Radiation-curable compositions containing modified pigments and their applications
The use of inorganic oxide-coated pigments in radiation-curable gravure inks addresses storage stability issues, enhancing ink stability and curing speed, leading to efficient and odor-free printing.
Patent Information
- Application Number
- JP2020548978
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-03-20
- Filing Date
- 2019-03-20
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2039-03-20
AI Technical Summary
Conventional gravure printing inks suffer from poor storage stability, which is not adequately addressed by existing technologies, and there is a need for improved methods to enhance production efficiency and ink performance.
A modified pigment is developed by coating the surface of pigments with inorganic oxide nanoparticles, such as silica, titania, or alumina, with specific properties like DBP oil absorption, particle size, and pH value, and incorporating it into a radiation-curable gravure printing ink composition with cationically polymerizable compounds and photoinitiators.
The modified pigment effectively prevents aggregation, enhances lipophilicity and wettability, improving the stability and curing speed of the ink, resulting in high storage stability and efficient printing with odor-free, high-quality prints.
Smart Images

Figure 0007556786000019 
Figure 0007556786000015 
Figure 0007556786000010
Abstract
Description
[Technical field]
[0001] The present invention relates to the fields of radiation curing, pigments and inks, and more particularly to modified pigments for use in radiation cured gravure printing inks and their applications. [Background technology]
[0002] Gravure inks, also known as gravure liquid inks, are pigmented colloidal dispersions that can be applied to a substrate by a suitable printing process to impart characters, patterns, and a variety of colors to the substrate.
[0003] Most gravure printing inks are volatile solvent-based inks, and are composed of pigments, solid resins, volatile solvents, fillers, and additives. With the increasing awareness of environmental conservation and energy saving, relatively "environmentally friendly" inks, such as water-based inks, photocurable inks, and electron beam curable inks, have been gradually developed and used as substitutes for solvent inks. For example, Chinese patent applications with application numbers 200580017917.1, 201510267026.7, and 201510994588.1 and US patent application with publication number US2009 / 0136759A disclose energy-curable gravure printing inks that do not contain volatile solvents. However, these conventional techniques mostly focus on the ease of wiping off the ink on the drum of the engraving plate, the appearance of the printed matter, adhesion fastness, abrasion resistance, weather resistance, etc., but there are few descriptions of methods for improving the storage stability and production efficiency of the ink, and there are no effective solutions.
[0004] Pigments are an important component of gravure printing inks, and are dispersed in the ink film as extremely small particles, mainly serving the roles of coloring and hiding. Because a large amount of pigment is added to the ink, it has a significant effect on the storage stability, viscosity, curing speed, and printing performance of the ink. Summary of the Invention [Problem to be solved by the invention]
[0005] The main objective of the present invention is to provide a modified pigment for radiation curable gravure printing inks and its application to solve the problem of poor storage stability of pigment-containing inks in the prior art. [Means for solving the problem]
[0006] In order to achieve the above object, according to one aspect of the present invention, there is provided a modified pigment for use in a radiation-curable gravure printing ink, the modified pigment comprising a pigment and inorganic oxide nanoparticles coated on the surface of the pigment, the modified pigment having a DBP oil absorption of 150 to 250 ml / 100 g, a particle size of 0.01 to 1 μm, and a pH value of 4.5 to 10.
[0007] Furthermore, the inorganic oxide is at least one selected from the group consisting of silica, titania, iron oxide, and alumina.
[0008] Furthermore, the modified pigment has a DBP oil absorption of 200 to 250 ml / 100 g, preferably 215 to 235 ml / 100 g, and a particle size of 0.1 to 0.8 μm, preferably 0.45 to 0.65 μm. Furthermore, the pH value of the modified pigment is 5-9, preferably 5.5-8.
[0009] Furthermore, the pigment is an organic pigment or an inorganic pigment, and preferably, the organic pigment is any one selected from azo dyes, thioindigo dyes, indanthrone dyes, isoindanthrone dyes, anthanthrone dyes, anthraquinone dyes, isoviolanthrone dyes, triphendioxazine dyes, quinacridone dyes, and phthalocyanine dyes, and preferably, the inorganic pigment is any one selected from carbon black, titania, silica, alumina, iron oxide, and sulfide.
[0010] According to another aspect of the present application, there is provided an application of the modified pigment in a radiation curable ink composition. Furthermore, the radiation curable ink composition is used as a gravure printing ink.
[0011] According to a further aspect of the present application there is provided a radiation curable gravure printing ink comprising a pigment which is the modified pigment described above.
[0012] Additionally, the radiation curable gravure printing ink further comprises a cationically polymerizable compound and a cationic photoinitiator.
[0013] Furthermore, the cationic polymerizable compound includes an oxetane compound and an epoxy compound, and preferably, the cationic polymerizable compound is composed of an oxetane compound and an epoxy compound.
[0014] Furthermore, the epoxy compound is an alicyclic epoxy compound, preferably an epoxy compound having an epoxycyclohexyl group.
[0015] Furthermore, the mass ratio of the oxetane compound to the epoxy compound is 2 to 5:1, preferably 2 to 4:1.
[0016] Furthermore, the cationic photoinitiator is one or a combination of two or more selected from iodonium salts, sulfonium salts, and arylferrocene salts. Furthermore, the radiation-curable gravure printing ink contains 2 to 20% by weight, preferably 5 to 15% by weight, of a modified pigment, 40 to 90% by weight, preferably 45 to 80% by weight, more preferably 60 to 80% by weight, of a cationic polymerizable compound, 1 to 25% by weight, preferably 3 to 20% by weight, more preferably 5 to 15% by weight, of a cationic photoinitiator, 0 to 30% by weight, preferably 0 to 20% by weight, of a filler, and 0 to 5% by weight, preferably 0 to 2% by weight, of a sensitizer.
[0017] Additionally, the radiation curable gravure printing ink further comprises a filler.
[0018] Furthermore, the radiation curable gravure printing ink further comprises a sensitizer, preferably the sensitizer is an anthracene-based sensitizer.
[0019] According to a further aspect of the present application there is provided the application of any one of the above radiation curable gravure printing inks to paper, plastic and film. Effect of the Invention
[0020] The technical solution of the present invention can effectively prevent pigment aggregation by coating the pigment surface with inorganic oxide nanoparticles, and the modified pigment has significantly improved oleophilicity and wettability, promotes the stability of the ink dispersion system, and further improves the storage stability of the ink containing the modified pigment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] It should be noted that, unless there is a contradiction, the embodiments and features of the embodiments of the present application can be combined with each other.
[0022] In view of the deficiencies of the prior art and the need for technological development, the main objective of the present invention is to provide a modified pigment for use in radiation curable gravure printing inks, which does not require the use of any volatile organic solvents, thereby greatly improving the storage stability of the ink while ensuring good appearance of the printed matter, excellent adhesion, and no odor, and the ink exhibits excellent curing speed.
[0023] The modified pigment used in the radiation curable gravure printing ink of the present invention comprises a pigment and inorganic oxide nanoparticles coated on the surface of the pigment, and has a DBP oil absorption of 150 to 250 ml / 100 g, a particle size of 0.01 to 1 μm, and a pH value of 4.5 to 10.
[0024] The inventors have surprisingly found that coating the pigment surface with inorganic oxide nanoparticles can effectively prevent pigment aggregation. The modified pigment can significantly improve oleophilicity and wettability, and also promote the stability of the ink dispersion. The oxide is at least one selected from silica, titania, iron oxide, and alumina. The pigment can be an organic pigment or an inorganic pigment. Suitable organic pigments include azo (including bisazo and condensed azo), thioindigo, indanthrone, isoindanthrone, anthranthrone, anthraquinone, isoviolanthrone, triphendioxazine, quinacridone, and phthalocyanine dye series. Preferably, the organic pigment is a phthalocyanine dye (especially copper phthalocyanine pigment), azo pigment, indanthrone, anthanthrone, and quinacridone. Suitable inorganic pigments include carbon black, titania, silica, alumina, iron oxide, and sulfide.
[0025] The inventors conducted experiments and found that the oil absorption and particle size of the modified pigment directly affect the color tone of the printed pattern and the appearance of the printed matter. Measurements in accordance with the GB / T5211.15-1988 standard showed that the DBP oil absorption of the modified pigment is preferably 150-250 ml / 100 g, more preferably 200-250 ml / 100 g, and even more preferably 215-235 ml / 100 g. The appropriate particle size range of the modified pigment is 0.01-1 μm, preferably 0.1-0.8 μm, and even more preferably 0.45-0.65 μm.
[0026] In the conventional gravure printing ink in this field, the pH value of the pigment contained is usually not limited. However, the researchers of the present invention found that when the pigment used has a pH value of ≦4, the ink is easy to gel in the storage tank, shortening the storage time, and when the pigment has a pH value of ≧10, the hardening speed of the ink is obviously reduced. Therefore, the inventors determined the appropriate pH range through multiple experiments and repeated verification, that is, the pH value of the modified pigment is 4.5-10, preferably 5-9, more preferably 5.5-8.
[0027] The pH value of the pigment is affected by the properties of the pigment itself, the surface condition, processing conditions, surface treatment agents, and other factors. In the present invention, the pH value of the modified pigment is determined by measuring the pH value of the solution in which the modified pigment is dispersed in distilled water according to the international GB / T1717-1986. The measurement method specifically includes preparing a 10% by weight (m / m) pigment suspension in a glass container using distilled water, attaching a stopper to the container, shaking vigorously for 1 minute, and then leaving it to stand for 5 minutes, and then removing the stopper and measuring the pH of the suspension to one decimal place.
[0028] As can be seen from the above, in the present application, pigment aggregation can be effectively prevented by coating the pigment surface with inorganic oxide nanoparticles, and the stability of gravure printing ink using this modified pigment can be further improved by controlling the pH value of the modified pigment. In addition, the color tone of the printing pattern formed using this pigment printing and the appearance of the printed matter can be improved by controlling the DBP oil absorption and particle size range of the modified pigment.
[0029] In view of the above-mentioned excellent properties of the modified pigment of the present invention, another object of the present invention is to provide an application of the modified pigment to a radiation-curable ink composition, which is particularly suitable for use as a gravure printing ink.
[0030] In response to this, the present invention provides a radiation-curable gravure printing ink containing the above-mentioned modified pigment (A). The content of the modified pigment relative to the total weight of the gravure printing ink is 2 to 20% by weight, preferably 5 to 15% by weight.
[0031] Particularly preferably, in addition to the above-mentioned modified pigment (A), the radiation-curable gravure printing ink of the present invention further comprises a cationically polymerizable compound (B) and a cationic photoinitiator (C).
[0032] Other components contained in the gravure printing ink are described in more detail below.
[0033] <Cationically polymerizable compound (B)> Cationically polymerizable compounds commonly used in the radiation curing field include oxetane-based compounds, epoxy-based compounds and vinyl ether-based compounds.
[0034] In the gravure printing ink of the present invention, it is advantageous to use an oxetane compound as the cationic polymerizable compound from the viewpoint of obtaining an excellent curing speed. In addition, in consideration of physical properties such as the appearance of the printed matter and adhesion to the substrate, it is preferable to use a combination of the oxetane compound (B1) and the epoxy compound (B2).
[0035] The oxetane compound (B1) that can be used may be a monofunctional compound or a polyfunctional compound. Examples of monofunctional compounds include, but are not limited to, 3-methyl-3-hydroxymethyloxetane, 3-ethyl-3-hydroxymethyloxetane, 3-ethyl-3-(hexyloxymethyl)oxetane, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-[(phenoxy)methyl]oxetane, 3-ethyl-3-(chloromethyl)oxetane, isobutoxymethyl(3-ethyl-3-oxetanylmethyl)ether, isobornyloxyethyl(3-ethyl-3-oxetanylmethyl)ether, isobornyl(3-ethyl-3-oxetanylmethyl)ether, 2-ethylhexyl(3-ethyl-3-oxetanylmethyl)ether, and ethyldiethyleneglycol(3-ethyl-3-oxetanylmethyl)ether.Examples of polyfunctional ones include bis[1-ethyl(3-oxetanyl)]methyl ether, 3,3-bis(chloromethyl)oxetane, 3,7-bis(3-oxetanyl)-5-oxa-nonane, 1,2-bis[(3-ethyl-3-oxetanylmethoxy)methyl]ethane, 1,3-bis[(3-ethyl-3-oxetanylmethoxy)methyl]propane, ethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, tricyclodecanediyldimethylene(3-ethyl-3-oxetanylmethyl)ether, trimethylolpropane tris(3-ethyl-3-oxetanylmethyl)ether, 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, Examples of the ether esters include, but are not limited to, 1,4-bis(3-ethyl-3-oxetanylmethoxy)butane, 1,6-bis(3-ethyl-3-oxetanylmethoxy)hexane, pentaerythritol tris(3-ethyl-3-oxetanylmethyl)ether, pentaerythritol tetra(3-ethyl-3-oxetanylmethyl)ether, polyethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, dipentaerythritol hexa(3-ethyl-3-oxetanylmethyl)ether, dipentaerythritol penta(3-ethyl-3-oxetanylmethyl)ether, dipentaerythritol tetra(3-ethyl-3-oxetanylmethyl)ether, and the like. Additionally, the oxetane-based compounds disclosed in Chinese patent applications having application numbers 201610548580.7, 201610550205.6, 201710706339.7 and 201710622973.2, the entire contents of which are incorporated herein by reference, may also be used in the composition.
[0036] In view of overall application performance, the oxetane compound (B1) is more preferably at least one selected from the following compounds:
[0037] TIFF0007556786000001.tif120170
[0038] The epoxy compound (B2) that can be used may be at least one selected from an alicyclic epoxy compound, a hydrogenated epoxy compound, an aromatic epoxy compound, and an aliphatic epoxy compound, and is preferably an alicyclic epoxy compound.
[0039] The "alicyclic epoxy compound" described in this specification refers to a compound having an alicyclic epoxy group. In order to further improve the curing speed, a polyfunctional alicyclic epoxy compound having two or more alicyclic epoxy groups in the molecule, or an alicyclic epoxy compound having one alicyclic epoxy group in the molecule and an unsaturated double bond group such as a vinyl group can be used.
[0040] As the alicyclic epoxy compound that can be used in the gravure printing ink of the present invention, an epoxy compound having an epoxycyclohexyl group is preferable, and examples thereof include 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, ε-caprolactone-modified-3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, di((3,4-epoxycyclohexyl)methyl)adipate, epoxycyclohexane, 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane, 3,4-epoxycyclohexylmethylmethacrylate, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane ... acrylate, 3,4-epoxycyclohexylmethyl acrylate, 1,2-epoxy-4-vinylcyclohexane, 4-vinyl-1-cyclohexene diepoxide, bicyclononadiene diepoxide, 3,4-epoxycyclohexane carboxylate, polymerization products of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexyl formate and caprolactone, 4-methyl-1,2-epoxycyclohexane, 2,2-bis(3,3'-epoxycyclohexyl)propane, 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane, and the like.
[0041] As the hydrogenated epoxy compound, a compound having a glycidyl ether group directly or indirectly bonded to a saturated aliphatic cyclic hydrocarbon skeleton is preferred, and a polyfunctional glycidyl ether compound is suitable. Such a hydrogenated epoxy compound is preferably a fully or partially hydrogenated aromatic epoxy compound, more preferably a hydrogenated aromatic glycidyl ether compound, and even more preferably a hydrogenated aromatic polyfunctional glycidyl ether compound. Specifically, it can be selected from hydrogenated bisphenol A type epoxy compounds, hydrogenated bisphenol S type epoxy compounds, hydrogenated bisphenol F type epoxy compounds, etc. More preferably, it is hydrogenated bisphenol A type epoxy compounds or hydrogenated bisphenol F type epoxy compounds.
[0042] The aromatic epoxy compound is a compound having an aromatic ring and an epoxy group in the molecule. The aromatic epoxy compound may be an epoxy compound having an aromatic ring conjugated system such as a bisphenol skeleton, a fluorene skeleton, a biphenyl skeleton, a naphthalene ring, or an anthracene ring. In order to achieve a higher refractive index, a compound having a bisphenol skeleton and / or a fluorene skeleton is preferred, and a compound having a fluorene skeleton is more preferred, thereby further improving the refractive index and further improving the mold releasability. In addition, a compound in which the epoxy group in the aromatic epoxy compound is a glycidyl group is preferred, and a compound in which the epoxy group is a glycidyl ether group (i.e., an aromatic glycidyl ether compound) is more preferred. In addition, since a higher refractive index can be achieved, it is also suitable to use a bromide of an aromatic epoxy compound, but since the Abbe number is slightly improved, it is preferably used according to the application.
[0043] Preferred examples of the aromatic epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, fluorene type epoxy compounds, aromatic epoxy compounds having a bromine substituent, etc. Among them, bisphenol A type epoxy compounds and fluorene type epoxy compounds are more preferred.
[0044] The aromatic glycidyl ether compound may be an Epi-bis type glycidyl ether type epoxy resin, a high molecular weight Epi-bis type glycidyl ether type epoxy resin, a novolak, an aralkyl type glycidyl ether type epoxy resin, or the like.
[0045] The epi-bis type glycidyl ether type epoxy resin can be a resin obtained by a condensation reaction between a bisphenol such as bisphenol A, bisphenol F, bisphenol S, or fluorene bisphenol and epihalohydrin.
[0046] The high molecular weight Epi-bis glycidyl ether type epoxy resin can be a resin obtained by further addition reaction of the above-mentioned Epi-bis glycidyl ether type epoxy resin with a bisphenol such as the above-mentioned bisphenol A, bisphenol F, bisphenol S, or fluorene bisphenol.
[0047] Preferred examples of the aromatic glycidyl ether compound include, but are not limited to, bisphenol A type compounds such as 828EL, 1003, and 1007 manufactured by Nippon Epoxy Resins Co., Ltd., and fluorene type compounds such as ONCOATEX-1020, ONCOATEX-1010, OGSOLEG-210, and OGSOLPG manufactured by Osaka Chemicals Co., Ltd. Among them, OGSOLEG-210 is particularly preferred.
[0048] The aliphatic epoxy compound is a compound having an aliphatic epoxy group, for example, an aliphatic glycidyl ether type epoxy resin. Preferred examples of the aliphatic glycidyl ether type epoxy resin include, but are not limited to, resins obtained by condensation reaction of a polyhydroxy compound with epihalohydrin. The polyhydroxy compound may be selected from ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, polypropylene glycol, glycerin, diglycerin, tetraglycerin, polyglycerin, trimethylolpropane and its multimer, pentaerythritol and its multimer, monosaccharides / polysaccharides (for example, glucose, fructose, lactose, maltose, etc.), etc. Among them, an aliphatic glycidyl ether type epoxy resin having a propylene glycol skeleton, an alkylene skeleton, or an alkylene oxide skeleton in the central skeleton is more suitable.
[0049] Examples of the vinyl ether compound include, but are not limited to, aryl vinyl ethers such as phenyl vinyl ether; alkyl vinyl ethers such as n-butyl vinyl ether and n-octyl vinyl ether; cycloalkyl vinyl ethers such as cyclohexyl vinyl ether; hydroxy-containing vinyl ethers such as 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether and 2-hydroxybutyl vinyl ether; and polyfunctional vinyl ethers such as hydroquinone divinyl ether, 1,4-butanediol divinyl ether, cyclohexane divinyl ether, cyclohexane dimethanol divinyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether and triethylene glycol divinyl ether.
[0050] In addition to the above, compounds having different kinds of cationic polymerizable groups in the molecule can also be used as cationic polymerizable compounds.For example, as an example of the compound having both epoxy group (e.g., alicyclic epoxy group) and vinyl ether group in the molecule, the compound described in JP-A-2009-242242 can be used; as an example of the compound having both oxetanyl group and vinyl ether group in the molecule, the compound described in JP-A-2008-266308 can be used.
[0051] The content of the cationic polymerizable compound of component (B) in the gravure printing ink can be appropriately adjusted depending on the type and performance of the substrate, and is suitably 40 to 90% by weight, preferably 45 to 80%, and more preferably 60 to 80% by weight. The mass ratio of the oxetane compound (B1) to the epoxy compound (B2) is preferably 2 to 5:1, and more preferably 2 to 4:1.
[0052] <Cationic Photoinitiator (C)> The cationic photoinitiator of component (C) can be one or a combination of two or more selected from iodonium salts, sulfonium salts, and arylferrocene salts.
[0053] Considering a number of factors, such as the composition and the effects of using the component in combination, for example, photoinitiation efficiency and curing speed, component (C) is preferably an iodonium salt and / or sulfonium salt photoinitiator, for example, TIFF0007556786000002.tif116170, or selected from compounds having the structures shown in the following formulas (I), (II), (III) and / or (V).
[0054] TIFF0007556786000003.tif90170
[0055] In the formula, R1 and R2 are each independently hydrogen, C1-C 20 Straight or branched alkyl groups, C4-C 20In these groups, the non-cyclic -CH2- may be optionally substituted by -O-, -S- or 1,4-phenylene group.
[0056] R3 and R4 are each independently hydrogen, C1-C 20 Straight or branched alkyl groups, C4-C 20 Cycloalkylalkyl or alkylcycloalkyl groups of the formula C6-C 20 In these groups, the non-cyclic -CH2- may be unforcibly replaced by -O-, -S- or 1,4-phenylene groups.
[0057] R5 is C6-C 20 substituted or unsubstituted aryl groups, C6-C 20 substituted or unsubstituted alkylaryl groups, C1-C 20 Straight or branched alkyl groups, C4-C 20 and a substituted or unsubstituted phenylthiophenyl group, in which the non-cyclic -CH2- may be unforcibly substituted by a carbonyl group, -O-, -S- or 1,4-phenylene group.
[0058] R6 and R7 each independently represent an alkyl group, a hydroxy group, an alkoxy group, an alkylcarbonyl group, an arylcarbonyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an arylthiocarbonyl group, an acyloxy group, an arylthio group, an aryl group, a heterocyclic hydrocarbon group, an aryloxy group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, a hydroxy(poly)alkyleneoxy group, a substitutable amino group, a cyano group, a nitro group, or a halogen atom.
[0059] m1 and m2 each represent the number of R6 and R7 and are selected from 0, 1, 2, 3, or 4.
[0060] X -are each independently - , ClO4 - , C.N. - , HSO4 - , NO3 - , CF3COO - , (BM4) - , (SbM6) - , (AsM6) - , (PM6) - , Al[OC(CF3)3]4 - , sulfonate radical ion, B(C6M5)4 - or [(Rf) b PF 6-b ] - wherein M represents a halogen (for example, F, Cl, Br, I), each Rf independently represents an alkyl group in which 80% or more of the hydrogen atoms are substituted with fluorine atoms, and b represents an integer of 1 to 5.
[0061] MtXn - is BF4 - , ClO4 - , FSO3 - , PF6 - , ASF6 - , SbF6 - , CF3SO3 - , (C6H5)4B - and other non-nucleophilic anions.
[0062] As a preferred structure, in the compounds of the structures shown in formula (I) and (II), R1 and R2 are each independently hydrogen, C1-C 12 Straight or branched alkyl groups, C4-C 10 In these groups, the non-cyclic -CH2- may be unnecessarily replaced by -O-; R3 and R4 are each independently hydrogen, C1-C 10 Straight or branched alkyl groups, C4-C 10 Cycloalkylalkyl or alkylcycloalkyl groups of the formula C6-C 12In these groups, the acyclic -CH2- may be unforcibly replaced by -O-, -S- or 1,4-phenylene groups; R5 is C6-C 10 substituted or unsubstituted aryl groups, C6-C 10 and a substituted or unsubstituted alkylaryl group, a substituted or unsubstituted phenylthiophenyl group, among these groups, 2- may be unforcibly substituted by a carbonyl group, -O-, -S- or 1,4-phenylene group; R6 and R7 are C1-C 10 Straight or branched alkyl groups, C1-C 10 Linear or branched alkoxy groups, C1-C 10 The alkylcarbonyl group and halogen are shown.
[0063] More preferably, the cationic moiety of the iodonium salt and sulfonium salt photoinitiators has the following structure:
[0064] TIFF0007556786000004.tif225170
[0065] TIFF0007556786000005.tif254170
[0066] More preferably, the anion moiety of the iodonium salt and sulfonium salt photoinitiators is Cl. - , Br - , PF6 - , SbF6 - , AsF6 - , BF4 - , C4F9SO3 - , B(C6H5)4 - , C8F 17 SO3 - , CF3SO3 - , Al[OC(CF3)3]4 - , (CF3CF2)2PF4 - , (CF3CF2)3PF3 - , [(CF3)2CF2]2PF4 - , [(CF3)2CF2]3PF3- , [(CF3)2CFCF2]2PF4 - , (CF3)2CFCF2]3PF3 - Examples include:
[0067] Commercially available cationic photoinitiators having the same structure, such as PAG20001, PAG20002, PAG30201, PAG30101, etc. manufactured by Changzhou Strong Electronic New Materials Co., Ltd., Irgacure 250 manufactured by BASF, Germany, etc. (but not limited thereto) can also be used in component (C) of the present invention.
[0068] The content of the cationic photoinitiator (C) in the gravure printing ink of the present invention is from 1 to 25 mass %, preferably from 3 to 20 mass %, and more preferably from 5 to 15 mass %.
[0069] <Filler (D)> Non-compulsorily, the radiation curable gravure printing ink of the present invention further contains a filler (D). There is no particular limitation on the type of filler of component (D), and any type commonly used in gravure printing inks can be used. Typically, the filler is at least one selected from nano calcium carbonate, aluminum hydroxide, barium sulfate, silica, talcum powder, and kaolin.
[0070] The content of component (D) in the gravure printing ink is 0 to 30% by mass, preferably 0 to 20% by mass.
[0071] <Other optional ingredients> In addition to the above components (A) to (D), depending on the needs of the product's usage environment, the gravure printing ink of the present invention may optionally contain organic and / or inorganic auxiliaries commonly used in this field, including, but not limited to, leveling agents, dispersants, curing agents, surfactants, defoamers, storage improvers, etc., which can be easily determined by those skilled in the art. The total content of the auxiliaries is 0 to 5% by mass, preferably 0 to 3% by mass.
[0072] Furthermore, a sensitizer may be added to the system to increase the photosensitivity of the gravure printing ink. In particular, when the radiation source is an LED, there is a tendency to add a sensitizer to the gravure printing ink. The type of sensitizer may be a pyrazoline-based compound, an acridine-based compound, an anthracene-based compound, a naphthalene-based compound, a coumarin-based compound, a tertiary amine-based compound, or the like. As the anthracene-based sensitizer compound, a compound having a structure represented by the following formula (III) and / or (IV) is particularly preferred.
[0073] TIFF0007556786000006.tif87170
[0074] In the general formula (III), R8 is C1-C 12 Alkyl groups, C1-C 12 Aryl group, C1-C8 alkoxy group or aryloxy group, C3-C 12 Cycloalkyl groups, C4-C 12 wherein one or more hydrogen atoms in these groups may be substituted by halogen or a hydroxy group; and X1 and Y1 each independently represent a hydrogen atom, an alkyl group, an alkoxy group, a halogen atom, a nitro group, a sulfonic acid group, a hydroxy group, or an amine group.
[0075] In the general formula (IV), R9 is C1-C 12 Alkyl groups, C1-C 12 Aryl group, C1-C8 alkoxy group or aryloxy group, C3-C 12 Cycloalkyl groups, C4-C 12 represents an alkylcycloalkyl group or a cycloalkylalkyl group, one or more hydrogen atoms of which may be substituted by a halogen or a hydroxyl group; n1 and n2 each independently represent an integer of 0 to 4; X2 and Y2 are the same or different and each independently represent a hydrogen atom, an alkyl group, an alkoxy group, a halogen atom, a nitro group, a sulfonic acid group, a hydroxyl group, or an amine group; and when n1 and n2 each represent 2 or more, X2 and Y2 are the same or different.
[0076] As an example, the anthracene-based compound can be one or a combination of more of the compounds shown below.
[0077] TIFF0007556786000007.tif254170
[0078] The content of the sensitizer in the gravure printing ink is from 0 to 5% by mass, and preferably from 0 to 2% by mass.
[0079] The gravure printing ink of the present invention can achieve quick drying by undergoing a polymerization reaction when irradiated with energy such as ultraviolet light, visible light, infrared light, electron beam, laser, etc. The light source for imparting energy is preferably one having a dominant wavelength in the range of 250 to 450 nm, and examples thereof include various light sources such as an ultra-high pressure mercury lamp, a high pressure mercury lamp, a medium pressure mercury lamp, a mercury xenon lamp, a metal halide lamp, a high power metal halide lamp, a xenon lamp, a pulsed xenon lamp, a deuterium lamp, an LED lamp, a fluorescent lamp, a Nd-YAG tripled wave laser, a He-Cd laser, a nitrogen laser, a Xe-Cl excimer laser, a Xe-F excimer laser, and a semiconductor pumped solid state laser.
[0080] The radiation-curable gravure printing ink of the present invention is obtained by uniformly mixing each compounding component, and the specific preparation process can be referred to a conventional method in the field of radiation-curable compositions. Typically, the preparation process includes modifying the pigment, and then blending, pre-dispersing, grinding, and filtering (filtering through a filter mesh of a specified size to obtain a product with a desired particle size) under conditions of constant temperature and humidity and in the absence of a radiation source.
[0081] The radiation-curable gravure printing ink of the present invention has excellent storage stability, is capable of high-speed printing, has high production efficiency, can be applied to the surfaces of a variety of substrates, particularly paper, plastic, film and other printed materials, and the printed materials produced have good appearance, strong adhesion, are odorless, and have strong market competitiveness.
[0082] The present invention will now be described in further detail with reference to specific examples, which should not be construed as limiting the scope of the invention.
[0083] 1. Preparation of modified pigments (1) Inorganic modified pigments Carbon black a-1 (Mitsubishi Chemical Corporation, MA100) was dried at 60-70℃ for 3 hours, then ground in a mortar until the average particle size was about 0.3μm. Then, 100g of carbon black was weighed and added to a 1L flask, 800ml of deionized water was added, and the mixture was stirred and ultrasonically dispersed to obtain a uniform suspension.
[0084] The suspension was heated to about 65°C in a thermostatic water bath and kept at that temperature, and the pH value was adjusted to 9.
[0085] Weigh out 11.8 g of Na2SiO3·9H2O and dissolve it in 110 ml of water to make a solution, which is then slowly dripped into the flask and 10% hydrochloric acid is added dropwise while stirring at a constant speed to adjust the pH value to the range of 4 to 9. After the dripping is complete, the mixture is stirred at a constant temperature for 30 min.
[0086] After the reaction was completed, the suspension was filtered, washed with deionized water, and dried at 105° C. for 20 minutes. It was confirmed by TEM detection that a black modified pigment A-1 coated with silica was obtained.
[0087] As a result of the measurements, the modified pigment A-1 had a DBP oil absorption value of 220 ml / 100 g, an average particle size of 0.46 μm (TEM measurement), and a pH value of 8.
[0088] Carbon black a-1 was replaced with another type of inorganic pigment, and the same oxide coating modification treatment was carried out according to the preparation method of A-1 to obtain the corresponding modified pigment, as shown in the table below.
[0089] [Table 1]
[0090] (2) Organically modified pigments Mix 150g of 20% by weight calcium chloride solution, 40g of anhydrous ethanol, and 20g of 10% by weight hydrochloric acid solution, then stir at 350r / min for 30min, add 30g of nanosilica, and ultrasonically disperse for 30min to obtain a dispersion, introduce carbon dioxide gas into the dispersion until no more precipitation occurs, leave for 8-10h, filter to obtain a filter cake, wash the filter cake 3-5 times with deionized water, put in an oven, and dry at 105-110℃ until it reaches a constant (unchanging) weight to obtain an ink absorbing matrix.
[0091] 10 g of the ink absorbing matrix and 20 g of CI Pigment Blue 61 (a-3) were added to 400 g of 5% by mass sodium carbonate solution, and the mixture was stirred at 350 rpm for 24 hours in a constant temperature water bath at 45°C to obtain a supporting solution.
[0092] 100 g of tetrabutyl titanate, 1 to 2 g of silane coupling agent KH-560, and 200 ml of deionized water were added to the support liquid, mixed uniformly, and then stirred at 350 rpm for 5 hours in a constant temperature water bath at 90°C to obtain a titania-coated organic pigment mixture.
[0093] The coated organic pigment mixture was put into a hydrothermal reactor, kept at 110°C for 5 hours, cooled to room temperature, filtered to obtain a filter cake, washed twice with deionized water, put into an oven and dried at 105°C to a certain weight, and the dried product was ground in a grinder to obtain organic modified pigment A-3. TEM detection confirmed that this organic modified pigment A-3 had a core-shell coated structure.
[0094] As a result of the measurements, the modified pigment A-3 had a DBP oil absorption value of 225 ml / 100 g, an average particle size of 0.56 μm, and a pH value of 5.5.
[0095] A-3 was replaced with another type of organic pigment, and the same oxide coating modification treatment was carried out according to the preparation method of A-3 to obtain the corresponding modified pigment, as shown in the table below.
[0096] [Table 2]
[0097] 2. Preparation of radiation-curable gravure printing ink According to the recipe shown in Table 3, the raw materials were stirred at a constant speed for 1 hour using a high-speed stirrer under yellow light conditions, then ground using a sand grinder and filtered through a 1 μm particle size filter to obtain a radiation-curable gravure printing ink. Unless otherwise specified, the amounts given in each example are parts by weight.
[0098] [Table 3]
[0099] In Table 3, the specific definitions of each component are as follows: Modified pigment: Same as the definition given in "1. Preparation of modified pigment".
[0100] TIFF0007556786000011.tif186170
[0101] B2-1: 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, manufactured by Jiangsu Tetra New Material Technology Co., Ltd.; B2-2: di((3,4-epoxycyclohexyl)methyl)adipate, manufactured by Jiangsu Taiter New Materials Technology Co., Ltd.; B2-3: 4-vinyl-1-cyclohexene diepoxide;
[0102] C-1: a mixed salt of bis(4-diphenylsulfonium)phenyl)sulfide bis(hexafluorophosphate) and diphenyl[4-(phenylthio)phenyl]sulfonium hexafluorophosphate, manufactured by Changzhou Tronly New Electronic Materials Co., Ltd.;
[0103] TIFF0007556786000012.tif182170
[0104] D-1: Silica A-200, manufactured by Evonik Degussa Specialty Chemicals, Germany; D-2: Titanium dioxide powder R706, manufactured by DuPont, USA; D-3: Calcium carbonate SW-01, manufactured by Nippon Houri Co., Ltd.;
[0105] TIFF0007556786000013.tif236170
[0106] E2: BYK 333, Evonik Degussa Specialty Chemicals, Germany; E3: Stabilizer hindered nitroxyl TIFF0007556786000014.tif74170
[0107] 3. Gravure printing ink performance testing and evaluation The printing was carried out using a Shotoku Co., Ltd. solvent-free gravure printing press (model: A380) equipped with an LED lamp with a wavelength of 395 nm as a radiation source.
[0108] The samples of the examples and comparative examples were tested and evaluated for performance in accordance with the industry standard QBT 1046-2012 for gravure plastic film surface printing inks.
[0109] (1) Storage stability test The storage stability of the ink under test was measured according to GB-T 6753.3-1986 ink storage stability test method. The ink was placed in a 50℃ oven and the ink viscosity was measured after 7 days. The evaluation grades are as follows: ○: Viscosity increase rate is 5% or less ◎: Viscosity increase rate is greater than 5% and less than 10% ●: Viscosity increase rate is greater than 10%.
[0110] (2) Hardening and drying speed test The ink to be tested was transferred to a PET film with a thickness of approximately 10 μm using an A380 gravure printer. Wavelength 395 nm, intensity 15 w / cm 2 The LED light source was used to evaluate the surface cure, using the finger touch method described in the coating drying time test standard GB / T 1728-1979, that is, when the coating is lightly touched with a finger, the surface is judged to be dry if it is smooth, non-sticky, and does not leave a fingerprint when pressed.
[0111] The drying rate is expressed as the maximum linear velocity (unit: m / min) required to achieve a surface drying effect. The evaluation results are summarized in Table 4.
[0112] 4. Performance testing and evaluation of printed matter The gravure printing ink was printed on a PET film substrate at a thickness of approximately 10 μm under the minimum linear speed condition at which the gravure printing ink can completely harden and dry (Example: 180 m / min, Comparative Example: 120 m / min). After leaving it for 24 hours, the physical properties of the print, i.e., the cured coating, such as adhesion fastness, appearance of the print, and residual odor, were tested and evaluated.
[0113] (1) Adhesion fastness test The test was conducted according to the GB / T 13217.7-91 gravure printing ink inspection standard. The specific method was to attach a tape conforming to the GB 7707 standard to the ink-printed surface under the conditions of 25±1℃ and 65%±5% humidity, and roll-press three times with a tape roller. After leaving it for 5 minutes, the test piece was clamped to disk A, and the tape exposed from the test piece was fixed to disk B, and then the device was started, disk A was rotated at a speed of 0.6-1.0 m / s to peel off the tape, and the part after the tape peeling was covered with a 20 mm wide semi-transparent millimeter graph paper. The number of grids occupied by the ink layer and the number of grids occupied by the ink layer that had been peeled off were counted and calculated using the following formula. A(%)=[A1 / (A1+A2)]×100%
[0114] (In the formula, A represents the adhesion fastness of the ink, A1 represents the number of grids in the ink layer, and A2 represents the number of grids in the ink layer that have been peeled off.) A ≥ 90 is considered to satisfy the performance index.
[0115] (2) Appearance test of printed matter The test was conducted in accordance with the GB / T 7707-2008 decorative gravure print standard, and the specific method was to place the print under the observation light source specified in CY / T 3 and visually inspect it. The print was deemed to pass if it was neat and clean, had no obvious ink stains, tailing, missing prints, doctor marks, smooth edges, uniform ink color, no obvious water ripples, no obvious deformations or missing prints, and failed in any other case.
[0116] (3) Residual odor test The freshly cured product was placed in a sealed bag and left in the sealed bag at room temperature for 24 hours, after which the bag was opened and judged by human smell. The evaluation grades are as follows: ○: No obvious odor ×: Has a pungent odor. The evaluation results are summarized in Table 4.
[0117] [Table 4]
[0118] From the evaluation results in Table 4, it can be seen that the gravure printing ink using modified pigments has significantly improved storage stability and is advantageous in increasing the ink curing speed. The coating adhesion is good, the printing pattern is clean, the edges are smooth, the ink color is uniform, and the product has no obvious odor.
[0119] In addition, the initiators in the components of Examples 2 and 3 were When the composition was changed to TIFF0007556786000016.tif34170, the same technical effect was obtained under the same preparation and test conditions.
[0120] 5. Further performance testing and evaluation The radiation-curable gravure printing inks containing the modified pigment of the present invention were applied to paper and plastic film substrates, respectively, to further verify their application performance.
[0121] (1)Paper base material With reference to the requirements for substrates and test methods in GB / T 26461-2011 gravure paper printing ink evaluation standard, the performance of the radiation curable gravure printing ink of the present invention when applied on paper substrate was evaluated.
[0122] A gravure printing ink composition was prepared according to the formulation in Table 5. The ink was printed on offset paper conforming to GB / T 10335.1 using a Shotoku solvent-free gravure printing machine (model: A380) with a wavelength of 395 nm and a light source intensity of 15 w / cm. 2 A LED lamp was used as the radiation source, and a printed pattern with a thickness of approximately 10 μm was obtained.
[0123] The storage stability, curing and drying speed, adhesion fastness of the coating, and appearance and odor of the printed matter were evaluated with reference to the above-mentioned evaluation methods. The test results are summarized in Table 5.
[0124] [Table 5]
[0125] In addition, the initiator in the formulation in Table 5 above is When the formula was changed to TIFF0007556786000018.tif41170, the same technical effect was obtained under the same preparation and test conditions.
[0126] (2) Plastic film substrate Referring to the requirements for substrates and test methods in QB / T 1046-2012 Gravure Plastic Film Surface Printing Ink Evaluation Standard, the performance of the radiation curable gravure printing ink of the present invention when applied to various plastic film substrates was evaluated separately.
[0127] A gravure printing ink composition was prepared according to the formulation in Table 6. The ink was printed on PET, PVC, PP and PE substrates using a Shotoku solvent-free gravure printer (Model: A380) with a wavelength of 395 nm and a light source intensity of 15 w / cm. 2 A LED light was used as the radiation source, resulting in a printed pattern with a thickness of approximately 10 μm.
[0128] Referring to the above evaluation methods, the storage stability, curing and drying speed, adhesion fastness of the coating to various plastic and film substrates, and appearance and odor of the printed matter of the ink composition were evaluated. The test results are summarized in Table 6.
[0129] [Table 6]
[0130] The initiator in the formulation in Table 6 above is When the composition was changed to one of the above-mentioned TIFF0007556786000020.tif49170, the same technical effect was obtained under the same preparation and test conditions.
[0131] Therefore, from the test results in Tables 5 and 6, it can be seen that the radiation-curable gravure printing ink containing the modified pigment of the present invention can be applied to the surfaces of various substrates and has excellent usability in all cases.
[0132] The preparation and testing process of Example 1 was repeated for each example radiation curable gravure printing ink in Table 7, and the test results are shown in Table 8. The amounts of each component in the examples in Table 7 are weight percentages.
[0133] [Table 7]
[0134] [Table 8]
[0135] The above is merely a preferred embodiment of the present invention, and is not intended to limit the present invention, and those skilled in the art can make various modifications and changes to the present invention. Any modifications, equivalent replacements, improvements, etc. made without departing from the spirit and principle of the present invention should be included in the patent scope of the present invention.
Claims
1. 1. A modified pigment for use in a radiation curable gravure printing ink comprising: A modified pigment comprising a pigment and inorganic oxide nanoparticles coated on the surface of the pigment, the modified pigment having a DBP oil absorption of 150 to 250 ml / 100 g, a particle size of 0.01 to 1 μm, and a pH value of 4.5 to 10.
2. 2. The modified pigment according to claim 1, wherein the inorganic oxide is at least one selected from the group consisting of silica, titania, iron oxide, and alumina.
3. 2. The modified pigment according to claim 1, wherein the DBP oil absorption is 200 to 250 ml / 100 g and the particle size is 0.1 to 0.8 μm.
4. The modified pigment according to claim 3, characterized in that the DBP oil absorption is 215 to 235 ml / 100 g.
5. The modified pigment according to claim 3, characterized in that the particle diameter is 0.45 to 0.65 μm.
6. 2. The modified pigment according to claim 1, characterized in that the pH value is between 5 and 9.
7. The modified pigment according to claim 6, characterized in that the pH value is 5.5 to 8.
8. The modified pigment according to any one of claims 1 to 6, characterized in that the pigment is an organic pigment or an inorganic pigment.
9. The modified pigment according to claim 8, wherein the organic pigment is any one selected from the group consisting of azo dyes, thioindigo dyes, indanthrone dyes, isoindanthrone dyes, anthanthrone dyes, anthraquinone dyes, isoviolanthrone dyes, triphendioxazine dyes, quinacridone dyes and phthalocyanine dyes.
10. 9. The modified pigment according to claim 8, wherein the inorganic pigment is any one selected from the group consisting of carbon black, titania, silica, alumina, iron oxide and sulfide.
11. 1. A pigmented radiation curable gravure printing ink comprising: A radiation-curable gravure printing ink, characterized in that the pigment is a modified pigment according to any one of claims 1 to 10.
12. 12. A radiation curable gravure printing ink according to claim 11, further comprising a cationically polymerizable compound and a cationic photoinitiator.
13. 13. The radiation curable gravure printing ink according to claim 12, wherein the cationically polymerizable compound comprises an oxetane compound and an epoxy compound.
14. 14. The radiation curable gravure printing ink of claim 13, wherein the epoxy compound is a cycloaliphatic epoxy compound.
15. The radiation-curable gravure printing ink according to claim 14, characterized in that the epoxy compound is an epoxy compound having an epoxycyclohexyl group.
16. 16. The radiation-curable gravure printing ink according to claim 13, wherein the mass ratio of the oxetane compound to the epoxy compound is 2-5:
1.
17. The radiation-curable gravure printing ink according to claim 16, characterized in that the mass ratio of the oxetane compound to the epoxy compound is 2-4:
1.
18. 13. The radiation-curable gravure printing ink according to claim 12, wherein the cationic photoinitiator is one or a combination of two or more selected from the group consisting of iodonium salts, sulfonium salts and arylferrocene salts.
19. 2 to 20% by weight of the modified pigment; 40 to 90% by weight of the cationically polymerizable compound; 1 to 25% by weight of the cationic photoinitiator; 0 to 30% by weight of a filler; 16. A radiation curable gravure printing ink according to claim 12, further comprising 0 to 5% by weight of a sensitizer.
20. The composition comprising: 5 to 15% by weight of the modified pigment; 45 to 80% by weight of the cationically polymerizable compound; 3 to 20% by weight of the cationic photoinitiator; 0 to 20% by weight of a filler; 20. A radiation curable gravure printing ink according to claim 19, comprising 0-2% by weight of a sensitizer.
21. The composition comprising: 5 to 15% by weight of the modified pigment; 60 to 80% by weight of the cationically polymerizable compound; 5 to 15% by weight of the cationic photoinitiator; 0 to 20% by weight of a filler; 20. The radiation curable gravure printing ink of claim 19, further comprising 0-2% by weight of a sensitizer.
22. 20. The radiation curable gravure printing ink of claim 19 further comprising a filler.
23. 20. The radiation curable gravure printing ink of claim 19 further comprising a sensitizer.
24. 24. A radiation curable gravure printing ink according to claim 23, wherein the sensitizer is an anthracene based sensitizer.
25. Application of the radiation-curable gravure printing ink according to any one of claims 11 to 24 to paper, plastics and films.
Citation Information
Patent Citations
Metallic pigment and ultraviolet-curable composition obtained by compounding the same
JP2011137083A
Titanium dioxide pigment and method for producing the same, and printing ink composition
JP2016000836A