Laminate and electronic component made of same

A curable hot melt silicone composition with controlled viscosity is used to create a void-free, stress-relaxing laminate for electronic components, addressing void and stress issues in large-area bonding and sealing.

JP7560231B2Active Publication Date: 2024-10-02DOW TORAY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020218374
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-28
Publication Date
2024-10-02
Estimated Expiration
2040-12-28

AI Technical Summary

Technical Problem

Existing methods for sealing or bonding large areas in electronic components using curable silicone compositions face challenges such as void formation, bubble removal complexity, and stress due to thermal expansion coefficient mismatch, leading to issues like warping and burrs.

Method used

A laminate structure using a curable hot melt silicone composition with specific properties, including a melt viscosity of 5000 Pa·s or less at 100°C, interposed between substrates, which is applied under reduced pressure and heated to form a void-free, stress-relaxing adhesive layer.

Benefits of technology

The laminate achieves void-free bonding with reduced stress, preventing warping and burrs, and allows for seamless adhesion to uneven surfaces, even with large areas, while maintaining excellent thermal resistance and flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560231000009
    Figure 0007560231000009
  • Figure 0007560231000010
    Figure 0007560231000010
  • Figure 0007560231000011
    Figure 0007560231000011
Patent Text Reader

Abstract

To provide a laminate comprising a substrate, and a flat silicone encapsulation layer which is adhered to the substrate and includes no void or the like, and a laminate in which, two substrates of a same kind or different kinds are adhered through a silicone layer which is held therebetween and includes no void or the like, and to provide a laminate which is formed by using a curable hot melt silicone composition layer having a specific composition, therefore in which stress is hardly applied to the substrate even after the composition is cured, and an electronic device having low stress and being formed of the laminate.SOLUTION: There is provided a laminate comprising: a substrate; and an organopolysiloxane resin including by at least 20 mol% of a whole siloxane unit, a siloxane unit selected from a group formed of a T unit and Q unit adhered to the substrate, and the laminate including a curable hot melt silicone composition layer in which melt viscosity at 100°C measured at a pressure of 2.5 MPa by a flow tester is 5000 Pa s or smaller.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate comprising one or two substrates and a curable hot-melt silicone composition layer adhered to the substrate, and a multi-layer laminate which may further comprise a functional layer. The laminate of the present invention includes a laminate comprising one substrate and a curable hot-melt silicone composition layer in contact therewith, and a laminate comprising two identical or different substrates and a curable hot-melt silicone composition layer interposed therebetween. The substrate may be, in particular, a substrate for an electronic device, for example, a semiconductor substrate or an electronic circuit board on which a semiconductor element is mounted. The laminate of the present invention can be produced by a simple method and at low cost by using the curable hot-melt silicone composition of the present invention, and the silicone layer of the obtained laminate has a feature that it has no or very few defects such as voids. In addition, the cured product obtained by curing the curable hot-melt silicone composition used in the present invention has excellent stress relaxation properties, so that an electronic part including or consisting of a laminate having little internal stress can be obtained. [Background technology]

[0002] Substrates for electronic devices (e.g., substrates for semiconductor devices, semiconductor devices mounted with semiconductor elements) on which elements used in electronic components are mounted may be sealed with a sealant to protect the elements from the outside and improve their durability. Adhesives may also be used to bond electronic components and substrates for electronic devices. Curable silicone compositions are often used as sealants and adhesives because they form cured products with excellent heat resistance, cold resistance, electrical insulation, weather resistance, water repellency, and transparency.

[0003] When the sealing or adhesive area is not large, a typical method is to apply a curable silicone composition that is liquid at room temperature to the substrate by dispensing, and then to cure the composition to form a sealing layer or adhesive layer. In this specification, room temperature refers to the temperature of the environment in which the person handling the curable silicone composition of the present invention is located. Room temperature generally refers to 0°C to 40°C, particularly 15°C to 30°C, and especially 18°C ​​to 25°C.

[0004] On the other hand, it is known that it becomes difficult to use a curable silicone composition that is liquid at room temperature when the area to be sealed or bonded is large, and when used as a sealant, for example, there are methods such as using compression molding as disclosed in Patent Document 1, or using a dam material to block the flow of the liquid sealant and seal as disclosed in Patent Document 2. However, compression molding causes the sealant to leak out of the substrate, forming so-called burrs after molding, which are difficult to remove, and there are problems such as the high cost of the mold used for molding itself.

[0005] In addition, the dispense recipe using the dam material has the problem that two types of material are required in the first place, and when sealing a large area, the process of removing bubbles that occur after dispensing is complicated.

[0006] Patent Documents 3 and 4 propose a process of sealing a semiconductor element by vacuum lamination using a hot-melt silicone film. However, the silicone film disclosed therein only softens at high temperatures and does not melt completely, so it is not possible to seal while forming a flat surface on an electronic device substrate having fine irregularities by liquefying it, and so a so-called conformal coating has been proposed.

[0007] On the other hand, when a silicone composition is used as an adhesive, there is a similar problem that when the adhesion area is large, it is difficult to completely remove bubbles from the adhesive layer obtained when a liquid curable silicone composition is used.

[0008] In addition, since silicone compositions generally form cured products with a high thermal expansion coefficient, when a large-area substrate is sealed or bonded, the difference in thermal expansion coefficient with the substrate causes a large stress to be applied to the resulting laminate. With the miniaturization of electronic components in recent years, the thickness of substrates has become thinner, and this has led to problems such as the laminate warping due to the generated stress. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 4607429 [Patent Document 2] JP 2014-237834 A [Patent Document 3] International Publication No. 2019 / 049794 [Patent Document 4] International Publication No. 2019 / 049791 Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention aims to provide a laminate comprising a substrate, particularly a semiconductor precursor substrate, a substrate for an electronic device, such as a semiconductor device mounting a semiconductor element, an electronic circuit board, and an electronic circuit mounting board, and a flat silicone sealing layer that is in close contact with the substrate and does not contain voids, etc., as well as a laminate having a structure in which two substrates of the same or different types are bonded together via a silicone layer that does not contain voids, etc. Furthermore, the present invention aims to provide a laminate in which the substrate is less susceptible to stress by using a silicone layer of a specific composition for the sealing layer or adhesive layer of the laminate, and a low-stress electronic device made of the laminate. [Means for solving the problem]

[0011] In one embodiment, the laminate of the present invention is a laminate comprising a substrate and a curable hot-melt silicone composition layer in contact with the substrate, The curable hot melt silicone composition is 1 SiO 3 / 2 (In the formula, R 1 are independently substituted or unsubstituted alkyl, particularly C1-C 12 an alkyl group, preferably a methyl group, or a substituted or unsubstituted aryl, especially a C6-C 20 aryl group, preferably a phenyl group) and SiO 4 / 2 The organopolysiloxane resin contains at least 20 mol % or more of siloxane units selected from the group consisting of siloxane units represented by the following formula (1): The curable hot-melt silicone composition is characterized in that it has a melt viscosity at 100°C (at the ultimate shear rate) of 5000 Pa·s or less, measured at a pressure of 2.5 MPa using a flow tester.

[0012] Another embodiment of the laminate of the present invention has a structure in which a curable hot-melt silicone composition layer is interposed between a first substrate and a second substrate, and the curable hot-melt silicone composition layer is further in contact with the second substrate on the surface opposite to the surface in contact with the first substrate.The laminate of this embodiment is particularly preferably in a structure in which a layer of the curable hot-melt silicone composition is interposed between two substrates arranged in parallel or nearly parallel.Therefore, in the latter case, the laminate has a three-layer structure of (first substrate-curable hot-melt silicone composition layer-second substrate).

[0013] In the above laminate, the curable hot-melt silicone composition layer may be one layer or two or more layers, and when the curable hot-melt silicone composition layer is two or more layers, the composition of the curable hot-melt silicone composition of adjacent layers is different from each other.When the curable hot-melt silicone composition layer is made of two or more different compositions, each layer can have different physical properties, such as different elastic modulus, when the composition is cured.In one embodiment of the present invention, the curable hot-melt silicone composition layer is preferably a single layer made of one kind of curable hot-melt silicone composition.

[0014] In the above laminate, when the laminate contains only one substrate, it is preferable that this substrate is an electronic component or a semiconductor precursor; and when the laminate contains two substrates, first and second, and a curable hot-melt silicone composition layer interposed between them, it is preferable that either one of the two substrates is an electronic component or a semiconductor precursor, or that both of the two substrates are electronic components or semiconductor precursors.

[0015] In one embodiment of the present invention, when the laminate includes two substrates, a first and a second substrate, it is preferred that the first substrate is a substrate that is an electronic component or a semiconductor precursor, and the second substrate is a release film.

[0016] In one embodiment of the present invention, when the laminate includes two substrates, a first and a second substrate, it is preferable that the first substrate and the second substrate are substrates that are the same or different types of electronic components or semiconductor precursors.

[0017] In the above laminate, R of the organopolysiloxane resin 1 SiO 3 / 2 Unit of R 1 is an aryl group, preferably an unsubstituted aryl group, and particularly preferably a phenyl group.

[0018] The curable hot-melt silicone composition for use in the laminate of the present invention comprises at least (A)SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: (B) A linear or branched organopolysiloxane that is liquid or plastic at 25°C. It is particularly preferred that the compound contains

[0019] The curable hot melt silicone composition used in the laminate of the present invention is -1It is particularly preferable that the melt viscosity at 100°C measured using a flow tester is 5000 Pa·s or less.

[0020] The curable hot-melt silicone composition for use in the laminate of the present invention is cured to give a cured product which, within a temperature range of -50°C to 200°C and extending to temperatures of at least 100°C, has a tan δ, defined as the ratio of storage modulus to loss modulus, of at least 0.05, and more preferably at least 0.1.

[0021] Furthermore, it is preferable that the curable hot-melt silicone composition used in the laminate of the present invention has a Shore A hardness of 40 or greater when cured.

[0022] The laminate of the present invention, which has one substrate and a curable hot-melt silicone composition layer in contact with the substrate, can be produced by the following steps: Step 1: a step of placing a sheet or film of a curable hot-melt silicone composition on a substrate placed in a reduced pressure chamber in such a way that the sheet or film can come into contact with the substrate in a subsequent step, or a step of placing a sheet or film of a curable hot-melt silicone composition on a substrate placed in the reduced pressure chamber, or a step of placing a substrate in a reduced pressure chamber with the sheet or film of a curable hot-melt silicone composition placed thereon in advance so that the substrate comes into contact with the substrate; Step 2: reducing the pressure in the vacuum chamber to a predetermined pressure; Step 3: heating the inside of the vacuum chamber under reduced pressure to melt the curable hot-melt silicone composition sheet or film and adhere it to the substrate, and if necessary, applying pressure to either or both of the substrate and the sheet or film after adhesion to pressurize the curable hot-melt silicone composition sheet or film to the substrate; and Step 4: releasing the vacuum within the vacuum chamber and removing from the chamber a laminate comprising a layer selected from the group consisting of a layer made of a curable hot-melt silicone composition, a cured layer and a semi-cured layer thereof, and a substrate in contact with said layer; It is preferable that the laminate is produced by a method comprising the steps of: In step 1, the step of placing a sheet or film made of a curable hot-melt silicone composition on a substrate placed in the chamber so that the substrate is in contact with the substrate can also be carried out after reducing the pressure inside the vacuum chamber.

[0023] Furthermore, among the laminates of the present invention, laminates having a structure in which a curable hot-melt silicone composition layer is interposed between two identical or different substrates are preferably produced by a method comprising, in step 1 of the method for producing a laminate having one substrate and a curable hot-melt silicone composition layer in contact with it as described above, further arranging a second substrate of the same or different type as the substrate (first substrate) on a surface other than the surface that will come into contact with the substrate in a later step or the surface in contact with the substrate, or a second substrate of the same or different type as the substrate (first substrate) on the other surface so as to be in contact with the sheet or film made of the curable hot-melt silicone composition in advance, in a step subsequent to step 1, particularly step 3, the first substrate is pressure-bonded to one surface of the curable hot-melt silicone composition sheet or film and the second substrate is pressure-bonded to the other surface.

[0024] Alternatively, a laminate of the present invention having two identical or different substrates and a curable hot-melt silicone composition layer sandwiched between them can be produced by preparing a laminate comprising a substrate (first substrate) and a curable hot-melt silicone composition layer laminated on one surface of the substrate in accordance with steps 1 to 4 described above, and then laminating a further substrate (second substrate) of the same or different type as the first substrate to the outer surface of the curable hot-melt silicone composition layer that is not in contact with the first substrate in the same manner as steps 1 to 4.

[0025] In one embodiment of the present invention, in the method for producing a laminate of the present invention described above, the temperature when the curable hot-melt silicone composition sheet or film is pressure-bonded to the substrate in step 3 is 50° C. or higher.

[0026] The laminate of the present invention may be produced by any one of the production methods of compression molding, press molding, or vacuum lamination.

[0027] One embodiment of the laminate of the present invention provides a laminate including a cured silicone layer obtained by curing the curable hot-melt silicone composition contained in the laminate described above. This laminate includes both laminates of (substrate-cured silicone layer) and (first substrate-cured silicone layer-second substrate) structures.

[0028] In one embodiment, the laminate of the present invention is an electronic component.

[0029] Furthermore, in one aspect of the present invention, as a means for solving the above problems, there is provided a novel multilayer laminate that can be used as an encapsulating sheet for encapsulating a substrate, for example a board, and this multilayer laminate may have a multilayer structure comprising a curable hot-melt silicone composition layer and a functional layer in contact with at least one surface of the curable hot-melt silicone composition layer. Effect of the Invention

[0030] The laminate of the present invention can be obtained by a simple method and at low cost by laminating the curable hot-melt silicone composition on a substrate and sealing the substrate, or can be produced by bonding two substrates of the same or different types together using a layer of the curable hot-melt silicone composition. Furthermore, the layer of the curable hot-melt silicone composition used in the present invention cures to form a cured product with excellent stress relaxation properties, and is therefore characterized in that it is possible to provide a laminate with small internal stress (and therefore less susceptible to problems such as warping over time) and electronic parts made of or including the laminate. [Brief description of the drawings]

[0031] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a method for producing a laminate of the present invention, which is carried out using a diaphragm-type vacuum laminator and a lamination jig. [Diagram 2] FIG. 2 is a schematic diagram of the apparatus used in the examples for producing the curable hot-melt silicone composition sheets. [Diagram 3] FIG. 3 is a graph illustrating the viscoelastic properties of a cured product of one curable hot-melt silicone composition of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the preferred embodiments. The present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present invention.

[0033] [Laminate] In one embodiment of the present invention, the laminate comprises at least one or more substrates and a curable hot-melt silicone composition layer in contact with the substrate. The substrate may be any substrate that is desired to be sealed or bonded with a silicone resin, but it is particularly preferred to use a substrate for an electronic device, particularly an electronic circuit board or an electronic circuit mounting board, a substrate for a semiconductor device, or a substrate for a semiconductor device carrying a semiconductor element, as the substrate. By using the curable hot-melt silicone composition of the present invention in an appropriate manner, a silicone sealing layer having few or no defects such as voids can be formed on the substrate. In another embodiment of the present invention, the laminate comprises two substrates, a first and a second, and a curable hot-melt silicone composition layer interposed therebetween. In this case, by using the curable hot-melt silicone composition of the present invention in an appropriate manner, a laminate in which two substrates of the same type or different types are bonded via a curable hot-melt silicone composition layer having few or no defects such as voids can be obtained. In this case, one of the two substrates is preferably a substrate for electronic devices, particularly an electronic circuit substrate or a substrate mounted with an electronic circuit, a substrate for semiconductor device, or a substrate for semiconductor device with a semiconductor element mounted thereon, and the other substrate is the same or different substrate selected from the above-mentioned substrates, or a completely different substrate or substrate, for example, a substrate for protecting a substrate for electronic devices, or a peelable protective sheet or film, for example, a protective film or a peelable film. Therefore, the laminate in this case includes a three-layer structure consisting of a first and a second substrate and a curable hot-melt silicone composition adhesive layer interposed between them and bonding the two substrates. In these embodiments, the laminate of the present invention is in a state in which the substrate, for example, a substrate for electronic devices, is temporarily fixed by the curable hot-melt silicone composition layer, and the silicone composition does not decrease in viscosity even when melted in a state in which no pressure is applied as described below, and does not flow due to its own weight, etc., so that the volume change that occurs in the silicone composition during curing is smaller than that of conventional liquid curable silicone compositions. Furthermore, by using a curable hot-melt silicone composition having excellent stress relaxation properties, as described below, it is possible to significantly reduce the stress that occurs in the laminate when the silicone composition cures.

[0034] Furthermore, in this specification, the curable hot-melt silicone composition sheet or film is also referred to simply as an "encapsulating sheet" for ease of description, but it should be noted that this term is used not only when the encapsulating sheet is used as a sealant, but also when it is used as an adhesive. Thus, the "encapsulating sheet" of the present invention includes both when it is used as a sealant and when it is used as an adhesive.

[0035] [Substrates or base materials for electronic devices] The substrate or base material that is a part of the laminate of the present invention is not particularly limited, but is particularly preferably a component used in electronic equipment or a substrate on which such a component is mounted.Examples of such a substrate include, but are not limited to, a substrate for electronic equipment, particularly an electronic circuit substrate or a substrate mounted with an electronic circuit, a substrate for semiconductor equipment, or a substrate for semiconductor equipment that is mounted with a semiconductor element.The cured product obtained by curing the curable hot melt silicone composition used in the present invention has excellent color resistance at high temperatures, so it can be particularly suitably used in the manufacture of a laminate using an optical semiconductor device as a substrate, which requires the transparency of the encapsulant. Therefore, the substrate may be, for example, a substrate on which an electronic circuit is mounted, and may be a substrate for various electronic devices or electronic materials (hereinafter, these are referred to as electronic substrates), such as a plastic substrate typified by a PCB substrate, a metal substrate typified by aluminum, copper, nickel, and silicon, and a ceramic substrate typified by aluminum nitride, alumina, and silicon carbide. With regard to such a laminate having a two-layer structure of an electronic substrate and a silicone layer, the silicone layer is generally called a "sealing layer", and depending on the application of the electronic material, it is often preferable that the surface of the sealing layer is flat. By manufacturing a laminate using a specific silicone layer described below and a specific sealing process, it is possible to make the surface have a flush flatness. Substrates for electronic devices or electronic materials often have circuits mounted thereon, and the substrate surface has irregularities, and in the sealing process, it is necessary to seal the substrate with a silicone layer along the shape of these irregularities without mixing in bubbles. As described below, by using a specific hot-melt silicone composition layer and laminating a curable hot-melt silicone composition layer on the substrate through a specific sealing process, it is possible to fill the gaps formed by the irregularities with silicone without mixing in bubbles.

[0036] On the other hand, the curable hot-melt silicone composition layer of the present invention or a layer obtained by curing the composition may be used as an "adhesive layer" to bond the same or different first and second substrates to form a three-layer laminate having a structure of (first substrate-curable hot-melt silicone composition layer-second substrate). In this case, a substrate selected from the above-mentioned substrates can be used as the substrate, but when such a substrate is used as the first substrate, the second substrate may be a substrate made of a material other than the above-mentioned substrate for electronic devices. As such a substrate, various materials such as glass plates, plastic plates, metal plates, and ceramic plates can be used, and the material can be selected according to the application of the electronic device to be produced. As described above, any material may be used as the substrate, but the surface where the curable hot-melt silicone composition layer and the substrate come into contact with each other, that is, the adhesive surface, should be free of voids and should completely fill the unevenness due to the circuitry of the substrate with the curable silicone composition. For this purpose, it is preferable to apply a layer made of a specific curable hot-melt silicone composition as described below to the substrate by a specific process.

[0037] Whether the laminate has the above-mentioned two-layer structure or three-layer structure, when the laminate is produced using a curable silicone composition that does not have hot melt properties and is liquid at room temperature, it is difficult to remove voids between the substrate and the silicone composition layer, and when the size of the laminate becomes large, it may be impossible to completely remove the voids.In contrast, the present invention uses a curable silicone composition that has hot melt properties, so it is possible to produce a laminate with a two-layer or three-layer structure without voids, regardless of the size of the laminate.

[0038] In addition, generally, any substrate (including substrate) has a low coefficient of thermal expansion, but the coefficient of thermal expansion of the silicone layer laminated on the substrate is high, so that when they are combined to form a laminate, a non-negligible level of stress occurs in the laminate. For this reason, a laminate in which the substrate is temporarily fixed by a layer made of a curable silicone composition having hot melt properties as defined in the present invention (a layer made of a curable hot melt silicone composition) is preferable because it can suppress the generation of stress. In particular, when the substrate 1 and the substrate 2 are different types in a three-layer laminate, the substrate 1 and the substrate 2 usually have different coefficients of thermal expansion, and it is assumed that the layer bonding them is subjected to considerable thermal stress. In order to meet such applications, it is preferable to use a silicone layer having specific cured product properties described below in the laminate of the present invention.

[0039] [Surface treatment of substrate or base material] In order to improve the adhesion between the substrate / substrate and the layer of the curable silicone composition having hot melt properties (the layer of the curable hot melt silicone composition), which is a part of the laminate of the present invention, if desired and within the scope of not impairing the technical effect of the present invention, the surface of the substrate / substrate may be subjected to a surface treatment such as an oxidation method or a roughening method, or a primer treatment, and then a layer of the curable hot melt silicone composition may be laminated. Here, examples of the oxidation method include corona discharge treatment, plasma discharge treatment, chromium oxidation treatment (wet), flame treatment, hot air treatment, ozone treatment, and ultraviolet irradiation treatment, and examples of the roughening method include sandblasting and spraying treatment. These surface treatment methods can be selected appropriately depending on the type of substrate / substrate and the required adhesion, but when a part of the laminate of the present invention is a glass plate, a plastic plate, a metal plate, a ceramic plate, etc., the effects obtained by the surface treatment, particularly the effect of improving adhesion, are high, and the operation is simple, so that the corona discharge treatment method is a preferred method. Such surface treatment can sometimes improve the contact interface adhesion after lamination, in particular the adhesion to the substrate / base material prior to the curing reaction of the layer made of the curable hot-melt silicone composition.

[0040] [Curable hot melt silicone composition] The curable hot melt silicone composition used in the laminate of the present invention is R 1 SiO 3 / 2 (In the formula, R 1 are independently substituted or unsubstituted alkyl, particularly C1-C 12 an alkyl group, preferably a methyl group, or a substituted or unsubstituted aryl, especially a C6-C 20 aryl group, preferably a phenyl group) and SiO 4 / 2 Any curable silicone composition having hot melt properties can be used, as long as it contains an organopolysiloxane resin containing at least 20 mol % or more of all siloxane units selected from the group consisting of siloxane units represented by the following formula: and the curable hot melt silicone composition has a melt viscosity of 5000 Pa·s or less at 100°C (at the limiting shear rate) measured at a pressure of 2.5 MPa using a flow tester. From the viewpoint of filling in the unevenness of the substrate without gaps and bonding the substrate and the silicone composition layer together without bubbles, i.e., without defects such as voids, the preferred melt viscosity under the above conditions is 3000 Pa·s or less, more preferably 1000 Pa·s or less, and even more preferably 500 Pa·s or less.

[0041] However, particularly preferred curable hot melt silicone compositions comprise at least (A)SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: (B) A curable silicone composition having hot melt properties, which contains a linear or branched organopolysiloxane that is liquid or plastic at 25°C.

[0042] Furthermore, the laminate of the present invention has a shear rate of 1 s -1It is preferable to use a curable hot-melt silicone composition having a melt viscosity of 5000 Pa·s or less at 100°C when measured in a liquid state, and a melt viscosity of 500 Pa·s or less at 100°C when measured at a pressure of 2.5 MPa using a flow tester.

[0043] Furthermore, the curable hot-melt silicone composition used in the laminate of the present invention is such that when it is cured, the cured product obtained has a tan δ, which is the ratio of storage modulus to loss modulus, of 0.05 or more, and more preferably 0.1 or more, within a temperature range of -50°C to 200°C and extending to temperatures of 100°C or more.

[0044] Furthermore, the curable hot-melt silicone composition used in the laminate of the present invention is preferably one that, when cured, results in a cured product that has a Shore A hardness of 40 or greater.

[0045] Below, several embodiments of the above-mentioned curable hot melt silicone composition used in the present invention will be described, but the curing reaction of the curable hot melt silicone composition is not limited to a specific reaction, and may be any curing reaction such as curing by hydrosilylation reaction, curing by radical reaction including organic peroxide curing and UV curing, and curing by condensation reaction. An example of a curable hot melt silicone composition that can be used in the present invention is a composition that is composed of at least (A) a curable organopolysiloxane resin and (C) a curing agent and / or (D) a curing catalyst, and optionally contains (B) a linear or branched polyorganosiloxane, (E) a curing retarder, and further (F) other additives such as a functional inorganic filler. The components (A) to (F) will be described below.

[0046] [Component (A)] Component (A) is the main component of the composition, and is an organopolysiloxane resin that is cured by a curing agent and / or a curing catalyst (C). Here, component (A) preferably has a curing reactive functional group, and the functional group is one or more functional groups selected from a condensation reactive group, a hydrosilylation reactive group, a radical reactive group, and a peroxide curing group, and is preferably a reactive group selected from a hydrosilylation reactive group and a radical reactive group, and is particularly preferably a curing reactive functional group containing a carbon-carbon double bond. When the functional group of component (A) is, for example, an alkenyl group among hydrosilylation reactive groups, the curing agent (C) is preferably a compound having a silicon-bonded hydrogen atom, particularly an organohydrogenpolysiloxane, and it is preferable to use a hydrosilylation reaction catalyst as the curing catalyst (D). In addition, when the functional group of component (A) is a radical reactive group, it is preferable to use a radical reaction initiator such as an organic peroxide as the curing agent (C). When the functional group of component (A) is a condensable silyl group such as silanol or a hydrolyzable silicon group, it is preferable to use as component (C) a compound capable of catalyzing a silanol condensation reaction as a curing catalyst.

[0047] Examples of hydrosilylation reactive groups that component (A) may have include alkenyl groups having 2 to 20 carbon atoms, such as vinyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, and dodecenyl, and silicon-bonded hydrogen atoms. The hydrosilylation reactive group is preferably an alkenyl group. The alkenyl group may be linear or branched, and is preferably a vinyl group or a hexenyl group. Component (A) preferably has at least two hydrosilylation reactive groups in one molecule.

[0048] Examples of groups bonded to silicon atoms other than the hydrosilylation reactive groups in component (A) include alkyl groups having 1 to 20 carbon atoms, halogen-substituted alkyl groups having 1 to 20 carbon atoms, aryl groups having 6 to 20 carbon atoms, halogen-substituted aryl groups having 6 to 20 carbon atoms, aralkyl groups having 7 to 20 carbon atoms, alkoxy groups, and hydroxyl groups. Specific examples include alkyl groups such as methyl groups, ethyl groups, propyl groups, butyl groups, pentyl groups, hexyl groups, heptyl groups, octyl groups, nonyl groups, decyl groups, undecyl groups, and dodecyl groups; aryl groups such as phenyl groups, tolyl groups, xylyl groups, naphthyl groups, anthracenyl groups, phenanthryl groups, and pyrenyl groups; aralkyl groups such as phenethyl groups and phenylpropyl groups; and groups in which some or all of the hydrogen atoms bonded to these groups are substituted with halogen atoms such as chlorine atoms and bromine atoms; and alkoxy groups such as methoxy groups, ethoxy groups, and propoxy groups. In particular, phenyl groups and hydroxyl groups are preferred.

[0049] Examples of the radical reactive group in component (A) include alkyl groups having 1 to 20 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, and dodecyl; alkenyl groups having 2 to 20 carbon atoms, such as vinyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, and dodecenyl; acrylic-containing groups, such as 3-acryloxypropyl and 4-acryloxybutyl; methacrylic-containing groups, such as 3-methacryloxypropyl and 4-methacryloxybutyl; and silicon-bonded hydrogen atoms. The radical reactive group is preferably an alkenyl group. The alkenyl group may be linear or branched, and is preferably a vinyl group or a hexenyl group. Component (A) preferably has at least two radical reactive groups in one molecule.

[0050] Examples of groups bonded to silicon atoms other than the radical reactive groups in component (A) include halogen-substituted alkyl groups having 1 to 20 carbon atoms, aryl groups having 6 to 20 carbon atoms, halogen-substituted aryl groups having 6 to 20 carbon atoms, aralkyl groups having 7 to 20 carbon atoms, alkoxy groups, and hydroxyl groups, and are the same as those mentioned above. In particular, phenyl groups and hydroxyl groups are preferred. In particular, component (A) is preferably such that 10 mol % or more of all organic groups in the molecule are aryl groups, particularly phenyl groups.

[0051] In the present invention, component (A) preferably contains organopolysiloxane resin fine particles having a curing reactive functional group, and the organopolysiloxane resin fine particles may be hot-melt as a whole molecule, or may contain organopolysiloxane resin fine particles that do not have hot-melt properties as a whole molecule. If the organopolysiloxane resin fine particles do not have hot-melt properties, it is preferable to use a linear or branched organopolysiloxane as further component (B) and use it as a mixture. Furthermore, it is possible and preferable to use organopolysiloxane resin fine particles that do not have a curing reactive functional group and do not have hot-melt properties as a whole molecule.

[0052] That is, at least a part or all of component (A) is (A1) Fine particles of a hot-melt organopolysiloxane resin having a softening point of 30° C. or higher and a curing reactive functional group containing at least one carbon-carbon double bond in the molecule. or The organopolysiloxane resin fine particles (component (A2)) may contain the following components (A2-1) and (A2-2) in a mass ratio of 0:100 to 90:10, preferably 0:100 to 75:25. (A2-1) A compound that does not have hot melt properties as a whole molecule, has a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: (A2-2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is not SiO 4 / 2 The organopolysiloxane resin contains siloxane units represented by the following formula (1) in an amount of at least 20 mol % based on the total siloxane units.

[0053] [Component (A1)] Component (A1) itself has hot melt properties and has a curing reactive functional group containing at least one carbon-carbon double bond in the molecule, and therefore is cured by the curing agent (C) described below. (A1) a resinous organopolysiloxane, (A2) an organopolysiloxane crosslinked product obtained by crosslinking at least one organopolysiloxane, and (A3) a block copolymer consisting of a resinous organosiloxane block and a linear organosiloxane block; and mixtures of at least two of these. It is preferable that the organopolysiloxane resin is composed of the above.

[0054] Component (A1) is a resinous organopolysiloxane having a hydrosilylation reactive group and / or a radical reactive group, and is preferably a hot-melt resinous organopolysiloxane having many T or Q units and an aryl group. Examples of such component (A1) include MQ resins, MDQ resins, MTQ resins, MDTQ resins, TD resins, TQ resins, and TDQ resins consisting of any combination of triorganosiloxy units (M units) (organo groups are methyl groups only, methyl groups and vinyl groups or phenyl groups), diorganosiloxy units (D units) (organo groups are methyl groups only, methyl groups and vinyl groups or phenyl groups), monoorganosiloxy units (T units) (organo groups are methyl groups, vinyl groups or phenyl groups) and siloxy units (Q units). It is preferred that component (A1) has at least two hydrosilylation reactive groups and / or radical reactive groups in the molecule, and that 10 mol % or more of all organic groups in the molecule are aryl groups, particularly phenyl groups.

[0055] Component (A2) is made by crosslinking at least one organopolysiloxane, and is less likely to crack when cured with curing agent (C), and can reduce cure shrinkage. Here, "crosslinking" refers to linking the organopolysiloxane, which is the raw material, to each other by hydrosilylation reaction, condensation reaction, radical reaction, and / or high-energy ray reaction. Examples of the hydrosilylation reactive group and radical reactive group (including high-energy ray reactive group) are the same as those described above, and examples of the condensation reactive group include a hydroxyl group, an alkoxy group, and an acyloxy group.

[0056] The units constituting component (A2) are not limited, and examples thereof include siloxane units and silalkylene group-containing siloxane units. In addition, it is preferable that the component (A2) has a resinous polysiloxane unit and a chain-like polysiloxane unit in the same molecule, since this gives the resulting cured product sufficient hardness and mechanical strength. That is, it is preferable that component (A2) is a crosslinked product of a resinous (resinous) organopolysiloxane and a chain-like (including linear or branched) organopolysiloxane. By introducing a resinous organopolysiloxane structure-chain-like organopolysiloxane structure into component (A2), component (A2) exhibits good hot melt properties and also exhibits good curability by the curing agent (C).

[0057] Component (A2) is (1) A resinous organopolysiloxane structure and a linear organopolysiloxane structure are linked in a molecule by alkylene bonds via a hydrosilylation reaction between an organopolysiloxane having at least two alkenyl groups per molecule and an organopolysiloxane having at least two silicon-bonded hydrogen atoms per molecule. (2) A resinous organopolysiloxane structure and a linear organopolysiloxane structure are linked in a molecule by a siloxane bond or an alkylene bond through a radical reaction of at least two organopolysiloxanes having at least two radical reactive groups in one molecule with an organic peroxide. (3) A resin-like organopolysiloxane structure and a linear organopolysiloxane structure are linked in a molecule through a siloxane (-Si-O-Si-) bond via a condensation reaction of at least two kinds of organopolysiloxane. Such component (A2) has a structure in which the resin structure and the organopolysiloxane portion of the chain structure are linked by an alkylene group or a new siloxane bond, and therefore the hot melt properties are significantly improved.

[0058] In the above (1) and (2), examples of the alkylene group contained in component (A2) include alkenyl groups having 2 to 20 carbon atoms, such as ethylene group, propylene group, butylene group, pentylene group, and hexylene group, which may be linear or branched, and are preferably ethylene or hexylene groups.

[0059] The crosslinked product of the resinous organopolysiloxane and the chain (including linear and branched) organopolysiloxane is composed, for example, of the following siloxane units and silalkylene group-containing siloxane units. M unit:R 1 R 2 2SiO 1 / 2 A siloxane unit represented by the formula: D unit:R 1 R 2 SiO 2 / 2 A siloxane unit represented by the formula: R 3 M / R 3 D unit:R 3 1 / 2 R 2 2SiO 1 / 2 and R 3 1 / 2 R 2 SiO 2 / 2 At least one siloxane unit selected from silalkylene group-containing siloxane units represented by the formula: T / Q unit:R 2 SiO 3 / 2 and SiO 4 / 2At least one siloxane unit selected from the siloxane units represented by

[0060] In the above formula, R 1 are each independently an alkyl group having 1 to 20 carbon atoms, a halogen-substituted alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a halogen-substituted aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, and examples of these groups are the same as those mentioned above. 1 is preferably a group selected from a methyl group, a vinyl group, and a phenyl group, provided that at least two R 1 is preferably an alkenyl group.

[0061] In addition, in the above formula, R 2 each independently represents an alkyl group having 1 to 20 carbon atoms, a halogen-substituted alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a halogen-substituted aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; 1 Examples of the groups are the same as those shown in R 2 is preferably a methyl group or a phenyl group.

[0062] In addition, in the above formula, R 3 is a linear or branched alkylene group having 2 to 20 carbon atoms bonded to a silicon atom in another siloxane unit. Examples of the alkylene group include the same groups as those mentioned above, and an ethylene group or a hexylene group is preferred.

[0063] The M unit is a siloxane unit constituting the terminal of component (A2), and the D unit is a siloxane unit constituting a linear polysiloxane structure. It is preferable that an alkenyl group is present on the M unit or D unit, particularly on the M unit. 3 M units and R 3The D unit is a siloxane unit that is bonded to a silicon atom in another siloxane unit via a silalkylene bond and to a silicon atom in another siloxane unit via an oxygen atom. The T / Q unit is a branched siloxane unit that gives the polysiloxane a resinous structure. 2 SiO 3 / 2 and / or SiO 4 / 2 In particular, in order to improve the hot melt property of component (A2) and adjust the content of aryl groups in component (A2), it is preferable that component (A2) contains a siloxane unit represented by R 2 SiO 3 / 2 It is preferable that the siloxane unit represented by R 2 It is preferred that the siloxane unit contains a phenyl group.

[0064] R 3 M / R 3 The D unit is one of the characteristic structures of component (A2), and R 3 It represents a structure in which silicon atoms are bridged via an alkylene group of the formula: 3 1 / 2 R 2 2SiO 1 / 2 and an alkylene group-containing siloxane unit represented by R 3 1 / 2 R 2 SiO 2 / 2 It is preferable that at least two of the total siloxane units constituting component (A2) are these alkylene group-containing siloxane units. 3 The preferred bond between the siloxane units having an alkylene group is as described above, and the bond between the two alkylene group-containing siloxane units is R 3 The number of is expressed as a bond valence of "1 / 2" like oxygen in the M unit. If R 3 If the number of is 1, then [O 1 / 2 R 2 2SiR 3 SiR 2 2O 1 / 2 ], [O 1 / 2 R2 2SiR 3 SiR 2 O 2 / 2 ] and [O 2 / 2 R 2 SiR 3 SiR 2 O 2 / 2 In component (A2), at least one selected from the structural units of siloxanes represented by the formula:] is contained, and each oxygen atom (O) is bonded to a silicon atom contained in the M, D, or T / Q unit. By having such a structure, component (A2) can be relatively easily designed to have a structure in which a linear polysiloxane structure consisting of D units and a resinous polysiloxane structure containing T / Q units are contained within the molecule, and the physical properties are remarkably excellent.

[0065] In the above (1), the polymerizable composition can be obtained by subjecting an organopolysiloxane having at least two alkenyl groups per molecule and an organopolysiloxane having at least two silicon-bonded hydrogen atoms per molecule (curing agent (C)) to a hydrosilylation reaction in a reaction ratio of [number of moles of alkenyl groups] / [number of moles of silicon-bonded hydrogen atoms]>1.

[0066] In the above (2), at least two types of organopolysiloxanes each having at least two radical reactive groups in one molecule can be subjected to a radical reaction with an organic peroxide (curing agent (C)) in an amount that is insufficient to react with all of the radical reactive groups in the system.

[0067] In the above (1) and (2), component (A2) is a product of a hydrosilylation reaction or a radical reaction between an organopolysiloxane having a resinous siloxane structure and an organopolysiloxane having a chain siloxane structure.

[0068] For example, component (A2) is (A R ) R in the molecule 2 SiO 3 / 2 (In the formula, R 2 is the same group as above.) and / or SiO4 / 2 and having an alkenyl group having 2 to 20 carbon atoms, a silicon-bonded hydrogen atom, or a radical-reactive group; and (A L ) R in the molecule 2 2SiO 2 / 2 A siloxane unit represented by the formula: 2 is the same group as above. R ) at least one linear organopolysiloxane having a group capable of hydrosilylation or radical reaction with component (a), the group being an alkenyl group having 2 to 20 carbon atoms or a silicon-bonded hydrogen atom, Ingredient (A R ) or component (A L ) in a ratio designed so that the hydrosilylation reactive groups and / or radical reactive groups remain after the reaction.

[0069] In the above (1), component (A R When at least a portion of component (A) is a resinous organopolysiloxane having an alkenyl group having 2 to 20 carbon atoms, L At least a portion of the above is preferably a linear organopolysiloxane having silicon-bonded hydrogen atoms.

[0070] Similarly, component (A R When at least a portion of component (A) is a resinous organopolysiloxane having silicon-bonded hydrogen atoms, L At least a portion of the above is preferably a chain organopolysiloxane having an alkenyl group having 2 to 20 carbon atoms.

[0071] Such a component (A2) is Component (a1): The following component (a 1-1 ) and / or the following component (a 1-2 ) having at least two alkenyl groups having 2 to 20 carbon atoms in the molecule, which is subjected to a radical reaction with an organic peroxide, or Component (a1), Organohydrogenpolysiloxane (a2), It is preferable that the hydrosilylation reaction is carried out in the presence of a hydrosilylation catalyst in such an amount that the molar ratio of silicon-bonded hydrogen atoms in component (a2) is 0.2 to 0.7 mol per mol of alkenyl groups having 2 to 20 carbon atoms contained in component (a1).

[0072] Component (a 1-1 ) is a polysiloxane with a relatively high amount of branching units, having the average unit formula: (R 4 3SiO 1 / 2 ) a (R 4 2SiO 2 / 2 ) b (R 4 SiO 3 / 2 ) c (SiO 4 / 2 ) d (R 5 O 1 / 2 ) e In the formula, R 4 each independently represents an alkyl group having 1 to 20 carbon atoms, a halogen-substituted alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a halogen-substituted aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; 1 Examples of the groups are the same as those shown in R 4 is preferably a methyl group, a vinyl group, or a phenyl group, provided that R 4 At least two of R are alkenyl groups. In addition, since the hot melt property is good, 4 Preferably, 10 mol % or more, or 20 mol % or more of R 5 is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and examples of the alkyl group include the same as those mentioned above.

[0073] In the formula, a is a number within the range of 0 to 0.7, b is a number within the range of 0 to 0.7, c is a number within the range of 0 to 0.9, d is a number within the range of 0 to 0.7, e is a number within the range of 0 to 0.1, and c+d is a number within the range of 0.3 to 0.9, and a+b+c+d is 1, and preferably a is a number within the range of 0 to 0.6, b is a number within the range of 0 to 0.6, c is a number within the range of 0 to 0.9, d is a number within the range of 0 to 0.5, e is a number within the range of 0 to 0.05, and c+d is a number within the range of 0.4 to 0.9, and a+b+c+d is 1. This is because when a, b, and c+d are each a number within the above range, the hardness and mechanical strength of the obtained cured product are excellent.

[0074] Such (a 1-1 ) component includes the following organopolysiloxanes: In the formula, Me, Ph, and Vi represent a methyl group, a phenyl group, and a vinyl group, respectively. (ViMe2SiO 1 / 2 ) 0.25 (PhSiO 3 / 2 ) 0.75 (HO 1 / 2 ) 0.02 (ViMe2SiO 1 / 2 ) 0.25 (PhSiO 3 / 2 ) 0.75 (ViMe2SiO 1 / 2 ) 0.20 (PhSiO 3 / 2 ) 0.80 (ViMe2SiO 1 / 2 ) 0.15 (Me3SiO 1 / 2 ) 0.38 (SiO 4 / 2 ) 0.47 (HO 1 / 2 ) 0.01 (ViMe2SiO 1 / 2 ) 0.13 (Me3SiO 1 / 2 ) 0.45 (SiO 4 / 2 ) 0.42 (HO 1 / 2 ) 0.01 (ViMe2SiO1 / 2 ) 0.15 (PhSiO 3 / 2 ) 0.85 (HO 1 / 2 ) 0.01 (MeSiO 2 / 2 ) 0.15 (MeViSiO 2 / 2 ) 0.10 (PhSiO 3 / 2 ) 0.75 (HO 1 / 2 ) 0.04 (MeViPhSiO 1 / 2 ) 0.20 (PhSiO 3 / 2 ) 0.80 (HO 1 / 2 ) 0.05 (ViMe2SiO 1 / 2 ) 0.15 (PhSiO 3 / 2 ) 0.75 (SiO 4 / 2 ) 0.10 (HO 1 / 2 ) 0.02 (Ph2SiO 2 / 2 ) 0.25 (MeViSiO 2 / 2 ) 0.30 (PhSiO 3 / 2 ) 0.45 (HO 1 / 2 ) 0.04 (Me3SiO 1 / 2 ) 0.20 (ViMePhSiO 1 / 2 ) 0.40 (SiO 4 / 2 ) 0.40 (HO 1 / 2 ) 0.08

[0075] Component (a 1-2 ) is a polysiloxane with a relatively high amount of linear siloxane units, having the average unit formula: (R 4 3SiO 1 / 2 ) a' (R 4 2SiO 2 / 2 ) b' (R 4 SiO3 / 2 ) c' (SiO 4 / 2 ) d' (R 5 O 1 / 2 ) e' In the formula, R is an organopolysiloxane having at least two alkenyl groups having 2 to 20 carbon atoms in one molecule. 4 and R 5 is the same group as defined above.

[0076] In the formula, a' is a number within the range of 0.01 to 0.3, b' is a number within the range of 0.4 to 0.99, c' is a number within the range of 0 to 0.2, d' is a number within the range of 0 to 0.2, e' is a number within the range of 0 to 0.1, and c'+d' is a number within the range of 0 to 0.2, and a'+b'+c'+d' is 1, and preferably a' is a number within the range of 0.02 to 0.20, b' is a number within the range of 0.6 to 0.99, c' is a number within the range of 0 to 0.1, d' is a number within the range of 0 to 0.1, j' is a number within the range of 0 to 0.05, and c'+d' is a number within the range of 0 to 0.1, and a'+b'+c'+d' is 1. This is because when a', b', c', and d' are each numbers within the above ranges, toughness can be imparted to the obtained cured product.

[0077] Such a component (a 1-2 ) includes the following organopolysiloxanes: In the formula, Me, Ph, and Vi represent a methyl group, a phenyl group, and a vinyl group, respectively. ViMe2SiO(MePhSiO) 18 SiMe2Vi, i.e. (ViMe2SiO 1 / 2 ) 0.10 (MePhSiO 2 / 2 ) 0.90 ViMe2SiO(MePhSiO) 30 SiMe2Vi, i.e. (ViMe2SiO 1 / 2 ) 0.063 (MePhSiO 2 / 2 ) 0.937 ViMe2SiO(MePhSiO) 150 SiMe2Vi, i.e. (ViMe2SiO1 / 2 ) 0.013 (MePhSiO 2 / 2 ) 0.987 ViMe2SiO(Me2SiO) 18 SiMe2Vi, i.e. (ViMe2SiO 1 / 2 ) 0.10 (MeSiO 2 / 2 ) 0.90 ViMe2SiO(Me2SiO) 30 SiMe2Vi, i.e. (ViMe2SiO 1 / 2 ) 0.063 (MeSiO 2 / 2 ) 0.937 ViMe2SiO(Me2SiO) 35 (MePhSiO) 13 SiMe2Vi, i.e. (ViMe2SiO 1 / 2 ) 0.04 (MeSiO 2 / 2 ) 0.70 (MePhSiO 2 / 2 ) 0.26 ViMe2SiO(Me2SiO) 10 SiMe2Vi, i.e. (ViMe2SiO 1 / 2 ) 0.17 (MeSiO 2 / 2 ) 0.83 (ViMe2SiO 1 / 2 ) 0.10 (MePhSiO 2 / 2 ) 0.80 (PhSiO 3 / 2 ) 0.10 (HO 1 / 2 ) 0.02 (ViMe2SiO 1 / 2 ) 0.20 (MePhSiO 2 / 2 ) 0.70 (SiO 4 / 2 ) 0.10 (HO 1 / 2 ) 0.01 HOMe2SiO(MeViSiO) 20 SiMe2OH Me2ViSiO(MePhSiO) 30SiMe2Vi Me2ViSiO(Me2SiO) 150 SiMe2Vi

[0078] Component (a 1-1 Component (a) is preferably used from the viewpoint of imparting hardness and mechanical strength to the resulting cured product. 1-2 ) can be added as an optional component from the viewpoint of imparting toughness to the obtained cured product, but when a crosslinking agent having many linear siloxane units is used in the following component (a2), it may be substituted therewith. In either case, it is preferable that the mass ratio of the component having many branched siloxane units to the component having many linear siloxane units is in the range of 50:50 to 100:0, or in the range of 60:40 to 100:0. This is because when the mass ratio of the component having many branched siloxane units to the component having many linear siloxane units is a value within the above range, the hardness and mechanical strength of the obtained cured product are good.

[0079] In addition, when the component (a1) is subjected to a radical reaction with an organic peroxide, 1-1 ) and component (a 1-2 ) in a ratio of 10:90 to 90:10, and it is possible to eliminate the need to use component (a2).

[0080] Component (a2) is a compound which reacts with component (a 1-1 ) and / or component (a 1-2 (a2) is a component (curing agent (C)) for crosslinking the above-mentioned siloxanes, and is an organopolysiloxane containing at least two silicon-bonded hydrogen atoms in one molecule. Examples of groups bonded to silicon atoms other than hydrogen atoms in the component (a2) include alkyl groups having 1 to 20 carbon atoms, halogen-substituted alkyl groups having 1 to 20 carbon atoms, aryl groups having 6 to 20 carbon atoms, halogen-substituted aryl groups having 6 to 20 carbon atoms, aralkyl groups having 7 to 20 carbon atoms, alkoxy groups, epoxy-containing groups, and hydroxyl groups, and examples of the same groups as those mentioned above.

[0081] Although not limited, such component (a2) preferably has the average composition formula: R6 k H m SiO (4-k-m) / 2 In the formula, R 6 is an alkyl group having 1 to 20 carbon atoms, a halogen-substituted alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a halogen-substituted aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, 1 Of these, a methyl group or a phenyl group is preferable.

[0082] In the above formula, k is a number in the range of 1.0 to 2.5, preferably 1.2 to 2.3, m is a number in the range of 0.01 to 0.9, preferably 0.05 to 0.8, and k+m is a number in the range of 1.5 to 3.0, preferably 2.0 to 2.7.

[0083] The component (a2) may be a resinous organohydrogenpolysiloxane having a large number of branched siloxane units, or a linear organohydrogenpolysiloxane having a large number of linear siloxane units. 2-1 ), an organohydrogenpolysiloxane represented by the following (a 2-2 ) or a mixture thereof.

[0084] Component (a 2-1 ) is the average unit formula: [R 7 3SiO 1 / 2 ] f [R 7 2SiO 2 / 2 ] g [R 7 SiO 3 / 2 ] h [SiO 4 / 2 ] i (R 5 O 1 / 2 ) j In the formula, R 7 each independently represents an alkyl group having 1 to 20 carbon atoms, a halogen-substituted alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a halogen-substituted aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, or a hydrogen atom, 1 In addition, in the formula, R 5 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and examples thereof include the same groups as those mentioned above.

[0085] In the above formula, f is a number in the range of 0 to 0.7, g is a number in the range of 0 to 0.7, h is a number in the range of 0 to 0.9, i is a number in the range of 0 to 0.7, j is a number in the range of 0 to 0.1, and h+i is a number in the range of 0.3 to 0.9, and f+g+h+i is 1, and preferably, f is a number in the range of 0 to 0.6, g is a number in the range of 0 to 0.6, h is a number in the range of 0 to 0.9, i is a number in the range of 0 to 0.5, j is a number in the range of 0 to 0.05, and h+i is a number in the range of 0.4 to 0.9, and f+g+h+i is 1.

[0086] Component (a 2-2 ) is the average unit formula: (R 7 3SiO 1 / 2 ) f' (R 7 2SiO 2 / 2 ) g' (R 7 SiO 3 / 2 ) h' (SiO 4 / 2 ) i' (R 5 O 1 / 2 ) j' In the formula, R is an organopolysiloxane having at least two silicon-bonded hydrogen atoms in one molecule. 7 and R 5 is the same group as defined above.

[0087] Furthermore, in the above formula, f' is a number in the range of 0.01 to 0.3, g' is a number in the range of 0.4 to 0.99, h' is a number in the range of 0 to 0.2, i' is a number in the range of 0 to 0.2, j' is a number in the range of 0 to 0.1, and h'+i' is a number in the range of 0 to 0.2, and f'+g'+h'+i' is 1, and preferably f' is a number in the range of 0.02 to 0.20, g' is a number in the range of 0.6 to 0.99, h' is a number in the range of 0 to 0.1, i' is a number in the range of 0 to 0.1, j' is a number in the range of 0 to 0.05, and h'+i' is a number in the range of 0 to 0.1, and f'+g'+h'+i' is 1.

[0088] As described above, in component (a2), the resin-like organopolysiloxane having many branched siloxane units imparts hardness and mechanical strength to the cured product, while the resulting organopolysiloxane having many linear siloxane units imparts toughness to the cured product. Therefore, component (a 2-1 ) and component (a 2-2 Specifically, when the branched siloxane unit is small in the component (a1), it is preferable to use the component (a2) appropriately. 2-1 When the amount of linear siloxane units in component (a1) is small, it is preferable to use component (a 2-2 It is preferable to mainly use component (a2). 2-1 ) and component (a 2-2 ) is preferably in the range of 50:50 to 100:0, or 60:40 to 100:0.

[0089] Examples of such component (a2) include the following organopolysiloxanes: In the formula, Me and Ph represent a methyl group and a phenyl group, respectively. Ph2Si(OSiMe2H)2, i.e., Ph 0.67 Me 1.33 H 0.67 SiO 0.67 HMe2SiO(Me2SiO) 20 SiMe2H, i.e., Me 2.00 H 0.09 SiO 0.95 HMe2SiO(Me2SiO) 55 SiMe2H, i.e., Me 2.00 H 0.04 SiO 0.98 PhSi(OSiMe2H)3, i.e., Ph 0.25 Me 1.50 H 0.75 SiO 0.75 (HMeSiO 1 / 2 ) 0.6 (PhSiO 3 / 2 ) 0.4 , i.e., Ph 0.40 Me 1.20 H 0.60 SiO 0.90

[0090] The amount of component (a2) added is an amount such that the molar ratio of silicon-bonded hydrogen atoms in component (a2) to the alkenyl groups in component (a1) is 0.2 to 0.7, and preferably 0.3 to 0.6, because when the amount of component (a2) added is within the above range, the initial hardness and mechanical strength of the resulting cured product are good.

[0091] The organic peroxide (curing agent (C)) used to cause the radical reaction of component (a1) is not limited to a specific one, but examples thereof include benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, p-methylbenzoyl peroxide, o-methylbenzoyl peroxide, 2,4-dicumyl peroxide, 2,5-dimethyl-bis(2,5-t-butylperoxy)hexane, di-t-butyl peroxide, t-butyl perbenzoate, and 1,6-hexanediol-bis-t-butyl peroxycarbonate. These may be used alone or in combination of two or more. Among them, 2,4-dichlorobenzoyl peroxide, p-methylbenzoyl peroxide, 2,5-dimethyl-bis(2,5-t-butylperoxy)hexane, and 2,4-dicumyl peroxide are preferred. The amount of the organic peroxide may be sufficient to cure the curable silicone composition. The organic peroxide can be used not only when reacting component (a1), but also when curing the curable silicone composition of the present invention by radical reaction. When a radical reaction is carried out using an organic peroxide, the component (a1) is 1-1 ) and component (a 1-2 It is preferable that the mass ratio of the organic peroxide is within the range of 10:90 to 90:10. The amount of the organic peroxide added is not limited, but is preferably within the range of 0.1 to 5 parts by mass, 0.2 to 3 parts by mass, or 0.2 to 1.5 parts by mass, relative to 100 parts by mass of the component (a1).

[0092] In addition, the hydrosilylation catalyst used for the hydrosilylation reaction between component (a1) and component (a2) is not limited, and a known hydrosilylation catalyst (component (D)) can be used. As the hydrosilylation catalyst, a compound or metal having a hydrosilylation catalytic action known in the art can be used. Examples of the hydrosilylation catalyst include platinum-based catalysts, rhodium-based catalysts, and palladium-based catalysts. Platinum-based catalysts are preferred because they can significantly accelerate the curing of the composition of the present invention. Examples of the platinum catalyst include platinum fine powder, chloroplatinic acid, an alcohol solution of chloroplatinic acid, platinum-alkenylsiloxane complexes, platinum-olefin complexes, platinum-carbonyl complexes, and catalysts in which these platinum catalysts are dispersed or encapsulated in thermoplastic resins such as silicone resins, polycarbonate resins, and acrylic resins. In particular, platinum-alkenylsiloxane complexes are preferred. Examples of this alkenylsiloxane include 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, alkenylsiloxanes in which a portion of the methyl groups of these alkenylsiloxanes have been substituted with ethyl groups, phenyl groups, etc., and alkenylsiloxanes in which the vinyl groups of these alkenylsiloxanes have been substituted with allyl groups, hexenyl groups, etc. In particular, because this platinum-alkenylsiloxane complex has good stability, it is preferable to use 1,3-divinyl-1,1,3,3-tetramethyldisiloxane as the hydrosilylation reaction catalyst, and it is preferable to add the complex in the form of an alkenylsiloxane solution to the other components that make up the curable silicone composition. In addition, from the standpoint of improving the handling of the platinum catalyst and the pot life of the curable silicone composition, a platinum-containing hydrosilylation reaction catalyst in the form of fine particles dispersed or encapsulated in a thermoplastic resin may be used. Note that non-platinum metal catalysts such as iron, ruthenium, and iron / cobalt may also be used as catalysts that promote the hydrosilylation reaction. The amount of the hydrosilylation catalyst added is preferably an amount such that the platinum-based metal atom in the hydrosilylation catalyst is in the range of 0.01 to 500 ppm, 0.01 to 100 ppm, or 0.01 to 50 ppm, by mass, relative to the total amount of components (a1) and (a2). Furthermore, when the curable silicone composition of the present invention is one that is cured by a hydrosilylation reaction, the above-mentioned hydrosilylation reaction catalyst can be used in any composition, regardless of whether it is made of components (a1) and (a2).

[0093] The above (A3) is obtained by subjecting the following components (a3) ​​and (a4) to a condensation reaction in the presence of a condensation reaction catalyst.

[0094] Component (a3) ​​has the average unit formula: (R 8 3SiO 1 / 2 ) p (R 8 2SiO 2 / 2 ) q (R 8 SiO 3 / 2 ) r (SiO 4 / 2 ) s (R 9 O 1 / 2 ) t In the formula, R 8 are each independently an alkyl group having 1 to 20 carbon atoms, a halogen-substituted alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a halogen-substituted aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, and examples of these groups are the same as those mentioned above. 9 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an acyl group having 2 to 5 carbon atoms, and examples of such groups include alkoxy groups such as methoxy and ethoxy groups, and acyloxy groups. Component (a3) ​​has at least one silicon-bonded hydroxyl group, silicon-bonded alkoxy group, or silicon-bonded acyloxy group in each molecule. In addition, at least two R 8 is an alkenyl group, and all R8 It is preferable that 10 mol % or more, or 20 mol % or more of these groups are phenyl groups.

[0095] In the above formula, p is a number within the range of 0 to 0.7, q is a number within the range of 0 to 0.7, r is a number within the range of 0 to 0.9, s is a number within the range of 0 to 0.7, t is a number within the range of 0.01 to 0.10, and r+s is a number within the range of 0.3 to 0.9, and p+q+r+s is 1, and preferably p is a number within the range of 0 to 0.6, q is a number within the range of 0 to 0.6, r is a number within the range of 0 to 0.9, s is a number within the range of 0 to 0.5, t is a number within the range of 0.01 to 0.05, and r+s is a number within the range of 0.4 to 0.9. This is because, when p, q, and r+s are each a number within the above range, a hot-melt silicone can be obtained that is flexible at 25°C, non-fluid, has low surface tack, and has a sufficiently low melt viscosity at high temperatures.

[0096] Component (a4) has the average unit formula: (R 8 3SiO 1 / 2 ) p' (R 8 2SiO 2 / 2 ) q' (R 8 SiO 3 / 2 ) r' (SiO 4 / 2 ) s' (R 9 O 1 / 2 ) t' In the formula, R 8 and R 9is the same group as above. Component (a4) has at least one silicon-bonded hydroxyl group, silicon-bonded alkoxy group, or silicon-bonded acyloxy group in one molecule. In the formula, p' is a number in the range of 0.01 to 0.3, q' is a number in the range of 0.4 to 0.99, r' is a number in the range of 0 to 0.2, s' is a number in the range of 0 to 0.2, t' is a number in the range of 0 to 0.1, and r'+s' is a number in the range of 0 to 0.2, and p'+q'+r'+s' is 1, and preferably p' is a number in the range of 0.02 to 0.20, q' is a number in the range of 0.6 to 0.99, r' is a number in the range of 0 to 0.1, s' is a number in the range of 0 to 0.1, t' is a number in the range of 0 to 0.05, and r'+s' is a number in the range of 0 to 0.1. This is because, when p', q', r', and s' are each numbers within the above ranges, a hot-melt silicone can be obtained that has flexibility at 25°C, yet is non-flowable, has low surface tack, and has a sufficiently low melt viscosity at high temperatures.

[0097] The condensation reaction catalyst for condensing the component (a3) ​​and the component (a4) is not particularly limited, and examples thereof include organic tin compounds such as dibutyltin dilaurate, dibutyltin diacetate, tin octenate, dibutyltin dioctate, and tin laurate; organic titanium compounds such as tetrabutyl titanate, tetrapropyl titanate, and dibutoxybis(ethylacetoacetate); acidic compounds such as hydrochloric acid, sulfuric acid, and dodecylbenzenesulfonic acid; alkaline compounds such as ammonia and sodium hydroxide; and amine compounds such as 1,8-diazabicyclo[5.4.0]undecene (DBU) and 1,4-diazabicyclo[2.2.2]octane (DABCO). Of these, organic tin compounds and organic titanium compounds are preferred. Not limited to the case where the component (a3) ​​and the component (a4) are used, when the curable hot melt silicone composition of the present invention is a composition that is cured by a condensation reaction, the above-mentioned condensation reaction catalyst can be used as a curing catalyst (component (D)).

[0098] The component (A3) is a block copolymer consisting of a resinous organosiloxane block and a linear organosiloxane block. Such a component (A3) preferably contains 40 to 90 mol % of a compound represented by the formula [R 1 2SiO 2 / 2 10 to 60 mol % of disiloxy units of the formula [R 1 SiO 3 / 2 It is preferable that the trisiloxy unit is composed of the above-mentioned trisiloxy unit [≡SiOH] and contains 0.5 to 35 mol % of silanol groups [≡SiOH]. 1 are each independently an alkyl group having 1 to 20 carbon atoms, a halogen-substituted alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a halogen-substituted aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, and examples of which are the same as those mentioned above. 1 is an alkenyl group. 1 2SiO 2 / 2 ] forms linear blocks having an average of 100 to 300 disiloxy units per linear block, and the trisiloxy units [R 1 SiO 3 / 2 ] is a resinous organosiloxane block copolymer having a weight average molecular weight of at least 20,000 g / mole and containing 0.5-4.5 mol % of at least one alkenyl group, wherein at least 30% of the non-linear blocks are bonded to each other and each linear block is bonded to at least one non-linear block via a -Si-O-Si- bond, and wherein the resinous organosiloxane block copolymer has a weight average molecular weight of at least 20,000 g / mole and contains 0.5-4.5 mol % of at least one alkenyl group.

[0099] Component (A3) is prepared by a condensation reaction of (a5) a resinous organosiloxane or a resinous organosiloxane block copolymer with (a6) a linear organosiloxane and, if necessary, (a7) a siloxane compound.

[0100] Component (a5) has the average unit formula: [R 1 2R 2 SiO 1 / 2 ] i [R1 R 2 SiO 2 / 2 ] ii [R 1 SiO 3 / 2 ] iii [R 2 SiO 3 / 2 ] iv [SiO 4 / 2 ] v In the formula, R 1 are each independently an alkyl group having 1 to 20 carbon atoms, a halogen-substituted alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a halogen-substituted aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, and examples of the same groups as those mentioned above are given. 2 each independently represents an alkyl group having 1 to 20 carbon atoms, a halogen-substituted alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a halogen-substituted aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; 1 The same groups as those shown below are exemplified.

[0101] In the above formula, i, ii, iii, iv, and v represent the mole fraction of each siloxy unit, where i is a number from 0 to 0.6, ii is a number from 0 to 0.6, iii is a number from 0 to 1, iv is a number from 0 to 1, and v is a number from 0 to 0.6, with the proviso that ii+iii+iv+v>0 and i+ii+iii+iv+v≦1. In addition, the component (a5) preferably contains 0 to 35 mol % of silanol groups [≡SiOH] in one molecule.

[0102] Component (a6) has the general formula: R 1 3-α (X) α SiO(R 1 2SiO) β Si(X) α R 1 3-α In the formula, R 1is the same as above, and examples thereof include the same groups as above. 5 , F, Cl, Br, I, -OC(O)R 5 , -N(R 5 )2, or -ON=CR 5 2 (where R 5 is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.) In the formula, each α is independently 1, 2, or 3, and β is an integer of 50 to 300.

[0103] Component (a7) has the general formula: R 1 R 2 2SiX In the formula, R 1 , R 2 and X are the same groups as defined above.

[0104] The condensation reaction catalyst for the condensation reaction of component (a5) with component (a6) and / or component (a7) is not limited, and examples thereof include organic tin compounds such as dibutyltin dilaurate, dibutyltin diacetate, tin octenate, dibutyltin dioctate, and tin laurate; organic titanium compounds such as tetrabutyl titanate, tetrapropyl titanate, and dibutoxybis(ethylacetoacetate); acidic compounds such as hydrochloric acid, sulfuric acid, and dodecylbenzenesulfonic acid; alkaline compounds such as ammonia and sodium hydroxide; and amine compounds such as 1,8-diazabicyclo[5.4.0]undecene (DBU) and 1,4-diazabicyclo[2.2.2]octane (DABCO).

[0105] Component (A1) exhibits hot melt properties, specifically, it is non-flowable at 25°C, and preferably has a melt viscosity at 100°C of 8000 Pa·s or less. Non-flowable means that it does not flow under no load, and indicates a state below the softening point measured by the ring and ball method for testing the softening point of hot melt adhesives as stipulated in JIS K 6863-1994 "Testing Method for Softening Point of Hot Melt Adhesives". In other words, to be non-flowable at 25°C, the softening point must be higher than 25°C.

[0106] Component (A1) preferably has a melt viscosity at 100° C. of 8000 Pa s or less, 5000 Pa s or less, or in the range of 10 to 3000 Pa s. When the melt viscosity at 100° C. is within the above range, the adhesiveness after cooling to 25° C. after hot melting is good, and the melt viscosity at 150° C. when mixed with the components described below to form a designated hot melt composition is sufficiently low.

[0107] [Component (A2)] Component (A2) is an organopolysiloxane resin mixture containing the following components (A2-1) and (A2-2) in a mass ratio of 0:100 to 90:10, preferably 0:100 to 75:25. (A2-1) A compound that does not have hot melt properties as a whole molecule, has a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: (A2-2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is not SiO 4 / 2 The organopolysiloxane resin contains siloxane units represented by the following formula (1) in an amount of at least 20 mol % based on the total siloxane units. The mixture may be in the form of fine particles, and is particularly preferably spherical silicone fine particles having an average primary particle size of 1 to 20 μm.

[0108] The component (A2-1) can control the elastic modulus of the obtained cured product by using a component having a curing reactive group having a carbon-carbon double bond in the molecule. Such a curing reactive group is a curable functional group that can react with hydrosilylation reaction or organic peroxide, or other radical mechanism, and forms a cured product by crosslinking reaction with other components. Such a curing reactive group is an alkenyl group or an acrylic group, for example, an alkenyl group having 2 to 10 carbon atoms such as a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, etc.; an acrylic group-containing monovalent organic group such as a 3-methacryloxypropyl group, a 3-acryloxypropyl group, etc., and is particularly preferably a vinyl group or a hexenyl group.

[0109] Component (A2-1) is an organopolysiloxane resin that does not have hot melt properties as a whole molecule and is solid in a solvent-free state. Here, not having hot melt properties means that the resin of component (A2-1) does not exhibit heat melting behavior at 200°C or less by itself, specifically, that it has no softening point or melt viscosity at 200°C or less. In component (A2-1), such physical properties are not particularly limited structurally, but it is preferable that the functional group in the organopolysiloxane resin is a monovalent hydrocarbon group having 1 to 10 carbon atoms, particularly a functional group selected from an alkyl group having 1 to 10 carbon atoms such as a methyl group, and that it does not substantially contain an aryl group such as a phenyl group. If the component contains a large amount of phenyl groups, the component may have hot melt properties, and SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.

[0110] Preferably, the functional groups bonded to silicon atoms in component (A2-1) are selected from alkenyl groups such as methyl and vinyl groups and (meth)acrylic groups ((meth)acrylic means acrylic and / or methacrylic), and it is preferred that 70 to 99 mol% of all functional groups bonded to silicon atoms are methyl groups, more preferably 80 to 99 mol% are methyl groups, and particularly preferably 88 to 99 mol% are methyl groups, and the remaining functional groups bonded to silicon atoms are alkenyl groups such as vinyl groups or (meth)acrylic groups. In this range, component (A2-1) can be designed as a component that is not hot-melt, but is particularly excellent in the color resistance of the cured product at high temperatures. Note that component (A2-1) may contain a small amount of hydroxyl groups or alkoxy groups.

[0111] Component (A2-1) is a solid organopolysiloxane resin in a solvent-free state, and contains SiO 4 / 2 The branched siloxane units are preferably at least 40 mol % or more of the total siloxane units, more preferably at least 50 mol %, and particularly preferably in the range of 50 to 90 mol %. R is a monovalent organic group, preferably a functional group selected from monovalent hydrocarbon groups having 1 to 10 carbon atoms, particularly alkyl and alkenyl groups having 1 to 10 carbon atoms such as methyl groups, and from the viewpoint of technical effect, it is preferable that R does not substantially contain aryl groups such as phenyl groups.

[0112] Preferably, the component (A2-1) is a copolymer having the following average unit formula: (R 1 3SiO 1 / 2 ) a (R 1 2SiO 2 / 2 ) b (R 1 SiO 3 / 2 ) c (SiO 4 / 2 ) d (R 2 O 1 / 2)e (In the formula, each R1 are independently monovalent hydrocarbon groups having 1 to 10 carbon atoms, provided that the total number of R 1 are 1 to 12 mol % of alkenyl groups or (meth)acrylic groups; 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; and a, b, c, d, and e are numbers that satisfy the following: 0.10≦a≦0.60, 0≦b≦0.70, 0≦c≦0.80, 0≦d≦0.65, 0≦e≦0.05, with the proviso that c+d>0.20 and a+b+c+d=1). The organopolysiloxane resin is a non-hot melt organopolysiloxane resin represented by the formula:

[0113] In the above average unit formula, each R 1 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl groups; vinyl, allyl, butenyl, pentenyl, hexenyl, or similar alkenyl groups; (meth)acrylic groups; phenyl, tolyl, xylyl, or similar aryl groups; benzyl, phenethyl, or similar aralkyl groups; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl groups. Furthermore, the total R 1 Preferably, 1 to 12 mol % of the total R 1 Of these, 2 to 10 mol % is an alkenyl group. If the content of alkenyl groups is less than the lower limit of the above range, the mechanical strength (hardness, etc.) of the resulting cured product may be insufficient. On the other hand, if the content of alkenyl groups is equal to or less than the upper limit of the above range, the composition containing this component can achieve good hot melt performance as a whole composition. 1 is preferably a functional group selected from an alkyl group having 1 to 10 carbon atoms, such as a methyl group, and an alkenyl group, such as a vinyl group or a hexenyl group. From the viewpoint of the technical effect of the invention, R 1 It is preferable that the component (A2-1-1) is substantially free of aryl groups such as phenyl groups. If the component (A2-1-1) contains a large amount of aryl groups such as phenyl groups, the component (A2-1-1) itself may become hot-melt, making it impossible to achieve the technical effects of the present invention. In addition, in the cured product, the SiO4 / 2 The effect of reinforcing the cured product specific to the group may decrease.

[0114] In the formula, R 2 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 2 The alkyl group of R is exemplified by methyl, ethyl, propyl, butyl, pentyl, or hexyl. 2 Functional group R containing 2 O 1 / 2 corresponds to the hydroxyl group or alkoxy group in component (A2-1-1).

[0115] In the above formula, a represents the general formula: R 1 3SiO 1 / 2 a is a number indicating the proportion of siloxane units. This number satisfies 0.1≦a≦0.60, and preferably 0.15≦a≦0.55. When a is equal to or greater than the lower limit of the above range, a composition containing this component can achieve good hot melt performance as a whole composition. On the other hand, when a is equal to or less than the upper limit of the above range, the mechanical strength (hardness, elongation, etc.) of the obtained cured product is not too low.

[0116] In the above formula, b represents the general formula: R 1 2SiO 2 / 2 This number satisfies 0≦b≦0.70, and preferably 0≦b≦0.60. When b is equal to or less than the upper limit of the above range, a composition containing this component can achieve good hot melt performance as a whole composition, and can also provide a composition that is less sticky at room temperature.

[0117] In the above formula, c represents the general formula: R 3 SiO 3 / 2 c is a number indicating the proportion of siloxane units. This number satisfies 0≦c≦0.80, and preferably 0≦c≦0.75. When c is equal to or less than the upper limit of the above range, the composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a tack-free composition with little stickiness at room temperature. In the present invention, c may be, and is preferably, 0.

[0118] In the above formula, d is SiO 4 / 2 It is necessary that d is 0.00≦d≦0.65, preferably 0.20≦d≦0.65, and particularly preferably 0.25≦d≦0.65. This is because within this numerical range, a composition containing this component can achieve good hot melt performance as a whole composition, and the resulting cured product has sufficient flexibility.

[0119] In the present invention, c or d may be 0, but it is necessary that c+d>0.20. If the value of c+d is less than the lower limit, the composition as a whole may not achieve good hot melt performance, and the technical effects of the present invention may not be fully achieved.

[0120] In the formula, e represents the general formula: R 2 O 1 / 2 e is a number indicating the proportion of units, which means a hydroxyl group or an alkoxy group bonded to a silicon atom that may be contained in the organopolysiloxane resin. This number satisfies 0≦e≦0.05, preferably 0≦e≦0.03. If e is equal to or less than the upper limit of the range, a material that realizes good hot melt performance as a whole composition can be obtained. In addition, the sum of a, b, c, and d, which are the sums of each siloxane unit, is ultimately equal to 1.

[0121] Component (A2-1) is an organopolysiloxane resin having the above characteristics, and from the viewpoint of ease of handling, is preferably a spherical organopolysiloxane resin fine particle having an average primary particle diameter of 1 to 20 μm as measured by a laser diffraction / scattering method or the like. By using such a fine particle component, the present composition can be prepared or produced as a curable granular composition having excellent handling, workability and hot melt properties. Here, the method for producing component (A2-1) is as described above.

[0122] [Component (A2-2)] Component (A2-2) is one of the main components of the curable hot-melt silicone composition of the present invention, and is an organopolysiloxane resin containing a curable reactive functional group that does not have hot-melt properties by itself, and is a component that realizes hot-melt properties of the composition as a whole and excellent stress relaxation properties of the cured product by combining it with the above-mentioned component (A2-1) and the component (B) described below in a specified quantitative range.Such component (A2-2) is preferably in the form of particles, either alone or in combination with other components (for example, the component (A2-1) which is a non-reactive organopolysiloxane resin, a part of the component (B) described below), and is particularly preferably spherical silicone fine particles with an average primary particle size of 1 to 20 μm.

[0123] Component (A2-2) is an organopolysiloxane resin that does not have hot melt properties as a whole molecule and is solid in a solvent-free state. Here, not having hot melt properties means that the resin of component (A2-2) does not exhibit heat melting behavior by itself, specifically, it means that it has no softening point and melt viscosity. In component (A2-2), such physical properties are not particularly limited structurally, but it is preferable that the functional group in the organopolysiloxane resin is a monovalent hydrocarbon group having 1 to 10 carbon atoms, particularly a functional group selected from an alkyl group having 1 to 10 carbon atoms such as a methyl group, and that it does not substantially contain an aryl group such as a phenyl group. If the component contains a large amount of a phenyl group, the component may have hot melt properties, and SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.

[0124] Component (A2-2) is a solid like component (A2-1), and is SiO 4 / 2The organopolysiloxane resin contains siloxane units represented by the formula (I) in an amount of at least 20 mol % of all siloxane units, but is characterized by having no curing reactive functional group containing at least one carbon-carbon double bond in the molecule. That is, component (A2-2) is characterized by not containing an alkenyl group such as a vinyl group as a functional group in the organopolysiloxane resin. Examples of functional groups in the organopolysiloxane include monovalent hydrocarbon groups having 1 to 10 carbon atoms, particularly alkyl groups having 1 to 10 carbon atoms such as a methyl group, and it is preferable that the resin is substantially free of aryl groups such as a phenyl group.

[0125] Preferably, the functional groups bonded to silicon atoms in component (A2-2) are alkyl groups having 1 to 10 carbon atoms, such as methyl groups, and it is preferred that 70 to 100 mol % of all the functional groups bonded to silicon atoms are methyl groups, more preferably 80 to 100 mol %, and particularly preferably 88 to 100 mol %. Within this range, component (A2) is not hot-melt and is SiO 4 / 2 It is possible to design this component as one that has an especially excellent reinforcing effect on the cured product containing the siloxane unit represented by the following formula: The component (A2-2) may contain a small amount of hydroxyl groups or alkoxy groups.

[0126] Component (A2-2) does not have a curing reactive group having a carbon-carbon double bond in the molecule, so it does not form a cured product by itself, but it has an effect of improving the hot melt property of the composition as a whole and reinforcing the cured product. In addition, it is a necessary component to achieve the technical effects of the present invention by using it in combination with component (A2-1) having a curing reactive group as necessary.

[0127] Component (A2-2) is a solid organopolysiloxane resin in the absence of a solvent, and contains branched siloxane units, SiO 4 / 2The siloxane unit represented by the formula (1) is contained in an amount of at least 20 mol % of all siloxane units. The amount of the siloxane unit is preferably at least 40 mol % of all siloxane units, more preferably at least 50 mol %, and particularly preferably in the range of 50 to 65 mol %.

[0128] Preferably, component (A2-2) is (A2-2-1) an average unit formula: (R 3 3SiO 1 / 2 ) f (R 3 2SiO 2 / 2 ) g (R 3 SiO 3 / 2 ) h (SiO 4 / 2 ) i (R 2 O 1 / 2)j (In the formula, each R 3 each independently represents a monovalent hydrocarbon group having 1 to 10 carbon atoms and no carbon-carbon double bonds; R 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; f, g, h, i, and j are numbers that satisfy the following: 0.35≦f≦0.55, 0≦g≦0.20, 0≦h≦0.20, 0.45≦i≦0.65, 0≦j≦0.05, and f+g+h+i=1). The organopolysiloxane resin is a non-hot melt organopolysiloxane resin represented by the formula:

[0129] In the above average unit formula, each R 3 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms and no carbon-carbon double bonds, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl radicals; phenyl, tolyl, xylyl, or similar aryl radicals; benzyl, phenethyl, or similar aralkyl radicals; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl radicals, where the total R 3It is preferable that 70 mol % or more of R are alkyl groups having 1 to 10 carbon atoms such as methyl groups, and it is particularly preferable that 88 mol % or more of R are methyl groups from the viewpoint of industrial production and the technical effect of the invention. 3 It is preferable that the component (A2) is substantially free of aryl groups such as phenyl groups. If the component (A2) contains a large amount of aryl groups such as phenyl groups, the component (A2) itself may become hot-melt, making it impossible to achieve the technical effects of the present invention, and the discoloration resistance of the cured product at high temperatures may deteriorate.

[0130] In the formula, R 2 is the same group as defined above.

[0131] In the formula, f represents the general formula: R 3 3SiO 1 / 2 f is a number indicating the proportion of siloxane units. This number satisfies 0.35≦f≦0.55, and preferably 0.40≦f≦0.50. When f is equal to or greater than the lower limit of the above range, a composition containing this component can achieve good hot melt performance as a whole composition. On the other hand, when f is equal to or less than the upper limit of the above range, the mechanical strength (hardness, etc.) of the obtained cured product is not too low.

[0132] In the formula, g represents a group represented by the general formula: R 1 2SiO 2 / 2 g is a number indicating the proportion of siloxane units. This number satisfies 0≦g≦0.20, and preferably 0≦g≦0.10. When g is equal to or less than the upper limit of the range, the composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a composition that is less sticky at room temperature. In the present invention, g may be 0, and is preferred.

[0133] In the formula, h represents the general formula: R 1 SiO 3 / 2 h is a number indicating the proportion of siloxane units. This number satisfies 0≦h≦0.20, and preferably 0≦h≦0.10. When h is equal to or less than the upper limit of the range, a composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a composition that is less sticky at room temperature. In the present invention, h may be 0, and is preferred.

[0134] In the formula, i is SiO 4 / 2 i is a number indicating the proportion of siloxane units, and it is necessary that 0.45≦i≦0.65, preferably 0.40≦i≦0.65, and particularly preferably 0.50≦i≦0.65. Within this numerical range, a composition containing this component can exhibit good hot melt properties as a whole composition, and the resulting cured product can have excellent mechanical strength and is not sticky as a whole composition, resulting in a composition with good handling and workability.

[0135] In the formula, j represents the general formula: R 2 O 1 / 2 is a number indicating the proportion of units, and the unit means a hydroxyl group or alkoxy group bonded to a silicon atom that may be contained in the organopolysiloxane resin. This number satisfies 0≦j≦0.05, preferably 0≦j≦0.03. If e is equal to or less than the upper limit of the range, a material that realizes good hot melt performance as a whole composition can be obtained. In addition, the sum of e, f, g, and h, which are the sums of each siloxane unit, is ultimately equal to 1.

[0136] [Component (B)] Component (B) is one of the components that is used together with components (A2-1) and (A2-2) to form the main component of the composition, and is a linear or branched organopolysiloxane that is liquid or plastic at 25° C. and has a curing reactive functional group containing at least two carbon-carbon double bonds in the molecule. When mixed with the above-mentioned solid organopolysiloxane resin particles, this type of curing reactive chain organopolysiloxane exhibits hot melt properties as a whole composition.

[0137] Like component (A2-1), component (B) must have a curing reactive group having a carbon-carbon double bond in the molecule. Such a curing reactive group is a functional group that is hydrosilylation reactive, radical reactive, or organic peroxide curable, and forms a cured product by a crosslinking reaction with other components. Such a curing reactive group is an alkenyl group or a (meth)acrylic group, and examples thereof include the same groups as those described above, and in particular, a vinyl group or a hexenyl group is preferable.

[0138] As described above, component (B) is a linear or branched organopolysiloxane that is liquid or plastic at 25°C (room temperature), and when mixed with component (A2-1) that is solid at room temperature, or with component (A2-1) and component (A2-2), the composition as a whole exhibits hot melt properties. The structure of component (B) is a small number of branched siloxane units (for example, the general formula: R 4 SiO 3 / 2 T units (R 4 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms) or SiO 4 / 2 The organopolysiloxane may be a branched organopolysiloxane having a Q unit represented by the formula: (B-1) The following structural formula: R 4 3SiO(SiR 4 2O) k SiR 4 3 (In the formula, each R 4 are independently monovalent hydrocarbon groups having 1 to 10 carbon atoms, provided that R 4 at least two of the groups are alkenyl groups or (meth)acrylic groups, and k is a number from 20 to 10,000. It is a linear diorganopolysiloxane represented by the following formula: Preferably, it is a linear diorganopolysiloxane having one alkenyl group at each of both ends of the molecular chain.

[0139] In the above formula, each R 4are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl groups; vinyl, allyl, butenyl, pentenyl, hexenyl, or similar alkenyl groups; phenyl, tolyl, xylyl, or similar aryl groups; benzyl, phenethyl, or similar aralkyl groups; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl groups. 4 At least two of R are alkenyl groups, preferably vinyl groups. 4 is preferably a functional group selected from an alkyl group having 1 to 10 carbon atoms, such as a methyl group, and an alkenyl group, such as a vinyl group or a hexenyl group, and all of R 4 At least two of R are alkenyl groups, and the remaining R 4 From the viewpoint of the technical effect of the invention, it is preferable that R 4 It is preferable that R is substantially free of aryl groups such as phenyl groups. If it contains a large amount of aryl groups such as phenyl groups, the color resistance of the cured product at high temperatures may deteriorate. Particularly preferably, R has an alkenyl group such as a vinyl group at each end of the molecular chain and other R 4 is preferably a methyl group.

[0140] In the above formula, k is a number of 20 to 10,000, preferably 30 to 9,000, and particularly preferably 45 to 8,000. When k is equal to or greater than the lower limit of the above range, a granular composition with little stickiness at room temperature can be obtained. On the other hand, when k is equal to or less than the upper limit of the above range, the composition as a whole can achieve good hot melt performance.

[0141] [Mass ratio of component (A2-1), component (A2-2), and component (B)] From the viewpoint of being able to appropriately adjust the properties such as the elastic modulus of the obtained cured product, the ratio of the components (A2-1) and (A2-2) may be in the range of 0:100 to 90:10, preferably 75:25, preferably in the range of 0:100 to 60:40, more preferably 0:100 to 55:45. Although the component (A2-2) itself does not have curability, it is possible to control the elastic modulus of the cured product of this composition at high temperatures by adding a small amount of the component (A2-1) in combination with the component (A2-2). When a functional inorganic filler described later is added to the composition, it is possible to achieve a suitable elastic modulus and flexibility by appropriately adjusting the amount of the functional inorganic filler added and the amount of the component (A2-1) used. For example, when the amount of the functional inorganic filler added is large or when it is desired to reduce the elastic modulus of the obtained cured product as much as possible, it is also possible to compound the composition with only the component (A2-2) without adding the component (A2-1). On the other hand, when a functional inorganic filler described below is not added, it is possible to adjust the elastic modulus at room temperature and at high temperatures to the desired values ​​by increasing the amount of component (A2) added. Furthermore, in order to achieve hot melt properties for the composition as a whole, the mass ratio of component (B), which is a linear or branched organopolysiloxane, to 100 parts by mass of component (A2), which is an organopolysiloxane resin, is in the range of 10 to 100 parts by mass, preferably in the range of 10 to 70 parts by mass, and more preferably in the range of 15 to 50 parts by mass. If the content of component (B) is within this range, the resulting curable silicone composition will achieve good hot melt properties, the mechanical strength of the resulting cured product will be increased, and the stickiness of the resulting composition at room temperature will be reduced, improving its handling and workability.

[0142] The mixture exhibiting hot melt properties containing the above-mentioned component (A2-1) or components (A2-1) and (A2-2) and component (B) can be crosslinked and cured using a curing agent (C) and / or a curing catalyst (D), and optionally a curing retarder (E), depending on the type of reactive functional group they have. For example, when the reactive functional group they have is an alkenyl group, they can be combined with a curing agent (C) having a silicon-bonded hydrogen atom capable of hydrosilylation reaction as a curing agent to obtain a composition that can be cured by hydrosilylation reaction. When the reactive functional group is a radical-reactive group such as a (meth)acrylic group and / or a vinyl group, a curable silicone composition can be obtained by using the above-mentioned organic peroxide as the curing agent (C). When the reactive functional group is a (meth)acrylic group, particularly an acrylic group, a photoradical initiator can be used as the curing agent (C) to obtain a UV-curable curable silicone composition. All of these are within the scope of the curable composition of the present invention.

[0143] When the curable hot-melt silicone composition sheet used in the present invention is produced in the manner described above, it can be obtained as a transparent film. However, if it is desired to impart functionality to the resulting cured product, then in addition to the above components, it may also contain (E) a functional filler.

[0144] [Other additives] The functional filler, which is the component (E), is a component that imparts mechanical properties and other properties to the cured product, and examples thereof include inorganic fillers, organic fillers, and mixtures thereof. Examples of the inorganic fillers include reinforcing fillers, white pigments, thermally conductive fillers, conductive fillers, phosphors, and mixtures of at least two of these, and examples of the organic fillers include silicone resin-based fillers, fluororesin-based fillers, and polybutadiene resin-based fillers. The shape of these fillers is not particularly limited, and may be spherical, spindle-shaped, flat, needle-shaped, or amorphous.

[0145] When the present composition is used as a sealant, protective agent, adhesive, or the like, it is preferable for at least a part of component (E) to contain a reinforcing filler, from the viewpoint of improving the mechanical strength, protective properties, and adhesive properties of the cured product.

[0146] The reinforcing filler may be added to improve the mechanical strength of the cured product, improve the protectiveness and adhesiveness, and maintain the solid particulate state as a binder filler of the curable silicone composition before curing. Examples of such reinforcing fillers include fumed silica, precipitated silica, fused silica, calcined silica, fumed titanium dioxide, quartz, calcium carbonate, diatomaceous earth, aluminum oxide, aluminum hydroxide, zinc oxide, and zinc carbonate. In addition, these reinforcing fillers may be surface-treated with a siloxane oligomer selected from organoalkoxysilanes such as methyltrimethoxysilane; organohalosilanes such as trimethylchlorosilane; organosilazanes such as hexamethyldisilazane; α,ω-silanol group-blocked dimethylsiloxane oligomers, α,ω-silanol group-blocked methylphenylsiloxane oligomers, and α,ω-silanol group-blocked methylvinylsiloxane oligomers. The particle size of the reinforcing filler is not limited, but the median size measured by laser diffraction / scattering particle size distribution measurement is preferably within the range of 1 nm to 500 μm.Furthermore, fibrous fillers such as calcium metasilicate, potassium titanate, magnesium sulfate, sepiolite, zonolite, aluminum borate, rock wool, and glass fiber may be used as the reinforcing filler.

[0147] Furthermore, in order to impart other functions to the cured product obtained using the composition, a white pigment, a thermally conductive filler, an electrically conductive filler, or a fluorescent material may be blended in. In addition, in order to improve the stress relaxation properties of the cured product, an organic filler such as silicone elastomer fine particles may be blended in.

[0148] The white pigment is a component that imparts whiteness to the cured product and improves light reflectivity, and the cured product obtained by curing the composition by blending the component can be used as a light reflector for light emitting / optical devices. Examples of the white pigment include metal oxides such as titanium oxide, aluminum oxide, zinc oxide, zirconium oxide, and magnesium oxide; hollow fillers such as glass balloons and glass beads; and other materials such as barium sulfate, zinc sulfate, barium titanate, aluminum nitride, boron nitride, and antimony oxide. Titanium oxide is preferred because of its high light reflectance and hiding power. Aluminum oxide, zinc oxide, and barium titanate are preferred because of their high light reflectance in the UV region. The average particle size and shape of the white pigment are not limited, but the average particle size is preferably within the range of 0.05 to 10.0 μm, or 0.1 to 5.0 μm. The white pigment may be surface-treated with a material selected from a silane coupling agent, silica, and aluminum oxide.

[0149] The thermally conductive filler or the conductive filler is added for the purpose of imparting thermal conductivity / conductivity (electrical conductivity) to the cured product, and specific examples thereof include fine metal powders such as gold, silver, nickel, copper, and aluminum; fine powders in which metals such as gold, silver, nickel, and copper are vapor-deposited or plated on the surface of fine powders such as ceramics, glass, quartz, and organic resins; metal compounds such as aluminum oxide, magnesium oxide, aluminum nitride, boron nitride, and zinc oxide; graphite, and mixtures of two or more of these. When electrical insulation is required for the composition, metal oxide powders or metal nitride powders are preferred, and aluminum oxide powder, zinc oxide powder, and aluminum nitride powder are particularly preferred, and these may be used in combination with each other in terms of type, particle size, particle shape, and the like according to the requirements for thermal conductivity / conductivity.

[0150] The phosphor is a component that is blended to convert the wavelength of light emitted from a light source (optical semiconductor element) when the cured product is used as a wavelength conversion material. There are no particular limitations on the phosphor, and examples of the phosphor include yellow, red, green, and blue light-emitting phosphors made of oxide-based phosphors, oxynitride-based phosphors, nitride-based phosphors, sulfide-based phosphors, oxysulfide-based phosphors, etc., which are widely used in light-emitting diodes (LEDs).

[0151] Examples of silicone fine particles include non-reactive silicone resin fine particles and silicone elastomer fine particles, with silicone elastomer fine particles being preferred from the standpoint of improving the flexibility or stress relaxation properties of the cured product.

[0152] Silicone elastomer microparticles are crosslinked products of linear diorganopolysiloxanes mainly composed of diorganosiloxy units (D units). Silicone elastomer microparticles can be prepared by crosslinking diorganopolysiloxanes by hydrosilylation reaction or condensation reaction of silanol groups, and can be preferably obtained by crosslinking an organohydrogenpolysiloxane having silicon-bonded hydrogen atoms at the side chain or end with a diorganopolysiloxane having unsaturated hydrocarbon groups such as alkenyl groups at the side chain or end under a hydrosilylation reaction catalyst. Silicone elastomer microparticles can take various shapes such as spherical, flat, and irregular, but from the viewpoint of dispersibility, spherical is preferable, and among them, true sphere is more preferable. Examples of commercially available silicone elastomer microparticles include "Trefil E Series" and "EP Powder Series" manufactured by Toray Dow Corning Co., Ltd., and "KMP Series" manufactured by Shin-Etsu Chemical Co., Ltd.

[0153] For the purpose of stably blending the functional filler as described above in the present composition, the filler may be surface-treated using a specific surface treatment agent in an amount of 0.1 to 2.0 mass%, 0.1 to 1.0 mass%, or 0.2 to 0.8 mass% relative to the total mass of component (E). Examples of such surface treatment agents include methylhydrogenpolysiloxane, silicone resin, metal soap, silane coupling agent, perfluoroalkylsilane, and fluorine compounds such as perfluoroalkyl phosphate salt.

[0154] In particular, when component (E) is a thermally conductive filler and is blended in large amounts in the curable silicone composition of the present invention, the thermally conductive filler is preferably a plate-shaped boron nitride powder having a suitable average particle size of 0.1 to 30 μm, a granular boron nitride powder having an average particle size of 0.1 to 50 μm, a spherical and / or crushed aluminum oxide powder having an average particle size of 0.01 to 50 μm, or a spherical and / or crushed graphite having an average particle size of 0.01 to 50 μm, or a mixture of two or more of these. Most preferably, it is a mixture of two or more of spherical and crushed aluminum oxide powders having an average particle size of 0.01 to 50 μm. In particular, by combining an aluminum oxide powder having a large particle size and an aluminum oxide powder having a small particle size in a ratio that follows the closest packing theoretical distribution curve, the packing efficiency is improved, and low viscosity and high thermal conductivity are possible.

[0155] Furthermore, it is particularly preferred that at least a part of the surface of the thermally conductive filler is treated with one or more types of organosilicon compounds. The preferred range of the treatment amount is as described above. Here, examples of the organosilicon compound that is the surface treatment agent are low molecular weight organosilicon compounds such as silane, silazane, siloxane, or the like, and organosilicon polymers or oligomers such as polysiloxane, polycarbosiloxane, or the like. A preferred example of silane is a so-called silane coupling agent. Representative examples of such silane coupling agents include alkyltrialkoxysilanes (methyltrimethoxysilane, vinyltrimethoxysilane, hexyltrimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, or the like), and organofunctional group-containing trialkoxysilanes (glycidoxypropyltrimethoxysilane, epoxycyclohexylethyltrimethoxysilane, methacryloxypropyltrimethoxysilane, aminopropyltrimethoxysilane, or the like). Preferred siloxanes and polysiloxanes include hexamethyldisiloxane, 1,3-dihexyl-tetramethyldisiloxane, trialkoxysilyl single-terminated polydimethylsiloxane, trialkoxysilyl single-terminated dimethylvinyl single-terminated polydimethylsiloxane, trialkoxysilyl single-terminated organofunctional group single-terminated polydimethylsiloxane, trialkoxysilyl doubly terminated polydimethylsiloxane, organofunctional group doubly terminated polydimethylsiloxane, or the like. When siloxanes are used, the number of siloxane bonds n is preferably in the range of 2 to 150. Examples of preferred silazanes are hexamethyldisilazane, 1,3-dihexyl-tetramethyldisilazane, or the like. Examples of preferred polycarbosiloxanes are polymers with Si-C-C-Si bonds in the polymer backbone.

[0156] The content of component (E) is not limited, but in order to obtain a cured product with excellent hardness and mechanical strength, it is preferable that the content be within the range of 10 to 2000 parts by mass, 10 to 1500 parts by mass, or 10 to 1000 parts by mass relative to the sum (100 parts by mass) of components (A) and (B).

[0157] The curable silicone composition of the present invention has hot-melt properties and contains an appropriate combination of components selected from the above components (A) to (D). From the standpoint of further improving the melting properties, it is also possible to add (E') hot-melt particles having a dropping point of 50°C or higher and a melt viscosity of 10 Pa s or less as measured with a rotational viscometer at 150°C.

[0158] As long as the above dropping point conditions and the kinetic viscosity conditions at 150°C are satisfied, the type of component (E) is not particularly limited, and one or more selected from various hot-melt synthetic resins, waxes, fatty acid metal salts, etc. can be used. The component (E) exhibits low kinetic viscosity at high temperatures (150°C) and forms a molten product with excellent fluidity. Furthermore, by selecting and using in combination a component suitable for the curing mechanism from the above components (A) to (D), the component (E) in the molten product of this composition spreads quickly throughout the composition at high temperatures, thereby reducing the viscosity of the substrate surface to which the molten composition is applied and the entire composition, and also rapidly reducing the surface friction of the substrate and the molten composition, thereby significantly increasing the fluidity of the entire composition. Therefore, the viscosity and fluidity of the molten composition can be greatly improved by adding only a small amount of the component (E) to the total amount of other components.

[0159] Component (E) may be a petroleum wax such as paraffin as long as it satisfies the above-mentioned conditions of dropping point and kinetic viscosity when melted, but from the viewpoint of the technical effect of the present invention, it is preferable that it is a hot melt component consisting of a fatty acid metal salt or a fatty acid ester of an erythritol derivative, and particularly preferable are metal salts of higher fatty acids such as stearic acid, palmitic acid, oleic acid, isononanoic acid, etc., pentaerythritol tetrastearate, dipentaerythritol adipic acid stearate, glycerin tri-18-hydroxystearate, and pentaerythritol full stearate. Here, the type of the fatty acid metal salt is not particularly limited, but suitable examples include alkali metal salts such as lithium, sodium, potassium, etc.; alkaline earth metal salts such as magnesium, calcium, barium, etc.; and zinc salts.

[0160] Particularly preferred as component (E) are (E0) fatty acid metal salts with a free fatty acid content of 5.0% or less, 4.0% or less, and 0.05 to 3.5% fatty acid metal salts and erythritol derivatives. Examples of such components include at least one metal stearate. Specifically, it is most preferred to use a hot melt component with a melting point of 150°C or less selected from calcium stearate (melting point 150°C), zinc stearate (melting point 120°C), magnesium stearate (melting point 130°C), pentaerythritol tetrastearate (melting point 60-70°C), pentaerythritol adipate stearate (melting point 55-61°C), pentaerythritol full stearate (melting point 62-67°C), etc.

[0161] The amount of component (E) used is 0.01 to 5.0 parts by mass, and may be 0.01 to 3.5 parts by mass, or 0.01 to 3.0 parts by mass, when the entire composition is taken as 100 parts by mass. If the amount of component (E) used exceeds the upper limit, the adhesiveness and mechanical strength of the cured product obtained from the curable silicone composition of the present invention may be insufficient. If the amount of component (E) used is less than the lower limit, sufficient fluidity may not be achieved when heated and melted.

[0162] The composition may further contain other optional components such as a cure retarder and an adhesion promoter, provided that the object of the present invention is not impaired.

[0163] In the case where the curing of the composition proceeds by hydrosilylation reaction, examples of the curing agent include alkyne alcohols such as 2-methyl-3-butyn-2-ol, 3,5-dimethyl-1-hexyn-3-ol, 2-phenyl-3-butyn-2-ol, and 1-ethynyl-1-cyclohexanol; enyne compounds such as 3-methyl-3-penten-1-yne and 3,5-dimethyl-3-hexen-1-yne; alkenyl-containing low molecular weight siloxanes such as tetramethyltetravinylcyclotetrasiloxane and tetramethyltetrahexenylcyclotetrasiloxane; and alkynyloxysilanes such as methyl-tris(1,1-dimethylpropynyloxy)silane and vinyl-tris(1,1-dimethylpropynyloxy)silane. Among these, it is particularly preferable to use a compound having a boiling point of 200° C. or more under atmospheric pressure. The content of the curing retarder in the curable silicone composition is not particularly limited, but it is preferably within the range of 1 to 10,000 ppm by mass with respect to the composition. In this specification, atmospheric pressure refers to the atmospheric pressure in the environment in which the curable silicone composition of the present invention is handled, such as in a laboratory or factory, and is not limited to a specific pressure, but will usually be within the range of 1 atmosphere (1013.25 hPa) to -100 hPa to +100 hPa, and is particularly 1 atmosphere.

[0164] The curable hot melt silicone composition of the present invention may contain an adhesion promoter. As the adhesion promoter, an organosilicon compound having at least one alkoxy group bonded to a silicon atom in one molecule is preferred. Examples of the alkoxy group include methoxy, ethoxy, propoxy, butoxy, and methoxyethoxy groups, and methoxy groups are particularly preferred. In addition, examples of groups bonded to silicon atoms other than the alkoxy group in the organosilicon compound include halogen-substituted or unsubstituted monovalent hydrocarbon groups such as alkyl groups, alkenyl groups, aryl groups, aralkyl groups, and halogenated alkyl groups; glycidoxyalkyl groups such as 3-glycidoxypropyl and 4-glycidoxybutyl groups; epoxycyclohexylalkyl groups such as 2-(3,4-epoxycyclohexyl)ethyl and 3-(3,4-epoxycyclohexyl)propyl groups; epoxyalkyl groups such as 3,4-epoxybutyl and 7,8-epoxyoctyl groups; acrylic group-containing monovalent organic groups such as 3-methacryloxypropyl groups; and hydrogen atoms. The organosilicon compound preferably has a group capable of reacting with the alkenyl group or silicon-bonded hydrogen atom in the composition, and more specifically, preferably has a silicon-bonded hydrogen atom or an alkenyl group.In addition, since it can provide good adhesion to various substrates, the organosilicon compound preferably has at least one epoxy-containing monovalent organic group in one molecule.Examples of such organosilicon compounds include organosilane compounds, organosiloxane oligomers, and alkyl silicates.Examples of the molecular structure of the organosiloxane oligomer or alkyl silicate include linear, partially branched linear, branched, cyclic, and net-like, and in particular, linear, branched, and net-like are preferred.Examples of organosilicon compounds include silane compounds such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 3-methacryloxypropyltrimethoxysilane; siloxane compounds having at least one silicon-bonded alkenyl group or silicon-bonded hydrogen atom, and at least one silicon-bonded alkoxy group in one molecule; a mixture of a silane compound or siloxane compound having at least one silicon-bonded alkoxy group and a siloxane compound having at least one silicon-bonded hydroxy group and at least one silicon-bonded alkenyl group in one molecule; a reaction mixture of an amino group-containing organoalkoxysilane and an epoxy group-containing organoalkoxysilane; an organic compound having at least two alkoxysilyl groups in one molecule and containing a bond other than a silicon-oxygen bond between the silyl groups; R a n Si(OR b ) 4-n (In the formula, R a is a monovalent epoxy-containing organic group, and R b is an alkyl group having 1 to 6 carbon atoms or a hydrogen atom; and n is a number ranging from 1 to 3. Examples of the adhesion promoter include epoxy group-containing silanes represented by the formula (I) or partial hydrolysis condensates thereof, a reaction mixture of a vinyl group-containing siloxane oligomer (including those with a linear or cyclic structure) and an epoxy group-containing trialkoxysilane, methyl polysilicate, ethyl polysilicate, and epoxy group-containing ethyl polysilicate. The adhesion promoter is preferably a low-viscosity liquid, and although there are no limitations on its viscosity, it is preferably within the range of 1 to 500 mPa·s at 25°C. Furthermore, although there are no limitations on the content of the adhesion promoter, it is preferably within the range of 0.01 to 10 parts by mass per 100 parts by mass of the total of the curable hot-melt silicone composition of the present invention.

[0165] In the present invention, a particularly suitable adhesion promoter is a reaction mixture of an amino group-containing organoalkoxysilane and an epoxy group-containing organoalkoxysilane. This component improves the initial adhesion to various substrates that the curable silicone composition comes into contact with during curing, and especially improves low-temperature adhesion to unwashed adherends. In addition, depending on the curing system, such as when the curable silicone composition containing this adhesion promoter is a condensation curing system, it may also act as a crosslinking agent. Such reaction mixtures are disclosed in JP-B-52-8854 and JP-A-10-195085.

[0166] Examples of alkoxysilanes having an amino group-containing organic group that constitute a component of such an adhesion promoter include aminomethyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)aminomethyltributoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, and 3-anilinopropyltriethoxysilane.

[0167] Examples of epoxy group-containing organoalkoxysilanes include 3-glycidoxyprolyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethylmethyldimethoxysilane.

[0168] The molar ratio of these alkoxysilanes having an amino group-containing organic group to those having an epoxy group-containing organic group is preferably within the range of (1:1.5) to (1:5), and particularly preferably within the range of (1:2) to (1:4). This component (e1) can be easily synthesized by mixing the above-mentioned alkoxysilanes having an amino group-containing organic group and alkoxysilanes having an epoxy group-containing organic group and reacting them at room temperature or under heating.

[0169] In particular, in the curable hot-melt silicone composition of the present invention, when an alkoxysilane having an amino group-containing organic group is reacted with an alkoxysilane having an epoxy group-containing organic group by the method described in JP-A-10-195085, a compound having the general formula: [ka] {where, R 1 is an alkyl group, an alkenyl group, or an alkoxy group, and R 2 may have the same or different general formula: [ka] (In the formula, R 4 is an alkylene group or an alkyleneoxyalkylene group, R 5 is a monovalent hydrocarbon group, R 6 is an alkyl group, and R 7 is an alkylene group, and R 8 is an alkyl group, an alkenyl group, or an acyl group, and a is 0, 1, or 2. R is a group selected from the group consisting of groups represented by 3 are the same or different hydrogen atoms or alkyl groups. It is particularly preferred that the compound contains a carbasilatrane derivative represented by the following structure: Examples of such carbasilatrane derivatives include carbasilatrane derivatives having a silicon-bonded alkoxy group or a silicon-bonded alkenyl group in one molecule, as represented by the following structure: [ka] (In the formula, Rc is a group selected from a methoxy group, an ethoxy group, a vinyl group, an allyl group, and a hexenyl group.)

[0170] In the present invention, a silatrane derivative represented by the following structural formula may be used as an adhesion promoter. [ka] R in the formula 1 are the same or different hydrogen atoms or alkyl groups, in particular R 1 is preferably a hydrogen atom or a methyl group. 2 represents a hydrogen atom, an alkyl group, or a group of the general formula: -R 4 -Si(OR 5 ) x R 6 (3-x) are the same or different groups selected from the group consisting of alkoxysilyl group-containing organic groups represented by the formula: 2 At least one of R is an alkoxysilyl group-containing organic group. 2 Examples of the alkyl group of R include a methyl group. 2 In the alkoxysilyl group-containing organic group, R 4 is a divalent organic group, and examples thereof include an alkylene group or an alkyleneoxyalkylene group, and particularly preferably an ethylene group, a propylene group, a butylene group, a methyleneoxypropylene group, or a methyleneoxypentylene group. 5 is an alkyl group having 1 to 10 carbon atoms, and is preferably a methyl group or an ethyl group. 6 is a substituted or unsubstituted monovalent hydrocarbon group, preferably a methyl group, and x in the formula is 1, 2, or 3, preferably 3.

[0171] Such an R 2 Examples of the alkoxysilyl group-containing organic group include the following groups. -(CH2)2Si(OCH3)2-(CH2)2Si(OCH3)2CH3 -(CH2)3Si(OC2H5)2-(CH2)3Si(OC2H5)(CH3)2 -CH2O(CH2)3Si(OCH3)3 -CH2O(CH2)3Si(OC2H5)3 -CH2O(CH2)3Si(OCH3)2CH3 -CH2O(CH2)3Si(OC2H5)2CH3 -CH2OCH2Si(OCH3)2-CH2OCH2Si(OCH3)(CH3)2

[0172] R in the above formula 3 is at least one group selected from the group consisting of substituted or unsubstituted monovalent hydrocarbon groups, alkoxy groups having 1 to 10 carbon atoms, glycidoxyalkyl groups, oxiranylalkyl groups, and acyloxyalkyl groups; R 3 Examples of the monovalent hydrocarbon group include alkyl groups such as methyl groups. 3 Examples of the alkoxy group of R include a methoxy group, an ethoxy group, and a propoxy group. 3 An example of the glycidoxyalkyl group of R is a 3-glycidoxypropyl group. 3 Examples of the oxiranylalkyl group of R include a 4-oxiranylbutyl group and an 8-oxiranyloctyl group. 3 Examples of the acyloxyalkyl group include an acetoxypropyl group and a 3-methacryloxypropyl group. 3 Preferably, the alkyl group, alkenyl group, or alkoxy group is used, more preferably an alkyl group or an alkenyl group, and particularly preferably a group selected from a methyl group, a vinyl group, an allyl group, and a hexenyl group.

[0173] Furthermore, the composition may contain other optional components, such as heat resistance agents such as iron oxide (red oxide), cerium oxide, cerium dimethylsilanolate, fatty acid cerium salts, cerium hydroxide, and zirconium compounds, as well as dyes, pigments other than white, and flame retardants, so long as the object of the present invention is not impaired.

[0174] Particularly preferred curable hot-melt silicone compositions for use in the present invention include the hydrosilylation-curable compositions described below.

[0175] [Preferred embodiments of the curable silicone composition] The curable hot melt silicone composition of the present invention is a SiO 4 / 2The silicone composition preferably has as its main components a carbon-carbon double bond-containing organopolysiloxane resin (component (A') below) containing siloxane units represented by the formula (I) in an amount of at least 20 mol % of all siloxane units, and a carbon-carbon secondary bond-containing linear or branched organopolysiloxane (component (B') below) that is liquid or plastic at 25°C, and contains an organohydrogenpolysiloxane (component (C') below) as a crosslinking agent, and a hydrosilylation reaction catalyst (component (D') below). In particular, the curable silicone composition of the present invention preferably uses, as the organohydrogenpolysiloxane having silicon-bonded hydrogen atoms as the crosslinking agent, an organohydrogenpolysiloxane that has a specific chemical structure and exhibits a mass loss rate of 10% or less after exposure to 100°C under atmospheric pressure for 1 hour, relative to the mass before exposure. In addition, the curable silicone composition of the present invention may optionally contain a hydrosilylation reaction retarder, i.e., a curing retarder having a boiling point of 200°C or higher at 1 atm. In addition, the composition of the present invention uses organopolysiloxane resins that do not have hot melt properties as components (A1') and (A2'), but is characterized in that the composition as a whole, including components (B') to (D'), has hot melt properties. In addition, with respect to the curable hot melt silicone composition of the preferred embodiment described below, unless otherwise specified, "having hot melt properties" means that the softening point of the composition is between 50 and 200°C, the composition has a melt viscosity at 150°C (preferably a melt viscosity of less than 1000 Pa·s), and has a flowable property. In this specification, the curable hot melt silicone composition means a curable silicone composition having hot melt properties.

[0176] [Particularly preferred curable hot melt silicone compositions] The curable hot-melt silicone composition of the present invention is a silicone rubber composition comprising a curing reactive functional group containing a carbon-carbon double bond in the (A1') molecule and a SiO 4 / 2and (A2') an organopolysiloxane resin which is solid at 25°C and does not have hot melt properties by itself, and which contains at least 20 mol % or more of siloxane units represented by the formula: 4 / 2The silicone composition is a heat-curable silicone composition comprising as main components an organopolysiloxane resin that is solid at 25°C and does not have hot-melt properties by itself, and that contains siloxane units represented by the following formula (A1'):(A2) in a mass ratio of 0:100 to 90:10, preferably 0:100 to 75:25, of all siloxane units (A') and a carbon-carbon secondary bond-containing linear or branched organopolysiloxane (component (B')) that is liquid or plastic at 25°C, and which contains an organohydrogenpolysiloxane (component (C')) as a crosslinking agent, and a hydrosilylation reaction catalyst (component (D')). The curable hot-melt silicone composition of the present invention is characterized in that it uses an organohydrogenpolysiloxane having a specific chemical structure as the crosslinking agent having silicon-bonded hydrogen atoms, and that the mass loss rate after exposure to 100°C under atmospheric pressure for 1 hour is 10% or less compared to the mass before exposure. In addition, the curable hot-melt silicone composition of the present invention may optionally use a hydrosilylation reaction retarder, so-called a curing retarder, in which case it is preferable to use a curing retarder having a boiling point of 200°C or higher, particularly a boiling point of 200°C or higher under 1 atmospheric pressure (1013.25hPa). In addition, the composition of the present invention uses organopolysiloxane resins as components (A1') and (A2') that do not have hot-melt properties by themselves, but has a further characteristic that the composition as a whole including components (B') to (D') has hot-melt properties. In the present invention, unless otherwise specified, "having hot-melt properties" means that the composition has a softening point between 50 and 200°C, has a melt viscosity at 150°C (preferably a melt viscosity of less than 1000 Pa s), and is flowable. Therefore, in this specification, the curable silicone composition of the present invention that has hot-melt properties is also referred to as a curable hot-melt silicone composition.

[0177] [The significance of combining ingredients that are less likely to volatilize] The composition of the present invention is characterized by using a combination of components that are difficult to volatilize at about 100 ° C. under atmospheric pressure, particularly at 1 atmosphere (1013.25 hPa), or components with a low volatile content, as components constituting the composition. This is because, in the production process of the curable hot melt silicone sheet or film of the present invention described below, in order to obtain a sheet or film that does not contain voids, it is necessary to melt and knead each component of the curable silicone composition and the composition obtained therefrom at a temperature range of 50 to 150 ° C. under reduced pressure, and a sheet or film that does not contain voids can be produced by using each component of the present invention. Each component is exposed to a predetermined temperature under reduced pressure for a very short time, but if a large amount of the active ingredient volatilizes under these kneading conditions, a problem occurs in that a composition with the designed characteristics cannot be obtained. In particular, when the amount of the crosslinking agent, such as organohydrogenpolysiloxane or a curing retarder, added is small relative to the total mass of the curable silicone composition, the volatilization of these components causes the characteristics of the composition (curing characteristics, physical properties of the cured product, etc.) to change significantly from the intended values. For this reason, it is necessary to use components that are less likely to volatilize in the present invention, particularly component (C') and optional component (E').

[0178] [Hot melt properties and composition of the curable silicone composition] The curable silicone composition of the present invention is characterized in that the composition as a whole has hot melt properties and is flowable under heating conditions. In particular, the curable silicone composition of the present invention preferably has a softening point of 50°C or higher and a melt viscosity at 150°C (preferably a melt viscosity of less than 1000 Pa s). Note that in the present invention, it is sufficient for the composition as a whole to have hot melt properties, and the individual components that make up the composition do not necessarily have hot melt properties.

[0179] More specifically, the curable silicone composition according to the present invention, i.e., the curable hot-melt silicone composition, contains the following components (A'), (B'), (C'), and (D') as essential components in the proportions shown below, and the composition as a whole exhibits hot-melt properties. (A') 100 parts by mass of an organopolysiloxane resin containing the following components (A1') and (A2') in a mass ratio of 0:100 to 90:10, preferably 0:100 to 75:25: (A1') A compound having a curing reactive functional group containing a carbon-carbon double bond in the molecule, and SiO 4 / 2 an organopolysiloxane resin which does not have hot melt properties by itself and is solid at 25°C, and which contains at least 20 mol % or more of siloxane units represented by the formula: (A2') A compound having no curing reactive functional group containing a carbon-carbon double bond in the molecule and having no SiO 4 / 2 an organopolysiloxane resin which does not have hot melt properties by itself and is solid at 25°C, and which contains siloxane units represented by the following formula (I) in an amount of at least 20 mol % based on all siloxane units; (B') 10 to 100 parts by mass of a linear or branched organopolysiloxane which has a curable functional group containing at least two carbon-carbon double bonds in the molecule and is liquid or plastic at 25°C; (C') The following average composition formula (1'): (R 4 3SiO 1 / 2 ) a (R 5 2SiO 2 / 2 ) b (R 5 SiO 3 / 2 ) c (SiO 4 / 2 ) d (1') (In the formula, R 4 and R 5 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms that does not contain an aliphatic unsaturated bond, and all R 4 At least two of the a, b, c, and d are hydrogen atoms, and a, b, c, and d are numbers that satisfy the conditions: 0.01≦a≦0.6, 0≦b, 0≦c≦0.9, 0≦d≦0.9, and a+b+c+d=1 and c+d≧0.2. and which has a mass loss rate of 10 mass% or less after exposure to 100°C under atmospheric pressure, particularly at 1 atmosphere, for 1 hour compared to before exposure (an amount such that the number of hydrogen atoms bonded to silicon atoms per alkenyl group bonded to silicon atoms contained in the entire composition is 0.5 to 20.0); and (D') a hydrosilylation reaction catalyst in an amount sufficient to cure the composition. Furthermore, the curable silicone composition may contain the following component (E′) as an optional component: (E') A cure retarder for hydrosilylation reactions having a boiling point of 200°C or higher under atmospheric pressure, particularly at 1 atmosphere. Furthermore, other additives known in the art may be added to the curable hot-melt silicone composition of the present invention, as long as the desired properties of the present invention are maintained. The additives are as described above.

[0180] The shape of the curable hot-melt silicone composition of the present invention is not particularly limited, but may be, for example, in the form of a sheet or film, and is particularly preferably in the form of a sheet or film. Below, components (A') to (D') and optional component (E') contained in the composition of the present invention will be explained.

[0181] [Component (A')] The curable silicone composition of the present invention comprises, as component (A'), a curable silicone having a curing reactive functional group containing a carbon-carbon double bond, SiO 4 / 2 and an organopolysiloxane resin which is solid at 25°C and does not exhibit hot melt properties by itself, and which contains at least 20 mol% or more of siloxane units represented by the formula (I) based on all siloxane units, and which does not have a curing reactive functional group containing a carbon-carbon double bond, and which is SiO 4 / 2 and an organopolysiloxane resin which does not exhibit hot melt properties by itself and is solid at 25°C, and which contains siloxane units represented by the formula: 1 / 2, R2SiO 2 / 2 , RSiO 3 / 2 (R represents a monovalent organic group, particularly a monovalent hydrocarbon group having 1 to 10 carbon atoms), or 2 O 1 / 2 (R 2 may contain a hydroxyl group or an alkoxy group represented by (wherein the siloxane unit is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms), but preferably, at least 20 mol % of the total siloxane units are SiO 4 / 2 It contains a siloxane unit represented by SiO 4 / 2 If the content of the siloxane unit represented by the formula (I) is less than 20 mol %, even if the organopolysiloxane resin contains other branched siloxane units (e.g., RSiO 3 / 2 ) in large amounts, the technical effect of the present invention may not be achieved.

[0182] Such organopolysiloxane resin of component (A') is (A1') A compound having a curing reactive functional group containing a carbon-carbon double bond in the molecule, and SiO 4 / 2 and an organopolysiloxane resin which does not have hot melt properties by itself and is solid at 25° C., and which contains at least 20 mol % or more of siloxane units represented by the formula: (A2') A compound having no curing reactive functional group containing a carbon-carbon double bond in the molecule and having no SiO 4 / 2 The organopolysiloxane resin is a solid at 25°C and does not have hot melt properties by itself, and contains at least 20 mol % of all siloxane units represented by the formula: In addition, component (A1') is an optional component in component (A'), and only component (A2') described below may be used as component (A'). The term "curing reactive" means that the component (C') can undergo a hydrosilylation reaction with the organohydrogensiloxane, thereby curing the entire composition.

[0183] The above component (A') does not exhibit hot melt properties by itself, but by using it in combination with the component (B') described below within a specified quantitative ratio range, the composition of the present invention as a whole can be made to have hot melt properties.

[0184] [Organopolysiloxane resin having a curing reactive functional group (A1')] The above component (A1') is one of the main components of the composition, and is SiO 4 / 2 The organopolysiloxane resin contains siloxane units represented by the following formula (1) in an amount of at least 20 mol % of all siloxane units, does not have hot melt properties by itself, and has a curing reactive functional group containing a carbon-carbon double bond in the molecule.

[0185] Component (A1') must have a curing reactive group having a carbon-carbon double bond in the molecule. Such a curing reactive group is a hydrosilylation reactive functional group, and can form a cured product by hydrosilylation crosslinking reaction with component (C'). Such a curing reactive group is particularly preferably an alkenyl group, such as a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, or other alkenyl group having 2 to 10 carbon atoms, and particularly preferably a vinyl group or a hexenyl group.

[0186] Component (A1') is an organopolysiloxane resin that does not have hot melt properties by itself and is solid in a solvent-free state. Here, not having hot melt properties means that the organopolysiloxane resin, which is component (A1'), does not exhibit heat melting behavior by itself at 200°C or less, specifically means that it has no softening point or melt viscosity at 200°C or less. In order for component (A1') to exhibit such physical properties, the functional groups in the organopolysiloxane resin are monovalent hydrocarbon groups having 1 to 10 carbon atoms, particularly functional groups selected from alkyl groups having 1 to 10 carbon atoms such as methyl groups, and do not substantially contain aryl groups such as phenyl groups, for example, the proportion of aryl groups in all silicon-bonded organic groups is preferably 5 mol% or less, more preferably 2 mol% or less, and it is particularly preferable that the component does not contain any aryl groups at all. When component (A1') contains a large amount of aryl groups such as phenyl groups as organic groups, the component may have hot melt properties by itself, and SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.

[0187] Preferably, the functional groups bonded to silicon atoms in the organopolysiloxane resin of component (A1') are selected from alkenyl groups such as methyl and vinyl, and it is preferred that 70 to 99 mol% of all the organic groups bonded to silicon atoms are methyl, more preferably 80 to 99 mol% are methyl, and particularly preferably 88 to 99 mol% are methyl, and the remaining organic groups bonded to silicon atoms are alkenyl groups such as vinyl. In this range, component (A1') does not have hot melt properties by itself, but is useful as a component that is particularly excellent in the color resistance at high temperatures of the cured product obtained from the curable silicone composition of the present invention. The organopolysiloxane resin of component (A1') may contain a small amount of hydroxyl or alkoxy groups.

[0188] Component (A1') is an organopolysiloxane resin that is solid in the absence of a solvent and contains SiO 4 / 2The siloxane unit represented by the formula (I) is preferably at least 20 mol % of the total siloxane units. 4 / 2 The units account for at least 40 mol % of all siloxane units, and preferably 50 mol % or more, and particularly preferably in the range of 50 to 90 mol %. The organic group R in the organopolysiloxane resin of component (A1') is a monovalent organic group, and is preferably a functional group selected from monovalent hydrocarbon groups having 1 to 10 carbon atoms, particularly alkyl and alkenyl groups having 1 to 10 carbon atoms, such as methyl groups, and from the viewpoint of technical effect, it is preferable that the group R is substantially free of aryl groups, such as phenyl groups, as described above.

[0189] Preferably, component (A1') is (A1-1') The average unit formula: (R 1 3SiO 1 / 2 ) a (R 1 2SiO 2 / 2 ) b (R 1 SiO 3 / 2 ) c (SiO 4 / 2 ) d (R 2 O 1 / 2)e (In the formula, each R 1 are independently monovalent hydrocarbon groups having 1 to 10 carbon atoms, provided that the total number of R 1 are 1 to 12 mole percent alkenyl groups; 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; and a, b, c, d, and e are numbers that satisfy the following: 0.10≦a≦0.60, 0≦b≦0.70, 0≦c≦0.80, 0≦d≦0.65, 0≦e≦0.05, with the proviso that c+d>0.20 and a+b+c+d=1). This organopolysiloxane resin is a solid at 25° C. and does not have hot melt properties by itself.

[0190] In the above average unit formula, each R 1are independently selected from the group consisting of monovalent hydrocarbon groups having 1 to 10 carbon atoms, for example, alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, and heptyl, particularly preferably methyl groups; alkenyl groups such as vinyl, allyl, butenyl, pentenyl, and hexenyl, particularly preferably vinyl groups and / or 1-hexenyl groups; aryl groups such as phenyl, tolyl, and xylyl, particularly preferably phenyl groups; and aralkyl groups such as benzyl and phenethyl. Furthermore, the total R 1 is an alkenyl group, and preferably, all R 1 Of these, 2 to 10 mol % is an alkenyl group, and particularly preferably a vinyl group. If the content of alkenyl groups is less than the lower limit of the above range, the mechanical strength (hardness, etc.) of the resulting cured product may be insufficient. On the other hand, if the content of alkenyl groups is equal to or less than the upper limit of the above range, the composition containing this component can achieve good hot melt performance as a whole composition. 1 is preferably a functional group selected from an alkyl group having 1 to 10 carbon atoms, such as a methyl group, and an alkenyl group, such as a vinyl group or a hexenyl group. From the viewpoint of the technical effects of the present invention, R 1 It is preferable that the component (A') does not substantially contain aryl groups such as phenyl groups. If the component (A') contains a large amount of aryl groups such as phenyl groups, the component (A') itself will have hot melt properties, which may make it impossible to achieve the technical effects of the present invention. In addition, in the cured product, SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.

[0191] In the above formula, R 2 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 2 Examples of the alkyl group of R include methyl, ethyl, propyl, butyl, pentyl, and hexyl. 2 Group R containing 2 O 1 / 2 corresponds to the hydroxyl group or alkoxy group contained in the organopolysiloxane resin of component (A').

[0192] In the above formula, a represents the general formula: R 13SiO 1 / 2 a is a number indicating the proportion of siloxane units. a satisfies 0.1≦a≦0.60, and preferably 0.15≦a≦0.55. When a is equal to or greater than the lower limit of the above range, a composition containing this component can achieve good hot melt performance as a whole composition. On the other hand, when a is equal to or less than the upper limit of the above range, the mechanical strength (hardness, elongation, etc.) of the cured product obtained by curing the curable silicone composition of the present invention is not too low.

[0193] In the above formula, b represents the general formula: R 1 2SiO 2 / 2 is a number indicating the proportion of siloxane units. b satisfies 0≦b≦0.70, and preferably 0≦b≦0.60. When b is equal to or less than the upper limit of the aforementioned range, a composition containing this component can achieve good hot melt performance as a whole composition, and can also provide a composition that is less sticky at room temperature.

[0194] In the above formula, c represents the general formula: R 3 SiO 3 / 2 is a number indicating the proportion of siloxane units. c satisfies 0≦c≦0.80, preferably 0≦c≦0.75. When c is equal to or less than the upper limit of the above range, a composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a low-tack or tack-free composition that is less sticky at room temperature. In the present invention, c may be 0, and it is preferable that c is 0.

[0195] In the above formula, d is a compound of the formula SiO 4 / 2 is a number indicating the proportion of siloxane units, and must be 0.00≦d≦0.65, preferably 0.20≦d≦0.65, and particularly preferably 0.25≦d≦0.65. When d is within the above-mentioned numerical range, a composition containing this component can achieve good hot melt performance as a whole composition, and the cured product obtained by curing the composition can have sufficient flexibility.

[0196] In the present invention, in the above formula, c or d may be 0, but it is necessary that c+d>0.20. If the value of c+d is 0.20 or less, the composition as a whole may not achieve good hot melt performance, and the technical effects of the present invention may not be fully achieved.

[0197] In the above formula, e represents the general formula: R 2 O 1 / 2 is a number indicating the proportion of units, and the unit means a hydroxyl group or alkoxy group bonded to a silicon atom that may be contained in the organopolysiloxane resin. e satisfies 0≦e≦0.05, and preferably 0≦e≦0.03. If e is equal to or less than the upper limit of the range, a material that realizes good hot melt performance as a whole composition can be obtained. In the above formula, the sum of a, b, c, and d, which are the sums of each siloxane unit, is equal to 1.

[0198] Although component (A1') is an organopolysiloxane resin having the above characteristics, it is solid at room temperature, so in order to physically mix it with component (B') described later, it is preferable to use it in a state of being dissolved in a solvent or a mixture of solvents selected from the group consisting of aromatic hydrocarbons such as toluene, xylene, and mesitylene; ethers such as tetrahydrofuran and dipropyl ether; silicones such as hexamethyldisiloxane, octamethyltrisiloxane, and decamethyltetrasiloxane; esters such as ethyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate; and ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone. The solvent used here can be efficiently removed in the process described later.

[0199] [Component (A2')] Component (A2') is one of the main ingredients of the composition, and is an organopolysiloxane resin that does not possess hot melt properties by itself, does not contain curing reactive functional groups, and is a solid at 25°C. By using this component in combination with the aforementioned components (A1') and (B') within specific quantitative ranges, it is a component that achieves hot melt properties of the curable silicone composition as a whole, and excellent stress relaxation properties of the cured product obtained by curing the curable silicone composition.

[0200] Component (A2') is an organopolysiloxane resin that does not have hot melt properties by itself and is solid in a solvent-free state. Here, not having hot melt properties means that the organopolysiloxane resin, which is component (A2'), does not exhibit heat melting behavior by itself at 200°C or less, specifically, it means that it has no softening point or melt viscosity at 200°C or less. In order for component (A2') to exhibit such physical properties, the functional groups in the organopolysiloxane resin are monovalent hydrocarbon groups having 1 to 10 carbon atoms, particularly functional groups selected from alkyl groups having 1 to 10 carbon atoms such as methyl groups, and do not substantially contain aryl groups such as phenyl groups, for example, the proportion of aryl groups in all silicon-bonded organic groups is preferably 5 mol% or less, more preferably 2 mol% or less, and it is particularly preferable that the component does not contain any aryl groups at all. When component (A2') contains a large amount of aryl groups such as phenyl groups as organic groups, the component may have hot melt properties, and SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.

[0201] Component (A2') is a solid at 25°C like component (A1'), and is SiO 4 / 2The organopolysiloxane resin contains siloxane units represented by the formula (I) in an amount of at least 20 mol % of all siloxane units, but is characterized by not having a curing reactive functional group containing at least one carbon-carbon double bond in the molecule. That is, component (A2') is characterized by not containing an alkenyl group such as a vinyl group as a functional group in the organopolysiloxane resin. Examples of groups contained in the organopolysiloxane resin of component (A2') include monovalent hydrocarbon groups having 1 to 10 carbon atoms, particularly alkyl groups having 1 to 10 carbon atoms such as a methyl group, and this organopolysiloxane resin is substantially free of aryl groups such as a phenyl group, for example, the proportion of aryl groups in all silicon-bonded organic groups is preferably 5 mol % or less, more preferably 2 mol % or less, and particularly preferably does not contain any aryl groups at all.

[0202] Preferably, the functional groups bonded to silicon atoms in component (A2') are alkyl groups having 1 to 10 carbon atoms, such as methyl groups, and it is preferred that 70 to 100 mol % of all the organic groups bonded to silicon atoms are methyl groups, more preferably 80 to 100 mol %, and particularly preferably 88 to 100 mol %. Within such ranges, component (A2') does not exhibit hot melt properties by itself and is highly compatible with SiO 4 / 2 It can be a component that has an especially excellent reinforcing effect on the cured product containing a siloxane unit represented by the following formula: The organopolysiloxane resin of component (A2') may contain a small amount of hydroxyl groups or alkoxy groups.

[0203] Since component (A2') does not have a curing reactive functional group having a carbon-carbon double bond in the molecule, it does not form a cured product by itself when combined with the organohydrogenpolysiloxane of component (C'), but it does have an effect of improving the hot melt properties of the curable silicone composition of the present invention as a whole and reinforcing the cured product obtained by curing the curable silicone composition. In addition, by using it in combination with component (A1') having a curing reactive functional group as necessary, it is possible to adjust the heat melting properties of the obtained curable silicone composition and the physical properties after curing of the composition.

[0204] Component (A2') is an organopolysiloxane resin that is solid at 25°C in the absence of a solvent and contains branched siloxane units, SiO 4 / 2 Preferably, the organopolysiloxane of component (A2') contains siloxane units represented by the formula: SiO 4 / 2 The units account for at least 40 mol % of all siloxane units, and preferably 50 mol % or more, and particularly preferably in the range of 50 to 65 mol %.

[0205] Preferably, component (A2') is a copolymer having the following average unit formula: (R 3 3SiO 1 / 2 ) f (R 3 2SiO 2 / 2 ) g (R 3 SiO 3 / 2 ) h (SiO 4 / 2 ) i (R 2 O 1 / 2)j (In the formula, each R 3 each independently represents a monovalent hydrocarbon group having 1 to 10 carbon atoms and no carbon-carbon double bonds; R 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; f, g, h, i, and j are numbers that satisfy the following: 0.35≦f≦0.55, 0≦g≦0.20, 0≦h≦0.20, 0.45≦i≦0.65, 0≦j≦0.05, and f+g+h+i=1). This organopolysiloxane resin does not have hot melt properties by itself.

[0206] In the above average unit formula, each R 3are independently monovalent hydrocarbon groups having 1 to 10 carbon atoms and not containing a carbon-carbon double bond, for example, alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, and heptyl, particularly preferably methyl groups; aryl groups such as phenyl, tolyl, and xylyl, particularly preferably phenyl groups; and aralkyl groups such as benzyl and phenethyl. Here, the total R 3 It is preferable that 70 mol % or more of R are alkyl groups having 1 to 10 carbon atoms, such as methyl groups, particularly methyl groups, and it is particularly preferable that 88 mol % or more of R are alkyl groups having 1 to 10 carbon atoms, particularly methyl groups, from the viewpoint of industrial production and the technical effect of the invention. 3 It is preferable that component (A2') is substantially free of aryl groups such as phenyl groups. If it contains a large amount of aryl groups such as phenyl groups, component (A2') itself will have hot-melt properties, which may make it impossible to achieve the technical effects of the present invention, and may also deteriorate the discoloration resistance at high temperatures of the cured product obtained by curing the curable silicone composition of the present invention.

[0207] In the above formula, R 2 is as mentioned above, but R 2 When is an alkyl group, examples of alkyl groups include methyl, ethyl, propyl, butyl, pentyl, and hexyl.

[0208] In the above formula, f represents the general formula: R 3 3SiO 1 / 2 f is a number indicating the proportion of siloxane units. f satisfies 0.35≦f≦0.55, and preferably 0.40≦f≦0.50. When f is equal to or greater than the lower limit of the aforementioned range, a curable silicone composition containing this component can achieve good hot melt performance as a whole composition. On the other hand, when f is equal to or less than the upper limit of the aforementioned range, the mechanical strength (hardness, etc.) of the obtained cured product will not be too low.

[0209] In the above formula, g represents the general formula: R 1 2SiO 2 / 2g is a number indicating the proportion of siloxane units. g satisfies 0≦g≦0.20, preferably 0≦g≦0.10. When g is equal to or less than the upper limit of the range, the curable silicone composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a composition that is less sticky at room temperature. In the present invention, g may be 0, and preferably g is 0.

[0210] In the above formula, h represents the general formula: R 1 SiO 3 / 2 h is a number indicating the proportion of siloxane units. h satisfies 0≦h≦0.20, preferably 0≦h≦0.10. When h is equal to or less than the upper limit of the range, the curable silicone composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a composition that is less sticky at room temperature. In the present invention, h may be 0, and it is preferable that h is 0.

[0211] In the above formula, i is SiO 4 / 2 is a number indicating the proportion of siloxane units, and it is necessary that 0.45≦i≦0.65, with 0.50≦i≦0.65 being particularly preferred. When i is within this numerical range, a curable silicone composition containing this component can achieve good hot melt performance as a whole composition, and the cured product obtained by curing the curable silicone composition can have excellent mechanical strength, and the composition as a whole can be made to be non-sticky and easy to handle.

[0212] In the above formula, j represents the general formula: R 2 O 1 / 2 is a number indicating the proportion of units, and the unit means a hydroxyl group or alkoxy group bonded to a silicon atom that may be contained in the organopolysiloxane resin. j satisfies 0≦j≦0.05, preferably 0≦j≦0.03. When j is equal to or less than the upper limit of the above range, the curable silicone composition as a whole can achieve good hot melt performance. In the above formula, the sum of f, g, h, and i, which are the sums of the respective siloxane units, is equal to 1.

[0213] Component (A2') is an organopolysiloxane resin having the above characteristics, and its handling properties are the same as those of the above-mentioned component (A1'). That is, component (A2') is a solid at room temperature (e.g., 25°C), and therefore, like component (A1'), in order to mix with component (B'), it is used in a dissolved state in the above-mentioned solvent or solvent mixture, and then the solvent is removed to prepare a curable silicone composition.

[0214] [Removal of volatile low molecular weight components from component (A')] In the production process of each of the components (A1') and (A2'), a volatile low molecular weight component is generated. Specifically, the volatile low molecular weight component has a structure of M4Q, and the M unit (R 3 3SiO 1 / 2 ) and Q units (SiO 4 / 2 ) is polymerized as a by-product. This structure has the effect of significantly lowering the hardness of the cured product obtained from the curable silicone composition of the present invention. The organopolysiloxane resins of components (A1') and (A2') are produced by polymerization reaction of raw material monomers in the presence of an organic solvent highly compatible with these, and a solid organopolysiloxane resin can be obtained by removing the organic solvent by drying under reduced pressure or the like, but the M4Q structure has high compatibility with the organopolysiloxane resin and is difficult to remove under drying conditions that remove the organic solvent. It has been known that the M4Q structure can be removed by exposing the organopolysiloxane resin containing it to a temperature of 200°C or higher for a short period of time, but if a curable silicone composition containing the M4Q structure is molded integrally with a substrate such as a semiconductor and then exposed to high temperatures to remove the M4Q structure, the volume of the cured product generated from the curable silicone composition will decrease and the hardness will increase significantly, which may cause the dimensions of the molded product to change and warp, etc. For this reason, in order to apply the curable silicone composition of the present invention to applications in which it is laminated to a substrate such as a semiconductor, it is preferable to remove the M4Q structure from the organopolysiloxane resin prior to the molding step in which the curable silicone composition is cured by laminating it to the substrate, or preferably prior to preparing the curable silicone composition while it is still in raw material form.

[0215] Methods for removing the M4Q structure from the organopolysiloxane resin include a method in which particulate organopolysiloxane resin is obtained in the organopolysiloxane resin production process, and then the particulate organopolysiloxane resin is dried in an oven or the like to remove the M4Q structure, or a method in which the M4Q structure is removed together with the organic solvent in a twin-screw kneader described below.

[0216] More specifically, component (A1') and component (A2') are produced in the presence of an organic solvent, and volatile components such as the M4Q structure appear as by-products during the production process. The volatile components can be removed by treating the obtained organopolysiloxane resin, which is the crude raw material, at a high temperature of about 200°C for a short period of time, so that it is possible to simultaneously remove the organic solvent and volatile components such as the M4Q structure from component (A1') and component (A2') using a twin-screw kneader set at a temperature of 200°C or higher. From the viewpoint of efficiently producing the curable hot-melt silicone composition of the present invention, it is preferable to carry out a process in which component (B'), which will be described later, is added to component (A2') dissolved in an organic solvent or a mixture of components (A1') and (A2') and mixed in a liquid state, and the mixture is fed into a twin-screw extruder set at 200°C or higher, and the volatile components such as the M4Q structure are removed together with the organic solvent. This method makes it possible to obtain a hot-melt mixture of components (A') and (B'), which can then be used in the step described below to knead with the remaining components that make up the curable silicone composition.

[0217] [Mass ratio of component (A1') to component (A2') in component (A')] In order to make the composition as a whole have hot melt properties, it is necessary to mix component (A2') or a mixture of components (A1') and (A2') with component (B') described later in a predetermined ratio, but the ratio of components (A1') and (A2') may be in the range of 0:100 to 90:10, preferably in the range of 0:100 to 85:25, more preferably 0:100 to 80:20, and particularly preferably 0:100 to 75:25. Component (A2') itself does not have a curing reactive functional group and therefore does not have curability, but in the composition, by using component (A2') in combination with component (A1'), it is possible to adjust to some extent the storage modulus, loss modulus, and tan δ calculated from the ratio of these of the cured product obtained by curing the curable composition, thereby making it possible to achieve suitable elastic modulus, flexibility, and stress relaxation properties of the cured product.

[0218] [Component (B')] Component (B') is one of the main components of the present curable silicone composition, and is a linear or branched organopolysiloxane that is liquid or plastic at 25°C and has a curable reactive functional group containing at least two carbon-carbon double bonds in the molecule. By mixing this type of curable reactive chain organopolysiloxane with the solid organopolysiloxane resin of component (A') described above, the composition as a whole can exhibit hot melt properties.

[0219] Component (B') is required to have a curing reactive functional group having a carbon-carbon double bond in the molecule. Such a curing reactive functional group has hydrosilylation reactivity and forms a cured product by a crosslinking reaction with other components. Such a curing reactive functional group is an alkenyl group similar to that of component (A1'), preferably an alkenyl group having 2 to 10 carbon atoms, and examples of the alkenyl group include vinyl, allyl, butenyl, pentenyl, and hexenyl, and particularly preferably a vinyl group or a hexenyl group.

[0220] Component (B') is a linear or branched organopolysiloxane that is liquid or plastic at 25°C (room temperature), and by mixing it with component (A') which is solid at room temperature, the composition as a whole can exhibit hot melt properties. The chemical structure of the organopolysiloxane of component (B') may be linear or may contain a small number of branched siloxane units (for example, the general formula: R 4 SiO 3 / 2 T units (R 4 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms) or SiO 4 / 2 The organopolysiloxane may be a branched organopolysiloxane having a Q unit represented by the formula: (B1') the following structural formula: R 4 3SiO(SiR 4 2O) k SiR 4 3 (In the formula, each R 4 are independently monovalent hydrocarbon groups having 1 to 10 carbon atoms, provided that R 4 at least two of the groups are alkenyl groups, and k is a number from 20 to 5,000. It is a linear diorganopolysiloxane represented by the formula: Preferably, it is a linear diorganopolysiloxane having an alkenyl group, particularly a vinyl group, at each of both ends of the molecular chain.

[0221] In the above formula, each R 4 are independently selected from the group consisting of monovalent hydrocarbon groups having 1 to 10 carbon atoms, for example, alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, and heptyl, particularly preferably methyl groups; alkenyl groups such as vinyl, allyl, butenyl, pentenyl, and hexenyl, particularly preferably vinyl and / or hexenyl groups; aryl groups such as phenyl, tolyl, and xylyl, particularly preferably phenyl groups; and aralkyl groups such as benzyl and phenethyl. Furthermore, R 4 At least two of R are alkenyl groups, preferably vinyl groups. 4is preferably a functional group selected from the group consisting of alkyl groups having 1 to 10 carbon atoms, such as a methyl group, and alkenyl groups, such as a vinyl group and a hexenyl group, and all R 4 At least two of the R 4 It is preferable that R is a methyl group. From the viewpoint of the technical effect of the invention, 4 Preferably, R is substantially free of aryl groups such as phenyl groups. If it contains a large amount of aryl groups such as phenyl groups, the coloration resistance of the cured product obtained from the curable silicone composition at high temperatures may deteriorate. Particularly preferably, R has an alkenyl group such as a vinyl group at each end of the molecular chain, and other R 4 is preferably a methyl group.

[0222] In the above formula, k is a number from 20 to 5,000, preferably from 30 to 3,000, and particularly preferably from 45 to 800. When k is equal to or greater than the lower limit of the above range, a curable silicone composition that is less sticky at room temperature can be obtained. On the other hand, when k is equal to or less than the upper limit of the above range, the curable silicone composition as a whole can achieve good hot melt performance.

[0223] Here, in order for the composition as a whole to exhibit hot melt properties, the amount of component (B') which is a linear or branched organopolysiloxane is in the range of 10 to 100 parts by mass, preferably in the range of 10 to 70 parts by mass, and more preferably in the range of 15 to 50 parts by mass, per 100 parts by mass of component (A') which is an organopolysiloxane resin. If the content of component (B') is within the above range, the resulting curable silicone composition will exhibit good hot melt properties, and the mechanical strength of the cured product obtained by curing the curable silicone composition can be increased, and the stickiness of the resulting curable silicone composition at room temperature can be reduced, thereby improving the handling and workability of the composition.

[0224] [Component (C')] Component (C') is an organohydrogenpolysiloxane having silicon-bonded hydrogen atoms that can be crosslinked in the presence of a hydrosilylation catalyst with the carbon-carbon double bonds contained in components (A') and (B') above, and specifically has the following average composition formula (1'): (R 4 3SiO 1 / 2 ) a (R 5 2SiO 2 / 2 ) b (R 5 SiO 3 / 2 ) c (SiO 4 / 2 ) d (R 2 O 1 / 2)e (1') (In the formula, R 4 are each independently a hydrogen atom or an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms and not containing an aliphatic unsaturated bond, R 5 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms that does not contain an aliphatic unsaturated bond, and all R 4 At least two of the a, b, c, and d are hydrogen atoms, and a, b, c, and d are numbers that satisfy the conditions: 0.01≦a≦0.6, 0≦b, 0≦c≦0.9, 0≦d≦0.9, and a+b+c+d=1 and c+d≧0.2. The organohydrogenpolysiloxane is characterized in that after exposure to 100° C. under atmospheric pressure for 1 hour, the mass loss rate compared to before exposure is 10% by mass or less.

[0225] In the above formula, each R 4 are the same or different, and each is a monovalent hydrocarbon group having 1 to 12 carbon atoms that does not have an aliphatic unsaturated carbon bond, or a hydrogen atom, provided that at least two, preferably at least three R 4 is a hydrogen atom. R other than a hydrogen atom 4The monovalent hydrocarbon radicals R are, for example, radicals selected from the group consisting of alkyl radicals, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, and heptyl, in particular methyl radicals; aryl radicals, such as phenyl, tolyl, and xylyl, in particular phenyl radicals; and aralkyl radicals, such as benzyl and phenethyl. 4 Preferably, the monovalent hydrocarbon groups represented by are independently a methyl group or a phenyl group.

[0226] In the formula, R 5 is a monovalent hydrocarbon group having 1 to 12 carbon atoms that does not have an aliphatic unsaturated carbon bond, and 4 Examples of the monovalent hydrocarbon group include the same groups as those of R 5 is preferably a group selected from a methyl group and a phenyl group.

[0227] In the formula, a, b, c, and d are numbers that satisfy the following conditions: 0.01≦a≦0.6, 0≦b, 0≦c≦0.9, 0≦d≦0.9, and a+b+c+d=1 and c+d≧0.2. H MT resin, M H T resin, M H MTQ resin, M H MQ resin, M H DQ resin and M H In the above resin notation, M, D, T, and Q represent M units, D units, T units, and Q units, respectively, and MH represents M units having a hydrogen atom.

[0228] In the above formula (1'), R 2 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 2 Examples of the alkyl group of R include methyl, ethyl, propyl, butyl, pentyl, and hexyl. 2 Group R containing 2 O 1 / 2 corresponds to the hydroxyl group or alkoxy group contained in the organohydrogenpolysiloxane of component (C').

[0229] In the above formula (1'), e represents the general formula: R 2 O1 / 2 is a number indicating the proportion of units, and the unit means a hydroxyl group or an alkoxy group bonded to a silicon atom that may be contained in the organopolysiloxane resin. e satisfies 0≦j≦0.05, and preferably 0≦j≦0.03. As described above, in the above formula (1'), the sum of a, b, c, and d, which are the sums of the respective siloxane units, is equal to 1.

[0230] The silicon-bonded hydrogen atom (SiH) of component (C') must be present in the M unit, because the SiH group present in the M unit has high hydrosilylation reactivity. If the SiH group is present in a unit other than the M unit, such as D or T unit, its hydrosilylation reactivity is extremely reduced, and if a curing inhibitor is present, the hydrosilylation reaction does not proceed or the reaction is extremely slow. Furthermore, by making the organohydrogenpolysiloxane into a branched structure containing T or Q units rather than a linear structure, the number of SiH groups in one molecule increases, and the hydrosilylation reactivity of the entire molecule is further increased. By using such an organohydrogenpolysiloxane with high reactivity, a curing system that is resistant to curing inhibition can be constructed.

[0231] On the other hand, it is known that crosslinking agents containing a relatively large number of M units having SiH groups produce a relatively large amount of low molecular weight active ingredients during the production process, and when such a crosslinking agent is added and the melt kneading process under degassing described below is carried out, the active ingredients volatilize, which can cause the problem that the curable silicone composition does not achieve the designed properties. In order to avoid this, the present invention requires the use of an organohydrogenpolysiloxane that has a mass loss rate of 10% by mass or less after exposure to 100°C under atmospheric pressure for 1 hour compared to before exposure. The specific molecular structure of the organohydrogenpolysiloxane of component (C') is M H Q Resin M H By changing the ratio of units to Q units, H Reduce the units, M H Q resin with D units. HA relatively large functional group such as a phenyl group may be introduced as the functional group of the T unit of the T resin. H T Ph (T Ph represents a phenyl group-substituted T unit), is compatible with other components in the composition of the present invention and will not separate from the composition, so long as its molecular weight is not too high.

[0232] Component (C') is preferably an organohydrogenpolysiloxane represented by the following average composition formula (2'). (HR 6 2SiO 1 / 2 ) e (R 6 2SiO 2 / 2 ) f (SiO 4 / 2 ) g (2') In formula (2'), R 6 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms and containing no aliphatic unsaturated bonds, and e, f, and g are numbers that satisfy the conditions 0.01≦e≦0.6, 0≦f≦0.9, 0.2≦g≦0.9, and e+f+g=1. Specific examples of the monovalent hydrocarbon group are as follows: 4 The monovalent hydrocarbon group represented by R is the same as that represented by R. 6 are preferably each independently a group selected from a methyl group and a phenyl group.

[0233] Furthermore, component (C') is preferably an organohydrogenpolysiloxane represented by the following average formula (3'). (HR 7 2SiO 1 / 2 ) h (R 7 2SiO 2 / 2 ) i (R 8 SiO 3 / 2 ) j (3') In formula (3'), R 7 and R 8are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms that does not contain an aliphatic unsaturated bond, and all R 8 At least 10 mol % of these are aryl groups, and h, i, and j are numbers that satisfy the conditions 0.01≦h≦0.6, 0≦i≦0.9, 0.2≦j≦0.9, and h+i+j=1. Specific examples of the monovalent hydrocarbon group are as follows: 4 The monovalent hydrocarbon group represented by R is the same as that represented by R. 8 is for all R 8 are preferably each independently selected from methyl and phenyl groups, provided that at least 10 mol % of these are phenyl groups.

[0234] The organohydrogenpolysiloxane represented by the average composition formula (2') and the organohydrogenpolysiloxane represented by the average composition formula (3') may be used alone or in combination.

[0235] The content of the organohydrogenpolysiloxane of component (C') in the curable silicone composition of the present invention is an amount sufficient to cure the curable silicone composition, and it is preferable that the number of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane of component (C') is such that, relative to the curing reactive functional groups containing carbon-carbon double bonds (for example, alkenyl groups such as vinyl groups) in components (A') and (B'), the number of silicon-bonded hydrogen atoms per alkenyl group relative to the silicon-bonded alkenyl groups contained in the entire curable silicone composition is 0.5 to 20.0, and particularly 1.0 to 10.

[0236] [Component (D')] Component (D') is a hydrosilylation catalyst for crosslinking the hydrosilylation reactive carbon-carbon double bonds contained in components (A') and (B') with the silicon-bonded hydrogen atoms, i.e., Si-H groups, contained in component (C') by hydrosilylation reaction to cure the curable silicone composition of the present invention. As the hydrosilylation catalyst of component (D'), compounds or metals having hydrosilylation catalytic action known in the art can be used, and examples include platinum-based catalysts, rhodium-based catalysts, and palladium-based catalysts, with platinum-based catalysts being preferred because they can significantly accelerate the curing of the composition. Examples of this platinum-based catalyst include platinum fine powder, chloroplatinic acid, alcohol solutions of chloroplatinic acid, platinum-alkenylsiloxane complexes, platinum-olefin complexes, platinum-carbonyl complexes, and catalysts in which these platinum-based catalysts are dispersed or encapsulated in thermoplastic resins such as silicone resins, polycarbonate resins, and acrylic resins, with platinum-alkenylsiloxane complexes being particularly preferred. Examples of this alkenylsiloxane include 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, alkenylsiloxanes in which a portion of the methyl groups of these alkenylsiloxanes have been substituted with ethyl groups, phenyl groups, etc., and alkenylsiloxanes in which the vinyl groups of these alkenylsiloxanes have been substituted with allyl groups, hexenyl groups, etc. In particular, because this platinum-alkenylsiloxane complex has good stability, it is preferable to use 1,3-divinyl-1,1,3,3-tetramethyldisiloxane as the hydrosilylation reaction catalyst, and it is preferable to add the complex in the form of an alkenylsiloxane solution to the other components that make up the curable silicone composition. In addition, from the standpoint of improving the handling of the platinum catalyst and the pot life of the curable silicone composition, a platinum-containing hydrosilylation reaction catalyst in the form of fine particles dispersed or encapsulated in a thermoplastic resin may be used. Note that non-platinum metal catalysts such as iron, ruthenium, and iron / cobalt may also be used as catalysts that promote the hydrosilylation reaction.

[0237] The amount of hydrosilylation catalyst, component (D'), added is not particularly limited as long as it is an amount that allows curing within the target time under the conditions for curing the curable silicone composition of the present invention. In general, when the hydrosilylation catalyst is a metal compound such as platinum, it is preferably an amount in which the metal atom is within the range of 0.01 to 100 ppm, 0.01 to 50 ppm, or 0.01 to 10 ppm by mass relative to the entire composition.

[0238] [Component (E')] In addition to the above components (A') to (D'), the curable silicone composition of the present invention may also optionally contain a cure retarder (E').

[0239] Although there are no particular limitations on the structure of the cure retarder, it is preferable that the boiling point be 200° C. or higher under atmospheric pressure, particularly at 1 atmospheric pressure. This is because if a compound with a low boiling point is used as a delayed curing agent when melting and kneading the raw materials under reduced pressure in the production process of the curable silicone composition sheet described below, part or all of the cure retarder will volatilize during the melting and kneading process, and there is a risk that the targeted cure retardation effect for the curable silicone composition will not be obtained.

[0240] The curable curing retarder used in the composition of the present invention is not particularly limited, but examples thereof include alkyne alcohols such as 2-methyl-3-butyn-2-ol, 3,5-dimethyl-1-hexyn-3-ol, 2-phenyl-3-butyn-2-ol, and 1-ethynyl-1-cyclohexanol; enyne compounds such as 3-methyl-3-penten-1-yne and 3,5-dimethyl-3-hexen-1-yne; alkenyl-containing low molecular weight siloxanes such as tetramethyltetravinylcyclotetrasiloxane and tetramethyltetrahexenylcyclotetrasiloxane; and alkynyloxysilanes such as methyl-tris(1,1-dimethylpropynyloxy)silane and vinyl-tris(1,1-dimethylpropynyloxy)silane. Of these, it is particularly preferable to use a compound having a boiling point of 200° C. or more under atmospheric pressure. The content of the curing retarder in the curable silicone composition is not particularly limited, but it is preferably within the range of 1 to 10,000 ppm by mass with respect to the composition.

[0241] [Other additives] In addition to the components described above, materials known in the art as additives that may be used in silicone compositions may be added to the curable silicone composition of the present invention. Examples of additives that can be used include, but are not limited to, those described above.

[0242] [Curable hot melt silicone composition sheet or film] In the present invention, when producing the laminate of the present invention, a curable hot melt silicone composition is applied onto a substrate to form a layer of the composition on the substrate. The method of providing the curable hot melt silicone composition on the substrate can be any method known as a method for applying a hot melt composition onto a substrate, and examples of such methods include compression molding, press molding, and vacuum lamination. It is preferable to produce the laminate of the present invention using any of these methods. However, the most preferred method is a method in which the curable hot melt silicone composition is formed into a sheet or film in advance, laminated onto a substrate or interposed between two substrates, heated to melt the sheet or film, and press-bond the substrate to the molten silicone composition to produce a laminate. In the following, a sheet or film made of the curable hot melt silicone composition of the present invention (as described above, in this specification, this is referred to as a "sealing sheet" whether it is used as a sealant or an adhesive) will be described. The component constituting the sealing sheet is a curable hot melt silicone composition having the above-mentioned thermal melting properties. The curable hot-melt silicone composition constituting the above-mentioned encapsulating sheet may have a melt viscosity at 100°C (at the ultimate shear rate) of 5000 Pa·s or less, measured at a pressure of 2.5 MPa using a flow tester. In addition, in the JIS Packaging Terminology Standards, a material with a thickness of less than 250 μm is called a film, and a material with a thickness of 250 μm or more is called a sheet, and although the terms sheet and film are used in this specification, these are collectively referred to as "sheet." Therefore, even when simply referring to a "sheet" in this specification, the thickness includes not only those with a thickness of 250 μm or more, but also those with a thickness of less than 250 μm.

[0243] In one embodiment of the present invention, the curable hot-melt silicone composition layer contained in the laminate may be one layer, or may have a multi-layer structure in which two or more layers are combined. When two or more curable hot-melt silicone composition layers are combined, curable hot-melt silicone composition layers with different compositions and properties are used for each layer. For example, a layer made of a composition with a lower melt viscosity is provided on the surface adhering to the first substrate, and a layer made of a composition with a higher melt viscosity is provided on the surface opposite to the first substrate, or a layer made of a composition with a high adhesive strength after curing is provided on the surface adhering to the first substrate, and a layer made of a composition with a lower surface tack after curing is provided on the surface opposite to the first substrate. However, the composition and physical properties of the two or more curable hot-melt compositions used when providing a curable hot-melt silicone composition layer in which two or more layers are combined can be set arbitrarily, and are not limited to a specific combination. In one preferred embodiment of the present invention, the curable hot-melt silicone composition layer contained in the laminate is a single layer made of one type of curable hot-melt silicone composition.

[0244] The method for producing the laminate having two or more layers of the curable hot-melt composition described above can be a method of stacking two or more layers of the curable hot-melt silicone composition one by one in order, and for this purpose, in any of the known methods such as compression molding, press molding, vacuum lamination, etc., a method can be used in which the first layer of the curable hot-melt silicone composition is stacked on the substrate, and then the second layer of the curable hot-melt silicone composition is stacked on top of that. The same applies to three or more layers.

[0245] [Curable hot melt silicone composition encapsulating sheet] The encapsulating sheet is used to encapsulate a substrate to be encapsulated, such as a substrate for an electronic device, to form a curable hot-melt silicone composition layer constituting the laminate of the present invention, or can be used to bond two substrates, particularly substrates, of the same or different types using a curable hot-melt silicone composition as an adhesive to form a laminate, and is a curable hot-melt silicone composition processed into a sheet or film. The encapsulating sheet may be used alone or in combination of two or more sheets. When two or more encapsulating sheets are used, two or more sheets of the same type may be used, or different types of encapsulating sheets may be combined. When combining two or more encapsulating sheets, it is generally preferable to combine the sheets so that they overlap. Before use, the encapsulating sheet may be laminated on a release film or interposed between two release films, and when the encapsulating sheet is interposed between two release films, the encapsulating sheet is usually used after peeling off at least one release film when used. The encapsulating sheet of the present invention is a sheet of a hot-melt curable silicone composition, and is characterized in that its melt viscosity (at the limiting shear rate) measured at 100°C with a flow tester at a pressure of 2.5 MPa is 5000 Pa·s or less. This is because, if the encapsulating sheet does not melt sufficiently when the encapsulating sheet is thermocompressed to a substrate under reduced pressure as described below, it is difficult to form a flat encapsulating layer on the substrate that is free of voids, i.e., free of bubbles. By using an encapsulating sheet prepared from a curable hot-melt silicone composition having a melt viscosity of 5000 Pa·s or less at 100°C, a flat silicone encapsulating layer free of voids can be formed on the substrate.

[0246] [Method for producing curable hot melt silicone composition sheet (encapsulating sheet)] To produce the laminate of the present invention, it is preferable to use a curable hot-melt silicone composition sheet (also referred to as an "encapsulating sheet" in this specification). The encapsulating sheet can be produced by any method known in the art, and is not limited to any particular method.

[0247] The curable hot-melt silicone composition sheet according to the present invention may be produced using organopolysiloxane resin fine particles as a raw material (Method A), or may be produced by dispersing an organopolysiloxane resin that is solid at room temperature, and optionally a chain diorganopolysiloxane, in an organic solvent, and then using the hot-melt solid content remaining after removing the organic solvent as a raw material (hot bulk method) (Method B). Specifically, the former (Method A) comprises the following steps: Step 1: mixing organopolysiloxane resin microparticles, a curing agent, and optionally a functional filler; Step 2: kneading the mixture obtained in step 1 while heating and melting it at a temperature of 120°C or less; Step 3: Laminating the heated, melted and kneaded mixture obtained in step 2 between two films, each having at least one release surface, to form a laminate; Step 4: stretching the mixture in the laminate obtained in step 3 between rolls to form a curable hot-melt silicone sheet having a specific thickness; The manufacturing method includes:

[0248] On the other hand, the latter (Method B) comprises the following steps: Step 1: A step of obtaining a hot-melt solid content by removing the organic solvent at a temperature of 150° C. or higher from a solution in which an organopolysiloxane resin that is solid at room temperature and, optionally, a linear diorganopolysiloxane are dispersed or dissolved in an organic solvent; Step 2: adding all the curing agents to the hot-melt solid obtained in step 1, and then kneading the mixture while heating and melting it at a temperature of 120°C or less; Step 3: Laminating the mixture obtained in step 2 after heating, melting and kneading between two films, each of which has at least one release surface; Step 4: A step of stretching the mixture in the laminate obtained in step 3 between rolls to form a curable hot melt silicone sheet having a specific thickness. The manufacturing method includes:

[0249] In either manufacturing method (Method A or Method B), steps 3 and 4 may be continuous and integrated steps, for example, the mixture obtained after heating and melting in step 2 may be laminated by being discharged or applied between films having at least one release surface directly below the rolls, and at the same time, the gap between the rolls may be adjusted to stretch the film to a specific thickness. In this way, a manufacturing method having a substantially integrated process of steps 3 and 4 is also included in the scope of the above manufacturing method. That is, steps 3 and 4 may be performed continuously and integrally by discharging or applying the mixture obtained in step 2 between two release films to sandwich the mixture between the two release films, for example, between two long release films, and passing the resulting laminate consisting of the two release films and the mixture sandwiched between them between rolls to stretch and mold the mixture between the release films and adjust the thickness to a predetermined value to obtain the desired laminate. Such a method of performing steps 3 and 4 integrally is also included in the above-mentioned production method.

[0250] In step 3 of the above-mentioned method A or method B, the step of laminating the mixture after heat melting between films is not particularly limited, and may be a step of (i) discharging or applying the mixture after heat melting from step 2 onto a first release film having a release surface, and then contacting the second release film with the surface of the mixture opposite to the surface contacting the first release film to interpose the mixture after heat melting between the first release film and the second release film, i.e., sandwiching the mixture, or (ii) discharging or applying the mixture after heat melting from step 2 between the first release film and the second release film having a release surface to interpose the mixture after heat melting between both release films. (ii) can be exemplified by a method in which the first and second release films are brought close to each other by an appropriate means, such as two rolls, and the mixture from step 2 is discharged or applied at the location where the two release films are close to each other, and the mixture is simultaneously or almost simultaneously sandwiched between the gap between the two release films. It is particularly preferable that the above-mentioned steps 3 and 4 are continuous steps.

[0251] Regarding these manufacturing methods, the applicants have proposed the entire process, including the manufacturing method and manufacturing apparatus used therefor, for curable silicone sheets in Japan Patent Application No. 2019-167832, Japan Patent Application No. 2019-167833, and their priority applications. In the present invention, these methods and manufacturing apparatus can be applied when forming the curable hot-melt silicone composition into a sheet or film.

[0252] More specifically, an example of a method for producing an encapsulating sheet will be described below using as an example a curable hot-melt silicone composition prepared using the above-mentioned components (A'), (B'), (C'), and (D') as essential components, and optionally using component (E'). However, an encapsulating sheet can be produced using any of the above-described curable hot-melt silicone compositions in accordance with the method described below. As described above, the encapsulating sheet according to the present invention has hot melt properties. A preferred example of the curable hot melt silicone composition used in the present invention is one that contains the above-mentioned components (A'), (B'), (C'), and (D') as essential components. In one embodiment, the method for producing the encapsulating sheet of the present invention includes the following steps 1 to 4. Step 1: mixing the components of the curable hot melt silicone composition, preferably at a temperature of 50° C. or higher; Step 2: kneading the mixture obtained in step 1 while heating and melting it; Step 3: forming a laminate by laminating the heat-melted mixture obtained in step 2 between two release films having at least one release surface such that the mixture is in contact with the release surface; and Step 4: The laminate obtained in step 3 is pressed between rolls to form a curable hot-melt silicone composition sheet having a specific thickness.

[0253] The curable hot-melt silicone composition used in the present invention and the composition formed into a certain shape, such as pellets, sheets, and films, have hot-melt properties. Here, "having hot-melt properties" means that the softening point of the material is within the range of 50°C to 200°C, and the material can be softened and changed in shape by heating, or can become flowable by heating. In addition, the encapsulating sheet according to the present invention does not have hot-melt properties by itself, as the organopolysiloxane resin component (A') that is a component of the encapsulating sheet, but shows hot-melt properties by combining it with components (B') and (C').

[0254] Each step of the above-mentioned method for producing the encapsulating sheet will be described in more detail below. [Process 1] The above step 1 is a step of producing a curable hot-melt silicone composition, preferably a composition in the form of granules or powder, by mixing the components of the curable hot-melt silicone composition, that is, an organopolysiloxane resin (component A', preferably in the form of fine particles), an organopolysiloxane that is liquid or plastic at 25°C (component B'), an organohydrogenpolysiloxane as a curing agent (component C'), and a hydrosilylation catalyst (component D'), and further, if desired, further additives (for example, component E'). Each of these components has been described above.

[0255] The mixture obtained by step 1, preferably a granular mixture, is a granular curable hot-melt silicone composition, and the composition as a whole has hot-melt properties. Meanwhile, the mixture is non-flowable at 25°C. Here, non-flowable means that it does not substantially deform and / or flow in the absence of external force, and preferably, when the granular composition obtained in step 1 is further molded into pellets or tablets, it does not substantially deform and / or flow at 25°C and in the absence of external force. Such non-flowable can be evaluated, for example, by placing the molded composition on a hot plate at 25°C, and not substantially deforming and / or flowing even when the composition is not subjected to external force or a certain load. When the composition is non-flowable at 25°C, the shape retention of the composition at that temperature is good, and the surface adhesion is low, so that the composition can be easily handled even in an uncured state.

[0256] The softening point of the mixture obtained in step 1 is not more than 200° C., and preferably not more than 150° C. Such a softening point means the temperature at which, when a composition having a height of 22 mm is pressed from above on a hot plate with a load of 100 grams for 10 seconds and the load is removed, the composition is deformed by 1 mm or more in the height direction.

[0257] In step 2, which will be described later, the mixture obtained in step 1 is heated to a temperature equal to or higher than the softening point of the mixture, thereby softening or melting the mixture and imparting a certain degree of fluidity to the mixture. By molding the softened or molten product, it is possible to produce an encapsulating sheet having hot-melt properties from, for example, the granular curable hot-melt silicone composition obtained in step 1.

[0258] The step of mixing the components (A') to (D') of the present invention and other optional components, such as component (E'), is not particularly limited, but can be carried out by powder mixing at a temperature lower than the softening point of the entire mixture obtained, preferably the softening point of component (A'). The powder mixer used in this production method is not particularly limited, and examples thereof include a single-screw or double-screw continuous mixer, a double roll, a Ross mixer, a Hobart mixer, a dental mixer, a planetary mixer, a kneader mixer, a lab miller, a small grinder, and a Henschel mixer, with the lab miller, small grinder, and Henschel mixer being preferred.

[0259] [Process 2] Step 2 is a step of kneading the mixture having heat meltability obtained in step 1 while heating and melting it. By heating and kneading the mixture having heat meltability at a temperature equal to or higher than its softening point, preferably at a temperature range of 50°C to 200°C, the entire composition is melted or softened and mixed, so that the components contained in the mixture can be mixed uniformly. When the mixture obtained in step 2 is pressure-molded into a sheet shape using a pressure device, for example, a two-roll press, in step 4, a thin-layered sheet having a uniform thickness can be formed by one pressurization, and there is a practical benefit in that the occurrence of molding defects and cracks in the sheet itself can be avoided. On the other hand, if the temperature at which the mixture is heated is less than the lower limit, the mixture is not softened sufficiently, and it may be difficult to obtain a molten or softened mixture in which each component is uniformly mixed throughout, even when mechanical force is used. When such a mixture in which the components are not uniformly mixed is pressure-molded into a sheet shape in step 4 through step 3, a thin-layered molded sheet having a uniform thickness cannot be formed, and breakage and / or cracks may occur in the sheet. Conversely, if the temperature at which the mixture is heated exceeds the upper limit, a hydrosilylation reaction occurs during mixing, and the entire mixture may significantly thicken or harden, losing hot melt properties, or forming a hardened product, which is not preferred. For this reason, the hydrosilylation catalyst of component (D') may not be mixed with other components from the beginning in step 1, but may be added after the mixture of other components is sufficiently mixed in step 2, and when component (D') is added, the temperature may be lowered within the range in which kneading is possible, and such a method is preferred. Alternatively, the hydrosilylation catalyst of component (D') may be dispersed in a thermoplastic resin or encapsulated in a thermoplastic resin in the form of fine particles, and such a method is preferred.

[0260] When the mixture obtained in step 1 has a low heat melt viscosity and is highly fluid, the mixture can be preliminarily molded in advance in step 3 described below, and then the mixture preliminarily molded into a shape similar to a sheet, for example, can be laminated on a release film. Specifically, if the melt viscosity of the mixture obtained by heating, melting, and kneading in step 2 is in the range of 1 to 1,000 Pa s at 150°C, as measured at a pressure of 2.5 MPa using a high-speed flow tester, the mixture can be preliminarily molded before being laminated on a release film in step 3.

[0261] On the other hand, if the mixture obtained in step 1 has a high heat melt viscosity and has poor fluidity even when melted, in step 2, the mixture obtained in step 1 may be melt-kneaded at a temperature equal to or higher than its softening point to form a homogeneous composition, and then, in step 3, the mixture may be laminated directly onto a release film without being pre-molded.

[0262] The kneading device used in step 2 is not limited, and may be a batch type kneader, Banbury mixer, Henschel mixer, planetary mixer, 2-roll mill, 3-roll mill, Ross mixer, Labo Plastomill, etc., equipped with heating and cooling functions, or a continuous type heating and kneading device, such as a single screw extruder or a twin screw extruder, equipped with heating and cooling functions, and may be selected according to the working efficiency in terms of processing time and the control ability of shear heat generation. From the viewpoint of shortening the processing time, a continuous type heating and kneading device, such as a single screw extruder or a twin screw extruder, may be used, or a batch type mixer, such as a Labo Plastomill, but a continuous type heating and kneading device, such as a single screw extruder or a twin screw extruder, is preferably used because of its good working efficiency.

[0263] [Process 3] Step 3 is a step in which the heat-melted mixture obtained in step 2 is sandwiched between two films each having at least one release surface and laminated together, and is a preliminary step for further pressure molding of this laminate in step 4. By forming a laminate in which the mixture obtained in step 2 is sandwiched between release films, pressure molding can be performed from above the release film using a roll to obtain a sheet-like molded product made of the curable silicone composition. Furthermore, after molding of the laminate, the properties of the release surface of the release sheet can be used to remove only the release film from the laminate containing the curable silicone composition sheet.

[0264] The mixture obtained in step 2 after heat melting is interposed between two release films to form a laminate. Depending on the form of use of the obtained curable silicone composition sheet (including film), it is preferable that both of the two release films have a release surface, and in step 3, it is particularly preferable to arrange the mixture obtained in step 2 between two release films so that it contacts the release surface of each release film to form a laminate. By having such a configuration of the laminate, a laminate (also called a laminate sheet) in which a thin layer of the curable silicone composition sheet is interposed between the release films and the release film can be peeled off from both sides of the curable silicone composition sheet can be obtained by pressure molding the curable silicone composition interposed between the release sheets in step 4, and further cutting the laminate as desired. Therefore, when using a curable silicone composition sheet, it is possible to peel off one of the release films arranged on both sides of the curable silicone resin sheet to expose the curable silicone resin sheet surface, or peel off both release films to expose only the curable silicone resin sheet, and use it without worrying about damaging the formed curable silicone resin sheet.

[0265] The substrate of the release film used in step 3 is not particularly limited, and examples thereof include paperboard, cardboard paper, clay-coated paper, polyolefin-laminated paper, particularly polyethylene-laminated paper, synthetic resin film / sheet, natural fiber cloth, synthetic fiber cloth, artificial leather cloth, and metal foil. In particular, synthetic resin films or sheets are preferred, and examples of synthetic resins include polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polycarbonate, polyethylene terephthalate, and nylon. In particular, when heat resistance is required, films of heat-resistant synthetic resins such as polyimide, polyether ether ketone, polyethylene naphthalate (PEN), liquid crystal polyarylate, polyamide imide, and polyether sulfone are preferred. On the other hand, in applications requiring visibility such as display devices, transparent substrates, specifically transparent materials such as polypropylene, polystyrene, polyvinylidene chloride, polycarbonate, polyethylene terephthalate, and PEN are preferred. As described above, the substrate can be made of paperboard, and the like, and the term release film is not particularly limited in terms of thickness.

[0266] As mentioned above, the thickness of the release film is not particularly limited, but is usually about 5 to 300 μm.

[0267] The release film has at least one release layer on its surface, and the release film is preferably used in step 3 so that the release layer comes into contact with the mixture obtained in step 2. This allows the curable hot-melt silicone composition sheet obtained by pressure molding through steps 3 and 4 to be easily peeled off from the release film. The release layer may also be called a release liner, separator, release layer, or release coating layer, and may be a release layer formed using a material having release coating ability, such as a silicone-based release agent, a fluorine-based release agent, an alkyd-based release agent, or a fluorosilicone-based release agent. Alternatively, the release film may be easily peeled off from the sealing sheet, i.e., the curable hot-melt silicone composition sheet, by physically forming fine irregularities on the surface of the substrate film, or by using a substrate that is difficult to adhere to the curable hot-melt silicone composition sheet of the present invention as the material of the substrate film.

[0268] In step 3, the mixture obtained in step 2 is sandwiched between two release films to form a laminate. The step is not particularly limited, but the mixture obtained in step 2 is supplied onto the release layer of one release film by being discharged or applied, the mixture is placed on the release layer, and the release layer of another release film is then attached to the mixture from above to form a laminate. In order to continuously manufacture curable silicone composition sheets by continuously performing the steps of placing the mixture on one release sheet and then stacking another release sheet on top of the mixture, each release film is transported via a rotating roll to a supply position for the mixture obtained from step 2, the mixture is supplied between the two release films, and the two release films and the mixture are laminated to form a laminate structure of release film / mixture (i.e., curable silicone composition) / release film.

[0269] In the above-mentioned continuous method, the amount of the mixture obtained in step 2 fed between the release films in step 3 can be designed according to the production speed and production scale of the laminate. As an example, the mixture obtained in step 2 can be fed between the release films at a feed rate of 1 to 10 kg / hour, but it goes without saying that this is not limited to this. However, in step 3, the amount or speed of the mixture fed when the mixture obtained in step 2 is interposed between the release films to form a laminate must be determined according to the average thickness of the curable silicone composition sheet designed in step 4, and the amount or speed of the mixture fed in step 4 must be within a range that allows the laminate obtained in step 3 to be further compressed to process the curable silicone composition sheet to a desired thickness.

[0270] When the mixture obtained in step 1 has a low heat melt viscosity and the melt has high fluidity, it is preferable to extrude the heat melted mixture obtained in step 2 onto one release film while forming it into a film using a die, and then overlay another release film on the extruded mixture to form a laminate in step 3. Here, the die is used to provisionally mold the mixture, and the type and thickness of the mixture during provisional molding are not particularly limited, but it is possible and preferable to use a T-shaped die to provisionally mold the mixture into a roughly sheet-like shape having a thickness in the range of 100 to 2000 μm (= 2 mm).

[0271] When the mixture obtained in step 1 has a low heat melt viscosity and the melt has a high fluidity, it is preferable to include a step of cooling or temperature adjustment of the entire laminate obtained in step 3 after the above-mentioned provisional molding, either as a step prior to step 4 or in step 4. This is because the heat melt is cooled to a high viscosity state or solid state to effectively perform the pressure molding in step 4. The cooling step is not particularly limited, but can be performed by cooling the mixture supplied or laminated on the film by a cooling roll or the like to a range of −50° C. to room temperature using a cooling means such as air cooling or a cooling solvent. Details of the temperature adjustment will be described in step 4.

[0272] On the other hand, if the mixture obtained in step 1 has a high heat melt viscosity and poor fluidity, in step 3, the mixture having poor fluidity, for example a semi-solid mixture, may be supplied onto a film without performing pre-molding, and laminated with a release film.

[0273] [Step 4] Step 4 is a step in which the laminate obtained in step 3 above is pressed between rolls to form a curable silicone composition sheet having a specific thickness, and a step in which the mixture obtained in step 2 is pressed and stretched from above the release film of the laminate obtained in step 3 to form an encapsulating sheet having a substantially uniform thickness.

[0274] In step 4, the pressure stretching of the encapsulating sheet sandwiched between the release films can be performed on the laminate obtained in step 3 using a known rolling method such as roll rolling. In particular, in the case of roll rolling, there is an advantage that an encapsulating sheet of a desired thickness can be designed by adjusting the gap between the rolls. For example, by pressing the laminate while adjusting the gap between the rolls to a constant value so that the average thickness is in the range of 10 to 2000 μm, an encapsulating sheet having excellent flatness and extremely few defects, such as voids, on the sheet surface and inside the sheet can be obtained. More specifically, in the case of roll rolling, it is particularly preferable that the gap between the rolls is adjusted to a range of 1.5 to 4.0 times the average thickness of the targeted encapsulating sheet.

[0275] In step 4, the laminate is pressed and the encapsulating sheet in the laminate, i.e., the curable hot-melt silicone composition sheet, is stretched to obtain a substantially flat encapsulating sheet having a thickness of 10 to 2000 μm. In step 3, the mixture after heating and melting in step 2 is roll-stretched in a form in which it is sandwiched between release films, to obtain a peelable laminate that includes an encapsulating sheet having hot-melt properties, which has low defects and is easy to peel from the release sheet, and has excellent handling properties due to being easily peelable from the release sheet, and from which the release film can be easily peeled.

[0276] [Temperature adjustment in step 4] In step 4, when the laminate obtained in step 3 is pressed between rolls to stretch the curable hot-melt silicone composition sheet, i.e., the encapsulating sheet, it is preferable that the rolls further have a temperature control function, and adjust the temperature of the entire laminate during roll rolling, and heat or cool it as necessary. This temperature control has the practical benefit of stably maintaining the gap between the rolls and improving the flatness and uniformity (uniformity of film thickness) of the encapsulating sheet obtained. The specific range of temperature control can be appropriately designed depending on the heat resistance of the release film used, the thickness (design thickness) of the encapsulating sheet, the reactivity of the curable hot-melt silicone composition that is a component of the encapsulating sheet, etc., but is generally within the range of 5 to 150 ° C.

[0277] [Cutting process] Step 4 can provide a peelable laminate in which a sealing sheet is interposed between release films. The laminate manufacturing method of the present invention may further include a step of cutting the laminate including the sealing sheet, if desired. In addition to or in place of the cutting step, the sealing sheet may include a step of winding the laminate into, for example, a roll using a winding device. This allows a desired size of sealing sheet, i.e., a peelable laminate including a curable hot-melt silicone composition sheet, to be obtained.

[0278] [Laminate] The laminate obtained by the above steps is a laminate having a structure in which a substantially flat sealing sheet made of a curable hot-melt silicone composition having a thickness of 10 to 2000 μm, which contains the above-mentioned components (A') to (D') as essential components and optionally component (E') as an optional component, is laminated between two release films having at least one release surface. It is preferable that both of the films have a surface structure that enhances the release surface or a release surface that has been surface-treated.

[0279] It is preferable that the encapsulating sheet having a release film on one or both sides thereof obtained as described above is used to produce the above-mentioned substrates, for example, substrates for electronic devices, such as electronic circuit boards and electronic circuit mounting boards, and a laminate comprising a curable hot-melt silicone composition layer laminated thereon, or a laminate comprising a substrate and a cured silicone composition layer laminated thereon.

[0280] When producing a sealing film having a curable hot-melt silicone composition layer having two or more layers consisting of two or more curable hot-melt silicone composition layers each having a different composition sandwiched between two release films, a method of carrying out steps 3 and 4 described above can be exemplified by, but is not limited to, discharging or applying a first curable hot-melt silicone composition that has been heated and melted onto one release film, optionally cooling the composition in some cases, and then discharging or applying a second curable hot-melt silicone composition onto the layer of composition, and then overlaying another release film on top of that.

[0281] It is preferable to use the encapsulating sheet obtained as described above, having a release film on one or both sides thereof, for producing a laminate of the present invention comprising the above-mentioned substrate, such as a substrate for an electronic device, for example an electronic circuit board or an electronic circuit mounting board, and a curable hot-melt silicone composition layer laminated thereon, or a laminate of the present invention comprising a substrate and a cured silicone composition layer laminated thereon.

[0282] In the above explanation of the method for producing the encapsulating sheet, an example was given in which a curable hot-melt silicone composition containing components (A') to (D') and optionally component (E') was used, but the curable hot-melt silicone composition used when producing the encapsulating sheet may be any of the curable hot-melt silicone compositions explained above.

[0283] [Characteristics of the curable hot-melt silicone composition and the layer made of said composition] [High temperature viscosity characteristics of the composition (thixotropy)] The curable hot-melt silicone composition used in the present invention has hot-melt properties, is fluid at temperatures of 100°C or higher, and allows for the measurement of viscosity. The viscosity is also strongly dependent on the shear applied during measurement, with the composition being thixotropic, meaning that the viscosity is high at low shear and low at high shear. Specifically, the curable hot-melt silicone composition used in the present invention has a shear rate of 1s at 100°C and 150°C when measured with a rheometer. -1 The viscosities at 100°C and 150°C are 5000 Pa·s or less and 1000 Pa·s or less, respectively, and when measured at a pressure of 2.5 MPa using a flow tester considered to be the limit shear rate, the viscosities at 100°C and 150°C are 500 Pa·s or less and 100 Pa·s or less, respectively. Such viscosity characteristics are advantageous in a process in which a curable hot melt silicone composition, for example, an encapsulating sheet made of the composition is temporarily attached to a substrate using a vacuum laminator or a vacuum low pressure press, and then the composition is cured under stationary conditions such as in an oven. In other words, when a curable hot melt silicone composition, for example, an encapsulating sheet, is temporarily attached to a substrate, pressure is applied instantaneously under a certain temperature condition to press the curable hot melt silicone composition onto the substrate, and since pressure is applied at this time, the viscosity is reduced, and the composition has excellent gap filling properties for substrates with many projections and recesses, while when the composition is subsequently left to harden in an oven or the like, no pressure is applied, so even if the composition is cured at a temperature of 150°C or higher, the viscosity of the curable hot melt silicone composition is high, so that no dripping occurs before the curing begins.

[0284] [Curing conditions for the curable hot melt silicone composition] The layer made of the curable hot-melt silicone composition contained in the laminate of the present invention undergoes curing when left at room temperature or when heated. When the layer of the curable hot-melt silicone composition is cured, a laminate made of a substrate and a silicone layer bonded thereto, or a laminate made of two substrates and a silicone layer interposed therebetween as an adhesive, is obtained, but from the viewpoint of promoting the curing of the curable hot-melt silicone composition, it is preferable to cure the obtained laminate made of the uncured or semi-cured curable hot-melt silicone composition and one or two substrates as it is at a temperature of 150° C. or higher for 1 hour or more. At this time, when the laminate is composed of one substrate and a layer made of curable hot-melt silicone composition, and the layer made of curable hot-melt silicone composition has a surface that is not in contact with the substrate, a release sheet may be attached to the surface of the layer made of curable hot-melt silicone composition that is not in contact with the substrate.At this time, the laminate of the present invention is prepared using the sealing sheet having the release film described above, and when the release film remains on the surface of the curable hot-melt silicone composition layer that is not in contact with the substrate, the release film can be peeled off after the curable hot-melt silicone composition layer is cured without peeling it off.

[0285] [Viscoelastic properties of the cured product] The cured product obtained by curing the curable hot-melt silicone composition used in the laminate of the present invention exhibits characteristic viscoelastic properties. When the dynamic viscoelasticity of a general silicone cured product is measured by varying the temperature, it exhibits a sharp glass transition at a certain temperature, although this differs depending on the network structure and the type of functional group. In other words, the curve of tan δ, which is the ratio of the storage modulus to the loss modulus, exhibits a sharp peak at a certain temperature. In general, when the value of tan δ is high, the applied force is dispersed (relaxed), so it can be said that a material with a high tan δ has excellent stress relaxation properties. Here, it is preferable that the cured product obtained by curing the curable hot-melt silicone composition used in the laminate of the present invention does not exhibit a sharp tan δ peak at a certain temperature, but exhibits a characteristic of a high tan δ value over a wide range of temperatures (Figure 3). For example, when the curable hot-melt silicone composition is cured at 150°C, the cured product has a thermal history of a temperature difference of 125°C until it returns to room temperature, 25°C, and when this composition is laminated and adhered to a substrate with a low thermal expansion coefficient, thermal stress occurs within this temperature range. If tan δ is low over the entire range within this temperature range, or if there is a very sharp peak of tan δ within this range, thermal stress continues to accumulate in the material over the specified temperature range. Alternatively, even if the material enters a region with high tan δ and stress relaxation begins, it immediately leaves the region, so sufficient relaxation does not occur. On the other hand, in the case of a silicone cured product with high tan δ over a wide range of temperature, this thermal stress relaxes over time, and warping, etc. that occurs when a laminate is formed using a thin substrate is greatly reduced. In other words, when a large-area thin substrate is encapsulated in one batch using such a curable hot-melt silicone composition, especially an encapsulating sheet made of such a composition, the thermal stress of the silicone cured product is relaxed, so that warping, etc. of the substrate is unlikely to occur.The same is true for a three-layer laminate in which a silicone layer is sandwiched between two substrates. For example, when two types of substrates having different thermal expansion coefficients are bonded together with a silicone layer to form a laminate, the laminate is likely to be subjected to stress due to the difference in the thermal expansion coefficients. Therefore, it is preferable to use a silicone layer having the above-mentioned stress relaxation properties, in order to prevent defects such as peeling and cracks caused by thermal stress in the resulting laminate.

[0286] [Hardness of the cured product obtained by curing the curable hot-melt silicone composition] The suitable hardness of the cured product obtained by curing the curable hot-melt silicone composition of the present invention is classified into two types depending on its application. When two substrates are bonded with a silicone layer interposed therebetween, that is, when both sides of the silicone layer are bonded to the substrate, it is preferable that the type A durometer hardness specified in JIS K 7215-1986 "Durometer hardness test method for plastics" is 40 or more. This is because if the hardness is below the above lower limit, the cured product tends to be too soft and brittle. On the other hand, in the case of a laminate in which a silicone layer is bonded to one substrate, for example, when the application of the curable hot-melt silicone composition is to seal a substrate, it is preferable that the type A durometer hardness is 60 or more. This is because if the hardness is below the above lower limit, the surface of the cured product becomes sticky and the handling properties are reduced.

[0287] [Layers other than the substrate and the curable hot-melt silicone composition layer] The layer made of the curable hot melt silicone composition constituting the laminate of the present invention may be one layer made of one type of composition, or may be two or more layers made of two or more different compositions. Furthermore, when the laminate of the present invention is made of one substrate and a layer made of the curable hot melt silicone composition, an additional layer may be provided on the surface of the layer made of the curable hot melt silicone composition that is not in contact with the substrate. Examples of the additional layer include a layer (release layer) made of a material with higher release properties than the layer made of the curable hot melt silicone composition, and a layer having water repellency and / or oil repellency. Such a layer can be formed by laminating a material having such properties on a layer not in contact with the laminate of the layer of the curable hot melt silicone composition. Materials exhibiting the above-mentioned properties can be those known in the art.

[0288] [Multi-layer laminate] The laminate of the present invention includes a multilayer laminate, and has a multilayer structure consisting of a curable hot-melt silicone composition layer and a functional layer in contact with one of the two surfaces of the layer. There are no particular limitations on the shape of the multilayer laminate, but it is preferably in the form of a sheet or film. In addition, in the JIS Packaging Terminology Standards, a material with a thickness of less than 250 μm is called a film, and a material with a thickness of 250 μm or more is called a sheet, and although the terms sheet and film are used in this specification, they are collectively referred to as "sheet" in this specification. Therefore, even when simply referring to a "sheet" in this specification, the thickness includes not only those with a thickness of 250 μm or more, but also those with a thickness of less than 250 μm.

[0289] In order to facilitate handling and storage of the multilayer laminate of the present invention, a release film (including a protective film; the same applies below) may be attached to either one of the two outer surfaces of the multilayer laminate, i.e., the outer surface of the functional layer not in contact with the curable hot-melt silicone composition layer, or the outer surface of the curable hot-melt silicone composition layer not in contact with the functional layer, and such a form of release laminate is also included in the present invention. In particular, a form in which a release film is attached to the outer surface of the curable hot-melt silicone composition layer is preferred. As another embodiment of the present invention, a release laminate in which a release film is attached to both the outer surface of the functional layer of the multilayer laminate of the present invention and the outer surface of the curable hot-melt silicone composition layer can be mentioned, and this is also included in the present invention. The release laminate refers to a multilayer laminate having a release film on at least one surface thereof, and the release film is configured to be peelable from the multilayer laminate. The release film may be one well known in the art, and is a film having a release layer on at least one surface of the base film. The substrate of the release film is not particularly limited, and examples thereof include paperboard, cardboard paper, clay-coated paper, polyolefin-laminated paper, particularly polyethylene-laminated paper, synthetic resin film / sheet, natural fiber cloth, synthetic fiber cloth, artificial leather cloth, and metal foil. In particular, synthetic resin films or sheets are preferred, and examples of synthetic resins include polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polycarbonate, polyethylene terephthalate, and nylon. When heat resistance is particularly required, films of heat-resistant synthetic resins such as polyimide, polyether ether ketone, polyethylene naphthalate (PEN), liquid crystal polyarylate, polyamide imide, and polyether sulfone are preferred. On the other hand, in applications requiring visibility such as display devices, transparent substrates, specifically transparent materials such as polypropylene, polystyrene, polyvinylidene chloride, polycarbonate, polyethylene terephthalate, and PEN are preferred. As described above, the substrate can be made of paperboard, and the like, and the term release film is not particularly limited in terms of thickness.

[0290] [Selection and design of functional layers for multi-layer laminates] The layer made of the curable hot melt silicone composition constituting the laminate of the present invention may be one layer made of one type of composition, or may be two or more layers made of two or more different compositions. Furthermore, when the laminate of the present invention is made of one substrate and a layer made of the curable hot melt silicone composition, an additional layer may be provided on the surface of the layer made of the curable hot melt silicone composition that is not in contact with the substrate. By providing layers having various functionalities as additional layers, it is possible to impart various functions to the laminate. For example, it is possible to provide a hard coat on the surface of the laminate by providing a layer that is much harder than the layer made of the curable hot melt silicone composition. Similarly, it is also possible to reduce the tack of the surface of the laminate by laminating a layer that is less tacky than the cured product made of the curable hot melt silicone composition. In addition, when the curable hot melt silicone composition layer is transparent and light-transmitting, it is also possible to control the optical properties of the laminate by laminating a layer with a different refractive index on the surface layer. Similarly, it is also possible to impart special optical properties to the laminate by providing a light-diffusing layer on the surface layer of the laminate.

[0291] As an example, the following combinations can be mentioned. One form of the curable hot melt silicone composition of the present invention is a composition containing the above-mentioned (A2') component, which has the effect of increasing the flexibility, stress relaxation, and adhesion of the obtained cured product, but at the same time has the characteristic of increasing the tack (adhesiveness) of the surface of the obtained cured product. Therefore, a cured product made of a composition containing a large amount of the (A2') component exhibits high stress relaxation and adhesion, but also has high surface tack. In order to reduce this surface tack, a layer of a cured product made of a non-hot melt silicone composition not containing the (A2') component can be laminated on the outermost surface of the laminate. Since such a non-hot melt silicone composition not containing the (A2') is liquid at 25°C, it is difficult to directly seal a large-area substrate without the generation of voids, i.e., without bubbles. In addition, the stress relaxation of the obtained cured product is poor, so there is a concern that high thermal stress will be generated if it is directly bonded to a substrate, but since it does not contain the (A2') component, the tack of the cured product surface is low. Here, the layer that directly seals the substrate is made of a curable hot-melt silicone composition that has good handling and stress relaxation properties, and the cured layer made of the non-hot-melt silicone composition is laminated on the surface of the curable hot-melt silicone composition as a functional layer, which can significantly reduce the tack of the curable hot-melt silicone composition containing a large amount of (A2') component and its cured product.In addition, when applied to the use of optical systems that require a transparent cured product, it is possible to provide a laminate that does not deteriorate in optical properties by matching the refractive index of the curable hot-melt silicone composition and the non-hot-melt silicone composition.

[0292] [Laminate formed from a non-peelable substrate and the above-described multi-layer laminate] The present invention also provides a laminate comprising a multilayer laminate including the above-mentioned functional layer and a curable hot-melt silicone composition layer, and a substrate that does not have peelability. This embodiment includes a laminate in the form of sealing a substrate, particularly a substrate, that does not have peelability, using the above-mentioned multilayer laminate as an encapsulating sheet. The substrate that does not have peelability may be any substrate that is to be covered or sealed with a silicone resin, but it is particularly preferable to use a substrate for an electronic device, particularly an electronic circuit board or an electronic circuit mounting board, a substrate for a semiconductor device, or a substrate for a semiconductor device that is equipped with a semiconductor element, as the substrate. By using the encapsulating sheet having the curable hot-melt silicone composition layer of the present invention in an appropriate manner, a silicone encapsulating layer with few or no defects such as voids can be formed on the substrate. In another embodiment of the present invention, the laminate comprises two substrates, a first and a second, and the above-mentioned multilayer laminate interposed therebetween. In this case, by using the multilayer laminate of the present invention in an appropriate manner, a laminate in which two substrates of the same type or different types are bonded via a curable hot-melt silicone composition layer and a functional layer that have few or no defects such as voids can be obtained. In this case, one of the two substrates is preferably a substrate for electronic devices, particularly an electronic circuit substrate or an electronic circuit mounting substrate, a substrate for semiconductor device, or a substrate for semiconductor device with a semiconductor element mounted thereon, and the other substrate can be the same or different substrate selected from the above-mentioned substrates, or a completely different substrate or substrate, for example, a substrate for protecting an electronic device substrate, i.e., a substrate for protecting the material and substrate laminated thereunder. Therefore, the laminate in this case includes a layer derived from a multilayer laminate including a first and a second substrate and a curable hot-melt silicone composition layer interposed between them to bond the two substrates. In these embodiments, the multilayer laminate of the present invention is in a state in which the substrate, for example, a substrate for electronic devices, is temporarily fixed by the curable hot-melt silicone composition layer, and the viscosity of the curable hot-melt silicone composition does not decrease even when melted in a state where no pressure is applied as described above, and does not flow due to its own weight, etc., so that the volume change that occurs in the silicone composition during curing is smaller than that of conventional liquid curable silicone compositions.Furthermore, by using the curable hot-melt silicone composition having excellent stress relaxation properties as described above, it is possible to significantly reduce the stress that occurs in the laminate when the silicone composition cures.

[0293] [Substrates or base materials for electronic devices] The substrate or base material that does not have peelability and is a part of the laminate of the present invention is not particularly limited, but is particularly preferably a component used in electronic equipment or a substrate on which such a component is mounted.Examples of such a substrate include, but are not limited to, a substrate for electronic equipment, particularly an electronic circuit substrate or a substrate mounted with an electronic circuit, a substrate for semiconductor equipment, or a substrate for semiconductor equipment that is mounted with a semiconductor element.The cured product obtained by curing the curable hot melt silicone composition used in the present invention has excellent color resistance at high temperatures, so it can be particularly suitably used in the manufacture of a laminate using an optical semiconductor device as a substrate, which requires the transparency of the encapsulant. Therefore, examples of substrates that do not have peelability include substrates on which electronic circuits are mounted, such as plastic substrates typified by PCB substrates, metal substrates typified by aluminum, copper, nickel, and silicon, and ceramic substrates typified by aluminum nitride, alumina, and silicon carbide, and various substrates for electronic devices or electronic materials (hereinafter, these are referred to as electronic substrates). With regard to such laminates having a two-layer structure of an electronic substrate and a silicone layer, the silicone layer is generally called a "sealing layer", and depending on the application of the electronic material, it is often preferable that the surface of the sealing layer is flat. By using a sealing sheet containing the multilayer laminate of the present invention described later and manufacturing the laminate using a specific sealing process, it is possible to make the surface of the multilayer laminate side have a flush flatness. Substrates for electronic devices or electronic materials often have circuits mounted thereon, and the substrate surface has irregularities, and in the sealing process, it is necessary to seal the substrate with a silicone layer along the shape of these irregularities without the inclusion of bubbles. As described below, by using a multi-layer laminate having a specific curable hot-melt silicone composition layer and laminating the curable hot-melt silicone composition layer onto a substrate using a specific sealing process, it is possible to fill the gaps caused by the unevenness with silicone without the inclusion of bubbles.

[0294] The functional layer of the multilayer laminate of the present invention may be a layer made of a second substrate having no peelability different from the substrate to be sealed using the multilayer laminate as an encapsulating sheet. As such a second substrate, various materials such as a substrate other than the substrate having no peelability described above, for example, a glass plate, a plastic plate, a metal plate, a ceramic plate, etc., can be used, and the material can be selected according to the application of the electronic device to be produced. As described above, any material may be used as the substrate, but the surface where the curable hot-melt silicone composition layer and the substrate having no peelability come into contact, i.e., the adhesive surface, does not contain voids, and the unevenness due to the circuit of the substrate must be completely filled with the curable silicone composition. For this purpose, it is preferable to apply the multilayer laminate to a substrate having no peelability by a specific process described herein using a layer made of a specific curable hot-melt silicone composition described herein.

[0295] In order to improve adhesion between the layer of a non-releasable second substrate, which is part of the configuration of the laminate of the present invention, and the layer of the curable hot-melt silicone composition, if desired and within the scope of the present invention, the surface of the above-mentioned board / substrate may be subjected to a surface treatment such as an oxidation method or a roughening method, or a primer treatment, and then a layer of the above-mentioned curable hot-melt silicone composition may be laminated thereon.

[0296] In addition, generally, even if the substrate (including the substrate) does not have any peelability, its thermal expansion coefficient is low, but the thermal expansion coefficient of the silicone layer laminated on the substrate is higher than that, so when they are combined to form a laminate, a non-negligible level of stress occurs in the laminate.For this reason, a laminate in which the substrate is temporarily fixed by a layer made of a curable silicone composition having hot melt properties as defined in the present invention (a layer made of a curable hot melt silicone composition) can suppress the generation of stress, and is preferable.Furthermore, it is preferable to use a curable hot melt silicone composition having the above-mentioned specific cured product characteristics in the laminate of the present invention.

[0297] [Laminate made of multi-layered laminate and non-peelable substrate] The multilayer laminate having a release film on both sides or one side thereof obtained as described above can be used as an encapsulant for covering a substrate to protect it from the external environment, and in such a case, the multilayer laminate described above can be called an encapsulating sheet. This encapsulating sheet can be used to encapsulate various substrates that do not have release properties, and such substrates may be any. Therefore, the present invention also provides a laminate in which a substrate that does not have release properties is encapsulated with the multilayer laminate. The substrate that does not have release properties is different from the substrate that is primarily formed with the multilayer laminate of the present invention, as in the above-mentioned release film, but is ultimately peeled off and removed, and includes, but is not limited to, a substrate for an electronic device that is to be encapsulated using the multilayer laminate of the present invention as an encapsulant, such as a semiconductor precursor substrate, an electronic circuit substrate, an electronic circuit mounting substrate, etc., but may be any substrate or substrate. Methods for laminating a substrate that does not have release properties onto the multilayer laminate of the present invention consisting of a functional layer and a curable hot melt silicone composition layer include known methods such as compression molding, press molding, and vacuum lamination, and in particular, the vacuum lamination method described below is preferred.

[0298] [Method for producing a laminate comprising a substrate and a curable hot-melt silicone composition layer] Among the laminates of the present invention, the laminate consisting of a substrate and a curable hot melt silicone composition layer adhered thereto can be produced by stacking the above-mentioned curable hot melt silicone composition, particularly a sheet of the composition, on the substrate, and heating and melting the curable hot melt silicone composition to adhere to the substrate. In the case of a laminate including two substrates and a layer consisting of a curable hot melt silicone composition interposed therebetween, the curable hot melt silicone composition, particularly a sheet of the composition, is stacked on the first substrate, and the curable hot melt silicone composition is heated and melted to adhere to the first substrate to form a layer consisting of the curable hot melt silicone composition, and then the surface of the second substrate is stacked on the surface of the layer consisting of the curable hot melt silicone composition that is not in contact with the first substrate, and the second substrate is adhered to the layer of the curable hot melt silicone composition that has been melted by heating and melting. Alternatively, the laminate consisting of the first substrate and the curable hot melt silicone composition layer adhered thereto can be produced by adhering the first substrate and the second substrate to each side of the sheet consisting of the curable hot melt silicone composition in a series of operations, respectively, without taking out the laminate consisting of the first substrate and the curable hot melt silicone composition layer adhered thereto as an intermediate from the production device. However, the method for producing the laminate of the present invention is not limited to these.When preparing a laminate using the above-mentioned sealing sheet consisting of two release films and a curable hot-melt silicone composition sheet interposed therebetween, that is, sandwiched between two release films, peeling off one release film, adhering the curable hot-melt silicone composition sheet to the first substrate with the surface of the side where the release film was peeled off, and leaving the other release film as it is, a laminate having the structure of (first substrate-curable hot-melt silicone composition layer-release film) is obtained, and this laminate is also within the scope of the present invention.

[0299] A method for producing the laminate of the present invention using the above-mentioned encapsulating sheet will be described below, but the method for producing the laminate is not limited thereto. In one embodiment, a laminate according to the present invention comprising a substrate and a curable hot-melt silicone composition layer in contact with the substrate, particularly in close contact with the substrate, can be produced by the following steps: Step 1: a step of placing a sheet or film made of a curable hot-melt silicone composition (also referred to as a "sealing sheet") on a substrate placed in a reduced pressure chamber in such a way that the sheet or film can come into contact with the substrate in a subsequent step, or a step of placing a sheet or film made of a curable hot-melt silicone composition on a substrate placed in the reduced pressure chamber, or a step of placing a substrate in a reduced pressure chamber with the sheet or film made of a curable hot-melt silicone composition placed thereon in advance so that it comes into contact with the substrate; Step 2: reducing the pressure in the vacuum chamber to a predetermined pressure; Step 3: heating the inside of the vacuum chamber under reduced pressure to melt the curable hot-melt silicone composition sheet or film and adhere it to the substrate, and if necessary, applying pressure to either or both of the substrate and the sheet or film after adhesion to pressurize the curable hot-melt silicone composition sheet or film to the substrate; and Step 4: releasing the vacuum within the vacuum chamber and removing from the chamber a laminate comprising a layer selected from the group consisting of a layer made of a curable hot-melt silicone composition, a cured layer and a semi-cured layer thereof, and a substrate in contact with said layer; The composition can be produced by a method comprising the steps of: Here, in the present invention, an encapsulating sheet is used that is made of a curable hot-melt silicone composition that has a melt viscosity of 5000 Pa·s or less at 100°C (at the limiting shear rate) measured at a pressure of 2.5 MPa using a flow tester. This method makes it possible to produce a laminate comprising a layer of a curable hot-melt silicone composition and a substrate in contact with said layer, while minimizing defects such as voids.

[0300] According to the method of the present invention, a curable hot-melt silicone composition sheet or film (hereinafter, even if simply described as "sheet", the sheet also includes a film unless otherwise specified) is heated under reduced pressure to melt the sheet, and the sheet is pressed against a substrate, for example, a substrate for an electronic device, and the substrate is covered with a silicone composition layer without air bubbles being trapped between the silicone composition sheet and the substrate, and the substrate can be sealed with the silicone composition, and an electronic device substrate having a flat surface sealing layer, for example, an electronic circuit board or an electronic circuit mounting substrate, particularly a semiconductor element, can be easily manufactured. This allows a laminate including a substrate and a curable hot-melt silicone composition layer in contact with the substrate to be obtained. In particular, in the method of the present invention, a curable hot-melt silicone composition sheet is used that has a sufficiently low melt viscosity of the silicone composition when the curable hot-melt silicone composition is heated and pressed against the substrate, so that even if the substrate is a substrate having fine irregularities, particularly a substrate having a large area, the substrate can be quickly and easily sealed with the curable silicone composition without air bubbles being trapped between the substrate and the silicone composition to produce a laminate. Furthermore, by curing this curable silicone composition, a laminate can be obtained in which a cured silicone composition layer is laminated on a substrate, i.e., the substrate is sealed with the cured silicone composition. Each of the above steps will be described in detail below.

[0301] [Steps 1 and 2] Step 1 is either (i) placing a curable hot-melt silicone composition sheet, i.e., a sealing sheet, in a reduced pressure chamber in advance so that the sealing sheet can be in direct contact with the substrate in a step subsequent to step 1, relative to the substrate placed in the reduced pressure chamber, (ii) placing a sealing sheet on the substrate placed in the chamber in the reduced pressure chamber, or (iii) placing a sealing sheet on the substrate outside the reduced pressure chamber in advance so that the sealing sheet is in contact with the substrate, and then installing the sheet in the reduced pressure chamber. (i) is a method in which the substrate and the sealing sheet are appropriately arranged in the reduced pressure chamber using a suitable means that allows the sealing sheet to come into direct contact with the substrate in the step after step 1, particularly in step 3 described later. Thus, the substrate and the sealing sheet are not in contact with each other when they are first arranged in the reduced pressure chamber, but in a later step, the sealing sheet is brought into contact with the substrate using a suitable means, for example, a diaphragm-type vacuum laminator described later. (ii) is a method in which the sealing sheet is placed on the substrate in the reduced pressure chamber when the substrate and the sealing sheet are arranged in the reduced pressure chamber. (iii) is a method in which the sealing sheet is placed on the substrate in advance and then placed in the reduced pressure chamber so that the sealing sheet comes into contact with the substrate before the substrate and the sealing sheet are placed in the reduced pressure chamber. Any of these may be used.

[0302] Depending on the shape of the substrate, this step 1 may be either step 1-1 or step 1-2 shown below. Whether step 1-1 or step 1-2 is preferred depends on whether the shape of the substrate allows air bubbles to escape easily between the substrate and the sealing sheet when a curable hot-melt silicone composition sheet is placed on the substrate surface, and the sheet is heated to melt and pressure-bonded to the substrate surface.

[0303] Step 1-1: When the substrate surface is uneven. When the surface of the substrate on which the sealing sheet is placed and adhered, for example, the surface of a substrate for an electronic device, is uneven, the number of paths for air bubbles to escape between the substrate surface and the sealing sheet increases when the sealing sheet is pressed against the substrate surface, and the air bubbles are easily removed. Therefore, even without a special operation, when the sealing sheet is melted and pressed against the substrate surface by heating under reduced pressure, almost all of the bubbles escape from between the substrate and the sealing sheet. For this reason, when sealing a substrate having a surface with many irregularities with the sealing sheet of the present invention, the sealing sheet may be placed on the substrate in a reduced pressure chamber (step 1 (ii) described above), or, before placing the substrate and the sealing sheet in the reduced pressure chamber, the sealing sheet may be placed and attached to the substrate surface at an arbitrary temperature, for example, room temperature, and then the substrate may be placed in the reduced pressure chamber (step 1 (iii) described above). At this time, it is not a problem if a small amount of air layer, so-called void, remains between the substrate and the sealing sheet, but the air layer remaining between the substrate and the sealing sheet may be pushed out and removed by any method, for example, by using a rubber roller. The surface of the substrate to which the encapsulating sheet is attached may be a part or the entire surface of the substrate, for example, one side of the substrate as the substrate, or even a part thereof.

[0304] In the case where the above method (ii) or (iii) is used in step 1, in either case, the substrate on which the encapsulating sheet is placed is placed in a reduced pressure chamber equipped with a heating means in step 1. An example of such a reduced pressure chamber is a vacuum laminating device. It is preferable to heat the reduced pressure chamber to a predetermined temperature before placing the substrate in the chamber. That is, in this case, the encapsulating sheet starts to be heated from the time when the substrate on which the encapsulating sheet is attached is placed in the heated reduced pressure chamber, or from the time when the encapsulating sheet is attached to the surface of the substrate placed in the reduced pressure chamber, and when the predetermined temperature is reached, the encapsulating sheet starts to melt. The suitable temperature in the reduced pressure chamber depends on the melting characteristics of the encapsulating sheet used, but the temperature in the reduced pressure chamber is preferably set to 50°C or higher, and more preferably set to 70°C or higher. In the case where the curable hot-melt silicone composition layer derived from the encapsulating sheet is also cured in step 3 described later, it is preferable to set the temperature in the reduced pressure chamber to 150°C or higher from the viewpoint of being able to cure in a short time.

[0305] When the above method (i) is used in step 1, the encapsulating sheet can be brought into contact with the substrate at any time up to the time when the heating chamber is heated under reduced pressure to melt the encapsulating sheet and adhere it to the substrate in step 3. For example, the time can be any time during the step of decompressing the inside of the decompression chamber to a predetermined pressure in step 2, or before the heating chamber is heated under reduced pressure to melt the encapsulating sheet and adhere it to the substrate in step 3. The above method (i) is effective for obtaining a laminate with no or few defects such as voids between the substrate and the encapsulating sheet, particularly when the substrate surface has few irregularities as described below, but can also be used when the substrate surface has many irregularities.

[0306] Step 2 following Step 1-1: Next, when the above method (ii) or (iii) is adopted, the pressure in the vacuum chamber containing the substrate with the encapsulating sheet placed on its surface is reduced to a predetermined pressure. The pressure in the chamber can be reduced by a conventionally known decompression means, for example, by operating a vacuum pump connected to the decompression chamber so that the inside of the decompression chamber can be reduced. Usually, the air pressure in the decompression chamber is reduced to 300 Pa or less, preferably 200 Pa or less, or 133 Pa or less. On the other hand, when the above method (i) is adopted, the step 2 of reducing the pressure in the decompression chamber may be performed after the substrate and the encapsulating sheet are brought into contact with each other, but as in the step 1-2 described below, it is preferable to contact the substrate and the encapsulating sheet by an appropriate means during the reduction of the pressure in the decompression chamber or after the pressure in the decompression chamber is reduced to a predetermined pressure.

[0307] Step 1-2: When the substrate surface is not very uneven Step 1-2 corresponds in particular to the above-mentioned method (i). When the surface of the substrate used has few irregularities, the path through which bubbles existing between the encapsulating sheet and the substrate surface can escape is reduced under reduced pressure, and when the encapsulating sheet and the substrate are heated and pressed, the bubbles existing between them, so-called voids, may not be completely removed from the interface between the encapsulating sheet and the substrate. Step 1-2 is a preferred step for use in such cases, and in order to prevent air bubbles, so-called voids, from remaining between the encapsulating sheet and the substrate after heat and pressure bonding, it is preferable to carry out the step of placing the encapsulating sheet on the substrate surface itself under reduced pressure, particularly under reduced pressure in a reduced pressure chamber using an appropriate means. When the encapsulating sheet is placed on the substrate surface, it is preferable that the substrate, for example, the substrate, has reached a temperature at which the encapsulating sheet can melt. This is because, by placing the encapsulating sheet on the substrate surface while melting it under reduced pressure and adhering it to the substrate surface, an air layer, for example, a void, is not substantially generated between the encapsulating sheet and the substrate, and therefore no voids remain between the encapsulating sheet and the substrate. In this case, even if there is a void between the sealing sheet and the substrate surface under reduced pressure, the void disappears in the subsequent process of pressurizing the molten sealing sheet and the substrate to adhere to each other. In order to carry out this method, any means capable of placing the sealing sheet on the substrate surface under reduced pressure can be used. For example, a special reduced pressure chamber equipped with such a means can be used, and the means is not particularly limited, but for example, a vacuum laminator having a lift pin lifting mechanism can be used. Alternatively, a diaphragm type vacuum laminator can be used by using a dedicated lamination jig. For example, the lamination jig has a structure that supports the sealing sheet with an elastic body such as a spring, and when the diaphragm rubber film is in a stationary position, the sealing sheet can be kept away from the heating means, and when pressure is applied to the diaphragm rubber film, the elastic body provided in the lamination jig can be pressed to bring the sealing sheet into contact with the heating means. In addition, the lamination jig may have a structure that protects the substrate and the sealing sheet so that the diaphragm rubber film does not directly contact the substrate, for example, the substrate and the sealing sheet, even when the diaphragm rubber film presses the lamination jig.

[0308] Step 2 following Step 1-2: Following the above-mentioned step 1-2, the pressure in the vacuum chamber is reduced to a predetermined target pressure. In this case, the sealing sheet is placed on the substrate under reduced pressure in the vacuum chamber, and when the pressure in the vacuum chamber is reduced, step 2 may be simply to confirm whether the pressure in the vacuum chamber is reduced to a predetermined pressure.

[0309] [Process 3] Process 3: Heat compression bonding process This step is a step in which the sealing sheet of the laminate in which the sealing sheet is placed on a part or the whole of the substrate surface in step 1, i.e., step 1-1 or step 1-2, is heated to a molten state, and the molten sealing sheet is pressed against the substrate at a low pressure to adhere to the substrate, thereby temporarily adhering or adhesively curing the sealing sheet and the substrate. The sealing sheet is made of the silicone composition having hot melt properties of the present invention, and when the sealing sheet is pressure-bonded to the substrate, the sheet needs to be molten. Therefore, the process is performed at a temperature equal to or higher than the melting temperature of the hot melt silicone composition, and the temperature is 50° C. or higher, preferably 70° C. or higher. Since this step is performed under reduced pressure, it is possible to prevent bubbles from remaining in the sealing layer formed from the sealing sheet after the sealing sheet is heat-pressed to the substrate, especially at the interface between the sealing layer and the substrate, by appropriately selecting the conditions of step 1-1 or 1-2 and step 2.

[0310] The encapsulating sheet is heated by a heating means provided in the reduced pressure chamber. For example, a hot plate provided in the reduced pressure chamber can be used as the heating means. Usually, the encapsulating sheet is heated by heating a substrate on which the encapsulating sheet is placed, such as a semiconductor substrate. For example, when a hot plate is used as the heating means, the substrate and the hot plate are brought into contact with each other, so that heat is transferred to the encapsulating sheet through the substrate, thereby heating the encapsulating sheet.

[0311] The method of applying pressure to the substrate and the sealing sheet in the thermocompression bonding process is not particularly limited, but examples include a diaphragm method in which compressed air is used to inflate rubber, and a press method in which pressure is applied by moving a press using hydraulic or pneumatic pressure. However, if the applied pressure is too high, there is a risk that the elements and other accessories mounted on the substrate may be deformed or damaged when an electronic device substrate is used as the substrate, and since the sealing sheet is melted during thermocompression bonding, there is a risk that the melted sealing sheet may flow out of the area to be sealed, so it is preferable to press the melted sealing sheet onto the substrate at a low pressure. Specifically, the pressure applied to the substrate and the sealing sheet is 1.2 MPa or less, preferably 0.7 MPa or less, and more preferably 0.5 MPa or less.

[0312] Usually, if the encapsulating sheet is only heat-pressed to the substrate, the time required for the pressing is within 1 minute. However, if the encapsulating sheet is to be pressed to the substrate and cured at the same time, it is preferable to set the heat-pressing temperature to 150° C. or higher and press the substrate and the encapsulating sheet for about 5 to 10 minutes. At this time, by not satisfying the conditions necessary for the curable hot-melt silicone composition constituting the encapsulating sheet to cure, a laminate is obtained that is composed of a substrate and an encapsulating sheet adhered thereto, with the encapsulating sheet in an uncured or semi-cured state. The surface of the encapsulating sheet of the laminate thus obtained, that is, the layer made of the curable hot-melt silicone composition, can have excellent flatness.

[0313] Step 4: Release the pressure Step 4 is a step of releasing the reduced pressure in the vacuum chamber and taking out from the vacuum chamber a laminate including a layer of the curable hot melt silicone composition derived from the sealing sheet and a substrate in contact with the layer, i.e., a substrate sealed with the above-mentioned sealing sheet, for example, a substrate for electronic devices such as a semiconductor substrate. If the sealing sheet does not melt but only softens at the temperature during the reduced pressure, this step can be a step of pressing the sealing sheet against the substrate by the pressure difference between the pressure during the reduced pressure in the vacuum chamber and the outside air after the reduced pressure is released. However, in the method of the present invention, the sealing sheet used is melted at the temperature in the chamber and thermocompressed to the substrate under reduced pressure, so this step is a step of taking out the substrate obtained in the thermocompression step and the laminate including the sealing sheet adhered to the substrate. "Releasing the reduced pressure in the vacuum chamber" usually means bringing outside air into the vacuum chamber to return the pressure in the vacuum chamber to atmospheric pressure. There is no limit to the rate at which the reduced pressure is returned to atmospheric pressure, and typically, the reduced pressure in the reduced pressure chamber is returned to atmospheric pressure at a rate of 10 kPa / sec, preferably at a rate of 50 kPa / sec, or 100 kPa / sec.

[0314] In one embodiment of the laminate of the present invention, the layer of the curable hot melt silicone composition derived from the sealing sheet constituting the laminate is in an uncured or semi-cured state, but the present invention also provides a laminate in which the curable hot melt silicone composition constituting the above-mentioned laminate is in a cured state, that is, a laminate including a layer of the cured curable hot melt silicone composition and a substrate in contact with the layer. In order to cure the curable hot melt silicone composition layer of the laminate, the laminate obtained by the above-mentioned method can be cured by proceeding with a curing reaction under conditions in which the curable hot melt silicone composition is cured. In addition, in the step of thermocompression bonding the sealing sheet to the substrate in the above-mentioned step 3, the curing reaction can also be proceeded under conditions in which the curing reaction of the curable hot melt silicone composition proceeds together with or after the thermocompression bonding.

[0315] In addition, in the above-mentioned laminate manufacturing method, when a sealing sheet made of the curable hot-melt silicone composition of the present invention is used, the sheet is preferably in the form of a laminate having a release film arranged on both sides or one side thereof so that the release surface is in contact with the sheet before use. Here, the thickness of the release film is not limited to a specific one, and therefore the release film also includes a thickness that is usually called a sheet. Specifically, such a laminate preferably has a structure of (i) release film / curable hot-melt silicone composition sheet, or (ii) release film / curable hot-melt silicone composition sheet / release film. Release films are known in the art, and examples thereof include paperboard, cardboard paper, clay-coated paper, polyolefin-laminated paper, particularly polyethylene-laminated paper, synthetic resin film or sheet, natural fiber cloth, synthetic fiber cloth, artificial leather cloth, and metal foil, all of which have been subjected to a release treatment on the surface. In particular, the release film is preferably a synthetic resin film or sheet with a release treatment on one or both sides thereof, and examples of synthetic resins include polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polycarbonate, polyethylene terephthalate, and polyamide. In particular, when heat resistance is required, heat-resistant synthetic resin films such as polyimide, polyether ether ketone, polyethylene naphthalate (PEN), liquid crystal polyarylate, polyamideimide, and polyethersulfone are suitable. On the other hand, in applications where visibility of the device is required through the release film in sealing a display device, etc., transparent substrates, specifically transparent materials such as polypropylene, polystyrene, polyvinylidene chloride, polycarbonate, polyethylene terephthalate, and PEN, are suitable as materials for the release film. When using an encapsulating sheet with such a release film attached, if the release sheet is attached to both sides of the encapsulating sheet, at least one release sheet is peeled off, and the encapsulating sheet is placed so that it is directly in contact with the substrate. At that time, the release sheet on the surface of the sealing sheet opposite to the surface in contact with the substrate may be left in that state to form a laminate including the substrate and the sealing sheet, or the release sheet may be peeled off from the sealing sheet at any stage.When a laminate consisting of an encapsulating sheet and a substrate is prepared without peeling the release sheet from the encapsulating sheet, the resulting laminate has a structure of release film / encapsulating sheet / substrate. In addition, a laminate having a different substrate instead of the release film, or a different layer, for example, a silicone polymer layer having a different composition from the curable hot-melt silicone composition constituting the encapsulating sheet, may be present between the release film and the encapsulating sheet, and these are also within the scope of the laminate of the present invention.

[0316] When using a sealing sheet in the above-mentioned method for producing a laminate of the present invention, a sealing sheet without a release film may be used, but it is preferable to use a sealing sheet with a release film attached only to one side. Therefore, when the sealing sheet has a release film on both sides, it is preferable to peel off the release film on one side of the sealing sheet when using the sealing sheet, and place the sealing sheet in a reduced pressure chamber while leaving the release film on the other side. This is because, for example, when a diaphragm-type vacuum laminator is used, the sealing sheet melts when heated to a temperature above the melting temperature, and when the sealing sheet is pressed against the substrate by the diaphragm, if the diaphragm and the sealing sheet come into direct contact with each other, the two will adhere to each other. Since a release film is interposed between the diaphragm and the sealing sheet, the problem of the sealing sheet adhering to such a diaphragm does not occur.

[0317] Furthermore, the laminate obtained by the above method may be cured completely or the curable hot-melt silicone composition contained in the laminate may be in an uncured or semi-cured state by heating the curable hot-melt silicone composition constituting the encapsulating sheet to a temperature at which the curable hot-melt silicone composition can be cured, for example, a temperature of 100°C or higher, in the above-mentioned step 3 and / or after step 3 and before step 4. Alternatively, a laminate may be obtained in which the curable hot-melt silicone composition contained in the laminate remains in an uncured or semi-cured state without carrying out a heat treatment for curing the curable hot-melt silicone composition. When obtaining a laminate consisting of uncured or semi-cured silicone layers without curing the curable hot-melt silicone composition layer of the laminate, in order to increase the surface flatness of the curable hot-melt silicone composition layer of the laminate as much as possible, it is preferable to prepare the laminate using the above-mentioned method without removing the release film attached to the surface opposite to the surface that contacts the substrate in the sealing sheet, obtain a laminate with the release film still attached to the curable hot-melt silicone composition layer that is in close contact with the laminate, and then peel off the release film from the cured silicone layer after curing the curable hot-melt silicone composition.This is because if the release film is peeled off while the curable hot-melt silicone composition layer is in an uncured state and then the composition layer is cured, the composition layer will melt due to heating, and the surface flatness of the composition layer will be damaged, and as a result, the flatness of the encapsulating silicone layer after curing may be damaged.

[0318] In order to thermally cure the curable hot-melt silicone composition layer of the laminate, an optimal curing temperature can be selected according to the curing system. When the curable hot-melt silicone composition is cured by a hydrosilylation reaction, the curing temperature is preferably 150°C or higher. When the curable hot-melt silicone composition is cured by an organic peroxide, the curing temperature is preferably 170°C or higher. In addition, when the curable hot-melt silicone composition is UV cured, it is preferable to irradiate the curable hot-melt silicone composition layer with UV light after removing the laminate from the vacuum chamber. When the composition layer is UV cured while the release film is still attached to the surface of the curable hot-melt silicone composition layer of the laminate obtained by the above steps 1 to 4, it is preferable to use a release film made of a material that can sufficiently transmit ultraviolet light.

[0319] [Method for producing a laminate comprising first and second substrates and a curable hot-melt silicone composition layer sandwiched between them] A laminate of this type has a construction of (first substrate-curable hot-melt silicone composition layer-second substrate). A laminate of this structure can be produced by slightly modifying the method for producing the laminate in the above-mentioned form in which a curable hot-melt silicone composition layer is adhered to one substrate. That is, in the above-mentioned step 1, similarly to the above-mentioned (i) to (iii), (i') two substrates and an encapsulating sheet interposed therebetween are arranged in a vacuum chamber using an appropriate means so that the encapsulating sheet can be brought into contact between the two substrates in a later step, (ii') in the vacuum chamber, an encapsulating sheet is placed on a first substrate, and a second substrate is placed on the encapsulating sheet, or (iii') a substrate in which an encapsulating sheet is placed on a first substrate in advance, and the first substrate is placed on the encapsulating sheet, is then placed in a vacuum chamber, and (iv) a combination of these, i.e., a method of contacting the first substrate with the encapsulating sheet and a method of contacting the outer surface of the encapsulating sheet with the second substrate are each independently selected from the above-mentioned (i) to (iii), thereby making it possible to produce a laminate having the above-mentioned structure, i.e., a laminate in which two substrates are bonded by a curable hot-melt silicone composition layer interposed therebetween.

[0320] [First transformation method] Therefore, in the above-mentioned step 1, a second substrate of the same or different type as the first substrate is further disposed on a surface of the encapsulating sheet arranged or placed in advance on the first substrate so as to be in contact with the first substrate in a later step or on a surface other than the surface in contact with the first substrate, particularly the opposite surface, so as to be in contact with the encapsulating sheet in a later step, or a second substrate of the same or different type as the substrate is further placed on a surface other than the surface in contact with the first substrate, particularly the opposite surface, so as to be in contact with the encapsulating sheet in advance, thereby making it possible to produce a laminate having a configuration of (first substrate-curable hot-melt silicone composition layer-second substrate) by the above-mentioned production method. In this case, the above also applies to this method with regard to the conditions for steps 1 to 4. Furthermore, as explained above, by curing the curable hot-melt silicone composition layer of the laminate comprising the above-mentioned two substrates and the curable hot-melt silicone composition layer interposed between them, a laminate in which the two substrates are bonded by the cured silicone layer can be obtained.

[0321] [Second transformation method] Another method for producing a laminate in which two substrates are bonded together by a curable hot-melt silicone adhesive layer interposed therebetween or a silicone layer formed by curing the adhesive layer is to produce a laminate having a substrate (first substrate) and a curable hot-melt silicone composition layer adhered thereto by the above-mentioned steps 1 to 4, and then to the surface of the curable hot-melt silicone composition layer that is not in contact with the first substrate, i.e., the outer surface, by repeating the above-mentioned steps 1 to 4, a second substrate is bonded to produce the desired laminate. In this case, the outer surface of the curable hot-melt silicone composition layer of the laminate initially produced having a configuration of (first substrate-curable hot-melt silicone composition layer) is regarded as one surface of the sealing sheet to which no substrate is bonded, and the above-mentioned explanation of steps 1 to 4 can be applied as it is. Therefore, for example, after obtaining a laminate comprising one substrate and a curable hot-melt silicone composition layer adhered thereto by steps 1 to 4 described above, the laminate obtained in step 4 can be removed from the reduced pressure chamber, or without being removed, and a second substrate can be attached to the surface of the curable hot-melt silicone composition layer on the side not adhered to the substrate, by repeating steps 1 to 4 in the same manner as above, thereby producing a laminate comprising a structure of (first substrate-curable hot-melt silicone composition layer-second substrate). EXAMPLES

[0322] The laminate of the present invention will be described in more detail based on examples and comparative examples. In the average unit formula and chemical formula of the raw material of the curable hot-melt silicone composition sheet used, Me, Vi, and Ph represent methyl group, vinyl group, and phenyl group, respectively. In addition, the hardness of the cured product used in each example and comparative example, the cycle time of the production process, and the produced curable hot-melt silicone composition sheet, that is, the laminate consisting of the sealing sheet and the semiconductor substrate, were measured by the following methods for the film thickness of the curable hot-melt silicone composition layer (also called the sealing layer) derived from the sealing sheet in the laminate, the flatness and tackiness of the laminate / sealing layer surface, the warpage of the laminate after the sealing layer is cured, and the cold-heat cycle durability of the laminate, and the results are shown in Table 1.

[0323] [Hardness of cured product] The hardness of a cured product made from the curable silicone composition of the present invention was measured using a Type D durometer as specified in JIS K 7215-1986 "Durometer hardness testing method for plastics."

[0324] [Manufacturing process cycle time] In each process shown below, the time required to obtain a laminate in which there are no voids at the interface between the encapsulating sheet and the substrate and the encapsulating layer on the substrate formed from the encapsulating sheet is completely pressure-bonded to the substrate from the state in which the encapsulating sheet and the substrate are separated or the encapsulating sheet is simply attached to the substrate at room temperature was measured. Specifically, the cycle time of each manufacturing process was determined as the time from the time when the substrate or the substrate with the encapsulating sheet placed thereon was placed in the reduced pressure chamber until the obtained laminate could be taken out of the reduced pressure chamber.

[0325] [Warping of laminate] In the examples and comparative examples, for a two-layer laminate consisting of a substrate and a sealing layer, one end of the laminate was fixed to a flat table with tape, and the lift of the unfixed end of the laminate from the surface of the table was measured using a ruler as the vertical distance from the surface of the table to the lifted end (lifted length). A lifted length of 1 mm or less was marked as ◯, a lifted length of 3 mm or less was marked as △, and a lifted length of 5 mm or more was marked as ×.

[0326] [Uniformity of sealing layer thickness] Using a flat substrate with a constant thickness, the thickness of the sealing layer of the laminate obtained by the following process was measured at five random points using a contact film thickness meter (Nikon Digital Microhead). If the difference between the maximum and minimum values ​​was 30 μm or less, it was marked as ◎, if it was 40 μm or less, it was marked as ◯, if it was 50 μm or less, it was marked as △, and if it was 50 μm or more, it was marked as ×.

[0327] [Surface flatness of laminate / sealing layer] The flatness of the surface of the sealing layer of the laminate obtained by the following process was evaluated using a laser microscope (Olympus 3D MEASURING LASER MICROSCOPE OLS4000). The flatness of the sealing layer surface was evaluated by measuring the distance from the bottom surface of the substrate to the surface of the sealing layer of the laminate at five random points, and marking a maximum difference of 1 μm or less as ◯ and a maximum difference of 5 μm or more as ×.

[0328] [Surface tack of laminate / sealing layer] The surface tack of the sealing layer of the laminate obtained by the following process was evaluated. The evaluation was performed by placing a PET film that had not been subjected to any surface treatment on the sealing layer, and applying 100 g / cm 2 A weight was pressed against the sealing layer for 30 seconds, and then if the PET film could be peeled off smoothly from the sealing layer, it was marked with an ◯, and if it could not be peeled off smoothly, it was marked with an ×.

[0329] [Laminated body durability during thermal cycles] The laminate obtained by the process below was subjected to a 100-cycle test using a thermal cycle tester (TSA-73EH manufactured by ESPEC) set to repeat -20°C and 5°C, with -20°C x 30 minutes and 5°C x 30 minutes being one cycle, and then the thermal cycle durability of the test specimen was evaluated visually. The laminate was evaluated by assigning X to those that had peeling or cracks after the test, ○ to those that had not, and ◎ to those that had not peeled or cracked after 500 cycles.

[0330] [Reference Example: Preparation of a Curable Hot Melt Silicone Composition Sheet] The following raw materials were used in each Reference Example. Silicon resin a1: White solid at 25°C, average unit formula: (Me2ViSiO 1 / 2 ) 0.05 (Me3SiO 1 / 2 ) 0.39 (SiO 4 / 2 ) 0.56 (HO 1 / 2 ) 0.02 The organopolysiloxane resin represented by the formula (vinyl group content = 1.9 mass%) Si resin a2: (Me3SiO 1 / 2 ) 0.44 (SiO 4 / 2 ) 0.56 (HO 1 / 2 ) 0.02 The organopolysiloxane resin (vinyl group content = 0 mass%) represented by the formula: Si polymer b: ViMe2SiO(Me2SiO) 800 SiViMe2 SiH siloxane c1: (PhSiO 3 / 2 ) 0.4 (HMeSiO 1 / 2 ) 0.6 (The amount of volatile components after aging for 1 hour in an oven at 100°C under atmospheric pressure, i.e., the mass loss rate, is 3.4% by mass.) SiH siloxane c2: (HMe2SiO 1 / 2 ) 0.52 (MeSiO2 / 2 ) 0.15 (SiO 4 / 2 ) 0.33 (The amount of volatile components after aging for 1 hour in an oven at 100°C under atmospheric pressure, i.e., the mass loss rate, is 2.9% by mass.)

[0331] (Reference example 1) 3.09 kg of Si resin a1, 3.77 kg of Si resin a2, and 2.69 kg of Si polymer b were dissolved in 4.00 kg of xylene in a pail can using a three-one motor. The obtained solution was fed into a twin-screw extruder with a maximum temperature set to 230°C, and xylene and low molecular weight organopolysiloxane components were removed under a vacuum degree of XX, resulting in a transparent mixture 1 exhibiting hot melt properties. Mixture 1 was received in a barrel pail can and cooled as it was to solidify. The amount of volatile components in this mixture was measured at 200°C for 1 hour, and was found to be 0.7% by mass.

[0332] The obtained hot-melt mixture 1 was fed to a twin-screw extruder at 170° C. through line 1 shown in FIG. 2 at a rate of 9.56 kg / hr using a hot melter for cylindrical pails (VersaPail melter manufactured by Nordson Corporation). Next, SiH siloxane c2 0.295 kg / hr, and Methyltris-1,1-dimethyl-2-propynyloxysilane (boiling point = 245 ° C.) in an amount of 3500 ppm relative to the total composition, The mixture was fed from line 2 shown in Figure 2. The temperature of the feed port was set to 150°C. Next, Si polymer b 0.15 kg / hr, A mixture consisting of a 1,3-divinyltetramethyldisiloxane solution of platinum 1,3-divinyltetramethyldisiloxane complex (an amount equivalent to 4.0 ppm by mass of platinum metal relative to the entire curable hot-melt silicone composition finally obtained) was fed from line 3-b in Figure 2 (the temperature set at the feeding section was 80°C), and the degree of vacuum inside the twin-screw extruder was -0.08 MPa, during which the components fed into the extruder were degassed, melted and kneaded. The outlet temperature of the twin-screw extruder was set to 80°C, and the mixture was supplied in the form of a semi-solid softened material onto a 125μm-thick release film (FL2-01, manufactured by Takara Line Corporation) at a supply rate of 5kg / hr, and the mixture was sandwiched between two release films so that the release surface of the release film was in contact with the mixture to form a laminate. The laminate was then pressed between rolls controlled at a temperature of 90°C to stretch the mixture, forming a laminate in which a 300μm-thick curable hot-melt silicone composition sheet was sandwiched between two release films, and the entire laminate was cooled by air cooling. The configuration of the manufacturing apparatus is shown in FIG. 2. When the release film was peeled off from the obtained laminate, a bubble-free, flat, homogeneous, tack-free, transparent curable hot-melt silicone composition sheet 1 was obtained. The melt viscosity of the obtained composition sheet was measured using a flow tester (CFT-500EX, manufactured by Shimadzu Corporation) at a temperature of 100°C, a nozzle diameter of 1 mm, and a pressure of 2.5 MPa, and was found to be 120 Pa·s.

[0333] [Reference examples 2~4] Instead of the mixture of Reference Example 1, the mixture of the composition shown in the table below was used (volatilized content measured at 200°C x 1 hour was 0.7% by mass for all), and SiH siloxane c1 was the organohydrogenpolysiloxane (feed amount) shown in the table below. The same procedure as Reference Example 1 was repeated to obtain a flat, homogeneous, tack-free, transparent curable hot-melt silicone composition sheet without bubbles, and the melt viscosity measured with a flow tester is shown in the table. For Reference Examples 3 and 4, the hardness of the sheet cured product was also measured and is shown in the table below. [Table 1]

[0334] [Example 1] The curable hot melt silicone composition sheet (sealing sheet) 1 interposed between the two release films obtained in Reference Example 1 was cut to a size (square) of 4.5 cm x 4.5 cm, and one of the two release films was peeled off from the sealing sheet 1. Thereafter, the surface of the sealing sheet 1 without the release film was placed on a semiconductor substrate (having a copper foil pattern with a thickness of 35 μm) with a size (square) of 6.0 cm x 6.0 cm and a thickness of 0.2 mm, and the sealing sheet 1 was manually bonded to the semiconductor substrate. The obtained laminate having a configuration of (release film-uncured silicone sealing layer-semiconductor substrate) was placed in a vacuum laminator device (V-130 manufactured by Nikko Materials Co., Ltd.), and lamination was performed for 30 seconds under conditions of a vacuum setting value of 5.0 hPa and temperatures of the upper and lower heat plates in the reduced pressure chamber of 110°C. After that, the reduced pressure in the reduced pressure chamber was released and returned to atmospheric pressure, and a laminate having a configuration of (release film-uncured silicone sealing layer-semiconductor substrate) without any bubbles or the like was obtained, which was firmly adhered. The laminate thus obtained was then placed in an oven set at 160°C to thermally cure the silicone sealing layer for 2 hours. After removing the laminate from the oven, the release film on the surface of the silicone sealing layer was peeled off to obtain Laminate 1 having a cured silicone sealing layer with a flat surface and a semiconductor substrate. The properties of Laminate 1 are shown in Table 2.

[0335] [Example 2] The curable hot melt silicone composition sheet 1 (encapsulating sheet 1) obtained in Reference Example 1 was cut to a size (square) of 4.5 cm x 4.5 cm, and one of the two release films was peeled off from the encapsulating sheet 1. Thereafter, the surface of the encapsulating sheet 1 without the release film was placed on a semiconductor substrate (having a copper foil pattern with a thickness of 35 μm placed thereon) with a size (square) of 6.0 cm x 6.0 cm and a thickness of 0.2 mm, and the encapsulating sheet 1 was manually bonded to the semiconductor substrate. The resulting laminate having a configuration of (release film-uncured silicone encapsulating layer-semiconductor substrate) was placed on the stage of a reduced pressure chamber of a vacuum laminator device (V-130 manufactured by Nikko Materials Co., Ltd.). Shim spacers with a thickness of 300 μm were placed on both sides of the silicone sealing layer on the semiconductor substrate, and lamination was performed for 5 minutes under conditions of a vacuum setting value of 5.0 hPa and a temperature of the upper and lower hot plates in the vacuum chamber of 180 ° C. After that, the vacuum in the vacuum chamber was released and returned to atmospheric pressure, and a laminate was obtained that was firmly adhered without any bubbles or other contaminants (release film - cured silicone sealing layer - semiconductor substrate). Next, the laminate thus obtained was placed in an oven set at 160 ° C. for 2 hours to completely cure the silicone sealing layer. After removing the laminate from the oven, the release film on the surface of the silicone sealing layer was peeled off to obtain a laminate 2 consisting of (cured silicone sealing layer with a flat surface - semiconductor substrate). The properties of the laminate 2 are shown in Table 2.

[0336] [Example 3] The curable hot melt silicone composition sheet 2 (sealing sheet 2) obtained in Reference Example 2 was cut to a size (square) of 4.5 cm x 4.5 cm, and one of the two release films was peeled off from the sealing sheet 2. The sealing sheet 2 was placed in a vacuum laminator device (V-130 manufactured by Nikko Materials Co., Ltd.) so that the release film remaining on one side of the sealing sheet 2 faces the stage side of the decompression chamber. Next, shim spacers having a thickness of 300 μm and bent into a dogleg shape were placed on both sides of the sealing sheet 2 so that the top of the shim spacers was a mountain shape higher than the sealing sheet 2, and a glass plate having a thickness of 1 mm and a size (square) of 6.0 cm x 6.0 cm was placed on the mountain-shaped shim spacers. This makes it possible to create a situation in which the glass plate and the sealing sheet 2 do not come into contact with each other until the decompression process in the decompression chamber is completed. Then, pressure is applied from the upper side of the glass plate, and the shim spacers are pressed and crushed by the glass plate, and the glass plate and the silicone sheet come into contact for the first time. In this state, the vacuum chamber was heated for 30 seconds under the conditions of a vacuum setting value of 5.0 hPa and the temperatures of the upper and lower heating plates in the vacuum chamber at 110°C. Then, the vacuum in the vacuum chamber was released and the pressure was returned to atmospheric pressure, and a laminate having a structure of (release film-uncured silicone sealing layer-glass plate) was obtained without any bubbles or other inclusions. The obtained laminate was placed in an oven set at 160°C to thermally cure the curable silicone sealing layer for 2 hours. After removing the laminate from the oven, the release film on the surface of the silicone sealing layer was peeled off to obtain a laminate 3 having a structure of (cured silicone sealing layer with a flat surface-glass plate). The properties of the laminate 3 are shown in Table 1.

[0337] [Example 4] After obtaining a laminate 4 consisting of (release film-uncured silicone sealing layer-glass plate 1) in the same manner as in Example 3, the release film was peeled off from the obtained laminate 4, and the laminate 4 was placed in a vacuum laminator device (V-130 manufactured by Nikko Materials Co., Ltd.) so that the glass plate 1 faces the stage side of the reduced pressure chamber. A shim spacer bent into a dogleg shape was placed on both sides of the uncured silicone sealing layer on the glass plate 1 so that the tops of the spacers were mountain-shaped, and a glass plate 2 having a size (square) of 6.0 cm x 6.0 cm and a thickness of 1 mm was placed on the mountain-shaped shim spacer. When the glass plate 2 was laminated on the uncured silicone sealing layer in the same manner as the glass plate 1 was laminated on the sealing sheet 2, a laminate having a configuration of (glass plate 1-uncured silicone sealing layer-glass plate 2) without any bubbles or the like was obtained. The obtained laminate was placed in an oven set at 160° C. for 2 hours to thermally cure the uncured silicone sealing layer, thereby obtaining Laminate 5 having a structure of (glass plate 1-cured silicone adhesive layer-glass plate 2). The properties of Laminate 5 are shown in Table 2.

[0338] [Comparative Example 1] Along the vertical and horizontal edge lines of a 6.0 cm x 6.0 cm (square) semiconductor substrate (with a 35 μm thick copper foil pattern), VE-6001 (a photocurab...

Claims

1. The following steps: Step 1: In a reduced pressure chamber, a substrate placed in the chamber is R 1 SiO 3/2 (In the formula, R 1 each independently represents a substituted or unsubstituted alkyl group or a substituted or unsubstituted aryl group, and 4/2 and a curable hot-melt silicone composition comprising an organopolysiloxane resin containing at least 20 mol % of all siloxane units selected from the group consisting of siloxane units represented by the following formula: -1 a step of positioning a sheet or film of a curable hot-melt silicone composition having a melt viscosity of 5000 Pa s or less at 100°C when measured at a pressure of 2.5 MPa (at an ultimate shear rate) using a flow tester, and which when cured forms a cured product having a tan δ, which is the ratio of storage modulus to loss modulus, of 0.05 or more in a temperature range from -50°C to 200°C and extending to 100°C or more; such that the sheet or film can come into contact with the substrate in a subsequent step; alternatively, a step of placing a sheet or film of the curable hot-melt silicone composition on a substrate placed in the chamber in a reduced pressure chamber; or a step of placing a substrate in a reduced pressure chamber, the substrate having a sheet or film of the curable hot-melt silicone composition previously placed therein such that the sheet or film is in contact with the substrate; Step 2: reducing the pressure in the vacuum chamber to a predetermined pressure; Step 3: heating the inside of the vacuum chamber under reduced pressure to melt the curable hot-melt silicone composition sheet or film and adhere it to the substrate; and Step 4: releasing the vacuum within the vacuum chamber and removing from the chamber a laminate comprising a layer selected from the group consisting of a layer made of a curable hot-melt silicone composition, a cured layer and a semi-cured layer thereof, and a substrate in contact with said layer; Including, A method for producing a laminate comprising a substrate and a layer of a curable hot-melt silicone composition in contact with the substrate.

2. 2. The method for producing a laminate according to claim 1, wherein in step 1, a sheet or film made of a curable hot-melt silicone composition is arranged or pre-placed on the substrate so as to be able to come into contact with the substrate in a later step, and a substrate which is the same as or different from the substrate is further arranged on a surface other than a surface which will come into contact with the substrate in a later step or a surface which is in contact with the substrate, so as to be able to come into contact with the sheet or film made of the curable hot-melt silicone composition in a later step, or a substrate which is the same as or different from the substrate is further placed on the other surface so as to be in contact with the sheet or film made of the curable hot-melt silicone composition in advance.

3. A method for producing a laminate obtained by the method for producing a laminate as recited in claim 1, comprising a substrate and, on one surface of the substrate, a curable hot-melt silicone composition layer derived from a sheet or film made of a curable hot-melt silicone composition, the method comprising the steps of further laminating a substrate that is the same as or different from the substrate, in a similar manner to steps 1 to 4, on an outer surface of the curable hot-melt silicone composition layer on the side not in contact with the substrate, thereby producing a laminate having two substrates that are the same or different and a curable hot-melt silicone composition layer sandwiched between them.

4. 2. The method of claim 1, wherein in step 3, the temperature when the curable hot-melt silicone composition sheet or film is pressure-bonded to the substrate is 50° C. or higher.

5. 2. The method of claim 1, wherein the curable hot-melt silicone composition layer has a multi-layer structure comprising a functional layer in contact with one surface of the curable hot-melt silicone composition layer.

6. The method for producing a laminate according to claim 1 , wherein the substrate is a substrate which is an electronic component or a semiconductor precursor.

7. 3. The method for producing a laminate according to claim 2, wherein the laminate is a laminate comprising a first substrate and a second substrate with a curable hot-melt silicone composition layer interposed therebetween, the first substrate being a substrate that is an electronic component or a semiconductor precursor, and the second substrate being a release film.

8. 3. The method for producing a laminate according to claim 2, wherein the laminate comprises a first substrate and a second substrate with a curable hot-melt silicone composition layer interposed therebetween, and both the first substrate and the second substrate are substrates which are electronic components or semiconductor precursors.

9. 9. A method for producing a laminate comprising a cured silicone layer, comprising the step of curing a curable hot-melt silicone composition layer contained in a laminate obtained by the method for producing a laminate according to any one of claims 1 to 8.

10. The method for producing a laminate according to claim 9, which is a method for producing an electronic component.

Citation Information

Patent Citations

  • Dam material composition for image display apparatus, and image display apparatus using the same

    JP2014237834A

  • Curable silicone composition, semiconductor sealant comprising the same and semiconductor device

    JP2016124967A

  • Method for manufacturing a semiconductor device and a semiconductor device.

    JP4607429B2

  • Curable silicone composition, curable hot-melt silicone, and optical device

    WO2016035285A1

  • Curable silicone composition, light-reflecting material, and method for producing same

    WO2018235492A1