Zirconia calcined body suitable for dental use and its manufacturing method
A zirconia calcined body produced through high-pressure press-molding and controlled firing maintains translucency in dental prostheses, enabling one-visit treatments by shortening firing times and addressing thickness-related translucency loss.
Patent Information
- Application Number
- JP2021516278
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-25
- Filing Date
- 2020-04-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-04-24
AI Technical Summary
Existing methods for manufacturing zirconia dental prostheses in dental clinics require long firing times, complicating calculations and preventing one-visit treatments, and result in reduced translucency when fired for short times with thicker prostheses.
A zirconia calcined body is produced using a specific manufacturing method involving press-molding zirconia and a stabilizer at high pressure, ensuring that at least part of the stabilizer remains undissolved, and is fired at controlled temperatures to maintain translucency regardless of thickness.
The method allows for one-visit treatments by shortening firing time while maintaining excellent translucency in zirconia sintered bodies, even with thicknesses of 10 mm or more, without requiring adjustments based on geometric characteristics.
Smart Images

Figure 0007558932000010 
Figure 0007558932000011 
Figure 0007558932000012
Abstract
Description
[Technical field]
[0001] The present invention relates to a zirconia calcined body and a method for producing the same, and further relates to a dental material comprising the zirconia calcined body and a method for producing a zirconia molded body for producing the zirconia calcined body. [Background technology]
[0002] Zirconia is a compound that undergoes phase transitions between multiple crystal systems. Therefore, partially stabilized zirconia (PSZ) and fully stabilized zirconia, which are made by dissolving stabilizers such as yttria (yttrium oxide; Y2O3) in zirconia to suppress the phase transition, are used in various fields.
[0003] In the dental field, zirconia materials have been used as frame materials because they have high strength but low translucency. In recent years, with the improvement in the translucency of zirconia materials, dental prostheses are often made only from zirconia. Patent Document 1 discloses a colored zirconia sintered body that has high translucency and is suitable for dental use (especially for front teeth).
[0004] Traditionally, dental prostheses made only from zirconia were often produced in dental laboratories, but in recent years, they have increasingly been produced simply in dental clinics, in which case the zirconia needs to be fired in a short period of time.
[0005] Furthermore, because zirconia has high strength, it is expected to be used in many cases, including not only single crowns but also multiple crowns and bridges, where strength is required.
[0006] Patent Document 1 describes that for many cases such as inlays and bridges, the firing conditions are determined based on changes in various factors such as the maximum lateral thickness, maximum occlusal thickness, and maximum cross-sectional area of the prosthesis.
[0007] Patent Document 2 describes a zirconia sintered body that has uniform translucency all the way to the inside when sintered at a heating rate of 5° C. / min or less and a maximum holding temperature of 1550° C. or more. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Special Publication No. 2016-540562 [Patent Document 2] JP 2017-128466 A Summary of the Invention [Problem to be solved by the invention]
[0009] In the method described in Patent Document 1, complex calculations are performed by computer, so the time required for manufacturing the prosthesis is unclear, and as a result, one-visit treatment may not be achieved.
[0010] In the method of Patent Document 2, since firing requires at least 10 hours or more, one-visit treatment cannot be achieved. Therefore, there is a demand for a zirconia calcined body that exhibits a color tone suitable for dental use (particularly for use in dental clinics) even when fired in a short time. There is also a demand for a zirconia calcined body that can maintain the translucency of the sintered body even when fired in a short time. Furthermore, when the sintered body is thick (for example, 10 mm or more) after firing in a short time, the translucency may decrease. Therefore, there is a demand for a zirconia calcined body that can suppress the decrease in the translucency of the sintered body even when fired in a short time and the thickness of the sintered body after firing is 10 mm or more.
[0011] Therefore, an object of the present invention is to provide a zirconia calcined body which can be subjected to one-visit treatment due to a short firing time and which has excellent translucency regardless of the thickness of the obtained zirconia sintered body, and a method for producing the same. [Means for solving the problem]
[0012] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by producing a zirconia calcined body using a zirconia molded body produced by a specific production method, or by making a zirconia calcined body having a thickness of 10 mm or more and a specific bulk density. Based on this finding, the present inventors have conducted further research and have completed the present invention.
[0013] That is, the present invention includes the following inventions.
[0014] [1] Zirconia, A method for producing a zirconia molded body containing a stabilizer capable of suppressing a phase transition of zirconia, At least a portion of the stabilizer is not solid-dissolved in zirconia, A method for producing a zirconia molded body, comprising the step of press-molding a mixed powder of zirconia and the stabilizer at a pressure of 175 MPa or more to obtain a zirconia molded body. [2] The method for producing a zirconia molded body according to [1], wherein the stabilizer contains yttria. [3] The abundance ratio f of yttria not dissolved in the zirconia is calculated based on the following formula (1): y The method for producing a zirconia molded body according to [2], wherein the content of the zirconia powder is greater than 0%.
number
number
[10] The zirconia calcined body according to [8] or [9], wherein the stabilizer contains yttria.
[11] The fraction of yttria not dissolved in zirconia calculated based on the following formula (1): y The zirconia calcined body according to
[10] , wherein the content of is greater than 0%.
number
[12] A dental material comprising the zirconia calcined body according to any one of [8] to
[11] .
[13] The dental material described in
[12] , wherein the dental material is in a disk or block shape. Effect of the Invention
[0015] According to the present invention, a zirconia calcined body that can be subjected to one-visit treatment due to a short firing time and that has excellent translucency regardless of the thickness of the obtained zirconia sintered body, and a manufacturing method thereof can be provided. In particular, according to the present invention, a zirconia calcined body that can suppress a decrease in translucency of the sintered body after firing even when the firing time is short and the thickness of the sintered body after firing is large (for example, 10 mm or more), and a manufacturing method thereof can be provided.
[0016] By using the zirconia calcined body of the present invention, translucency can be maintained for many cases even if the firing conditions do not change depending on the geometric characteristics of the prosthesis, such as the maximum wall thickness or maximum component cross-sectional area or volume, the treatment time can be clearly defined before the prosthesis is manufactured, and a zirconia prosthesis can be obtained with a total firing time of 30 minutes or less under the above firing conditions. [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 is a schematic diagram of a zirconia sintered body in the case where the zirconia calcined body of the present invention has a multi-layer structure. [Diagram 2] 1 is an X-ray diffraction pattern of the calcined body produced in Example 1. [Diagram 3] 1 is an X-ray diffraction pattern of the calcined body produced in Example 3. [Figure 4] 1 shows an X-ray diffraction pattern of the calcined body produced in Comparative Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The zirconia calcined body of the present invention contains zirconia and a stabilizer capable of suppressing a phase transition of zirconia, and at least a part of the stabilizer is not solid-dissolved in the zirconia. The zirconia calcined body has a bulk density of 3.0 g / cm as measured by the Archimedes method using a test piece of the calcined body having a thickness of 10 mm or more, the test piece being made from the zirconia calcined body. 3 It is important that the bulk density is 3.1 g / cm or more. By satisfying this condition, the firing time is short, and the obtained zirconia sintered body has excellent translucency regardless of the thickness. The bulk density is preferably 3.1 g / cm or more. 3or more. The lower limit of the thickness of the test piece of the calcined body is preferably 12 mm or more, more preferably 13 mm or more, even more preferably 14 mm or more, and particularly preferably a thickness of the calcined body that will become a sintered body having a thickness of 10 mm or more when fired for 30 minutes. On the other hand, the upper limit is not particularly limited, and may be, for example, 40 mm or less, or 30 mm or less. The details of the method for measuring the bulk density will be described later in the examples. In addition, the bulk density measured by the Archimedes method using a test piece of the calcined body having a thickness of less than 10 mm made from the zirconia calcined body is also 3.0 g / cm. 3 It is preferable that the content is 3.1 g / cm or more. 3 Furthermore, the ratio of the bulk density measured by the Archimedes method using a test piece of the calcined body having a thickness of 10 mm or more to the bulk density measured by the Archimedes method using a test piece of a calcined body having a thickness of less than 10 mm produced from the zirconia calcined body is preferably 90% or more, more preferably 95% or more, and even more preferably 100%, in terms of excellent light transmittance regardless of thickness.
[0019] As described above, the zirconia calcined body of the present invention has a short firing time and has excellent translucency regardless of the thickness of the zirconia sintered body obtained. More specifically, the zirconia calcined body of the present invention is a zirconia calcined body containing zirconia and a stabilizer capable of suppressing the phase transition of zirconia, and the zirconia calcined body is fired for 30 minutes to prepare a first sintered body having a thickness of 1 mm and a second sintered body having a thickness of 10 mm. When the first translucency (hereinafter also simply referred to as "first translucency") of a test piece having a thickness of 0.5 mm prepared from the first sintered body is compared with the second translucency (hereinafter also simply referred to as "second translucency") of a test piece having a thickness of 0.5 mm prepared from the second sintered body, the ratio (ΔL2* / ΔL1*) of the second translucency to the first translucency is 90% or more, preferably 92% or more, and more preferably 95% or more. Moreover, the first translucency (ΔL1*) and the second translucency (ΔL2*) are preferably 10 or more, more preferably 12 or more, further preferably 14 or more, and particularly preferably 16 or more. The details of the method for measuring the translucency will be described later in the Examples. The firing temperature when the zirconia calcined body is fired to obtain a sintered body is, for example, preferably 1400° C. or more, more preferably 1450° C. or more. Moreover, the firing temperature is, for example, preferably 1650° C. or less, more preferably 1600° C. or less.
[0020] The zirconia calcined body of the present invention will be described in detail below. The zirconia calcined body can be a precursor (intermediate product) of the zirconia sintered body. In the present invention, the zirconia calcined body can refer to, for example, a block of zirconia particles (powder) that is not completely sintered.
[0021] The zirconia calcined body of the present invention contains zirconia and a stabilizer capable of suppressing the phase transition of zirconia. The stabilizer is preferably capable of forming partially stabilized zirconia. Examples of the stabilizer include calcium oxide (CaO), magnesium oxide (MgO), yttria, cerium oxide (CeO2), scandium oxide (Sc2O3), niobium oxide (Nb2O5), lanthanum oxide (La2O3), erbium oxide (Er2O3), praseodymium oxide (Pr6O 11 Examples of the stabilizer include oxides such as zirconia oxide (Sm2O3), samarium oxide (Sm2O3), europium oxide (Eu2O3) and thulium oxide (Tm2O3), and yttria is preferred. The stabilizer content in the zirconia calcined body and its sintered body of the present invention can be measured by, for example, inductively coupled plasma (ICP) emission spectrometry, fluorescent X-ray analysis, etc. In the zirconia calcined body of the present invention, the stabilizer content is preferably 0.1 to 18 mol%, more preferably 1 to 15 mol%, based on the total moles of zirconia and stabilizer.
[0022] The main crystal system of the zirconia in the calcined zirconia of the present invention is preferably a monoclinic system. In the present invention, the term "main crystal system is a monoclinic system" means that the proportion of the monoclinic system in the zirconia calculated by the following formula (2) with respect to the total amount of all crystal systems (monoclinic system, tetragonal system, and cubic system) in the zirconia is f m In the calcined zirconia of the present invention, the monoclinic fraction f in the zirconia calculated by the following formula (2) is m is preferably 55% or more, more preferably 60% or more, even more preferably 70% or more, even more preferably 75% or more, particularly preferably 80% or more, even more particularly preferably 85% or more, and most preferably 90% or more, based on the total amount of monoclinic, tetragonal and cubic crystals. mcan be calculated from the following formula (2) based on the peaks in the X-ray diffraction (XRD) pattern using CuKα radiation. The main crystal system in the calcined zirconia body may contribute to increasing the shrinkage temperature and shortening the firing time.
[0023] In the calcined zirconia body of the present invention, the peaks of the tetragonal and cubic crystal systems may not be substantially detected. m can be set to 100%.
[0024]
number
[0025] In formula (2), I m (111) and I m (11-1) indicates the peak intensity of the (111) and (11-1) planes of the monoclinic crystal system of zirconia, respectively. t (111) indicates the peak intensity of the (111) plane of the zirconia tetragonal crystal system. I c (111) indicates the peak intensity of the (111) plane of the cubic crystal system of zirconia.
[0026] In the zirconia calcined body of the present invention, it is necessary that at least a part of the stabilizer is not solid-dissolved in zirconia. The fact that a part of the stabilizer is not solid-dissolved in zirconia can be confirmed, for example, by the XRD pattern. When a peak derived from the stabilizer is confirmed in the XRD pattern of the zirconia calcined body, the stabilizer that is not solid-dissolved in zirconia is present in the zirconia calcined body. When the entire amount of the stabilizer is solid-dissolved, basically, a peak derived from the stabilizer is not confirmed in the XRD pattern. However, depending on conditions such as the crystal state of the stabilizer, even if there is no peak of the stabilizer in the XRD pattern, the stabilizer may not be solid-dissolved in zirconia. When the main crystal system of zirconia is a tetragonal and / or cubic system and there is no peak of the stabilizer in the XRD pattern, it is considered that most of the stabilizer, basically all of it, is solid-dissolved in zirconia. In the zirconia calcined body of the present invention, the entire stabilizer does not have to be solid-dissolved in zirconia. In the present invention, the term "the stabilizer is solid-dissolved" means that, for example, an element (atom) contained in the stabilizer is solid-dissolved in zirconia.
[0027] From the viewpoint of strength and translucency of the zirconia sintered body produced from the zirconia calcined body of the present invention, it is preferable to contain yttria as a stabilizer. The content of yttria is preferably 3 mol% or more, more preferably 3.5 mol% or more, even more preferably 3.8 mol% or more, and particularly preferably 4.0 mol% or more, based on the total moles of zirconia and yttria. When the content of yttria is 3 mol% or more, the translucency of the zirconia sintered body can be increased. In addition, the content of yttria is preferably 7.5 mol% or less, more preferably 7.0 mol% or less, even more preferably 6.5 mol% or less, and particularly preferably 6.0 mol% or less, based on the total moles of zirconia and yttria. When the content of yttria is 7.5 mol% or less, the strength reduction of the zirconia sintered body can be suppressed.
[0028] In the zirconia calcined body of the present invention, the abundance rate f of yttria that is not dissolved in zirconia (hereinafter sometimes referred to as "undissolved yttria") is y The fraction of undissolved yttria f can be calculated based on the following formula (1). y is preferably greater than 0%, more preferably 1% or more, even more preferably 2% or more, and particularly preferably 3% or more. y The upper limit of may be, for example, 15% or less, but preferably depends on the yttria content in the zirconia calcined body. When the yttria content is 3 mol% or more and less than 4.5 mol%, f y When the yttria content is 4.5 mol% or more and less than 5.8 mol%, f y When the yttria content is 5.8 mol% or more and less than 7.5 mol%, f y The fraction of undissolved yttria in the calcined zirconia body, f y In the case of a calcined body containing zirconia whose main crystal system is monoclinic, the translucency is affected by the calcination temperature. It is also affected by the average particle size of the raw material mixed powder containing zirconia and yttria. The presence of undissolved yttria in the calcined zirconia body allows a zirconia sintered body with high translucency to be obtained even after short firing time.
[0029] In the zirconia calcined body of the present invention, when the yttria content is 3 mol% or more and less than 4.5 mol%, f y is preferably 0.5% or more, more preferably 1.0% or more, and even more preferably 2.0% or more. When the yttria content is 4.5 mol% or more and less than 5.8 mol%, f y is preferably 1% or more, more preferably 2% or more, and even more preferably 3% or more. When the yttria content is 5.8 mol% or more and 7.5 mol% or less, f yis preferably 2% or more, more preferably 3% or more, and even more preferably 4% or more. In the zirconia calcined body of the present invention, when the yttria content is 3 mol% or more and less than 4.5 mol%, f m / f y is preferably 20 to 200, more preferably 25 to 100, and further preferably 30 to 60. When the yttria content is 4.5 mol% or more and less than 5.8 mol%, f m / f y is preferably 5 to 45, more preferably 10 to 40, and further preferably 15 to 35. When the content of yttria is 5.8 mol % or more and 7.5 mol % or less, f m / f y is preferably 2-40, more preferably 5-35, and further preferably 10-30.
[0030]
number
[0031] In formula (1), I y (111) indicates the peak intensity of the (111) plane of yttria at around 2θ=29° in the XRD pattern using CuKα radiation. m (111) and I m (11-1) indicates the peak intensity of the (111) and (11-1) planes of the monoclinic crystal system of zirconia. t (111) indicates the peak intensity of the (111) plane of the zirconia tetragonal crystal system. I c (111) indicates the peak intensity of the (111) plane of the cubic crystal system of zirconia.
[0032] The above formula (1) is I y By substituting other peaks in place of (111), this method can also be applied to calculate the undissolved fraction of stabilizers other than yttria.
[0033] The bending strength of the calcined zirconia body of the present invention is preferably 15 MPa or more in order to ensure strength that enables mechanical processing, and is preferably 70 MPa or less, more preferably 60 MPa or less, in order to facilitate mechanical processing.
[0034] The bending strength can be measured in accordance with ISO 6872:2015 (Dentistry-Ceramic materials), but the test specimen is 5 mm x 10 mm x 50 mm in size, with only the size of the test specimen being changed. The test specimen's face and C face (the face where the corner of the test specimen is chamfered at an angle of 45°) are surface-finished in the longitudinal direction with 600-grain sandpaper. The test specimen is placed so that the widest face faces vertically (load direction). In the three-point bending test measurement, the support distance (span) is 30 mm, and the crosshead speed is 0.5 mm / min.
[0035] The zirconia calcined body of the present invention may contain additives other than zirconia and stabilizers, as long as the effects of the present invention are achieved. Examples of the additives include colorants (including pigments, composite pigments, and fluorescent agents), alumina (Al2O3), titanium oxide (TiO2), silica (SiO2), etc.
[0036] Examples of the pigment include oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, Tb and Er (specifically, NiO, Cr2O3, etc.), and oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd and Tb are preferred, and oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Sm, Eu, Gd and Tb are more preferred. In addition, the zirconia calcined body of the present invention may not contain erbium oxide (Er2O3). Examples of the composite pigment include (Zr,V)O2, Fe(Fe,Cr)2O4, (Ni,Co,Fe)(Fe,Cr)2O4·ZrSiO4, (Co,Zn)Al2O4, etc. Examples of the fluorescent agent include Y2SiO5:Ce, Y2SiO5:Tb, (Y,Gd,Eu)BO3, Y2O3:Eu, YAG:Ce, ZnGa2O4:Zn, BaMgAl 10 O 17 :Eu, etc.
[0037] The zirconia calcined body of the present invention can be produced by firing (i.e., calcining) a zirconia molded body formed from a raw material powder containing zirconia particles and a stabilizer at a temperature at which the zirconia particles do not sinter. The zirconia molded body of the present invention contains zirconia and a stabilizer capable of suppressing the phase transition of zirconia, and at least a part of the stabilizer is not solid-dissolved in the zirconia. The method for producing the zirconia molded body of the present invention includes a step of press-molding a mixed powder consisting of zirconia and the stabilizer at a pressure of 175 MPa or more to obtain a zirconia molded body (hereinafter also referred to as a "zirconia molded body production step"). Not only zirconia calcined bodies having a small thickness after sintering, but also zirconia calcined bodies having a large thickness after sintering (for example, zirconia calcined bodies having a thickness of 10 mm or more) have a zirconia density of 3.0 g / cm. 3From the viewpoint of obtaining a bulk density of 190 MPa or more, the pressure is preferably 190 MPa or more, more preferably 200 MPa or more, even more preferably 215 MPa or more, and particularly preferably 220 MPa or more. By performing press molding at the above pressure, the bulk density of the zirconia molded body (and thus the obtained zirconia calcined body) can be increased regardless of the thickness. The upper limit of the pressure when the mixed powder is press molded is not particularly limited, and may be 600 MPa or less, 500 MPa or less, or 400 MPa or less. If the pressure is too high, cracks may occur when the molded body is removed from the mold. In this specification, the pressure of 175 MPa or more means the maximum pressure during press molding. The zirconia molded body is calcined at 800 to 1200 ° C. to obtain the zirconia calcined body of the present invention. The calcination temperature is not particularly limited, and may be 850 ° C. or more, 900 ° C. or more, or 950 ° C. or more. The calcination temperature may be 1150° C. or less, 1100° C. or less, or 1050° C. or less. Conventionally, as zirconia powders used in the method for producing a zirconia molded body, commercially available products such as yttria-stabilized tetragonal zirconia polycrystals (Y-TZP, yttria content: 3 mol%, TZ-3Y grade or product name "Zpex", manufactured by Tosoh Corporation) whose main crystal system is tetragonal, partially stabilized zirconia (PSZ, yttria content: 5 to 5.3 mol%, TZ-5Y grade or product name "Zpex Smile", manufactured by Tosoh Corporation) whose main crystal system is tetragonal and cubic, and partially stabilized zirconia (PSZ) whose main crystal system is cubic are known, but in the method for producing a zirconia molded body of the present invention, it is preferable to use zirconia powder whose main crystal system is monoclinic. The stabilizer used in the method for producing a zirconia molded body of the present invention is the same as that used in the above-mentioned calcined zirconia body.
[0038] Hereinafter, a preferred example of the method for producing a zirconia calcined body of the present invention will be described in detail. First, a raw powder of a zirconia molded body is produced. A mixture is produced using zirconia powder whose main crystal system is monoclinic and a powder of a stabilizer (e.g., yttria powder) so as to have a desired content of the stabilizer (e.g., yttria). In the method for producing a zirconia calcined body of the present invention, it is preferable to use zirconia powder whose main crystal system is monoclinic. Next, this mixture is added to water to produce a slurry, which is wet-pulverized and mixed in a ball mill until the desired particle size (e.g., average particle size 0.15 μm or less) is reached. The pulverized slurry is dried with a spray dryer and granulated. The obtained powder is fired at a temperature (e.g., 800 to 1200° C.) at which the zirconia particles do not sinter, to produce a powder (primary powder). A pigment may be added to the primary powder. Then, the primary powder is added to water to prepare a slurry, which is then wet-pulverized and mixed in a ball mill until the desired particle size (for example, an average particle size of 0.13 μm or less) is reached. Additives such as binders are added to the pulverized slurry as necessary, and the slurry is then dried in a spray dryer to prepare a mixed powder (secondary powder). The secondary powder is filled into a predetermined mold, the upper surface is leveled off to make the upper surface flat, an upper mold is set, and the secondary powder is press-molded by a uniaxial press molding machine to obtain a zirconia molded body. As described above, the pressure when the mixed powder is press-molded must be 175 MPa or more. The press molding may be a multi-stage or single-stage (only one time) press molding as long as it is 175 MPa or more, but a single-stage press molding may be used because it can be easily manufactured and is industrially advantageous. The obtained zirconia molded body may or may not be further molded by CIP (Cold Isostatic Press). One preferred embodiment is a method for producing a calcined zirconia body, the method including the steps of: press-molding a mixed powder containing zirconia and a stabilizer capable of suppressing the phase transition of zirconia at a pressure of 175 MPa or more to obtain a zirconia molded body; and firing the obtained zirconia molded body at 800 to 1200° C., wherein at least a part of the stabilizer is not solid-dissolved in the zirconia. Another preferred embodiment is a method for producing a calcined zirconia body that does not include a CIP molding step.
[0039] As described later, when manufacturing a zirconia calcined body having a multi-layer structure, the primary powder may be divided into at least two (preferably four) in the manufacturing method in order to make the zirconia compact have a multi-layer structure. Hereinafter, for example, a case where the primary powder is divided into four will be described. A pigment is added to each of the first to fourth powders. In order to generate a difference in the pigment content, one of the powders may not be added with a pigment, and the other may be added with a pigment. Then, each powder to which the pigment has been added is added to water to prepare a slurry, and wet-pulverized and mixed in a ball mill until the desired particle size is reached. Additives such as a binder are added to the pulverized slurry as necessary, and the slurry is dried with a spray dryer to prepare four types of powders (secondary powders) of the first to fourth powders. Next, the first powder of the secondary powder is filled into a predetermined mold, and the upper surface of the first powder is leveled by grinding the upper surface, and the second powder is subsequently filled on the first powder, and the upper surface of the second powder is leveled by grinding the upper surface. Similarly, the third powder is filled on the second powder, and the upper surface of the third powder is smoothed by grinding the upper surface. Furthermore, the fourth powder is filled on the third powder, and the upper surface of the fourth powder is smoothed by grinding the upper surface. Finally, the upper mold is set, and the four types of secondary powder (mixed powder) are press molded by a uniaxial press molding machine. As described above, the pressure when press molding the mixed powder needs to be 175 MPa or more. The obtained four-layered zirconia molded body may or may not be further subjected to CIP molding.
[0040] Next, the zirconia molded body obtained as described above is calcined to obtain a zirconia molded body. The calcination temperature when calcining the zirconia molded body of the present invention is, for example, preferably 800°C or higher, more preferably 900°C or higher, and even more preferably 950°C or higher, in order to ensure blocking. The calcination temperature is, for example, preferably 1200°C or lower, more preferably 1150°C or lower, and even more preferably 1100°C or lower, in order to improve dimensional accuracy. That is, the calcination temperature is preferably 800°C to 1200°C in the method for producing the zirconia calcined body of the present invention. It is considered that the solid solution of the stabilizer does not proceed at such a calcination temperature.
[0041] The zirconia calcined body of the present invention can be suitably used as a dental material. The dental material can have, for example, a disk (disk) shape, a block (rectangular parallelepiped) shape, or a dental product shape (for example, a crown shape). The zirconia calcined body of the present invention also includes a dental product (for example, a crown-shaped prosthesis) processed from a calcined zirconia disk using a CAD / CAM (Computer-Aided Design / Computer-Aided Manufacturing) system.
[0042] The zirconia calcined body of the present invention can produce a sintered body with high translucency even by firing for a short time. The sintered body produced by firing the zirconia calcined body of the present invention at a proper firing temperature for a certain time is defined as the third sintered body. The sintered body produced by firing the zirconia calcined body of the present invention at the proper firing temperature for 120 minutes is defined as the fourth sintered body. When the third sintered body is fired for 30 minutes and the translucency of the third sintered body and the fourth sintered body are compared, the translucency of the third sintered body is preferably 85% or more of the translucency of the fourth sintered body, more preferably 90% or more, even more preferably 95% or more, and particularly preferably substantially the same. The thickness of the third sintered body and the fourth sintered body when evaluating the translucency may be, for example, 1.2 mm. Furthermore, when the firing time of the third sintered body is 15 minutes, the translucency of the third sintered body is preferably 85% or more of the translucency of the fourth sintered body, more preferably 90% or more, even more preferably 95% or more, and particularly preferably substantially equal. From the above, the zirconia calcined body of the present invention has the above-mentioned advantages regarding short-time firing. The appropriate firing temperature can be specified by the following method. First, the zirconia calcined body is fired at various temperatures for 120 minutes, and then both sides are polished with #600 to obtain a sample of a zirconia sintered body having a thickness of 1.2 mm. The appearance of the obtained sample is visually observed. A state in which the zirconia calcined body is highly transparent and the background is transparent can be considered to be sufficiently fired. On the other hand, a state in which the transparency is low or the state in which the zirconia is cloudy can be judged to be insufficiently fired. Based on this judgment, the lowest temperature at which it can be considered to be sufficiently fired is the appropriate firing temperature for the zirconia calcined body.
[0043] By firing the zirconia calcined body of the present invention, a zirconia sintered body having excellent translucency can be obtained regardless of the thickness. A general dental porcelain firing furnace can be used for the firing (sintering) process of the zirconia calcined body. A commercially available dental porcelain firing furnace may be used. Examples of commercially available products include "Noritake Katana (registered trademark) F-1N" and "Noritake Katana (registered trademark) F-2" (both of which are SK Medical Electronics Co., Ltd.). The firing temperature is not particularly limited, but it is preferably performed at 1400 to 1650°C. The firing time when firing the zirconia calcined body of the present invention is not particularly limited, but it may be within 60 minutes, within 45 minutes, or within 30 minutes. By firing for such a short time, a zirconia sintered body having excellent translucency can be obtained regardless of the thickness.
[0044] The zirconia calcined body of the present invention may have a structure having a single composition, but may have a multi-layer structure from the viewpoint of reproducing a color tone suitable for dental use. For example, the multi-layer structure may be such that the content of each of the zirconia, stabilizer, pigment, and components that affect the appearance of the zirconia sintered body is changed for each layer. More specifically, when the zirconia calcined body of the present invention has a multi-layer structure, when (L*, a*, b*) after sintering according to the L*a*b* color system of a first point in a section from one end to the other end of a straight line extending in a first direction from the one end to the other end of the zirconia calcined body is (L1, a1, b1), and (L*, a*, b*) after sintering according to the L*a*b* color system of a second point in a section from the other end to 25% of the total length is (L2, a2, b2), L1 is 68.0 or more and 90.0 or less, a1 is equal to or greater than -3.0 and equal to or less than 4.5, b1 is 0.0 or more and 24.0 or less, L2 is between 60.0 and 85.0, a2 is between -2.0 and 7.0, b2 is 4.0 or more and 28.0 or less, L1>L2, a1 <a2であり、 b1 <b2であり、 It is preferable that the increase / decrease tendency of (L*, a*, b*) after sintering in the L*a*b* color system does not change from the first point to the second point. More preferably, L1 is 69.0 or more and 89.0 or less, a1 is equal to or greater than -2.7 and equal to or less than 4.0, b1 is 1.0 or more and 23.5 or less, L2 is between 61.5 and 84.5, a2 is between -1.5 and 6.5, b2 is 5.5 or more and 26.0 or less. More preferably, L1 is 70.0 or more and 87.0 or less, a1 is between -2.5 and 3.7, b1 is 2.0 or more and 23.0 or less, L2 is between 63.0 and 84.0, a2 is between -1.2 and 6.0, b2 is between 7.0 and 24.0. By satisfying the above range, it is possible to match the color tone of an average natural tooth.
[0045] In addition, when the zirconia calcined body of the present invention has a multi-layer structure, L1-L2 is greater than 0 and less than or equal to 12.0, a2-a1 is greater than 0 and equal to or less than 6.0; It is preferable that b2-b1 is more than 0 and is equal to or less than 12.0. More preferably, L1-L2 is greater than 0 and less than or equal to 10.0, a2-a1 is greater than 0 and less than or equal to 5.5; b2-b1 is more than 0 and not more than 11.0. L1-L2 is greater than 0 and equal to or less than 8.0, a2-a1 is greater than 0 and less than or equal to 5.0; b2-b1 is more than 0 and not more than 10.0. L1-L2 is 1.0 or more and 7.0 or less, a2-a1 is 0.5 or more and 3.0 or less, b2-b1 is 1.6 or more and 6.5 or less. Most preferably, L1-L2 is 1.5 or more and 6.4 or less, a2-a1 is 0.8 or more and 2.6 or less, b2-b1 is between 1.7 and 6.0. By satisfying the above range, the color tone of natural teeth can be more suitably reproduced.
[0046] When the zirconia calcined body of the present invention has a multi-layer structure, it is preferable that the color of the zirconia sintered body obtained by firing the zirconia calcined body changes from one end connecting both ends to the other end. Hereinafter, a description will be given using FIG. 1 as a schematic diagram of the zirconia sintered body. On a straight line extending in a first direction Y from one end P to the other end Q of the zirconia sintered body 10 shown in FIG. 1, it is preferable that the increasing or decreasing trends of the L* value, a* value, and b* value do not change in the opposite direction. That is, when the L* value tends to decrease on a straight line from one end P to the other end Q, it is preferable that there is no section in which the L* value substantially increases. For example, as shown in FIG. 1, when the first point A and the second point D are points on the straight line connecting the one end P to the other end Q, on the straight line connecting the first point A and the second point D, when the L* value tends to decrease from the first point A to the second point D, it is preferable that there is no section in which the L* value increases by 1 or more, and more preferably there is no section in which the L* value increases by 0.5 or more. Furthermore, when the a* value tends to increase on the line from one end P to the other end Q, it is preferable that there is no section where the a* value substantially decreases. For example, on the line connecting the first point A and the second point D, when the a* value tends to increase from the first point A to the second point D, it is preferable that there is no section where the a* value decreases by 1 or more, and it is more preferable that there is no section where the a* value decreases by 0.5 or more. Furthermore, when the b* value tends to increase on the line connecting the one end P to the other end Q, it is preferable that there is no section where the b* value substantially decreases. For example, on the line connecting the first point A and the second point D, when the b* value tends to increase from the first point A to the second point D, it is preferable that there is no section where the b* value decreases by 1 or more, and it is more preferable that there is no section where the b* value decreases by 0.5 or more.
[0047] Regarding the direction of color change in the zirconia sintered body 10, it is preferable that the a* value and the b* value tend to increase when the L* value tends to decrease from one end P to the other end Q. For example, from one end P to the other end Q, the color changes from white to light yellow, light orange, or light brown.
[0048] In the zirconia sintered body 10 of FIG. 1, a point between the first point A and the second point D on the line connecting one end P to the other end Q is defined as the third point B. When (L*, a*, b*) of the third point B in the L*a*b* color system is (L3, a3, b3), L3 is 66.0 or more and 89.0 or less, a3 is between -2.5 and 6.0, b3 is 1.5 or more and 25.0 or less, L1>L3>L2, a1 <a3<a2であり、 b1 <b3<b2である、 It is preferred.
[0049] Furthermore, the point between the third point B and the second point D is the fourth point C. If the (L*, a*, b*) of the fourth point in the L*a*b* color system is (L4, a4, b4), then L4 is 62.0 or more and 86.0 or less, a4 is between -2.2 and 7.0, b4 is between 3.5 and 27.0, L1>L3>L4>L2, a1 <a3<a4<a2であり、 b1 <b3<b4<b2である、 It is preferred.
[0050] The (L*, a*, b*) values for the above multi-layer structure were measured by processing each layer of zirconia sintered body into a disk with a diameter of 14 mm and a thickness of 1.2 mm (both sides were polished with #600) using a Konica Minolta, Inc. spectrophotometer CM-3610A, with a D65 light source, measurement mode SCI, measurement diameter / illumination diameter = φ8mm / φ11mm, and a white background.
[0051] In the zirconia sintered body 10 of FIG. 1, the first point A is preferably located in a section from one end P to 25% of the length between one end P and the other end Q (hereinafter referred to as "total length"). The third point B is preferably located in a section from 30% of the total length from the one end P to 70% of the total length from the one end P, and may be located, for example, at a distance of 45% of the total length from the one end P. The second point D is preferably located in a section from the other end Q to 25% of the total length. The fourth point C is preferably located in a section from 30% of the total length from the other end Q to 70% of the total length from the other end Q, and may be located, for example, at a distance of 45% of the total length from the other end Q (i.e., 55% of the total length from the one end P).
[0052] The above has been explained using the schematic diagram of Fig. 1, but in the present invention, for example, when the zirconia calcined body and its sintered body have a dental crown shape, the above-mentioned "one end" and "other end" preferably refer to one point on the end on the incisal end side and one point on the end on the root side. The one point may be a point on the end face or a point on the cross section. The point located in the section from one end or the other end to 25% of the total length refers to, for example, a point away from one end or the other end at a distance equivalent to 10% of the height of the dental crown.
[0053] When the zirconia calcined body of the present invention has a disk shape or a hexahedral shape such as a rectangular parallelepiped, the above-mentioned "one end" and "other end" preferably refer to a point on the upper and lower (bottom) faces. The point may be a point on an end face or a point on a cross section. A point located within 25% of the total length from one end or the other end refers to, for example, a point away from one end or the other end at a distance equivalent to 10% of the thickness of the hexahedron or disk.
[0054] In the present invention, the "first direction from one end to the other end" means the direction in which the color changes. For example, the first direction is preferably the direction in which the powder is layered in the manufacturing method described below. For example, when the zirconia calcined body has a crown shape, the first direction is preferably the direction connecting the incisal side and the base side.
[0055] The zirconia sintered body obtained by firing the zirconia calcined body of the present invention can be suitably used for dental products. Examples of dental products include copings, frameworks, crowns, crown bridges, abutments, implants, implant screws, implant fixtures, implant bridges, implant bars, brackets, denture bases, inlays, onlays, orthodontic wires, laminate veneers, and the like. In addition, a suitable method can be selected as a manufacturing method depending on each application, and for example, a dental product can be obtained by cutting the zirconia calcined body of the present invention and then sintering it. In addition, it is preferable to use a CAD / CAM system in the cutting process.
[0056] The present invention includes embodiments in which the above configurations are combined in various ways within the scope of the technical concept of the present invention, as long as the effects of the present invention are achieved. EXAMPLES
[0057] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples, and many modifications within the scope of the technical concept of the present invention are possible by those having ordinary skill in the art.
[0058] [Preparation of zirconia calcined body] The zirconia calcined bodies of the respective Examples and Comparative Examples were prepared according to the following procedure.
[0059] (Examples 1 to 6, Comparative Example 1) First, a mixture was prepared using approximately 100% monoclinic zirconia powder and yttria powder so that the content of yttria was as shown in Table 1. Next, this mixture was added to water to prepare a slurry, and the mixture was wet-pulverized and mixed in a ball mill until the average particle size was 0.15 μm or less. The pulverized slurry was dried with a spray dryer, and the obtained powder was fired at 950° C. for 2 hours to prepare a powder (primary powder). The average particle size can be determined by a laser diffraction scattering method. Specifically, the laser diffraction scattering method can be measured, for example, by a laser diffraction particle size distribution measuring device (SALD-2300: manufactured by Shimadzu Corporation) using a 0.2% sodium hexametaphosphate aqueous solution as a dispersion medium.
[0060] Water was added to the obtained primary powder to prepare a slurry, which was then wet-milled and mixed in a ball mill until the average particle size was 0.13 μm or less. A binder was added to the milled slurry, which was then dried in a spray dryer to prepare a mixed powder (secondary powder).
[0061] Next, a mold having an inner dimension of 24 mm × 19 mm was filled with the secondary powder in an amount to a predetermined thickness, and the upper surface was smoothed to make it flat. Finally, the upper mold was set, and the secondary powder was press-molded for 90 seconds with a uniaxial press molding machine at the pressure shown in Table 1 to obtain a zirconia molded body.
[0062] The obtained zirconia molded body was fired at 1000° C. for 2 hours to produce a zirconia calcined body.
[0063] Comparative Example 2 The zirconia molded body was obtained in the same manner as in Example 2, except that the pressing pressure during press molding was 30 MPa. The zirconia molded body was then subjected to CIP molding at 170 MPa for 5 minutes, and then fired at 1000°C for 2 hours to produce a zirconia calcined body.
[0064] (Comparative Examples 3 to 6) In Comparative Examples 3 and 4, "Zpex (registered trademark)" manufactured by Tosoh Corporation (main crystal system is tetragonal) was used as the secondary powder, and in Comparative Examples 5 and 6, "Zpex Smile (registered trademark)" manufactured by Tosoh Corporation (main crystal system is tetragonal and cubic: the total of tetragonal and cubic is approximately 90%) was used as the secondary powder. The zirconia calcined bodies were prepared in the same manner as in Example 1, except that the secondary powder was used.
[0065] [Frequency of undissolved yttria f y Measurement of For the zirconia calcined bodies of Examples 1 to 6 and Comparative Examples 1 to 6, XRD patterns were measured using CuKα radiation. y Table 1 shows the f y The measurement results are shown in Fig. 2. Fig. 2 shows the XRD pattern of the calcined zirconia body produced in Example 1. Fig. 3 shows the XRD pattern of the calcined zirconia body produced in Example 3. Fig. 4 shows the XRD pattern of the calcined zirconia body produced in Comparative Example 5.
[0066] As shown in FIG. 4, in the zirconia calcined body of Comparative Example 5, no peak of monoclinic zirconia was confirmed. Also, no peak of yttria was confirmed. Comparative Examples 3, 4 and 6 showed similar results. On the other hand, from FIG. 2 and FIG. 3, in the zirconia calcined bodies of Examples 1 and 3, peaks of monoclinic, tetragonal and cubic zirconia were confirmed, and the peaks of monoclinic zirconia (peak numbers 5 and 8 in FIG. 2 and 3) were higher in intensity. Examples 2, 4 to 6 showed similar results. Also, in all of the zirconia calcined bodies of the Examples, a peak of yttria (peak number 6 in FIG. 2 and FIG. 3) was confirmed at 2θ of about 29.4°. From the above results, it is considered that in the zirconia calcined bodies of Examples 1 to 6, some yttria is present without being solid-dissolved in zirconia, and in the zirconia calcined bodies of Comparative Examples 1 to 6, all yttria is solid-dissolved in zirconia.
[0067] [Measurement of bulk density of calcined zirconia body] For the zirconia calcined bodies of Examples 1 to 6 and Comparative Examples 1 to 6, the amount of secondary powder filled when manufacturing the zirconia molded body was adjusted to produce calcined bodies with a thickness of less than 10 mm and calcined bodies with a thickness of 10 mm or more, and the bulk density of each was measured by the Archimedes method. Specifically, calcined bodies with thicknesses of 2 mm and 14 mm were produced. A density measurement kit (ML-DNY-43) was attached to an electronic balance (ML204 / 02) manufactured by Mettler Toledo Co., Ltd., and the bulk density was measured by the Archimedes method from the mass of the sample measured in air and the mass of the sample measured while suspended in water. The measurement results are shown in Table 1.
[0068] [Measurement of translucency of zirconia calcined body after firing] For the zirconia calcined bodies of Examples 1 to 6 and Comparative Examples 1 to 6, the amount of filling of the secondary powder when manufacturing the zirconia molded body was adjusted to prepare a calcined body having a thickness of 1 mm after firing and a calcined body having a thickness of 10 mm after firing. The calcined bodies were fired at the firing temperature and firing time shown in Table 1 using an electromagnetic induction type electric furnace using SiC as a heating element, to obtain a first sintered body having a thickness of 1 mm and a second sintered body having a thickness of 10 mm. The firing time indicates the total time from the start of firing until the maximum temperature in Table 1 is reached, and then the temperature is cooled to 800°C. Each of the obtained sintered bodies was polished to a thickness of 0.5 mm to obtain a translucent test piece. The final finishing was performed with a #2000 abrasive cloth paper. The calculation was performed using the L* value of the lightness (color space) in the L*a*b* color system (JIS Z 8781-4:2013 Colorimetry-Part 4: CIE 1976 L*a*b* color space) measured using a dental color measuring device (Olympus Corporation, 7band LED light source, Crystaleye). The L* value measured with the sample background set to white was taken as the first L* value, and the L* value measured with the sample background set to black for the same sample for which the first L* value was measured was taken as the second L* value, and the value (ΔL*) obtained by subtracting the second L* value from the first L* value was taken as the numerical value indicating the translucency. In addition, the ratio of the translucency of the second sintered body (second translucency ΔL2*) to the translucency of the first sintered body (first translucency ΔL1*) was calculated using the numerical value. The measurement results are shown in Table 1.
[0069] [Table 1]
[0070] As shown in Table 1, the pressing pressure in Comparative Example 1 is lower than that in Example 2, and the primary pressing pressure and the pressing pressure during CIP molding in Comparative Example 2 are both lower than that in Example 2. As a result, in Comparative Examples 1 and 2, the bulk density of the calcined body with a thickness of 10 mm or more was 3.0 g / cm 3 The second translucency ΔL2* of the sintered body having a thickness of 10 mm is also low, with the ratio of the second translucency to the first translucency being below 90%.
[0071] In addition, in comparison with Examples 1 and 2, the abundance ratio of undissolved yttria f y As a result, the second translucency ΔL2* of the sintered body having a thickness of 10 mm is extremely low, and the ratio of the second translucency to the first translucency is also very small.
[0072] On the other hand, the zirconia calcined bodies of Examples 1 to 6, even though they were sintered bodies with a thickness of 10 mm, exhibited high translucency equivalent to that of a sintered body with a thickness of 1 mm, indicating that they could be sintered in a short time and had excellent translucency after sintering regardless of the thickness.
[0073] With respect to numerical ranges set forth herein, unless otherwise stated, any numerical value or range falling within the range should be construed as being specifically set forth herein. [Industrial Applicability]
[0074] The zirconia calcined body of the present invention can be used as a dental material. [Explanation of symbols]
[0075] 10 Zirconia sintered body A 1st point B 3rd point C 4th point D 2nd point P one end Q Other end L total length Y 1st direction
Claims
1. Zirconia and A method for producing a zirconia molded body containing a stabilizer capable of suppressing a phase transition of zirconia, At least a portion of the stabilizer is not solid-dissolved in zirconia, A method for producing a zirconia molded body, comprising the step of press-molding a mixed powder of zirconia and the stabilizer at a pressure of 175 MPa or more to obtain a zirconia molded body, wherein the press-molding is uniaxial pressing.
2. The method for producing a zirconia compact according to claim 1 , wherein the stabilizer comprises yttria.
3. The abundance ratio f of yttria not dissolved in the zirconia is calculated based on the following formula (1): y The method for producing a zirconia molded body according to claim 2, wherein the content of zirconia is more than 0%. [0010] (However, I y (111) indicates the peak intensity of the (111) plane of yttria at about 2θ=29° in the X-ray diffraction pattern using CuKα radiation, and I m (111) and I m (11-1) indicates the peak intensity of the (111) and (11-1) planes of the monoclinic system of zirconia in the X-ray diffraction pattern, and I t (111) indicates the peak intensity of the (111) plane of the zirconia tetragonal system in the X-ray diffraction pattern, and I c (111) indicates the peak intensity of the (111) plane of the cubic crystal system of zirconia in the X-ray diffraction pattern.
4. The method for producing a zirconia molded body according to any one of claims 1 to 3, wherein the pressure in the press molding is 200 MPa or more.
5. The method for producing a zirconia molded body according to any one of claims 1 to 4, wherein the main crystal system of the zirconia is a monoclinic system.
6. The ratio f of monoclinic crystals in zirconia is calculated by the following formula (2): m The method for producing a zirconia molded body according to claim 5, wherein the content of the zirconia powder is 55% or more. [0025] (In the formula, I m (111) and I m (11-1) indicate the peak intensities of the (111) and (11-1) planes of the monoclinic crystal system of zirconia, respectively. t (111) indicates the peak intensity of the (111) plane of the zirconia tetragonal system. c (111) indicates the peak intensity of the (111) plane of the cubic crystal system of zirconia.)
7. A method for producing a calcined zirconia body, comprising firing the zirconia molded body obtained by the method according to any one of claims 1 to 6 at 800 to 1200°C.
8. Zirconia and A zirconia calcined body having a thickness of 10 mm or more, comprising: the stabilizing agent comprises yttria; The content of yttria is 3 mol% or more and 7.5 mol% or less with respect to the total moles of zirconia and yttria, At least a portion of the yttria is not solid-dissolved in the zirconia, A test piece of the calcined zirconia body having a thickness of 10 mm or more is used to measure a bulk density of 3.0 g / cm3 by the Archimedes method. 3 That's all. the zirconia calcined body is fired for 30 minutes to prepare a first sintered body having a thickness of 1 mm and a second sintered body having a thickness of 10 mm; when a first translucency of a test piece having a thickness of 0.5 mm prepared from the first sintered body is compared with a second translucency of a test piece having a thickness of 0.5 mm prepared from the second sintered body, a ratio of the second translucency to the first translucency is 90% or more; The abundance ratio f of yttria not dissolved in the zirconia is calculated based on the following formula (1): y is 1.0% or more, When the yttria content is 3 mol% or more and less than 4.5 mol%, it is 1.0% or more, When the yttria content is 4.5 mol% or more and less than 5.8 mol%, it is 2% or more, When the yttria content is 5.8 mol% or more and 7.5 mol% or less, it is 3% or more; [0010] (However, I y (111) indicates the peak intensity of the (111) plane of yttria at about 2θ=29° in the X-ray diffraction pattern using CuKα radiation, and I m (111) and I m (11-1) indicates the peak intensity of the (111) and (11-1) planes of the monoclinic system of zirconia in the X-ray diffraction pattern, and I t (111) indicates the peak intensity of the (111) plane of the zirconia tetragonal system in the X-ray diffraction pattern, and I c (111) indicates the peak intensity of the (111) plane of the cubic crystal system of zirconia in the X-ray diffraction pattern. Zirconia calcined body.
9. A dental material comprising the zirconia calcined body according to claim 8.
10. The dental material according to claim 9, wherein the dental material is in the shape of a disk or a block.
Citation Information
Patent Citations
Zirconia ceramic bone implantation prosthesis and preparation method thereof
CN109095921A
Sintered body of zirconia and method for manufacturing the same
JP2011073907A
Light-transmitting zirconia sintered compact, zirconia powder and application thereof
JP2015143178A
Method for producing translucent zirconia sintered compact, translucent zirconia sintered compact obtained by the production method, and calcined body before sintering for producing translucent zirconia sintered compact
JP2016060687A
How to Plan Sintering of Dental Prosthetic Parts
JP2016540562A