Method for producing polymer used as base film for cell culture and cell culture vessel

A novel polymer production method controls molecular weight and functional group ratios in poly(2-N,N-dimethylaminoethyl methacrylate) by mixing monomers and a radical initiator, addressing production challenges and enabling effective cell culture base membranes and containers.

JP7556290B2Active Publication Date: 2024-09-26NISSAN CHEM CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020538462
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-24
Filing Date
2019-08-22
Publication Date
2024-09-26
Estimated Expiration
2039-08-22

AI Technical Summary

Technical Problem

Conventional methods for producing poly(2-N,N-dimethylaminoethyl methacrylate) face challenges in controlling the ratio of cationic to anionic functional groups and molecular weight, requiring multiple steps and being difficult to control hydrolysis ratios.

Method used

A method involving the preparation of a mixture containing specific monomers, a radical polymerization initiator, and an organic solvent, followed by heating and stirring to polymerize the mixture, which allows for controlling the molecular weight and ratio of cationic to anionic functional groups without relying on ultraviolet irradiation.

Benefits of technology

This method enables the easy production of poly(2-N,N-dimethylaminoethyl methacrylate) with controlled molecular weight and functional group ratios, facilitating the formation of a cell culture base membrane and container.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556290000026
    Figure 0007556290000026
  • Figure 0007556290000025
    Figure 0007556290000025
  • Figure 0007556290000027
    Figure 0007556290000027
Patent Text Reader

Abstract

The present invention provides a method for producing a polymer used as a base film for cell culture, a base film forming agent for cell culture, and a method for producing a base film and a cell culture vessel. The following formula (I): [In the formula, U a1 and U a2 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a1 represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a2 represents a linear or branched alkylene group having 1 to 5 carbon atoms], a radical polymerization initiator, and an organic solvent; and a polymerization step of heating and stirring the mixture to polymerize the monomer and prepare a polymer. A method for producing a polymer for use as a substratum for cell culture, comprising:
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polymer for use as a base membrane for cell culture and to the manufacture of a cell culture vessel comprising said base membrane. [Background technology]

[0002] Poly(2-N,N-dimethylaminoethyl methacrylate) (PDMAEMA), a polymer of 2-N,N-dimethylaminoethyl methacrylate (DMAEMA), is known as a temperature-responsive polymer having a cloud point of about 32°C.

[0003] In a conventional method for producing PDMAEMA, a mixture containing DMAEMA is prepared (preparation step), and then this mixture is irradiated with ultraviolet light (irradiation step) to radically polymerize DMAEMA, thereby producing PDMAEMA.

[0004] There was also a demand for producing PDMAEMA-derived polymers with altered physical properties by converting some of the ester groups, including the cationic 2-N,N-dimethylaminoethyl groups, attached to the side chains of PDMAEMA into anionic carboxyl groups through hydrolysis.

[0005] However, when using the above-mentioned conventional method for producing PDMAEMA to produce a polymer derived from PDMAEMA having a cationic 2-N,N-dimethylaminoethyl group and an anionic carboxyl group, it is necessary to radically polymerize DMAEMA having a cationic 2-N,N-dimethylaminoethyl group in a side chain via an ester group by irradiation with ultraviolet light, and then generate anionic carboxyl groups by hydrolyzing a portion of the ester group, which results in many steps required for production, and also in difficulty in controlling the hydrolysis ratio and molecular weight.

[0006] In order to solve such problems, Patent Document 1 reports the production of a polymer derived from poly(2-N,N-dimethylaminoethyl methacrylate) having cationic functional groups and anionic functional groups by irradiating DMAEMA with ultraviolet light in the presence of water to cause radical polymerization (see, for example, Patent Document 1).

[0007] However, even when the above-mentioned method for producing PDMAEMA is used, there are problems in that it is difficult to control the ratio of cationic functional groups and anionic functional groups, and it is also difficult to control the molecular weight. Furthermore, there is a problem in that only methacrylic acid obtained by hydrolyzing DMAEMA can be used as the anionic functional group.

[0008] In Patent Document 2, it is reported that PDMAEMA is prepared by irradiating DMAEMA with ultraviolet light in the absence of water, and then an anionic monomer is introduced and irradiated with ultraviolet light to produce a polymer having a DMAEMA block sequence and a random sequence of DMAEMA and an anionic monomer. The above production method can impart selectivity to anionic functional groups (see, for example, Patent Document 2).

[0009] However, even when the above-mentioned production methods are used, it is difficult to control the ratio of cationic functional groups to anionic functional groups, and it is also difficult to control the molecular weight and molecular weight distribution. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2014-162865 A [Patent Document 2] JP 2017-14323 A [Non-patent literature]

[0011] [Non-Patent Document 1] Wetering P et al, J Controlled Release 49, p59-69, 1997. [Non-Patent Document 2] Wetering P at al, Macromolecules 31, p8063-8068, 1998. Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention aims to simply produce a polymer derived from poly(2-N,N-dimethylaminoethyl methacrylate) from a monomer having a cationic functional group and preferably a monomer further having an anionic functional group, without relying on irradiation with light such as ultraviolet light, while controlling the molecular weight and molecular weight distribution, preferably by controlling the ratio of the cationic functional group to the anionic functional group, and further to provide a base film for cell culture, a base film forming agent for cell culture, and a cell culture vessel, which contain the above polymer. [Means for solving the problem]

[0013] That is, the present invention is as follows: [1] The following formula (I): [ka] [In the formula, U a1 and U a2 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a1 represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a2 represents a linear or branched alkylene group having 1 to 5 carbon atoms], a radical polymerization initiator, and an organic solvent; and a polymerization step of heating and stirring the mixture to polymerize the monomer to prepare a polymer. A method for producing a polymer for use as a sublayer for cell culture, comprising:

[0014] [2] Further, the formula (II): [ka] [In the formula, R b represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms] in the mixture.

[0015] [3] The method for producing a polymer according to [1] or [2], further comprising containing in the mixture a monomer having two or more carbon-carbon unsaturated bonds.

[0016] [4] The monomer having two or more carbon-carbon unsaturated bonds is represented by the following formula (III): [ka] [In the formula, R c and R d each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R e represents a linear or branched alkylene group having 1 to 5 carbon atoms, and n represents a number from 1 to 50.

[0017] [5] The method for producing a polymer according to any one of [1] to [4], wherein a molar ratio of units derived from a monomer represented by formula (I) / units derived from a monomer represented by formula (II) in the polymer is 100 / 0 to 50 / 50.

[0018] [6] The method for producing a polymer according to any one of the items [1] to [5], wherein the weight average molecular weight (Mn) of the polymer is 20,000 to 1,000,000, and the ratio (Mw / Mn) of the weight average molecular weight (Mw) of the polymer to the number average molecular weight (Mn) is 1.01 to 10.00.

[0019] [7] The method for producing the polymer according to any one of [1] to [6], wherein the polymer is used as a base membrane for cell culture by adhering cells and then peeling them off to obtain a cell aggregate.

[0020] [8] [1] to [7] A method for producing a base film-forming agent for cell culture, comprising a step of mixing a polymer obtained by the production method according to any one of the above items with an aqueous solution.

[0021] [9] [8] A method for producing a base film for cell culture, comprising a step of applying the base film forming agent for cell culture obtained by the production method described above to the surface of a container or substrate and drying it.

[0022]

[10] Prior to the coating and drying step, a copolymer including a repeating unit including an organic group represented by the following formula (a) and a repeating unit including an organic group represented by the following formula (b) is prepared: [ka] [In the formula, U a11 , U a12 , U b11 , U b12 and U b13 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; An - represents an anion selected from the group consisting of a halide ion, an inorganic acid ion, a hydroxide ion, and an isothiocyanate ion. and a solvent, and applying the composition for forming a coating film to a surface of a container or a substrate, and drying the composition.

[0023]

[11] The method for producing a base film for cell culture described in [9], wherein the container or substrate has the ability to inhibit cell adhesion.

[0024]

[12] A method for manufacturing a cell culture vessel, comprising a step of applying a base film forming agent for cell culture obtained by the manufacturing method described in [8] to a surface of a vessel or a substrate, and drying the agent.

[0025]

[13] Prior to the coating and drying step, a copolymer including a repeating unit including an organic group represented by the following formula (a) and a repeating unit including an organic group represented by the following formula (b) is prepared: [ka] [In the formula, U a11 , U a12 , U b11 , U b12 and U b13 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; An - represents an anion selected from the group consisting of a halide ion, an inorganic acid ion, a hydroxide ion, and an isothiocyanate ion. and a solvent, and applying the composition for forming a coating film to a surface of the vessel or substrate, and drying the composition.

[0026]

[14] The method for producing a cell culture vessel according to

[12] , wherein the vessel or substrate has the ability to inhibit cell adhesion.

[0027]

[15] The following formula (I): [ka] [In the formula, U a1 and Ua2 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a1 represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a2 A method for producing a cell aggregate, comprising using a polymer containing a unit derived from a monomer represented by the formula: represents a linear or branched alkylene group having 1 to 5 carbon atoms as a base membrane for cell culture.

[0028]

[16] The polymer may further comprise a compound represented by the formula (II): [ka] [In the formula, R b The method for producing a cell aggregate described in

[15] , wherein the copolymer contains a unit derived from a monomer represented by the following formula: represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms.

[0029]

[17] The following formula (I): [ka] [In the formula, U a1 and U a2 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a1 represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a2 Use of a polymer containing units derived from a monomer represented by the following formula: [wherein represents a linear or branched alkylene group having 1 to 5 carbon atoms] as a base membrane for cell culture, in which cells are attached and then detached to obtain cell aggregates.

[0030]

[18] The polymer may further comprise a compound represented by the formula (II): [ka] [In the formula, R b represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms]. Use of the copolymer as a base membrane for cell culture, as described in

[17] , in which cells are adhered and then detached to obtain a cell aggregate. Effect of the Invention

[0031] According to the present invention, a polymer derived from poly(2-N,N-dimethylaminoethyl methacrylate) can be easily produced from a monomer having a cationic functional group and preferably a monomer further having an anionic functional group, without relying on light irradiation such as ultraviolet light, while controlling the molecular weight and molecular weight distribution, and further controlling the ratio of the cationic functional group and the anionic functional group as desired. By producing the polymer while controlling the molecular weight, the coatability on the substrate can be easily improved. [Brief description of the drawings]

[0032] [Figure 1] FIG. 13 is a diagram showing the results of surface profile measurement of the polymers of Synthesis Examples 3 and 8 using a contact needle film thickness meter in Example 2 (surface profile observation of coated films). [Diagram 2] 13 shows photographs of the state of adherent cells on polymer-coated plates having the polymers of Synthesis Example 3 and Synthesis Example 4 as base films in Example 4 (4-3. Cell adhesion experiment). [Diagram 3] 13 is a photograph showing the state of cell aggregates in a polymer-coated plate having the polymers of Synthesis Example 3 and Synthesis Example 4 as a base film in Example 4 (4-4. Observation of cell aggregates). [Figure 4] 1 shows photographs of the state of cells in polymer-coated dishes having the polymers of Synthesis Examples 1, 10, 11 and 12 as base films in Example 5 (5-3. Cell attachment experiment). [Diagram 5]1 shows photographs of the appearance of cell aggregates in polymer-coated dishes having the polymers of Synthesis Examples 1, 10, 11 and 12 as base films in Example 5 (5-4. Observation of cell aggregates). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] [Polymers used as substrates for cell culture] The polymer used as the base membrane for cell culture in the present application is The following formula (I): [ka]

[0034] [In the formula, U a1 , U a2 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a1 represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a2 represents a linear or branched alkylene group having 1 to 5 carbon atoms].

[0035] The polymer is a compound represented by the following formula (II): [ka] [In the formula, R b represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms].

[0036] In this specification, unless otherwise defined, examples of a "linear or branched alkyl group having 1 to 5 carbon atoms" include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a s-butyl group, a t-butyl group, an n-pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 1,1-dimethylpropyl group, a 1,2-dimethylpropyl group, a 2,2-dimethylpropyl group, and a 1-ethylpropyl group. R a1 and R b are preferably each independently selected from a hydrogen atom and a methyl group. U a1 and U a2 are each preferably independently selected from a hydrogen atom, a methyl group, an ethyl group, a n-propyl group, an isopropyl group, and a n-butyl group, more preferably a methyl group or an ethyl group, and most preferably a methyl group.

[0037] In this specification, unless otherwise defined, examples of the "straight-chain or branched alkylene group having 1 to 5 carbon atoms" include a methylene group, an ethylene group, a propylene group, a trimethylene group, a tetramethylene group, a 1-methylpropylene group, a 2-methylpropylene group, a dimethylethylene group, an ethylethylene group, a pentamethylene group, a 1-methyl-tetramethylene group, a 2-methyl-tetramethylene group, a 1,1-dimethyl-trimethylene group, a 1,2-dimethyl-trimethylene group, a 2,2-dimethyl-trimethylene group, a 1-ethyl-trimethylene group, etc. a2 is preferably selected from an ethylene group and a propylene group.

[0038] Therefore, the cationic monomer represented by the above formula (I) includes 2-N,N-dimethylaminoethyl methacrylate, N-isopropylacrylamide, etc., with 2-N,N-dimethylaminoethyl methacrylate being preferred.The anionic monomer represented by the above formula (II) includes acrylic acid, methacrylic acid, etc., with methacrylic acid being preferred.

[0039] The molar ratio of the units derived from the monomer represented by formula (I) / the units derived from the monomer represented by formula (II) in the polymer is 100 / 0 to 50 / 50, preferably 98 / 2 to 50 / 50, more preferably 98 / 2 to 60 / 40, and particularly preferably 98 / 2 to 70 / 30. This is because if the molar ratio of formula (II) is 51 or more, the polymer becomes excessively anionic, resulting in a decrease in the adhesive force of cells.

[0040] (Monomers with two or more carbon-carbon unsaturated bonds) The polymer may be a polymer obtained by polymerizing a monomer having two or more carbon-carbon unsaturated bonds together with the monomer represented by formula (I) / formula (II). The monomer having two or more carbon-carbon unsaturated bonds is specifically a monomer having two or more carbon-carbon double bonds, such as a polyfunctional acrylate compound, a polyfunctional acrylamide compound, a polyfunctional polyester, or an isoprene compound.

[0041] Preferred specific examples include monomers represented by the following formulas (III) to (V). [ka]

[0042] [ka]

[0043] [ka]

[0044] In the formula, R c and R d each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R erepresents a linear or branched alkylene group having 1 to 5 carbon atoms, and n represents a number from 1 to 50. Among these, a monomer represented by formula (III) is preferred.

[0045] The molar ratio of the monomers represented by formulas (III) to (V) to the entire polymer is preferably 0 to 5.0%, and more preferably 0 to 3.0%. If the molar ratio of the formulae (III) to (V) is 5.0% or more, excessive crosslinking may result in high molecular weight, which may cause gelation during production, making production difficult. R c and R d are preferably each independently selected from a hydrogen atom and a methyl group. R e is preferably selected from methylene, ethylene and propylene groups, most preferably ethylene groups. Although n is a number from 1 to 50, n is preferably a number from 1 to 30, and more preferably, n is a number from 1 to 10.

[0046] The difference between the mol% value of the monomer represented by formula (II) relative to the total amount of the polymer and the mol% value of the monomer represented by formula (II) relative to the total amount of monomers charged in the preparation step is 0 to 10 mol%. The polymer of the present application has a small difference between the monomer charge ratio and the actual measured value of the produced polymer, which is 0 to 10 mol%, due to the production method described below. More preferably, it is 0 to 8 mol%.

[0047] The number average molecular weight (Mn) of the polymer is preferably from 20,000 to 1,000,000, and more preferably from 50,000 to 800,000.

[0048] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the polymer is 1.01 to 10.00, preferably 1.2 to 8.0, preferably 1.4 to 6.0, preferably 1.5 to 5.0, and preferably 1.6 to 4.5.

[0049] The number average molecular weight (Mn) and the number average molecular weight (Mn) can be determined, for example, by gel filtration chromatography described in the examples. By using the polymer of the present application, it is possible to form cell aggregates by adhering cells and then detaching them. The cell aggregate refers to a structure formed as a result of cell aggregation, and is not limited to a spherical or ring shape. Compared to cell aggregates produced by non-adhesive culture on a conventional low-adhesion cell plate, this method has the advantage of being able to adjust the size of the cell aggregate by specifying the adhesion area (cell aggregates of any size can be produced).

[0050] [Method of manufacturing a polymer to be used as a base film forming agent for cell culture] The polymer of the present application can be produced by a thermal polymerization method. For example, a monomer of the above formula (I) is dissolved in an organic solvent, a radical polymerization initiator is added, and then the above formula (II) is added as necessary, and further, as necessary, a monomer having two or more carbon-carbon unsaturated bonds (monomers represented by formulas (III) to (V) and the like) is added to form a mixture, which is then thoroughly stirred to make it homogenous, and then the mixture is heated to, for example, 51°C or higher, for example, 51 to 180°C, 51 to 150°C, 51 to 130°C, or 51 to 100°C, for example, the reflux temperature of the solvent (for example, 66 to 85°C for tetrahydrofuran), while flowing nitrogen, and stirred for, for example, 1 to 48 hours to obtain a polymer. The obtained polymer may be purified by reprecipitation or dialysis.

[0051] In one embodiment, the composition can be prepared by a production method including the steps of dissolving the monomer of formula (I) in a solvent, adding a polymerization initiator, and then reacting (polymerizing) the monomer of formula (II) in the solvent at a total concentration of both compounds of 0.01% by mass to 40% by mass, as required.

[0052] Examples of the organic solvent used in the above polymerization include ether solvents such as tetrahydrofuran and 1,4-dioxane, aliphatic alcohol solvents having 1 to 4 carbon atoms such as methanol, ethanol and isopropanol, aromatic hydrocarbon solvents such as toluene, and mixtures thereof.

[0053] In order to efficiently advance the polymerization reaction, it is desirable to use a radical polymerization initiator. Examples of radical polymerization initiators include azo polymerization initiators such as dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries, Ltd.), 2,2'-azobis(2,4-dimethylvaleronitrile) (V-65, Fujifilm Wako Pure Chemical Industries, Ltd.), 2,2'-azobis(isobutyronitrile) (AIBN, Fujifilm Wako Pure Chemical Industries, Ltd.), 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]n hydrate (VA-057, Fujifilm Wako Pure Chemical Industries, Ltd.), and 2,2'-(N-butyl-2-methylpropionamide) (VAm-110, Fujifilm Wako Pure Chemical Industries, Ltd.). The amount of the polymerization initiator added is 0.05% by mass to 5% by mass based on the total weight of the monomers used in the polymerization. The use of a polymerization initiator not only improves the efficiency of the polymerization reaction, but also enables the adjustment of the physical properties of the polymer by modifying the terminal functional groups.

[0054] [Method of manufacturing a base film forming agent for cell culture] A base film forming agent for cell culture can be produced by mixing the polymer with an aqueous solution by a method known per se. The aqueous solution may be water, a salt-containing aqueous solution such as physiological saline or a phosphate buffer solution, or a mixed solvent of water or a salt-containing aqueous solution with an alcohol. The alcohol may be an alcohol having 2 to 6 carbon atoms, such as ethanol, propanol, isopropanol, 1-butanol, 2-butanol, isobutanol, t-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 1-heptanol, 2-heptanol, 2,2-dimethyl-1-propanol (=neopentyl alcohol), 2-methyl-1-propanol, 2-methyl-1-butanol, 2-methyl-2-butanol (=t-amyl alcohol), 3-methyl-1-butanol, 3-methyl-3-pentanol, cyclopentanol, 1-hex ... Examples of suitable solvents include cyclohexanol, 2-hexanol, 3-hexanol, 2,3-dimethyl-2-butanol, 3,3-dimethyl-1-butanol, 3,3-dimethyl-2-butanol, 2-ethyl-1-butanol, 2-methyl-1-pentanol, 2-methyl-2-pentanol, 2-methyl-3-pentanol, 3-methyl-1-pentanol, 3-methyl-2-pentanol, 3-methyl-3-pentanol, 4-methyl-1-pentanol, 4-methyl-2-pentanol, 4-methyl-3-pentanol, and cyclohexanol. These solvents may be used alone or in combination. In addition to the copolymer and the solvent, the undercoat forming agent may contain other substances as required within the range that does not impair the performance of the undercoat film to be obtained, such as pH adjusters, crosslinking agents, preservatives, surfactants, primers for improving adhesion to containers or substrates, antifungal agents, and sugars.

[0055] [Method of manufacturing base film for cell culture, method of manufacturing cell culture vessel, cell culture vessel] The agent for forming a base film for cell culture can be applied to the surface of a vessel or a substrate and then dried to produce a base film for cell culture or a cell culture vessel containing the base film. Here, the "surface" refers to the surface that comes into contact with the contents, such as cells or a cell culture solution. Examples of the container or substrate include dishes or petri dishes, such as Petri dishes, tissue culture dishes, and multi-dishes, which are generally used for cell culture, flasks, such as cell culture flasks and spinner flasks, bags, such as plastic bags, Teflon (registered trademark) bags, and culture bags, plates, such as microplates, microwell plates, multi-plates, and multi-well plates, chamber slides, tubes, trays, bottles, such as roller bottles, etc. Preferred are petri dishes or dishes, plates, and trays.

[0056] Examples of the material of the container or the substrate include glass, metal, a metal-containing compound or a metalloid-containing compound, activated carbon, and resin. Examples of the metal include typical metals (alkali metals: Li, Na, K, Rb, Cs; alkaline earth metals: Ca, Sr, Ba, Ra), magnesium group elements: Be, Mg, Zn, Cd, Hg, aluminum group elements: Al, Ga, In, rare earth elements: Y, La, Ce, Pr, Nd, Sm, Eu, tin group elements: Ti, Zr, Sn, Hf, Pb, Th, iron group elements: Fe, Co, Ni, earth elements: V, Nb, Ta, chromium group elements: Cr, Mo, W, U, manganese group elements: Mn, Re, precious metals: Cu, Ag, Au, platinum group elements: Ru, Rh, Pd, Os, Ir, Pt, etc. Examples of metal-containing compounds or metalloid-containing compounds include ceramics, which are sintered bodies whose basic component is a metal oxide and are hardened by heat treatment at high temperatures; semiconductors such as silicon, metal oxides or metalloid oxides (silicon oxide, alumina, etc.), metal carbides or metalloid carbides, metal nitrides or metalloid nitrides (silicon nitride, etc.), metal borides or metalloid borides, and other inorganic solid materials; aluminum, nickel titanium, and stainless steel (SUS304, SUS316, SUS316L, etc.).

[0057] The resin may be a natural resin or a derivative thereof, or a synthetic resin. Examples of the natural resin or a derivative thereof include cellulose, cellulose triacetate (CTA), nitrocellulose (NC), and cellulose with immobilized dextran sulfate. Examples of the synthetic resin include polyacrylonitrile (PAN), polyester polymer alloy (PEPA), polystyrene (PS), polysulfone (PSF), polyethylene terephthalate (PET), polymethyl methacrylate (PMMA), polyvinyl alcohol (PVA), polyurethane (PU), ethylene vinyl alcohol (EVAL), polyethylene (PE), polyester, polypropylene (PP), polyvinylidene fluoride (PVDF), polyethersulfone (PES), polycarbonate (PC), polyvinyl chloride (PVC), polytetrafluoroethylene (PTFE), ultra-high molecular weight polyethylene (UHPE), polydimethylsiloxane (PDMS), acrylonitrile-butadiene-styrene resin (ABS), and Teflon (registered trademark). In the production of the cell culture vessel of the present invention, since no high temperature treatment is required when coating the polymer so that it is present on at least a portion of the surface of the vessel or substrate, resins with low heat resistance can also be used.

[0058] The container or substrate may be made of one material or a combination of two or more materials. Among these materials, glass, silicon, silicon oxide, polystyrene (PS), polypropylene (PP), polyethersulfone (PES), polyethylene terephthalate (PET), polycarbonate (PC), polyvinyl chloride (PVC), Teflon (registered trademark), cycloolefin polymer (COP), polydimethylsiloxane (PDMS), or stainless steel (SUS304, SUS316, SUS316L, etc.) alone or in combination is preferred, and glass, polystyrene (PS), polypropylene (PP), stainless steel (SUS304, SUS316, SUS316L, etc.), or polydimethylsiloxane (PDMS) is particularly preferred.

[0059] The method for applying the base film forming agent for cell culture of the present application can be, for example, an inkjet method, a screen printing method, a slit coating method, a roll-to-roll method, etc., but it is preferably carried out by a printing technique such as an inkjet method or screen printing.

[0060] As another application method, for example, the container is immersed in the above-mentioned undercoat forming agent, the undercoat forming agent is added to the container and left to stand for a predetermined time, or the coating agent is applied to the surface of the container or substrate. In the case of a container, for example, a cell culture container, the undercoat forming agent is added to the container and left to stand for a predetermined time. The addition can be performed, for example, by adding an amount of undercoat forming agent that is 0.5 to 1 times the total volume of the container using a syringe or the like. The standing is performed by appropriately selecting the time and temperature depending on the material of the container or substrate and the type of undercoat forming agent for cell culture, for example, 1 minute to 24 hours, preferably 5 minutes to 3 hours, at 10 to 80°C. This allows the production of a cell culture container having a undercoat film for cell culture on at least a part of the surface of the container, preferably over the entire surface.

[0061] Furthermore, the base film for cell culture on the surface of a container or substrate obtained by such a method can be used as a cell culture container, either as it is without a drying step or after washing with water or the medium of the sample to be subjected to cell culture (e.g., water, a buffer solution, a culture medium, etc.), after a step of contacting the base film with at least a portion of the surface of the container or substrate, preferably after a step of adding a base film forming agent for cell culture and leaving the base film for a predetermined period of time.

[0062] That is, after the step of contacting with at least a portion of the surface of the container or substrate, preferably after the step of adding a base film forming agent for cell culture and leaving it to stand for a predetermined period of time, the container or substrate can be used as a cell culture container without undergoing a drying step within 48 hours, preferably within 24 hours, more preferably within 12 hours, even more preferably within 6 hours, even more preferably within 3 hours, and even more preferably within 1 hour, either as is or after washing with water or the medium of the sample to be subjected to cell culture (e.g., water, a buffer solution, a culture medium, etc., particularly preferably a culture medium (e.g., DMEM medium (Dulbecco's modified Eagle's medium))).

[0063] The container may be subjected to a drying process, which is carried out in air or vacuum, preferably at a temperature in the range of −200° C. to 200° C. The drying process removes the solvent in the undercoat film forming agent, thereby completely fixing the agent to the substrate.

[0064] The undercoat film can be formed by drying at room temperature (10°C to 35°C, preferably 20°C to 30°C, e.g. 25°C), but in order to form the undercoat film more quickly, it may be dried at, for example, 40°C to 50°C. If the drying temperature is less than -200°C, an uncommon refrigerant must be used, which is not versatile, and drying takes a long time due to solvent sublimation, making it inefficient. If the drying temperature is more than 200°C, thermal decomposition of the polymer occurs. A more preferred drying temperature is 10°C to 180°C, and a more preferred drying temperature is 20°C to 150°C.

[0065] The base membrane for cell culture of the present invention is produced through the above-mentioned simple steps. In addition, in order to remove impurities, unreacted monomers, etc. remaining on the base film for cell culture, a step of washing with at least one solvent selected from water and an aqueous solution containing an electrolyte may be carried out. Washing is preferably performed by washing with running water or ultrasonic washing. The aqueous solution containing water and an electrolyte may be heated, for example, to a temperature in the range of 40°C to 95°C. The aqueous solution containing an electrolyte is preferably PBS, saline (containing only sodium chloride), Dulbecco's phosphate buffered saline, Tris buffered saline, HEPES buffered saline, and Veronal buffered saline, and PBS is particularly preferred. After adhesion, the coating film remains firmly attached to the substrate without being dissolved even when washed with water, PBS, alcohol, etc.

[0066] The maximum and minimum thicknesses of the base film for cell culture of the present invention are in the range of 1 to 1000 nm, and preferably in the range of 5 to 500 nm.

[0067] The container or substrate may be subjected to a cell adhesion inhibiting treatment before the above-mentioned base film coating and drying process. A container or substrate having cell adhesion inhibiting ability can be produced, for example, by a process of coating a known coating film forming composition having cell adhesion inhibiting ability. An example of a coating film forming composition having cell adhesion inhibiting ability is a copolymer comprising a repeating unit containing an organic group represented by the following formula (a) and a repeating unit containing an organic group represented by the following formula (b): [ka] [In the formula, U a11 , U a12 , U b11 , U b12 and U b13 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; An - represents an anion selected from the group consisting of a halide ion, an inorganic acid ion, a hydroxide ion, and an isothiocyanate ion. and a solvent, and applying the composition for forming a coating film to the surface of a container or a substrate, and drying the composition.

[0068] The straight-chain or branched alkyl group having 1 to 5 carbon atoms is the same as that described above. For example, the composition for forming a coating film described in WO2014 / 196650 can be used as the composition for forming a coating film. The method for applying the composition for forming a coating film is not particularly limited, and a typical application method such as spin coating, dip coating, or solvent casting can be used.

[0069] The drying step of the coating film is carried out in air or vacuum at a temperature in the range of −200° C. to 180° C. The drying step removes the solvent in the composition for forming a coating film, and also forms ionic bonds between the copolymers of formula (a) and formula (b) to completely adhere to the substrate.

[0070] The coating film can be formed by drying at room temperature (10°C to 35°C, e.g., 25°C), but in order to form the coating film more quickly, it may be dried at, for example, 40°C to 50°C. A drying process at extremely low to low temperatures (around -200°C to -30°C) by the freeze-drying method may also be used. Freeze-drying is called vacuum freeze-drying, and is a method in which the material to be dried is usually cooled with a refrigerant and the solvent is removed by sublimation in a vacuum state. Common refrigerants used in freeze-drying include a mixture of dry ice and methanol (-78°C), liquid nitrogen (-196°C), etc.

[0071] If the drying temperature is below -200°C, an uncommon refrigerant must be used, resulting in lack of versatility, and drying takes a long time due to solvent sublimation, resulting in poor efficiency. If the drying temperature is above 200°C, the ionic bond reaction on the coating film surface proceeds too much, causing the surface to lose hydrophilicity, and the ability to inhibit adhesion of biological materials is not exerted. The more preferred drying temperature is 10°C to 180°C, and the more preferred drying temperature is 25°C to 150°C.

[0072] After drying, in order to remove impurities remaining on the coating film, unreacted monomers, etc., and further to adjust the ion balance of the copolymer in the film, it is desirable to wash the film with running water or ultrasonic cleaning with one or more solvents selected from water and an aqueous solution containing an electrolyte. The aqueous solution containing water and an electrolyte may be heated, for example, to a temperature in the range of 40°C to 95°C. The aqueous solution containing an electrolyte is preferably PBS, saline (containing only sodium chloride), Dulbecco's phosphate buffered saline, Tris buffered saline, HEPES buffered saline, and Veronal buffered saline, and PBS is particularly preferred. After adhesion, the coating film remains firmly attached to the substrate without being eluted even when washed with water, PBS, alcohol, etc. Even if a biological material adheres to the formed coating film, it can be easily removed by washing with water, etc., and the substrate surface on which the coating film is formed has the ability to inhibit adhesion of biological material. The coating film has a thickness of preferably 5 to 1000 nm, and more preferably 5 to 500 nm.

[0073] In addition, the cell culture vessel may be a commercially available cell culture dish that has been treated to reduce cell adhesion, or a cell culture vessel that has the ability to inhibit cell adhesion. For example, the cell culture vessel described in JP 2008-61609 A may be used, but is not limited to this.

[0074] Having the ability to inhibit cell adhesion means that the relative absorbance (WST OD450nm) (%) ((absorbance (WST OD450nm) of the example) / (absorbance (WST OD450nm) of the comparative example)) when compared to a case without a coating film or without a low cell adhesion treatment, measured using a fluorescence microscope using a method described in the examples of WO2016 / 093293, is 50% or less, preferably 30% or less, and more preferably 20% or less.

[0075] [Method of manufacturing cell aggregates] The method for producing a cell aggregate of the present application comprises the steps of: [ka]

[0076] [In the formula, U a1 , U a2 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a1 represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a2 This is a method for producing cell aggregates, which is carried out on a base membrane for cell culture obtained from a polymer containing units derived from a monomer represented by the formula [representing a linear or branched alkylene group having 1 to 5 carbon atoms], by a method known per se, for example, the method described in the Examples. The above-mentioned cell culture base membrane comprises a monomer-derived unit represented by formula (I) and a monomer-derived unit represented by formula (II):

[0077] [ka] [In the formula, R b represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms]. EXAMPLES

[0078] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0079] <Method of measuring molecular weight> The weight average molecular weights shown in the following synthesis examples are the results obtained by gel filtration chromatography (hereinafter abbreviated as GFC). (Measurement conditions) Equipment: HLC-8320GPC (Tosoh Corporation) GFC column: TSKgel G6000+3000PWXL-CP ·Flow rate: 1.0ml / min Eluent: Salt-containing water / organic mixed solvent Column temperature: 40℃ Detector: RI Injection concentration: polymer solids 0.05% by mass ·Injection volume: 100μL Calibration curve: Cubic approximation curve Standard sample: Polyethylene oxide (Agilent) x 10 types

[0080] <Synthesis Example 1> Preparation of a polymer for use as a base film forming agent for cell culture by thermal polymerization (1) 27.04 g of tetrahydrofuran was added to 9.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.01 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the above tetrahydrofuran solution while maintaining the temperature at 20°C or less. The mixture containing all of the above, which was thoroughly stirred and homogenized, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and the temperature was raised to the reflux temperature while stirring. A polymer was obtained as a reaction product by heating and stirring while maintaining the above environment for 24 hours. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive homopolymer (yield: 6.4 g, yield: 71%). The weight-average molecular weight of this polymer measured by GFC was 250,000, and the polydispersity was 2.0 (Synthesis Example Polymer 1).

[0081] <Synthesis Example 2> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (2) 37.10 g of tetrahydrofuran was added to 9.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.02 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 0.26 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.) were added to the above tetrahydrofuran solution while maintaining the temperature at 20°C or lower. The mixture containing all of the above, which was thoroughly stirred and made uniform, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and the temperature was raised to the reflux temperature while stirring. A polymer was obtained as a reaction product by heating and stirring while maintaining the above environment for 24 hours. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer (yield: 6.6 g, yield: 71%). The weight-average molecular weight of this polymer measured by GFC was 24,000, and the polydispersity was 2.0 (Synthesis Example Polymer 2).

[0082] <Synthesis Example 3> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (3) 41.94 g of tetrahydrofuran was added to 10.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.01 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 0.48 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.) were added to the above tetrahydrofuran solution while maintaining the temperature at 20°C or lower. The mixture containing all of the above, which was thoroughly stirred and made uniform, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and the temperature was raised to the reflux temperature while stirring. The above environment was maintained for 24 hours, and a polymer was obtained as a reaction product by heating and stirring. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer (yield: 7.3 g, yield: 69%). The weight-average molecular weight of this polymer measured by GFC was 290,000, and the polydispersity was 1.9 (Synthesis Example Polymer 3).

[0083] <Synthesis Example 4> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (4) 38.26 g of tetrahydrofuran was added to 9.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.02 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 0.55 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.) were added to the above tetrahydrofuran solution while maintaining the temperature at 20°C or lower. The mixed liquid containing all of the above, which was thoroughly stirred and made homogeneous, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and heated to the reflux temperature while stirring. A polymer was obtained as a reaction product by heating and stirring while maintaining the above environment for 24 hours. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer (yield: 7.2 g, yield: 75%). The weight-average molecular weight of this polymer measured by GFC was 250,000, and the polydispersity was 1.9 (Synthesis Example Polymer 4).

[0084] <Synthesis Example 5> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (5) 41.00 g of tetrahydrofuran was added to 9.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.02 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 1.23 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.) were added to the above tetrahydrofuran solution while maintaining the temperature at 20°C or less. The mixed liquid containing all of the above, which was thoroughly stirred and made homogeneous, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and heated to the reflux temperature while stirring. A polymer was obtained as a reaction product by heating and stirring while maintaining the above environment for 24 hours. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer (yield: 5.8 g, yield: 57%). The weight-average molecular weight of this polymer measured by GFC was 270,000, and the polydispersity was 2.1 (Synthesis Example Polymer 5).

[0085] <Synthesis Example 6> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (6) 44.58 g of tetrahydrofuran was added to 9.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.03 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 2.11 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.) were added to the above tetrahydrofuran solution while maintaining the temperature at 20°C or lower. The mixture containing all of the above, which was thoroughly stirred and made uniform, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and the temperature was raised to the reflux temperature while stirring. The above environment was maintained for 24 hours, and a polymer was obtained as a reaction product by heating and stirring. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer (yield: 9.6 g, yield: 86%). The weight-average molecular weight of this polymer measured by GFC was 270,000, and the polydispersity was 2.4 (Synthesis Example Polymer 6).

[0086] <Synthesis Example 7> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (7) 41.94 g of tetrahydrofuran was added to 10.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.01 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.), 0.48 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.), and 0.21 g of polyethylene glycol dimethacrylate (n = about 4) (Tokyo Chemical Industry Co., Ltd.) were added to the above tetrahydrofuran solution while maintaining the temperature at 20 ° C or less. The mixed liquid containing all of the above, which was thoroughly stirred and made uniform, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and the temperature was raised to the reflux temperature while stirring. A polymer was obtained as a reaction product by heating and stirring while maintaining the above environment for 24 hours. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. The reaction product was purified by dialysis for 72 hours. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer. The weight-average molecular weight of this polymer measured by GFC was 660,000, and the polydispersity was 3.8 (Synthesis Example Polymer 7).

[0087] <Synthesis Example 8> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (8) 43.30 g of ethanol was added to 10.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.31 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 0.48 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.) were added to the above ethanol solution while maintaining the temperature at 20 ° C or less. The mixed liquid containing all of the above, which was thoroughly stirred and became homogeneous, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and heated to the reflux temperature while stirring. A polymer was obtained as a reaction product by heating and stirring while maintaining the above environment for 24 hours. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer. The weight-average molecular weight of this polymer measured by GFC was 88,000, and the polydispersity was 2.4 (Synthesis Example Polymer 8).

[0088] <Synthesis Example 9> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (9) 41.94 g of tetrahydrofuran was added to 10.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.01 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 0.48 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.) were added to the above tetrahydrofuran solution while maintaining the temperature at 20°C or lower. The mixture containing all of the above, which was thoroughly stirred and homogenized, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and the temperature was raised to 60°C while stirring. A polymer was obtained as a reaction product by heating and stirring while maintaining the above environment for 24 hours. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer. The weight-average molecular weight of this polymer measured by GFC was 140,000, and the polydispersity was 2.5 (Synthesis Example Polymer 9).

[0089] <Synthesis Example 10> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (10) 31.46 g of ethanol was added to 10.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.01 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 0.48 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.) were added to the above ethanol solution while maintaining the temperature at 20 ° C or less. The mixed liquid containing all of the above, which was thoroughly stirred and became homogeneous, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and heated to the reflux temperature while stirring. A polymer was obtained as a reaction product by heating and stirring while maintaining the above environment for 24 hours. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer. The weight-average molecular weight of this polymer measured by GFC was 770,000, and the polydispersity was 4.1 (Synthesis Example Polymer 10).

[0090] <Synthesis Example 11> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (11) 43.90 g of ethanol was added to 10.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.01 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 0.97 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.) were added to the above ethanol solution while maintaining the temperature at 20 ° C or less. The mixed liquid containing all of the above, which was thoroughly stirred and made homogeneous, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and heated to the reflux temperature while stirring. A polymer was obtained as a reaction product by heating and stirring while maintaining the above environment for 24 hours. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer. The weight-average molecular weight of this polymer measured by GFC was 660,000, and the polydispersity was 3.6 (Synthesis Example Polymer 11).

[0091] <Synthesis Example 12> Preparation of polymer for use as a base film forming agent for cell culture by thermal polymerization (10) 70.00 g of ethanol was added to 10.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and dissolved thoroughly. Next, 0.01 g of dimethyl 1,1'-azobis(1-cyclohexanecarboxylate) (VE-073, Fujifilm Wako Pure Chemical Industries Co., Ltd.) and 2.35 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.) were added to the above ethanol solution while maintaining the temperature at 20 ° C. or less. The mixed liquid containing all of the above, which was thoroughly stirred and made homogeneous, was added to a three-neck flask equipped with a cooling tube, and nitrogen was flowed and heated to the reflux temperature while stirring. A polymer was obtained as a reaction product by heating and stirring while maintaining the above environment for 24 hours. The reaction product was reprecipitated with hexane, which is a poor solvent, and the precipitate was collected by filtration and dried under reduced pressure. The obtained powder was dissolved in pure water, and the solution was transferred to a dialysis tube. Dialysis was performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (AS ONE Corporation, model number: SYGF0605MNXX104), and the filtrate was freeze-dried to obtain a temperature-responsive polymer. The weight-average molecular weight of this polymer measured by GFC was 570,000, and the polydispersity was 3.6 (Synthesis Example Polymer 12).

[0092] <Comparative Synthesis Example 1> Preparation of polymer by photopolymerization (1) 10.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and 500 μL of water were added to a 30 mL soft glass transparent vial and thoroughly stirred to make the mixture homogenous. The mixture (liquid) was then deoxygenated by purging with nitrogen gas for 15 minutes. After that, the reaction mixture was subjected to a high-pressure mercury lamp (USHIO, model number: UM-102) to measure the illuminance at 365 nm to be 0.1 mW / cm 2The reaction product was polymerized by irradiating it with ultraviolet light at about 25°C for 19 hours while adjusting the distance so that the reaction product was polymerized. The reaction product became viscous after 5 hours and solidified (gelled) after 18 hours, and a polymer was obtained as the reaction product. This reaction product was poorly soluble in 2-propanol, and only the partially dissolved portion was transferred to a dialysis tube. The solution was a stringy viscous material and difficult to handle. Dialysis was then performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (manufactured by AS ONE Corporation, model number: SYGF0605MNXX104), and the obtained filtrate was freeze-dried to obtain Comparative Synthesis Example Polymer 1 (yield: 1.5 g, yield: 15%).

[0093] <Comparative Synthesis Example 2> Preparation of polymer by photopolymerization (2) 10.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and 1000 μL of water were added to a 30 mL soft glass transparent vial and thoroughly stirred to make the mixture homogenous. The mixture (liquid) was then deoxygenated by purging with nitrogen gas for 15 minutes. After that, the reaction mixture was subjected to a high-pressure mercury lamp (USHIO, model number: UM-102) to measure the illuminance at 365 nm to be 0.1 mW / cm 2 The reaction product was polymerized by irradiating it with ultraviolet light at about 25°C for 19 hours while adjusting the distance so that the reaction product was polymerized. The reaction product became viscous after 5 hours and solidified after 18 hours, and a polymer was obtained as the reaction product. This reaction product was poorly soluble in 2-propanol, and only the partially dissolved solution was transferred to a dialysis tube. The solution was a stringy viscous material and difficult to handle. Dialysis was then performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (manufactured by AS ONE Corporation, model number: SYGF0605MNXX104), and the obtained filtrate was freeze-dried to obtain Comparative Synthesis Example Polymer 2 (yield: 2.6 g, yield: 26%).

[0094] <Comparative Synthesis Example 3> Preparation of polymer by photopolymerization (3) 10.00 g of 2-(dimethylamino)ethyl methacrylate (Tokyo Chemical Industry Co., Ltd.) and 500 μL of water were added to a 30 mL soft glass transparent vial and thoroughly stirred to make the mixture homogenous. The mixture (liquid) was then deoxygenated by purging with nitrogen gas for 15 minutes. After that, the reaction mixture was subjected to a high-pressure mercury lamp (USHIO, model number: UM-102) to measure the illuminance at 365 nm to be 0.1 mW / cm 2 The reaction product was polymerized by irradiating it with ultraviolet light at about 25°C for 19 hours while adjusting the distance so that the reaction product was polymerized. The reaction product became viscous after 5 hours and solidified after 18 hours, and a polymer was obtained as the reaction product. This reaction product was poorly soluble in 2-propanol, and only the partially dissolved solution was transferred to a dialysis tube. The solution was a stringy viscous material and difficult to handle. Dialysis was then performed for 72 hours to purify the reaction product. The solution containing the reaction product was filtered through a 1.0 μm glass fiber filter (manufactured by AS ONE Corporation, model number: SYGF0605MNXX104), and the obtained filtrate was freeze-dried to obtain Comparative Synthesis Example Polymer 3 (yield: 3.3 g, yield: 33%).

[0095] Example 1 (Polymer composition analysis by 1H-NMR measurement) The nuclear magnetic resonance spectra (NMR) of Polymers 1 to 12 and Polymers 1 to 3 were measured using a nuclear magnetic resonance apparatus (manufactured by BRUKER, model number: ASC End500) with heavy water (DO) as the standard. Representative peaks common to Polymers 1 to 6 are shown below.

[0096] 1H-NMR (in D2O) δ 0.8-1.2 (br, -CH2-C(CH3)-), 1.6-2.0 (br, -CH2-C(CH3)-), 2.2-2.4 (br, -N(CH3)2), 2.5-2.7 (br, -CH2-N(CH3)2), 4.0-4.2 (br, -O-CH2-).

[0097] Here, the ratio of the number of functional amino groups in the side chain to the number of functional carboxyl groups in the side chain was calculated from the number of protons A in the methyl group -CH2-C(CH3)- (δ 0.8-1.2) in the main chain (three per monomer molecule in the case of a homopolymer of DMAEMA) and the number of methyl protons B in the -O-CH2- group (δ 4.0-4.2) in the side chain (two per monomer molecule in the case of a homopolymer of DMAEMA). As a result, the composition ratio of 2-(dimethylamino)ethyl methacrylate (hereinafter abbreviated as "DM") / methacrylic acid (hereinafter abbreviated as "MA") in Synthesis Examples 1 to 12 synthesized by thermal polymerization was 100 / 0 in Synthesis Example 1, 95 / 5 in Synthesis Example 2, 95 / 5 in Synthesis Example 3, 88 / 12 in Synthesis Example 4, 82 / 18 in Synthesis Example 5, 76 / 24 in Synthesis Example 6, 89 / 11 in Synthesis Example 7, 92 / 8 in Synthesis Examples 8 to 10, 85 / 15 in Synthesis Example 11, and 70 / 30 in Synthesis Example 12. In the case of the comparative synthesis examples synthesized by photopolymerization, the ratio was 99 / 1 in all of Comparative Synthesis Examples 1, 2, and 3, making it difficult to control the ratio of DM and MA. From the above results, it was confirmed that the ratio of DM and MA can be controlled in the polymer synthesized by thermal polymerization compared to the polymer synthesized by photopolymerization, and the polymer can be obtained in a higher yield. Detailed results are shown in Table 1.

[0098] For the polymers synthesized in Synthesis Examples 1 to 12, the weight average molecular weight Mw ranged from 88,000 to 770,000, making it possible to produce a wide range of polymers. The molecular weight distribution (PDI) ranged from 1.9 to 4.1, making it possible to produce a wide range of polymers from small to relatively large. All polymers were synthesized without gelation. On the other hand, when this polymer is synthesized by photopolymerization, it is difficult to control the molecular weight and molecular weight distribution in a small range. For example, the patent publication (Patent No. 5746240) states that when synthesized in the same manner as Comparative Synthesis Example 1, the PDI is 3.0, when synthesized in the same manner as Comparative Synthesis Example 2, the PDI is 4.3, and when synthesized in the same manner as Comparative Synthesis Example 3, the PDI is 7.4. In addition, when synthesized in photopolymerization, all polymers gel during synthesis, making it difficult to control not only the molecular weight but also the reaction itself. If the molecular weight distribution becomes extremely large, there is a concern that low molecular weight components will be eluted and high molecular weight components will be precipitated. Considering these points, by synthesizing a polymer using thermal polymerization, it is possible to stably produce a polymer while controlling the molecular weight and molecular weight distribution, compared to synthesis using photopolymerization.

[0099] [Table 1]

[0100] Example 2: Measurement of the surface shape of the coating film Example polymers 3 and 8, which have different molecular weights, were dissolved in sterile water to a concentration of 0.5 mg / mL, to produce a base film forming agent for cell culture. Using an inkjet device (MICROJET, model number: LaboJet-600), 200 nL of each solution was applied to a silicon substrate treated with hexamethyldisilazane. After drying at room temperature for 5 minutes to harden the film, the surface shape of the applied film was measured using a microshape measuring instrument (Kosaka Laboratory, model number: ET-4000A). The measurement conditions were a measuring force of 100 μN and a feed speed of 0.05 mm / sec. In the case of Polymer 3 (Mw = 290,000), the periphery of the coating film was raised, while the inside was flat. On the other hand, in the case of Polymer 8 (Mw = 88,000), in addition to the periphery of the coating film, a bulge was also observed in the center. It was found that the cross-sectional shape of the coating film changes depending on the molecular weight and molecular weight distribution of the polymer.

[0101] Example 3: Preparation of an aqueous polymer solution for producing a base film forming agent for cell culture Polymer 1 of Synthesis Example to Polymer 12 of Synthesis Example were each dissolved in sterilized water to a concentration of 1 mg / mL to prepare aqueous polymer solutions 1 to 12.

[0102] <Example 4: Cell aggregate production test> (4-1. Preparation of low cell attachment plates) According to the manufacturing method described in Example 30 of WO2014 / 196650, a coating solution was prepared from a copolymer-containing varnish. The prepared coating solution was added to the wells of a 12-well cell culture plate (BD Biosciences, #351143) at 500 μL (solid content 0.5% by mass) per well, and the plate was left to stand at room temperature for 1 hour, after which the excess coating solution was removed. The plate was dried overnight at 50 ° C. using an oven (Advantec Toyo Co., Ltd., dryer FC-612). Then, 500 μL of sterilized water was added per well, removed, and washed. The plate was washed twice more in the same manner, and dried overnight at 50 ° C. to obtain a low cell adhesion plate.

[0103] (Production of a base film forming agent for cell culture, preparation of polymer-coated plates to be used as a base film for cell culture) The 1 mg / mL aqueous polymer solutions obtained from Polymer 3 and Polymer 4 were diluted with sterile water to 100 μg / mL to produce base film forming agents 3 and 4 for cell culture. 1 μL of each of the prepared aqueous polymer solutions was dropped onto the low cell adhesion plate and dried at room temperature for 30 minutes to obtain a polymer-coated plate to be used as a base film for cell culture in the test.

[0104] (4-2. Cell preparation) Human bone marrow-derived mesenchymal stem cells (PromoCell) were used. Mesenchymal stem cell growth medium Mesenchymal Stem Cell Growth Medium 2 (PromoCell) was used as the medium for culturing the cells. The cells were statically cultured for more than 2 days in a 10 cm diameter petri dish (10 mL of medium) at 37°C / CO2 incubator with 5% carbon dioxide concentration. The cells were then washed with 4 mL of Hepes BSS solution (PromoCell), and 4 mL of trypsin-EDTA solution (PromoCell) was added and allowed to stand at room temperature for 5 minutes. 4 mL of Trypsin Neutralizing Solution (PromoCell) was added to detach the cells and collect them. The suspension was centrifuged (Tomy Seiko Co., Ltd., model number LC-230, 200×g / 3 minutes, room temperature), the supernatant was removed, and the above medium was added to prepare a cell suspension.

[0105] (4-3. Cell attachment experiment) Add 5.9 x 10 cell suspension to the plate prepared above. 5 cells / well (1.75×10 5 cells / cm 2 ), 500μL of each was added. Then, the wells were left to stand for 3.5 hours in a 37℃ / CO2 incubator with 5% carbon dioxide concentration. After standing, non-adherent cells and medium were removed, and the wells were washed with PBS to leave only the adherent cells on the wells. After washing, 500μL / well of new medium was added, and the state of the adherent cells was observed and photographed using an inverted research microscope IX73 (Olympus Corporation). As a result, as shown in Figure 2, adhesion of cells to the areas coated with base film forming agent 3 for cell culture and base film forming agent 4 for cell culture was confirmed.

[0106] (4-4. Observation of cell aggregates) The plate tested above was left to stand for another day in a 37°C / CO2 incubator. After standing, the state of the cells was observed using an inverted research microscope IX73 (Olympus Corporation). As a result, as shown in FIG. 3, it was confirmed that the cells adhered to the base film forming agent 3 for cell culture and the base film forming agent 4 for cell culture were peeled off from the plate and aggregated to form cell aggregates (spheroids). This demonstrated that the base film containing the polymer of the present application is useful as a base film for cell culture vessels.

[0107] <Example 5: Cell aggregate production test> (5-1. Production of a base film forming agent for cell culture and preparation of a polymer-coated plate to be used as a base film for cell culture) The 1 mg / mL aqueous polymer solutions obtained from Synthesis Examples 1, 10, 11, and 12 were diluted with sterile water to 50 μg / mL to produce undercoat film forming agents for cell culture 5, 6, 7, and 8. 1 μL of the aqueous polymer solutions produced were dropped onto low cell adhesion dishes (Sumitomo Bakelite Co., Ltd., #MS-9035X) and dried at 50° C. for 30 minutes to obtain polymer-coated dishes to be used as undercoats for cell culture in the test.

[0108] (5-2. Cell Preparation) Human bone marrow-derived mesenchymal stem cells (PromoCell) were used. Mesenchymal stem cell growth medium Mesenchymal Stem Cell Growth Medium 2 (PromoCell) was used as the medium for culturing the cells. The cells were statically cultured for more than 2 days in a 10 cm diameter petri dish (10 mL of medium) at 37°C / CO2 incubator with 5% carbon dioxide concentration. The cells were then washed with 4 mL of Hepes BSS solution (PromoCell), and 4 mL of trypsin-EDTA solution (PromoCell) was added and allowed to stand at room temperature for 5 minutes. 4 mL of Trypsin Neutralizing Solution (PromoCell) was added to detach the cells and collect them. The suspension was centrifuged (Tomy Seiko Co., Ltd., model number LC-230, 220×g / 3 minutes, room temperature), the supernatant was removed, and the above medium was added to prepare a cell suspension.

[0109] (5-3. Cell attachment experiment) Add 2.7 x 10 cell suspension to the plate prepared above. 6 cells / 3mL / dish (3×10 5 cells / cm 2 ) was added. The wells were then left to stand for 2 hours in a 37°C / CO2 incubator with 5% carbon dioxide. After standing, non-adherent cells and medium were removed, and the wells were washed with PBS to leave only the adherent cells on the wells. After washing, 2 mL of new medium was added per dish, and the state of the adherent cells was observed and photographed using an EVOS FL Auto (ThermoFisherScientific). As a result, as shown in Figure 4, cell adhesion was confirmed to the areas coated with base film forming agent for cell culture 5, base film forming agent for cell culture 6, base film forming agent for cell culture 7, and base film forming agent for cell culture 8.

[0110] (5-4. Observation of cell aggregates) The plate tested above was then subjected to time-lapse photography using EVOS FL Auto. The time-lapse photography was performed under conditions of 37°C / 5% CO2, with the same field of view photographed every hour. As a result, as shown in FIG. 5, it was confirmed that the cells adhered to the base film forming agent 5 for cell culture, the base film forming agent 6 for cell culture, the base film forming agent 7, and the base film forming agent 8 were peeled off from the plate and aggregated to form cell aggregates (spheroids). This demonstrated that the base film containing the polymer of the present application is useful as a base film for cell culture vessels. [Industrial Applicability]

[0111] The polymer obtained by the production method of the present invention can be used as an agent for forming a base film for cell culture. The agent for forming a base film of the present invention can be used to produce a base film for cell culture and a cell culture vessel containing the same.

Claims

1. The following formula (I): [Formula 1] [In the formula, U a1 and U a2 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a1 represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R a2 represents a linear or branched alkylene group having 1 to 5 carbon atoms; [chemical 2] [In the formula, R b represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms), a radical polymerization initiator, and an organic solvent; a polymerization step of heating and stirring the mixture to polymerize the monomer to prepare a polymer; and a step of mixing the polymer obtained in the above step with an aqueous solution.

2. The method according to claim 1, further comprising the step of adding a monomer having two or more carbon-carbon unsaturated bonds to the mixture.

3. The monomer having two or more carbon-carbon unsaturated bonds is represented by the following formula (III): [C3] [In the formula, R c and R d each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; R e represents a linear or branched alkylene group having 1 to 5 carbon atoms, and n represents a number from 1 to 50.

4. The method according to any one of claims 1 to 3, wherein the molar ratio of the unit derived from the monomer represented by formula (I) to the unit derived from the monomer represented by formula (II) in the polymer is 98 / 2 to 50 / 50.

5. The method according to any one of claims 1 to 4, wherein the number average molecular weight (Mn) of the polymer is 20,000 to 1,000,000, and the ratio (Mw / Mn) of the weight average molecular weight (Mw) of the polymer to the number average molecular weight (Mn) is 1.01 to 10.

00.

6. A method for producing a base film for cell culture, comprising a step of applying a base film forming agent for cell culture obtained by the method for producing a base film for cell culture according to any one of claims 1 to 5 to a surface of a container or a substrate, and drying the applied agent.

7. Before the coating and drying step, a copolymer including a repeating unit including an organic group represented by the following formula (a) and a repeating unit including an organic group represented by the following formula (b) is prepared: [C4] [In the formula, U a11 , U a12 , U b11 , U b12 and U b13 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; An - represents an anion selected from the group consisting of a halide ion, an inorganic acid ion, a hydroxide ion, and an isothiocyanate ion. The method according to claim 6, further comprising the step of applying a coating film-forming composition comprising: and a solvent to a surface of a container or a substrate; and drying the composition.

8. The method according to claim 6 , wherein the container or substrate has an ability to inhibit cell adhesion.

9. A method for producing a cell culture vessel, comprising a step of applying the agent for forming a base film for cell culture obtained by the method for producing a cell culture vessel according to any one of claims 1 to 5 to a surface of a vessel or a substrate, and drying the applied agent.

10. Before the coating and drying step, a copolymer including a repeating unit including an organic group represented by the following formula (a) and a repeating unit including an organic group represented by the following formula (b) is prepared: [C5] [In the formula, U a11 , U a12 , U b11 , U b12 and U b13 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 5 carbon atoms; An - represents an anion selected from the group consisting of a halide ion, an inorganic acid ion, a hydroxide ion, and an isothiocyanate ion. The method according to claim 9 , further comprising the step of applying a coating film-forming composition comprising: and a solvent to a surface of a container or a substrate; and drying the composition.

11. The method according to claim 9 , wherein the container or substrate has an ability to inhibit cell adhesion.

12. A method for producing a cell aggregate, comprising using a cell culture vessel obtained by the method according to any one of claims 9 to 11.

Citation Information

Patent Citations

  • Coating composition for culturing adhesive cell

    JP1993292957A

  • Method for producing embryoid bodies from primate embryonic stem cells

    JP2003523766A

  • Method for extracting domoic acid by selective adsorption using halogenated carboxylic acid derivatives

    JP2009524634A

  • Production method of temperature-responsive polymer, temperature-responsive polymer, production method of cell culture vessel, and cell culture vessel

    JP2014162865A

  • Cell culture substrate, method for producing the same, and cell culture method using the same

    JP2016192957A