Acrylic-olefin composite resin composition, non-aqueous resin composition, method for producing non-aqueous resin composition, method for producing acrylic-olefin composite resin composition, coating composition, ink composition, adhesive composition, film and molding material

The acrylic olefin composite resin composition with controlled water content and SP parameter solvent system addresses adhesion and stability issues, providing enhanced adhesion to polyolefin substrates and stable solvent solubility.

JP7559925B2Active Publication Date: 2024-10-02MITSUBISHI CHEM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023506824
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-16
Filing Date
2022-01-27
Publication Date
2024-10-02
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

Existing resin compositions face challenges in achieving both excellent adhesion to polyolefin base materials and storage stability, particularly due to issues with solubility in solvents and separation over time, as well as the environmental concerns associated with using chlorine-containing compounds.

Method used

A composite resin composition comprising acrylic olefin resin with specific structural units and a water content of 0.01% to 10%, combined with an organic solvent system having a solubility parameter (SP) range of 8.0 to 9.2, enhances adhesion and stability by forming strong chemical bonds and maintaining dispersion.

Benefits of technology

The composition exhibits superior adhesion to polyolefin substrates and maintains storage stability, ensuring effective use in applications requiring solvent solubility and environmental compliance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559925000001
    Figure 0007559925000001
  • Figure 0007559925000002
    Figure 0007559925000002
  • Figure 0007559925000003
    Figure 0007559925000003
Patent Text Reader

Abstract

Provided is an acryl-olefin composite resin composition that has excellent storage stability and adhesiveness with respect to a polyolefin base material. The acryl-olefin composite resin composition according to the present invention contains an acryl-olefin composite resin C. The acryl-olefin composite resin C includes a structural unit derived from a (meth)acrylic monomer a, and a structure derived from an olefin resin B. The water content of the acryl-olefin composite resin composition is 0.01-10 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an acrylic olefin hybrid resin composition and a method for producing the same, a non-aqueous resin composition and a method for producing the same, a coating composition, an ink composition, an adhesive composition, a film, and a molding material. This application claims priority based on Japanese Patent Application No. 2021-042195, filed on March 16, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] Polyolefin resins, which are polymers of olefin monomers, have excellent mechanical properties and chemical resistance, and are easy to mold at low cost, so they are widely used in a variety of applications. Furthermore, polyolefin resins are also highly recyclable, so their applications are expanding further in light of recent global environmental issues. However, because polyolefin resins have low polarity, they are generally considered difficult to adhere to polyolefin substrates.

[0003] Known methods for improving adhesion to polyolefin-based substrates include chemically treating the surface of the polyolefin-based substrate with a chemical or the like, and oxidizing the surface by corona discharge treatment, plasma treatment, flame treatment, or the like. However, these methods have the problem that they require special equipment and are not effective in improving adhesion.

[0004] On the other hand, a method for improving adhesion to polyolefin-based substrates is known in which an ink, paint or adhesive containing a chlorinated polyolefin is applied to the surface of the polyolefin-based substrate. However, due to the recent growing concern about environmental issues, there is a tendency to avoid the use of chlorine-containing compounds such as chlorinated polyolefins, and therefore, in recent years, there has been an increasing demand for resin compositions composed of compounds that do not contain chlorine.

[0005] Patent Document 1 describes a resin solution containing a graft copolymer obtained by graft polymerizing a specific monomer onto an olefin polymer, which is a chlorine-free resin that has high adhesion to polyolefin substrates. However, the resin solution described in Patent Document 1 separates over time, and therefore has a problem with storage stability.

[0006] Patent Document 2 describes a solid resin that is said to have no concerns about storage stability, and that contains a graft copolymer obtained by graft polymerizing a specific monomer onto an olefin polymer. However, the method described in Patent Document 2 does not provide good solubility in the solvent used, and therefore poses a problem when used in applications requiring solubility in a solvent, such as inks, paints, and adhesives. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japan Special Publication No. 2012-521454 [Patent Document 2] Japanese Patent Publication No. 2002-338778 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention aims to provide an acrylic-olefin composite resin composition having excellent adhesion to polyolefin substrates and excellent storage stability, a nonaqueous resin composition containing a composite resin composition having excellent adhesion to polyolefin substrates and excellent storage stability, and methods for producing the same. [Means for solving the problem]

[0009] That is, the present invention relates to the following items [1] to

[21] .

[0010] [1] An acrylic olefin composite resin composition D containing an acrylic olefin composite resin C, The acrylic olefin composite resin C contains a structural unit derived from a (meth)acrylic monomer a and a structure derived from an olefin resin B, The acrylic olefin composite resin composition D has a water content of 0.01% by mass or more and 10% by mass or less. [2] an acrylic resin A containing a structural unit derived from the (meth)acrylic monomer a, and The acrylic olefin composite resin composition D according to [1] further contains the olefin resin B. [3] The acrylic olefin composite resin composition D according to [1] or [2], which is in the form of particles. [4] The acrylic olefin composite resin composition D according to [3], having a mass average particle diameter of 10 μm or more and 2,500 μm or less. [5] The acrylic olefin composite resin composition D according to any one of [1] to [4], wherein the olefin resin B contains at least one of an ethylene-propylene copolymer and a polypropylene. [6] The acrylic olefin composite resin composition D according to any one of [1] to [5], wherein the mass ratio of the total mass of the structural units derived from all monomers constituting the olefin resin B to the total mass of the structural units derived from the (meth)acrylic monomer a is 1 to 100%. [7] A non-aqueous resin composition E comprising the acrylic olefin composite resin composition D according to any one of [1] to [6]. [8] The nonaqueous resin composition E according to [7], further comprising an organic solvent. [9] The nonaqueous resin composition E according to [8], wherein the organic solvent includes an organic solvent having a solubility parameter (SP value) of 8.0 or less and an organic solvent having a SP value of 9.2 or more.

[10] The organic solvent having an SP value of 8.0 or less is contained in an amount of 5% by mass or more and 80% by mass or less based on the total mass of the organic solvents; The nonaqueous resin composition E according to [9] contains an organic solvent having an SP value of 9.2 or more in an amount of 10 mass % or more and 70 mass % or less relative to the total mass of the organic solvents.

[11] The nonaqueous resin composition E according to [9] or

[10] , wherein the organic solvent having an SP value of 8.0 or less contains a compound having a cycloalkane structure.

[12] The nonaqueous resin composition E according to any one of [9] to

[11] , wherein the organic solvent having an SP value of 9.2 or more contains a ketone solvent.

[13] A method for producing the nonaqueous resin composition E according to any one of [9] to

[12] , comprising the steps of: A method for producing a non-aqueous resin composition E, comprising mixing an acrylic olefin composite resin composition D according to any one of [1] to [6] with an organic solvent containing 50 mass% or more of an organic solvent having an SP value of less than 9.2, and allowing the acrylic olefin composite resin composition D and the organic solvent having an SP value of 9.2 or more to coexist.

[14] A method for producing an acrylic-olefin composite resin composition D containing an acrylic-olefin composite resin C having a structural unit derived from a (meth)acrylic monomer a and a structure derived from an olefin resin B, comprising: A method for producing an acrylic-olefin composite resin composition D, comprising suspension polymerizing the (meth)acrylic monomer a in the presence of the olefin resin B.

[15] A coating composition comprising the acrylic olefin composite resin composition D according to any one of [1] to [6].

[16] An ink composition comprising the acrylic olefin composite resin composition D according to any one of [1] to [6].

[17] An adhesive composition comprising the acrylic olefin composite resin composition D according to any one of [1] to [6].

[18] A film or molding material comprising the acrylic olefin composite resin composition D according to any one of [1] to [6].

[19] A coating composition comprising the non-aqueous resin composition E according to any one of [7] to

[12] .

[20] An ink composition comprising the non-aqueous resin composition E according to any one of [7] to

[12] .

[21] An adhesive composition comprising the non-aqueous resin composition E according to any one of [7] to

[12] . Effect of the Invention

[0011] According to the present invention, it is possible to provide an acrylic-olefin composite resin composition having excellent adhesion to polyolefin substrates and excellent storage stability, a nonaqueous resin composition containing a composite resin composition having excellent adhesion to polyolefin substrates and excellent storage stability, and methods for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In the present invention, "(meth)acrylic" is a general term for "acrylic" and "methacrylic". "(meth)acrylate" is a general term for "acrylate" and "methacrylate".

[0013] The acrylic olefin composite resin composition D of the present invention (hereinafter also referred to as "composite resin composition D") contains an acrylic olefin composite resin C (hereinafter also referred to as "resin C"), in which the resin C contains a structural unit derived from a (meth)acrylic monomer a (hereinafter also referred to as "monomer a") and a structure derived from an olefin resin B (hereinafter also referred to as "resin B"), and the moisture content of the composite resin composition D is 0.01% or more and 10% or less. In order to obtain good adhesion to polyolefin-based substrates and good storage stability, the composite resin composition D preferably further contains, in addition to the resin C, an acrylic resin A (hereinafter also referred to as “resin A”) containing a structural unit derived from the monomer a, and a resin B.

[0014] The state in which the structure derived from resin B and the structural unit derived from monomer a are present in resin C is, for example, A state in which the structure derived from resin B and the constitutional units derived from monomer a are bonded together by chemical bonds such as covalent bonds, ionic bonds, and hydrogen bonds; A state in which the resin exists as secondary particles that are aggregates of primary particles of resin B and primary particles of a resin having structural units derived from monomer a; A state in which a resin having a structure derived from resin B and a constitutional unit derived from monomer a exists in a core-shell structure; a state in which a resin having a structure derived from resin B and a constitutional unit derived from monomer a is present in a microphase-separated structure such as a sea-island structure or an interconnected structure; In terms of obtaining good adhesion to polyolefin substrates and good storage stability of the composite resin composition, it is preferable that the structure derived from resin B and the constituent units derived from monomer a are bonded together by chemical bonds such as covalent bonds, ionic bonds, hydrogen bonds, etc., or that they exist as secondary particles that are aggregates of primary particles of resin B and primary particles of a resin having constituent units derived from monomer a; it is more preferable that the structure derived from resin B and the constituent units derived from monomer a are bonded together by chemical bonds such as covalent bonds, ionic bonds, hydrogen bonds, etc.

[0015] The composite resin composition D may be in a particulate form, for example, in a solid form such as granular form obtained by crushing a lump, powder form, or pellet form, or in a particulate form in a suspended state, or in a particulate form in an emulsified state. From the viewpoint of handling when dissolving in an organic solvent, the composite resin composition D is preferably in a particulate form obtained by crushing a lump, or in a particulate form in a suspended state.

[0016] Resin A and Resin C each have at least one constituent unit derived from monomer a.

[0017] Examples of the monomer a include alkyl (meth)acrylates having a straight or branched hydrocarbon skeleton, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, i-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and 4-t-butylcyclohexyl (meth)acrylate; Alkyl (meth)acrylates having an alicyclic skeleton, such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecanyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; (meth)acrylic acid esters having a glycidyl group, such as glycidyl (meth)acrylate and hydroxybutyl (meth)acrylate glycidyl ether; (meth)acrylic acid esters having an aromatic ring, such as phenoxy (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, nonylphenol EO adduct (meth)acrylate, and o-biphenyloxyethyl (meth)acrylate; (meth)acrylate salts such as ammonium (meth)acrylate, sodium (meth)acrylate, and potassium (meth)acrylate; (meth)acrylates having a cyclic ether, such as tetrahydrofurfuryl (meth)acrylate; (Meth)acrylates having an amino group, such as N-dimethylaminoethyl (meth)acrylate and N-diethylaminoethyl (meth)acrylate; (meth)acrylamide derivatives such as (meth)acrylamide, (meth)acrylamide diacetone acrylamide, N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-ethoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, and (meth)acryloylmorpholine; Monomers having a phosphoric acid group, such as 2-(meth)acryloyloxyethyl acid phosphate, 2-(meth)acryloyloxyethyl acid phosphate monoethanolamine salt, diphenyl((meth)acryloyloxyethyl)phosphate, (meth)acryloyloxypropyl acid phosphate, 3-chloro-2-acid phosphooxypropyl (meth)acrylate, acid phosphooxypolyoxyethylene glycol mono(meth)acrylate, and acid phosphooxypolyoxypropylene glycol (meth)acrylate; 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 1,2-dihydroxyethyl (meth)acrylate, 1,2-dihydroxypropyl (meth)acrylate, 1,2-dihydroxybutyl (meth)acrylate, 1,2-dihydroxy-5-ethylhexyl (meth)acrylate, 1,1-dihydroxyethyl (meth)acrylate, 1,1-dihydroxypropyl (meth)acrylate, 1,1-dihydroxybutyl (meth)acrylate, 1,2,3-trihydroxypropyl (meth)acrylate, 1,2,3-trihydroxybutyl (meth)acrylate, 1,1,2-trihydroxypropyl (meth)acrylate, 1,1,2-trihydroxybutyl (meth)acrylate, and other hydroxyalkyl (meth)acrylates; Hydroxy(meth)acrylates having an aromatic ring, such as 2-hydroxy-3-phenoxypropyl(meth)acrylate; Hydroxypolyethylene oxide mono(meth)acrylate, hydroxypolypropylene oxide mono(meth)acrylate, hydroxy(polyethylene oxide-polypropylene oxide) mono(meth)acrylate, hydroxy(polyethylene oxide-propylene oxide) mono(meth)acrylate, hydroxy(polyethylene oxide-polytetramethylene oxide) mono(meth)acrylate, hydroxy(polyethylene oxide-tetramethylene oxide) mono(meth)acrylate, hydroxy(polypropylene oxide-polytetramethylene oxide) mono(meth)acrylate, hydroxy(polypropylene oxide-polytetramethylene oxide) mono(meth)acrylate, 1,2-dihydroxypolyethyl oxide (meth)acrylate, 1,2-dihydroxypolypropylene oxide (meth)acrylate, polyhydroxyalkyl (meth)acrylate; hydroxypolyalkylene oxide (meth)acrylates such as 1,2,3-trihydroxypropylene glycol (meth)acrylate and 1,1,2-trihydroxypropylene glycol (meth)acrylate; Examples of the carboxyl group-containing (meth)acrylate include acrylic acid, methacrylic acid, mono(2-(meth)acryloyloxyethyl) succinate, and ω-carboxy-polycaprolactone mono(meth)acrylate.

[0018] From the viewpoint of adhesion to polyolefin-based substrates and storage stability of the composite resin composition D, it is preferable to contain at least one of alkyl (meth)acrylates having a linear or branched hydrocarbon skeleton and alkyl (meth)acrylates having an alicyclic skeleton, more preferably at least one of methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, cyclohexyl (meth)acrylate and isobornyl (meth)acrylate, and further preferably both methyl (meth)acrylate and n-butyl (meth)acrylate. The monomer a may be used alone or in combination of two or more kinds.

[0019] Resin A and Resin C may contain a structural unit derived from a monomer other than the monomer a in the copolymerization component. Examples of monomers other than the monomer a include aromatic vinyl monomers such as styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, and chlorostyrene; Vinyl cyanide monomers such as acrylonitrile, methacrylonitrile, α-cyanoacrylate, dicyanovinylidene, and fumaronitrile; Monomers having a carboxyl group, such as crotonic acid, isocrotonic acid, cinnamic acid, itaconic acid, maleic acid, fumaric acid, citraconic acid, mesaconic acid, and glutaconic acid; Sulfonic acid group-containing monomers such as vinyl sulfonic acid and 2-acrylamido-2-methylpropanesulfonic acid; Multifunctional monomers such as divinylbenzene, divinylnaphthalene, and divinyl ether; Vinyl monomers such as vinyl acetate and vinyl propionate; Conjugated diene monomers such as 1,3-butadiene, isoprene, 2-chloro-1,3-butadiene, and chloroprene can be mentioned. The monomers other than the monomer a may be used alone or in combination of two or more kinds.

[0020] From the viewpoint of the storage stability of the composite resin composition D, the resin A preferably contains 50% by mass or more, and more preferably 80% by mass or more, of the constituent units derived from the monomer a. When the mass ratio of the constituent units derived from the monomer a in the resin A is equal to or more than the above lower limit, the storage stability of the composite resin composition D tends to be improved.

[0021] Resin A may have any structure, such as a random copolymer, a graft copolymer, a block copolymer, a straight chain structure, or a branched structure.

[0022] The weight average molecular weight Mw of resin A measured by gel permeation chromatography (GPC) is preferably 5,000 to 500,000, more preferably 10,000 to 300,000, from the viewpoints of heat resistance, adhesion to polyolefin-based substrates, and storage stability of composite resin composition D. If it is equal to or greater than the lower limit, adhesion tends to improve. If it is equal to or less than the upper limit, storage stability of composite resin composition D tends to improve.

[0023] The glass transition temperature (Tg) of resin A is preferably 0°C or more and 150°C or less, more preferably 15°C or more and 100°C or less, and even more preferably 25°C or more and 80°C or less, from the viewpoints of heat resistance, adhesion to polyolefin-based substrates, and storage stability of composite resin composition D. If it is equal to or more than the lower limit, adhesion tends to be improved. If it is equal to or less than the upper limit, storage stability of composite resin composition D tends to be improved.

[0024] In this specification, the "glass transition temperature (Tg)" (unit: ° C.) is calculated by the Fox formula shown in the following formula (1).

[0025]

number

[0026] The symbols in formula (1) have the following meanings: Wi: mass fraction of monomer i Tgi: Tg of the homopolymer of monomer i (℃) For the Tg of a homopolymer, the value described in "Polymer Handbook, 4th Edition, John Wiley & Sons" can be used. For the Tg of a homopolymer not described in "Polymer Handbook, 4th Edition, John Wiley & Sons", the actual value measured by the method described in JIS standard K-7121-1987 "Method of measuring transition temperature of plastics" can be used.

[0027] Resin A and Resin C can be produced by commonly known polymerization methods such as bulk polymerization, solution polymerization, suspension polymerization, etc. Among these, suspension polymerization is preferred because it can give resins in the form of spherical particles that are easy to handle. Resin A and Resin C can be produced, for example, by the following suspension polymerization method.

[0028] The method for producing Resin A and Resin C preferably includes a polymerization step, a first dehydration step, a washing step, a second dehydration step, and a drying step.

[0029] (Polymerization process) The polymerization step is a step of obtaining resin A or resin C by suspension polymerization of monomer a and, if necessary, a monomer other than monomer a. As the suspension polymerization method, a known method can be adopted, and an example thereof includes a method in which monomer a and, if necessary, a monomer other than monomer a are polymerized in water in the presence of a polymerization auxiliary in a vessel having a polymerization temperature control function and a stirring function.

[0030] Examples of the polymerization aid include a polymerization initiator, a chain transfer agent, a dispersant, and a dispersion aid. Examples of the polymerization initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), benzoyl peroxide, and lauroyl peroxide. Examples of the chain transfer agent include t-dodecyl mercaptan, n-dodecyl mercaptan, octyl thioglycolate, and α-methylstyrene dimer. Examples of the dispersant include surfactants that stably disperse monomers in water, such as a copolymer of 2-sodium sulfoethyl methacrylate, potassium methacrylate, and methyl methacrylate, a copolymer of 3-sodium sulfopropyl methacrylate, and methyl methacrylate, a copolymer of sodium methacrylate and methacrylic acid, polyvinyl alcohol, polyvinylpyrrolidone, hydroxyethyl cellulose, and hydroxypropyl cellulose. Examples of the dispersion aid include sodium sulfate, sodium carbonate, sodium dihydrogen phosphate, disodium hydrogen phosphate, potassium chloride, calcium acetate, magnesium sulfate, and manganese sulfate.

[0031] Resins obtained by suspension polymerization (e.g., Resin A, Resin B, and Resin C) are obtained in the form of a slurry. By dehydrating the slurry, bead-like resin particles that are usually close to spherical are obtained.

[0032] (Dehydration process) The dehydration process includes a first dehydration process in which the slurry after the suspension polymerization is dehydrated using a dehydrator or the like to separate the resin (e.g., resin A, resin B, resin C) from the reaction liquid, and a second dehydration process in which the resin particles (e.g., resin A, resin B, resin C) after the washing process are dehydrated using a dehydrator or the like to separate the resin particles (e.g., resin A, resin B, resin C particles) from the washing liquid. Various dehydrators can be used in each dehydration step, and for example, a centrifugal dehydrator, a dehydrator with a mechanism for sucking and removing water on a porous belt, etc. can be appropriately selected and used. One dehydrator may be used, or two of the same model may be prepared and used in each dehydration step, or multiple different models of dehydrators may be used. A model that suits the purpose can be appropriately selected in terms of product quality, capital investment costs, productivity, operating costs, etc. When the balance between product quality and production speed is important, a dedicated dehydrator may be used for each dehydration step.

[0033] (Cleaning process) The washing step increases the purity of the resin (eg, Resin A, Resin B, Resin C). Examples of the resin washing method include a method of adding a washing liquid to the resin particles dehydrated in the first dehydration step to re-slurry the resin and stir and mix it, a method of performing a dehydration step in a dehydrator having a washing function, and then adding a washing liquid to wash the resin, etc. Also, these washing methods may be combined to wash the resin (e.g., resin A, resin B, and resin C).

[0034] The type and amount of the cleaning solution may be selected so as to achieve the purpose of the cleaning process. Examples of the cleaning agent include water (ion-exchanged water, distilled water, purified water, etc.), an aqueous solution in which a sodium salt is dissolved, and methanol.

[0035] (drying process) The drying step is a step of drying the particles of the resin (for example, resin A, resin B, or resin C) after the second dehydration step. Water remains on the surface of the resin particles after the second dehydration step. If the inside of the resin is close to being saturated with water, it is preferable to dry the resin in order to further reduce the water content of the resin. Various types of dryers can be used for drying, including dryers that heat and dry under reduced pressure, dryers that use heated air to air-transport resin particles through a pipe while simultaneously drying them, and dryers that blow heated air from below a porous plate to move the resin particles above while drying them.

[0036] Resin B has at least one constitutional unit derived from an olefin monomer b (hereinafter also referred to as "monomer b").

[0037] Resin B may have a reactive group. Examples of the reactive group include a carboxyl group, an epoxy group, an isocyanate group, a sulfonic acid group, a hydroxyl group, and an amino group. The reactive group may be an acid anhydride structure of a carboxyl group.

[0038] Examples of monomer b include ethylene, propylene, butene-1, pentene-1, hexene-1, heptene-1, octene-1, cyclopentene, cyclohexene, and norbornene.

[0039] Examples of resin B include a homopolymer of monomer b; Copolymers of ethylene and propylene; a copolymer of at least one of ethylene and propylene and a monomer copolymerizable with ethylene and propylene (e.g., an α-olefin having 4 or more carbon atoms (e.g., butene-1, pentene-1, hexene-1, heptene-1, octene-1, cyclopentene, cyclohexene, norbornene)); Copolymers of two or more α-olefins having 4 or more carbon atoms; Copolymers of α-olefins having two or more carbon atoms and aromatic monomers, or hydrogenated products thereof; Conjugated diene block copolymers and hydrogenated products thereof are included. The monomer b may be used alone or in combination of two or more kinds.

[0040] The mass ratio of the structural unit derived from the olefin monomer b to the total mass of the structural units constituting the resin B is preferably 50 mass% or more, more preferably 65 mass% or more, even more preferably 75 mass% or more, and is preferably 100 mass% or less. If it is less than the above lower limit, the adhesion to the polyolefin substrate tends to be improved.

[0041] From the viewpoint of adhesion to polyolefin-based substrates, resin B is preferably a polymer having a structural unit derived from propylene, more preferably polypropylene, ethylene-propylene copolymer, ethylene-propylene-butene copolymer, or propylene-butene copolymer, and even more preferably polypropylene or ethylene-propylene copolymer. The mass ratio of the propylene-derived structural unit in the polymer having the propylene-derived structural unit is preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 70 mass% or more, and is preferably 100 mass% or less. If it is less than the above lower limit, the adhesion to the polyolefin-based substrate tends to be improved.

[0042] Resin B may have any structure, such as a random copolymer, a graft copolymer, a block copolymer, a linear copolymer, or a branched copolymer.

[0043] The melting point (Tm) of resin B is preferably 125° C. or lower, more preferably 110° C. or lower, even more preferably 95° C. or lower, and preferably 50° C. or higher. If it is equal to or higher than the lower limit, the adhesion to the polyolefin-based substrate tends to be improved. If it is equal to or lower than the upper limit, the storage stability of the composite resin composition D tends to be improved. In this specification, the "melting point (Tm)" (unit: °C) is measured by differential scanning calorimetry (DSC).

[0044] The weight average molecular weight Mw of resin B measured by gel permeation chromatography (GPC) is preferably 3000 to 500000, more preferably 6000 to 200000, and even more preferably 10000 to 100000, from the viewpoint of heat resistance and adhesion to polyolefin-based substrates. If it is equal to or greater than the lower limit, the adhesiveness tends to improve. If it is equal to or less than the upper limit, the solvent solubility tends to improve.

[0045] There is no particular limitation on the method for producing resin B, but for example, it can be produced by polymerizing an olefin by radical polymerization, cationic polymerization, anionic polymerization, coordination polymerization, etc. Each of these polymerization methods may be a living polymerization method.

[0046] Examples of catalysts used in coordination polymerization include Ziegler-Natta catalysts and single-site catalysts. In general, single-site catalysts can have sharp molecular weight distributions and stereoregularity distributions by designing the ligands. Examples of single-site catalysts include metallocene catalysts and Brookhart-type catalysts. Metallocene catalysts include, for example, C1 symmetrical type, C2 symmetrical type, C2V symmetrical type, and CS symmetrical type, and can be appropriately selected depending on the stereoregularity of the desired polyolefin.

[0047] The polymerization method of the resin B is not particularly limited, and may be any method such as solution polymerization, suspension polymerization, bulk polymerization, gas phase polymerization, etc. In the case of solution polymerization or suspension polymerization, examples of the polymerization solvent include aromatic hydrocarbons such as toluene and xylene; aliphatic hydrocarbons such as hexane, heptane, and octane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; halogenated hydrocarbons; esters; ketones; and ethers. Aromatic hydrocarbons, aliphatic hydrocarbons, and alicyclic hydrocarbons are preferred, and toluene, xylene, heptane, and cyclohexane are more preferred. The polymerization solvent may be used alone or in combination of two or more kinds.

[0048] When resin B has a reactive group, examples of the production method include a method in which an olefin resin and a radical polymerizable monomer having a reactive group are reacted by heating and stirring in a solution, a method in which an olefin resin and a radical polymerizable monomer having a reactive group are reacted by melting, heating and stirring in the absence of a solvent, a method in which an olefin resin and a radical polymerizable monomer having a reactive group are reacted by heating and kneading in an extruder, and a production method in which a radical polymerizable monomer having a reactive group is graft polymerized onto an olefin resin. When produced in a solution, the polymerization solvents exemplified in the production method of resin B by solution polymerization or suspension polymerization can be used as the solvent.

[0049] When Resin B has a reactive group, the content of the reactive group per gram of Resin B is preferably 0.01 to 1 mmol / g, more preferably 0.05 to 0.5 mmol / g, and even more preferably 0.1 to 0.3 mmol / g.

[0050] Resin C can be produced by radically polymerizing a mixture of a monomer mixture containing monomer a and resin B in the presence of a radical polymerization initiator. In this production method, resin A may be produced at the same time by radically polymerizing only the monomer mixture containing monomer a. In other words, a composite resin composition D may be obtained, which is a three-type resin composition of resin A, unreacted resin B, and resin C. The composite resin composition D is preferably a resin composition of resin A, resin B, and resin C. When the composite resin composition D is a resin composition of resin A, resin B, and resin C, the mass ratios of resin A, resin B, and resin C in the composite resin composition D can be adjusted by adjusting the amounts of monomer a, which is the raw material for resin A, and resin B used in accordance with the desired physical properties of the composite resin composition D.

[0051] When the composite resin composition D contains the resin A, the mass ratio of the resin A in the composite resin composition D is preferably 45% by mass or more and 95% by mass or less, more preferably 55% by mass or more and 90% by mass or less. If it is equal to or more than the lower limit, the storage stability when dispersed in a solvent tends to be improved. If it is equal to or less than the upper limit, the adhesion to a polyolefin substrate tends to be improved.

[0052] When the composite resin composition D contains the resin B, the mass ratio of the resin B in the composite resin composition D is preferably 5% by mass or more and 55% by mass or less, more preferably 10% by mass or more and 45% by mass or less. If it is equal to or more than the lower limit, the adhesion to the polyolefin substrate tends to be improved. If it is equal to or less than the upper limit, the storage stability when dispersed in a solvent tends to be improved.

[0053] When the composite resin composition D contains resin A and resin B, the mass ratio of resin C in the composite resin composition D is preferably 0.001 mass% or more and 10 mass% or less, more preferably 0.01 mass% or more and 4 mass% or less, and even more preferably 0.05 mass% or more and 2 mass% or less. If it is equal to or more than the above lower limit, the storage stability when the composite resin composition D is dispersed in a solvent tends to be improved. If it is equal to or less than the above upper limit, the viscosity when the composite resin composition D is dispersed in a solvent tends to be reduced.

[0054] The mass ratios of resin A, resin B, and resin C contained in the composite resin composition D are 1 H-NMR and 13 It can be measured by a known method using C-NMR or the like.

[0055] The polymerization method for obtaining the resin C may be any known polymerization method, such as radical polymerization such as bulk polymerization, solution polymerization, suspension polymerization, or emulsion polymerization, anionic polymerization, group transfer polymerization (GTP), or coordination anionic polymerization. In view of ease of recovery of the resin, bulk polymerization and suspension polymerization are preferred, and in view of particle size control, suspension polymerization is more preferred.

[0056] Examples of methods for producing resin C by suspension polymerization include a method in which a mixture of a monomer mixture containing monomer a and resin B is added to water, a dispersant, a radical polymerization initiator, and optionally a chain transfer agent, etc., to form an aqueous suspension, which is then stirred to disperse the monomers into droplets of about 0.05 to 2.5 mm, and polymerization is allowed to proceed under heating. The polymerization temperature is preferably 0° C. or higher and 200° C. or lower, more preferably 20° C. or higher and 150° C. or lower, and even more preferably 50° C. or higher and 100° C. or lower. If the temperature is below the upper limit, the dispersion stability of the polymer tends to improve. If the temperature is above the lower limit, the solubility of the resin C in the solvent tends to improve.

[0057] The aqueous suspension of resin C can be produced, for example, by the following method. Method 1: Resin B is added to a monomer mixture containing monomer a, and the mixture is heated and stirred to form a mixture of resin B and a monomer mixture containing monomer a. A radical polymerization initiator, water, and a dispersant are then added and the mixture is stirred to polymerize. Method 2: A method in which a mixture of monomer a and monomers other than monomer a and resin B are added to water and heated and stirred to form a mixture of a monomer mixture containing monomer a and resin B, and then a radical polymerization initiator and a dispersant are added and stirred to polymerize.

[0058] As a method for adding the chain transfer agent, for example, in either method 1 or method 2, the chain transfer agent may be mixed in advance with the monomer mixture containing monomer a, or the chain transfer agent may be added to a mixture of the monomer mixture containing monomer a and resin B.

[0059] Examples of the radical polymerization initiator used in producing the aqueous suspension of resin C include organic peroxides and azo compounds, with organic peroxides being preferred. The radical polymerization initiator may be used alone or in combination of two or more kinds.

[0060] Examples of organic peroxides used as radical polymerization initiators include o-methylbenzoyl peroxide, bis-3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, cyclohexanone peroxide, benzoyl peroxide, methyl ethyl ketone peroxide, dicumyl peroxide, lauroyl peroxide, diisopropylbenzene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, t-hexylperoxy-2-ethylhexanoate, t-butyl peroxypivalate, t-butyl peroxyneoheptanoate, t-butyl peroxyneodecanoate, and t-butyl peroxyneodecanoate. Examples of peroxyalkylene oxides include t-butylperoxy-2-ethylhexanoate, t-butylperoxylaurate, t-butylperoxyacetate, t-butylperoxyisobutyrate, t-butylperoxyisononanoate, t-butylperoxybenzoate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxymaleic acid, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, di-t-butylperoxyhexahydroterephthalate, 1,6-di-(t-butylperoxycarbonyloxy)hexane, t-butylperoxyisonanoate, t-butylperoxyisopropyl carbonate, and t-butylperoxy 2-ethylhexyl carbonate.

[0061] Examples of the azo compound used as the radical polymerization initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile).

[0062] From the viewpoint of high hydrogen abstraction ability, t-butyl peroxypivalate, t-butyl peroxyneoheptanoate, t-butyl peroxyneodecanoate, t-butyl peroxy-2-ethylhexanoate, t-butyl peroxylaurate, t-butyl peroxyacetate, t-butyl peroxyisobutyrate, t-butyl peroxyisononanoate, t-butyl peroxybenzoate, t-butyl peroxy-3,5,5-trimethylhexanoate, t-butyl peroxymaleic acid, t-butyl peroxyisopropyl monocarbonate, t-butyl peroxy-2-ethylhexyl monocarbonate, di-t-butyl peroxyhexahydroterephthalate, 1,6-di-(t-butylperoxycarbonyloxy)hexane, t-butyl peroxyisonanoate, t-butyl peroxyisopropyl carbonate, and t-butyl peroxy 2-ethylhexyl carbonate are preferred.

[0063] From the viewpoint of reactivity in suspension polymerization, t-butylperoxy-2-ethylhexanoate, t-butylperoxylaurate, t-butylperoxyisobutyrate, di-t-butylperoxyhexahydroterephthalate, and 1,6-di-(t-butylperoxycarbonyloxy)hexane are more preferred.

[0064] The amount of the radical polymerization initiator used is preferably 0.0001 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, and even more preferably 0.1 to 2 parts by mass, relative to 100 parts by mass of the total of the monomer mixture containing the monomer a and the resin B. If the amount is equal to or more than the lower limit, the adhesiveness tends to be improved. If the amount is equal to or less than the upper limit, the solvent solubility tends to be improved.

[0065] The hydrogen abstraction ability refers to an index showing the ease with which a hydrogen abstraction reaction occurs, which is one of the reactions involving radical species generated from an organic peroxide. The hydrogen abstraction ability of the organic peroxide can be measured by the methods described in various literature (for example, Polymer Journal, 29, 366 (1997), Polymer Journal, 29, 940 (1997), Polymer Journal, 29, 733 (1997)).

[0066] In general, in the polymerization of vinyl monomers using organic peroxides with high hydrogen abstraction ability, the polymerization reaction of vinyl monomers is likely to occur in which the radical species generated undergoes an addition reaction to vinyl monomers. Therefore, by carrying out radical polymerization of a mixture of monomers containing monomer a and resin B in the presence of a radical polymerization initiator with high hydrogen abstraction ability, resin C having a constitutional unit derived from monomer a and a structure derived from resin B can be efficiently obtained. In addition, in the polymerization of vinyl monomers using organic peroxides with high hydrogen abstraction ability, the polymerization reaction of vinyl monomers is caused by the radical species generated undergoing an addition reaction to vinyl monomers, and also by the polymerization reaction of vinyl monomers due to hydrogen abstraction from substances that easily give hydrogen, such as solvents and additives. From the viewpoint of the reactivity of the polymerization reaction, bulk polymerization and suspension polymerization that do not contain a solvent are preferred, and suspension polymerization is more preferred from the viewpoint of particle size control.

[0067] Examples of chain transfer agents used in the production of the aqueous suspension of Resin C include hydrogen, mercaptans, α-methylstyrene dimer, terpenoids, and cobalt chain transfer agents. The chain transfer agent may be used alone or in combination of two or more kinds.

[0068] Examples of the chain transfer agent include n-octyl mercaptan, n-dodecyl mercaptan, tert-dodecyl mercaptan, n-octyl mercaptan, n-tetradecyl mercaptan, n-hexyl mercaptan, and 2-ethylhexyl thioglycolate.

[0069] The amount of the chain transfer agent used is preferably 0.01 parts by mass or more and 10 parts by mass or less, more preferably 0.05 parts by mass or more and 5 parts by mass or less, and even more preferably 0.1 parts by mass or more and 2 parts by mass or less, relative to 100 parts by mass of the total of the mixture of monomers containing monomer a and resin B. If the amount is more than the lower limit, the solubility in the solvent tends to improve. If the amount is less than the upper limit, the adhesion to the polyolefin substrate tends to improve.

[0070] Examples of dispersants used in producing an aqueous suspension of resin C include poly(meth)acrylic acid metal salts, alkali metal salts of copolymers of (meth)acrylic acid and methyl (meth)acrylate, polyvinyl alcohol having a saponification degree of 70 to 100%, and methyl cellulose. From the viewpoint of dispersibility, alkali metal salts of copolymers of (meth)acrylic acid and methyl (meth)acrylate and polyvinyl alcohol are preferred, and alkali metal salts of copolymers of (meth)acrylic acid and methyl (meth)acrylate are more preferred. The dispersing agent may be used alone or in combination of two or more kinds.

[0071] The amount of the dispersant used is preferably 0.001 to 10 mass%, more preferably 0.005 to 5 mass%, and even more preferably 0.01 to 2 mass%, based on 100 parts by mass of the total of the monomer mixture containing monomer a and resin B. If the amount is equal to or greater than the lower limit, the dispersibility during suspension polymerization tends to be good. If the amount is equal to or less than the upper limit, the solubility in the solvent tends to be improved.

[0072] An electrolyte such as sodium carbonate, sodium sulfate, or sodium hydrogen carbonate may be used for the purpose of improving the dispersion stability of the aqueous suspension of resin C during suspension polymerization. Examples of the method for adding an electrolyte when using one include the above-mentioned method 1 and method 2, a method in which the electrolyte is dissolved in water in advance and used for polymerization, and a method in which the electrolyte is added in a solid state together with water to the monomer solution and used for polymerization.

[0073] As a method for obtaining the composite resin composition D, the same method as the method for obtaining the resin C can be used. A method for producing a composite resin composition D containing an acrylic olefin resin C having a structural unit derived from a monomer a and a structure derived from a resin B, the method for producing the composite resin composition D by suspension polymerization of the monomer a in the presence of the resin B, can be the same as the method for producing the resin C. As the monomer a and resin B that can be used in the production of the composite resin composition D, the monomer a and resin B used in the production method for obtaining the composite resin C can be used.

[0074] The mass average particle size of the composite resin composition D of the present invention is preferably 10 μm or more and 2500 μm or less, more preferably 100 μm or more and 2000 μm or less, and even more preferably 150 μm or more and 1500 μm or less. If it is equal to or more than the lower limit, the adhesion area between the resins is reduced, so that the resins are less likely to fuse together, and the storage stability of the composite resin composition D is improved. If it is equal to or less than the upper limit, the solvent solubility of the composite resin composition D is improved. The mass-average particle size can be calculated by using a standard sieve to shake and classify 20 g of granular resin for 5 minutes.

[0075] In the composite resin composition D, the mass ratio of the total mass of the constituent units derived from all monomers constituting the resin B to the total mass of the constituent units derived from the monomer a is preferably 1 to 100%, more preferably 6 to 90%, and even more preferably 20 to 80%. If it is equal to or greater than the lower limit, the adhesion to the polyolefin substrate tends to be improved. If it is equal to or less than the upper limit, the storage stability of the composite resin composition D tends to be improved.

[0076] The water content of the composite resin composition D is 0.01% or more and 10% or less, preferably 0.05% or more and 5% or less, and more preferably 0.1% or more and 3% or less. If it is less than the upper limit, the adhesion to the polyolefin substrate is improved. If it is more than the lower limit, the composite granular resin is less likely to be charged, and the risk of dust explosion is reduced. Examples of methods for adjusting the moisture content of the composite resin composition D include a method of adjusting drying conditions such as the degree of vacuum, drying temperature, and drying time when drying the composite resin composition D, and a method of adding a moisture regulator such as a dehydrating agent to the composite resin composition D.

[0077] Examples of dehydrating agents used in the method for adjusting the water content of the composite resin composition D include inorganic compounds such as anhydrous sodium sulfate, anhydrous magnesium sulfate, and phosphorus pentoxide; and organic compounds having a carboxylic acid anhydride group, such as maleic anhydride modified resins. The method of adding a moisture regulator such as a dehydrating agent to the composite resin composition D has the following problems: it reduces the active ingredient concentration of the composite resin composition D, thereby reducing the effects obtained by the present invention; it requires a complicated operation of separating and purifying the moisture regulator such as a dehydrating agent; and if the composite resin composition D is stored, the moisture content may be reduced too much below the lower limit over time, increasing the risk of a dust explosion. Therefore, a method of adjusting the drying conditions, such as the degree of vacuum, drying temperature, and drying time, when drying the composite resin composition D is simple and preferable as a method of adjusting the moisture content of the composite resin composition D.

[0078] The non-aqueous resin composition E of the present invention (hereinafter also referred to as “composition E”) contains the composite resin composition D of the present invention. When composition E contains composite resin composition D of the present invention, the dispersibility of composition E is improved, and the storage stability of composition E becomes good. It is preferable that the composition E further contains an organic solvent. When the composition E contains an organic solvent, the composition E may be in a state where the composite resin composition D is completely dissolved in the organic solvent, or in a state where the composite resin composition D is partially dissolved and dispersed in the organic solvent.

[0079] The organic solvent may be any organic solvent capable of dissolving a part or the whole of the composite resin composition D.

[0080] Examples of the organic solvent include aromatic hydrocarbons such as xylene (solubility parameter (SP value): 8.8) and toluene (SP value: 8.9); Alicyclic hydrocarbons such as methylcyclocyclohexane (SP value: 7.8) and cyclohexane (SP value: 8.2); Ketones such as acetone (SP value: 9.9), methyl ethyl ketone (SP value: 9.3), methyl propyl ketone (SP value: 8.7), and methyl isobutyl ketone (SP value: 8.4); Esters such as ethyl acetate (SP value: 9.1), n-propyl acetate (SP value: 8.8), n-butyl acetate (SP value: 8.5), i-propyl acetate (SP value: 8.4), and i-butyl acetate (SP value: 8.3); Alcohols such as methanol (SP value: 14.5), ethanol (SP value: 12.7), n-butanol (SP value: 11.4), cyclohexanol (SP value: 11.4), n-propyl alcohol (SP value: 12.0), isopropyl alcohol (SP value: 11.5), n-butanol (SP value: 11.4), i-butanol (SP value: 11.1), t-butanol (SP value: 10.6), and n-hexanol (SP value: 10.7); Glycols such as ethylene glycol (SP value: 14.6) and propylene glycol (SP value: 12.6); glycol esters such as ethylene glycol monomethyl ether acetate (SP value: 9.2), propylene glycol monomethyl ether acetate (SP value: 8.2), diethylene glycol monobutyl ether acetate (SP value: 8.5), and diethylene glycol monoethyl ether acetate (SP value: 8.5); Glycol ethers such as diethylene glycol monomethyl ether (SP value: 10.2), diethylene glycol monoethyl ether (SP value: 10.2), diethylene glycol monobutyl ether (SP value: 9.5), and propylene glycol monomethyl ether (SP value: 10.1); Hydrocarbons such as n-octane (SP value: 7.6), i-octane (SP value: 7.5), n-heptane (SP value: 7.4), n-hexane (SP value: 7.3), n-pentane (SP value: 7.0), and Isopar E (manufactured by Exxon Chemical Co., Ltd.); Ethers such as tetrahydrofuran (SP value: 9.1) and diethyl ether (SP value: 7.4) are included. From the viewpoint of the solubility of the composite resin composition D, the organic solvent preferably contains both an organic solvent having an SP value of 8.0 or less and an organic solvent having an SP value of 9.2 or more. As the organic solvent having an SP value of 8.0 or less, a compound having a cycloalkane structure is preferable, and as the organic solvent having an SP value of 9.2 or more, a ketone-based solvent is preferable.

[0081] In this specification, the "solubility parameter (SP value)" is expressed in units of (cal / cm 3 ) 1 / 2 The solubility parameter is expressed by the following formula: and can be determined by the Fedors method described in Polymer Engineering and Science, Vol. 14, 147 (1974).

[0082] The content ratio of the organic solvent having an SP value of 8.0 or less to the total mass of all organic solvents is preferably 5% by mass or more and 80% by mass or less, more preferably 20% by mass or more and 72% by mass or less, and even more preferably 25% by mass or more and 65% by mass or less. If it is more than the lower limit, the adhesion to the polyolefin substrate tends to be improved. If it is less than the upper limit, the storage stability of composition E tends to be improved. The content ratio of the organic solvent having an SP value of 9.2 or more to the total mass of all organic solvents is preferably 10% by mass or more and 70% by mass or less, more preferably 15% by mass or more and 60% by mass or less, and even more preferably 25% by mass or more and 40% by mass or less. If it is equal to or more than the lower limit, the storage stability of composition E tends to improve. If it is equal to or less than the upper limit, the adhesion to polyolefin substrates tends to improve.

[0083] The composition E can be produced, for example, by the following method. Method 3: A method of stirring a mixture of the composite resin composition D and an organic solvent. Method 4: A method in which a part or all of composite resin composition D is mixed with an organic solvent containing 50 mass% or more of an organic solvent having an SP value of less than 9.2, and then the mixed liquid of composite resin composition D is allowed to coexist with an organic solvent having an SP value of 9.2 or more. Method 4 is preferred because composition E is less likely to separate after dissolution or dispersion and composition E has good storage stability. The composition E may be produced at room temperature or at elevated temperature.

[0084] In method 4, the combination of organic solvents used when mixing a part or all of the composite resin composition D in the presence of an organic solvent containing 50 mass% or more of an organic solvent having an SP value of less than 9.2 preferably contains at least one organic solvent having an SP value of 8.0 or less. The ratio of the organic solvent having an SP value of 8.0 or less to the organic solvent used when mixing a part or all of the composite resin composition D is preferably 25 mass% or more and 100 mass% or less, more preferably 35 mass% or more and 95 mass% or less, and even more preferably 45 mass% or more and 90 mass% or less. If it is equal to or more than the lower limit, the adhesion to the polyolefin substrate tends to be improved. If it is equal to or less than the upper limit, the storage stability of the composition E tends to be improved.

[0085] In method 4, the content of the organic solvent having an SP value of 9.2 or more is preferably 10% by mass or more and 70% by mass or less, more preferably 15% by mass or more and 60% by mass or less, and even more preferably 25% by mass or more and 40% by mass or less, based on the total mass of all organic solvents. If it is equal to or more than the lower limit, the storage stability of composition E tends to be improved. If it is equal to or less than the upper limit, the adhesion to polyolefin substrates tends to be improved.

[0086] In methods 3 and 4, the organic solvent having an SP value of less than 9.2 preferably contains at least one of the above-mentioned hydrocarbons and alicyclic hydrocarbons, and at least one of an ester and a ketone, from the viewpoint of making composition E less susceptible to separation, more preferably contains an alicyclic hydrocarbon and either an ester or a ketone, even more preferably contains an alicyclic hydrocarbon and an ester, and particularly preferably contains a compound having a cycloalkane structure and an ester.

[0087] In Method 3 and Method 4, the organic solvent having an SP value of 8.0 or less is preferably the above-mentioned hydrocarbon or alicyclic hydrocarbon, more preferably a compound having a cycloalkane structure, and further preferably methylcyclohexane.

[0088] In methods 3 and 4, the organic solvent having an SP value of 9.2 or more is preferably the above-mentioned ketone, alcohol, or glycol, more preferably ketone, and further preferably acetone or methyl ethyl ketone.

[0089] Composition E of the present invention may contain other resins in addition to resin A, resin B and resin C, as long as the adhesion to the substrate is not impaired. Examples of other resins include polyaromatic vinyl compounds such as polystyrene; polyester resins; polyurethane resins; alkyd resins; epoxy resins; cellulose-based resins such as nitrocellulose, cellulose acetate butyrate, cellulose acetate propionate, and cellulose acetate; and vinyl chloride / vinyl acetate copolymer-based resins such as vinyl chloride resins, vinyl chloride / vinyl acetate copolymer resins, and vinyl acetate resins.

[0090] To composition E of the present invention, various additives can be added, as necessary, by a general blending method, such as, for example, electrical conductivity imparting agents such as carbon black and ferrite; inorganic fillers; lubricants; plasticizers; organic peroxides; lubricating agents such as aluminum paste and mica; antioxidants; ultraviolet absorbers; agents for imparting weather resistance; agents for imparting radiation resistance; agents for imparting thermal stability; surface conditioners; crosslinking agents; curing catalysts; pigment sedimentation prevention agents; and silane coupling agents.

[0091] The composite resin compositions D and E of the present invention have excellent adhesion to the surface of a substrate made of a polyolefin resin, which was difficult to adhere to using conventional techniques. Examples of substrates made of polyolefin-based resins include films such as polyethylene film (PE), unoriented polypropylene film (CPP), oriented polypropylene film (OPP), ethylene-vinyl acetate copolymer film (EVA), ethylene-vinyl alcohol copolymer film (EVOH), polyvinyl chloride film (PVC), and the like; and molded articles for automobile parts and molded articles for home appliances made of polyolefins such as high-pressure polyethylene, medium-low pressure polyethylene, polypropylene, and poly-4-methyl-1-pentene, or polyolefin-based resins such as ethylene-propylene copolymers, ethylene-butene copolymers, and propylene-butene copolymers. The composite resin composition D and the composition E of the present invention have excellent adhesion to substrates other than the substrates made of the polyolefin-based resins described above, such as plastic films such as polyethylene terephthalate film (PET), amorphous polyethylene terephthalate film (A-PET), polycarbonate film, polybutylene terephthalate (PBT)-based resin film, non-oriented nylon film, biaxially oriented nylon film, polyvinylidene chloride film, polyvinyl alcohol film, and polystyrene film; polymer substrates such as acrylic resins such as polymethyl methacrylate and copolymers having structural units derived from methyl methacrylate, polyester resins, resin alloys made of polypropylene and synthetic rubber, polyamide resins, unsaturated polyester resins, polybutylene terephthalate resins, polycarbonate resins, and polystyrene resins; metal substrates such as untreated steel plates and steel plates plated with zinc or aluminum oxide films; and non-ferrous metal substrates such as copper plates, aluminum plates, aluminum foils, aluminum alloy plates, and titanium plates.

[0092] The substrate to be printed with the composite resin composition D and composition E of the present invention may be a substrate molded by any known molding method such as injection molding, compression molding, blow molding, extrusion molding, rotational molding, etc., or may be a substrate that has been subjected to a surface treatment for improving adhesion such as corona treatment, plasma treatment, undercoat treatment, primer coat treatment, etc. In addition, a pigment may be blended into the substrate, or a metal or the like may be vapor-deposited on the substrate surface. Examples of substrates having a metal or the like vapor-deposited on the substrate surface include films having metals such as aluminum, gold, silver, copper, nickel, zinc, titanium, cobalt, indium, and chromium vapor-deposited on the substrate surface; and films having aluminum oxide and silicon oxide vapor-deposited on the substrate surface.

[0093] The adhesive composition of the present invention contains at least one of the composite resin composition D and the composition E of the present invention.

[0094] Applications of the adhesive composition include, for example, hot melt adhesives and heat seal adhesives.

[0095] Heat seal adhesives are adhesives used to hermetically seal packaging containers for food, medicines, industrial products, daily necessities, cosmetics, etc., with lids, and are used on various plastic films, vapor-deposited films, aluminum foil, paper, nonwoven fabrics, glass, etc. as packaging containers and lids. The aluminum foil may be a single layer of aluminum foil, may be an aluminum foil having a primer layer (e.g., a resin layer containing a vinyl chloride-vinyl acetate copolymer), or may be a laminate containing an aluminum foil and a sealant film (e.g., a laminate having an aluminum foil, an adhesive layer, and a sealant film in this order). When a laminate containing an aluminum foil and a sealant film is used as a lid material, the adhesive composition of the present invention is preferably used as an adhesive layer interposed between the sealant film and the container.

[0096] Examples of methods for applying the adhesive composition include a bar coater method, a gravure coating method, a roll coating method, a knife coating method, and a kiss coating method. After the adhesive composition is applied to the substrate, it may be dried by heating. For example, when the adhesive composition is applied to aluminum foil, the drying conditions are preferably within the range of 100 to 200° C. for 5 to 1000 seconds. The thickness of the adhesive composition after heat drying is appropriately set depending on the lid material and container to be adhered, and is preferably 0.1 to 40 μm, more preferably 1 to 20 μm, and even more preferably 3 to 15 μm.

[0097] The coating composition of the present invention contains at least one of the composite resin composition D and the composition E of the present invention.

[0098] Examples of the coating method for applying the coating composition include spray coating, brush coating, dip coating, roll coating, and flow coating. The temperature and time for drying the applied coating composition can be appropriately selected depending on the type and content of the solvent in the coating composition, specifically, the evaporation rate of the solvent and the drying conditions. From the viewpoint of the heat resistance of the substrate, the drying temperature is preferably room temperature to 200°C. From the viewpoint of the heat resistance of the substrate, the drying temperature is preferably equal to or lower than the heat resistance temperature of the substrate. From the viewpoint of the drying property of the coating composition, the drying time is preferably 1 minute or more, more preferably 30 minutes or more, and is preferably 24 hours or less.

[0099] The ink composition of the present invention contains at least one of composite resin composition D and composition E.

[0100] The hues of colorants that can be used in the ink composition include, for example, five process basic colors, including white, yellow, red, indigo, and black; three process gamut colors, including red (orange), grass (green), and purple; transparent yellow, peony, vermilion, brown, gold, silver, and pearl; and a nearly transparent medium (containing an extender pigment as necessary) for adjusting color density as base colors. The ink composition can be mixed with a white colorant to form a white ink, and other inks can be mixed with the ink. In addition, organic pigments, inorganic pigments, and dyes can be mixed as necessary.

[0101] Among inorganic pigments, examples of white inorganic pigments include titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, and silica. Titanium oxide is preferably used as a pigment for white ink in terms of coloring power, hiding power, chemical resistance, and weather resistance. Examples of inorganic pigments other than white pigments include pigments such as carbon black, aluminum, and mica.

[0102] Among the colorants, examples of colored colorants include organic pigments, inorganic pigments, and dyes used in general inks, paints, and recording materials. Examples of organic pigments that can be used in combination with the ink composition include azo-based, phthalocyanine-based, anthraquinone-based, perylene-based, perinone-based, quinacridone-based, thioindigo-based, dioxazine-based, isoindolinone-based, quinophthalone-based, azomethine azo-based, dictopyrrolopyrrole-based, and isoindoline-based pigments. From the standpoint of cost and light resistance, it is preferable to use copper phthalocyanine for indigo ink and CI Pigment No. Yellow 83 for transparent yellow ink as the organic pigment.

[0103] In order to ensure coloring power, the content of the colorant in the ink composition is preferably 1 to 50% by mass based on the total mass of the ink composition. The colorants may be used alone or in combination of two or more.

[0104] It is preferable to use a dispersant in combination with the colorant in order to stably disperse the colorant in the ink composition. As the dispersant, anionic, nonionic, cationic, amphoteric or other surfactants can be used.

[0105] From the viewpoint of storage stability and printability of the ink, the content of the dispersant in the ink composition is preferably 0.05% by mass or more and 5% by mass or less, and more preferably 0.1% by mass or more and 2% by mass or less, based on the total mass of the ink composition. The dispersants may be used alone or in combination of two or more.

[0106] The printing ink composition containing the ink composition of the present invention can be used in general printing methods such as gravure printing, flexographic printing, etc. In addition, the printing ink composition can be used at a viscosity and concentration suitable for various printing methods.

[0107] The acrylic olefin composite resin composition D of the present invention can also be used for a film or a molding material. Examples of applications of the film or the molding material include automobile parts, home appliance parts, medical parts, construction parts, and packaging materials.

[0108] The molding material may contain additives, such as ultraviolet absorbers, antioxidants, weather resistance agents, plasticizers, lubricants, antistatic agents, colorants, pigments, flame retardants, and dispersants, which are commonly used in the field of resin compositions, as necessary. Examples of the molding method for the molding material include injection molding, blow molding, vacuum / pressure molding, T-die extrusion molding, profile extrusion molding, calendar molding, and inflation molding. In view of good moldability and high productivity, injection molding is preferred. EXAMPLES

[0109] EXAMPLES The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0110] <Measurement of weight average molecular weight (Mw)> To measure the weight average molecular weight, a Tosoh high-speed GPC device HLC-8320GPC type (detector: RI detector) was used. As columns, two Tosoh TSKgel superHZM-M (4.6 mm ID x 15 cmL) and one Tosoh TSKgel HZ2000 (4.6 mm ID x 15 cmL) were connected and used. Tetrahydrofuran (containing dibutylhydroxytoluene as a stabilizer) was used as the eluent, the flow rate was 0.35 mL / min, the injection port temperature was 40°C, the oven temperature was 40°C, and the RI detector temperature was 40°C. As a sample, 10 μL of a resin concentration adjusted with tetrahydrofuran to 0.2 mass% was injected.

[0111] <Measurement of mass average particle size> The mass-average particle size was measured by shaking 20 g of the granular resin using a standard sieve for 5 minutes to classify it.

[0112] <Moisture content measurement> The moisture content of the granular resin immediately after drying at 105° C. for 2 hours was set to 0%, and the moisture content was calculated from the loss in the mass of the acrylic resin before and after drying.

[0113] <Synthesis of dispersant (1)> In a polymerization apparatus equipped with a stirrer, a cooling tube, and a thermometer, 900 parts by mass of deionized water, 60 parts by mass of sodium 2-sulfoethyl methacrylate, 10 parts by mass of potassium methacrylate, and 12 parts by mass of methyl methacrylate (MMA) were added and stirred, and the polymerization temperature was raised to 50°C while replacing the inside of the polymerization apparatus with nitrogen. 0.08 parts by mass of 2,2'-azobis(2-methylpropionamidine) dihydrochloride was added to the obtained mixture as a polymerization initiator, and the polymerization temperature was raised to 60°C. At the same time as the addition of the polymerization initiator, a dropping pump was used to continuously drop MMA at a rate of 0.24 parts by mass / min for 75 minutes to add a total of 18 parts by mass. The obtained mixture was kept at a polymerization temperature of 60°C for 6 hours, and then cooled to room temperature to obtain a dispersant (1). The solid content concentration of the dispersant (1) was 10% by mass.

[0114] <Synthesis of acrylic olefin composite resin C> (Synthesis Examples 1 to 7, 9 to 12: Synthesis of Resins 1 to 7, 9 to 12) In a polymerization apparatus equipped with a stirrer, a cooling tube, and a thermometer, 200 parts by mass of deionized water and 0.10 parts by mass of sodium sulfate (Na2SO4) were added and stirred to obtain a uniform aqueous solution. The obtained aqueous solution was added with the amounts of (meth)acrylic monomer a, chain transfer agent, and olefin resin B shown in Table 1, and the mixture was heated to 70°C and held for 1 hour to dissolve the olefin resin B in the (meth)acrylic monomer a. 0.50 parts by mass of dispersant (1) was added to the obtained mixture to obtain a dispersion, which was then cooled to 30°C. After cooling, the amount of radical polymerization initiator shown in Table 1 was added, the inside of the polymerization apparatus was fully replaced with nitrogen, the dispersion was heated to 80°C and held for 2 hours, and then further heated to 90°C and held for 1 hour. The reaction liquid was cooled to 40°C to obtain a suspension containing a granular resin. The obtained suspension was filtered through a filter cloth, and the filtrate was washed with deionized water, dehydrated, and dried at 40°C for 16 hours to obtain an acrylic olefin composite resin composition D (resins 1 to 7, 9, 10, and 12) containing a particulate acrylic olefin composite resin C having a structural unit derived from a (meth)acrylic monomer a and a structure derived from an olefin resin B. After drying, deionized water was added to obtain a particulate acrylic olefin composite resin D (resin 11) containing a particulate acrylic olefin composite resin C having a structural unit derived from a (meth)acrylic monomer a and a structure derived from an olefin resin B. Table 1 shows the weight average molecular weight, average particle size, and water content of the acrylic olefin composite resin D (resins 1 to 7 and 9 to 12).

[0115] <Synthesis of acrylic resin A> (Synthesis Example 8: Synthesis of Resin 8) In a polymerization apparatus equipped with a stirrer, a cooling tube, and a thermometer, 145 parts by mass of deionized water, 0.10 parts by mass of sodium sulfate (Na2SO4), and 0.25 parts by mass of dispersant (1) were added and stirred to obtain a uniform aqueous solution. The (meth)acrylic monomer a, chain transfer agent, and radical polymerization initiator shown in Table 1 were added to the obtained aqueous solution to obtain a dispersion. The atmosphere inside the polymerization apparatus was sufficiently replaced with nitrogen, and the obtained dispersion was heated to 80°C while continuing stirring, and then held for 2 hours, and further heated to 90°C and held for 1 hour to obtain a suspension containing a granular resin. The obtained suspension was filtered through a filter cloth, and the filtrate was washed with deionized water, dehydrated, and dried at 40°C for 16 hours to obtain a particulate acrylic resin A (resin 8). The weight average molecular weight, mass average particle size, and water content of the acrylic resin A (resin 8) are shown in Table 1.

[0116] The numerical values ​​for each component in Table 1 indicate parts by mass.

[0117] [Table 1]

[0118] The abbreviations listed in Table 1 are as follows. MMA: Methyl methacrylate (Mitsubishi Chemical Corporation, Acryester M) nBMA: n-butyl methacrylate (manufactured by Mitsubishi Chemical Corporation, Acryester B) MAA: Methacrylic acid (Mitsubishi Chemical Corporation, methacrylic acid) PBO: t-butyl peroxy-2-ethylhexanoate (Perbutyl O, manufactured by Nippon Oil & Fats Co., Ltd.) PHO: t-Hexylperoxy-2-ethylhexanoate (Perhexyl O, manufactured by Nippon Oil & Fats Co., Ltd.) MSD: α-methylstyrene dimer (Nofumer MSD, manufactured by Nippon Oil & Fats Co., Ltd.) nDM: n-dodecyl mercaptan (Kanto Chemical Co., Ltd., 1-dodecanethiol) PP1602: Ethylene-propylene copolymer resin (CLARIANT, LICOCENE PP1602) PP2602: Ethylene-propylene copolymer resin (CLARIANT, LICOCENE PP2602) PP3602: Ethylene-propylene copolymer resin (CLARIANT, LICOCENE PP3602) S600: Polypropylene (Idemitsu Kosan Co., Ltd., L-MODU S600) S400: Polypropylene (Idemitsu Kosan Co., Ltd., L-MODU S400)

[0119] <Examples 1 to 20 and Comparative Examples 1 to 3> The storage stability and adhesion to polyolefin substrates of the resin compositions were evaluated according to the following methods. The results are shown in Tables 2 and 3.

[0120] <Evaluation of storage stability of resin composition> The resin and initial solvent in the amounts shown in Tables 2-3 were added to a 200 mL flask equipped with a stirrer, a cooling tube, and a thermometer, and stirred at 25°C. After confirming that the enlarged particles had disappeared from the obtained blended liquid, additional solvent A or additional solvent B in which the resin had been dissolved was added and stirred at 25°C for 10 minutes. Thereafter, the stirring was stopped, and it was confirmed whether the initial appearance of the composition was in a dispersed state or a transparent state, and the mixture was allowed to stand for 24 hours. The appearance of the reaction solution in the obtained flask after 24 hours was visually evaluated according to the following evaluation criteria. (Evaluation Criteria) A: No change B: Low fluidity, but no two-layer separation, no practical problem C: No two-layer separation, but poor fluidity and unusable level D: Both separated into two fluid layers and had poor storage stability. E: Separation into two layers, one of which is non-fluid, and poor storage stability.

[0121] <Evaluation of adhesion to polyolefin substrate> (Examples 1 to 18) A 20% methyl ethyl ketone resin solution of vinyl chloride vinyl acetate copolymer (VINNOL H15 / 45M, manufactured by WACKER Co., Ltd.) was applied to a hard aluminum foil (A1N30H-H18, manufactured by Takeuchi Metal Foil Co., Ltd.) using a bar coater so that the thickness after drying would be 1 μm, and the surface of the hard aluminum foil was primer-treated by drying for 1 minute at 80°C. The resin solution immediately after the preparation for the evaluation of solubility in solvents was applied to the primer surface of the hard aluminum foil using a bar coater so that the thickness after drying would be 5 μm, and then dried for 3 minutes at 180°C. A CPP film (Super Foil E0025NA, manufactured by Mitsubishi Chemical Co., Ltd.) was placed on the coated surface, and a heat seal tester (TP-701, manufactured by Tester Sangyo Co., Ltd.) was used to measure the thickness at 180°C and 0.5 kgf / cm. 2 The sealed area was cut out to a width of 15 mm and pulled in a 180° direction at a speed of 250 mm / min using a tensile tester (Shimadzu Corporation, small tabletop tester EZ) to measure the peel strength (unit: N / 15 mm) and evaluate it according to the following criteria.

[0122] (Examples 19 and 20) The resin solution prepared for the evaluation of solubility in solvents was applied to a hard aluminum foil (Takeuchi Metal Foil Co., Ltd., A1N30H-H18) using a bar coater so that the thickness after drying would be 5 μm, and then dried at 180°C for 3 minutes. A CPP film (Mitsubishi Chemical Co., Ltd., Super Foil E0025NA) was placed on the coated surface, and the film was tested at 180°C and 0.5 kgf / cm using a heat seal tester (Tester Sangyo Co., Ltd., TP-701). 2 The sealed area was cut out to a width of 15 mm and pulled in a 180° direction at a speed of 250 mm / min using a tensile tester (Shimadzu Corporation, small tabletop tester EZ) to measure the peel strength (unit: N / 15 mm) and evaluate it according to the following criteria.

[0123] (Evaluation Criteria) A: 8 or more B: 5 or more and less than 8 C: 1 or more and less than 5 D: Less than 1

[0124] The numerical values ​​for each component in Tables 2 and 3 indicate parts by mass.

[0125] [Table 2]

[0126] [Table 3]

[0127] As shown in Tables 2 to 3, Examples 1 to 20 used composite resin composition D containing resin C having a structural unit derived from monomer a and a structure derived from resin B and having a moisture content of 0.01% or more and 10% or less, and therefore had excellent storage stability and adhesion to polyolefin substrates.

[0128] On the other hand, Comparative Example 1, which used resin A but not composite resin composition D, which contains resin C having a structural unit derived from monomer a and a structure derived from resin B and has a moisture content of 0.01% or more and 10% or less, had poor adhesion to polyolefin substrates.

[0129] Comparative Example 2, in which resin A and resin B were mixed, was poor in solubility in solvents and adhesion to olefin substrates.

[0130] Comparative Example 3, which used an acrylic olefin composite resin composition containing resin C having a structural unit derived from monomer a and a structure derived from resin B but having a moisture content outside the range of 0.01% to 10%, separated into two layers after 24 hours and had poor storage stability. [Industrial Applicability]

[0131] The acrylic olefin composite resin composition of the present invention has excellent adhesion to polyolefin substrates and storage stability, and can be suitably used in the fields of printing inks, UV inks, pressure sensitive adhesives, adhesives, hot melt adhesives, ceramic sintering agents, paints, primers, heat sealing agents, molding materials, toners, etc.

Claims

1. An acrylic olefin composite resin composition D containing an acrylic olefin composite resin C, The acrylic olefin composite resin C contains a structural unit derived from a (meth)acrylic monomer a and a structure derived from an olefin resin B, The olefin resin B is at least one selected from the group consisting of polypropylene, ethylene-propylene copolymer, ethylene-propylene-butene copolymer, and propylene-butene copolymer; a mass ratio of the total mass of the structural units derived from all monomers constituting the olefin resin B to the total mass of the structural units derived from the (meth)acrylic monomer a is 1 to 100%; Acrylic olefin composite resin composition D having a water content of 0.01% by mass or more and 10% by mass or less.

2. An acrylic resin A containing a structural unit derived from the (meth)acrylic monomer a, and The acrylic olefin composite resin composition D according to claim 1, further comprising the olefin resin B.

3. The acrylic olefin composite resin composition D according to claim 1 or 2, which is in a particulate form.

4. The acrylic olefin composite resin composition D according to claim 3, having a mass average particle diameter of 10 μm or more and 2,500 μm or less.

5. The acrylic olefin composite resin composition D according to any one of claims 1 to 4, wherein the olefin resin B comprises at least one of an ethylene-propylene copolymer and a polypropylene.

6. A non-aqueous resin composition E comprising the acrylic olefin composite resin composition D according to any one of claims 1 to 5.

7. The non-aqueous resin composition E according to claim 6 , further comprising an organic solvent.

8. The nonaqueous resin composition E according to claim 7 , wherein the organic solvent comprises an organic solvent having a solubility parameter (SP value) of 8.0 or less and an organic solvent having a SP value of 9.2 or more.

9. The organic solvent having an SP value of 8.0 or less is contained in an amount of 5% by mass or more and 80% by mass or less relative to the total mass of the organic solvents, The nonaqueous resin composition E according to claim 8 , wherein the organic solvent having an SP value of 9.2 or more is contained in an amount of 10 mass % or more and 70 mass % or less relative to the total mass of the organic solvents.

10. The nonaqueous resin composition E according to claim 8 or 9, wherein the organic solvent having an SP value of 8.0 or less contains a compound having a cycloalkane structure.

11. The nonaqueous resin composition E according to any one of claims 8 to 10, wherein the organic solvent having an SP value of 9.2 or more includes a ketone solvent.

12. A method for producing the non-aqueous resin composition E according to any one of claims 6 to 11, comprising the steps of: A method for producing a non-aqueous resin composition E, comprising mixing the acrylic olefin composite resin composition D according to any one of claims 1 to 5 with an organic solvent containing 50 mass% or more of an organic solvent having an SP value of less than 9.2, and allowing the acrylic olefin composite resin composition D and the organic solvent having an SP value of 9.2 or more to coexist.

13. A method for producing an acrylic olefin composite resin composition D containing an acrylic olefin composite resin C having a structural unit derived from a (meth)acrylic monomer a and a structure derived from an olefin resin B, comprising: The olefin resin B is at least one selected from the group consisting of polypropylene, ethylene-propylene copolymer, ethylene-propylene-butene copolymer, and propylene-butene copolymer; a mass ratio of the total mass of the structural units derived from all monomers constituting the olefin resin B to the total mass of the structural units derived from the (meth)acrylic monomer a is 1 to 100%; A method for producing an acrylic-olefin composite resin composition D, comprising suspension polymerizing the (meth)acrylic monomer a in the presence of the olefin resin B.

14. A coating composition comprising the acrylic olefin composite resin composition D according to any one of claims 1 to 5.

15. An ink composition comprising the acrylic olefin composite resin composition D according to any one of claims 1 to 5.

16. An adhesive composition comprising the acrylic olefin composite resin composition D according to any one of claims 1 to 5.

17. A film or molding material comprising the acrylic olefin composite resin composition D according to any one of claims 1 to 5.

18. A coating composition comprising the non-aqueous resin composition E according to any one of claims 6 to 11.

19. An ink composition comprising the non-aqueous resin composition E according to any one of claims 6 to 11.

20. An adhesive composition comprising the non-aqueous resin composition E according to any one of claims 6 to 11.

Citation Information

Patent Citations

  • Manufacture of thermoplastic resin

    JP1984187012A

  • Graft copolymer and polyolefinic resin composition containing this copolymer

    JP1995010935A

  • Graft copolymer composition, thermoplastic resin composition containing the same, and molded item thereof

    JP2002338778A

  • Propylene copolymer, composition and adhesive comprising the same

    JP2004067729A

  • Coating composition containing propylene-based polymer and method for using the same

    JP2004269866A