to 5.0%.
5. The core material has an electrical conductivity of 54% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the core material matrix is 0.3 × 10 4 ~2.4 x 10 4 pieces / mm 2 5. The aluminum alloy brazing sheet for heat exchangers according to claim 3 or 4,
6. After subjecting a heat treatment equivalent to brazing a heat exchanger, which involves heating to 600°C, holding for 5 minutes, and then cooling to 300°C at 60°C / min, the core material has an electrical conductivity of 43% IACS or more, and the number of Al-Fe compound particles or Al-Fe-Si compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the core material matrix is 0.3 × 10 4 ~2.4 x 10 4 pieces / mm 2 The aluminum alloy brazing sheet for heat exchangers according to any one of claims 3 to 5, characterized in that
7. An aluminum alloy brazing sheet for heat exchangers as described in any one of claims 3 to 6, characterized in that after undergoing a heat treatment equivalent to heat exchanger brazing, which involves heating to 600°C, holding for 5 minutes, and then cooling to 300°C at 60°C / min, the pitting potential difference between the core material and the brazing material surface is 80 mV or more.
Citation Information
Patent Citations
Aluminum brazing sheet
JP1992178291A
Aluminum brazing sheet
JP1992178292A
High strength and high thermal conduction aluminum alloy material, material fin for heat exchanger and method for producing the aluminum alloy material
JP2002256365A
Aluminum alloy fin material for heat exchanger and manufacturing method thereof
JP2014074198A
Aluminum alloy bus bar
JP2015025147A