Diamine or diamine composition, polyamide, molded article, fiber, film, or sheet, method for producing diamine and / or dicarboxylic acid, method for producing diamine and / or diamine composition, and method for producing polyamide

By depolymerizing polyamide 66 with an alkali (earth) metal compound at elevated temperatures and distilling to minimize amino alcohol, the method enhances the efficiency and purity of monomer recovery, facilitating effective recycling and reducing environmental impact.

JP7559982B2Active Publication Date: 2024-10-02TORAY INDUSTRIES INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023573395
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2023-10-26
Publication Date
2024-10-02
Estimated Expiration
2043-10-26

AI Technical Summary

Technical Problem

Existing methods for depolymerizing polyamide 66 to recover monomers are inefficient, with low yields and high impurity levels, particularly due to the presence of amino alcohol compounds that inhibit polymerization, making recycling of polyamide 66 inadequate for sustainable resource use.

Method used

A method involving the depolymerization of polyamide using an alkali (earth) metal compound at elevated temperatures to minimize amino alcohol content, followed by distillation to produce high-purity diamines and dicarboxylic acids, which are then repolymerized into polyamide with improved properties.

Benefits of technology

The method achieves high yields of diamines and dicarboxylic acids with reduced amino alcohol content, enabling efficient recycling of polyamide materials and reducing global warming gas emissions by utilizing waste polyamide as a resource.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559982000001
    Figure 0007559982000001
  • Figure 0007559982000002
    Figure 0007559982000002
Patent Text Reader

Abstract

The present invention provides: a diamine or diamine composition in which, in a diamine obtained by depolymerization of a polyamide, there is little content of an aminoalcohol compound, which is a polymerization inhibiting component; and a method for producing a diamine and a dicarboxylic acid which makes it possible to obtain the same with high efficiency and high purity. Provided is a diamine or a diamine composition which is obtained by depolymerization of a polyamide, wherein there is not more than 6.0×10-5 mol of an aminoalcohol represented by chemical formula (1) per 1 g of diamine. Chemical formula (1): H2N-R-OH (where R is a residue including at least one type of group selected from among C3-12 aliphatic groups, alicyclic groups, and aromatic groups)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a diamine or diamine composition, a polyamide using the same, and a method for producing a diamine and a dicarboxylic acid. [Background technology]

[0002] In recent years, interest in global environmental issues has increased, triggered by the marine plastic problem, and awareness of the need to build a sustainable society is spreading. Global environmental issues include global warming, resource depletion, and water shortages. Many of these issues are caused by the increase in resource consumption and greenhouse gas emissions due to the use of fossil fuels and the rapid development of industry since the Industrial Revolution. Therefore, in order to build a sustainable society, technologies for recycling fossil resources such as plastics and reducing greenhouse gas emissions are becoming increasingly important. In particular, polyamide 66, which is used in large quantities in various fields such as automobiles and electrical and electronic applications, emits a large amount of greenhouse gases during the production of the monomer. Therefore, there is a demand for technology to return products containing polyamide 66 to the monomer and recycle them. As a technique for depolymerizing polyamides composed of diamines and dicarboxylic acids such as polyamide 66, and returning them to monomers for recycling, a method of hydrolysis in the presence of an inorganic base compound such as sodium hydroxide at a temperature lower than the melting point of polyamide 66, such as 220°C, is known (see, for example, Patent Document 1 and Non-Patent Document 1). Furthermore, as a method for depolymerizing polyamides consisting of diamines and dicarboxylic acids without using an inorganic base compound, there have been disclosed a method in which the polyamide is contacted with high-temperature, high-pressure water to recover the diamine and dicarboxylic acid, which are raw material monomers, and a method in which the polyamide is contacted with high-temperature water and then further hydrolyzed using an enzyme to obtain the diamine and dicarboxylic acid (see, for example, Patent Documents 2-3 and Non-Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 7-507556 [Patent Document 2] JP 2001-302597 A [Patent Document 3] International Publication No. 2023 / 149514 [Non-patent literature]

[0004] [Non-Patent Document 1] Chemical Abstract 15 (1959) 14558g [Non-Patent Document 2] Polymer Degradation and Stability 83 (2004) 389-393 Summary of the Invention [Problem to be solved by the invention]

[0005] The method disclosed in Patent Document 2 and Non-Patent Document 2, which uses water in a subcritical or supercritical state to decompose polyamide 66, has a monomer yield of at most 25%, which is not sufficient for achieving resource recycling. Non-Patent Document 2 also describes that the reaction mixture contains oligomers, and that the reaction mixture contains cyclic by-products in amounts equal to or greater than the monomers due to the deammonia cyclization reaction of diamine in subcritical water and the decarboxylation cyclization reaction of dicarboxylic acid in supercritical water. The method using an enzyme reaction in Patent Document 3 produces hexamethylenediamine in an 82% yield and adipic acid in a 72% yield, but the yield is not yet sufficiently improved despite the two-stage hydrolysis process. According to the method for decomposing polyamide 66 disclosed in Patent Document 1, polyamide 66 is reacted in an aqueous sodium hydroxide solution at 220°C for 6 hours, followed by separation and purification, to obtain hexamethylenediamine in a yield of 92% and adipic acid in a yield of 81%. In Non-Patent Document 1, the reaction time is shortened to 1 hour compared to the method in Patent Document 1, and each monomer is obtained in a yield of 90%, but this is still not efficient. Furthermore, although Patent Document 1 confirms that diamine is produced by depolymerization, it does not disclose whether the diamine is of a quality sufficient to be used as a raw material for polyamide. An object of the present invention is to provide a diamine or diamine composition obtained by depolymerizing a polyamide, which has a low content of aminoalcohol compounds, which are polymerization inhibitors, and a method for producing a diamine and / or a dicarboxylic acid that can obtain the diamine or diamine composition with high efficiency and high purity. [Means for solving the problem]

[0006] In order to solve the above problems, the present invention has the following configuration. [1] A diamine or diamine composition obtained by depolymerizing a polyamide, in which the amino alcohol represented by the chemical formula (1) is present in an amount of 6.0 × 10 per 1 g of diamine. -5 mol or less of a diamine or diamine composition. Chemical formula (1): H2N-R-OH (In the formula, R is a residue containing at least one selected from an aliphatic group, an alicyclic group, and an aromatic group having 3 to 12 carbon atoms.) [2] 0.010 × 10 amino alcohol per 1 g of diamine -5 mol or more. [3] A diamine or diamine composition obtained by depolymerizing polyamide is used as a polymerization raw material, and the terminal structure represented by the chemical formula (2) is 3.0 × 10 -5 mol / g or less. Chemical formula (2):-NH-R-OH (In the formula, R is a residue containing at least one selected from an aliphatic group, an alicyclic group, and an aromatic group having 3 to 12 carbon atoms.) [4] A molded article, fiber, film, or sheet made using the polyamide described in [3] above. [5] A method for producing a diamine and / or a dicarboxylic acid, comprising the steps of: mixing (A) a polyamide composition containing a polyamide containing X mol of dicarboxylic acid residues; and (B) an aqueous solution of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these, containing Y 1 mol of alkali metal ions and / or Y 2 mol of alkaline earth metal ions, so as to satisfy formula (1); and maintaining the temperature at 230°C or higher for 0.1 to 45 minutes. Formula (1): 1.6≦(Y1+2×Y2) / X<2.4 [6] The method for producing a diamine and / or a dicarboxylic acid according to the above [5], wherein the temperature in the holding step is equal to or higher than the melting point of the polyamide composition (A) as determined by differential scanning calorimetry and lower than 400°C. [7] The method for producing a diamine and / or dicarboxylic acid according to the above item [5], wherein the mass ratio of the polyamide composition (A) to the aqueous solution of an alkali (earth) metal compound (B) selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these is 1:Z, and Z is 1.0 or more and 10.0 or less. [8] The method for producing a diamine and / or a dicarboxylic acid according to the above [5], wherein the yields of both the diamine and the dicarboxylic acid from the polyamide composition (A) are 70 mol % or more. [9] When the amount of diamine contained in the reaction mixture (C) obtained by contacting a polyamide composition (A) with an aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these is X' mol, and the amount of amino alcohol represented by the chemical formula (1) is Y' mol, Y' / X' is 4.0 × 10 -3 A method for producing a diamine and / or a dicarboxylic acid according to the above item [5], which is as follows: Chemical formula (1): H2N-R-OH (In the formula, R is a residue containing at least one selected from an aliphatic group, an alicyclic group, and an aromatic group having 3 to 12 carbon atoms.)

[10] The method for producing a diamine and / or a dicarboxylic acid according to the above [5], wherein the polyamide composition (A) is a waste product.

[11] A method for producing the diamine or diamine composition according to the above item [1], comprising the following steps (1) to (3) in this order: (1) A step of producing a diamine and a dicarboxylate by contacting a polyamide composition (A) with an aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these. (2) A step of separating the diamine and dicarboxylate produced in step (1). (3) A step of distilling the diamine separated in step (2)

[12] A method for producing a polyamide, comprising a step of polycondensing a raw material containing a diamine or a diamine composition obtained by the method for producing a diamine or a diamine composition according to

[11] above. Effect of the Invention

[0007] According to the present invention, it is possible to provide a diamine or diamine composition which can be suitably used as a repolymerization raw material and contains a small amount of amino alcohol, which is a polymerization inhibitor.Furthermore, it is possible to provide a method for producing diamine and dicarboxylic acid in a short time and with high efficiency by reacting a polyamide composition with an aqueous solution of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these containing a specific amount of alkali (earth) metal ions at 230°C or higher for a short time, thereby reducing the amount of amino alcohol produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will be described in detail below with reference to the embodiments. The diamine or diamine composition of the present invention is a diamine or diamine composition obtained by depolymerizing a polyamide, and has an aminoalcohol represented by chemical formula (1) of 6.0×10 per 1 g of diamine. -5 mol or less. Chemical formula (1): H2N-R-OH (In the formula, R is a residue containing at least one selected from an aliphatic group, an alicyclic group, and an aromatic group having 3 to 12 carbon atoms.) Here, the amino alcohol represented by chemical formula (1) is a specific compound that is generated when polyamide is depolymerized. Specifically, it is a compound that is generated when one of the amino groups of the diamine component contained in the polyamide to be depolymerized is converted to a hydroxyl group. The amino alcohol represented by chemical formula (1) is easily generated when polyamide is depolymerized with high-temperature, high-pressure water.

[0009] In the present invention, the polyamide to be depolymerized is a polymer or copolymer having diamine and dicarboxylic acid residues as main structural units. Here, "having diamine and dicarboxylic acid residues as main structural units" refers to having diamine and dicarboxylic acid residues in 50 mol % or more of all structural units, and a preferred embodiment has these residues in 80 mol % or more.

[0010] In the present invention, the polyamide to be depolymerized is preferably a homopolymer or copolymer obtained by polycondensation of a diamine and a dicarboxylic acid. Representative examples of diamines include aliphatic diamines such as tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, 2-methylpentamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2,2,4- / 2,4,4-trimethylhexamethylenediamine, and 5-methylnonamethylenediamine; aromatic diamines such as metaxylylenediamine and paraxylylenediamine; and alicyclic diamines such as 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, bis(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminopropyl)piperazine, and aminoethylpiperazine. Representative examples of dicarboxylic acids include aliphatic dicarboxylic acids such as adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid, aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodiumsulfoisophthalic acid, 2,6-naphthalenedicarboxylic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid, and alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, and 1,3-cyclopentanedicarboxylic acid, etc. In the present invention, two or more types of polyamide homopolymers or copolymers derived from these raw materials may be blended. The structure of R in the compound (1) obtained by depolymerizing the polyamide includes an aliphatic group, an alicyclic group, and an aromatic group having 3 to 12 carbon atoms.

[0011] In the present invention, the polyamide to be depolymerized may be a polyamide copolymer obtained by copolymerizing an amino acid and a lactam, or may be a blend of a polyamide homopolymer or copolymer obtained by polycondensation of an amino acid and a lactam, provided that the object of the present invention is not impaired. Representative examples of the raw material include amino acids such as 6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and paraaminomethylbenzoic acid, and lactams such as ε-caprolactam and ω-laurolactam.

[0012] Specific examples of the polyamide include polyhexamethylene adipamide (nylon 66), polytetramethylene adipamide (nylon 46), polytetramethylene sebacamide (nylon 410), polypentamethylene adipamide (nylon 56), polypentamethylene sebacamide (nylon 510), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecamide (nylon 612), polydecamethylene adipamide (nylon 106), polydecamethylene sebacamide (nylon 10 10), Polydecamethylene dodecamide (Nylon 1012), Polycaproamide / Polyhexamethylene adipamide copolymer (Nylon 6 / 66), Polycaproamide / Polyhexamethylene terephthalamide copolymer (Nylon 6 / 6T), Polyhexamethylene adipamide / Polyhexamethylene terephthalamide copolymer (Nylon 66 / 6T), Polyhexamethylene adipamide / Polyhexamethylene isophthalamide copolymer (Nylon 66 / 6I), Polyhexamethylene terephthalamide / Poly Polyhexamethylene isophthalamide copolymer (nylon 6T / 6I), polyhexamethylene terephthalamide / polydodecanamide copolymer (nylon 6T / 12), polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 6T / 6I), polyxylylene adipamide (nylon XD6), polyxylylene sebacamide (nylon XD10), polyhexamethylene terephthalamide / polypentamethylene terephthalamide Examples of such copolymers include polyhexamethylene terephthalamide / poly-2-methylpentamethylene terephthalamide copolymer (nylon 6T / M5T), polypentamethylene terephthalamide / polydecamethylene terephthalamide copolymer (nylon 5T / 10T), polynonamethylene terephthalamide (nylon 9T), polydecamethylene terephthalamide (nylon 10T), polydodecamethylene terephthalamide (nylon 12T), and copolymers thereof. Two or more of these may be blended. Here, " / " indicates a copolymer, and the same applies below.

[0013] The polyamide to be depolymerized in the present invention may be a polyamide composition containing a polymerization catalyst, a thermoplastic resin other than polyamide, a dye, various additives, a fibrous filler, a non-fibrous filler, etc., within the scope of the present invention. The fibrous filler is not particularly limited as long as it has a fibrous shape. Examples of the fibrous filler include glass fiber, carbon fiber, potassium titanate whisker, zinc oxide whisker, aluminum borate whisker, aramid fiber, alumina fiber, silicon carbide fiber, ceramic fiber, asbestos fiber, gypsum fiber, and metal fiber. On the other hand, examples of non-fibrous fillers include wollastonite, zeolite, sericite, kaolin, mica, talc, clay, pyrophyllite, bentonite, montmorillonite, asbestos, aluminosilicate, alumina, silicon oxide, magnesium oxide, zirconium oxide, titanium oxide, iron oxide, calcium carbonate, magnesium carbonate, dolomite, calcium sulfate, barium sulfate, magnesium hydroxide, calcium hydroxide, aluminum hydroxide, glass beads, ceramic beads, boron nitride, silicon carbide, silica, etc. Two or more of these may be blended.

[0014] The polyamide to be depolymerized in the present invention may be a resin molded article containing polyamide. The resin molded article containing polyamide includes polyamide products, industrial waste generated in the manufacturing process of polyamide products, or used waste of polyamide products. Specific examples of polyamide products include engine peripheral parts such as radiator tanks and oil pans, automobile parts such as gears, electrical and electronic parts such as connectors and switches, parts for industrial machinery such as fasteners and cable ties, industrial fiber structures such as airbags, fiber structures for clothing, sheets, films, molded articles, etc. Furthermore, product scraps, pellet scraps, lump scraps, etc. generated in the production process of these may be used.

[0015] In the method for producing a diamine and / or a dicarboxylic acid of the present invention, the polyamide composition (A) is preferably a waste material. By using the polyamide composition (A) as a waste material, fossil resources can be recycled. Furthermore, since there is no need to incinerate the waste material, the amount of greenhouse gas emissions can be reduced.

[0016] The diamine or diamine composition of the present invention contains 6.0×10 -5 mol or less. Chemical formula (1): H2N-R-OH In the formula, R is a residue containing at least one selected from an aliphatic group, an alicyclic group, and an aromatic group having 3 to 12 carbon atoms.

[0017] When the diamine or diamine composition obtained by the present invention is reused as a polyamide raw material, if a specific amount of the aminoalcohol represented by chemical formula (1) is contained, it acts as an end-blocking agent and inhibits polymerization. The present invention aims to regenerate the diamine or diamine composition to a practically usable quality that allows repolymerization. The aminoalcohol represented by chemical formula (1) contained in the diamine or diamine composition is present in an amount of 6.0×10 per 1 g of diamine. -5 By keeping the amount of amino alcohol per 1 g of diamine at 2.0 × 10 mol or less, the degree of polymerization of polyamide can be increased to a practically usable level. -5 mol or less is preferable, and 1.0×10 -5 mol or less is preferable, and 0.5×10 -5 On the other hand, the present inventors have determined that the amount of the amino alcohol in the diamine composition is at least 0.010 × 10 mol per 1 g of the diamine. -5It was found that when recycled diamine containing 1000 mol or more (detection limit of gas chromatography described in the examples) is polymerized, the degree of polymerization is higher than that of polyamide polymerized under the same conditions from petroleum-derived diamine. It is believed that trace amounts of amino alcohol have little effect as the above-mentioned end-blocking agent, but act like a plasticizer, lowering the melt viscosity of the polyamide, thereby increasing molecular mobility and promoting the polymerization reaction. In the present invention, the amount of amino alcohol represented by chemical formula (1) contained in the diamine or diamine composition is measured by quantitative analysis by gas chromatography (GC) described in the examples.

[0018] The method for producing a diamine or a diamine composition of the present invention preferably includes the following steps (1) to (3) in this order. (1) A step of producing a diamine and a dicarboxylate by contacting a polyamide composition (A) with an aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these. (2) A step of separating the diamine and dicarboxylate produced in step (1). (3) A step of distilling the diamine separated in the step (2). As used herein, reference to alkaline (earth) metal compounds refers to both compounds containing alkali metal atoms, e.g., lithium, sodium, potassium, and alkaline earth atoms, e.g., magnesium, calcium, barium, and mixtures thereof.

[0019] The method for producing the diamine and dicarboxylate in step (1) is not particularly limited. For example, when the depolymerization reaction is carried out in a batch manner, a reaction mixture containing the diamine and the alkali (earth) metal salt of the dicarboxylate can be obtained after the depolymerization reaction. When the depolymerization reaction is carried out in a continuous manner, a reaction mixture containing the diamine and the alkali (earth) metal salt of the dicarboxylate can be obtained as the reaction proceeds. The state of the reaction mixture is not particularly limited, and examples thereof include an aqueous solution, a slurry, and a paste.

[0020] As a method for separating the diamine and dicarboxylate in step (2), a known method such as extraction or solid-liquid separation can be selected according to the properties of the diamine and dicarboxylate produced. When an aqueous solution of sodium hydroxide is used as the aqueous solution of an alkali (earth) metal compound selected from polyamide 66, hydroxide, oxide, carbonate, and a mixture containing two or more of these as the polyamide, both the diamine and the dicarboxylate are water-soluble, so it is particularly preferable to separate them by extraction. In addition, if there is a component insoluble in water in the reaction mixture, it can be separated in advance by a known method such as solid-liquid separation and then subjected to step (2). When sodium hydroxide is used as the aqueous solution of an alkali (earth) metal compound selected from polyamide 610, hydroxide, oxide, carbonate, and a mixture containing two or more of these as the polyamide, the dicarboxylate can be precipitated by cooling, so separation can also be performed by solid-liquid separation.

[0021] In step (3), it is preferable to distill the diamine separated from the dicarboxylate in step (2) to reduce the content of the amino alcohol represented by chemical formula (1). For example, when polyamide 66 is used as the polyamide, the boiling point of the raw material monomer hexamethylenediamine is 204°C, and the boiling point of 6-amino-1-hexanol, an amino alcohol in which one amino group of hexamethylenediamine is converted to a hydroxyl group, is 225°C. By distillation purification, the content of the amino alcohol, which is a polymerization inhibitor, can be reduced, and the quality can be improved to a level where it can be repolymerized for practical use, which is preferable. The diamine or diamine composition obtained in this way can be used as a polymerization raw material for polyamide, similar to the diamine and carboxylic acid produced from petroleum-derived raw materials.

[0022] The polyamide of the present invention contains a diamine or a diamine composition obtained by depolymerizing a polyamide as a polymerization raw material, and has a terminal structure represented by chemical formula (2) of 3.0 × 10 -5 mol / g or less. Chemical formula (2):-NH-R-OH (In the formula, R is a residue containing at least one selected from an aliphatic group, an alicyclic group, and an aromatic group having 3 to 12 carbon atoms.)

[0023] In the present invention, the content of the terminal structure represented by chemical formula (2) can be quantified by hydrolyzing the polyamide with hydrochloric acid, and then analyzing the amino alcohol trimethylsilylated with N,O-bis(trimethylsilyl)trifluoroacetamide (BSTFA reagent) by gas chromatography (GC). The content of the terminal structure referred to here is calculated as the molar equivalent of the terminal structure represented by chemical formula (2) per gram of polyamide. By setting the content within this range, it is possible to obtain a polyamide with a high degree of polymerization to a practically usable level. 1.0×10 -5 mol / g or less is more preferable, and 0.5×10 -5 mol / g or less is more preferable, and 0 mol / g is most preferable.

[0024] In the present invention, the amount of the amino alcohol represented by the above chemical formula (1) is about 0.010 × 10 -5 In the polyamide obtained by polymerizing 100 mol of the diamine composition, the terminal structure represented by the above chemical formula (2) was 0 mol / g (below the detection limit of gas chromatography), and the effect of having a higher degree of polymerization than the polyamide shown in Reference Example 1 in which the reagent diamine was polymerized was confirmed.

[0025] The method for producing a polyamide of the present invention includes a step of polycondensing a raw material containing the diamine or diamine composition of the present invention. The polyamide of the present invention can be produced by polycondensation of diamine or diamine composition obtained by depolymerizing polyamide with dicarboxylic acid as it is or as a salt thereof as one of the raw material components. When producing polyamide, the degree of polymerization is high when the equimolar ratio of the amount of carboxyl end group and the amount of amino end group of the monomer is appropriately maintained. In order to mix the diamine and dicarboxylic acid uniformly, it is preferable that the diamine, dicarboxylic acid, and salts thereof are uniformly dissolved in the polymerization system. In addition, it is preferable to carry out the polycondensation reaction while heating. The preferable lower limit of the temperature is 150°C, and the preferable upper limit of the temperature is 400°C.

[0026] The polyamides thus obtained can be processed and used in various products such as injection molded products, extrusion molded products, fiber structures, films, etc., in the same manner as polyamides produced from petroleum-derived raw materials. These products are useful as automobile parts, electrical and electronic parts, industrial machinery applications, industrial fiber structures, clothing fiber structures, sheets, films, and other applications.

[0027] The molded article, fiber, film, or sheet of the present invention is made using the polyamide of the present invention. The polyamide of the present invention contains, as a polymerization raw material, a diamine or a diamine composition obtained by depolymerizing the polyamide. Therefore, the obtained polyamide can be a recycled material with low environmental impact that contributes to resource recycling and reduction of greenhouse gas emissions.

[0028] The method for producing a diamine and a dicarboxylic acid of the present invention comprises the steps of mixing a polyamide composition (A) containing a polyamide containing X mol of dicarboxylic acid residues with an aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these, containing Y 1 mol of alkali metal ions and / or Y 2 mol of alkaline earth metal ions, so as to satisfy formula (1), and maintaining the mixture at a temperature of 230°C or higher for 0.1 to 45 minutes. Formula (1): 1.6≦(Y1+2×Y2) / X<2.4 In the present invention, the temperature and time during which the components are mixed and maintained within the above ranges may be referred to as the reaction temperature and reaction time, respectively. The pressure during which the components are maintained may be referred to as the reaction pressure.

[0029] As described above, the method for producing a diamine and / or a dicarboxylic acid of the present invention is characterized by mixing a polyamide-containing polyamide composition (A) with an aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these, to produce diamines and dicarboxylic acids that are polyamide monomers constituting the polyamide composition (A).

[0030] Examples of the polyamide composition (A) containing a polyamide include compositions containing the above-mentioned polyamide to be depolymerized, a polymerization catalyst, a thermoplastic resin other than polyamide, a dye, various additives, a fibrous filler, a non-fibrous filler, etc.

[0031] The aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these is prepared by blending an alkali (earth) metal compound and water. Examples of the alkali (earth) metal hydroxide include lithium hydroxide, sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, and barium hydroxide. Examples of the alkali (earth) metal oxide include lithium oxide, sodium oxide, potassium oxide, magnesium oxide, calcium oxide, and barium oxide. Examples of the alkali (earth) metal carbonate include normal salts and acid salts (bicarbonates). Examples of normal salts include dilithium carbonate, disodium carbonate, dipotassium carbonate, magnesium carbonate, calcium carbonate, and barium carbonate. Examples of the alkali metal bicarbonate include lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, magnesium carbonate, calcium carbonate, and barium carbonate. In the present invention, two or more types selected from these alkali (earth) metal hydroxides, alkali (earth) metal oxides, and alkali (earth) metal carbonates may be blended and used. As the alkaline (earth) metal, sodium, potassium, and calcium are preferred from the viewpoint of protecting mineral resources, and sodium and potassium are more preferred, and sodium is particularly preferred, from the viewpoint of increasing the production rate of diamines and dicarboxylic acids. In addition, for the purpose of increasing the hydrolysis reactivity with polyamide, hydroxides, oxides, and normal salts of carbonates are preferred, and hydroxides and oxides are particularly preferred. There is no particular restriction on the water used here, but any water such as tap water, deionized water, distilled water, and well water may be used. From the viewpoint of suppressing side reactions due to the influence of coexisting salts, deionized water and distilled water are preferably used as the water.

[0032] The amount of alkali metal ions in the aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these is set according to the polyamide content in the polyamide composition (A). When the dicarboxylic acid residue of the polyamide contained in the polyamide composition (A) is X mol, the alkali metal ion contained in the aqueous solution (B) of the alkali (earth) metal compound is Y1 mol, and the alkaline earth metal ion is Y2 mol, (Y1+2×Y2) / X is 1.6 or more and less than 2.4. By controlling (Y1+2×Y2) / X within this range, the yield of diamines and dicarboxylic acids can be improved in the hydrolysis of the polyamide composition (A), and the amount of amino alcohol represented by the above chemical formula (1) can be reduced. (Y1+2×Y2) / X is preferably 1.8 or more, more preferably 1.9 or more, and particularly preferably 2.0 or more. On the other hand, it is more preferably 2.2 or less. The amount of dicarboxylic acid residues contained in the polyamide composition (A) was measured by proton nuclear magnetic resonance spectroscopy ( 1 Quantitation can be achieved from the spectrum obtained by 1 H-NMR.

[0033] In the present invention, the yields of the diamine and dicarboxylic acid obtained by depolymerizing the polyamide contained in the polyamide composition (A) are preferably 70 mol% or more. The yields referred to here are expressed as molar percentages of the amounts of the diamine and dicarboxylic acid contained in the reaction mixture, with the number of moles of the diamine residue and the number of moles of the dicarboxylic acid residue contained in the polyamide composition (A) being 100, respectively. The yields are preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 95 mol% or more. In the present invention, the yield of the diamine is calculated by quantitative analysis by gas chromatography (GC) as described in the examples. In addition, in the present invention, the yield of the dicarboxylic acid is calculated by quantitative analysis by ion chromatography (IC) as described in the examples. The yields of the diamine and dicarboxylic acid are in the preferred ranges, so that the recycling rate can be increased.

[0034] There is no particular restriction on the amount of the aqueous solution (B) of an alkaline (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these, but when the mass ratio of the polyamide composition (A) to the aqueous solution (B) of an alkaline (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these is 1:Z, Z is preferably 1 or more. If Z is less than 1, when the polyamide composition (A) and the aqueous solution (B) of an alkaline (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these are mixed at 230°C or higher, the dispersibility and solubility of the polyamide composition (A) in water tend to decrease, and the reaction efficiency tends to decrease. It is more preferably 2.0 or more, and even more preferably 3.0 or more. On the other hand, Z is preferably 10 or less, more preferably 8.0 or less, and even more preferably 6.0 or less. The present invention relates to a highly efficient method for producing diamines and dicarboxylic acids by depolymerizing a polyamide composition (A) for the purpose of achieving both the cyclical use of fossil resources and the reduction of greenhouse gas emissions. Water has a specific heat capacity of 4.3 kJ / kg K and a heat of vaporization of 2,250 kJ / kg, which are extremely high compared to other organic solvents. Therefore, it is important to reduce the amount of water used. By keeping the amount of aqueous solution (B) containing an alkali (earth) metal compound selected from a certain range of hydroxides, oxides, carbonates, and mixtures containing two or more of these, within these ranges, it is possible to achieve both efficient production of diamines and dicarboxylic acids and energy conservation.

[0035] There is no particular limitation on the method for preparing the aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these. The aqueous solution may be prepared in advance by mixing the alkali (earth) metal compound with water, or the aqueous solution may be prepared by mixing the alkali (earth) metal compound with water when contacting the polyamide composition (A) in the reaction vessel.

[0036] The method for producing a diamine and / or a dicarboxylic acid of the present invention is characterized in that a polyamide composition (A) is contacted with an aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these at a temperature of 230°C or higher for 0.1 to 45 minutes to produce a diamine and a dicarboxylic acid. In the method for producing a diamine and / or dicarboxylic acid of the present invention, the reaction time of the polyamide composition (A) and the aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these is 0.1 to 45 minutes. As described above, the reaction time in the present invention refers to the total time of holding at a temperature of 230°C or higher, and the time during which the polyamide composition (A) and the aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these are mixed in a reaction vessel at a temperature of 230°C or higher is included in the reaction time, including the temperature rise process until the reaction temperature is reached and the cooling process after the reaction at the reaction temperature. If the reaction time exceeds 45 minutes, it is not preferable because it leads to a decrease in the yield of diamines and dicarboxylic acids and an increase in the amount of amino alcohol produced. It is preferably 45 minutes or less, more preferably 40 minutes or less, and even more preferably 35 minutes or less. On the other hand, if the reaction time is less than 0.1 minutes, the depolymerization reaction cannot be sufficiently advanced, and the yield of diamines and dicarboxylic acids is reduced. 0.1 minutes or more is preferable, 1 minute or more is more preferable, and 3 minutes or more is even more preferable.

[0037] The amount of aminoalcohol represented by chemical formula (1) can be reduced by contacting polyamide composition (A) with aqueous solution (B) of an alkaline (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these, for a reaction time within the above-mentioned preferred range. The aminoalcohol is thought to be generated when one of the NH2 groups of the diamine, which is the depolymerization product of polyamide composition (A), is converted to an OH group through a nucleophilic substitution reaction. The amount of aminoalcohol represented by chemical formula (1) in the present invention is determined when the amount of diamine contained in reaction mixture (C) after depolymerization is X' mol and the amount of aminoalcohol represented by chemical formula (1) is Y' mol, and Y' mol is satisfied, Y' / X' is 4.0 x 10 -3 It is preferable that the value is 3.0×10 or less. -3 Less than 2.0×10 is more preferable. -3 Less than 1.0×10 is even better. -3 The following is particularly preferred. The amount of diamine and aminoalcohol represented by chemical formula (1) can be calculated by quantitative analysis by gas chromatography (GC) as described in the Examples. When the amount of aminoalcohol represented by chemical formula (1) is within the preferred range, the diamine or diamine composition obtained after subsequent purification can be repolymerized to obtain a polyamide with a high molecular weight.

[0038] The reaction temperature in the method for producing a diamine and / or dicarboxylic acid of the present invention is 230°C or higher. The reaction temperature is the temperature during contacting the polyamide composition (A) with an aqueous solution (B) of an alkaline (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these in a temperature-controlled reaction vessel, and may be a constant temperature or a temperature that varies with time. There are no particular limitations on the temperature during the temperature increase process until the reaction temperature is reached or the cooling process after the reaction at the reaction temperature, as long as it is less than 230°C. By setting the reaction temperature at 230°C or higher, the time required for the hydrolysis reaction of the polyamide composition (A) can be shortened, and the production efficiency of the diamine and dicarboxylic acid can be increased.

[0039] Furthermore, the reaction temperature is preferably a temperature equal to or higher than the melting point of the polyamide composition (A) determined by differential scanning calorimetry and lower than 400°C. By setting the reaction temperature equal to or higher than the melting point of the polyamide composition (A), the polyamide composition (A) becomes easily dispersed and dissolved in water, and the reaction efficiency can be improved. When the pressure of water is increased to 22.1 MPa and the temperature to 374.2°C, the polyamide composition (A) becomes neither liquid nor gaseous. Water in this state is called supercritical water, and since it has both the solubility of a liquid and the diffusibility of a gas, it has attracted attention as a reaction field for decomposing polymers. In addition, hot water in the vicinity of the critical point of the temperature and pressure slightly lower than the critical point of water is called subcritical water. Although subcritical water is water, it has the characteristics of (i) a low dielectric constant and (ii) a high ionic product, and the dielectric constant and ionic product of subcritical water depend on the temperature and partial pressure of water and can be controlled. Due to the low dielectric constant, it becomes an excellent solvent for organic compounds despite being water, and due to the high ionic product, the hydrogen ion and hydroxide ion concentrations are high, resulting in excellent hydrolysis action. By setting the reaction temperature to less than 400°C, it is possible to suppress undesirable reactions such as thermal decomposition while utilizing a reaction field having excellent characteristics of supercritical water or subcritical water when mixing and reacting the polyamide resin (A) with the aqueous solution (B) of an alkaline (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these. In addition, by setting the reaction temperature to less than 374.2°C, it is possible to preferably control the ion product by utilizing the subcritical state of water, thereby improving the reaction efficiency and shortening the reaction time, which is preferable. Furthermore, in order to suppress the over-reaction of the diamine and dicarboxylic acid, the reaction temperature is more preferably less than 350°C, and even more preferably less than 300°C. On the other hand, in order to promote the depolymerization reaction, it is more preferable to set the reaction temperature to 250°C or higher, and even more preferable to set the reaction temperature to 270°C or higher.

[0040] The melting point of the polyamide composition (A) in the present invention is the temperature of an endothermic peak that appears when the polyamide composition (A) is heated from 40°C to 300°C at a heating rate of 10°C / min under a nitrogen flow using a differential scanning calorimeter manufactured by TA Instruments. However, when two or more endothermic peaks are detected, the temperature of the endothermic peak detected on the highest temperature side is taken as the melting point. If the melting point of the polyamide composition (A) exceeds 400°C, the thermal decomposition reaction of the polyamide composition (A) progresses, and the recovery rate of the diamine and dicarboxylic acid decreases, which is not preferable. There is no particular limit to the lower limit of the melting point of the polyamide composition (A), but a preferable lower limit is 50°C. If the melting point of the polyamide composition (A) is 50°C or higher, the polyamide becomes solid at room temperature, and thus the polyamide has excellent handleability.

[0041] In addition, the reaction pressure is preferably higher than the saturated vapor pressure. By making the reaction pressure higher than the saturated vapor pressure, water can be maintained in a liquid state and the reaction can proceed easily, so the pressure of the aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these is preferably higher than the saturated vapor pressure. In addition, there is no particular limit to the upper limit of the reaction pressure, but an example is 22.1 MPa or less. By being in this pressure range, the ionic product of water tends to be high, so this is preferable. As a method for setting the reaction pressure in this pressure range, a method of pressurizing the inside of a pressure vessel and sealing it can be mentioned. To pressurize the inside of the pressure vessel, a gas may be sealed in addition to the polyamide composition (A), the aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these. Examples of the gas to be sealed include air, argon, and nitrogen. From the viewpoint of suppressing side reactions such as oxidation reactions, it is preferable to use nitrogen or argon as the gas to be sealed. In addition, the inside of the pressure vessel can also be pressurized by introducing high-pressure water. When using high-pressure water, the pressure vessel may be in a state where there is no gas inside. The degree of gas pressure is not particularly limited as it is set to the desired pressure, but can be 0.3 MPa or more.

[0042] In the present invention, the polyamide composition (A) and the aqueous solution (B) of an alkaline (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these can be mixed in various known reaction methods such as batch and continuous. For example, in the case of batch, autoclaves equipped with a stirrer and a heating function, vertical or horizontal reactors, and vertical or horizontal reactors equipped with a compression mechanism such as a cylinder in addition to a stirrer and a heating function can be used. In the case of continuous, extruders equipped with a heating function, tubular reactors, tubular reactors equipped with a mixing mechanism such as a baffle, line mixers, vertical or horizontal reactors, vertical or horizontal reactors equipped with a stirrer, and towers can be used. In addition, the atmosphere in the production is preferably a non-oxidizing atmosphere, more preferably an inert atmosphere such as nitrogen, helium, and argon, and even more preferably a nitrogen atmosphere from the viewpoints of economy and ease of handling.

[0043] There is no particular limitation on the method for recovering the diamine and dicarboxylic acid produced by the method of the present invention, and any method can be adopted. For example, when the depolymerization reaction is carried out in a batch system, a reaction mixture (C) of diamine and dicarboxylic acid alkali (earth) metal salt can be obtained after the depolymerization reaction. When the depolymerization reaction is carried out in a continuous system, a reaction mixture (C) of diamine and dicarboxylic acid alkali (earth) metal salt can be obtained as the reaction proceeds. The diamine and dicarboxylic acid alkali (earth) metal salt can be separated from the obtained reaction mixture (C) by a known method such as extraction, and the separated dicarboxylic acid alkali (earth) metal salt can be converted to dicarboxylic acid under acidic conditions, and the diamine and dicarboxylic acid can be recovered by a known method such as distillation and solid-liquid separation. In addition, if there is a water-insoluble component in the reaction mixture (C), it can be separated in advance by a known method such as solid-liquid separation and subjected to a diamine and dicarboxylic acid recovery process. In order to reduce the content of amino alcohol in the diamine, it is particularly preferable to purify the diamine by distillation. In order to obtain a diamine and a dicarboxylic acid of higher purity, they may be further purified by a known method.

[0044] The diamine and dicarboxylic acid obtained by the method for producing a diamine and / or a dicarboxylic acid of the present invention can be used as a polymerization raw material for polyamide, similar to the diamine and carboxylic acid produced from a petroleum-derived raw material. Polyamide resins can be produced by subjecting the diamine and / or dicarboxylic acid directly or a salt thereof to thermal polycondensation. In the present invention, polyamide can be regenerated by repolymerizing the diamine and / or dicarboxylic acid obtained by depolymerizing the polyamide, and therefore it can become a recycled material with low environmental impact that contributes to resource recycling and reduction of greenhouse gas emissions.

[0045] The polyamide thus obtained can be processed and used in various products such as injection molded products, extrusion molded products, fiber structures, films, etc., in the same manner as polyamides produced from petroleum-derived raw materials. These products are useful as automobile parts, electric and electronic parts, industrial machinery applications, industrial fiber structures, clothing fiber structures, sheets, films, and other applications. EXAMPLES

[0046] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.

[0047] The following raw materials were used in each example. (A-1) Polyamide 66: "Amilan" (registered trademark) manufactured by Toray Industries, Inc., CM3001-N, melting point 262°C (A-2) Polyamide 66 waste: Polyamide 66 airbag fabric recovered from scrapped cars (A-3) Polyamide 66 waste: Silicone-coated airbag fabric made of polyamide 66 recovered from scrapped cars, with an estimated silicone content of 25 g / m 2 (A-4) Polyamide 66 waste: GF30% reinforced polyamide 66 molding waste (crushed sprues and runners) Sodium hydroxide: Kanto Chemical Co., Ltd., special grade reagent Sodium carbonate: Kanto Chemical Co., Ltd., special grade reagent Sodium bicarbonate: Fujifilm Wako Pure Chemical Industries, Ltd. Grade 1 Adipic acid: Fujifilm Wako Pure Chemical Industries, Ltd., special grade Hexamethylenediamine: Grade 1 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.

[0048] Evaluation method (Aminoalcohol content in diamine composition (GC)) The amount of amino alcohol in the diamine composition was calculated by quantitative analysis using gas chromatography (GC). Equipment: Shimadzu GC-2010 Column: Agilent Technologies DB-5 0.32mm x 30m (0.25μm) Carrier gas: Helium Detector: Flame ionization detector (FID) Sample: About 0.02 g of the diamine composition was taken, diluted with about 10 g of deionized water, and components insoluble in the deionized water were separated and removed by filtration to prepare a sample for gas chromatography measurement. Quantitative determination of amino alcohol: The amount of amino alcohol was quantified by the absolute calibration curve method.

[0049] (Diamine yield, amount of amino alcohol in the reaction mixture (GC)) The amounts of diamine and aminoalcohol in the reaction mixture (C) were calculated by quantitative analysis using gas chromatography (GC), and the diamine yield was determined from the calculated diamine amount. Equipment: Shimadzu GC-2010 Column: Agilent Technologies DB-5 0.32mm x 30m (0.25μm) Carrier gas: Helium Detector: Flame ionization detector (FID) Sample: Approximately 0.15 g of the reaction mixture was taken, diluted with approximately 10 g of deionized water, and components insoluble in the deionized water were separated and removed by filtration to prepare a sample for gas chromatography measurement. Quantitative determination of diamine: The amount of diamine was quantified by the absolute calibration curve method. Quantitative determination of amino alcohol: The amount of amino alcohol was quantified by the absolute calibration curve method.

[0050] (Dicarboxylic acid yield (IC)) The dicarboxylic acid yield was calculated by quantitatively analyzing the sodium dicarboxylate in the reaction mixture (C) by ion chromatography (IC). Equipment: Shimadzu HIC-20Asuper Column: Shimadzu Shim-pack IC-SA2 (250mm x 4.6mm ID) Detector: Electrical conductivity detector (suppressor) Eluent: 4.0 mM sodium bicarbonate / 1.0 mM sodium carbonate aqueous solution Flow rate: 1.0ml / min Injection volume: 50 microliters Column temperature: 30℃ Sample: Approximately 0.02 g of the reaction mixture was taken, diluted with approximately 10 g of deionized water, and components insoluble in deionized water were separated and removed by filtration to prepare a sample for ion chromatography measurement. Quantitative determination of dicarboxylic acid: The amount of sodium dicarboxylate was quantified by the absolute calibration curve method.

[0051] (Polyamide melting point (DSC)) Approximately 5.0 mg of polyamide was heated under a nitrogen flow from 40°C to 300°C at a heating rate of 10°C / min using a differential thermal analyzer (TG / DTA7200 manufactured by Hitachi High-Tech Science). The temperature of the endothermic peak that appeared when this was done was taken as the melting point. However, when two or more endothermic peaks were detected, the temperature of the endothermic peak detected on the highest temperature side was taken as the melting point.

[0052] (Molecular weight of polyamide) Approximately 2.5 mg of the polyamide obtained in each of the Examples and Comparative Examples was dissolved in 4 ml of hexafluoroisopropanol (0.005N sodium trifluoroacetate added), and the resulting solution was filtered through a 0.45 μm filter. The resulting solution was used to measure the number average molecular weight (Mn) by GPC measurement. The measurement conditions are shown below. Pump: e-Alliance GPC system (Waters) Detector: Differential refractometer Waters 2414 (manufactured by Waters) Column: Shodex HFIP-806M (2 columns) + HFIP-LG Solvent: Hexafluoroisopropanol (0.005N sodium trifluoroacetate added) Flow rate: 1ml / min Sample injection volume: 0.1 ml Temperature: 30℃ Molecular weight standards: polymethyl methacrylate.

[0053] (Aminoalcohol content at polyamide terminals (GC)) Approximately 50 mg of the polyamide resin obtained in each Example and Comparative Example was precisely weighed and placed in a glass ampoule with a capacity of 16 ml, and 8 ml of 6N hydrochloric acid solution was added, and the ampoule was sealed. This was placed in a pressure-resistant container and heated at 180°C for 20 hours for hydrolysis treatment. After cooling, the ampoule was taken out and the contents were concentrated to dryness. Furthermore, after removing the hydrochloric acid, the dried product obtained by drying was trimethylsilylated using N,O-bis(trimethylsilyl)trifluoroacetamide (BSTFA reagent). The reaction product was diluted with dehydrated acetonitrile to prepare a gas chromatography measurement sample. The measurement conditions are shown below. Equipment: Shimadzu GC-2010 Column: Agilent Technologies DB-5 0.32mm x 30m (0.25μm) Carrier gas: Helium Detector: Flame ionization detector (FID) Determination of amino alcohol: The amount of amino alcohol was determined by the absolute calibration method using the amino alcohol of the trimethylsilylated reagent.

[0054] [Example 1] A SUS316L autoclave equipped with a stirrer was charged with polyamide 66 (A-1) having a melting point of 262°C and an aqueous sodium hydroxide solution in the amounts shown in Table 1. The molar ratio Y1 / X, expressed as the amount of polyamide 66 blended (X moles) and the amount of sodium hydroxide blended (Y1 moles), was 2.11. The reaction vessel was replaced with nitrogen, and the vessel was sealed under a nitrogen pressure of 0.5 MPa, and the reaction was carried out by holding the vessel at 280°C for 15 minutes while stirring at 200 rpm. The pressure in the system during the reaction was 6.5 MPa. After the reaction was completed, the reaction mixture was cooled to room temperature and collected. The total time for mixing the polyamide composition and the aqueous sodium hydroxide solution in the reaction vessel at 230°C or higher was 40 minutes. The diamine yield (X') calculated by gas chromatography of the recovered reaction mixture was 98 mol%, and the dicarboxylic acid yield calculated by high performance liquid chromatography was 95 mol%. The amount of amino alcohol (Y') was 0.14 mol%, and the Y' / X' ratio was 1.4 × 10 -3 It was. [Examples 2 to 9, Comparative Examples 1 to 3] The type of raw material polyamide, the amount and concentration of the aqueous sodium hydroxide solution, the amount of deionized water, the reaction temperature, and the reaction time were appropriately changed to carry out depolymerization of the polyamide in the same manner as in Example 1. In Comparative Example 3, the reaction was carried out at a temperature lower than 230°C, and therefore the reaction time was set to the treatment time at 220°C (60 minutes).

[0055] [Examples 10 and 11] Depolymerization of polyamide was carried out in the same manner as in Example 1, except that sodium hydroxide was changed to sodium carbonate or sodium hydrogen carbonate. The reaction conditions, yields of the reaction products, and quantitative analysis results for Examples 1 to 11 and Comparative Examples 1 to 3 are shown in Tables 1 and 2.

[0056] [Table 1]

[0057] [Table 2]

[0058] Examples 1 to 11 show that by contacting a polyamide with an aqueous solution containing a preferred amount of an alkali metal hydroxide or an alkali metal carbonate, hydrolysis can be sufficiently advanced, and the yield of diamine and dicarboxylic acid can be increased while the amount of aminoalcohol represented by chemical formula (1) can be reduced. In Comparative Example 1, in which Y1 / X was larger than the preferred range, the yield of diamine decreased and the amount of amino alcohol produced increased, compared with Example 1, in which the reaction was carried out under substantially the same conditions except for Y1 / X. When the amount of alkali metal hydroxide was excessive, both diamine and dicarboxylic acid could not be obtained in good yield even if the reaction temperature and reaction time conditions were satisfied, and the amount of amino alcohol produced increased. On the other hand, in Comparative Example 2, in which the reaction was carried out for a long period of time exceeding the preferred range, the amount of amino alcohol produced was greater than in Example 1, in which the reaction was carried out under substantially the same conditions except for the reaction time. In Comparative Example 3, in which the reaction temperature was less than 230° C., the reaction time was set to 60 minutes, and diamine and dicarboxylic acid were obtained in good yields, but the amount of amino alcohol produced remained large.

[0059] Thus, it is found that by contacting the polyamide composition with an aqueous solution containing a preferred amount of an alkali metal hydroxide and / or an alkali metal carbonate at a temperature of 230° C. or higher for 0.1 to 45 minutes, hydrolysis can be sufficiently advanced, and the yield of diamine and dicarboxylic acid can be increased while the amount of aminoalcohol represented by chemical formula (1) can be reduced. Furthermore, as described in Patent Document 1 and Non-Patent Document 1, if the reaction temperature is lower than the preferred range, the reaction takes a long time and the amount of aminoalcohol becomes greater than when the reaction is carried out at the preferred reaction temperature. When selecting polyamide 66 as the polyamide, 6-amino-1-hexanol, an amino alcohol derived from hexamethylenediamine residues, has a boiling point of 225°C, close to the boiling point of hexamethylenediamine, 204°C. Therefore, if the amount of amino alcohol in the reaction mixture is large, it will be difficult to separate and remove it by distillation, making it difficult to use it for recycling.

[0060] [Reference example 1] 5.15g of hexamethylenediamine and 6.47g of adipic acid were dissolved in 12.6g of deionized water to prepare a salt solution. This salt solution was charged into a reaction vessel, sealed, and substituted with nitrogen. The heater on the outer periphery of the reaction vessel was set to a temperature of 290°C, and heating was started. After the pressure inside the vessel reached 1.75MPa, the pressure inside the vessel was maintained at 1.75MPa while releasing moisture to the outside of the system, and the temperature inside the vessel was raised to 237°C. After the temperature inside the vessel reached 237°C, the pressure inside the vessel was adjusted to normal pressure over 1 hour (temperature inside the vessel when normal pressure was reached: 257°C). Subsequently, the vessel was maintained for 60 minutes while flowing nitrogen (nitrogen flow) to obtain polyamide 66 (maximum temperature reached: 274°C). The number average molecular weight of the obtained polyamide 66 was 14300g / mol, and the melting point was 262°C.

[0061] [Example 12] Diamine was extracted with isobutanol from the reaction mixture obtained in the same manner as in Example 1, concentrated using an evaporator, and then distilled at 84 to 90°C and 3±1 hPa to obtain a crude diamine composition. The crude diamine composition was distilled again at 84 to 90°C and 3±1 hPa to obtain a diamine composition. The amino alcohol content in this diamine composition was 0.80×10 per 1 g of diamine. -5 It was mol. 15 mL of 35% aqueous hydrochloric acid was added to the aqueous dicarboxylic acid solution from which the diamine had been removed by extraction, to obtain a slurry solution in which the dicarboxylic acid had precipitated. The slurry solution was heated in an oil bath at 80°C to form a homogeneous solution, and then allowed to stand at room temperature for 12 hours to precipitate crude adipic acid. Deionized water was added to the crude adipic acid recovered by vacuum filtration in an amount twice the mass of the crude adipic acid, and the mixture was heated again in an oil bath at 80°C to form a homogeneous solution, and then allowed to stand at room temperature for 12 hours. The precipitated adipic acid was recovered by vacuum filtration and dried in a vacuum oven set at 110°C for 12 hours to obtain adipic acid. Polyamide 66 was produced in the same manner as in Reference Example 1, except that 5.14 g of the diamine composition thus obtained and 6.50 g of adipic acid were used as polymerization raw materials. The number average molecular weight of the resulting recycled polyamide 66 was 15,300 g / mol, the melting point was 262° C., and the amino alcohol terminal group amount was 0.41×10 -5 The mass ratio was mol / g.

[0062] [Example 13] The reaction mixture obtained in the same manner as in Example 3 was subjected to two rounds of distillation in the same manner as in Example 12 to obtain a diamine composition. The amino alcohol content in this diamine composition was 0.010×10 per 1 g of diamine. -5 Adipic acid and polyamide 66 were produced in the same manner as in Example 12. The number average molecular weight of the resulting recycled polyamide 66 was 15,000 g / mol, the melting point was 262°C, and the amount of amino alcohol terminal groups was 0 mol / g (below the detection limit of gas chromatography).

[0063] [Comparative Example 4] A diamine composition and adipic acid were produced in the same manner as in Example 12 from the reaction mixture obtained in the same manner as in Comparative Example 1. The amino alcohol content in the diamine composition was 6.4 × 10 per 1 g of diamine. -5 Polyamide 66 was produced in the same manner as in Reference Example 1, except that this diamine composition and adipic acid were used as polymerization raw materials. The number average molecular weight of the resulting recycled polyamide 66 was 11,000 g / mol, the melting point was 261° C., and the amino alcohol terminal group amount was 3.3×10-5 The mass ratio was mol / g. Therefore, from Reference Example 1, Example 12, and Example 13, it was found that the polyamide obtained by depolymerizing the diamine composition of the present invention obtained by depolymerizing the polyamide and repolymerizing adipic acid has a larger number average molecular weight than the polyamide obtained by polymerizing the reagent diamine and the reagent dicarboxylic acid. On the other hand, from Reference Example 1 and Comparative Example 4, the amino alcohol content in the diamine composition was 6.0 × 10 -5 The polyamide repolymerized with a diamine composition larger than 3.0 × 10 mol had terminal -5 It was found that the diamine composition had an amino alcohol-derived structure of 1000 mol / g or more, and the number average molecular weight was small. It is presumed that the polymerization was inhibited by the amino alcohol in the diamine composition. 6-amino-1-hexanol, an amino alcohol derived from hexamethylenediamine residues, has a boiling point of 225°C, which is close to the boiling point of hexamethylenediamine, 204°C, so it is believed that the large amount of amino alcohol in the reaction mixture made it difficult to remove by distillation. [Industrial Applicability]

[0064] The diamine composition of the present invention contains few impurities, and therefore can be suitably used as a raw material for repolymerization of polyamide. In particular, the diamine composition of the present invention can be obtained by depolymerization of polyamide, which contributes to resource recycling and reduction of greenhouse gas emissions.

Claims

1. A diamine or diamine composition obtained by depolymerizing a polyamide homopolymer or copolymer obtained by polycondensation of a diamine and a dicarboxylic acid, the diamine or diamine composition comprising an amino alcohol represented by the chemical formula (1) of 6.0 × 10 per gram of diamine. -5 mol or less. Chemical formula (1): H 2 N-R-OH (In the formula, R is a residue containing at least one selected from an aliphatic group, an alicyclic group, and an aromatic group having 3 to 12 carbon atoms.)

2. The amino alcohol is 0.010 x 10 per 1 g of diamine. -5 2. The diamine composition of claim 1, wherein the diamine composition is 1 to 2 mol.

3. A method for producing a polyamide homopolymer or copolymer comprising the steps of: (a) depolymerizing a polyamide homopolymer or copolymer obtained by polycondensation of a diamine and a dicarboxylic acid; and (b) depolymerizing a diamine or a diamine composition as a polymerization raw material, the method comprising the steps of: -5 mol / g or less. Chemical formula (2): -NH-R-OH (In the formula, R is a residue containing at least one selected from an aliphatic group, an alicyclic group, and an aromatic group having 3 to 12 carbon atoms.)

4. A molded article, fiber, film, or sheet, which is obtained by using the polyamide according to claim 3.

5. A polyamide composition (A) containing a polyamide homopolymer or copolymer containing X mol of dicarboxylic acid residues and diamine residues, and an alkali metal ion Y 1 mol and / or alkaline earth metal ions are 2 A method for producing a diamine and / or a dicarboxylic acid, comprising the steps of: mixing an aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these, so as to satisfy formula (1); and maintaining the mixture at a temperature of 230° C. or higher for 0.1 to 45 minutes. Formula (1): 1.6≦(Y 1 +2 x Y 2 ) / X<2.4

6. 6. The method for producing a diamine and / or a dicarboxylic acid according to claim 5, wherein the temperature in the holding step is equal to or higher than the melting point of the polyamide composition (A) determined by differential scanning calorimetry and lower than 400°C.

7. 6. The method for producing a diamine and / or a dicarboxylic acid according to claim 5, wherein, when the mass ratio of the polyamide composition (A) to the aqueous solution of an alkali (earth) metal compound (B) selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these is 1:Z, Z is 1.0 or more and 10.0 or less.

8. The method for producing a diamine and / or a dicarboxylic acid according to claim 5, wherein the yields of both the diamine and the dicarboxylic acid from the polyamide composition (A) are 70 mol % or more.

9. When the amount of diamine contained in the reaction mixture (C) obtained by contacting the polyamide composition (A) with an aqueous solution (B) of an alkaline (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these is X' mol, and the amount of aminoalcohol represented by the chemical formula (1) is Y' mol, Y' / X' is 4.0 × 10 -3 The method for producing a diamine and / or a dicarboxylic acid according to claim 5, wherein: Chemical formula (1): H 2 N-R-OH (In the formula, R is a residue containing at least one selected from an aliphatic group, an alicyclic group, and an aromatic group having 3 to 12 carbon atoms.)

10. The method for producing a diamine and / or a dicarboxylic acid according to claim 5, wherein the polyamide composition (A) is a waste product.

11. A method for producing the diamine or diamine composition according to claim 1, comprising the following steps (1) to (3) in this order: (1) A step of producing a diamine and a dicarboxylate by contacting a polyamide composition (A) with an aqueous solution (B) of an alkali (earth) metal compound selected from hydroxides, oxides, carbonates, and mixtures containing two or more of these. (2) A step of separating the diamine and dicarboxylate produced in the step (1). (3) A step of distilling the diamine separated in the step (2).

12. A method for producing a polyamide, comprising a step of polycondensing a raw material containing a diamine or a diamine composition obtained by the method for producing a diamine or a diamine composition according to claim 11.

Citation Information

Patent Citations

  • Recycling method of polyamide-66 fishing net wastes

    CN107056625A

  • Process for producing adipic acid and hexanediamine by depolymerization of nylon-66

    CN1611477A

  • JP1964-023390B

  • Method for simultaneously producing dicarboxylic acid and diamine from polyamide

    JP1995507556A

  • Nitrate hydrolysis of polyamides

    JP1998510295A