Method for preparing a tissue-adhesive sheet

The method of impregnating a fibrous sheet with reactive polymer particles using an electric field addresses the inadequacies of existing bleeding control techniques by achieving rapid and effective hemostasis and tissue adhesion in surgical procedures.

JP7555981B2Active Publication Date: 2024-09-25GATT TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021577637
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-12
Filing Date
2020-07-09
Publication Date
2024-09-25
Estimated Expiration
2040-07-09

AI Technical Summary

Technical Problem

Existing surgical techniques for controlling bleeding during parenchymal tissue procedures, such as liver or kidney surgery, are inadequate, with methods like suture control and electrocautery being insufficient, necessitating the development of alternative hemostatic products.

Method used

A method for preparing tissue adhesive sheets involves providing a fibrous sheet with three-dimensional interconnected spaces and impregnating it with reactive polymer particles using an electric field to create covalent bonds with blood components, enhancing hemostasis and tissue adhesion.

Benefits of technology

The method achieves effective distribution of reactive polymer particles within the fibrous sheet, ensuring rapid blood coagulation and tissue sealing without affecting the structural integrity of the sheet, and outperforms traditional impregnation methods by using very small particles that dissolve quickly, providing superior hemostatic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555981000001
    Figure 0007555981000001
  • Figure 0007555981000002
    Figure 0007555981000002
  • Figure 0007555981000003
    Figure 0007555981000003
Patent Text Reader

Abstract

The present invention provides a method for preparing a tissue adhesive sheet that can be suitably applied as an implantable hemostatic or sealing construct during a surgical procedure, the method comprising the steps of: providing a fibrous sheet comprising three-dimensional interconnected interstitial spaces; providing reactive polymer particles comprising a water-soluble electrophilic polymer carrying at least three reactive electrophilic groups, wherein the reactive electrophilic groups are capable of reacting with amine groups in blood under the formation of covalent bonds; placing the fibrous sheet and the reactive polymer particles between two electrodes; and simultaneously subjecting the fibrous sheet and the reactive polymer particles to an electric field of 0.1 to 40 kV / mm, thereby impregnating the interconnected interstitial spaces of the fibrous sheet with the reactive polymer particles.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] [Technical field of the invention] The present invention relates to a method for preparing a tissue adhesive sheet, the method comprising: providing a fibrous sheet comprising three-dimensional interconnected void spaces; providing a reactive polymer particle comprising a water-soluble electrophilic polymer carrying at least three reactive electrophilic groups, the reactive electrophilic groups being capable of reacting with amine groups in blood under formation of covalent bonds; placing the fibrous sheet and reactive polymer particles between two electrodes; simultaneously subjecting the fibrous sheet and the reactive polymer particles to an electric field of 0.1-40 kV / mm to impregnate the reactive polymer particles into the interconnected interstitial spaces of the fibrous sheet. The present invention relates to a method comprising the steps of:

[0002] The present invention allows for efficient distribution of reactive polymer particles within the fibrous sheet and the production of a tissue-adhesive sheet with excellent adhesive properties.

[0003] [Background of the invention] One of the main challenges during surgical procedures on parenchymal tissue is to achieve control of bleeding. Suture control, electrocautery and ultrasonic sealing are often inadequate, for example during liver or kidney surgery. As a result, procedures such as liver resection or partial nephrectomy require alternative methods to control bleeding. To this end, a wide range of topical hemostatic products have been developed and are clinically available.

[0004] Boerman et al. (Next Generation Hemostatic Materials Based on NHS-Ester Functionalized Poly(2-oxazoline)s, Biomacromolecules (2017), 18, 2529-2538) describe a synthetic, non-bioactive hemostatic product obtained by coating N-hydroxysuccinimide ester (NHS)-functionalized poly(2-oxazoline)s (NHS-POx) onto gelatin patches, which acts by forming covalent crosslinks between the polymer, host blood proteins, gelatin, and tissue to seal wound sites and prevent blood loss during surgical procedures.

[0005] US Patent Application Publication No. 2010 / 0233246 describes a biocompatible polymeric device comprising a collagen sponge or sheet impregnated with a two-component reactive polyethylene glycol powder, the reactive powder comprising a first polyethylene glycol having nucleophilic groups and a second polyethylene glycol having electrophilic groups, the polyethylene glycol powder remaining non-reactive in the dry state.

[0006] US Patent Application Publication No. 2011 / 0250257 describes an anhydrous fibrous sheet comprising a first component of a fibrous polymer containing electrophilic or nucleophilic groups and a second component capable of crosslinking with the first component to form a crosslinked hydrogel adherent to biological tissue when the sheet is exposed to an aqueous medium in contact with biological tissue, the second component being either a fibrous polymer containing electrophilic groups when the first component contains nucleophilic groups, or a fibrous polymer containing nucleophilic groups when the first component contains electrophilic groups, or a second component being capable of crosslinking with the first component to form a crosslinked hydrogel adherent to biological tissue when the sheet is exposed to an aqueous medium in contact with biological tissue, the second component being either a fibrous polymer containing electrophilic groups when the first component contains nucleophilic groups, or a fibrous polymer containing nucleophilic groups when the first component contains electrophilic groups, An anhydrous fibrous sheet is described in which the component is a coating on the fibrous polymer of a first component, said coating containing electrophilic groups if the first component contains nucleophilic groups, or containing nucleophilic groups if the first component contains electrophilic groups, or a second component is a dry powder dispersed and entrapped within the interstices of the fibrous polymer of the first component, said powder containing electrophilic groups if the first component contains nucleophilic groups, or containing nucleophilic groups if the first component contains electrophilic groups.

[0007] WO 2011 / 124640 is a) providing a sponge comprising a matrix of biomaterial in dry form; b) providing one reactive polymeric material in the form of a dry powder; c) contacting a) with b) such that the material of b) is present on at least one surface of the sponge; and d) A step of adhering the material of b) to the sponge of a). The present invention describes a method for making a hemostatic sponge, comprising: Adhesion can be achieved by melting for a sufficiently long period of time.

[0008] WO 2012 / 057628 describes a tissue-adhesive medical product comprising at least 1% by weight of dry matter of electrophilically activated polyoxazoline (EL-POx), said EL-POx comprising at least two reactive electrophilic groups, including at least one pendant electrophilic group. In addition to EL-POx, the medical product may also contain nucleophilically activated polyoxazoline (NU-POx). Examples of tissue-adhesive products include adhesive tissue tapes, tissue sealants, hemostatic porous materials and implants.

[0009] WO 2016 / 056901 describes an adhesive hemostatic product selected from a coated mesh, a coated foam or a coated powder, the hemostatic product comprising: a porous solid substrate having a porosity of at least 5 vol.% and comprising an exterior surface comprising a nucleophilic polymer containing reactive nucleophilic groups; and An adherent coating covering at least a portion of a solid substrate, said coating comprising an electrophilically activated polyoxazoline (EL-POx), said EL-POx containing an average of at least one reactive electrophilic group. This application describes an adhesive hemostatic product comprising:

[0010] The adhesive hemostatic product is produced by a method that includes providing a porous solid substrate, coating the substrate with a coating solution that includes EL-POx and a solvent, and removing the solvent.

[0011] No. 6,733,845 describes a method for electrostatically impregnating a powder into a network of fibers or filaments to produce a composite comprising a rigid or flexible matrix in intimate contact with said network, by placing the powder and the network of fibers or filaments between two electrodes that are electrically isolated and insulated from each other, the electrodes being respectively connected to oppositely charged poles of an AC voltage electrostatic generator, and simultaneously subjecting the powder and the network of fibers or filaments between the electrodes to an electrostatic field having an AC voltage of at least 5 kV for at least 2 seconds.

[0012] [Summary of the invention] The present inventors have developed a method for preparing a tissue-adhesive sheet that can be suitably applied as an implantable hemostatic or sealing construct during a surgical procedure. The method of the present invention comprises: providing a fibrous sheet comprising three-dimensional interconnected void spaces; providing a reactive polymer particle comprising a water-soluble electrophilic polymer carrying at least three reactive electrophilic groups, the reactive electrophilic groups being capable of reacting with amine groups in blood under formation of covalent bonds; placing the fibrous sheet and reactive polymer particles between two electrodes; simultaneously subjecting the fibrous sheet and the reactive polymer particles to an electric field of 0.1-40 kV / mm to impregnate the reactive polymer particles into the interconnected interstitial spaces of the fibrous sheet. Includes.

[0013] When blood is absorbed by the tissue adhesive sheet of the present invention as it enters the interstitial spaces, the reactive polymer particles in the sheet begin to dissolve as soon as they are "wet" by the blood, allowing the electrophilic polymer to react with reactive nucleophilic groups in the blood and tissue, resulting in blood clotting and tissue sealing, both of which contribute to hemostasis. The hemostatic properties of the fibrous sheet containing reactive polymer particles benefit from the "deep" impregnation by the reactive polymer particles within the fibrous sheet, and their homogenous distribution. The method of the present invention allows the achievement of both desirable properties.

[0014] In addition, the method of the present invention offers the advantage that, unlike impregnation with liquids, it does not affect the structural integrity or mechanical properties of the fibrous sheet. Moreover, compared to mechanical impregnation methods that utilize shaking or vibration, the method of the present invention does not impose mechanical stress and achieves more effective impregnation, especially with very small (<100 μm) reactive polymer particles.

[0015] Another aspect of the present invention relates to a tissue adhesive sheet obtainable by the method of the present invention.

[0016] [Detailed Description of the Invention] A first aspect of the present invention provides a method for preparing a tissue adhesive sheet, said method comprising: providing a fibrous sheet comprising three-dimensional interconnected void spaces; providing a reactive polymer particle comprising a water-soluble electrophilic polymer carrying at least three reactive electrophilic groups, the reactive electrophilic groups being capable of reacting with amine groups in blood under formation of covalent bonds; placing the fibrous sheet and reactive polymer particles between two electrodes; simultaneously subjecting the fibrous sheet and the reactive polymer particles to an electric field of 0.1-40 kV / mm to impregnate the reactive polymer particles into the interconnected interstitial spaces of the fibrous sheet. The present invention relates to a method comprising the steps of:

[0017] The term "tissue adhesive" as used herein refers to the ability of a tissue adhesive sheet to adhere to tissue through the formation of covalent bonds between the sheet and the tissue. The formation of these covalent bonds typically requires the presence of water.

[0018] The term "interstitial space" as used herein refers to the void ("empty") space within the fibrous sheet. The interstitial space within the fibrous sheet allows for the introduction of reactive polymer particles into the sheet. Blood and other bodily fluids can also enter the interstitial space, thereby allowing dissolution of the water-soluble electrophilic polymer within the reactive polymer particles.

[0019] The "water-soluble electrophilic polymer carrying reactive electrophilic groups" used according to the present invention carries at least three reactive groups capable of reacting with amine groups in tissues and blood under the formation of covalent bonds. The water-soluble electrophilic polymer has a molecular weight of at least 1 kDa and a solubility in distilled water at 20° C. of at least 50 g / L.

[0020] The term "water absorption capacity" as used herein is a measure of the ability of a tissue adhesive sheet to absorb water. Water absorption capacity is measured by weighing a sample of the dry sheet (weight = W d ), and then the sample is immersed in distilled water (37°C) for 45 minutes. The sample is then removed from the water, and the water adhering to the outside of the substrate is removed, after which the sample is weighed again (weight = W w ). Water absorption capacity=100%×(W w -W d ) / W d Water absorption capacity is a measure of the porosity of a substrate and its ability to swell in the presence of water.

[0021] The term "collagen" as used herein refers to the major structural protein in the extracellular space of various connective tissues in the animal body. Collagen forms a characteristic triple helix of three polypeptide chains. Depending on the degree of mineralization, collagen tissues can be either strong (bone) or flexible (tendon) or have a gradient from strong to flexible (cartilage). Unless otherwise indicated, the term "collagen" also includes denatured collagens other than gelatin.

[0022] The term "gelatin" as used herein refers to a mixture of peptides and proteins produced by partial hydrolysis of collagen extracted from the skin, bones and connective tissues of animals such as domestic cattle, chickens, pigs and fish. During hydrolysis, the natural molecular bonds between the individual collagen strands are broken down into forms that are more easily reconstituted.

[0023] The term "polyoxazoline" as used herein refers to poly(N-acylalkyleneimine) or poly(aroylalkyleneimine), further referred to as POx. An example of POx is poly(2-ethyl-2-oxazoline). The term "polyoxazoline" also encompasses copolymers of POx.

[0024] The reactive polymer particles may be homogeneously distributed within the interstitial spaces of the fibrous sheet, in the sense that the particle density is substantially the same throughout the sheet. The reactive polymer particles may also be non-uniformly distributed through the thickness of the sheet. In certain applications, it may be advantageous for the reactive polymer particles to exhibit a gradient in density, for example, in that the density of the reactive polymer particles is lowest near the side of the sheet that is intended to be applied to the bleeding wound and highest near the opposite side of the sheet.

[0025] The diameter distribution of reactive polymer particles may be determined by laser diffraction, preferably using a Malvern Mastersizer 2000 in combination with a Stainless Steel Sample Dispersion Unit. The sample dispersion unit is filled with approximately 120 ml of cyclohexane and the unit is allowed to stabilize for 5-10 minutes at a stirring speed of 1800 rpm, after which a background measurement (blank measurement) is taken. The sample tube is shaken and rotated horizontally 20 times. Approximately 50 mg is then dispersed in the sample dispersion unit containing cyclohexane. Once the sample is introduced into the dispersion unit, it is stirred at 1800 rpm for 1 minute 30 seconds to ensure that all particles are properly dispersed, after which measurements are taken. No sonication is performed on the dispersed particles. The average particle size is determined by D[4,3], the volume weighted average diameter (ΣniDi 4 ) / (ΣniDi 3 )

[0026] In a preferred embodiment, the method of the present invention comprises the step of impregnating a fibrous sheet with 5-90%, more preferably 10-80%, even more preferably 20-75%, and most preferably 50-70% of reactive polymer particles, said percentages being calculated by weight of the fibrous sheet.

[0027] According to a particularly preferred embodiment, the tissue adhesive sheet of the present invention is bioabsorbable, i.e. the sheet, the reactive polymer particles, and any other components of the tissue adhesive sheet are eventually absorbed by the body. Absorption of the sheet and the reactive polymer particles typically requires chemical degradation (e.g., hydrolysis) of the polymers contained therein. Complete bioabsorption of the tissue adhesive sheet by the human body is typically achieved in 1-10 weeks, preferably 2-8 weeks.

[0028] The tissue adhesive sheets of the present invention are preferably sterile.

[0029] The tissue adhesive sheet of the present invention typically has an uncompressed average thickness of 0.5 to 25 mm, more preferably in the range of 1 to 10 mm, and most preferably in the range of 1.5 to 5 mm.

[0030] The tissue adhesive sheet preferably has a thickness of 200 mg / cm 3 less than 150 mg / cm 3 less than 10-100 mg / cm 3 It has an uncompressed density of

[0031] The tissue adhesive sheet of the present invention is preferably essentially anhydrous. Typically, the tissue adhesive sheet has a moisture content of 5 wt.% or less, more preferably 2 wt.% or less, and most preferably 1 wt.% or less.

[0032] The water absorption capacity of the tissue adhesive sheet is preferably at least 50%, more preferably in the range of 100% to 800%, and most preferably in the range of 200% to 500%.

[0033] The fibrous sheets utilized in the methods of the present invention are preferably water resistant, ie, the sheets are not water soluble and do not disintegrate in water at neutral pH conditions (pH 7) and a temperature of 37°C.

[0034] The fibers of the fibrous sheet preferably have an average diameter of 1 to 500 μm, more preferably 2 to 300 μm, most preferably 5 to 200 μm. The average diameter of the fibers can be suitably determined using a microscope.

[0035] Typically, at least 50 wt.%, more preferably at least 80 wt.%, of the fibers of the fibrous sheet have a diameter of 1 to 300 μm and a length of at least 1 mm.

[0036] Preferably, at least 50 wt.%, more preferably at least 80 wt.%, of the fibers in the fibrous sheet have an aspect ratio (ratio of length to diameter) of at least 1000.

[0037] The fibrous sheet comprises at least 50 wt.%, more preferably at least 80 wt.%, and most preferably at least 90 wt.%, fibers containing gelatin, collagen, cellulose, modified cellulose, carboxymethyl dextran, PLGA, sodium hyaluronate / carboxymethyl cellulose, polyvinyl alcohol, chitosan, or combinations thereof.

[0038] In an embodiment of the invention, the fibrous support structure does not comprise oxidized regenerated cellulose.

[0039] Preferred fibrous sheets have an air permeability of at least 0.1 L / min×cm 2 , more preferably at least 0.5 L / min×cm 2 The air permeability is determined according to EN ISO 9237:1995 (Determination of the air permeability of textile fabrics).

[0040] The fibers in the fibrous sheet may be produced by methods known in the art, such as electrospinning, electroblown spinning, and high-speed rotary atomizer spinning. The production of fibrous sheets by high-speed rotary atomizer spinning is described in U.S. Patent Application Publication No. 2015 / 0010612. Commercially available hemostatic fibrous sheets can also be used as the fibrous sheet.

[0041] The reactive polymer particles utilized in the method of the present invention preferably contain at least 10 wt.% water-soluble electrophilic polymer. More preferably, the reactive polymer particles contain at least 50 wt.%, more preferably at least 90 wt.% water-soluble electrophilic polymer.

[0042] The method of the present invention, unlike impregnation techniques that utilize shaking or vibration, offers the advantage that very small reactive polymer particles can be effectively distributed in the fibrous sheet. This is advantageous because small particles dissolve faster than larger particles due to their high surface / volume ratio. Thus, the hemostatic properties of tissue adhesive sheets containing very small reactive polymer particles are generally superior to tissue adhesive sheets containing larger reactive polymer particles. Thus, in a highly preferred embodiment, the reactive polymer particles have a volume weighted mean diameter (D[4,3], (Σn i D 4 ) / (Σn i D 3 )).

[0043] According to certain preferred embodiments, at least 80 vol.% of the reactive polymer particles have a diameter in the range of 5 to 200 μm, more preferably in the range of 10 to 120 μm, and most preferably in the range of 12 to 100 μm.

[0044] The reactive polymer particles of the present invention may be prepared in a variety of ways, such as by milling, by spray drying a polymer solution, by freeze drying, by spray cooling a polymer melt, by granulating a powder mixture, or by fluidized bed coating.

[0045] The water-soluble electrophilic polymer contained in the reactive polymer particles typically has a molecular weight of at least 2 kDa, more preferably at least 5 kDa, and most preferably from 10 to 100 kDa.

[0046] The water-soluble electrophilic polymer has a solubility in distilled water at 20° C. of at least 100 g / L, more preferably at least 200 g / L.

[0047] The water-soluble electrophilic polymers utilized by the present invention preferably contain at least 4 reactive electrophilic groups, more preferably at least 8 reactive electrophilic groups, even more preferably at least 16 reactive electrophilic groups, and most preferably at least 32 reactive electrophilic groups.

[0048] The water-soluble electrophilic polymer present in the reactive polymer particles is preferably selected from polyoxazoline, polyethylene glycol, polyvinylpyrrolidone, polyurethane (e.g., as described in WO 2017 / 171551), and combinations thereof. Even more preferably, the electrophilic polymer is selected from polyoxazoline, polyethylene glycol, and combinations thereof. Most preferably, the electrophilic polymer is polyoxazoline.

[0049] Polyoxazolines containing reactive electrophilic groups have repeating units of the following formula (I): (CHR 1 ) m NCOR 2 (In the formula, R 2 and R 1 each of which is H, optionally substituted C 1~22 alkyl, optionally substituted cycloalkyl, optionally substituted aralkyl, and optionally substituted aryl, and m is 2 or 3. It is preferred that the polyoxazoline is derived from a polyoxazoline represented by the formula:

[0050] Preferably, R in formula (I) 1 and R 2 H and C 1~8 Alkyl, even more preferably H and C 1~4 R is selected from alkyl. 1 is most preferably H. The integer m in formula (I) is preferably equal to 2.

[0051] According to a preferred embodiment, the polyoxazoline is a polymer, even more preferably a homopolymer of 2-alkyl-2-oxazoline, said 2-alkyl-2-oxazoline being selected from 2-methyl-2-oxazoline, 2-ethyl-2-oxazoline, 2-propyl-2-oxazoline, 2-butyl-2-oxazoline and combinations thereof. Preferably, the polyoxazoline is a homopolymer of 2-propyl-2-oxazoline or 2-ethyl-oxazoline. Most preferably, the polyoxazoline is a homopolymer of 2-ethyl-oxazoline.

[0052] According to certain preferred embodiments, the water-soluble electrophilic polymer comprises at least 20 oxazoline units, more preferably at least 30 oxazoline units, and most preferably at least 80 oxazoline units. The electrophilic polymer preferably comprises an average of at least 0.05 reactive electrophilic groups per oxazoline residue. Even more preferably, the electrophilic polymer comprises an average of at least 0.1 reactive electrophilic groups per oxazoline residue. Most preferably, the electrophilic polymer comprises an average of 0.12 to 0.5 reactive electrophilic groups per oxazoline residue.

[0053] The water-soluble electrophilic polymer typically bears an average of at least 10, more preferably at least 20, reactive electrophilic groups.

[0054] The polyoxazoline may carry reactive electrophilic groups at its side chains (pendant reactive electrophilic groups), at its termini or both. The polyoxazoline utilized according to the present invention advantageously contains one or more pendant reactive electrophilic groups. Typically, the polyoxazoline contains 0.03-0.5 pendant reactive electrophilic groups per monomer, more preferably 0.04-0.35 pendant reactive electrophilic groups per monomer, even more preferably 0.05-0.25 pendant reactive electrophilic groups per monomer.

[0055] The polyethylene glycol (PEG) comprising reactive electrophilic groups applied according to the present invention is preferably a multi-arm PEG or star-shaped PEG comprising at least three arms, more preferably at least four arms, terminated with reactive electrophilic groups.

[0056] The reactive polymer particles in the tissue adhesive sheet preferably comprise a water-soluble electrophilic polymer bearing a reactive electrophilic group selected from carboxylate esters, sulfonate esters, phosphonate esters, pentafluorophenyl esters, p-nitrophenyl esters, p-nitrothiophenyl esters, acid halide groups, anhydrides, ketones, aldehydes, isocyanates, thioisocyanates, isocyano, epoxides, activated hydroxyl groups, olefins, glycidyl ethers, carboxyls, succinimidyl esters, sulfosuccinimidyl esters, maleimides (maleimidyl), ethenesulfonyl, imidoesters, acetoacetates, haloacetals, orthopyridyl disulfides, dihydroxyphenyl derivatives, vinyls, acrylates, acrylamides, iodoacetamides, and combinations thereof. More preferably, the reactive electrophilic group is selected from carboxylate esters, sulfonate esters, phosphonate esters, pentafluorophenyl esters, p-nitrophenyl esters, p-nitrothiophenyl esters, acid halide groups, anhyinidrides, ketones, aldehydes, isocyanates, thioisocyanates, isocyano, epoxides, activated hydroxyl groups, glycidyl ethers, carboxyls, succinimidyl esters, sulfosuccinimidyl esters, imido esters, dihydroxyphenyl derivatives, and combinations thereof. Even more preferably, the reactive electrophilic group is selected from haloacetals, orthopyridyl disulfides, maleimides, vinyl sulfones, dihydroxyphenyl derivatives, vinyls, acrylates, acrylamides, iodoacetamides, succinimidyl esters, and combinations thereof. Most preferably, the reactive electrophilic group is selected from maleimides, vinyls, acrylates, acrylamides, succinimidyl esters, sulfosuccinimidyl esters, and combinations thereof.

[0057] Examples of succinimidyl esters which may be utilized include succinimidyl glutarate, succinimidyl propionate, succinimidyl succinamide, succinimidyl carbonate, disuccinimidyl suberate, bis(sulfosuccinimidyl)suberate, dithiobis(succinimidyl propionate), bis(2-succinimidooxycarbonyloxy)ethyl sulfone, 3,3'-dithiobis(sulfosuccinimidyl-propionate), succinimidyl carbamate, sulfosuccinimidyl(4-iodoacetyl)acetate, and the like. sulfosuccinimidyl esters, ...

[0058] Examples of dihydroxyphenyl derivatives that may be utilized include dihydroxyphenylalanine, 3,4-dihydroxyphenylalanine (DOPA), dopamine, 3,4-dihydroxyhydroccinamic acid (DOHA), norepinephrine, epinephrine, and catechol.

[0059] In an advantageous embodiment of the present invention, besides the water-soluble electrophilic polymer, the reactive polymer particles additionally contain a nucleophilic crosslinker containing at least two reactive nucleophilic groups capable of reacting with the reactive electrophilic groups of the water-soluble electrophilic polymer under the formation of covalent bonds. The introduction of a nucleophilic crosslinker provides the advantage that the hemostatic and adhesive properties of the sheet may be improved, since the water-soluble electrophilic polymer reacts with the nucleophilic crosslinker when blood enters the sheet. This crosslinking reaction leads to the formation of a hydrogel that fixes the flow of blood and sticks to the tissue by forming covalent bonds between the reactive electrophilic groups in the hydrogel and the amine / thiol groups in the tissue. The combination of the water-soluble electrophilic polymer and the nucleophilic crosslinker in a single particle ensures that these two reactive components can be homogeneously distributed throughout the hemostatic sheet, that no separation occurs during transportation and handling, and that these components can react with each other immediately when the particle comes into contact with blood.

[0060] Reactive polymer particles, i.e. reactive hybrid particles, containing a combination of a water-soluble polymer carrying a reactive electrophilic group and a nucleophilic crosslinker may be produced by wet granulation, preferably under reduced pressure, followed by drying. The granulation liquid should be selected so that little or no reaction occurs between the water-soluble electrophilic polymer and the nucleophilic crosslinker during granulation. This can be achieved, for example, by utilizing a granulation liquid in which at least one of these two components is insoluble. Most preferably, the water-soluble polymer carrying a reactive electrophilic group is insoluble in the granulation liquid.

[0061] According to a particularly preferred embodiment, the reactive polymer particles are particle agglomerates comprising (i) electrophilic particles containing a water-soluble electrophilic polymer, and (ii) nucleophilic particles containing a nucleophilic crosslinker.

[0062] The electrophilic particles preferably contain at least 30 wt.%, more preferably at least 50 wt.%, and most preferably at least 80 wt.% water-soluble electrophilic polymer.

[0063] The nucleophilic particles preferably contain at least 30 wt.%, more preferably at least 50 wt.%, and most preferably at least 80 wt.% nucleophilic crosslinker.

[0064] The nucleophilic crosslinker preferably contains at least three reactive nucleophilic groups. The reactive nucleophilic groups of the nucleophilic crosslinker are preferably selected from amine groups, thiol groups and combinations thereof. More preferably, these reactive nucleophilic groups are amine groups. According to a preferred embodiment, the reactive nucleophilic groups present in the nucleophilic crosslinker are primary amine groups.

[0065] Preferably, the nucleophilic crosslinking agent is selected from proteins, chitosan, synthetic polymers carrying reactive nucleophilic groups, carbohydrate polymers carrying reactive nucleophilic groups, and combinations thereof. Even more preferably, the nucleophilic crosslinking agent is selected from gelatin, collagen, chitosan, and combinations thereof.

[0066] In the method of the present invention, the fibrous sheet and the reactive polymer particles are simultaneously subjected to an electric field of preferably 0.5 to 30 kV / mm, more preferably 1 to 10 kV / mm.

[0067] According to a particularly preferred embodiment, the fibrous sheet and the reactive polymer particles are simultaneously subjected to an alternating electric field. Preferably, the electric field is applied for at least 10 s -1 , preferably at least 50s -1 Frequency of 100s, most preferably -1 It alternates at a frequency of .

[0068] Impregnation of the fibrous sheet may be effectively achieved in the process of the present invention by preparing a layer of reactive polymer particles adjacent to the fibrous sheet and placing the fibrous sheet and the adjacent layer of reactive polymer particles between two electrodes. Impregnation may also be achieved by preparing a stack containing two or more fibrous sheets separated by a layer of reactive polymer particles and placing this stack between two electrodes.

[0069] In a preferred embodiment of the method of the present invention, the fibrous sheet and the reactive polymer particles are placed between a lower electrode and an upper electrode that are electrically insulated from each other by a dielectric and connected to respective poles of an AC generator, thereby simultaneously subjecting the fibrous sheet and the reactive polymer particles to an electric field.

[0070] The fibrous sheet and reactive polymer particles are preferably passed between a lower electrode and an upper electrode while simultaneously subjecting the fibrous sheet and reactive polymer particles to an electric field. Thus, a roll of the fibrous sheet can be suitably semi-continuously impregnated with reactive polymer particles by the method of the present invention.

[0071] In a preferred embodiment, the fibrous sheet and the reactive polymer particles are simultaneously exposed to the electric field for at least 0.1 seconds, more preferably at least 5 seconds, and most preferably at least 30 seconds.

[0072] Another aspect of the present invention relates to a tissue adhesive sheet obtainable by the method previously described herein.

[0073] The present invention is further illustrated by the following non-limiting examples. EXAMPLES

[0074] Generally, whenever the residual moisture content after drying (in the dry powder, granulation and / or fibrous sheet) is not specified, the level is below 2.0% w / w.

[0075] Powders with a D[4,3" of 40 μm or less were produced by milling followed by sieving through a 250 mesh sieve (Haver and Boecker, serial number 47181315). Particles that did not pass through the sieve were re-milled and re-sieved until all powder was below 250 mesh.

[0076] (Preparation of Water-Soluble Electrophilic Polymers (NHS-POx)) NHS side chain activated poly[2-(ethyl / hydroxy-ethyl-amido-ethyl / NHS-ester-ethyl-ester-ethyl-amido-ethyl)-2-oxazoline] terpolymer containing 20% ​​NHS ester groups (=EL-POx, 20% NHS) was synthesized as follows: Poly[2-(ethyl / methoxy-carbonyl-ethyl)-2-oxazoline] copolymer (DP=+ / -100) was synthesized by CROP using 60% 2-ethyl-2-oxazoline (EtOx) and 40% 2-methoxycarbonyl-ethyl-2-oxazoline (MestOx). 1 Secondly, the polymer containing 40% 2-methoxycarbonyl-ethyl groups was reacted with ethanolamine to give a statistical copolymer containing 40% 2-hydroxy-ethyl-amido-ethyl groups ( 1 H-NMR) was then used to obtain a copolymer with half of the 2-hydroxy-ethyl-amido-ethyl groups reacted with succinic anhydride, 1 A terpolymer with 60% 2-ethyl, 20% 2-hydroxy-ethyl-amido-ethyl and 20% 2-carboxy-ethyl-ester-ethyl-amido-ethyl groups was obtained by H-NMR. Finally, the 2-carboxy-ethyl-ester-ethyl-amido-ethyl groups were activated by N-hydroxysuccinimide (NHS) and diisopropylcarbodiimide (DIC) to obtain EL-POx, 20% NHS. 1According to H-NMR, NHS-POx contained 20% NHS-ester groups. NHS-POx was dissolved in water between 2 and 8 °C (60 g in 300 mL) and lyophilized by cooling at minus 80 °C for 30 min. The lyophilized powder so obtained was dried in a Rotavap at 40 °C until the moisture content was less than 0.8% w / w as determined by Karl Fischer titration. This dry (white) powder was ground either using a Retsch Ultra Centrifugal Mill ZM200 equipped with a 12-tooth indented rotor combined with a spacing sieve with 0.25 mm trapezoidal holes until the average particle size was 35 μm or less (D[4,3]) or using a benchtop coffee grinder until the average particle size was about 70 μm (D[4,3]) and vacuum sealed in alu-alu bags.

[0077] (Staining of NHS-POx powder) 20 g of NHS-POx powder was dissolved in water and mixed with 50 mg of Brilliant Blue FCF (Sigma Aldrich) using a high-speed disperser (Ultra-Turrax, IKA). Immediately after mixing (2 min), the solution was frozen at -78 °C and then freeze-dried overnight. The so-obtained freeze-dried powder was dried in a Rotavap at 40 °C until the residual moisture content was less than 0.8% w / w as determined by Karl Fischer titration. The dry (blue) powder was then milled using a Retsch Ultra Centrifugal Mill ZM200 until a blue-stained NHS-POx powder with an average particle size of 35 μm or less (D[4,3]) was obtained and vacuum-sealed in an alu-alu bag.

[0078] (Preparation of nucleophilic crosslinker (NU-POx)) Polyoxazolines containing ethyl and amine groups in the alkyl side chains were synthesized by CROP of EtOx and MestOx followed by amidation of the methyl ester side chains with ethylenediamine to give poly(2-ethyl / aminoethylamidoethyl-2-oxazoline) copolymers (NU-POx). 1According to H-NMR, NU-POx contained 10% NH2. NU-POx was dissolved in water between 2 and 8 °C (60 g in 300 mL) and freeze-dried by cooling at minus 80 °C for 30 min. The freeze-dried powder so obtained was dried in a Rotavap at 40 °C until the moisture content was less than 0.8% w / w as determined by Karl Fischer titration. The dried powder was milled using a Retsch Ultra Centrifugal Mill ZM200 to an average particle size of ≤35 μm (D[4,3]) and vacuum sealed in alu-alu bags.

[0079] (Preparation of reactive polymer particles (NHS-POx / NU-POx granules)) Blue or white (undyed) NHS-POx powder was wetted with isopropyl alcohol (IPA) in a high shear mixer until a homogenous snow-like powder containing approximately 1-2% w / w IPA was obtained. After this, NU-POx powder was added and mixed. The wetted blue NHS-POx powder was mixed with NU-POx powder in a 1:1 molar ratio, where the molar ratio refers to the ratio of the number of NHS groups provided by NHS-POx to the number of amine groups provided by NU-POx.

[0080] After mixing, 1 The wet granulation was dried under vacuum until the IPA content was less than 0.1% w / w as determined by H-NMR. The dried granulation was milled using a Retsch Ultra Centrifugal Mill ZM200 to an average particle size of 50 μm or less than 35 μm (D[4,3]) and vacuum sealed in alu-alu bags.

[0081] 1 The NHS-POX / NU-POx granules (1:1) were analyzed using H-NMR spectroscopy. 25 mg of granules were dissolved in trifluoroacetic acid (0.20 mL) by sonication for 20 min. After complete dissolution of the granules, the sample was diluted with deuterated dimethyl sulfoxide (DMSO-d6) (0.80 mL) containing maleic acid (2.5 mg / mL) as an internal standard and transferred to an NMR tube. 1H-NMR spectra were recorded. From the spectra obtained, the amount of NHS bound to NHS-POx can be calculated, along with the molar ratio of NHS and amine groups present in the granulate. The amount of NHS bound to NHS-POx in the granulate is comparable to the amount of NHS bound to the NHS-POx starting material, indicating that no collapse or cross-linking occurs during granulation.

[0082] Total polymer recovery in the NMR samples, i.e., the combination of NHS-POx and NU-POx, was determined using known amounts of an internal standard (maleic acid) and recorded NMR spectra of different concentrations of NHS-POx and NU-POx. 1 The total polymer recovery was determined using a calibration curve generated from the H-NMR spectrum and was determined to be 99 percent, indicating that no insoluble crosslinked material was formed.

[0083] The NHS-POX / NU-POx granules (1:1) were further analyzed by size exclusion chromatography. 20 mg of the granules were treated with acetic anhydride (1.00 mL) at 50° C. for 1 h. Methanol (2.00 mL) was then added and the mixture was stirred at 50° C. for an additional 1 h. An aliquot (0.75 mL) was taken and all volatiles were removed under reduced pressure. The sample was dissolved in N,N-dimethylacetamide (2.50 mL) containing 50 mM lithium chloride, the eluent for SEC analysis. SEC was measured against poly(methyl methacrylate) standards and the M was calculated from the resulting size exclusion chromatogram. n , M w and PDI were determined. The PDI was below 1.5, indicating that no cross-linking occurred during granulation. Analytical validation of this size exclusion chromatography method showed that intentional cross-linking of NHS-POx and NU-POx at a level of 0.05 mol% increased the PDI to above 2.5.

[0084] (Preparation of reactive polymer particles (NHS-POx / NU-POx / P188 granules)) Reactive NHS-POx / NU-POx granules were prepared as described above. Reactive NHS-POx / NU-POx granules coated with P188 at 1.5%, 2.5%, 3.5%, 5% and 10% w / w were then prepared by heating the NHS-POx / NU-POx granules with P188 powder in a high shear mixer at 65°C for 10 minutes and then cooling to ambient conditions. The coated granules were milled using a Retsch Ultra Centrifugal Mill ZM200 to an average particle size of 40 μm or less (D[4,3]) and vacuum sealed in alu-alu bags.

[0085] The particle size distribution of the granules thus obtained was approximately 90 vol.% < 80 μm, 50 vol.% < 40 μm, and 10 vol.% < 10 μm.

[0086] 1 The NHS-POx / NU-POx / P188 granules were analyzed using H-NMR spectroscopy. 25 mg of powder was dissolved in trifluoroacetic acid (0.20 mL) by sonication for 20 min. After complete dissolution of the granules, the sample was diluted with deuterated dimethyl sulfoxide (DMSO-d6) (0.80 mL) and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 98 percent compared to NHS-POx.

[0087] The NHS-POx / NU-POx / P188 granules were further analyzed by size exclusion chromatography. 20 mg of granules were treated with acetic anhydride (1.00 mL) at 50° C. for 1 h. Methanol (2.00 mL) was then added and the mixture was stirred at 50° C. for an additional 1 h. An aliquot (0.75 mL) was taken and all volatiles were removed under reduced pressure. The sample was dissolved in N,N-dimethylacetamide (2.50 mL) containing 50 mM lithium chloride, the eluent for SEC analysis. SEC was measured against poly(methyl methacrylate) standards and the M was calculated from the resulting size exclusion chromatogram. n , M wand PDI were determined. The PDI was less than 1.5, indicating that no cross-linking occurred during granulation.

[0088] (Preparation of reactive polymer particles (NHS-POx / Gelita Spon granules)) 7.01 g of pre-dried gelatin powder (Gelita-SPON®, formerly Gelita Medical GmbH) with a moisture content of less than 0.2% w / w was dispersed in dichloromethane (200 mL) using a high shear mixer operating at 20,000 rpm for 20 min. NHS-POx (7.02 g) was then added and stirring was continued for 5 min. NHS-POx did not dissolve. All volatiles were removed from the suspension under reduced pressure. The resulting powder was ground using a coffee grinder until the average particle size was ≤95 μm (D[4,3]), vacuum sealed in an alu-alu bag, further dried under reduced pressure and vacuum sealed in an alu-alu bag.

[0089] The particle size distribution of the granules thus obtained was approximately 90 vol.% < 190 μm, 50 vol.% < 80 μm and 10 vol.% < 15 μm.

[0090] Granulated material 1 The NHS-POx were analyzed by H-NMR spectroscopy. For this purpose, 1.0 mL of deuterated chloroform (CDCl3) containing 5% (v / v) acetic acid was added to 25 mg of the granulation. The NHS-POx were selectively extracted by ultrasonicating the sample for 20 min. The dispersion was passed through a 0.22 μm filter and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 97 percent compared to NHS-POx.

[0091] The granulation was further analyzed by size exclusion chromatography (SEC) analysis. An aliquot (0.15 mL) of the filtered NHS-POx extract described above was diluted with N,N-dimethylacetamide (1.00 mL) containing 50 mM lithium chloride, the eluent for SEC analysis. The sample was analyzed by SEC against a poly(methyl methacrylate) standard with a PDI of 1.45, indicating that no crosslinking had occurred.

[0092] (Preparation of reactive polymer particles (NHS-POx / NU-POx / PEG3000 granules)) Reactive NHS-POx / NU-POx granules were prepared as described above. Reactive NHS-POx / NU-POx granules coated with 5% and 10% w / w PEG3000 were then prepared by heating the NHS-POx / NU-POx granules with PEG (MW 3 kDa) powder in a high shear mixer at 65° C. for 10 minutes and then cooling to ambient conditions. The coated granules were milled using a Retsch Ultra Centrifugal Mill ZM 200 and vacuum sealed in alu-alu bags.

[0093] 1 The NHS-POx / NU-POx / PEG3000 granules were analyzed using H-NMR spectroscopy. 25 mg of powder was dissolved in trifluoroacetic acid (0.20 mL) by sonication for 20 min. After complete dissolution of the granules, the sample was diluted with deuterated dimethyl sulfoxide (DMSO-d6) (0.80 mL) and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 96 percent compared to NHS-POx.

[0094] The NHS-POx / NU-POx / PEG granules were further analyzed by size exclusion chromatography. 20 mg of the granules were treated with acetic anhydride (1.00 mL) at 50° C. for 1 h. Methanol (2.00 mL) was then added and the mixture was stirred at 50° C. for an additional 1 h. An aliquot (0.75 mL) was taken and all volatiles were removed under reduced pressure. The sample was dissolved in N,N-dimethylacetamide (2.50 mL) containing 50 mM lithium chloride, the eluent for SEC analysis. SEC was measured against poly(methyl methacrylate) standards and the M was determined from the resulting size exclusion chromatogram. n , M w and PDI were determined. The PDI was less than 1.5, indicating that no cross-linking occurred during granulation.

[0095] (Preparation of reactive polymer particles (NHS-POx / NU-PEG)) NHS-POx coated with 5% w / w NU-PEG was prepared by heating NHS-POx (D[4,3]≦35 μm) with PEG diamine (MW 10 kDa) powder in a high shear mixer at 65° C. for 10 min, followed by cooling to ambient conditions. The coated granulation was milled using a Retsch Ultra Centrifugal Mill ZM 200 and vacuum sealed in alu-alu bags.

[0096] 1 H-NMR spectroscopy was used to analyze the NHS-POx / NU-PEG reactive polymer particles. 25 mg of powder was dissolved in trifluoroacetic acid (0.20 mL) by sonication for 20 min. After complete dissolution of the granulation, the sample was diluted with deuterated dimethyl sulfoxide (DMSO-d6) (0.80 mL) and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 95 percent compared to NHS-POx.

[0097] The NHS-POx / NU-PEG reactive polymer particles were further analyzed by size exclusion chromatography. 20 mg of powder was treated with acetic anhydride (1.00 mL) at 50° C. for 1 h. Methanol (2.00 mL) was then added and the mixture was stirred at 50° C. for an additional 1 h. An aliquot (0.75 mL) was taken and all volatiles were removed under reduced pressure. The sample was dissolved in N,N-dimethylacetamide (2.50 mL) containing 50 mM lithium chloride, the eluent for SEC analysis. SEC was measured against poly(methyl methacrylate) standards and the M was calculated from the resulting size exclusion chromatogram. n , M w and PDI were determined. The PDI was less than 1.5, indicating that no cross-linking occurred during granulation.

[0098] (fibrous sheet) The following commercially available hemostatic products were selected for use as fibrous sheets in the preparation of tissue adhesive sheets according to the present invention: Gelita Tuft-It®: A cohesive fibrous sheet consisting of eight layers of reduced cross-linked gelfoam fibers. The eight layers, each approximately 2 mm thick, measure 50 mm x 75 mm. The moisture content of Gelita Tuft-It® is 15% or less. The product is dried in a vacuum oven at 40°C for several hours to reduce the moisture content to 2.0% w / w or less (determined gravimetrically) before being impregnated with agglomerated particles. SURGICEL® SNoW™: A cohesive fibrous sheet consisting of an absorbent nonwoven fabric prepared by controlled oxidation of regenerated cellulose (ORC). Dimensions were 5.1 cm x 10.2 cm and moisture content was 2.0% w / w or less. SURGICELS® NU-KNIT® / SURGICELS® SNoW™ Hybrid: A dense, absorbent knit of fibers prepared by controlled oxidation of regenerated cellulose (ORC), available in multiple sizes (e.g., 15.2 cm x 22.9 cm), was sewn to SURGICELS® SNoW™ and cut to dimensions of 5.1 cm x 10.2 cm. Adhesive fibrous sheets of PEM:oxidized regenerated cellulose (ORC) and polyglactin 910 with dimensions (length, width) 97.0-102.5 mm and thickness 1.40-2.50 mm were prepared as follows: Poly(glycolide-co-lactide) (PGL, 90 / 10 mol / mol) was melt spun into fibers. 80 denier multifilament yarns were consolidated into 800 denier consolidated yarns. The consolidated yarns were crimped at approximately 110°C. The crimped yarns were chopped into staple fibers with a length of approximately 1.25''. 20 g of crimped staple fibers were precisely weighed and spread evenly on the feed conveyor belt of a multi-roller carding machine. The environmental conditions (temperature: 21°C / 55% RH) were controlled. The staple fibers were then carded to create a nonwoven batt. The batt was removed from the pick-up roller and cut into four equal parts. These were re-fed into the carding machine perpendicular to the collection direction. After this second pass, the batt was weighed (19.8 g: 99% fabric yield) and compressed into felt. The compressed felt was precisely spread over the ORC fabric and firmly attached by two passes through the needle punching machine. The multi-layer fabric was trimmed and rinsed in three separate isopropyl alcohol baths to remove spin finish and machine oils. The rinsed multi-layer fabric was dried in a 70° C. oven for 30 minutes, cooled and weighed. The moisture content was below 2.0% w / w.

[0099] (Impregnation method) machine The Fibroline SL-Preg laboratory machine moves particles between electrodes by applying a voltage of up to 40 kV at a frequency of up to 200 Hz for up to 60 seconds. The two electrode plates are approximately 50 x 40 cm in size. The upper plate is grounded.

[0100] The following standard settings were used: 40 kV, 100 Hz, 20–30 s.

[0101] array After attaching the 3D printed PMMA array to the lower electrode plate, the powder was poured into the array by gravity. A scraping carton or metal spatula was used to fill the array with reactive polymer powder. The array was 50 x 75 x 4 mm and contained 22 x 33 = 726 square wells (inner dimensions of each well: 2 x 2 x 2 mm). The total volume of the 726 wells was approximately 5.8 mL.

[0102] Spacer A spacer mask was placed over the array. The use of spacers allows for up and down movement of the particles when subjected to an alternating electric field. If no spacers are used, penetration into and distribution through the support is limited.

[0103] Different spacer heights are needed for different substrates. For TUFT-IT and SNoW, the mask height was 3mm. This results in an electrode distance of 3+4mm=7mm. For the NU-IT / SNoW hybrid, the mask height was 1.5mm. This results in an electrode distance of 1.5+4mm=5.5mm.

[0104] (Bleeding experiment) Hemostatic efficacy was assessed using standardized ex-vivo and in-vivo porcine bleeding models. All models used heparin to prolong clotting times, increasing the activated clotting time (ACT) by approximately 2-3 fold.

[0105] Ex-vivo model: A live ex-vivo porcine model with a fresh liver perfused with fresh heparinized blood from the slaughterhouse to mimic the actual in-vivo environment as closely as possible. The liver is attached to a perfusion machine that maintains oxygenation, blood pH, temperature and blood pressure within the biologic boundaries. Two livers and 10 liters of heparinized blood (5000 units / L) are collected at the slaughterhouse. The livers are shipped on ice and the blood at ambient temperature. Within 2 hours of collection, the liver is inspected for lesions and closed with gloves and cyanoacrylate glue. Perfusion parameters: flow rate 600 ml / min, pressure 10-12 mmHg, temperature 37°C (+ / - 1°C), carbogen 0.25 liters per minute. A circular bleeding wound (8 mm diameter) is created on the liver surface using a flat round rotary scraping tool, with a rubber onlay so that the depth of the punched bleeding area is always 3 mm. Once the liver is properly perfused (check color and temperature), test the sample according to the following procedure: cut the sample to the appropriate size (2.7 x 2.7 cm); turn on the camera; check the number of sites with the camera; punch an 8 mm biopsy; cut and remove the biopsy; remove blood from the bleeding site with gauze (2x); collect blood with pre-weighed gauze for 30 seconds; score bleeding (by 2 investigators); place the sample on the bleeding site with pre-moistened gauze (saline) and hold with slight pressure for 1 minute; observe for 5 minutes (check and score for adhesion and hemostasis) and repeat after 30 minutes.

[0106] Porcine in-vivo model: A standardized combined penetrating splenic rupture was induced in anesthetized pigs (domestic pig, female, weight range: 40 kg, adult). A midline laparotomy was performed to access the spleen and other organs. Using this model, several types of surgical procedures were performed: A circular biopsy punch is used to create subcapsular standardized lesions (0.8 mm diameter) in the liver and / or spleen. A test article approximately 2 x 2 cm is used to cover the lesion and manual tamponade is applied. Use a scalpel to create subcapsular standardized lesions in the liver and / or spleen. Remove the desired liver lobe or spleen edge using standard techniques, leaving the cut surface exposed. Cover the resection surface with a 7.5 x 5 cm or 10 x 5 cm coupon and apply manual tamponade. The left and right kidneys are identified and isolated using a combination of blunt and sharp dissection. The left and right kidneys are dissected out so that they can be grasped with one hand, and the caudal pole of the kidney (approximately 2.5 ± 1 cm diameter x 1 ± 0.5 cm depth) is guillotine excised with a scalpel. The target application site is aspirated and wiped clean of blood, and the test article is immediately applied to the site of active bleeding. A 7.5 x 5 cm or 10 x 5 cm test article is used to cover the resection surface and apply manual tamponade. The same procedure is repeated at the cranial pole of the kidney.

[0107] Rat in-vivo model: One hundred male Wistar (WU) rats ranging in weight from 270 to 300 grams are used. All rats are treated with 0.02 mg / kg subcutaneous buprenorphine at least 15 minutes before surgery. Induction anesthesia is administered by inhaling 5% isoflurane in a 1:1 mixture of pressurized air and oxygen in an induction chamber. The maintenance dose is 3.5% isoflurane administered through a nose-mouth mask (also in a 1:1 mixture of pressurized air and oxygen). Rats are prepared by shaving and disinfecting the skin with iodine and a sterile cover. Rats are secured to a 15° inclined platform with the head elevated above the tail (Murakimi 2008). Body temperature is maintained at 38°C using a heating pad and lamp, and surgery is performed through a 4-5 cm midline laparotomy using strict aseptic technique. The abdomen is opened through a midline abdominal incision, and the left lateral liver lobe is isolated. The lobe is placed on a piece of sturdy paper and the excision is performed. The distal portion of the liver lobe is cut off approximately 3 mm from the edge using a scalpel. One patch (15 mm x 25 mm) is gently applied to the left lateral liver lobe adjacent to the wound, followed by manual tamponade with moist gauze for 1 minute. The right portion of the median liver lobe is then prepared, a partial excision is performed, and a second patch of the same dimensions is applied in the same manner.

[0108] Throughout all ex-vivo and in-vivo procedures described herein, the hemostatic product is applied with pre-moistened gauze (saline) using gentle pressure and held in place for 1 minute. After application of the product, it is scored for clotting and adhesion to the tissue.

[0109] Patch scoring system: Clotting ++++ Achieved immediately after tamponade +++ Achieved <10 seconds after tamponade ++ Achieved <30 seconds after tamponade + Achieved within 3 minutes of tamponade Achieved after + / - 3 minutes, apply second tamponade - Not achieved

[0110] Patch scoring system: 10 minutes after application ++++ Very strong adhesion (patch breaks upon removal) +++ Strong adhesion (patch breaks when removed) ++ Strong adhesion (patch can be removed without damage) + Moderate adhesion (patch can be removed without damage) + / - Mild adhesion (patch can be removed without damage) - Not achieved

[0111] [Example 1] [Impregnation of 70 μm NHS-POx or 35 μm dyed NHS-POx into Tuft-IT] Impregnation of Tuft-IT with 70 μm NHS-POx (n=186) The average weight of the unimpregnated Tuft-It was 0.74 g. The average impregnation was 0.93 g, which corresponds to an overall impregnation efficiency of about 56% (impregnation efficiency =

number

[0112] Impregnation of double-tufted IT with 35 μm blue NHS-POx (n=26) The average weight of the unimpregnated Tuft-It was 1.55 g. The average impregnation was 2.78 g, which corresponds to an overall impregnation efficiency of about 64%. Although the average loss was about 10%, it was not necessary to recover NHS-POx from the array and reuse it for impregnation. Again, no correlation was observed between the weight of the unimpregnated sheet and the impregnation level (in grams).

[0113] [Example 2] [Impregnation of 50 μm or 35 μm reactive NHS-POx / NU-POx into PEM] Impregnation of PEM with 50 μm NHS-POx / NU-POx granules (n=186) The average weight of the unimpregnated PEM was 0.71 g. The average impregnation was 1.65 g, which corresponds to an overall impregnation efficiency of about 70%. The average loss was about 10%, but it was not necessary to recover the polymer from the array and reuse it for impregnation. No correlation was observed between the weight of the unimpregnated sheet and the impregnation level (in grams).

[0114] Impregnation of 35μm NHS-POx / NU-POx granules into PEM (n=20) The average weight of the unimpregnated PEM was 0.72 g. The average impregnation was 1.53 g, which corresponds to an overall impregnation efficiency of about 68%. The average loss was about 5%, but it was not necessary to recover the polymer from the array and reuse it for impregnation. No correlation was observed between the weight of the unimpregnated sheet and the impregnation level (in grams).

[0115] [Example 3] [Impregnation of 50 μm or 35 μm reactive NHS-POx / NU-POx into NU-nit / SNoW hybrid] Impregnation of 50μm NHS-POx / NU-POx granules into NU-nit / SNoW hybrid (n=5) The average weight of the unimpregnated NU-nit / SNoW hybrids was 1.56 g. The average impregnation was 3.47 g, which corresponds to an overall impregnation efficiency of about 55%. The average loss was about 10%, but it was not necessary to recover the polymer from the array and reuse it for impregnation. No correlation was observed between the weight of the unimpregnated sheet and the impregnation level (in grams).

[0116] Impregnation of 35μm NHS-POx / NU-POx granules into NU-nit / SNoW hybrid (n=12) The average weight of the unimpregnated NU-nit / SNoW hybrids was 1.52 g. The average impregnation was 2.87 g, which corresponds to an overall impregnation efficiency of about 65%. The average loss was about 5%, but it was not necessary to recover the polymer from the array and reuse it for impregnation. No correlation was observed between the weight of the unimpregnated sheet and the impregnation level (in grams).

[0117] [Example 4] [Impregnation of 40 μm NHS-POx / NU-POx / P188 (5 and 10%) granules into PEM] 5%P188: The average weight of the unimpregnated PEM was 1.04 g (n=11). The average impregnation was 2.50 g, which corresponds to an overall impregnation efficiency of about 70%.

[0118] 10%P188 The average weight of the unimpregnated PEM was 1.03 g (n=6). The average impregnation was 2.56 g, which corresponds to an overall impregnation efficiency of about 71%.

[0119] 5%PEG3000: The weight of the unimpregnated PEM was 0.96 g (n=1). The impregnation was 2.19 g, which corresponds to an overall impregnation efficiency of about 70%.

[0120] 10% PEG 3000: The weight of the unimpregnated PEM was 1.02 g (n=1). The impregnation was 2.48 g, which corresponds to an overall impregnation efficiency of about 71%.

[0121] NHS-POx / NU-PEG: The weight of the unimpregnated PEM was 1.01 g (n=1). The impregnation was 1.47 g, which corresponds to an overall impregnation efficiency of about 59%.

[0122] [Example 5] [Impregnation of 40 μm NHS-POx / NU-POx / P188 (1.5, 2.5, 3.5, 5 and 10%) granules into NU-nit / SNoW hybrid] 1.5% P188: The average weight of the unimpregnated NU-nit / SNoW hybrid was 1.55 g (n=1). The average impregnation was 1.90 g, which corresponds to an overall impregnation efficiency of about 55%.

[0123] 2.5% P188: The average weight of the unimpregnated NU-nit / SNoW hybrids was 1.53 g (n=1). The average impregnation was 1.77 g, which corresponds to an overall impregnation efficiency of about 54%.

[0124] 3.5% P188: The average weight of the unimpregnated NU-nit / SNoW hybrids was 1.45 g (n=1). The average impregnation was 1.19 g, which corresponds to an overall impregnation efficiency of about 45%.

[0125] 5%P188: The average weight of the unimpregnated NU-nit / SNoW hybrids was 1.52 g (n=12). The average impregnation was 2.87 g, which corresponds to an overall impregnation efficiency of about 65%.

[0126] 10%P188: The average weight of the unimpregnated NU-nit / SNoW hybrids was 1.52 g. The average impregnation was 2.61 g, which corresponds to an overall impregnation efficiency of about 63%.

[0127] [Example 6] [Impregnation of 100 μm reactive NHS-POx / Gelita Spon granules into PEM] The average weight of the unimpregnated PEM was 0.79 g (n=1). The average impregnation after two cycles (one for 20 s and one for 30 s) was 1.15 g, which corresponds to an overall impregnation efficiency of about 60%. The amount of granulation that could be applied to the array was limited due to swelling of the granulation, and two cycles were required to achieve a reasonable impregnation efficiency (or % loading).

[0128] [Example 7] Tuft-It is made from 0.75 grams of gelatin fibers and can hold up to 1 gram of NHS-POx (see Example 1). To increase the loading capacity beyond 1 g of NHS-POx, a so-called "Tuft-It-Plus" was made from standard Tuft-It by evenly dispersing 0.5 grams of standard Gelita Spon between the n=8 layers.

[0129] Increasing the density of Tuft-It has two main results: [1] the bulk material is increased, achieving better hemostasis + [2] the capacity to retain more NHS-POx is increased, improving hemostasis.

[0130] Tuft-It-Plus was impregnated with 70 μm of NHS-POx. Using a double spacer, the loading of NHS-POx could be increased to 1.5 g per support (double masks of 3 mm each give a powder and array thickness of 3 + 3 + 4 mm, with a total height between electrodes of 10 mm).

[0131] [Example 8] The impregnated sheets described in Examples 1 to 7 were used to carry out bleeding experiments.

[0132] A summary of the samples tested is shown in Table 1.

[0133] [Table 1]

[0134] The results of the bleeding studies are summarized in Tables 2 and 3 (NT = not tested).

[0135] [Table 2]

[0136] [Table 3]

[0137] [Example 9] Experiments were conducted to determine the effect of NU-POx content of reactive NHS-POx / NU-POx granulations on the in-vivo performance of hemostatic patches.

[0138] (Impregnation method) Hemostatic patches (Gelita Tuft-It®; 50×75 mm, approximately 0.7 g) were impregnated with reactive NHS-POx / NU-POx granules prepared by acetone granulation in molar ratios of 1:0.10, 1:0.20, and 1:0.40, the molar ratio referring to the ratio of the number of NHS groups provided by NHS-POx to the number of amine groups provided by NU-POx. The same hemostatic patches were also impregnated with reactive NHS-POx powder.

[0139] Using a Fibroline SL-Preg lab machine, 1 gram of granulation / powder was distributed throughout the patch. The hemostatic patch was then cemented, dried, loaded into an alu-alu pouch containing 1 gram of silica, and vacuum sealed.

[0140] machine The Fibroline SL-Preg laboratory machine moves particles between electrodes by applying voltages of up to 40 kV at frequencies of up to 200 Hz for periods of up to 60 seconds. The two electrode plates are approximately 50 x 40 cm in size. The upper plate is grounded.

[0141] The following standard settings were used: 40 kV, 100 Hz, 20 s.

[0142] array After attaching the 3D printed PMMA array to the lower electrode plate, the powder was poured into the array by gravity. A scraping carton or metal spatula was used to fill the array with reactive polymer powder. The array was 50 x 75 x 4 mm and contained 22 x 33 = 726 square wells (inner dimensions of each well: 2 x 2 x 2 mm). The total volume of the 726 wells was approximately 5.8 mL.

[0143] Spacer A spacer mask was placed on top of the array. The use of a spacer allows the particles to move up and down when subjected to an alternating electric field. If a spacer is not used, it limits penetration into and distribution through the carrier. In the case of the Tuft-IT this was a 3mm mask. This gives an electrode distance of 3+4mm=7mm.

[0144] The in vivo performance of hemostatic patches containing NHS-POx:NU-POx granules (0, 10, 20 and 40 percent of amine groups from NU-POx, percentages calculated based on the number of NHS groups provided by NHS-POx) or NHS-POx powder was evaluated in a non-heparinized in-vivo porcine model. Details of the tested patches are shown in Table 4.

[0145] [Table 4]

[0146] (In vivo test) Studies were performed on adult female domestic pigs (40-50 kg). No anticoagulant was applied. Patch performance was tested on both the spleen and liver. The spleen or liver were located and exposed as necessary over the course of the study period, and their natural moisture was maintained by covering them with saline-soaked sponges.

[0147] Different types of damage created: Liver: abrasion, biopsy punch and excision wound Spleen: resection wound

[0148] Appropriately sized portions of liver parenchyma were abraded / punched to induce moderate to severe bleeding. Liver abrasions were made with a scalpel and a 1x1 cm2 template, and circular punches were made using an 8 mm circular biopsy punch. Liver and spleen resection wounds were made using a surgical knife.

[0149] Patches were applied immediately after tissue excision or scarification: Biopsy punch and 2 x 2 cm pieces for scraping Complete 7.5 x 5 cm patch for excision wound

[0150] The test patch was applied to the bleeding tissue and gently pressed by applying pressure using gauze pre-moistened with saline solution. Tamponade was applied initially for a 10 second period, followed by a 30 second interval, up to a total of 5 minutes.

[0151] An unimpregnated Tuft-IT patch was used as a reference (referred to as Tuft-IT).

[0152] The results of the in vivo studies are summarized in Table 5.

[0153] [Table 5]

[0154] Patches 1-4 showed very strong tissue adhesion, whereas only mild adhesion was observed for the Tuft-IT patch.

[0155] Patches 1 and 2 showed very little swelling after application, while patches 3-4 showed more significant, but still acceptable, swelling.

[0156] [Example 10] Hemostatic patches (Gelita Tuft-It®; 50×75 mm, approximately 0.7 g) were impregnated with either a solution of NHS-POx, NHS-POx powder, or NHS-POx / NU-POx granules. The NHS-POx / NU-POx granules used were made by acetone granulation at a molar ratio of 1:0.20 (see Example 9).

[0157] A spray solution containing NHS-POx was prepared by dissolving NHS-POx in a 1:1 mixture of isopropyl alcohol and dichloromethane (200 g / L). Using a laboratory glass sprayer and pressurized air, 5 mL of this spray solution was impregnated into the patches in one spray cycle. The total amount of NHS-POx delivered in this manner was 1 gram per patch. After impregnation, the patches were dried in an oven at 40° C. for 2 hours and then stored in a desiccator for 2 days before being loaded into an alu-alu pouch containing 1 g of silica and vacuum sealed.

[0158] Additionally, using the procedure described in Example 9, patches were impregnated with 1 gram of NHS-POx powder or 1 gram of NHS-POx / NU-POx granulation.

[0159] The performance of the so-prepared patches was tested in triplicate in an ex vivo liver perfusion model under mild (<20 mL / min) and severe bleeding (>50 mL / min) conditions. A circular bleeding wound (8 mm diameter) was created on the liver surface using a flat round rotary scraping tool, and a rubber onlay was used to ensure that the punched bleeding area was always 3 mm deep. The results are shown in Table 6.

[0160] [Table 6]

Claims

1. 1. A method for preparing a tissue adhesive sheet, the method comprising: providing a fibrous sheet comprising three-dimensional interconnected void spaces; providing a reactive polymer particle comprising a water-soluble electrophilic polymer bearing at least three reactive electrophilic groups, said reactive electrophilic groups being capable of reacting with amine groups in blood to form covalent bonds; placing the fibrous sheet and the reactive polymer particles between two electrodes; simultaneously subjecting the fibrous sheet and the reactive polymer particles to an electric field of 0.1-40 kV / mm to impregnate the reactive polymer particles into the interconnected interstitial spaces of the fibrous sheet. A method comprising:

2. The method of claim 1 , wherein the tissue adhesive sheet is bioabsorbable.

3. The method of claim 1 or 2, wherein the fibers of the fibrous sheet have an average diameter of 1 to 500 μm.

4. The method according to any one of claims 1 to 3, wherein the reactive polymer particles have a volume weighted average diameter of from 10 to 100 µm.

5. The method according to any one of claims 1 to 4, wherein the fibrous sheet has a felt, woven or knitted structure.

6. The method of any one of claims 1 to 5, wherein the fibrous sheet has an average uncompressed thickness of 0.5 to 25 mm.

7. The fibrous sheet is 200 mg / cm 3 The method of any one of claims 1 to 6, wherein the uncompressed density is less than

8. 8. The method of any one of claims 1 to 7, wherein the fibrous sheet comprises at least 50 wt.% fibers containing gelatin, collagen, cellulose, modified cellulose, carboxymethyl dextran, PLGA, sodium hyaluronate / carboxymethyl cellulose, polyvinyl alcohol, chitosan, or combinations thereof.

9. A method described in any one of claims 1 to 8, wherein the method includes a step of impregnating the fibrous sheet with 5 to 90% of the reactive polymer particles, the percentage being calculated by the weight of the fibrous sheet.

10. The method of any one of claims 1 to 9, wherein the reactive polymer particles contain at least 10 wt.% of the water-soluble electrophilic polymer.

11. The method of any one of claims 1 to 10, wherein the water-soluble electrophilic polymer is selected from polyoxazoline, polyethylene glycol, polyvinylpyrrolidone, polyurethane, and combinations thereof.

12. 12. The method of any one of claims 1 to 11, wherein the fibrous sheet and the reactive polymer particles are placed between a lower electrode and an upper electrode electrically insulated from each other by a dielectric and connected to respective poles of an AC generator, thereby subjecting the fibrous sheet and the reactive polymer particles to the electric field.

13. 13. The method of claim 12, wherein the fibrous sheet and the reactive polymer particles are passed between the lower electrode and the upper electrode while subjecting the fibrous sheet and the reactive polymer particles to the electric field.

14. The method of any one of claims 1 to 13, wherein the fibrous sheet is subjected to the electric field for at least 0.1 seconds.

Citation Information

Patent Citations

  • Filling of fibers or filament networks with powder, in particular method of filling for the production of composites

    JP2001521834A

  • tissue adhesive construct

    JP2006523113A

  • Hemostatic sponge

    JP2013523296A

  • Crosslinked polymer derived from electrophilic activated polyoxazoline and implant

    JP2017008315A

  • Tissue-adhesive porous hemostatic product

    JP2017531488A