V-ribbed belt, power transmission mechanism, and method for manufacturing V-ribbed belt
The V-ribbed belt with a twisted aliphatic polyamide core and surface layer maintains tension in high humidity conditions, addressing the tension drop issue in low modulus belts, ensuring reliable power transmission.
Patent Information
- Application Number
- JP2022033261
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-11
- Filing Date
- 2022-03-04
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2042-03-04
AI Technical Summary
Existing low modulus V-ribbed belts fail to maintain sufficient tension during running when stored in high humidity environments due to water absorption, leading to a significant drop in belt tension retention rate.
A V-ribbed belt design with a twisted cord made of aliphatic polyamide fibers and a surface layer, featuring a compressed layer with ribs, which maintains a low 3.5% modulus and high shrinkage stress, allowing easy installation using a stretching method even in high humidity conditions.
The belt maintains sufficient tension during running by suppressing sudden drops, even when stored in high humidity, ensuring reliable power transmission without the need for additional tension mechanisms.
Smart Images

Figure 0007555985000003 
Figure 0007555985000004 
Figure 0007555985000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a V-ribbed belt for use in, for example, an accessory drive system of an automobile engine. [Background technology]
[0002] Friction transmission belts are widely used to drive automobile engines and general industrial machines. Examples of friction transmission belts include flat belts, V-belts, and V-ribbed belts, and friction transmission belts are used to distinguish them from meshing transmission belts such as toothed belts that transmit power by mechanically engaging the teeth of the belt with the tooth grooves of a pulley. Among them, V-ribbed belts are widely used to drive automobile engine accessories because they can achieve both high transmission capacity and flex fatigue resistance.
[0003] In the field of power transmission belts, the ease with which a belt stretches is expressed as "elongation rate" or "elastic modulus." "Elongation rate" is how easily a belt stretches, while "elastic modulus" is how difficult it is to stretch, so they are inversely related. In other words, "low elastic modulus (low modulus)" and "high elongation rate (high elongation)" mean the same thing.
[0004] For power transmission belts, the tension at which the belt is attached to the pulley has a large effect on the transmission performance, durability life, fuel efficiency, etc., so it is necessary to maintain the tension even while the vehicle is running. However, if the belt stretches and slackens while in operation, the tension will decrease, so basically, a belt that does not stretch, that is, a belt with a high modulus (low elongation) is suitable. In particular, the more severe the driving conditions are for the application, the more necessary a "high modulus (low elongation)" belt is.
[0005] From this perspective, power transmission belts are classified into grades according to the level of elastic modulus. The elastic modulus of a belt is most significantly affected by the choice of fiber material used for the core wire, and in the case of a V-ribbed belt, typical core wires are generally made of polyester fiber as the "standard" grade, aramid fiber as a grade with a higher modulus (low elongation), and aliphatic polyamide (nylon) fiber as a grade with a lower modulus than the standard. In this specification, a V-ribbed belt with a lower modulus (high elongation) grade than the standard is referred to as a "low modulus belt."
[0006] In other words, a "low modulus belt" is a belt that uses a core wire mainly made of aliphatic polyamide fiber, which has a lower elastic modulus than a standard V-ribbed belt (core wire made of polyester fiber), and ensures the slight elongation (about 1 to 5%) necessary for attachment to a pulley.
[0007] Next, a method for mounting a V-ribbed belt on a pulley will be described. The following methods are used to mount a V-ribbed belt on a pulley.
[0008] (A) Tension is applied to a relaxed belt suspended between two or more pulleys by pushing or pulling the belt with a tensioner (tension pulley). (B) With the belt suspended between two or more pulleys in a relaxed state, tension is applied to the belt by moving at least one pulley shaft to increase the distance between the pulley shafts. (C) A belt that is slightly shorter than the layout circumference between the pulleys is suspended on one pulley, and while the belt is stretched (by about 1 to 5%) using a jig, the belt is fitted onto the other pulleys (stretch fitting method using a jig).
[0009] Among these, the above method (C), in which the belt is fitted onto other pulleys while being stretched using a jig, cannot be performed with a V-ribbed belt with a high modulus standard (with polyester fiber core). A belt that has the slight stretch required for this purpose is a "low modulus belt."
[0010] Regarding low modulus belts, Patent Document 1 discloses a power transmission belt (low modulus belt) characterized in that it has a reference circumference that is 2.0 to 3.5% shorter than the layout circumference of two or more rotating bodies (pulleys) that are arranged apart from each other and on which the power transmission belt is to be attached, and that the tension in the circumferential direction when attached to the rotating bodies is 30 to 150 N / rib.
[0011] This power transmission belt can maintain sufficient tension even after being attached to a rotating body, and does not stretch at an early stage after the start of driving of the power transmission mechanism including the power transmission belt and the rotating body, thereby ensuring reliable power transmission. In addition, a low modulus belt has the advantage that a sudden drop in tension is suppressed compared to a belt with a high modulus, and that a method of attaching the belt to a pulley layout that does not use a tensioning mechanism (tension pulley, tensioner, etc.) while keeping the center distance of the pulley to be attached fixed (the stretching attachment method using a jig described above in (C)) can be used. The adoption of this method eliminates the need for a tensioning mechanism or a center distance expanding mechanism as described above in (A) and (B), contributing to a lighter engine and lower costs. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2011-012790 A Summary of the Invention [Problem to be solved by the invention]
[0013] Patent Document 1 discloses that in a low modulus belt, by ensuring that the tension of the belt when installed is at a certain level or higher, it is possible to maintain sufficient tension after the belt is installed in the pulley layout.
[0014] However, in the case of the low modulus belt described in Patent Document 1, the tension of the belt when mounted can be maintained at a certain level or higher using the stretch mounting method using a jig, which prevents a sudden drop in tension after mounting to the pulley layout and makes it possible to maintain sufficient tension only when the belt is stored in a relatively low humidity environment (e.g., 23°C x 50%) and mounted to the pulley layout.
[0015] On the other hand, it was found that when a belt stored in a relatively high humidity environment (e.g., 23°C x 90%) is mounted on the pulley layout, there is a possibility that the belt will not be able to maintain sufficient belt tension during operation (i.e., the belt tension retention rate will be significantly reduced) compared to when a belt stored in a relatively low humidity environment (e.g., 23°C x 50%) is mounted on the pulley layout.
[0016] This was believed to be due to a decrease in the belt's physical properties (modulus) caused by the absorption of water by the cord (aliphatic polyamide fiber).
[0017] An object of the present invention is to provide a V-ribbed belt that is stretchable in the longitudinal direction and can maintain sufficient tension during operation even when stored in a high humidity environment and then mounted on a pulley layout by a stretch mounting method using a jig. [Means for solving the problem]
[0018] In order to solve the above problems, the present invention provides a V-ribbed belt including an annular belt body having a plurality of ribs extending along the belt longitudinal direction formed in an inner peripheral compressed layer, and a core wire embedded in the belt body along the longitudinal direction of the belt body, the core wire is a twisted cord formed of fibers including aliphatic polyamide fibers, The stress required to stretch the V-ribbed belt by 3.5% is 290 to 360 N per rib, and the belt dry heat shrinkage stress, defined as the stress (N) per five core wires generated after applying an initial load of 147 N to the V-ribbed belt and leaving it in an atmosphere at 100°C for 30 minutes, is 125 to 200 N.
[0019] According to the above configuration, a twisted cord made of fibers containing aliphatic polyamide fibers is used as a low modulus belt, and the stress required to stretch the V-ribbed belt by 3.5% (3.5% modulus) is kept at a relatively low level of 290 to 360 N / rib, resulting in the effect that the V-ribbed belt can be easily attached by a stretch-mounting method using a jig to a drive system in which the layout circumference between pulleys is slightly longer than the standard circumference of the V-ribbed belt. At the same time, despite the above modulus being kept at a relatively low level, the belt dry heat shrinkage stress is ensured at a relatively high level of 125 to 200 N. Therefore, not only when a V-ribbed belt stored in a relatively low humidity environment (e.g., 23°C x 50%) is attached to a pulley layout using the stretch-mounting method with a jig, but also when a V-ribbed belt (whose core wire portion has absorbed water) stored in a relatively high humidity environment (e.g., 23°C x 90%) is attached to a pulley layout using the stretch-mounting method with a jig, it is possible to obtain the effect of suppressing a sudden decrease in tension during running and maintaining sufficient belt tension (in detail, the modulus decreases due to water absorption by the core wire, making it prone to elongation, but since the shrinkage stress is ensured at a sufficiently large level, it is possible to suppress the elongation of the V-ribbed belt and suppress a decrease in the belt tension retention rate).
[0020] Further, in the above V-ribbed belt, at least a portion of the rib has a friction transmission surface capable of contacting a pulley around which the V-ribbed belt is wound, The friction transmission surface may be characterized in that it has a surface layer laminated on a compression layer.
[0021] According to the above configuration, the properties of the frictional power transmission surface can be modified according to the required characteristics. Furthermore, even if a V-ribbed belt having a surface layer on the frictional power transmission surface is attached to a pulley layout by a stretch-attaching method using a jig, it is possible to obtain the effect of suppressing a sudden drop in tension during running and maintaining sufficient belt tension.
[0022] Moreover, the present invention may be characterized in that in the above V-ribbed belt, the surface layer is a fiber layer, a coating layer, a rubber layer, or a resin layer.
[0023] According to the above-mentioned configuration, the surface layer, which has high adhesion to the compressed layer and is easily integrated with the compressed layer, can be provided by a simple method.
[0024] The present invention also relates to the above V-ribbed belt, and two or more pulleys spaced apart from each other to which the V-ribbed belt is attached. The power transmission mechanism is characterized in that a reference circumferential length of the V-ribbed belt before installation is shorter than a layout circumferential length of the two or more pulleys by 1.0 to 3.5%.
[0025] According to the above configuration, a twisted cord made of fibers containing aliphatic polyamide fibers is used as the core wire of the low modulus belt, and the stress required to stretch the belt by 3.5% (3.5% modulus) is kept at a relatively low level of 290 to 360 N / rib. Therefore, the belt can be easily attached to a drive system in which the layout circumference of two or more pulleys arranged apart from each other is 1.0 to 3.5% longer than the reference circumference of the belt by a stretch-mounting method using a jig, and sufficient tension can be applied to the belt.
[0026] The present invention also provides a method for producing the above V-ribbed belt, A crosslinking process is a process for forming a crosslinked belt precursor by integrating laminated materials constituting an uncrosslinked belt precursor including a core wire, which is a prototype of the V-ribbed belt, The method includes a step of expanding an expandable bladder at a predetermined expansion rate to expand an outer diameter of the bladder, and stretching the core wire wound around the outer periphery of the bladder in accordance with the expansion of the outer diameter of the bladder, The elongation rate of the precursor including the core wire in the crosslinking step is in the range of 1.0 to 4.0%.
[0027] According to the above manufacturing method, the manufactured V-ribbed belt naturally has residual stress resulting from the tension applied to the core wire when it is wound (core wire winding tension) as well as residual stress resulting from the stretching of the bladder during the crosslinking process. This ensures that the dry heat shrinkage stress is at a relatively high level. In other words, even if a V-ribbed belt stored in a high humidity environment (where the core wire portion has absorbed water) is mounted on a pulley layout with a fixed center distance and no tension applying mechanism, it is possible to reliably obtain the effect of suppressing a sudden drop in tension during running and maintaining sufficient belt tension during running (suppressing a drop in belt tension retention rate). Effect of the Invention
[0028] It is possible to provide a V-ribbed belt that is stretchable in the longitudinal direction and can maintain sufficient tension during operation even when stored in a high humidity environment and then attached to a pulley layout by a stretch-attaching method using a jig. [Brief description of the drawings]
[0029] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a V-ribbed belt of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of a V-ribbed belt 1 having a surface layer. [Diagram 3] FIG. 3 is an explanatory diagram of the configuration of the power transmission mechanism and a method of mounting the V-ribbed belt between pulleys. [Figure 4] FIG. 4 is an explanatory diagram of a method for installing a V-ribbed belt between pulleys. [Diagram 5] FIG. 5 is an explanatory diagram of a method for installing a V-ribbed belt between pulleys. [Figure 6] FIG. 6 is an explanatory diagram of a method for installing a V-ribbed belt between pulleys. [Figure 7] FIG. 7(a) is a schematic perspective view showing an example of an inner mold of a belt forming apparatus for producing a V-ribbed belt, and FIG. 7(b) is an enlarged schematic cross-sectional view of the upper portion thereof. [Figure 8] FIG. 8 is an explanatory diagram showing the state of the belt forming device in the forming process. [Figure 9] FIG. 9 is a diagram showing a belt molding apparatus in which an inner mold is combined with an outer mold, and more specifically, FIG. 9 is a schematic oblique view (a) showing the process of inserting the inner mold with the uncrosslinked belt precursor attached thereto into the outer mold, and FIG. 9 is a partially enlarged schematic cross-sectional view (b) showing the state in which the inner mold has been inserted into the outer mold. [Figure 10] FIG. 10 shows the state of the belt forming apparatus during the crosslinking process, and in detail, it is a schematic perspective view (a) of the state in which the bladder of the belt forming apparatus is inflated with the inner mold inserted into the outer mold, and a partially enlarged schematic cross-sectional view (b) of the same. [Figure 11] FIG. 11 shows a belt forming apparatus in a finishing process, and is a schematic oblique view (a) showing the process of removing the inner mold from the belt forming apparatus, and a partially enlarged schematic cross-sectional view (b) showing the state after the inner mold has been removed from the belt forming apparatus. [Figure 12] FIG. 12 is a conceptual diagram illustrating a manufacturing method of a V-ribbed belt. [Figure 13] FIG. 13 is a graph showing the relationship between the belt elongation rate in the crosslinking step and the belt dry heat shrinkage stress for the V-ribbed belts of Examples 1 to 8 and Comparative Examples 1, 3 and 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] (Embodiment) Hereinafter, an example of an embodiment of the present invention will be described with reference to the drawings.
[0031] (V-ribbed belt 1) 1, the V-ribbed belt 1 of this embodiment has a configuration in which a compression layer 2, an adhesive layer 4 in which a core wire 6 is embedded, and an extension layer 5 made of a fabric (woven fabric, knitted fabric, nonwoven fabric, etc.) or a rubber composition are laminated in this order from the lower surface (inner peripheral surface) of the belt to the upper surface (outer peripheral surface) of the belt. A plurality of grooves with a V-shaped cross section extending in the belt longitudinal direction are formed in the compression layer 2, and a plurality of ribs 3 (four in the example shown in FIG. 1) with a V-shaped cross section (inverted trapezoid) are formed between these grooves, and two inclined surfaces (surfaces) of each of these ribs 3 form frictional transmission surfaces that contact a pulley to transmit power (frictional transmission).
[0032] The adhesive layer 4 is provided for the purpose of improving the adhesion between the tension layer 5 and the compression layer 2, but is not essential. The adhesive layer 4 may be formed in such a manner that the entire core wire 6 is embedded in the adhesive layer 4, or the core wire 6 is embedded between the adhesive layer 4 and the tension layer 5 or between the adhesive layer 4 and the compression layer 2. As shown in FIG. 2, the adhesive layer may not be provided. At least the compression layer 2 may be formed of a rubber composition described in detail below, and the adhesive layer 4 may be formed of a conventional rubber composition used as the adhesive layer 4. The tension layer 5 may be formed of a conventional fabric or rubber composition used as the tension layer 5, and may be the same rubber composition as the compression layer 2 or a different rubber composition.
[0033] As another embodiment, as shown in Fig. 2, the surface of the rib 3, i.e., the surface of the compressed layer 2, may be coated (laminated) with a surface layer 7. In this embodiment, the surface layer 7 forms a friction transmission surface that contacts the pulley. Similarly, the surface of the rib 3 of the V-ribbed belt 1 shown in Fig. 1, i.e., the surface of the compressed layer 2, may be coated (laminated) with a surface layer 7.
[0034] As described above, the V-ribbed belt of the present invention is not particularly limited as long as it comprises a ring-shaped belt body 10 having a plurality of ribs 3 extending along the belt longitudinal direction formed in the inner compressed layer 2, and a core wire 6 embedded in the belt body 10 along the longitudinal direction of the belt body 10.
[0035] (Compression layer 2, tension layer 5, adhesive layer 4: rubber composition) The compression layer 2, the adhesive layer 4, and the tension layer 5 may be formed of a rubber composition containing a rubber component. As the rubber component, a vulcanizable or crosslinkable rubber may be used, and examples thereof include diene rubber (natural rubber, isoprene rubber, butadiene rubber, chloroprene rubber, styrene butadiene rubber, acrylonitrile butadiene rubber (nitrile rubber), hydrogenated nitrile rubber, etc.), ethylene-α-olefin elastomer, chlorosulfonated polyethylene rubber, alkylated chlorosulfonated polyethylene rubber, epichlorohydrin rubber, acrylic rubber, silicone rubber, urethane rubber, and fluororubber. These rubber components may be used alone or in combination of two or more. Preferred rubber components are ethylene-α-olefin elastomer (ethylene-propylene copolymer (EPM), ethylene-propylene-diene terpolymer (EPDM), etc.) and chloroprene rubber. Furthermore, ethylene-α-olefin elastomers (ethylene-propylene copolymer (EPM), ethylene-propylene-diene terpolymer (EPDM), etc.) are particularly preferred because they have ozone resistance, heat resistance, cold resistance, and weather resistance and can reduce the belt weight. When the rubber component contains an ethylene-α-olefin elastomer, the proportion of the ethylene-α-olefin elastomer in the rubber component may be 50% by mass or more (particularly about 80 to 100% by mass), and 100% by mass (only ethylene-α-olefin elastomer) is particularly preferred.
[0036] The rubber composition may further contain short fibers. Examples of the short fibers include polyolefin fibers (polyethylene fibers, polypropylene fibers, etc.), polyamide fibers (polyamide 6 fibers, polyamide 66 fibers, polyamide 46 fibers, aramid fibers, etc.), polyalkylene arylate fibers (e.g., polyethylene terephthalate (PET) fibers, polytrimethylene terephthalate (PTT) fibers, polybutylene terephthalate (PBT) fibers, polyethylene naphthalate (PEN) fibers, etc.) 2-4 Alkylene C 8-14Examples of the short fibers include synthetic fibers such as arylate fibers, vinylon fibers, polyvinyl alcohol fibers, and polyparaphenylene benzobisoxazole (PBO) fibers; natural fibers such as cotton, hemp, and wool; and inorganic fibers such as carbon fibers. These short fibers can be used alone or in combination of two or more. In order to improve dispersibility and adhesiveness in the rubber composition, the short fibers may be subjected to a conventional adhesive treatment (or surface treatment) in the same manner as the core wire 6.
[0037] The rubber composition may further contain conventional additives. Examples of conventional additives include vulcanizing agents or crosslinking agents (sulfur-based vulcanizing agents, organic peroxides, etc.), co-crosslinking agents (bismaleimides, etc.), vulcanization assistants or vulcanization accelerators (thiuram-based accelerators, etc.), vulcanization retarders, metal oxides (zinc oxide, magnesium oxide, calcium oxide, barium oxide, iron oxide, copper oxide, titanium oxide, aluminum oxide, etc.), reinforcing agents (e.g., carbon black, silicon oxides such as hydrated silica), fillers (clay, calcium carbonate, talc, etc.), and the like. , mica, etc.), softeners (e.g., oils such as paraffin oil and naphthenic oil), processing agents or processing aids (stearic acid, metal stearates, wax, paraffin, fatty acid amides, etc.), anti-aging agents (antioxidants, heat anti-aging agents, flex crack inhibitors, ozone degradation inhibitors, etc.), colorants, tackifiers, plasticizers, coupling agents (silane coupling agents, etc.), stabilizers (ultraviolet absorbers, heat stabilizers, etc.), flame retardants, antistatic agents, etc. These additives can be used alone or in combination of two or more. The metal oxide may act as a crosslinking agent. In particular, the rubber composition constituting the adhesive rubber layer 4 may contain an adhesion improver (resorcinol-formaldehyde co-condensate, amino resin, etc.).
[0038] The rubber compositions constituting the compressible layer 2, the adhesive layer 4, and the tensile layer 5 may be the same as or different from each other. Similarly, the short fibers contained in the compressible layer 2, the adhesive layer 4, and the tensile layer 5 may be the same as or different from each other.
[0039] (Stretch layer 5: fabric) The tensile layer 5 may be formed of a fabric. The fabric may be formed of a fabric material (preferably a woven fabric) such as a woven fabric, a wide-angle woven fabric, a knitted fabric, or a nonwoven fabric, and if necessary, may be subjected to an adhesion treatment such as a treatment with an RFL treatment liquid (dipping treatment, etc.), a friction treatment in which a rubber composition for the adhesive layer is rubbed into a fabric material, or a lamination (coating) of the rubber composition for the adhesive layer and the fabric material, and then laminated to the compression layer 2 and / or the adhesive layer 4 in the above-mentioned form.
[0040] (Surface layer 7) In the V-ribbed belt 1 in which the surface of the rib 3, i.e., the surface of the compressed layer 2, is coated (laminated) with a surface layer 7, the surface layer 7 which coats the surface of the compressed layer 2 and constitutes the friction transmission surface in contact with the pulley, need only have a form (structure) that can be laminated onto the compressed layer 2, and the properties of the friction transmission surface can be modified by appropriately selecting the form (structure) according to the required characteristics of the belt.
[0041] Examples of the surface layer 7 include a fiber layer, a resin layer, a rubber layer, and a coating layer. Examples of the fiber layer include a woven fabric layer and a flocked layer. Examples of the resin layer include a skin layer (film layer) made of resin alone, which is formed by melting and solidifying a thermoplastic resin such as polyethylene, and a fiber-resin mixed skin layer (film layer) in which fibers are mixed in. For example, a skin layer (surface layer 7) made of thermoplastic resin integrated with the compressed layer 2 can be formed by disposing a nonwoven fabric made of thermoplastic resin fibers on the surface of the compressed layer 2, melting the nonwoven fabric by applying pressure and heat in a crosslinking process described later, and then cooling and solidifying it.
[0042] The rubber layer is a crosslinked product of a rubber composition for a surface layer, which is different from the rubber composition for a compression layer, and which contains various compounding agents for adjusting the properties of the friction transmission surface. Examples of compounding agents include inorganic particles (metal carbonates, clay, talc, etc.) and resin particles (polyolefin-based resin particles, fluorine-based resin particles, etc.) that act as lubricants to stabilize the friction state, plasticizers for increasing hydrophilicity (wettability with water), surfactants, hydrophilic resin particles (polyvinyl alcohol-based resin particles, polyvinylpyrrolidone-based resin particles, etc.), and short fibers for lowering the friction coefficient of the friction transmission surface. An uncrosslinked rubber sheet of a rubber composition for a surface layer containing these compounding agents is placed on the surface of the compression layer 2, and a surface rubber layer (surface layer 7) integrated with the compression layer 2 can be formed by applying pressure and heat in a crosslinking process described later.
[0043] Examples of the coating layer include an adhesion layer formed by scattering or spraying various particles exemplified as compounding agents of the rubber layer, and a coating layer formed by applying a liquid composition in which various particles or a rubber composition containing various particles is dispersed in a solvent. As a method for scattering or spraying various particles, a conventional powder coating method (for example, an electrostatic coating method in which the coating is sprayed by a spray, or a fluidized bed dip coating method in which the coating is immersed in a fluidized bed of particles) can be used. As a method for applying a liquid composition, a conventional method, for example, a coater method, a casting method, a dip method, a spray method, a spinner method, etc. can be used. Of these methods, the coater method and the spray method can be used. After performing these operations (scattering, spraying, coating) on the surface of the compression layer 2, a coating layer (surface layer 7) integrated with the compression layer 2 can be formed by pressurizing and heating in a crosslinking process described later.
[0044] Among these, a fiber layer is preferably used, and a fabric layer is particularly preferred, from the viewpoint of high performance such as noise resistance, abrasion resistance, and low friction coefficient. A fabric layer (surface layer 7) integrated with the compressible layer 2 can be formed by disposing a fabric on the surface of the compressible layer 2 and applying pressure and heat in the crosslinking process described below. The fabric layer is usually made of at least one type of fabric selected from knitted fabric, woven fabric, nonwoven fabric, etc. Among these fabrics, knitted fabric is preferably used because of its excellent durability and extensibility. Since knitted fabric has excellent elasticity, it is suitable for laminating the fabric layer along the contour (rib shape, etc.) of the friction transmission surface. Furthermore, it expands following the flow of rubber in the crosslinking process, and can prevent the rubber composition of the compressible layer 2 from being exposed to the friction transmission surface.
[0045] The knitted fabric may be weft knitted or warp knitted. Weft knitting has excellent elasticity, so when the knitted fabric is weft knitted, the knitted fabric can be attached more easily to the friction transmission surface on which the rib shape is formed. Examples of weft knitted single-layer knitted fabrics include plain knitted fabrics (plain knitted fabrics), elastic knitted fabrics, tuck knitted fabrics, and pearl knitted fabrics, while examples of multi-layer knitted fabrics include smooth knitted fabrics, interlock knitted fabrics, double rib knitted fabrics, single pique knitted fabrics, ponte roma knitted fabrics, milano rib knitted fabrics, double jersey knitted fabrics, and pique knitted fabrics (front pique knitted fabrics, back pique knitted fabrics, and both sides pique knitted fabrics). Examples of warp knitted single-layer knitted fabrics include single denby and single cord knitted fabrics, while examples of multi-layer knitted fabrics include half tricot, double denby, double atlas, double cord knitted fabrics, and double tricot knitted fabrics.
[0046] In addition, the yarns used to knit the knitted fabric may be yarns made of a single type of fiber (single yarns) or yarns made of multiple types of fibers (composite yarns). Although each of these can be used alone, it is preferable to use them in combination because they can impart different properties to the knitted fabric. For example, the knitted fabric may be knitted with polyester-based composite yarns and cellulose-based natural spun yarns (e.g., cotton yarns). The polyester-based composite yarns are composite yarns containing polyester fibers and fibers other than polyester fibers. The polyester-based composite yarns may be bulky processed yarns. The bulky processed yarns are processed yarns that have a large cross-sectional bulk by causing the fibers to shrink (shrinkage) or by covering the core yarn with another yarn. The bulky processed yarns include conjugated yarns, covered yarns, shrink-processed yarns, woolly processed yarns, taslan processed yarns, and interlaced processed yarns, and conjugated yarns and covered yarns are preferable as polyester-based composite yarns.
[0047] Conjugate yarns have a cross-sectional structure in which two types of polymers are bonded together in the fiber axis direction. When heat is applied during manufacturing or processing, shrinkage occurs due to the difference in the shrinkage rate of the two polymers, resulting in a bulky yarn. For example, there are conjugate yarns made of polytrimethylene terephthalate (PTT) and polyethylene terephthalate (PET) (PTT / PET conjugate yarns) and conjugate yarns made of polybutylene terephthalate (PBT) and polyethylene terephthalate (PET) (PBT / PET conjugate yarns). Covered yarns are yarns that increase the bulk of the cross-section of the entire yarn by covering (covering) the periphery of the core yarn with another yarn. For example, there are covered yarns (PET / PU covered yarns) in which a highly elastic polyurethane (PU) yarn is used as a core and its surface is covered with polyethylene terephthalate (PET), and covered yarns (PA / PU covered yarns) in which a PU core is used and its surface is covered with polyamide (PA). Of these, as the polyester composite yarn contained in the knitted fabric, PTT / PET conjugate yarn or PET / PU covered yarn, which have excellent elasticity and abrasion resistance, are preferred.
[0048] Examples of natural spun cellulose yarns include yarns spun from cellulose fibers (pulp fibers) derived from natural plants, such as bamboo fiber, sugarcane fiber, seed hair fiber (cotton fiber (cotton linter), kapok, etc.), ginseng bark fiber (e.g., hemp, paper mulberry, mitsumata, etc.), leaf fiber (e.g., Manila hemp, New Zealand hemp, etc.), cellulose fibers derived from animals, such as wool, silk, and sea squirt cellulose, bacterial cellulose fiber, and algae cellulose. Of these, cotton fiber is preferred because of its excellent water absorbency.
[0049] The knitting ratio of the cellulose-based natural spun yarn is preferably 50 to 95% by mass. The knitted fabric may be single-layered or multi-layered, and a multi-layered knitted fabric is preferred to more reliably prevent the rubber of the belt body 10 from seeping out.
[0050] By knitting a knitted fabric containing a bulky yarn, the bulkiness of the knitted fabric can be increased. 3 / g or more is preferable, and 2.4 cm 3 / g or more. The upper limit is not particularly limited, but is, for example, 4.0 cm 3 / g or less, or 3.5 cm 3 / g or less. 3 / g) is the mass per unit area (g / cm) of the thickness of the knitted fabric (cm) 2 In order to more reliably prevent the rubber of the belt body 10 from seeping out onto the frictional power transmission surface, it is also preferable to provide a bulky layer of the knitted fabric on the frictional power transmission surface.
[0051] When the knitted fabric has a multi-layered structure, the water absorption at the frictional power transmission surface can be further increased by distributing a large amount of cellulose-based natural spun yarn, which has excellent water absorption properties, in the thickness direction of the knitted fabric in the layer on the frictional power transmission surface side. When knitting a multi-layered knitted fabric, it is also possible to knit one layer with only cellulose-based natural spun yarn or with cellulose-based natural spun yarn and polyester-based composite yarn, and knit the other layer with only polyester-based composite yarn, thereby knitting a multi-layered knitted fabric in which one layer has a large amount of cellulose-based natural spun yarn. By disposing the layer with a large amount of cellulose-based natural spun yarn on the frictional power transmission surface side, the water absorption at the frictional power transmission surface can be further increased.
[0052] In addition, the knitted fabric may be subjected to an adhesive treatment in order to improve the adhesiveness with the rubber composition constituting the compression layer 2. Examples of such adhesive treatment of the knitted fabric include immersion treatment in a resin-based treatment liquid in which an epoxy compound or an isocyanate compound is dissolved in an organic solvent (toluene, xylene, methyl ethyl ketone, etc.), immersion treatment in a resorcin-formalin-latex liquid (RFL liquid), and immersion treatment in a rubber paste in which a rubber composition is dissolved in an organic solvent. Other adhesive treatment methods include, for example, a friction treatment in which the knitted fabric and the rubber composition are passed through a calendar roll to imprint the rubber composition on the knitted fabric, a spreading treatment in which rubber paste is applied to the knitted fabric, and a coating treatment in which a rubber composition is laminated on the knitted fabric. By subjecting the knitted fabric to an adhesive treatment in this way, it is possible to improve the adhesiveness with the compression layer 2 and prevent the knitted fabric from peeling off during the running of the V-ribbed belt 1. In addition, by subjecting the knitted fabric to an adhesive treatment, it is also possible to improve the abrasion resistance of the ribs 3.
[0053] The fiber layer may be a flocked layer. The flocked layer can be formed on the surface of the compressed layer 2 by using a known electrostatic flocking machine.
[0054] As described above, by having the surface layer 7 on the friction transmission surface of the V-ribbed belt 1, even when the V-ribbed belt 1 is attached to a pulley layout by the stretch-attaching method using a jig described later, it is possible to suppress a sudden drop in tension during running and to obtain the effect of maintaining sufficient belt tension.
[0055] (Core 6) In the belt body 10 (adhesive layer 4) of the V-ribbed belt 1, a core wire 6 functioning as a tension member is embedded along the belt longitudinal direction. The core wire 6 is usually arranged in a spiral shape, with twisted yarn cords extending approximately parallel to the belt longitudinal direction and extending in parallel at a predetermined interval in the belt width direction. When arranged in a spiral shape, the angle of the core wire 6 with respect to the belt longitudinal direction may be, for example, 5° or less, and from the viewpoint of belt running properties, the closer to 0° the more preferable. For example, in the embodiment shown in FIG. 1, the core wire 6 is embedded at a predetermined interval (or pitch) (or at equal intervals) from one end to the other end in the belt width direction of the adhesive layer 4. The interval (spinning pitch), which is the distance between the centers of adjacent core wires 6, may be larger than the core wire diameter depending on the core wire diameter, and may be, for example, about 0.5 to 2 mm, preferably 0.7 to 1.7 mm, and more preferably 0.8 to 1.5 mm.
[0056] For the core wire 6, a twisted cord containing aliphatic polyamide fibers (nylon fibers) in the raw yarn is used in order to relatively lower the elastic modulus (compared to standard grade polyester fibers). Examples of aliphatic polyamide fibers include polyamide 6, polyamide 66, and polyamide 46. For example, the above twisted cord having a total fineness of 4800 to 7200 dtex can be used, which is obtained by plying filament groups of 800 to 1200 dtex with a first twist number of 8 to 13 times / 10 cm and a first twist number of 15 to 30 times / 10 cm. The fibers constituting the twisted cord may be aliphatic polyamide fibers alone or in combination with other fibers.
[0057] The average diameter (average wire diameter) of the core wire 6 may be, for example, about 0.3 to 1.5 mm, preferably about 0.5 to 1.3 mm, and more preferably about 0.7 to 1.2 mm.
[0058] (3.5% modulus and dry heat shrinkage stress of V-ribbed belt 1) The V-ribbed belt 1 has a stress (3.5% modulus) required to elongate the V-ribbed belt 1 by 3.5% of 290 to 360 N per rib 3 (290 to 360 N / rib) (see examples described later).
[0059] Furthermore, the V-ribbed belt 1 has a belt dry heat shrinkage stress of 125 to 200 N (see examples, etc., described later) which is defined as the stress (N) per five core wires 6 generated after applying an initial load of 147 N to the V-ribbed belt 1 (a measurement sample consisting of five core wires 6 cut into strips from the V-ribbed belt 1, as described in detail later) and leaving it in an atmosphere at 100°C for 30 minutes.
[0060] When the 3.5% modulus of the V-ribbed belt 1 is less than 290 N / rib and / or the belt dry heat shrinkage stress is less than 125 N, even if the tension of the V-ribbed belt 1 when installed in a pulley layout is maintained at a certain level or above (30 to 150 N / rib), when the V-ribbed belt 1 stored in a relatively high humidity environment (for example, 23°C x 90%) is installed in a pulley layout using a stretching installation method with a jig (see the method of installation on a pulley described below), the belt tension drops significantly during operation, making it difficult to maintain sufficient tension of the V-ribbed belt 1 during operation after installation in the pulley layout, and depending on the degree of load, slippage or noise may occur when the V-ribbed belt 1 is running. On the other hand, when the belt dry heat shrinkage stress of the V-ribbed belt 1 exceeds 200 N, the belt dimensional shrinkage over time (including dry heat shrinkage) tends to become excessive. Also, when the 3.5% modulus of the V-ribbed belt 1 is greater than 360 N, it becomes difficult to attach the V-ribbed belt 1 by stretching it 3.5% using the stretch attachment method using a jig. Considering the above reasons, in this embodiment, the 3.5% modulus and the dry heat shrinkage stress of the V-ribbed belt 1 are set within the above ranges.
[0061] (How to install a V-ribbed belt on a pulley) Next, the configuration of a power transmission mechanism 20 according to one embodiment of the present invention and a method of mounting the V-ribbed belt 1 on pulleys 21 and 22 will be described with reference to FIGS.
[0062] The power transmission mechanism 20 is applied to, for example, an accessory drive system of an automobile engine, and includes a V-ribbed belt 1 and two pulleys 21, 22 of the same diameter (pulley layout). The shafts of the pulleys 21, 22 are fixed, that is, the distance between these shafts cannot be changed. A plurality of grooves are formed on the outer circumferential surfaces of the pulleys 21, 22 along the circumferential direction, which can engage with the ribs 3 of the V-ribbed belt 1. The V-ribbed belt 1 is attached to the pulleys 21, 22 by winding the belt around and spanning between the pulleys 21, 22, with the ribs 3 on the inner circumferential side and the tension layer 5 on the outer circumferential side.
[0063] One pulley 21 is a drive pulley connected to the output shaft of the engine (the crankshaft of a reciprocating engine, the eccentric shaft of a rotary engine, etc.), and the other pulley 22 is a driven pulley attached to a driven shaft connected to various accessories (an air conditioner, a water pump, an alternator, etc.). When the drive pulley 21 rotates due to the torque of the output shaft, the V-ribbed belt 1 runs in conjunction with the rotation of the drive pulley 21. The driven pulley 22 rotates in conjunction with the running of the V-ribbed belt 1, thereby driving the various accessories.
[0064] One pulley 21 has a two-stage configuration and includes two pulleys 21a, 21b stacked in the axial direction. Each of the pulleys 21a, 21b has the same size and shape as the other pulley 22. These pulleys 21a, 21b are integral with each other and rotate together when the power transmission mechanism 20 is driven. The axial length of the pulleys 21a, 21b, 22 is approximately the same as the width of the V-ribbed belt 1, and the V-ribbed belt 1 is wound around the lower pulley 21b of one pulley 21 and the other pulley 22.
[0065] The V-ribbed belt 1 is attached to the pulleys 21 and 22, for example, by the following method. First, the layout peripheral length Lp of the pulleys 21 and 22 is obtained (obtaining step). Here, the "layout perimeter of the pulleys" refers to the length of a line (i.e., the path of the belt) formed in a ring shape along the outer periphery of two or more pulleys arranged at a distance from each other to which the belt is to be attached. In this embodiment, the "layout perimeter Lp of the pulleys 21, 22" refers to the length of a line (i.e., the path of the V-ribbed belt 1) formed in a ring shape along the outer periphery of the pulleys 21, 22 arranged at a distance from each other to which the V-ribbed belt 1 is to be attached. In this embodiment, the pulleys 21, 22 have the same diameter and the V-ribbed belt 1 extends in parallel between the pulleys 21, 22, so that the layout perimeter Lp is roughly calculated as the sum of the semicircular circumference of each pulley 21, 22 and twice the center distance between the pulleys 21, 22. The layout perimeter Lp may be obtained by calculation or may be obtained by actual measurement or the like.
[0066] Next, a V-ribbed belt 1 having a reference circumferential length Lb that is 1.0 to 3.5% shorter than the layout circumferential length Lp acquired in the above acquisition step is prepared (preparation step). Here, the "reference circumference of the belt" refers to the length of the belt in the longitudinal direction when the belt is wound around two flat pulleys (pulleys with no grooves on the outer circumferential surface) with the surface on which the ribs are formed facing outward, and tension is applied to the belt to the extent that the longitudinal deflection of the belt is removed. In this embodiment, the "reference circumference of the belt Lb" refers to the length of the V-ribbed belt 1 in the longitudinal direction when the V-ribbed belt 1 is wound around two flat pulleys (rotating bodies with no grooves on the outer circumferential surface) with the surface on which the ribs 3 are formed facing outward, and tension is applied to the V-ribbed belt 1 to the extent that the longitudinal deflection of the V-ribbed belt 1 is removed. In addition, "the reference circumference Lb is 1.0 to 3.5% shorter than the layout circumference Lp" means that the sum of the reference circumference Lb and the length of 1.0 to 3.5% of the reference circumference Lb is equal to the layout circumference Lp.
[0067] Next, the V-ribbed belt 1 prepared in the preparation step is attached to the pulleys 21, 22 while being stretched in the longitudinal direction (attachment step). The mounting step may be performed using a jig 50, for example, as shown in Figs. 4 to 6. That is, first, as shown in Fig. 4, a connecting portion 60a of a wrench 60 is fixed to a boss 21c of one pulley 21, and a curved portion 51 of the jig 50 having a curved shape along the outer periphery of the pulley 21 is aligned along the outer periphery of the upper pulley 21a, and the jig 50 is disposed so that a line connecting the axes 21x, 22x of the pulleys 21, 22 and a line connecting the axis 21x and the jig 50 are substantially perpendicular in a plan view. Then, the V-ribbed belt 1 is inserted between the curved portion 51 and the protruding portion 52 of the jig 50 and is placed in contact with the guide 53, and is then stretched over the other pulley 22 and the connecting portion 60a of the wrench 60. The guide 53 is formed by rounding a corner of the main body 50a of the jig 50 (the lower end side of the surface from which the protruding portion 52 protrudes in Fig. 4). The V-ribbed belt 1 is bent by the guide 53, and the portion below the guide 53 is disposed along the outer periphery of the lower pulley 21b.
[0068] Thereafter, while the jig 50 is fixed to the upper pulley 21a, the pulley 21 is rotated by approximately 110° in the A direction using the wrench 60 (see FIG. 5). At this time, the upper pulley 21a and the lower pulley 21b rotate together, and the jig 50 fixed to the upper pulley 21a also rotates by approximately 110° in the A direction about the axis 21x. During this rotation, a tensile force in the longitudinal direction is gradually applied to the V-ribbed belt 1, and the tension generated in the V-ribbed belt 1 at this time acts to press the jig 50 against the upper pulley 21a. In the state of FIG. 5, the V-ribbed belt 1 is separated from the connecting portion 60a of the wrench 60, and the portion of the V-ribbed belt 1 corresponding to the trajectory of the rotation of the jig 50 is wound around the lower pulley 21b.
[0069] Thereafter, when the pulley 21 is further rotated by approximately 10° in the direction A using the wrench 60 from the state shown in Fig. 5, the V-ribbed belt 1 moves downward from between the curved portion 51 and the protruding portion 52 of the jig 50 so that the elastic energy stored by the tensile force is minimized, and moves away from the jig 50 and the upper pulley 21a to be wound around the lower pulley 21b, as shown in Fig. 6. Thereafter, the jig 50 is withdrawn.
[0070] In the above-described installation step, the tension in the belt longitudinal direction when the V-ribbed belt 1 is installed on the pulleys 21, 22 (tension of the V-ribbed belt 1 when installed) is at a level of approximately 100 to 250 N / rib. The V-ribbed belt 1 installed by the installation method of this embodiment is installed on the pulleys 21, 22 with its circumferential length stretched by 1.0 to 3.5% from the reference circumferential length and with a tension of 100 to 250 N / rib in the longitudinal direction.
[0071] If the tension of the V-ribbed belt 1 when installed is small, the V-ribbed belt 1 is likely to stretch in the longitudinal direction, making it difficult for the V-ribbed belt 1 to maintain sufficient tension after installation on the pulleys 21, 22. On the other hand, if the tension of the V-ribbed belt 1 when installed is large, installation of the V-ribbed belt 1 becomes difficult, and problems arise with the durability of the pulleys 21, 22 and the shafts to which they are attached.
[0072] According to the V-ribbed belt 1 and power transmission mechanism 20 of this embodiment, the above problem can be avoided by setting the tension of the V-ribbed belt 1 during installation to 100 to 250 N / rib.
[0073] Furthermore, by making the reference peripheral length Lb of the V-ribbed belt 1 1.0 to 3.5% shorter than the layout peripheral length Lp of the pulleys 21, 22, a method of attaching the V-ribbed belt 1 to the pulleys 21, 22 while stretching it using the jig 50 as described above can be used, that is, a method that does not require a tensioning mechanism or a mechanism for moving the center distance and that makes the attachment work easy.
[0074] The V-ribbed belt 1 is applied to an accessory drive system of an automobile engine. In this case, since a tensioning mechanism or a mechanism for changing the center distance is not required as described above, it can contribute to fuel saving and cost reduction by reducing the weight of the engine.
[0075] (Manufacturing method of V-ribbed belt 1) The V-ribbed belt 1 of this embodiment can be manufactured by a belt forming device including an outer mold 81 and an inner mold 71 that can be inserted into and detached from the hollow portion of the outer mold 81, as shown in FIGS.
[0076] As shown in Fig. 7, the shape of the inner mold 71, which is a metal mold, is columnar or cylindrical. A bladder 75 is attached to the outer circumferential surface of the inner mold 71. This bladder 75 is formed of a crosslinked body of a rubber composition that is stretchable and airtight. This bladder 75 is attached with the entire circumference of both end faces (upper end face and lower end face) in the longitudinal direction being in close contact with an upper end flange 72a and a lower end flange 72b, respectively. Therefore, the gap between the outer circumferential surface of the inner mold 71 and the inner circumferential surface of the bladder 75 is sealed by the flanges at both the upper and lower ends.
[0077] Furthermore, the inner mold 71 is provided with a fluid supply passage 73 that penetrates the upper end flange 72a and the inner mold 71. In the inner mold 71, when a fluid such as air is supplied between the outer peripheral surface of the inner mold 71 and the inner peripheral surface of the bladder 75 through this fluid supply passage 73, the bladder 75 expands outward as the fluid flows in. Furthermore, when no fluid is supplied from the fluid supply passage 73, the bladder 75 is in close contact with the outer peripheral surface of the inner mold 71.
[0078] As shown in Fig. 9, the outer die 81 has a cylindrical shape into which the inner die 71 can be inserted, and as shown in Fig. 9(b), molding convex parts 84 are formed on the inner peripheral surface which becomes the molding surface of the outer die 81. The molding convex parts 84 are formed in a mold shape (inverted shape) corresponding to the desired rib 3, and protrude over the entire inner peripheral surface of the outer die 81, with a large number of them being formed in parallel at predetermined regular intervals on the inner peripheral surface of the outer die 81 in a direction perpendicular to the circumferential direction.
[0079] The V-ribbed belt 1 of this embodiment is manufactured using the above-mentioned belt forming device, and in this specification, the method of manufacturing the V-ribbed belt of this embodiment is referred to as the "bladder expansion method." The following method can be exemplified as a first manufacturing method using the bladder expansion method. Specifically, the V-ribbed belt 1 is obtained through a molding step of molding an uncrosslinked belt precursor 10A, a crosslinking step of crosslinking the uncrosslinked belt precursor 10A, and a finishing step of manufacturing the V-ribbed belt 1 from a crosslinked belt precursor (belt sleeve 10B).
[0080] (molding process) The molding step is a step of forming an uncrosslinked belt precursor 10A using an inner mold 71 having a bladder 75 attached to its outer circumferential surface.
[0081] FIG. 8 shows the state of the belt forming device in the forming process, and in detail, it is a schematic perspective view (a) of the state in which the uncrosslinked belt precursor 10A is mounted on the inner mold 71 of FIG. 7, and an enlarged schematic cross-sectional view (b) of the upper part of the uncrosslinked belt precursor 10A. As shown in FIG. 8, the uncrosslinked belt precursor 10A is formed as a laminate of the core wire 6 wound in a spiral shape around the outer circumferential surface of the bladder 75 and the precursor sheet wound around the outer circumferential surface of the bladder 75. In the embodiment of FIG. 8, the precursor sheet uses at least two types of sheets including an uncrosslinked rubber sheet, and the lamination materials of the sheet 5a for forming the tension layer, the twisted yarn cord for forming the core wire 6, and the uncrosslinked rubber sheet 2a for forming the compression layer are wound and laminated from the inner circumferential side around the outer circumferential surface of the bladder 75 to form the uncrosslinked belt precursor 10A. The sheet 5a for forming the tension layer is made of a cloth or an uncrosslinked rubber sheet. In addition, when the core wire 6 is embedded in the adhesive layer 4, an uncrosslinked rubber sheet for forming an adhesive layer in which to embed the core wire 6 may be provided between the sheet 5a for forming the extension layer and the uncrosslinked rubber sheet 2a, and the layer structure is not limited to the above.
[0082] In the case of an embodiment in which a surface layer 7 constituting a friction transmission surface is provided on the surface of the compression layer 2, the material constituting the surface layer 7 is disposed on the outermost side of the laminate (the outer peripheral surface of the uncrosslinked rubber sheet 2a for forming the compression layer). Depending on the embodiment, the method of disposing the material may involve laminating a surface layer sheet material 7a (fabric, uncrosslinked rubber sheet, resin sheet, etc.), or the outer peripheral surface may be subjected to a treatment such as electrostatic flocking, powder coating, or application of a liquid composition.
[0083] In addition, in the uncrosslinked belt precursor 10A formed in this step, residual stress resulting from the winding tension of the cord remains.
[0084] (Crosslinking process) The crosslinking step is a step of compressing (molding) the uncrosslinked belt precursor 10A into a desired shape corresponding to the shape of a mold, and crosslinking the rubber components constituting each rubber layer to bond and integrate the laminated materials constituting the uncrosslinked belt precursor 10A, thereby forming a belt sleeve 10B (crosslinked belt precursor) (FIG. 11(b) to be described later). In this crosslinking step, the uncrosslinked belt precursor 10A is crosslinked, and the ribs 3 are formed to obtain the belt sleeve 10B, so that in the crosslinking step, a compression layer is formed at the same time as the crosslinking.
[0085] Fig. 9 shows a preparation stage for subjecting the uncrosslinked belt precursor 10A to the crosslinking step, as described above in detail. Fig. 10 shows the state of the belt forming apparatus in the crosslinking step, specifically, (a) is a schematic perspective view of the belt forming apparatus in which the inner mold 71 is inserted into the outer mold 81 of Fig. 9 and the bladder 75 is inflated, and (b) is a partially enlarged schematic cross-sectional view thereof.
[0086] 9, in order to subject the uncrosslinked belt precursor 10A to the crosslinking step, the inner mold 71 on which the uncrosslinked belt precursor 10A is mounted is inserted into the cylindrical interior (hollow interior) of an outer mold 81. The interior of the outer mold 81 is formed as a sealed hollow portion around the entire circumference, with a heating / cooling jacket 82, and above an outer peripheral wall 81a of the outer mold 81, a heat medium supply port 83 for supplying a heating medium such as steam is formed, and below the outer peripheral wall 81a, a coolant supply port 85 for supplying a coolant such as cooling water is formed.
[0087] In the crosslinking step, as shown in Fig. 10, a heating medium is supplied from a heat medium supply port 83 to heat the outer mold 81 with a heating / cooling jacket 82, and a fluid such as air is supplied from a fluid supply path 73 between the outer periphery of the inner mold 71 and the inner periphery of the bladder 75, and as shown in Fig. 10(b), the bladder 75 is expanded toward the inner periphery (molding convex portion 84) of the outer mold 81 by the pressure of the fluid, and the uncrosslinked belt precursor 10A wrapped around the outer periphery of the bladder 75 is pressed against the inner periphery of the outer mold 81, and the uncrosslinked belt precursor 10A is heated and pressurized between the bladder 75 and the outer mold 81. At this time, the uncrosslinked belt precursor 10A is pressed against the inner periphery of the outer mold 81 and pressurized, so that the outer periphery of the uncrosslinked belt precursor 10A is pressed into the concave portion between the molding convex portions 84 of the outer mold 81, and the rib 3 can be formed on the outer periphery. The heating temperature is, for example, 120 to 180° C., the molding pressure is, for example, 0.5 to 1.5 MPa, and the heating time is, for example, 15 to 30 minutes. Through this process, the uncrosslinked belt precursor 10A is crosslinked and molded to obtain the belt sleeve 10B (see FIG. 11(b)).
[0088] The belt sleeve 10B formed in this step has residual stress resulting from the winding tension of the cord 6, as well as residual stress resulting from the stretching of the cord 6 in the cross-linking step.
[0089] The belt elongation rate in the crosslinking step can be expressed as a ratio (percentage) of the elongated length of the core wire 6 in the crosslinking step to the reference circumferential length of the uncrosslinked belt precursor 10A (molded body). For example, referring to Fig. 12, if the diameter of the circumference passing through the center of the cross section of the core wire 6 in Fig. 12(a) (before the bladder is expanded) is D, and the diameter of the circumference passing through the center of the cross section of the core wire 6 in Fig. 12(b) (when the bladder is expanded) is D', the belt elongation rate in the crosslinking step can be calculated as a percentage (D'-D) / D. The belt stretch rate in the crosslinking step is proportional to the expansion rate (expansion rate) of the bladder. The larger the belt stretch rate in the crosslinking step, the easier it is to press the uncrosslinked belt precursor 10A into the outer mold 81 by the expansion (expansion) of the bladder 75, that is, the easier it is to form the rib 3. Conversely, the smaller the belt stretch rate in the crosslinking step, the more difficult it is to press the uncrosslinked belt precursor 10A into the outer mold 81, that is, the easier it is to form the rib 3.
[0090] In the present embodiment, from the viewpoint of ease of formation of the rib 3, the belt elongation rate in the crosslinking step is preferably in the range of 1 to 5%. If the belt elongation rate in the crosslinking step is less than 1%, the formation of the rib 3 becomes insufficient, and if the belt elongation rate in the crosslinking step is more than 5%, molding defects such as disturbance of the arrangement of the cords 6 tend to occur. Furthermore, as described above, from the viewpoint of preventing excessive temporal shrinkage of the belt dimensions (including dry heat shrinkage) while maintaining a relatively high level of the belt dry heat shrinkage stress, the belt elongation rate in the crosslinking step is preferably in the range of 1 to 4%.
[0091] (Finishing process) In the finishing step, the V-ribbed belt 1 is manufactured from the belt sleeve 10B obtained in the cross-linking step. Fig. 11 shows the belt forming apparatus in the finishing step, and is a schematic perspective view (a) showing the step of removing the inner mold 71 from the belt forming apparatus in the state shown in Fig. 10, and a partially enlarged schematic cross-sectional view (b) showing the state after the inner mold 71 has been removed from the belt forming apparatus.
[0092] In the crosslinking step, after the belt sleeve 10B is crosslinked and heating is stopped, the supply of fluid from the fluid supply passage 73 is stopped to contract the bladder 75 and return it to the state before expansion, and a cooling medium is further supplied from the coolant supply port 85 to cool the outer mold 81. When the bladder 75 contracts to the original state, the outer diameter of the bladder 75 is reduced and becomes smaller than the inner diameter of the crosslinked belt sleeve 10B, so that the inner mold 71 can be removed from the outer mold 81 while leaving the crosslinked belt sleeve 10B on the inner circumference of the outer mold 81, as shown in FIG.
[0093] The inner mold 71 is removed from the outer mold 81, and the belt sleeve 10B having multiple ribs 3 on the outer circumference is removed from the outer mold 81. Then, the belt sleeve 10B is cut into rings of a specified width in the belt longitudinal direction using a cutter to separate the belt into individual pieces, and the inner and outer circumference sides are turned inside out (inverted) to complete the V-ribbed belt 1.
[0094] As described above, the manufacturing method (first manufacturing method) of the V-ribbed belt 1 by the bladder expansion method has been described. However, as a second manufacturing method by the bladder expansion method, a method including a step of forming a preform as described below may be used. Specifically, the method includes the steps of winding only the uncrosslinked rubber sheet 2a for forming the compression layer around the outer peripheral surface of the bladder 75 to form a first uncrosslinked precursor, expanding the bladder 75 toward the inner peripheral surface (molding protrusion 84) of the outer mold 81 to form a preform (semi-crosslinked state) with the rib 3 formed on the outer peripheral surface, releasing the expansion of the bladder 75 to separate the inner mold 71 to which the bladder 75 is attached from the outer mold 81 to which the preform is closely attached, forming a second uncrosslinked precursor in which the uncrosslinked rubber sheet 2a for forming the tension layer and the core wire 6 are sequentially arranged on the outer peripheral surface of the bladder 75, and further expanding the bladder 75 again to press the second uncrosslinked precursor from the inner peripheral side against the outer mold 81 to which the preform is closely attached, thereby integrally crosslinking it with the preform, to obtain a belt sleeve with the rib 3 formed on the outermost peripheral surface. In addition, in the case where a surface layer 7 is provided on the surface of the compression layer 2, a laminate in which a material constituting the surface layer 7 is arranged on the outer peripheral surface of the uncrosslinked rubber sheet 2a for forming the compression layer described above is used as the first uncrosslinked precursor.
[0095] Of these methods, the first manufacturing method has simple steps and is excellent in productivity, while the second manufacturing method reduces the expansion rate of the core wire 6 by narrowing the gap between the inner die 71 and the outer die 81, thereby suppressing damage to the core wire 6 and suppressing deterioration in durability of the V-ribbed belt 1. The manufacturing method can be selected based on which of productivity and durability is prioritized.
[0096] Furthermore, in the above manufacturing method, the V-ribbed belt 1 is manufactured so that residual stress resulting from the tension (core winding tension) applied to the core 6 when the core 6 is wound remains in the V-ribbed belt 1 (core 6) as well as residual stress resulting from the elongation of the core 6 accompanying the expansion of the bladder 75 in the crosslinking process. By doing so, the belt dry heat shrinkage stress is raised to a level at which a decrease in the belt tension retention rate can be suppressed according to the degree of elongation of the belt sleeve 10B (core 6) in the crosslinking process.
[0097] Furthermore, by making the elongation rate of the belt sleeve 10B (core wire 6) in the crosslinking process to be within the range of 1.0 to 4.0%, it is possible to produce a V-ribbed belt 1 that can be attached to the pulley layout of the power transmission mechanism 20 while stretching the V-ribbed belt 1 by 1.0 to 3.5% using a jig, and has a 3.5% modulus within the range of 290 to 360 N / rib and a belt dry heat shrinkage stress within the range of 125 to 200 N.
[0098] According to the above-mentioned V-ribbed belt 1, as a low modulus belt, a twisted cord formed of fibers containing aliphatic polyamide fibers is used for the core wire 6, and the stress required to stretch the V-ribbed belt 1 by 3.5% (3.5% modulus) is kept at a relatively low level of 290 to 360 N / rib, thereby achieving the effect that the V-ribbed belt 1 can be easily attached by a stretch mounting method using a jig 50 to a drive system in which the layout circumference Lp of the pulleys 21, 22 arranged apart from each other is 1.0 to 3.5% longer than the reference circumference Lb of the V-ribbed belt 1. At the same time, despite the modulus being kept at a relatively low level, the belt dry heat shrinkage stress is ensured at a relatively high level of 125 to 200 N. Therefore, not only when the V-ribbed belt 1 stored in a relatively low humidity environment (e.g., 23°C x 50%) is attached to a pulley layout by the stretch-mounting method using the jig 50, but also when the V-ribbed belt 1 (whose core wire portion has absorbed water) stored in a relatively high humidity environment (e.g., 23°C x 90%) is attached to a pulley layout by the stretch-mounting method using the jig 50, an effect of suppressing a sudden decrease in tension during running and maintaining sufficient belt tension can be obtained (in detail, the modulus decreases due to water absorption by the core wire, making it prone to elongation, but since the shrinkage stress is ensured at a sufficiently large level, the elongation of the V-ribbed belt 1 can be suppressed, and a decrease in the belt tension retention rate can be suppressed). EXAMPLES
[0099] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In addition, the following describes a method for preparing a rubber composition, a method for producing a belt, and a method for measuring or evaluating each physical property.
[0100] [Materials used] (Rubber composition) The rubber composition shown in Table 1 was kneaded in a Banbury mixer, and the kneaded rubber was passed through a calendar roll to form a rolled rubber sheet of a predetermined thickness, to prepare an uncrosslinked rubber sheet for forming a compression layer and an uncrosslinked rubber sheet for forming an extension layer. The components in Table 1 are as follows.
[0101] (Rubber composition compounding) [Table 1] EPDM: "NORDEL (registered trademark) IP3640" manufactured by Dow Chemical Japan Co., Ltd., ethylene content 55%, ethylidene norbornene content 1.8% Zinc oxide: Seido Chemical Industry Co., Ltd., "Zinc oxide type 3" Stearic acid: NOF Corp. "Camellia Stearate" Carbon black HAF: "Seat (registered trademark) 3" manufactured by Tokai Carbon Co., Ltd. Paraffin oil: "Diana (registered trademark) Process Oil" manufactured by Idemitsu Kosan Co., Ltd. Anti-aging agent: "Nonflex (registered trademark) OD3" manufactured by Seiko Chemical Co., Ltd. Organic peroxide: "Perkadox (registered trademark) 14RP" manufactured by Kayaku Akzo Co., Ltd. Nylon staple fiber: Asahi Kasei Corporation's "Nylon 66", fiber length approx. 0.5 mm
[0102] (Core) Two bundles of 940 dtex polyamide 66 (nylon 66) fibers were aligned to prepare a first twisted yarn, and then three first twisted yarns were aligned and second twisted in the opposite direction to the first twist to prepare a ply-twisted cord with a total fineness of 5640 dtex and a core diameter of 1.0 mm. The ply-twisted cord was then immersed in the RFL treatment solution described below and dried to prepare a treated cord.
[0103] (Knitted fabric (surface layer)) Cotton spun yarn (40 count, 1 strand) as absorbent fiber and PTT / PET conjugate yarn (fineness 84 dtex) as non-absorbent fiber were knitted to produce a knitted fabric with a weft knit structure (piqué, 2 layers). The knitted fabric was immersed in the RFL treatment solution described below and then dried to produce a treated knitted fabric. The average thickness of the knitted fabric in the belt was 0.6 mm.
[0104] (RFL processing fluid) A solution containing 2.6 parts by mass of resorcin, 1.4 parts by mass of 37% by mass formalin, 17.2 parts by mass of vinylpyridine-styrene-butadiene copolymer latex, and 78.8 parts by mass of water was prepared.
[0105] [Manufacturing of V-ribbed belts] The V-ribbed belts of Examples 1 to 8 and Comparative Examples 2 and 4 were produced by the first manufacturing method using the bladder expansion method described in the above embodiment, with a core wire winding tension of 20 N per core wire and an arrangement pitch of the core wires of approximately 1.2 mm, resulting in 6PK1200 (rib pitch 3.56 mm, rib height 2.0 mm, rib angle 40°, number of ribs 6, reference circumference 1200 mm, belt width approximately 21 mm) V-ribbed belts. These V-ribbed belts were produced in the manner shown in Fig. 2, that is, without an adhesive layer, with the surface of the compression layer covered with knitted fabric, and the frictional power transmission surface formed of the knitted fabric layer (surface layer).
[0106] The V-ribbed belt of Comparative Example 3 was produced by the second manufacturing method (a method including a step of forming a semi-crosslinked preform) using the bladder expansion method described in the above embodiment, with a core wire winding tension of 20 N per core wire and an arrangement pitch of the core wires of approximately 1.2 mm, to the same specifications (shape and dimensions) as the above Examples 1 to 8 and Comparative Examples 2 and 4.
[0107] The V-ribbed belt of Comparative Example 1 was produced by the grinding method used in the examples of Patent Document 1, with a core winding tension of 20 N per core and a core arrangement pitch of about 1.2 mm, 6PK1200 (rib pitch 3.56 mm, rib height 2.9 mm, rib angle 40°, number of ribs 6, reference circumference 1200 mm, belt width about 21 mm). The grinding method is a method in which an uncrosslinked rubber sheet for forming an extension layer, a core, and an uncrosslinked rubber sheet for forming a compression layer are wound around the outer periphery of a cylindrical mold from the inner periphery to form an uncrosslinked belt precursor, crosslinking molding is performed in a known crosslinking device (such as a vulcanizing can) to produce a belt sleeve, and ribs are formed by grinding. The grinding method is a manufacturing method in which the core wire is not stretched during crosslinking molding (elongation rate 0%). In this belt, the surface of the compression layer becomes the grinding surface, so no surface layer was provided. Table 2 shows the core wire preparation conditions, friction transmission surface configurations, belt manufacturing conditions (belt elongation rate in the crosslinking process), and belt evaluation results for the V-ribbed belts prepared in Examples 1 to 8 and Comparative Examples 1 to 4.
[0108] [Table 2]
[0109] In the V-belts of Examples 1 to 8 and Comparative Examples 1 to 4, the elongation rate of the belt sleeve (core wire) in the crosslinking process (hereinafter, "belt elongation rate in the crosslinking process") was varied successively from 0% to 4.5%.
[0110] A predetermined gap is provided between the inner peripheral surface of the outer mold and the outer peripheral surface of the molded body (see FIG. 12). The larger the gap is and the smaller the belt size (reference circumference), the larger the belt elongation rate must be in the crosslinking step. In Examples 1 to 8 and Comparative Examples 2 to 4, the belt elongation rate levels in the crosslinking step were set by varying the size of the gap (in practice, changing the thickness of the bladder) by changing the outer diameter (thickness) of the bladder for an outer mold with the same inner diameter.
[0111] In addition, the heat-set stretch ratio, which is one of the manufacturing conditions of the core wire, was varied within a range of ±1% around 2%. In general, there is a tendency that increasing the heat-set stretch ratio increases the modulus, and decreasing the heat-set stretch ratio decreases the modulus.
[0112] [Evaluation of V-ribbed belts] For Examples 1 to 8 and Comparative Examples 1 to 4 shown in Table 2, evaluations (belt 3.5% modulus, belt dry heat shrinkage stress, belt dry heat shrinkage rate, belt tension retention rate (after storage in a high humidity environment, after storage in a low humidity environment)) were performed to determine whether a V-ribbed belt (low modulus belt) capable of solving the problems was obtained.
[0113] [Belt evaluation (items, methods, standards)] <Belt 3.5% modulus> This is the stress required to stretch a belt by 3.5%, and is measured and evaluated as a basic proxy characteristic for whether or not a belt functions as a low modulus belt.
[0114] (Measurement method) The belt was wrapped around two rib-grooved pulleys, and one of the pulleys was pulled at a speed of 50 mm / min. The stress required to stretch the belt by 3.5% was measured from the relationship between the pulley movement distance and the load, and converted into stress (N / rib) per rib (3.56 mm). The measurements were performed on a belt that had been left in a free state (without external force applied) for one day in a low humidity environment (23°C x 50%).
[0115] (Judgment criteria) From the viewpoint of a basic substitute characteristic of whether or not a belt functions as a low modulus belt, if the belt's 3.5% modulus is within the range of 290 to 360 N / rib, it is evaluated that there is no problem in practical use and that the belt functions as a low modulus belt, and it is rated as A. If the 3.5% modulus of the belt was outside the range of 290 to 360 N / rib, it was evaluated as not functioning as a low modulus belt and was rated b. From the viewpoint of suitability for practical use in this application (whether or not it functions as a low modulus belt), belts rated A were determined to be at the pass level.
[0116] <Belt shrinkage stress when heated in dry heat> This is measured as a substitute characteristic for reliability evaluation of whether the dynamic performance of the belt is sufficiently ensured (for example, the belt tension retention rate described later). The "belt dry heat shrinkage stress" defined in this invention is, as mentioned above, "the stress (N) per five core wires generated after applying an initial load of 147 N to the belt and leaving it in an atmosphere at 100°C for 30 minutes."
[0117] (Measurement method) (1) The rubber layer with the core wire embedded in it is cut into strips from the belt. (2) Remove excess core wires from both sides of the rubber layer to prepare a measurement sample (250 mm long) consisting of five core wires. (3) An initial load of 147 N is applied to the measurement sample consisting of five core wires (distance between chucks: 200 mm), and the sample is left for 30 minutes in an atmosphere of 100°C (in a thermostatic chamber). The value (N) detected by the load detector (load cell) after the sample is left for 30 minutes is read, and this value is regarded as the belt dry heat shrinkage stress (N / 5 wires).
[0118] (Judgment criteria) From the viewpoint of mainly being a substitute characteristic for whether or not the dynamic performance of the belt is sufficiently secured, if the dry heat shrinkage stress of the belt is within the range of 125 to 200 N / 5 pieces, there is no problem in practical use, it is evaluated as satisfying the dynamic performance of the belt, and it is rated as A. If the dry heat shrinkage stress of the belt was outside the range of 125 to 200 N / 5 pieces, the belt was evaluated as not satisfying the dynamic performance and given a grade of b. From the viewpoint of suitability for practical use in this application (ensuring the dynamic performance of the belt), belts rated A were determined to be at the pass level.
[0119] <Belt dry heat shrinkage rate> This is measured as part of the belt dimensional stability evaluation.
[0120] (Measurement method) The belt was left in a free state (without external force applied) in a 120°C atmosphere (in a thermostatic chamber) for 1 hour, and the rate of change in the belt outer periphery length before and after leaving it was determined as the belt dry heat shrinkage rate.
[0121] (Judgment criteria) Mainly from the viewpoint of ensuring the dimensional stability of the belt, if the dry heat shrinkage rate of the belt is 2.3% or less, it is deemed that there is no problem in practical use and the dimensional stability of the belt can be ensured, and it was rated as A. If the belt dry heat shrinkage rate exceeds 2.3%, it is evaluated that the dimensional stability of the belt cannot be ensured, and it is rated as b. From the viewpoint of suitability for practical use in this application (ensuring dimensional stability of the belt), belts rated A were deemed to be at the pass level.
[0122] <Belt tension retention rate (after storage in high humidity environment, after storage in low humidity environment)> This is measured as part of a reliability evaluation to determine whether the dynamic performance of the belt is sufficiently secured. The belt was stored in a high humidity or low humidity environment for 30 days, and then attached to a pulley layout using a jig stretching method and run. The belt tension retention rate during running was calculated (see below for detailed measurement method).
[0123] (Measurement method) A belt stored in a free state (without external force) in a high humidity environment (23°C x 90%) (in a constant temperature and humidity chamber) for 30 days (corresponding to the time it takes for the moisture content of the core wire of the belt to reach equilibrium), or a belt stored in a free state in a low humidity environment (23°C x 50%) (in a constant temperature and humidity chamber) for 30 days, was hung on a pulley layout that includes a driving pulley (120φ) and a driven pulley (120φ), has a fixed center distance, does not have a tensioning mechanism, and has a layout circumference that is 3% longer than the reference circumference of the belt. At this time, the circumference of the belt stretches by 3% from the reference circumference by being installed between the pulleys, and for example, the belt of Example 1 is applied with a tension when installed of about 185N / rib, and the belt of Example 8 is applied with a tension when installed of about 230N / rib. Then, the drive pulley was rotated at 4800 rpm in the same environment as the belt storage environment (in a constant temperature and humidity chamber of 23°C x 90%, or in a constant temperature and humidity chamber of 23°C x 50%), and the belt was run without load for 2 minutes. The belt tension during running (belt tension during 2 minutes of running) was calculated from the axle load detected by the axle load detector (load cell), and this was divided by the belt tension value during 2 minutes of running one day after the belt was stored in the same environment (initial stage of storage), and the resulting percentage was determined as the belt tension retention rate (%).
[0124] (Judgment criteria) Mainly from the viewpoint of ensuring the dynamic performance of the belt, in either case of belts stored in a high humidity environment or a low humidity environment, if the belt tension retention rate is 90% or more, there is absolutely no problem in practical use, and the belt's dynamic performance is evaluated as being fully satisfied, and it is rated as A. In both cases, the belt tension retention rate is 85% or more for belts stored in a high humidity environment and for belts stored in a low humidity environment. However, if the belt tension retention rate is 85% or more and less than 90% for either case, there is no problem in practical use, and the belt is evaluated as satisfying its dynamic performance and given a grade of b. If the belt tension retention rate was less than 85% for either the belt stored in a high humidity environment or the belt stored in a low humidity environment, the belt was evaluated as not satisfying dynamic performance and given a rating of C. From the viewpoint of suitability for practical use in this application (ensuring the dynamic performance of the belt), belts rated A and B were deemed to be at the pass level.
[0125] [Overall Judgment] The overall criteria for judging (ranking) a low modulus belt as capable of solving this problem were determined as follows, based on the results of the judgments in the above four belt evaluations (belt 3.5% modulus, belt dry heat shrinkage stress, belt dry heat shrinkage rate, belt tension retention rate (after storage in a high humidity environment, after storage in a low humidity environment)). Rank A: If the belt was rated A in all four of the above belt evaluations, it was deemed to be completely satisfactory for practical use and was given the highest rank. Rank B: In the above four belt evaluations, if the three evaluations of "Belt 3.5% modulus," "Belt dry heat shrinkage stress," and "Belt dry heat shrinkage rate" were all rated "A," but the evaluation of "Belt tension retention rate (after storage in a high humidity environment, after storage in a low humidity environment)" was rated "B," then the belt is deemed to have no practical problems but is ranked slightly lower than Rank A. Rank C: In the four belt evaluations above, if any one of the three evaluations, "Belt 3.5% modulus," "Belt dry heat shrinkage stress," and "Belt dry heat shrinkage rate," was rated as b, and / or if "Belt tension retention rate (after storage in high humidity environment, after storage in low humidity environment)" was rated as c, the belt was deemed to be insufficient in terms of solving this issue (failed).
[0126] [Evaluation Results] Fig. 13 shows a relationship diagram between the belt elongation rate in the crosslinking process and the belt dry heat shrinkage stress for the V-ribbed belts of Examples 1 to 8 and Comparative Examples 1, 3 and 4. The belt elongation rate in the crosslinking process and the belt dry heat shrinkage stress showed a nearly linear proportional relationship. Table 2 shows the evaluation results of the V-ribbed belts of the examples and comparative examples.
[0127] (Effects obtained) According to Table 2, from the results of Examples 1 to 8, it was found that by producing a V-ribbed belt so that the belt elongation rate in the crosslinking process is within the range of 1.0 to 4.0%, a low modulus belt can be obtained that combines the belt characteristics characterized by the present invention (3.5% modulus of 290 to 360 N / rib (judgment a) and belt dry heat shrinkage stress of 125 to 200 N (judgment a)). As a result, it was found that it is possible to provide a V-ribbed belt that can maintain sufficient tension during operation [belt tension retention rate (after storage in a high humidity environment, after storage in a low humidity environment) of 90% or more (judgment a) or 85% or more but less than 90% (judgment b) (overall judgment is also rank A or B)] even when the belt is stored in a high humidity environment and is installed in a pulley layout in which it is installed using a jig stretching method, which was the problem concerned.
[0128] As can be seen from the graph in Figure 13, this supports the idea (design concept) that a V-ribbed belt possessing the belt characteristics characteristic of the present invention can be obtained by manufacturing the belt so that residual stress resulting from the tension applied to the core wire when it is wound (core wire winding tension) remains in the belt (core wire) as well as residual stress resulting from the stretching of the core wire during the crosslinking process; this can increase the belt dry heat shrinkage stress to a level that suppresses a decrease in the belt tension retention rate depending on the degree of belt elongation in the crosslinking process.
[0129] (Considerations regarding evaluation results) Examples 4 to 8 (Compare with Examples 1 to 3) In the case of belts manufactured so that the belt elongation rate in the crosslinking process is within the range of 2.0 to 4.0% (Examples 4 to 8), compared to the case of belts manufactured so that the belt elongation rate in the crosslinking process is within the range of 1.0 to 1.5% (Examples 1 to 3), it was found that the belt dry heat shrinkage stress was within the same pass level (a rating) range (125 to 200 N / 5 pieces) but could be raised to a higher level (approximately 150 to approximately 200 N / 5 pieces), and the belt tension retention rate after storage in a high humidity environment (23°C x 90%) could be raised to a higher level (90.0 to 99.6%, a rating) (the overall rating was also Rank A).
[0130] Examples 1 to 8 In the case of Example 5, the belt 3.5% modulus was 315 N / rib, while the belt 2.0% modulus was 180 N / rib. Similarly, the belt 2.0% modulus in Examples 1 to 8 was within the range of about 165 N / rib (Example 1) to about 205 N / rib (Example 8).
[0131] Comparative Example 1 In Comparative Example 1, the belt was produced (produced by grinding method) with a belt elongation rate of 0% in the crosslinking process, so residual stress due to the elongation of the cord in the crosslinking process could not be imparted to the belt (cord), and the belt dry heat shrinkage stress was only 101 N / 5 pieces (grade b). Therefore, the belt tension retention rate after storage in a high humidity environment (23°C x 90%) remained at a level of less than 85% (grade c), and it was determined that the belt did not satisfy the dynamic performance (overall grade C).
[0132] Comparative Example 2 In Comparative Example 2, like Examples 1 to 8 and Comparative Example 4, a belt was produced by the first manufacturing method using the bladder expansion method (a method that does not include a step of forming a preform in a semi-crosslinked state). However, since the belt elongation rate in the crosslinking step was set to a level below 1.0% (0.5%), the formation of the ribs was insufficient and a belt could not be produced.
[0133] Comparative Example 3 Comparative Example 3 is the only one in which the belt was produced by the second manufacturing method using the bladder expansion method (a method including a step of forming a preform in a semi-crosslinked state). Although the belt elongation rate in the crosslinking step was set to a level below 1.0% (0.5%), it was still possible to form ribs and produce the belt. However, because the belt elongation rate during the crosslinking process was set at a level below 1.0% (0.5%), the residual stress caused by the elongation of the core wire during the crosslinking process could not be fully imparted to the belt (core wire), and the belt's dry heat shrinkage stress was only 120 N / 5 wires (rating b). As a result, the belt tension retention rate after storage in a high humidity environment (23°C x 90%) remained at a level of less than 85% (rating C), and the belt was determined to not satisfy the dynamic performance requirements (overall rating: Rank C).
[0134] Comparative Example 4 In Comparative Example 4, the belt elongation rate in the crosslinking process was set to a relatively high level of 4.5%, and the belt dry heat shrinkage stress was 210 N / 5 pieces, exceeding 200 N / 5 pieces (rating b). Therefore, the belt dry heat shrinkage rate exceeded the allowable upper limit (2.3%) (rating b), and it was determined that the dimensional stability of the belt could not be ensured (overall rating rank C). Therefore, the belt dynamic evaluation (evaluation of belt tension retention rate) was not performed. [Explanation of symbols]
[0135] 1 V-ribbed belt 2. Compression layer 3. Ribs 4 Adhesive layer 5 stretch layers 6 core wire 7 Surface layer 10 Belt body 20 Power transmission mechanism
Claims
1. A V-ribbed belt comprising: an annular belt body in which a plurality of ribs extending along a belt longitudinal direction are formed in a compressed layer on an inner circumferential side; and a core wire embedded in the belt body along the longitudinal direction of the belt body, the core wire is a twisted cord formed of fibers including aliphatic polyamide fibers, The stress required to elongate the V-ribbed belt by 3.5% is 290 to 360 N per rib, and the dry heat shrinkage stress of the belt, defined as the stress (N) per five core wires generated after applying an initial load of 147 N to the V-ribbed belt and leaving it in an atmosphere at 100°C for 30 minutes, is 150 to 200 N.
2. At least a portion of the rib has a friction transmission surface capable of contacting a pulley around which the V-ribbed belt is wound, 2. The V-ribbed belt according to claim 1, wherein the friction transmission surface has a surface layer laminated on a compression layer.
3. 3. The V-ribbed belt according to claim 2, wherein the surface layer is a fiber layer, a coating layer, a rubber layer, or a resin layer.
4. A V-ribbed belt according to any one of claims 1 to 3, two or more pulleys arranged apart from each other to which the V-ribbed belt is attached, A power transmission mechanism, characterized in that a reference circumferential length of the V-ribbed belt before installation is 1.0 to 3.5% shorter than a layout circumferential length of the two or more pulleys.
5. A method for manufacturing a V-ribbed belt according to any one of claims 1 to 3, A crosslinking process is a process for forming a crosslinked belt precursor by integrating laminated materials constituting an uncrosslinked belt precursor including a core wire, which is a prototype of the V-ribbed belt, The method includes a step of expanding an expandable bladder at a predetermined expansion rate to expand an outer diameter of the bladder, and stretching the core wire wound around the outer periphery of the bladder in accordance with the expansion of the outer diameter of the bladder, A method for producing a V-ribbed belt, wherein an elongation rate of the precursor including the core wires in the crosslinking step is within a range of 2.0 to 4.0%.
Citation Information
Patent Citations
A laser beam machining device -
JP1989002790A
V-ribbed belt
JP2003194152A
Friction transmission belt and method of manufacturing the same
JP2013145032A