Thermal expansion refractory
The thermally expandable refractory material with graphite A and an expansion start retardant ensures sustained expansion to close gaps and prevent fire spread by delaying expansion onset, addressing the limitations of conventional materials.
Patent Information
- Application Number
- JP2020103395
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-15
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-06-15
AI Technical Summary
Conventional thermally expandable fireproof materials fail to effectively close gaps between fittings and frames due to warping, allowing fire to spread despite initial expansion, as they lose expansion capability over time.
A thermally expandable refractory material containing thermally expandable graphite A and an expansion start retardant, such as thermally expandable graphite B or an endothermic agent, is developed to delay the start of expansion, ensuring sustained expansion even after prolonged exposure to heat.
The material maintains excellent thermal expansion properties even after prolonged heat exposure, effectively closing gaps and preventing fire spread by delaying the expansion onset.
Smart Images

Figure 0007557289000004 
Figure 0007557289000005 
Figure 0007557289000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermally expandable refractory material containing thermally expandable graphite. [Background technology]
[0002] In the field of construction, fireproof materials are used in building materials such as fittings, pillars, and wall materials for fire prevention. As fireproof materials, thermally expandable fireproof materials, which are resins mixed with thermally expandable graphite in addition to flame retardants and inorganic fillers, are used (see, for example, Patent Document 1). Such thermally expandable fireproof materials expand when heated, and the combustion residue forms a fireproof insulation layer, thereby exhibiting fireproof insulation performance. A thermally expandable fire-resistant material containing thermally expandable graphite is placed, for example, in the gap between fittings such as doors and windows installed in openings of a building and the frames surrounding them, such as door frames and window frames; in the event of a fire, the sheet expands in the thickness direction to close the gap between the fittings and the frames and prevent the fire from spreading. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-141463 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, it has been found that even when a heat-expandable fire-resistant material containing heat-expandable graphite is used, in the event of a fire, over a long period of time, heat can cause fittings such as doors and windows to warp, widening the gap between the fittings and the frames. In such cases, the heat-expandable fire-resistant material may not be able to expand sufficiently to close the gap, making it impossible to prevent the fire from spreading. Therefore, the present invention aims to provide a heat-expandable fire-resistant material that has superior heat expansion properties (late-stage expansion properties) after a long period of time has passed during a fire compared to conventional fire-resistant materials, and that can easily close the gap between the building materials and the frame material even after the gap has widened, thereby preventing the spread of fire. [Means for solving the problem]
[0005] As a result of intensive research to solve the above problems, the present inventors have found that the above problems can be solved by a thermally expandable fireproof material containing a resin, thermally expandable graphite A, and an expansion initiation retarder that delays the initiation of expansion of the thermally expandable graphite A. That is, the present invention relates to the following [1] to
[15] . [1] A thermally expandable fire-resistant material comprising a resin, thermally expandable graphite A, and an expansion initiation retarder that delays the initiation of expansion of the thermally expandable graphite A. [2] The thermally expandable fireproof material according to the above [1], wherein the expansion initiation retarder is at least one selected from thermally expandable graphite B having a lower expansion initiation temperature than thermally expandable graphite A, and a heat-absorbing agent. [3] The thermally expandable fireproof material according to the above item [2], wherein the thermal expansion onset temperature of the thermally expandable graphite A is TA and the thermal expansion onset temperature of the thermally expandable graphite B is TB, and the difference between TA and TB (TA-TB) is 40°C or more. [4] The thermally expandable fireproof material according to the above [2] or [3], wherein the ratio of the content of the thermally expandable graphite A to the content of the thermally expandable graphite B (content of the thermally expandable graphite A / content of the thermally expandable graphite B) is 10 / 90 to 90 / 10. [5] The thermally expandable fireproof material according to any one of the above [2] to [4], wherein the difference between the thermal expansion onset temperature of the thermally expandable graphite A and the endothermic onset temperature of the heat absorption agent, TA-TC, is 30°C or more. [6] The heat-expandable fire-resistant material according to any one of the above [2] to [5], wherein the ratio of the content of the heat-expandable graphite A to the content of the heat-absorbing agent (content of the heat-expandable graphite A / content of the heat-absorbing agent) is 90 / 10 to 99 / 1. [7] The thermally expandable fire-resistant material according to any one of the above [1] to [6], wherein the total thermally expandable graphite content is 20 to 500 parts by mass per 100 parts by mass of the resin. [8] The thermally expandable fire-resistant material according to any one of the above [1] to [7], further comprising a flame retardant. [9] The thermally expandable fire-resistant material according to any one of the above [1] to [8], wherein the resin is a thermoplastic resin.
[10] The thermally expandable fire-resistant material according to any one of the above [1] to [9], wherein the resin is at least one selected from the group consisting of ethylene-vinyl acetate copolymer, polyvinyl acetate resin, chloroprene rubber, phenol resin, polyacrylonitrile resin, and polycarbonate resin.
[11] The thermally expandable fire-resistant material according to any one of the above [1] to
[10] , wherein the resin is at least one selected from an ethylene-vinyl acetate copolymer containing a high-Vac component having a vinyl acetate content of 20% by mass or more, and a polyvinyl acetate resin.
[12] The thermally expandable fire-resistant material according to
[10] or
[11] above, wherein the ethylene-vinyl acetate copolymer contains a low MFR component having a melt flow rate (MFR) at 190°C of 8.0 g / 10 min or less.
[13] The thermally expandable fire-resistant material according to any one of the above [1] to
[12] , wherein the resin is a phenolic resin.
[14] The thermally expandable fire-resistant material according to the above
[13] , wherein the phenolic resin is a novolac type.
[15] The thermally expandable fireproof material according to any one of the above [1] to
[14] , further comprising a crosslinking agent. Effect of the Invention
[0006] According to the present invention, it is possible to provide a heat-expandable fire-resistant material that has excellent heat expansion properties even after a long time has passed during a fire, and that is capable of easily closing the gap even after the gap between the fitting and the frame material has widened, thereby preventing the spread of fire. In this specification, excellent heat expansion properties even after a long time has passed during a fire are sometimes referred to as excellent late-stage expansion properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] [Thermally expandable fireproof material] The thermally expandable fireproof material of the present invention is a thermally expandable fireproof material containing a resin, thermally expandable graphite A, and an expansion start retarder that delays the start of expansion of the thermally expandable graphite A. Hereinafter, the thermally expandable fireproof material of the present invention may also be simply referred to as a fireproof material.
[0008] The fire-resistant material of the present invention contains thermally expandable graphite A. This allows the gap between the fittings and the frame material to be blocked in the event of a fire, preventing the spread of fire. In the present invention, when the fire-resistant material contains one type of thermally-expandable graphite, the one type of thermally-expandable graphite is referred to as thermally-expandable graphite A, and when the fire-resistant material contains two or more types of thermally-expandable graphite, the thermally-expandable graphite having the highest thermal expansion onset temperature is referred to as thermally-expandable graphite A, and the others are referred to as thermally-expandable graphite B.
[0009] (Expansion start retardant) The thermally expandable fireproof material of the present invention contains an expansion start retarder that delays the start of expansion of the thermally expandable graphite A. By containing the expansion start retarder, the later expansion property of the fireproof material is improved, and therefore, even after the gap between the fitting and the frame material has widened, the gap can be easily blocked, and the spread of fire can be prevented. The expansion start retarder is a compound capable of delaying the expansion start of thermally expandable graphite A by the action of heat insulation or heat absorption, and the type thereof is not limited. Examples of the expansion start retarder include thermally expandable graphite B, which has a lower expansion start temperature than thermally expandable graphite A, heat absorption agents, and foaming agents, but from the viewpoint of enhancing the later expansion property, it is preferable to use at least one selected from thermally expandable graphite B and heat absorption agents.
[0010] (Thermal Expandable Graphite) The thermally expandable graphite B, which is an expansion initiation retarder for the thermally expandable graphite A, has a lower expansion initiation temperature than the thermally expandable graphite A. This is thought to cause the thermally expandable graphite B to expand earlier than the thermally expandable graphite A during a fire, forming an expansion insulating layer around the thermally expandable graphite A, which delays the initiation of expansion of the thermally expandable graphite A. This increases the later expansion of the fire-resistant material.
[0011] From the viewpoint of further delaying the onset of expansion of thermally expandable graphite A, when the thermal expansion onset temperature of thermally expandable graphite A is TA and the thermal expansion onset temperature of the thermally expandable graphite B is TB, the difference between TA and TB (TA-TB) is preferably 40°C or more, more preferably 60°C or more, and even more preferably 80°C or more. From the viewpoint of enhancing the late expansion property, TA is preferably 160° C. or more, more preferably 170° C. or more, even more preferably 190° C. or more, and usually 300° C. or less. From the viewpoint of easily adjusting the difference between TA and TB within a desired range, TB is preferably 160° C. or less, more preferably 150° C. or less, even more preferably 130° C. or less, and usually 100° C. or more. The fire-resistant material of the present invention may contain a plurality of thermally expandable graphites B. In this case, TB is a weighted average value calculated from the expansion start temperatures and contents of the individual thermally expandable graphites. The expansion starting temperature of the thermally expandable graphite can be measured using a rheometer, and the expansion starting temperature is determined as the temperature at which the load increases due to the expansion of the thermally expandable graphite when the thermally expandable graphite is heated at a constant heating rate. The detailed measurement method is as described in the Examples.
[0012] From the viewpoint of enhancing the late expansion property of the fire-resistant material, the ratio of the content of thermally expandable graphite A to the content of thermally expandable graphite B (content of thermally expandable graphite A / content of thermally expandable graphite B) is preferably 10 / 90 to 90 / 10, more preferably 20 / 80 to 80 / 20, and even more preferably 40 / 60 to 60 / 40.
[0013] In the case where thermally expandable graphite A and thermally expandable graphite B are used in combination, from the viewpoint of enhancing the later expansion property of the fireproof material, the content of thermally expandable graphite A is preferably 10 to 250 parts by mass, more preferably 25 to 150 parts by mass, and even more preferably 50 to 100 parts by mass, relative to 100 parts by mass of the resin. The content of thermally expandable graphite B is preferably 10 to 250 parts by mass, more preferably 25 to 150 parts by mass, and even more preferably 50 to 100 parts by mass, relative to 100 parts by mass of the resin.
[0014] In addition, the total content of thermally expandable graphite contained in the fireproof material is preferably 20 to 500 parts by mass, more preferably 50 to 300 parts by mass, even more preferably 100 to 250 parts by mass, and even more preferably 110 to 200 parts by mass, relative to 100 parts by mass of the resin, from the viewpoint of increasing the later expansion property of the fireproof material. If the content of thermally expandable graphite is equal to or greater than these lower limits, the expansion pressure of the thermally expandable fireproof material is easily increased. If the content of thermally expandable graphite is equal to or less than these upper limits, shape retention, processability, and the like are improved.
[0015] The fireproof material of the present invention contains the above-mentioned thermally expandable graphite A and, if necessary, thermally expandable graphite B. These thermally expandable graphites are conventionally known substances that expand when heated, and are produced by treating raw material powders such as natural scaly graphite, pyrolytic graphite, and kish graphite with a strong oxidizing agent to generate graphite intercalation compounds. Examples of the strong oxidizing agent include inorganic acids such as concentrated sulfuric acid, nitric acid, and selenic acid, concentrated nitric acid, perchloric acid, perchlorates, permanganates, dichromates, and hydrogen peroxide. Thermally expandable graphite is a crystalline compound that maintains the layered structure of carbon. The thermally expandable graphite may be subjected to a neutralization treatment. That is, the thermally expandable graphite obtained by treating with a strong oxidizing agent or the like as described above may be further neutralized with ammonia, an aliphatic lower amine, an alkali metal compound, an alkaline earth metal compound, or the like.
[0016] The thermally expandable graphite in the present invention has an average aspect ratio of preferably at least 15, more preferably at least 20, and usually at most 1000. When the average aspect ratio of the thermally expandable graphite is equal to or more than these lower limit values, the expansion pressure of the refractory material is easily increased. The aspect ratio of the thermally expandable graphite is determined by measuring the maximum dimension (long diameter) and minimum dimension (short diameter) of 10 or more (e.g., 50) pieces of thermally expandable graphite, and averaging the ratio (maximum dimension / minimum dimension). Note that the thermally expandable graphites A and B in the present invention may have the same or different average aspect ratios.
[0017] The average particle size of the thermally expandable graphite is preferably 50 to 500 μm, and more preferably 100 to 400 μm. The average particle size of the thermally expandable graphite is determined as the average of the maximum dimensions of 10 or more (for example, 50) pieces of thermally expandable graphite. The minimum and maximum dimensions of the thermally expandable graphite can be measured, for example, using a field emission scanning electron microscope (FE-SEM). The thermally expandable graphites A and B in the present invention may have the same or different average particle diameters.
[0018] (Thermal absorption agent) In the present invention, a heat absorbing agent can be used as an expansion start retarder. It is considered that by using the heat absorbing agent, the expansion of the heat expandable graphite A is delayed and the later expansion of the fire resistant material is enhanced because the heat absorbing agent absorbs heat around the heat expandable graphite A during a fire. The endothermic agent used as the expansion start retarder has an endothermic start temperature equal to or lower than the expansion start temperature of thermally expandable graphite A. That is, when the endothermic start temperature of the endothermic agent is TC, the difference between the thermal expansion start temperatures TA and TC of thermally expandable graphite A (TA-TC) is 0°C or more. The difference between TA and TC (TA-TC) is preferably 10°C or more, and more preferably 30°C or more. When the value of TA-TC is in such a range, the expansion start of thermally expandable graphite A is easily delayed. The fireproof material of the present invention may contain a plurality of endothermic agents. In this case, TC is a weighted average value calculated from the endothermic onset temperatures and contents of the plurality of endothermic agents. The endothermic onset temperature of the endothermic agent can be measured by a thermogravimetric differential thermal analyzer (TG-DTA), specifically, by the method described in the Examples.
[0019] From the viewpoint of enhancing the late expansion property of the fire-resistant material, the ratio of the content of thermally expandable graphite A to the content of heat-absorbing agent (content of thermally expandable graphite A / content of heat-absorbing agent) in the fire-resistant material is preferably 90 / 10 to 99 / 1, more preferably 92 / 8 to 98 / 2, and even more preferably 94 / 6 to 96 / 4. The content of the heat-absorbing agent in the fireproof material is preferably 0.5 to 15 parts by mass, more preferably 2 to 10 parts by mass, and even more preferably 4 to 8 parts by mass, relative to 100 parts by mass of the resin, from the viewpoint of increasing the late expansion property of the fireproof material and improving moldability.
[0020] The endothermic amount of the endothermic agent is preferably 500 J / g or more, more preferably 600 J / g or more, and even more preferably 900 J / g or more. When the endothermic amount of the endothermic agent is within the above range, the heat absorption is improved, and the fire resistance is better. The endothermic amount of the endothermic agent is usually 4000 J / g or less, preferably 3000 J / g or less, and even more preferably 2000 J / g or less. The endothermic heat can be measured using a thermogravimetric differential thermal analyzer (TG-DTA), specifically, by the method described in the Examples.
[0021] The average particle size of the heat absorbing agent is more preferably 0.5 to 60 μm, further preferably 0.8 to 40 μm, and even more preferably 0.8 to 10 μm. When the average particle size of the heat absorbing agent is within the above range, the dispersibility of the heat absorbing agent in the fireproof material is improved, and the heat absorbing agent can be uniformly dispersed in the resin. The average particle size of the heat absorbing agent and the flame retardant described below is the median diameter (D50) value measured by a laser diffraction / scattering type particle size distribution measuring device.
[0022] The type of the heat absorbing agent is not particularly limited, but examples thereof include metal hydroxides, boron compounds, and metal salts. Examples of metal hydroxides include aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and hydrotalcite. The boron-based compound may be zinc borate, which may be a hydrate such as 2ZnO·3B2O5·3.5H2O. The metal salts include calcium sulfate, magnesium sulfate, etc., and the metal salts may be hydrates. Among these, calcium sulfate, aluminum hydroxide, calcium hydroxide, etc. are preferred as the heat absorbing agent.
[0023] The fireproof material of the present invention may contain a foaming agent as an expansion start retarder. As the foaming agent, either an organic foaming agent or an inorganic foaming agent can be used without any particular limitation. Examples of organic foaming agents include compounds having a nitroso group such as N,N'-dinitrosopentamethylenetetramine, compounds having an azo group such as azodicarbonamide and barium azodicarboxylate, 4,4-oxybis(benzenesulfonylhydrazide), hydrazodicarbonamide, etc. Examples of inorganic foaming agents include sodium hydrogen carbonate, etc. When a foaming agent is used, the amount of the foaming agent is not particularly limited, but is preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 8 parts by mass, relative to 100 parts by mass of the resin.
[0024] (resin) The fire-resistant material of the present invention contains a resin in which thermally expandable graphite A, an expansion initiation retarder, etc. are dispersed. The resin contained in the fireproof material of the present invention is preferably a thermoplastic resin, although it is not particularly limited. Examples of the resin include, but are not particularly limited to, polyolefin resins such as polypropylene resin, polyethylene resin, and ethylene-vinyl acetate copolymer, polyvinyl acetate resin, polyvinyl chloride resin, and rubber-based resins such as chloroprene rubber, fluororesins such as polytetrafluoroethylene, phenol resins, polycarbonate resins, and polyacrylonitrile resins. Among these, from the viewpoint of increasing the late expansion property and expansion pressure of the fire-resistant material and improving fire resistance, it is preferable that the resin is at least one selected from the group consisting of ethylene-vinyl acetate copolymer, polyvinyl acetate resin, chloroprene rubber, phenol resin, polyacrylonitrile resin, and polycarbonate resin.
[0025] <Ethylene-vinyl acetate copolymer, polyvinyl acetate> Among the above-mentioned resins, resins with a high vinyl acetate content are preferred from the viewpoint of increasing the post-expansion property of the fireproof material and improving its fire resistance. Specifically, the resin is preferably at least one selected from ethylene-vinyl acetate copolymers containing a high Vac component with a vinyl acetate content of 20% by mass or more and polyvinyl acetate resins, and more preferably polyvinyl acetate resins. The high Vac component with a vinyl acetate content of 20% by mass or more means an ethylene-vinyl acetate copolymer component with a vinyl acetate content of 20% by mass or more. Ethylene-vinyl acetate copolymers and polyvinyl acetate resins are non-chlorine-based resins, so they are unlikely to generate dioxins, and can be kneaded with thermally expandable graphite at a relatively low temperature without containing a plasticizer, and the moldability of the fireproof material is also good, so they are preferably used as resins contained in the fireproof material.
[0026] From the viewpoint of enhancing the late expansion properties of the fireproof material, the vinyl acetate content of the high-Vac component is preferably 25% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, and even more preferably 70% by mass or more.
[0027] The ethylene-vinyl acetate copolymer may contain an ethylene-vinyl acetate copolymer component (low Vac component) having a vinyl acetate content of less than 20% by mass, as long as the effects of the present invention are not impaired. From the viewpoint of increasing the late expansion property and expansion pressure of the fireproof material, the content of the high Vac component is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 100% by mass, based on the total amount of the ethylene-vinyl acetate copolymer.
[0028] From the viewpoint of increasing the expansion pressure of the fireproof material and improving the moldability, the ethylene-vinyl acetate copolymer preferably contains an ethylene-vinyl acetate copolymer component (hereinafter also referred to as a low MFR component) having a melt flow rate (MFR) of 8.0 g / 10 min or less at 190° C. The melt flow rate (MFR) of the low MFR component at 190° C. is more preferably 6.0 g / 10 min or less, and even more preferably 1.0 g / 10 min or less. From the viewpoint of the moldability of the fireproof material, the melt flow rate (MFR) of the low MFR component at 190° C. is preferably 0.05 g / 10 min or more, more preferably 0.1 g / 10 min or more, and even more preferably 0.3 g / 10 min or more. The melt flow rate of the ethylene-vinyl acetate copolymer at 190° C. is a value measured under a load of 2.16 kg in accordance with JIS K7210:1999.
[0029] Based on the total amount of the ethylene-vinyl acetate copolymer, the content of the low MFR component is preferably 70% by mass or more, and more preferably 90% by mass or more.
[0030] In addition, since MFR and vinyl acetate content are separate parameters that indicate the structure of an ethylene-vinyl acetate copolymer, there exist components that correspond to both low MFR components and high Vac components.
[0031] When using a high Vac component having a vinyl acetate content of 20% by mass or more and less than 50% by mass among ethylene-vinyl acetate copolymers, the high Vac component is preferably the above-mentioned low MFR component from the viewpoint of increasing the expansion pressure and improving fire resistance, etc. In other words, the MFR (190°C) of the high Vac component is preferably 8.0 g / 10 min or less, more preferably 6.0 g / 10 min or less, even more preferably 1.0 g / 10 min or less, and preferably 0.05 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 0.3 g / 10 min or more. When using a high Vac component having a vinyl acetate content of 50% by mass or more among ethylene-vinyl acetate copolymers, the Mooney viscosity ML(1+4) of the high Vac component at 100°C is preferably 10 to 50, more preferably 20 to 40, from the viewpoint of increasing the expansion pressure and improving fire resistance.
[0032] The polyvinyl acetate resin is a homopolymer of vinyl acetate, and by using this as a resin contained in the fireproof material, the late expansion property of the fireproof material is further increased, and the fire resistance is effectively improved. The weight average molecular weight of the polyvinyl acetate resin is preferably 100,000 to 1,000,000, more preferably 200,000 to 600,000, and even more preferably 300,000 to 500,000, from the viewpoint of improving the moldability of the fireproof material and increasing the expansion pressure. In this specification, the weight average molecular weight is a standard polystyrene equivalent value obtained by measurement by gel permeation chromatography (GPC).
[0033] <Resin: Chloroprene rubber> Chloroprene rubber can reduce the proportion of carbon contained in the fire-resistant material, and is therefore preferably used as the resin contained in the fire-resistant material from the viewpoint of enhancing fire resistance. As the chloroprene rubber, a sulfur-modified type (G type), a non-sulfur-modified type (W type), etc. can also be used. The Mooney viscosity ML(1+4) of the chloroprene rubber at 100° C. is preferably from 60 to 120, more preferably from 70 to 90. The chloroprene rubber having the Mooney viscosity ML(1+4) at 100° C. in the above range is likely to increase the expansion pressure of the fire-resistant material. In this specification, the Mooney viscosity is measured in accordance with JIS K6300.
[0034] When chloroprene rubber is used, the fireproof material preferably contains a plasticizer, which will be described later. From the viewpoint of improving the moldability of the fireproof material, among the plasticizers described later, an aliphatic ester plasticizer is preferable, among which an aliphatic ester plasticizer having an ether bond is more preferable, and dibutoxyethoxyethyl adipate is even more preferable. An example of a commercially available product of dibutoxyethoxyethyl adipate is Adeka Cizer RS-107 manufactured by ADEKA CORPORATION, which is called an adipate ether ester type. The amount of plasticizer used relative to the resin will be described later.
[0035] <Resin: Phenol resin> The fireproof material of the present invention preferably uses a phenolic resin as the resin. By using a phenolic resin, the late expansion property of the fireproof material is likely to be increased, and the fire resistance is likely to be improved. The phenolic resin is not particularly limited, but from the viewpoint of improving the moldability of the fireproof material, a novolac type phenolic resin is preferred. Novolac-type phenolic resins are resins obtained by reacting phenols with aldehydes in the presence of an acid catalyst. Here, the phenols are compounds having a phenol skeleton, mainly phenol, but also cresol, alkylphenols, etc. Examples of the alkylphenols include pt-butylphenol, p-octylphenol, p-nonylphenol, etc. Examples of the aldehydes that can be used include formaldehyde, furfural, higher aldehydes, etc. The acid catalyst may be an organic acid or an inorganic acid, and examples of the acid catalyst that can be used include strong acids such as oxalic acid, sulfuric acid, and paratoluenesulfonic acid, and metal salt catalysts such as Ca, Zn, Cd, Pb, and Co.
[0036] <Resin: Specific resin> The fireproof material of the present invention can improve the late expansion property of the fireproof material by containing at least one specific resin selected from polycarbonate resin, polyacrylonitrile resin, polyimide, polyether ether ketone (PEEK), and fluororesin. For example, even when an ethylene-vinyl acetate copolymer consisting of only the low Vac component is used as the resin, the late expansion property of the fireproof material can be improved by using it in combination with the specific resin, thereby improving the fire resistance. The specific resin is preferably at least one selected from polycarbonate resin and polyacrylonitrile resin. From the viewpoint of improving the moldability of the fire-resistant material, it is preferable to use at least one resin selected from ethylene-vinyl acetate copolymer and polyvinyl acetate in combination with the specific resin, and it is more preferable to use the ethylene-vinyl acetate copolymer in combination with the specific resin. When the specific resin is used, the content of the specific resin is preferably 5% by mass or more, more preferably 10% by mass or more, and preferably 50% by mass or less, more preferably 30% by mass or less, based on the total amount of resin contained in the fireproof material. When the content of the specific resin is equal to or more than these lower limits, the late expansion property of the fireproof material can be increased, and the fire resistance can be improved. When the content of the specific resin is equal to or less than these upper limits, the moldability of the fireproof material can be improved.
[0037] As the resin, only the specific resin may be used alone, but in this case, it is preferable to use a plasticizer in combination from the viewpoint of improving the moldability of the fireproof material. The type and amount of the plasticizer will be described later.
[0038] (Plasticizer) The fireproof material of the present invention may contain a plasticizer. By using a plasticizer, moldability is likely to be good. When a plasticizer is used, the content of the plasticizer is not particularly limited, but is preferably 10 to 200 parts by mass, more preferably 20 to 60 parts by mass, relative to 100 parts by mass of the resin. When the content of the plasticizer is equal to or more than these lower limits, the moldability of the fireproof material is improved. When the content of the plasticizer is equal to or less than these upper limits, the post-expansion property of the fireproof material is easily improved, and the expansion pressure is easily increased, thereby improving the fireproof property.
[0039] Specific examples of the plasticizer include di-2-ethylhexyl phthalate (DOP), di-n-octyl phthalate, diisononyl phthalate (DINP), diisodecyl phthalate (DIDP), diundecyl phthalate (DUP), or phthalate esters of higher alcohols or mixed alcohols having about 10 to 13 carbon atoms, di-2-ethylhexyl adipate (DOA), diisobutyl adipate (DIBA), dibutyl adipate (DBA), di-n-octyl adipate, di- Examples of the plasticizer include aliphatic ester plasticizers such as n-decyl adipate, diisodecyl adipate, di-2-ethylhexyl azelate, dibutyl sebacate, di-2-ethylhexyl sebacate, and dibutoxyethoxyethyl adipate; trimellitic acid ester plasticizers such as tri-2-ethylhexyl trimellitate (TOTM), tri-n-octyl trimellitate, tridecyl trimellitate, triisodecyl trimellitate, and di-n-octyl-n-decyl trimellitate; and process oils such as mineral oil.
[0040] (Crosslinking agent) The fireproof material of the present invention may contain a crosslinking agent. By using the crosslinking agent, the crosslinking of the resin proceeds due to the heat during a fire, and the later expansion of the fireproof material increases, improving the fireproofing. In addition, as the crosslinking of the resin proceeds, the viscosity increases, and the expansion pressure also increases, improving the fireproofing.
[0041] As the crosslinking agent, any known agent can be used without limitation, and examples thereof include organic peroxides and azo compounds. Examples of organic peroxides include 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 3-di-t-butyl peroxide, t-dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne, dicumyl peroxide, α,α'-bis(t-butylperoxyisopropyl)benzene, n-butyl-4,4-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)butane, 1,1-bis(t-butylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, t-butylperoxybenzoate, benzoyl peroxide, and t-butylperoxy-2-ethylhexyl carbonate. Examples of the azo compound include azobisisobutyronitrile and azobis(2,4-dimethylvaleronitrile).
[0042] Among the above-mentioned crosslinking agents, those that are unlikely to undergo a crosslinking reaction at the temperature (e.g., 70°C to 150°C) at which the components are kneaded when producing a fireproof material and that are likely to undergo a crosslinking reaction of the resin due to heat during a fire are preferred. From this viewpoint, the crosslinking agent is preferably dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, t-butylperoxy-2-ethylhexyl monocarbonate, or the like.
[0043] When the fireproof material contains a crosslinking agent, the content of the crosslinking agent is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and further preferably 1 to 5 parts by mass, based on 100 parts by mass of the resin.
[0044] (Flame retardant) The fire-resistant material of the present invention preferably contains a flame retardant, which improves fire resistance. Examples of the flame retardant include various phosphoric acid esters such as triphenyl phosphate (triphenyl phosphate), tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, and xylenyl diphenyl phosphate, metal phosphates such as sodium phosphate, potassium phosphate, and magnesium phosphate, metal phosphites such as sodium phosphite, potassium phosphite, magnesium phosphite, and aluminum phosphite, ammonium polyphosphate, red phosphorus, etc. Examples of the flame retardant also include compounds represented by the following general formula (1).
[0045] [ka]
[0046] In the general formula (1), R 1 and R 3 R are the same or different and represent hydrogen, a linear or branched alkyl group having 1 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms. 2 represents a hydroxyl group, a linear or branched alkyl group having 1 to 16 carbon atoms, a linear or branched alkoxyl group having 1 to 16 carbon atoms, an aryl group having 6 to 16 carbon atoms, or an aryloxy group having 6 to 16 carbon atoms.
[0047] Specific examples of the compound represented by the general formula (1) include methylphosphonic acid, dimethyl methylphosphonate, diethyl methylphosphonate, ethylphosphonic acid, n-propylphosphonic acid, n-butylphosphonic acid, 2-methylpropylphosphonic acid, t-butylphosphonic acid, 2,3-dimethyl-butylphosphonic acid, octylphosphonic acid, phenylphosphonic acid, dioctylphenylphosphonate, dimethylphosphinic acid, methylethylphosphinic acid, methylpropylphosphinic acid, diethylphosphinic acid, dioctylphosphinic acid, phenylphosphinic acid, diethylphenylphosphinic acid, diphenylphosphinic acid, bis(4-methoxyphenyl)phosphinic acid, etc. The flame retardants may be used alone or in combination of two or more.
[0048] As the flame retardant of the present invention, boron compounds and metal hydroxides can also be used. The boron-based compound may, for example, be zinc borate. Examples of metal hydroxides include aluminum hydroxide, magnesium hydroxide, calcium hydroxide, hydrotalcite, etc. When a metal hydroxide is used, water is generated by the heat generated by ignition, and the fire can be quickly extinguished.
[0049] Among the flame retardants, red phosphorus, phosphate esters such as triphenyl phosphate (triphenyl phosphate), aluminum phosphite, ammonium polyphosphate, and zinc borate are preferred from the viewpoints of safety, cost, etc. Among them, aluminum phosphite and ammonium polyphosphate are more preferred, and aluminum phosphite is even more preferred. Since aluminum phosphite has expansive properties, a fireproof material containing it is likely to have an increased expansion pressure, and is likely to more effectively improve fire resistance.
[0050] The average particle size of the flame retardant is preferably 1 to 200 μm, more preferably 1 to 60 μm, further preferably 3 to 40 μm, and further preferably 5 to 20 μm. When the average particle size of the flame retardant is within the above range, the dispersibility of the flame retardant in the fire-resistant material is improved, and the flame retardant can be uniformly dispersed in the resin and the amount of the flame retardant blended with respect to the resin can be increased. When the average particle size is outside the above range, the flame retardant is difficult to disperse in the resin, and it becomes difficult to uniformly disperse the flame retardant in the resin and to blend a large amount of the flame retardant in the resin. The average particle size of the flame retardant is the median diameter (D50) measured by a laser diffraction / scattering particle size distribution measuring device.
[0051] The content of the flame retardant in the fire-resistant material of the present invention is preferably 15 to 1000 parts by mass, more preferably 20 to 300 parts by mass, and even more preferably 30 to 100 parts by mass, relative to 100 parts by mass of the resin. When the content of the flame retardant is equal to or greater than these lower limits, the fire resistance of the fire-resistant material is improved. When the content of the flame retardant is equal to or less than these upper limits, the flame retardant is easily dispersed uniformly in the resin, and the moldability is excellent.
[0052] (Inorganic filler) The fire-resistant material of the present invention may further contain an inorganic filler other than the flame retardant and the thermally expandable graphite. The inorganic filler other than the flame retardant and the thermally expandable graphite is not particularly limited, and examples thereof include metal oxides such as alumina, zinc oxide, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, antimony oxide, and ferrite, metal carbonates such as basic magnesium carbonate, calcium carbonate, magnesium carbonate, zinc carbonate, strontium carbonate, and barium carbonate, silica, diatomaceous earth, dawsonite, barium sulfate, talc, clay, mica, montmorillonite, bentonite, activated clay, sepiolite, imogolite, sericite, glass fiber, glass beads, silica-based balloons, aluminum nitride, boron nitride, silicon nitride, carbon black, graphite, carbon fiber, carbon balloons, charcoal powder, various metal powders, potassium titanate, magnesium sulfate, lead zirconate titanate, zinc stearate, calcium stearate, aluminum borate, molybdenum sulfide, silicon carbide, stainless steel fiber, various magnetic powders, slag fiber, fly ash, and dewatered sludge. These inorganic fillers may be used alone or in combination of two or more kinds.
[0053] The average particle size of the inorganic filler is preferably 0.5 to 100 μm, more preferably 1 to 50 μm. When the content of the inorganic filler is low, a small particle size is preferable from the viewpoint of improving dispersibility, whereas when the content is high, a large particle size is preferable because the viscosity of the refractory material increases and the moldability decreases as the content increases.
[0054] When the fireproof material of the present invention contains an inorganic filler other than the flame retardant and the thermally expandable graphite, the content thereof is preferably 10 to 300 parts by mass, more preferably 10 to 200 parts by mass, based on 100 parts by mass of the resin. When the content of the inorganic filler is within the above range, the mechanical properties of the fireproof material can be improved.
[0055] The fireproof material of the present invention can contain various additive components as required within the scope of the invention. The type of the additive component is not particularly limited, and various additives can be used. Examples of such additives include lubricants, shrinkage inhibitors, crystal nucleating agents, colorants (pigments, dyes, etc.), ultraviolet absorbers, antioxidants, antiaging agents, dispersants, gelation accelerators, fillers, reinforcing agents, flame retardant assistants, antistatic agents, surfactants, vulcanizing agents, and surface treatment agents. The amount of additive added can be appropriately selected within a range that does not impair moldability, etc. The additives may be used alone or in combination of two or more.
[0056] (Expansion pressure) The fireproof material of the present invention has an expansion pressure of 3.0 N / cm 2 It is preferable that the expansion pressure of the fireproof material is 3.0N / cm or more. 2 If the above is the case, even if the building materials are exposed to flames for a long period of time in the event of a fire, the force of sealing the gaps between the building materials can be maintained, the fireproof material is less likely to peel off from the building materials, and the fire resistance is improved. In order to improve the fire resistance, the expansion pressure of the thermally expandable fireproof material is preferably 5.0 N / cm 2 More preferably, it is 7.0 N / cm 2 More preferably, it is 10.0 N / cm 2 That is all. The higher the expansion pressure of the thermally expandable fireproof material, the better, but in practice, it is 50N / cm 2 The following is the result. The expansion pressure of the fireproof material can be adjusted by the amount of thermally expandable graphite, the type of resin, whether or not a crosslinking agent is used, and so on.
[0057] The expansion pressure in the present invention is the expansion pressure at 500° C., and is measured as follows. (1) Prepare a sheet of fireproof material measuring 1.8 mm thick, 25 mm wide, and 25 mm long. (2) Place a hot plate and a force gauge 1.2 cm away from the surface of the hot plate. (3) The surface of the hot plate is heated to 500°C, the above-mentioned sheet-like fireproof material is placed on the surface of the hot plate, and a ceramic plate (made of calcium silicate, thickness 2 mm, width 30 mm, length 30 mm) is further placed on the fireproof material. (4) When the above fireproof material is heated on a hot plate at 500°C for 250 seconds, the expansion pressure is calculated by dividing the maximum stress measured with a force gauge by the area of the jig.
[0058] The expansion ratio of the fireproof material of the present invention is not particularly limited, but from the viewpoint of obtaining good fire resistance, it is preferably 10 to 500 times, more preferably 50 to 300 times, and further preferably 100 to 250 times. The expansion ratio can be determined by heating a sheet-shaped refractory material with a thickness of 1.8 mm, width of 25 mm and length of 25 mm at 600°C for 30 minutes and dividing the thickness of the refractory material after heating by the thickness of the refractory material before heating.
[0059] The fireproof material is preferably in the form of a sheet, and the thickness thereof is not particularly limited, but is preferably 0.2 to 10 mm, more preferably 0.5 to 3.0 mm, from the viewpoints of fire resistance and ease of handling.
[0060] (Method of manufacturing fireproof materials) The fireproof material of the present invention can be produced, for example, as follows. First, predetermined amounts of thermally expandable graphite A, resin, expansion initiation retarder, plasticizer which is blended as necessary, flame retardant, crosslinking agent, inorganic filler, and other components are kneaded in a kneading machine such as a kneading roll to obtain a fire-resistant resin composition. Next, the obtained fire-resistant resin composition is molded into a sheet or the like by a known molding method such as press molding, calendar molding, extrusion molding, etc., to obtain a fire-resistant material. The temperature during kneading and the temperature for forming into a sheet are preferably lower than the expansion start temperature of the thermally expandable graphite, and when a crosslinking agent is added, the temperature is preferably such that the crosslinking agent is unlikely to crosslink. Therefore, the kneading temperature is preferably 70 to 150°C, more preferably 90 to 140°C. The temperature for forming into a sheet is preferably 80 to 130°C, more preferably 90 to 120°C.
[0061] (Laminated sheet) The fireproof material of the present invention may be laminated with other sheet members or pressure-sensitive adhesive layers to form a laminate sheet. The laminate sheet includes, for example, a substrate and a fireproof material laminated on one or both sides of the substrate. The substrate is usually a woven fabric or nonwoven fabric. The fibers used for the woven fabric or nonwoven fabric are not particularly limited, but are preferably noncombustible or semi-noncombustible materials, such as glass fibers, ceramic fibers, cellulose fibers, polyester fibers, carbon fibers, graphite fibers, and thermosetting resin fibers. The laminate sheet can be obtained, for example, by forming the fire-resistant resin composition into a sheet on a substrate.
[0062] The laminate sheet may also include a fireproof material and an adhesive layer. The adhesive layer may be laminated on one or both sides of the fireproof material, for example. Furthermore, the laminate sheet may include a fireproof material, a substrate, and an adhesive layer. Such a laminate sheet may have a fireproof material on one side of the substrate and an adhesive layer on the other side, or a fireproof material and an adhesive layer may be provided in this order on one side of the substrate. The adhesive layer can be formed, for example, by transferring an adhesive coated on a release paper to the laminate sheet.
[0063] The fireproof material of the present invention and the laminated sheet using the same can be used specifically for various fittings in detached houses, apartment buildings, high-rise houses, high-rise buildings, commercial facilities, public facilities, and the like, various vehicles such as automobiles and trains, ships, and aircraft, among which it is preferable to use it for fittings. As fittings, specifically, they can be used for walls, beams, pillars, floors, bricks, roofs, boards, windows, shoji screens, doors, doors, sliding doors, transoms, wiring, piping, and the like, but are not limited thereto. The fireproof material of the present invention and the laminated sheet using the same can be applied, particularly to gaps in fittings such as windows, doors, and doors, to prevent flames from penetrating through the gaps in the event of a fire or the like. EXAMPLES
[0064] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0065] [Evaluation method] (I)Late distensibility The fireproof materials of each Example and Comparative Example were cut to a predetermined size (thickness 1.8 mm, width 25 mm, length 25 mm). The fireproof materials of the predetermined size were placed on the bottom surface of a stainless steel plate (98 mm square, thickness 0.3 mm) and fed into an electric furnace set at 160°C. The temperature was increased to 400°C at a rate of 5°C / min, and the fireproof materials were removed at 300°C and 400°C, and the expansion ratios at 300°C and 400°C were measured. The expansion ratio at 300°C is "thickness of the fireproof material at 300°C / thickness of the fireproof material before heating", and the expansion ratio at 400°C is "thickness of the fireproof material at 400°C / thickness of the fireproof material before heating". The later stage expansion property was evaluated by the following formula (I). The higher the value of formula (I), the better the later stage expansion property is judged to be. Formula (I) (Expansion ratio at 400°C) / (Expansion ratio at 300°C) The evaluation was based on the following criteria. A: The value of formula (I) is 1.7 or more B: The value of formula (I) is 1.5 or more and less than 1.7 C: The value of formula (I) is 1.2 or more and less than 1.5 D: The value of formula (I) is less than 1.2
[0066] (II) Expansion pressure The inflation pressure was measured by the following procedure. (1) The fireproof materials of each of the examples and comparative examples were cut to a predetermined size (thickness 1.8 mm, width 25 mm, length 25 mm). (2) A hot plate and a force gauge (Makita, ZTA-500N) were placed 1.2 cm away from the surface of the hot plate. 2 ) A plate-shaped jig was used. (3) The surface of the hot plate was heated to 500°C, the above-mentioned sheet-like fireproof material was placed on the surface of the hot plate, and a ceramic plate (made of calcium silicate, thickness 2 mm, width 30 mm, length 30 mm) was further placed on top of the fireproof material. (4) The above fireproof material was heated on a hot plate at 500° C. for 250 seconds, and the maximum stress measured with a force gauge was divided by the area of the jig to obtain the expansion pressure.
[0067] (III) Expansion ratio The expansion ratio was determined by cutting the refractory material of each Example and Comparative Example to a specified size (thickness 1.8 mm, width 25 mm, length 25 mm). The refractory material of the specified size was placed on the bottom surface of a stainless steel plate (98 mm square, thickness 0.3 mm), fed into an electric furnace, and heated at 600°C for 30 minutes. The thickness of the refractory material after heating was divided by the thickness of the refractory material before heating to determine the expansion ratio.
[0068] (IV) Fire resistance time A door component for evaluating fire resistance time was produced, consisting of a door made of a calcium silicate board (manufactured by Nippon Insulation Co., Ltd.) and a door frame. A gap of 1 cm was left between the side of the door of the door component for evaluating fire resistance time and the door frame. A fireproof material of each Example and Comparative Example cut to a specified size (thickness 1.8 mm, width 25 mm, length 1000 mm) was attached to the side of the door. It was then heated in a fireproof furnace according to the standard heating curve of ISO834, and the time until the fireproof material peeled off was measured. The longer the time until it peeled off, the more excellent the fireproofing of the fireproof material. Evaluation was based on the following criteria S: Time to peel off is 110 minutes or more A: The time it takes to peel off is between 105 and 110 minutes B: Time to peel off is more than 100 minutes but less than 105 minutes C: Time to peel off is between 95 and 100 minutes D: Time to peel off is less than 95 minutes
[0069] (VI) Formability When kneading with rolls, if the material is too hard to flow or too soft to flow easily and cannot maintain its shape, the yield will decrease. Moldability was determined by the yield of the material that could be taken out in sheet form after kneading, as shown below. A: 90% or more B: 70% or more but less than 90% C: 50% or more but less than 70% D: Less than 50%
[0070] (VII) Expansion start temperature of thermally expandable graphite In a rheometer ("Discovery HR-2", manufactured by TA Instruments), 0.5 g of a sample of thermally expandable graphite was placed on the sample stage and wrapped in aluminum foil to prevent the powder from falling off. The sample was grounded with a 25 mm diameter cone plate until the load became 0 [N]. From that state, the sample was heated at a constant heating rate (10 °C / min) from the set temperature of 50 °C using a Peltier heater, and the point when the load became 0.1 N was taken as the expansion start temperature.
[0071] (VIII) Endothermic onset temperature of endothermic agent The measurements were performed using a thermogravimetric differential thermal analyzer (TG-DTA). The measurement conditions were: from room temperature to 1000°C, the heating rate was 4°C / min, and the weight of the endothermic agent was 10 mg. The temperature at which the weight started to decrease from the obtained TG curve was determined as the endothermic onset temperature.
[0072] The various components used in each of the examples and comparative examples are as follows. (thermoplastic resin) 1. Ethylene-vinyl acetate copolymer EVA (1) "EV180" manufactured by Dow Polychemicals, Ltd. MFR at 190℃: 0.2g / 10min Vinyl acetate content: 33% by weight EVA (2) "EV260" manufactured by Dow Polychemicals, Inc. MFR at 190℃: 6.0g / 10min Vinyl acetate content: 28% by weight EVA (3) "V422" manufactured by Dow Polychemicals, Ltd. MFR at 190℃: 0.9g / 10min Vinyl acetate content: 20% by weight EVM (1) Lanxus "Revaprene 800" Mooney viscosity at 100°C ML(1+4): 27 Vinyl acetate content: 80% by weight
[0073] 2. Polyvinyl acetate resin Polyvinyl acetate (1) "VINNAPAS 4FS" manufactured by Tomoe Chemical Industry Co., Ltd. Weight average molecular weight: 300,000 g / mol Polyvinyl acetate (2) "VINNAPAS 25FS" manufactured by Tomoe Chemical Industry Co., Ltd. Weight average molecular weight: 500,000 g / mol
[0074] 3. Chloroprene rubber Chloroprene 1 "Skyprene TSR-56" manufactured by Tosoh Corporation Mooney viscosity at 100℃ ML(1+4):70 Chloroprene 2 "Skyprene 640" manufactured by Tosoh Corporation Mooney viscosity at 100℃ ML(1+4): 85
[0075] 4. Polyacrylonitrile resin ·“P-90H” manufactured by Shaoxing Gimel Advanced Materials Technology 5. Polycarbonate resin "Toughlon" manufactured by Idemitsu Kosan Co., Ltd. 6.Phenol Resin Novolac type phenolic resin "PR-50235" manufactured by Sumitomo Bakelite Co., Ltd.
[0076] (Thermal Expandable Graphite) Thermally expandable graphite: Fuji Graphite Co., Ltd. "EXP-50S120K", expansion start temperature 120℃ -Thermal expandable graphite: Fuji Graphite Co., Ltd. "EXP50S160", expansion start temperature 160℃ - Thermally expandable graphite ADT351, thermal expansion start temperature 170℃ Thermally expandable graphite: Fuji Graphite Co., Ltd. "EXP50HO", expansion start temperature 200℃
[0077] (Thermal absorption agent) Calcium sulfate, manufactured by Taihei Chemical Co., Ltd., endothermic start temperature 160℃, endothermic amount 700J / g Aluminum hydroxide, Nippon Light Metal Co., Ltd. "BF013", endothermic start temperature 200℃, endothermic amount 900J / g Calcium hydroxide, Suzuki Kogyo Co., Ltd. "CAOH-2", endothermic start temperature 421℃, endothermic amount 980J / g
[0078] (Flame retardant) Aluminum phosphite "APA100" manufactured by Taihei Chemical Industry Co., Ltd.
[0079] (Liquid plasticizer) Adipic acid ether ester type (ADEKA Cizer RS-107, manufactured by ADEKA Corporation)
[0080] (Examples 1 to 33, Comparative Examples 1 to 6) Resin, thermally expandable graphite, heat absorbing agent, flame retardant, and plasticizer were put into a roll and kneaded at 120°C for 5 minutes according to the formulation shown in Tables 1 to 4 to obtain a fire-resistant resin composition. The obtained fire-resistant resin composition was press-molded at 100°C for 3 minutes to obtain a sheet-shaped fire-resistant material having a thickness of 1.8 mm. The evaluation results are shown in Table 1.
[0081] [Table 1]
[0082] [Table 2]
[0083] [Table 3]
[0084] [Table 4]
[0085] As shown in the above examples, it was found that the fireproof material of the present invention containing the expansion start retarder, which is thermally expandable graphite or a heat-absorbing agent, has excellent late expansion property, long fire resistance time, and excellent fire resistance. In contrast, it was found that the fireproof materials of each comparative example not containing the expansion start retarder have poor late expansion property, short fire resistance time, and poor fire resistance.
Claims
1. The composition contains a resin, thermally expandable graphite A, and an expansion start retarder that delays the expansion start of the thermally expandable graphite A, the resin comprises an ethylene-vinyl acetate copolymer; The ethylene-vinyl acetate copolymer is an ethylene-vinyl acetate copolymer containing a high Vac component having a vinyl acetate content of 20% by mass or more, The expansion initiation retarder is thermally expandable graphite B having an expansion initiation temperature lower than that of the thermally expandable graphite A (excluding those containing zinc oxide).
2. 2. The thermally expandable refractory material according to claim 1, wherein the thermal expansion start temperature of the thermally expandable graphite A is TA and the thermal expansion start temperature of the thermally expandable graphite B is TB, and the difference between TA and TB (TA-TB) is 40°C or more.
3. The ratio of the content of the thermally expandable graphite A to the content of the thermally expandable graphite B (content of the thermally expandable graphite A / content of the thermally expandable graphite B) is 10 / 90 to 90 / 10. The thermally expandable fireproof material according to claim 1 or 2.
4. The thermally expandable fireproof material according to any one of claims 1 to 3, wherein the total content of thermally expandable graphite is 20 to 500 parts by mass per 100 parts by mass of resin.
5. The thermally expandable fire-resistant material according to any one of claims 1 to 4, further comprising a flame retardant.
6. The ethylene-vinyl acetate copolymer contains a low MFR component having a melt flow rate (MFR) of 8.0 g / 10 min or less at 190 ° C. The thermally expandable fire-resistant material according to any one of claims 1 to 5.
7. The thermally expandable fireproof material according to any one of claims 1 to 6, further comprising a crosslinking agent.
Citation Information
Patent Citations
Fire-resistant sheet-like molded article and sheet laminate
JP1999323148A
Thermally expandable resin composition
JP2012214646A
Thermally-expansible bond for external wall
JP2014159731A
Thermo expandable joint material for outside wall
JP2015098772A
Resin composition and molded body