Negative photosensitive composition comprising a black colorant

A negative photosensitive composition with an alkali-soluble resin and a black colorant with specific transmittance properties addresses the challenges of high resolution and light-shielding in display devices, forming thick films effectively and using low-concentration alkaline developers for environmental friendliness.

JP7556068B2Active Publication Date: 2024-09-25MERCK PATENT GMBH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023004596
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-31
Filing Date
2023-01-16
Publication Date
2024-09-25
Estimated Expiration
2040-07-29

AI Technical Summary

Technical Problem

Existing negative photosensitive compositions used in display devices face challenges in achieving high resolution and effective light-shielding properties, particularly when forming thick films, and there is a need for compositions that can be developed with low-concentration alkaline developers to reduce environmental impact.

Method used

A negative photosensitive composition comprising an alkali-soluble resin, a black colorant with specific transmittance properties, a polymerization initiator, and a solvent, which allows for the formation of cured films with high resolution and excellent light-shielding capabilities, and can be developed using low-concentration alkaline developers.

Benefits of technology

The composition achieves high resolution and excellent light-shielding properties, enabling the formation of thick films suitable for display devices, while being environmentally friendly by using low-concentration alkaline developers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556068000001
    Figure 0007556068000001
  • Figure 0007556068000002
    Figure 0007556068000002
  • Figure 0007556068000003
    Figure 0007556068000003
Patent Text Reader

Abstract

To provide a negative photosensitive composition capable of forming a cured film with high resolution and high light-shielding properties. [Solution] A negative-tone photosensitive composition comprising (I) an alkali-soluble resin, (II) a black colorant, (III) a polymerization initiator, and (IV) a solvent, wherein the black colorant (II) has a transmittance ratio, expressed as [transmittance at a wavelength of 365 nm] / [transmittance at a wavelength of 500 nm], of 1.2 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative-type photosensitive composition containing a black colorant. The present invention also relates to a method for producing a cured film using the composition, a cured film formed from the composition, and a display device having the cured film. [Background technology]

[0002] The black matrix for color filters used in color display devices is formed by dispersing light-shielding black pigments such as carbon black in an alkali-soluble resin to form a resist composition, which is then applied, exposed, developed, and patterned. For example, in liquid crystal display elements, black matrices are used to prevent light leakage from between non-switching pixels and maintain high contrast. In addition, amorphous silicon and oxide semiconductors generate leakage current due to photoexcitation when exposed to light, so the black matrix layer blocks light from reaching the thin film transistors, thereby suppressing leakage current.

[0003] When a resist composition containing the above black pigment is used, the black pigment absorbs light during exposure, preventing the light from reaching the bottom of the resist film, adversely affecting patterning, making it difficult to achieve high resolution compared to normal resist compositions. A material capable of achieving a thicker film is required as a partition material for display devices, but when a resist composition containing a black pigment is used to form a thicker film, the effect of absorption by the black pigment becomes even greater than in the case of a thin film. In addition, in consideration of the environmental impact, there has been a demand for the development of a composition that can be developed with a low-concentration alkaline developer other than an organic developer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-203599 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a negative-type photosensitive composition capable of forming a cured film having high resolution and excellent light-shielding properties. [Means for solving the problem]

[0006] The negative-type photosensitive composition according to the present invention comprises (I) an alkali-soluble resin, (II) a black colorant, (III) a polymerization initiator, and (IV) a solvent, and the black colorant (II) has a transmittance ratio, expressed as [transmittance at a wavelength of 365 nm] / [transmittance at a wavelength of 500 nm], of 1.2 or more.

[0007] The method for producing a cured film according to the present invention comprises applying the above-mentioned negative photosensitive composition to a substrate to form a coating film, exposing the coating film to light, and developing the coating film.

[0008] The cured film according to the present invention is produced by the method described above.

[0009] A display device according to the present invention comprises the above-mentioned cured film. Effect of the Invention

[0010] The negative-type photosensitive composition according to the present invention can form a cured film having high resolution and excellent light-shielding properties. Furthermore, the negative-type photosensitive composition according to the present invention can be developed using a low-concentration alkaline developer other than an organic developer, and is also environmentally friendly. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described in detail. In this specification, unless otherwise specified, the symbols, units, abbreviations and terms have the following meanings. In this specification, unless otherwise specified, the singular includes the plural, and "a" or "the" means "at least one." In this specification, unless otherwise specified, a concept may be expressed by a plurality of kinds, and when an amount (e.g., mass % or mole %) is described, the amount means the sum of the plurality of kinds. "And / or" includes all combinations of elements and also includes the use of a single element.

[0012] In this specification, when a numerical range is indicated using ~ or -, it includes both endpoints and the units are the same. For example, 5 to 25 mol % means 5 mol % or more and 25 mol % or less.

[0013] In this specification, the term "hydrocarbon" refers to a group containing carbon and hydrogen and, where necessary, oxygen or nitrogen. The term "hydrocarbon group" refers to a monovalent or divalent or higher hydrocarbon group. In this specification, the term "aliphatic hydrocarbon" refers to a linear, branched or cyclic aliphatic hydrocarbon, and the term "aliphatic hydrocarbon group" refers to a monovalent or divalent or higher aliphatic hydrocarbon. The term "aromatic hydrocarbon" refers to a hydrocarbon containing an aromatic ring, which may have an aliphatic hydrocarbon group as a substituent or may be condensed with an alicyclic ring, if necessary. The term "aromatic hydrocarbon group" refers to a monovalent or divalent or higher aromatic hydrocarbon. The term "aromatic ring" refers to a hydrocarbon having a conjugated unsaturated ring structure, and the term "alicyclic ring" refers to a hydrocarbon having a ring structure but not including a conjugated unsaturated ring structure.

[0014] In this specification, alkyl means a group in which one arbitrary hydrogen has been removed from a linear or branched saturated hydrocarbon, and includes linear alkyl and branched alkyl, and cycloalkyl means a group in which one hydrogen has been removed from a saturated hydrocarbon containing a cyclic structure, and optionally includes a linear or branched alkyl in the cyclic structure as a side chain.

[0015] In this specification, aryl refers to a group obtained by removing one arbitrary hydrogen from an aromatic hydrocarbon. Alkylene refers to a group obtained by removing two arbitrary hydrogens from a linear or branched saturated hydrocarbon. Arylene refers to a hydrocarbon group obtained by removing two arbitrary hydrogens from an aromatic hydrocarbon.

[0016] In this specification, "C x~y ", "C x ~C y " and "C x " refers to the number of carbons in a molecule or substituent. For example, C 1~6 Alkyl refers to an alkyl having 1 to 6 carbon atoms (methyl, ethyl, propyl, butyl, pentyl, hexyl, etc.). In addition, as used herein, fluoroalkyl refers to an alkyl group in which one or more hydrogen atoms have been replaced with fluorine, and fluoroaryl refers to an aryl group in which one or more hydrogen atoms have been replaced with fluorine.

[0017] In the present specification, when a polymer has multiple types of repeating units, these repeating units are copolymerized. The copolymerization may be alternating copolymerization, random copolymerization, block copolymerization, graft copolymerization, or a mixture thereof. In this specification, % means % by mass, and ratio means mass ratio.

[0018] In this specification, the unit of temperature is Celsius. For example, 20 degrees means 20 degrees Celsius.

[0019] <Negative Photosensitive Composition> The negative photosensitive composition according to the present invention (hereinafter, simply referred to as "composition") comprises (I) an alkali-soluble resin, (II) a specific black colorant, (III) a polymerization initiator, and (IV) a solvent. Each component contained in the composition according to the present invention will be described in detail below. The composition according to the present invention is a negative type photosensitive composition for thick films that is effective for films of 100 μm or less, but is even more effective when forming thick films. In the present invention, a thick film means a film having an average film thickness of 5 to 100 μm (preferably 5 to 25 μm, more preferably 8 to 20 μm). In the present invention, the average film thickness is determined by measuring the film thickness at 3 to 5 points using a stylus-type surface profiler manufactured by ULBAC Corporation, and averaging the measured values. The viscosity of the composition according to the present invention is preferably 0.1 to 10,000 cP, and more preferably 1.0 to 8,000 cP, where the viscosity is measured at 25° C. using a rotational viscometer.

[0020] (I) Alkali-soluble resin The composition according to the present invention comprises an alkali-soluble resin. The alkali-soluble resin used in the present invention preferably contains an acryloyl group. The alkali-soluble resin used in the present invention is not particularly limited, but is preferably selected from polysiloxanes and acrylic resins that contain siloxane bonds in the main skeleton. Among these, it is more preferable to use polysiloxanes from the viewpoint of dispersibility of the black colorant and heat resistance. The alkali-soluble resin used in the present invention may have a carboxyl group. By having a carboxyl group, the solubility of the alkali-soluble resin in a low-concentration developer can be improved.

[0021] (Polysiloxane) The alkali-soluble resin preferably contains a siloxane (Si-O-Si) bond as the main skeleton. In the present invention, a polymer containing a siloxane bond as the main skeleton is called a polysiloxane. The skeleton structure of polysiloxane can be classified into a silicone skeleton (the number of oxygen atoms bonded to a silicon atom is 2), a silsesquioxane skeleton (the number of oxygen atoms bonded to a silicon atom is 3), and a silica skeleton (the number of oxygen atoms bonded to a silicon atom is 4) according to the number of oxygen atoms bonded to the silicon atom. In the present invention, any of these may be used. The polysiloxane molecule may contain a combination of a plurality of these skeleton structures. Preferably, the polysiloxane used in the present invention contains a silsesquioxane skeleton. Polysiloxane generally has a silanol group or an alkoxysilyl group. Such silanol group and alkoxysilyl group refer to hydroxyl group and alkoxy group that are directly bonded to silicon that forms siloxane skeleton. Here, silanol group and alkoxysilyl group have the effect of promoting the curing reaction when forming a cured film using the composition, and are also considered to contribute to the reaction with silicon-containing compound described later. Therefore, it is preferable that polysiloxane has these groups.

[0022] The polysiloxane used in the present invention preferably comprises a repeating unit represented by the formula (Ia'): [ka] (In the formula, R a1’ is hydrogen or methyl, Each m' is independently an integer of 1 to 6, preferably an integer of 1 to 3, and most preferably 3. The present invention relates to a method for producing a semiconductor device comprising the steps of:

[0023] As described later, polysiloxane containing a repeating unit represented by formula (Ia) can be obtained by (1) reacting an acryloyl group-containing silane monomer to obtain an acryloyl group-containing polysiloxane, and (2) cleaving the carbon-carbon double bond in the obtained acryloyl group-containing polysiloxane and polymerizing it. If unreacted acryloyl groups remain in this step (2), it becomes a polysiloxane having a repeating unit represented by formula (Ia'). A polysiloxane obtained only by step (1) without carrying out step (2) is also one aspect of the present invention. In other words, a polysiloxane that does not contain a repeating unit represented by formula (Ia) but contains a repeating unit represented by formula (Ia') is also a suitable aspect.

[0024] Preferably, the polysiloxane used in the present invention comprises a repeating unit represented by formula (Ia): [ka] (In the formula, R a1 is hydrogen or methyl, ma is each independently an integer of 1 to 6, preferably an integer of 1 to 3, and most preferably 3; and An acrylic polymeric unit represented by formula (a): [ka] (In the formula, R a2 are each independently hydrogen or methyl; R a3 is hydrogen, 1 to 6 valences, C 1~50 wherein one or more methylenes may be replaced by oxy, imino, and / or carbonyl; R a3 If is multivalent, R a3 connects the carbonyloxy in formula (a) to the carbonyloxy contained in another repeating unit represented by formula (a), na is an integer equal to or greater than 0. comprising At least one repeating unit * in formula (Ia) is bonded to another repeating unit * represented by formula (Ia) directly or via an acrylic polymerized unit represented by formula (a).

[0025] In the acrylic polymerization unit represented by formula (a), the formula (a) may be bonded to another formula (a) to form a block. However, if there are many acrylic polymerization units, the heat resistance tends to decrease. Therefore, in one molecule of polysiloxane, The sum of na / (the number of repeating units represented by (Ia)+the sum of na) is preferably 0.15 or less, and more preferably 0.05 or less. As long as na satisfies the above conditions, it is not particularly limited, but is preferably 0 to 6, more preferably 0 to 4, and even more preferably 1 or 2. When a plurality of (a)s are included, each na may be the same or different. R a3 Since the heat resistance of fluorine tends to decrease as the number of carbon atoms increases, hydrogen or C 1~30 is preferably a hydrocarbon group of the formula: 1~20 is a hydrocarbon group. The acrylic polymer unit represented by the formula (a) is not essential, but is preferably contained in order to improve adhesion.

[0026] R a3 Examples include the following: [ka] [ka] [ka]

[0027] Of the above, hydrogen, tris-(2-acryloxyethyl)isocyanurate, and dipentaerythritol hexaacrylate are preferred. When the repeating unit represented by formula (a) is a group derived from an acrylic compound containing a plurality of double bonds, it is preferred that some of the double bonds remain uncleaved.

[0028] Among the polymerization units represented by formula (a), R a3 may be an acrylic polymerization unit which is a group obtained by removing a plurality of hydrogen atoms, preferably two or three hydrogen atoms, from a nitrogen- and / or oxygen-containing cyclic aliphatic hydrocarbon compound containing a hydrocarbon group substituted with an amino group, an imino group, and / or a carbonyl group (preferably a group obtained by removing two or three hydrogen atoms from a nitrogen-containing aliphatic hydrocarbon ring containing an imino group and / or a carbonyl group, more preferably a five- or six-membered ring containing nitrogen as a constituent member, and most preferably a group obtained by removing two or three hydrogen atoms from a piperidine derivative, a pyrrolidine derivative, or an isocyanurate derivative).

[0029] The repeating units represented by formulae (Ia) and (Ia') preferably account for 10 to 100 mol % of the total number of repeating units in the polysiloxane, since a high compounding ratio reduces heat resistance. In this specification, "with respect to the total number of repeating units of the polysiloxane" means the total number of repeating units of the siloxane of the polysiloxane, and for example, the acrylic polymerization unit represented by formula (a) is not included in this total number.

[0030] The polysiloxane according to the present invention preferably contains a repeating unit represented by formula (Ib). [ka] (In the formula, R b1 is hydrogen, C 1~30 represents a linear, branched or cyclic, saturated or unsaturated, aliphatic or aromatic hydrocarbon group; The aliphatic hydrocarbon group and the aromatic hydrocarbon group may each be substituted with fluorine, hydroxy, alkoxy, aldehyde (-CHO), carboxyl, or -COOR' (wherein R' is an alkyl group having 1 to 8 carbon atoms); and In the aliphatic hydrocarbon group and the aromatic hydrocarbon group, one or more methylenes may be replaced by oxy or imino, provided that R b1 is not hydroxy or alkoxy) The above methylene includes the terminal methyl. In addition, the above phrase "optionally substituted with fluorine, hydroxy, alkoxy, aldehyde, carboxyl, or -COOR'" means that a hydrogen atom directly bonded to a carbon atom in the aliphatic hydrocarbon group and aromatic hydrocarbon group may be substituted with fluorine, hydroxy, alkoxy, aldehyde, carboxyl, or -COOR'. The same applies to other similar descriptions in this specification.

[0031] In the repeating unit represented by formula (Ib), R b1 Examples of the fluoroalkyl include (i) alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, and decyl; (ii) aryl groups such as phenyl, tolyl, and benzyl; (iii) fluoroalkyl groups such as trifluoromethyl, 2,2,2-trifluoroethyl, and 3,3,3-trifluoropropyl; (iv) fluoroaryl groups; (v) cycloalkyl groups such as cyclohexyl; (vi) nitrogen-containing groups having an amino or imide structure such as isocyanate and amino; (vii) oxygen-containing groups having an epoxy structure such as glycidyl; and (viii) carboxyl-containing groups such as carboxymethyl and dicarboxyl. Preferred are methyl, ethyl, propyl, butyl, pentyl, hexyl, phenyl, tolyl, glycidyl, and isocyanate. Preferred fluoroalkyl groups are perfluoroalkyl groups, particularly trifluoromethyl and pentafluoroethyl. R b1When R is methyl, the raw material is easily available, the hardness of the film after curing is high, and the film has high chemical resistance, which is preferable. b1 When R is phenyl, this is preferable because it increases the solubility of the polysiloxane in a solvent and makes the cured film less susceptible to cracking. b1 It is preferable that the compound has a hydroxyl, glycidyl, isocyanate or amino group, since this improves the adhesion to the substrate.

[0032] The polysiloxane used in the present invention includes, for example, those having the following structure. [ka]

[0033] If the compounding ratio of the repeating unit represented by formula (Ib) is high, the strength and heat resistance of the cured film formed will increase but the adhesion will decrease, so it is preferable that the compounding ratio is 0 to 90 mol % based on the total number of repeating units of the polysiloxane.

[0034] The polysiloxane used in the present invention preferably comprises a repeating unit represented by formula (Ic). [ka]

[0035] The polysiloxane used in the present invention may contain a repeating unit represented by formula (Id). [ka] During the ceremony, R d1 is a group obtained by removing multiple hydrogen atoms from a nitrogen- and / or oxygen-containing cyclic aliphatic hydrocarbon compound containing an amino group, an imino group, and / or a carbonyl group, where the cyclic aliphatic hydrocarbon compound has a cyclic structure, but may also contain a linear or branched structure as necessary.

[0036] In formula (Id), Rd1 is preferably a group obtained by removing multiple, more preferably two or three, hydrogen atoms from a nitrogen-containing aliphatic hydrocarbon ring containing an imino group and / or a carbonyl group, more preferably a five- or six-membered ring containing nitrogen as a constituent member. For example, it may be a group obtained by removing two or three hydrogen atoms from piperidine, pyrrolidine, and isocyanurate. The group not bonded to oxygen in formula (Id) connects Si atoms contained in multiple repeating units together.

[0037] If the compounding ratio of the repeating units represented by formula (Id) and formula (Ic) is high, the sensitivity of the composition may decrease, the compatibility with solvents and additives may decrease, and the film stress may increase, making cracks more likely to occur. Therefore, the compounding ratio is preferably 40 mol % or less, and more preferably 20 mol % or less, based on the total number of repeating units of the polysiloxane.

[0038] The polysiloxane used in the present invention may contain a repeating unit represented by formula (Ie). [ka] During the ceremony, R e1 are each independently hydrogen, C 1~30 represents a linear, branched or cyclic, saturated or unsaturated, aliphatic or aromatic hydrocarbon group; The aliphatic hydrocarbon group and the aromatic hydrocarbon group may be substituted with fluorine, hydroxy or alkoxy; and In the aliphatic hydrocarbon group and the aromatic hydrocarbon group, methylene may be replaced by oxy or imino, provided that R e1 is not hydroxy or alkoxy. The above methylene includes the terminal methyl.

[0039] In the repeating unit represented by formula (Ie), R e1Examples of the fluoroalkyl include (i) alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, and decyl, (ii) aryl groups such as phenyl, tolyl, and benzyl, (iii) fluoroalkyl groups such as trifluoromethyl, 2,2,2-trifluoroethyl, and 3,3,3-trifluoropropyl, (iv) fluoroaryl groups, (v) cycloalkyl groups such as cyclohexyl, (vi) nitrogen-containing groups having an amino or imide structure such as isocyanate and amino, and (vii) oxygen-containing groups having an epoxy structure such as glycidyl. Preferred are methyl, ethyl, propyl, butyl, pentyl, hexyl, phenyl, tolyl, glycidyl, and isocyanate. Preferred fluoroalkyl groups are perfluoroalkyl groups, particularly trifluoromethyl and pentafluoroethyl. R e1 When R is methyl, the raw material is easily available, the hardness of the film after curing is high, and the film has high chemical resistance, which is preferable. e1 When R is phenyl, this is preferable because it increases the solubility of the polysiloxane in a solvent and makes the cured film less susceptible to cracking. e1 It is preferable that the compound has a hydroxyl, glycidyl, isocyanate or amino group, since this improves the adhesion to the substrate.

[0040] By having the repeating unit represented by the above formula (Ie), the polysiloxane used in the present invention can have a partially linear structure. However, since the heat resistance is reduced, it is preferable that the linear structure portion is small. Specifically, it is preferable that the repeating unit represented by the formula (Ie) is 30 mol % or less with respect to the total number of repeating units of the polysiloxane.

[0041] The polysiloxane used in the present invention has a structure in which the repeating units or blocks described above are bonded, but it is preferable that the polysiloxane has a silanol group at the end. Such a silanol group is formed by bonding the repeating units or blocks to the bonds described above. 0.5 H is bonded.

[0042] The mass average molecular weight of the polysiloxane used in the present invention is not particularly limited. However, the higher the molecular weight, the more the coating property tends to be improved. On the other hand, the lower the molecular weight, the fewer restrictions on synthesis conditions, and the easier the synthesis, while polysiloxanes with very high molecular weights are difficult to synthesize. For these reasons, the mass average molecular weight of the polysiloxane is usually 1,500 to 20,000, and from the viewpoint of solubility in organic solvents and solubility in alkaline developers, it is preferably 2,000 to 15,000. Here, the mass average molecular weight is the polystyrene-equivalent mass average molecular weight, which can be measured by gel permeation chromatography using polystyrene as a standard.

[0043] The polysiloxane used in the present invention may be a mixture of a polysiloxane containing repeating units represented by (Ia) and / or (Ia') and a polysiloxane containing any of repeating units represented by (Ib) to (Ie) but not containing repeating units represented by (Ia) and / or (Ia').

[0044] The polysiloxane containing (Ia) is, for example, The process is as follows: (1) Formula (ia): [ka] (In the formula, R a1’’ is hydrogen or methyl, ma'' is an integer of 1 to 6, preferably an integer of 1 to 3, and most preferably 3; and R ia is linear or branched, C 1~6 (It is alkyl) or a mixture thereof and optionally hydrolyzing and polymerizing the compound in the presence of an acidic or basic catalyst to obtain an acryloyl group-containing polysiloxane. (2) Cleavage of the carbon-carbon double bonds in the resulting acryloyl group-containing polysiloxane and polymerization. can be obtained by Here, the above mixture may be a mixture of a silane monomer represented by formula (ia) and another silane monomer represented by formula (ia), a mixture of silane monomers represented by the following formulas (ib) to (ie), or a mixture of a compound other than the silane monomer.

[0045] The polysiloxane obtained by the above process gives a composition exhibiting excellent properties, and the resulting structure includes, for example, those exemplified above, but since various structures can be obtained depending on the types and compounding ratios of monomers, it is considered that structures other than those exemplified above can also be obtained.

[0046] [Process (1)] In the formula (ia), preferred R ia Examples of R include methyl, ethyl, n-propyl, isopropyl, and n-butyl. ia There are multiple R ia may be the same or different.

[0047] The silane monomer represented by formula (ia) is reacted with a silane monomer represented by formula (ib): R b1’ -Si-(OR ib )3(ib) (In the formula, R b1’ is hydrogen, C 1~30 represents a linear, branched or cyclic, saturated or unsaturated, aliphatic or aromatic hydrocarbon group; The aliphatic hydrocarbon group and the aromatic hydrocarbon group may be substituted with fluorine, hydroxy, alkoxy, aldehyde (-CHO), carboxyl, or -COOR' (wherein R' is an alkyl group having 1 to 8 carbon atoms); and In the aliphatic hydrocarbon group and the aromatic hydrocarbon group, methylene may be replaced by oxy or imino, provided that R b1’ is not hydroxy or alkoxy, R ib is linear or branched, C 1~6(It is alkyl) It is preferable to further combine a silane monomer represented by the following formula: In formula (ib), preferred R b1’ is the above preferred R b1 The preferred R ib Examples of aryl groups include methyl, ethyl, n-propyl, isopropyl, and n-butyl.

[0048] Specific examples of the silane monomer represented by formula (ib) include methyltrimethoxysilane, methyltriethoxysilane, methyltriisopropoxysilane, methyltri-n-butoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltriisopropoxysilane, ethyltri-n-butoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-butyltrimethoxysilane, n-butyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, decyltrimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, trifluoromethyltrimethoxysilane, trifluoromethyltriethoxysilane, and 3,3,3-trifluoropropyltrimethoxysilane. Among these, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, and phenyltrimethoxysilane are preferred. The silane monomer represented by formula (ib) may be used in combination of two or more kinds.

[0049] The silane monomers represented by the above formula (ia) and / or (ib) can be further combined with the silane monomers represented by the following formula (ic) and / or (id) to obtain an acrylic polymerized polysiloxane. By using the silane monomers represented by the formula (ic) and / or formula (id) in this manner, a polysiloxane containing the repeating units (Ic) and / or (Id) can be obtained. Si(OR ic )4(ic) R d1’ -Si-(OR id )3(id) in the formula, Ric and R id are each independently linear or branched, C 1~6 R is an alkyl group, for example, methyl, ethyl, n-propyl, isopropyl, and n-butyl. ic and R id is contained multiple times in one monomer, but each R ic and R id may be the same or different, R d1’ is a group obtained by removing multiple hydrogens from a nitrogen- and / or oxygen-containing cyclic aliphatic hydrocarbon compound, including an amino group, an imino group, and / or a carbonyl group. d1’ is the above preferred R d1 is the same as:

[0050] Specific examples of the silane monomer represented by formula (ic) include tetramethoxysilane, tetraethoxysilane, tetraisopropoxysilane, and tetra-n-butoxysilane.

[0051] Specific examples of the silane monomer represented by formula (id) include tris-(3-trimethoxysilylpropyl)isocyanurate, tris-(3-triethoxysilylpropyl)isocyanurate, and tris-(3-trimethoxysilylethyl)isocyanurate.

[0052] Furthermore, a silane monomer represented by the following formula (ie) may be combined: When the silane monomer represented by formula (ie) is used, a polysiloxane containing the repeating unit (Ie) can be obtained. (R e1’ )2-Si-(OR ie )2(ie) wherein: R ie are each independently linear or branched, C 1~6 R is an alkyl group, for example, methyl, ethyl, n-propyl, isopropyl, and n-butyl. ie is contained multiple times in one monomer, but each R iemay be the same or different, R e1’ are each independently hydrogen, C 1~30 represents a linear, branched or cyclic, saturated or unsaturated, aliphatic or aromatic hydrocarbon group; The aliphatic hydrocarbon group and the aromatic hydrocarbon group may be substituted with fluorine, hydroxy or alkoxy; and In the aliphatic hydrocarbon group and the aromatic hydrocarbon group, methylene may be replaced by oxy or imino, provided that R e1’ is not hydroxy or alkoxy. e1’ is the above preferred R e1 is the same as:

[0053] Specific examples of the silane monomer represented by the formula (ie) include dimethyldiethoxysilane, diphenyldimethoxysilane, and the like.

[0054] [Process (2)] In the step (2), the carbon-carbon double bonds of the acryloyl groups in the resulting acryloyl group-containing polysiloxane are cleaved and polymerized. In this reaction, it is preferable to use, as a polymerization initiator, an azo initiator such as 2,2'-azabisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, or 2,2'-azobis(2-methylpropionate) dimethyl; or a peroxide initiator such as dibenzoyl peroxide, tert-butyl hydroperoxide (70% aqueous solution), α,α-dimethylbenzyl hydroperoxide, tert-butyl peroxide, or bis(1-methyl-1-phenylethyl) peroxide. The carbon-carbon double bond of the acryloyl group is cleaved and polymerized, but some of it may remain without cleavage or polymerization. If it is polymerized, it contributes to low-concentration development, and if it is not polymerized, it has the effect of promoting hardening through the acrylic reaction. The content of the polymerization initiator is not particularly limited, but is preferably 0.1 to 500 mol % based on the number of acrylic functional groups.

[0055] In step (2), Formula (a'): [ka] (In the formula, R a2’ is hydrogen or methyl, R a3’ is C 1~50 In the hydrocarbon group, one or more methylenes may be replaced by oxy, imino, and / or carbonyl. a3’ is the above preferred R a3 is the same as x is an integer of 1 to 6, preferably an integer of 3 to 6. The polymerization reaction may be carried out in the presence of an acrylic acid ester monomer represented by the following formula: The above methylene also includes a terminal methyl.

[0056] The acrylic acid monomer represented by formula (a') may also be a nitrogen- and / or oxygen-containing cyclic aliphatic hydrocarbon compound containing an amino group, an imino group, and / or a carbonyl group, which may have multiple acrylic acid esters in the molecule (preferably a nitrogen-containing aliphatic hydrocarbon ring containing an imino group and / or a carbonyl group, more preferably a 5- or 6-membered ring containing nitrogen as a constituent member, and most preferably a piperidine derivative, a pyrrolidine derivative, or an isocyanurate derivative).

[0057] Examples of the acrylic acid ester monomer represented by formula (a') include methoxypolyethylene glycol acrylate, methoxypolyethylene glycol methacrylate, phenoxypolyethylene glycol acrylate, isostearyl acrylate, polyethylene glycol diacrylate, propoxylated bisphenol A diacrylate, tricyclodecane dimethanol diacrylate, 1,6-hexanediol diacrylate, dipropylene glycol diacrylate, ethoxylated isocyanuric acid triacrylate, ethoxylated glycerin triacrylate, trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, ethoxylated pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, and the like, and preferred are methoxypolyethylene glycol acrylate, tricyclodecane dimethanol diacrylate, and ethoxylated isocyanuric acid triacrylate.

[0058] In addition, in the radical polymerization reaction, the molecular weight can be controlled by appropriately using a known chain transfer agent, polymerization inhibitor, molecular weight regulator, etc. Furthermore, the polymerization reaction may be carried out in one stage or in two or more stages. The temperature of the polymerization reaction is not particularly limited, but is typically within the range of 50°C to 200°C, preferably 80°C to 150°C.

[0059] The polysiloxane acrylic-polymerized in step (2) has a complex three-dimensional structure due to the acrylic polymerization, which is believed to contribute to improving heat resistance and adhesion to the substrate. When a low-concentration developer is used, it is preferable to use polysiloxane that has been acrylic polymerized in the step (2). When a thick film is to be formed, it is preferable that the polysiloxane containing either (Ia) or (Ia') contains residual acryloyl groups. In the polysiloxane (Ia) acrylic polymerized in step (2), in a normal reaction, not all of the acryloyl groups react, and some acryloyl groups remain unpolymerized.

[0060] The mass average molecular weight of the acrylic-polymerized polysiloxane obtained in step (2) is preferably 1.4 to 5 times, and more preferably 1.4 to 3 times, the mass average molecular weight of the acryloyl group-containing polysiloxane obtained in step (1).

[0061] (Acrylic resin) The acrylic resin (also referred to as an acrylic polymer) used in the present invention can be selected from commonly used acrylic resins, such as polyacrylic acid, polymethacrylic acid, alkyl polyacrylate, alkyl polymethacrylate, etc. The acrylic resin used in the present invention preferably contains a repeating unit containing an acryloyl group, and also preferably further contains a repeating unit containing a carboxyl group and / or a repeating unit containing an alkoxysilyl group.

[0062] The repeating unit containing a carboxyl group is not particularly limited as long as it is a repeating unit containing a carboxyl group in the side chain, but is preferably a repeating unit derived from an unsaturated carboxylic acid, an unsaturated carboxylic anhydride, or a mixture thereof.

[0063] The repeating unit containing an alkoxysilyl group may be any repeating unit containing an alkoxysilyl group in the side chain, but is preferably a repeating unit derived from a monomer represented by the following formula (B). X B -(CH2) a -Si(OR B ) b (CH3) 3-b (B) In the formula, X B is a vinyl group, a styryl group, or a (meth)acryloyloxy group, and R B is a methyl group or an ethyl group, a is an integer of 0 to 3, and b is an integer of 1 to 3.

[0064] The polymer preferably contains a repeating unit containing a hydroxyl group, which is derived from a hydroxyl-containing unsaturated monomer.

[0065] The weight average molecular weight of the alkali-soluble resin according to the present invention is not particularly limited, but is preferably 1,000 to 40,000, and more preferably 2,000 to 30,000. Here, the weight average molecular weight is the polystyrene equivalent weight average molecular weight determined by gel permeation chromatography. The number of acid groups is generally 40 to 190 mgKOH / g, and more preferably 60 to 150 mgKOH / g, in terms of the acid value of the solid content, from the viewpoint of enabling development with a low-concentration alkaline developer and achieving both reactivity and storage stability.

[0066] Since polysiloxanes containing acryloyl groups can form thick films even when used alone, it is preferable to use polysiloxanes containing (Ia') and / or (Ia) as the alkali-soluble resin. When using a polysiloxane that does not contain (Ia') and (Ia), a mixture of the polysiloxane and an acrylic resin can be used as an alkali-soluble resin. In this case, the blending ratio of the acrylic resin and the polysiloxane is not particularly limited, but when the coating film is to be made thick, it is preferable that the blending ratio of the acrylic resin is high, while when applied to a high-temperature process, or from the viewpoint of transparency and chemical resistance after curing, it is preferable that the blending ratio of the polysiloxane is high. For these reasons, the blending ratio of the polysiloxane and the acrylic resin is preferably 90:10 to 10:90, and more preferably 85:15 to 25:75.

[0067] The composition according to the present invention is applied to a substrate, imagewise exposed, and developed to form a cured film. At this time, it is necessary that the solubility of the exposed and unexposed parts differs, and the coating film in the unexposed parts should have a certain level of solubility in a developer. For example, if the dissolution rate of the coating film after prebaking in a 2.38% aqueous solution of tetramethylammonium hydroxide (hereinafter sometimes referred to as TMAH) (hereinafter sometimes referred to as alkaline dissolution rate or ADR, described in detail later) is 50 Å / sec or more, it is considered possible to form a pattern by exposure-development. However, the solubility required varies depending on the average film thickness of the cured film to be formed and the development conditions, so an alkali-soluble resin should be appropriately selected according to the development conditions. Although it varies depending on the type and amount of photosensitizer and silanol condensation catalyst contained in the composition, for example, if the average film thickness is 0.1 to 100 μm (1,000 to 1,000,000 Å), the dissolution rate in a 2.38% TMAH aqueous solution is preferably 50 to 20,000 Å / sec, and more preferably 100 to 10,000 Å / sec.

[0068] [Measurement and calculation method of alkaline dissolution rate (ADR)] The alkaline dissolution rate of an alkali-soluble resin is measured and calculated as follows, using an aqueous TMAH solution as the alkaline solution.

[0069] The alkali-soluble resin is diluted to 35% by mass in propylene glycol monomethyl ether acetate (PGMEA) and dissolved at room temperature while stirring for 1 hour. In a clean room with a temperature of 23.0±0.5°C and humidity of 50±5.0%, 1 cc of the prepared alkali-soluble resin solution is dropped onto the center of a 4-inch, 525μm-thick silicon wafer using a pipette, and spin-coated to a thickness of 2±0.1μm. The solvent is then removed by heating on a hot plate at 100°C for 90 seconds. The thickness of the coating is measured using a spectroscopic ellipsometer (JA Woollam).

[0070] Next, the silicon wafer with this film was gently immersed in a 6-inch glass petri dish containing 100 ml of a TMAH aqueous solution of a given concentration adjusted to 23.0±0.1°C, and then left to stand, and the time until the coating film disappeared was measured. The dissolution rate was calculated by dividing the time until the film disappeared at a portion 10 mm inside from the edge of the wafer. If the dissolution rate is significantly slow, the wafer was immersed in the TMAH aqueous solution for a certain period of time, and then heated on a hot plate at 200°C for 5 minutes to remove the moisture that was taken into the film during the dissolution rate measurement, and the film thickness was measured, and the dissolution rate was calculated by dividing the change in film thickness before and after immersion by the immersion time. The above measurement method was performed five times, and the average of the obtained values ​​was taken as the dissolution rate of the alkali-soluble resin.

[0071] (II) Black colorant The composition according to the present invention contains a black colorant. In the present invention, the black colorant has a characteristic light absorption property. Specifically, the transmittance of the black pigment at a wavelength of 365 nm is I 365 , the transmittance at a wavelength of 500 nm is I 500 Then, I 365 / I 500 The transmittance ratio R is expressed as 365 / 500 is 1.2 or more, preferably 2.0 or more. Black colorants such as carbon black generally absorb not only visible light but also ultraviolet light. In this case, when a composition containing a black colorant is applied to a substrate to form a coating film, the black colorant absorbs ultraviolet light due to exposure, and the light does not reach the bottom of the coating film, so that a pattern may not be formed. However, a black colorant that satisfies the specific absorbance according to the present invention has low absorption of ultraviolet light and high absorption of visible light. Therefore, even when a thick film is formed, a pattern can be formed. And, since the visible light is highly absorbent, the formed cured film has high light-shielding properties and can function as a partition material for a display device. Here, the transmittance is measured by applying a composition in which 10 mass % of a black colorant is dispersed, based on the total mass of the resin, to form a film with a thickness of 10 μm, curing the film at 230°C, and then measuring the resulting film using UV-vis-NIR (Hitachi High-Technologies Corporation).

[0072] The black colorant used in the present invention may be an inorganic pigment or an organic pigment, or a combination of two or more pigments, so long as it satisfies the above-mentioned absorbance.

[0073] As an inorganic pigment, for example, zirconium nitride is preferable, specifically, "NITBLACK UB-1" by Mitsubishi Materials Corporation can be mentioned.

[0074] When the black colorant used in the present invention is an organic pigment, it is preferable to combine two or more kinds of pigments. A black colorant can be obtained by mixing each color such as red, green, and blue. The organic pigment is selected from those having structures such as azo, phthalocyanine, quinacridone, benzimidazolone, isoindolinone, dioxazine, indanthrene, and perylene. A preferred combination of pigments is, for example, a combination of one selected from the group consisting of CI Pigment Orange 43, CI Pigment Orange 64, and CI Pigment Orange 72, and CI Pigment Blue 60. This combination may be further combined with other organic pigments.

[0075] The content of the black colorant used in the present invention is preferably from 3 to 80% by mass, and more preferably from 5 to 50% by mass, based on the total mass of the composition. The content of the black colorant is based on the mass of the pigment itself. In other words, although the black colorant may be obtained in a dispersed state using a dispersant, in this case, the mass of the black colorant does not include anything other than the pigment.

[0076] The black colorant used in the present invention may be used in combination with a dispersant, such as an organic compound-based dispersant such as the polymer dispersant described in JP-A-2004-292672.

[0077] (III) Polymerization initiator The composition according to the present invention comprises a polymerization initiator. The polymerization initiator may be one that generates an acid, a base or a radical when exposed to radiation, or one that generates an acid, a base or a radical when exposed to heat. In the present invention, the reaction starts immediately after radiation exposure, and the reheating step performed after radiation exposure and before the development step can be omitted. Therefore, the former is preferred in terms of shortening the process and costs, and a photoradical generator is more preferred.

[0078] The photoradical generator can improve the resolution by strengthening the shape of the pattern or increasing the contrast of development. The photoradical generator used in the present invention is a photoradical generator that releases radicals when irradiated with radiation. Here, examples of radiation include visible light, ultraviolet light, infrared light, X-rays, electron beams, α rays, and γ rays.

[0079] The amount of the photoradical generator to be added varies depending on the type of active substance generated by the decomposition of the photoradical generator, the amount generated, the required sensitivity, and the dissolution contrast between the exposed and unexposed parts, but is preferably 0.001 to 50 mass%, more preferably 0.01 to 30 mass%, based on the total mass of the alkali-soluble resin. If the amount added is less than 0.001 mass%, the dissolution contrast between the exposed and unexposed parts may be too low, and the addition effect may not be obtained. On the other hand, if the amount added of the photoradical generator is more than 50 mass%, cracks may occur in the formed coating, or coloring due to the decomposition of the photoradical generator may become significant, so that the colorless transparency of the coating may decrease. In addition, if the amount added is large, the thermal decomposition of the photoradical generator may cause deterioration of the electrical insulation of the cured product or gas emission, which may cause problems in the subsequent process. In addition, the resistance of the coating to a photoresist stripping solution containing monoethanolamine or the like as a main component may decrease.

[0080] Examples of photoradical generators include azo-based, peroxide-based, acylphosphine oxide-based, alkylphenone-based, oxime ester-based, and titanocene-based initiators. Among them, alkylphenone-based, acylphosphine oxide-based, and oxime ester-based initiators are preferred, and 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one, and 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one are preferred. 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime), and the like.

[0081] (IV) Solvent The composition according to the present invention contains a solvent. The solvent is not particularly limited as long as it can uniformly dissolve or disperse the above-mentioned alkali-soluble resin, black colorant, polymerization initiator, and additives added as necessary. Examples of the solvent that can be used in the present invention include ethylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether, diethylene glycol dialkyl ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether, ethylene glycol alkyl ether acetates such as methyl cellosolve acetate and ethyl cellosolve acetate, and propene glycol monomethyl ether and propylene glycol monoethyl ether. Examples of the solvent include propylene glycol monoalkyl ethers, propylene glycol alkyl ether acetates such as PGMEA, propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate, aromatic hydrocarbons such as benzene, toluene, and xylene, ketones such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone, and cyclohexanone, alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, and glycerin, esters such as ethyl lactate, ethyl 3-ethoxypropionate, and methyl 3-methoxypropionate, and cyclic esters such as γ-butyrolactone. Among these, from the viewpoints of availability, ease of handling, and polymer solubility, it is preferable to use propylene glycol alkyl ether acetates or esters and alcohols having a straight or branched chain with an alkyl group having 4 or 5 carbon atoms. From the viewpoints of coatability and storage stability, it is preferable that the solvent ratio of alcohol is 5 to 80%.

[0082] The solvent content of the composition according to the present invention can be adjusted arbitrarily depending on the method of applying the composition. For example, when applying the composition by spray coating, the solvent content of the composition can be 90% by mass or more. In addition, in the case of slit coating used for applying to large substrates, the solvent content is usually 60% by mass or more, preferably 70% by mass or more. The properties of the composition of the present invention do not change significantly depending on the amount of the solvent.

[0083] The composition according to the present invention essentially comprises the above-mentioned (I) to (IV), but may be combined with additional compounds as necessary. The materials that may be combined are described below.

[0084] (V) Compounds containing two or more (meth)acryloyloxy groups The composition according to the present invention may further contain a compound containing two or more (meth)acryloyloxy groups (hereinafter, for the sake of simplicity, it may be referred to as a (meth)acryloyloxy group-containing compound). Here, the (meth)acryloyloxy group is a general term for an acryloyloxy group and a methacryloyloxy group. This compound is a compound that can react with the acryloyl group-containing polysiloxane and the alkali-soluble resin to form a crosslinked structure. Here, in order to form a crosslinked structure, a compound containing two or more reactive groups, acryloyloxy groups or methacryloyloxy groups, is necessary, and it is preferable to contain three or more acryloyloxy groups or methacryloyloxy groups in order to form a higher-order crosslinked structure.

[0085] As such a compound containing two or more (meth)acryloyloxy groups, esters obtained by reacting (α) a polyol compound having two or more hydroxyl groups with (β) two or more (meth)acrylic acids are preferably used. Examples of this polyol compound (α) include compounds having a basic skeleton of saturated or unsaturated aliphatic hydrocarbons, aromatic hydrocarbons, heterocyclic hydrocarbons, primary, secondary or tertiary amines, ethers, etc., and having two or more hydroxyl groups as substituents. This polyol compound may contain other substituents, such as a carboxyl group, a carbonyl group, an amino group, an ether bond, a thiol group, a thioether bond, etc., within the scope of not impairing the effects of the present invention.

[0086] Preferred polyol compounds include alkyl polyols, aryl polyols, polyalkanolamines, cyanuric acid, and dipentaerythritol. When the polyol compound (α) has three or more hydroxyl groups, it is not necessary that all the hydroxyl groups are reacted with meth(acrylic acid), and they may be partially esterified. In other words, the ester may have unreacted hydroxyl groups. Examples of such esters include tris(2-acryloxyethyl)isocyanurate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol octa(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, polytetramethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, ditrimethylolpropane tetraacrylate, tricyclodecane dimethanol diacrylate, 1,9-nonanediol diacrylate, 1,6-hexanediol diacrylate, and 1,10-decanediol diacrylate. Among these, tris(2-acryloxyethyl)isocyanurate and dipentaerythritol hexaacrylate are preferred from the viewpoints of reactivity and the number of crosslinkable groups. In addition, two or more of these compounds can be combined to adjust the shape of the pattern to be formed. Specifically, it is preferable to combine a compound containing three (meth)acryloyloxy groups with a compound containing two (meth)acryloyloxy groups.

[0087] From the viewpoint of reactivity, it is preferable that such a compound has a smaller molecule than the alkali-soluble resin, and therefore the molecular weight is preferably 2,000 or less, and more preferably 1,500 or less.

[0088] The content of the (meth)acryloyloxy group-containing compound is adjusted depending on the type of polymer or (meth)acryloyloxy group-containing compound used, but from the viewpoint of compatibility with the resin, it is preferably 5 to 1000 mass%, more preferably 10 to 800 mass%, based on the total mass of the alkali-soluble resin. When a low-concentration developer is used, it is preferably 30 to 800 mass. These (meth)acryloyloxy group-containing compounds may be used alone or in combination of two or more kinds.

[0089] (VI) Sugar The composition according to the present invention may further contain a sugar. The sugar may be any of monosaccharides, oligosaccharides, and polysaccharides, but is preferably an oligosaccharide. Here, in the present specification, the oligosaccharide refers to a sugar formed by dehydration condensation of 2 to 10 molecules of a monosaccharide, and also includes a cyclic oligosaccharide (for example, cyclodextrin). Among these sugars, cyclodextrin or a disaccharide formed by condensing two molecules of a monosaccharide is preferable, and more preferably, a disaccharide formed by condensing two molecules of a monosaccharide. In addition, the sugar is preferably added with an alkylene oxide having 1 to 6 carbon atoms, more preferably an alkylene oxide having 2 to 5 carbon atoms, and even more preferably ethylene oxide or propylene oxide. In other words, it is preferable that a hydroxyl group (-OH) contained in the sugar is replaced with -(CxH2x-O-)yH. Here, x is an integer of 2 to 6, preferably an integer of 2 to 5, more preferably 2 or 3, and y is an integer of 1 to 8, more preferably an integer of 2 to 5. According to the study by the present inventors, it has been found that such sugars have a dissolution-promoting effect in a developer. Since sugars have hydrophilic and hydrophobic properties, they dissolve in the solvent in the composition and also in the developer, and are considered to have a dissolution-promoting effect. Such an effect is particularly beneficial when the development of the composition according to the present invention is carried out with a low-concentration developer.

[0090] The content of the sugar used in the present invention is preferably from 1 to 80% by mass, and more preferably from 5 to 50% by mass, based on the total mass of the alkali-soluble resin.

[0091] The content of components other than (I) to (VI) in the entire composition is preferably 30% or less, more preferably 20% or less, and even more preferably 10% or less, based on the total mass of the composition.

[0092] (VII) Other Additives The composition according to the present invention may contain other additives, if necessary. Such additives include a developer dissolution promoter, a scum remover, an adhesion enhancer, a polymerization inhibitor, a defoamer, a surfactant, a sensitizer, a crosslinking agent, and a hardener.

[0093] The developer dissolution promoter or scum remover adjusts the solubility of the formed film in the developer and prevents scum from remaining on the substrate after development. Crown ethers can be used as such additives. The crown ether with the simplest structure has the general formula (-CH2-CH2-O-) nIn the present invention, among these, those in which n is 4 to 7 are preferred. Crown ethers are sometimes called x-crown-y-ethers, where the total number of atoms constituting the ring is x and the number of oxygen atoms contained therein is y. In the present invention, those selected from the group consisting of crown ethers in which x=12, 15, 18, or 21 and y=x / 3, as well as benzo-condensates and cyclohexyl-condensates thereof are preferred. More preferred specific examples of crown ether are 21-crown-7 ether, 18-crown-6-ether, 15-crown-5-ether, 12-crown-4-ether, dibenzo-21-crown-7-ether, dibenzo-18-crown-6-ether, dibenzo-15-crown-5-ether, dibenzo-12-crown-4-ether, dicyclohexyl-21-crown-7-ether, dicyclohexyl-18-crown-6-ether, dicyclohexyl-15-crown-5-ether, and dicyclohexyl-12-crown-4-ether. In the present invention, among these, those selected from 18-crown-6-ether and 15-crown-5-ether are most preferred. The content is preferably 0.05 to 15 mass%, more preferably 0.1 to 10 mass%, based on the total mass of the alkali-soluble resin.

[0094] The adhesion enhancer has the effect of preventing the pattern from peeling off due to stress applied after baking when a cured film is formed using the composition according to the present invention. As the adhesion enhancer, imidazoles and silane coupling agents are preferable, and among imidazoles, 2-hydroxybenzimidazole, 2-hydroxyethylbenzimidazole, benzimidazole, 2-hydroxyimidazole, imidazole, 2-mercaptoimidazole, and 2-aminoimidazole are preferable, and 2-hydroxybenzimidazole, benzimidazole, 2-hydroxyimidazole, and imidazole are particularly preferable.

[0095] The silane coupling agent is preferably a known one, and examples thereof include an epoxy silane coupling agent, an amino silane coupling agent, and a mercapto silane coupling agent. Specifically, 3-glycidoxypropyl trimethoxysilane, 3-glycidoxypropyl triethoxysilane, N-2-(aminoethyl)-3-aminopropyl trimethoxysilane, N-2-(aminoethyl)-3-aminopropyl triethoxysilane, 3-aminopropyl trimethoxysilane, 3-aminopropyl triethoxysilane, 3-ureidopropyl triethoxysilane, 3-chloropropyl triethoxysilane, 3-mercaptopropyl trimethoxysilane, and 3-isocyanate propyl triethoxysilane are preferred. These can be used alone or in combination, and the amount of addition is preferably 0.05 to 15 mass% based on the total mass of the alkali-soluble resin.

[0096] Also, as the silane coupling agent, a silane compound or a siloxane compound having an acid group can be used. Examples of the acid group include a carboxyl group, an acid anhydride group, and a phenolic hydroxyl group. When a monobasic acid group such as a carboxyl group or a phenolic hydroxyl group is included, it is preferable that a single silicon-containing compound has a plurality of acid groups.

[0097] Specific examples of such silane coupling agents include those represented by formula (C): X n Si(OR 3 ) 4-n (C) In this case, X or R 3 A combination of multiple repeating units having different repeating units can be used.

[0098] In the formula, R 3 Examples of the alkyl group include a hydrocarbon group, for example, an alkyl group such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, and an n-butyl group. 3 There are multiple R 3may be the same or different.

[0099] Examples of X include those having an acid group such as a phosphonium, borate, carboxyl, phenol, peroxide, nitro, cyano, sulfo, or alcohol group, as well as those in which the acid group is protected with an acetyl, aryl, amyl, benzyl, methoxymethyl, mesyl, tolyl, trimethoxysilyl, triethoxysilyl, triisopropylsilyl, or trityl group, and an acid anhydride group.

[0100] Of these, R 3 Preferred are those having a methyl group as X and a carboxylic acid anhydride group as X, for example, an acid anhydride group-containing silicone. More specifically, a compound represented by the following formula (X-12-967C (trade name, Shin-Etsu Chemical Co., Ltd.)) or a polymer containing a corresponding structure at the end or side chain of a silicon-containing polymer such as silicone is preferred. [ka] Also preferred are compounds in which an acid group such as thiol, phosphonium, borate, carboxyl, phenol, peroxide, nitro, cyano, or sulfo group is added to the terminal of dimethyl silicone. Examples of such compounds include the compounds represented by the following formula (X-22-2290AS and X-22-1821 (both trade names, Shin-Etsu Chemical Co., Ltd.)). [ka]

[0101] When the silane coupling agent contains a silicone structure, if the molecular weight is too large, the compatibility with the polysiloxane contained in the composition becomes poor, the solubility in the developer is not improved, reactive groups remain in the film, and chemical resistance to the post-processing process cannot be maintained, etc., and there is a possibility of adverse effects. Therefore, the mass average molecular weight of the silane coupling agent is preferably 5000 or less, more preferably 4000 or less. The content of the silane coupling agent is preferably 0.01 to 15 mass% based on the total mass of the alkali-soluble resin.

[0102] As the polymerization inhibitor, nitrone, nitroxide radical, hydroquinone, catechol, phenothiazine, phenoxazine, hindered amine and their derivatives, as well as ultraviolet absorbers can be added. Among them, methylhydroquinone, catechol, 4-t-butylcatechol, 3-methoxycatechol, phenothiazine, chlorpromazine, phenoxazine, and hindered amines such as TINUVIN 144, 292, and 5100 (BASF), and ultraviolet absorbers such as TINUVIN 326, 328, 384-2, 400, and 477 (BASF) are preferred. These can be used alone or in combination, and the content is preferably 0.01 to 20% by mass based on the total mass of the alkali-soluble resin.

[0103] As an antifoaming agent, alcohol (C1~ 18 ), higher fatty acids such as oleic acid and stearic acid, higher fatty acid esters such as glycerin monolaurate, polyethers such as polyethylene glycol (PEG) (Mn200 to 10,000) and polypropylene glycol (PPG) (Mn200 to 10,000), silicone compounds such as dimethyl silicone oil, alkyl-modified silicone oil, and fluorosilicone oil, and organosiloxane surfactants, the details of which are given below. These can be used alone or in combination, and the content is preferably 0.1 to 3 mass% based on the total mass of the alkali-soluble resin.

[0104] The composition according to the present invention may contain a surfactant as necessary. The surfactant is added for the purpose of improving coating properties, developability, etc. Examples of surfactants that can be used in the present invention include nonionic surfactants, anionic surfactants, and amphoteric surfactants.

[0105] Examples of nonionic surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene oleyl ether, and polyoxyethylene cetyl ether; acetylene glycol derivatives such as polyoxyethylene fatty acid diesters, polyoxyethylene fatty acid monoesters, polyoxyethylene polyoxypropylene block polymers, acetylene alcohol, acetylene glycol, polyethoxylates of acetylene alcohol, and polyethoxylates of acetylene glycol; fluorine-containing surfactants such as Fluorad (trade name, Sumitomo 3M Limited), Megafac (trade name, DIC Corporation), and Sulfuron (trade name, Asahi Glass Co., Ltd.); and organic siloxane surfactants such as KP341 (trade name, Shin-Etsu Chemical Co., Ltd.). Examples of the acetylene glycol include 3-methyl-1-butyn-3-ol, 3-methyl-1-pentyn-3-ol, 3,6-dimethyl-4-octyne-3,6-diol, 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,5-dimethyl-1-hexyne-3-ol, 2,5-dimethyl-3-hexyne-2,5-diol, and 2,5-dimethyl-2,5-hexanediol.

[0106] Examples of the anionic surfactant include ammonium salts or organic amine salts of alkyldiphenyl ether disulfonic acids, ammonium salts or organic amine salts of alkyldiphenyl ether sulfonic acids, ammonium salts or organic amine salts of alkylbenzene sulfonic acids, ammonium salts or organic amine salts of polyoxyethylene alkyl ether sulfates, and ammonium salts or organic amine salts of alkyl sulfates.

[0107] Further, examples of amphoteric surfactants include 2-alkyl-N-carboxymethyl-N-hydroxyethylimidazolium betaine, lauric acid amidopropyl hydroxysulfone betaine, and the like.

[0108] These surfactants can be used alone or in combination of two or more kinds, and the content thereof is preferably from 0.005 to 1 mass %, more preferably from 0.01 to 0.5 mass %, based on the total mass of the composition.

[0109] If necessary, a sensitizer can be added to the composition of the present invention. Sensitizers preferably used in the composition according to the present invention include coumarin, ketocoumarin and derivatives thereof, thiopyrylium salts, acetophenones, and the like, specifically, p-bis(o-methylstyryl)benzene, 7-dimethylamino-4-methylquinolone-2, 7-amino-4-methylcoumarin, 4,6-dimethyl-7-ethylaminocoumarin, 2-(p-dimethylaminostyryl)-pyridylmethyl iodide, 7-diethylaminocoumarin, 7-diethylamino-4-methylcoumarin, 2,3,5,6-1H,4H-tetrahydro-8-methylquinolizino-<9,9a,1-gh>coumarin, 7-diethylamino-4-trifluoromethylcoumarin, 7-dimethylamino-4-trifluoromethylcoumarin, 7-amino-4-trifluoro ... Examples of sensitizing dyes include tetrahydroquinolizino-<9,9a,1-gh>coumarin, 7-ethylamino-6-methyl-4-trifluoromethylcoumarin, 7-ethylamino-4-trifluoromethylcoumarin, 2,3,5,6-1H,4H-tetrahydro-9-carboethoxyquinolizino-<9,9a,1-gh>coumarin, 3-(2'-N-methylbenzimidazolyl)-7-N,N-diethylaminocoumarin, N-methyl-4-trifluoromethylpiperidino-<3,2-g>coumarin, 2-(p-dimethylaminostyryl)-benzothiazolylethyl iodide, 3-(2'-benzimidazolyl)-7-N,N-diethylaminocoumarin, 3-(2'-benzothiazolyl)-7-N,N-diethylaminocoumarin, and pyrylium salts and thiopyrylium salts represented by the following chemical formulas. The addition of a sensitizing dye enables patterning using an inexpensive light source such as a high-pressure mercury lamp (360 to 430 nm). The content of the sensitizing dye is preferably 0.05 to 15% by mass, more preferably 0.1 to 10% by mass, based on the total mass of the alkali-soluble resin. [ka]

[0110] In addition, a compound containing an anthracene skeleton can also be used as the sensitizer. Specific examples include compounds represented by the following formula: [ka] In the formula, R 31 each independently represents a substituent selected from the group consisting of an alkyl group, an aralkyl group, an allyl group, a hydroxyalkyl group, an alkoxyalkyl group, a glycidyl group, and a halogenated alkyl group, R 32 each independently represents a substituent selected from the group consisting of a hydrogen atom, an alkyl group, an alkoxy group, a halogen atom, a nitro group, a sulfonic acid group, a hydroxyl group, an amino group, and a carboalkoxy group; Each k is independently an integer selected from 0 and 1 to 4.

[0111] When such a sensitizer having an anthracene skeleton is used, the content thereof is preferably 0.01 to 5% by mass based on the total mass of the alkali-soluble resin.

[0112] <Method of forming a cured film> The method for forming a cured film according to the present invention comprises applying the above-mentioned composition to a substrate to form a coating film, exposing the coating film to light, and developing the coating film. The method for forming a cured film will be described in the order of steps as follows.

[0113] (1) Coating process First, the composition is applied to a substrate. The coating film of the composition in the present invention can be formed by any method conventionally known as a coating method for photosensitive compositions. Specifically, the method can be selected from dip coating, roll coating, bar coating, brush coating, spray coating, doctor coating, flow coating, spin coating, slit coating, and the like. As the substrate to which the composition is applied, a suitable substrate such as a silicon substrate, a glass substrate, or a resin film can be used. Various semiconductor elements may be formed on these substrates as necessary. When the substrate is a film, gravure coating can also be used. If desired, a drying step can be separately provided after the coating. If necessary, the coating step can be repeated once or twice or more to form the coating film having a desired thickness.

[0114] (2) Pre-bake process After forming a coating film by applying the composition, the coating film is preferably prebaked (preheated) in order to dry the coating film and reduce the amount of solvent remaining in the coating film. The prebaking step can be carried out at a temperature of generally 50 to 150° C., preferably 90 to 120° C., for 10 to 300 seconds, preferably 30 to 120 seconds, when using a hot plate, or for 1 to 30 minutes when using a clean oven.

[0115] (3) Exposure process After the coating film is formed, the surface of the coating film is irradiated with light. The light source used for the light irradiation can be any light source that has been conventionally used in pattern formation methods. Examples of such light sources include high-pressure mercury lamps, low-pressure mercury lamps, metal halide lamps, xenon lamps, laser diodes, LEDs, etc. Ultraviolet rays such as g-rays, h-rays, and i-rays are usually used as the irradiated light. Except for ultrafine processing such as semiconductors, light of 360 to 430 nm (high-pressure mercury lamps) is generally used for patterning of several μm to several tens of μm. The energy of the irradiated light varies depending on the light source and the thickness of the coating film, but is generally 5 to 2000 mJ / cm. 2 , preferably 10 to 1000 mJ / cm 2The irradiation light energy is 5 mJ / cm 2 If it is lower than 2000mJ / cm, sufficient resolution may not be obtained. 2 If it is higher than this, overexposure will occur, which may lead to the occurrence of halation.

[0116] A general photomask can be used to irradiate light in a pattern. Such a photomask can be arbitrarily selected from known ones. The environment during irradiation is not particularly limited, but generally, the ambient atmosphere (air) or nitrogen atmosphere may be used. In addition, when a film is formed on the entire surface of the substrate, the entire surface of the substrate may be irradiated with light. In the present invention, the patterned film also includes the case where a film is formed on the entire surface of the substrate.

[0117] (4) Post-exposure baking process After the exposure, post-exposure baking can be performed as necessary to promote the interpolymer reaction in the film by the polymerization initiator. This heating process is different from the heating process (6) described later, and is not performed to completely harden the coating film, but is performed so that only the desired pattern remains on the substrate after development and the other parts can be removed by development. Therefore, it is not essential to the present invention.

[0118] When the post-exposure heating is performed, a hot plate, an oven, a furnace, or the like can be used. The heating temperature should not be excessively high because it is not preferable that the acid, base, or radical generated in the exposed region by light irradiation diffuses to the unexposed region. From this viewpoint, the range of the heating temperature after exposure is preferably 40°C to 150°C, more preferably 60°C to 120°C. In order to control the curing speed of the composition, stepwise heating can be applied as necessary. In addition, the atmosphere during heating is not particularly limited, but can be selected from an inert gas such as nitrogen, under vacuum, under reduced pressure, in oxygen gas, and the like, for the purpose of controlling the curing speed of the composition. In addition, the heating time is preferably a certain amount or more in order to maintain a higher uniformity of the temperature history in the wafer surface, and is preferably not excessively long in order to suppress the diffusion of the generated acid, base, or radical. From this viewpoint, the heating time is preferably 20 seconds to 500 seconds, more preferably 40 seconds to 300 seconds.

[0119] (5)Developing process After exposure, if necessary, post-exposure heating is performed, and then the coating film is developed. Any developer used in the development of photosensitive compositions can be used as the developer used in the development. Preferred developers include alkaline developers that are aqueous solutions of alkaline compounds such as tetraalkylammonium hydroxide, choline, alkali metal hydroxide, alkali metal metasilicate (hydrate), alkali metal phosphate (hydrate), aqueous sodium carbonate solution, ammonia, alkylamine, alkanolamine, and heterocyclic amine, and particularly preferred alkaline developers are aqueous solutions of tetramethylammonium hydroxide, potassium hydroxide, sodium hydroxide, and sodium carbonate. These alkaline developers may further contain water-soluble organic solvents such as methanol and ethanol, or surfactants, as necessary. In the present invention, development can be performed using a developer with a lower concentration than the 2.38% by mass TMAH developer that is normally used as a developer. Examples of such a developer include a 0.05 to 1.5 mass % TMAH aqueous solution, a 0.1 to 2.5 mass % sodium carbonate aqueous solution, a 0.01 to 1.5 mass % potassium hydroxide aqueous solution, etc. The development time is usually 10 to 300 seconds, and preferably 30 to 180 seconds. The developing method can be selected from conventionally known methods. Specific examples include immersion (dip) in a developer, paddle, shower, slit, cap coat, spray, etc. This development can provide a pattern. After development with a developer, it is preferable to wash with water.

[0120] (6)Heating process After development, the pattern film obtained is cured by heating. The heating device used in the heating step can be the same as that used in the post-exposure heating described above. The heating temperature in this heating step is not particularly limited as long as it is a temperature at which the coating film can be cured, and can be determined arbitrarily. However, if the silanol group of the polysiloxane remains, the chemical resistance of the cured film may become insufficient, or the dielectric constant of the cured film may become high. From this viewpoint, the heating temperature is generally selected to be relatively high. However, the composition according to the present invention can be cured at a relatively low temperature. Specifically, it is preferable to cure by heating at 350°C or less, and in order to keep the residual film rate after curing high, the curing temperature is more preferably 300°C or less, and particularly preferably 250°C or less. On the other hand, in order to promote the curing reaction and obtain a sufficient cured film, the curing temperature is preferably 70°C or more, and more preferably 100°C or more. In addition, the heating time is not particularly limited, and is generally 10 minutes to 24 hours, preferably 30 minutes to 3 hours. In addition, this heating time is the time after the temperature of the pattern film reaches the desired heating temperature. Usually, it takes several minutes to several hours for the pattern film to reach a desired temperature from the temperature before heating.

[0121] The cured film thus formed exhibits the effects of the present application as long as it has an average thickness of 100 μm or less, and is preferably a film having an average thickness of 5 to 100 μm. More preferably, it is 5 to 25 μm, and further preferably, it is 8 to 20 μm. The optical density (OD) of the cured film is preferably 2 or more on average at a wavelength of 400 to 700 nm. Here, the optical density is measured by a Spectrophotometer CM-5 (Konica Minolta). The cured film according to the present invention has excellent light-shielding properties and can be used as a partition material for display devices. Since the cured film according to the present invention can be made thick, it can be suitably used for quantum dots and organic electroluminescence devices, which require a thicker partition material.

[0122] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples and comparative examples.

[0123] Gel permeation chromatography (GPC) was performed using an HLC-8220GPC type high-speed GPC system (product name, Tosoh Corporation) and two Super Multipore HZ-N type GPC columns (product name, Tosoh Corporation). The measurements were performed under analytical conditions of monodisperse polystyrene as the standard sample, tetrahydrofuran as the developing solvent, a flow rate of 0.6 milliliters / minute, and a column temperature of 40°C.

[0124] <Synthesis Example 1: Synthesis of Polysiloxane A> A 2L flask equipped with a stirrer, thermometer, and cooling tube was charged with 36.7g of 25% by mass TMAH aqueous solution, 600ml of IPA, and 3.0g of water, and then a mixed solution of 17g of methyltrimethoxysilane, 29.7g of phenyltrimethoxysilane, 7.6g of tetramethoxysilane, and 43.4g of 3-(methacryloyloxy)propyltrimethoxysilane was prepared in a dropping funnel. The mixed solution was dropped at 40°C, stirred at the same temperature for 2 hours, and then neutralized by adding a 10% HCl aqueous solution. 400ml of toluene and 600ml of water were added to the neutralized solution, which was separated into two layers, and the water layer was removed. The solution was further washed three times with 300ml of water, and the organic layer obtained was concentrated under reduced pressure to remove the solvent, and PGMEA was added to the concentrate so that the solid concentration was 30% by mass, to obtain a polysiloxane solution. The polysiloxane obtained at this stage had an Mw of 3722. A 100 mL flask equipped with a stirrer, thermometer, and condenser was charged with 14.7 g of the polysiloxane solution, 0.35 g of methacrylic acid, and 0.63 g of azabisisobutyronitrile, and stirred at 80° C. for 4 hours to obtain a solution of polysiloxane A. The resulting polysiloxane A had an Mw of 5,966.

[0125] <Synthesis Example 2: Synthesis of Polysiloxane A'> In a 2L flask equipped with a stirrer, a thermometer, and a cooling tube, 125.0 g of 50% 2-hydroxyethyltrimethylammonium hydroxide aqueous solution and 40 g of 1-methoxy-2-propanol were charged, and then a mixed solution of 108.8 g of methyltrimethoxysilane, 118.8 g of phenyltrimethoxysilane, 41.6 g of tetramethoxysilane, and 99.2 g of 3-(methacryloyloxy)propyltrimethoxysilane was prepared in a dropping funnel. The mixed solution was dropped into a solution cooled to 5°C on ice, stirred at the same temperature for 2 hours, and then neutralized by adding a 10% HCl aqueous solution. 400 ml of toluene and 600 ml of water were added to the neutralized solution, which was separated into two layers, and the water layer was removed. The solution was further washed three times with 300 ml of water, and the organic layer obtained was concentrated under reduced pressure to remove the solvent, and PGMEA was added to the concentrate so that the solid concentration was 30 mass%, to obtain a polysiloxane solution A'. The polysiloxane A' obtained at this stage had Mw of 2,000.

[0126] <Synthesis Example 3: Synthesis of Polysiloxane B> A 2L flask equipped with a stirrer, thermometer, and cooling tube was charged with 36.7g of 25% by mass TMAH aqueous solution, 600ml of IPA, and 3.0g of water, and then a mixed solution of 17g of methyltrimethoxysilane, 29.7g of phenyltrimethoxysilane, 7.6g of tetramethoxysilane, and 43.4g of 3-(methacryloyloxy)propyltrimethoxysilane was prepared in a dropping funnel. The mixed solution was dropped at 40°C, stirred at the same temperature for 2 hours, and then neutralized by adding a 10% HCl aqueous solution. 400ml of toluene and 600ml of water were added to the neutralized solution, which was separated into two layers, and the water layer was removed. The solution was further washed three times with 300ml of water, and the organic layer obtained was concentrated under reduced pressure to remove the solvent, and PGMEA was added to the concentrate so that the solid concentration was 30% by mass, to obtain a polysiloxane solution. The polysiloxane obtained at this stage had an Mw of 3722. A 100 mL flask equipped with a stirrer, thermometer, and condenser was charged with 7.35 g of the polysiloxane solution, 0.85 g of ethoxylated isocyanuric acid triacrylate, and 0.63 g of azabisisobutyronitrile, and stirred at 80° C. for 4 hours to obtain a polysiloxane B solution. The resulting Polysiloxane B had Mw of 6,100.

[0127] <Synthesis Example 4: Synthesis of Acrylic Polymer A> 500g of PGMEA was added to a 2L separable flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube, and the temperature was raised to 95°C. Then, 160g of methacrylic acid, 100g of methyl methacrylate, and 16.6g of t-butylperoxy-2-ethylhexanoate (Perbutyl O; NOF Corporation) were added dropwise over 3 hours. After the dropwise addition, the mixture was stirred at room temperature for 4 hours to synthesize a polymer solution. To this polymer solution, 160g of 3,4-epoxycyclohexylmethylacrylate, 1.5g of triphenylphosphine, and 1.0g of methylhydroquinone were added and reacted at 110°C for 6 hours under a nitrogen atmosphere. After the reaction, the mixture was diluted with PGMEA so that the solid content was 35% by mass, and an acrylic polymer A with Mw of 11,000 was obtained.

[0128] <Synthesis Example 5: Synthesis of Acrylic Polymer B> In a 2 L flask equipped with a stirrer, thermometer, and condenser, 500 g of bisphenol F type epoxy resin (Nippon Steel Chemical & Material Corporation, "YDF2001 (trade name)"), 80 g of acrylic acid, 0.5 g of methylhydroquinone, and 150 g of carbitol acetate were mixed and heated to 90°C and stirred. Next, after cooling to 60°C, 2 g of trioctylmethylammonium chloride was mixed and heated to 110°C to cause a reaction. Next, 230 g of tetrahydrophthalic anhydride and 85 g of carbitol acetate were mixed, heated to 80°C, and stirred for 6 hours to obtain a reaction mixture. The resulting acrylic polymer B had Mw=12,300.

[0129] <Synthesis Example 6: Synthesis of Acrylic Polymer C> A 1L flask equipped with a stirrer, thermometer, condenser and nitrogen gas inlet tube was charged with 16.4g of azobisisobutyronitrile and 120g of butanol, and heated to an appropriate temperature under a nitrogen gas atmosphere, referring to the 10-hour half-life temperature of the initiator. Separately, a mixture of 13.0g of methacrylic acid, 46.5g of KBM-502, 6.5g of 2-hydroxyethyl methacrylate and 60.0g of methyl methacrylate was prepared, and the mixture was dropped into the solvent over 4 hours. After that, the mixture was reacted for 3 hours to obtain acrylic polymer C with Mw 7,000.

[0130] <Example 1> To a solution containing 100 parts by mass of polysiloxane A obtained in Synthesis Example 1, 6.0 parts by mass of BASF's "Irgacure OXE-02" as a polymerization initiator, 300 parts by mass each of dipentaerythritol hexaacrylate (Shin-Nakamura Chemical Co., Ltd. "A-DPH") and polyethylene glycol #600 diacrylate (Shin-Nakamura Chemical Co., Ltd. "A-600") as (meth)acryloyloxy group-containing compounds, 0.01 mass% of "AKS-10" (Shin-Etsu Chemical Co., Ltd.) as a surfactant based on the total mass of the composition, and PGMEA were added to prepare a 35% solution. Furthermore, organic pigment A (pigment orange, pigment blue) was added as a black colorant to prepare a dispersion in which the pigment orange and pigment blue were each 7% by mass, totaling 14% by mass, and a dispersant (BYK-Chemie "DisperBYK-2000") was added to a total of 20% by mass based on the total mass of the composition, to obtain the composition of Example 1. 365 / 500 But it is 1.3.

[0131] <Examples 2 to 20 and Comparative Examples 1 to 3> Compositions were prepared by modifying the composition of Example 1 as shown in Tables 1 to 3. In the tables, the values ​​other than those for the black colorant indicate parts by mass. [Table 1] [Table 2] [Table 3] In the table, Acrylic polymer A: "RN-081F" (Natoco Co., Ltd.) Organic pigment A: A mixture of pigment orange and pigment blue (Tokyo Chemical Industry Co., Ltd.). When adding organic pigment A, it was dispersed in the dispersant "DisperBYK-2000" (Big Chemie) before being added. 365 / 500 =1.3 Inorganic pigment B: Mitsubishi Materials Corporation "NITBLACK UB-1", R 365 / 500 =4.0. MnFe: JFE Chemical Corporation, R 365 / 500 =0.4. TiN: Mitsubishi Materials Corporation, R 365 / 500 =0.7. Carbon black: BASF, R 365 / 500 =0.3. Polymerization initiator A: "Irgacure OXE-02" (BASF). Compound A: dipentaerythritol hexaacrylate ("A-DPH" from Shin-Nakamura Chemical Co., Ltd.). Compound B: polyethylene glycol #600 diacrylate ("A-600" from Shin-Nakamura Chemical Co., Ltd.). Compound C: 2-hydroxy-3-acryloyloxypropyl methacrylate (Shin-Nakamura Chemical Co., Ltd. "701A"). Sugar A: Ethylene oxide adduct of sucrose Surfactant A: "AKS-10" (Shin-Etsu Chemical Co., Ltd.).

[0132] Each of the compositions obtained was applied onto a silicon wafer by spin coating, and after application, the wafer was prebaked on a hot plate at 100°C for 90 seconds to prepare an average film thickness of 2 μm or 10 μm. The wafer was exposed using an i-line exposure machine, developed using a 2.38% TMAH aqueous solution or 0.025% KOH, and rinsed with pure water for 30 seconds. As a result, it was confirmed whether a 10 μm contact hole (C / H) pattern was formed or not. The results obtained are as shown in Tables 1 and 2. It was confirmed that a pattern was formed (OK) in all examples. In Example 20, a pattern was formed, but slight peeling was observed at an average film thickness of 10 μm. In Comparative Example 1, when the average film thickness was 10 μm, no pattern was formed (NG), and peeling occurred, so the resolution was not measured. In Comparative Examples 2 and 3, when the average film thickness was 2 μm and 10 μm, no pattern was formed (NG).

[0133] When the average film thickness was 10 μm, the resolution was determined as the minimum mask size at which a contact hole was formed using an optical microscope (MX61A-F, OLYMPUS Corporation). The results are shown in Tables 1 and 2.

[0134] When the average film thickness was 10 μm and a pattern size of 10 μm was formed, the mask size and pattern width were observed by cross section using SEM and compared, and evaluated as follows. The results are shown in Tables 1 and 2. A: The difference between the pattern width and the mask size is within 5%. B: The difference between the pattern width and the mask size is more than 5% and less than 10%. C: The difference between the pattern width and the mask size is more than 10% D: The pattern is peeled off or floating off the board.

[0135] Each composition was applied onto a glass plate to form a coating film having an average thickness of 10 μm. The coating film was baked in air at 230° C. for 30 minutes, and then the transmittance at wavelengths of 400 to 700 nm was measured using a Spectrophotometer CM-5 (Konica Minolta) and converted into OD.

Claims

1. (I) an alkali-soluble resin, (II) a black colorant, (III) a polymerization initiator, (IV) a solvent, and (VI) sugar comprising the (II) black colorant is composed only of substances having a transmittance ratio expressed as [transmittance at a wavelength of 365 nm] / [transmittance at a wavelength of 500 nm] of 1.2 or more; The black colorant (II) contains one or more pigments, and The negative photosensitive composition, wherein the alkali-soluble resin is a polysiloxane having a silsesquioxane skeleton.

2. The composition according to claim 1 , wherein the alkali-soluble resin has an acryloyl group.

3. The polysiloxane contains a repeating unit represented by formula (Ia'): 【Chemistry 1】 (In the formula, R a1’ is hydrogen or methyl, Each m' is independently an integer of 1 to 6. The composition of claim 1 or 2, comprising:

4. The polysiloxane is Repeating units represented by formula (Ia): 【Chemistry 2】 (In the formula, R a1 is hydrogen or methyl, ma are each independently an integer of 1 to 6, and An acrylic polymerized unit represented by formula (a): 【Chemistry 3】 (In the formula, R a2 are each independently hydrogen or methyl; R a3 is hydrogen, 1 to 6 valences, C 1~50 In the hydrocarbon group, one or more methylenes may be replaced by oxy, imino, and / or carbonyl; R a3 When is multivalent, R a3 connects a carbonyloxy in formula (a) to a carbonyloxy contained in another repeating unit represented by formula (a), n a is an integer equal to or greater than 0. comprising The composition according to any one of claims 1 to 3, wherein at least one * in the repeating unit of formula (Ia) is bonded to * in another repeating unit represented by formula (Ia) directly or via an acrylic polymerized unit represented by formula (a).

5. The composition according to any one of claims 1 to 4, wherein the content of the black colorant is 3 to 80 mass% based on the total mass of the alkali-soluble resin.

6. The composition according to any one of claims 1 to 5, further comprising (V) a compound containing two or more (meth)acryloyloxy groups.

7. The composition according to any one of claims 1 to 6, wherein the content of the compound (V) containing two or more (meth)acryloyloxy groups is 5 to 1000 mass% based on the total mass of the alkali-soluble resin (I).

8. The polysiloxane comprises a repeating unit represented by formula (Ic): 【Chemistry 4】 The composition according to any one of claims 1 to 7, comprising:

9. The composition according to any one of claims 1 to 8, wherein the sugar (VI) has an alkylene oxide having 1 to 6 carbon atoms added thereto.

10. The composition according to any one of claims 1 to 9, wherein the (VI) sugar is an oligosaccharide.

11. A method for producing a cured film, comprising: applying the composition according to any one of claims 1 to 10 to a substrate to form a coating film, exposing the coating film to light, and developing the coating film.

12. The method for producing a cured film according to claim 11, wherein the cured film has an average thickness of 5 to 100 μm.

13. The method for producing a cured film according to claim 11 or 12, wherein the cured film has an average optical density (OD) of 2 or more in a wavelength range of 400 to 700 nm.

14. A method for manufacturing a display device, comprising the method according to any one of claims 11 to 13.

Citation Information

Patent Citations

  • Photosensitive resin composition, cured product and production method of the same, production method of resin pattern, cured film, liquid crystal display device, organic el display device, and touch panel display device

    JP2016071245A

  • Colored photosensitive resin composition

    JP2017090720A

  • Zirconium nitride powder and manufacturing method therefor

    JP2018203599A

  • Negative photosensitive resin composition, cured film, element and display apparatus including cured film, production method for the same

    JP2019045865A

  • Photosensitive composition, colored pattern and method for producing same

    WO2018061988A1