Photosensitive resin composition and its uses

The photosensitive resin composition addresses storage stability and substrate adhesion issues by incorporating specific components, enabling fine pattern formation and high adhesion to glass substrates, suitable for color filters in display devices.

JP7556810B2Active Publication Date: 2024-09-26NIPPON SHOKUBAI CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021049550
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-24
Publication Date
2024-09-26
Estimated Expiration
2041-03-24

AI Technical Summary

Technical Problem

Existing photosensitive resin compositions used in photolithography for image display devices face challenges with storage stability and substrate adhesion when ultraviolet absorbers are added, leading to issues such as pixel peeling or chipping and reduced storage stability, especially during fine pattern formation.

Method used

A photosensitive resin composition containing an alkali-soluble resin, polymerizable monomer, coloring material, photopolymerization initiator, ultraviolet absorber, and solvent, with specific structural units and components that enhance storage stability and substrate adhesion, including the use of an oxime-based initiator and ultraviolet absorbers like benzotriazole and benzophenone compounds.

Benefits of technology

The composition achieves reduced viscosity change during storage, allows for fine pattern formation with high adhesion to glass substrates, and is suitable for color filters in display devices, improving storage stability and substrate adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556810000009
    Figure 0007556810000009
  • Figure 0007556810000012
    Figure 0007556810000012
  • Figure 0007556810000010
    Figure 0007556810000010
Patent Text Reader

Abstract

To provide: a photosensitive resin composition capable of reducing viscosity change during storage and providing a cured product having small line thickening and high adhesion to a glass substrate, etc.; a cured film obtained by applying such a photosensitive resin composition to a base material and curing the same; a display member capable of achieving high color purity and high brightness by including the cured film; and a display.SOLUTION: A photosensitive resin composition includes an alkali soluble resin, a polymerizable monomer, a color material, a photoinitiator, an ultraviolet absorbent and a solvent. The alkali soluble resin has a specific structure having a hetero ring in a main chain; the photosensitive resin composition preferably has a viscosity change rate of 120% or less after being stored at 40°C for 65 hours; and the content of water is more preferably 0.14 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition and uses thereof, and more preferably to a photosensitive resin composition containing a colorant, a cured product thereof, and a color filter. [Background technology]

[0002] Photosensitive resin compositions are used in photolithography, and are materials whose solubility in a developer changes depending on the presence or absence of exposure, and can be used to obtain a cured product in a predetermined pattern. Photolithography is used in the manufacture of components for image display devices, the manufacture of circuit boards for electronic devices, the manufacture of semiconductor elements, and the like. In these technical fields, it is required that the cured product be obtained in a fine pattern, and that the cured product have high adhesion to the substrate. One of the uses of the photosensitive resin composition is a material for a color filter used in an image display device such as a liquid crystal display device. A color filter is usually produced by applying a photosensitive resin composition containing a color material such as a pigment and a photocurable monomer or resin to a transparent substrate, followed by photolithography or the like. In recent years, with the demand for miniaturization and high performance of image display devices, a photosensitive resin composition capable of forming a color filter formed with a fine pixel pattern is required so as to contribute to the improvement of brightness, contrast, etc. In order to make the pixel pattern finer, it is effective to add an ultraviolet absorber, but when the pixel pattern is created, the ultraviolet absorber absorbs the exposure energy, so that the deep part is not sufficiently exposed to light, and pixel peeling or pixel loss of R, G, and B pixels occurs during development, or the storage stability of the photosensitive resin composition is reduced by the addition of the ultraviolet absorber. In order to solve the above problems, a curable resin composition containing a specific ultraviolet absorbent is known (see, for example, Patent Document 1). Furthermore, a photosensitive resin composition is known that contains an ultraviolet absorber precursor and does not crystallize even when stored under high temperature conditions for a certain period of time, and has excellent storage stability (see, for example, Patent Document 2).

[0003] In view of the above, ultraviolet absorbents are added to photosensitive resin compositions to which photolithography is applied in order to exhibit various properties, but there is room for further improvement in storage stability and substrate adhesion for forming fine patterns. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-178407 A [Patent Document 2] JP 2001-235856 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to provide a photosensitive resin composition which has excellent storage stability even when an ultraviolet absorber is added, is suitable for fine pattern processing by photolithography, is free from line thickening, and can exhibit good adhesion to a substrate, and a cured product thereof. [Means for solving the problem]

[0006] As a result of intensive research, the present inventors have found a photosensitive resin composition containing a colorant, a cured product thereof, and uses thereof. <1> ~ <7> This is achieved by: <1> A photosensitive resin composition comprising an alkali-soluble resin, a polymerizable monomer, a colorant, a photopolymerization initiator, an ultraviolet absorber, and a solvent, the alkali-soluble resin being represented by the following general formula (1) or (2):

[0007] [ka] (In the formula, R 1 and R 3 R are the same or different and represent a hydrogen atom or an organic group having 1 to 30 carbon atoms. 2represents a hydrogen atom or a methyl group. X, Y and Z are the same or different and represent a methylene group, a methylene group in which a hydrogen atom has been substituted with a methyl group, an oxygen atom, a sulfur atom, or an imino group, with the proviso that at least one of X, Y and Z represents an oxygen atom, a sulfur atom or an imino group. A photosensitive resin composition comprising a heterocycle-containing structural unit represented by the following formula: <2> The photopolymerization initiator is an oxime-based initiator. <1> The photosensitive resin composition according to claim 1. <3> The ultraviolet absorber is at least one selected from the group consisting of benzotriazole compounds, benzophenone compounds, and triazine compounds. <1> or <2> The photosensitive resin composition according to claim 1. <4> The photosensitive resin composition is characterized in that the viscosity change rate after storage at 40° C. for 65 hours is 120% or less. <1> ~ <3> 10. The photosensitive resin composition according to claim 9, <5> the above <1> ~ <4> 2. A cured product obtained by curing the photosensitive resin composition according to claim 1. <6> the above <5> A color filter comprising the cured product according to claim 1. <7> the above <6> A display device having the color filter according to claim 1. Effect of the Invention

[0008] By using the photosensitive resin composition of the present invention, it is possible to reduce the change in viscosity during storage even when an ultraviolet absorber is added, and to obtain a cured product with little line thickening and high adhesion to a glass substrate, etc. Such a photosensitive resin composition is particularly suitable as a resist for a color filter, and the cured product, display device member, and display device obtained by curing the composition are very useful in various fields such as electronic information materials and optical materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below. In addition, a combination of two or more of the individual preferred embodiments of the present invention described below is also a preferred embodiment of the present invention. In this specification, "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid", and "(meth)acrylate" means "acrylate and / or methacrylate". In this specification, the numerical range "Min to Max" means a range equal to or greater than the minimum value Min and equal to or less than the maximum value Max. Furthermore, when the upper and lower limit values ​​are described as suitable numerical values ​​in stages, a numerical range obtained by appropriately combining the upper and lower limit values ​​described separately is also a suitable numerical range. [Photosensitive resin composition] As described above, the photosensitive resin composition of the present invention contains an alkali-soluble resin, a polymerizable monomer, a coloring material, a photopolymerization initiator, an ultraviolet absorber, and a solvent. By containing these components, it is suitable as a resist for a color filter, and for example, it is possible to form a fine pixel pattern and provide a colored cured film that can exhibit good substrate adhesion. Each of these components can be used alone or in combination. In addition, if necessary, it may further contain one or more other components. Each component will be described below. In this specification, the term "total solid content" refers to the total amount of components forming a cured product, i.e., the total amount of components (solid content, non-volatile content) excluding the solvent and the like that volatilizes during the formation of a cured product. Specifically, it refers to the total solid content mass of the alkali-soluble resin, the polymerizable monomer, the colorant, and, if any, other components forming a cured product (e.g., photopolymerization initiator, ultraviolet absorber, dispersant, etc.), together with said components.

[0010] (A) Alkali-soluble resin The alkali-soluble resin is a resin (preferably a polymer) that exhibits alkali solubility, and preferably has an acid group in the molecule. Examples of the acid group include functional groups that undergo a neutralization reaction with alkaline water, such as a carboxyl group, a phenolic hydroxyl group, a carboxylic anhydride group, a phosphoric acid group, and a sulfonic acid group, and the resin may have only one of these groups, or may have two or more of these groups. Among these, a carboxyl group or a carboxylic anhydride group is preferable, and a carboxyl group is more preferable. The alkali-soluble resin may act as a binder resin in the resin composition. The acid value (AV) of the alkali-soluble resin is preferably, for example, 20 mgKOH / g or more. This allows sufficient alkali solubility to be expressed, making it possible to give a cured product with better developability (development speed). More preferably, it is 50 mgKOH / g or more, and even more preferably, it is 70 mgKOH / g or more. The higher the acid value, the more pronounced the effect of the present invention is, that is, excellent substrate adhesion and developability. More preferably, it is 90 mgKOH / g or more, particularly preferably 95 mgKOH / g or more, and most preferably 99 mgKOH / g or more. In addition, the upper limit of the acid value is not particularly limited, but, for example, from the viewpoint of improving the curability and water resistance of the cured product, it is preferably 300 mgKOH / g or less. More preferably, it is 250 mgKOH / g or less, even more preferably 200 mgKOH / g or less, and particularly preferably 150 mgKOH / g or less. In this specification, the acid value of a resin (polymer) can be determined by the method described in the examples below. The weight average molecular weight (Mw) of the alkali-soluble resin is, for example, preferably 5000 or more. This allows a cured product with better heat resistance and mechanical strength to be obtained. More preferably, it is 6000 or more, even more preferably 7000 or more, and particularly preferably 8000 or more. The upper limit of Mw is, for example, preferably 50,000 or less. This allows the viscosity of the resin composition to become more appropriate, making it easier to form a coating film, thereby further improving developability. More preferably, it is 30,000 or less, and even more preferably 20,000 or less. In this specification, the weight average molecular weight can be measured by the method described in the examples below. The above-mentioned alkali-soluble resin has a heterocyclic structure in the main chain. By having a heterocyclic structure in the main chain, the photosensitive resin composition has excellent basic performance (adhesion, curability, dry resolubility, etc.) that contributes to plate making when producing a color filter, etc., and excellent basic performance (heat resistance, transparency, etc.) that contributes to the reliability and spectral characteristics of the cured product. Furthermore, the photosensitive resin composition has high dispersibility of color materials, and storage stability can be improved. The heterocyclic structure is also called a heterocyclic structure, and is preferably a 4- to 6-membered ring structure from the viewpoint of stable polymerization activity. More preferably, it is a 5- to 6-membered ring structure. Moreover, the heteroatom constituting the heterocyclic structure is preferably an oxygen atom, a sulfur atom, or a nitrogen atom, and more preferably an oxygen atom or a sulfur atom from the viewpoint of improving transparency. Among them, an oxygen atom is even more preferable from the viewpoint of suppressing coloration, etc. The alkali-soluble resin preferably has a heterocyclic structure in the main chain in the form of a heterocyclic ring-containing structural unit represented by the above general formula (1) or (2). Among them, the form having the heterocyclic ring-containing structural unit represented by the above general formula (1) is more preferable from the viewpoint of further improving the dispersibility and curability of the colorant in the presence of an ultraviolet absorber. In the above formulas (1) and (2), from the viewpoint of improving flexibility, it is preferable that X and Z represent a methylene group. In this case, Y preferably represents an oxygen atom, a sulfur atom, or an imino group, more preferably an oxygen atom or a sulfur atom, and even more preferably an oxygen atom. Thus, it is particularly preferable that X and Z in the above formula represent a methylene group and Y represents an oxygen atom, that is, the above alkali-soluble resin has a tetrahydrofuran ring and / or a tetrahydropyran ring in the main chain. It is most preferable that the main chain has a tetrahydrofuran ring. In the above general formulas (1) and (2), R 1 and R 3 are the same or different and represent a hydrogen atom or an organic group having 1 to 30 carbon atoms. When the molecule contains two or more heterocycle-containing structural units represented by general formula (1) or (2), R 1 and R 3 is R in other building blocks. 1 and R 3 may be the same as or different from R 2 The same applies to. The organic group having 1 to 30 carbon atoms is not particularly limited and may be appropriately selected depending on the purpose or application, but is preferably, for example, a hydrocarbon group having 1 to 30 carbon atoms which may have a substituent. The number of carbon atoms is preferably 1 to 25, more preferably 1 to 12, and further preferably 1 to 8. Specific examples of the organic group having 1 to 30 carbon atoms include linear saturated hydrocarbon groups such as methyl, ethyl, n-propyl, i-propyl, n-butyl, s-butyl, t-butyl, n-amyl, s-amyl, t-amyl, n-hexyl, s-hexyl, n-heptyl, n-octyl, s-octyl, t-octyl, 2-ethylhexyl, capryl, nonyl, decyl, undecyl, lauryl, tridecyl, myristyl, pentadecyl, cetyl, heptadecyl, stearyl, nonadecyl, eicosyl, seryl, and melissyl; alkoxy-substituted saturated chain hydrocarbon groups in which some of the hydrogen atoms of a saturated chain hydrocarbon group have been replaced with alkoxy groups, such as methoxyethyl, methoxyethoxyethyl, methoxyethoxyethoxyethyl, 3-methoxybutyl, ethoxyethyl, ethoxyethoxyethyl, phenoxyethyl, and phenoxyethoxyethyl; hydroxy-substituted saturated chain hydrocarbon groups in which some of the hydrogen atoms of a saturated chain hydrocarbon group have been replaced with hydroxyl groups, such as hydroxyethyl, hydroxypropyl, and hydroxybutyl; halogen-substituted saturated chain hydrocarbon groups in which some of the hydrogen atoms of a saturated chain hydrocarbon group have been replaced with halogens, such as fluoroethyl, difluoroethyl, chloroethyl, dichloroethyl, bromoethyl, and dibromoethyl; chain unsaturated hydrocarbon groups such as vinyl, allyl, methallyl, crotyl, and propargyl, and chain unsaturated hydrocarbon groups in which some of the hydrogen atoms have been replaced with alkoxy groups, hydroxyl groups, or halogens; cyclopentyl, cyclohexyl, 4-methylcyclohexyl, 4-t-butylcyclohexyl, tricyclodecanyl, isobornyl, adamantyl, dicyclopentyl, Examples of the aromatic hydrocarbon group include alicyclic hydrocarbon groups such as tadienyl, and alicyclic hydrocarbon groups in which some of the hydrogen atoms are replaced with alkoxy groups, hydroxyl groups, or halogens; aromatic hydrocarbon groups such as phenyl, methylphenyl, dimethylphenyl, trimethylphenyl, 4-t-butylphenyl, benzyl, diphenylmethyl, diphenylethyl, triphenylmethyl, cinnamyl, naphthyl, and anthranyl, and aromatic hydrocarbon groups in which some of the hydrogen atoms are replaced with alkoxy groups, hydroxyl groups, or halogens; and the like, which may further have a substituent bonded thereto. Among these, from the viewpoint of improving heat resistance, groups having primary or secondary carbon atoms that are difficult to be eliminated by acid or heat, such as methyl, ethyl, cyclohexyl, and benzyl, are preferred. Above R 1 and R 3 are particularly preferably the same or different and are a hydrogen atom or a methyl group. 2 is particularly preferably a hydrogen atom. In the above alkali-soluble resin, the content ratio of the heterocycle-containing structural unit present in the main chain may be appropriately set according to the purpose and use of the photosensitive resin composition and the molecular weight of the alkali-soluble resin. For example, it is preferably 1 to 99 mol%, more preferably 2 to 80 mol%, even more preferably 5 to 60 mol%, and most preferably 5 to 50 mol% relative to 100 mol% of all repeating units. In addition, when the alkali-soluble resin has a high molecular weight, the performance tends to be expressed even if the molar ratio of the heterocycle-containing structural unit is small, and when the molecular weight is low, the performance tends to be easily expressed by increasing the molar ratio. From this viewpoint, the number of heterocycle-containing structural units (also referred to as the average number of functional groups) contained in one main chain is preferably 0.5 or more, more preferably 1.0 or more, and even more preferably 2.0 or more. The above-mentioned alkali-soluble resin can be produced, for example, by polymerizing a monomer component including a monomer having an acid group and a monomer capable of introducing the above-mentioned (1) and / or (2) heterocyclic structure into the main chain skeleton of the polymer, but it is also preferable to produce it by introducing a polymerizable double bond into the side chain of the polymer (also called a base polymer) obtained by the polymerization. The side chain double bond-containing polymer obtained by the latter production method is also preferable as the alkali-soluble resin of the present invention. Among these, from the viewpoint of photosensitivity, curability, thermal decomposition resistance, etc., it is particularly preferable that the above-mentioned alkali-soluble resin is a side chain double bond-containing polymer. One or more types of each of the raw material monomers can be used, and the monomer component (also called a monomer composition) that forms the base polymer is also called a "base polymer component". The raw material components and polymerization method of the alkali-soluble resin will be further described below.

[0011] -Raw material components (monomers, etc.)- (i) Monomers having an acid group The monomer having an acid group is a compound having an acid group and a polymerizable double bond in the molecule. For example, unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, cinnamic acid, vinylbenzoic acid, etc.; unsaturated polyvalent carboxylic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, etc.; unsaturated monocarboxylic acids in which the unsaturated group and the carboxyl group are chain-extended, such as mono(2-acryloyloxyethyl) succinate, mono(2-methacryloyloxyethyl) succinate, etc.; unsaturated acid anhydrides such as maleic anhydride, itaconic anhydride, etc.; phosphoric acid group-containing unsaturated compounds such as Light Ester P-1M (manufactured by Kyoeisha Chemical Co., Ltd.); etc. can be mentioned. Among these, from the viewpoints of versatility, availability, etc., it is preferable to use carboxylic acid-based monomers (unsaturated monocarboxylic acids, unsaturated polyvalent carboxylic acids, unsaturated acid anhydrides). In terms of reactivity, alkali solubility, and the like, unsaturated monocarboxylic acids are more preferred, (meth)acrylic acid (that is, acrylic acid and / or methacrylic acid) is even more preferred, and methacrylic acid is particularly preferred. The blending ratio of the monomer having an acid group is preferably, for example, 5% by mass or more relative to 100% by mass of the total amount of the base polymer component. This provides a resin composition with more sufficient solubility in alkali and more useful for applications requiring developability. In addition, in order to better maintain the excellent appearance and adhesion of the cured product, the blending ratio is preferably 70% by mass or less. It is more preferably 10 to 60% by mass, and even more preferably 15 to 50% by mass. (ii) A monomer capable of introducing a heterocyclic structure into the main chain of a polymer Examples of monomers capable of introducing a heterocyclic structure into the main chain skeleton of a polymer include monomers having a double bond-containing heterocyclic structure in the molecule and monomers that impart a heterocyclic structure to the main chain skeleton by cyclic polymerization. Among them, monomers represented by the following general formula (3) or (4) are preferred. The resulting alkali-soluble resin has a heterocyclic ring-containing structural unit represented by the above-mentioned general formula (1) or (2). More preferred is a monomer represented by the following general formula (3).

[0012] [ka] The symbols in the above general formulae (3) and (4) are the same as the respective symbols in the above general formulae (1) and (2). Among them, it is particularly preferable that X and Z represent a methylene group and Y represents an oxygen atom. Preferred examples of the monomer represented by the above general formula (3) include the following compounds. α-Allyloxymethylacrylic acid, methyl α-allyloxymethylacrylate, ethyl α-allyloxymethylacrylate, n-propyl α-allyloxymethylacrylate, i-propyl α-allyloxymethylacrylate, n-butyl α-allyloxymethylacrylate, s-butyl α-allyloxymethylacrylate, t-butyl α-allyloxymethylacrylate, n-amyl α-allyloxymethylacrylate, s-amyl α-allyloxymethylacrylate, t-amyl α-allyloxymethylacrylate, α-allyloxymethyl n-Hexyl acrylate, s-hexyl α-allyloxymethyl acrylate, n-heptyl α-allyloxymethyl acrylate, n-octyl α-allyloxymethyl acrylate, s-octyl α-allyloxymethyl acrylate, t-octyl α-allyloxymethyl acrylate, 2-ethylhexyl α-allyloxymethyl acrylate, capryl α-allyloxymethyl acrylate, nonyl α-allyloxymethyl acrylate, decyl α-allyloxymethyl acrylate, undecyl α-allyloxymethyl acrylate, α-allyloxymethyl Lauryl acrylate, tridecyl α-allyloxymethylacrylate, myristyl α-allyloxymethylacrylate, pentadecyl α-allyloxymethylacrylate, cetyl α-allyloxymethylacrylate, heptadecyl α-allyloxymethylacrylate, stearyl α-allyloxymethylacrylate, nonadecyl α-allyloxymethylacrylate, eicosyl α-allyloxymethylacrylate, ceryl α-allyloxymethylacrylate, melissyl α-allyloxymethylacrylate, methoxy α-allyloxymethylacrylate Ethyl, methoxyethoxyethyl α-allyloxymethylacrylate, methoxyethoxyethoxyethyl α-allyloxymethylacrylate, 3-methoxybutyl α-allyloxymethylacrylate, ethoxyethyl α-allyloxymethylacrylate, ethoxyethoxyethyl α-allyloxymethylacrylate, phenoxyethyl α-allyloxymethylacrylate, phenoxyethoxyethyl α-allyloxymethylacrylate, hydroxyethyl α-allyloxymethylacrylate, hydroxypropyl α-allyloxymethylacrylate,α-Allyloxymethylacrylic acid hydroxybutyl, α-Allyloxymethylacrylic acid fluoroethyl, α-Allyloxymethylacrylic acid difluoroethyl, α-Allyloxymethylacrylic acid chloroethyl, α-Allyloxymethylacrylic acid dichloroethyl, α-Allyloxymethylacrylic acid bromoethyl, α-Allyloxymethylacrylic acid dibromoethyl, α-Allyloxymethylacrylic acid vinyl, α-Allyloxymethylacrylic acid allyl, α-Allyloxymethylacrylic acid methallyl, α-Allyloxymethylacrylic acid crotyl, α-Allyloxymethylacrylic acid propargyl, α-Allyloxymethylacrylic acid cyclopentyl, α-Allyloxymethylacrylic acid cyclohexyl, α-Allyloxymethylacrylic acid 4-methylcyclohexyl, α-Allyloxymethylacrylic acid 4-t-butylcyclohexyl, α-Allyloxymethylacrylic acid 4-t-butylcyclohexyl, tricyclodecanyl α-allyloxymethylacrylate, isobornyl α-allyloxymethylacrylate, adamantyl α-allyloxymethylacrylate, dicyclopentadienyl α-allyloxymethylacrylate, phenyl α-allyloxymethylacrylate, methylphenyl α-allyloxymethylacrylate, dimethylphenyl α-allyloxymethylacrylate, trimethylphenyl α-allyloxymethylacrylate, 4-t-butylphenyl α-allyloxymethylacrylate, benzyl α-allyloxymethylacrylate, diphenylmethyl α-allyloxymethylacrylate, diphenylethyl α-allyloxymethylacrylate, triphenylmethyl α-allyloxymethylacrylate, cinnamyl α-allyloxymethylacrylate, naphthyl α-allyloxymethylacrylate, anthranyl α-allyloxymethylacrylate, etc., Preferred examples of the monomer represented by the above general formula (4) include the following compounds. Dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, diethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, di(n-propyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(isopropyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(n-butyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(isobutyl)-2,2'-[oxybis(methylene)]bis-2- propenoate, di(t-butyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(t-amyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(stearyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(lauryl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(2-ethylhexyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(1-methoxyethyl)-2,2 '-[oxybis(methylene)]bis-2-propenoate, di(1-ethoxyethyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, dibenzyl-2,2'-[oxybis(methylene)]bis-2-propenoate, diphenyl-2,2'-[oxybis(methylene)]bis-2-propenoate, dicyclohexyl-2,2'-[oxybis(methylene)]bis-2-propenoate, di(t-butylcyclohexyl)-2,2'-[oxybis(methylene)]bis-2-propenoate propenoate, di(dicyclopentadienyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(tricyclodecanyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(isobornyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, diadamantyl-2,2'-[oxybis(methylene)]bis-2-propenoate, di(2-methyl-2-adamantyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, and the like. The blending ratio of the monomer capable of introducing a heterocyclic structure into the main chain skeleton of the polymer is, for example, preferably 2% by mass or more relative to 100% by mass of the total amount of the base polymer component. This can further improve adhesion, heat resistance, dispersibility of the colorant, and storage stability. From the viewpoint of preventing gelation during polymerization and efficiency, it is preferably 60% by mass or less. It is more preferably 3 to 50% by mass, and even more preferably 5 to 40% by mass.

[0013] (iii) Monomers having a cyclic structure The base polymer component also preferably contains a monomer having a cyclic structure (excluding compounds corresponding to the monomer (ii) above). Preferred examples of the monomer having a cyclic structure include cyclic structure-containing (meth)acrylic acid ester monomers; aromatic vinyl compounds; and the like. Examples of the cyclic structure-containing (meth)acrylic acid ester monomer include cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, 1-adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, biphenyl (meth)acrylate, o-biphenyloxyethyl (meth)acrylate, o-biphenyloxyethoxyethyl (meth)acrylate, m-biphenyloxyethyl acrylate, p-biphenyloxyethyl (meth)acrylate, and o-biphenyloxy-2-hydroxypropane. Examples of the monomer include biphenyl group-containing monomers such as o-phenylphenol glycidyl ether acrylate, p-biphenyloxy-2-hydroxypropyl (meth)acrylate, m-biphenyloxy-2-hydroxypropyl (meth)acrylate, N-(meth)acryloyloxyethyl-o-biphenyl carbamate, N-(meth)acryloyloxyethyl-p-biphenyl carbamate, N-(meth)acryloyloxyethyl-m-biphenyl carbamate, and o-phenylphenol glycidyl ether acrylate; naphthalene ring-containing monomers such as vinyl naphthalene; terphenyl (meth)acrylate; and o-terphenyloxyethyl (meth)acrylate. Examples of the aromatic vinyl compound include styrene, vinyl toluene, and α-methyl styrene. Among the monomers having a cyclic structure described above, cyclic structure-containing (meth)acrylic acid ester monomers and aromatic vinyl compounds are preferred because they have good transparency and are less likely to impair heat resistance. More preferred are cyclic structure-containing (meth)acrylic acid ester monomers. Even more preferred are cyclohexyl (meth)acrylate, benzyl (meth)acrylate, o-biphenyloxyethyl (meth)acrylate, and o-biphenyloxyethoxyethyl (meth)acrylate. The blending ratio of the monomer having the cyclic structure is not particularly limited, but is preferably 0 to 80% by mass, for example, relative to 100% by mass of the total amount of the base polymer component. Among these, from the viewpoints of heat resistance, hardness, colorant dispersibility, development speed, transparency, etc., it is more preferably 2 to 80% by mass, even more preferably 10 to 75% by mass, and particularly preferably 20 to 70% by mass. (iv) Other monomers The base polymer component may also contain, as necessary, one or more other monomers (also referred to as other monomers) that are copolymerizable with at least one of the above-mentioned monomers. The other monomer is not particularly limited, and examples thereof include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, methyl 2-ethylhexyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate (excluding those corresponding to the monomers (ii) and (iii) above); (meth)acryloylmorpholine, (meth)acrylamide, N-methyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, N-isobutyl(meth)acrylamide, N-t-butyl(meth)acrylamide, Examples of (meth)acrylamides include diacetone (meth)acrylamide, Nt-octyl (meth)acrylamide, diacetone (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, N-cyclohexyl (meth)acrylamide, N-phenyl (meth)acrylamide, N-benzyl (meth)acrylamide, N-triphenylmethyl (meth)acrylamide, and N,N-dimethyl (meth)acrylamide (excluding those corresponding to the monomers (ii) and (iii) above); butadiene or substituted butadiene compounds such as butadiene and isoprene; ethylene or substituted ethylene compounds such as ethylene, propylene, vinyl chloride, and acrylonitrile; and vinyl esters such as vinyl acetate. Among these, (meth)acrylic acid esters are preferred in terms of good transparency and resistance to deterioration in heat resistance, and more preferably methyl (meth)acrylate. The blending ratio of the other monomers is not particularly limited, but is preferably 0 to 80% by mass, for example, relative to 100% by mass of the total amount of the base polymer component. Among these, from the viewpoints of heat coloration resistance, colorant dispersibility, etc., it is more preferably 0.1 to 80% by mass, even more preferably 1 to 50% by mass, and particularly preferably 1 to 20% by mass. In terms of achieving finer patterns, it is particularly preferable in the present invention to have a structural unit represented by the following general formula (5) (hereinafter also referred to as "structural unit (α)"), which will be described in detail below.

[0014] [ka] (In the formula, R 4 R represents a hydrogen atom or a methyl group. 5 represents a linear or branched hydrocarbon group having 4 to 20 carbon atoms. The alkali-soluble resin included in the present invention has the above structural unit (α) and can provide a cured product that is excellent in pattern fineness, pattern linearity and adhesion. In the above general formula (5), R 4 represents a hydrogen atom or a methyl group. From the viewpoint of development speed, R 4 is preferably a hydrogen atom. In the above general formula (5), R 5 represents a linear or branched hydrocarbon group having 4 to 20 carbon atoms. Examples of the linear or branched hydrocarbon group having 4 to 20 carbon atoms include an n-butyl group, a 1-methylpropyl group, a 2-methylpropyl group, a 1,1-dimethylethyl group, an n-pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 2,2-dimethylpropyl group, a 1-ethylpropyl group, an n-hexyl group, a 1,1-dimethylpropyl group, a 1,2-dimethylpropyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 4-methylpentyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 1,3-dimethylbutyl group, a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, Examples of such groups include an n-butyl group, a 3,3-dimethylbutyl group, a 1-ethylbutyl group, a 2-ethylbutyl group, a 1,2,2-trimethylpropyl group, a 1-ethyl-1-methylpropyl group, a 1-ethyl-2-methylpropyl group, an n-heptyl group, an n-octyl group, a 2-ethylhexyl group, an n-nonyl group, an isononyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, an n-hexadecyl group, an n-heptadecyl group, an n-octadecyl group, an n-nonadecyl group, and an n-eicosyl group. The linear or branched hydrocarbon group having 4 to 20 carbon atoms is preferably a linear or branched hydrocarbon group having 4 to 18 carbon atoms, and more preferably a linear or branched hydrocarbon group having 4 to 10 carbon atoms. Above R 5 Specific examples of the alkyl group include preferably an isononyl group, an n-dodecyl group, an n-butyl group, and a 2-ethylhexyl group, more preferably an isononyl group, an n-butyl group, and a 2-ethylhexyl group, and even more preferably a 2-ethylhexyl group and an isononyl group.

[0015] Preferred examples of the monomer that provides the structural unit (α) include compounds represented by the following general formula (6). CH 2 =CR 4 -C(O)-OR 5 (6) (In the formula, R 4 R represents a hydrogen atom or a methyl group. 5 represents a linear or branched hydrocarbon group having 4 to 20 carbon atoms. By polymerizing a monomer component containing such a monomer compound, an alkali-soluble resin having the above structural unit (α) can be obtained. R in the above general formula (6) 4 and R 5 are R in the above general formula (5), 4 and R 5 The same can be mentioned. Specific examples of monomers that provide the structural unit (α) include n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate, etc. Preferred are n-butyl (meth)acrylate, isononyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-dodecyl (meth)acrylate, etc., more preferred are isononyl (meth)acrylate and 2-ethylhexyl (meth)acrylate. The alkali-soluble resin may have only one type of the structural unit (α), or may have two or more types. Considering the compatibility of the pattern fineness, pattern linearity, and adhesion of the alkali-soluble resin, the content of the structural unit (α) is preferably 10% by mass or more relative to 100% by mass of all structural units of the alkali-soluble resin. The content of the structural unit (α) is more preferably 20% by mass or more, and even more preferably 30% by mass or more relative to 100% by mass of all structural units of the alkali-soluble resin, and is also preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less.

[0016] -Polymerization method- As a method for polymerizing the monomer components, a commonly used method such as bulk polymerization, solution polymerization, emulsion polymerization, etc. can be used, and may be appropriately selected according to the purpose and application. Among them, solution polymerization is preferable because it is industrially advantageous and easy to adjust the structure such as molecular weight. In addition, as the polymerization mechanism of the monomer components, a polymerization method based on a mechanism such as radical polymerization, anionic polymerization, cationic polymerization, coordination polymerization, etc. can be used, but a polymerization method based on a radical polymerization mechanism is preferable because it has a high cyclization rate (for example, the ratio of the constitutional unit represented by the general formula (1) or (2) produced from the monomer represented by the general formula (3) or (4)) and is industrially advantageous. In addition, the polymerization concentration and polymerization temperature vary depending on the type and ratio of the monomers used and the molecular weight of the target polymer, but it is preferable to set the polymerization temperature to 40 to 150°C and the polymerization concentration to 20 to 50% by mass, and more preferably to set the polymerization temperature to 60 to 130°C and the polymerization concentration to 30 to 45%. When a solvent is used in the polymerization, the solvent is not particularly limited as long as it is a solvent used in a normal radical polymerization reaction, but it is preferable in terms of efficiency to use a solvent that is used in the subsequent preparation of a photosensitive resin composition. The solvent may be one or more kinds. Specific examples of the solvent include the following compounds: Monoalcohols such as methanol, ethanol, isopropanol, n-butanol, and s-butanol; glycols such as ethylene glycol and propylene glycol; cyclic ethers such as tetrahydrofuran and dioxane; glycol monoethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, and 3-methoxybutanol; glycol ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, propylene glycol dimethyl ether, and propylene glycol diethyl ether; Glycol monoethers such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether acetate, dipropylene glycol monobutyl ether acetate, and 3-methoxybutyl acetate; esters; alkyl esters such as methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, methyl propionate, ethyl propionate, butyl propionate, methyl lactate, ethyl lactate, butyl lactate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl acetoacetate, and ethyl acetoacetate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene; aliphatic hydrocarbons such as hexane, cyclohexane, and octane; amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; and the like. Among these, from the viewpoint of polymerization efficiency, it is preferable to use esters of glycol monoethers, monoalcohols and / or glycol monoethers. It is more preferable to use at least esters of glycol monoethers, and it is also preferable to use esters of glycol monoethers and glycol monoethers in combination. In the above polymerization, one or more polymerization initiators may be used as necessary. The polymerization initiator is not particularly limited, and examples thereof include organic peroxides such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, di-t-butyl peroxide, lauroyl peroxide, benzoyl peroxide, t-butylperoxyisopropylcarbonate, t-amylperoxy-2-ethylhexanoate, and t-butylperoxy-2-ethylhexanoate; azo compounds such as 2,2'-azobis(isobutyronitrile), 1,1'-azobis(cyclohexanecarbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), and dimethyl 2,2'-azobis(2-methylpropionate); hydrogen peroxide, persulfates, etc. In addition, reducing agents such as transition metal salts and amines may be used in combination with the polymerization initiator. The amount of the polymerization initiator used may be appropriately set according to the type and amount of the monomer used, polymerization reaction conditions such as polymerization temperature and concentration, and the molecular weight of the target polymer, and is not particularly limited, but for example, it is preferably 0.1 to 20 parts by mass per 100 parts by mass of the total amount of the base polymer component. This makes it possible to easily obtain a polymer having a weight average molecular weight in a preferred range without gelation. It is more preferably 0.5 to 15 parts by mass. In the above polymerization, a chain transfer agent may be used, if necessary, for molecular weight adjustment. Examples of the chain transfer agent include mercaptan-based chain transfer agents such as n-dodecyl mercaptan, mercaptopropionic acid, mercaptoacetic acid, and methyl mercaptoacetate, α-methylstyrene dimer, and also the compounds described in JP-A-2015-22175

[0047] . Among these, it is preferable to use n-dodecyl mercaptan and / or mercaptopropionic acid, since they have a high chain transfer effect, can reduce the amount of residual monomers, and are easily available. When a chain transfer agent is used, the amount of the chain transfer agent may be appropriately set according to the type and amount of the monomer used, polymerization reaction conditions such as polymerization temperature and concentration, and the molecular weight of the target polymer, and is not particularly limited, but for example, it is preferably 0.1 to 15 parts by mass per 100 parts by mass of the total amount of the base polymer component. This makes it possible to easily obtain a polymer having a weight average molecular weight in a preferred range without gelation. It is more preferably 0.5 to 10 parts by mass, and even more preferably 1 to 8 parts by mass.

[0017] -Method for introducing polymerizable double bonds into side chains- The alkali-soluble resin preferably also contains a polymerizable double bond in the side chain. By having a polymerizable double bond in the side chain, it can be cured by heat or light. Therefore, the thermal decomposition resistance is improved, the sensitivity to light is improved, the resin is cured with less light, and the mechanical strength after curing is also high. As a method for introducing a polymerizable double bond into the side chain, a method of adding a compound containing a functional group that can be bonded to an acid group and a polymerizable double bond to the base polymer can be mentioned. In the compound having a functional group and a polymerizable double bond that can be bonded to the acid group, the polymerizable double bond may be, for example, a (meth)acryloyl group, a vinyl group, an allyl group, a methallyl group, etc., and the compound is preferably one or more of these. Among these, from the viewpoint of the reactivity of the resulting polymer, a (meth)acryloyl group is preferred. In addition, the functional group that can be bonded to the acid group may be, for example, an epoxy group, an oxazoline group, a hydroxyl group, an oxetanyl group, an isocyanate group, etc., and the compound is preferably one or more of these. Among these, an epoxy group, an oxazoline group, or a hydroxyl group is preferred, and from the viewpoint of the speed of the modification reaction, heat resistance, and dispersibility, an epoxy group (including a glycidyl group) is more preferred. Examples of the compound having a functional group and a polymerizable double bond that can be bonded to the acid group include compounds having a hydroxyl group and a double bond, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and allyl alcohol; compounds having an epoxy group and a double bond, such as glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, β-ethylglycidyl (meth)acrylate, vinylbenzyl glycidyl ether, allyl glycidyl ether, 3,4-epoxycyclohexylmethyl (meth)acrylate, allyl glycidyl ether, and vinylcyclohexene oxide; compounds having an oxazoline group and a double bond, such as vinyloxazoline and isopropenyloxazoline; and the like. One or more of these can be used. Among them, it is preferable to use a compound (monomer) having an epoxy group and a (meth)acryloyl group. In particular, glycidyl (meth)acrylate and / or 3,4-epoxycyclohexylmethyl (meth)acrylate are more preferred from the viewpoints of high reactivity, ease of reaction control, ease of availability, and ability to simultaneously introduce not only radically polymerizable double bonds but also hydroxyl groups. The amount of the compound containing a functional group and a polymerizable double bond that can be bonded to the acid group is preferably 2 to 95 parts by mass relative to 100 parts by mass of the total amount of the monomer component (base polymer component) that gives the base polymer. When the amount of the compound is within this range, the curability of the photosensitive resin composition is further increased, the strength after curing is more sufficient, the storage stability of the obtained polymer (side chain double bond-containing polymer) is further improved, and coloring in the cured product is sufficiently suppressed. More preferably, it is 10 parts by mass or more, even more preferably 20 parts by mass or more, and particularly preferably 30 parts by mass or more. When the amount of addition is large, the effect of the present invention is more effectively exerted, and it is possible to give a cured product that is more excellent in adhesion, solvent resistance, and developability. The upper limit is more preferably 85 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 75 parts by mass or less. The method of adding a compound containing a functional group capable of bonding with an acid group and a polymerizable double bond to a part of the acid group in the base polymer is not particularly limited, and may be a known method. The reaction temperature is preferably, for example, 60°C to 140°C. In addition, it is preferable to use known catalysts such as amine compounds such as triethylamine and dimethylbenzylamine; ammonium salts such as tetraethylammonium chloride; phosphonium salts such as tetraphenylphosphonium bromide; and amide compounds such as dimethylformamide. As a result of the introduction of the double bonds, the double bond equivalent (meaning the molecular weight (g) per 1 mole of double bonds) of the resulting alkali-soluble resin (side-chain double bond-containing polymer) is preferably 250 to 4000 g / mol. When the double bond equivalent is within this range, the sensitivity to light is increased and developability is improved, coloration during curing is further suppressed, and storage stability and solubility in solvents are further improved. It is more preferably 270 to 3000 g / mol, even more preferably 300 to 2000 g / mol, and particularly preferably 320 to 2000 g / mol. The double bond equivalent is a measure of the amount of double bonds contained in a molecule, and for compounds of the same molecular weight, the larger the double bond equivalent value, the less double bonds are introduced. The double bond equivalent can be calculated from the amount of polymer or compound to introduce double bonds. It can also be measured by titration, elemental analysis, NMR, IR, and other analyses, as well as differential scanning calorimetry. In this specification, the double bond equivalent is calculated according to the following formula. Double bond equivalent=(weight of base polymer+weight of compound containing a functional group capable of bonding to an acid group and a polymerizable double bond) / (number of moles of compound containing a functional group capable of bonding to an acid group and a polymerizable double bond) Alternatively, it may be calculated by measuring the number of ethylenic double bonds contained per gram of polymer in accordance with the iodine value testing method described in JIS K 0070:1992. In the photosensitive resin composition of the present invention, the content (solid content) of the alkali-soluble resin is, for example, preferably 5 to 50 parts by mass relative to 100 parts by mass of the total solid content of the photosensitive resin composition. This allows the action and effect of the alkali-soluble resin to be more fully exhibited. It is more preferably 10 to 45 parts by mass, and even more preferably 15 to 40 parts by mass. (B) Polymerizable monomer The polymerizable monomer is a low molecular weight compound having a polymerizable unsaturated bond (also called a polymerizable unsaturated group) that can be polymerized by irradiation of active energy rays such as free radicals, electromagnetic waves (e.g., infrared rays, ultraviolet rays, X-rays, etc.), and electron beams. For example, a monofunctional compound having one polymerizable unsaturated group in the molecule and a polyfunctional compound having two or more polymerizable unsaturated groups can be mentioned. The molecular weight is not particularly limited, but from the viewpoint of handling, it is preferably 3000 or less, and more preferably 2000 or less.

[0018] Examples of the monofunctional polymerizable monomer include, among the compounds exemplified as other monomers preferably contained in the monomer component of the alkali-soluble resin, (meth)acrylic acid esters; (meth)acrylamides; unsaturated monocarboxylic acids; unsaturated polycarboxylic acids; unsaturated monocarboxylic acids in which the unsaturated group and the carboxyl group are chain-extended; unsaturated acid anhydrides; aromatic vinyls; conjugated dienes; vinyl esters; vinyl ethers; N-vinyl compounds; unsaturated isocyanates; and N-substituted maleimides.

[0019] Examples of the polyfunctional polymerizable monomer include the following compounds. Bifunctional (meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, bisphenol A alkylene oxide di(meth)acrylate, and bisphenol F alkylene oxide di(meth)acrylate acrylate compounds; trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, ethylenediaminetetraacetate ... Ethylene oxide added to trimethylolpropane tri(meth)acrylate, Ethylene oxide added to ditrimethylolpropane tetra(meth)acrylate, Ethylene oxide added to pentaerythritol tetra(meth)acrylate, Ethylene oxide added to dipentaerythritol hexa(meth)acrylate, Propylene oxide added to trimethylolpropane tri(meth)acrylate, Propylene oxide added to ditrimethylolpropane tetra(meth)acrylate, Propylene oxide added to pentaerythritol hexa(meth)acrylate trifunctional or higher polyfunctional (meth)acrylate compounds such as erythritol tetra(meth)acrylate, propylene oxide-added dipentaerythritol hexa(meth)acrylate, ε-caprolactone-added trimethylolpropane tri(meth)acrylate, ε-caprolactone-added ditrimethylolpropane tetra(meth)acrylate, ε-caprolactone-added pentaerythritol tetra(meth)acrylate, and ε-caprolactone-added dipentaerythritol hexa(meth)acrylate; Ethylene glycol divinyl ether, diethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butylene glycol divinyl ether, hexanediol divinyl ether, bisphenol A alkylene oxide divinyl ether, bisphenol F alkylene oxide divinyl ether, trimethylolpropane trivinyl ether, ditrimethylolpropane tetravinyl ether, glycerin trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, dipentaerythritol hexavinyl ether, ethylene oxide-added trimethylolpropane trivinyl ether, ethylene oxide-added ditrimethylolpropane tetravinyl ether, ethylene oxide-added pentaerythritol tetravinyl ether polyfunctional vinyl ethers such as dipentaerythritol vinyl ether and ethylene oxide-added dipentaerythritol hexavinyl ether; vinyl ether group-containing (meth)acrylic acid esters such as 2-vinyloxyethyl (meth)acrylate, 3-vinyloxypropyl (meth)acrylate, 1-methyl-2-vinyloxyethyl (meth)acrylate, 2-vinyloxypropyl (meth)acrylate, 4-vinyloxybutyl (meth)acrylate, 4-vinyloxycyclohexyl (meth)acrylate, 5-vinyloxypentyl (meth)acrylate, 6-vinyloxyhexyl (meth)acrylate, 4-vinyloxymethylcyclohexylmethyl (meth)acrylate, p-vinyloxymethylphenylmethyl (meth)acrylate, 2-(vinyloxyethoxy)ethyl (meth)acrylate, and 2-(vinyloxyethoxyethoxyethoxy)ethyl (meth)acrylate; Ethylene glycol diallyl ether, diethylene glycol diallyl ether, polyethylene glycol diallyl ether, propylene glycol diallyl ether, butylene glycol diallyl ether, hexanediol diallyl ether, bisphenol A alkylene oxide diallyl ether, bisphenol F alkylene oxide diallyl ether, trimethylolpropane triallyl ether, ditrimethylolpropane tetraallyl ether, glycerin triallyl ether, pentaerythritol tetraallyl ether, dipentaerythritol pentaallyl ether, dipentaerythritol hexaallyl ether, ethylene oxide-added trimethylolpropane triallyl ether, ethylene oxide-added ditrimethylolpropane tetraallyl ether, ethylene oxide-added pentaerythritol tetraallyl ether, ethylene oxide-added dipentaerythritol hexaallyl ether polyfunctional allyl ethers such as allyl ether; allyl group-containing (meth)acrylic acid esters such as allyl (meth)acrylate; polyfunctional (meth)acryloyl group-containing isocyanurates such as tri(acryloyloxyethyl)isocyanurate, tri(methacryloyloxyethyl)isocyanurate, alkylene oxide-added tri(acryloyloxyethyl)isocyanurate, and alkylene oxide-added tri(methacryloyloxyethyl)isocyanurate; polyfunctional allyl group-containing isocyanurates such as triallyl isocyanurate; polyfunctional urethane (meth)acrylates obtained by reacting polyfunctional isocyanates such as tolylene diisocyanate, isophorone diisocyanate, and xylylene diisocyanate with hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; polyfunctional aromatic vinyls such as divinylbenzene; and the like.

[0020] A particularly preferred polymerizable monomer, a polyfunctional (meth)acrylate compound having two or more functional groups, will be described in detail below. A polyfunctional (meth)acrylate compound having two or more functionalities (hereinafter also simply referred to as a "polyfunctional (meth)acrylate compound") is a compound having two or more (meth)acryloyl groups in one molecule. By including such a compound, the photosensitive resin composition has excellent photosensitivity and curability, and it is possible to obtain a cured product having extremely high hardness and high transparency. The functionality of the polyfunctional (meth)acrylate compound is preferably 3 or more, more preferably 4 or more, and even more preferably 5 or more. In addition, from the viewpoint of further suppressing cure shrinkage, the functionality is preferably 10 or less, more preferably 8 or less, and even more preferably 6 or less. In addition, the (meth)acryloyl group means a methacryloyl group and / or an acryloyl group, and from the viewpoint of superior reactivity, an acryloyl group is preferable. In other words, it is particularly preferable that the polyfunctional (meth)acrylate compound is a polyfunctional acrylate compound having two or more acryloyl groups.

[0021] The content ratio of the polymerizable monomer may be appropriately set according to the type of polymerizable monomer and the alkali-soluble resin used, as well as the purpose and application, but from the viewpoint of superior developability and curability, it is preferably 2 parts by mass or more and preferably 85 parts by mass or less relative to 100 parts by mass of the total solid content of the photosensitive resin composition. The lower limit is more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, and particularly preferably 15 parts by mass or more, and the upper limit is more preferably 75 parts by mass or less, even more preferably 60 parts by mass or less, particularly preferably 50 parts by mass or less, and most preferably 40 parts by mass or less. The content of the polymerizable monomer is preferably 50 parts by mass or more and 500 parts by mass or less relative to 100 parts by mass of the alkali-soluble resin. When the content of the polymerizable monomer is within this range, a cured product having higher adhesion and hardness can be obtained, and in combination with the preferred weight average molecular weight of the alkali-soluble resin being 5000 or more, the developability is further improved. More preferably, the content is 80 parts by mass or more, even more preferably, 100 parts by mass or more, and particularly preferably, 120 parts by mass or more. In addition, from the viewpoint of further improving the developability, the content is more preferably 400 parts by mass or less. More preferably, the content is 300 parts by mass or less, particularly preferably, 200 parts by mass or less, and most preferably, 150 parts by mass or less.

[0022] (C) Color material As the coloring material, for example, a pigment or a dye is preferably used. These may be used alone or in combination of two or more. A pigment and a dye may also be combined. For example, when forming red, blue, and green pixels of a color filter, a method of combining coloring materials such as blue and purple, green and yellow, etc. to exhibit the desired color characteristics is preferably used. In addition, when forming a black matrix, it can be formed using a black coloring material. Among the above pigments and dyes, for example, in terms of durability, pigments (e.g., organic pigments or inorganic pigments) are superior, and, for example, in terms of improving the brightness of panels, etc., dyes are superior, so they may be appropriately selected or used in combination according to the desired characteristics. Among pigments, organic pigments are more preferable. In addition, since a composition capable of suppressing a decrease in storage stability due to pigment aggregation has been found in the photosensitive resin composition of the present invention, it is preferable to use at least a pigment as a colorant, and excellent dispersibility can be exhibited even if the photosensitive resin composition contains an ultraviolet absorber described later. Examples of the pigments include organic pigments such as azo pigments, phthalocyanine pigments, polycyclic pigments (e.g., quinacridone, perylene, perinone, isoindolinone, isoindoline, dioxazine, thioindigo, anthraquinone, quinophthalone, metal complex, diketopyrrolopyrrole, etc.), and dye lake pigments; white pigments (e.g., titanium oxide, zinc oxide, zinc sulfide, clay, talc, barium sulfate, calcium carbonate, etc.), chromatic pigments (e.g., yellow lead, cadmium, etc.), and the like. Examples of inorganic pigments that can be used include inorganic pigments such as chrome vermilion, nickel titanium, chrome titanium, yellow iron oxide, red iron oxide, zinc chromate, red lead, ultramarine, Prussian blue, cobalt blue, chrome green, chromium oxide, bismuth vanadate, etc., black pigments (e.g. carbon black, bone black, graphite, iron black, titanium black, etc.), glitter pigments (e.g. pearl pigments, aluminum pigments, bronze pigments, etc.), fluorescent pigments (e.g. zinc sulfide, strontium sulfide, strontium aluminate, etc.), etc. Examples of pigment colors that can be used include yellow, red, purple, blue, green, brown, black, and white. The above pigments may also be surface-treated, such as with rosin, surfactant, resin-based dispersant, pigment derivative, oxide film, silica coating, wax coating, etc., depending on the purpose or application. Specific examples of the above pigments are shown below by color and Color Index (CI; published by The Society of Dyers and Colourists) number, but the color materials of the present invention are not limited to these. These may be used alone or in combination of two or more kinds. In the following, "CI" means Color Index, and the numbers mean Color Index numbers. Examples of yellow pigments include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 9, 10, 12, 13, 14, 15, 16, 17, 20, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 41, 42, 43, 48, 49, 53, 55, 60, 61, 61:1, 62, 62:1, 63, 65, 71, 73, 74, 75, 77, 81, 83, 87, 93, 94, 95, 97, 98, 99, 100, 101, 104, 105, 106, 108, 109, 110, 111, 113, 114, 116, 117, 119, 120, 123, 124, 126, 127, 128, 129, 130, 131, 132, 133, 134, 135, 136, 137, 138, 139, 140, 141, 142, 143, 144, 145, 146, 147, 148, 149, 150, 151, 152, 153, 154, 155, 156, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 178, 179, 180, 181, 182, 183, 184, 185, 186, 187, 188, 189, 190, 191, 192, 193, 194, 195, 196, 197, 1 33, 134, 136, 138, 139, 142, 147, 148, 150, 151, 152, 153, 154, 155, 156, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170. 172, 173, 174, 175, 176, 179, 180, 181, 182, 183, 184, 185, 188, 189, 190, 191, 191:1, 192, 193, 194, 195, 196, 197, 198, 199, 200, 202, 203, 204, 205, 206, 207, 208, 209, 209:1, 212, 213, 214, 215, 219, etc. Examples of orange pigments include CI Pigment Orange 1, 2, 3, 4, 5, 13, 15, 16, 17, 19, 20, 21, 22, 23, 24, 31, 34, 36, 38, 39, 40, 43, 46, 48, 49, 51, 60, 61, 62, 64, 65, 67, 68, 69, 70, 71, 72, 73, 74, 75, 77, 78, 79, and 81. Examples of purple pigments include CI Pigment Violet 1, 1:1, 2, 2:2, 3, 3:1, 3:3, 5, 5:1, 13, 14, 15, 16, 17, 19, 23, 25, 27, 29, 31, 32, 36, 37, 38, 39, 42, 44, 47, 49, and 50. Examples of red pigments include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 21, 22, 23, 31, 32, 37, 38, 40, 41, 42, 47, 48, 48:1, 48:2, 48:3, 48:4, 48:5, 49, 49:1, 49:2, 50:1, 52, 52:1, 52:2, 53, 53:1, 53:2, 53:3, 5 4, 57, 57:1, 57:2, 58, 58:2, 58:4, 60, 60:1, 63, 63:1, 63:2, 64, 64:1, 68, 69, 81, 81:1, 81:2, 81:3, 81:4, 83, 88, 89, 90:1, 95, 97, 101, 101:1, 102, 104, 105, 106, 108, 108:1, 109, 112, 113, 114, 122, 123, 136, 144, 14 6, 147, 149, 150, 151, 164, 166, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 178, 179, 180, 181, 182, 183, 184, 185, 187, 188, 190, 193, 194, 200, 202, 206, 207, 208, 209, 210, 211, 213, 214, 215, 216, 220, 221, 22 4, 226, 230, 231, 232, 233, 235, 236, 237, 238, 239, 242, 243, 245, 247, 248, 249, 250, 251, 253, 254, 255, 256, 257, 258, 259, 260, 262, 263, 264, 265, 266, 267, 268, 269, 270, 271, 272, 273, 274, 275, 276, 279, etc. Examples of blue pigments include CI Pigment Blue 1, 1:2, 9, 14, 15, 15:1, 15:2, 15:3, 15:4, 15:5, 15:6, 16, 17, 17:1, 19, 24, 24:1, 25, 26, 27, 28, 29, 33, 35, 36, 56, 56:1, 60, 61, 61:1, 62, 63, 66, 67, 68, 71, 72, 73, 74, 75, 76, 78, 79, and 80. Examples of green pigments include CI Pigment Green 1, 2, 4, 7, 8, 10, 13, 15, 17, 18, 19, 26, 36, 45, 48, 50, 51, 54, 55, and 58. Examples of brown pigments include CI Pigment Brown 5, 6, 23, 24, 25, 32, 41, and 42. Examples of black pigments include aniline black, carbon black, lamp black, bone black, iron black, titanium black, CI Pigment Black 1, 6, 7, 9, 10, 11, 12, 13, 20, 31, 32, and 34. Examples of white pigments include CI Pigment White 1, 2, 4, 5, 6, 7, 11, 12, 18, 19, 21, 22, 23, 26, 27, and 28. As the dye, for example, organic dyes described in JP-A-2010-9033, JP-A-2010-211198, JP-A-2009-51896, and JP-A-2008-50599 can be used. Among them, azo dyes, anthraquinone dyes, phthalocyanine dyes, quinoneimine dyes, quinoline dyes, nitro dyes, carbonyl dyes, methine dyes, and the like are preferred. The content ratio of the coloring material (i.e., the total ratio of the pigment and the dye) can be appropriately set depending on the purpose and application, but the content ratio of the coloring material is preferably in the range of 3 to 70 parts by mass, more preferably 5 to 60 parts by mass, and further preferably 10 to 50 parts by mass, based on 100 parts by mass of the total solid content of the photosensitive resin composition.

[0023] (D) Photopolymerization initiator The photosensitive resin composition of the present invention also preferably contains a photopolymerization initiator. The photopolymerization initiator is preferably a radically polymerizable photopolymerization initiator. The radically polymerizable photopolymerization initiator generates polymerization initiation radicals by irradiation with active energy rays such as electromagnetic waves and electron beams, and one or more of commonly used initiators can be used. In addition, one or more of photosensitizers and photoradical polymerization accelerators may be used in combination as necessary. By using a photosensitizer and / or a photoradical polymerization accelerator together with the photopolymerization initiator, the sensitivity and curability are further improved.

[0024] The photopolymerization initiator is not particularly limited, but examples thereof include the following compounds. 2-Dimethylamino-2-methyl-1-phenylpropan-1-one, 2-diethylamino-2-methyl-1-phenylpropan-1-one, 2-methyl-2-morpholino-1-phenylpropan-1-one, 2-dimethylamino-2-methyl-1-(4-methylphenyl)propan-1-one, 2-dimethylamino-1-(4-ethylphenyl)-2-methylpropan-1-one, 2-dimethylamino-1-(4-isopropylphenyl)-2-methylpropan-1-one, 1-(4-butylphenyl)-2-methylpropan-1-one phenyl)-2-dimethylamino-2-methylpropan-1-one, 2-dimethylamino-1-(4-methoxyphenyl)-2-methylpropan-1-one, 2-dimethylamino-2-methyl-1-(4-methylthiophenyl)propan-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-benzyl-2-dimethylamino-1-(4-dimethylamino α-aminoketone compounds such as 2-dimethylamino-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone; 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propanone, alkylphenone compounds such as 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone; Halomethylated triazine compounds such as 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-ethoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, and 2-(4-ethoxycarbonylnaphthyl)-4,6-bis(trichloromethyl)-s-triazine; 2-trichloromethyl-5-(2'-benzofuryl) -1,3,4-oxadiazole, 2-trichloromethyl-5-[β-(2'-benzofuryl)vinyl]-1,3,4-oxadiazole, 4-oxadiazole, 2-trichloromethyl-5-furyl-1,3,4-oxadiazole and other halomethylated oxadiazole compounds; 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4,6-trichlorophenyl)-4,4',5,5' - Biimidazole compounds such as tetraphenyl-1,2'-biimidazole; oxime ester compounds such as 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); titanocene compounds such as bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium benzoic acid ester compounds such as p-dimethylaminobenzoic acid and p-diethylaminobenzoic acid; acridine compounds such as 9-phenylacridine; α-hydroxyketone compounds such as 1-hydroxycyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one; and the like. Among the above photopolymerization initiators, it is particularly preferable to use at least an oxime-based initiator such as the above oxime ester compound, from the viewpoint of achieving excellent adhesion and fine pattern processability. The content ratio of the photopolymerization initiator is not particularly limited, and it is preferable to set it appropriately in consideration of the ratio of other components such as coloring materials, but for example, it is preferably 0.5 to 30 parts by mass relative to 100 parts by mass of the total solid content of the photosensitive resin composition. This further improves the curability and adhesion. More preferably, it is 1 to 25 parts by mass, and even more preferably 1.5 to 20 parts by mass. In addition, examples of photosensitizers and photoradical polymerization accelerators that may be used in combination with the photopolymerization initiator include dye-based compounds such as xanthene dyes, coumarin dyes, 3-ketocoumarin compounds, and pyrromethene dyes; dialkylaminobenzene-based compounds such as ethyl 4-dimethylaminobenzoate and 2-ethylhexyl 4-dimethylaminobenzoate; and mercaptan-based hydrogen donors such as 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, and 2-mercaptobenzimidazole. The content (total amount) of the photosensitizer and the photoradical polymerization accelerator may be appropriately set depending on the purpose and application, and is not particularly limited, but from the viewpoint of the balance between the curability, the effect of decomposition products, and economic efficiency, it is preferably 0.001 to 20 parts by mass, more preferably 0.01 to 15 parts by mass, and further preferably 0.05 to 10 parts by mass, based on 100 parts by mass of the total solid content of the photosensitive resin composition of the present invention. The oxime initiators which are particularly preferably used in the present invention will be described in detail below. Oxime initiators are preferred because they have high sensitivity and polymerization efficiency, can be cured regardless of the coloring material (colorant) concentration, and can easily be designed to have a high coloring material concentration. Specific examples of the oxime initiator include compounds described in JP-A-2001-233842, JP-A-2000-80068, and JP-A-2006-342166. Specific examples of the oxime initiator include 3-benzoyloxyiminobutan-2-one, 3-acetoxyiminobutan-2-one, 3-propionyloxyiminobutan-2-one, 2-acetoxyiminopentan-3-one, 2-acetoxyimino-1-phenylpropan-1-one, 2-benzoyloxyimino-1-phenylpropan-1-one, 3-(4-toluenesulfonyloxy)iminobutan-2-one, and 2-ethoxycarbonyloxyimino-1-phenylpropan-1-one.

[0025] Examples of the oxime initiator include compounds described in J. C. S. Perkin II (1979) pp. 1653-1660), J. C. S. Perkin II (1979) pp. 156-162, Journal of Photopolymer Science and Technology (1995) pp. 202-232, JP-A No. 2000-66385, JP-A No. 2000-80068, JP-T No. 2004-534797, and JP-A No. 2006-342166. Commercially available products such as IRGACURE-OXE01 (manufactured by BASF) and IRGACURE-OXE02 (manufactured by BASF) are also suitable for use. In addition, TRONLY TR-PBG-304, TRONLY TR-PBG-309, TRONLY TR-PBG-305 (manufactured by CHANGZHOU TRONLY NEW ELECTRONIC MATERIALS CO., LTD.), and ADEKA ARCLES NCI-930 (manufactured by ADEKA) can also be used.

[0026] Further examples of oxime-based initiators other than those described above include the compound described in JP-T-2009-519904 in which an oxime is linked to the carbazole N-position, the compound described in U.S. Pat. No. 7,626,957 in which a heterosubstituent is introduced at the benzophenone moiety, and the compounds described in JP-A-2010-15025 and U.S. Pat. Appln. KOKAI Publication No. 2009-292039 in which a nitro group is introduced at the dye moiety. The compound, an oxime-based initiator described in International Patent Publication No. 2009-131189, a compound containing a triazine skeleton and an oxime skeleton in the same molecule described in U.S. Patent No. 7,556,910, a compound having an absorption maximum at 405 nm and good sensitivity to a g-line light source described in JP-A-2009-221114, etc. may be used. Preferably, for example, paragraphs 0274 to 0275 of JP-A-2013-29760 can be referred to, the contents of which are incorporated herein by reference.

[0027] As the photoradical polymerization initiator, an oxime-based initiator having a fluorene ring can also be used. Specific examples of oxime-based initiators having a fluorene ring include compounds described in JP 2014-137466 A, the contents of which are incorporated herein by reference.

[0028] As the photoradical polymerization initiator, an oxime-based initiator having a fluorine atom can also be used. Specific examples of the oxime-based initiator having a fluorine atom include the compounds described in JP-A-2010-262028, compounds 24, 36 to 40 described in JP-T-2014-500852, and compound (C-3) described in JP-A-2013-164471. The contents of this specification are incorporated herein by reference.

[0029] As the photoradical polymerization initiator, an oxime-based initiator having a nitro group can be used. Specific examples of the oxime-based initiator having a nitro group include the compounds described in paragraphs 0031 to 0047 of JP 2013-114249 A and paragraphs 0008 to 0012 and 0070 to 0079 of JP 2014-137466 A, and Adeka Arcles NCI-831 (manufactured by ADEKA Corporation). As the oxime-based initiator, a compound having a maximum absorption wavelength in the wavelength region of 350 nm to 500 nm is preferable, a compound having an absorption wavelength in the wavelength region of 360 nm to 480 nm is more preferable, and a compound having high absorbance at 365 nm and 405 nm is particularly preferable.

[0030] From the viewpoint of sensitivity, the molar absorption coefficient of the oxime initiator at 365 nm or 405 nm is preferably 1,000 to 300,000, more preferably 2,000 to 300,000, and particularly preferably 5,000 to 200,000. The molar absorption coefficient of the compound can be measured by a known method. Specifically, for example, it is preferable to measure the molar absorption coefficient with an ultraviolet-visible spectrophotometer (Varian Cary-5 spectrophotometer) using ethyl acetate as a solvent at a compound concentration of 0.01 g / L.

[0031] The oxime initiators may be used in combination of two or more kinds, if necessary.

[0032] The content of the oxime initiator is preferably 0.1 to 50 parts by mass, more preferably 0.5 to 30 parts by mass, further preferably 1 to 25 parts by mass, and most preferably 1.5 to 20 parts by mass, based on the total solid content of the photosensitive resin composition. Within this range, better sensitivity and fine pattern formability can be obtained. (E) Ultraviolet absorbers (UV absorbers) The photosensitive resin composition of the present invention contains an ultraviolet absorber. The ultraviolet absorber is preferably a compound having a maximum absorption wavelength in the wavelength range of 300 to 400 nm, more preferably a compound having a maximum absorption wavelength in the wavelength range of 320 to 380 nm. By using such a compound, the occurrence of development residues between patterns can be effectively suppressed. In addition, a fine pattern can be formed. Furthermore, the occurrence of color mixing between adjacent pixels of different hues can be effectively suppressed.

[0033] Examples of the ultraviolet absorbent that can be used include conjugated diene compounds, methyldibenzoyl compounds, coumarin compounds, salicylate compounds, benzophenone compounds, benzotriazole compounds, acrylonitrile compounds, triazine compounds, and benzodithiazole compounds. Among these, benzotriazole compounds, benzophenone compounds, and triazine compounds are preferred, and benzophenone compounds are particularly preferred. The benzotriazole compound may be represented by the following formula (7) or (8).

[0034] [ka] In formulas (7) and (8), R 6 and R 8 each independently represents a hydrogen atom, a hydroxyl group, an amino group, an alkyl group having 1 to 6 carbon atoms which may have a substituent, a phenyl group which may have a substituent, a substituent having a sulfonyl group, or -A 1 -A 2 A 1 is a carbonyl group, an alkanediyl group having 1 to 12 carbon atoms, a cycloalkylene group having 3 to 12 carbon atoms, or -A 11 -O- and A 11 A is an alkanediyl group having 1 to 12 carbon atoms. 2 is a hydrogen atom, a halogen atom, a cyano group, a hydroxy group, an alkoxy group having 1 to 6 carbon atoms, a carboxy group, or a dialkylamino group in which each alkyl group has 1 to 6 carbon atoms.

[0035] In formulas (7) and (8), R 7 and R 9 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkyl group having 1 to 6 carbon atoms which may have a substituent, an alkoxy group having 1 to 6 carbon atoms, a substituent having a sulfonyl group, or an organic group represented by the following formula (9):

[0036] [ka] (In the formula, R 10is a hydrogen atom or an optionally substituted alkyl group having 1 to 12 carbon atoms. d is 0 or 1. Benzotriazole compounds include benzotriazole, 1-hydroxybenzotriazole, 1-methylbenzotriazole, 1-hydroxymethylbenzotriazole, 1-ethylbenzotriazole, 1-(1-hydroxyethyl)benzotriazole, 1-(2-hydroxyethyl)benzotriazole, 1-propylbenzotriazole, 1-(1-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(3-hydroxypropyl)benzotriazole, 4-hydroxy-1H-benzotriazole, 1-(1-hydroxypropyl)benzotriazole, 1-(2-hydroxypropyl)benzotriazole, 1-(3-hydroxypropyl)benzotriazole, 1-(1 ... Triazole, 5-methyl-1H-benzotriazole, benzotriazole-5-carboxylic acid, 1-methylbenzotriazole-5-carboxylic acid, 1-ethylbenzotriazole-5-carboxylic acid, 1-tert-butylbenzotriazole-5-carboxylic acid, 1-(2-cyclopentylethyl)benzotriazole-5-carboxylic acid, 1H-benzotriazole-4-sulfonic acid, 1H-benzotriazole-1-acetonitrile, 1H-benzotriazole-1-carboxaldehyde, 2-methyl-2H-benzotriazole, 2-ethyl- 2H-benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-amyl-5'-isobutylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-isobutyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-isobutyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-isobutyl-5'-propylphenyl) -5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-[2'-hydroxy-5'-(1,1,3,3-tetramethyl)phenyl]benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole, 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy, 2-(2H-benzotriazol-2-yl)-4,Examples of the benzotriazole compound include 6-bis(1-methyl-1-phenylethyl)phenol, 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, etc. Commercially available products include TINUVIN PS, TINUVIN 99-2, TINUVIN 109, TINUVIN 328, TINUVIN 384-2, TINUVIN 900, TINUVIN 928, TINUVIN 171, and TINUVIN 1130 (all manufactured by BASF). As the benzotriazole compound, the MYUA series manufactured by Miyoshi Oil Co., Ltd. (The Chemical Daily, February 1, 2016) may be used.

[0037] The benzophenone compound may be a compound represented by the general formula (10).

[0038] [ka] In the general formula (10), R 11 and R 12 are each a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. A specific example of the compound represented by the general formula (10) is 2,2'-dihydroxy-4,4'-dimethoxybenzophenone (in the general formula (10), R 11 =R 12 = Methyl group compound, 2,2',4,4'-tetrahydroxybenzophenone (R 11 =R 12 =Hydroxy group compounds and the like can be mentioned. Commercially available products include Ubinal A, Ubinal 3049, and Ubinal 3050 (all manufactured by BASF). The triazine compounds include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-piperonyl-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-( 5-methylfuran-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine, and the like. Commercially available products include TINUVIN 1577FF, TINUVIN 400, and TINUVIN 411L (all manufactured by BASF). In the present invention, the following ultraviolet absorbents are preferred.

[0039] [ka]

[0040] [ka]

[0041] [ka]

[0042] [ka]

[0043] [ka] In the photosensitive resin composition of the present invention, the content of the ultraviolet absorber is preferably 0.1 to 20 parts by mass based on the total solid content of the photosensitive resin composition. The upper limit is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less. The lower limit is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more. When the content of the ultraviolet absorber is within the above range, it is possible to form a fine pattern, and the occurrence of development residue between patterns and the occurrence of color mixing between adjacent pixels of different hues can be effectively suppressed. The content of the ultraviolet absorber is preferably 10 to 500 parts by mass relative to 100 parts by mass of the photopolymerization initiator. The upper limit is preferably 450 parts by mass or less, more preferably 300 parts by mass or less, and even more preferably 200 parts by mass or less. The lower limit is preferably 15 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 25 parts by mass or more. When the content of the ultraviolet absorber is within the above range, the occurrence of development residue between patterns and the occurrence of color mixing between adjacent pixels of different hues can be effectively suppressed. The content of the ultraviolet absorber is preferably 1 to 40 parts by mass relative to 100 parts by mass of the colorant. The upper limit is preferably 35 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less. The lower limit is preferably 1.1 parts by mass or more, more preferably 1.5 parts by mass or more, and even more preferably 2 parts by mass or more. When the content of the ultraviolet absorber is within the above range, the occurrence of development residue between patterns and the occurrence of color mixing between adjacent pixels of different hues can be effectively suppressed. (F) Solvent The photosensitive resin composition also preferably contains a solvent. The solvent is preferably used as a diluent or the like. Specifically, the solvent is preferably used for the purposes of lowering the viscosity to improve the handling property, forming a coating film by drying, and serving as a dispersion medium for a coloring material, and is a low-viscosity organic solvent or water that can dissolve or disperse each component contained in the photosensitive resin composition.

[0044] The above-mentioned solvent may be any commonly used solvent and may be appropriately selected depending on the purpose and application, and is not particularly limited, but examples thereof include the following compounds, etc. These may be used alone or in combination of two or more kinds. Monoalcohols such as methanol, ethanol, isopropanol, n-butanol, and s-butanol; glycols such as ethylene glycol and propylene glycol; cyclic ethers such as tetrahydrofuran and dioxane; glycol monoethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, and 3-methoxybutanol; glycol ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, propylene glycol dimethyl ether, and propylene glycol diethyl ether; ethylene glycol monomethyl ether acetone esters of glycol monoethers such as ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether acetate, dipropylene glycol monobutyl ether acetate, and 3-methoxybutyl acetate; alkyl esters such as methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, methyl propionate, ethyl propionate, butyl propionate, methyl lactate, ethyl lactate, butyl lactate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl acetoacetate, and ethyl acetoacetate;Ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.; aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, etc.; aliphatic hydrocarbons such as hexane, cyclohexane, octane, etc.; amides such as dimethylformamide, dimethylacetamide, N-methylpyrrolidone, etc.; water; etc.; Among them, it is preferable to use esters of glycol monoethers, monoalcohols, and / or glycol monoethers. It is more preferable to use at least esters of glycol monoethers, and it is also preferable to use in combination esters of glycol monoethers and glycol monoethers. The content ratio of the solvent is not particularly limited, and is preferably set appropriately depending on the form of use of the photosensitive resin composition (for example, coating, etc.). For example, it is preferable to set the content ratio of the solvent so that the total solid content (solid content concentration) in 100% by mass of the photosensitive resin composition is 1 to 90% by mass. The total solid content in 100% by mass of the photosensitive resin composition is more preferably 5 to 70% by mass, and even more preferably 10 to 50% by mass. The content of the solvent is preferably 10 to 90% by mass, and more preferably 20 to 80% by mass, relative to 100% by mass of the total amount of the photosensitive resin composition of the present invention.

[0045] (G) Dispersant The photosensitive resin composition of the present invention also preferably contains a dispersant. The dispersant is not particularly limited, but for example, it is preferable that the dispersant has an interactive site with the colorant and an interactive site with the dispersion medium (alkali-soluble resin, solvent, etc.) and has a function of stabilizing the dispersion of the colorant in the dispersion medium. In general, dispersants that are classified into resin-type dispersants (polymer dispersants), surfactants (low-molecular dispersants), and dye derivatives and are commonly used may be used. Examples of the resin-type dispersant include polycarboxylates such as polyurethane and polyacrylate, unsaturated polyamides, polycarboxylic acids, polycarboxylate amine salts, polycarboxylate ammonium salts, polycarboxylate alkylamine salts, polysiloxanes, long-chain polyaminoamide phosphates, hydrogen-containing polycarboxylates, amides formed by the reaction of poly(lower alkyleneimines) with polyesters having free carboxyl groups, and their salts, (meth)acrylic acid-styrene copolymers, (meth)acrylic acid-(meth)acrylic acid ester copolymers, styrene-maleic acid copolymers, polyvinyl alcohol, polyvinylpyrrolidone, polyesters, modified polyacrylates, and ethylene oxide / polypropylene oxide adducts. Among these, from the structural standpoint, resins having a graft structure in which the main chain is an anchor chain having an interactive site with the colorant and the graft chain is a compatible chain having an interactive property with the dispersion medium, and resins in which the anchor chain and the compatible chain are in a block structure are particularly preferably used. Examples of the surfactant include anionic surfactants such as polyoxyethylene alkyl ether sulfate, sodium dodecylbenzenesulfonate, sodium alkylnaphthalenesulfonate, sodium alkyldiphenyletherdisulfonate, monoethanolamine lauryl sulfate, triethanolamine lauryl sulfate, ammonium lauryl sulfate, sodium stearate, and sodium lauryl sulfate; nonionic surfactants such as polyoxyethylene oleyl ether, polyoxyethylene lauryl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene sorbitan monostearate, and polyethylene glycol monolaurate; cationic surfactants such as alkyl quaternary ammonium salts and their ethylene oxide adducts; alkyl betaines such as alkyl dimethylaminoacetate betaine, and amphoteric surfactants such as alkyl imidazolines; and the like. The dye derivative is a compound having a structure in which a functional group is introduced into the dye. Examples of the functional group include a sulfonic acid group, a sulfonamide group and its quaternary salt, a dialkylamino group, a hydroxyl group, a carboxyl group, an amide group, and a phthalimide group, and examples of the structure of the parent dye include azo, anthraquinone, quinophthalone, phthalocyanine, quinacridone, benzimidazolone, isoindoline, dioxazine, indanthrene, perylene, and diketopyrrolopyrrole.

[0046] The content ratio of the dispersant is not particularly limited and may be appropriately set depending on the purpose and application, but considering the balance between dispersion stability, durability (heat resistance, light resistance, weather resistance, etc.), transparency, etc., the solid content of the dispersant is preferably 0.01 to 100 parts by mass, more preferably 0.1 to 90 parts by mass, and even more preferably 0.5 to 80 parts by mass, relative to 100 parts by mass of the total solid content of the colorant. (H) Other Ingredients The photosensitive resin composition of the present invention may also contain one or more other components within a range that does not impair the effects of the present invention. For example, binder resins other than alkali-soluble resins, heat resistance improvers, leveling agents, coupling agents, development aids, fillers such as aluminum hydroxide, talc, clay, and barium sulfate, defoamers, metal oxide particles, quantum dot particles, sensitizers, release agents, lubricants, plasticizers, antioxidants, flame retardants, polymerization inhibitors, thickeners, thermosetting resins such as epoxy resins, phenolic resins, and polyvinylphenols, curing agents, reactive diluents, stabilizers, flame retardant aids, curing aids such as polyfunctional thiol compounds, fluorine-based additives, cationic polymerizable compounds, and acid generators. The amount of the other components used may be appropriately determined depending on the purpose and application, but for example, it is preferably 0 to 70 parts by mass, more preferably 0.01 to 70 parts by mass, still more preferably 0.1 to 60 parts by mass, and particularly preferably 0.3 to 50 parts by mass, relative to 100 parts by mass of the total solid content of the photosensitive resin composition.

[0047] [Method for producing photosensitive resin composition] The method for producing the photosensitive resin composition of the present invention is not particularly limited, and for example, the above-mentioned components can be mixed and dispersed using various mixers and dispersers to prepare the composition. The dispersion step and the mixing step are not particularly limited, and may be performed by a normal method, or may further include other steps that are normally performed. Specifically, for example, after preparing a colorant dispersion liquid (mill base) containing a colorant, a dispersant, a binder resin (alkali-soluble resin, etc.), and a solvent, it is preferable to further add a transparent resist liquid (also called a clear resist liquid) containing a polymerizable monomer, a photopolymerization initiator, an ultraviolet absorber, a binder resin (alkali-soluble resin, etc.), and a solvent to prepare the composition. It is preferable to filter the obtained photosensitive resin composition using a filter or the like to remove fine dust. In preparing the colorant dispersion, it is preferable to disperse the colorant into fine particles using a dispersing machine such as a paint conditioner, a bead mill, a roll mill, a ball mill, a jet mill, a homogenizer, a kneader, a blender, etc. More preferably, after kneading and dispersing with a roll mill, a kneader, a blender, etc., fine dispersion is performed with a media mill such as a bead mill filled with beads of 0.01 to 1 mm.

[0048] - Viscosity change rate - The photosensitive resin composition containing the specific component of the present invention has a small viscosity change rate and excellent storage stability, and can be transported or stored for a long time and used under the same process conditions for a long period of time. That is, the viscosity change rate after storage for 65 hours at 40°C is preferably 120% or less of the initial viscosity (viscosity immediately after preparation). More preferably, it is 110% or less, even more preferably 105% or less, and particularly preferably 103% or less. The viscosity change rate can be specifically evaluated, for example, by the following method. The viscosity of the photosensitive resin composition is measured immediately after preparation and after storage for 65 hours at 40° C. In the present invention, the viscosity is measured by the method described in (8) in the Examples below. The photosensitive resin composition of the present invention has a water content of preferably 0.14% by mass or less, more preferably 0.12% by mass or less, more preferably less than 0.10% by mass, particularly preferably 0.08% by mass or less, more particularly preferably 0.06% by mass or less, and most preferably 0.04% by mass or less, based on the entire photosensitive resin composition (100% by mass). This results in a photosensitive resin composition with a smaller viscosity change rate and excellent storage stability. In addition, in consideration of the amount of water contained in the raw material and the manufacturing cost of purification, etc., the lower limit of the water content is 0.001% by mass, preferably 0.005% by mass, more preferably 0.01% by mass, and even more preferably 0.02% by mass. This can further reduce the viscosity change rate and improve the storage stability. The water is (ultra)pure water, ion-exchanged water, distilled water, etc. Although the detailed mechanism is unclear, it is speculated that water inhibits the dispersibility of coloring materials such as pigments and the compatibility of alkali-soluble resins and ultraviolet absorbers, and that water decomposes photopolymerization initiators. In the present invention, it has been found that the use of the above-mentioned specific ultraviolet absorber and specific photopolymerization initiator (e.g., oxime-based initiator) can further suppress viscosity change and sensitivity decrease. It is presumed that the oxime ester compound is less susceptible to decomposition by water because the oxime ester compound has at least one group selected from a branched alkyl group and a cyclic alkyl group, which inhibits nucleophilic attack by water on the oxime ester site. For this reason, it is presumed that by using the above-mentioned oxime ester compound and setting the water content to 0.001 to 0.12 mass% relative to 100 mass% of the total amount of the photosensitive resin composition, a photosensitive resin composition with small viscosity change and excellent sensitivity stability over time can be obtained. In the present invention, the water content in the photosensitive resin composition is a value measured by the Karl Fischer method. The Karl Fischer method is a method for measuring the water content in a composition using a Karl Fischer reagent (composed of iodine, sulfur dioxide, a base, and a solvent such as alcohol) that reacts selectively and quantitatively with water. This method includes coulometric titration and volumetric titration, and either method may be used.

[0049] [Uses of the photosensitive resin composition] The photosensitive resin composition of the present invention can reduce the viscosity change during storage, and can provide a cured product with small line thickening and high adhesion to glass substrates and the like even when a fine pattern is formed, and can be used for various applications such as resist materials, various coating agents, paints, etc. Preferred applications include components of various display devices such as liquid crystal, organic EL, quantum dot, and micro LED liquid crystal displays, solid-state imaging devices, and touch panel display devices, black matrices, photospacers, black column spacers, inks, printing plates, printed wiring boards, semiconductor devices, photoresists, insulating films, films, organic protective films, and various optical material components and electric and electronic devices. Among them, the photosensitive resin composition is useful as a material for producing color filters, optical waveguides, and the like (for example, an alkali-developable negative resist material), and this can sufficiently increase the reliability of the display quality and imaging quality of various display devices to a degree that can fully meet the demand for high performance in recent years. In particular, the photosensitive resin composition is extremely useful for color filter applications. As described above, the photosensitive resin composition is suitable for use as a raw material for a color filter or a raw material for an optical waveguide. In addition, the photosensitive resin composition is also suitable for use as a protective film (such as a protective film for a color filter or a protective film for a touch panel type display device) or an insulating film (such as an insulating film for a touch panel type display device) in various display devices.

[0050] <Cured product> The cured product (cured film) of the present invention is obtained by curing the photosensitive resin composition of the present invention described above, and can be obtained by irradiating (exposing) the resin composition with active energy rays. Specifically, for example, it is preferable to obtain the cured product by applying the resin composition to a substrate (also called a base material), drying the resin composition, and irradiating (exposing) the applied surface with active energy rays. Since the photosensitive resin composition of the present invention is preferably used as a resist material, one of the preferred embodiments of the present invention is a form in which the cured product obtained by curing the photosensitive resin composition is a resist cured film. The cured film preferably has a film thickness of 0.1 to 20 μm. This can fully meet the demand for low height of members and display devices using the cured film. More preferably, it is 0.5 to 10 μm, and even more preferably, it is 0.5 to 8 μm. The substrate to which the photosensitive resin composition is applied is not particularly limited, and examples thereof include transparent glass substrates such as white plate glass, blue plate glass, and silica-coated blue plate glass; sheets, films, or substrates made of thermoplastic resins such as polyester, polycarbonate, polyolefin, polysulfone, ring-opening polymers of cyclic olefins, and hydrogenated products thereof; sheets, films, or substrates made of thermosetting resins such as epoxy resins and unsaturated polyester resins; metal substrates such as aluminum plates, copper plates, nickel plates, and stainless steel plates; ceramic substrates; semiconductor substrates having photoelectric conversion elements; glass substrates having a coloring material layer on the surface (color filters for LCDs); and the like. The substrates may be subjected to corona discharge treatment, ozone treatment, chemical treatment with a silane coupling agent, or the like, as necessary.

[0051] The method for applying the photosensitive resin composition to a substrate is not particularly limited, and examples thereof include spin coating, slit coating, roll coating, and cast coating, and any of these methods can be preferably used. The coating film after application to the substrate can be dried using, for example, a hot plate, an IR oven, a convection oven, etc. Drying conditions are appropriately selected depending on the boiling point of the solvent component contained, the type of curing component, the film thickness, the performance of the dryer, etc., but it is usually preferable to perform drying at a temperature of 50 to 160° C. for 10 to 300 seconds.

[0052] Examples of the light source for the active energy ray include lamp light sources such as xenon lamps, halogen lamps, tungsten lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, metal halide lamps, medium pressure mercury lamps, low pressure mercury lamps, carbon arcs, and fluorescent lamps, and laser light sources such as argon ion lasers, YAG lasers, excimer lasers, nitrogen lasers, helium cadmium lasers, and semiconductor lasers. Examples of the exposure system include the proximity system, mirror projection system, and stepper system, with the proximity system being preferably used. In addition, in the step of irradiating the active energy ray, depending on the application, the active energy ray may be irradiated through a predetermined mask pattern. In this case, the exposed portion is cured, and the cured portion is made insoluble or hardly soluble in a developer.

[0053] If necessary, after the active energy ray irradiation step, a step of developing with a developer to remove the unexposed areas and form a pattern (also referred to as a "developing step") may be carried out. This allows a patterned cured film to be obtained. The development treatment in the above-mentioned developing step can usually be carried out at a development temperature of 10 to 50° C. by a method such as immersion development, spray development, brush development, ultrasonic development or the like. As the active energy ray, preferably, short-wavelength radiation such as KrF excimer laser (wavelength 248 nm) or ArF excimer laser (wavelength 193 nm) is used, more preferably, ArF excimer laser is used, but other than that, g-ray (wavelength 436 nm), i-ray (wavelength 365 nm), X-ray (several nm to tens of nm), electron beam (several hundred pm or less), etc. may be used. In order to reduce deformation of the resist pattern (resist sidewall shape), the exposed resist film is baked (pre-development bake, pre-bake) by performing a heat treatment at a relatively high temperature, for example, by a hot plate, an oven, or infrared irradiation, as necessary. Thereafter, the resist film is further developed to form a resist pattern. The bake temperature during the pre-development bake is not particularly limited, but is preferably within the range of 120°C to 250°C. The bake time is appropriately set according to the bake temperature, the type of resist film, etc. The resist film having a resist pattern formed thereon by development is subjected to post-baking (final baking) in order to evaporate and remove the developer and rinsing solution remaining in or on the surface of the resist film and to strengthen the adhesion to the substrate. The baking temperature and baking time during the post-baking are not particularly limited as long as they are set at a temperature at which the resist pattern shape is not softened or deformed. An example of an embodiment having the cured film is a color filter having the cured film on a substrate (base material). A method for producing the color filter is described in detail below. The components constituting the color filter are specifically three primary color (RGB) pixels, a resin black matrix, a protective film, a columnar spacer, etc., and it is preferable that at least one of these components constituting the color filter has a cured film formed from the photosensitive resin composition of the present invention. Here, when forming RGB pixels, the resin composition of the present invention contains color materials of the three primary colors, red, green, and blue, and when forming a resin black matrix, it contains a black color material. The above color filter can be produced, for example, as follows. 1) The photosensitive resin composition is coated (applied) on a substrate by a known coating method, and dried to produce a coating film. The substrate is preferably a transparent substrate, and specific examples thereof include glass (preferably non-alkali glass) and transparent plastics. Known coating methods include spin coating and spraying, with spin coating being preferred. Regarding drying conditions, the drying temperature is preferably room temperature to 120°C, more preferably 60 to 100°C. The drying time is preferably 10 seconds to 60 minutes, more preferably 30 seconds to 10 minutes. In addition, it is preferable to heat and dry under normal pressure or vacuum. 2) Then, a photomask (patterning film) having openings corresponding to the desired pattern shape is placed on the coating film obtained in 1) above in a contact or non-contact state, and the coating film is irradiated with light to cure. The light means not only visible light but also radiation such as ultraviolet light, X-rays, and electron beams, with ultraviolet light being most preferred. A high-pressure mercury lamp is generally used as a source of ultraviolet light. 3) After the light irradiation in 2), development is carried out with a solvent, water, an aqueous alkaline solution, or the like. Among these, an aqueous alkaline solution is preferred because it is less environmentally hazardous and allows development with high sensitivity. The alkaline component in the aqueous alkaline solution is not particularly limited, but potassium hydroxide, sodium hydroxide, and / or sodium carbonate, or the like, are preferred. The concentration of the alkaline component is preferably 0.01 to 5 mass% in 100 mass% of the aqueous alkaline solution. When the concentration of the alkaline component is within this range, the solubility of the alkali-soluble resin is further improved, and the developability (development speed) can be further increased. It is more preferably 0.05 to 3 mass%, and even more preferably 0.1 to 1 mass%. A surfactant may be added to the aqueous alkaline solution. 4) The above steps 1) to 3) are carried out using a photosensitive resin composition containing a black color material to form a resin black matrix on a substrate. 5) Next, the color material of the photosensitive resin composition is changed successively to red (R), green (G), and blue (B), and the above steps 1) to 3) are repeated to form R, G, and B pixels to prepare RGB pixels. 6) Next, for the purpose of protecting the RGB pixels formed on the substrate and improving the surface smoothness, a protective film is formed as necessary. 7) When the color filter is a color filter for a liquid crystal display device, it is preferable to further form a columnar spacer. The columnar spacer can be produced by applying a photosensitive resin composition to a surface on which the spacers are to be formed in a thickness that corresponds to a desired spacer height, and then carrying out the above steps 1) to 3).

[0054] Here, when producing a color filter, it is preferable to further promote curing by heating after development (post-baking) when producing each member, and to completely remove the solvent if it remains. The temperature during post-baking is preferably 70 to 300°C. By setting this temperature, it is possible to more sufficiently suppress the coloring of pixels and the decrease in smoothness of the coating film due to thermal decomposition, and curing proceeds further and the coating film strength is further increased. The temperature is more preferably 100 to 250°C, even more preferably 150 to 230°C, and particularly preferably 180 to 230°C. Post-baking may be performed after development in forming each member (after the above 3) when producing each member), or may be performed after all members are formed.

[0055] <Display device members and display devices> The member for display device and the display device of the present invention have the above-mentioned cured product (cured film), but may further have one or more other constituent members. In recent years, with the progress of technology in display devices, etc., there is a strong demand for higher performance for each member used, and by using the photosensitive resin composition of the present invention, the reliability of the display quality and image quality of various display devices can be sufficiently improved to a degree that can fully meet such needs. The display device is not particularly limited, but for example, a liquid crystal display device, an organic EL display device, a solid-state image sensor, a touch panel display device, etc. are suitable. As the touch panel display device, a capacitance type display device is particularly preferred. The display device member may be a film-like single-layer or multi-layer member composed of the cured film, or a member in which the single-layer or multi-layer member is further combined with other layers, or a member containing the cured film in its structure (e.g., a color filter, etc.). EXAMPLES

[0056] The present invention will be described in more detail below with reference to examples. However, the following examples do not limit the present invention, and all modifications and variations within the scope of the present invention are included in the technical scope of the present invention. The present invention will be specifically described below with reference to manufacturing examples, examples, comparative examples, and characteristic evaluations. In the examples and comparative examples, % means mass % and parts means mass parts unless otherwise specified. Furthermore, the weight (wt %) measured in the present invention is the same value as the mass (wt %). (1) Weight average molecular weight: Mw Measurements were performed using GPC (HLC-8220GPC, manufactured by Tosoh Corporation) with THF as the eluent and a TSKgel SuperHZM-N (manufactured by Tosoh Corporation) column, and calculations were made in terms of standard polystyrene. (2) Solids Approximately 0.3 g of the copolymer solution prepared in the manufacturing example was weighed out in an aluminum cup, and about 1 g of acetone was added to dissolve it, and then it was naturally dried at room temperature. After that, it was dried at 140°C for 3 hours using a hot air dryer (product name: PHH-101, manufactured by Espec Corporation), and then it was cooled in a desiccator and its weight was measured. From the weight loss, the weight of the solid content (resin) of the polymer solution was calculated. (3) Acid value 1.5 g of the copolymer solution prepared in the Production Example was precisely weighed out, dissolved in a mixed solvent of 90 g of acetone and 10 g of water, and titrated with a 0.1 N KOH aqueous solution. The titration was performed using an automatic titrator (product name: COM-555, manufactured by Hiranuma Sangyo Co., Ltd.), and the acid value per 1 g of polymer was calculated from the solid content concentration (mg KOH / g). (4) Moisture content 1.0 g of the photosensitive resin composition B (Blue resist) prepared in the examples and comparative examples was precisely weighed and titrated with a titrant (HYDRANAL Composite 5K, manufactured by Wako Pure Chemical Industries, Ltd.) The titration was performed using an automatic moisture measuring device (product name: AQV-200, manufactured by Hiranuma Sangyo Co., Ltd.).

[0057] The following alkali-soluble resins were used: [Production Example 1] Production of copolymer solution (A-1) A separable flask with a cooling tube was prepared as a reaction vessel. On the other hand, 15 g of (α-allyloxymethyl)methyl acrylate (AOMA), 20 g of methacrylic acid (MAA), 55 g of isononyl acrylate (AIN), 10 g of methyl methacrylate (MMA), and 2 g of t-butylperoxy-2-ethylhexanoate (trade name "Perbutyl (registered trademark) O", manufactured by Nippon Oil & Fats Co., Ltd., hereinafter also referred to as PBO) were charged as a monomer composition into the monomer dropping vessel and mixed by stirring. In addition, 1.2 g of β-mercaptopropionic acid (MPA) and 18 g of propylene glycol monomethyl ether acetate (PGMEA) were charged as a chain transfer agent solution into the chain transfer agent dropping vessel and mixed by stirring.

[0058] 112g of PGMEA and 56g of propylene glycol monomethyl ether (PGME) were charged into the reaction vessel, and after replacing with nitrogen, the temperature of the reaction vessel was raised to 90°C by heating in an oil bath while stirring. After the temperature of the reaction vessel stabilized at 90°C, the monomer composition and the chain transfer agent solution were dropped. While maintaining the temperature at 90°C, the monomer composition was dropped over 180 minutes and the chain transfer agent solution was dropped over 210 minutes. After the drop of the chain transfer agent solution was completed, 0.5g of PBO was added. After another 30 minutes, the vessel was heated to 115°C. After maintaining the temperature at 115°C for 1 hour, a gas inlet tube was attached to the separable flask, and bubbling of a mixed gas of oxygen / nitrogen = 7 / 93 (v / v) was started. Next, 8 g of glycidyl methacrylate (GMA), 0.04 g of 6-tert-butyl-2,4-xylenol (trade name "Topanol", manufactured by Tokyo Chemical Industry Co., Ltd.) as a polymerization inhibitor, and 0.4 g of dimethylbenzylamine (DMBA) as a catalyst were charged into the reaction vessel, and the mixture was reacted at 110°C for 1 hour and at 115°C for 7 hours. After that, the mixture was cooled to room temperature to obtain a copolymer solution (A-1) containing 36.8% by weight (mass%) of resin. The weight average molecular weight (Mw) of the resin was 13000, and the acid value was 100 mgKOH / g. The production conditions, solid content concentration, weight average molecular weight (Mw) and acid value of the copolymer solution are shown in Table 1 together with Production Examples 2 to 7. [Production Example 2] Production of copolymer solution (A-2) A separable flask equipped with a cooling tube was prepared as a reaction vessel. On the other hand, 15g of AOMA, 14.7g of MAA, 69.3g of AIN, 1g of MMA, and 2g of PBO were charged as a monomer composition in the monomer dropping vessel and mixed with stirring. In addition, 2.3g of MPA and 18g of PGMEA were charged as a chain transfer agent solution in the chain transfer agent dropping vessel and mixed with stirring.

[0059] PGMEA112g and PGME56g were charged into the reaction vessel, and after replacing with nitrogen, the temperature of the reaction vessel was raised to 90°C by heating in an oil bath while stirring. After the temperature of the reaction vessel stabilized at 90°C, the monomer composition and the chain transfer agent solution were dropped. While maintaining the temperature at 90°C, the monomer composition was dropped over 180 minutes and the chain transfer agent solution was dropped over 210 minutes. After the chain transfer agent solution was dropped, PBO0.5g was added. After another 30 minutes, the vessel was heated to 115°C. After maintaining 115°C for 1 hour, a gas inlet tube was attached to the separable flask, and bubbling of oxygen / nitrogen=7 / 93 (v / v) mixed gas was started. Next, GMA10g, topanol0.04g as a polymerization inhibitor, and DMBA0.4g as a catalyst were charged into the reaction vessel, and the reaction was carried out at 110°C for 1 hour and at 115°C for 7 hours. The mixture was then cooled to room temperature to obtain a copolymer solution (A-2) containing 36.4% by weight of resin. The resin had a weight average molecular weight (Mw) of 9000 and an acid value of 70 mgKOH / g. The production conditions, solid content, weight average molecular weight (Mw) and acid value of the copolymer solution are shown in Table 1. [Production Example 3] Production of copolymer solution (A-3) A separable flask equipped with a cooling tube was prepared as a reaction vessel. On the other hand, 15 g of dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate (MD), 14.7 g of MAA, 69.3 g of AIN, 1 g of MMA, and 2 g of PBO were charged as a monomer composition into the monomer dropping vessel and mixed with stirring. In addition, 2.3 g of MPA and 18 g of PGMEA were charged as a chain transfer agent solution into the chain transfer agent dropping vessel and mixed with stirring.

[0060] PGMEA112g and PGME56g were charged into the reaction vessel, and after replacing with nitrogen, the temperature of the reaction vessel was raised to 90°C by heating in an oil bath while stirring. After the temperature of the reaction vessel stabilized at 90°C, the monomer composition and the chain transfer agent solution were dropped. While maintaining the temperature at 90°C, the monomer composition was dropped over 180 minutes and the chain transfer agent solution was dropped over 210 minutes. After the chain transfer agent solution was dropped, PBO0.5g was added. After another 30 minutes, the vessel was heated to 115°C. After maintaining 115°C for 1 hour, a gas inlet tube was attached to the separable flask, and bubbling of oxygen / nitrogen=7 / 93 (v / v) mixed gas was started. Next, GMA10g, topanol0.04g as a polymerization inhibitor, and DMBA0.4g as a catalyst were charged into the reaction vessel, and the reaction was carried out at 110°C for 1 hour and at 115°C for 7 hours. The mixture was then cooled to room temperature to obtain a copolymer solution (A-3) containing 36.4% by weight of resin. The resin had a weight average molecular weight (Mw) of 9000 and an acid value of 72 mgKOH / g. The production conditions, solid content, weight average molecular weight (Mw) and acid value of the copolymer solution are shown in Table 1. [Production Example 4] Production of copolymer solution (A-4) A separable flask equipped with a cooling tube was prepared as a reaction vessel. On the other hand, 15g of AOMA, 36.5g of MAA, 47g of benzyl methacrylate (BzMA), 1.5g of MMA, and 2g of PBO were charged as a monomer composition into the monomer dropping vessel and mixed with stirring. Also, 3.2g of MPA and 18g of PGMEA were charged as a chain transfer agent solution into the chain transfer agent dropping vessel and mixed with stirring.

[0061] PGMEA112g and PGME56g were charged into the reaction vessel, and after replacing with nitrogen, the temperature of the reaction vessel was raised to 90°C by heating in an oil bath while stirring. After the temperature of the reaction vessel stabilized at 90°C, the monomer composition and the chain transfer agent solution were dropped. While maintaining the temperature at 90°C, the monomer composition was dropped over 180 minutes and the chain transfer agent solution was dropped over 210 minutes. After the chain transfer agent solution was dropped, PBO0.5g was added. After another 30 minutes, the vessel was heated to 115°C. After maintaining 115°C for 1 hour, a gas inlet tube was attached to the separable flask, and bubbling of oxygen / nitrogen=7 / 93 (v / v) mixed gas was started. Next, GMA33g, topanol0.04g as a polymerization inhibitor, and DMBA0.4g as a catalyst were charged into the reaction vessel, and the reaction was carried out at 110°C for 1 hour and at 115°C for 7 hours. The mixture was then cooled to room temperature to obtain a copolymer solution (A-4) containing 42.1% by weight of resin. The resin had a weight average molecular weight (Mw) of 9200 and an acid value of 126 mgKOH / g. The production conditions, solid content, weight average molecular weight (Mw) and acid value of the copolymer solution are shown in Table 1. [Production Example 5] Production of copolymer solution (A-5) A separable flask equipped with a cooling tube was prepared as a reaction vessel. On the other hand, 15g of AOMA, 35.5g of MAA, 47g of cyclohexyl methacrylate (CHMA), 2.5g of MMA, and 2g of PBO were charged as a monomer composition in a monomer dropping vessel and mixed with stirring. In addition, 4.0g of MPA and 18g of PGMEA were charged as a chain transfer agent solution in a chain transfer agent dropping vessel and mixed with stirring.

[0062] PGMEA112g and PGME56g were charged into the reaction vessel, and after replacing with nitrogen, the temperature of the reaction vessel was raised to 90°C by heating in an oil bath while stirring. After the temperature of the reaction vessel stabilized at 90°C, the monomer composition and the chain transfer agent solution were dropped. While maintaining the temperature at 90°C, the monomer composition was dropped over 180 minutes and the chain transfer agent solution was dropped over 210 minutes. After the chain transfer agent solution was dropped, PBO0.5g was added. After another 30 minutes, the vessel was heated to 115°C. After maintaining 115°C for 1 hour, a gas inlet tube was attached to the separable flask, and bubbling of oxygen / nitrogen=7 / 93 (v / v) mixed gas was started. Next, GMA33g, topanol0.04g as a polymerization inhibitor, and DMBA0.4g as a catalyst were charged into the reaction vessel, and the reaction was carried out at 110°C for 1 hour and at 115°C for 7 hours. The mixture was then cooled to room temperature to obtain a copolymer solution (A-5) containing 41.8% by weight of resin. The resin had a weight average molecular weight (Mw) of 6,500 and an acid value of 101 mgKOH / g. The production conditions, solid content, weight average molecular weight (Mw) and acid value of the copolymer solution are shown in Table 1. [Production Example 6] Production of copolymer solution (A-6) A separable flask equipped with a cooling tube was prepared as a reaction vessel. On the other hand, 15g of AOMA, 34g of acrylic acid (AA), 47g of AIN, 4g of MMA, and 2g of PBO were charged as a monomer composition in a monomer dropping vessel and mixed with stirring. In addition, 3.2g of MPA and 18g of PGMEA were charged as a chain transfer agent solution in a chain transfer agent dropping vessel and mixed with stirring.

[0063] PGMEA112g and PGME56g were charged into the reaction vessel, and after replacing with nitrogen, the temperature of the reaction vessel was raised to 90°C by heating in an oil bath while stirring. After the temperature of the reaction vessel stabilized at 90°C, the monomer composition and the chain transfer agent solution were dropped. While maintaining the temperature at 90°C, the monomer composition was dropped over 180 minutes and the chain transfer agent solution was dropped over 210 minutes. After the chain transfer agent solution was dropped, PBO0.5g was added. After another 30 minutes, the vessel was heated to 115°C. After maintaining 115°C for 1 hour, a gas inlet tube was attached to the separable flask, and bubbling of oxygen / nitrogen=7 / 93 (v / v) mixed gas was started. Next, GMA33g, topanol0.04g as a polymerization inhibitor, and DMBA0.4g as a catalyst were charged into the reaction vessel, and the reaction was carried out at 110°C for 1 hour and at 115°C for 7 hours. The mixture was then cooled to room temperature to obtain a copolymer solution (A-6) containing 42.0% by weight of resin. The resin had a weight average molecular weight (Mw) of 9200 and an acid value of 99 mgKOH / g. The production conditions, solid content, weight average molecular weight (Mw) and acid value of the copolymer solution are shown in Table 1. [Production Example 7] Production of copolymer solution (A-7) A separable flask equipped with a cooling tube was prepared as a reaction vessel. On the other hand, 36.5g of MAA, 62g of AIN, 1.5g of MMA, and 2g of PBO were charged as a monomer composition in the monomer dropping vessel and mixed with stirring. In addition, 3.2g of MPA and 18g of PGMEA were charged as a chain transfer agent solution in the chain transfer agent dropping vessel and mixed with stirring.

[0064] PGMEA112g and PGME56g were charged into the reaction vessel, and after replacing with nitrogen, the temperature of the reaction vessel was raised to 90°C by heating in an oil bath while stirring. After the temperature of the reaction vessel stabilized at 90°C, the monomer composition and the chain transfer agent solution were dropped. While maintaining the temperature at 90°C, the monomer composition was dropped over 180 minutes and the chain transfer agent solution was dropped over 210 minutes. After the chain transfer agent solution was dropped, PBO0.5g was added. After another 30 minutes, the vessel was heated to 115°C. After maintaining 115°C for 1 hour, a gas inlet tube was attached to the separable flask, and bubbling of oxygen / nitrogen=7 / 93 (v / v) mixed gas was started. Next, GMA33g, topanol0.04g as a polymerization inhibitor, and DMBA0.4g as a catalyst were charged into the reaction vessel, and the reaction was carried out at 110°C for 1 hour and at 115°C for 7 hours. The mixture was then cooled to room temperature to obtain a copolymer solution (A-7) containing 41.8% by weight of resin. The resin had a weight average molecular weight (Mw) of 9500 and an acid value of 100 mgKOH / g. The production conditions, solid content, weight average molecular weight (Mw) and acid value of the copolymer solution are shown in Table 1.

[0065] [Table 1] (Example 1 to Example 3, Example 6 and Comparative Examples 1 to 6 6 ) Photosensitive resin composition B (Blue resist) preparation 9.51g of the copolymer solution (A-1) as the binder resin (i.e., 3.5g of resin), 2.86g of DISPERBYK-2001 as the dispersant (1.3g of non-volatile content: manufactured by BYK Japan, hereafter referred to as byk2001), 1.6g of the pigment CI Pigment Violet 23 (manufactured by Clariant, hereafter referred to as PV23) as the coloring material, and 6.4g of CI Pigment Blue 15:6 (manufactured by BASF, hereafter referred to as PB15:6) were weighed into a 225ml mayonnaise bottle and diluted with PGMEA so that the non-volatile content concentration was 20% by weight. 64g of zirconia beads with a diameter of 1.0mm were added to this, and the bottle was covered. This was shaken with a paint shaker for 3 hours to perform a dispersion treatment. To this dispersion, 4.4 g of dipentaerythritol hexaacrylate (represented as DPHA) as a polyfunctional monomer, 4.89 g of the above copolymer solution (A-1) as a binder resin (i.e., 1.8 g of resin), 0.6 g of ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) (trade name "IRGACURE (registered trademark) OXE02", manufactured by BASF Japan Ltd., hereinafter referred to as OXE02) as a photopolymerization initiator, and 0.4 g of SEESORB707 (S707) (manufactured by Shipro Chemical Co., Ltd.) as a UV absorber were added, and the mixture was diluted with PGMEA so that the non-volatile content concentration was 20% by weight. After removing the zirconia beads, the mixture was filtered through a filter with a pore size of 1.0 μm to prepare a photosensitive resin composition B1. Similarly, photosensitive resin compositions B2 to B10 were prepared using the copolymer solutions (A-2 to A-7) as the binder resin. For resin composition B10, after the moisture content was measured, ion-exchanged water was added so that the moisture content was 0.15 mass %. The following UV absorbers (UVA) were used: TINUVIN 479 (T479), TINUVIN 326 (T326), TINUVIN 384 (T384) (BASF Japan) SEESORB707 (S707), SEESORB107 (S107) (manufactured by Shipro Chemicals) <Developing method> The above photosensitive resin compositions B1 to B10 were applied onto a 10 cm square glass substrate using a spin coater and dried in an oven at 90° C. for 3 minutes. After drying, a photomask having a line and space of 2 to 100 μm was placed 100 μm away from the coating, and the coating was irradiated with 100 mJ / cm 2 using a UV aligner (product name "TME-150RNS", manufactured by TOPCON Corporation) equipped with a 2.0 kW ultra-high pressure mercury lamp. 2 (converted into 365 nm illuminance). After UV irradiation, a 0.05% aqueous potassium hydroxide solution was sprayed onto the coating film using a spin developer to dissolve and remove the unexposed areas, and the remaining exposed areas were developed by washing with pure water for 10 seconds to form a line and space pattern. The obtained pattern was subjected to the above evaluations (5) to (7). The results are shown in Table 2. (5) Development speed The development speed was determined as the shortest time required for a pattern to be formed upon development. (6) Adhesion After exposure, alkaline development was performed for the above-mentioned development speed (shortest time) + 10 seconds, and then the presence or absence of defects in the pattern was observed. The minimum line and space mask width without defects was defined as adhesion. (7) CD (thick line) The width and height of the pattern were measured using a laser microscope (product name "VK-9700", manufactured by Keyence Corporation). The CD was calculated by subtracting the width of the mask used to create the measured pattern from the width of the pattern after measurement. (8) Resin composition B stability The viscosity of Resin Composition B at 25° C. was measured using a cone-plate type rotational viscometer (TVE22LT, manufactured by Toki Sangyo Co., Ltd.) The viscosity immediately after preparation was compared with that after storage at 40° C. for 65 hours. A standard rotor (name: 1°34´×R24) was used for the cone plate. The rate of change in Table 2 was calculated using the following formula. Rate of change = Measurement value after storing for 65 hours at 40℃ / Measurement value immediately after adjustment (Formula)

[0066] [Table 2] By comparing the Examples and Comparative Examples, the superiority of the photosensitive resin composition containing the specific component of the present invention (mixed solution of mill base and clear resist) was confirmed. In Comparative Example 1 (composition B7) and Comparative Example 3 (composition B9), since no ultraviolet absorbent is contained, the CD value is high and line thickening is noticeable compared to the compositions containing other ultraviolet absorbents. In Comparative Example 2 (composition B8), since the alkali-soluble resin does not contain a resin having a specific structure with a heterocycle in the main chain, it is understood that the viscosity change rate is high and the storage stability is low. ~ Example 3, Example 6 (Composition B1 ~ composition B3, Composition B6) contains a resin with a specific structure having a heterocycle in the main chain as an alkali-soluble resin, and therefore has a low viscosity change rate and high storage stability. Comparative Example 5 Comparing (Composition B4) with Comparative Example 4 (Composition B10), it can be seen that by reducing the water content in the composition from 0.15% by mass to 0.04% by mass, the viscosity change rate is reduced and storage stability is improved. In Examples 1 to 3 (Compositions B1 to B3) in which AIN (isononyl acrylate) was used as the resin raw material, the CD value was low, the fineness was good, the viscosity change rate was low, and the storage stability was good. Comparative Example 5 (Composition B4) and Comparative Example 6 In the case of (Composition B5), the CD value was slightly high, but the adhesion was high and the storage stability was good. It is considered that the inclusion of a resin using a monomer raw material having a long chain hydrocarbon group such as AIN results in good micronization. Example 2 and Example 3 (Compositions B2 and B3) containing S107 (benzophenone compound) as the ultraviolet absorbent had particularly low CD values ​​and good micronization. In Example 6 (composition B6), the amount of GMA added as the alkali-soluble resin is large, and it is believed that the development speed is high because the resin contains a resin that is highly hydrophilic due to the hydroxyl group generated when GMA is added. [Industrial Applicability]

[0067] Components such as color filters having fine pixel patterns obtained by curing the photosensitive resin composition of the present invention can be suitably used in the electric and electronic fields, such as image display devices.

Claims

1. A photosensitive resin composition comprising an alkali-soluble resin, a polymerizable monomer, a colorant, a photopolymerization initiator, an ultraviolet absorber, and a solvent, the alkali-soluble resin being represented by the following general formula (1) or (2): 【Chemistry 1】 (In the formula, R 1 and R 3 R is the same or different and represents a hydrogen atom or an organic group having 1 to 30 carbon atoms. 2 represents a hydrogen atom or a methyl group. X, Y and Z are the same or different and represent a methylene group, a methylene group in which a hydrogen atom is substituted with a methyl group, an oxygen atom, a sulfur atom, or an imino group. However, at least one of X, Y and Z represents an oxygen atom, a sulfur atom or an imino group. A photosensitive resin composition comprising a heterocycle-containing structural unit represented by the following general formula (5), and a structural unit represented by the following general formula (6): 【Chemistry 2】 (In the formula, R 4 represents a hydrogen atom or a methyl group; R 5 represents an n-pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 2,2-dimethylpropyl group, a 1-ethylpropyl group, an n-hexyl group, a 1,1-dimethylpropyl group, a 1,2- dimethylpropyl group, 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 4-methylpentyl group, 1,1-dimethylbutyl group, 1,2-dimethylbutyl group, 1,3-dimethylbutyl group, 2,2-dimethylbutyl group, 2,3-dimethylbutyl group, 3,3-dimethylbutyl group, 1-ethylbutyl group, 2-ethylbutyl group, 1,2,2-trimethylpropyl group, 1-ethyl-1-methylpropyl group, 1-ethyl-2-methylpropyl group, n-heptyl group, n-octyl group, 2-ethylhexyl group, n-nonyl group, isononyl group, n-decyl group, n-undecyl group, n-dodecyl group, n-tridecyl group, n-tetradecyl group, n-pentadecyl group, n-hexadecyl group, n-heptadecyl group, n-octadecyl group, n-nonadecyl group, or n-eicosyl group.

2. The photosensitive resin composition according to claim 1, characterized in that the monomer providing the structural unit represented by the general formula (5) is hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, or behenyl (meth)acrylate.

3. A photosensitive resin composition as described in claim 1 or 2, characterized in that the acid value of the alkali-soluble resin is 20 mg KOH / g or more and 100 mg KOH / g or less.

4. A photosensitive resin composition described in any one of claims 1 to 3, characterized in that the content ratio of the structural unit represented by the general formula (5) is 20 mass% or more and 80 mass% or less, relative to 100 mass% of all structural units of the alkali-soluble resin.

5. 5. The photosensitive resin composition according to claim 1, wherein the photopolymerization initiator is an oxime-based initiator having a maximum absorption wavelength in a wavelength region of 350 nm to 500 nm.

6. 6. The photosensitive resin composition according to claim 1, wherein the ultraviolet absorber is at least one selected from the group consisting of a benzotriazole compound, a benzophenone compound, and a triazine compound.

7. The photosensitive resin composition according to claim 6, wherein the ultraviolet absorber is a benzophenone compound represented by general formula (10). 【Chemistry 3】 (In the formula, R 11 and R 12 each represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.)

8. A cured product obtained by curing the photosensitive resin composition according to any one of claims 1 to 7.

9. A color filter comprising the cured product according to claim 8.

10. A display device comprising the color filter according to claim 9.

Citation Information

Patent Citations

  • Photosensitive resin composition and image forming method

    JP2001235856A

  • Novel alkali-soluble resin having main chain ring structure, and use thereof

    JP2010168581A

  • Curable resin composition for photo spacer, and columnar spacer

    JP2013178407A

  • Coloring composition for color filter and color filter

    JP2018066778A

  • Photosensitive resin composition

    JP2020177091A