Meltblown nonwoven fabric

By controlling resin melt viscosity and mechanical energy in the melt blowing process, the formation of thick fibers is suppressed, leading to high-quality nonwoven fabrics suitable for filters and transdermal administration sheets.

JP7556009B2Active Publication Date: 2024-09-25KURARAY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022182267
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-09-08
Filing Date
2022-11-15
Publication Date
2024-09-25
Estimated Expiration
2038-08-27

AI Technical Summary

Technical Problem

Existing melt blowing methods for cyclic olefin resins result in the formation of thick fibers due to mechanochemical reactions, which are not addressed by prior art, and this affects the quality and performance of nonwoven fabrics.

Method used

The method involves controlling the viscosity of the resin melt before introduction into the kneading section and minimizing mechanical energy, such as compressive stress, to suppress the formation of thick fibers by using a specific range of viscosity and screw rotation speed ratios.

Benefits of technology

This approach results in nonwoven fabrics with suppressed thick fibers, improved density, and enhanced performance characteristics, suitable for applications requiring high quality and uniformity, such as filters and transdermal administration sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556009000003
    Figure 0007556009000003
  • Figure 0007556009000004
    Figure 0007556009000004
  • Figure 0007556009000005
    Figure 0007556009000005
Patent Text Reader

Abstract

Provided is a meltblown nonwoven fabric made of fibers containing a cyclic olefin resin. [Solution] The meltblown nonwoven fabric is a meltblown nonwoven fabric composed of fibers containing a cyclic olefin resin, and the average value of data having a fiber diameter larger than the third quartile obtained by dividing the data into quartiles from small to large fiber diameter data among fiber diameter data of 100 points randomly selected in an SEM image magnified 1000 times is 30 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Related Applications

[0001] This application claims priority from Japanese Patent Application No. 2017-173124, filed September 8, 2017, the entire contents of which are incorporated herein by reference. [Technical field]

[0002] The present invention relates to a meltblown (MB) nonwoven fabric composed of fibers containing a cyclic olefin resin and in which the inclusion of large diameter fibers is reduced, and a method for producing the meltblown (MB) nonwoven fabric. [Background technology]

[0003] Cyclic olefin resins have various properties, such as high transparency, high heat resistance, chemical resistance, low elution of impurities, and low adsorption, and are therefore molded by various methods and used in a variety of applications, including medical applications such as drug packaging materials and inspection containers, optical applications such as lenses and optical films, and electronic device applications.

[0004] For example, Patent Document 1 (JP 2001-210549 A) ​​describes an electret made of a resin composition containing a cyclic hydrocarbon polymer, and describes that the electret can be made into a form such as a film, sheet, fiber, or nonwoven fabric, and that the melt-blowing method is preferably used to make the nonwoven fabric into an electret. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2001-210549 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in Patent Document 1, regarding the manufacturing method of the meltblown nonwoven fabric, only the conditions of a general meltblowing method are described, and in the examples, only a film is produced.

[0007] Therefore, an object of the present invention is to provide a meltblown nonwoven fabric composed of fibers containing a cyclic olefin resin and suppressing the inclusion of thick fibers, a filter using the same, and a support for a transdermal administration sheet and a transdermal administration sheet (particularly a transdermal absorption agent and a patch).

[0008] Another object of the present invention is to provide a method for producing a meltblown nonwoven fabric made of fibers containing a cyclic olefin resin, which can suppress the inclusion of thick fibers. [Means for solving the problem]

[0009] As a result of intensive research to achieve the above-mentioned object, the inventors of the present invention have found that (i) when the melt-blowing method is applied to a cyclic olefin resin, the mechanical energy acting during kneading of the resin causes the decomposition of the main chain, and the decomposed double bonds form new bonds with each other, inducing a phenomenon called a "mechanochemical reaction" in which gelation occurs, and therefore, in MB nonwoven fabrics obtained using cyclic olefin resins, bead-like lumps called shot are generated, and even if shot is not mixed in, fibers thicker than the allowable thickness will be mixed in as a defect due to the mechanochemical reaction. Then, (ii) they found that in the melt-blowing method, when mechanical energy (especially compressive stress) is applied to the resin during kneading of the resin in the extruder or during supply to the die, a mechanochemical reaction of the resin is likely to occur. As a result of further research, (iii) they found that by using a method of not compressing the resin as much as possible by reducing the viscosity of the molten resin before it is introduced into the kneading section or by reducing the ratio (Q / N) of the discharge rate of the resin kneaded product (Q) to the screw rotation speed (N), it is possible to obtain an MB nonwoven fabric in which the generation of thick fibers is suppressed, which led to the completion of the present invention.

[0010] That is, the present invention can be configured in the following manner. [Aspect 1] A meltblown nonwoven fabric composed of fibers containing a cyclic olefin resin, wherein the average value of data having a fiber diameter larger than the third quartile obtained by dividing the data into quartiles from small fiber diameter data to large fiber diameter data out of 100 fiber diameter data points randomly selected in a 1000x magnified SEM image is 30 μm or less.

[0011] [Aspect 2] 2. The meltblown nonwoven fabric according to claim 1, wherein the cyclic olefin resin is a copolymer containing at least a norbornene unit.

[0012] [Aspect 3] A meltblown nonwoven fabric according to aspect 1 or 2, having an air permeability of 10 to 550 cm as measured in accordance with JIS L 1906. 3 / cm 2 · s, meltblown nonwoven fabric.

[0013] Aspect 4 The meltblown nonwoven fabric according to any one of aspects 1 to 3, having a basis weight of 10 to 50 g / m 2 Meet the meltblown nonwoven fabric.

[0014] Aspect 5 A meltblown nonwoven fabric according to any one of aspects 1 to 4, which satisfies the following formula (1): 80≦B / A≦800 (1) [Wherein, A: thickness (mm), B: air permeability (cm 3 / cm 2 s)

[0015] Aspect 6 A meltblown nonwoven fabric according to any one of aspects 1 to 5, comprising fibers having an average fiber diameter of 1 to 15 μm.

[0016] Aspect 7 A filter using the meltblown nonwoven fabric according to any one of the first to sixth aspects.

[0017] Aspect 8 A support used in a transdermal administration sheet that releases an active ingredient, the support comprising the meltblown nonwoven fabric according to any one of the first to sixth aspects.

[0018] Aspect 9 The active ingredient, Aspects 9. A transdermal administration sheet comprising at least the support described in 8.

[0019] Aspect 10 a melting step of heating and melting a resin composition containing at least a cyclic olefin resin in a supply section to obtain a resin melt; A kneading step of introducing the resin melt into a kneading section and kneading the resin melt by rotating a screw under heating to obtain a resin kneaded product; a discharge step of discharging the resin kneaded material from a nozzle together with air; A method for producing a melt-blown nonwoven fabric containing a cyclic olefin resin, comprising at least a collecting step of collecting the filamentous material discharged from the nozzle with a collecting surface to obtain a web, The method for producing a meltblown nonwoven fabric, wherein the viscosity η of the molten resin introduced into the kneading section is 80 to 200 poise.

[0020] Aspect 11 A method for producing a meltblown nonwoven fabric according to aspect 10, wherein the method satisfies the following formula (2): 20≦(Q×η) / N≦ 100 (2) [In the formula, Q represents the discharge amount (kg / hr) of the resin mixture from the nozzle, η represents the viscosity (poise) of the resin melt introduced into the kneading section, and N represents the screw rotation speed (rpm)]

[0021] It should be noted that any combination of at least two elements disclosed in the claims and / or the specification and / or the drawings is included in the present invention. In particular, any combination of two or more of the claims described in the claims is included in the present invention. Effect of the Invention

[0022] According to the MB nonwoven fabric of the present invention, even though it is composed of fibers containing cyclic olefin resins that cause specific side reactions, it is possible to obtain an MB nonwoven fabric in which the inclusion of thick fibers is suppressed, and it is possible to provide filters and transdermal administration sheets (particularly transdermal absorption agents and patches) using this MB nonwoven fabric.

[0023] Furthermore, in the present invention, when producing a nonwoven fabric by the melt-blowing method, the viscosity of the molten resin before being introduced into the kneading section is set within a specific range, thereby making it possible to suppress the occurrence of a "mechanochemical reaction" that is specific to cyclic olefin resins, and as a result, a method for producing a melt-blown nonwoven fabric in which the inclusion of thick fibers is suppressed can be provided. [Brief description of the drawings]

[0024] The present invention will be more clearly understood from the following description of preferred embodiments with reference to the accompanying drawings. However, the embodiments and drawings are merely for illustration and explanation, and should not be used to define the scope of the present invention, which is defined by the appended claims. [Figure 1] FIG. 1 is a schematic cross-sectional view showing an apparatus used for producing an MB nonwoven fabric according to one embodiment of the present invention. [Diagram 2] 1 is an SEM image (magnification: 300 times) of the MB nonwoven fabric obtained in Reference Example 1. [Diagram 3] 1 is a SEM image (magnification: 300x) of the MB nonwoven fabric obtained in Example 2. [Figure 4] 1 is an SEM image (magnification: 300 times) of the MB nonwoven fabric obtained in Reference Example 3. [Diagram 5]1 is a SEM image (magnification: 300x) of the MB nonwoven fabric obtained in Example 4. [Figure 6] 1 is a SEM image (magnification: 300 times) of the MB nonwoven fabric obtained in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] (Meltblown nonwoven fabric) The MB nonwoven fabric of the present invention is composed of fibers containing a cyclic olefin resin, and the average value of data having a fiber diameter larger than the third quartile obtained by dividing the data into quartiles from small to large fiber diameter data out of 100 fiber diameter data randomly selected from a scanning electron microscope (SEM) image magnified 1000 times is 30 μm or less.

[0026] A "quartile" is the value that divides data values ​​into four equal parts when they are sorted in ascending order of magnitude. The value in the smallest 1 / 4 of the data is called the first quartile, the value in the smallest 2 / 4 of the data is called the second quartile (median), and the value in the smallest 3 / 4 of the data is called the third quartile.

[0027] The MB nonwoven fabric of the present invention has few thick fibers derived from mechanochemical reactions, and has an average fiber diameter (Db) of 30 μm or less, preferably 20 μm or less, and more preferably 16 μm or less, which is the average value of data having a fiber diameter larger than the third quartile of fiber diameter data of 100 points randomly selected in a scanning electron microscope image of the nonwoven fabric magnified 1000 times. By reducing the average value of data having a fiber diameter larger than the third quartile of the fiber diameter data, the nonwoven fabric can be made denser, have a good texture, and be made into a nonwoven fabric with a good feel. The lower limit of the average fiber diameter Db is not particularly limited, and may be, for example, the average fiber diameter of the fibers constituting the nonwoven fabric.

[0028] In addition, from the viewpoint of improving the denseness of the nonwoven fabric, the average fiber diameter of the fibers constituting the MB nonwoven fabric of the present invention may be, for example, 1 to 15 μm, preferably 1 to 12 μm, more preferably 1 to 10 μm, and even more preferably 1 to 8 μm. The average fiber diameter refers to the average value of all measured fiber diameter data, and is a value measured by the method described in the examples below.

[0029] In addition, from the viewpoint of improving the denseness and uniformity of the texture of the nonwoven fabric, the MB nonwoven fabric of the present invention may have a CV value of the average fiber diameter of the fibers constituting the nonwoven fabric of, for example, 110% or less, preferably 105% or less. The lower limit of the CV value is not particularly limited, but may be 50% or more. The CV value of the average fiber diameter refers to the ratio of the standard deviation of the measured fiber diameter data to the average fiber diameter, and is an index that represents the variation in fiber diameter distribution, and is a value measured by the method described in the examples described later.

[0030] In addition, in the MB nonwoven fabric of the present invention, from the viewpoint of improving the denseness and uniformity of the texture of the nonwoven fabric, the average fiber diameter (Db), which is the average value of data (76th to 100th data) having a fiber diameter larger than the third quartile of fiber diameter data of 100 points randomly selected in a scanning electron microscope image of the nonwoven fabric enlarged 1000 times, may be, for example, 4.0 or less, preferably 3.5 or less, as Db / Dc, relative to the average fiber diameter (Dc), which is the average value of data (26th to 75th data) having a fiber diameter larger than the first quartile and smaller than the third quartile. In addition, from the viewpoint of uniformity, it is preferable that Db / Dc is 1 or more.

[0031] The fibers constituting the MB nonwoven fabric of the present invention are fibers containing a cyclic olefin resin. For example, the resin composition constituting the fibers may contain 50% by mass or more of a cyclic olefin resin, preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 98% by mass or more.

[0032] In addition, the MB nonwoven fabric of the present invention may contain a thermoplastic resin other than the cyclic olefin resin described below, without any particular limitation, so long as the effects of the present invention can be achieved. For example, examples of the thermoplastic resin include linear polyolefin resins (e.g., polyethylene resins, polypropylene resins), polyester resins (e.g., polyethylene terephthalate resins, polybutylene terephthalate resins), etc.

[0033] In addition, from the viewpoint of low elution, at least a part of the fiber surface of the fibers constituting the MB nonwoven fabric of the present invention may be formed from a cyclic olefin resin described below.

[0034] In addition, the fibers constituting the MB nonwoven fabric of the present invention are not particularly limited as long as the effects of the present invention can be achieved, and may be composite fibers, for example, core-sheath type fibers, side-by-side type fibers, or sea-island type fibers.

[0035] The weight of the MB nonwoven fabric of the present invention can be appropriately determined depending on the application. The weight is not particularly limited. For example, from the viewpoint of weight reduction and denseness, the weight is, for example, 10 to 50 g / m 2 and preferably 10 to 45 g / m 2 Approximately, more preferably 10 to 40 g / m 2 The basis weight is a value measured by the method described in the examples below.

[0036] The thickness of the MB nonwoven fabric of the present invention can be appropriately determined depending on the application, and the thickness is not particularly limited, but from the viewpoint of weight reduction and texture, the thickness may be, for example, about 0.10 to 1.00 mm, preferably about 0.10 to 0.85 mm, and more preferably about 0.10 to 0.70 mm. The thickness is a value measured by the method described in the examples below.

[0037] The air permeability of the MB nonwoven fabric of the present invention can be appropriately determined depending on the application, and the air permeability is not particularly limited. For example, from the viewpoint of denseness, the air permeability is, for example, 10 to 550 cm 3 / cm 2 s, preferably 10 to 500 cm 3 / cm 2 s, more preferably 10 to 400 cm 3 / cm 2 The air permeability may be about 1 / s. The air permeability is a value measured by the method described in the examples described later.

[0038] In addition, the MB nonwoven fabric of the present invention is preferably excellent in density despite its thinness. For example, the air permeability B (cm) of the nonwoven fabric with respect to the thickness A (mm) is 3 / cm 2 The ratio (B / A) of the amount of oxygen (s) may be 80≦B / A≦800, preferably 90≦B / A≦500, and more preferably 100≦B / A≦400.

[0039] The MB nonwoven fabric of the present invention can be used for various applications such as medical, cosmetic, and sanitary materials, industrial materials, daily necessities, and clothing. In particular, it can be suitably used for various filters such as filters for filtering liquids such as water, air filters (e.g., air filters for clean rooms), transdermal administration sheets (e.g., transdermal absorption agents, patches), etc., and is particularly suitable for use in liquid filtering filters and transdermal administration sheets (e.g., transdermal absorption agents, patches) due to its excellent low elution of impurities.

[0040] When the MB nonwoven fabric of the present invention is used in various filters, the collection efficiency of the filter measured in accordance with JIS T 8151 is preferably 85% or more, more preferably 88% or more, and even more preferably 90% or more. The pressure loss of the filter measured in accordance with JIS T 8151 is preferably 15 Pa or less, more preferably 13 Pa or less, and even more preferably 10 Pa or less. The collection efficiency and pressure loss are values ​​measured by the methods described in the examples described later. The MB nonwoven fabric of the present invention is very effective as an air filter with low pressure loss and high collection efficiency. In addition, since the cyclic olefin resin is a polymer approved by the FDA (U.S. Food and Drug Administration) with low elution, it is expected to be applied to filters for filtration of liquids such as purified water. When used as a filter for filtration of liquids such as purified water, the fiber diameter of the MB nonwoven fabric may be narrowed, and for example, the average fiber diameter of the MB nonwoven fabric may be 1 to 8 μm, preferably 1 to 7 μm.

[0041] Furthermore, for medical and cosmetic applications, the MB nonwoven fabric of the present invention has excellent low elution of impurities and can reduce migration of active ingredients such as drugs to the nonwoven fabric, and therefore can be suitably used in transdermal administration sheets (preferably transdermal absorption agents, patches) that release active ingredients (e.g., pharmaceutical or cosmetic active ingredients, preferably pharmaceutical active ingredients), and the transdermal administration sheet can include at least the active ingredient and the MB nonwoven fabric of the present invention as a support. Specifically, in the transdermal administration sheet, the MB nonwoven fabric of the present invention can be used as a support for holding a liquid containing the active ingredient, or as a support (backing) for supporting a semi-solid or solid containing the active ingredient.

[0042] (Cyclic olefin resin) The cyclic olefin resin is a polymer or copolymer containing a structural unit derived from a cyclic olefin in the main chain. The cyclic olefin is an unsaturated hydrocarbon compound having at least one olefinic double bond in a cyclic hydrocarbon structure, such as norbornene, dicyclopentadiene, or tetracyclododecene, and is introduced by using this as a monomer. Depending on the production method, the cyclic olefin resin may be an addition polymer of a cyclic olefin or a hydrogenated product thereof; an addition copolymer of a cyclic olefin and an α-olefin or a hydrogenated product thereof; and a ring-opening (co)polymer of a cyclic olefin or a hydrogenated product thereof. The cyclic olefin resin in the present invention may be, for example, an addition copolymer of a cyclic olefin and an α-olefin from the viewpoint of having both characteristics and cost.

[0043] Examples of the cyclic olefin include monocyclic olefins such as cyclopentene, cyclohexene, cyclooctene, cyclopentadiene, and 1,3-cyclohexadiene; bicyclo[2.2.1]hept-2-ene (norbornene), 5-methyl-bicyclo[2.2.1]hept-2-ene, 5,5-dimethyl-bicyclo[2.2.1]hept-2-ene, 5-ethyl-bicyclo[2.2.1]hept-2-ene, 5-butyl-bicyclo[2.2.1]hept-2-ene, and 5-ethylene. 2-ring cyclic olefins such as 5-hexyl-bicyclo[2.2.1]hept-2-ene, 5-octyl-bicyclo[2.2.1]hept-2-ene, 5-octadecyl-bicyclo[2.2.1]hept-2-ene, 5-methylidene-bicyclo[2.2.1]hept-2-ene, 5-vinyl-bicyclo[2.2.1]hept-2-ene, 5-propenyl-bicyclo[2.2.1]hept-2-ene; tricyclo[4.3.0.1 2,5 ]Deca-3,7-diene (dicyclopentadiene), tricyclo[4.3.0.1 2,5 ]dec-3-ene, tricyclo[4.4.0.1 2,5 ]Undeca-3,7-diene or tricyclo[4.4.0.1 2,5 ]Undeca-3,8-diene or partially hydrogenated products thereof (or an adduct of cyclopentadiene and cyclohexene) 2,5 ]undec-3-ene, 5-cyclopentyl-bicyclo[2.2.1]hept-2-ene, 5-cyclohexyl-bicyclo[2.2.1]hept-2-ene, 5-cyclohexenyl-bicyclo[2.2.1]hept-2-ene, 5-phenyl-bicyclo[2.2.1]hept-2-ene, and other three-ring cyclic olefins; tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene (tetracyclododecene), 8-methyltetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-ethyltetracyclo[4.4.0.1 2,5 .1 7,10]dodec-3-ene, 8-methylidenetetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-ethylidenetetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-vinyltetracyclo[4,4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-propenyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, a 4-ring cyclic olefin; 8-cyclopentyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-cyclohexyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-cyclohexenyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-phenyl-cyclopentyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, tetracyclo[7.4.1 3,6 .0 1,9 .0 2,7 ]Tetradeca-4,9,11,13-tetraene (1,4-methano-1,4,4a,9a-tetrahydrofluorene), tetracyclo[8.4.1 4,7 .0 1,10 .0 3,8 ]Pentadeca-5,10,12,14-tetraene (1,4-methano-1,4,4a,5,10,10a-hexahydroanthracene), pentacyclo[6.6.1.1 3,6 .0 2,7 .0 9,14 ]-4-Hexadecene, Pentacyclo[6.5.1.1 3,6 .0 2,7 .0 9,13 ]-4-Pentadecene, Pentacyclo[7.4.0.0 2,7 .1 3,6 .1 10,13 ]-4-Pentadecene, Heptacyclo[8.7.0.1 2,9 .1 4,7 .1 11,17.0 3,8 .0 12,16 ]-5-Eicosene, heptacyclo[8.7.0.1 2,9 .0 3,8 .1 4,7 .0 12,17 .1 13,l6 Examples of the cyclic olefins include polycyclic olefins such as tetramers of cyclopentadiene and cyclopentadiene. These cyclic olefins may be used alone or in combination of two or more kinds.

[0044] Specific examples of α-olefins copolymerizable with cyclic olefins include α-olefins having 2 to 20 carbon atoms, preferably 2 to 8 carbon atoms, such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. These α-olefins may be used alone or in combination of two or more.

[0045] The polymerization method and hydrogenation method of the cyclic olefin or the cyclic olefin and the α-olefin are not particularly limited, and can be carried out according to known methods.

[0046] The cyclic olefin resin of the present invention is preferably a copolymer containing at least a norbornene unit using at least norbornene as the cyclic olefin, and particularly preferably a copolymer of ethylene and norbornene.

[0047] For example, in a copolymer of ethylene and norbornene, from the viewpoints of processability and elution, the mass ratio of norbornene units to the total of ethylene units and norbornene units may be 60 to 99 mass%, and preferably 63 to 90 mass%.

[0048] (Meltblown nonwoven fabric manufacturing method) The method for producing the MB nonwoven fabric of the present invention includes a melting step of heating and melting a resin composition containing a cyclic olefin resin in a supply section to obtain a resin melt; a kneading step of introducing the molten resin into a kneading section and kneading the molten resin by rotating a screw under heating to obtain a resin kneaded product; A discharge step of discharging the resin kneaded material from a nozzle together with air; and The method includes at least a collecting step of collecting the filamentous material discharged from the nozzle on a collecting surface to obtain a web.

[0049] FIG. 1 is a schematic cross-sectional view showing an apparatus 100 used for producing an MB nonwoven fabric according to one embodiment of the present invention. As shown in FIG. 1, the apparatus 100 includes at least an extruder 10, a die 40, and a collection member 60. The extruder 10 includes at least a cylinder 30 and a screw 20 rotating in the cylinder 30. The screw 20 includes a supply section 22 for supplying a resin solid material and a kneading section 24 for kneading the resin supplied from the supply section 22. In FIG. 1, a resin composition containing a cyclic olefin resin is heated and melted in the supply section 22 of the screw 20 of the extruder 10, and introduced into the kneading section 24. 1, the kneading section 24 is composed of a compression section 26 and a metering section 28. For example, a solid resin composition (resin solid matter) charged from a hopper 12 is sent from a supply section 22 to the kneading section 24 toward a die 40 by the rotation of the screw 20 in a cylinder 30.

[0050] Typically, in the screw 20, the feed section 22 has grooves of the same depth (Hp), and the compression section 26 has grooves that become gradually shallower in the flow direction X. The groove depth of the screw 20 is shallowest in the metering section 28, which has grooves of the same depth (Hm) (where Hp>Hm).

[0051] In the screw 20, the groove of the screw 20 becomes shallower in the flow direction X in the kneading section 24, so that the mechanical energy acting on the resin melt between the screw 20 and the inner wall of the cylinder 30 increases as the resin melt is propelled in the flow direction X. The resin kneaded material that has passed through the kneading section 24 is then fed into the die 40. Next, the resin kneaded material is discharged from the nozzle 42, and the discharged filamentous material 50 is collected on the collection surface 62, thereby producing a nonwoven fabric.

[0052] (Melting process) 1, in the melting process, in the supply section 22 of the screw 20 provided in the cylinder 30, the resin composition containing at least a cyclic olefin resin is transported by the rotation of the screw 20 and is heated and melted by a known heating means such as a heater provided in the cylinder 30. In the supply section 22, the resin solid material supplied from the hopper 12 forms a solid bed between the screw 20 and the cylinder 30 and moves in the flow direction X.

[0053] In a normal method, the solid bed is not broken in the supply section, but is broken in the kneading section 24 to form a resin melt. However, in the present invention, by increasing the heating temperature in the supply section 22 to a level at which the solid bed is broken, a resin melt having a specific viscosity can be formed in the supply section 22. Note that, although the above description has been given using a single-screw extruder as an example, any known extruder such as a single-screw extruder or a multi-screw extruder (two or more screws) can be used as the extruder 10.

[0054] In the manufacturing method of the MB nonwoven fabric of the present invention, whereas the resin composition is conventionally introduced into the kneading section as a solid or containing a solid, by forming the resin melt into a specific low viscosity before heating and kneading in the kneading section, it is possible to reduce the mechanical energy acting on the resin melt, such as the shear stress caused by the rotation of the screw in the kneading process and the compressive stress applied when it is fed into the die or discharged from the nozzle. This makes it possible to suppress the "mechanochemical reaction" characteristic of cyclic olefin resins, and as a result, the generation of thick fibers can be suppressed.

[0055] The heating temperature in the supply section can be appropriately determined depending on the viscosity characteristics and thermal decomposition temperature of the cyclic olefin resin and other thermoplastic resins contained in the resin composition, and may be, for example, 200 to 400° C., preferably 250 to 390° C., and more preferably 300 to 380° C. By increasing the heating temperature in the supply section, it is possible to reduce the viscosity η of the resin melt.

[0056] The viscosity η of the resin melt at the heating temperature in the supply section may be 80 to 200 poise, preferably 85 to 195 poise, and more preferably 90 to 190 poise. The viscosity is a value measured by the method described in the examples described later. The resin melt adjusted to a predetermined viscosity in the supply section is introduced into the kneading section.

[0057] (Kneading process) The resin melt preliminarily melted in the supply section 22 is then introduced into the kneading section 24, where it is kneaded by the rotation of the screw 20 under heating to obtain a resin kneaded product. By lowering the viscosity of the resin melt in advance in the supply step, it is possible to suppress the compressive stress applied to the resin kneaded product when it is introduced into the die in the kneading step.

[0058] Regarding the screw, the product (Q×η) / N of the ratio Q / N of the discharge rate Q (kg / hr) of the resin kneaded product in the discharge step described below to the screw rotation speed N (rpm) and the viscosity η (poise) of the resin melt may be, for example, 20 to 100, preferably 30 to 90, and more preferably 40 to 80. (Q×η) / N is a parameter that reflects the viscosity when the resin is kneaded with the mechanical energy given to the resin by the rotation of the screw, and by setting it in the above range, it is possible to reduce the mechanical energy, particularly the compressive stress, given to the resin, and the "mechanochemical reaction" that occurs in the cyclic olefin resin can be suppressed.

[0059] From the viewpoint of reducing the mechanical energy, particularly the compressive stress, given to the resin, the ratio Q / N of the discharge rate Q (kg / hr) of the resin kneaded product in the discharge step described below to the screw rotation speed N (rpm) may be 0.1 to 2.0, preferably 0.2 to 1.5, and more preferably 0.3 to 1.0. Q / N refers to the amount of resin processed per screw rotation speed, and by setting this value in the above range, the mechanical energy that the resin receives in the kneading section can be kept small.

[0060] In addition, from the viewpoint of reducing the viscosity of the resin mixture and reducing the compressive stress applied to the resin mixture when it is fed to the die, the ratio (L / D) of the axial length (L) of the screw to the diameter (D) of the screw may be 15 to 40, preferably 18 to 40, and more preferably 20 to 40.

[0061] The heating temperature in the kneading section can be appropriately determined depending on the viscosity characteristics and thermal decomposition temperature of the cyclic olefin resin and other thermoplastic resins contained in the resin composition, and may be, for example, 230 to 400°C, preferably 250 to 390°C, and more preferably 300 to 380°C, from the viewpoint of reducing the viscosity of the resin kneaded product.

[0062] (Discharge process) The obtained resin mixture is introduced into a die 40 equipped with a nozzle 42 for ejecting the resin mixture and air injection grooves (not shown) provided on both sides of the nozzle 42, and is ejected from the nozzle 42 together with air injected from the air injection grooves.

[0063] The nozzle hole diameter is not particularly limited as long as fibers having a predetermined fiber diameter can be obtained, but may be, for example, 0.01 to 1.0 mm, preferably 0.05 to 0.8 mm, and more preferably 0.1 to 0.5 mm.

[0064] The heating temperature in the die, i.e., the spinning temperature, can be appropriately determined depending on the viscosity characteristics and thermal decomposition temperature of the cyclic olefin resin and other thermoplastic resins contained in the resin composition, and may be, for example, 300 to 400°C, preferably 320 to 395°C, and more preferably 350 to 390°C, from the viewpoint of adjusting the discharge amount of the resin kneaded product.

[0065] (Collection process) The discharged filamentous material 50 discharged from the nozzle 42 is collected on the collection surface 62 of the collection member 60 to obtain a web. The collection member 60 is not particularly limited as long as it is a member generally used as a collection member when manufacturing MB nonwoven fabric, and may be a rotating roll or a conveyor belt. For example, as shown in FIG. 1, the collection member 60 may be a conveyor belt that rotates in one direction, and the discharged filamentous material 50 is accumulated on the collection surface 62, and the MB nonwoven fabric is continuously formed as the conveyor belt rotates.

[0066] (Charging process) When the MB nonwoven fabric of the present invention is used in various filters, it may be subjected to an electrification treatment (treatment to impart electrification) in order to further improve the collection performance of the MB nonwoven fabric. "Electrification" refers to the state in which the MB nonwoven fabric is electrically charged, and preferably has a surface charge density (a value obtained by dividing the amount of charge measured using a Faraday cage [electrostatic charge meter] by the measured area) of 1.0×10 -10 Coulomb / cm 2 More preferably, 1.5×10 -10 Coulomb / cm 2 More preferably, 2.0×10 -10 Coulomb / cm 2 That's all.

[0067] Methods for imparting electrostatic charge to MB nonwoven fabrics include appropriate electret treatments such as a method of imparting an electric charge by friction or contact, a method of irradiating active energy rays (e.g., electron beams, ultraviolet rays, X-rays, etc.), a method using gas discharge such as corona discharge or plasma, a method using a high electric field, a hydrocharging method using a polar solvent such as water, etc. Among these, the corona discharge method and hydrocharging method are preferred because they can obtain high electrostatic charge with a relatively low amount of electricity.

[0068] The apparatus and conditions used for the corona discharge method are not particularly limited, and for example, a DC high-voltage stabilized power supply can be used under the following conditions: linear distance between electrodes to which voltage is applied: 5 to 70 mm (preferably 10 to 50 mm), applied voltage: -50 to -10 kV and / or 10 to 50 kV (preferably -40 to -20 kV and / or 20 to 40 kV), temperature: room temperature (20°C) to 100°C (preferably 30 to 80°C), treatment time: 0.1 to 20 seconds (preferably 0.5 to 10 seconds).

[0069] In the hydrocharging method, for example, a polar solvent such as water or an organic solvent (preferably water from the viewpoint of productivity of wastewater treatment, etc.) is sprayed onto the MB nonwoven fabric, or the MB nonwoven fabric is vibrated while being sprayed, thereby electrifying the fabric. The pressure of the polar solvent collided with the MB nonwoven fabric is preferably 0.1 to 5 MPa, more preferably 0.5 to 3 MPa, and the suction pressure from the bottom is preferably 500 to 5000 mmH2O, more preferably 1000 to 3000 mmH2O. The hydrocharging treatment time is preferably 0.01 to 5 seconds, more preferably 0.02 to 1 second. The charged MB nonwoven fabric after the hydrocharging method is preferably dried at a temperature of, for example, 40 to 100°C, preferably 50 to 80°C. EXAMPLES

[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples and comparative examples, various physical properties were measured by the following methods.

[0071] [Viscosity of resin melt (poise)] For the cyclic olefin resins used in each Example and Comparative Example, a Toyo Seiki Capillograph 1B model was used, and the temperature of the supply section of each Example and Comparative Example was set, and the shear rate was r = 1200 sec -1 The viscosity was measured under the following conditions: The viscosity measured under these conditions was taken as the viscosity (η) of the molten resin introduced into the kneading section.

[0072] [Mean fiber diameter, 3rd quartile Super average fiber diameter] The MB nonwoven fiber structure was observed using a scanning electron microscope. The diameters of 100 randomly selected fibers were measured from the electron microscope photographs magnified 1000 times, and the average fiber diameter, CV value, average fiber diameter Dc of fibers with diameters larger than the first quartile and smaller than the third quartile, and average fiber diameter Db of fibers with diameters larger than the third quartile were calculated from the fiber diameter distribution.

[0073] [Metaku] According to JIS L 1913 "General nonwoven fabric test method" 6.2, the basis weight (g / m 2 ) was measured.

[0074] Thickness The thickness of the MB nonwoven fabric was measured according to JIS L 1913 "General nonwoven fabric testing method" 6.1.

[0075] [Breathability] In accordance with JIS L 1096 "Testing methods for woven and knitted fabrics" 8.26, the air permeability (cm 3 / cm 2 ·s) was measured.

[0076] [Collection performance] Collection efficiency (%) and pressure loss (Pa) In accordance with JIS T 8151, the charged nonwoven fabric was cut into a piece with a diameter of 11 cm and placed on a sample stand with a filtration section of 8.6 cm diameter (filtration area: 58.1 cm 2The collection efficiency (%) and pressure loss (Pa) were measured when filtering NaCl particles (average particle size: 0.1 μm) at a filter size of 20 L / min, air volume of 20 L / min, and face velocity of 5.7 cm / sec.

[0077] ( Reference example 1) As a cyclic olefin resin, an ethylene-norbornene copolymer having a norbornene content of 75% by mass (manufactured by Polyplastics Co., Ltd., product name "TOPAS" 5013) was heated and melted at 360°C in the supply section, and the resin melt was introduced into the kneading section. The viscosity (η) of the resin melt introduced into the kneading section was 100 poise. In the kneading section, the resin melt was kneaded at a screw rotation speed (N) of 5.0 rpm while being heated at 380°C. The obtained resin kneaded product was supplied to a die having a nozzle with a nozzle single hole diameter (diameter) of 0.15 mm, nozzle single hole length / nozzle single hole diameter = 10, and nozzle hole pitch of 0.75 mm, and hot air at a temperature of 340°C was blown at an air volume of 15 Nm per 1 m of nozzle width. 3 The resin mixture was discharged from the nozzle at a spinning temperature of 380°C and a discharge rate (Q) of 2.2 kg / hr while being sprayed at a rate of 100 / min. The filamentous material discharged from the nozzle was collected in a collection net and had a basis weight of 34.2 g / m 2 A cyclic olefin meltblown nonwoven fabric having a thickness of 0.430 mm was obtained. An enlarged electron microscope photograph of the obtained meltblown nonwoven fabric is shown in FIG.

[0078] Example 2 Other than the nozzle diameter being 0.3 mm, Reference example The same procedure as in Example 1 was carried out. The basis weight of the obtained meltblown nonwoven fabric was 31.8 g / m 2 The thickness is 0.608 mm, and an enlarged electron microscope photograph is shown in FIG.

[0079] ( Reference example 3) The heating temperature in the supply section was 350°C, the kneading conditions in the kneading section were heating at 360°C, the screw rotation speed (N) was 10.5 rpm, and the spinning conditions were a spinning temperature of 360°C and a discharge rate (Q) of 4.3 kg / hr, with the exception that the resin melt was discharged from the nozzle. The viscosity (η) of the resin melt introduced into the kneading section was 150 poise. The basis weight of the obtained meltblown nonwoven fabric was 31.2 g / m 2 The thickness is 0.612 mm, and an enlarged electron microscope photograph is shown in FIG.

[0080] Example 4 The same procedure as in Example 2 was carried out, except that the resin used was an ethylene-norbornene copolymer with a norbornene content of 75% by mass (manufactured by Polyplastics Co., Ltd., product name "TOPAS" 6013). The viscosity (η) of the molten resin introduced into the kneading section was 180 poise. The basis weight of the obtained meltblown nonwoven fabric was 20.7 g / m 2 The thickness is 0.286 mm, and an enlarged electron microscope photograph is shown in FIG.

[0081] Comparative Example 1 The heating temperature in the supply section was 300°C, the kneading conditions in the kneading section were heating at 320°C, the screw rotation speed (N) was 10.8 rpm, and the spinning conditions were a spinning temperature of 320°C and a discharge rate (Q) of 4.8 kg / hr, with the exception that the resin melt was discharged from the nozzle. The viscosity (η) of the resin melt introduced into the kneading section was 270 poise. The basis weight of the obtained meltblown nonwoven fabric was 70.3 g / m 2 The thickness is 1.154 mm, and an enlarged electron microscope photograph is shown in FIG.

[0082] [Table 1]

[0083] As shown in Table 1, in Comparative Example 1, the viscosity of the resin melt introduced into the kneading section was high, and (Q×η) / N was also high, so mechanical energy was applied to the cyclic olefin resin, and many thick fibers were present due to the mechanochemical reaction (FIG. 6). Due to the inclusion of these thick fibers, the average fiber diameter and the average fiber diameter Db of fibers larger than the third quartile of the MB nonwoven fabric of Comparative Example 1 were Reference Examples 1 and 3 and Examples 2 and 4 The air permeability was larger than that of the MB nonwoven fabric. Reference Examples 1 and 3 and Examples 2 and 4 The thickness was larger than that of the original and the density was insufficient.

[0084] on the other hand, Reference Examples 1 and 3 and Examples 2 and 4 In the case of the PTFE-CNT, the viscosity of the molten resin introduced into the kneading section was controlled to be low, which made it possible to suppress the generation of thick fibers resulting from the mechanochemical reaction (Figs. 2-5). Reference Examples 1 and 3 and Examples 2 and 4 In the MB nonwoven fabric, both the average fiber diameter and the average fiber diameter Db of fibers larger than the third quartile were smaller than those in Comparative Example 1.

[0085] In addition, the obtained MB nonwoven fabric had a smaller air permeability than that of Comparative Example 1, and the denseness could be improved. Reference example 1 And examples The MB nonwoven fabrics of Examples 2 and 4 had a small air permeability per thickness (B / A) and were particularly excellent in density. In particular, the MB nonwoven fabrics of Examples 2 and 4 had a good feel to the touch, probably because the CV value of the average fiber diameter of the constituent fibers could be suppressed to 90% or less.

[0086] Example 5 The meltblown nonwoven fabric obtained in Example 2 was subjected to a charging treatment by a corona discharge method. The specific conditions of the corona discharge method are as follows. The collection efficiency (%) and pressure loss (Pa) of the obtained charged nonwoven fabric were measured according to the above-mentioned method. The results are shown in Table 2. Power supply: DC high voltage stabilized power supply - Linear distance between electrodes to which voltage is applied: 35 mm Applied voltage: -28kV ·Applied current: 8.0mA ·Temperature: 25℃ Processing time: 1 second

[0087] Example 6 A charged nonwoven fabric was obtained in the same manner as in Example 5, except that the meltblown nonwoven fabric obtained in Example 4 was used instead of the meltblown nonwoven fabric obtained in Example 2. The collection efficiency (%) and pressure loss (Pa) of the obtained charged nonwoven fabric were measured according to the methods described above. The results are shown in Table 2.

[0088] [Table 2]

[0089] The charged nonwoven fabrics obtained in Examples 5 and 6 have a collection efficiency of 85% or more and a pressure loss of 10 Pa or less, and can therefore be suitably used for various filter applications. [Industrial Applicability]

[0090] As described above, the MB nonwoven fabric of the present invention can be used for various applications such as medical, cosmetic, and sanitary materials, industrial materials, daily necessities, and clothing. In particular, since it has excellent density and low elution of impurities, it can be suitably used in liquid filtration filters, air filters (e.g., clean room air filters), transdermal administration sheets (e.g., transdermal absorption agents, patches), etc.

[0091] As described above, a preferred embodiment of the present invention has been described with reference to the drawings, but various additions, modifications, or omissions can be made without departing from the spirit of the present invention, and such additions, modifications, or omissions are also included in the scope of the present invention. [Explanation of symbols]

[0092] 10... Extruder 12 Hopper 20···Screw 22...Supply section 24...Kneading section 26...Compression section 28...Measuring part 30···Cylinder 40···Die 42 Nozzle 50....Extruded filament 60...Collection member 62...Collection surface

Claims

1. A meltblown nonwoven fabric composed of fibers containing a cyclic olefin resin, wherein the average value of data having a fiber diameter larger than the third quartile obtained by dividing the data into quartiles from small fiber diameter data to large fiber diameter data out of fiber diameter data of 100 points randomly selected in an SEM image magnified 1000 times is 30 μm or less, and the CV value of the average fiber diameter is 90% or less.

2. The meltblown nonwoven fabric according to claim 1, wherein the cyclic olefin resin is a copolymer containing at least a norbornene unit.

3. The meltblown nonwoven fabric according to claim 1 or 2, having an air permeability of 10 to 550 cm as measured in accordance with JIS L 1906. 3 / cm 2 A meltblown nonwoven fabric.

4. The meltblown nonwoven fabric according to any one of claims 1 to 3, having a basis weight of 10 to 50 g / m 2 This is meltblown nonwoven fabric.

5. The meltblown nonwoven fabric according to any one of claims 1 to 4, wherein the meltblown nonwoven fabric satisfies the following formula (1). 80≦B / A≦800 (1) [Wherein, A: thickness (mm), B: air permeability (cm 3 / cm 2 s) represents

6. The meltblown nonwoven fabric according to any one of claims 1 to 5, comprising fibers having an average fiber diameter of 1 to 15 μm.

7. The meltblown nonwoven fabric according to any one of claims 1 to 6, wherein the ratio Db / Dc of the average fiber diameter (Db), which is the average value of data having fiber diameters larger than the first quartile and smaller than the third quartile, to the average fiber diameter (Dc), which is the average value of data having fiber diameters larger than the third quartile, is 3.5 or less.

8. The meltblown nonwoven fabric according to any one of claims 1 to 7, having a thickness of 0.10 to 0.85 mm.

9. A filter using the meltblown nonwoven fabric according to any one of claims 1 to 8.

10. A support used in a transdermal administration sheet that releases an active ingredient, comprising the meltblown nonwoven fabric according to any one of claims 1 to 8.

11. A transdermal administration sheet comprising at least an active ingredient and the support according to claim 10.

Citation Information

Patent Citations

  • Electlet

    JP2001210549A

  • Production of microfiber webs containing cycloolefin polymers

    JP2003504523A

  • Nonwoven amorphous fiber web and method of making same

    JP2005526923A

  • Filter for liquid filtration for trapping trace metal

    JP2011231163A

  • Fiber or fibrous molded article

    JP2011256490A