tire

By incorporating nylon 56 with biomass-derived monomers in the tire's belt cover layer, the use of petroleum-derived materials is reduced, enhancing high-speed durability and tire uniformity through controlled shrinkage and rigidity retention.

JP7560772B2Active Publication Date: 2024-10-03THE YOKOHAMA RUBBER CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023005681
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-01-18
Publication Date
2024-10-03
Estimated Expiration
2043-01-18

AI Technical Summary

Technical Problem

The need to reduce the use of petroleum-derived raw materials and minimize environmental burden in tire production, particularly in the belt cover layer, which is typically made of nylon 66.

Method used

Using nylon 56, which contains biomass-derived monomers, specifically 50% or more of 1,5 pentanediamine, in the organic fiber cords of the tire's belt cover layer, ensuring a tensile stiffness retention rate of 90% or more and a dry heat shrinkage rate of 3.5% or less, and maintaining a twist coefficient between 1050 to 1750.

Benefits of technology

This approach reduces the use of petroleum-derived materials, enhances high-speed durability by maintaining tensile rigidity, and prevents excessive shrinkage, thereby improving tire uniformity and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560772000004
    Figure 0007560772000004
  • Figure 0007560772000005
    Figure 0007560772000005
  • Figure 0007560772000006
    Figure 0007560772000006
Patent Text Reader

Abstract

To provide a tire capable of reducing a load to an environment by reducing a used amount of a raw material derived from petroleum.SOLUTION: In a tire having an organic fiber cord C in a tire constitution member, at least one yarn Y of the organic fiber cord C is constituted of nylon 56 including a raw material derived from biomass in a monomer. Or in the tire having at least one organic fiber filament in the tire constitution member, at least one organic fiber filament is constituted of nylon 56 including the raw material derived from the biomass in the monomer.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tire having organic fiber filaments or organic fiber cords in tire constituent members, and more specifically, to a tire that enables a reduction in the amount of petroleum-derived raw materials used and a reduction in the burden on the environment. [Background technology]

[0002] For example, in a pneumatic tire, a carcass layer is installed between a pair of bead portions, and multiple belt layers including belt cords inclined with respect to the tire circumferential direction are arranged on the outer peripheral side of the carcass layer in the tread portion, and a belt cover layer including organic fiber cords oriented in the tire circumferential direction is arranged on the outer peripheral side of the belt layers (for example, see Patent Document 1).

[0003] The belt cover layer suppresses the rising of the belt layer during high-speed running, and contributes to improving high-speed durability. Nylon 66 fiber cords are generally used as the organic fiber cords for the belt cover layer. Thus, nylon 66 is widely recognized as a tire constituent material in the tire industry.

[0004] However, with growing environmental awareness around the world, there is a demand to reduce the use of petroleum-derived raw materials and to reduce the burden on the environment, and therefore there is a need for biomass-derived materials that can be used as an alternative to nylon 66. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6456784 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a tire which makes it possible to reduce the amount of petroleum-derived raw materials used and reduce the burden on the environment. [Means for solving the problem]

[0008] the above In order to achieve the object, the tire of the present invention has an organic fiber cord in which one to three yarns are twisted together as a tire component, and at least one yarn of the organic fiber cord is made of nylon 56 containing a biomass-derived raw material as a monomer. 、 50% by weight or more of the 1,5-pentanediamine, which is a monomer of the nylon 56, is derived from biomass, The tire component is a belt cover layer, The organic fiber cord has a tensile stiffness retention rate, which is a ratio of the initial tensile stiffness at 80°C to the initial tensile stiffness at 20°C, of ​​90% or more, and a dry heat shrinkage rate of 3.5% or less. It is characterized by the above. Effect of the Invention

[0009] As a result of extensive research into tire constituent materials, the inventors discovered that nylon 56 containing biomass-derived raw materials as monomers is an effective substitute for nylon 66, and that such nylon 56 can be used at a practical level as a tire constituent material, which led to the present invention.

[0010] That is, in the present invention 、 In a tire having an organic fiber cord among its tire components, at least one yarn of the organic fiber cord is made of nylon 56, which contains biomass-derived raw materials as monomers, thereby reducing the amount of petroleum-derived raw materials such as nylon 66 used and mitigating the burden on the environment.

[0011] In the present invention, it is preferable that 50% by weight or more of 1,5-pentanediamine, which is a monomer of nylon 56, is derived from biomass, which makes it possible to fully enjoy the effect of reducing the amount of petroleum-derived raw materials used.

[0012] In the present invention, the tire constituent member is preferably a belt cover layer. Since nylon 66 is generally used for the belt cover layer, the amount of petroleum-derived raw materials used can be reduced by replacing nylon 66 with nylon 56 containing biomass-derived raw materials as monomers.

[0013] The organic fiber cord used in the belt cover layer preferably has a tensile stiffness retention rate of 90% or more, which is the ratio of the initial tensile stiffness at 80°C to the initial tensile stiffness at 20°C, and a dry heat shrinkage rate of 3.5% or less. Nylon 56 has the characteristic of low temperature dependency of tensile stiffness. By making use of such a characteristic of nylon 56, the organic fiber cord used in the belt cover layer has a tensile stiffness retention rate of 90% or more, so that sufficient tensile stiffness can be secured even during high-speed running, and high-speed durability can be improved. In addition, the organic fiber cord used in the belt cover layer has a dry heat shrinkage rate of 3.5% or less, so that excessive shrinkage of the belt cover layer can be suppressed, and the tire uniformity can be maintained well.

[0014] In addition, it is preferable that the final twist coefficient K, represented by the following formula (1), of the organic fiber cord used in the belt cover layer is in the range of 1050 to 1750. This can effectively improve high-speed durability. K = T√D (1) Here, T is the number of twists (turns / 10 cm) of the organic fiber cord, and D is the total fineness (dtex) of the organic fiber cord.

[0015] The tire of the present invention is preferably a pneumatic tire, but may be a non-pneumatic tire. In the case of a pneumatic tire, the inside of the tire can be filled with air, an inert gas such as nitrogen, or other gases. [Brief description of the drawings]

[0016] [Figure 1] 1 is a meridian cross-sectional view showing a pneumatic tire according to an embodiment of the present invention. [Diagram 2]2 is a development view showing a belt layer and a belt cover layer of the pneumatic tire of FIG. 1. FIG. [Diagram 3] 5(a) to 5(c) are cross-sectional views showing organic fiber cords constituting a belt cover layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings, in which: Fig. 1 shows a pneumatic tire according to an embodiment of the present invention.

[0018] As shown in FIG. 1, the pneumatic tire of this embodiment includes a tread portion 1 extending circumferentially around the tire to form an annular shape, a pair of sidewall portions 2, 2 arranged on either side of the tread portion 1, and a pair of bead portions 3, 3 arranged radially inward of the sidewall portions 2.

[0019] A carcass layer 4 is mounted between a pair of bead portions 3, 3. This carcass layer 4 includes a plurality of carcass cords extending in the tire radial direction, and is folded back from the inside to the outside of the tire around a bead core 5 disposed in each bead portion 3. As the carcass cords of the carcass layer 4, organic fiber cords such as rayon fiber cords or polyester fiber cords are preferably used. A bead filler 6 made of a rubber composition having a triangular cross section is disposed on the outer periphery of the bead core 5.

[0020] On the other hand, a plurality of belt layers 7 are embedded on the outer peripheral side of the carcass layer 4 in the tread portion 1. These belt layers 7 include a plurality of belt cords inclined with respect to the tire circumferential direction, and are arranged so that the belt cords cross each other between layers. In the belt layers 7, the inclination angle of the belt cords with respect to the tire circumferential direction is set in the range of 10° to 40°, for example. As the belt cords of the belt layers 7, steel cords are preferably used.

[0021] A belt cover layer 8 is arranged on the outer periphery of the belt layer 7, in which organic fiber cords C are arranged at an angle of, for example, 5° or less with respect to the tire circumferential direction, for the purpose of improving high-speed durability. The belt cover layer 8 may be a full cover layer that covers the entire width of the belt layer 7, or a pair of edge cover layers that locally cover both ends of the belt layer 7 in the tire width direction, either alone or in combination. The belt cover layer 8 may be formed, for example, as shown in FIG. 2, by spirally winding a strip material 10 in the tire circumferential direction, in which at least one organic fiber cord C is aligned and covered with a coating rubber.

[0022] It should be noted that the above-described tire internal structure shows a typical example of a pneumatic tire, but is not limited thereto.

[0023] In the above-mentioned pneumatic tire, as shown in Fig. 3(a) to (c), the organic fiber cord C constituting the belt cover layer 8 has a structure in which one to three yarns Y are twisted together. At least one yarn Y of the organic fiber cord C is made of nylon 56 containing a biomass-derived raw material as a monomer. Each yarn Y is preferably made of one thick organic fiber filament or several hundred thin organic fiber filaments, and all the organic fiber filaments are made of nylon 56 containing a biomass-derived raw material as a monomer, but at least one organic fiber filament may be made of nylon 56 containing a biomass-derived raw material as a monomer.

[0024] In this way, in a tire having an organic fiber cord C among its tire constituent members, at least one yarn Y of the organic fiber cord C or its organic fiber filament is made of nylon 56 containing a biomass-derived raw material as a monomer, thereby reducing the amount of petroleum-derived raw materials such as nylon 66 used and mitigating the burden on the environment.

[0025] Nylon 56 is made by reacting 1,5-pentanediamine (C5H 14 N2) and adipic acid (CH10 O4) (n is an integer). While adipic acid is a petroleum-derived raw material, 1,5-pentanediamine can be produced, for example, by fermenting glucose obtained from corn. If a biomass-derived raw material (1,5-pentanediamine) is used as the raw material for nylon 56, the amount of petroleum-derived raw materials used can be reduced.

[0026] [ka]

[0027] In the above tire, it is preferable that 50% by weight or more of 1,5 pentanediamine, which is a monomer of nylon 56, is derived from biomass. This makes it possible to fully enjoy the effect of reducing the amount of petroleum-derived raw materials used. For example, if the entire amount of 1,5 pentanediamine, which is a raw material of nylon 56, is derived from biomass, the unit molecular weight of nylon 56 is 208, and the unit molecular weight of 1,5 pentanediamine in nylon 56 is 100, so the biomass-derived raw material ratio of nylon 56 is 48% by weight (100 / 208 x 100%).

[0028] Table 1 below shows specific application examples 1 to 7. Table 1 shows the relationship between the biomass-derived raw material ratio of 1,5-pentanediamine, which is a raw material for nylon 56, the twist structure of the organic fiber cord, the number of yarns using biomass-derived raw materials, and the biomass-derived raw material ratio of the organic fiber cord, for an organic fiber cord made of nylon 56. Using biomass-derived raw materials for at least a portion of the yarn as in application examples 1 to 7 can contribute to reducing the amount of petroleum-derived raw materials used.

[0029] [Table 1]

[0030] In the above-mentioned pneumatic tire, it is preferable that the organic fiber cord C constituting the belt cover layer 8 has a tensile stiffness retention rate, which is the ratio of the initial tensile stiffness at 80°C to the initial tensile stiffness at 20°C, of ​​90% or more and a dry heat shrinkage rate of 3.5% or less.

[0031] As described above, the organic fiber cord C used in the belt cover layer 8 has a tensile stiffness retention rate, which is the ratio of the initial tensile stiffness at 80°C to the initial tensile stiffness at 20°C, of ​​90% or more, so that sufficient tensile stiffness can be ensured even during high-speed running, thereby improving high-speed durability.

[0032] Here, if the tensile stiffness retention rate, which is the ratio of the initial tensile stiffness at 80°C to the initial tensile stiffness at 20°C, is lower than 90%, the tensile stiffness of the belt cover layer 8 decreases during high-speed running, and the effect of improving high-speed durability decreases. The tensile stiffness retention rate is the percentage of the initial tensile stiffness at 80°C to the initial tensile stiffness at 20°C of the organic fiber cord C. The "initial tensile stiffness" is the slope in the range of 0N to 44.1N of the load-strain curve obtained when a tensile test is carried out under the conditions of a gripping distance of 250mm and a pulling speed of 300±20mm / min in accordance with JIS L1017 "Testing Method for Chemical Fiber Tire Cords".

[0033] In addition, since the dry heat shrinkage rate of the organic fiber cord C used in the belt cover layer 8 is 3.5% or less, excessive shrinkage of the belt cover layer 8 is suppressed, and the uniformity of the pneumatic tire can be well maintained.

[0034] Here, if the dry heat shrinkage rate of the organic fiber cord C used in the belt cover layer 8 is higher than 3.5%, the uniformity of the pneumatic tire will deteriorate due to excessive shrinkage of the belt cover layer 8. The "dry heat shrinkage rate" is the dry heat shrinkage rate (%) of a sample cord measured when heated under the conditions of a sample length of 500 mm and heating conditions of 150°C for 30 minutes in accordance with JIS L1017 "Test method for synthetic fiber tire cords."

[0035] In the above pneumatic tire, it is preferable that the organic fiber cord C used in the belt cover layer 8 has a final twist coefficient K, represented by the following formula (1), in the range of 1050 to 1750. This can effectively improve high-speed durability. K = T√D (1) Here, T is the number of twists (turns / 10 cm) of the organic fiber cord C, and D is the total fineness (dtex) of the organic fiber cord C.

[0036] Here, if the final twist coefficient K of the organic fiber cord C is smaller than 1050, the radial growth of the tire during high-speed running is small, but the high-speed durability is reduced due to deterioration in fatigue resistance of the organic fiber cord C. Conversely, if it is larger than 1750, the radial growth of the tire during high-speed running is large, so the high-speed durability is reduced.

[0037] The number of final twists T of the organic fiber cord C used in the belt cover layer 8 is preferably in the range of 20 times / 10 cm to 40 times / 10 cm. Furthermore, the total fineness D of the organic fiber cord C is preferably in the range of 1800 dtex to 3000 dtex. On the premise of such number of final twists T and total fineness D, by setting the final twist coefficient K within the above range, high-speed durability can be effectively improved.

[0038] In the above-described embodiment, the case where nylon 56 containing a biomass-derived raw material as a monomer is used for the organic fiber cord C used in the belt cover layer has been described. However, in the present invention, nylon 56 containing a biomass-derived raw material as a monomer can be applied to organic fiber filaments or organic fiber cords included in various tire constituent members.

[0039] Examples of such tire components include a carcass layer, a belt layer, a side reinforcing layer, a chafer, a bead cover, and a bead fastening thread. In the case of a carcass layer, the present invention can be applied to a carcass cord. In the case of a belt layer, the present invention can be applied to a belt cord. In the case of a side reinforcing layer, the present invention can be applied to a reinforcing cord. In the case of a chafer, the present invention can be applied to a thread constituting the reinforcing cloth. A bead cover is a fabric material wound around a bead core made of a bead wire to bundle the bead core, and the present invention can be applied to a thread constituting the fabric material. A bead fastening thread is a thread wound around a bead core made of a bead wire to bundle the bead core, and the present invention can be applied to the thread. In either case, the present invention contributes to a reduction in the amount of petroleum-derived raw materials used. EXAMPLES

[0040] In a pneumatic tire having a tire size of 245 / 40R18 and including a tread portion, a pair of sidewall portions, and a pair of bead portions, a carcass layer is mounted between the pair of bead portions, multiple belt layers including belt cords inclined with respect to the tire circumferential direction are arranged on the outer circumferential side of the carcass layer in the tread portion, and a belt cover layer including organic fiber cords oriented in the tire circumferential direction is arranged on the outer circumferential side of the belt layer. Conventional tires and Examples 1 to 6 were manufactured with variously different specifications of the organic fiber cords in the belt cover layer.

[0041] As the organic fiber cord, the case where a nylon 66 fiber cord was used was indicated as "N66", and the case where a nylon 56 fiber cord was used was indicated as "N56". The nylon 56 fiber cord has a structure in which two yarns are twisted together, and the two yarns Y are composed of nylon 56 (biomass-derived raw material ratio = 48 wt%) containing biomass-derived raw materials as monomers. The fineness of the organic fiber cord, the number of final twists T, the final twist coefficient K, the initial tensile stiffness (0N to 44.1N) at 20°C and 80°C, the tensile stiffness retention rate, which is the ratio of the initial tensile stiffness at 80°C to the initial tensile stiffness at 20°C, and the dry heat shrinkage rate were set as shown in Table 2. The initial tensile stiffness at 20°C and 80°C was indicated as an index with the value of the initial tensile stiffness at 20°C of the conventional example set to 100.

[0042] The uniformity and high-speed durability of these test tires were evaluated by the following evaluation methods, and the results are shown in Table 2.

[0043] Uniformity: Each test tire was attached to a uniformity tester and the radial force variation (RFV) was measured. The evaluation results were expressed as an index using the reciprocal of the measured value, with the conventional example being set at 100. The higher the index value, the better the uniformity.

[0044] Fast durability: Each test tire was mounted on a wheel with a rim size of 18 x 7.0J, the air pressure was set to 220 kPa, and the tire was mounted on a drum testing machine with a smooth steel drum surface and a diameter of 1707 mm, and a running test was performed while controlling the ambient temperature at 38 ± 3 ° C. In the running test, the tire was run for 20 minutes under conditions of an initial speed of 120 km / h and a load of 88% of the maximum JATMA load, and when the running was completed, the speed was increased by 10 km / h and the tire was run for another 20 minutes. In this way, the speed increase and the running for 20 minutes were repeated without interruption, and the test was continued until the tire was destroyed, and the total running distance until destruction was measured. The evaluation results were shown as an index with the conventional example being 100. The higher the index value, the better the high-speed durability.

[0045] [Table 2]

[0046] As can be seen from Table 1, the tires of Examples 1 to 6 reached a sufficiently practical level in comparison with the conventional example using nylon 66 fiber cords. In particular, the tires of Examples 1 to 5 had improved high-speed durability while maintaining good uniformity. [Explanation of symbols]

[0047] 1 Tread section 2 Sidewall 3 Bead section 4 Carcass layer 5 Bead Core 6 Bead Filler 7 Belt layer 8 Belt cover layer 10 Strip material C Organic fiber cord Y Yarn

Claims

1. A tire having an organic fiber cord in which one to three yarns are twisted together in a tire component, at least one yarn of the organic fiber cord being made of nylon 56 containing a biomass-derived raw material as a monomer, 50% by weight or more of the 1,5-pentanediamine monomer of the nylon 56 is derived from biomass, The tire component is a belt cover layer, The organic fiber cord has a tensile stiffness retention rate, which is a ratio of the initial tensile stiffness at 80°C to the initial tensile stiffness at 20°C, of ​​90% or more, and a dry heat shrinkage rate of 3.5% or less.

2. The tire according to claim 1, characterized in that the organic fiber cord has a final twist coefficient K, represented by the following formula (1), in the range of 1,050 to 1,750. K=T√D...(1) Here, T is the number of twists (turns / 10 cm) of the organic fiber cord, and D is the total fineness (dtex) of the organic fiber cord.

Citation Information

Patent Citations

  • Heat energy storing material composition

    JP1989056784A

  • Fiber, rubber-reinforcing cord and reinforced rubber

    JP2009068132A

  • Pneumatic tire and method for manufacturing the same

    JP2017141002A

  • Pneumatic tire

    JP2017210096A