Thermosetting resin composition and semiconductor device
A thermosetting resin composition with specific components is used to enhance the connection reliability between copper wires and bonding pads in semiconductor devices by protecting against corrosion, addressing the corrosion issues caused by moisture and chlorine elements in the sealing resin.
Patent Information
- Application Number
- JP2022566942
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-29
- Filing Date
- 2021-11-30
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-11-30
AI Technical Summary
The use of copper wires for bonding in semiconductor devices leads to corrosion issues at the bonding interface due to moisture and chlorine elements in the sealing resin, resulting in decreased bond strength and increased electrical resistance, which existing technologies have struggled to address effectively.
A thermosetting resin composition is applied to cover at least a portion of the bonding wire and bonding interface, comprising a thermosetting resin, a curing agent, and an inorganic filler, with specific ratios and components to enhance connection reliability and protect against corrosion.
The resin composition improves the connection reliability between the bonding pad and wire by preventing corrosion and maintaining electrical integrity, leading to a highly reliable semiconductor device.
Smart Images

Figure 0007559836000003 
Figure 0007559836000004 
Figure 0007559836000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin composition and a semiconductor device manufactured using the same. More specifically, the present invention relates to a thermosetting resin composition used to protect a joint between an electrode pad and a bonding wire in a semiconductor device in which an electrode pad of a semiconductor chip is electrically connected by a bonding wire and the semiconductor chip and the bonding wire are sealed with a cured product of the thermosetting resin composition. [Background technology]
[0002] Semiconductor devices are usually distributed with a semiconductor chip sealed (packaged) in resin together with bonding wires. Inside the package, the electrode pads of the semiconductor chip and electrode leads partially exposed from the resin package are electrically connected by bonding wires. Therefore, electrical connection between the semiconductor chip and the mounting substrate is achieved by connecting the electrode leads as external terminals to the wiring of the mounting substrate.
[0003] Conventionally, gold wires have been mainly used as bonding wires connecting electrode pads and electrode leads, but in recent years, the use of copper wires, which are cheaper than gold wires, has been considered in order to reduce the use of expensive gold. When copper wires are used as wires to connect to aluminum electrode pads, which are the mainstream in recent years, if moisture penetrates into the bonding interface between the electrode pad and the bonding wire, corrosion of aluminum is likely to progress near the bonding interface. This may cause an electrical open between the pad and the wire. In addition, the chlorine element in the sealing resin and the intermetallic compound formed at the bonding interface between the electrode pad and the bonding wire may cause a corrosion reaction, which may increase the electrical resistance of the joint and reduce the bonding strength.
[0004] As a technique for improving the connection reliability between a pad and a wire, for example, Patent Document 1 describes a method for improving the long-term reliability of the joint between a bonding wire and an electrode by optimizing the alloying additive elements of the bonding wire.
[0005] However, in the above Patent Document 1, it was difficult to obtain sufficient connection reliability between the bonding wire and the electrode. The present inventors have studied a technique for coating the bonding wire and the bonding pad with a wire coating material in order to improve the connection reliability between the bonding wire and the bonding pad. When coating with a wire coating material, it has been found that an important technical issue is to optimize the composition of the resin composition used as the wire coating material to improve the connection reliability between the bonding wire and the bonding pad while maintaining good application properties. Furthermore, the present inventors have found that peeling of the wire coating material, etc. may occur due to thermal history. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2003-133362 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to provide a thermosetting resin composition for covering at least a portion of a bonding wire and a bonding interface, which can improve the connection reliability between a bonding pad and a bonding wire, and a semiconductor having excellent electrical reliability obtained using this thermosetting resin composition. [Means for solving the problem]
[0008] As a result of careful investigation, the inventors have discovered that the above-mentioned problems can be solved in a semiconductor device comprising a mounting plate, a semiconductor chip mounted on the mounting plate and having a bonding pad, bonding wires joined to the bonding pads and connecting the semiconductor chip to the mounting plate, and a resin sealing body that seals the semiconductor chip, the mounting surface of the mounting plate for the semiconductor chip, and the bonding wires, by covering at least a portion of the bonding wire and the bonding layer with resin, and have completed the present invention.
[0010] According to the present invention, A mounting plate; a semiconductor chip mounted on the mounting plate and having bonding pads; a bonding wire bonded to the bonding pad for connecting the semiconductor chip and the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the semiconductor chip mounting surface of the mounting plate, and the bonding wires, A thermosetting resin composition used to cover at least a portion of the bonding wire and the bonding pad, The thermosetting resin composition includes a thermosetting resin, a curing agent, an inorganic filler, and a solvent, the thermosetting resin includes a novolac phenolic resin, The curing agent is Epoxy resin and Contains an alkoxymethyl glycoluril compound, There is provided a thermosetting resin composition, in which the content of the inorganic filler is 40% by mass or more and 85% by mass or less based on the total solid content of the thermosetting resin composition.
[0011] Further, according to the present invention, A mounting plate; a semiconductor chip mounted on the mounting plate and having bonding pads; a bonding wire bonded to the bonding pad for connecting the semiconductor chip and the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the mounting surface of the mounting plate for the semiconductor chip, and the bonding wires; The semiconductor device is provided, wherein the wire coating material is made of a cured product of the above thermosetting resin composition. Effect of the Invention
[0012] According to the present invention, there are provided a thermosetting resin composition capable of improving the connection reliability between a semiconductor chip and a bonding wire, and a highly reliable semiconductor device manufactured using the same. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic cross-sectional view of a semiconductor device according to an embodiment of the present invention; [Diagram 2] 2 is an enlarged cross-sectional view of a bonding portion between a semiconductor chip and a bonding wire in the semiconductor device shown in FIG. 1 according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar symbols and their explanations are omitted as appropriate. In addition, all drawings are for explanatory purposes only. The shapes and dimensional ratios of each member in the drawings do not necessarily correspond to actual articles. In this specification, the expression "a to b" in the explanation of a numerical range means "a or more and b or less" unless otherwise specified. For example, "5 to 90% by mass" means "5% by mass or more and 90% by mass or less".
[0015] In a first embodiment, the thermosetting resin composition of the present invention comprises: A mounting plate; a semiconductor chip mounted on the mounting plate and having bonding pads; a bonding wire bonded to the bonding pad for connecting the semiconductor chip and the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the semiconductor chip mounting surface of the mounting plate, and the bonding wires, A thermosetting resin composition used to cover at least a portion of the bonding wire and the bonding pad, The thermosetting resin composition includes a thermosetting resin, a curing agent, and a solvent, The viscosity of the thermosetting resin composition measured with a rotational viscometer is 20 mPa·s or more.
[0016] In a second embodiment, the thermosetting resin composition of the present invention comprises: A mounting plate; a semiconductor chip mounted on the mounting plate and having bonding pads; a bonding wire bonded to the bonding pad for connecting the semiconductor chip and the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the semiconductor chip mounting surface of the mounting plate, and the bonding wires, A thermosetting resin composition used to cover at least a portion of the bonding wire and the bonding pad, The thermosetting resin composition includes a thermosetting resin, an inorganic filler, and a solvent, The content of the inorganic filler is 40% by mass or more and 85% by mass or less based on the total solid content of the thermosetting resin composition.
[0017] Moreover, the semiconductor device according to this embodiment has A mounting plate; a semiconductor chip having bonding pads mounted on the mounting plate; a bonding wire bonded to the bonding pad for connecting the semiconductor chip and the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the mounting surface of the mounting plate on which the semiconductor chip is mounted, and the bonding wires; a wire coating material that coats a connection portion between the bonding wire and the bonding pad; The wire coating material is made of a cured product of the above-mentioned thermosetting resin composition.
[0018] The wire coating material in this embodiment corresponds to the thermosetting resin composition of the present invention, and the semiconductor device 10 in this embodiment corresponds to the semiconductor device of the present invention.
[0019] (Semiconductor device 10) Fig. 1 is a cross-sectional view of a semiconductor device 10 according to this embodiment. As shown in Fig. 1, the semiconductor device 10 includes a semiconductor chip 1, a circuit board 2, connection pads 8, a resin sealant (sealing resin) 4, external electrode terminals 6, and bonding wires 7. In the semiconductor device 10, the semiconductor chip 1 is fixed onto the connection pads 8 on the circuit board 2 via a die attach material 9. The electrode pads (not shown) of the semiconductor chip 1 and the circuit board 2 are connected by the bonding wires 7. The surface of the circuit board 2 on which the semiconductor chip 1 is mounted is sealed by the resin sealant 4. The electrode pads on the circuit board 2 are internally joined to the external electrode terminals 6 on the non-sealed surface side of the circuit board 2.
[0020] (Semiconductor chip 1) The type of the semiconductor chip 1 is not particularly limited, and any type of semiconductor chip can be used. The semiconductor chip 1 is mounted on the circuit board 2 via a die attach layer 9 so that the back surface of the semiconductor chip 1 contacts the upper surface of the connection pad 8. On the upper surface of the semiconductor chip 1, a bonding wire 7 is electrically connected to the semiconductor chip 1 via a bonding layer (bonding pad) 17 using a wire bonding method, and the connection portion between the semiconductor chip 1 and the bonding wire 7 is covered with a resin coating material (wire coating material) 5. Here, FIG. 2 shows an enlarged view of the connection portion between the semiconductor chip 1 and the bonding wire 7 in FIG. 1. As shown in FIG. 2, the semiconductor chip 1 has a barrier layer 18 and a bonding layer 17 on its upper surface, and is electrically connected to one end of the bonding wire 7 via the bonding layer 17, and the connection portion between the semiconductor chip 1 and the bonding wire 7 is covered with a wire coating material 5 made of a cured product of the thermosetting resin composition of this embodiment described in detail below.
[0021] According to this configuration, the bonding layer 17 and a part of the bonding wire 7 are covered with the wire coating material 5 made of the cured product of the thermosetting resin composition of this embodiment. Therefore, even if moisture penetrates into the resin package, the moisture can be blocked by the wire coating material 5, so that the bonding interface (bonding layer 17) between the semiconductor chip 1 and the bonding wire 7 can be prevented from coming into contact with moisture and corroding. In addition, the corrosion of the bonding interface (bonding layer 17) between the semiconductor chip 1 and the bonding wire 7 due to moisture and chlorine ions contained in the resin sealing body 4 can be suppressed. Furthermore, even if corrosion occurs, its spread can be suppressed. In addition, the bonding wire 7 and the bonding layer 19 can be prevented from being oxidized by the oxygen contained in the resin sealing body 4. As a result, the connection reliability between the pads and the wires can be improved, and a semiconductor device with excellent reliability can be obtained.
[0022] (Circuit board 2) The circuit board 2 included in the semiconductor device 10 of this embodiment is used as a mounting board for the semiconductor chip 1. The circuit board 2 is provided with external electrode terminals 6 on its back surface. The circuit board 2 is also provided with wiring on the top surface and inside of the circuit board 2. The circuit board 2 is further provided with connection pads 8 on the top surface of the circuit board 2 via the wiring. As shown in FIG. 2, it is not necessary for the entire back surface of the connection pads 8 to be connected to the wiring, and it is sufficient that only a part of the connection pads 8 is connected to the wiring, but the entire back surface of the connection pads 8 may be connected to the wiring. The circuit board 2 is also connected to the semiconductor chip 1 via the connection pads 8.
[0023] The type of circuit board 2 used in this embodiment is not particularly limited, and a circuit board having copper wiring patterned on an organic insulating base material such as glass epoxy material, BT (bismaleimide triazine), resin, polyimide, etc. can be used.
[0024] (Bonding wire 7) The bonding wire 7 is used to electrically connect the semiconductor chip 1 and the circuit board 2. Specifically, one end of the bonding wire 7 is electrically connected to the upper surface of the semiconductor chip 1 via a bonding layer 19, and the other end of the bonding wire 7 is electrically connected to the upper surface of the circuit board 2 via a wiring 11. A wire bonding method is used for this electrical connection. Note that the type of wire bonding used in this embodiment is not particularly limited, and any type of wire bonding such as ball bonding and stitch bonding may be used.
[0025] The bonding wire 7 used in this embodiment may be made of any one of aluminum, silver, and copper as a conductive material. The bonding wire 7 may be coated with a metal in advance.
[0026] (External electrode terminal 6) The external electrode terminals 6 are spherical and provided on the back side (non-sealed surface side) of the circuit board 2. One of the external electrode terminals 6 is connected to wiring (not shown), and thus power for driving the semiconductor chip 1 is supplied from the external electrode terminals 6 to the semiconductor chip 1 via the wiring and bonding wires 7. As the external electrode terminals 6, spherical terminals using solder balls, land-shaped terminals using gold, or the like are used.
[0027] (8 connection pads) The connection pads 8 are connected to the upper surface of the circuit board 2 via wiring. In general, when the semiconductor chip 1 and the circuit board 2 are electrically connected using a wire bonding method, it is desirable that the connection pads 8 on which the semiconductor chip 1 is mounted be disposed on the periphery of the semiconductor chip 1.
[0028] (Resin sealing body 4) 1, the resin encapsulant (encapsulating resin) 4 is used to encapsulate the semiconductor chip 1 on the circuit board 2, and is formed on the circuit board 2 so as to entirely cover the semiconductor chip 1, the bonding wires 7, the connection pads 8, the joints between the semiconductor chip 1 and the bonding wires 7, the joints between the bonding wires 7 and the circuit board 2, and an insulating layer (not shown) that covers the wiring. The resin encapsulant 4 is generally formed by a transfer molding method or a compression molding method in which a press and a mold are used to apply pressure to mold the resin, but the present embodiment is not limited to this, and any type of forming method may be used.
[0029] The resin encapsulant 4 is made of a material commonly used in the relevant field, and can be produced using, for example, an encapsulating resin composition containing an epoxy resin, a curing agent, a curing accelerator, and an inorganic filler.
[0030] Examples of epoxy resins to be blended in the encapsulating resin composition for producing the resin encapsulating body 4 include crystalline epoxy resins such as biphenyl-type epoxy resins, bisphenol-type epoxy resins, and stilbene-type epoxy resins; novolac-type epoxy resins such as phenol novolac-type epoxy resins and cresol novolac-type epoxy resins; polyfunctional epoxy resins such as triphenolmethane-type epoxy resins and alkyl-modified triphenolmethane-type epoxy resins; aralkyl-type epoxy resins such as phenol aralkyl-type epoxy resins having a phenylene skeleton and phenol aralkyl-type epoxy resins having a biphenylene skeleton; naphthol-type epoxy resins such as dihydroxynaphthalene-type epoxy resins and epoxy resins obtained by glycidyl etherifying a dimer of dihydroxynaphthalene; triazine nucleus-containing epoxy resins such as triglycidyl isocyanurate and monoallyl diglycidyl isocyanurate; and bridged cyclic hydrocarbon compound-modified phenol-type epoxy resins such as dicyclopentadiene-modified phenol-type epoxy resins. These may be used alone or in combination of two or more.
[0031] The lower limit of the total epoxy resin content is not particularly limited, but is preferably 3% by mass or more, and more preferably 5% by mass or more, based on the total encapsulating resin composition. When the total epoxy resin content is within the above range, there is little risk of wire breakage due to increased viscosity. In addition, the upper limit of the total epoxy resin content is not particularly limited, but is preferably 15% by mass or less, and more preferably 13% by mass or less, based on the total epoxy resin composition. When the upper limit of the total epoxy resin content is within the above range, there is little risk of a decrease in moisture resistance reliability due to an increase in water absorption.
[0032] As the curing agent to be mixed in the encapsulating resin composition for producing the resin encapsulated body 4, for example, any one of a polyaddition type curing agent, a catalyst type curing agent, and a condensation type curing agent can be used.
[0033] Examples of the polyaddition type curing agent include aliphatic polyamines such as diethylenetriamine (DETA), triethylenetetramine (TETA), and metaxylylenediamine (MXDA), aromatic polyamines such as diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS), as well as polyamine compounds including dicyandiamide (DICY) and organic acid dihydralazide; alicyclic acid anhydrides such as hexahydrophthalic anhydride (HHPA), methyltetrahydrophthalic anhydride (MTHPA), and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic acid (BTDA); polyphenol compounds such as novolac-type phenolic resins and phenol polymers; polymercaptan compounds such as polysulfides, thioesters, and thioethers; isocyanate compounds such as isocyanate prepolymers and blocked isocyanates; and organic acids such as carboxylic acid-containing polyester resins.
[0034] Examples of catalyst-type curing agents include tertiary amine compounds such as benzyldimethylamine (BDMA) and 2,4,6-trisdimethylaminomethylphenol (DMP-30); imidazole compounds such as 2-methylimidazole and 2-ethyl-4-methylimidazole (EMI24); and Lewis acids such as BF3 complexes.
[0035] Examples of the condensation type curing agent include phenolic resin-based curing agents such as novolac type phenolic resins and resol type phenolic resins; urea resins such as methylol group-containing urea resins; and melamine resins such as methylol group-containing melamine resins.
[0036] Among these, phenolic resin-based curing agents are preferred from the viewpoint of the balance of flame resistance, moisture resistance, electrical properties, curability, storage stability, etc. Examples of phenolic resin-based curing agents include novolac-type resins such as phenol novolac resins and cresol novolac resins; multifunctional phenolic resins such as triphenolmethane-type phenolic resins; modified phenolic resins such as terpene-modified phenolic resins and dicyclopentadiene-modified phenolic resins; aralkyl-type resins such as phenol aralkyl resins having a phenylene skeleton and / or biphenylene skeleton, and naphthol aralkyl resins having a phenylene skeleton and / or biphenylene skeleton; and bisphenol compounds such as bisphenol A and bisphenol F, which may be used alone or in combination of two or more. From the viewpoint of further improving high-temperature storage properties and high-temperature operating properties, multifunctional phenolic resins such as triphenolmethane-type phenolic resins are preferred, and triphenolmethane-type phenolic resins are particularly preferred.
[0037] The lower limit of the total blending ratio of the curing agent is not particularly limited, but is preferably 0.8% by mass or more, and more preferably 1.5% by mass or more, based on the total encapsulating resin composition. If the lower limit of the blending ratio is within the above range, sufficient fluidity can be obtained. In addition, the upper limit of the total blending ratio of the curing agent is not particularly limited, but is preferably 10% by mass or less, and more preferably 8% by mass or less, based on the total encapsulating resin composition. If the upper limit of the blending ratio is within the above range, there is little risk of causing a decrease in moisture resistance reliability due to an increase in water absorption rate.
[0038] In addition, when a phenolic resin-based curing agent is used as the curing agent, the compounding ratio of the epoxy resin to the phenolic resin-based curing agent is preferably such that the equivalent ratio (EP) / (OH) of the number of epoxy groups (EP) in the total epoxy resin to the number of phenolic hydroxyl groups (OH) in the total phenolic resin-based curing agent is 0.8 or more and 1.3 or less. When the equivalent ratio is within this range, there is little risk of causing a decrease in the curability of the epoxy resin composition for semiconductor encapsulation or a decrease in the physical properties of the cured resin.
[0039] As the inorganic filler to be blended in the encapsulating resin composition for producing the resin encapsulant 4, those generally used in epoxy resin compositions for semiconductor encapsulation can be used, such as fused silica, crystalline silica, talc, alumina, titanium white, silicon nitride, etc. The most preferably used is fused silica. These inorganic fillers may be used alone or in combination. These inorganic fillers may be surface-treated with a coupling agent. The shape of the filler is preferably as spherical as possible and have a broad particle size distribution in order to improve flowability.
[0040] The content of the inorganic filler is not particularly limited, but the lower limit of the content of the inorganic filler is preferably 82% by mass or more, more preferably 85% by mass or more, based on the entire epoxy resin composition. If the content is within the range not below the lower limit, low moisture absorption and low thermal expansion are obtained, so there is little risk of insufficient moisture resistance reliability. In addition, the upper limit of the content of the inorganic filler is preferably 92% by mass or less, more preferably 89% by mass or less, based on the entire epoxy resin composition. If the content is within the range not exceeding the upper limit, there is little risk of poor filling during molding due to reduced fluidity, or wire flow in a semiconductor device due to high viscosity.
[0041] A curing accelerator may be further blended into the encapsulating resin composition for producing the resin encapsulation body 4. The curing accelerator may be any accelerator that accelerates the crosslinking reaction between the epoxy group of the epoxy resin and the functional group of the curing agent (e.g., the phenolic hydroxyl group of a phenolic resin-based curing agent), and may be any accelerator that is generally used in epoxy resin compositions. Examples of the accelerator include diazabicycloalkenes such as 1,8-diazabicyclo(5,4,0)undecene-7 and derivatives thereof; organic phosphines such as triphenylphosphine and methyldiphenylphosphine; imidazole compounds such as 2-methylimidazole; tetra-substituted phosphonium tetra-substituted borates such as tetraphenylphosphonium tetraphenylborate; and adducts of phosphine compounds and quinone compounds, and the like. These may be used alone or in combination of two or more.
[0042] The lower limit of the blending ratio of the curing accelerator is not particularly limited, but is preferably 0.05% by mass or more, and more preferably 0.1% by mass or more, based on the entire encapsulating resin composition. When the lower limit of the blending ratio of the curing accelerator is within the above range, there is little risk of causing a decrease in curability. In addition, the upper limit of the blending ratio of the curing accelerator is not particularly limited, but is preferably 1% by mass or less, and more preferably 0.5% by mass or less, based on the entire encapsulating resin composition. When the upper limit of the blending ratio of the curing accelerator is within the above range, there is little risk of causing a decrease in fluidity.
[0043] (Wire Coating Material 5) The wire coating material 5 is used to coat the bonded portion between the semiconductor chip 1 and the bonding wire 7. The wire coating material 5 of the present invention will be specifically described below.
[0044] [First embodiment] In the first embodiment, the wire coating material 5 is made from a cured product of a thermosetting resin composition containing a thermosetting resin, a curing agent, and a solvent. Hereinafter, components blended in the thermosetting resin composition for producing the wire coating material 5 (hereinafter referred to as "thermosetting resin composition for wire coating material" or "thermosetting resin composition") will be described.
[0045] <Thermosetting resin> As the thermosetting resin to be blended in the thermosetting resin composition for wire coating material of this embodiment, novolac type phenolic resins such as phenol novolac resin, cresol novolac resin, bisphenol novolac resin, phenol-biphenyl novolac resin, biphenyl aralkyl type phenolic resin, allylated novolac type phenolic resin, and xylylene novolac type phenolic resin; reaction products of phenolic compounds such as novolac type phenolic resin, resol type phenolic resin, and cresol novolac resin with aldehyde compounds; reaction products of phenolic compounds such as phenol aralkyl resin with dimethanol compounds; hydroxystyrene resin; polyamide resin; polybenzoxazole resin; polyimide resin; and cyclic olefin resin can be used. Among them, from the viewpoint of the heat resistance of the obtained thermosetting resin composition for wire coating material, it is preferable to use phenol novolac resin, and in particular, it is preferable to use phenol-biphenyl novolac resin.
[0046] The thermosetting resin is blended in an amount of, for example, 10% by mass or more and 95% by mass or less, preferably 20% by mass or more and 90% by mass or less, and more preferably 30% by mass or more and 85% by mass or less, based on the total solid content of the thermosetting resin composition.
[0047] <Hardening agent> As the curing agent to be blended in the thermosetting resin composition for wire coating material of this embodiment, a compound having a group capable of reacting with the thermosetting resin by heat is used. Examples of the hardener include compounds having a methylol group, such as 1,2-benzenedimethanol, 1,3-benzenedimethanol, 1,4-benzenedimethanol (paraxylene glycol), 1,3,5-benzenetrimethanol, 4,4-biphenyldimethanol, 2,6-pyridinedimethanol, 2,6-bis(hydroxymethyl)-p-cresol, and 4,4'-methylenebis(2,6-dialkoxymethylphenol); phenols such as phloroglucide; compounds having an alkoxymethyl group, such as 1,4-bis(methoxymethyl)benzene, 1,3-bis(methoxymethyl)benzene, 4,4'-bis(methoxymethyl)biphenyl, 3,4'-bis(methoxymethyl)biphenyl, 3,3'-bis(methoxymethyl)biphenyl, 2,6-methylnaphthalenedicarboxylate, and 4,4'-methylenebis(2,6-dimethoxymethylphenol); methylolmelamine compounds, such as hexamethylolmelamine and hexabutanolmelamine; alkylated urea resins; cyano compounds such as dicyanoaniline, dicyanophenol, and cyanophenylsulfonic acid; isocyanate compounds such as 1,4-phenylene diisocyanate and 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate; epoxy group-containing compounds such as ethylene glycol diglycidyl ether, bisphenol A diglycidyl ether, triglycidyl isocyanurate, phenoxy type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, naphthalene type epoxy resins, biphenyl type epoxy resins, and phenol novolac resin type epoxy resins; and maleimide compounds such as N,N'-1,3-phenylene dimaleimide and N,N'-methylene dimaleimide.
[0048] The content of the curing agent in the thermosetting resin composition for wire coating material is preferably 0.1 mass % or more, more preferably 1 mass % or more, and even more preferably 3 mass % or more, based on the total solid content of the thermosetting resin composition (excluding inorganic filler), from the viewpoint of improving toughness and chemical resistance during low-temperature curing. From the viewpoint of improving the chemical resistance of the cured film, the content of the curing agent in the thermosetting resin composition is preferably 60 mass % or less, more preferably 50 mass % or less, and even more preferably 40 mass % or less, when the solid content (excluding the inorganic filler) of the thermosetting resin composition is 100 mass %.
[0049] <Solvent> Examples of the solvent that can be used in the thermosetting resin composition for wire coating materials of this embodiment include N-methylpyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, N-ethyl-2-pyrrolidone, tetramethyluric acid, ethyl lactate, N,N-dimethylacetamide, dimethylsulfoxide, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, dipropylene glycol monomethyl ether, methyl lactate, butyl lactate, methyl-1,3-butylene glycol acetate, 1,3-butylene glycol-3-monomethyl ether, methyl pyruvate, ethyl pyruvate, and methyl-3-methoxypropionate. Among these, γ-butyrolactone is preferred from the viewpoint of viscosity control.
[0050] In the first embodiment, the solvent can be used in an appropriate amount to set the viscosity of the thermosetting resin composition in a desired range, for example, in an amount of 10 mass % or more and 50 mass % or less with respect to the entire thermosetting resin composition.
[0051] <Inorganic filler> The thermosetting resin composition for wire coating materials of the present embodiment may contain an inorganic filler. By using an inorganic filler, the fluidity and thixotropy can be adjusted to desired values.
[0052] Examples of inorganic fillers that can be used include silica such as fused silica and crystalline silica, talc, alumina, titanium white, silicon nitride, etc. Among these, it is preferable to use a silica filler from the viewpoint of controlling thixotropy.
[0053] When an inorganic filler is used, the average particle size of the inorganic filler is preferably 5.0 μm or less. In this specification, the average particle size refers to the volume-based median diameter (d50) measured by a laser diffraction method in accordance with ISO-13320 (2009), unless otherwise specified. The average particle size of the inorganic filler is preferably 4.0 μm or less, more preferably 3.0 μm or less. If the average particle size exceeds 5.0 μm, the inorganic filler is likely to settle. Furthermore, coarse particles are likely to be contained, the nozzle of the jet dispenser described below is worn, and the discharged resin composition is likely to scatter outside the desired area. The lower limit of the average particle size is not particularly limited. However, if the average particle size is less than 0.5 μm, the viscosity of the resin composition for wire coating material is likely to increase, so that it is preferably 0.5 μm or more, more preferably 1.0 μm or more. In one embodiment, the average particle size of the inorganic filler used in the present invention is 0.5 μm or more and 5.0 μm or less, preferably 1.0 μm or more and 3.0 μm or less.
[0054] When inorganic filler is used, the content of silica filler in the thermosetting resin composition for wire coating material of the present embodiment is, for example, 0 to 50 mass% based on the total weight of the thermosetting resin composition. If the content is too high, the viscosity of the epoxy resin composition becomes too high, and it may be difficult to apply it with a jet dispenser. If the content of inorganic filler is too high, voids may occur in the cured product.
[0055] <Acid generator> The thermosetting resin composition for wire coating material of the present embodiment may contain an acid generator from the viewpoint of stably forming a cured film. Specifically, the acid generator is a compound that generates an acid by absorbing thermal energy or light energy.
[0056] From the standpoint of improving low temperature curing properties and chemical resistance, the acid generator preferably contains a sulfonium compound or a salt thereof (herein, referred to as "component (e1)"). Component (e1) is specifically a sulfonium salt having a sulfonium ion as a cation part. In this case, the anion part of component (e1) is specifically a boride ion, an antimony ion, a phosphorus ion, or a sulfonate ion such as a trifluoromethanesulfonate ion, and is preferably a boride ion or an antimony ion, more preferably a boride ion, from the viewpoint of improving the reaction rate at low temperatures. These anions may have a substituent.
[0057] The content of component (e1) in the thermosetting resin composition is preferably 0.005% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.02% by mass or more, from the viewpoint of improving the curability at low temperatures, when the solid content (excluding the filler) of the thermosetting resin composition is taken as 100% by mass. Moreover, from the viewpoint of suppressing deterioration in reliability, the content of component (E) in the photosensitive resin composition is preferably 15 mass % or less, more preferably 10 mass % or less, and even more preferably 8 mass % or less, when the total solid content of the photosensitive resin composition is 100 mass %.
[0058] <Other additives> The thermosetting resin composition for wire coating materials of the present embodiment may contain other additives, such as coupling agents, other inorganic fillers, stabilizers, and leveling agents, if desired.
[0059] (Characteristics of thermosetting resin composition for wire coating material) The first thermosetting resin composition for wire coating materials has the above-mentioned composition and has a viscosity of 20 mPa s or more as measured by a rotational viscometer, which improves the flowability and dispensability of the thermosetting resin composition when it is applied, as described below.
[0060] Since the first thermosetting resin composition for wire coating material is intended to be applied by a jet dispenser, it is preferable that the viscosity at the nozzle tip temperature is low so that the thermosetting resin composition can be discharged at high speed from a fine hole with an inner diameter of several hundred μm. In addition, it is preferable that the thermosetting resin composition after discharge has fluidity. For this reason, the viscosity of the thermosetting resin composition at 30°C is 2000 mPa·s or less, preferably 1000 mPa·s or less, more preferably 800 mPa·s or less. In addition, from the viewpoint of handling, the viscosity is preferably 100 mPa·s or more. In the present invention, the viscosity can be determined in accordance with Japanese Industrial Standard JIS K6833. Specifically, the viscosity at 30°C can be determined by reading the value 1 minute after the start of measurement using an E-type viscometer at a rotation speed of 1 rpm. There is no particular limitation on the equipment, rotor, or measurement range used.
[0061] The first thermosetting resin composition for wire coating materials has thixotropy due to the above composition. Here, the thermosetting resin composition having thixotropy means that the thermosetting resin composition has a viscoelastic property in which the viscosity decreases when the thermosetting resin composition is subjected to shear stress (when the shear rate is increased), and the viscosity recovers and the flow is suppressed when the shear stress is released (when the shear rate is decreased).
[0062] The thixotropy of the thermosetting resin composition is determined by the viscosity η of the thermosetting resin composition at a standard shear rate of 10 rpm. 10 (Pa s) and the viscosity η of the thermosetting resin composition at a shear rate of 20 rpm 20 (Pa s) (x1=η 10 / η 20 The thixotropic coefficient, expressed as the coefficient of thixotropy ( If the thixotropic coefficient is in the range of 0.8 to 2.0, when the thermosetting resin composition is applied using a jet dispenser, the thermosetting resin composition flows appropriately while being extruded from the jet dispenser and stops flowing after being extruded, making it difficult for the composition to flow out of a specified area (maintaining the applied shape), and thus enabling the composition to be applied to a specified area.
[0063] Chloride ions (Cl) in thermosetting resin compositions for wire coating materials - ) and sulfide ions (S 2- The concentration of chloride ions (Cl) is 10 ppm or less. Therefore, the bonding wire coated with the wire coating material 5 is not corroded. - ) and sulfide ions (S 2- ) has the property of dissolving and corroding aluminum, silver, and copper. Among aluminum, silver, and copper, aluminum is more likely to dissolve in Cl. - and S 2- The corrosion concentration threshold is 100 ppm. - and S 2- If the concentration is below 100 ppm, neither aluminum, silver, nor copper will be corroded.
[0064] [Second embodiment] In the second embodiment, the wire coating material 5 is made of a cured product of a thermosetting resin composition containing a thermosetting resin, an inorganic filler, and a solvent. Hereinafter, the components blended in the thermosetting resin composition according to the second embodiment will be described.
[0065] <Thermosetting resin> The thermosetting resin used in the thermosetting resin composition of the second embodiment may be the same as that in the first embodiment. The preferred aspects of the thermosetting resin are also the same as those in the first embodiment.
[0066] The thermosetting resin is blended in an amount of, for example, 10% by mass or more and 95% by mass or less, preferably 20% by mass or more and 90% by mass or less, and more preferably 30% by mass or more and 85% by mass or less, based on the total solid content of the thermosetting resin composition (excluding inorganic filler).
[0067] <Inorganic filler> The thermosetting resin composition for wire coating material of the second embodiment contains an inorganic filler as an essential component. The content of the inorganic filler is 40 mass% or more, preferably 50 mass% or more, more preferably 60 mass% or more, and most preferably 65 mass% or more, based on the total solid content of the thermosetting resin composition of this embodiment. By using the above amount, the thermal shrinkage of the obtained wire coating material is suppressed, and therefore peeling between the semiconductor chip 1 and the connection pad 8, the semiconductor chip 1 and the barrier layer 18, or the barrier layer 18 and the bonding layer 19 can be suppressed.
[0068] The content of the inorganic filler is 85% by mass or less, and preferably 80% by mass or less, based on the total solid content of the thermosetting resin composition of this embodiment, which improves the applicability using a jet dispenser or the like and prevents cracks from occurring in the wire coating material.
[0069] Examples of inorganic fillers that can be used include silica such as fused silica and crystalline silica, talc, alumina, titanium white, silicon nitride, and the like. Among them, it is preferable to use silica from the viewpoint of controlling thixotropy. As the silica, fused spherical silica or fused crushed silica can be used, and among them, it is preferable to use fused spherical silica. In addition, the shape of the inorganic filler is preferably as spherical as possible from the viewpoint of increasing the content of the inorganic filler while suppressing the increase in the melt viscosity of the obtained thermosetting resin composition, and it is preferable that the particle size distribution is broad.
[0070] When an inorganic filler is used, the average particle size of the inorganic filler is preferably 0.01 μm or more, more preferably 0.1 μm or more, and most preferably 0.3 μm or more. This effectively prevents the inorganic filler from settling in the thermosetting resin composition. It also prevents the nozzle of the jet dispenser from wearing out, which makes the discharged resin composition more likely to scatter outside the desired area. The average particle size is preferably 10 μm or less, more preferably 5 μm or less, and most preferably 3 μm or less, which can improve the applicability using a jet dispenser or the like.
[0071] <Solvent> The solvent used in the thermosetting resin composition of the second embodiment may be the same as that in the first embodiment. The preferred aspects of the solvent are also the same as those in the first embodiment.
[0072] In the second embodiment, the solvent can be used in an appropriate amount for adjusting the viscosity of the thermosetting resin composition to a desired range, for example, in an amount of 10 mass % or more and 70 mass % or less with respect to the entire thermosetting resin composition.
[0073] <Hardening agent> The thermosetting resin composition of the second embodiment may contain a curing agent. When a curing agent is used, the curing agent may be the same as that in the first embodiment. The preferred aspects of the curing agent are also the same as those in the first embodiment.
[0074] In addition, when a curing agent is used, the content of the curing agent in the thermosetting resin composition for wire coating material is preferably 0.1 mass % or more, more preferably 1 mass % or more, and even more preferably 3 mass % or more, based on the total solid content of the thermosetting resin composition (excluding inorganic filler), from the viewpoint of improving toughness and chemical resistance during low-temperature curing. From the viewpoint of improving the chemical resistance of the cured film, the content of the curing agent in the thermosetting resin composition is preferably 60 mass % or less, more preferably 50 mass % or less, and even more preferably 40 mass % or less, when the solid content (excluding the inorganic filler) of the thermosetting resin composition is 100 mass %.
[0075] <Other additives> The thermosetting resin composition for wire coating materials of the second embodiment may contain other additives such as an acid generator, an adhesion aid, other inorganic fillers, a stabilizer, a surfactant, etc., as in the first embodiment, if desired.
[0076] (Characteristics of thermosetting resin composition for wire coating material) The thermosetting resin composition for wire coating material of the second embodiment has a storage modulus at 25 ° C. measured by a dynamic viscoelasticity measuring device under the conditions of a measurement temperature of 20 ° C. to 300 ° C., a heating rate of 5 ° C. / min, a frequency of 1 Hz, and a tensile mode, of 2 GPa or more and 20 GPa or less, preferably 3 GPa or more and 18 GPa or less. The wire coating material obtained from the thermosetting resin composition for wire coating material has a storage modulus in the above range, so that it can maintain sufficient rigidity at low temperatures and has low elasticity at high temperatures during sealing or operation, and therefore can maintain softness, and can relieve thermal stress generated in the bonding wire and connection at high temperatures.
[0077] In the thermosetting resin composition for wire coating materials of the present embodiment, the content of chloride ions in a cured product obtained by heat-treating the thermosetting resin composition at 175°C for 120 minutes, as measured by the following procedure, is 0.01 ppm or more and 10 ppm or less, and preferably 0.01 ppm or more and 6 ppm or less. (procedure) 50 mL of pure water is added to 5 g of the cured product of the thermosetting resin composition, and hot water extraction is performed at 125° C. for 24 hours to obtain an extract. The obtained extract is analyzed by ion chromatography to measure the ion concentration in the cured product of the thermosetting resin composition. The thermosetting resin composition for wire coating material of this embodiment having a chloride ion content in the above range can inhibit corrosion of the bonding interface (bonding layer 19) between the semiconductor chip and the bonding wire caused by chloride ions.
[0078] The thermosetting resin composition for wire coating material of this embodiment has a glass transition temperature of 150°C to 350°C, preferably 180°C to 300°C, and more preferably 200°C to 280°C, as measured by a dynamic viscoelasticity measuring device under conditions of a measurement temperature of 20°C to 300°C, a heating rate of 5°C / min, a frequency of 1Hz, and a tensile mode, for a cured product obtained by heat-treating the thermosetting resin composition for wire coating material for 120 minutes. The wire coating material obtained from the thermosetting resin composition for wire coating material has excellent heat resistance by having a glass transition temperature in the above range.
[0079] The thermosetting resin composition for wire coating material of this embodiment has a viscosity measured at 20 rpm and 25 ° C. using a Brookfield BH type rotational viscometer of 20 mPa · s to 2000 mPa · s, preferably 100 mPa · s to 1800 mPa · s, more preferably 150 mPa · s to 1500 mPa · s. Since the thermosetting resin composition for wire coating material of this embodiment is intended for application by a jet dispenser, it is preferable that the viscosity at the nozzle tip temperature is low so that the thermosetting resin composition can be discharged at high speed from a fine hole with an inner diameter of several hundred μm. In addition, it is preferable that the thermosetting resin composition after discharge has fluidity. The thermosetting resin composition for wire coating material of this embodiment having a viscosity in the above range has excellent applicability by a jet dispenser.
[0080] The thermosetting resin composition for wire coating materials of this embodiment has a thixotropic ratio, expressed as viscosity a / viscosity b, of 0.1 or more and 3.0 or less, and preferably 0.5 or more and 2.0 or less. Viscosity a: Viscosity measured using a Brookfield BH type rotational viscometer at 10 rpm and 25°C. Viscosity b: Viscosity measured using a Brookfield BH type rotational viscometer at 20 rpm and 25°C.
[0081] The thermosetting resin composition for wire coating material of the present embodiment has the above composition and thus has thixotropy. Here, the thermosetting resin composition having thixotropy means that the thermosetting resin composition has a viscoelastic property in which the viscosity decreases when the thermosetting resin composition is subjected to shear stress (when the shear rate is increased), and the viscosity recovers and the flow is suppressed when the shear stress is released (when the shear rate is decreased).
[0082] If the thixotropy ratio is in the range of 0.1 to 3.0, when the thermosetting resin composition is applied using a jet dispenser, the thermosetting resin composition flows appropriately while being extruded from the jet dispenser and stops flowing after being extruded, making it difficult for the composition to flow out of a specified area (maintaining the applied shape), and thus enabling the composition to be applied to a specified area.
[0083] (Method of manufacturing a semiconductor device) The semiconductor device of this embodiment is produced by the following method using the thermosetting resin composition for wire coating material according to the first and second embodiments described above. (1) Wire bonding process: First, on the upper surface of the semiconductor chip 1, the bonding wire 7 is connected to the semiconductor chip 1 via a bonding layer 19 made of, for example, aluminum. Then, on the upper surface of the circuit board 2, the bonding wire 7 is connected to the circuit board 2 via a wiring 11. (2) Coating step: Next, using a jet dispenser, the above-mentioned thermosetting resin composition for wire coating material is applied to the joint between the semiconductor chip 1 and the bonding wire 7. In this way, the joint between the semiconductor chip 1 and the bonding wire 7, including the bonding layer 19, is coated with the wire coating material 5. (3) Encapsulating process: Finally, the entire surface of the semiconductor device 30, including the semiconductor chip 1, the surface on which the semiconductor chip is mounted on the circuit board 2, the bonding wires 7, the joint between the semiconductor chip 1 and the bonding wires 7, and the joint between the bonding wires 7 and the circuit board 2, is covered with a resin encapsulant 4 made of an encapsulating resin different from the resin constituting the wire coating material 5.
[0084] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Examples of embodiments are given below. 1. A mounting plate; a semiconductor chip mounted on the mounting plate and having bonding pads; a bonding wire bonded to the bonding pad for connecting the semiconductor chip and the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the semiconductor chip mounting surface of the mounting plate, and the bonding wires, A thermosetting resin composition used to cover at least a portion of the bonding wire and the bonding pad, The thermosetting resin composition includes a thermosetting resin, a curing agent, and a solvent, The thermosetting resin composition has a viscosity of 20 mPa·s or more as measured by a rotational viscometer. 2. The thermosetting resin composition described in 1., which is applied to at least a portion of the bonding wire and to the junction between the bonding pad and the bonding wire using a jet dispenser. 3. The thermosetting resin composition according to 1 or 2, wherein the thermosetting resin is present in an amount of 10 mass % or more based on the total solid content of the thermosetting resin composition. 4. The thermosetting resin composition according to any one of 1. to 3., wherein the concentration of chloride ions and sulfide ions is 10 ppm or less. 5. The thermosetting resin composition according to any one of 1. to 4., wherein the thermosetting resin comprises at least one selected from the group consisting of a novolac type epoxy resin, a reaction product of a phenol compound and an aldehyde compound, a reaction product of a phenol compound and a dimethanol compound, a hydroxystyrene resin, a polyamide resin, a polybenzoxazole resin, a polyimide resin, and a cyclic olefin resin. 6. The thermosetting resin composition according to any one of 1. to 5., wherein the solvent comprises at least one selected from N-methylpyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, N-ethyl-2-pyrrolidone, tetramethyluric acid, ethyl lactate, N,N-dimethylacetamide, dimethylsulfoxide, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, dipropylene glycol monomethyl ether, methyl lactate, butyl lactate, methyl-1,3-butylene glycol acetate, 1,3-butylene glycol-3-monomethyl ether, methyl pyruvate, ethyl pyruvate, and methyl-3-methoxypropionate. 7. The thermosetting resin composition according to any one of 1. to 6., further comprising an inorganic filler. 8. A mounting plate; a semiconductor chip having bonding pads mounted on the mounting plate; a bonding wire bonded to the bonding pad for connecting the semiconductor chip and the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the mounting surface of the mounting plate on which the semiconductor chip is mounted, and the bonding wires; a wire coating material that coats a connection portion between the bonding wire and the bonding pad; 8. A semiconductor device, wherein the wire coating material is a cured product of the thermosetting resin composition according to any one of 1. to 7. 9. A mounting plate; a semiconductor chip mounted on the mounting plate and having bonding pads; a bonding wire bonded to the bonding pad for connecting the semiconductor chip and the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the semiconductor chip mounting surface of the mounting plate, and the bonding wires, A thermosetting resin composition used to cover at least a portion of the bonding wire and the bonding pad, The thermosetting resin composition includes a thermosetting resin, an inorganic filler, and a solvent, A thermosetting resin composition, wherein the content of the inorganic filler is 40% by mass or more and 85% by mass or less based on the total solid content of the thermosetting resin composition. 10. The thermosetting resin composition according to 9., wherein the inorganic filler has an average particle size of 0.01 μm or more and 10 μm or less in weight-based particle size distribution measured by a laser diffraction / scattering particle size distribution measurement method. 11. The thermosetting resin composition according to 9. or 10., The thermosetting resin composition is heat-treated at 175°C for 120 minutes, and the cured product is measured using a dynamic viscoelasticity measuring device under conditions of a measurement temperature of 20°C to 300°C, a heating rate of 5°C / min, a frequency of 1 Hz, and a tensile mode, and the storage modulus at 25°C is 2 GPa or more and 20 GPa or less. 12. The thermosetting resin composition according to any one of 9. to 11., A thermosetting resin composition, wherein a cured product obtained by heat-treating the thermosetting resin composition at 175°C for 120 minutes has a chloride ion content of 0.01 ppm or more and 10 ppm or less, as measured by the following procedure. (procedure) 50 mL of pure water is added to 5 g of the cured product of the thermosetting resin composition, and hot water extraction is performed at 125° C. for 24 hours to obtain extracted water. The obtained extracted water is analyzed by ion chromatography to measure the ion concentration in the cured product of the thermosetting resin composition. 13. The thermosetting resin composition according to any one of 9. to 12., The thermosetting resin composition is heat-treated at 175°C for 120 minutes to obtain a cured product, which has a glass transition temperature of 150°C or higher and 350°C or lower, as measured using a dynamic viscoelasticity measuring device (DMA) under conditions of an initial temperature of 20°C, a measurement temperature range of 20 to 300°C, a heating rate of 5°C / min, and a frequency of 1 Hz. 14. The thermosetting resin composition according to any one of 9. to 13., having a viscosity of 20 mPa·s or more and 2,000 mPa·s or less, measured at 20 rpm and 25°C using a Brookfield BH type rotational viscometer. 15. The thermosetting resin composition according to any one of 9. to 14., wherein the thixotropic ratio represented by viscosity a / viscosity b is 0.1 or more and 3.0 or less. Viscosity a: Viscosity measured using a Brookfield BH type rotational viscometer at 10 rpm and 25°C; Viscosity b: Viscosity measured using a Brookfield BH type rotational viscometer at 20 rpm and 25°C. 16. The thermosetting resin composition according to any one of 9. to 15., which is applied using a jet dispenser so as to cover the connection portion between the bonding wire and the bonding pad. 17. The thermosetting resin composition according to any one of 9. to 17., wherein the inorganic filler comprises at least one selected from the group consisting of silica, talc, alumina, titanium white, and silicon nitride. 18. The thermosetting resin composition according to any one of 9. to 17., wherein the thermosetting resin comprises at least one selected from the group consisting of a novolac-type phenolic resin, a reaction product of a phenolic compound and an aldehyde compound, a reaction product of a phenolic compound and a dimethanol compound, a hydroxystyrene resin, a polyamide resin, a polybenzoxazole resin, a polyimide resin, and a cyclic olefin resin. 19. The thermosetting resin composition according to any one of 9. to 18., wherein the solvent comprises at least one selected from N-methylpyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, N-ethyl-2-pyrrolidone, tetramethyluric acid, ethyl lactate, N,N-dimethylacetamide, dimethyl sulfoxide, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, dipropylene glycol monomethyl ether, methyl lactate, butyl lactate, methyl-1,3-butylene glycol acetate, 1,3-butylene glycol-3-monomethyl ether, methyl pyruvate, ethyl pyruvate, and methyl-3-methoxypropionate. 20. A mounting plate; a semiconductor chip having bonding pads mounted on the mounting plate; a bonding wire bonded to the bonding pad for connecting the semiconductor chip and the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the mounting surface of the mounting plate on which the semiconductor chip is mounted, and the bonding wires; a wire coating material that coats a connection portion between the bonding wire and the bonding pad; 20. A semiconductor device, wherein the wire coating material is a cured product of the thermosetting resin composition according to any one of 9. to 19. EXAMPLES
[0085] EXAMPLES Hereinafter, the present invention will be described with reference to examples and comparative examples, but the present invention is not limited to these. Details of each raw material component used in the examples are shown below.
[0086] (solvent) Solvent 1: γ-butyrolactone (Merck (AZ Electronic Materials)) Solvent 2: Propylene glycol monomethyl ether acetate (Merck Performance Materials) Solvent 3: 2-heptanone (Tokyo Chemical Industry Co., Ltd.) (resin) Resin 1: Phenolic resin (Sumitomo Bakelite Co., Ltd., weight average molecular weight 54040) Resin 2: Epoxy resin (Nippon Kayaku Co., Ltd., EPPN201) Resin 3: Polynorbornene resin (Avatrel 2590, manufactured by Promerus) Resin 4: Bisphenol A type epoxy resin (Mitsubishi Chemical Corporation, jER1256) (hardening agent) Hardener 1: A mixture of tetrakis(methoxymethyl)glycoluril, methanol, and formaldehyde (Daito Chemistry, CROLIN-318) Hardener 2: Linear epoxy resin (Mitsubishi Chemical, JER YX7105) Hardener 3: 2-undecylmethylimidazole (C11Z, manufactured by Shikoku Chemical Industries Co., Ltd.) (Coupling Agent) Coupling agent 1: 3-methacryloxypropylmethyldimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-503P) Coupling agent 2: 3-glycidoxypropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-403E) Coupling agent 3: 3-mercapto-1,2,4-triazole (manufactured by Huaihua Wangda Biotechnology Co., Ltd.) Coupling agent 4: Triethoxysilylpropylmaleamic acid (Silica particles) Silica particle 1: Spherical silica (Admatechs, SE-2100, particle size 0.58 um) Silica particle 2: Spherical silica (Admatechs, UF-320, particle size 2.80um) (Acid Generator) Acid generator 1: (4,8-di-n-butoxy-1-naphthyl)sulfonium tetrakispentafluorophenylborate (thermal acid generator, DSP, Gokyo Food & Chemical Co., Ltd., ZK-1722) Acid generator 2: (4-acetoxyphenyl)benzyl(methyl)sulfonium = tetrakis(pentafluorophenyl)borate thermal acid generator (manufactured by Sanshin Chemical Industry, SI-B3A) Acid generator 3: Photoacid generator (manufactured by San-Apro Co., Ltd.) (Surfactant) Surfactant 1: Copolymer of 2-[N-perfluorobutylsulfonyl-N-methylamino)ethyl acrylate, poly(oxyalkylene glycol) monoacrylate, and poly(oxyalkylene glycol) diacrylate (3M, FC-4432) Surfactant 2: Perfluoroalkyl polymer (C4 type) (DIC, R-41)
[0087] (Examples A1 to A6, Comparative Example A1) (Preparation of Thermosetting Resin Composition) For each of the Examples and Comparative Examples, a thermosetting resin composition was prepared as follows. In each Example A and Comparative Example A, the components shown in Table 1 were mixed in the amounts shown in Table 1 in a solvent to prepare a varnish-like resin composition.
[0088] (Physical Properties of Varnish-like Resin Composition) The varnish-like resin composition obtained above was measured for the following physical properties. The measurement results and evaluation results of the physical properties are shown in Table 1. In the table, "-" indicates that the measurement was not performed.
[0089] (1. Viscosity) The viscosity of the varnish-like resin composition at 25° C. was measured using a rotational viscometer. The results are shown in Table 1.
[0090] (2. Thixotropy) The thixotropy of the resin composition was evaluated by determining the thixotropic coefficient (x1) using a Brookfield BH type rotational viscometer according to the following procedure. The varnish-like resin composition obtained above was placed in a wide-mouthed light-shielding bottle (100 ml), and the liquid temperature was adjusted to 25°C ± 0.5°C using a thermostatic water bath. Next, the mixture was stirred 40 times over a period of 12 to 15 seconds using a glass rod, and then a specified rotor was installed and allowed to stand for 5 minutes, after which the scale was read after rotating at 20 rpm for 3 minutes. Viscosity η 20 The viscosity η measured at 25°C and 10 rpm was calculated by multiplying this scale by the coefficient in the conversion table. 10 The results are shown in Table 1. x1=η 10 / η 20
[0091] (3. Application with a jet dispenser) (3.1 Jet Dispenser Discharge Pressure) The air supply pressure was set to a predetermined value using the external controller MJET-3-CTR attached to the jet dispenser manufactured by Musashi Engineering. The minimum pressure at which the varnish-like resin composition was discharged from the syringe was measured as the "discharge pressure" of the jet dispenser. The results are shown in Table 1. The lower the discharge pressure, the better the application properties of the jet dispenser. The syringe temperature during discharge is also shown in Table 1. (3.2 Tip contamination during application - Wetting and spreading) The varnish-like resin composition was applied to the bonding wire using a jet dispenser. The surface state of the chip immediately after application was photographed with a camera (manufactured by Keyence Corporation) attached to the jet dispenser. Based on the photograph, the degree of contamination was evaluated as "low" when 10 to 30% of the chip's surface area (3.5 mm x 3.5 mm) was covered with the varnish-like resin composition after application, "normal" when more than 30% to 60% was covered, and "high" when more than 60% of the surface was covered. The area was calculated manually from the photographic image. The results are shown in Table 1. The lower the degree of contamination, the better the applicability. (3.3 Presence or absence of voids) The above varnish-like resin composition was applied onto the chip and cured by heating. After the curing process, the entire surface of the chip was observed from above at a magnification of 100 times using an optical microscope (manufactured by Keyence Corporation). When the surface of the cured product was not uniform and even one void due to bubbles or void between the filler and the resin was observed under the optical microscope, the void was recorded as "present", and when no void was observed at all, the void was recorded as "absent". The results are shown in Table 1.
[0092] (Physical Properties of Cured Resin Composition) (growth rate) The above-mentioned varnish-like resin composition was applied to a 6-inch wafer, and then the resin film was obtained by removing the solvent through heat treatment at 120°C for 240 seconds. Then, the resin film was heat-treated in an oven to be cured. The heat treatment was performed by replacing the atmosphere in the oven in which the wafer was placed with nitrogen at 30°C for 30 minutes, heating the oven to each curing temperature (175°C or 220°C) at a heating rate of 5°C / min, and then holding the oven at the curing temperature for 120 minutes. After the heat treatment, the temperature in the oven was lowered to 70°C or lower at a heating rate of 5°C / min, and the wafer was removed. Then, the resin film was peeled off from the wafer using hydrofluoric acid and dried at 60°C for 10 hours. In this way, a resin film cured at each of the above-mentioned curing temperatures was obtained for each of the examples and comparative examples. Next, the tensile elongation of each of the resin films was measured as follows. First, a tensile test (tensile speed: 0.05 mm / min) was performed on a test piece (width 10 mm × length 60 mm or more × thickness 0.005 to 0.01 mm) made of a resin film in an atmosphere with a temperature of 23°C and a humidity of 55%. The tensile test was performed using a tensile tester (Tensilon RTC-1210A) manufactured by Orientec Co., Ltd. Next, the tensile elongation was calculated from the results of the tensile test. Here, the above tensile test was performed five times, n = 5, and the average value of the tensile elongation was calculated and shown as the measured value.
[0093] (Reliability evaluation of semiconductor devices) A semiconductor device was produced according to the method described in the above-mentioned "Method of producing a semiconductor device". When producing the semiconductor device, the thermosetting resin composition for wire coating and the encapsulating resin were cured at a temperature of 175°C or 220°C. A DC voltage of 20V was applied to the semiconductor device obtained at each curing temperature for 240 hours in an environment at a temperature of 130°C. The number of defects (leakage defects) of the semiconductor device was investigated 40 hours, 80 hours, 120 hours, and 240 hours after the start of the measurement. n=10. The results are shown in Table 1 as the number of defects out of 10 samples.
[0094] [Table 1]
[0095] The thermosetting resin composition for wire coating of Example A was excellent in coatability with a jet dispenser. Furthermore, the semiconductor device produced using the resin composition for wire coating of the Example was excellent in reliability.
[0096] (Examples B1 to B3, Comparative Examples B1 to B4) (Preparation of Thermosetting Resin Composition) For each of the Examples and Comparative Examples, a thermosetting resin composition was prepared as follows. In each of the Examples and Comparative Examples, the components shown in Table 2 were mixed in the amounts shown in Table 2 in a solvent to prepare a varnish-like resin composition.
[0097] (Physical Properties of Varnish-like Resin Composition) The varnish-like resin composition obtained above was measured for the following physical properties. The measurement results and evaluation results of the physical properties are shown in Table 2.
[0098] (viscosity) The viscosity of the varnish-like resin composition was measured at 20 rpm and 25° C. using a Brookfield BH type rotational viscometer. The results are shown in Table 2.
[0099] (thixotropy) The thixotropy of the resin composition was evaluated by the thixotropy ratio (x1) using a rotational viscometer according to the following procedure. The viscosity measured at 10 rpm and 25°C using a Brookfield BH rotational viscometer was taken as viscosity a, and the viscosity measured at 20 rpm and 25°C using a Brookfield BH rotational viscometer was taken as viscosity b. The thixotropy was calculated according to the following formula. The results are shown in Table 2. x1=viscosity a / viscosity b
[0100] (Physical properties of cured resin composition) (storage modulus, glass transition temperature) The storage modulus and glass transition temperature of the cured product of the resin composition obtained in each example were measured as follows. The above-mentioned varnish-like resin composition was applied to a 6-inch wafer, and then heat-treated at 120°C for 240 seconds to remove the solvent, thereby obtaining a resin film. The resin film was then heat-treated in an oven to harden it. The heat treatment was carried out by replacing the atmosphere in the oven in which the wafer was placed with nitrogen at 30°C for 30 minutes, heating it to 175°C at a heating rate of 5°C / min, and then holding it at that hardening temperature for 120 minutes. After the heat treatment, the temperature in the oven was lowered to 70°C or lower at a heating rate of 5°C / min, and the wafer was removed. The resin film was then peeled off from the wafer using hydrofluoric acid, and dried at 60°C for 10 hours, and a test piece measuring 4 mm wide x 20 mm long x 10 μm thick was obtained from the obtained hardened film. Measurements were performed on the test pieces of each example using a dynamic viscoelasticity measuring machine (DMA, Hitachi High-Tech Science Corporation, DMA7100) under conditions of a starting temperature of 20°C, a measurement temperature range of 20 to 300°C, a heating rate of 5°C / min, and a frequency of 1 Hz, and from the measurement results, Tg (°C) and storage modulus (GPa) at 25°C were calculated. The results are shown in Table 2. Note that in Comparative Example B4, a sample could not be prepared, and therefore "measurement not possible" is indicated.
[0101] (chlorine ion content) The chloride ion concentration of the cured product of the resin composition obtained in each example was measured as follows. First, the resin composition obtained above was cured in an oven at 175°C for 120 minutes to obtain a cured product. 5 g of the obtained sample and 50 ml of pure water were placed in a Teflon (registered trademark) pressure-resistant container and sealed, and treated (hot water extraction) at a temperature of 125°C and a relative humidity of 100%RH for 24 hours. Next, after cooling to room temperature, the extracted water was centrifuged and filtered with a 20 μm filter, and the filtrate was used as the extracted water. The obtained extracted water was analyzed by ion chromatography using an ion chromatograph (manufactured by Thermo Fisher Scientific Co., Ltd.), and the chloride ion concentration in the extracted water was measured. The obtained chloride ion concentration results are shown in Table 2.
[0102] (Performance evaluation of wire coating materials) (Whether or not peeling occurs) According to the method described in the above "Method of Manufacturing a Semiconductor Device", the resin composition obtained in each example was used as a wire coating material to coat the wire bonding portion with a maximum film thickness of 50 μm to fabricate a semiconductor device. The fabricated semiconductor device was cut and polished at the wire bonding portion, and the cross section was observed using an SEM. The results are shown in Table 2, with peeling "present" if peeling was observed between the semiconductor chip 1 and the connection pad 8, between the semiconductor chip 1 and the barrier layer 18, or between the barrier layer 18 and the bonding layer 19, and "absent" if no peeling was observed.
[0103] (Cracks or not) According to the method described in the above "Method of manufacturing a semiconductor device", the resin composition obtained in each example was used as a wire coating material to coat the wire bonding portion with a maximum film thickness of 50 μm, to prepare a semiconductor device. The wire bonding portion of the fabricated semiconductor device was cut and polished, and the cross section was observed using an SEM. The results are shown in Table 2. If even one crack was observed on the cross section of the wire coating material 5, it was recorded as "crack present." If no cracks were observed, it was recorded as "no crack present."
[0104] [Table 2]
[0105] The semiconductor device produced using the resin composition of Example B as a wire coating material had excellent reliability without peeling between the components in the semiconductor device or cracks in the wire coating material.
[0106] This application claims priority based on Japanese Patent Application No. 2020-200772, filed on December 3, 2020, and Japanese Patent Application No. 2021-054709, filed on March 29, 2021, the disclosures of which are incorporated herein in their entirety.
Claims
1. A mounting plate; a semiconductor chip mounted on the mounting plate and having bonding pads; bonding wires bonded to the bonding pads to connect the semiconductor chip to the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the mounting surface of the mounting board for the semiconductor chip, and the bonding wires, A thermosetting resin composition used to cover at least a portion of the bonding wire and the bonding pad, The thermosetting resin composition includes a thermosetting resin, a curing agent, an inorganic filler, and a solvent, the thermosetting resin includes a novolac phenolic resin, the curing agent comprises an epoxy resin and an alkoxymethyl glycoluril compound; A thermosetting resin composition, wherein the content of the inorganic filler is 40% by mass or more and 85% by mass or less based on the total solid content of the thermosetting resin composition.
2. 2. The thermosetting resin composition according to claim 1, wherein the inorganic filler has an average particle size of 0.01 μm or more and 10 μm or less in weight-based particle size distribution measured by a laser diffraction / scattering particle size distribution measurement method.
3. The thermosetting resin composition according to claim 1 or 2, The thermosetting resin composition is heat-treated at 175°C for 120 minutes, and the cured product is subjected to measurement using a dynamic viscoelasticity measuring device under the conditions of a measurement temperature of 20°C to 300°C, a temperature rise rate of 5°C / min, a frequency of 1 Hz, and a tensile mode, and the storage modulus at 25°C is 2 GPa or more and 20 GPa or less.
4. The thermosetting resin composition according to any one of claims 1 to 3, The thermosetting resin composition is heat-treated at 175°C for 120 minutes, and the cured product has a chloride ion content of 0.01 ppm or more and 10 ppm or less, as measured by the following procedure. (procedure) 50 mL of pure water is added to 5 g of the cured product of the thermosetting resin composition, and the mixture is subjected to hot water extraction at 125°C for 24 hours to obtain extracted water. The extracted water is analyzed by ion chromatography to measure the ion concentration in the cured product of the thermosetting resin composition.
5. The thermosetting resin composition according to any one of claims 1 to 4, The thermosetting resin composition is heat-treated at 175°C for 120 minutes, and the cured product has a glass transition temperature of 150°C or higher and 350°C or lower, as measured using a dynamic mechanical analyzer (DMA) under the following conditions: an initial temperature of 20°C, a measurement temperature range of 20 to 300°C, a heating rate of 5°C / min, and a frequency of 1 Hz.
6. 6. The thermosetting resin composition according to claim 1, wherein the viscosity measured at 20 rpm and 25°C using a Brookfield BH type rotational viscometer is 20 mPa·s or more and 2000 mPa·s or less.
7. The thermosetting resin composition according to any one of claims 1 to 6, wherein a thixotropy ratio represented by viscosity a / viscosity b is 0.1 or more and 3.0 or less: Viscosity a: Viscosity measured using a Brookfield BH type rotational viscometer at 10 rpm and 25°C; Viscosity b: Viscosity measured at 20 rpm and 25°C using a Brookfield BH type rotational viscometer.
8. 8. The thermosetting resin composition according to claim 1, which is applied using a jet dispenser so as to cover the connection portion between the bonding wire and the bonding pad.
9. 9. The thermosetting resin composition according to claim 1, wherein the inorganic filler comprises at least one selected from the group consisting of silica, talc, alumina, titanium white, and silicon nitride.
10. 10. The thermosetting resin composition according to claim 1, wherein the solvent comprises at least one selected from N-methylpyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, N-ethyl-2-pyrrolidone, tetramethyluric acid, ethyl lactate, N,N-dimethylacetamide, dimethyl sulfoxide, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, dipropylene glycol monomethyl ether, methyl lactate, butyl lactate, methyl-1,3-butylene glycol acetate, 1,3-butylene glycol-3-monomethyl ether, methyl pyruvate, ethyl pyruvate, and methyl-3-methoxypropionate.
11. A mounting plate; a semiconductor chip having bonding pads mounted on the mounting plate; bonding wires bonded to the bonding pads to connect the semiconductor chip to the mounting plate; a resin encapsulant that encapsulates the semiconductor chip, the mounting surface of the mounting board on which the semiconductor chip is mounted, and the bonding wires; a wire coating material that coats the connection portion between the bonding wire and the bonding pad, A semiconductor device, wherein the wire coating material comprises a cured product of the thermosetting resin composition according to claim 1 .
Citation Information
Patent Citations
Positive-type photosensitive resin composition, cured film and manufacturing method thereof, pattern, mems structure manufacturing method, dry and wet etching method
CN103019034A
Semiconductor device and manufacture thereof
JP1992221842A
Semiconductor device and bonding wire for the same
JP2003133362A
Method of manufacturing electronic part and semiconductor device
JP2004327557A
Layered product for transfer and method for forming optical element
JP2017090508A