Light-scattering photosensitive resin composition, color filter, and image display device
The photosensitive resin composition forms a light scattering pixel layer with optimized surface roughness and scattering particles to enhance brightness and color mixing in color filters, addressing brightness reduction and manufacturing costs associated with quantum dot-based filters.
Patent Information
- Application Number
- JP2021035126
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-13
- Filing Date
- 2021-03-05
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2041-03-05
AI Technical Summary
Existing color filters using quantum dots face issues with brightness reduction due to the introduction of a scattering layer, leading to decreased light efficiency and increased manufacturing costs, particularly affecting blue pixels.
A photosensitive resin composition is developed that forms a light scattering pixel layer with a surface roughness of 50 Å or more, containing scattering particles, an alkali-soluble resin, a photopolymerizable compound, and a photopolymerization initiator, optimized to enhance brightness and adjust scattering particle content for improved light emission.
The composition increases brightness by controlling surface roughness and scattering particle distribution, ensuring high luminance and effective color mixing, while avoiding the use of coloring agents to maintain transmission efficiency.
Smart Images

Figure 0007555853000001 
Figure 0007555853000002 
Figure 0007555853000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a light-scattering photosensitive resin composition, a color filter, and an image display device, and more particularly, to a light-scattering photosensitive resin composition, a color filter, and an image display device that can increase the brightness of light entering from a backlight unit or a quantum dot pixel layer. [Background technology]
[0002] Color filters are widely used in imaging devices, liquid crystal displays (LCDs), and the like, and their range of application is expanding.
[0003] In recent years, a pigment dispersion method using a pigment-dispersed photosensitive resin has been applied as one of the methods for implementing color filters. However, such a pigment dispersion method has problems in that the light efficiency is reduced because a part of the light irradiated from the light source is absorbed by the color filter during the process of transmitting the light through the color filter, and the color reproducibility is reduced due to the characteristics of the pigment contained in the color filter.
[0004] A color filter using quantum dots has been proposed as a solution to these problems. For example, Korean Patent Publication No. 10-2009-0036373 discloses that by replacing an existing color filter with a light-emitting layer made of quantum dot phosphor, the light-emitting efficiency can be improved and the display quality of a display device can be improved.
[0005] However, in the case of color filters containing quantum dots, the performance of the color filter may be somewhat degraded due to a decrease in the efficiency of the quantum dots, especially the efficiency of blue quantum dots, and in the case of blue quantum dots, there is a problem that the overall manufacturing cost increases due to their high cost.
[0006] Therefore, a color filter was proposed that uses a light source that emits blue light, has a red pattern layer containing red quantum dot particles, and a green pattern layer containing green quantum dot particles, and has a blue pixel layer that does not contain quantum dot particles in a position corresponding to the blue pattern layer, so that the red quantum dot particles emit red light and the green quantum dot particles emit green light, and the blue pixel layer allows the blue light to pass through, resulting in a blue color.
[0007] However, in the case of blue, direct light occurs, making it difficult to achieve clear color mixing. To solve this problem, a technology has been developed to introduce a scattering layer into the blue pixel layer for the purpose of scattering light. However, the introduction of a scattering layer causes a problem of reduced luminance. Therefore, there is a need to develop a photosensitive resin composition to improve the efficiency of blue pixels. Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a light-scattering photosensitive resin composition capable of improving the problem of brightness reduction caused by the introduction of a scattering layer.
[0009] Another object of the present invention is to provide a light-scattering pixel layer formed from the photosensitive resin composition.
[0010] It is still another object of the present invention to provide a color filter including the light-scattering pixel layer.
[0011] It is a further object of the present invention to provide an image display device comprising the above color filter. [Means for solving the problem]
[0012] On the other hand, the present invention is A photosensitive resin composition for forming a light-scattering pixel layer, The photosensitive resin composition includes scattering particles, an alkali-soluble resin, a photopolymerizable compound, a photopolymerization initiator, and a solvent, The light-scattering pixel layer formed from the photosensitive resin composition has a surface roughness of 50 Å or more.
[0013] In one embodiment of the present invention, the light-scattering pixel layer formed from the photosensitive resin composition may have a luminance of 60% or more relative to a light source based on a thickness of 10 μm.
[0014] In one embodiment of the invention, the light source may be a blue light source.
[0015] In one embodiment of the present invention, the wavelength of the blue light source may be in the range of 380 nm to 530 nm.
[0016] In an embodiment of the present invention, the scattering particles may satisfy the following mathematical formula 1:
[0017]
number
[0018] In one embodiment of the present invention, the alkali-soluble resin may have a substituent derived from glycidyl (meth)acrylate, and the repeating unit having the substituent derived from glycidyl (meth)acrylate may be contained in an amount of 10 to 50 mol % relative to 100 mol % of the total repeating units constituting the alkali-soluble resin.
[0019] In one embodiment of the present invention, the repeating unit having a substituent derived from glycidyl (meth)acrylate may be a repeating unit represented by the following Chemical Formula 1.
[0020] [ka]
[0021] In the above formula, Ra and Rb are each independently hydrogen or methyl.
[0022] In one embodiment of the present invention, the photoinitiator may have a maximum absorption wavelength (λmax) at a wavelength of 360 nm or less.
[0023] On the other hand, the present invention provides a light-scattering pixel layer formed from the photosensitive resin composition.
[0024] On the other hand, the present invention provides a color filter comprising the light-scattering pixel layer.
[0025] On the other hand, the present invention provides an image display device comprising the above-mentioned color filter. Effect of the Invention
[0026] The photosensitive resin composition according to the present invention can increase the brightness of the light-scattering pixel layer by controlling the surface roughness of the light-scattering pixel layer to 50 Å or more. In addition, since the photosensitive resin composition according to the present invention can increase the brightness, it is easy to adjust the content of scattering particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] The present invention will now be described in more detail.
[0028] One embodiment of the present invention is a photosensitive resin composition for forming a light-scattering pixel layer, comprising: scattering particles (A), an alkali-soluble resin (B), a photopolymerizable compound (C), a photopolymerization initiator (D), and a solvent (E), The light-scattering pixel layer formed from the photosensitive resin composition has a surface roughness of 50 Å or more.
[0029] The surface roughness means an arithmetic average roughness Ra. In the present invention, the method for measuring the surface roughness of the light-scattering pixel layer is not particularly limited, and may be measured by, for example, the method presented in the experimental examples described later.
[0030] In one embodiment of the present invention, the surface roughness of the light-scattering pixel layer is adjusted to 50 Å or more, for example, in the range of 50 Å to 300 Å, thereby improving the total reflection of light entering from a backlight unit and increasing the brightness. If the surface roughness of the light-scattering pixel layer is less than 50 Å, the brightness of the light-scattering pixel layer may decrease.
[0031] The surface roughness of the light-scattering pixel layer can be adjusted by appropriately changing the types and compositions of the components contained in the photosensitive resin composition described below.
[0032] The light-scattering pixel layer formed from the photosensitive resin composition is characterized in that the luminance of the pixel layer is 60% or more relative to a light source based on a thickness of 10 μm.
[0033] The light source may be a blue light source, and the wavelength of the blue light source may be in the range of 380 nm to 530 nm.
[0034] When the luminance is 60% or more, it is advantageous for adjusting the color mixing balance between the light-scattering pixel layer and the red pixel layer and / or the green pixel layer.
[0035] Scattered particles (A) In one embodiment of the present invention, the scattering particles serve to increase the path of light emitted from a light source, thereby improving overall light efficiency.
[0036] The photosensitive resin composition of the present invention containing the scattering particles can be suitably used to act as a blue pixel by a blue light source, and if a colorant other than the scattering particles is contained, a problem of reduced transmission efficiency of blue light generated from the light source may occur. Therefore, it is preferable that the photosensitive resin composition of the present invention does not contain a colorant other than the scattering particles. In the present invention, the scattering particles include a metal oxide.
[0037] The metal oxide may comprise an oxide of one or more metals selected from the group consisting of Li, Be, B, Na, Mg, Al, Si, K, Ca, Sc, V, Cr, Mn, Fe, Ni, Cu, Zn, Ga, Ge, Rb, Sr, Y, Mo, Cs, Ba, La, Hf, W, Tl, Pb, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Ti, Sb, Sn, Zr, Nb, Ce, Ta, In, and combinations thereof.
[0038] For example, the metal oxide may include one or more selected from the group consisting of Al2O3, SiO2, ZnO, ZrO2, BaTiO3, TiO2, Ta2O5, Ti3O5, ITO, IZO, ATO, ZnO-Al, Nb2O3, SnO, MgO, and combinations thereof. If necessary, a material that has been surface-treated with a compound having an unsaturated bond, such as an acrylate, may also be used.
[0039] The scattering particles may satisfy the following mathematical formula 1:
[0040]
number
[0041] That is, the content of scattering particles having a particle size of 100 nm or more may be equal to or greater than the content of scattering particles having a particle size of less than 100 nm. When the content of scattering particles having a particle size of 100 nm or more and the content of scattering particles having a particle size of less than 100 nm satisfy the above mathematical formula 1, the scattering effect is increased, which is advantageous in performing the role of a blue pixel layer.
[0042] The scattering particles may have a limited average particle size and a limited content in the entire composition so that the luminous intensity of the color filter can be maximized.
[0043] In the present invention, the "average particle size" may refer to the number-average particle size, and can be determined, for example, from an image observed by a field emission scanning electron microscope (FE-SEM) or a transmission electron microscope (TEM). Specifically, it can be obtained by extracting several samples from the observation image of the FE-SEM or TEM, measuring the diameters of these samples, and calculating the arithmetic average value.
[0044] For example, the metal oxide contained in the scattering particles of the present invention may have an average particle size in the range of 30 to 500 nm, preferably 30 to 300 nm. When the average particle size of the metal oxide satisfies the above range, the scattering effect is increased, and the photosensitive resin composition containing the scattering particles can perform the role of blue pixels by a blue light source, which is preferable. In addition, the development of sinking in the composition can be suppressed to obtain a surface of uniform quality, so the average particle size may be appropriately adjusted within the above range.
[0045] The scattering particles may be contained in the range of 0.1 to 50% by weight, preferably 0.5 to 30% by weight, and more preferably 0.5 to 20% by weight, based on 100% by weight of the total solid content in the photosensitive resin composition. When the scattering particles are contained within the above range, it is advantageous that a scattering pixel having excellent luminous intensity can be manufactured. Specifically, when the scattering particles are contained within the above range, it is advantageous that the desired luminous intensity can be easily secured and the deterioration of the stability of the composition can be suppressed. Meanwhile, the photosensitive resin composition of the present invention can be used to perform the role of a blue pixel by a blue light source when cured, and if a colorant other than the scattering particles is included, there may be a problem that the transmittance efficiency of blue light emitted from the light source is reduced.
[0046] Therefore, the present invention is characterized in that it does not contain any colorant other than the scattering particles.
[0047] Alkali-soluble resin (B) The alkali-soluble resin has reactivity due to the action of light or heat and alkali solubility, and acts as a dispersion medium for solid matters such as scattering particles, thereby performing the function of a binder resin.
[0048] Specifically, the alkali-soluble resin has a substituent derived from glycidyl (meth)acrylate, and the repeating unit having the substituent derived from glycidyl (meth)acrylate is preferably contained in an amount of 10 to 50 mol % relative to 100 mol % of the total repeating units constituting the alkali-soluble resin, from the viewpoint of controlling the surface roughness of the light-scattering pixel layer.
[0049] If the repeating unit having a substituent derived from glycidyl (meth)acrylate is contained in an amount of less than 10 mol % relative to 100 mol % of the total repeating units constituting the alkali-soluble resin, the taper angle of the pattern cross section may become poor, and if it is contained in an amount of more than 50 mol %, the reflow characteristics may increase, resulting in residues and taper dragging, and the luminance of the light-scattering pixel layer may decrease.
[0050] The repeating unit having a substituent derived from glycidyl (meth)acrylate may be a repeating unit represented by the following chemical formula 1.
[0051] [ka]
[0052] In the above formula, Ra and Rb are each independently hydrogen or methyl.
[0053] The alkali-soluble resin having a substituent derived from glycidyl (meth)acrylate may be obtained by reacting a copolymer of an unsaturated carboxyl group-containing monomer and another monomer copolymerizable therewith with glycidyl (meth)acrylate.
[0054] Examples of the unsaturated carboxyl group-containing monomer include unsaturated monocarboxylic acids, unsaturated dicarboxylic acids, unsaturated tricarboxylic acids, and other unsaturated polycarboxylic acids having two or more carboxyl groups in the molecule.
[0055] Examples of the unsaturated monocarboxylic acid include acrylic acid, methacrylic acid, crotonic acid, α-chloroacrylic acid, and cinnamic acid.
[0056] Examples of the unsaturated dicarboxylic acid include maleic acid, fumaric acid, itaconic acid, citraconic acid, and mesaconic acid.
[0057] The unsaturated polycarboxylic acid may be an acid anhydride, and specific examples thereof include maleic anhydride, itaconic anhydride, and citraconic anhydride. The unsaturated polycarboxylic acid may be a mono(2-(meth)acryloyloxyalkyl)ester thereof, and examples thereof include mono(2-acryloyloxyethyl) succinate, mono(2-methacryloyloxyethyl) succinate, mono(2-acryloyloxyethyl) phthalate, and mono(2-methacryloyloxyethyl) phthalate. The unsaturated polycarboxylic acid may be a mono(meth)acrylate of a dicarboxy polymer at both ends thereof, and examples thereof include ω-carboxypolycaprolactone monoacrylate and ω-carboxypolycaprolactone monomethacrylate.
[0058] The carboxyl group-containing monomers may be used alone or in combination of two or more kinds.
[0059] Examples of other monomers copolymerizable with the carboxyl group-containing monomer include aromatic vinyl compounds such as styrene, α-methylstyrene, o-vinyltoluene, m-vinyltoluene, p-vinyltoluene, p-chlorostyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-vinylbenzyl methyl ether, m-vinylbenzyl methyl ether, p-vinylbenzyl methyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, and indene;Methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-propyl acrylate, n-propyl methacrylate, i-propyl acrylate, i-propyl methacrylate, n-butyl acrylate, n-butyl methacrylate, i-butyl acrylate, i-butyl methacrylate, sec-butyl acrylate, sec-butyl methacrylate, t-butyl acrylate, t-butyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl acrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl acrylate, 3-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, allyl acrylate, allyl methacrylate, benzyl acrylate, benzyl methacrylate, silyl unsaturated carboxylic acid esters such as cyclohexyl acrylate, cyclohexyl methacrylate, phenyl acrylate, phenyl methacrylate, 2-methoxyethyl acrylate, 2-methoxyethyl methacrylate, 2-phenoxyethyl acrylate, 2-phenoxyethyl methacrylate, methoxydiethylene glycol acrylate, methoxydiethylene glycol methacrylate, methoxytriethylene glycol acrylate, methoxytriethylene glycol methacrylate, methoxypropylene glycol acrylate, methoxypropylene glycol methacrylate, methoxydipropylene glycol acrylate, methoxydipropylene glycol methacrylate, isobornyl acrylate, isobornyl methacrylate, dicyclopentadienyl acrylate, dicyclopentadiethyl methacrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-phenoxypropyl methacrylate, glycerol monoacrylate, and glycerol monomethacrylate;Unsaturated carboxylic acid aminoalkyl esters such as 2-aminoethyl acrylate, 2-aminoethyl methacrylate, 2-dimethylaminoethyl acrylate, 2-dimethylaminoethyl methacrylate, 2-aminopropyl acrylate, 2-aminopropyl methacrylate, 2-dimethylaminopropyl acrylate, 2-dimethylaminopropyl methacrylate, 3-aminopropyl acrylate, 3-aminopropyl methacrylate, 3-dimethylaminopropyl acrylate, and 3-dimethylaminopropyl methacrylate; unsaturated carboxylic acid glycidyl esters such as glycidyl acrylate and glycidyl methacrylate; carboxylic acid vinyl esters such as vinyl acetate, vinyl propionate, vinyl butylate, and vinyl benzoate; vinyl methyl ether, vinyl ethyl ether, and alicyclic esters. unsaturated ethers such as glycidyl ether; vinyl cyanide compounds such as acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, and vinylidene cyanide; unsaturated amides such as acrylamide, methacrylamide, α-chloroacrylamide, N-2-hydroxyethyl acrylamide, and N-2-hydroxyethyl methacrylamide; unsaturated imides such as maleimide, N-phenylmaleimide, and N-cyclohexylmaleimide; aliphatic conjugated dienes such as 1,3-butadiene, isoprene, and chloroprene; and macromonomers having a monoacryloyl group or monomethacryloyl group at the end of the polymer molecular chain of polystyrene, polymethyl acrylate, polymethyl methacrylate, poly-n-butyl acrylate, poly-n-butyl methacrylate, and polysiloxane. These monomers may be used alone or in combination of two or more.
[0060] The acid value of the alkali-soluble resin is preferably in the range of 20 to 200 (KOHmg / g). When the acid value is within the above range, the solubility in a developer is improved, the non-exposed portion becomes easily dissolved, and the sensitivity is increased, and as a result, the pattern of the exposed portion remains at the time of development, improving the film remaining ratio, which is preferable. Here, the acid value is a value measured as the amount (mg) of potassium hydroxide required to neutralize 1 g of the polymer, and can usually be determined by titration with an aqueous potassium hydroxide solution.
[0061] In addition, an alkali-soluble resin having a polystyrene-equivalent weight average molecular weight (hereinafter, abbreviated as "weight average molecular weight") measured by gel permeation chromatography (GPC; using tetrahydrofuran as an eluent) of 3,000 to 200,000, preferably 5,000 to 100,000, is preferred. When the molecular weight is within the above range, the hardness of the coating film is improved, the residual film rate is high, the solubility of the non-exposed portion in the developer is excellent, and the resolution tends to be improved, which is preferable.
[0062] The molecular weight distribution of the alkali-soluble resin (B) [weight average molecular weight (Mw) / number average molecular weight (Mn)] is preferably in the range of 1.5 to 6.0, more preferably in the range of 1.8 to 4.0. When the molecular weight distribution [weight average molecular weight (Mw) / number average molecular weight (Mn)] is in the range of 1.5 to 6.0, it is preferable because the developability is excellent.
[0063] The alkali-soluble resin (B) may be contained in a range of usually 5 to 85% by weight, preferably 10 to 80% by weight, more preferably 50 to 75% by weight, based on 100% by weight of the total solid content in the photosensitive resin composition. When the alkali-soluble resin (B) is contained within the above range, the solubility in the developer is sufficient, development residues are unlikely to occur on the substrate in non-pixel areas, and film reduction in pixel areas of exposed areas is unlikely to occur during development, which tends to improve leakage properties in non-pixel areas, which is preferable.
[0064] Photopolymerizable compound (C) The photopolymerizable compound contained in the photosensitive resin composition of the present invention is a compound that can be polymerized by the action of light and a photopolymerization initiator described later, and examples of the photopolymerizable compound include monofunctional monomers, bifunctional monomers, and other polyfunctional monomers.
[0065] The type of the monofunctional monomer is not particularly limited, and examples thereof include nonylphenylcarbitol acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-ethylhexylcarbitol acrylate, 2-hydroxyethyl acrylate, and N-vinylpyrrolidone.
[0066] The type of the bifunctional monomer is not particularly limited, and examples thereof include 1,6-hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, bis(acryloyloxyethyl)ether of bisphenol A, and 3-methylpentanediol di(meth)acrylate.
[0067] The type of the polyfunctional monomer is not particularly limited, and examples thereof include trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, ethoxylated dipentaerythritol hexa(meth)acrylate, propoxylated dipentaerythritol hexa(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0068] Commercially available examples of the photopolymerizable compound include Miramer M600 manufactured by Miwon Specialty Chemicals, but are not limited thereto.
[0069] The photopolymerizable compound may be contained in the range of 5 to 60% by weight, preferably 10 to 50% by weight, relative to 100% by weight of the total solid content in the photosensitive resin composition. When contained within the above range, it has an advantage in terms of strength and smoothness of the pixel portion.
[0070] If the photopolymerizable compound is contained in an amount less than the above range, the strength of the coating film may be slightly reduced, and if the photopolymerizable compound is contained in an amount exceeding the above range, the smoothness may be slightly reduced. Therefore, it is preferable that the photopolymerizable compound is contained within the above range.
[0071] Photoinitiator (D) In one embodiment of the present invention, the photopolymerization initiator may be any photopolymerization initiator that is generally used in photosensitive resin compositions.
[0072] For example, the photopolymerization initiator may be an acetophenone-based, benzophenone-based, triazine-based, thioxanthone-based, oxime-based, benzoin-based, or biimidazole-based compound.
[0073] Examples of acetophenone compounds include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, and oligomers of 2-hydroxy-2-methyl[4-(1-methylvinyl)phenyl]propan-1-one. Of these, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one may preferably be used.
[0074] Examples of the benzophenone compounds include benzophenone, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, 4,4'-bis(dimethylamino)benzophenone, and 4,4'-bis(diethylamino)benzophenone.
[0075] The triazine compounds include 2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(3',4'-dimethoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4'-methoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine, 2-biphenyl-4,6-bis(trichloromethyl)-s-triazine, bis(trichloromethyl)-6-styryl-s-triazine, 2-(naphtho 1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, 1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl(piperonyl)-6-triazine, 2,4-trichloromethyl(4'-methoxystyryl)-6-triazine, and the like. Examples of thioxanthone compounds include 2-isopropylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, and 1-chloro-4-propoxythioxanthone.
[0076] Examples of oxime compounds include o-ethoxycarbonyl-α-oxyimino-1-phenylpropan-1-one, and representative commercially available products include Irgacure OXE 01 and OXE 02 manufactured by BASF. Examples of the benzoin compounds include benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, and benzyl dimethyl ketal.
[0077] Examples of biimidazole compounds include 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2,3-dichlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(alkoxyphenyl)biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(trialkoxyphenyl)biimidazole, and imidazole compounds in which the phenyl groups at the 4,4',5,5' positions are substituted with carboalkoxy groups.
[0078] In particular, from the standpoint of controlling the surface roughness of the light-scattering pixel layer, it is preferable that the light-scattering pixel layer has a maximum absorption wavelength (λmax) at a wavelength of 360 nm or less.
[0079] Specifically, examples of photopolymerization initiators having a maximum absorption wavelength (λmax) value of 360 nm or less include 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(o-benzoyloxime) (trade name: Irgacure OXE-01), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (trade name: Irgacure 369), and the like.
[0080] The photopolymerization initiator may be used in the range of 0.01 to 10 wt%, preferably 0.01 to 5 wt%, based on 100 wt% of the solid content in the photosensitive resin composition. This content range is determined in consideration of the photopolymerization rate of the photopolymerizable compound and the physical properties of the final coating film. If the content of the photopolymerization initiator is less than the range, the polymerization rate is low, which may lengthen the overall process time, and conversely, if the content exceeds the range, an excessive reaction may cause an excessive crosslinking reaction, which may result in a decrease in the physical properties of the coating film. Therefore, the photopolymerization initiator is appropriately used within the range.
[0081] In addition, a photopolymerization initiator assistant may be used together with the photopolymerization initiator, and using the photopolymerization initiator assistant together with the photopolymerization initiator is preferable because the photosensitive resin composition becomes more sensitive and the productivity is improved. As the photopolymerization initiator assistant, preferably, one or more compounds selected from the group consisting of amines and carboxylic acid compounds may be used.
[0082] Such a photopolymerization initiator assistant is usually used in an amount of 10 mol or less, preferably in the range of 0.01 to 5 mol, per mol of the photopolymerization initiator. When the photopolymerization initiator assistant is used within the above range, the polymerization efficiency can be increased, and the effect of improving productivity can be expected.
[0083] Solvent (E) In one embodiment of the present invention, the type of the solvent (E) is not particularly limited as long as it allows the photosensitive resin composition to have an appropriate viscosity and can easily dissolve the remaining components, and various organic solvents used in the field of photosensitive resin compositions may be used.
[0084] Specific examples thereof include ethylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether; diethylene glycol dialkyl ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; ethylene glycol alkyl ether acetates such as methyl cellosolve acetate and ethyl cellosolve acetate; propylene glycol monomethyl ether acetate; Examples of the alkylene glycol alkyl ether acetate include alkylene glycol alkyl ether acetates such as butyl ether acetate, propylene glycol monopropyl ether acetate, methoxybutyl acetate, and methoxypentyl acetate; aromatic hydrocarbons such as benzene, toluene, xylene, and mesitylene; ketones such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, and glycerin; esters such as ethyl 3-ethoxypropionate and methyl 3-methoxypropionate; and cyclic esters such as γ-butyrolactone.
[0085] Among these solvents, from the viewpoint of coatability and drying property, preferably, an organic solvent having a boiling point of 100° C. to 200° C. may be used, more preferably, alkylene glycol alkyl ether acetates, ketones, esters such as ethyl 3-ethoxypropionate and methyl 3-methoxypropionate may be used, and even more preferably, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, cyclohexanone, ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, etc. These solvents may be used alone or in combination of two or more kinds.
[0086] The solvent may be contained in the range of usually 50 to 90% by weight, preferably 50 to 85% by weight, based on 100% by weight of the entire photosensitive resin composition. When the content of the solvent satisfies the above range, the coating property tends to be good when the composition is coated with a coating device such as a roll coater, a spin coater, a slit and spin coater, a slit coater (sometimes called a die coater), or an inkjet, which is preferable.
[0087] Additives (F) The photosensitive resin composition according to one embodiment of the present invention may further contain an additive (F) in addition to the above-mentioned components, if necessary.
[0088] The type of the additive (F) may be determined according to the needs of the user, and is not particularly limited in the present invention. For example, the additive (F) may include a filler, another polymer compound, a thermosetting agent, a surfactant, an adhesion promoter, an antioxidant, and an anti-aggregation agent.
[0089] Examples of the filler include glass, silica, and alumina.
[0090] Specific examples of the other polymer compounds include thermosetting resins such as epoxy resins and maleimide resins, and thermoplastic resins such as polyvinyl alcohol, polyacrylic acid, polyethylene glycol monoalkyl ether, polyfluoroalkyl acrylate, polyester, and polyurethane.
[0091] Examples of the surfactant include polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, polyethylene glycol diesters, sorbitan fatty acid esters, fatty acid modified polyesters, tertiary amine modified polyurethanes, and polyethyleneimines. Other product names include KP (manufactured by Shin-Etsu Chemical Co., Ltd.), POLYFLOW (manufactured by Kyoeisha Chemical Co., Ltd.), EFTOP (manufactured by Tohchem Products Co., Ltd.), MEGAFAC (manufactured by Dainippon Ink and Chemicals, Inc.), Flourad (manufactured by Sumitomo 3M Limited), Asahi guard, Surflon (all manufactured by Asahi Glass Co., Ltd.), SOLSPERSE (manufactured by Zeneca Corporation), EFKA (manufactured by EFKA Chemicals), and PB821 (manufactured by Ajinomoto Co., Inc.).
[0092] Examples of the adhesion promoter include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.
[0093] Specific examples of the antioxidant include 2,2'-thiobis(4-methyl-6-t-butylphenol) and 2,6-di-t-butyl-4-methylphenol.
[0094] Specific examples of the anti-aggregation agent include sodium polyacrylate.
[0095] Among these additives, those skilled in the art may appropriately add additives whose contents are not exemplified within the range that does not impair the effects of the present invention. For example, the additives may be used in the range of 0.05 to 10% by weight, preferably 0.1 to 10% by weight, more preferably 0.1 to 5% by weight, based on 100% by weight of the total photosensitive resin composition, but are not limited thereto.
[0096] According to an embodiment of the present invention, the additive may include an antioxidant. When the antioxidant is further included, there is an advantage that an effect of preventing thermal aging during post-baking in a process for forming a cured product can be expected.
[0097] The antioxidant may include at least one selected from the group consisting of phosphorus-based antioxidants, sulfur-based antioxidants, and phenol-based antioxidants, and in this case, yellowing that may occur due to a light source after the display is manufactured can be suppressed. The antioxidant may be a combination of a phenol-phosphorus-based compound, a phenol-sulfur-based compound, a phosphorus-sulfur-based compound, or a phenol-phosphorus-sulfur-based compound.
[0098] The type of the phenol-based antioxidant is not particularly limited, and specific examples thereof include 3,9-bis[2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethoxy]-2,4,8,10-tetraoxaspiro[5.5]undecane, pentaerythrityl tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 1,3,5-trimethyl-2,4,6-tris(3'5'-di-t-butyl-4-hydroxybenzyl)benzene, triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 4,4'-thiobis(6-t-butyl-3-methylphenol), tris-(3,5-di-t-butyl-4-hydroxybenzyl )-isocyanurate, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-isocyanurate, 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamic acid amide), 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 2,4-bis[(octylthio)methyl]-O-cresol, 1,6-hexanediol-bis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], octadecyl Examples of such hydroxyphenols include 3-(3,5-di-tert-butyl-4-hydroxyphenol)propionate, 2,2'-methylenebis(4-methyl-6-t-butylphenol), 4,4'-butylidene-bis(3-methyl-6-t-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,1,5-tris(4-hydroxybenzyl)benzene, and tetrakis[methylene-3-(3,5'-di-t-butyl-4'-hydroxyphenylpropionate)]methane.
[0099] Among these phenolic antioxidants, the following are particularly recommended from the viewpoints of heat resistance and prevention of heat-induced discoloration: 3,9-bis[2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethoxy]-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3,5-trimethyl-2,4,6-tris(3'5'-di-t-butyl-4-hydroxybenzyl)benzene, pentaerythrityl tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 4,4'-thiobis(6-t-butyl-3-methylphenol), tris -(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-isocyanurate, 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamic acid amide), 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, and 2,4-bis[(octylthio)methyl]-O-cresol are preferred.
[0100] Commercially available products include Irganox 1010 (manufactured by BASF), Sumilizer BBM-S (manufactured by Sumitomo Chemical), ADK STAB AO-80 (manufactured by ADEKA), Sumilizer GP (manufactured by Sumitomo Chemical), and Irganox 1035 (manufactured by BASF).
[0101] The type of the phosphorus-based antioxidant is not particularly limited, and specific examples thereof include 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, diisodecylpentaerythritol diphosphite, bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, 2,2'-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphite, and the like. HORASU, 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butylde-benz[d,f][1,3,2]dioxaphosphepine, triphenyl phosphite, diphenyl isodecyl phosphite, phenyl diisodecyl phosphite, 4,4'-butylidene-bis(3-methyl-6-t-butylphenylditridecyl)phosphite, octadecyl phosphite, tris(nonylphenyl)phosphite, 9,10- Dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(3,5-di-t-butyl-4-hydroxybenzyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-decyloxy-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, tris(2,4-di-t-butylphenyl)phosphite, cyclic neopentanetetraylbis(2,4-di-t-butylphenyl)phosphite sphite, cyclic neopentanetetraylbis(2,6-di-t-butylphenyl)phosphite, 2,2-methylenebis(4,6-di-t-butylphenyl)octylphosphite, tris(2,4-di-t-butylphenyl)phosphite, tetrakis(2,4-di-t-butylphenyl)[1,1-biphenyl]-4,4'diylbisphosphonite, bis[2,4-bis(1,1-dimethylethyl)-6-methylphenyl]ethyl ester, and phosphonic acid.
[0102] Among these phosphorus-based antioxidants, from the standpoint of heat resistance and prevention of heat discoloration, 2,2'-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, and 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenz[d,f][1,3,2]dioxaphosphepine, etc. are preferred.
[0103] The type of the sulfur-based antioxidant is not particularly limited, and specific examples include 2,2-bis({[3-(dodecylthio)propionyl]oxy}methyl)-1,3-propanediyl-bis[3-(dodecylthio)propionate], 2-mercaptobenzimidazole, dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, pentaerythrityl-tetrakis(3-laurylthiopropionate), and 2-mercaptobenzimidazole.
[0104] Among these sulfur-based antioxidants, 2,2-bis({[3(dodecylthio)propionyl]oxy}methyl)-1,3-propanediyl-bis[3-(dodecylthio)propionate], 2-mercaptobenzimidazole, and the like are preferred from the standpoint of heat resistance and prevention of heat discoloration.
[0105] The antioxidant may be contained in the range of 0.1 to 30% by weight, preferably 0.5 to 20% by weight, based on 100% by weight of the total solid content in the photosensitive resin composition according to the present invention. When the content of the antioxidant satisfies the above range, it is advantageous in terms of solving the problem of brightness reduction. One embodiment of the present invention relates to a light-scattering pixel layer formed from the above-described photosensitive resin composition.
[0106] In addition, one embodiment of the present invention relates to a color filter including the above-mentioned light-scattering pixel layer. The color filter according to one embodiment of the present invention is characterized in that it includes a light-scattering pixel layer formed by applying the above-mentioned photosensitive resin composition on a substrate, exposing it to light in a predetermined pattern, and developing it. The pattern forming method using the photosensitive resin composition according to the present invention will be described in detail below.
[0107] The method of forming a pattern using the photosensitive resin composition according to the present invention may be a method known in the art, and typically includes a coating step, an exposure step, and a removal step. The photosensitive resin composition according to the present invention is coated on a substrate, and photocured and developed to form a pattern, so that it can be used as a light-scattering pixel layer (pixel layer for blue pixels). The light-scattering pixel layer may appear white due to scattering when light is not introduced from a light source. Specifically, the photosensitive resin composition is applied to a thickness of 2.0 to 3.4 μm on a glass substrate that is not coated with anything or a glass substrate that is coated with a SiNx (protective film) to a thickness of 500 to 1,500 Å by a suitable method such as spin coating or slit coating. After coating, light is irradiated to form a pattern required for the color filter. After light irradiation, the coating layer is treated with an alkaline developer, whereby the non-irradiated part of the coating layer dissolves and the pattern required for the color filter is formed. By repeating this process for the number of R, G, and B colors required, a color filter having a desired pattern can be obtained. In addition, in the above process, the image pattern obtained by development can be further heated or cured by exposure to actinic radiation, etc., to further improve crack resistance, solvent resistance, etc.
[0108] One embodiment of the present invention relates to an image display device including the above-mentioned color filter. The color filter according to the present invention can be applied to various image display devices such as electroluminescent displays (EL), plasma display panels (PDP), field emission displays (FED), organic light emitting diodes (OLED), and quantum dot light-emitting diodes (QLED), as well as conventional liquid crystal displays (LCD).
[0109] The image display device according to the present invention includes a configuration known in the art, except for the inclusion of the above-mentioned color filter. EXAMPLES
[0110] The present invention will be described in more detail below with reference to examples, comparative examples, and experimental examples. It will be obvious to those skilled in the art that these examples, comparative examples, and experimental examples are merely for the purpose of explaining the present invention, and the scope of the present invention is not limited thereto.
[0111] Synthesis Example 1: Synthesis of alkali-soluble resin B-1 A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was prepared. Furthermore, 100 parts by weight of a monomer consisting of 5 mol% N-benzylmaleimide, 15 mol% cyclohexyl methacrylate, 5 mol% methyl methacrylate, 20 mol% rosin methacrylate and 55 mol% acrylic acid was added with 40 parts by weight of propylene glycol monomethyl ether acetate (hereinafter also referred to as PGMEA) and stirred and mixed to prepare a monomer dropping funnel. Further, 6 parts by weight of n-dodecanediol and 24 parts by weight of PGMEA were added and stirred and mixed to prepare a chain transfer agent dropping funnel. Next, 395 parts by weight of PGMEA was introduced into the flask, and the atmosphere in the flask was replaced with nitrogen from air, and the temperature of the flask was raised to 90° C. while stirring. Next, the dropping of the monomer and the chain transfer agent from the dropping funnel was started. The dropping was continued for 2 hours while maintaining the temperature at 90° C., and after 1 hour, the temperature was raised to 110° C. and maintained for 3 hours, after which a gas inlet tube was introduced and bubbling of a mixed gas of oxygen / nitrogen=5 / 95 (v / v) was started. Next, 45 mol % of glycidyl methacrylate, 0.4 parts by weight of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts by weight of triethylamine were added to the flask relative to 100 mol % of the monomer, and the reaction was continued at 110°C for 6 hours. Thereafter, the mixture was cooled to room temperature to obtain an alkali-soluble resin having a weight average molecular weight of 11,100 and an acid value based on solid content of 70 mgKOH / g.
[0112] Synthesis Example 2: Synthesis of alkali-soluble resin B-2 A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was prepared. Furthermore, 100 parts by weight of a monomer consisting of 10 mol% N-benzylmaleimide, 25 mol% cyclohexyl methacrylate, 5 mol% methyl methacrylate, 25 mol% rosin methacrylate and 35 mol% acrylic acid was added with 40 parts by weight of propylene glycol monomethyl ether acetate (hereinafter also referred to as PGMEA) and stirred and mixed to prepare a monomer dropping funnel. Further, 6 parts by weight of n-dodecanediol and 24 parts by weight of PGMEA were added and stirred and mixed to prepare a chain transfer agent dropping funnel.
[0113] Next, 395 parts by weight of PGMEA was introduced into the flask, and the atmosphere in the flask was replaced with nitrogen from air, and the temperature of the flask was raised to 90° C. while stirring. Next, the dropping of the monomer and the chain transfer agent from the dropping funnel was started. The dropping was continued for 2 hours while maintaining the temperature at 90° C., and after 1 hour, the temperature was raised to 110° C. and maintained for 3 hours, after which a gas inlet tube was introduced and bubbling of a mixed gas of oxygen / nitrogen=5 / 95 (v / v) was started. Next, 30 mol % of glycidyl methacrylate, 0.4 parts by weight of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts by weight of triethylamine were added to the flask relative to 100 mol % of the monomer, and the reaction was continued at 110°C for 6 hours. Thereafter, the mixture was cooled to room temperature to obtain an alkali-soluble resin having a weight average molecular weight of 11,600 and an acid value based on solid content of 50 mgKOH / g.
[0114] Synthesis Example 3: Synthesis of alkali-soluble resin B-3 A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was prepared. Furthermore, 100 parts by weight of monomer consisting of 5 mol% N-benzylmaleimide, 25 mol% cyclohexyl methacrylate, 5 mol% methyl methacrylate, 40 mol% rosin methacrylate and 25 mol% acrylic acid was added with 40 parts by weight of propylene glycol monomethyl ether acetate (hereinafter also referred to as PGMEA) and stirred and mixed to prepare a monomer dropping funnel. Further, 6 parts by weight of n-dodecanediol and 24 parts by weight of PGMEA were added and stirred and mixed to prepare a chain transfer agent dropping funnel.
[0115] Next, 395 parts by weight of PGMEA was introduced into the flask, and the atmosphere in the flask was replaced with nitrogen from air, and the temperature of the flask was raised to 90° C. while stirring. Next, the dropping of the monomer and the chain transfer agent from the dropping funnel was started. The dropping was continued for 2 hours while maintaining the temperature at 90° C., and after 1 hour, the temperature was raised to 110° C. and maintained for 3 hours, after which a gas inlet tube was introduced and bubbling of a mixed gas of oxygen / nitrogen=5 / 95 (v / v) was started. Next, 15 mol % of glycidyl methacrylate, 0.4 parts by weight of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts by weight of triethylamine were added to the flask relative to 100 mol % of the monomer, and the reaction was continued at 110°C for 6 hours. Thereafter, the mixture was cooled to room temperature to obtain an alkali-soluble resin having a weight average molecular weight of 11,500 and an acid value based on solid content of 62 mgKOH / g.
[0116] Synthesis Example 4: Synthesis of alkali-soluble resin B-4 A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was prepared. Further, 100 parts by weight of a monomer consisting of 5 mol% N-benzylmaleimide, 5 mol% cyclohexyl methacrylate, 10 mol% methyl methacrylate, 10 mol% rosin methacrylate and 70 mol% acrylic acid was added with 40 parts by weight of propylene glycol monomethyl ether acetate (hereinafter also referred to as PGMEA) and stirred and mixed to prepare a monomer dropping funnel. Further, 6 parts by weight of n-dodecanediol and 24 parts by weight of PGMEA were added and stirred and mixed to prepare a chain transfer agent dropping funnel.
[0117] Next, 395 parts by weight of PGMEA was introduced into the flask, and the atmosphere in the flask was replaced with nitrogen from air, and the temperature of the flask was raised to 90° C. while stirring. Next, the dropping of the monomer and the chain transfer agent from the dropping funnel was started. The dropping was continued for 2 hours while maintaining the temperature at 90° C., and after 1 hour, the temperature was raised to 110° C. and maintained for 3 hours, after which a gas inlet tube was introduced and bubbling of a mixed gas of oxygen / nitrogen=5 / 95 (v / v) was started.
[0118] Next, 60 mol % of glycidyl methacrylate, 0.4 parts by weight of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts by weight of triethylamine were added to the flask relative to 100 mol % of the monomer, and the reaction was continued at 110°C for 6 hours. Thereafter, the mixture was cooled to room temperature to obtain an alkali-soluble resin having a weight average molecular weight of 12,300 and an acid value based on solid content of 74 mgKOH / g.
[0119] Examples and Comparative Examples: Preparation of Photosensitive Resin Composition Photosensitive resin compositions were prepared by mixing the components according to the compositions in Table 1 below (% by weight).
[0120] [Table 1]
[0121] (A) Scattering particles (white particles): TiO2 (DuPont, R102, 210 nm) (B-1) Alkali-soluble resin: Synthesis example 1 (B-2) Alkali-soluble resin: Synthesis example 2 (B-3) Alkali-soluble resin: Synthesis Example 3 (B-4) Alkali-soluble resin: Synthesis Example 4 (C-1) Photopolymerizable compound: dipentaerythritol hexaacrylate (Kayarad DPHA, manufactured by Nippon Kayaku Co., Ltd.) (D-1) Photopolymerization initiator: Irgacure OXE01 (manufactured by BASF), λmax: 327 nm (D-2) Photoinitiator: NCI-831 (ADEKA), λmax: 365nm (F-1) Antioxidant: Sumilizer GP (Sumitomo Chemical Co., Ltd.) (F-2) Epoxy resin: ESCN 195XL (Sumitomo Chemical Co., Ltd.) (F-3) Leveling agent: F-554 (DIC) (E-1) Solvent: Propylene glycol monomethyl ether acetate (PGMEA) Experimental Example: The light-scattering pixel layers were prepared using the photosensitive resin compositions prepared in the Examples and Comparative Examples as described below, and the surface roughness and luminance for a blue light source were measured as described below. The results are shown in Table 2 below.
[0122] <Manufacture of Light-Scattering Pixel Layer Substrate> A light-scattering pixel layer substrate was manufactured using the photosensitive resin compositions prepared in the Examples and Comparative Examples. That is, each of the photosensitive resin compositions was applied onto a glass substrate by spin coating, and then placed on a heating plate and maintained at 100° C. for 3 minutes to remove the solvent and form a coating film.
[0123] Next, a test photomask having a square transmission pattern of 20 mm×20 mm and a line pattern of 1 to 100 μm was placed on the coating film, and ultraviolet rays were irradiated at a distance of 100 μm from the test photomask.
[0124] At this time, an ultra-high pressure mercury lamp (product name: USH-250D) manufactured by Ushio Electric Co., Ltd. was used as the ultraviolet light source, and the irradiation was performed at 200 mJ / cm under air atmosphere. 2 The light was irradiated at an exposure dose of 100 nm (based on 365 nm), and no special optical filters were used.
[0125] The coating film irradiated with ultraviolet light was developed by immersing it in a KOH aqueous solution developer of pH 10.5. The substrate on which the coating film was formed was washed with distilled water, dried by blowing nitrogen gas, and heated in a heating oven at 230°C for 20 minutes to produce a light-scattering pixel layer substrate. The thickness of the light-scattering pixel layer thus produced was 10 μm.
[0126] (1) Surface roughness The surface roughness of the light-scattering pixel layer was measured (unit: Å) using a DEKTAK (Veeco) surface roughness measuring device.
[0127] (2) Luminance relative to blue light source A blue light emitting element was arranged on the substrate surface of the light scattering pixel layer substrate prepared using the photosensitive resin composition prepared in the Examples and Comparative Examples, and the luminance to a blue light source was measured using a luminance meter (CAS 140 CT, Instrument System Co., Ltd.) The luminance was calculated as a relative value relative to the luminance value measured when only a blue light source was placed without a light scattering pixel layer substrate and the luminance value was set to 100%.
[0128] [Table 2]
[0129] As shown in Table 2, it can be confirmed that the photosensitive resin compositions of Examples 1 to 3 in which the light-scattering pixel layer according to the present invention has a surface roughness of 50 Å or more have increased brightness to a blue light source compared to the photosensitive resin compositions of Comparative Examples 1 and 2 in which the light-scattering pixel layer has a surface roughness of less than 50 Å.
[0130] Although specific parts of the present invention have been described in detail above, it is clear to those skilled in the art that such specific descriptions are merely preferred embodiments and do not limit the scope of the present invention. Those skilled in the art will be able to make various applications and modifications within the scope of the present invention based on the above content. Therefore, the true scope of the invention is to be defined by the following claims and their equivalents.
Claims
1. A photosensitive resin composition for forming a light-scattering pixel layer, The photosensitive resin composition includes scattering particles, an alkali-soluble resin, a photopolymerizable compound, a photopolymerization initiator, and a solvent, the alkali-soluble resin has a substituent derived from glycidyl (meth)acrylate, and the repeating unit having the substituent derived from glycidyl (meth)acrylate is contained in an amount of 15 to 45 mol % relative to 100 mol % of the total repeating units constituting the alkali-soluble resin; The photopolymerization initiator has a maximum absorption wavelength (λmax) at a wavelength of 360 nm or less, A photosensitive resin composition, the light-scattering pixel layer formed from said photosensitive resin composition having a surface roughness of 50 Å or more (excluding the case where the photosensitive resin composition contains quantum dots).
2. 2. The photosensitive resin composition according to claim 1, wherein a light-scattering pixel layer formed from the photosensitive resin composition has a luminance of 60% or more relative to a light source based on a thickness of 10 μm.
3. The photosensitive resin composition according to claim 2 , wherein the light source is a blue light source.
4. The photosensitive resin composition according to claim 3, wherein the wavelength of the blue light source is in the range of 380 nm to 530 nm.
5. The photosensitive resin composition according to claim 1 , wherein the scattering particles satisfy the following mathematical formula 1: [0010]
6. The photosensitive resin composition according to claim 1 , wherein the repeating unit having a substituent derived from glycidyl (meth)acrylate is a repeating unit represented by the following chemical formula 1: 【Chemistry 1】 In the above formula, Ra and Rb are each independently hydrogen or methyl.
7. A light-scattering pixel layer formed from the photosensitive resin composition according to any one of claims 1 to 6.
8. A color filter comprising the light-scattering pixel layer of claim 7.
9. An image display device comprising the color filter according to claim 8.
Citation Information
Patent Citations
Self-luminous photosensitive resin composition, color filter and image display device manufactured using the same
JP2019537064A
Metal oxide photosensitive resin composition, color filter and image display device manufactured using the same
JP2020501176A
A color filter and an image display device comprising thereof
KR1020200023965A