Method for calcining nickel hydroxide particles and method for producing nickel oxide fine powder using the same
The method addresses production challenges by firing nickel hydroxide particles in a controlled atmosphere and recovering sulfuric acid from exhaust gases, producing high-quality nickel oxide powder suitable for electronic components and fuel cells.
Patent Information
- Application Number
- JP2020003824
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-01-14
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-01-14
AI Technical Summary
Existing methods for producing fine nickel oxide powder face challenges such as high production costs, particle coarsening at high temperatures, and corrosion of equipment due to sulfuric acid in exhaust gases, leading to impurities in the final product.
A method involving the firing of nickel hydroxide particles in a non-reducing atmosphere with controlled temperature and oxygen partial pressure, followed by sulfuric acid recovery and detoxification of exhaust gases, to produce high-quality nickel oxide powder.
This method efficiently recovers fine nickel oxide powder with low sulfur content and prevents corrosion, ensuring high-quality raw materials for electronic components and solid oxide fuel cells.
Smart Images

Figure 0007559325000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for calcining nickel hydroxide particles, which is an intermediate raw material for nickel oxide fine powder used in electronic components, electrodes of solid oxide fuel cells, etc., and a method for producing nickel oxide fine powder using the same. [Background technology]
[0002] Nickel oxide fine powder is used in various applications, including electronic component materials, and an example of an application of electronic component materials is ferrite parts, which are composite metal oxides. Ferrite parts can be manufactured by mixing nickel oxide fine powder with other raw materials such as iron oxide and zinc oxide, and then firing the mixture. In the process of mixing and firing a plurality of powder raw materials, as in this method of manufacturing ferrite parts, the firing reaction is controlled by a solid-phase diffusion reaction, so it is generally preferable that the powder raw materials have a finer shape. This is because if the powder raw material has a finer shape, the probability of contact with other materials increases and the activity of the particles increases, so that the reaction can proceed uniformly even at a low temperature and in a short time. Thus, it is an important requirement to use fine powders with small particle sizes for the powders used as raw materials for composite metal oxides in order to increase production efficiency.
[0003] The applications of nickel oxide fine powder are expanding beyond electronic components such as the above-mentioned ferrite components. For example, nickel oxide fine powder is used as an electrode material for solid oxide fuel cells, which are expected to be a new power generation system that takes both the environment and energy into consideration. In general, a cell stack for a solid oxide fuel cell has a structure in which single cells each consisting of an air electrode, a solid electrolyte, and a fuel electrode are stacked in order. For this fuel electrode, for example, a mixture of nickel or nickel oxide and a solid electrolyte consisting of stabilized zirconia is used. During power generation, nickel metal is produced at the fuel electrode by reduction with a fuel gas such as hydrogen or hydrocarbon, and the three-phase interface consisting of nickel, the solid electrolyte, and voids becomes a reaction field for the fuel gas and oxygen. Therefore, as in the case of using the above-mentioned ferrite components, it is an important requirement for improving power generation efficiency to use fine powder with a small particle size for the raw material powder used for the fuel electrode.
[0004] Furthermore, nickel oxide fine powder used for the above-mentioned electrode material applications is required to have a low content of impurity elements. Among impurity elements, chlorine (Cl) and sulfur (S) in particular may react with the silver used in the electrodes to cause electrode deterioration and may corrode the firing furnace during the firing process, so it is desirable to reduce them as much as possible. Also, in the traditional application of ferrite parts, electronic parts have recently tended to become increasingly highly functional, so there is a demand to further reduce the content of impurity elements in nickel oxide fine powder used as a raw material.
[0005] Under these circumstances, for example, Patent Document 1 proposes a technology for reducing the sulfur content to 300 to 900 ppm in terms of S and the chlorine content to 100 ppm in terms of Cl at the stage of ferrite powder, which is the raw material for the ferrite material. It is described that the ferrite material of Patent Document 1 can be densified without using additives even when fired at low temperatures, and that ferrite cores and laminated chip components manufactured using this raw material have excellent moisture resistance and temperature characteristics.
[0006] On the other hand, in order to reduce the impurity content in the manufacturing stage of nickel oxide fine powder, a method is generally adopted in which nickel salts such as nickel sulfate, nickel nitrate, nickel carbonate, and nickel hydroxide or nickel metal powder is fired under an oxidizing atmosphere. For example, Patent Document 2 proposes a method for manufacturing nickel oxide powder by a dry method in which a dehydration step of nickel sulfate as a raw material by calcination at 450 to 600°C and a decomposition step of nickel sulfate by roasting at 1000 to 1200°C are clearly separated. It is described that this manufacturing method makes it possible to stably manufacture nickel oxide powder with a low sulfur content and a small average particle size.
[0007] As a method for producing nickel oxide fine powder partially by a wet method in contrast to the above-mentioned dry method, a method has been proposed in which an aqueous solution containing a nickel salt such as nickel sulfate or nickel chloride is neutralized with an alkali such as an aqueous sodium hydroxide solution to crystallize nickel hydroxide particles, which are then roasted. For example, Patent Document 3 proposes a method for producing nickel oxide fine powder by neutralizing an aqueous solution of nickel sulfate with an alkali to produce nickel hydroxide particles, heat-treating the obtained nickel hydroxide particles at a temperature exceeding 850°C and less than 1050°C to produce a sintered body of nickel oxide particles, and crushing the obtained sintered body of nickel oxide particles.
[0008] Patent Document 4 also proposes a method for producing nickel oxide fine powder by pelletizing nickel hydroxide particles obtained by neutralizing an aqueous nickel sulfate solution with an alkali, and then heat treating the pellets at a temperature of 750 to 950°C while introducing a non-reducing gas in a roller hearth kiln or the like. It is described that in these methods for producing nickel oxide fine powder, sulfates, mainly nickel sulfate, remaining without being neutralized, suppress sintering during heat treatment, and nickel sulfate decomposes if the heat treatment temperature exceeds 850°C in the air, for example, making it possible to simultaneously achieve fine particle size and control of the sulfur content. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2002-198213 A [Patent Document 2] JP 2004-123488 A [Patent Document 3] Patent No. 5907169 [Patent Document 4] JP 2019-099394 A Summary of the Invention [Problem to be solved by the invention]
[0010] Although the manufacturing method of Patent Document 2 can obtain nickel oxide fine powder with a low impurity content, this manufacturing method has a problem of high production costs because it requires heat treatment in two stages. In addition, if the roasting temperature is increased to reduce the sulfur content, the particles become coarse, and if the roasting temperature is decreased to suppress the coarsening of the particles, the sulfur content increases, so it has been difficult to simultaneously control the particle size and the sulfur content to optimal values.
[0011] In the manufacturing methods of Patent Documents 3 and 4, nickel oxide fine powder having a fine particle size and a controlled sulfur content can be obtained. However, since the nickel oxide fine powder is likely to fly up, a non-negligible amount of the nickel oxide fine powder is discharged together with the exhaust gas. Therefore, it is necessary to separate and recover the nickel oxide fine powder from the exhaust gas using a dust collector such as an electric dust collector.
[0012] However, in the heat treatments of Patent Documents 3 and 4, the heat treatment temperatures exceed 750°C, and therefore the exhaust gas generated during the heat treatment contains H2O generated by the decomposition of nickel hydroxide and SO2 generated by the decomposition of nickel sulfate. x The SO contained in this exhaust gas x Of these, SO3 can be reacted with H2O in the exhaust gas to be recovered as sulfuric acid, making it relatively easy to render the exhaust gas harmless.
[0013] However, there was a problem that the sulfuric acid thus produced corrodes the nickel oxide fine powder collected by the dust collector, and corrodes ducts, piping systems, etc. that come into contact with the exhaust gas. If the ducts, piping systems, etc. corrode, the iron and chromium eluted thereby may be mixed into the nickel oxide fine powder collected by the dust collector, thereby degrading the quality of the product.
[0014] The present invention has been made in consideration of the above-mentioned conventional problems, and aims to reduce SO generated during the production of nickel oxide fine particles using nickel hydroxide particles generated from nickel sulfate, which is widely used in industry, as a raw material. x The present invention aims to provide a method for calcining nickel hydroxide particles, which is capable of recovering nickel oxide fine powder emitted along with exhaust gas containing nickel hydroxide without compromising the quality of the nickel oxide fine powder, and a method for producing nickel oxide fine powder using the same. [Means for solving the problem]
[0015] In order to achieve the above object, the method for calcining nickel hydroxide particles according to the present invention comprises the steps of: Composed of non-reducing gases A method for calcining nickel hydroxide particles, comprising the steps of: calcining nickel hydroxide particles containing a sulfuric acid component in a calcination furnace into which an atmospheric gas is introduced to produce nickel oxide particles; and treating an exhaust gas discharged from the calcination furnace in a dust collector and a sulfuric acid recovery device in a downstream stage, When the atmospheric gas is air, the firing temperature in the firing furnace is set to 850 to 950°C, and when the atmospheric gas has an oxygen partial pressure of 1 kPa or less, the firing temperature in the firing furnace is set to 750 to 950°C. The temperature of the exhaust gas is controlled until it is discharged from the dust collector. Except for those in which the exhaust gas is cooled by direct heat exchange with a fluid The sulfuric acid recovery apparatus is characterized in that the temperature of the sulfuric acid is controlled so as to exceed the sulfuric acid dew point temperature, and is controlled so as to be equal to or lower than the sulfuric acid dew point temperature during the period from when the sulfuric acid is discharged from the dust collector until when the sulfuric acid is introduced into the sulfuric acid recovery apparatus.
[0016] The method for producing nickel oxide fine powder according to the present invention is characterized in that nickel oxide particles having the form of a sintered body obtained by the above-mentioned method for firing nickel hydroxide particles according to the present invention are subjected to a crushing treatment to obtain nickel oxide fine powder. Effect of the Invention
[0017] According to the present invention, the SO generated during the production of nickel oxide particles is x The nickel oxide fine powder discharged along with the exhaust gas can be recovered from the exhaust gas containing nickel oxide without losing its quality. This makes it possible to efficiently produce high-quality nickel oxide fine powder suitable as a raw material for electronic component materials such as ferrite parts and cell materials for solid oxide fuel cells. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a schematic flow diagram of a calcination facility preferably used in the method for calcining nickel hydroxide particles according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, a method for calcining nickel hydroxide particles containing a sulfuric acid component according to an embodiment of the present invention and a method for producing nickel oxide fine powder using this calcination method will be described, and then the physical properties of the nickel oxide fine powder produced by the method for producing nickel oxide fine powder will be described.
[0020] 1. Method for calcining nickel hydroxide particles containing sulfuric acid components In the method for calcining nickel hydroxide particles containing a sulfuric acid component according to the embodiment of the present invention, nickel hydroxide particles containing a sulfuric acid component are used as a raw material, and the nickel hydroxide particles are charged into a calcination furnace, and calcination treatment is carried out under a predetermined temperature condition while introducing a non-reducing gas, preferably a gas as an atmospheric gas, into the calcination furnace. As a result, the nickel hydroxide is thermally decomposed to generate nickel oxide particles and HO gas, and the sulfuric acid component is thermally decomposed to generate SO x Gas is generated.
[0021] Therefore, the exhaust gas discharged from the calcination furnace contains H2O gas generated by the thermal decomposition of the nickel hydroxide and SO2 gas generated by the thermal decomposition of the sulfuric acid component. x The exhaust gas contains SO xSince nickel oxide is an air pollutant, emission standards have been established. In addition, fine particles of nickel oxide particles generated by the above thermal decomposition are discharged entrained in the air flow of the exhaust gas. If the fine nickel oxide particles discharged entrained in the exhaust gas are discharged directly into the atmosphere, the product yield will decrease.
[0022] Therefore, the exhaust gas discharged from the calcination furnace is generally introduced into an exhaust gas treatment facility, where fine nickel oxide particles contained in the exhaust gas are first collected using a dust collector such as a bag filter or an electric dust collector, and then the exhaust gas is introduced into a sulfuric acid recovery unit to recover the above SO x Among these, SO3 is reacted with H2O to generate sulfuric acid. The exhaust gas treated in the sulfuric acid recovery unit is introduced into a detoxification unit for further detoxification as necessary, and the SO2 and other SO3 remaining in the exhaust gas are detoxified. x is removed until it meets the emission standards.
[0023] In the method for calcining nickel hydroxide particles according to an embodiment of the present invention, the temperature of the exhaust gas is controlled to exceed the sulfuric acid dew point of the exhaust gas in order to prevent corrosion by sulfuric acid until the exhaust gas is discharged from the dust collector, and is controlled to be equal to or lower than the sulfuric acid dew point of the exhaust gas in order to efficiently recover SO3 as sulfuric acid during the period from the exhaust gas discharged from the dust collector to the sulfuric acid recovery device. Hereinafter, the raw materials used in the method for calcining nickel hydroxide particles according to an embodiment of the present invention, the calcination equipment for carrying out the calcination method, and the calcination conditions will be described in detail.
[0024] (1) Raw materials The raw material used in the method for calcining nickel hydroxide particles according to the embodiment of the present invention is nickel hydroxide particles containing a sulfuric acid component. This sulfuric acid component is mainly composed of nickel sulfate, and is mainly present inside or on the surface of the nickel hydroxide particles. The reason for this is that, as described below, nickel hydroxide particles are generally produced by neutralizing an aqueous nickel sulfate solution with a basic solution containing sodium, which causes crystallization, and unreacted nickel sulfate remains in the nickel hydroxide particles. The nickel hydroxide particles used as the raw material are not limited to those produced by the above crystallization, and for example, a mixture of nickel hydroxide particles and nickel sulfate particles may be used.
[0025] As described above, by using nickel hydroxide particles containing a sulfuric acid component, the sintering of the nickel oxide particles after the nickel hydroxide particles are thermally decomposed can be suppressed by the action of the sulfuric acid component. Since the sulfuric acid component such as nickel sulfate is easily thermally decomposed by increasing the firing temperature above the temperature at which the nickel hydroxide is thermally decomposed, for example, by performing a firing treatment at a temperature equal to or higher than the temperature at which nickel sulfate is thermally decomposed, a nickel oxide fine powder with a low sulfur content can be obtained.
[0026] The content of the sulfuric acid component in the nickel hydroxide particles is preferably 0.5 to 2.0 mass% in terms of sulfur content. If the sulfur content is less than 0.5 mass%, the above-mentioned sintering suppression effect becomes insufficient, and nickel oxide fine powder may not be obtained. Conversely, the sulfur content may exceed 2.0 mass%, but in this case, SO generated during the firing treatment may be x Since the amount of gas increases, the processing load increases, which is undesirable from the viewpoint of production costs. The form of the nickel hydroxide particles used as the raw material is not limited to a dry powder, and various forms such as a cake-like wet product after washing and dehydration, or a molded product made of nickel hydroxide particles can be used.
[0027] (2) Firing equipment As shown in FIG. 1 , the calcination equipment used in the method for calcining nickel hydroxide particles according to the embodiment of the present invention is composed of a calcination furnace 1 in which nickel hydroxide particles containing the above-mentioned sulfuric acid component are calcined in the presence of a predetermined atmospheric gas to produce nickel oxide particles, a dust collector 2 in which fine nickel oxide particles are collected from the exhaust gas discharged from the exhaust port of the calcination furnace 1 and discharged together with the exhaust gas, a sulfuric acid recovery device 3 in which the exhaust gas from which the fine nickel oxide particles have been removed in the dust collector is treated to produce sulfuric acid, and a decontamination device 4 in which air pollutants contained in the exhaust gas treated in the sulfuric acid recovery device 3 are removed to a level that satisfies the emission standards, and these devices are connected to each other by ducts and piping.
[0028] The structure of the firing furnace 1 is not particularly limited as long as it can perform firing treatment while continuously introducing atmospheric gas into the furnace, and examples of such furnaces include a pusher furnace in which a container filled with the material to be fired is pushed by a pusher to transport it from one end to the other end of the furnace, a roller hearth kiln in which a container filled with the material to be fired is transported from one end to the other end of the furnace by a group of rollers installed in the furnace, and a rolling furnace such as a rotary kiln in which a cylindrical rotor installed rotatably with its central axis slightly tilted from the horizontal direction is rotated around the central axis, and the material to be fired is introduced from one end on the upper side, and the material is rolled and fired. All of these firing furnaces can provide high productivity, so they are generally selected according to the production volume, etc.
[0029] The calcination furnace 1 is provided with an air inlet, and the calcination process is carried out in a non-reducing atmosphere by introducing atmospheric gas such as air from the air inlet. This atmospheric gas is exhausted from the exhaust port of the calcination furnace 1 as exhaust gas together with gas generated by the calcination process. Specifically, in the calcination furnace 1, nickel hydroxide and nickel sulfate contained in the raw materials undergo thermal decomposition as shown in the following reaction formulas [Formula 1] to [Formula 3] by the calcination process in a non-reducing atmosphere, which produces nickel oxide and SO2 and SO3. x Gases, water vapor (H2O) and oxygen (O2) are evolved.
[0030] [Formula 1] Ni(OH)2 →NiO+H2O [Formula 2] 2NiSO4 → 2NiO+2SO2+O2 [Formula 3] NiSO4 → NiO+SO3
[0031] The gas generated by the above pyrolysis is released into the atmosphere in the firing furnace 1 and mixes with the atmospheric gas introduced from the above air inlet, so in order to efficiently proceed with the firing process, it is preferable to continuously introduce the atmospheric gas from the air inlet and continuously exhaust the exhaust gas from the above exhaust port. That is, according to Le Chatelier's principle, the partial pressure of water vapor in the atmosphere in the firing furnace 1, SO x The lower the partial pressure of oxygen and the partial pressure of oxygen, the more the reactions in the above reactions 1 to 3 proceed to the right. x If the gas containing water vapor, SO, and oxygen can be carried by the air current in the kiln 1 and quickly transported to the exhaust port and exhausted, the water vapor, SO x In addition, the partial pressure of oxygen is reduced, which can promote the thermal decomposition of nickel hydroxide and nickel sulfate.
[0032] However, when exhaust gas is continuously discharged while continuously introducing atmospheric gas into the calcination furnace 1 as described above, the air current formed in the calcination furnace 1 tends to stir up nickel oxide particles having fine shapes, and some of the nickel oxide particles are discharged from the exhaust port together with the exhaust gas. Therefore, as shown in Fig. 1, the exhaust gas discharged from the exhaust port of the calcination furnace 1 is first introduced into a dust collector 2 to recover the nickel oxide particles entrained therein, and then introduced into a sulfuric acid recovery device 3 at the rear stage to recover the SO2 contained in the exhaust gas. x Sulfuric acid is generated from the sulfuric acid recovery unit 3. The exhaust gas discharged from the sulfuric acid recovery unit 3 is introduced into a detoxification unit 4 as necessary for detoxification. In some cases, the raw material nickel hydroxide particles may be contained in the exhaust gas without reacting.
[0033] As described above, the dust collection method of the dust collector 2 that collects nickel oxide particles from the exhaust gas is not particularly limited, and a cyclone that applies centrifugal force, an electric dust collector that applies static electricity, a filter-type dust collector (bag filter) that applies gas-solid separation by a filter, etc. can be adopted, but a filter-type dust collector is preferred because it can easily increase the collection rate of nickel oxide particles and can reuse the collected nickel oxide particles at a relatively low cost. As the temperature of the exhaust gas needs to be maintained above the sulfuric acid dew point temperature as described later, the material of the filter used in this filter-type dust collector is one that has heat resistance so that it can be used under said temperature conditions, and for example, a ceramic filter is preferably used.
[0034] In the method for calcining nickel hydroxide particles containing a sulfuric acid component according to the embodiment of the present invention, the temperature of the exhaust gas is controlled so as to exceed the sulfuric acid dew point temperature until it is discharged from the dust collector 2. The reason for this is that if the temperature of the exhaust gas when it is treated by the dust collector 2 is equal to or lower than the sulfuric acid dew point temperature, sulfuric acid is easily generated by the SO3 contained in the exhaust gas, and the nickel oxide particles recovered by the dust collector 2 may be corroded by the generated sulfuric acid, or piping components (iron, chromium, etc.) eluted by the sulfuric acid may be mixed into the nickel sulfate particles.
[0035] By carrying out the above-mentioned temperature control, the nickel oxide particles recovered in the dust collector 2 can be mixed with most of the nickel oxide particles discharged from the calcination furnace 1, or can be reused as a raw material for the calcination process. The sulfuric acid dew point temperature of the exhaust gas may be determined by measurement using a commercially available dew point meter, or may be determined by measuring the SO3 concentration and HO concentration of the exhaust gas using a gas composition measuring device such as gas chromatography and comparing these concentrations with a calibration curve prepared in advance.
[0036] The sulfuric acid recovery device 3 located at the rear of the dust collector 2 is a device that generates sulfuric acid from water vapor and SO3 contained in the exhaust gas, and the specific device configuration is not particularly limited, and known technology can be used. For example, a wet type device that generates sulfuric acid by absorbing SO3 into circulating concentrated sulfuric acid or water, or a device that utilizes the principle that water vapor reacts with SO3 to become sulfuric acid when condensed can be used. Note that, before absorbing or reacting SO3 as described above, a process of oxidizing SO2 to SO3 using a catalyst or the like may be performed. In the sulfuric acid recovery device 3 that recovers sulfuric acid from SO3 in this way, it is desirable that the temperature of the exhaust gas is lower than the temperature at which the water vapor condenses, that is, the sulfuric acid dew point temperature. Therefore, the temperature of the exhaust gas is controlled so that it is lower than the sulfuric acid dew point temperature during the time from when it is discharged from the dust collector 2 to when it is introduced into the sulfuric acid recovery device 3.
[0037] The detoxification device 4 removes sulfur oxides such as SO2 in the exhaust gas discharged from the sulfuric acid recovery device 3 until the emission standard is met. There is no particular limitation on the method for removing sulfur oxides such as SO2 in the detoxification device 4, and a known method can be used. For example, there can be mentioned an absorption neutralization method in which the exhaust gas is brought into gas-liquid contact with an alkaline aqueous solution circulating in a packed tower.
[0038] (3) Firing conditions In the calcination method according to the embodiment of the present invention, in order to prevent the produced nickel oxide from being reduced to nickel, it is preferable to continuously introduce a non-reducing gas into the calcination furnace 1 to make the atmosphere during the calcination treatment in the calcination furnace 1 a non-reducing atmosphere, and more preferably an air atmosphere or a low oxygen partial pressure atmosphere. In the case of an air atmosphere, the calcination temperature, i.e., the atmospheric temperature in the calcination furnace 1, is preferably in the range of 850 to 950°C, and in the case of a low oxygen partial pressure atmosphere, the calcination temperature is preferably in the range of 750 to 950°C. The above calcination temperature can be measured with a thermometer provided in the calcination furnace 1. Hereinafter, the reason why the above calcination conditions are preferable will be explained from the viewpoint of the reaction mechanism.
[0039] Nickel hydroxide particles change into nickel oxide at temperatures of 600°C or higher, while nickel sulfate decomposes at temperatures of 850°C or higher in the air atmosphere, and at temperatures of about 750°C or higher in a non-reducing atmosphere with a low oxygen partial pressure. As can be seen from the above [Equation 2] and [Equation 3], the reason why the decomposition temperature differs depending on the atmosphere in the sintering furnace 1 is due to the presence of SO in the atmospheric gas. x This is because the lower the partial pressure of O2, the more the decomposition reaction of nickel sulfate is accelerated.
[0040] More specifically, when the atmosphere in the calcination furnace 1 during the calcination process is an air atmosphere, the oxygen partial pressure is 21 kPa when converted from 1 atmosphere, which is the air atmosphere (air atmosphere), and the decomposition temperature of nickel sulfate is 840°C. Therefore, in the calcination process in an air atmosphere at a calcination temperature of less than 850°C, the thermal decomposition of nickel sulfate is difficult to proceed, and sulfur components remain in the nickel oxide particles, so that nickel oxide fine powder with a sulfur content of 100 mass ppm or less may not be obtained. On the other hand, when the calcination temperature exceeds 950°C, sintering of nickel oxide particles generated by thermal decomposition of nickel hydroxide particles proceeds too much, and it becomes difficult to crush the secondary particles generated by this sintering to a desired particle size or to refine them to primary particles in the subsequent crushing process. As a result, there is a risk that a powder having a specific surface area and D50 suitable for use as an electronic component material or battery material cannot be obtained.
[0041] On the other hand, as can be seen from the above [Formula 2], the decomposition of nickel sulfate is promoted by calcining in an atmosphere with a lower oxygen partial pressure, so that when the atmosphere in the calcination furnace 1 during the calcination treatment is a low oxygen partial pressure atmosphere, nickel oxide powder with a sulfur content reduced to the same level as that in the air atmosphere can be obtained even if the calcination temperature is lowered compared to the air atmosphere. Therefore, the amount of energy consumed during the calcination treatment can be reduced.
[0042] Specifically, in a non-reducing atmosphere in which the oxygen partial pressure is reduced to 1 kPa, the decomposition temperature of nickel sulfate is 750° C. Therefore, in a firing treatment at a firing temperature of 750° C., a non-reducing atmosphere with an oxygen partial pressure of 1 kPa or less is preferable, a non-reducing atmosphere with an oxygen partial pressure of 0.5 kPa or less is more preferable, and a non-reducing atmosphere with an oxygen partial pressure of 100 Pa or less is even more preferable. If the oxygen partial pressure exceeds 1 kPa, the thermal decomposition of nickel sulfate becomes insufficient under temperature conditions of a firing temperature of less than 750° C., and nickel oxide fine powder with a sulfur content of 100 mass ppm or less may not be obtained.
[0043] However, even if the oxygen partial pressure in the atmosphere in the firing furnace during the firing treatment exceeds 1 kPa, there are conditions under which nickel sulfate can be thermally decomposed by setting the firing temperature to 800° C. or higher as long as the atmosphere is a non-reducing atmosphere with a low oxygen partial pressure. In this case, it is preferable to select the firing temperature within a temperature range of 950° C. or lower, taking into consideration the time required for thermal decomposition.
[0044] When the oxygen partial pressure is 21 kPa or less, if the firing temperature exceeds 950°C, the sintering of the nickel oxide particles obtained by thermal decomposition of the nickel hydroxide particles proceeds too much, as in the case of the air atmosphere, and it becomes difficult to pulverize the secondary particles obtained by this sintering by crushing or the like, and there is a risk that a powder having a desired specific surface area and D50 suitable for electronic component materials and battery materials cannot be obtained. There is no particular limit to the lower limit of the oxygen partial pressure, but a value of 10 Pa can sufficiently reduce the sulfur content of the nickel oxide powder. Of course, this does not exclude cases where the oxygen partial pressure is even lower.
[0045] The non-reducing gas introduced into the calcination furnace 1 is preferably a gas mainly composed of one selected from air, nitrogen, carbon dioxide, water vapor, argon, and helium. In this case, one selected from air, nitrogen, carbon dioxide, water vapor, argon, and helium may be introduced directly into the calcination furnace 1, or when the main component is nitrogen, carbon dioxide, water vapor, argon, or helium other than air, the gas may be introduced into the calcination furnace 1 after containing oxygen at an oxygen partial pressure of less than 21 kPa, preferably at an oxygen partial pressure of 1 kPa or less. Alternatively, the amount of exhaust of the atmospheric gas in the calcination furnace 1 may be adjusted so that the atmosphere in the calcination furnace 1 is reduced in pressure and the oxygen partial pressure is less than 21 kPa, preferably at an oxygen partial pressure of 1 kPa or less.
[0046] 2. Manufacturing method of nickel oxide fine powder Next, a method for producing nickel oxide fine powder according to an embodiment of the present invention will be described. The method for producing nickel oxide fine powder includes a crystallization step of mixing a nickel sulfate aqueous solution with a sodium hydroxide solution to cause a neutralization reaction to crystallize nickel hydroxide particles, a firing step of firing the nickel hydroxide particles containing a sulfuric acid component obtained in the crystallization step in a firing furnace into which a specific atmospheric gas is introduced as described above to produce nickel oxide powder, and a crushing step of crushing the sintered body of the nickel oxide powder obtained in the firing step to obtain nickel oxide fine powder. The nickel hydroxide particles containing a sulfuric acid component used as a raw material in the above-mentioned firing step may be produced by a method other than the above-mentioned crystallization step.
[0047] The nickel oxide fine powder obtained by the above manufacturing method can suppress the sulfur content to 100 mass ppm or less, even when nickel hydroxide particles containing a sulfuric acid component produced by crystallization from an aqueous solution of nickel sulfate, which is widely used in nickel plating, are used as the raw material, and the average particle size D50 (particle size at 50% of the volume of the particle amount in the particle size distribution) measured by a laser scattering method can be made to be 0.6 μm or less. In addition, the specific surface area can be made to be 2 m or less. 2 / g or more. This makes it possible to obtain nickel oxide fine powder suitable for applications such as electronic component materials and electrode materials for solid oxide fuel cells. Hereinafter, the crystallization step, calcination step, and crushing step constituting the method for producing nickel oxide fine powder according to the embodiment of the present invention will be described in detail, excluding the calcination step already described.
[0048] (1) Crystallization process The crystallization step is a step in which an aqueous nickel sulfate solution and a sodium hydroxide solution are mixed as raw materials in a reaction tank to cause a neutralization reaction, thereby crystallizing nickel hydroxide particles. Nickel sulfate hexahydrate, for example, can be used as the nickel sulfate used as the raw material, but since the resulting nickel oxide fine powder is ultimately used as a material for electronic components or batteries, it is desirable for the impurities contained in the nickel sulfate to be less than 100 ppm by mass in order to prevent corrosion.
[0049] An aqueous solution is prepared by adding an appropriate amount of water to the nickel sulfate and mixing. In this preparation, the concentration of nickel in the nickel sulfate aqueous solution is not particularly limited, but it is preferable to set the nickel concentration to 50 to 150 g / L. If the nickel concentration is less than 50 g / L, the productivity is too low. Conversely, if the nickel concentration exceeds 150 g / L, the anion concentration in the nickel sulfate aqueous solution becomes too high, and the sulfur content in the nickel hydroxide produced by crystallization becomes high. As a result, the sulfur content, which becomes an impurity in the nickel oxide fine powder produced using this as an intermediate raw material, may not be suppressed to 100 mass ppm or less as described above. The solvent for sodium hydroxide used for neutralization is not particularly limited, and may be water or a mixture of water and a water-soluble organic solvent such as alcohol.
[0050] In the above crystallization step, in order to efficiently produce homogeneous nickel hydroxide particles, it is preferable to adopt a continuous crystallization method. In this case, it is preferable to prepare a sodium hydroxide solution and an aqueous nickel sulfate solution, which is an aqueous nickel salt solution, in advance, and add these two previously prepared solutions in parallel and continuously to a solution being sufficiently stirred in a reaction tank, preferably by a so-called double jet method.
[0051] That is, the neutralization reaction is not carried out by adding one of the nickel salt aqueous solution and the sodium hydroxide solution to the other of the two solutions stored in the reaction tank beforehand, but is preferably carried out by simultaneously and continuously adding the nickel salt aqueous solution and the sodium hydroxide solution to the liquid in the reaction tank that is sufficiently stirred and in a turbulent state, preferably while continuing the stirring. In this case, the liquid placed in the reaction tank beforehand is preferably pure water adjusted to a predetermined pH by adding sodium hydroxide.
[0052] During the neutralization reaction, it is preferable to adjust the pH of the reaction solution in the reaction tank to within the range of 8.3 to 9.0. If the pH is lower than 8.3, the concentration of anion components such as sulfate ions remaining in the nickel hydroxide particles increases, and these ions are converted into a large amount of SO 2 during the subsequent calcination step. x On the other hand, if the pH is higher than 9.0, the precipitated nickel hydroxide particles become too fine, and the filterability of the slurry containing these fine nickel hydroxide particles is quickly reduced when the slurry is subjected to solid-liquid separation using a filtration device, for example, or sintering proceeds too much in the subsequent firing step, making it difficult to obtain a fine nickel oxide powder even when the slurry is treated in the crushing step described below.
[0053] At pH 9.0 or less, which is the preferable neutralization condition, a small amount of nickel may remain in the aqueous solution after the reaction, but in this case, the amount of nickel in the filtrate obtained by the filtration can be reduced by raising the pH to about 10 after the crystallization is almost complete. It is preferable to keep the pH almost constant during the neutralization reaction, and it is particularly preferable to control the pH to a constant value within a range of ±0.2 around the set value. If the pH fluctuates beyond this range, there is a risk of impurities increasing or the specific surface area of the nickel oxide powder decreasing.
[0054] There is no particular restriction on the temperature of the reaction solution during the neutralization reaction, and it may be about room temperature, but it is preferable that the temperature is within the range of 50 to 70°C, since nickel hydroxide particles can be sufficiently grown. This can prevent the nickel hydroxide particles from excessively containing sulfur, and can suppress impurities such as sodium from being entrained in the nickel hydroxide particles, thereby reducing the impurity grade of the finally obtained nickel oxide fine powder. If the liquid temperature is less than 50°C, the nickel hydroxide particles will not grow sufficiently, and the amount of impurities such as sulfur entrained in the nickel hydroxide particles may increase. Conversely, if the liquid temperature exceeds 70°C, the amount of water evaporated increases, and the concentration of impurities such as sulfur in the aqueous solution increases, so that the impurity grade of the generated nickel hydroxide particles such as sulfur may increase.
[0055] In the above crystallization step, the reaction time of the neutralization reaction is preferably 0.2 to 5 hours. Here, the reaction time of the neutralization reaction is the time during which a predetermined neutralization reaction condition is maintained. For example, when the neutralization reaction is carried out in a continuous complete mixing tank type reaction tank, the reaction time is the time obtained by dividing the effective volume by the total supply amount of the nickel sulfate aqueous solution and the alkaline aqueous solution, which corresponds to the residence time in this case. For example, when the nickel sulfate aqueous solution and the alkaline aqueous solution are supplied at a total rate of 20 L / h to a reaction tank whose effective volume is maintained at 10 L by providing an overflow section, the reaction time is 10 / 20=0.5 hours.
[0056] If the reaction time is less than 0.2 hours, the amount of sulfur remaining in the nickel hydroxide particles is likely to increase, and conversely, if it exceeds 5 hours, the amount of sodium remaining in the nickel hydroxide particles is likely to increase. Therefore, in either case, there is a risk that the impurity quality of the finally obtained nickel oxide fine powder will increase. After the neutralization reaction is completed, the precipitate or slurry containing the nickel hydroxide particles obtained by crystallization is introduced into a solid-liquid separation means such as a filter press, a centrifuge, or a filter, where a solid-liquid separation process is performed to recover the solid side consisting of the nickel hydroxide particle group in the form of a wet lump (hereinafter also referred to as a cake or wet cake).
[0057] The cake recovered by the solid-liquid separation may be washed with a washing liquid such as water as necessary. In this case, a preferred washing method is repulping washing, in which the cake is washed in the form of a slurry by adding a washing liquid to the cake and stirring it, and then the slurry is introduced into a solid-liquid separation means to separate the solid content from the washing liquid. This repulping washing can effectively remove anions such as sulfate ions and sodium components mixed in the nickel hydroxide particles, so when it is required to particularly reduce the impurity quality of the finally obtained nickel oxide fine powder, it is preferable to perform repulping washing before the calcination treatment, and in that case, it is more preferable to use pure water as the washing liquid.
[0058] When repulp washing is performed using water, the mixing ratio of water to nickel hydroxide particles is not particularly limited as long as the alkali metal components such as sodium contained in the nickel hydroxide can be sufficiently removed, but in general, it is preferable to mix 1 L of washing solution to 50 to 150 g of nickel hydroxide, and more preferably to mix 1 L of washing solution to about 100 g of nickel hydroxide. With the above mixing ratio, the concentration of impurities such as alkali metals remaining in the nickel hydroxide can be sufficiently reduced and the nickel hydroxide particles can be well dispersed.
[0059] The washing time in the above-mentioned repulping washing is not particularly limited as long as the residual impurities in the nickel hydroxide particles can be sufficiently reduced, but it is generally preferable to adjust it appropriately according to the washing conditions such as the mixing ratio and temperature of the above-mentioned washing solution. If impurities such as alkali metals are not sufficiently reduced by one washing, it is preferable to repeat the above-mentioned repulping washing several times. In particular, alkali metals such as sodium cannot be removed by the heat treatment in the subsequent calcination step, so it is preferable to remove them sufficiently by this washing treatment.
[0060] When pure water is used as the washing liquid, for example, washing can be repeated until the electrical conductivity of the washing liquid measured after washing is equal to or lower than a predetermined value, thereby suppressing the variation in the quality of impurities. The solid-liquid separation means employed in the above-mentioned repulp washing is not particularly limited, and known solid-liquid separation means such as filtration can be used. This solid-liquid separation means again produces a wet cake consisting of nickel hydroxide particle groups. The obtained wet cake is dried as necessary, and then calcined in the above-mentioned calcination step. The conditions of this drying treatment are not particularly limited, and it is preferable to dry it in an air atmosphere at about 100 to 150°C for about 8 to 24 hours, for example.
[0061] (2) Crushing process The crushing step is a step of breaking the sintered body of nickel oxide particles produced by the above-mentioned firing step to separate the bonds between primary particles, thereby obtaining nickel oxide fine powder. That is, as described above, nickel hydroxide particles are thermally decomposed to produce nickel oxide particles in the firing step, and although the nickel oxide particles are prevented from becoming coarse by the sulfuric acid component as described above, the resulting fine primary particles of nickel oxide are sintered to some extent due to the influence of high temperature. In order to break the sintered parts of the sintered body consisting of secondary particles produced by this sintering, a crushing treatment is performed on the nickel oxide powder after the firing treatment. In this crushing treatment, secondary particles are caused to collide with each other or a compressive force or a shear force is applied to the secondary particles to produce nickel oxide fine powder having a desired particle size.
[0062] The crushing device used in this crushing process is not particularly limited, and a general one can be used. For example, it may be a grinder that charges nickel oxide powder together with crushing media such as a bead mill or a ball mill into a container and rotates the container to perform the crushing process, or it may be a grinder such as a jet mill that uses the fluid energy of the nickel oxide powder itself to perform the crushing process by shearing or collision between particles without using crushing media. In addition, depending on the target particle size, a grinder such as Masscolloider (registered trademark) may be used. The sintered body of nickel oxide generated in the previous firing process is usually a secondary particle formed by agglomeration and sintering of primary particles with an average particle size D50 of about 0.3 to 0.6 μm. For example, when the particle size of the target powder is about 10 to 20 μm in average particle size D50, a grinder can be used, and when it is required to crush the powder to almost primary particles, a grinder can be used.
[0063] 3.Physical properties of nickel oxide fine powder The nickel oxide fine powder produced by the manufacturing method consisting of the above-mentioned series of steps has a controlled sulfur content and an extremely small and fine particle size. Specifically, by appropriately adjusting the conditions of each of the above-mentioned steps, the sulfur content can be reduced to 100 mass ppm or less, more preferably 50 mass ppm or less, and by crushing to almost primary particles, the average particle size D50 measured by a laser scattering method can be reduced to 0.6 μm or less, more preferably 0.3 to 0.6 μm, and even more preferably 0.35 to 0.50 μm.
[0064] Furthermore, the nickel oxide fine powder has a specific surface area of 2.0 m2 as measured by the BET method. 2 Although there is no particular upper limit to this specific surface area, the nickel oxide fine powder obtained by the above-described manufacturing method usually has a specific surface area of 6.0 m 2 This specific surface area can be increased to a more preferable range of 3.0 to 6.0 m / g by appropriately adjusting the crushing conditions, etc. 2 / g, the particularly preferred range is 3.5 to 5.0 m 2 / g. Thus, the nickel oxide fine powder produced by the manufacturing method according to the embodiment of the present invention is particularly suitable as an electronic component material, such as a material for ferrite parts, or a battery material, such as an electrode material for solid oxide fuel cells. Note that the electrode material for solid oxide fuel cells preferably has a sulfur content of 100 ppm by mass or less. [Explanation of symbols]
[0065] 1. Calcination furnace, 2. Dust collector, 3. Sulfuric acid recovery device, 4. Harmful substance removal device
Claims
1. A method for calcining nickel hydroxide particles, comprising the steps of: calcining nickel hydroxide particles containing a sulfuric acid component in a calcination furnace into which an atmospheric gas consisting of a non-reducing gas is introduced to produce nickel oxide particles; and treating an exhaust gas discharged from the calcination furnace in a dust collector and a sulfuric acid recovery device in a downstream stage, When the atmospheric gas is air, the firing temperature in the firing furnace is set to 850 to 950°C, and when the atmospheric gas has an oxygen partial pressure of 1 kPa or less, the firing temperature in the firing furnace is set to 750 to 950°C. A method for calcining nickel hydroxide particles, comprising: controlling the temperature of the exhaust gas so that it exceeds the sulfuric acid dew point temperature until it is discharged from the dust collector, except for a case in which the exhaust gas is cooled by direct heat exchange with a fluid; and controlling the temperature of the exhaust gas so that it is equal to or lower than the sulfuric acid dew point temperature during the period from when the exhaust gas is discharged from the dust collector to when the exhaust gas is introduced into the sulfuric acid recovery device.
2. 2. The method for calcining nickel hydroxide particles according to claim 1, wherein the non-reducing gas is mainly composed of one gas selected from the group consisting of air, nitrogen, carbon dioxide, water vapor, argon, and helium.
3. 3. The method for calcining nickel hydroxide particles according to claim 2, wherein the calcination temperature in the calcination furnace is set to 800 to 950° C. when the oxygen partial pressure of the atmospheric gas is within a range of more than 1 kPa and less than 21 kPa.
4. The method for calcining nickel hydroxide particles according to any one of claims 1 to 3, characterized in that the nickel hydroxide particles containing a sulfuric acid component are produced by crystallization caused by mixing an aqueous nickel sulfate solution with a sodium hydroxide solution.
5. A method for producing a fine nickel oxide powder, comprising the steps of: subjecting nickel oxide particles having a sintered form obtained by the method for firing nickel hydroxide particles according to any one of claims 1 to 4 to a crushing treatment to obtain a fine nickel oxide powder.
6. The nickel oxide fine powder has a sulfur content of 100 mass ppm or less, an average particle size D50 of 0.6 μm or less, and a specific surface area of 2.0 m 2 The method for producing a nickel oxide fine powder according to claim 5, wherein the nickel oxide fine powder has a surface area of 100 μm or more.
Citation Information
Patent Citations
JP1973006395U
Carbostyryl derivative
JP1984007169A
Low-temperature baked high-performance ferrite material and ferrite part
JP2002198213A
Method for manufacturing nickel oxide powder
JP2004123488A
Method for producing nickel oxide and fluidization calcinating furnace
JP2018012625A