Method for producing a paste-like hardening composition for denture base
A two-stage mixing process for paste-type denture base materials ensures high strength, toughness, and stable paste properties by dissolving the soluble polymer in a monomer at a specific temperature before combining with a porous crosslinked polymer, addressing issues of viscosity control and adhesion.
Patent Information
- Application Number
- JP2020156304
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-17
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-09-17
AI Technical Summary
Existing paste-type denture base materials face challenges in achieving high strength, toughness, and stable paste properties during preparation and long-term storage, with issues related to viscosity control and adhesion to gloves or dental models.
A method involving a two-stage mixing process is employed, where a (meth)acrylic acid-based polymerizable monomer and a soluble non-crosslinked polymer are mixed at a predetermined temperature to ensure complete dissolution, followed by kneading with a monomer-absorbing porous crosslinked polymer to create a paste-like curable composition.
The method produces a curable composition with high bending strength, breaking energy, and stable paste properties that maintain adhesion to dental models while avoiding adherence to gloves, ensuring efficient production and long-term storage stability.
Smart Images

Figure 0007560051000001 
Figure 0007560051000002 
Figure 0007560051000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a hardenable composition for a denture base. More specifically, the present invention relates to a method for producing a paste-like hardenable composition suitable for a paste-type denture base resin, a hard lining material for a denture base, and a denture base repair resin. [Background technology]
[0002] A hardenable composition for denture bases is a composition used for the manufacture and repair of denture bases, and known materials using this composition include denture base resins used when making new dentures, hard denture base lining materials used to rebase dentures that have become incompatible with the patient's oral mucosa after long-term use and restore them to a usable state, and denture base repair resins used for lining denture bases, repairing rebased or broken dentures, etc.
[0003] As a hardenable composition for a denture base, a polymerizable hardenable composition containing a polymerizable monomer such as methyl methacrylate, a (meth)acrylic acid-based polymer such as polymethyl methacrylate or polyethyl methacrylate, and a polymerization initiator is generally used. As the polymerization initiator, a chemical (redox) polymerization initiator, a photopolymerization initiator, a thermal polymerization initiator, or a combination of these is used, and the above material is provided in different forms depending on the type of polymerization initiator used.
[0004] For example, when using a chemical polymerization initiator containing a combination of an oxidizing agent (sometimes simply referred to as a "radical initiator") and a reducing agent (sometimes referred to as a "polymerization accelerator"), which can react immediately upon contact among the above-mentioned materials, the oxidizing agent and the reducing agent need to be stored separately (packaged separately), and are usually provided as a powder-liquid type consisting of a liquid agent mainly composed of a polymerizable monomer and a reducing agent, and a powder agent mainly composed of a (meth)acrylic acid-based polymer and an oxidizing agent (see Patent Documents 1 and 2), or as a two-paste type in which a polymerizable monomer and a (meth)acrylic acid-based polymer are blended with an oxidizing agent and a reducing agent, respectively, to form a paste (see Patent Document 3).
[0005] The two-paste type denture base material proposed in the above Patent Document 3 is composed of two components, each of which contains a methacrylate without a urethane bond, a methacrylate with a urethane bond, a polyurethane powder with cross-linked bonds, and a filler, with one component containing an oxidizing agent (radical initiator) and the other a reducing agent (polymerization accelerator). It is known that a composition composed of such two components provides sufficient operation time to form a denture base material, making it excellent in operability, and furthermore, the hardened body formed by the material has appropriate elasticity, resulting in less damage to the restored area.
[0006] Two-paste denture base materials that use such chemical polymerization initiators have the advantage that polymerization begins by mixing the two pastes, and therefore no special equipment such as a polymerization apparatus is required. However, there is room for improvement in that each paste needs to be measured and mixed, making the process of producing a hardened body complicated.
[0007] On the other hand, various one-paste denture base materials using a photopolymerization initiator or a thermal polymerization initiator have been proposed. For example, Patent Document 4 proposes a denture base resin material that is made by mixing a polymerizable monomer, at least one polymer selected from an alkyl (meth)acrylate homopolymer, an alkyl (meth)acrylate copolymer, and an alkyl (meth)acrylate-styrene copolymer, and a thermal polymerization catalyst and / or a photopolymerization catalyst, and that is characterized in that at least a part of the polymer component is dissolved in the polymerizable monomer. Patent Document 5 also proposes a one-paste denture base resin composition that is made of a polymerizable monomer and / or oligomer having a specific range of elastic modulus during polymerization, an organic filler and / or an organic-inorganic composite filler having a specific range of elastic modulus, and a polymerization initiator made of a heat-polymerization type polymerization initiator and / or a photopolymerization type polymerization initiator.
[0008] 1 Paste-type denture base materials require equipment such as a polymerization apparatus for hardening, but have the advantage of being easy to use, since they do not require measuring or mixing, maintain their paste properties until heat or light is applied, and can start polymerizing at any time. Furthermore, the denture base resin composition described in Patent Document 5 is known to have the characteristics that the obtained hardened product has excellent bending strength and elastic energy properties, as well as excellent impact resistance, due to the use of a material with an appropriate elastic modulus. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 11-335222 [Patent Document 2] Special Publication No. 4-042364 [Patent Document 3] JP 2000-175941 A [Patent Document 4] JP 2000-254152 A [Patent Document 5] JP2002-104912A Summary of the Invention [Problem to be solved by the invention]
[0010] As described above, the one-paste type and two-paste type denture base materials have appropriate elasticity, good bending strength and impact resistance, and some are known to be easy to handle. However, they are not necessarily satisfactory in terms of strength and toughness, and depending on the filling material used, it is difficult to control the paste properties, and strength may be low, so there is still room for improvement.
[0011] Furthermore, because paste-type denture base materials are often handled with gloved hands due to their form, they need to be less sticky so as not to adhere to the gloves. On the other hand, when used to make new dentures, they need to adhere to the plaster model, and when used to reline or repair denture bases, they need to adhere to the dentures. In other words, from the viewpoint of ease of use, paste-type denture base hardenable compositions are required to have paste properties with appropriate viscosity that do not adhere to gloves but adhere to plaster models and dentures.
[0012] Thus, in paste-type hardenable compositions for denture bases, there is a demand for one-paste types that provide good operability for the paste itself and high strength and toughness for the hardened product, while there is a demand for two-paste types that provide good operability for each paste and for the mixture of both pastes (mixed paste) and that provide high strength and toughness for the hardened product of the mixed paste.
[0013] The present inventors have proposed a paste-like hardenable composition (hereinafter also referred to as "already proposed paste-like hardenable composition") containing a (meth)acrylic acid-based polymerizable monomer, a porous organic crosslinked polymer capable of absorbing the (meth)acrylic acid-based polymerizable monomer, and a (meth)acrylic acid-based non-crosslinked polymer as a paste-like hardenable composition for one-paste-type denture base hardenable composition and two-paste-type denture base hardenable composition that meet the above requirements (Patent Application Nos. 2019-4801 and 2019-48536). Note that "paste" generally means a non-settling non-Newtonian fluid, and "paste-like" in this specification means a high-viscosity paste having plastic deformability, particularly a non-aqueous high-viscosity paste.
[0014] The above-mentioned previously proposed paste-like curable compositions solve the above-mentioned problems. However, subsequent studies by the present inventors revealed that when the components are simply mixed and kneaded during preparation, not only does it take a long time to prepare the composition, but the obtained paste-like curable composition may not exhibit the desired paste properties, or the paste properties may change when stored for a long period of time.
[0015] Therefore, an object of the present invention is to provide a method for producing the previously proposed paste-like curable composition with high efficiency and high reproducibility in a state in which the composition can exhibit its inherent properties. [Means for solving the problem]
[0016] The present invention is intended to solve the above problems newly recognized by the present inventors, and one aspect of the present invention is A method for producing a paste-like hardenable composition for a denture base comprising: component A: a component consisting of a (meth)acrylic acid-based polymerizable monomer that is liquid at room temperature and normal pressure; component B: a component consisting of a (meth)acrylic acid-based non-crosslinked polymer that can be dissolved in component A; and component C: a component consisting of a porous organic crosslinked polymer that can absorb component A, Mix components A and B at a specified temperature: T MIX (° C.) to obtain a liquid composition in which component B is dissolved in component A; A second step of mixing and kneading the liquid composition obtained in the first step with component C to obtain a paste-like composition; Includes In the first step, Component B is 5 to 40 (parts by mass) per 100 (parts by mass) of component A, and Temperature:T MIX A formation in Minutes The amount of saturation solubility is less than the amount of powder Dissolve component B in component A while dispersing the viscous component B. stomach, In the second step, the C component is mixed and kneaded in an amount of 65 / R to 165 / R (parts by mass) when the amount (parts by mass) of the A component absorbed per unit amount (parts by mass) of the C component measured in accordance with JIS K5101-13-1 is defined as the absorption amount R (parts by mass of the A component / parts by mass of the C component). The method for producing a paste-like hardenable composition for a denture base is characterized by the following: In the present invention, the term "room temperature and normal pressure" refers to 25°C and 1 atmospheric pressure (≒1013 hPa).
[0018] In addition, the first step uses component A or a part of component A as a dispersion medium, for B component of The saturated dissolution amount is at the temperature: T MIX A component in for B component of The dispersion medium and the condition that the amount of the solubility is less than the saturated solubility are used. powder The dispersion medium is mixed with component B in the form of a solid. powder a dispersing step for obtaining a dispersion liquid in which the solid component B is dispersed, and powder The total amount of B component in the solid state is contained, and the temperature of the system is T MIX It is preferable that the method further comprises a dissolving step of dissolving component B to achieve the state in which the above-mentioned mixture is obtained.
[0019] In the above preferred embodiment, the maximum amount (parts by mass) of component B soluble in 100 parts by mass of a (meth)acrylic acid-based polymerizable monomer component having a predetermined composition at a predetermined temperature and normal pressure is added to the polymerizable monomer component at the predetermined temperature. for B component of When the solubility is calculated, the component A or a part of the component A which serves as a dispersion medium in the dispersion step is for B component of The dispersant is dissolved in water at a temperature where the solubility is 5 or less. powder The dispersion medium is mixed with component B in the form of a solid. powder It is preferable to obtain a dispersion in which component B in a solid form is dispersed.
[0020] In the preferred embodiment, the component A is T MIX A component A1 is a (meth)acrylic acid-based polymerizable monomer having a solubility of component B of 5 or less in T MIX and a component A2 consisting of a (meth)acrylic acid-based polymerizable monomer having a solubility of component B exceeding 5 in the above dispersion. transformation In the process, component A1 is used as a dispersion medium, and powder A dispersion liquid in which the solid component B is dispersed is obtained, and in the dissolving step, the dispersion liquid is mixed with component A2 to dissolve the entire amount of component A and powder After the temperature reaches T MIX It is preferable to dissolve component B in the above-mentioned manner. Effect of the Invention
[0021] According to the manufacturing method of the present invention, it is possible to efficiently produce a paste-like hardenable composition for denture base that can give a hardened product having both high bending strength (strength) and breaking energy (toughness), and that not only has paste properties with appropriate viscosity so that it does not adhere to gloves but adheres to plaster models and dentures, but can also maintain such paste properties even after long-term storage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The target of the manufacturing method of the present invention is a novel paste-like hardenable composition for denture bases, comprising component A: a component consisting of a (meth)acrylic acid-based polymerizable monomer that is liquid at room temperature and normal pressure (hereinafter, the polymerizable monomer may be simply referred to as a "monomer" and component A as a "monomer component"); component B: a component consisting of a (meth)acrylic acid-based non-crosslinked polymer that can be dissolved in component A (hereinafter, also referred to as a "soluble non-crosslinked polymer"); and component C: a component consisting of a porous organic crosslinked polymer that can absorb component A (hereinafter, also referred to as a "monomer-absorbent porous crosslinked polymer"). The composition can give a hardened body that has both high bending strength (strength) and breaking energy (toughness), and has paste properties with appropriate viscosity such that it does not adhere to gloves but adheres to plaster models and dentures.
[0023] Without being bound by theory, the present inventors speculate that the mechanism by which the above-mentioned paste-like hardenable composition for denture base exhibits such excellent effects is as follows.
[0024] In other words, we believe that the high bending strength (strength) of the cured body is due to the use of a crosslinked polymer with a high elastic modulus as the organic filler. As for the high toughness despite the use of a crosslinked polymer, we believe that this is due to the anchor effect that occurs when component A penetrates into the pores of component C, a monomer-absorbent porous crosslinked polymer, and hardens, thereby increasing the interfacial bonding strength between the matrix and the organic filler in the cured body.
[0025] Regarding the paste properties, this is thought to be because component C (monomer-absorbent porous cross-linked polymer) does not inhibit the effect of adjusting the paste properties by dissolving component B in component A, which is seen in a two-component system of component B (soluble non-cross-linked polymer) and component A (monomer). For example, a cross-linked polymer that does not have monomer-absorbent properties (does not have pores) other than component C. powder When a monomer-absorbent porous cross-linked polymer (component C) is added, it is difficult to disperse uniformly due to poor affinity. Therefore, when the amount of the polymer is increased, the range of adjustment of the paste properties becomes narrow. In addition, the paste may become hard due to aggregation and precipitation during long-term storage. powder Blending the body Ta In this case, the monomer component penetrates into the pores and becomes compatible with the monomer, making it easy to disperse uniformly and allowing the dispersed state to be maintained for a long period of time, which is thought to make it difficult to inhibit the above-mentioned effect of component C.
[0026] The paste-like hardenable composition for denture base, which is the target of the manufacturing method of the present invention, has such excellent features. However, as described above, subsequent studies by the present inventors have revealed that if the components are simply mixed and kneaded during production, it takes a long time to prepare and the desired paste properties and the desired storage stability regarding the paste properties cannot be obtained.
[0027] The present inventors presumed that the cause of such a problem is as follows, and investigated a solution based on this assumption. That is, the problem of the time required for preparation is solved by the fact that the soluble non-crosslinked polymer (component B) is usually powder The body is used, and its dissolution into the monomer is powder It is thought that the monomer penetrates into the particle, causing it to swell and gradually dissolve. powder When the polymer was mixed with a large amount of monomer at once, it swelled. powderIt was believed that this was caused by the bodies adhering to each other and forming lumps, which significantly reduced the contact area with the monomer. As for the inability to obtain the desired paste properties, it was believed that this was caused by the presence of a portion of the soluble non-crosslinked polymer (component B) in a state that was not dissolved in the monomer during paste preparation, which made it difficult to obtain the desired paste properties, and even if the desired paste properties could be adjusted, the remaining polymer gradually dissolved, making the paste properties unstable.
[0028] The present invention was made based on the above-mentioned hypothesis regarding the new problem and its cause. powder The above problem is solved by dispersing the solid component B in the component A while completely dissolving the component B.
[0029] That is, the manufacturing method of the present invention comprises mixing components A and B at a predetermined mixing temperature: T MIX (° C.) to obtain a liquid composition in which component B is dissolved in component A; and a second step of mixing and kneading the liquid composition obtained in the first step with component C to obtain a paste-like composition. MIX Below the saturated solubility of component A in powder The feature of this method is that component B is dissolved while dispersing the solid component B in component A.
[0030] Various raw materials used in the manufacturing method of the present invention and each step in the manufacturing method of the present invention will be described in detail below. In this specification, unless otherwise specified, the expression "x to y" using numerical values x and y means "x or more and y or less". In such an expression, when a unit is added only to the numerical value y, the unit is also applied to the numerical value x. In addition, in this specification, the term "(meth)acrylic" means both "acrylic" and "methacrylic". Similarly, the term "(meth)acrylate" means both "acrylate" and "methacrylate", and the term "(meth)acryloyl" means both "acryloyl" and "methacryloyl".
[0031] 1. Various raw materials used in the manufacturing method of the present invention First, the production method and each component used in the paste-like hardenable composition for denture base of the present invention will be described.
[0032] 1-1. Component A: Monomer As the (meth)acrylic acid-based polymerizable monomer that is liquid at room temperature and normal pressure used as component A (monomer component) in the manufacturing method of the present invention, among the (meth)acrylic acid-based polymerizable monomers generally used for dental use, those that are liquid at room temperature and normal pressure when used alone or in a mixture of two or more kinds are used. As described above, "room temperature and normal pressure" in the present invention means 25°C and 1 atm (≒1013 hPa).
[0033] Specific examples of such (meth)acrylic acid-based polymerizable monomers include monofunctional (meth)acrylic acid-based polymerizable monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, hydroxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 2-methacryloxyethyl propionate, and acetoacetoxyethyl (meth)acrylate, 1,6-bis(methacrylethyloxycarbonylamino)trimethylhexane, 2,2-bis(methacryloyloxyphenyl)propane, and acrylates corresponding to these methacrylates, 2-hydroxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate. Examples of the polymerizable monomer include difunctional (meth)acrylic acid polymerizable monomers such as 2-hydroxyethyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, and 2-hydroxyethyl (meth)acrylate; and trifunctional (meth)acrylic acid polymerizable monomers such as trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and trimethylolmethane tri(meth)acrylate.
[0034] These (meth)acrylic acid-based polymerizable monomers can be used alone or in combination of two or more. In particular, when a monofunctional monomer is used in combination with a difunctional or trifunctional or higher functional monomer, it is preferable to use a larger amount of the difunctional or trifunctional or higher functional monomer, since this can improve the mechanical properties such as strength and durability of the resulting cured product.
[0035] 1-2. Component B: Soluble non-crosslinked polymer The component B used in the manufacturing method of the present invention is soluble in the component A, and can be any non-crosslinked (non-crosslinked) (meth)acrylic acid-based polymer that is generally used in dentistry and is in the form of a granule or powder in the air at room temperature, without any particular limitation. Specifically, the component B being soluble in the component A means that all of the component B blended in 100 parts by mass of the component A at 25°C is soluble, as judged by visual observation.
[0036] Examples of (meth)acrylic acid-based non-crosslinked polymers that can be suitably used include methyl (meth)acrylate, ethyl (meth)acrylate, t-butyl (meth)acrylate, n-butyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, isopropyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and 3-hydroxypropyl (meth)acrylate. Examples of the monomers include homopolymers or copolymers of 2-hydroxy-1,3-dimethacryloxypropane, isobutyl (meth)acrylate, butoxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, glycidyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and benzyl (meth)acrylate, and copolymers of (meth)acrylic acid monomers such as poly(styrene-ethyl methacrylate) and other polymerizable monomers. These may be used alone or in combination of two or more.
[0037] The average molecular weight of the component B is not particularly limited, but from the viewpoint of the solubility and ease of adjusting the paste properties, it is preferably 50,000 or more and less than 1,000,000, and more preferably 100,000 or more and 700,000 or less. The particle size is not particularly limited, but if it is too large, it will dissolve slowly in the component A, which will require a long time for production and will tend to reduce the work efficiency, so it is preferably 100 μm or less.
[0038] The blending amount of the above-mentioned component B is preferably 5 to 40 parts by mass, and more preferably 15 to 30 parts by mass, per 100 parts by mass of component A.
[0039] 1-3.C component: Monomer-absorbent porous cross-linked polymer The component C (monomer-absorbent porous crosslinked polymer) used in the manufacturing method of the present invention is a polymer having crosslinks composed of organic material, which is granular or powdery (agglomeration of fine particles) in the air at room temperature, and has pores inside the particles that communicate with the outside, and has a large number of pores on the surface into which the (meth)acrylic acid-based polymerizable monomer can penetrate. However, from the viewpoint of strength enhancement, it is preferable to use an absorption amount defined as the amount (g) of the component A absorbed per unit amount of the monomer-absorbent porous organic crosslinked polymer, which is measured according to the "refined linseed oil method" of JIS K5101-13-1 (using the (meth)acrylic acid-based polymerizable monomer instead of refined linseed oil), of preferably 1.5 g / g or more, more preferably 2.0 g / g or more and 5.0 g / g or less.
[0040] The material of the monomer-absorbent porous organic crosslinked polymer is not particularly limited as long as it is a crosslinked polymer, but from the viewpoint of affinity with the (meth)acrylic acid-based polymerizable monomer, crosslinked polyalkyl (meth)acrylates such as crosslinked polymethyl methacrylate, crosslinked polyethyl methacrylate, crosslinked polymethyl acrylate, polystyrene, polyvinyl chloride, etc. are preferred. As such porous crosslinked polymers, polymers described in JP-B-4-51522 and JP-A-2002-265529 can be used. As such porous crosslinked polymers, commercially available "Technopolymer MBP-8" (Sekisui Chemical Co., Ltd.) and the like can be used.
[0041] The average pore size of the monomer-absorbent porous organic crosslinked polymer is preferably 1 to 100 nm, and particularly preferably 5 to 50 nm. The average pore size refers to the average size of pores formed on the surface of the primary particles of the porous crosslinked polymer, not the aggregated pores of secondary particles formed by the aggregation of the porous crosslinked polymer particles. The average pore size can be calculated from the pore distribution of the particles measured using a mercury intrusion pore distribution measuring device.
[0042] When the average pore diameter is smaller than 1 nm, the amount of the (meth)acrylic acid-based polymerizable monomer that penetrates into the pores decreases, and the anchor effect in the hardened body also decreases, making it difficult to obtain sufficient strength. When the average pore diameter is larger than 100 nm, the amount of penetration is large, but the anchor effect decreases, making it difficult to obtain sufficient strength.
[0043] The particle size of the monomer-absorbent porous organic crosslinked polymer is not particularly limited, but the average particle size is preferably 1 to 50 μm, and particularly preferably 3 to 30 μm. The average particle size means the average particle size of the primary particles of the porous crosslinked polymer particles, and is measured using a particle size distribution measuring device using a laser diffraction / scattering method. If the average particle size is smaller than 1 μm, the paste before hardening tends to become sticky and the operability tends to decrease, and if the average particle size is larger than 50 μm, the specific surface area tends to be small, making it difficult to obtain sufficient strength and toughness in the hardened body. The particle shape is not particularly limited, and either pulverized particles or spherical particles can be used.
[0044] The amount of the monomer-absorbing porous organic crosslinked polymer is determined to be an optimal amount depending on the amount of absorption. For example, a porous organic crosslinked polymer with a large amount of absorption absorbs a large amount of monomer, so that the apparent amount of monomer is small, and the desired paste properties can be obtained with a relatively small amount of absorption. On the other hand, a porous organic crosslinked polymer with a small amount of absorption can be blended in a relatively large amount. Specifically, when the amount (parts by mass) of the A component absorbed per unit amount (parts by mass) of the C component measured in accordance with the above JIS K5101-13-1 is R (parts by mass of the A component / parts by mass of the C component), the amount is preferably 65 / R to 165 / R (parts by mass). When the C component exceeds 165 / R, the cured body tends to be hard and brittle, and the paste tends to be hard. Also, when it is less than 65 / R, the anchor effect tends to decrease and the hardness tends to decrease. From the viewpoint of curing, the amount of the C component is preferably 80 / R to 150 / R, particularly 100 / R to 140 / R.
[0045] In addition, even if it is an organic crosslinked polymer, a non-porous organic crosslinked polymer that does not have pores on the surface is difficult to dissolve and swell in the above (meth)acrylic acid-based polymerizable monomer and has poor interaction with the matrix, so it may aggregate and settle in the paste and harden the paste, and if it is blended in a large amount, the properties of the paste may change during storage (specifically, it may harden), and the operability of the paste may decrease. Therefore, when blending a non-porous organic crosslinked polymer, it is preferable to blend the amount of the polymer to 10 parts by mass or less relative to 100 parts by mass of the above (meth)acrylic acid-based polymerizable monomer, and it is more preferable not to blend it at all.
[0046] 1-4.Other ingredients In the manufacturing method of the present invention, a polymerization initiator used in dental materials can be suitably used. Examples of the polymerization initiator include a chemical (redox) polymerization initiator, a photopolymerization initiator, a thermal polymerization initiator, or a combination thereof.
[0047] When the hardenable composition for denture base produced by the present invention is of one-paste type, it is preferable to use a photopolymerization initiator and / or a thermal polymerization initiator as the polymerization initiator, and to completely or substantially not contain a chemical polymerization initiator. Note that, here, "substantially not containing" means that the inclusion of a trace amount is permitted as long as it does not adversely affect the storage stability and does not affect the effects of the present invention.
[0048] On the other hand, in the case of the two-paste type, any initiator that can polymerize and harden the A component can be used without any restrictions, and known polymerization initiators can be used. For example, radical polymerization initiators used in the dental field include chemical polymerization initiators (room temperature redox initiators), photopolymerization initiators, thermal polymerization initiators, etc., and these can be used alone or in combination. In the case of the two-paste type, it is preferable to distribute the polymerization initiator so that polymerization starts when the two pastes are mixed, from the viewpoint of storage stability.
[0049] A chemical polymerization initiator is a polymerization initiator that consists of two or more components, and generates polymerization active species at around room temperature by mixing all the components just before use. Representative examples of such chemical polymerization initiators are organic peroxide / amine compound-based ones.
[0050] Representative examples of organic peroxides used as such chemical polymerization initiators include ketone peroxides, peroxyketals, hydroperoxides, diaryl peroxides, peroxy esters, diacyl peroxides, and peroxydicarbonates. Specific examples include methyl ethyl ketone peroxide, cyclohexano peroxide, p-methane hydroperoxide, diisopropylbenzene peroxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, benzoyl peroxide, di-n-propyl peroxydicarbonate, and 1,1,3,3-tetramethylbutyl peroxyneodecanoate.
[0051] The suitable amount of these organic peroxides to be used varies depending on the type of organic peroxide used and cannot be generally limited, but it is preferable to use 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of component A. In addition, when component A is divided into two compositions in the two paste type, the amount of component A may be appropriately determined by taking the total amount of (meth)acrylic acid-based polymerizable monomers contained in the two compositions as 100 parts by mass. The same applies to the case where the amount of each composition to be used is specified relative to the mass of component A.
[0052] As the tertiary amine for generating radicals upon contact with these organic peroxides, any known compound can be used without any particular limitation. Specific examples of tertiary amine compounds that can be suitably used include anilines such as N,N-dimethylaniline, N,N-diethylaniline, N,N-dipropylaniline, N,N-dibutylaniline, and N-methyl,N-β-hydroxyethylaniline; toluidines such as N,N-dimethyl-p-toluidine, N,N-diethyl-p-toluidine, N,N-dipropyl-p-toluidine, N,N-dibutyl-p-toluidine, p-tolyldiethanolamine, and p-tolyldipropanolamine; anisidines such as N,N-dimethyl-anisidine, N,N-diethyl-p-anisidine, N,N-dipropyl-p-anisidine, and N,N-dibutyl-p-anisidine; morpholines such as N-phenylmorpholine and N-tolylmorpholine; bis(N,N-dimethylaminophenyl)methane; and bis(N,N-dimethylaminophenyl)ether. These amine compounds may be used as salts with organic acids such as hydrochloric acid, phosphoric acid, acetic acid, propionic acid, etc. Among the above tertiary amine compounds, N,N-diethyl-p-toluidine, N,N-dipropyl-p-toluidine, p-tolyldiethanolamine, and p-tolyldipropanolamine are preferably used from the viewpoints of high polymerization activity, low irritation, and low odor.
[0053] The amount of the tertiary amine compound used is preferably within a range from 0.05 to 5 parts by mass, and more preferably from 0.1 to 3 parts by mass, per 100 parts by mass of the component A.
[0054] Specific examples of the photopolymerization initiator include benzoin alkyl ethers such as benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether; benzil ketals such as benzil dimethyl ketal and benzil diethyl ketal; diaryl ketones such as benzophenone, anthraquinone, and thioxanthone; α-diketones such as diacetyl, benzil, camphorquinone, and 9,10-phenanthraquinone; and bisacylphosphine oxides such as bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. These can be used alone or in combination of different types.
[0055] The photopolymerization initiator is preferably used in combination with a reducing compound. Suitable reducing compounds include tertiary amines such as 2-(dimethylamino)ethyl methacrylate, ethyl pN,N-dimethylaminobenzoate, N-methyldiethanolamine, dimethylaminobenzaldehyde, and terephthalaldehyde; sulfur-containing compounds such as 2-mercaptobenzoxazole, 1-decanethiol, thiosalicylic acid, and thiobenzoic acid; and N-phenylalanine.
[0056] In addition, in order to further enhance the activity of the photopolymerization initiator, it is also a preferred embodiment to add a photoacid generator. Examples of photoacid generators include diaryliodonium salt compounds, sulfonium salt compounds, sulfonic acid ester compounds, halomethyl-substituted S-triazine conductors, and pyridinium salt compounds. When a photoacid generator is used, the photopolymerization initiator is preferably an α-diketone such as camphorquinone, and more preferably a reducing compound such as ethyl pN,N-dimethylaminobenzoate is used in combination.
[0057] Examples of the thermal polymerization initiator include peroxides such as benzoyl peroxide, p-chlorobenzoyl peroxide, tert-butylperoxy-2-ethylhexanoate, tert-butylperoxydicarbonate, and diisopropylperoxydicarbonate, and azo compounds such as azobisisobutyronitrile.
[0058] The blending amount of the photopolymerization initiator and the thermal polymerization initiator may be the amount of the polymerization initiator used when the photopolymerization initiator or the thermal polymerization initiator is used alone, or the total amount of the polymerization initiators when the photopolymerization initiator and the thermal polymerization initiator are used in combination, as long as it is a catalytic amount (i.e., an amount that can function as a polymerization initiator and perform sufficient polymerization). The specific amount varies depending on the type of polymerization initiator used and cannot be generally limited, but it is preferably used in the range of 0.05 to 5 parts by mass, and more preferably used in the range of 0.1 to 3 parts by mass, relative to 100 parts by mass of the A component.
[0059] The amount of the reducing agent or photoacid generator used is preferably within a range from 0.05 to 5 parts by mass, and more preferably from 0.1 to 3 parts by mass, per 100 parts by mass of the component A.
[0060] Furthermore, in the production method of the present invention, inorganic fillers such as calcium carbonate, magnesium oxide, barium sulfate, titanium oxide, potassium titanate, aluminum hydroxide, silica powder, glass powder, diatomaceous earth, silica, calcium silicate, talc, alumina, mica, and quartz glass; granular organic-inorganic composite fillers obtained by adding a polymerizable monomer to inorganic particles in advance, forming a paste, polymerizing the resulting mixture, and pulverizing the mixture; polymerization inhibitors such as butylhydroxytoluene and methoxyhydroquinone; ultraviolet absorbers such as 4-methoxy-2-hydroxybenzophenone and 2-(2-benzotriazole)-p-cresol; polymerization regulators such as α-methylstyrene dimer; colorants, pigments, fragrances, and the like can be added within a range that does not impair the effects of the present invention.
[0061] 2. The manufacturing method of the present invention As described above, the production method of the present invention includes the steps of: Mix component A (monomer) and component B (soluble non-crosslinked polymer) at a specified temperature: T MIX (° C.) to obtain a liquid composition in which component B is dissolved in component A; and a second step of mixing and kneading the liquid composition obtained in the first step with component C (monomer-absorbent porous crosslinked polymer) to obtain a paste-like composition.
[0062] 2-1.First step In the first step, component A (monomer) and component B (soluble non-crosslinked polymer) are mixed at a predetermined temperature: T MIX (°C) to obtain a liquid composition in which component B is dissolved in component A. In order to prevent undissolved component B from remaining in the intended paste-like hardenable composition for denture base, which is the intended product, and thus preventing the desired paste properties from being obtained, Component B is mixed in an amount of 5 to 40 (parts by mass) per 100 (parts by mass) of component A, and Temperature:T MIX A component in for Component B of Amount below the saturated solubility powder The solid B component is dispersed in A component while dissolving B component.
[0063] The mixing temperature is usually a temperature above room temperature, but when dissolving the B component, if the B component is difficult to dissolve, it is preferable to set the temperature at 45 to 60°C. If it is determined that stirring is difficult due to an increase in the viscosity of the mixed liquid, the stirring can be stopped and the mixed liquid can be kept warm to dissolve the B component. The temperature at which the B component is kept warm is preferably about the same as the temperature at which the B component is stirred and dissolved. When dissolving is performed at such a temperature, if dissolution is completely completed, usually, precipitation of the B component does not occur even if it is cooled to room temperature. After keeping warm, visually check that there is no remaining dissolution at 25°C, and if there is any remaining dissolution, keep warm until all of it is dissolved. It is preferable to keep warm for a certain period of time even if dissolution of the A component is confirmed by stirring alone.
[0064] The first step preferably includes the following dispersing step and dissolving step, because this allows the component B to be efficiently dissolved in the component A.
[0065] Dispersion process: Component A or a part of component A is used as a dispersion medium. for B component of The saturated dissolution amount is at the temperature: T MIX In the A component Against Component B of The dispersion medium and the condition that the amount of the solubility is less than the saturated solubility are used. powder The dispersion medium is mixed with component B in the form of a solid. powder This is a process for obtaining a dispersion liquid in which component B in a solid form is dispersed.
[0066] Dissolving step: The dispersion obtained in the dispersing step is mixed with the total amount of component A. powder The total amount of B component in the solid state is contained, and the temperature of the system is T MIX A process for dissolving component B so that the resulting solution is in the above-mentioned state.
[0067] Further, because it is possible to efficiently obtain a liquid composition in which component B is dissolved in component A in a short time, the maximum amount (parts by mass) of component B that is soluble in 100 parts by mass of a (meth)acrylic acid-based polymerizable monomer component that is liquid at room temperature and normal pressure and has a predetermined composition at a predetermined temperature is added to the polymerizable monomer component at the predetermined temperature. for B component of When the solubility is calculated, the component A or a part of the component A which serves as a dispersion medium in the dispersion step is for B component of The dispersant is dissolved in water at a temperature where the solubility is 5 or less. powder The dispersion medium is mixed with component B in the form of a solid. powder It is preferable to obtain a dispersion in which component B is dispersed in a solid form.
[0068] Specifically, it is preferable to employ the method shown in (1) or (2) below.
[0069] (1) Component A for B component of At a temperature where the solubility is 5 or less, powder Mix the body-shaped B component powder After dispersing the solid component B, the temperature of the mixture is increased to T MIX By increasing the concentration to powder A method in which component B is dissolved while dispersing the viscous component B.
[0070] (2) As component A, T MIX A component A1 is a (meth)acrylic acid-based polymerizable monomer having a solubility of component B of 5 or less in T MIX and a mixture of A2 component consisting of a (meth)acrylic acid-based polymerizable monomer having a solubility of B component in the range of 5 or more, powder After preparing a dispersion liquid in which the solid B component is dispersed, the dispersion liquid and A2 component are mixed under stirring. MIX By mixing with powder A method in which component B is dissolved while dispersing the viscous component B.
[0071] The liquid composition obtained in the first step usually has a loss tangent at 23° C.: tanδ (23)is in the range of 1.0 to 3.0, preferably 1.5 to 3.0, and a hardenable composition for a denture base obtained by using the liquid composition has good paste properties. The loss tangent tan δ is the ratio of the storage elastic modulus to the loss elastic modulus, and the larger the loss elastic modulus is, that is, the higher the viscosity of the substance is, the larger tan δ is. When tan δ is smaller than 1.0, the elasticity is strong. The tan δ of the liquid composition (23) The value can be measured using a modular compact rheometer MCR302 (manufactured by Anton Paar).
[0072] When the aforementioned polymerization initiator, polymerization inhibitor, ultraviolet absorber, or the like is used as other components, these components may be added at any stage. However, it is preferable to dissolve these components in component A before mixing components A and B in the first step.
[0073] 2-2.Second process In the second step, the liquid composition obtained in the first step and component C (monomer-absorbent porous crosslinked polymer) are mixed and kneaded to obtain a paste-like composition.
[0074] When the liquid composition obtained in the first step and component C are mixed under stirring at room temperature and normal pressure, the mixture becomes generally mochi-like and can be seen to be cohesive, but the time required for this varies depending on the combination of monomers and monomer-absorbent porous crosslinked polymers used. In order to minimize unevenness in the paste, it is preferable to continue kneading for another 10 minutes or more after confirming with the naked eye that the paste has become homogenous. In addition, if the paste obtained is too hard or too soft, the paste properties can be controlled by adding the liquid composition or component C as appropriate. Since the paste after kneading contains air bubbles, it is preferable to defoam it under vacuum conditions. By the above method, a one-paste type hardening composition for denture base can be produced.
[0075] When the filler described above is used as another component, the filler may be added at any stage, but is preferably added at the same time as mixing the liquid composition and component C in the second step.
[0076] The manufacturing method of the present invention is not limited to the manufacture of a one-paste type hardenable composition for a denture base, but can also be applied to the manufacture of a two-paste type hardenable composition for a denture base, in which when two pastes are made into a first composition and a second composition, respectively, components A, B, and C are contained in both compositions, or can be applied as a manufacturing method for one of the compositions when only one of the compositions contains the three components A to C.
[0077] 3. Hardenable composition for denture base obtained by the method of the present invention 3-1. Storage method The paste-like denture base hardenable composition produced by the production method of the present invention is preferably stored in a light-shielding container to prevent deterioration during storage, particularly when a photopolymerization initiator is used. The paste form is not particularly limited, and may be molded into a rod, horseshoe, sheet, sphere, prism, or the like and stored in a container, or may be stored in a tube or bottle without being molded.
[0078] 3-2.How to use When the hardenable composition for denture base obtained by the production method of the present invention is used as a denture base resin, a hard lining material, or a repair resin, it can be used by a known method.
[0079] When making a new denture using the one-paste type, an impression of the patient's mouth is taken and a plaster model is made. The denture base is formed on the plaster model using the hardenable denture base composition produced according to the present invention. The model is then set in an articulator and the artificial teeth are aligned. The model is then polymerized and hardened by light irradiation or heat, and the denture is then prepared by performing shape correction and polishing.
[0080] When making a new denture using the two-paste type, an impression of the patient's mouth is taken and a plaster model is made. On the plaster model, a denture base is formed using a denture base hardening composition which is a mixture of both the first composition and / or the second composition produced by the present invention. The model is then set in an articulator and the artificial teeth are aligned. After that, if a photopolymerization catalyst or a thermal polymerization catalyst is used, the model is polymerized and hardened by irradiation with light or heat, and shape correction and polishing are performed to prepare the denture.
[0081] When repairing a poorly fitting denture, adhesive and separating materials are applied as necessary to the denture that no longer fits in the patient's mouth, paste (a paste made by mixing the first and second compositions in the case of a two-paste type) is applied and adjusted to fit the patient's mouth, and then, if a photopolymerization catalyst or thermal polymerization catalyst is used, it is polymerized and hardened by exposure to light or heat, and the shape is corrected and polished to improve the fit of the denture. When lining the mucosal surface, a thin layer of paste can be applied, and when extending the base, a rod-shaped paste can be applied by wrapping it around the denture. EXAMPLES
[0082] EXAMPLES In order to specifically explain the present invention, examples and comparative examples will be given below, but the present invention is not limited to these in any way.
[0083] 1. Regarding the various compounds used in the examples and comparative examples The names, characteristics, and abbreviations (when abbreviations are used) of the various compounds used in each Example and Comparative Example are shown below.
[0084] 1-1. Component A: (meth)acrylic acid-based polymerizable monomer HPr: 2-methacryloyloxyethyl propionate (monofunctional polymerizable monomer) ND: Nonamethylenediol dimethacrylate (bifunctional polymerizable monomer) UDMA: 1,6-bis(methacryloyloxycarbonylamino)trimethylhexane ·TT: Trimethylolpropane trimethacrylate (trifunctional polymerizable monomer).
[0085] 1-2. Component B: Soluble non-crosslinked polymer powder body PMMA: Polymethyl methacrylate (average particle size (d): 20 μm, weight average molecular weight (Mw): 250,000) PEMA: Polyethyl methacrylate (d: 35 μm, Mw 500,000) P(EMA-MMA): Polyethyl methacrylate-methyl methacrylate copolymer (ethyl methacrylate / methyl methacrylate=50 / 50, d: 40μm, Mw: 1 million) ·PBMA: Polybutyl methacrylate (d: 60μm, Mw: 150,000).
[0086] 1-3. Component C: Monomer-absorbent porous organic cross-linked polymer powder body The abbreviations, components, average particle size, and average pore size of the polymers used (all manufactured by Sekisui Plastics) are shown in Table 1.
[0087] [Table 1]
[0088] 1-4. Polymerization initiator CQ: Camphorquinone ·BPO: Benzoyl peroxide DMBE: Ethyl 4-(N,N-dimethylamino)benzoate ·DEPT: N,N-Diethyl-p-toluidine.
[0089] 1-4.Non-porous organic cross-linked polymers PMMA-X: Polymethyl methacrylate (d: 8μm, manufactured by Sekisui Chemical Industry Co., Ltd.).
[0090] 2. Examples and Comparative Examples Example 1 (1) Raw materials A mixture of 50 parts by mass of HPr and 50 parts by mass of ND was used as Component A, PEMA was used as Component B, and PMMA-P8 was used as Component C. Also, CQ and DMBE were used as polymerization initiators. The composition of the curable composition for denture base, which is the production target, is summarized in Table 2.
[0091] Note that for Component A at the mixing temperature for the above-mentioned Component B of Regarding solubility, it was evaluated as being either equal to or greater than a certain value, or less than a certain value, for the sake of convenience. Specifically, a predetermined amount: X parts by mass of Component B was used with respect to 100 parts by mass of Component A, and stirring was carried out for 3 hours using a stirrer at the mixing temperature, and the presence or absence of undissolved residue was visually confirmed. When there was no undissolved residue and it was completely dissolved, the above solubility was X or more, and when undissolved residue was confirmed, the solubility was less than X. The former (X or more) was denoted as "X<", and the latter (less than X) was denoted as "<X". When visual confirmation was carried out at X = 25 parts by mass in accordance with this method, since there was no undissolved residue, the above-mentioned Component A for the above-mentioned Component B of the solubility can be said to be 25 or more (25<).
[0092] Also, when the monomer absorption amount R of PMMA-P8, which is Component C, with respect to the above-mentioned Component A was measured by the following method, it was 2.4. Note that the blending amount of Component C was 50 parts by mass, and it was within the range of 65 / R = 27.1 to 165 / R = 68.8.
[0093] [Method for Measuring Monomer Absorption Amount] In the refined linseed oil method described in JIS K5101-13-1, the part where refined linseed oil is used was replaced with Component A used in each example or comparative example (when a plurality of monomers were mixed and used, a monomer mixture of the same composition) for measurement. Specifically, a predetermined amount (g) [M BThe C component (g) [M (g)] was placed on a glass plate, and the A component monomer was gradually added from a burette, 4 or 5 drops at a time, each time kneading the monomer into the polymer with a palette knife. This process was repeated until a mass of monomer and polymer was formed, after which one drop at a time was added, and the process was repeated until the paste became smooth and hard, and the amount of A component monomer (g) [M (g)] used until the end point was determined. A The time required for the operation to reach the end point was set within 25 minutes.
[0094] The above M B (g) and M A Based on (g), the following formula Monomer absorption amount R=M A (g) / M B (g) The monomer absorption was calculated according to the following:
[0095] (2) First step Mixing temperature (T MIX ) was brought to room temperature, 25° C., and a liquid composition in which the component B was dissolved in the component A was prepared as follows. That is, 8g of HPr and 8g of ND were added as component A to a screw tube bottle (25ml) containing a stirrer, and 80mg of CQ (0.5 parts by mass relative to 100 parts by mass of component A) and 80mg of DMBE (0.5 parts by mass relative to 100 parts by mass of component A) were added as polymerization initiators, and these were stirred at room temperature and normal pressure {25°C, 1 atm (≒1013hPa)}, while adding 4g of PEMA (25 parts by mass relative to 100 parts by mass of component A) as component B little by little so as not to cause aggregation, and the entire amount of component B was added, and stirring was continued until the solution became uniform. After that, the resulting mixture was kept warm in a 45°C incubator for 2 hours, and after natural cooling to 25°C, it was confirmed by visual inspection that there was no remaining residue. In addition, the above-mentioned component A for The component B of Since the solubility is 25 or more, it can be said that the saturated solubility of the component B in 16 g of the component A is 4 g or more.
[0096] (3) Loss tangent of liquid composition: tan δ measurement The liquid composition thus obtained was measured using a modular compact rheometer MCR302 (manufactured by Anton Paar) with a cone plate of 20 mm diameter and 1° angle at a frequency of 1 Hz, a measurement temperature of 23° C., and a shear strain (vibration) of 0.1%, and the tan δ was evaluated to be 1.7. Note that the average value from 60 seconds after the start of the measurement when the measurement was performed for 5 minutes under the above conditions was taken as the loss tangent: tan δ of the liquid composition.
[0097] (4) Second step 19 g of the liquid composition obtained in the first step was transferred to a mortar, 7.5 g (50 parts by mass relative to 100 parts by mass of component A) of PMMA-P8 as component C was added thereto, and mixed with a pestle for 10 minutes at 25° C. After mixing, it was visually confirmed that a uniform paste had been formed, and the paste obtained after further mixing for 10 minutes was degassed under vacuum conditions to obtain a paste-like hardenable composition for denture bases.
[0098] (5) Manufacturing time The time required for the first step was 3 hours and 30 minutes, and the time required for the second step (the time required to complete the final degassing of the paste) was 30 minutes, and the total production time for both steps was 4.0 hours.
[0099] (6) Evaluation of hardenable paste-type denture base composition The denture base hardening composition obtained in the second step was evaluated for paste hardness, paste adhesion, and paste properties after one month, and the hardened product was evaluated for bending strength, elastic modulus, and breaking energy. The evaluation methods are shown below.
[0100] [Paste hardness evaluation method] The paste (denture base hardening composition) was loaded into a SUS nut-shaped mold, the surface was smoothed, and the paste was left for 2 minutes in the dark to maintain a constant temperature of 23° C. A SUS rod with a diameter (Φ) of 5 mm was attached as a pressure-sensitive shaft to a Sun Rheometer CR-150 (manufactured by Sun Scientific Co., Ltd.), and the maximum load [g] when the paste was compressed to a depth of 2 mm at a speed of 240 mm / min was recorded as the paste hardness.
[0101] [Paste adhesion evaluation method] Wearing gloves, the paste (denture base hardenable composition) was evaluated according to the following criteria, with a rating of ⊚ to ×. ◎: Does not adhere to gloves, but adheres to dentures and plaster △: Adheres to gloves, but can be removed from gloves when attached to dentures or plaster ×: Adheres to gloves, does not stick to dentures or plaster. Does not adhere to gloves, does not stick to plaster. Does not stick.
[0102] [How to evaluate paste properties after one month] The paste (denture base hardenable composition) was stored at 23° C. for one month and evaluated according to the following criteria from ⊚ to ×. ◎: No change from immediately after paste preparation △: There is a slight change in viscosity immediately after the paste is prepared. ×: There is a significant change in viscosity immediately after the paste is prepared.
[0103] [Methods for evaluating bending strength, elastic modulus, and breaking energy of hardened materials] A 30×30×2 mm polytetrafluoroethylene mold was filled with the paste (denture base hardening composition), and when a photopolymerization catalyst was used, both sides were pressed with polyethylene film and then irradiated with light for 5 minutes using a dental laboratory photopolymerization device α Light V (Morita Co., Ltd.) to produce a hardened body. When a thermal polymerization catalyst was used, both sides were pressed with polyethylene film and then immersed in water, boiled, and heated for 1 hour to produce a hardened body. When a chemical polymerization catalyst was used, both sides were pressed with polyethylene film and then hardened to produce a hardened body. The hardened body was then polished with #800 and #1500 waterproof abrasive paper, and then cut into a 4×30×2 mm square column shape. The obtained hardened body was immersed in water and left at 37°C for 24 hours. The test piece was attached to a testing machine (Shimadzu Corporation, Autograph AG-1) and a three-point bending test was performed with a support distance of 20 mm and a crosshead speed of 1 mm / min to measure bending strength, elastic modulus, and breaking energy.
[0104] The results of these evaluations are shown in Tables 3 and 4. As shown in Tables 3 and 4, the paste had good properties, did not adhere to gloves, and adhered to dentures and plaster. The paste properties after one month did not change from those immediately after preparation, and the storage stability was excellent. In addition, the bending strength of the hardened body was 78 MPa and the breaking energy was 90 N mm, both of which were high, confirming that the paste has high strength and toughness.
[0105] [Table 2]
[0106] [Table 3]
[0107] [Table 4]
[0108] Examples 2 to 7, 9 to 16 A hardenable composition for denture base was produced in the same manner as in Example 1, except that the paste composition was changed as shown in Table 2. In all Examples, component B was completely dissolved at the mixing temperature. In Table 2, "↑" means "same as above," and the numbers in parentheses () indicate parts by mass. The obtained hardenable composition for denture base was evaluated in the same manner as in Example 1. The results are shown in Tables 3 and 4.
[0109] All of Examples 2 to 7 and 9 to 16 had high strength and toughness, and the pastes were also excellent in operability and storage stability.
[0110] Example 8 The composition of the paste was changed as shown in Table 2, and the mixing of the A component, the B component, and the polymerization initiator in the manufacturing method of Example 1 was performed by heating to a temperature of 55° C. (T MIX A hardenable composition for denture base was produced and evaluated in the same manner as in Example 1, except that the temperature was adjusted to 55° C. (at 55° C.) and the resulting mixed solution was kept in an incubator at 55° C. for 2 hours. The results are shown in Tables 3 and 4.
[0111] Although the component B used in Example 8 is difficult to dissolve in the component A at room temperature, it was completely dissolved by mixing while heating, and the dissolved state was maintained even at room temperature (25° C.). A paste excellent in paste operability and storage stability was obtained, and it also had high strength and toughness.
[0112] Example 17 As shown in Table 2, the two pastes were designated the first composition (a) and the second composition (b), and each composition was produced and evaluated in the same manner as in Example 1. The bending strength, elastic modulus, and breaking energy were the physical properties of the hardened body obtained by mixing Examples 17(a) and (b). The results are shown in Tables 3 and 4.
[0113] Example 17 is a two-paste type hardenable composition for a denture base, which, like the one-paste type, had high strength and toughness, and was also excellent in paste handling and storage stability.
[0114] Example 18 The composition of the paste was the same as in Example 1, and in the liquid composition preparation process, component A and a polymerization initiator were added to a screw tube bottle (25 ml) and stirred at room temperature and normal pressure, and then the mixture was cooled to 2°C, and while maintaining the temperature at 2°C, component B was added and stirred until component B was uniformly dispersed. At this time, the solubility of component B in component A at 2°C was less than 5. After that, the mixture was stirred again at room temperature and normal pressure until it became uniform, and the production and evaluation were performed in the same manner as in Example 1. The results are shown in Tables 3 and 4.
[0115] In Example 18, component A was cooled and mixed under conditions where the solubility of component B was less than 5. This allowed component B to be dispersed quickly and uniformly in component A, and the time required for the first step was significantly reduced to 2 hours and 30 minutes, thereby shortening the production time.
[0116] Example 19 The composition of the paste was the same as in Example 1, and in the liquid composition preparation process, component B, CQ, and ND of component A were added to a screw tube bottle and stirred until component B was uniformly dispersed. Then, the other component A, HPr, was added, and the mixture was stirred until it became uniform. Except for this, the production and evaluation were performed in the same manner as in Example 1. The results are shown in Tables 3 and 4. The solubility of component B in ND at 25°C was less than 5, and the solubility in HPr was 25 or more.
[0117] In Example 19, by adding component B to ND, which is one of component A in which the solubility of component B at 25°C is less than 5, component B was quickly and uniformly dispersed in component A, and the time required for the first step was significantly shortened to 2 hours and 30 minutes, leading to a reduction in production time.
[0118] Comparative Example 1 In a screw cap (25 ml) containing a stirrer, 8 g of HPr and 8 g of ND were added as component A, 4 g of PEMA (25 parts by mass relative to 100 parts by mass of component A) as component B, 8 g of PMMA-P8 (50 parts by mass relative to 100 parts by mass of component A) as component C, 80 mg of CQ (0.5 parts by mass relative to 100 parts by mass of component A) as a polymerization initiator, and 80 mg of DMBE (0.5 parts by mass relative to 100 parts by mass of component A) were added in that order, and the mixture was stirred for 30 minutes at room temperature and normal pressure. The viscosity of the mixture increased and stirring became difficult, so the mixture was added to a mortar and mixed with a pestle at room temperature and normal pressure for 10 minutes to obtain a paste-like hardening composition for denture base. Evaluation was performed in the same manner as in Example 1. The results are shown in Tables 3 and 4.
[0119] In Comparative Example 1, the paste was produced in one step, so that component B remained and the paste properties changed significantly when stored for a long period of time.
[0120] Comparative Example 2 A hardenable composition for denture base was produced and evaluated in the same manner as in Example 1, except that 8 g of HPr and 8 g of ND as component A, 80 mg of CQ (0.5 parts by mass relative to 100 parts by mass of component A) and 80 mg of DMBE (0.5 parts by mass relative to 100 parts by mass of component A) as polymerization initiators were added to a screw cap bottle (25 ml) containing a stirrer, and 4 g of PEMA (25 parts by mass relative to 100 parts by mass of component A) as component B was added all at once while stirring at room temperature and normal pressure. The results are shown in Tables 3 and 4.
[0121] In Comparative Example 2, the non-crosslinked polymer, which is component B, was added all at once, and as a result, component B aggregated instead of being dispersed in component A, and it took a long time to dissolve. In addition, component B remained, and the paste properties changed significantly when stored for a long period of time.
[0122] Comparative Example 3 A hardenable composition for a denture base was produced and evaluated in the same manner as in Example 1, except that the composition of the paste was changed as shown in Table 2. The results are shown in Tables 3 and 4.
[0123] In Comparative Example 3, a non-porous organic cross-linked polymer was used instead of the porous organic cross-linked polymer (component C), so the strength of the cured body was low and the paste properties after one month had changed significantly from immediately after preparation.
Claims
1. Component A: a component consisting of a (meth)acrylic acid-based polymerizable monomer that is liquid at room temperature and normal pressure; Component B: a component consisting of a (meth)acrylic acid-based non-crosslinked polymer that is soluble in component A; and Component C: a component consisting of a porous organic crosslinked polymer capable of absorbing component A; A method for producing a paste-like hardenable composition for a denture base comprising: The A component and the B component are mixed at a predetermined temperature: T MIX (° C.) to obtain a liquid composition in which component B is dissolved in component A; A second step of mixing and kneading the liquid composition obtained in the first step with component C to obtain a paste-like composition; Includes In the first step, the component B is mixed with 100 parts by mass of the component A at a temperature of T MIX While dispersing powdered B component in A component in an amount equal to or less than the saturated solubility amount of B component in A component, B component is dissolved; In the second step, the C component is mixed and kneaded in an amount of 65 / R to 165 / R (parts by mass) when the amount (parts by mass) of the A component absorbed per unit amount (parts by mass) of the C component measured in accordance with JIS K5101-13-1 is defined as the absorption amount R (parts by mass of the A component / parts by mass of the C component); A method for producing a paste-like hardenable composition for denture base, comprising the steps of:
2. The first step comprises: Component A or a part of component A is used as a dispersion medium, and the saturated dissolution amount of component B in the dispersion medium is at a temperature of T MIX a dispersing step of mixing the dispersion medium with the powdered B component under conditions such that the saturated solubility of the B component in the A component is less than the saturated solubility of the B component in the A component in the dispersion medium to obtain a dispersion liquid in which the powdered B component is dispersed in the dispersion medium; and The dispersion obtained in the dispersing step contains the entire amount of the A component and the entire amount of the powdery B component, and the temperature of the system is T MIX a dissolving step of dissolving component B in such a state that A method for producing the paste-like hardenable composition for denture base according to claim 1, comprising:
3. When the maximum amount (parts by mass) of component B soluble in 100 parts by mass of a (meth)acrylic acid-based polymerizable monomer component that is liquid at room temperature and normal pressure and has a predetermined composition at a predetermined temperature is taken as the solubility of component B in the polymerizable monomer component at the predetermined temperature, In the dispersing step, the dispersion medium and the powdered B component are mixed at a temperature at which the solubility of the B component in the A component or a part of the A component serving as the dispersion medium is 5 or less, thereby obtaining a dispersion liquid in which the powdered B component is dispersed in the dispersion medium. A method for producing the paste-like hardenable composition for denture base according to claim 2.
4. As the A component, T MIX A component A1 is a (meth)acrylic acid-based polymerizable monomer having a solubility of component B of 5 or less in T MIX and a component A2 consisting of a (meth)acrylic acid-based polymerizable monomer having a solubility of component B exceeding 5 in In the dispersing step, a dispersion liquid is obtained in which a powdery B component is dispersed in an A1 component using an A1 component as a dispersion medium, In the dissolving step, the dispersion liquid and the A2 component are mixed to form a state containing the entire amount of the A component and the entire amount of the powdery B component, and then the mixture is heated to a temperature of T MIX Dissolve component B in A method for producing the paste-like hardenable composition for denture base according to claim 3.
Citation Information
Patent Citations
Japanese syllabary-based calling device
JP1992042364A
Material for crown or material for denture base
JP1999335222A
Repair material composition for denture base
JP2000175941A
Resin material for dental plate
JP2000254152A
Resin composition for dental tooth plate
JP2002104912A