Anode active material, alkaline storage battery, and method for producing anode active material
A TiCr-based hydrogen storage alloy with a metastable BCC structure, coated with a catalytic and oxygen-affinity metal layer, addresses the cost issue of vanadium and enhances capacity by managing oxide film diffusion, resulting in improved alkaline storage battery performance.
Patent Information
- Application Number
- JP2021135619
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-23
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-08-23
AI Technical Summary
TiCrV-based hydrogen storage alloys with a body-centered cubic structure (BCC) offer excellent capacity characteristics but are hindered by the high cost of vanadium, and reducing its proportion complicates maintaining the BCC structure as a stable phase.
A TiCr-based hydrogen storage alloy with a metastable BCC structure is coated with a layer containing a catalytic metal and an oxygen-affinity metal, where the oxide film at the interface is managed to ensure oxygen diffusion during heat treatment, maintaining the BCC structure and enhancing capacity characteristics.
The described negative electrode active material achieves improved capacity characteristics by ensuring the BCC structure is maintained while facilitating hydrogen diffusion, overcoming the limitations of TiCrV-based alloys.
Smart Images

Figure 0007559706000006 
Figure 0007559706000007 
Figure 0007559706000008
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a negative electrode active material, an alkaline storage battery, and a method for producing a negative electrode active material. [Background technology]
[0002] Hydrogen storage alloys are known as negative electrode active materials for alkaline storage batteries. For example, Patent Document 1 discloses a method for manufacturing a hydrogen storage alloy electrode, which includes a step of mixing a hydrogen storage alloy that contains at least Ti, does not contain Ni, has a body-centered cubic structure, and has a spherical particle shape with Ni powder, applying a shear force to the resulting mixture to cause Ni to adhere to the surface of the hydrogen storage alloy, and a step of heat-treating the hydrogen storage alloy with Ni adhered to the surface to form an alloy layer containing at least Ti and Ni on the surface part of the hydrogen storage alloy. Furthermore, an example of Patent Document 1 discloses a TiCrV-based hydrogen storage alloy. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-141061 A Summary of the Invention [Problem to be solved by the invention]
[0004] TiCrV-based hydrogen storage alloys with a body-centered cubic (BCC) structure have the advantage of having excellent capacity characteristics. On the other hand, since V (vanadium) is expensive, it is desirable to reduce the proportion of V in the hydrogen storage alloy. However, if the proportion of V in the hydrogen storage alloy is low, it becomes difficult to produce a hydrogen storage alloy with a BCC structure as a stable phase.
[0005] In response to this, the present inventors have found that it is possible to prepare a TiCr-based hydrogen storage alloy that does not contain V and has a BCC structure as a metastable phase, for example, by using a gas atomization method. However, the TiCr-based hydrogen storage alloy that has a BCC structure as a metastable phase does not exhibit capacity characteristics and does not function as a negative electrode active material.
[0006] The present disclosure has been made in view of the above-mentioned circumstances, and has as its main object to provide a negative electrode active material having good capacity characteristics. [Means for solving the problem]
[0007] In the present disclosure, there is provided a negative electrode active material for use in an alkaline storage battery, the negative electrode active material comprising a base material containing Ti and Cr and having a BCC structure as a metastable phase, and a coating layer covering the base material and containing a catalytic metal and an oxygen affinity metal having an oxygen affinity equal to or higher than that of Ti, the negative electrode active material having an oxide film at the interface between the coating layer and the base material, and a maximum oxygen concentration C of the oxide film in the vicinity of the interface is determined by Auger electron spectroscopy. MAX (at%) and the above C MAX The position P1 where the above C MAX Half the value is 1 / 2C MAX In the region on the coat layer side of P1, MAX The position where A In the region on the base material side of position P1, MAX The position where B Let P1 be the first digit of P A The distance to the first thickness T of the oxide film is A (nm), and the above P1 to P B The distance to the second thickness T of the oxide film is B (nm), and the above P A From the above P B The distance from the oxide film to the target is defined as the thickness T (nm) of the oxide film, and the measurement interval in the depth direction is defined as D I (nm), the negative electrode active material is (i)T above B For the above TA Proportion (T A / T B ) is 1.50 or more, (ii) The above T A and the above T B The difference (T A -T B ) but the above D I Greater than (iii) the above C against the above T MAX The ratio of (C MAX / T) is 0.035 or less, The present invention provides a negative electrode active material that satisfies at least one of the above.
[0008] According to the present disclosure, by satisfying at least one of the above (i) to (iii), a negative electrode active material having good capacity characteristics is obtained.
[0009] In the above disclosure, the negative electrode active material may satisfy the above (i).
[0010] In the above disclosure, the negative electrode active material may satisfy the above (ii).
[0011] In the above disclosure, the negative electrode active material may satisfy the above (iii).
[0012] In the above disclosure, the coating layer may contain at least one of Ni, Pd and Pt as the catalytic metal.
[0013] In the above disclosure, the coating layer may contain Ti as the oxygen affinity metal.
[0014] In the above disclosure, the coating layer may contain La as the oxygen affinity metal.
[0015] In the above disclosure, the base material may contain V, and the proportion of V in the base material may be less than 10 at %.
[0016] In the above disclosure, the base material does not necessarily need to contain V.
[0017] The present disclosure also provides an alkaline storage battery having a positive electrode active material layer, a negative electrode active material layer, and an electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, wherein the negative electrode active material layer contains the above-mentioned negative electrode active material.
[0018] According to the present disclosure, since the negative electrode active material layer contains the above-mentioned negative electrode active material, an alkaline storage battery having good capacity characteristics is obtained.
[0019] The present disclosure also provides a method for producing a negative electrode active material for use in an alkaline storage battery, the method comprising the steps of: coating a base material that contains Ti and Cr and has a BCC structure as a metastable phase with a coating layer that contains a catalytic metal and an oxygen affinity metal that has an oxygen affinity equal to or greater than that of Ti; forming a precursor; and subjecting the precursor to a heat treatment so as to diffuse oxygen contained in an oxide film that is present at the interface between the coating layer and the base material while maintaining the BCC structure in the base material.
[0020] According to the present disclosure, a precursor is subjected to a heat treatment so as to diffuse oxygen contained in an oxide film present at the interface between a coating layer and a base material while maintaining the BCC structure of the base material, thereby obtaining a negative electrode active material having good capacity characteristics. Effect of the Invention
[0021] The negative electrode active material according to the present disclosure has an effect of having good capacity characteristics. [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic cross-sectional view illustrating an example of a negative electrode active material according to the present disclosure. [Diagram 2] FIG. 2 is a ternary diagram illustrating the composition of a base material in the present disclosure. [Diagram 3]FIG. 1 is a schematic cross-sectional view illustrating an alkaline storage battery according to the present disclosure. [Figure 4] FIG. 1 is a schematic cross-sectional view illustrating an alkaline storage battery according to the present disclosure. [Diagram 5] FIG. 2 is a flow diagram illustrating a method for producing a negative electrode active material according to the present disclosure. [Figure 6] 1 shows the results of AES analysis of the precursor prepared in Comparative Example 1. [Figure 7] 1 shows the results of AES analysis of the precursor prepared in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The negative electrode active material, the alkaline storage battery, and the method for producing the negative electrode active material will be described in detail below.
[0024] A.Negative electrode active material FIG. 1 is a schematic cross-sectional view illustrating an example of an anode active material in the present disclosure. The anode active material 10 shown in FIG. 1 has a base material 1 and a coating layer 2 that coats the base material 1. The base material 1 contains Ti and Cr, and contains a BCC structure as a metastable phase. The coating layer 2 contains a catalyst metal and an oxygen affinity metal having an oxygen affinity equal to or higher than that of Ti. Furthermore, the base material 1 has an oxide film 3 on the surface on the coating layer 2 side. That is, the oxide film 3 exists between the coating layer 2 and the base material 1. The oxide film 3 is typically a passivation film of the base material 1. In the present disclosure, the diffusion state of oxygen contained in the oxide film 3 satisfies a predetermined condition.
[0025] According to the present disclosure, the diffusion state of oxygen contained in the oxide film satisfies a predetermined condition, and thus the negative electrode active material has good capacity characteristics. As described above, the TiCrV-based hydrogen storage alloy having a body-centered cubic structure (BCC structure) has the advantage of having excellent capacity characteristics. On the other hand, since V (vanadium) is expensive, it is desired to reduce the proportion of V in the hydrogen storage alloy. However, if the proportion of V in the hydrogen storage alloy is low, it becomes difficult to prepare a hydrogen storage alloy having a BCC structure as a stable phase.
[0026] In response to this, the present inventors have found that it is possible to prepare a TiCr-based hydrogen storage alloy that does not contain V and has a BCC structure as a metastable phase, for example, by using a gas atomization method. However, the TiCr-based hydrogen storage alloy that has a BCC structure as a metastable phase does not exhibit capacity characteristics and does not function as a negative electrode active material.
[0027] Therefore, the present inventors have investigated using a TiCr-based hydrogen storage alloy containing a BCC structure as a metastable phase as a base material and coating the base material with a coating layer having a catalytic effect. However, as described in the comparative example below, the capacity characteristics were not achieved by simply coating the base material with a coating layer. Therefore, the inventors have conducted detailed investigations into the interface between the base material and the coating layer, and have found that the oxide film present at the interface between the base material and the coating layer inhibits hydrogen diffusion necessary for charge / discharge reactions.
[0028] For example, in the case of a negative electrode active material containing a BCC structure as a stable phase, the BCC structure does not transform into another structure by heat treatment. Therefore, for example, by heat treating the negative electrode active material at a sufficiently high temperature (for example, 700°C or higher), it is possible to remove the oxide film by thermal diffusion. In contrast, in the case of a negative electrode active material containing a BCC structure as a metastable phase, if the material is heat treated at a high temperature, the oxide film can be removed, but the BCC structure cannot be maintained. Conversely, if the material is heat treated at a temperature at which the BCC structure can be maintained, the oxide film cannot be removed. In other words, in the case of a negative electrode active material containing a BCC structure as a metastable phase, there is a unique problem that it is difficult to maintain the BCC structure and remove the oxide film at the same time.
[0029] Therefore, the inventors of the present invention conducted extensive research and found that by adding an oxygen affinity metal having an oxygen affinity equal to or greater than Ti to the coating layer, the oxygen contained in the oxide film can be actively diffused to the coating layer even when the coating layer is heat-treated at a temperature at which the BCC structure can be maintained. In other words, it was found that oxygen can be peeled off from the oxide film and moved to the coating layer. As a result, the inhibition of hydrogen diffusion by the oxide film was alleviated, and as a result, a negative electrode active material having good capacity characteristics was obtained.
[0030] In the present disclosure, the diffusion state of oxygen contained in the oxide film is identified by elemental analysis using Auger electron spectroscopy (AES). Specifically, the maximum oxygen concentration C MAX (at%) and C MAX Next, we find the position P1 where C MAX Half the value is 1 / 2C MAX In the area on the coat layer side of P1, 1 / 2C MAX The position where A In addition, in the region closer to the base material than position P1, 1 / 2C MAX The position where B Next, from P1 to P A The distance to the first thickness T of the oxide film A (nm). Also, P1 to P B The distance to the second thickness T of the oxide film B (nm). Also, P A From P B The distance to the oxide film is calculated as the thickness T (nm).
[0031] In this disclosure, T A T B In other words, it is preferable that the thickness of the oxide film on the coating layer side (first thickness) is relatively large and the thickness of the oxide film on the base material side (second thickness) is relatively small, based on P1. B T for A Proportion (T A / T B) is, for example, 1.50 or more, may be 1.70 or more, may be 2.00 or more, or may be 2.30 or more. B T for A Proportion (T A / T B ) is not particularly limited in its upper limit.
[0032] Also, T A and T B The difference (T A -T B ) is, for example, 20 nm or more, may be 40 nm or more, may be 60 nm or more, or may be 80 nm or more. A and T B The difference (T A -T B ) is not particularly limited. In addition, in AES, the measurement interval in the depth direction is set to D I As described later, in depth analysis by AES, element concentration measurement on the outermost surface of the measurement target and surface etching by sputtering are repeated. Therefore, the data obtained by depth analysis is not continuous data, but discrete data measured for each surface etching. The measurement interval calculated from the sputtering rate is D1 (nm). (T A -T B )≦D I In the case of (T A -T B )>D I In the case of (T), the oxygen distribution is asymmetric with respect to the peak of the oxygen concentration, and more oxygen is diffused to the coating layer side than to the base material side. A -T B ) but D I Larger is better. D I for (T A -T B ) is, for example, 1.1 or more, may be 1.5 or more, or may be 2.0 or more.
[0033] Also, C against TMAX The ratio of (C MAX / T) is preferably small. MAX The smaller the value of / T, the more oxygen diffusion has progressed. MAX / T is, for example, 0.035 or less, may be 0.030 or less, or may be 0.025 or less.
[0034] In the present disclosure, it is preferable that one of (i) to (iii) is satisfied, and two or all of (i) to (iii) may be satisfied. (i)(T A / T B ) ≧ 1.50 (ii) (T A -T B )>D I (iii) C MAX / T≦0.035 The preferred ranges for (i) to (iii) are as described above.
[0035] 1. Base material The base material in the present disclosure contains Ti and Cr, and contains a BCC structure as a metastable phase. The fact that the BCC structure corresponds to a metastable phase is judged by the fact that the BCC structure transforms into a Laves structure, which is a stable phase, when the base material is heated to a melting point. Note that TiCr-based hydrogen storage alloys having a Laves structure can hardly store hydrogen in a pressure range (for example, 0.1 MPa to 0.0001 MPa) that is mainly used in alkaline storage batteries. Also, as shown in FIG. 2, for example, in the ternary diagram of Ti, Cr, and V, in a region where the proportion of V is high, the BCC structure is generated as a stable phase. In this region, the BCC structure is maintained even when the base material is heated to a melting point. On the other hand, in a region where the proportion of V is low, the BCC structure cannot exist as a stable phase and is generated as a metastable phase. In the present disclosure, even when the proportion of expensive V is low or when expensive V is not included, the negative electrode active material has good capacity characteristics while maintaining the BCC structure as a metastable phase.
[0036] The base material is usually a hydrogen storage alloy containing Ti and Cr. The base material preferably contains Ti and Cr as the main components. "Mainly composed of Ti and Cr" means that the total ratio of Ti and Cr is the highest among all metals constituting the base material. The total ratio of Ti and Cr to all metals constituting the base material is, for example, 50 at% or more, may be 70 at% or more, may be 90 at% or more, or may be 95 at% or more. The composition of the base material is determined, for example, by dissolving the base material in acid and measuring it by inductively coupled plasma optical emission spectroscopy (ICP-OES).
[0037] The ratio of Ti and Cr in the base material is not particularly limited as long as the BCC structure can be maintained as a metastable phase. The ratio of Ti to the total of Ti and Cr (Ti / (Ti+Cr)) is, for example, 30 at% or more, and may be 40 at% or more. On the other hand, the ratio of Ti to the total of Ti and Cr (Ti / (Ti+Cr)) is, for example, 70 at% or less, and may be 60 at% or less.
[0038] The base material may contain only Ti and Cr as metals, or may further contain other metals (metals other than Ti and Cr). Examples of other metals include V (vanadium). The base material may contain V, or may not contain V. In the former case, the proportion of V in the base material is preferably a proportion that allows the BCC structure to be maintained as a metastable phase, not as a stable phase. This is because, even when the proportion of expensive V is small, it is possible to obtain a negative electrode active material having good capacity characteristics while maintaining the BCC structure. The proportion of V in the base material is, for example, 25 at% or less, may be 15 at% or less, or may be less than 10 at%. In addition, the base material may contain Mo (molybdenum) as another metal. The proportion of Mo in the base material is, for example, 20 at% or less, may be 15 at% or less.
[0039] The base material contains the BCC structure as a metastable phase. The definition of the metastable phase is as described above. The BCC structure refers to a body-centered cubic lattice structure. A crystal phase having a BCC structure is called a BCC phase. The base material preferably contains the BCC phase as a main phase. "Containing the BCC phase as a main phase" means that the proportion of the BCC phase in the base material is the highest among all the crystal phases constituting the base material. The proportion of the BCC phase in all the crystal phases constituting the base material is, for example, 50% by weight or more, may be 70% by weight or more, or may be 90% by weight or more. The proportion of the BCC phase in the base material can be determined, for example, by a quantitative analysis method using X-ray diffraction (for example, a quantitative method using an R value, the Rietveld method). The base material may contain only the BCC phase as a crystal phase, or may contain other crystal phases in addition to the BCC phase.
[0040] The shape of the base material may be, for example, particulate. The average particle size of the base material (D 50 ) is, for example, 1 μm or more and 500 μm or less.
[0041] 2. Coating layer The coating layer in the present disclosure covers the base material and contains a catalytic metal and an oxygen affinity metal having an oxygen affinity equal to or greater than that of Ti.
[0042] The catalytic metal is a metal constituting a catalyst that promotes at least one of the hydrogen absorption reaction and the hydrogen release reaction. Examples of the catalytic metal include Group 10 elements such as Ni, Pd, and Pt. The coating layer may contain one type of catalytic metal, or may contain two or more types of catalytic metals. The coating layer may contain Ni as a main component as a catalytic metal. The ratio of Ni to all catalytic metals contained in the coating layer is, for example, 50 at% or more, 70 at% or more, or 90 at% or more. The coating layer may contain Pd as a main component as a catalytic metal. The ratio of Pd to all catalytic metals contained in the coating layer is, for example, 50 at% or more, 70 at% or more, or 90 at% or more.
[0043] The oxygen affinity metal in the present disclosure is Ti or a metal having a higher oxygen affinity than Ti. When the metal having a higher oxygen affinity than Ti is Me, Me is usually a metal located below Ti at a temperature of 298K in an Ellingham diagram. Examples of Me include rare earth elements. Rare earth elements include Sc, Y, and 15 elements (La to Lu) belonging to the lanthanoids. Examples of Me include Mg, Al, and Ca. The coating layer may contain one type of oxygen affinity metal, or may contain two or more types of oxygen affinity metals.
[0044] The proportions (at%) of the catalytic metal and the oxygen affinity metal in the coating layer are not particularly limited. The proportion (at%) of the catalytic metal may be smaller than, the same as, or larger than the proportion (at%) of the oxygen affinity metal. The composition of the coating layer may be, for example, Ti x Ni (1≦x≦2), LaNi5. The composition of the coating layer is preferably a composition that exhibits hydrogen storage capacity. This is because hydrogen diffusion occurs smoothly. The hydrogen storage capacity of the coating layer is, for example, 0.6% by weight or more, and may be 1.0% by weight or more.
[0045] The coating layer covers the base material. The coverage of the coating layer with respect to the base material is, for example, 50% or more, may be 70% or more, or may be 100%. The average thickness of the coating layer is not particularly limited, but may be, for example, 100 nm or more, may be 300 nm or more, or may be 500 nm or more. On the other hand, the average thickness of the coating layer is, for example, 3000 nm or less, may be 2000 nm or less, or may be 1500 nm or less.
[0046] 3.Negative electrode active material The negative electrode active material in the present disclosure has the above-mentioned base material and coating layer. The shape of the negative electrode active material may be, for example, particulate. The average particle diameter (D 50) is, for example, 1 μm or more and 500 μm or less. The negative electrode active material according to the present disclosure is used in an alkaline storage battery.
[0047] B. Alkaline storage battery Fig. 3 is a schematic cross-sectional view illustrating an alkaline storage battery according to the present disclosure. The alkaline storage battery 20 shown in Fig. 3 has a positive electrode active material layer 11 containing Ni(OH)2 as a positive electrode active material, a negative electrode active material layer 12 containing the above-mentioned negative electrode active material (MH), and an electrolyte layer 13 formed between the positive electrode active material layer 11 and the negative electrode active material layer 12 and containing an alkaline solution. The alkaline storage battery 20 shown in Fig. 3 corresponds to a so-called nickel-metal hydride battery (Ni-MH battery), in which the following reaction occurs: Positive electrode: NiOOH+H2O+e - ⇔ Ni(OH)2+OH - Negative electrode: MH+OH - ⇔ M+H2O+e -
[0048] Fig. 4 is a schematic cross-sectional view illustrating an alkaline storage battery according to the present disclosure. In the alkaline storage battery 20 shown in Fig. 4, the positive electrode active material layer 11 is a layer that uses oxygen (O2) as the positive electrode active material. For example, oxygen is supplied from the atmosphere during discharge and released into the atmosphere during charge. The alkaline storage battery 20 shown in Fig. 4 corresponds to a so-called air-metal hydride battery (Air-MH battery), in which the following reaction occurs: Positive electrode: O2+2H2O+4e - ⇔ 4OH - Negative electrode: MH+OH - ⇔ M+H2O+e -
[0049] According to the present disclosure, since the negative electrode active material layer contains the above-mentioned negative electrode active material, an alkaline storage battery having good capacity characteristics is obtained.
[0050] 1.Negative electrode active material layer The negative electrode active material layer contains at least the negative electrode active material described in "A. Negative Electrode Active Material" above. The negative electrode active material layer may further contain at least one of a conductive material and a binder. The addition of a conductive material improves the electronic conductivity of the negative electrode active material layer. Examples of the conductive material include metal powders such as Ni powder, oxides such as cobalt oxide, graphite, and carbon materials such as carbon nanotubes. Examples of the binder include celluloses such as carboxymethyl cellulose (CMC), polyols such as polyvinyl alcohol (PVA), and fluororesins such as polyvinylidene fluoride (PVDF).
[0051] 2.Cathode active material layer The positive electrode active material layer contains at least a positive electrode active material. The positive electrode active material layer may further contain at least one of a conductive material and a binder. Examples of the positive electrode active material include a metal element, an alloy, and a hydroxide. In particular, the positive electrode active material preferably contains Ni element, and more preferably nickel hydroxide. The conductive material and the binder are the same as those described for the negative electrode. In addition, when the positive electrode active material of the positive electrode active material layer is air, it is preferable to contain a catalyst that promotes the electrode reaction. Examples of the catalyst include a precious metal such as Pt, and a composite oxide such as a perovskite oxide.
[0052] 3. Electrolyte layer The electrolyte layer is formed between the positive electrode and the negative electrode, and contains an alkaline solution as an electrolyte. Examples of solutes in the alkaline solution include metal hydroxides such as potassium hydroxide (KOH) and sodium hydroxide (NaOH). Examples of solvents in the alkaline solution include water. The ratio of water to the entire solvent in the electrolyte is, for example, 50 mol% or more, and may be 70 mol% or more, or may be 90 mol% or more. The concentration of the solute in the alkaline solution is, for example, 3 mol / L or more, and may be 5 mol / L or more. A separator may be disposed between the positive electrode and the negative electrode, and the separator may be impregnated with the alkaline solution.
[0053] 4. Alkaline storage batteries The alkaline storage battery in the present disclosure contains at least the above-mentioned negative electrode active material layer, positive electrode active material layer, and electrolyte layer. The alkaline storage battery may have a positive electrode current collector that collects electrons from the positive electrode active material layer. Examples of the material for the positive electrode current collector include stainless steel, nickel, iron, titanium, and the like. Examples of the shape of the positive electrode current collector include foil, mesh, and porous. The alkaline storage battery may also have a negative electrode current collector that collects electrons from the negative electrode active material layer. Examples of the material for the negative electrode current collector include copper, stainless steel, nickel, iron, titanium, and carbon. Examples of the shape of the negative electrode current collector include foil, mesh, and porous. In addition, a known exterior body can be used as the exterior body of the alkaline storage battery. The use of the alkaline storage battery is not particularly limited, and it can be used for any purpose.
[0054] C. Method for manufacturing negative electrode active material FIG. 5 is a flow diagram illustrating a method for producing a negative electrode active material according to the present disclosure. In the production method shown in FIG. 5, first, a predetermined base material is coated with a predetermined coating layer to form a precursor (precursor formation step). The base material in the precursor contains Ti and Cr, and contains a BCC structure as a metastable phase. The coating layer in the precursor contains a catalytic metal and an oxygen affinity metal having an oxygen affinity equal to or higher than that of Ti. Next, the precursor is heat-treated under predetermined conditions (heat treatment step). Specifically, the precursor is heat-treated so as to diffuse oxygen contained in an oxide film present at the interface between the coating layer and the base material while maintaining the BCC structure in the base material.
[0055] According to the present disclosure, a precursor is subjected to a heat treatment so as to diffuse oxygen contained in an oxide film present at the interface between a coating layer and a base material while maintaining the BCC structure of the base material, thereby obtaining a negative electrode active material having good capacity characteristics.
[0056] 1. Precursor formation process The precursor formation process in the present disclosure is a process in which a base material containing Ti and Cr and having a BCC structure as a metastable phase is coated with a coating layer containing a catalytic metal and an oxygen affinity metal having an oxygen affinity equal to or greater than that of Ti to form a precursor.
[0057] Details of the base material and the coating layer are the same as those described in "A. Negative electrode active material" above. In addition, as a method for synthesizing the base material, for example, a method of quenching a molten metal containing the constituent materials of the base material can be mentioned. As such a method, for example, a gas atomizing method and a roll quenching method can be mentioned. In addition, as a method for coating the base material with a coating layer, for example, a PVD method such as a sputtering method or a vacuum deposition method; a CVD method such as a thermal CVD method can be mentioned.
[0058] 2.Heat treatment process The heat treatment process in the present disclosure is a process of heat treating the precursor so as to diffuse oxygen contained in the oxide film present at the interface between the coating layer and the base material while maintaining the BCC structure of the base material. Since the coating layer contains an oxygen affinity metal, the oxygen contained in the oxide film present on the surface of the base material diffuses more toward the coating layer side than toward the base material side by the heat treatment. In addition, since the base material after the heat treatment maintains the BCC structure, good capacity characteristics are obtained.
[0059] The heat treatment temperature is not particularly limited, but may be, for example, 300°C or higher, 400°C or higher, or 450°C or higher. If the heat treatment temperature is low, the oxygen contained in the oxide film is less likely to diffuse. On the other hand, the heat treatment temperature is, for example, 600°C or lower. If the heat treatment temperature is high, the BCC structure in the base material is easily transformed into the Laves structure, which is a stable phase.
[0060] The heat treatment time is not particularly limited, but is, for example, 30 minutes or more, may be 1 hour or more, or may be 1.5 hours or more. On the other hand, the heat treatment time is, for example, 10 hours or less. In addition, the atmosphere during the heat treatment is not particularly limited, but in order to avoid oxidation, a low-oxygen atmosphere such as a vacuum or an inert gas atmosphere is preferable. In addition, in the present disclosure, it is preferable to adjust the heat treatment conditions so that the negative electrode active material described in the above "A. Negative electrode active material" is obtained.
[0061] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0062] [Comparative Example 1] Using the gas atomization method, Ti 45 Cr 45 Mo 10 A powder of the base material (hydrogen storage alloy) with the composition (at%) was produced. Specifically, a gas atomizer was used to spray high-pressure Ar gas onto a molten TiCrMo alloy, quenching the molten alloy and obtaining a base material containing the BCC structure as a metastable phase. The powder of the base material obtained was classified into particles with a particle size of 38 μm to 100 μm using a 38 μm sieve and a 100 μm sieve.
[0063] The surface of the obtained base material was coated with a catalyst (Ni) and an oxygen affinity metal (Ti) to form a coating layer on the base material. Specifically, the base material was entirely coated with a coating layer by barrel sputtering so that the average thickness of the coating layer was 300 nm. This resulted in a precursor having a base material containing a BCC structure as a metastable phase and a coating layer containing Ni and Ti. The ratio (at%) of Ni and Ti in the coating layer was Ni:Ti=1:1.
[0064] [Example 1] In the same manner as in Comparative Example 1, a precursor was obtained. The obtained precursor was heat-treated under the conditions of vacuum, 500 °C, and 2 hours. As a result, a negative electrode active material having a base material containing a BCC structure as a metastable phase and a coating layer containing Ni and Ti was obtained.
[0065] [Comparative Example 2] In the same manner as in Comparative Example 1, a classified base material was obtained. By coating the surface of the obtained base material with a catalyst (Ni), a coating layer was formed on the base material. Specifically, the entire surface of the base material was coated with the coating layer by barrel sputtering so that the average thickness of the coating layer was 1000 nm. As a result, a precursor having a base material containing a BCC structure as a metastable phase and a coating layer containing Ni was obtained.
[0066] [Comparative Example 3] In the same manner as in Comparative Example 2, a precursor was obtained. The obtained precursor was heat-treated under the conditions of vacuum, 500 °C, and 2 hours. As a result, a negative electrode active material having a base material containing a BCC structure as a metastable phase and a coating layer containing Ni was obtained.
[0067] [Evaluation] (Auger Electron Spectroscopy) Elemental analysis by Auger spectroscopy (AES) was performed on the precursors obtained in Comparative Examples 1 and 2 and the negative electrode active materials obtained in Example 1 and Comparative Example 3. For the measurement, an Auger electron spectrometer (JAMP-9510F) manufactured by JEOL Ltd. was used. The Ar ion etching conditions and analysis conditions are as follows. <Ar Ion Etching Conditions> ·Acceleration voltage: 2 kV ·Filament current: 20 mA ·Etching interval: 30 seconds <Analysis Conditions> ·Acceleration voltage: 10 kV ·Irradiation current: 10 nA ·Beam diameter: 80 nm, ·Mode: High sensitivity mode (M5·MULTI mode) ·Step interval: 1 eV
[0068] In addition, Ar ion etching was performed on a sample in which SiO2 was laminated to a thickness of 100 nm on a Si substrate, and the time it took for the oxygen spectrum intensity to be reduced to half was measured, from which the etching rate (depth etched (SiO2 equivalent value) per Ar ion etching operation) was calculated.
[0069] As representative examples, Fig. 6 shows the results for the precursor (before heat treatment) obtained in Comparative Example 1, and Fig. 7 shows the results for the negative electrode active material (after heat treatment) obtained in Example 1. Note that in Figs. 6 and 7, the atomic concentration of oxygen (O) is shown five times larger for convenience.
[0070] As shown in FIG. 6, the interface was determined as the point where the Ni concentration in the coating layer (the Ni concentration in the coating layer region not containing Cr in the base material) was 1 / 2. Next, the maximum oxygen concentration C MAX The position P1 was specified. The vicinity refers to a region that is 100 nm or less away from the interface. Next, in the region on the coating layer side from P1, MAX The position P of the oxygen concentration curve where A Next, in the region closer to the base material than P1, 1 / 2C MAX The position P of the oxygen concentration curve where B Next, P1 to P A The distance to the first thickness T of the oxide film A Similarly, P1 to P B The distance to the second thickness T of the oxide film B Also, P A From P B The distance from the surface to the oxide film was calculated as the thickness T of the oxide film. A and T B , T=T A +T B The results are shown in Table 1.
[0071] In addition, in depth analysis by AES, element concentration measurement on the outermost surface of the measurement target and surface etching by sputtering are repeated. Therefore, the data obtained by depth analysis is not continuous data, but discrete data measured for each surface etching. The measurement interval (nm) calculated from the sputtering rate is shown in Table 1. The measurement interval is an SiO2 equivalent value.
[0072] As shown in FIG. 7, the oxide film thickness and maximum oxygen concentration were also determined for Example 1 in the same manner as in FIG. 6. Although not shown, the oxide film thickness and maximum oxygen concentration were also determined for Comparative Examples 2 and 3 in the same manner as in FIG. 6. The results are shown in Table 1. Based on the values shown in Table 1, T A / T B , T A -T B and C MAX The results are shown in Table 2.
[0073] [Table 1]
[0074] [Table 2]
[0075] As shown in Tables 1 and 2, in Example 1, compared with Comparative Examples 1 to 3, T A / T B In other words, the oxygen contained in the oxide film on the surface of the base material was diffused more toward the coating layer side than toward the base material side. A -T B is the measurement interval D I The oxygen distribution was generally symmetrical with respect to the peak of the oxygen concentration. A -T B is the measurement interval D IThe oxygen distribution was asymmetrical with respect to the peak of the oxygen concentration, and more oxygen was diffused to the coating layer side than to the base material side. MAX In other words, the heat treatment caused a large amount of oxygen to diffuse from the oxide film on the surface of the base material.
[0076] (Charge / discharge test) Using the precursors obtained in Comparative Examples 1 and 2 and the negative electrode active materials obtained in Example 1 and Comparative Example 3, evaluation cells were fabricated.
[0077] First, the negative electrode was prepared. A precursor or negative electrode active material, Ni as a conductive material, and two types of binders (carboxymethyl cellulose (CMC) and polyvinyl alcohol (PVA)) were added in a weight ratio of (precursor or negative electrode active material):conductive material:CMC:PVA=49:49:1:1, and the mixture was kneaded to prepare a paste-like composition. This paste-like composition was applied to porous nickel, dried at 80°C, and then roll pressed at 490 MPa to obtain a negative electrode.
[0078] Next, the positive electrode was prepared. Nickel hydroxide (Ni(OH)2), conductive cobalt oxide (CoO), and two types of binders (carboxymethyl cellulose (CMC) and polyvinyl alcohol (PVA)) were added in a weight ratio of Ni(OH)2:CoO:CMC:PVA=88:10:1:1, and then kneaded to prepare a paste-like composition. This paste-like composition was applied to porous nickel, then dried at 80°C, and roll pressed at 490 MPa to obtain a positive electrode. The capacity ratio of the negative electrode and positive electrode was adjusted to negative electrode:positive electrode=1:3.
[0079] Next, an electrolyte solution was prepared. Pure water was added to KOH to adjust the KOH concentration to 6 mol / L to obtain an electrolyte solution. After that, the electrolyte solution and a separator (PE / PP nonwoven fabric) were placed in a container, and further, a negative electrode (working electrode), a positive electrode (counter electrode), and a Hg / HgO electrode (reference electrode) were placed to obtain an evaluation cell.
[0080] A charge / discharge test was conducted on the obtained evaluation cell. The charge / discharge test was conducted by constant current charging and discharging in an environment at a temperature of 25°C. Charging was performed at a rate of C / 5 for 10 hours, and discharging was performed at a rate of C / 10 until the working electrode potential reached -0.5V. The results are shown in Table 3.
[0081] [Table 3]
[0082] As shown in Table 3, in Comparative Example 1, almost no discharge capacity was obtained, but in Example 1, a discharge capacity of 330 mAh / g was obtained. This is presumably because the BCC structure in the base material was maintained during the heat treatment, and the oxygen contained in the oxide film present on the surface of the base material diffused more toward the coating layer side than toward the base material side. On the other hand, in Comparative Example 2, no discharge capacity was obtained, and in Comparative Example 3, almost no discharge capacity was obtained. This is presumably because the BCC structure in the base material was maintained during the heat treatment, but the oxygen contained in the oxide film present on the surface of the base material did not diffuse more toward the coating layer side than toward the base material side.
[0083] [Examples 2 to 20] An evaluation cell was obtained in the same manner as in Example 1, except that the composition of the base material, the particle size of the base material, the composition of the coating layer, the thickness of the coating layer, and the heat treatment conditions were changed as shown in Table 4. A charge-discharge test was performed on the obtained evaluation cell in the same manner as above. The results are shown in Table 4.
[0084] [Table 4]
[0085] As shown in Table 4, in Examples 2 to 20, good capacitance characteristics were obtained.
[0086] [Comparative Examples 4 and 5] An evaluation cell was obtained in the same manner as in Comparative Example 3, except that the composition of the base material and the composition of the coating layer were changed as shown in Table 5. The obtained evaluation cell was subjected to a charge-discharge test in the same manner as above. The results are shown in Table 5.
[0087] [Table 5]
[0088] As shown in Table 5, almost no charge capacity was obtained in Comparative Example 4. In Comparative Example 5, a certain level of discharge capacity was obtained by using Pd as a catalyst, but the discharge capacity was smaller than those in the above-mentioned Examples 1 to 20. In this way, it was confirmed that the negative electrode active material in the present disclosure has good capacity characteristics. [Explanation of symbols]
[0089] 1 … Base material 2 … Coat layer 3. Oxide film 10 … Negative electrode active material 11... Positive electrode active material layer 12 … Negative electrode active material layer 13 … Electrolyte layer 20...Alkaline storage battery
Claims
1. A negative electrode active material for use in an alkaline storage battery, comprising: The negative electrode active material is A base material containing Ti and Cr, containing a BCC structure as a metastable phase, and having a V ratio of less than 10 at %; a coating layer that coats the base material and contains a catalytic metal and an oxygen affinity metal having an oxygen affinity equal to or higher than that of Ti; Equipped with an oxide film is present at the interface between the coating layer and the base material; The maximum oxygen concentration C of the oxide film in the vicinity of the interface was determined by Auger electron spectroscopy. MAX (at%) and the C MAX Position P where 1 and MAX Half the value is 1 / 2C MAX And, P 1 In the region on the coat layer side, MAX The position where A At position P 1 In the region closer to the base material than MAX The position where B And, P 1 From the above P A The distance to the first thickness T of the oxide film A (nm), and P 1 From the above P B The distance to the second thickness T of the oxide film B (nm), and P A From the above P B The distance from the oxide film to the surface of the oxide layer is defined as the thickness T (nm), and the measurement interval in the depth direction is defined as D I (nm), The negative electrode active material is (i) Said T B The above T A The proportion of (T A / T B ) is 1.50 or more; (ii) Said T A and the T B The difference between (T A -T B ) is the D I Greater than (iii) the C relative to the T MAX The ratio of (C MAX / T) is 0.035 or less; The negative electrode active material satisfies at least one of the above.
2. The negative electrode active material according to claim 1 , wherein the negative electrode active material satisfies the condition (i).
3. The negative electrode active material according to claim 1 or 2, which satisfies the condition (ii).
4. The negative electrode active material according to claim 1 , wherein the negative electrode active material satisfies the condition (iii).
5. 5. The negative electrode active material according to claim 1, wherein the coating layer contains at least one of Ni, Pd, and Pt as the catalytic metal.
6. The negative electrode active material according to claim 1 , wherein the coating layer contains Ti as the oxygen affinity metal.
7. The negative electrode active material according to claim 1 , wherein the coating layer contains La as the oxygen affinity metal.
8. The negative electrode active material according to claim 1 , wherein the base material contains the V.
9. The negative electrode active material according to claim 1 , wherein the base material does not contain V.
10. An alkaline storage battery having a positive electrode active material layer, a negative electrode active material layer, and an electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, An alkaline storage battery, wherein the negative electrode active material layer contains the negative electrode active material according to any one of claims 1 to 9.
11. A method for producing a negative electrode active material for use in an alkaline storage battery, comprising the steps of: a precursor forming step of coating a base material containing Ti and Cr, containing a BCC structure as a metastable phase, and having a V ratio of less than 10 at %, with a coating layer containing a catalytic metal and an oxygen affinity metal having an oxygen affinity equal to or higher than that of Ti to form a precursor; a heat treatment step of performing a heat treatment on the precursor so as to diffuse oxygen contained in an oxide film present at the interface between the coating layer and the base material while maintaining the BCC structure in the base material; The method for producing a negative electrode active material comprising the steps of:
12. The method for producing a negative electrode active material according to claim 11, wherein the heat treatment temperature in the heat treatment step is 300° C. or more and 600° C. or less.
13. The method for producing a negative electrode active material according to claim 11 or 12, wherein a heat treatment time in the heat treatment step is 30 minutes or more and 10 hours or less.
Citation Information
Patent Citations
Hydrogen storage alloy electrode and manufacture thereof
JP1997063569A
Hydrogen storage alloy electrode and manufacture thereof
JP1997312157A
Method of activating hydrogen storage alloy for ni / Mh secondary battery
JP2001196056A
Hydrogen storage alloy electrode and its manufacturing method
JP2002141061A
Hydrogen storage alloy for electrode, method for manufacturing hydrogen storage alloy for electrode, and electrode of hydrogen storage alloy
JP2003013104A