Multilayer Ceramic Capacitors

The multilayer ceramic capacitor design addresses dielectric breakdown by strategically arranging internal electrode layers with recesses to enhance conductivity and reduce capacitance, improving breakdown voltage and resistance.

JP7560382B2Active Publication Date: 2024-10-02MURATA MFG CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021027614
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-24
Publication Date
2024-10-02
Estimated Expiration
2041-02-24

AI Technical Summary

Technical Problem

Existing multilayer ceramic capacitors face dielectric breakdown issues when subjected to high electric fields due to the overlap of external and internal electrodes, which concentrates the electric field and reduces capacitance.

Method used

The design incorporates a specific arrangement of internal electrode layers with recesses to avoid overlap, increasing the number of first internal electrode layers without sandwiching second internal electrode layers, and arranging second internal electrode layers to minimize electric field concentration, thereby reducing capacitance while enhancing conductivity and suppressing dielectric breakdown.

Benefits of technology

This configuration improves breakdown voltage and reduces direct current resistance, allowing for lower capacitance without dielectric breakdown, even under high electric fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560382000002
    Figure 0007560382000002
  • Figure 0007560382000003
    Figure 0007560382000003
  • Figure 0007560382000004
    Figure 0007560382000004
Patent Text Reader

Abstract

To provide a multilayer ceramic capacitor capable of suppressing dielectric breakdown to occur between an internal electrode layer and an external electrode while enabling reduction in capacitance of a capacitor even when a high electric field is applied.SOLUTION: A multilayer ceramic capacitor includes a laminate in which a plurality of dielectric layers are laminated, first internal electrode layers drawn out to both end surfaces of the laminate, second internal electrode layers drawn out on both side surfaces of the laminate, first and second external electrodes which are connected to the first internal electrode layers and arranged on both end surfaces, and third and fourth external electrodes which are connected to the second internal electrode layers and arranged on both side surfaces. The number of first internal electrode layers is greater than the number of second internal electrode layers, and two or more first internal electrode layers are continuously laminated. In the first internal electrode layers, recess portions are formed so as not to overlap with the third and the fourth external electrodes arranged on parts of both the main surfaces when the multilayer ceramic capacitor is viewed in the height direction.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer ceramic capacitor. [Background technology]

[0002] For example, chip-type electronic components having a general structure as described in Patent Document 1 are known as decoupling capacitors used to stabilize the power supply voltage supplied to integrated circuit components (ICs) that operate at high speed, and as noise suppression components for power lines that supply power to integrated circuit components (ICs).

[0003] The chip-type electronic component described in Patent Document 1 is formed by alternately stacking a number of dielectric green sheets each having a through electrode printed on one surface and a number of dielectric green sheets each having a capacitor electrode printed on one surface in a direction perpendicular to the through electrode, with external electrodes connected to the through electrodes and the capacitor electrodes. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Utility Model Application Publication No. 02-082022 Summary of the Invention [Problem to be solved by the invention]

[0005] However, for example, in a feedthrough capacitor such as that described in Patent Document 1, in order to achieve even lower capacitance, if a design is adopted in which the capacitor electrode is arranged on the outermost surface side of the electronic component body, the width of the capacitor electrode is smaller than the width of the external electrode connected to the capacitor electrode, and the external electrode connected to the capacitor electrode overlaps with the feedthrough electrode in the stacking direction, when a high electric field is applied, the electric field will concentrate in the area where the feedthrough electrode and the external electrode overlap, and dielectric breakdown may occur between the feedthrough electrode and the external electrode connected to the capacitor electrode.

[0006] Therefore, a primary object of the present invention is to provide a multilayer ceramic capacitor that enables the capacitance of the capacitor to be reduced while suppressing dielectric breakdown that occurs between internal electrode layers and external electrodes even when a high electric field is applied. [Means for solving the problem]

[0007] The multilayer ceramic capacitor according to the present invention comprises a laminate having a plurality of laminated dielectric layers, the laminate having first and second main faces opposing each other in a height direction, first end faces and second end faces opposing each other in a length direction perpendicular to the height direction, and first and second side faces opposing each other in a width direction perpendicular to the height direction and the length direction; a plurality of first internal electrode layers arranged on the plurality of dielectric layers and extended to the first end faces and the second end faces; a plurality of second internal electrode layers arranged on the plurality of dielectric layers and extended to the first side faces and the second side faces; and a plurality of second internal electrode layers arranged on the first end faces and connected to the first internal electrode layers. a first external electrode disposed on a second end face and connected to a first internal electrode layer; a second external electrode disposed on a first side face, extending from the first side face to be disposed on a part of the first main surface and a part of the second main surface and connected to the second internal electrode layer; and a fourth external electrode disposed on a second side face, extending from the second side face to be disposed on a part of the first main surface and a part of the second main surface and connected to the second internal electrode layer, wherein the number of the first internal electrode layers is greater than the number of the second internal electrode layers, and the first internal electrode layers are Without sandwiching a second internal electrode layer between layers Two or more sheets are stacked in succession The internal electrode laminate isa recess is formed in the first internal electrode layer so as not to overlap with the third external electrode arranged on a part of the first main surface and a part of the second main surface, and the fourth external electrode arranged on a part of the first main surface and a part of the second main surface, when the multilayer ceramic capacitor is viewed from the height direction; the second internal electrode layer is arranged at least between the first internal electrode layer located closest to the first main surface and the first main surface, and at least between the first internal electrode layer located closest to the second main surface and the second main surface, and the length in the longitudinal direction of the second internal electrode layer is smaller than the maximum length in the longitudinal direction of the third external electrode arranged on a part of the first main surface and a part of the second main surface, and the fourth external electrode arranged on a part of the first main surface and a part of the second main surface.

[0008] In the multilayer ceramic capacitor according to the present invention, the number of first internal electrode layers is greater than the number of second internal electrode layers, and the first internal electrode layers are Without sandwiching a second internal electrode layer between layers Two or more sheets are stacked in succession The internal electrode laminate is As a result, not only is the number of first internal electrode layers increased and the number of first internal electrode layers connected in parallel increased while suppressing an increase in the capacitance of the multilayer ceramic capacitor, but also the conductivity between the first internal electrode layers and the external electrodes is improved, thereby suppressing an increase in DC resistance. Furthermore, in the multilayer ceramic capacitor according to the present invention, the recess is formed so that the first internal electrode layer does not overlap with the third external electrode arranged on a part of the first main surface and a part of the second main surface, and the fourth external electrode arranged on a part of the first main surface and a part of the second main surface, when the multilayer ceramic capacitor is viewed from the height direction. Therefore, even if a high electric field is applied to the multilayer ceramic capacitor according to the present invention, dielectric breakdown can be suppressed between the third external electrode and the fourth external electrode connected to the second internal electrode layer, and the first internal electrode layer. Furthermore, in the multilayer ceramic capacitor according to the present invention, the second internal electrode layer is disposed at least between the first internal electrode layer located closest to the first main surface and the first main surface, and at least between the first internal electrode layer located closest to the second main surface and the second main surface, so that the current path to the mounting board can be shortened, a low ESL effect can be obtained, and even when a high electric field is applied to the multilayer ceramic capacitor according to the present invention, dielectric breakdown can be suppressed between the first internal electrode layer and the third and fourth external electrodes connected to the second internal electrode layer, resulting in an improvement in the dielectric breakdown voltage (BDV) of the multilayer ceramic capacitor. Furthermore, in the multilayer ceramic capacitor according to the present invention, the longitudinal length of the second internal electrode layer is smaller than the maximum longitudinal length of the third external electrode arranged on a portion of the first main surface and a portion of the second main surface and the fourth external electrode arranged on a portion of the first main surface and a portion of the second main surface, thereby enabling a lower capacitance to be achieved while maintaining a reduced DC resistance. Effect of the Invention

[0009] According to the present invention, it is possible to provide a multilayer ceramic capacitor that enables the capacitance of the capacitor to be reduced while suppressing dielectric breakdown that occurs between the internal electrode layers and the external electrodes even when a high electric field is applied.

[0010] The above and other objects, features and advantages of the present invention will become more apparent from the following detailed description of the preferred embodiments of the present invention, which proceeds with reference to the accompanying drawings. [Brief description of the drawings]

[0011] [Figure 1] 1 is an external perspective view showing an example of a multilayer ceramic capacitor (three-terminal type multilayer ceramic capacitor) according to an embodiment of the present invention. [Diagram 2]FIG. 1A is a top view showing an example of a multilayer ceramic capacitor (three-terminal multilayer ceramic capacitor) according to an embodiment of the present invention, and FIG. 1B is a perspective view of each internal electrode layer as seen from the top view shown in FIG. [Diagram 3] 1 is a side view showing an example of a multilayer ceramic capacitor (three-terminal multilayer ceramic capacitor) according to an embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. [Diagram 5] 2 is a cross-sectional view taken along line VV in FIG. 1. [Figure 6] 6 is a cross-sectional view taken along line VI-VI in FIG. [Figure 7] FIG. 7 is a cross-sectional view taken along line VII-VII in FIG. [Figure 8] 1. FIG. 5 is a cross-sectional view corresponding to FIG. 4, showing a modified example of the multilayer ceramic capacitor shown in FIG. [Figure 9] 1. FIG. 6 is a cross-sectional view corresponding to FIG. 5, showing a modified example of the multilayer ceramic capacitor shown in FIG. [Figure 10] FIG. 2(a) is an LT cross-sectional view showing an example of a multilayer ceramic capacitor according to Comparative Example 1 and Comparative Example 2, and FIG. 2(b) is a WT cross-sectional view thereof. [Figure 11] 10(a) is a cross-sectional view taken along line XIa-XIa in FIG. 10(a), and FIG. 10(b) is a cross-sectional view taken along line XIb-XIb in FIG. 10(a). [Figure 12] 5(a) is a cross-sectional view corresponding to FIG. 4 and showing an example of a multilayer ceramic capacitor according to Comparative Example 3 and Comparative Example 4, and FIG. 5(b) is a cross-sectional view corresponding to FIG. [Figure 13] FIG. 11 is a schematic cross-sectional view showing an example of a method for measuring the thickness of a dielectric layer. [Figure 14] FIG. 13 is a diagram showing the relationship between element thickness and breakdown voltage in each sample of an example and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] 1. Multilayer ceramic capacitors DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A multilayer ceramic capacitor according to an embodiment of the present invention will be described. The multilayer ceramic capacitor according to the embodiment is a three-terminal multilayer ceramic capacitor.

[0013] FIG. 1 is an external perspective view showing an example of a multilayer ceramic capacitor (three-terminal type multilayer ceramic capacitor) according to an embodiment of the present invention. FIG. 2(a) is a top view showing an example of a multilayer ceramic capacitor (three-terminal type multilayer ceramic capacitor) according to an embodiment of the present invention, and FIG. 2(b) is a perspective view of each internal electrode layer as seen from the top view shown in (a). FIG. 3 is a side view showing an example of a multilayer ceramic capacitor (three-terminal type multilayer ceramic capacitor) according to an embodiment of the present invention. FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. 1. FIG. 5 is a cross-sectional view taken along line VV in FIG. 1. FIG. 6 is a cross-sectional view taken along line VI-VI in FIG. 4. FIG. 7 is a cross-sectional view taken along line VII-VII in FIG. 4.

[0014] As shown in FIGS. 1 to 3, the multilayer ceramic capacitor 10 includes a laminate 12 having a substantially rectangular parallelepiped shape, and external electrodes 30, for example.

[0015] The laminate 12 has a plurality of laminated dielectric layers 14 and a plurality of internal electrode layers 16 laminated on the dielectric layers 14. Furthermore, the laminate 12 has a first main surface 12a and a second main surface 12b facing in a height direction x, a first side surface 12c and a second side surface 12d facing in a width direction y perpendicular to the height direction x, and a first end surface 12e and a second end surface 12f facing in a length direction z perpendicular to the height direction x and the width direction y.

[0016] It should be noted that the L dimension in the length direction z of the laminate 12 is not necessarily longer than the W dimension in the width direction y.

[0017] The external electrodes 30 are disposed on the first end face 12e side, the second end face 12f side, the first side face 12c side, and the second side face 12d side of the laminate 12. The external electrodes 30 include a first external electrode 30a, a second external electrode 30b, a third external electrode 30c, and a fourth external electrode 30d. Details of the first external electrode 30a, the second external electrode 30b, the third external electrode 30c, and the fourth external electrode 30d will be described later.

[0018] The corners and ridges of this laminate 12 are rounded. The corners are the parts where three adjacent faces of the laminate intersect, and the ridges are the parts where two adjacent faces of the laminate intersect. In addition, unevenness may be formed on part or all of the first main surface 12a and the second main surface 12b, the first side surface 12c and the second side surface 12d, and the first end surface 12e and the second end surface 12f.

[0019] The dimensions of the laminate 12 are not particularly limited.

[0020] The laminate 12 has an inner layer portion 18, and a first outer layer portion 20a and a second outer layer portion 20b arranged so as to sandwich the inner layer portion 18 in the height direction x.

[0021] The inner layer portion 18 includes a plurality of dielectric layers 14 and a plurality of internal electrode layers 16. The inner layer portion 18 includes the internal electrode layer 16 located closest to the first principal surface 12a in the height direction x to the internal electrode layer 16 located closest to the second principal surface 12b.

[0022] The first main surface side outer layer portion 20a is located on the first main surface 12a side. The first main surface side outer layer portion 20a is an assembly of multiple dielectric layers 14 located between the first main surface 12a and the internal electrode layer 16 closest to the first main surface 12a. The second main surface side outer layer portion 20b is located on the second main surface 12b side. The second main surface side outer layer portion 20b is an assembly of a plurality of dielectric layers 14 located between the second main surface 12b and the internal electrode layer 16 closest to the second main surface 12b. The dielectric layer 14 used in the first outer layer portion 20a and the second outer layer portion 20b may be the same as the dielectric layer 14 used in the inner layer portion 18.

[0023] The laminate 12 has a first side outer layer portion 22a located on the first side 12c side and formed from a plurality of dielectric layers 14 located between the first side 12c and the outermost surface of the inner layer portion 18 on the first side 12c side. Similarly, the laminate 12 has a second side outer layer portion 22b located on the second side 12d side and formed from a plurality of dielectric layers 14 located between the second side 12d and the outermost surface of the inner layer portion 18 on the second side 12d side. 5 shows the range of the first side surface side outer layer portion 22a and the second side surface side outer layer portion 22b in the width direction y. The size of the width of the first side surface side outer layer portion 22a and the second side surface side outer layer portion 22b in the width direction y is also called the W gap or side gap.

[0024] The dielectric layer 14 can be formed of a dielectric material, for example, a ceramic material. As such a dielectric material, for example, a dielectric ceramic containing a component such as BaTiO3, CaTiO3, SrTiO3, or CaZrO3 can be used. When the dielectric material is contained as a main component, a subcomponent such as a Mn compound, an Fe compound, a Cr compound, a Co compound, or a Ni compound may be added in a smaller amount than the main component depending on the desired characteristics of the laminate 12.

[0025] The thickness of the dielectric layer 14 after firing is preferably 30 μm or more and 80 μm or less. The number of dielectric layers 14 to be laminated is preferably 15 or more and 300 or less. Note that this number of dielectric layers 14 is the total number of the dielectric layers 14 in the inner layer portion 18 and the dielectric layers 14 in the first main surface side outer layer portion 20a and the second main surface side outer layer portion 20b.

[0026] The inner layer electrode portion 16 has, as the multiple internal electrode layers 16, a multiple number of first internal electrode layers 16a and a multiple number of second internal electrode layers 16b.

[0027] The first internal electrode layer 16 a is disposed on the dielectric layer 14 . As shown in FIG. 6, the first internal electrode layer 16a extends between the first end 12e and the second end 12f of the laminate 12 and has a first region 26a at its center, a second region 26b extending from the first region 26a and drawn to the first end face 12e of the laminate 12, and a third region 26c extending from the first region 26a and drawn to the second end face 12f of the laminate 12. The first region 26a is located at the center on the dielectric layer 14. The second region 26b is exposed to the first end face 12e of the laminate 12, and the third region 26c is exposed to the second end face 12f of the laminate 12. Therefore, the first internal electrode layer 16a is not exposed to the first side face 12c and the second side face 12d of the laminate 12. The shape of the first internal electrode layer 16a is not particularly limited, but is preferably rectangular, although the corners may be rounded.

[0028] When the multilayer ceramic capacitor 10 is viewed from the height direction x, as shown in FIG. 2(b), the first internal electrode layer 16a has a recess 29a formed therein so as not to overlap with the third external electrode 30c disposed on a part of the first principal surface 12a and a part of the second principal surface 12b, and a recess 29b formed therein so as not to overlap with the fourth external electrode 30d disposed on a part of the first principal surface 12a and a part of the second principal surface 12b. More specifically, in the first region 26a of the first internal electrode layer 16a, on the first side surface 12c side, there is a recess 29a which is an area where the internal electrode layer 16 is not formed, and on the second side surface 12d side, there is a recess 29b which is an area where the internal electrode layer 16 is not formed. As a result, even if a high electric field is applied to the multilayer ceramic capacitor 10, dielectric breakdown can be suppressed between the first internal electrode layer 16a and the third external electrode 30c and the fourth external electrode 30d connected to the second internal electrode layer 16b.

[0029] The shape of the recess 29a is not particularly limited as long as it does not overlap with the third external electrode 30c disposed on a portion of the first principal surface 12a and the second principal surface 12b when the multilayer ceramic capacitor 10 is viewed from the height direction x. Similarly, the shape of the recess 29b is not particularly limited as long as it does not overlap with the fourth external electrode 30d arranged on a portion of the first principal surface 12a and the second principal surface 12b when the multilayer ceramic capacitor 10 is viewed from the height direction x. In this embodiment, the recesses 29a and 29b are semicircular in shape.

[0030] The second internal electrode layer 16b is disposed on a dielectric layer 14 different from the dielectric layer 14 on which the first internal electrode layer 16a is disposed. As shown in FIG. 7, the second internal electrode layer 16b extends between the first side surface 12c and the second side surface 12d of the laminate 12 and has a fourth region 28a at its center, a fifth region 28b extending from the fourth region 28a and drawn to the first side surface 12c, and a sixth region 28c extending from the fourth region 28a and drawn to the second side surface 12d. The fourth region 28a is located at the center on the dielectric layer 14. The fifth region 28b is exposed to the first side surface 12c of the laminate 12, and the sixth region 28c is exposed to the second side surface 12d of the laminate 12. Therefore, the second internal electrode layer 16b is not exposed to the first end surface 12e and the second end surface 12f of the laminate 12. The shapes of the fourth region 28a, the fifth region 28b and the sixth region 28c of the second internal electrode layer 16b are not particularly limited, but are preferably rectangular, although the corners of each region may be rounded.

[0031] The second internal electrode layer 16b is arranged at least between the first internal electrode layer 16a located closest to the first main surface 12a and the first main surface 12a, and at least between the first internal electrode layer 16a located closest to the second main surface 12b and the second main surface 12b. This makes it possible to shorten the current path to the mounting board, obtain a low ESL (equivalent series resistance) effect, and suppress dielectric breakdown between the first internal electrode layer 16a and the third external electrode 30c and the fourth external electrode 30d connected to the second internal electrode layer 16b, even when a high electric field is applied to the multilayer ceramic capacitor 10. As a result, the dielectric breakdown voltage (BDV) of the multilayer ceramic capacitor 10 can be improved.

[0032] The length in the longitudinal direction z of the second internal electrode layer 16b is smaller than the maximum length in the longitudinal direction z of the third external electrode 30c arranged on a portion of the first main surface 12a and a portion of the second main surface 12b and the fourth external electrode 30d arranged on a portion of the first main surface 12a and a portion of the second main surface 12b. This allows for a lower capacitance while keeping the DC resistance low.

[0033] It is preferable that the fourth region 28a of the second internal electrode layer 16b does not extend in the direction of the first end face 12e or the direction of the second end face 12f, and that the width in the longitudinal direction z connecting the first end face 12e and the second end face 12f in the fourth region 28a of the second internal electrode layer 16b is the same as the width in the longitudinal direction z connecting the first end face 12e and the second end face 12f in the fifth region 28b and the sixth region 28c of the second internal electrode layer 16b. As a result, by adjusting only the area of ​​the second internal electrode layer 16b without changing the area of ​​the first internal electrode layer 16a, the capacitance of the multilayer ceramic capacitor 10 can be reduced while maintaining the DC resistance at a low level.

[0034] The first region 26a of the first internal electrode layer 16a and the fourth region 28a of the second internal electrode layer 16b face each other.

[0035] The number of the first internal electrode layers 16a is greater than the number of the second internal electrode layers 16b, and two or more first internal electrode layers 16a are laminated in succession. As a result, in the multilayer ceramic capacitor 10 shown in Fig. 1, not only is the number of first internal electrode layers 16a increased while suppressing an increase in capacitance, and the number of first internal electrode layers 16a connected in parallel is increased, but also the conductivity between the first internal electrode layers 16a and the external electrodes 30 is improved, making it possible to suppress an increase in DC resistance.

[0036] The inner layer portion 18 of the laminate 12 has a capacitance forming portion 19 where the first internal electrode layer 16a and the second internal electrode layer 16b face each other via the dielectric layer 14 to form a capacitance, and an internal electrode laminate portion 24 which is a region where two or more first internal electrode layers 16a are laminated in succession. The capacitance forming portion 19 is what allows the multilayer ceramic capacitor 10 to exhibit the characteristics of a capacitor.

[0037] In the multilayer ceramic capacitor 10 shown in Fig. 1, the second internal electrode layer 16b may be arranged so as to divide the internal electrode laminate portion 24, which is a region in which two or more first internal electrode layers 16a are continuously laminated, as shown in Fig. 8 and Fig. 9. In this case, the internal electrode laminate portion 24 is divided into a first internal electrode laminate portion 24a and a second internal electrode laminate portion 24b by one second internal electrode layer 16b. This disperses the aggregates of the first internal electrode layers 16a, improving the heat dissipation effect and providing the effect of suppressing a temperature rise.

[0038] Also, the second internal electrode layer 16b arranged so as to divide the internal electrode laminated portion 24, which is a region in which two or more first internal electrode layers 16a are continuously laminated, into a plurality of pieces may be arranged singly. This makes it possible to laminate more first internal electrode layers 16a, thereby obtaining the effect of reducing the DC resistance.

[0039] On the other hand, the second internal electrode layer 16b arranged so as to divide the internal electrode laminated portion 24, which is a region in which two or more first internal electrode layers 16a are laminated in succession, into a plurality of pieces may be arranged by laminating two or more layers in succession. This makes it possible to make the connectivity with the third external electrode 30c formed on the first side surface 12c and the fourth external electrode 30d formed on the second side surface 12d more sufficient even if the number of the second internal electrode layers 16b is reduced.

[0040] The thickness of the dielectric layer 14 located between the first internal electrode layer 16a and the second internal electrode layer 16b is preferably 30 μm or more, so that the effect of the present invention can be exhibited in a more prominent region.

[0041] The thickness of the dielectric layer 14 located between the first internal electrode layer 16a and the second internal electrode layer 16b is preferably greater than the thickness of the dielectric layer 14 located between the first internal electrode layers 16a. This makes it possible to stack more first internal electrode layers 16a, thereby making it possible to further increase the effect of reducing DC resistance.

[0042] When the multilayer ceramic capacitor 10 is viewed from the height direction x, the distance on the same plane between an end side of the third external electrode 30c arranged on a part of the first main surface 12a and a part of the second main surface 12b and a fourth external electrode 30d arranged on a part of the first main surface 12a and a part of the second main surface 12b and an end side of the recess 29a of the first internal electrode layer 16a, and the distance on the same plane between an end side of the third external electrode 30c arranged on a part of the first main surface 12a and a part of the second main surface 12b and a fourth external electrode 30d arranged on a part of the first main surface 12a and a part of the second main surface 12b and an end side of the recess 29b of the first internal electrode layer 16a are preferably at least 100 μm. This makes it possible to more significantly suppress dielectric breakdown between the first internal electrode layer 16a and the third external electrode 30c and the fourth external electrode 30d connected to the second internal electrode layer 16b, even when a high electric field is applied.

[0043] In the first internal electrode layer 16a, the shortest distance in the width direction y between the recesses 29a and 29b is shorter than the shortest distance in the width direction y of a portion of the first internal electrode layer 16a where the recesses 29a and 29b are not formed. This makes it possible to more significantly suppress dielectric breakdown between the first internal electrode layer 16a and the third external electrode 30c and the fourth external electrode 30d connected to the second internal electrode layer 16b, even when a high electric field is applied.

[0044] The total number of the first internal electrode layers 16a and the second internal electrode layers 16b is preferably 15 or more and 200 or less. The number of the first internal electrode layers 16a is not particularly limited, but is preferably, for example, 50 or more and 100 or less. The number of the second internal electrode layers 16b is at least less than the number of the first internal electrode layers 16a. Specifically, the number of the second internal electrode layers 16b is not particularly limited, but is preferably, for example, 1 to 20.

[0045] The thickness of the first internal electrode layer 16a and the second internal electrode layer 16b is not particularly limited, but is preferably, for example, about 0.5 μm or more and 2.0 μm or less. The thickness of the fourth region 28a of the second internal electrode layer 16b is not particularly limited, but is preferably, for example, about 30 μm or more and 80 μm or less.

[0046] The first internal electrode layer 16a and the second internal electrode layer 16b can be made of an appropriate conductive material, such as a metal such as Ni, Cu, Ag, Pd, or Au, or an alloy containing at least one of these metals, such as an Ag-Pd alloy.

[0047] External electrodes 30 are arranged on the first end face 12e side, the second end face 12f side, the first side face 12c side, and the second side face 12d side of the laminate 12. The external electrodes 30 include a first external electrode 30a, a second external electrode 30b, a third external electrode 30c, and a fourth external electrode 30d.

[0048] A first external electrode 30a is disposed on the first end face 12e of the laminate 12. The first external electrode 30a is disposed so as to extend from the first end face 12e of the laminate 12 and cover a portion of each of the first main face 12a, the second main face 12b, the first side face 12c, and the second side face 12d. The first external electrode 30a is electrically connected to the second region 26b of the first internal electrode layer 16a exposed at the first end face 12e of the laminate 12. The first external electrode 30a may be disposed only on the first end face 12e of the laminate 12.

[0049] A second external electrode 30b is disposed on the second end face 12f of the laminate 12. The second external electrode 30b is disposed so as to extend from the second end face 12f of the laminate 12 and cover a portion of each of the first main face 12a, the second main face 12b, the first side face 12c, and the second side face 12d. The second external electrode 30b is electrically connected to the third region 26c of the first internal electrode layer 16a exposed at the second end face 12f of the laminate 12. The second external electrode 30b may be disposed only on the second end face 12f of the laminate 12.

[0050] A third external electrode 30c is disposed on the first side surface 12c of the laminate 12. The third external electrode 30c is disposed so as to extend from the first side surface 12c to cover a part of the first main surface 12a and the second main surface 12b. The third external electrode 30c is electrically connected to a fifth region 28b of the second internal electrode layer 16b exposed at the first side surface 12c of the laminate 12.

[0051] A fourth external electrode 30d is disposed on the second side surface 12d of the laminate 12. The fourth external electrode 30d is disposed so as to extend from the second side surface 12d and cover a part of the first main surface 12a and the second main surface 12b. The fourth external electrode 30d is electrically connected to a sixth region 28c of the second internal electrode layer 16b exposed at the second side surface 12d of the laminate 12.

[0052] The external electrode 30 includes a base electrode layer 32 disposed on the surface of the laminate 12 , and a plating layer 34 disposed so as to cover the base electrode layer 32 .

[0053] The base electrode layer 32 includes a first base electrode layer 32a, a second base electrode layer 32b, a third base electrode layer 32c, and a fourth base electrode layer 32d.

[0054] The first base electrode layer 32a is disposed on the surface of the first end face 12e of the laminate 12 and is formed so as to extend from the first end face 12e to cover a portion of each of the first main surface 12a, the second main surface 12b, the first side surface 12c, and the second side surface 12d. The second base electrode layer 32b is disposed on the surface of the second end face 12f of the laminate 12 and is formed so as to extend from the second end face 12f to cover a portion of each of the first main surface 12a, the second main surface 12b, the first side surface 12c, and the second side surface 12d. The first base electrode layer 32a may be arranged only on the surface of the first end face 12e of the laminate 12, and the second base electrode layer 32b may be arranged only on the surface of the second end face 12f of the laminate 12.

[0055] The third base electrode layer 32c is disposed on the surface of the first side surface 12c of the laminate 12, and is formed so as to extend from the first side surface 12c to cover a portion of each of the first main surface 12a and the second main surface 12b. The fourth base electrode layer 32d is disposed on the surface of the second side surface 12d of the laminate 12, and is formed so as to extend from the second side surface 12d to cover a portion of each of the first principal surface 12a and the second principal surface 12b.

[0056] The base electrode layer 32 includes at least one selected from a baked layer, a conductive resin layer, a thin film layer, and the like. Hereinafter, each of the configurations in which the base electrode layer 32 is the baked layer, the conductive resin layer, and the thin film layer will be described.

[0057] (For baked layers) The baking layer includes a glass component and a metal component. The glass component of the baking layer includes at least one selected from B, Si, Ba, Mg, Al, Li, etc. The metal component of the baking layer includes at least one selected from, for example, Cu, Ni, Ag, Pd, Ag-Pd alloy, Au, etc. The baking layer may be a multi-layered layer. The baking layer is formed by applying a conductive paste containing a glass component and a metal component to the laminate 12 and baking it. The baking layer may be formed by simultaneously baking a laminated chip having an internal electrode layer 16 and a dielectric layer 14 and a conductive paste applied to the laminated chip, or may be formed by baking a laminated chip having an internal electrode layer 16 and a dielectric layer 14 to obtain a laminate 12, and then applying a conductive paste to the laminate 12 and baking it. In addition, when the baking layer is formed by simultaneously baking a laminated chip having an internal electrode layer 16 and a dielectric layer 14 and a conductive paste applied to the laminated chip, it is preferable to form the baking layer by baking a layer to which a dielectric material has been added instead of the glass component.

[0058] The thickness of the first base electrode layer 32a located at the first end face 12e in the center in the height direction x, in the direction connecting the first end face 12e and the second end face 12f, is preferably about 3 μm or more and 70 μm or less. Furthermore, the thickness in the direction connecting the first end face 12e and the second end face 12f at the center in the height direction x of the second base electrode layer 32b located on the second end face 12f is preferably about 3 μm or more and 70 μm or less.

[0059] When the first base electrode layer 32a is provided on a part of the first main surface 12a and a part of the second main surface 12b, and a part of the first side surface 12c and a part of the second side surface 12d, the thickness in the height direction connecting the first main surface 12a and the second main surface 12b at the center in the longitudinal direction z of the first base electrode layer 32a located on the first main surface 12a and the second main surface 12b, the first side surface 12c and the second side surface 12d is preferably, for example, approximately 3 μm or more and 40 μm or less. Furthermore, when the second base electrode layer 32b is provided on a part of the first principal surface 12a and a part of the second principal surface 12b, and a part of the first side surface 12c and a part of the second side surface 12d, the thickness in the height direction connecting the first principal surface 12a and the second principal surface 12b at the center in the longitudinal direction z, which is the second base electrode layer 32b located on the first principal surface 12a and the second principal surface 12b, the first side surface 12c and the second side surface 12d, is preferably, for example, approximately 3 μm or more and 40 μm or less.

[0060] The thickness of the third base electrode layer 32c located on the first side surface 12c at the center in the height direction x in the direction connecting the first side surface 12c and the second side surface 12d is preferably about 3 μm or more and 70 μm or less. Furthermore, the thickness in the direction connecting the first side surface 12c and the second side surface 12d at the center in the height direction x of the fourth base electrode layer 32d located on the second side surface 12d is preferably about 3 μm or more and 70 μm or less.

[0061] (In the case of a conductive resin layer) The conductive resin layer may be a multi-layered layer. The conductive resin layer may be disposed on the baked layer so as to cover the baked layer, or may be disposed directly on the laminate 12 . The conductive resin layer includes a thermosetting resin and a metal. The conductive resin layer may completely cover the underlying electrode layer 32 or may cover only a portion of the underlying electrode layer 32 . Since the conductive resin layer contains a thermosetting resin, it is more flexible than a conductive layer made of, for example, a plating film or a fired conductive paste. Therefore, even if the multilayer ceramic capacitor 10 is subjected to a physical shock or a shock caused by a thermal cycle, the conductive resin layer functions as a buffer layer and can prevent the multilayer ceramic capacitor 10 from cracking.

[0062] The metal contained in the conductive resin layer may be Ag, Cu, Ni, Sn, Bi, or an alloy containing any of these. Metal powders whose surfaces are coated with Ag can also be used. When using metal powders whose surfaces are coated with Ag, it is preferable to use Cu, Ni, Sn, Bi or alloy powders thereof as the metal powder. The reason why Ag conductive metal powder is used as the conductive metal is that Ag has the lowest resistivity among metals and is therefore suitable as an electrode material, and Ag is a precious metal and therefore does not oxidize and has high weather resistance. In addition, it is possible to use a cheaper base metal while maintaining the above-mentioned properties of Ag.

[0063] Furthermore, as the metal contained in the conductive resin layer, Cu or Ni that has been subjected to an anti-oxidation treatment can also be used. The metal contained in the conductive resin layer may be a metal powder having a surface coated with Sn, Ni, or Cu. When using a metal powder having a surface coated with Sn, Ni, or Cu, it is preferable to use Ag, Cu, Ni, Sn, Bi, or an alloy powder thereof as the metal powder.

[0064] In the conductive resin layer, conductive fillers come into contact with each other, forming electrical paths within the conductive resin layer.

[0065] The metal contained in the conductive resin layer may be spherical or flat, but it is preferable to use a mixture of spherical metal powder and flat metal powder.

[0066] As the resin for the conductive resin layer, various known thermosetting resins such as epoxy resin, phenol resin, urethane resin, silicone resin, polyimide resin, etc., can be used. Among them, epoxy resin, which has excellent heat resistance, moisture resistance, adhesion, etc., is one of the most suitable resins.

[0067] In addition, the conductive resin layer preferably contains a curing agent together with the thermosetting resin. When an epoxy resin is used as the base resin, various known compounds such as phenol-based, amine-based, acid anhydride-based, imidazole-based, active ester-based, and amide-imide-based compounds can be used as the curing agent for the epoxy resin.

[0068] The thickness of the conductive resin layer located at the center in the height direction x of the laminate 12, which is located at the first end face 12e and the second end face 12f, is preferably, for example, about 10 μm or more and 150 μm or less.

[0069] (For thin layer) When a thin film layer is provided as the base electrode layer 32, the thin film layer is formed by a thin film forming method such as sputtering or vapor deposition, and is a layer of 1 μm or less in thickness in which metal particles are deposited.

[0070] The plating layer 34 includes a first plating layer 34a, a second plating layer 34b, a third plating layer 34c and a fourth plating layer 34d. The first plating layer 34a, the second plating layer 34b, the third plating layer 34c and the fourth plating layer 34d each contain at least one selected from, for example, Cu, Ni, Sn, Ag, Pd, an Ag-Pd alloy, Au and the like.

[0071] The first plating layer 34a is disposed so as to cover the first base electrode layer 32a. The second plating layer 34b is disposed so as to cover the second base electrode layer 32b. The third plating layer 34c is disposed so as to cover the third base electrode layer 32c. The fourth plating layer 34d is disposed so as to cover the fourth base electrode layer 32d.

[0072] The plating layer 34 may be formed of multiple layers. In this case, the plating layer 34 preferably has a two-layer structure including a lower plating layer formed by Ni plating on the base electrode layer 32 and an upper plating layer formed by Sn plating on the lower plating layer. That is, the first plating layer 34a has a first lower plating layer and a first upper plating layer located on the surface of the first lower plating layer. The second plating layer 34b has a second lower plating layer and a second upper plating layer located on the surface of the second lower plating layer. The third plating layer 34c has a third lower plating layer and a second upper plating layer located on the surface of the third lower plating layer. The fourth plating layer 34d has a fourth lower plating layer and a second upper plating layer located on the surface of the fourth lower plating layer.

[0073] The lower plating layer made of Ni plating is used to prevent the base electrode layer 32 from being eroded by solder when mounting the multilayer ceramic capacitor 10, and the upper plating layer made of Sn plating is used to improve the wettability of the solder when mounting the multilayer ceramic capacitor 10, making it easier to mount. The thickness of each plating layer is preferably 2.0 μm or more and 15.0 μm or less.

[0074] The external electrodes 30 may be formed only by plating layers without providing the base electrode layer 32 . Although not shown, a structure in which a plating layer is provided without providing a base electrode layer 32 will be described below.

[0075] Any one or each of the first external electrode 30a to the fourth external electrode 30d may not be provided with the base electrode layer 32, and the plating layer may be formed directly on the surface of the laminate 12. That is, the multilayer ceramic capacitor 10 may have a structure including a plating layer electrically connected to the first internal electrode layer 16a and the second internal electrode layer 16b. In such a case, the plating layer may be formed after a catalyst is disposed on the surface of the laminate 12 as a pretreatment.

[0076] In addition, when a plating layer is formed directly on the laminate 12 without providing the base electrode layer 32, the reduction in the thickness of the base electrode layer 32 can be converted into a lower height, i.e., a thinner body, or into the thickness of the laminate 12, i.e., the thickness of the inner layer portion 18, thereby improving the design freedom of the thin chip.

[0077] The plating layer preferably includes a lower-layer plating electrode formed on the surface of the laminate 12, and an upper-layer plating electrode formed on the surface of the lower-layer plating electrode. Each of the lower-layer plating electrode and the upper-layer plating electrode preferably includes at least one metal selected from, for example, Cu, Ni, Sn, Pb, Au, Ag, Pd, Bi, or Zn, or an alloy containing the metal. Furthermore, the lower layer plated electrode is preferably formed using Ni, which has solder barrier properties, and the upper layer plated electrode is preferably formed using Sn or Au, which has good solder wettability.

[0078] Also, for example, when the first internal electrode layer 16a and the second internal electrode layer 16b are formed using Ni, it is preferable that the lower-layer plating electrode is formed using Cu, which has good bonding properties with Ni. The upper-layer plating electrode may be formed as necessary, and each of the first external electrode 30a to the fourth external electrode 30d may be composed of only the lower-layer plating electrode. The plating layer may be formed such that the upper-layer plating electrode is the outermost layer, or other plating electrodes may be formed on the surface of the upper-layer plating electrode.

[0079] Here, when the external electrodes 30 are formed by plating layers alone without providing the base electrode layer 32, the thickness of each plating layer disposed without providing the base electrode layer 32 is preferably 1 μm or more and 15 μm or less.

[0080] Furthermore, it is preferable that the plating layer does not contain glass.The metal ratio per unit volume of the plating layer is preferably 99 volume % or more.

[0081] The dimension in the length direction z of the multilayer ceramic capacitor 10, including the laminate 12 and the first external electrode 30a to the fourth external electrode 30d, is defined as dimension L, the dimension in the height direction x of the multilayer ceramic capacitor 10, including the laminate 12 and the first external electrode 30a to the fourth external electrode 30d, is defined as dimension T, and the dimension in the width direction y of the multilayer ceramic capacitor 10, including the laminate 12 and the first external electrode 30a to the fourth external electrode 30d, is defined as dimension W. The dimensions of the multilayer ceramic capacitor 10 are not particularly limited, but the L dimension in the length direction z is 1.0 mm or more and 3.2 mm or less, the W dimension in the width direction y is 0.5 mm or more and 2.5 mm or less, and the T dimension in the height direction x is 0.3 mm or more and 2.5 mm or less. The dimensions of the multilayer ceramic capacitor 10 can be measured using a microscope.

[0082] 1, by virtue of the above configuration, it is possible to suppress dielectric breakdown between the first internal electrode layer 16a and the third external electrode 30c and the fourth external electrode 30d connected to the second internal electrode layer 16b, even when a high electric field is applied to the multilayer ceramic capacitor 10. As a result, it is possible to improve the dielectric breakdown voltage (BDV) of the multilayer ceramic capacitor 10.

[0083] 2. Manufacturing method of multilayer ceramic capacitors Next, a method for producing the multilayer ceramic capacitor according to the present invention will be described.

[0084] First, a dielectric sheet for the dielectric layer and a conductive paste for the internal electrode are prepared. The dielectric sheet and the conductive paste for the internal electrode layer contain a binder and a solvent. The binder and the solvent may be known.

[0085] A conductive paste for the internal electrode layers is printed in a predetermined pattern on the dielectric sheet by, for example, screen printing, gravure printing, etc. In this way, a dielectric sheet on which the pattern of the first internal electrode layer is formed, and a dielectric sheet on which the pattern of the second internal electrode layer is formed are prepared.

[0086] More specifically, a screen plate for printing the first internal electrode layer and a screen plate for printing the second internal electrode layer are prepared separately, and the patterns of each internal electrode layer can be printed using a printer capable of printing the two types of screen plates separately.

[0087] Here, in order to obtain a desired structure, sheets on which the first internal electrode layer and the second internal electrode layer are printed are laminated to form a portion that becomes the internal layer portion 18. At this time, the number of sheets on which the first internal electrode layer is printed is greater than the number of sheets on which the second internal electrode layer is printed, and two or more sheets on which the first internal electrode layer is printed are laminated in succession.

[0088] Next, a predetermined number of dielectric sheets on which the pattern of the internal electrode layer is not printed are laminated to form a portion that will become the second main surface side outer layer portion 20b on the second main surface side. After that, the portion that will become the internal layer portion 18 formed by the above-mentioned process is laminated on the portion that will become the second main surface side outer layer portion 20b, and a predetermined number of dielectric sheets on which the pattern of the internal electrode layer is not printed are laminated on the portion that will become the internal layer portion 18 to form a portion that will become the first main surface side outer layer portion 20a on the first main surface side. In this way, a laminated sheet is produced.

[0089] Next, the laminated sheets are pressed in the lamination direction by means of a hydrostatic press or the like to produce a laminated block.

[0090] Next, the laminated block is cut to a predetermined size to obtain laminated chips. At this time, corners and edges of the laminated chips may be rounded by barrel polishing or the like.

[0091] The cut-out laminated chip is then fired to produce the laminate 12. The firing temperature depends on the materials of the dielectric layers 14 and the internal electrode layers 16, but is preferably 900° C. or higher and 1400° C. or lower.

[0092] (base electrode layer) Subsequently, a third base electrode layer 32c of a third external electrode 30c is formed on a first side surface 12c of the laminate 12 obtained by firing, and a fourth base electrode layer 32d of a fourth external electrode 30d is formed on a second side surface 12d of the laminate 12. When forming a baked layer as the base electrode layer 32, a conductive paste containing a glass component and a metal component is applied, and then a baking process is performed to form a baked layer as the base electrode layer 32. The temperature of the baking process at this time is preferably 700°C or higher and 900°C or lower.

[0093] Here, various methods can be used to form the baked layer. For example, a method of applying conductive paste by extruding it through a slit can be used. In this method, by increasing the amount of conductive paste extruded, the base electrode layer 32 can be formed not only on the first side surface 12c and the second side surface 12d, but also on a part of the first main surface 12a and a part of the second main surface 12b. Alternatively, the base electrode 32 may be formed by using a roller transfer method. In the case of the roller transfer method, when the base electrode layer 32 is formed not only on the first side surface 12c and the second side surface 12d but also on a part of the first main surface 12a and a part of the second main surface 12b, the base electrode 32 can be formed on a part of the first main surface 12a and a part of the second main surface 12b by increasing the pressing pressure during the roller transfer.

[0094] Next, a first base electrode layer 32a of the first external electrode 30a is formed on a first end face 12e of the laminate 12 obtained by firing, and a second base electrode layer 32b of the second external electrode 30b is formed on a second end face 12f of the laminate 12. As in the case of forming the base electrode layer 32 of the third external electrode 30c and the fourth external electrode 30d, when forming a baked layer as the base electrode layer 32, a conductive paste containing a glass component and a metal component is applied, and then a baking process is performed to form a baked layer as the base electrode layer 32. The temperature of the baking process at this time is preferably 700°C or higher and 900°C or lower.

[0095] The baked layer serving as the base electrode layer 32 of the first external electrode 30a and the second external electrode 30b can be formed by a method of applying a conductive paste by extruding it through a slit or a roller transfer method.

[0096] Regarding the baking process, the third base electrode layer 32c of the third external electrode 30c, the fourth base electrode layer 32d of the fourth external electrode 30d, the first base electrode layer 32a of the first external electrode 30a, and the second base electrode layer 32b of the second external electrode 30b may be baked simultaneously, or the third base electrode layer 32c of the third external electrode 30c and the fourth base electrode layer 32d of the fourth external electrode 30d, and the first base electrode layer 32a of the first external electrode 30a and the second base electrode layer 32b of the second external electrode 30b may be baked separately.

[0097] (Conductive resin layer) When the base electrode layer 32 is formed of a conductive resin layer, the conductive resin layer can be formed by the following method. The conductive resin layer may be formed on the surface of a baked layer, or the conductive resin layer may be formed directly on the laminate 12 without forming a baked layer.

[0098] The conductive resin layer is formed by applying a conductive resin paste containing a thermosetting resin and a metal component onto the baking layer or the laminate 12, and then performing a heat treatment at a temperature of 250°C to 550°C to thermally cure the resin and form a conductive resin layer. The atmosphere during the heat treatment is preferably an N2 atmosphere. In addition, in order to prevent the resin from scattering and the oxidation of various metal components, it is preferable to suppress the oxygen concentration to 100 ppm or less.

[0099] The conductive resin paste can be applied in the same manner as the method for forming the base electrode layer 32 as a baked layer, for example, by a method of applying the conductive resin paste by extruding it through a slit or a roller transfer method.

[0100] (thin film layer) When the base electrode layer 32 is formed as a thin film layer, masking or the like is performed, and the base electrode layer can be formed by a thin film formation method such as sputtering or vapor deposition where the external electrode 30 is to be formed. The base electrode layer formed as a thin film layer is a layer of 1 μm or less in which metal particles are deposited.

[0101] (Plating electrode) Furthermore, plating electrodes may be provided in the second region 26a, the third region 26b, the fifth region 28b, and the sixth region 28c where the internal electrode layers 16 of the laminate 12 are exposed without providing the base electrode layer 32. In this case, they can be formed by the following method.

[0102] The first end face 12e and the second end face 12f of the laminate 12 are plated to form lower-layer plating electrodes on the second region 26b and the third region 26c, which are exposed portions of the first internal electrode layer 16a. Similarly, the first side face 12c and the second side face 12d of the laminate 12 are plated to form lower-layer plating electrodes on the fifth region 28b and the sixth region 28c, which are exposed portions of the second internal electrode layer 16b. Either electrolytic plating or electroless plating may be used for plating, but electroless plating has the disadvantage of requiring pretreatment with a catalyst or the like to improve the plating deposition rate, which complicates the process. Therefore, it is usually preferable to use electrolytic plating. As a plating method, it is preferable to use barrel plating. In addition, an upper-layer plating electrode formed on the surface of the lower-layer plating electrode may be formed in the same manner, if necessary.

[0103] Subsequently, as required, a plating layer 34 is formed on the surface of the base electrode layer 32, the surface of the conductive resin layer or the surface of the lower-layer plating electrode, or the surface of the upper-layer plating electrode. More specifically, in this embodiment, a Ni plating layer is formed as a lower plating layer on the base electrode layer 32, which is a baked layer, and a Sn plating layer is formed as an upper plating layer. The Ni plating layer and the Sn plating layer are formed successively, for example, by barrel plating. Either electrolytic plating or electroless plating may be used for plating. However, electroless plating has the disadvantage that pretreatment with a catalyst or the like is required to improve the plating deposition speed, which complicates the process. Therefore, it is usually preferable to use electrolytic plating.

[0104] In the manner described above, the multilayer ceramic capacitor 10 according to the present embodiment is manufactured.

[0105] 3. Experimental Example Next, in order to confirm the effect of the multilayer ceramic capacitor according to the present invention described above, a multilayer ceramic capacitor was manufactured as an experimental sample, and an experiment was carried out to measure the dielectric breakdown voltage (BDV) of the multilayer ceramic capacitor.

[0106] As examples, multilayer ceramic capacitors having internal structures as shown in Figures 4 to 9 were prepared, and as comparative examples, multilayer ceramic capacitors having no recesses in the first internal electrode layers as shown in Figures 10 to 12 were prepared. The examples and comparative examples were fabricated so that the capacitance, rated voltage, and thickness of the dielectric layers were the same.

[0107] (1) Specification of samples in the examples First, according to the above-mentioned method for producing a multilayer ceramic capacitor, multilayer ceramic capacitors according to Examples 1 to 4 having the following specifications were produced.

[0108] Example 1 · Structure of multilayer ceramic capacitor: 3 terminals (see Figure 1) · Multilayer ceramic capacitor dimensions L×W×T (including design values): 1.6mm×0.8mm×0.6mm Dielectric layer material: BaTiO3 Capacitance: 0.47nF Rated voltage: 100V Dielectric layer thickness: 23.3μm ·LT cross-section structure: see Figure 8 ·WT cross-sectional structure: see Figure 9 ·Internal electrode layer structure First internal electrode layer Material: Ni Shape: See Figure 6 Number of sheets: 65 Thickness: 1.0μm Second internal electrode layer Material: Ni Shape: See Figure 7 Number of sheets: 3 Thickness: 1.0μm External electrode structure A first external electrode and a second external electrode Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 45μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm Third and fourth external electrodes Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 30 μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm

[0109] Example 2 · Structure of multilayer ceramic capacitor: 3 terminals (see Figure 1) · Multilayer ceramic capacitor dimensions L×W×T (including design values): 1.6mm×0.8mm×0.6mm Dielectric layer material: BaTiO3 Capacitance: 0.33nF Rated voltage: 100V Dielectric layer thickness: 30.0μm ·LT cross-section structure: see Figure 8 ·WT cross-sectional structure: see Figure 9 ·Internal electrode layer structure First internal electrode layer Material: Ni Shape: See Figure 6 Number of sheets: 57 Thickness: 1.0μm Second internal electrode layer Material: Ni Shape: See Figure 7 Number of sheets: 3 Thickness: 1.0μm External electrode structure A first external electrode and a second external electrode Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 45μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm Third and fourth external electrodes Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 30 μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm

[0110] Example 3 · Structure of multilayer ceramic capacitor: 3 terminals (see Figure 1) · Multilayer ceramic capacitor dimensions L×W×T (including design values): 1.6mm×0.8mm×0.6mm Dielectric layer material: BaTiO3 Capacitance: 0.22nF Rated voltage: 100V Dielectric layer thickness: 37.7μm ·LT cross-section structure: see Figure 4 ·WT cross-sectional structure: see Figure 5 ·Internal electrode layer structure First internal electrode layer Material: Ni Shape: See Figure 6 Number of sheets: 70 Thickness: 1.0μm Second internal electrode layer Material: Ni Shape: See Figure 7 Number of sheets: 2 Thickness: 1.0μm External electrode structure A first external electrode and a second external electrode Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 45μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm Third and fourth external electrodes Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 30 μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm

[0111] Example 4 · Structure of multilayer ceramic capacitor: 3 terminals (see Figure 1) · Multilayer ceramic capacitor dimensions L×W×T (including design values): 1.6mm×0.8mm×0.6mm Dielectric layer material: BaTiO3 Capacitance: 0.10nF Rated voltage: 100V Dielectric layer thickness: 75.7μm ·LT cross-section structure: see Figure 4 ·WT cross-sectional structure: see Figure 5 ·Internal electrode layer structure First internal electrode layer Material: Ni Shape: See Figure 6 Number of sheets: 70 Thickness: 1.0μm Second internal electrode layer Material: Ni Shape: See Figure 7 Number of sheets: 2 Thickness: 1.0μm External electrode structure A first external electrode and a second external electrode Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 45μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm Third and fourth external electrodes Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 30 μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm

[0112] (2) Specifications of the samples in the comparative example Next, multilayer ceramic capacitors according to Comparative Examples 1 to 4 having the following specifications were fabricated.

[0113] The multilayer ceramic capacitors of Comparative Examples 1 and 2 are three-terminal multilayer ceramic capacitors identical to the multilayer ceramic capacitors of Examples 1 and 2, except that no recesses are formed in the first internal electrode layers, as compared with the multilayer ceramic capacitors of Examples 1 and 2. FIG. 10(a) is an LT cross-sectional view showing an example of a multilayer ceramic capacitor according to Comparative Example 1 and Comparative Example 2, and FIG. 10(b) is a WT cross-sectional view thereof. The multilayer ceramic capacitor 1A according to Comparative Example 1 and Comparative Example 2 has a rectangular parallelepiped laminate 2, external electrodes 3 arranged on both end faces thereof, and external electrodes 4 arranged on both side faces thereof. The laminate 2 has a plurality of laminated dielectric layers 5, and a plurality of first internal electrode layers 6a and second internal electrode layers 6b laminated on the dielectric layers 5. The second internal electrode layer 6b is arranged so as to divide the internal electrode laminated portion 7, which is a region in which two or more first internal electrode layers 6a are continuously laminated. At this time, the internal electrode laminated portion 7 is divided into a first internal electrode laminated portion 7a and a second internal electrode laminated portion 7b by one second internal electrode layer 6b. The detailed specifications are shown below.

[0114] Comparative Example 1 · Structure of multilayer ceramic capacitor: 3 terminals (see Figure 9) · Multilayer ceramic capacitor dimensions L×W×T (including design values): 1.6mm×0.8mm×0.6mm Dielectric layer material: BaTiO3 Capacitance: 0.47μF Rated voltage: 100V Dielectric layer thickness: 23.3μm · LT cross section structure: see Figure 10(a) ·WT cross-sectional structure: see Figure 10(b) ·Internal electrode layer structure First internal electrode layer Material: Ni Shape: See Figure 11(a) Number of sheets: 65 Thickness: 1.0μm Second internal electrode layer Material: Ni Shape: See Figure 11(b) Number of sheets: 3 Thickness: 1.0μm External electrode structure A first external electrode and a second external electrode Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 45μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm Third and fourth external electrodes Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 30 μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm

[0115] Comparative Example 2 · Structure of multilayer ceramic capacitor: 3 terminals (see Figure 9) · Multilayer ceramic capacitor dimensions L×W×T (including design values): 1.6mm×0.8mm×0.6mm Dielectric layer material: BaTiO3 Capacitance: 0.33μF Rated voltage: 100V Dielectric layer thickness: 30.0μm · LT cross section structure: see Figure 10(a) ·WT cross-sectional structure: see Figure 10(b) ·Internal electrode layer structure First internal electrode layer Material: Ni Shape: See Figure 11(a) Number of sheets: 57 Thickness: 1.0μm Second internal electrode layer Material: Ni Shape: See Figure 11(b) Number of sheets: 3 Thickness: 1.0μm External electrode structure A first external electrode and a second external electrode Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 45μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm Third and fourth external electrodes Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 30 μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm

[0116] The multilayer ceramic capacitors of Comparative Examples 3 and 4 are three-terminal multilayer ceramic capacitors identical to the multilayer ceramic capacitors of Examples 3 and 4, except that no recesses are formed in the first internal electrode layers, as compared with the multilayer ceramic capacitors of Examples 3 and 4. FIG. 12(a) is a cross-sectional view corresponding to FIG. 4 showing an example of a multilayer ceramic capacitor according to Comparative Example 3 and Comparative Example 4, and FIG. 12(b) is a cross-sectional view corresponding to FIG. 5. The multilayer ceramic capacitor 1B according to Comparative Example 2 has a rectangular parallelepiped laminate 2, external electrodes 3 arranged on both end faces thereof, and external electrodes 4 arranged on both side faces thereof. The laminate 2 has a plurality of laminated dielectric layers 5, and a plurality of first internal electrode layers 6a and second internal electrode layers 6b laminated on the dielectric layers 5. The number of the first internal electrode layers 6a is greater than the number of the second internal electrode layers 6b, and two or more first internal electrode layers 6a are laminated in succession. In the multilayer ceramic capacitor 1B shown in FIG. 12, the second internal electrode layer 6b is arranged between the first internal electrode layer 6a located closest to the first main surface side and the first main surface, and between the first internal electrode layer 6a located closest to the second main surface side and the second main surface. The internal electrode laminate portion 7 is not divided by the first internal electrode layer 6a. The detailed specifications are shown below.

[0117] Comparative Example 3 · Structure of multilayer ceramic capacitor: 3 terminals (see Figure 9) · Multilayer ceramic capacitor dimensions L×W×T (including design values): 1.6mm×0.8mm×0.6mm Dielectric layer material: BaTiO3 Capacitance: 0.22μF Rated voltage: 100V Dielectric layer thickness: 37.7μm · LT cross section structure: see Figure 12(a) ·WT cross-sectional structure: see Figure 12(b) ·Internal electrode layer structure First internal electrode layer Material: Ni Shape: See Figure 11(a) Number of sheets: 70 Thickness: 1.0μm Second internal electrode layer Material: Ni Shape: See Figure 11(b) Number of sheets: 2 Thickness: 1.0μm External electrode structure A first external electrode and a second external electrode Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 45μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm Third and fourth external electrodes Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 30 μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm

[0118] Comparative Example 4 · Structure of multilayer ceramic capacitor: 3 terminals (see Figure 9) · Multilayer ceramic capacitor dimensions L×W×T (including design values): 1.6mm×0.8mm×0.6mm Dielectric layer material: BaTiO3 Capacitance: 0.10μF Rated voltage: 100V Dielectric layer thickness: 75.7μm · LT cross section structure: see Figure 12(a) ·WT cross-sectional structure: see Figure 12(b) ·Internal electrode layer structure First internal electrode layer Material: Ni Shape: See Figure 11(a) Number of sheets: 70 Thickness: 1.0μm Second internal electrode layer Material: Ni Shape: See Figure 11(b) Number of sheets: 2 Thickness: 1.0μm External electrode structure A first external electrode and a second external electrode Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 45μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm Third and fourth external electrodes Base electrode layer: A fired layer containing conductive metal (Cu) and glass components Thickness at the center of the end face: 30 μm Plating layer: Two-layer structure of Ni plating layer and Sn plating layer Ni plating layer thickness: 4μm Sn plating layer thickness: 4μm

[0119] (3) Capacitance measurement method The capacitance was measured using a capacitance measuring instrument (LCR meter) under measurement conditions based on the standard (JIS C 5101-1:2010).

[0120] (4) Measurement method for the thickness of the dielectric layer For the samples according to each of the examples and comparative examples, the thickness of the dielectric layer was measured as follows. That is, first, the sample multilayer ceramic capacitor was surrounded by resin. At this time, the LT side of each sample multilayer ceramic capacitor was exposed. The LT side is the length and height side, and is the side on which the internal electrode layer, including the connection part to the external electrode, is exposed by polishing. The LT side was polished with a polisher, finishing at a depth of 1 / 2 in the width direction y of the laminate, exposing the LT cross section. Ion milling was performed on this polished surface to remove sagging caused by polishing, and a cross section for observation was obtained. Next, as shown in Figure 13, a perpendicular line perpendicular to the internal electrode layer was drawn at 1 / 2 the position in the longitudinal direction z of the LT cross section. Next, the region where the internal electrode layers of the sample were laminated (internal electrode laminated portion) was divided into three equal parts in the height direction x, and divided into three regions: an upper part U, a middle part M, and a lower part D. Then, five dielectric layers were selected from the center of each region in the height direction x, and the thicknesses of these dielectric layers on the perpendicular line were measured. As a result, the thicknesses of the dielectric layers and internal electrode layers were measured at a total of 15 locations (3 regions x 5 layers) for each sample, and the average value was calculated. The thickness of the dielectric layer was measured using a scanning electron microscope.

[0121] (5) Measurement method for dielectric breakdown voltage In the multilayer ceramic capacitors as samples according to the examples and comparative examples, wiring was connected from a DC power source to the first and second external electrodes, a voltage was applied between the first and second internal electrode layers, and the breakdown voltage was measured. The voltage was increased at a rate of 50 V / s, and the detection current was 83 mA.

[0122] As experimental results, the measurement results of the dielectric breakdown voltage are shown in Table 1 and FIG.

[0123] [Table 1]

[0124] (6) Experimental results According to Table 1 and FIG. 14, in the structures of Comparative Examples 1 to 4, when a high electric field is applied, dielectric breakdown may occur between the third external electrode and the fourth external electrode arranged on a part of the first principal surface and a part of the second principal surface and between the first internal electrode layer and the third external electrode and the fourth external electrode arranged on a part of the first principal surface and between the third external electrode and the fourth external electrode and between the fourth external electrode and the first internal electrode layer. From Comparative Example 1 to Comparative Example 4, a phenomenon occurred in which the dielectric layer becomes thicker, but the breakdown voltage (BDV) does not increase significantly.

[0125] On the other hand, in the structures of the present invention of Examples 1 to 4, the results showed that as the thickness of the dielectric layer increased from Example 1 to Example 4, the dielectric breakdown voltage (BDV) of the multilayer ceramic capacitor increased significantly.

[0126] From the above, it has been shown that the structure of the multilayer ceramic capacitor sample according to the embodiment can suppress the dielectric breakdown between the third and fourth external electrodes connected to the second internal electrode layer and the first internal electrode layer, and as a result, it has become clear that the dielectric breakdown voltage (BDV) of the multilayer ceramic capacitor can be improved.

[0127] As described above, the embodiment of the present invention has been disclosed in the above description, but the present invention is not limited thereto. In other words, various modifications can be made to the above-described embodiments in terms of mechanism, shape, material, quantity, position, arrangement, etc. without departing from the scope of the technical idea and purpose of the present invention, and these are included in the present invention. [Explanation of symbols]

[0128] 10 Multilayer ceramic capacitors 12 Laminate 12a First main surface 12b Second main surface 12c First aspect 12d. Second Aspect 12e First end face 12f Second end face 14 Dielectric layer 16 Internal electrode layer 16a First internal electrode layer 16b Second internal electrode layer 18 Inner Layer 19 Capacity forming part 20a: First main surface side outer layer portion 20b Second main surface side outer layer portion 22a First side outer layer 22b Second side outer layer 24 Internal electrode laminate 24a First internal electrode laminate 24b Second internal electrode laminate 26a First Area 26b Second Area Section 26c Third Area 28a Fourth Area 28b Fifth Zone 28c Sixth Area 29a, 29b Recess 30 External electrode 30a First external electrode 30b Second external electrode 30c Third external electrode 30d Fourth external electrode 32 Base electrode layer 32a First base electrode layer 32b Second base electrode layer 32c Third base electrode layer 32d Fourth base electrode layer 34 Plating layer 34a First plating layer 34b Second plating layer 34c Third plating layer 34d Fourth plating layer x Height direction y Width direction z Length direction

Claims

1. a laminate having a plurality of laminated dielectric layers, the laminate having a first main surface and a second main surface opposed to each other in a height direction, a first end surface and a second end surface opposed to each other in a length direction perpendicular to the height direction, and a first side surface and a second side surface opposed to each other in a width direction perpendicular to the height direction and the length direction; a plurality of first internal electrode layers disposed on the plurality of dielectric layers and extending to the first end surface and the second end surface; a plurality of second internal electrode layers disposed on the plurality of dielectric layers and extending to the first side surface and the second side surface; a first external electrode disposed on the first end face and connected to the first internal electrode layer; a second external electrode disposed on the second end face and connected to the first internal electrode layer; a third external electrode disposed on the first side surface, extending from the first side surface to a portion of the first main surface and a portion of the second main surface, and connected to the second internal electrode layer; a fourth external electrode disposed on the second side surface, extending from the second side surface to a portion of the first main surface and a portion of the second main surface, and connected to the second internal electrode layer; A multilayer ceramic capacitor comprising: the number of the first internal electrode layers is greater than the number of the second internal electrode layers, and the first internal electrode layers are provided as an internal electrode laminate portion in which two or more first internal electrode layers are continuously laminated without sandwiching the second internal electrode layers between the layers; a recess is formed in the first internal electrode layer so as not to overlap with the third external electrode disposed on a part of the first main surface and a part of the second main surface and the fourth external electrode disposed on a part of the first main surface and a part of the second main surface when the multilayer ceramic capacitor is viewed from the height direction; the second internal electrode layer is disposed at least between the first internal electrode layer located closest to the first main surface and the first main surface, and at least between the first internal electrode layer located closest to the second main surface and the second main surface, a length in the longitudinal direction of the second internal electrode layer is smaller than a maximum length in the longitudinal direction of the third external electrode arranged on a portion of the first main surface and a portion of the second main surface and the fourth external electrode arranged on a portion of the first main surface and a portion of the second main surface.

2. the second internal electrode layer extends between the first side surface and the second side surface of the laminate, and has a region located in a central portion of the dielectric layer, and a region extending from the region located in the central portion of the dielectric layer to the first side surface and the second side surface, 2. The multilayer ceramic capacitor according to claim 1, wherein a length in a longitudinal direction connecting the first end face and the second end face of a region located in a central portion of the dielectric layer is the same as a length in a longitudinal direction connecting the first end face and the second end face of the extended region.

3. 3. The multilayer ceramic capacitor according to claim 1, wherein the second internal electrode layer is arranged so as to divide an area provided as the internal electrode laminate portion into a plurality of parts.

4. 4. The multilayer ceramic capacitor according to claim 3, wherein the second internal electrode layer, which is arranged so as to divide the region provided as the internal electrode laminate portion into a plurality of portions, is arranged as a single layer.

5. 4. The multilayer ceramic capacitor according to claim 3, wherein the second internal electrode layer, which is disposed so as to divide the region provided as the internal electrode laminate portion into a plurality of parts, is formed by laminating two or more sheets of the second internal electrode layer in succession.

6. 6. The multilayer ceramic capacitor according to claim 1, wherein a thickness of a dielectric layer located between the first internal electrode layer and the second internal electrode layer is greater than a thickness of a dielectric layer located between the first internal electrode layers.

7. 7. The multilayer ceramic capacitor according to claim 1, wherein the dielectric layer located between the first internal electrode layer and the second internal electrode layer has a thickness of 30 [mu]m or more.

8. 8. The multilayer ceramic capacitor according to claim 1, wherein a shortest distance in the width direction of the first internal electrode layer in a portion where the recess is formed is shorter than a shortest distance of the first internal electrode layer in a portion where the recess is not formed.

Citation Information

Patent Citations

  • JP1990082022U

  • Multilayer capacitor

    JP2011049490A

  • Feedthrough capacitor, and mounting structure for the same

    JP2012104736A