Flux paint, coating, aluminum tube for heat exchanger, and heat exchanger assembly

The flux paint with Zn-free flux, synthetic resin, and acidic phosphate ester addresses adhesion issues in brazing paints for heat exchangers, ensuring robust brazing bondability and preventing peeling, thereby enhancing the quality of heat exchanger assemblies.

JP7560283B2Active Publication Date: 2024-10-02MA ALUMINUM CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020123277
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-17
Publication Date
2024-10-02
Estimated Expiration
2040-07-17

AI Technical Summary

Technical Problem

Existing brazing paints for heat exchangers with aluminum tubes and fins suffer from insufficient coating film adhesion, leading to peeling and potential brazing defects, especially during assembly and resizing processes.

Method used

A flux paint composition containing Zn-free flux, synthetic resin, and acidic phosphate ester is used, which enhances coating film adhesion to aluminum surfaces by improving hardness and electrical interaction, preventing peeling during assembly and brazing processes.

Benefits of technology

The flux paint ensures robust brazing bondability by maintaining coating film integrity, preventing peeling and ensuring uniform brazing without defects, even under mechanical stress, thus improving the quality of heat exchanger assemblies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560283000009
    Figure 0007560283000009
  • Figure 0007560283000010
    Figure 0007560283000010
  • Figure 0007560283000011
    Figure 0007560283000011
Patent Text Reader

Abstract

To provide a flux coating and a coated film which can be applied to a heat exchanger having a brazed configuration, and can improve adhesion in a coated film state, and a heat exchanger having the coated film.SOLUTION: A flux coating contains a Zn-free flux, a synthetic resin, an organic solvent, and acid phosphate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flux paint, a coating film, an aluminum tube for a heat exchanger, and a heat exchanger. assembly Regarding. [Background technology]

[0002] Conventionally, in order to assemble a heat exchanger having a structure in which fins and a plurality of tubes are integrated, a method of applying a flux to the surface of the materials to be brazed or a method of applying a mixed composition of flux and brazing material has been carried out, and a brazing coating composition with an improved component composition suitable for brazing has been proposed. A coating composition for brazing is generally a mixed coating composition of a brazing material, flux, synthetic resin, and an organic solvent. This mixed coating composition is applied to the tube to be joined to the fin, and after assembling the fin and tube, the whole is heated to the brazing temperature to perform brazing.

[0003] Furthermore, the following Patent Document 1 discloses a highly insulating aluminum coating material that is excellent in insulation properties, processability, coating film adhesion, and scratch resistance. This highly insulating aluminum coating material has a chemical conversion coating formed on an aluminum substrate and a coating film formed on the chemical conversion coating. This coating film has a hardness of 10 N / mm 2 ~100N / mm 2 It has a glass transition temperature of 120°C to 160°C, and contains 70 to 90% by weight of epoxy-amino resin, 10 to 30% by weight of barium sulfate, 0 to 5% by weight of an organic silicone compound, and 0 to 28% by weight of polyacrylic acid. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-074109 A Summary of the Invention [Problem to be solved by the invention]

[0005] The inventors have been conducting research and development into a brazing paint for use in assembling heat exchangers in which fins and tubes are brazed together, the brazing paint comprising a powdered brazing material, a Zn-containing flux, and a synthetic resin blended in an organic solvent. As part of this research and development, the inventors also conducted research into a brazing paint made by mixing brazing powder, a Zn-free flux, and a synthetic resin in an organic solvent, and discovered that when this brazing paint was applied to the surface of a tube to obtain a coating, the coating adhesion was insufficient.

[0006] If the coating adhesion to the tube surface is poor, the coating is likely to peel off when the tube is inserted along the through holes or slits formed in the fins for assembling the heat exchanger, and there is a risk that the brazing ability will decrease in the areas where the coating peels off. In addition, depending on the heat exchanger to which the product is applied, it may be necessary to resize a portion of the tube. It has been found that when a portion of the tube is processed using a tool such as a die in order to resize the tube, there is a problem in that the coating film easily peels off in the processed portion.

[0007] The present invention aims to provide a flux paint and coating that can be applied to heat exchangers in which fins and tubes are brazed and that can improve adhesion to aluminum in a coating state, as well as an aluminum fin and heat exchanger equipped with said coating. [Means for solving the problem]

[0008] The flux paint of the present invention is characterized by containing a Zn-free flux, a synthetic resin, an organic solvent, and an acidic phosphate ester. In the flux paint of the present invention, the acidic phosphate ester is represented by the following chemical formula (1), in which n is 1 or 2 and R is each independently a compound represented by an alkyl group, and the above-mentioned "each R is independently" in the chemical formula (1) means R in the following chemical formula (2) (when n is 2):1 and R 2 may be different groups.

[0009] [ka]

[0010] [ka]

[0011] In the flux paint of the present invention, acidic The content of the phosphate ester is preferably 0.04% by mass or more and 6.5% by mass or less based on the mass of the synthetic resin. In the flux paint of the present invention, acidic It is preferable that the phosphate ester contains one or more of methyl acid phosphate, ethyl acid phosphate, propyl acid phosphate, isopropyl acid phosphate, butyl acid phosphate, octyl acid phosphate, 2-ethylhexyl acid phosphate, decyl acid phosphate, lauryl acid phosphate, stearyl acid phosphate, oleyl acid phosphate, behenyl acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, dipropyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, dioctyl acid phosphate, di-2-ethylhexyl acid phosphate, dilauryl acid phosphate, and distearyl acid phosphate.

[0012] The flux coating material of the present invention may contain a Zn-containing flux. The flux paint of the present invention may contain a brazing material. The coating film of the present invention is preferably made of any of the flux paints described above. The aluminum tube for heat exchanger of the present invention is characterized by having the coating film described above. do. Heat exchanger of the present invention assembly is as mentioned earlier. for heat exchanger Aluminum Tube and a fin attached to the aluminum tube via the coating film provided on the aluminum tube. Equipped with Then, it becomes a heat exchanger by brazing. It is characterized by: Effect of the Invention

[0013] The flux paint according to the present invention contains a Zn-free flux, a synthetic resin, an organic solvent, and an acidic phosphate. The addition of the acidic phosphate makes the flux paint less likely to peel off when formed as a coating on the surface of aluminum. Furthermore, the hardness of the coating film increases, which improves the adhesion of the coating film when formed on the surface of aluminum. Adhesion is improved due to electrical interaction between the polar groups in the acidic phosphate ester and the aluminum surface.

[0014] Furthermore, if the flux paint contains a brazing material, it becomes a flux paint that can be used for brazing, and can be applied to an aluminum tube to obtain a coating film for brazing. With this brazing coating, when an aluminum tube and a fin are assembled and brazed to form a heat exchanger, the coating will not peel off even if the aluminum tube provided with the brazing coating and the fin come into contact with each other and rub against each other during assembly. Therefore, it is possible to provide a heat exchanger having good brazing bondability without causing brazing defects by using an aluminum tube having a brazing coating of a desired amount at a desired position.

[0015] In addition, in the case of flux paint that does not contain brazing material, it is possible to manufacture a heat exchanger in which the tubes and fins are brazed together by combining it with a clad fin on which a brazing material layer is formed. Alternatively, it is also possible to combine it with a brazing rod or paste separately as a source of brazing material. Flux is essential for normal brazing, so if the tubes are not coated with flux, after assembling the components into the heat exchanger, the flux must be applied in some way, such as by immersing them in a flux liquid or spraying it on. On the other hand, if the tubes are coated with flux, the flux coating process can be omitted, which is an advantage when manufacturing heat exchangers. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a front view of a heat exchanger according to a first embodiment manufactured by applying a flux coating according to the present invention. [Diagram 2] 1 is a partial cross-sectional view of a heat exchanger according to a first embodiment, taken along a longitudinal section of a tube in a longitudinal direction thereof. [Diagram 3] FIG. 2 is a partial cross-sectional view showing the heat exchanger assembly before brazing the heat exchanger of the first embodiment. [Figure 4] FIG. 11 is a perspective view showing a heat exchanger according to a second embodiment manufactured by applying a flux coating according to the present invention. [Diagram 5] FIG. 6 is a cross-sectional view taken along a plane perpendicular to the longitudinal direction of a tube in a heat exchanger of a second embodiment. [Figure 6] FIG. 11 is a cross-sectional view taken along a longitudinal direction of a tube in a heat exchanger according to a second embodiment, showing a state before a brazing step. [Figure 7] FIG. 11 is a cross-sectional view taken along a longitudinal direction of a tube in a heat exchanger according to a second embodiment, showing a state after a brazing process. [Figure 8] 1 is a graph showing the relationship between the amount of phosphate ester added and pencil hardness in samples obtained in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings. The flux paint of this embodiment is a paint obtained by adding a brazing material, a Zn-free flux, a synthetic resin, and an acidic phosphate ester to an organic solvent in a predetermined amount. In addition to the Zn-free flux, this flux paint may also contain a portion of a Zn-containing flux. Since the flux paint contains a brazing material, it can be called a brazing flux paint, and a brazing flux coating film can be obtained by applying this flux paint.

[0018] The brazing material contained in the flux paint may be brazing material powder such as Si powder or alloy powder containing Si. As the Zn-free flux, one or more of the following can be selected and used: LiF, KF, CaF2, AlF3, K2SiF6, KAlF4, K3AlF6, and K2AlF5·5H2O. As the Zn-containing flux, one or two of KZnF3 and ZnF3 can be selected and used. As the synthetic resin, one or more of acrylic resins, resins having a polyether skeleton, and cellulose-based resins can be selected and used. As the organic solvent, one or more of IPA (isopropyl alcohol), MMB (3-methoxy-3-methyl-1-butanol), formic acid, dibutyl phthalate (DBP), ethyl acetate, and phenol can be used.

[0019] An ester that can be used as the acidic phosphate ester is, for example, represented by the following chemical formula (1): In the following chemical formula (1), n ​​is 1 or 2, and each R is independently a compound represented by an alkyl group. The above description of "each R is independent" for the chemical formula (1) means, for example, in the following chemical formula (2) (when n is 2), R 1 and R 2 may be different groups.

[0020] [ka]

[0021] [ka]

[0022] The phosphate ester preferably contains one or more of methyl acid phosphate, ethyl acid phosphate, propyl acid phosphate, isopropyl acid phosphate, butyl acid phosphate, octyl acid phosphate, 2-ethylhexyl acid phosphate, decyl acid phosphate, lauryl acid phosphate, stearyl acid phosphate, oleyl acid phosphate, behenyl acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, dipropyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, dioctyl acid phosphate, di-2-ethylhexyl acid phosphate, dilauryl acid phosphate, and distearyl acid phosphate.

[0023] "Content of brazing filler metal in flux paint: 1.5 to 60% by mass" The content of the brazing material in the flux paint is preferably in the range of 1.5% by mass to 60% by mass. If the brazing filler metal content is less than 1.5 mass %, the amount of brazing filler metal required for the coating cannot be secured, and brazeability decreases. If the brazing filler metal content exceeds 60 mass%, the coating will contain excessive brazing filler metal. In the case where silicon powder is used as the brazing filler metal, unreacted silicon residue will be generated and the corrosion depth of the tube will increase, which is disadvantageous in terms of preventing fin separation.

[0024] "Flux content in flux paint: 2.5 to 60 mass%" The content of the Zn-free flux in the flux paint is preferably in the range of 2.5 mass % or more and 60 mass % or less. If the flux content is less than 2.5% by mass, the formation of the brazing filler metal will be insufficient, and the destruction and removal of the oxide film on the surface of the material to be brazed (tube) will be insufficient, resulting in poor brazing. On the other hand, if the flux content exceeds 60% by mass, the coating film will be too thick, causing a large gap between the fin and the tube during brazing, which may result in poor joining.

[0025] "Synthetic resin content in flux paint: 4.5 to 14.5% by mass" The synthetic resin content (binder content) in the flux paint is preferably in the range of 4.5 mass % or more and 14.5 mass % or less. If the binder content in the flux paint is less than 4.5% by mass, the hardness of the coating film decreases, and the workability (resistance to peeling of the coating film) decreases. On the other hand, if the binder content exceeds 14.5% by mass, the brazing property may decrease due to the influence of the fillet not being formed due to the coating film not reacting.

[0026] "Organic solvent content in flux paint: 25.5 to 83% by mass" The organic solvent content in the flux paint is preferably in the range of 25.5% by mass or more and 83% by mass or less. If the organic solvent content is less than 25.5% by mass, the paint viscosity becomes too high, resulting in a lack of paint spreadability, and the brazing property may be reduced due to the non-uniformity of the flux and brazing material.If the organic solvent content is more than 83% by mass, the paint viscosity becomes too low, resulting in an excessive paint spreadability, and the corrosion resistance and brazing property may be reduced due to the non-uniformity of the flux and brazing material.

[0027] "Content of acid phosphate ester relative to the total mass of synthetic resin (solid content) in flux paint: 0.04 to 6.5 mass%" The content of the acidic phosphate in the flux paint is preferably in the range of 0.04% by mass or more and 6.5% by mass or less based on the total mass of the synthetic resin in the paint. Acid phosphate esters are added to improve the adhesion of coatings to aluminum, and also to improve coating hardness (pencil hardness) when acrylic resins are used. If the content of the acidic phosphate ester is less than 0.04% by mass relative to the total mass of the synthetic resin, the effect of improving the coating adhesion may be insufficient, and if the content of the acidic phosphate ester is more than 6.5% by mass relative to the mass of the synthetic resin, the coating hardness may decrease. The acidic phosphate ester has the effect of making the paint of the above-mentioned composition resistant to peeling from aluminum and improving the hardness of the coating film. It is also believed that the electrical interaction between the polar groups in the acidic phosphate ester and the aluminum surface is effective in improving adhesion.

[0028] When applying the above-mentioned flux paint to the surface of aluminum to form a coating film, it is desirable that the application amount of each component be within the following range. Brazing powder coating amount: 1-30g / m 2 " The amount of brazing powder (brazing material) applied is 1g / m 2 More than 30g / m 2 The following range is preferable: If the amount of applied brazing powder is too small, the brazing properties may be reduced, whereas if the amount is too large, the fillet may be preferentially corroded due to excessive brazing powder formation.

[0029] Zn-free flux coating amount: 3 to 30 g / m 2 " The amount of Zn-free flux applied is 3 g / m 2 More than 30g / m 2 The following ranges are preferred: The amount of Zn-free flux applied to the flux coating is 3 g / m 2 If the applied amount of Zn-free flux is less than 30 g / m, the formation of the brazing filler is insufficient, and the destruction and removal of the oxide film on the surface of the material to be brazed (aluminum tube) is insufficient, leading to poor brazing. 2If the thickness of the coating exceeds this value, the gap between the fin and the tube will be large during brazing, which may result in poor joining.

[0030] Zn-containing flux coating amount: 3 to 30 g / m 2 " The amount of Zn-containing flux applied is 3 g / m 2 More than 30g / m 2 The following ranges are preferred: The amount of Zn-containing flux applied in the flux coating is 3 g / m 2 If the amount of Zn-containing flux applied is less than 30 g / m, the effect of improving corrosion resistance cannot be obtained. 2 If the thickness of the coating exceeds this value, the gap between the fin and the tube will be large during brazing, and resistance to fin peeling may decrease.

[0031] Synthetic resin (binder) coating amount: 0.5 to 10 g / m 2 " The amount of binder applied in the flux coating is 0.5 g / m 2 If the coating amount is less than 8.3 g / m, the hardness of the coating film decreases, and the workability (resistance to peeling of the coating film) decreases. 2 If the temperature exceeds this range, the brazing property may be deteriorated due to the influence of the non-formation of the fillet caused by the non-reaction of the coating film. Note that the binder usually evaporates due to heating during brazing.

[0032] The brazing flux paint described above is used by being applied to an aluminum plate or a tube made of aluminum or an aluminum alloy, such as a flat multi-hole tube described later. The coating can be applied to the required surface of an aluminum plate or tube using a coating device such as a roll coater so that the coating amount of each of the above-mentioned components is ensured, and then heated and dried (baked) in a heating furnace or the like for several minutes at a temperature of 140 to 180°C to obtain a coating film.

[0033] Hereinafter, an embodiment in which the flux paint according to the present invention is applied to an aluminum fin and a heat exchanger will be described with reference to the accompanying drawings. Note that the drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand. "First embodiment of heat exchanger" FIG. 1 is a perspective view showing a first embodiment of a heat exchanger according to the present invention. This heat exchanger 30 is an all-aluminum heat exchanger used for applications such as heat exchangers for indoor and outdoor units of room air conditioners, outdoor units for HVAC (Heating Ventilating Air Conditioning), and heat exchangers for automobiles.

[0034] The heat exchanger 30 of this first embodiment is composed of header pipes 31, 32 arranged upright and parallel to each other and spaced apart from each other as shown in Figure 1, tubes 33 consisting of a plurality of flat tubes arranged parallel to the header pipes 31, 32 and spaced apart from each other and joined perpendicularly to the header pipes 31, 32, and corrugated fins (corrugated fins) 34 attached to each tube 33.

[0035] A plurality of slits 36 are formed at regular intervals on the opposing side surfaces of the header pipes 31, 32 in the longitudinal direction of each pipe, and the tubes 33 are installed between the header pipes 31, 32 by inserting ends of the tubes 33 into the opposing slits 36 of the header pipes 31, 32. In addition, fins 34 are arranged on the upper and lower sides of the plurality of tubes 33, 33 installed at specified intervals between the header pipes 31, 32, and these fins 34 are brazed to the upper or lower side of the tubes 33.

[0036] 2, a first fillet portion 38 is formed with brazing material at the portion where the end of the tube 33 is inserted into the slit 36 ​​of the header pipes 31, 32, and the tube 33 is brazed to the header pipes 31, 32. Also, in the corrugated fin 34, the crest portions of the waves face the front or back surface of the adjacent tube 33, and a second fillet portion 39 is formed with brazing material generated in the portion between them, and the corrugated fin 34 is brazed to the front and back surfaces of the tube 33.

[0037] The fin 34 has a plate-shaped base material 34a made of an alloy based on pure aluminum such as JIS 1050 series or JIS 3003 series aluminum alloy, and a hydrophilic coating 35a attached to the entire surface (front, back and both side surfaces) of the base material 34a. The tube 33 is made of, for example, a pure aluminum-based material such as JIS 1050 or an alloy based on JIS 3003 aluminum alloy. The header pipes 31, 32 are made of, for example, an aluminum alloy based on Al-Mn.

[0038] The heat exchanger 30 of this embodiment is manufactured by assembling header pipes 31, 32 with a plurality of tubes 33 and a plurality of fins 34 installed between them to form a heat exchanger assembly 41 as shown in FIG. 3, and then heating and brazing the assembly. 3, the tube 33 before brazing has a brazing flux coating 37 formed on its upper surface 33A and lower surface 33B. The tube 33 is, for example, a flat multi-hole tube having a plurality of refrigerant passages 33C formed therein. This brazing flux coating film 37 is a coating film obtained by applying the brazing flux paint having the composition described above to the upper surface 33A and the lower surface 33B of the tube 33 with a roll coater and drying it. The composition of the brazing flux paint used here is as described above, and the application amount of each component of the coating film is also as described above. In addition, the drying conditions after coating are also within the range described above.

[0039] When the brazing flux coating film 37 contains a Zn-containing flux, a Zn melting diffusion layer (sacrificial anode layer) 42 shown in Fig. 2 is formed on the front and back sides of the tube 33 by heating during brazing. When the brazing flux coating film 37 does not contain a Zn-containing flux, the Zn melting diffusion layer (sacrificial anode layer) 42 shown in Fig. 2 is not generated.

[0040] When a heat exchanger assembly 41 consisting of the header pipes 31, 32, tubes 33 and fins 34 assembled as shown in Fig. 3 is heated to a temperature equal to or higher than the melting point of the brazing material in a heating furnace or the like in an inert gas atmosphere and then cooled, the brazing material layer 44 and the brazing flux coating 37 melt to join the header pipe 31 and the tube 33, and the tube 33 and the fin 34, respectively, as shown in Fig. 2, to obtain the heat exchanger 30 having the structure shown in Fig. 1 and Fig. 2. At this time, the brazing material layer 44 on the inner peripheral surface of the header pipe 31 melts and flows near the slits 36, forming a fillet 38 to join the header pipe 31 and the tube 33. In addition, the brazing flux coating 37 on the surface of the tube 33 melts and becomes Al-Zn brazing material, Al-Si brazing material, or Al-Si-Zn brazing material, which flows near the fins 34 by capillary force and forms a fillet 39 to join the tubes 33 and the fins 34. Reference numeral 31A denotes a core material of the header pipe 11, and reference numeral 43 denotes a coating layer containing Zn for forming a sacrificial anode layer on the header pipes 31 and 32.

[0041] 3, when constructing a heat exchanger assembly 41, both ends of the tubes 33 are inserted into slits 36 provided in the left and right header pipes 31, 32, and the tubes 33 are assembled so that the corrugated fins 34 are positioned above and below the tubes 33. The apexes of the corrugated fins 34 are positioned so as to contact the upper or lower surface of the tubes 33. When constructing this heat exchanger assembly 41, the tubes 33 inevitably rub against the fins 34 or the header pipes 31, 32. Here, if the brazing flux coating 37 has sufficient hardness and high coating adhesion, peeling of the brazing flux coating 37 can be prevented.

[0042] During brazing, the brazing flux coating 37 and brazing material layer 44 are melted by heating to an appropriate temperature in an appropriate atmosphere such as an inert gas atmosphere. This increases the activity of the flux, causing Zn in the flux to precipitate on the surface of the material to be brazed (tube 33) and diffuse in the thickness direction, and also destroys the oxide films on the surfaces of both the brazing material and the material to be brazed, promoting wetting between the brazing material and the material to be brazed. The brazing conditions are not particularly limited. For example, the heat exchanger assembly 101 may be heated to a brazing temperature (achieved temperature) of 580 to 620° C. at a heating rate of 5° C. / min or more in a furnace, held at the brazing temperature for 30 seconds or more, and then cooled from the brazing temperature to 400° C. at a cooling rate of 10° C. / min or more.

[0043] The brazing flux coating 37 having the above-mentioned composition has high hardness and excellent adhesion to aluminum. Therefore, even if the tubes 33 and the fins 34 come into contact and rub against each other when the heat exchanger assembly 41 is assembled, or even if the ends of the tubes 33 rub against the inner surfaces of the slits 36 of the header pipes 31 and 32, the flux coating 37 on the tubes or at the tube ends will not peel off. Therefore, no brazing defects are produced during brazing, and the heat exchanger 30 with excellent brazing joinability can be obtained.

[0044] "Second embodiment of heat exchanger" Figures 4 to 7 show a heat exchanger of a second embodiment of the present invention, and this heat exchanger 11 includes a pair of left and right header pipes 14, a plurality of flat tubes 22 arranged vertically between the left and right header pipes 14, and a plurality of fins 13 brazed to the outer surface (upper or lower surface) 12b of the tube body 12 that constitutes these tubes 22, as shown in Figure 4. 4, a supply pipe 15 that supplies refrigerant to the tubes 22 via the header pipe 14 is connected to the upper end of the header pipe 14 on the right side. A recovery pipe 16 that recovers the refrigerant that has passed through the tubes 22 is connected to the lower end of the header pipe 14 on the left side. The tubes 22, fins 13, header pipe 14, supply pipe 15, and recovery pipe 16 are all made of aluminum or an aluminum alloy.

[0045] Fig. 5 is a partial cross-sectional view of the heat exchanger 11 taken along a plane perpendicular to the longitudinal direction of the tubes 22. As shown in Fig. 5, a plurality of (six in this embodiment) refrigerant flow paths 12a are formed in the interior of the tubular body 12 constituting the tubes 22, aligned along the width direction. Also, as shown in Fig. 5, a plurality of cutout portions 19 having a shape corresponding to the cross-sectional shape of the tubes 22 are formed in the fins 13 at predetermined intervals above and below. The tubes 22 are fitted into these cutout portions 19, respectively, and each tube 22 is fixed to the fins 13 by brazing. 5, the outer surface 12b of the tubular body 12 constituting the tube 22 is composed of a flat front surface (upper surface) 6A and a back surface (lower surface) 6B, and a first side surface 6C and a second side surface 6D adjacent to the front surface 6A and the back surface 6B. The first side surface 6C is located on the opening side of the cutout portion 19 of the fin 13 and is open to the outside. The second side surface 6D is located on the opposite side of the first side surface 6C and is surrounded by the cutout portion 19.

[0046] 6 and 7 are partial cross-sectional views taken along the longitudinal direction of the tubes 22 in the heat exchanger 11, with Fig. 6 showing the state before the brazing process and Fig. 7 showing the state after the brazing process. A plurality of fins 13 are arranged in parallel along the longitudinal direction of the tubes 22, and the tubes 22 are inserted into each of the cutouts 19. The plurality of fins 13 are arranged in parallel to each other at regular intervals. The fins 13 have bent portions 20 at the periphery of the cutouts 19 that are bent to one side in the thickness direction of the fins 13 along the outer surfaces 12b of the tubes 22. The fin 13 has a plate-shaped substrate 3 made of aluminum or an aluminum alloy, and a hydrophilic coating 1 provided on almost the entire first surface 3a and second surface 3b of the substrate 3 and on the other side surfaces.

[0047] 6, a tube 22 before brazing is used, which has a brazing flux coating 5 formed in advance on the outer surfaces (upper and lower surfaces) 12b of a tube body 12. The brazing flux coating 5 is applied to the upper, lower and side surfaces of the tube body 12 over an entire area to be joined with the fins 13. As an example, the brazing flux coating 5 is formed on the region of the outer surface 12b of the tube 12 that abuts against the fins 13, that is, on the front surface 6A and the back surface 6B of the tube 12. The tubes 22 and fins 13 are arranged so that the tubes 22 pierce and penetrate multiple fins 13 arranged at regular intervals, and the tubes 22 are fitted into the cutout portions 19 of the fins 13. After brazing, the fins 13 and tubes 22 are individually fixed as shown in Figure 7.

[0048] The brazing flux coating film 5 before brazing shown in Fig. 6 is a coating film obtained by applying the brazing flux paint having the composition described above to the upper and lower surfaces of the tube 22 using a coating device such as a roll coater and drying it. The composition of the brazing flux paint used here is as described above, and the application amount of each component as the coating film is also as described above. In addition, the drying conditions after coating are also within the range described above. In the heat exchanger 11 before brazing shown in Fig. 6, the brazing flux coating 5 on the tube 22 is located between the tube 22 and a portion (opposing surface 20a) of the bent portion 20 of the fin 13 facing the tube 22. The brazing flux coating 5 is solidified while being filled between the opposing surface 20a and the tube 22 by being cooled after being heated to about 600°C (brazing process), and becomes a fillet 5A (brazing material layer) as shown in Fig. 7, which brazes and joins the fin 13 and the tube 22. Reference symbol 1a in Fig. 7 indicates the hydrophilic coating after brazing.

[0049] In the heat exchanger 11 having the configuration shown in FIGS. 5 and 7, the tubes 22 must also be arranged so that they pierce and penetrate the multiple fins 13 arranged at regular intervals before brazing, as shown in FIG. In this case, the tubes 22 inevitably rub against the fins 13 or the header pipes 14, 14. If the brazing flux coating 5 has sufficient hardness and high coating adhesion, peeling of the brazing flux coating 5 can be prevented.

[0050] The brazing flux coating 5 having the above-mentioned composition has high hardness and excellent adhesion to aluminum, so that when the tube 22 and the fin 13 are assembled as shown in FIG. 6, the flux coating 5 on the tube does not peel off. Therefore, no defective brazing occurs during brazing, and the heat exchanger 11 has excellent brazing joinability.

[0051] Incidentally, the heat exchangers 11 and 30 described so far are merely examples to which the brazing flux paint of the present invention is applied, and it goes without saying that the paint and coating film of the present invention can be widely applied to heat exchangers of general brazing structure. EXAMPLES

[0052] The present invention will be described in more detail below by showing examples, but the present invention is not limited to these examples. <<Sample Preparation>> An aluminum alloy for tubes containing 0.4 mass% Si and 0.3 mass% Mn, with the remainder being unavoidable impurities and Al, was melted and extruded to obtain a flat multi-hole tube for heat exchangers (wall thickness 0.26 mm x width 12.0 mm x total thickness 1.4 mm: 17 holes) with a flat cross-sectional shape made of the aluminum alloy. A brazing flux paint having the composition shown in Tables 1 and 2 was applied to the front and back surfaces of this flat multi-hole tube using a bar coater in the amount shown in Tables 1 and 2, and then dried at 150°C for 5 minutes to obtain flat multi-hole tubes with brazing flux coatings of Examples 1 to 19 and Comparative Examples 1 to 30.

[0053] In the samples shown in Tables 1 and 2, silicon powder (D(99) particle size 10 μm) was used as the brazing material, NOCOLOK FLUX (NOCOLOK is a registered trademark of Solvay Fluor) was used as the flux, acrylic resin was used as the synthetic resin, and a mixed solvent of 3-methoxy-3-methyl-1-butanol and isopropyl alcohol was used as the organic solvent. The brazing flux coatings on these flat multi-hole pipes were subjected to pencil hardness measurement (pencil scratch test: 750 g load), and the results are shown in Tables 1 and 2 below.

[0054] For the paints shown in Tables 1 and 2 and those containing brazing material, a heat exchanger test specimen with three rows of flat tubes was assembled by combining a flat multi-hole tube with a corrugated fin (JIS 3000 series alloy) shown in Figures 1 and 2, and a brazing process was performed by heating to 600°C for 2 minutes in a heating furnace in a nitrogen gas atmosphere. Regarding the paints shown in Tables 1 and 2, for the paints not containing brazing material, a heat exchanger test specimen with three rows of flat tubes was assembled by combining a flat multi-hole tube with a corrugated fin made of a brazing sheet shown in Figures 1 and 2 (a brazing sheet in which an Al-Si alloy layer made of JIS 4343 alloy with a thickness of 10 μm is bonded to a JIS 3000 series alloy plate), and a brazing process was performed by heating to 600°C for 2 minutes in a heating furnace in a nitrogen gas atmosphere. To evaluate the brazing property, 50 brazed parts of each heat exchanger formed by brazing were visually inspected. Those with no brazing defects were judged as passing (○), and those with even one brazing defect were judged as failing (×). The results are shown in Tables 1 and 2. Incidentally, the corrugated fins made from a JIS 3000 series alloy are just one example, and it goes without saying that other aluminum alloys that are generally used for fins may also be used for the corrugated fins.

[0055] [Table 1]

[0056] [Table 2]

[0057] The samples of Examples 1 to 19 shown in Table 1 are samples in which the content of acidic phosphate ester relative to the mass of the solid content of the synthetic resin was varied in the range of 0.04 mass% to 6.5 mass%, and all samples showed a coating pencil hardness of 3 B or 4 B. The samples of Examples 1 to 8 are flux paints to which no Si powder has been added, and the samples of Examples 9 to 19 are brazing flux paints to which Si powder has been added. In contrast, Comparative Examples 1 and 2 are flux paints in which the amount of acidic phosphate ester added is less than the desired range and too much, respectively, and although the brazeability was excellent, the coating hardness was reduced. Comparative Examples 3 and 4 are examples with a high or low flux content, Comparative Example 5 is an example with a high organic solvent content, Comparative Example 6 is an example with a high flux amount, Comparative Examples 7 and 8 are examples with a high or low synthetic resin content, Comparative Example 9 is an example with a low coating amount, and Comparative Example 10 is an example with a high coating amount. In Comparative Example 9, the coating amount was small, and the amount of synthetic resin (solid content) in the paint was also small, so the amount of synthetic resin (solid content) contained in the coating film was within the desired range (0.5 to 10 g / m 2 ) is a smaller sample. In Comparative Example 10, the coating amount was large and the amount of synthetic resin (solid content) in the paint was also relatively large, so the amount of synthetic resin (solid content) contained in the coating film was within the desired range (0.5 to 10 g / m 2 ) more samples. Comparative Examples 11 and 12 are brazing paints in which the amount of acidic phosphate added is less than the desired range and more than the desired range, respectively, and the brazing properties and the coating hardness were both reduced. Comparative Example 13 is an example where the amount of organic solvent is large, Comparative Example 14 is an example where the amount of synthetic resin is small, Comparative Example 15 is an example where the amount of Si powder is large, Comparative Example 16 is an example where the amount of Si powder is small, Comparative Example 17 is an example where the amount of organic solvent is small and the application amount is large, Comparative Example 18 is an example where the amount of synthetic resin is large and the application amount is also large, Comparative Example 19 is an example where the amount of flux is large, and Comparative Example 20 is an example where the amount of flux is small. Comparative Example 21 is an example where the amount of organic solvent is small and the amount of application is large, Comparative Example 22 is an example where the amount of flux application is small, Comparative Example 23 is an example where the amount of synthetic resin is large, Comparative Example 24 is an example where the amount of synthetic resin application is small, Comparative Example 25 is an example where the amount of synthetic resin application is large, and Comparative Example 26 is an example where the amount of synthetic resin application is small. In Comparative Example 22, the coating amount was relatively large, but the amount of flux in the paint was small, so the amount of flux contained in the coating film was within the desired range (3 to 30 g / m 2 ) is a smaller sample. In Comparative Example 25, the synthetic resin content in the paint was relatively high, and the amount of synthetic resin in the paint was also high, so the amount of synthetic resin applied in the coating film was within the desired range (0.5 to 10.0 g / m 2 ) more samples. In Comparative Example 26, the synthetic resin content in the paint was relatively low, and the coating amount was not large, so the amount of synthetic resin coating contained in the coating film was within the desired range (0.5 to 10 g / m 2 ) is a smaller sample. Comparative Examples 27 to 30 are examples in which the content of acidic phosphate is high.

[0058] Figure 8 shows some of the results shown in Table 1 (flux 40%, synthetic resin (solid) 10%, coating amount 12.5 g / m 2 ) is shown on a graph, with the vertical axis showing pencil hardness (750g load) and the horizontal axis showing the amount of phosphate ester added, and the graph showing the correlation between them. From the results shown in FIG. 8, it can be seen that if the amount of phosphate ester added is in the range of 0.04 mass % to 6.5 mass % with respect to the mass of the synthetic resin, a coating hardness of 4B or more can be obtained. Even within the above range, it is considered more preferable to set the content of the phosphate ester in the range of 0.2 to 1.5% by mass relative to the mass of the synthetic resin. [Explanation of symbols]

[0059] 5... brazing flux coating, 11... heat exchanger, 12... tube body, 13... fins, 14... header tube, 15... supply tube, 16... recovery tube, 19... notch portion, 22... tube, 30...heat exchanger, 31, 32...header pipes, 33...tube, 33A...upper surface, 33B...lower surface, 34...fins, 36...slits, 37...brazing coating, 38...first fillet portion, 39...second fillet portion, 41...heat exchanger assembly.

Claims

1. A flux paint comprising a zinc-free flux, a synthetic resin, an organic solvent, and an acidic phosphoric acid ester.

2. The acidic phosphate ester is represented by the following chemical formula (1), in which n is 1 or 2, and R is a compound represented by each independently an alkyl group or an alkenyl group. The above-mentioned "each R is independently" in the chemical formula (1) means R in the following chemical formula (2) (when n is 2): 1 and R 2 2. The flux coating material according to claim 1, characterized in that: [Formula 1] [chemical 2]

3. 3. The flux paint according to claim 1, wherein the acidic phosphate ester is contained in an amount of 0.04% by mass to 6.5% by mass based on the mass of the synthetic resin.

4. The flux paint according to any one of claims 1 to 3, characterized in that the acidic phosphate ester contains one or more of methyl acid phosphate, ethyl acid phosphate, propyl acid phosphate, isopropyl acid phosphate, butyl acid phosphate, octyl acid phosphate, 2-ethylhexyl acid phosphate, decyl acid phosphate, lauryl acid phosphate, stearyl acid phosphate, oleyl acid phosphate, behenyl acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, dipropyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, dioctyl acid phosphate, di-2-ethylhexyl acid phosphate, dilauryl acid phosphate, and distearyl acid phosphate.

5. The flux paint according to any one of claims 1 to 4, further comprising a Zn-containing flux.

6. The flux paint according to any one of claims 1 to 5, further comprising a brazing material.

7. A coating film comprising the flux paint according to any one of claims 1 to 6.

8. An aluminum tube for a heat exchanger, comprising the coating film according to claim 7.

9. 9. A heat exchanger assembly comprising the aluminum tube for a heat exchanger according to claim 8 and fins attached to the aluminum tube via the coating film provided on the aluminum tube, the assembly being formed into a heat exchanger by brazing.

Citation Information

Patent Citations

  • Brazing binder and heat exchanger member

    JP2005028400A

  • Paste-like composition for aluminum brazing, aluminum-containing member coated therewith, and method of brazing aluminum-containing member using the same

    JP2007275898A

  • Aluminum coating material

    JP2015074109A

  • Aluminum alloy tube for heat exchanger

    JP2017060989A

  • Composition for aluminum brazing

    JP2018164937A