Manufacturing method of mag-carbon bricks for LF pots

The method for producing magcarbon bricks with controlled compositions and molding techniques addresses the issues of high elasticity and expansion, enhancing durability and thermal stress resistance.

JP7557328B2Active Publication Date: 2024-09-27KROSAKI HARIMA CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020168678
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-05
Publication Date
2024-09-27
Estimated Expiration
2040-10-05

AI Technical Summary

Technical Problem

Existing magcarbon bricks for LF pots suffer from high elasticity and expansion due to low graphite content, leading to peeling and horizontal joint opening, and have issues with thermal stress and corrosion resistance.

Method used

A manufacturing method for magcarbon bricks with specific compositions of scaly graphite, silicon carbide, aluminum, and magnesia, along with controlled heat treatment and pressure molding, to reduce elasticity and enhance durability.

Benefits of technology

The method results in magcarbon bricks with low elastic modulus and high residual expansion, effectively preventing peeling and horizontal joint opening, while maintaining corrosion resistance and reducing energy loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557328000002
    Figure 0007557328000002
  • Figure 0007557328000001
    Figure 0007557328000001
Patent Text Reader

Abstract

To provide a method of producing LF-ladle magnesia-carbon bricks of low elasticity with a low graphite content, capable of suppressing opening of a horizontal joint from occurring while in use.SOLUTION: The method of producing LF-ladle magnesia-carbon bricks, includes kneading, molding and subsequently heat-treating a refractory raw material composition containing 3 to 9 mass% of scaly graphite, 1.5 to 4 mass% of aluminum, 1 to 6 mass% of silicon carbide, and 80 to 94 mass% of magnesia, with the content therein of expanded graphite being 2 mass% or less (including 0).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a magmatic carbon brick for a ladle furnace (LF ladle) used in a molten steel ladle (LF ladle) used in the LF (Ladle Furnace) process in a steelmaking process. In the present invention, the molten steel ladle used in the LF (Ladle Furnace) process is referred to as "LF ladle". [Background technology]

[0002] In LF ladles, the inside is lined with refractory material, and usually, unburned bricks containing castable or graphite are used for the metal line, and mag-carbon bricks (magnesia carbon bricks) are used for the slag line.

[0003] Magnesium-carbon bricks generally contain 10-20% by mass of graphite, giving them high thermal conductivity, and when used as lining bricks, the temperature of the steel shell of the molten steel ladle rises, causing problems such as a decrease in strength and deformation of the steel shell. This can also cause heat dissipation, which can lower the temperature of the molten steel and lead to energy loss in the molten steel ladle. To reduce this energy loss, it is possible to use magnesium-carbon bricks with a low graphite content, but reducing the amount of graphite makes the bricks highly elastic and highly expandable, resulting in a problem of insufficient durability.

[0004] In particular, in LF ladles, the molten steel is heated by electrodes, which creates a larger temperature difference than in other molten steel ladles, and this causes greater thermal stress in the mag-carbon bricks lining the LF ladles. For this reason, if mag-carbon bricks with reduced graphite are used in LF ladles, the bricks are more likely to peel off from their working surfaces due to thermal stress, shortening their lifespan. Furthermore, the bricks lining LF ladles repeatedly expand and contract in the vertical direction (up and down), which causes the gaps in the horizontal joints to become larger than in other molten steel ladles, and the insertion of metal into the cracks caused by the gaps promotes peeling.

[0005] For example, Patent Document 1 discloses a graphite-containing basic refractory material consisting of 40-90% by weight of spinel-dispersed periclase clinker, 3-9% by weight of graphite, and the remainder being magnesia clinker. This spinel-dispersed periclase clinker is described as having excellent spalling resistance because it has the effect of dispersing and attenuating the propagation of cracks. However, this spinel-dispersed periclase clinker contains 5-15% by weight of Al2O3, so there is a problem that the corrosion resistance is insufficient when applied to the slag line of an LF ladle.

[0006] In addition, in the examples of Patent Document 2, a mag-carbon brick with a graphite content of 2 mass% is disclosed, but this mag-carbon brick has a problem that the brick has high expansion and high elasticity due to its low graphite content. As a result, when the mag-carbon brick of this example is used in the slag line of an LF ladle, cracks parallel to the working surface are generated and spalling from the working surface is likely to occur for the above-mentioned reasons.

[0007] Patent Document 3 discloses a magnesia-carbonaceous unfired brick produced by adding metal powder and a binder to 100 wt% of a refractory aggregate composition mainly composed of 1 to 12 wt% thin-walled expanded graphite having a thickness of 12 μm or less, 0.5 to 10 wt% silicon carbide having a particle size of 150 mesh (Tyler standard sieve) or less, and the remainder being magnesia. However, as in Patent Document 2, the mag-carbon brick containing thin-walled expanded graphite has a problem of poor corrosion resistance because the filling of the clay during molding is poor and the structure has a high porosity. Therefore, when used in a slag line, the corrosion resistance is significantly reduced, shortening the life of the LF ladle. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Laid-Open No. 63-195161 [Patent Document 2] Patent No. 6026495 [Patent Document 3] JP 2000-319063 A Summary of the Invention [Problem to be solved by the invention]

[0009] The problem to be solved by the present invention is to provide a method for producing a mag-carbon brick for LF ladle which has low elasticity even with a low graphite content and can suppress the occurrence of gaps in horizontal joints during use. [Means for solving the problem]

[0010] The inventors have found that by adding a specific amount of silicon carbide to a mag-carbon brick with a low graphite content, the elastic modulus is reduced and the residual expansion is increased, and as a result, it is possible to obtain a mag-carbon brick for LF ladle with excellent durability by suppressing the occurrence of peeling from the working surface of the brick or opening of horizontal joints.

[0011] That is, according to the present invention, the following 1 to 2 The manufacturing method of mag-carbon bricks for LF pots is provided by 1. A method for producing a mag-carbon brick for an LF pot, comprising kneading a refractory raw material mixture containing 3-9 mass% of flaky graphite, 1.5-4 mass% of aluminum, 1-6 mass% of silicon carbide, and 80-94 mass% of magnesia, and having an expanded graphite content of 2 mass% or less (including 0), forming the mixture, and then heat-treating the mixture. And, When molding, the bricks are pressed using the upper and lower surfaces of the brick as the pressure surfaces, based on the position when the bricks are lined in the LF ladle. Manufacturing method of mag-carbon bricks for LF pots. 2. The thickness of the brick after molding in the direction of pressure applied during molding is 80 to 120 mm. 1 A method for producing the mag-carbon brick for LF ladle described in claim 1. Effect of the Invention

[0012] The mag-carbon bricks for LF ladles obtained by the manufacturing method of the present invention have a low elastic modulus and a large residual expansion even though they have a low graphite content. As a result, even when used in LF ladles with a larger temperature difference than other molten steel ladles, the bricks have excellent durability by suppressing peeling from the moving surface or opening of horizontal joints. In addition, the low graphite content makes it possible to suppress energy loss. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is an explanatory diagram showing a pressure direction during molding and a shape after molding in one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The refractory raw material composition used in the present invention contains 3 to 9 mass% of flaky graphite, 1.5 to 4 mass% of aluminum, 1 to 6 mass% of silicon carbide, and 80 to 94 mass% of magnesia, and the content of expanded graphite is 2 mass% or less (including 0).

[0015] Of these raw materials, magnesia is used as the main raw material in an amount of 80 to 94 mass% because it is a raw material with excellent slag resistance. If the magnesia content is less than 80 mass%, the slag resistance is insufficient, and if it exceeds 94 mass%, the spalling resistance is insufficient. As the magnesia, electrofused magnesia or sintered magnesia can be used, and magnesia having an MgO purity of 93 mass % or more can be used.

[0016] Silicon carbide is used at 1 to 6% by mass for the purpose of increasing the residual expansion and decreasing the elastic modulus. If silicon carbide is less than 1% by mass, these effects become insufficient, and if it exceeds 6% by mass, SiO2 generated by oxidation (SiC+O2→SiO2+C) produces a low melting point substance, decreasing corrosion resistance. Silicon carbide also has the effect of preventing oxidation, similar to aluminum, which will be described later. Silicon carbide generally used for refractories can be used without any problem, and silicon carbide with a SiC purity of 80% or more can be used. The particle size of silicon carbide can be 0.1 mm or less. By making the particle size 0.1 mm or less, the effect of increasing the residual expansion and the effect of decreasing the elastic modulus can be further improved.

[0017] In the present invention, the "particle size" refers to the size of the sieve mesh. For example, a particle size of 0.1 mm or less means that the particle passes through a sieve mesh of 0.1 mm.

[0018] It is presumed that silicon carbide in the brick exists in two types of states: one that is oxidized to SiO2 as described above when heated, and the other that is not oxidized and exists as it is. The oxidized SiO2 expands in volume, which is thought to contribute to increasing the residual expansion. On the other hand, silicon carbide that does not oxidize has a very large difference in thermal expansion coefficient from magnesia, which is the main raw material, and therefore, when the brick is heated, it is thought that gaps are generated around the silicon carbide particles due to the difference in expansion. Even after the temperature of the brick is lowered, the brick remains expanded, so gaps remain around the silicon carbide particles, which is thought to reduce the elastic modulus of the brick. Moreover, since the content of scaly graphite in the mag-carbon brick of the present invention is low, the thermal stress absorption effect (the effect of reducing the elastic modulus) of the scaly graphite is insufficient, and therefore the effect of reducing the elastic modulus by adding silicon carbide becomes more prominent.

[0019] The flake graphite is used in an amount of 3 to 9% by mass in order to reduce the elastic modulus. If the amount of flake graphite is less than 3% by mass, the elastic modulus becomes high, and if it exceeds 9% by mass, the thermal conductivity of the brick increases, resulting in large energy loss. It is known that the thermal conductivity of a mag-carbon brick is determined by the graphite content (for example, the diagram in Patent Document 1), and in the present invention, the upper limit of the flake graphite content is set to 9% by mass, which is not yet at a practical level for mag-carbon bricks for the slag line of LF ladles. As for the flaky graphite, the flaky graphite usually used in magnesium carbon bricks can be used.

[0020] Aluminum is used in an amount of 1.5 to 4% by mass for the purposes of preventing oxidation, imparting residual expansion, and imparting strength. If the aluminum content is less than 1.5% by mass, the strength becomes insufficient, and if it exceeds 4% by mass, the elastic modulus becomes high. Aluminum becomes Al2O3 when oxidized, and this Al2O3 reacts with MgO to impart residual expansion, but at the same time, it also densifies the structure. For this reason, if too much aluminum is used, there is a problem of reduced spalling resistance. Therefore, in the present invention, by using silicon carbide in combination, the amount of aluminum required for oxidation prevention and the like can be reduced, and there is also the advantage that the residual expansion can be increased while suppressing the decrease in spalling resistance.

[0021] In the present invention, the use of expanded graphite is not necessary, but if it is desired to further reduce the elastic modulus, it can be used at 2 mass % or less. However, if the amount of expanded graphite exceeds 2 mass %, the corrosion resistance decreases. The term "expanded graphite" used herein refers to graphite that is expanded several tens or even a hundred times by rapidly heating scaly graphite with sulfuric acid or the like contained between its structures, and in the present invention, this expanded graphite is crushed and made into a thin-walled shape. The expanded graphite may also be any commercially available material generally used as a raw material for refractories.

[0022] In addition to the above, the refractory raw material blend of the present invention can contain raw materials that are generally used as raw materials for magnesium-carbon bricks without adverse effects, so long as the total amount of these raw materials is about 5 mass % or less. Specifically, these raw materials include aluminum alloys, silicon, borides, pitch, carbon black, fibers, glass, etc.

[0023] The manufacturing method of the mag-carbon brick of the present invention is characterized by using the above-mentioned refractory raw material mixture, and is otherwise the same as the manufacturing method of a general mag-carbon brick. That is, an appropriate amount of binder is added to the refractory raw material mixture, kneaded, molded, and then heat-treated. The heat treatment temperature can be about 150 to 800°C. As the binder, a phenol resin, a furan resin, or the like with a solvent can be used.

[0024] In the manufacturing method of the mag-carbon brick of the present invention, it is preferable to perform pressure molding by using the upper and lower surfaces of the brick as the pressurizing surfaces based on the position when the brick is lined in the LF ladle. This allows the scaly graphite in the brick to be oriented parallel to the pressurizing surfaces, thereby reducing the elastic modulus in the up-down direction (vertical direction) when the brick is lined in the LF ladle, and reducing the thermal stress when the brick is used. As a result, the effect of suppressing peeling from the working surface of the brick can be obtained. As the molding machine, a hydraulic press or a friction press that is generally used in brick manufacturing can be used.

[0025] Furthermore, in the manufacturing method of the mag-carbon brick of the present invention, the thickness of the molded brick is preferably 80 to 120 mm in the pressure direction during molding. The thickness of the molded brick is almost the same after heat treatment, and the brick's vertical thickness (thickness in the direction of stacking height) as a product to be lined in an LF ladle is also about 80 to 120 mm. On the other hand, the thickness of bricks for conventional LF ladle in the direction of stacking height is 230 mm. That is, by making the thickness of the brick after molding 80 to 120 mm, the number of horizontal joints when lining the bricks increases compared to the conventional method. As a result, the horizontal joints act as an expansion absorption space, and the stress on the bricks when they thermally expand can be alleviated. EXAMPLES

[0026] The refractory raw material mixture shown in Table 1 was mixed with an appropriate amount of phenolic resin as a binder, and then formed into a drumstick-shaped brick shape as shown in Figure 1 using an oil press. The brick was then heat-treated (dried) at a maximum temperature of 250°C for 5 hours to obtain a mag-carbon brick. The pressure was applied in the direction of the arrow (up and down) in Figure 1 during molding, and the top and bottom surfaces of the brick were the pressure surfaces based on the position when the brick was lined in the LF ladle. The thickness of the brick after molding was 100 mm in the pressure direction during molding. The thickness of the mag-carbon brick after heat treatment (drying treatment) was also 100 mm. Samples for measuring physical properties were cut out from the mag-carbon brick, and the hot bending strength, residual expansion coefficient and elastic modulus were measured, and the corrosion resistance was evaluated.

[0027] The hot bending strength was measured in a nitrogen atmosphere at 1400°C in accordance with JIS R 2656. A hot bending strength of 12 MPa or more was considered to be acceptable.

[0028] The residual expansion coefficient is the result of measuring the linear change rate after reduction firing for 3 hours at 1400°C. A residual expansion coefficient of 0.5% or more was considered to pass.

[0029] The elastic modulus is the result of measuring the sonic elastic modulus after reduction baking at 1400℃ for 3 hours. In measuring the sonic elastic modulus, a sample with a size of 50×50×50mm was buried in coke breeze, heated to 1400℃ in an electric furnace, held for 3 hours, and allowed to cool naturally. After that, the sound velocity in the pressure direction and the non-pressure direction perpendicular to the pressure direction during molding of the sample were measured, and the elastic modulus in the pressure direction and the non-pressure direction were calculated. The lower the elastic modulus, the more effective it is in improving spalling resistance. Specifically, a sample was deemed to pass if its elastic modulus in the pressure direction was 25GPa or less and its elastic modulus in the non-pressure direction was 35GPa or less.

[0030] The corrosion resistance was evaluated by a rotational corrosion test. In the rotational corrosion test, the inner surface of a drum having a horizontal rotation axis was lined with a test brick, slag was charged and heated to erode the brick surface. The heat source was an oxygen-propane burner, the test temperature was 1750°C, the slag composition was CaO: 40% by mass, SiO2: 20% by mass, Al2O3: 20% by mass, FeO+Fe2O3: 20% by mass, and the discharge and charging of the slag was repeated 10 times every 30 minutes. After the test was completed, the dimensions of the maximum melted part of each brick (remaining dimensions of the brick) were measured and expressed as a corrosion resistance index, with the remaining dimensions of the brick in Example 1 listed in Table 1 being 100. The smaller the corrosion resistance index value, the better the corrosion resistance, and specifically, a value of 100 or less was considered to be acceptable.

[0031] The overall evaluation was made as pass (◯) if all the above evaluations were passed, and as fail (×) otherwise.

[0032] [Table 1]

[0033] Examples 1 to 3 have different silicon carbide contents within the range of the present invention, and all of them have excellent corrosion resistance, sufficient residual expansion coefficient, and low elastic modulus. In contrast, Comparative Example 1 does not contain silicon carbide, has a small residual expansion coefficient, and a high elastic modulus. Comparative Example 2 has a silicon carbide content exceeding the upper limit of the present invention, and has reduced corrosion resistance.

[0034] Examples 4 to 6 have different flake graphite contents within the range of the present invention, and all of them show good results. In contrast, Comparative Example 3 has a flake graphite content below the lower limit of the present invention, and has a high elastic modulus.

[0035] Examples 7 to 9 have different aluminum contents within the range of the present invention, and all of them show good results. In contrast, Comparative Example 4 has an aluminum content below the lower limit of the present invention, and the hot bending strength is reduced. Comparative Example 5 has an aluminum content above the upper limit of the present invention, and the elastic modulus is high.

[0036] Examples 11 and 12 contain 2 mass% or less of expandable graphite, and show good results. In contrast, Comparative Example 6 contains more than the upper limit of the present invention, and the corrosion resistance is reduced.

Claims

1. A method for producing a mag-carbon brick for an LF ladle, comprising kneading a refractory raw material composition containing 3 to 9 mass% of flake graphite, 1.5 to 4 mass% of aluminum, 1 to 6 mass% of silicon carbide, and 80 to 94 mass% of magnesia, and having an expanded graphite content of 2 mass% or less (including 0), forming the mixture, and then heat-treating the mixture, This manufacturing method for mag-carbon bricks for LF pots involves pressurizing the upper and lower surfaces of the brick as pressure surfaces, based on the position of the brick when it is lined in the LF pot.

2. 2. The method for producing a mag-carbon brick for an LF pot according to claim 1, wherein the thickness of the formed brick in the direction of pressure application during forming is 80 to 120 mm.

Citation Information

Patent Citations

  • MgO-C material slag line brick for steel ladle

    CN101811881A

  • Rotating device of alternating magnetic field

    JP1985026495A

  • Graphite-containing basic refractories

    JP1988195161A

  • Magnesia-carbon unburned refractory brick and molten steel vacuum degassing treatment equipment lined with the same

    JP2000319063A

  • Immersion tube of vacuum degassing furnace

    JP2011111627A