Low-resistance tungsten film and manufacturing method

By employing a PVD tungsten liner layer and CVD tungsten film without a TiN layer, the method addresses high resistance issues in conventional tungsten deposition, achieving low resistance and effective filling in intricate features, suitable for advanced device nodes.

JP7559070B2Active Publication Date: 2024-10-01APPLIED MATERIALS INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022542962
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-25
Filing Date
2021-07-20
Publication Date
2024-10-01
Estimated Expiration
2041-07-20

AI Technical Summary

Technical Problem

Conventional tungsten deposition processes result in high resistance due to the use of titanium nitride (TiN) layers and difficulty in reducing the resistance of bulk CVD tungsten grown on nucleation layers, especially as aspect ratios increase and feature sizes decrease, leading to unacceptably high line or via contact resistance.

Method used

A method involving a physical vapor deposition (PVD) of a tungsten liner layer followed by a chemical vapor deposition (CVD) of a tungsten film, where the grain size of the liner layer is controlled to be greater than 100 angstroms, and the processes are conducted under vacuum or load lock conditions without an air break, eliminating the need for a TiN layer.

Benefits of technology

The method reduces tungsten stack resistance to less than 13 μΩ·cm, providing improved conductivity and filling capabilities in features with aspect ratios up to 40:1, particularly beneficial for device nodes below 25 nm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559070000001
    Figure 0007559070000001
  • Figure 0007559070000002
    Figure 0007559070000002
  • Figure 0007559070000003
    Figure 0007559070000003
Patent Text Reader

Abstract

An apparatus and method are presented for providing an electronic device with a tungsten film stack, in which a tungsten liner formed by physical vapor deposition is filled with a tungsten film formed directly on top of the tungsten liner by chemical vapor deposition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE

[0002] Embodiments of the present disclosure relate to the field of electronic device manufacturing, and in particular to integrated circuit (IC) manufacturing. In particular, embodiments of the present disclosure are directed to low resistivity tungsten films and methods for making low resistivity tungsten films. [Background technology]

[0002] Integrated circuits are made possible by processes that fabricate intricately patterned layers of materials on substrate surfaces. Producing patterned materials on substrates requires controlled methods for depositing the desired materials. Selectively depositing a film on one surface relative to a different surface is useful for patterning and other applications.

[0003] In conventional fill schemes utilizing tungsten deposition processes, a titanium nitride (TiN) layer is deposited on a dielectric substrate as a barrier and liner layer, followed by a nucleation or seed layer of bulk CVD tungsten (W) film. The TiN layer has a high resistivity, and it is difficult to reduce the resistivity of the bulk CVD tungsten grown on the nucleation layer. As aspect ratios (ratio of trench or via height to trench or via width) increase and / or feature sizes such as feature width decrease, tungsten film stacks produced by conventional processes have unacceptably high line or via contact resistance. Summary of the Invention [Problem to be solved by the invention]

[0004] Thus, there is a need for improved methods for forming tungsten layers, films, and materials, and for obtaining devices including such tungsten layers, films, and materials. [Means for solving the problem]

[0005] An apparatus and method for depositing a metal film is described. In one embodiment, a method for forming a tungsten stack on a substrate includes forming a tungsten liner layer on a surface of the substrate using a physical vapor deposition process, and forming a tungsten film directly on the tungsten liner layer using a chemical vapor deposition process.

[0006] One or more embodiments are directed to a method of forming a tungsten stack on a substrate, the method including placing the substrate on a substrate support in a physical vapor deposition chamber, forming a tungsten liner layer on a surface of the substrate using a physical vapor deposition process, controlling the grain size of the tungsten liner layer to be greater than 100 angstroms, and forming a tungsten film directly on the tungsten liner layer using a chemical vapor deposition process.

[0007] In another aspect, an electronic device comprises a tungsten liner layer physically vapor deposited on a surface and a chemical vapor deposited film directly over the tungsten liner layer.

[0008] So that the above-mentioned features of the present disclosure can be understood in detail, a more particular description of the present disclosure briefly summarized above will be had by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the present disclosure can admit of other equally effective embodiments, and therefore should not be considered as limiting the scope of the present disclosure. The embodiments described herein are illustrated by way of example, and not by way of limitation, in the figures of the accompanying drawings, in which like reference numerals denote like elements. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view of a semiconductor device according to one or more embodiments of the present disclosure. [Diagram 2] 1 is a cross-sectional view of a semiconductor device according to one or more embodiments of the present disclosure. [Diagram 3] 1 is a flowchart of a method according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In the accompanying figures, similar components and / or features may have the same reference label. Furthermore, various components of the same type may be distinguished by following the reference label with a dash and a second label that distinguishes among these similar components. If only a first reference label is used herein, the description applies to any of the similar components having the same first reference label, regardless of the second label.

[0011] Before describing several embodiments of the present disclosure, it is to be understood that the disclosure is not limited to the details of structure or process steps set forth in the following description, as the disclosure is capable of other embodiments and of being practiced or carried out in various ways.

[0012] As used herein, "substrate" refers to any substrate surface or material surface formed on a substrate on which a film treatment is performed during a manufacturing process. For example, substrate surfaces on which treatment can be performed include materials such as silicon, silicon oxide, strained silicon, silicon-on-insulator (SOI), carbon-doped silicon oxide, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other material such as metals, metal nitrides, metal alloys, and other conductive materials, depending on the application. Substrates include, without limitation, semiconductor wafers. Substrates can undergo pretreatment processes to polish, etch, reduce, oxidize, hydroxylate, anneal, and / or bake the substrate surface. In addition to film treatments performed directly on the surface of the substrate itself, the present disclosure also provides that any of the disclosed film treatment steps can also be performed on an underlying layer formed on the substrate, as disclosed in more detail below, and the term "substrate surface" includes such an underlying layer, as the context indicates. Thus, for example, when a film / layer or partial film / layer is deposited on a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface.

[0013] As used herein and in the appended claims, the terms "precursor," "reactant," "reactive gas," and the like are used interchangeably to refer to any gas species capable of reacting with the substrate surface.

[0014] As used herein, the term "liner" refers to a layer formed conformally along at least a portion of the sidewalls and / or bottom surface of an opening such that a significant portion of the opening prior to deposition of the layer remains unfilled after deposition of the layer. In some embodiments, the liner can be formed along the entire sidewalls and bottom surface of the opening. A liner can also be formed on a planar surface of a planar substrate.

[0015] Advantageously, the physical vapor deposited tungsten liner layer, with the chemical vapor deposited tungsten film immediately above the physical vapor deposited tungsten liner layer, shows a clear stack resistance advantage compared to a conventional device including a TiN layer + nucleation layer followed by tungsten deposited by chemical vapor deposition (CVD). In some embodiments, there may be an air break or exposure of the substrate to ambient conditions between the deposition of the tungsten liner layer by physical vapor deposition (PVD) and the deposition of the tungsten film by CVD. However, in certain embodiments, there is no air break between the formation of the tungsten liner layer by the PVD process and the formation of the tungsten film by the CVD process. In other words, these two processes are completed under vacuum or load lock conditions. In some embodiments, the process including the deposition of the tungsten liner layer using PVD with no bias power applied to the substrate support supporting the substrate results in improved properties in terms of grain size and orientation to improve the stack resistance of the tungsten stack consisting of the tungsten liner layer and the tungsten film. In some embodiments, the PVD process is performed using Kr process gas to further tailor the device properties. In one or more embodiments, the tungsten liner layer includes α-W, and the tungsten liner layer is free of β-W.

[0016] An apparatus and method for depositing a metal film is described with reference to FIGS. 1-3. In one embodiment, the method 200 includes forming a tungsten stack on a substrate 102. The method includes forming a tungsten liner layer 106 on a surface of the substrate 102 using a physical vapor deposition process, and then forming a tungsten film 108 directly on the tungsten liner layer using a chemical vapor deposition process. In one or more embodiments, the tungsten liner layer 106 is substantially free of tungsten oxide. In some embodiments, the tungsten stack including the tungsten liner layer 106 and the tungsten film 108 formed by this method does not include a TiN layer or a nucleation layer. In one or more embodiments, the method 200 includes forming a dielectric layer 110 on the substrate surface prior to forming the tungsten liner layer 106.

[0017] In some embodiments, the substrate surface comprises a feature. In some embodiments, the feature is selected from a trench, a via, or a peak. In a particular embodiment, the feature comprises a trench. In some embodiments, the method 200 further comprises forming a tungsten liner layer in a PVD chamber at 202, removing the substrate from the PVD chamber, exposing the substrate to an ambient atmosphere, and treating the tungsten liner layer to remove tungsten oxide from the tungsten liner layer at 206. As used herein, "ambient atmosphere" refers to an atmosphere that is not under a vacuum and is not exposed to air. In some embodiments, treating the tungsten liner layer comprises exposing the tungsten liner layer to hydrogen gas and treating the tungsten liner layer with WF 6 The method includes exposing the substrate to a gas.

[0018] In other embodiments, the method 200 further includes forming a tungsten liner layer in a PVD chamber at 204, removing the substrate from the PVD chamber at 206, and placing the substrate in a CVD chamber without exposing it to an ambient atmosphere at 208. A tungsten film 108 is deposited directly over the tungsten liner layer 106 to form a W film stack at 210. In some embodiments, the trench has a width W of 5 nm or more and 65 nm or less, 5 nm or more and 55 nm or less, 5 nm or more and 45 nm or less, 5 nm or more and 35 nm or less, 5 nm or more and 32 nm or less, 5 nm or more and 25 nm or less, or 5 nm or more and 22 nm or less.

[0019] In some embodiments, the method 200 further includes, at 202, placing the substrate on a substrate support in the physical vapor deposition chamber, and no bias voltage is applied to the substrate support.

[0020] Another aspect of the disclosure relates to a method of forming a tungsten stack on a substrate, the method including the steps of placing the substrate on a substrate support in a physical vapor deposition process chamber, forming a tungsten liner layer on the surface of the substrate using a physical vapor deposition process, controlling the grain size of the tungsten liner layer to be greater than 100 angstroms, and forming a tungsten film directly on the tungsten liner layer using a chemical vapor deposition process. In some embodiments, controlling the grain size of the tungsten liner layer includes not applying a bias voltage to the substrate support during the physical vapor deposition process. In some embodiments, the CVD deposited tungsten film has a grain size greater than 250 angstroms. In some embodiments, the PVD deposited tungsten liner layer has a grain size greater than 100 angstroms and the tungsten film has a grain size greater than 250 angstroms. In one or more embodiments, the tungsten stack has a resistivity of less than 13 μΩ·cm, less than 12.5 μΩ·cm, less than 12 μΩ·cm, less than 11.5 μΩ·cm, or less than 11 μΩ·cm. In some embodiments, using Kr as a process gas during the PVD process has a beneficial effect on increasing the grain size of the tungsten liner layer. Experimental data showed that when Ar is used as a process gas for the PVD process at room temperature (about 25° C.), the W liner layer grain size is 137 angstroms, and when Ar is used as a process gas for the PVD process at 325° C., the W liner layer grain size increases to 180 angstroms. However, when Kr is used as a process gas for the PVD process at room temperature (about 25° C.), the W liner layer grain size increases to 210 angstroms. In a tungsten stack including CVD deposited films on each of these liner layers, using Ar as the process gas for the PVD process at room temperature (~25 °C), the W liner layer grain size was 137 Å and the stack resistance was ~11 μΩ·cm.When Ar was used as the process gas for the PVD process at 325°C, the grain size of the W liner layer increased to 180 Å, and the stack resistance of the stack including the CVD deposited film on the tungsten liner layer was approximately 9.8 μΩ·cm. When Kr was used as the process gas for the PVD process at room temperature (approximately 25°C), the grain size of the W liner layer increased to 210 Å, and the stack resistance of the stack including the CVD deposited film on the tungsten liner layer was approximately 9.6 μΩ·cm.

[0021] Another aspect of the disclosure relates to an electronic device comprising a physically vapor deposited tungsten liner layer on a surface and a chemically vapor deposited tungsten film directly on the tungsten liner layer. In some embodiments, the physically vapor deposited tungsten liner has a grain size greater than 100 angstroms. In some embodiments, the chemically vapor deposited tungsten film has a grain size greater than 250 angstroms. In one or more embodiments, the substrate surface comprises a feature selected from the group consisting of a trench, a via, and a peak. In one or more embodiments, the feature is a trench having a width less than 65 nm.

[0022] In some embodiments, the W liner layer has a grain size greater than 100 angstroms, greater than 150 angstroms, or greater than 200 angstroms, and the tungsten film stack including the tungsten liner layer and the tungsten film has a stack resistance less than 10 μΩ·cm. In some embodiments, the device comprises a trench having a width W of 5 nm to 65 nm, 5 nm to 55 nm, 5 nm to 45 nm, 5 nm to 35 nm, 5 nm to 32 nm, 5 nm to 25 nm, or 5 nm to 22 nm. In some embodiments, the trench has an aspect ratio of depth or height H to width W of about 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, or 40:1 or greater. In one or more embodiments, the aspect ratio is greater than 10:1.

[0023] In some embodiments, the tungsten film formed on the PVD deposited liner layer is formed by exposing the substrate to a plasma formed from a first gas. In some embodiments, the first gas comprises a tungsten precursor gas. In some embodiments, the first gas comprises tungsten pentachloride (WCl 5 ) or tungsten hexachloride (WCl 6 In another embodiment, the first gas comprises a fluorine-free tungsten halide precursor, such as WOCl. 4 or WO 2 Cl 2 In another embodiment, the first gas comprises a fluorine-free tungsten oxyhalide precursor, such as tungsten pentabromide (WBr 5 ) or tungsten hexabromide (WBr 6 In some embodiments, the first gas is selected from the group consisting of chlorine-free tungsten halide precursors such as hydrogen (H 2 ) or ammonia (NH 3 ) or hydrazine (N 2 H 4 ) and a reactive gas such as argon (Ar), helium (He), or nitrogen (N 2 The method further includes a carrier gas, such as a tungsten precursor gas, and a reactant gas, together with the tungsten precursor gas. In some embodiments, the carrier gas is an inert gas. In some embodiments, the first gas consists of or consists essentially of a tungsten precursor gas, a reactant gas, and a carrier gas. In some embodiments, the first gas consists of or consists essentially of a chlorine-free, fluorine-free halide tungsten precursor, a hydrogen-containing gas, and an inert gas. The carrier gas can be provided at a flow rate of about 10 sccm to about 10 slm.

[0024] The methods of the present invention may be utilized with any device node, but may be particularly advantageous at device nodes of about 25 nm or less, such as from about 5 nm to about 25 nm.

[0025] Although the figures show a substrate with a single feature for purposes of illustration, one of ordinary skill in the art will understand that there may be multiple features. The shape of the feature may be any suitable shape, including, but not limited to, peaks, trenches, and cylindrical vias. In a particular embodiment, the feature is a trench. In another specific embodiment, the feature is a via. As used in this context, the term "feature" refers to any intentionally formed surface irregularity. Suitable examples of features include, but are not limited to, a trench having a top, two sidewalls, and a bottom, a peak having a top and two sidewalls extending upward from the surface, and a via having sidewalls extending downward from the surface and an open bottom. The feature may have any suitable aspect ratio (the ratio of the depth or height H of the feature to the width of the feature). In some embodiments, the aspect ratio is about 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, or 40:1 or more. In one or more embodiments, the aspect ratio is greater than 10:1.

[0026] In one or more embodiments, the at least one feature extends a depth or height H from the top surface of the substrate or the top surface of the tungsten liner layer to a bottom surface. The at least one feature has a width W defined by a first sidewall and a second sidewall. A tungsten film is deposited on the tungsten layer to fill the at least one feature and extend above the top surface of the tungsten layer. The tungsten film can be recessed to lower a top of the metal film to a height below the top surface of the tungsten liner layer to form a recessed metal film. The tungsten film can be stretched to form a pillar extending from the at least one feature.

[0027] 1 and 2, one or more embodiments are directed to a method of forming a semiconductor device 100. A substrate 102 includes a feature 104 filled with a tungsten film 108. The feature 104 is shown in the form of a trench having a width W and a depth or height H.

[0028] In one or more embodiments, the tungsten film 108 is a CVD deposited tungsten film. In one embodiment, the tungsten film is a gap-fill layer. As shown in FIG. 1, in one embodiment, the tungsten film 108 is deposited on the tungsten liner layer 106 over the top 114 of the feature 104, the sidewalls 116 of the feature 104, and the top 118 of the dielectric layer 110.

[0029] In one or more embodiments, the tungsten film 108 is a seed gap fill layer. In one embodiment, the seed gap fill layer is a selectively grown seed film. As shown in FIG. 1, in one embodiment, the tungsten film 108 is deposited on the tungsten liner layer 106 over the top 114 of the feature 104, the sidewalls 116 of the feature 104, and the top 118 of the dielectric layer 110.

[0030] As shown in FIG. 2, in another embodiment, a tungsten film 108 is deposited on the tungsten liner layer 106 over the top 114 of the feature 104, the sidewalls 116 of the feature 104, and the top surface 120 of the substrate 102.

[0031] In one or more embodiments, the tungsten film 108 is a tungsten layer. In one or more embodiments, the tungsten layer is a tungsten gap-fill layer.

[0032] In one or more embodiments, a dielectric layer 110 is formed on the substrate 102. The dielectric layer may be any suitable dielectric material, including, but not limited to, titanium or silicon nitrides, oxides, or carbides. The dielectric layer 110 may be formed conformally or non-conformally on the substrate 102.

[0033] In one embodiment, the dielectric layer 110 comprises a dielectric material having a k value of less than 5. In one embodiment, the dielectric layer 110 comprises a dielectric material having a k value of less than 2. In at least some embodiments, the dielectric layer 110 comprises an oxide, a carbon-doped oxide, a porous silicon dioxide, a carbide, an oxycarbide, a nitride, an oxynitride, an oxycarbonitride, a polymer, a phosphosilicate glass, a fluorosilicate (SiOF) glass, an organo-silicon glass (SiOCH), or any combination thereof. In at least some embodiments, the dielectric layer 110 can comprise a photosensitive material such as polyimide, an epoxy, benzocyclobutene (BCB), and a WPR series material, or a spin-on glass.

[0034] In one embodiment, the thickness of the dielectric layer 110 is approximately in the range of about 10 nanometers (nm) to about 2 micrometers (μm). In one embodiment, the dielectric layer 110 is deposited using one of a number of deposition techniques, such as, but not limited to, chemical vapor deposition processes ("CVD"), physical vapor deposition processes ("PVD"), molecular beam epitaxy ("MBE"), metalorganic chemical vapor deposition processes ("MOCVD"), atomic layer deposition ("ALD"), spin-on, or other insulating deposition techniques known to those skilled in the art of microelectronic device manufacturing.

[0035] In one embodiment, the tungsten liner layer 106 is deposited on the dielectric layer 110. In one embodiment, the tungsten liner layer 106 is a conductive liner. In some embodiments, the tungsten liner layer 106 is formed by a PVD process.

[0036] In one embodiment, the tungsten liner layer 106 is deposited to a thickness in the range of about 5 Å to about 35 Å. In one embodiment, the tungsten liner layer 106 is deposited to a thickness in the range of about 10 Å to about 30 Å.

[0037] Although the present disclosure has been described herein with reference to specific embodiments, it should be understood that these embodiments are merely illustrative of the principles and applications of the present disclosure. It will be apparent to those skilled in the art that various modifications and variations can be made to the disclosed method and apparatus without departing from the spirit and scope of the present disclosure. That is, the present disclosure covers modifications and variations that come within the scope of the appended claims and their equivalents.

Claims

1. 1. A method for forming a tungsten stack on a substrate and filling a trench, comprising the steps of: forming a tungsten liner layer on a surface of the dielectric material and on a surface of the trench, the surface comprising two sidewalls and a bottom, the tungsten liner layer covering the two sidewalls and the bottom, the tungsten liner layer being formed using a physical vapor deposition process using Kr as a process gas; forming a tungsten film directly over the tungsten liner layer using a chemical vapor deposition process; Including, The method of claim 1, wherein forming the tungsten film does not include forming a nucleation layer on the tungsten liner layer, and the trench has a width of less than 65 nm.

2. The method of claim 1 , wherein the tungsten liner layer is substantially free of tungsten oxide.

3. The method of claim 2 , wherein the tungsten stack formed by the method does not include a TiN layer.

4. The method of claim 1 , wherein the trench has a height to width aspect ratio of about 5:1 or greater.

5. 3. The method of claim 2, wherein the method further comprises forming the tungsten liner layer in a PVD chamber, removing the substrate from the PVD chamber, exposing the substrate to an ambient atmosphere, and treating the tungsten liner layer to remove tungsten oxide from the tungsten liner layer.

6. The step of treating the tungsten liner layer includes the steps of exposing the tungsten liner layer to hydrogen gas and treating the tungsten liner layer with WF 6 The method of claim 5 including the step of exposing to a gas.

7. 3. The method of claim 2, wherein the method further comprises forming the tungsten liner layer in a PVD chamber, removing the substrate from the PVD chamber, and placing the substrate in a CVD chamber without exposure to an ambient atmosphere.

8. The method of claim 4 , wherein the trench has a width of less than 25 nm.

9. the tungsten stack has a stack resistor; the method further comprising disposing the substrate on a substrate support in a physical vapor deposition chamber and applying no bias voltage to the substrate support; 3. The method of claim 2, wherein not applying a bias voltage to the substrate support controls grain size of the tungsten liner layer and improves the stack resistance.

10. 1. A method for forming a tungsten stack on a substrate and filling a trench, comprising the steps of: placing the substrate on a substrate support in a physical vapor deposition processing chamber; forming a tungsten liner layer having a grain size on a surface of a dielectric material and on a surface of a trench consisting of two sidewalls and a bottom, the tungsten liner layer covering the two sidewalls and the bottom and formed using a physical vapor deposition process using Kr as a process gas; controlling the grain size of the tungsten liner layer to be greater than 100 angstroms; forming a tungsten film directly over the tungsten liner layer using a chemical vapor deposition process; Including, The method of claim 1, wherein forming the tungsten film does not include forming a nucleation layer on the tungsten liner layer, and the trench has a width of less than 65 nm.

11. 11. The method of claim 10, wherein controlling the grain size of the tungsten liner layer comprises applying no bias voltage to the substrate support during the physical vapor deposition process.

12. The method of claim 11 , wherein the tungsten film has a grain size greater than 250 angstroms.

Citation Information

Patent Citations

  • Semiconductor integrated circuit device and its manufacture and manufacturing apparatus used therefor

    JP1996162534A

  • PVD-imp tungsten and tungsten nitride as liner, barrier and / or seed layer for application of tungsten, aluminum and copper

    JP2001200358A

  • Systems and methods for selective tungsten deposition in vias

    US20120077342A1