Water-absorbing resin particles
Water-absorbing resin particles with controlled gel flow and absorption properties effectively address the issue of liquid backflow in absorbent articles by maintaining absorption under load, improving their performance.
Patent Information
- Application Number
- JP2021504997
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-08
- Filing Date
- 2020-03-05
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2040-03-05
AI Technical Summary
Existing absorbent articles suffer from liquid backflow when a load is applied, such as from a wearer's weight, due to insufficient absorption performance.
The development of water-absorbing resin particles with a specific gel flow test force of 5 to 14 N, a physiological saline water retention amount of 30 to 60 g/g, and a 2-hour water absorption value of 15 ml/g under a 4.14 kPa load, achieved through controlled polymerization and crosslinking processes.
These properties significantly reduce the amount of liquid backflow in absorbent articles, enhancing their absorption capacity and maintaining liquid retention under pressure.
Smart Images

Figure 0007561117000002 
Figure 0007561117000003 
Figure 0007561117000004
Abstract
Description
[Technical field]
[0001] The present invention relates to water-absorbent resin particles. [Background technology]
[0002] Water-absorbent resins are used in the field of sanitary products, specifically as materials for absorbents contained in absorbent articles such as diapers (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2006-199805 A [Patent Document 2] International Publication No. 2006 / 123561 Summary of the Invention [Problem to be solved by the invention]
[0004] After the absorbent article has absorbed liquid, if a load is applied to the absorbent article due to the weight of the wearer or the like, the liquid that was once absorbed may flow back onto the surface of the absorbent article. If the absorbent article has insufficient absorption performance, the amount of flow back tends to be large.
[0005] An object of the present invention is to provide water-absorbent resin particles capable of reducing the amount of backflow in an absorbent article. [Means for solving the problem]
[0006] The present inventors have unexpectedly found that a higher outflow rate of the swollen gel reduces the amount of backflow in the absorbent article.
[0007] The water-absorbent resin particles of the present invention have a gel outflow test force of 5 to 14 N, as measured by the following method. Gel outflow test force measurement method: The water-absorbent resin particles are made to absorb physiological saline in an amount 29 times that of the water-absorbent resin particles under stirring to prepare a swollen gel. 20 g of the swollen gel is evenly placed in a cylinder with an inner diameter of 5 cm and a hole with a diameter of 5 mm at the bottom. The swollen gel in the cylinder is compressed at a speed of 10 mm / min using a tool with a diameter of 4.9 cm, and the test force at the time when a part of the swollen gel flows out from the hole at the bottom of the cylinder is recorded as the gel outflow test force.
[0008] The water-absorbent resin particles preferably have a saline water retention capacity of 30 to 60 g / g.
[0009] The water-absorbent resin particles preferably have a saline water absorption value of 15 ml / g or more for 2 hours under a load of 4.14 kPa.
[0010] The present invention also provides an absorbent body containing water-absorbent resin particles.
[0011] The present invention also provides an absorbent article comprising the above-mentioned absorbent body.
[0012] The absorbent article may be a diaper.
[0013] The present invention also provides a method for measuring a gel outflow test force, comprising: making a water-absorbent resin particle absorb physiological saline in an amount 29 times that of the water-absorbent resin particle under stirring to prepare a swollen gel; evenly placing 20 g of the swollen gel in a cylinder having an inner diameter of 5 cm and a hole having a diameter of 5 mm at the bottom; compressing the swollen gel in the cylinder at a speed of 10 mm / min using a tool having a diameter of 4.9 cm; and recording a test force at a time when a part of the swollen gel flows out from the hole at the bottom of the cylinder as a gel outflow test force.
[0014] The present invention also provides a method for producing water-absorbent resin particles, comprising selecting water-absorbent resin particles having a gel outflow test force of 5 to 14 N measured by the above-mentioned measuring method.
[0015] The present invention also provides a method for reducing the amount of backflow of an absorbent article, which comprises setting the gel outflow test force of the water-absorbent resin particles measured by the above-mentioned measuring method to 5 to 14 N. Effect of the Invention
[0016] The present invention provides water-absorbent resin particles capable of reducing the amount of backflow in absorbent articles. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a cross-sectional view showing an example of an absorbent article. [Diagram 2] FIG. 2 is a plan view showing the general shape of the stirring blade used in the examples. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing a measuring device for gel outflow test force. [Figure 4] 1 is a graph showing an example of gel outflow test force measurement results. [Diagram 5] FIG. 2 is a schematic diagram showing a measuring device for water absorption under load. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Preferred embodiments of the present invention will be described in detail below, however, the present invention is not limited to the following embodiments.
[0019] In this specification, "acrylic" and "methacrylic" are collectively referred to as "(meth)acrylic". "Acrylate" and "methacrylate" are similarly referred to as "(meth)acrylate". "(Poly)" refers to both the case where the "poly" prefix is present and the case where it is not present. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a certain numerical range can be arbitrarily combined with the upper limit or lower limit of the numerical range of another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the Examples. "Water-soluble" refers to a solubility of 5% by mass or more in water at 25°C. The materials exemplified in this specification may be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. In this specification, physiological saline refers to an aqueous solution of NaCl with a concentration of 0.9% by mass, unless otherwise specified.
[0020] The water-absorbent resin particles according to this embodiment have a gel outflow test force of 5 to 14 N, as measured by the following method. Gel outflow test force measurement method: Water-absorbent resin particles are made to absorb physiological saline in an amount 29 times that of the water-absorbent resin particles under stirring to prepare a swollen gel. 20 g of the swollen gel is evenly placed in a cylinder with an inner diameter of 5 cm and a hole with a diameter of 5 mm at the bottom. The swollen gel in the cylinder is compressed at a speed of 10 mm / min using a tool with a diameter of 4.9 cm, and the test force at the time when a part of the swollen gel flows out from the hole at the bottom of the cylinder is recorded as the gel outflow test force. A more specific measurement method will be shown in the examples below.
[0021] The water-absorbent resin particles according to the present embodiment may have a gel outflow test force of 13.5 N or less, 13 N or less, or 12.5 N or less. The gel outflow test force of the water-absorbent resin particles may be, for example, 6 N or more, 7 N or more, 8 N or more, or 10 N or more.
[0022] The water retention capacity of physiological saline of the water-absorbent resin particles according to the present embodiment is preferably in the following range. From the viewpoint of easily obtaining an excellent permeation rate in an absorbent article, the water retention capacity is preferably 30 g / g or more, 35 g / g or more, 40 g / g or more, 43 g / g or more, or 45 g / g or more. From the viewpoint of easily obtaining an excellent permeation rate in an absorbent article, the water retention capacity is preferably 80 g / g or less, 75 g / g or less, 70 g / g or less, 65 g / g or less, 60 g / g or less, 55 g / g or less, 52 g / g or less, or 50 g / g or less. From these viewpoints, the water retention capacity is preferably 30 to 80 g / g, and more preferably 40 to 65 g / g. The water retention capacity may be the water retention capacity at room temperature (25°C ± 2°C). The water retention capacity can be measured by the method described in the examples described later.
[0023] The two-hour value of physiological saline water absorption (water absorption under load) of the water absorbent resin particles according to the present embodiment under a load of 4.14 kPa may be, for example, 15 ml / g or more, 18 ml / g or more, or 20 ml / g or more. The physiological saline water absorption under a load of 4.14 kPa may be, for example, 35 ml / g or less, 30 ml / g or less, or 25 ml / g or less. The physiological saline water absorption under a load of 4.14 kPa is measured by the method described in the examples below.
[0024] The shape of the water-absorbent resin particles may be substantially spherical, crushed, granular, etc. The median particle size of the water-absorbent resin particles may be 250 to 850 μm, 300 to 700 μm, or 300 to 600 μm. The water-absorbent resin particles according to the present embodiment may have a desired particle size distribution at the time when the polymer particles are obtained by the production method described later, but the particle size distribution may be adjusted by performing an operation such as particle size adjustment using classification with a sieve.
[0025] The water-absorbent resin particles according to the present embodiment may include, for example, a crosslinked polymer formed by polymerization of a monomer including an ethylenically unsaturated monomer. The crosslinked polymer has a monomer unit derived from the ethylenically unsaturated monomer. That is, the water-absorbent resin particles according to the present embodiment may have a structural unit derived from the ethylenically unsaturated monomer.
[0026] The method of polymerizing the monomer includes reversed-phase suspension polymerization, aqueous solution polymerization, bulk polymerization, precipitation polymerization, etc. Among these, the reversed-phase suspension polymerization or aqueous solution polymerization is preferred from the viewpoint of ensuring good water absorption properties of the obtained water absorbent resin particles and easy control of the polymerization reaction. In the following, the reversed-phase suspension polymerization is taken as an example to explain the method of polymerizing the ethylenically unsaturated monomer.
[0027] The ethylenically unsaturated monomer is preferably water-soluble, and examples thereof include (meth)acrylic acid and its salts, 2-(meth)acrylamido-2-methylpropanesulfonic acid and its salts, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, N-methylol(meth)acrylamide, polyethylene glycol mono(meth)acrylate, N,N-diethylaminoethyl(meth)acrylate, N,N-diethylaminopropyl(meth)acrylate, and diethylaminopropyl(meth)acrylamide. When the ethylenically unsaturated monomer contains an amino group, the amino group may be quaternized. The functional groups of the above monomers, such as carboxyl groups and amino groups, can function as functional groups capable of crosslinking in the surface crosslinking step described below. These ethylenically unsaturated monomers may be used alone or in combination of two or more.
[0028] Among these, from the viewpoint of industrial availability, the ethylenically unsaturated monomer preferably contains at least one compound selected from the group consisting of (meth)acrylic acid and its salts, acrylamide, methacrylamide, and N,N-dimethylacrylamide, and more preferably contains at least one compound selected from the group consisting of (meth)acrylic acid and its salts, and acrylamide. From the viewpoint of further improving water absorption properties, the ethylenically unsaturated monomer further preferably contains at least one compound selected from the group consisting of (meth)acrylic acid and its salts.
[0029] As the monomer, a monomer other than the above ethylenically unsaturated monomer may be partially used. Such a monomer may be used by mixing with an aqueous solution containing the above ethylenically unsaturated monomer. The amount of the ethylenically unsaturated monomer used may be 70 to 100 mol%, 80 to 100 mol%, 90 to 100 mol%, 95 to 100 mol%, or 100 mol% based on the total amount of monomers (total amount of monomers for obtaining water absorbent resin particles. For example, total amount of monomers that provide structural units of a crosslinked polymer. The same applies below.). Among them, (meth)acrylic acid and salts thereof may be 70 to 100 mol%, 80 to 100 mol%, 90 to 100 mol%, 95 to 100 mol%, or 100 mol% based on the total amount of monomers. "Ratio of (meth)acrylic acid and salts thereof" means the ratio of the total amount of (meth)acrylic acid and salts thereof.
[0030] According to the present embodiment, as an example of the water-absorbent resin particles, it is possible to provide water-absorbent resin particles containing a crosslinked polymer having a structural unit derived from an ethylenically unsaturated monomer, the ethylenically unsaturated monomer containing at least one compound selected from the group consisting of (meth)acrylic acid and salts thereof, and the ratio of the (meth)acrylic acid and the salts thereof is 70 to 100 mol % based on the total amount of monomers for obtaining the water-absorbent resin particles.
[0031] The ethylenically unsaturated monomer is usually preferably used as an aqueous solution. The concentration of the ethylenically unsaturated monomer in the aqueous solution containing the ethylenically unsaturated monomer (hereinafter referred to as the aqueous monomer solution) is usually 20% by mass or more and saturation concentration or less, preferably 25 to 70% by mass, more preferably 30 to 55% by mass. Examples of the water used include tap water, distilled water, and ion-exchanged water.
[0032] When the ethylenically unsaturated monomer used contains an acid group, the aqueous monomer solution may be used after neutralizing the acid group with an alkaline neutralizing agent. The degree of neutralization of the ethylenically unsaturated monomer with the alkaline neutralizing agent is 10 to 100 mol %, preferably 50 to 90 mol %, and more preferably 60 to 80 mol % of the acid group in the ethylenically unsaturated monomer, from the viewpoint of increasing the osmotic pressure of the resulting water-absorbing resin particles and further improving the water-absorbing properties such as water retention. Examples of the alkaline neutralizing agent include alkali metal salts such as sodium hydroxide, sodium carbonate, sodium hydrogen carbonate, potassium hydroxide, and potassium carbonate; and ammonia. These alkaline neutralizing agents may be used in the form of an aqueous solution in order to simplify the neutralization operation. The above-mentioned alkaline neutralizing agents may be used alone or in combination of two or more kinds. The neutralization of the acid group of the ethylenically unsaturated monomer can be carried out, for example, by dropping an aqueous solution of sodium hydroxide, potassium hydroxide, or the like into the above-mentioned aqueous monomer solution and mixing.
[0033] In the reversed phase suspension polymerization method, an aqueous monomer solution is dispersed in a hydrocarbon dispersion medium in the presence of a surfactant, and an ethylenically unsaturated monomer is polymerized using a radical polymerization initiator or the like.
[0034] Examples of the surfactant include nonionic surfactants and anionic surfactants. Examples of the nonionic surfactant include sorbitan fatty acid esters, polyglycerin fatty acid esters, sucrose fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene glycerin fatty acid esters, sorbitol fatty acid esters, polyoxyethylene sorbitol fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene castor oil, polyoxyethylene hardened castor oil, alkylaryl formaldehyde condensed polyoxyethylene ethers, polyoxyethylene polyoxypropylene block copolymers, polyoxyethylene polyoxypropyl alkyl ethers, and polyethylene glycol fatty acid esters. Examples of the anionic surfactant include fatty acid salts, alkylbenzene sulfonates, alkylmethyl taurate salts, polyoxyethylene alkylphenyl ether sulfates, polyoxyethylene alkyl ether sulfonates, polyoxyethylene alkyl ether phosphates, and polyoxyethylene alkylaryl ether phosphates. Among these, from the viewpoints of obtaining a good W / O type reverse phase suspension state, easily obtaining water absorbent resin particles with a suitable particle size, and being easily available industrially, it is preferable that the surfactant contains at least one compound selected from the group consisting of sorbitan fatty acid esters, polyglycerin fatty acid esters, and sucrose fatty acid esters. Furthermore, from the viewpoint of improving the water absorption properties of the obtained water absorbent resin particles, it is more preferable that the surfactant contains a sucrose fatty acid ester. These surfactants may be used alone or in combination of two or more.
[0035] From the viewpoint of obtaining sufficient effect relative to the amount used and being economical, the amount of the surfactant is preferably 0.05 to 10 parts by mass, more preferably 0.08 to 5 parts by mass, and further preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the aqueous ethylenically unsaturated monomer solution.
[0036] In addition, a polymeric dispersant may be used together with the above-mentioned surfactant. Examples of the polymeric dispersant include maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-modified EPDM (ethylene-propylene-diene-terpolymer), maleic anhydride-modified polybutadiene, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, maleic anhydride-butadiene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, oxidized ethylene-propylene copolymer, ethylene-acrylic acid copolymer, ethyl cellulose, and ethylhydroxyethyl cellulose. Among these polymeric dispersants, it is particularly preferable to use maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, and oxidized ethylene-propylene copolymer, from the viewpoint of dispersion stability of the monomer. These polymeric dispersants may be used alone or in combination of two or more.
[0037] From the viewpoint of obtaining sufficient effect relative to the amount used and being economical, the amount of the polymer dispersant is preferably 0.05 to 10 parts by mass, more preferably 0.08 to 5 parts by mass, and further preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the aqueous ethylenically unsaturated monomer solution.
[0038] The radical polymerization initiator is preferably water-soluble, and examples thereof include persulfates such as potassium persulfate, ammonium persulfate, and sodium persulfate; peroxides such as methyl ethyl ketone peroxide, methyl isobutyl ketone peroxide, di-t-butyl peroxide, t-butyl cumyl peroxide, t-butyl peroxyacetate, t-butyl peroxyisobutyrate, t-butyl peroxypivalate, and hydrogen peroxide; 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(N-phenylamidino)propane] dihydrochloride, 2,2 Examples of the azo compounds include 2,2'-azobis[2-(N-allylamidino)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}dihydrochloride, 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], and 4,4'-azobis(4-cyanovaleric acid). These radical polymerization initiators may be used alone or in combination of two or more. Among these, potassium persulfate, ammonium persulfate, sodium persulfate, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, and 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride are preferred, and at least one azo compound selected from the group consisting of 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, and 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride is more preferred. The proportion of the azo compound is preferably from 20 to 100 mol %, more preferably from 35 to 90 mol %, and further preferably from 50 to 85 mol %, based on the total amount of the radical polymerization initiator.
[0039] The amount of the radical polymerization initiator used may be 0.00005 to 0.01 moles per mole of the ethylenically unsaturated monomer. When the amount of the radical polymerization initiator used is 0.00005 moles or more, the polymerization reaction does not take a long time and is efficient. When the amount used is 0.01 moles or less, the polymerization reaction tends not to occur abruptly.
[0040] The above radical polymerization initiators can also be used as redox polymerization initiators in combination with reducing agents such as sodium sulfite, sodium hydrogen sulfite, ferrous sulfate, and L-ascorbic acid.
[0041] In the polymerization reaction, the aqueous solution of the ethylenically unsaturated monomer used in the polymerization may contain a chain transfer agent. Examples of the chain transfer agent include hypophosphites, thiols, thiolic acids, secondary alcohols, and amines.
[0042] In addition, in order to control the particle size of the water-absorbent resin particles, a thickener may be contained in the ethylenically unsaturated monomer aqueous solution used for polymerization. As the thickener, for example, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, carboxymethyl cellulose, polyacrylic acid, polyacrylic acid (partially) neutralized product, polyethylene glycol, polyacrylamide, polyethyleneimine, dextrin, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, polyethylene oxide, etc. can be used. Note that, if the stirring speed during polymerization is the same, the higher the viscosity of the ethylenically unsaturated monomer aqueous solution, the larger the median particle size of the obtained particles tends to be.
[0043] Examples of the hydrocarbon dispersion medium include chain aliphatic hydrocarbons such as n-hexane, n-heptane, 2-methylhexane, 3-methylhexane, 2,3-dimethylpentane, 3-ethylpentane, and n-octane; alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, cyclopentane, methylcyclopentane, trans-1,2-dimethylcyclopentane, cis-1,3-dimethylcyclopentane, and trans-1,3-dimethylcyclopentane; and aromatic hydrocarbons such as benzene, toluene, and xylene. These hydrocarbon dispersion media may be used alone or in combination of two or more. The hydrocarbon dispersion medium may contain at least one compound selected from the group consisting of chain aliphatic hydrocarbons having 6 to 8 carbon atoms and alicyclic hydrocarbons having 6 to 8 carbon atoms. From the viewpoint of industrial availability and stable quality, the hydrocarbon dispersion medium may contain n-heptane, cyclohexane, or both of them. From the same viewpoint, for example, commercially available Exxolheptane (manufactured by ExxonMobil Corp.: containing 75 to 85% of n-heptane and isomeric hydrocarbons) may be used as the mixture of the hydrocarbon dispersion medium.
[0044] The amount of the hydrocarbon dispersion medium used is preferably 30 to 1000 parts by mass, more preferably 40 to 500 parts by mass, and even more preferably 50 to 300 parts by mass, relative to 100 parts by mass of the aqueous monomer solution, from the viewpoint of adequately removing the heat of polymerization and making it easy to control the polymerization temperature. When the amount of the hydrocarbon dispersion medium used is 30 parts by mass or more, the polymerization temperature tends to be easily controlled. When the amount of the hydrocarbon dispersion medium used is 1000 parts by mass or less, the polymerization productivity tends to be improved, which is economical.
[0045] Usually, internal crosslinking due to self-crosslinking may occur during polymerization, but the water absorption properties of the water-absorbing resin particles may be controlled by further applying internal crosslinking using an internal crosslinking agent. Examples of the internal crosslinking agent used include di- or tri(meth)acrylic acid esters of polyols such as ethylene glycol, propylene glycol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin; unsaturated polyesters obtained by reacting the above polyols with unsaturated acids such as maleic acid and fumaric acid; bis(meth)acrylamides such as N,N'-methylenebis(meth)acrylamide; di- or tri(meth)acrylic acid esters obtained by reacting polyepoxides with (meth)acrylic acid; di(meth)acrylic acid carbamyl esters obtained by reacting polyisocyanates such as tolylene diisocyanate and hexamethylene diisocyanate with hydroxyethyl (meth)acrylate. compounds having two or more polymerizable unsaturated groups, such as allylated starch, allylated cellulose, diallyl phthalate, N,N',N''-triallyl isocyanurate, and divinylbenzene; polyglycidyl compounds, such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and polyglycerol polyglycidyl ether; haloepoxy compounds, such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin; and isocyanate compounds, such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate, having two or more reactive functional groups. Among these internal crosslinking agents, it is preferable to use a polyglycidyl compound, more preferable to use a diglycidyl ether compound, and particularly preferable to use (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, or (poly)glycerin diglycidyl ether. These crosslinking agents may be used alone or in combination of two or more.
[0046] The amount of the internal crosslinking agent is preferably 0 to 0.03 mol, more preferably 0.00001 to 0.01 mol, and even more preferably 0.00002 to 0.005 mol per mol of the ethylenically unsaturated monomer, from the viewpoint of suppressing the water-soluble property by moderate crosslinking of the obtained polymer and exhibiting a sufficient water absorption amount.
[0047] An aqueous phase containing components such as an ethylenically unsaturated monomer, a radical polymerization initiator, and, if necessary, an internal crosslinking agent is mixed with an oil phase containing components such as a hydrocarbon-based dispersion medium, a surfactant, and, if necessary, a polymer-based dispersant, and the like, and the mixture is heated under stirring, whereby reversed-phase suspension polymerization can be carried out in a water-in-oil system.
[0048] When performing reversed-phase suspension polymerization, an aqueous monomer solution containing an ethylenically unsaturated monomer is dispersed in a hydrocarbon dispersion medium in the presence of a surfactant and, if necessary, a polymeric dispersant. In this case, the surfactant and the polymeric dispersant may be added either before or after the addition of the aqueous monomer solution, so long as they are added before the start of the polymerization reaction.
[0049] Among them, from the viewpoint of easily reducing the amount of the hydrocarbon dispersion medium remaining in the obtained water absorbent resin, it is preferable to disperse an aqueous monomer solution in a hydrocarbon dispersion medium having a polymeric dispersant dispersed therein, and then further disperse a surfactant therein, and then carry out polymerization.
[0050] Such reverse phase suspension polymerization can be carried out in one stage or in multiple stages of two or more stages, and is preferably carried out in two to three stages from the viewpoint of increasing productivity.
[0051] When performing reversed-phase suspension polymerization in two or more stages, after performing reversed-phase suspension polymerization in the first stage, an ethylenically unsaturated monomer is added to the reaction mixture obtained in the polymerization reaction in the first stage and mixed, and reversed-phase suspension polymerization in the second stage and thereafter may be performed in the same manner as in the first stage. In reversed-phase suspension polymerization in each stage after the second stage, in addition to the ethylenically unsaturated monomer, it is preferable to add the above-mentioned radical polymerization initiator and internal crosslinking agent within the range of the molar ratio of each component to the ethylenically unsaturated monomer as described above, based on the amount of the ethylenically unsaturated monomer added during reversed-phase suspension polymerization in each stage after the second stage, to perform reversed-phase suspension polymerization. Note that, in reversed-phase suspension polymerization in each stage after the second stage, an internal crosslinking agent may be used as necessary. When an internal crosslinking agent is used, it is preferable to add the above-mentioned radical polymerization initiator and internal crosslinking agent within the range of the molar ratio of each component to the ethylenically unsaturated monomer as based on the amount of the ethylenically unsaturated monomer to be used in each stage, to perform reversed-phase suspension polymerization.
[0052] The temperature of the polymerization reaction varies depending on the radical polymerization initiator used, but from the viewpoint of quickly progressing the polymerization and shortening the polymerization time to improve economic efficiency and easily removing the polymerization heat to smoothly carry out the reaction, the temperature is preferably 20 to 150°C, more preferably 40 to 120°C. The reaction time is usually 0.5 to 4 hours. The end of the polymerization reaction can be confirmed, for example, by the cessation of the temperature rise in the reaction system. As a result, the polymer of the ethylenically unsaturated monomer is usually obtained in the form of a hydrogel.
[0053] After the polymerization, a crosslinking agent may be added to the obtained hydrogel polymer and the polymer may be heated to perform post-polymerization crosslinking. By performing post-polymerization crosslinking, the degree of crosslinking of the hydrogel polymer can be increased, and the water absorption properties can be more favorably improved.
[0054] Examples of crosslinking agents for crosslinking after polymerization include polyols such as ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin; compounds having two or more epoxy groups such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, and (poly)glycerin diglycidyl ether; haloepoxy compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin; compounds having two or more isocyanate groups such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate; oxazoline compounds such as 1,2-ethylenebisoxazoline; carbonate compounds such as ethylene carbonate; and hydroxyalkylamide compounds such as bis[N,N-di(β-hydroxyethyl)]adipamide. Among these, preferred are polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, (poly)propylene glycol polyglycidyl ether, polyglycerol polyglycidyl ether, etc. These crosslinking agents may be used alone or in combination of two or more.
[0055] The amount of the crosslinking agent used in the post-polymerization crosslinking is preferably 0 to 0.03 mol, more preferably 0 to 0.01 mol, and even more preferably 0.00001 to 0.005 mol, per 1 mol of the ethylenically unsaturated monomer, from the viewpoint of allowing the resulting hydrous gel polymer to be appropriately crosslinked and thereby exhibiting favorable water absorption properties.
[0056] The timing of adding the post-polymerization crosslinking agent may be after the polymerization of the ethylenically unsaturated monomer used in the polymerization, and in the case of multi-stage polymerization, it is preferable to add it after the multi-stage polymerization. In addition, taking into consideration heat generation during and after polymerization, retention due to process delay, opening of the system when the crosslinking agent is added, and fluctuation in moisture due to addition of water accompanying the addition of the crosslinking agent, the crosslinking agent for post-polymerization crosslinking is preferably added in the region of [moisture content immediately after polymerization ±3% by mass] from the viewpoint of moisture content (described later).
[0057] Subsequently, the obtained hydrogel polymer is dried to remove water. By drying, polymer particles containing a polymer of an ethylenically unsaturated monomer are obtained. Examples of the drying method include (a) a method in which the hydrogel polymer is dispersed in a hydrocarbon dispersion medium and azeotropic distilled by heating from the outside, and the hydrocarbon dispersion medium is refluxed to remove water, (b) a method in which the hydrogel polymer is taken out by decantation and dried under reduced pressure, and (c) a method in which the hydrogel polymer is filtered through a filter and dried under reduced pressure. Among them, the method (a) is preferably used because of the simplicity of the production process.
[0058] The particle size of the water-absorbent resin particles can be controlled, for example, by adjusting the rotation speed of the agitator during the polymerization reaction, or by adding a powdered inorganic flocculant to the system after the polymerization reaction or at the beginning of drying. By adding the flocculant, the particle size of the obtained water-absorbent resin particles can be increased. Examples of the powdered inorganic flocculant include silica, zeolite, bentonite, aluminum oxide, talc, titanium dioxide, kaolin, clay, hydrotalcite, etc., and among them, silica, aluminum oxide, talc, or kaolin are preferred from the viewpoint of flocculation effect.
[0059] In the reversed-phase suspension polymerization, the method of adding the powdered inorganic flocculant is preferably a method in which the powdered inorganic flocculant is previously dispersed in the same type of hydrocarbon dispersion medium or water as that used in the polymerization, and then mixed into the hydrocarbon dispersion medium containing the hydrous gel under stirring.
[0060] In the production of the water-absorbent resin particles according to the present embodiment, it is preferable to crosslink (surface crosslink) the surface portion of the hydrogel polymer using a crosslinking agent in the drying step or any of the steps thereafter. The surface crosslinking is preferably performed at a timing when the hydrogel polymer has a specific water content. The timing of the surface crosslinking is preferably when the water content of the hydrogel polymer is 5 to 50% by mass, more preferably when it is 10 to 40% by mass, and even more preferably when it is 15 to 35% by mass.
[0061] The water content (mass%) of the hydrous gel polymer is calculated by the following formula. Moisture content=[Ww / (Ww+Ws)]×100 Ww: The water content of the hydrous gel polymer, calculated by subtracting the water content discharged outside the system in the drying process from the water content contained in the aqueous liquid before polymerization in all polymerization processes, plus the water content used as necessary when mixing a powdered inorganic flocculant, a surface crosslinking agent, etc. Ws: The solid content calculated from the amounts of the ethylenically unsaturated monomer, crosslinking agent, initiator, and other materials that constitute the hydrous gel polymer.
[0062] Examples of the surface cross-linking agent for performing surface cross-linking include compounds having two or more reactive functional groups. Examples of the surface cross-linking agent include polyols such as ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin; polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and (poly)glycerol polyglycidyl ether; epichlorohydrin, epibromohydrin, α-methylepichlorohydrin, Examples of the epoxy compounds include haloepoxy compounds such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate; oxetane compounds such as 3-methyl-3-oxetane methanol, 3-ethyl-3-oxetane methanol, 3-butyl-3-oxetane methanol, 3-methyl-3-oxetane ethanol, 3-ethyl-3-oxetane ethanol, and 3-butyl-3-oxetane ethanol; oxazoline compounds such as 1,2-ethylenebisoxazoline; carbonate compounds such as ethylene carbonate; and hydroxyalkylamide compounds such as bis[N,N-di(β-hydroxyethyl)]adipamide. Among these, polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and polyglycerol polyglycidyl ether are more preferred. These surface cross-linking agents may be used alone or in combination of two or more kinds.
[0063] The amount of the surface crosslinking agent is usually 0.00001 to 0.02 mol, preferably 0.00005 to 0.01 mol, and more preferably 0.0001 to 0.005 mol, relative to 1 mol of the ethylenically unsaturated monomer used in the polymerization, from the viewpoint of allowing the resulting hydrogel polymer to be appropriately crosslinked and thus exhibiting suitable water absorption properties.
[0064] From the viewpoint of sufficiently increasing the crosslinking density in the surface portion of the polymer particle and increasing the gel strength of the water-absorbent resin particle, the amount of the surface crosslinking agent used is preferably 0.00001 mol or more, and from the viewpoint of increasing the water retention capacity of the water-absorbent resin particle, the amount is preferably 0.02 mol or less.
[0065] After the surface cross-linking reaction, the water and the hydrocarbon dispersion medium are distilled off by a known method to obtain polymer particles which are a surface-cross-linked, dry product.
[0066] The polymerization reaction can be carried out using various stirrers having stirring blades. As the stirring blades, flat blades, lattice blades, paddle blades, propeller blades, anchor blades, turbine blades, Pfaudler blades, ribbon blades, full zone blades, Max Blend blades, etc. can be used. The flat blades have a shaft (stirring shaft) and a flat plate part (stirring part) arranged around the shaft. The flat plate part may have slits, etc. When flat blades are used as the stirring blades, the crosslinking reaction in the polymer particles is easily carried out uniformly, and the gel outflow test force is easily adjusted to a desired range suitable for the present invention while maintaining water absorption properties such as water retention.
[0067] The water-absorbent resin particles according to the present embodiment may be composed of only polymer particles, but may further contain various additional components selected from, for example, inorganic powders, surfactants, oxidizing agents, reducing agents, metal chelating agents, radical chain inhibitors, antioxidants, antibacterial agents, deodorants, gel stabilizers, flow improvers (lubricants), etc. The additional components may be disposed inside the polymer particles, on the surfaces of the polymer particles, or both.
[0068] The water-absorbent resin particles according to the present embodiment preferably contain inorganic particles. Examples of inorganic particles include silica particles such as amorphous silica. The amorphous silica may be hydrophilic amorphous silica. For example, the inorganic particles can be arranged on the surface of the polymer particles by mixing the polymer particles with the inorganic particles. The inorganic particles here usually have a minute size compared to the size of the polymer particles. For example, the average particle size of the inorganic particles may be 0.1 to 50 μm, 0.5 to 30 μm, or 1 to 20 μm. The average particle size here can be a value measured by a dynamic light scattering method or a laser diffraction / scattering method. When the amount of inorganic particles added is within the above range, water-absorbent resin particles having good water absorption properties can be easily obtained.
[0069] For example, the fluidity of the water-absorbent resin particles can be improved by adding 0.05 to 5 parts by mass of amorphous silica as inorganic particles to 100 parts by mass of the polymer particles. When the water-absorbent resin particles contain inorganic particles, the ratio of the inorganic particles to the mass of the polymer particles may be 0.05% by mass or more, 0.1% by mass or more, 0.2% by mass or more, 0.5% by mass or more, 1.0% by mass or more, or 1.5% by mass or more, or 5.0% by mass or less, 3.5% by mass or less, 1.5% by mass or less, 1.0% by mass or less, 0.8% by mass or less, 0.5% by mass or less, or 0.3% by mass or less.
[0070] The method for producing water-absorbent resin particles according to the present embodiment may include a step of selecting water-absorbent resin particles having a gel outflow test force of 5 to 14 N measured by the above-mentioned method. The above-mentioned production method may include a step of measuring the gel outflow test force. The properties of the water-absorbent resin particles to be selected may satisfy the above-mentioned aspects of the water-absorbent resin particles (for example, a specific range of physiological saline water retention capacity, a specific range of physiological saline water absorption capacity under a load of 4.14 kPa after 2 hours, etc.).
[0071] The water-absorbent resin particles according to the present embodiment have excellent absorbency of body fluids such as urine and blood, and can be applied to fields such as hygiene products such as paper diapers, sanitary napkins, and tampons, pet sheets, and animal excrement treatment materials such as dog or cat litter mixtures, for example.
[0072] The water-absorbent resin particles according to the present embodiment can be suitably used in an absorbent body. The absorbent body according to the present embodiment contains water-absorbent resin particles. The content of the water-absorbent resin particles in the absorbent body is set to 100 to 1000 g per square meter of the absorbent body (i.e., 100 to 1000 g / m2) from the viewpoint of obtaining sufficient liquid absorption performance when the absorbent body is used in an absorbent article. 2 ), and more preferably 150 to 800 g / m 2 , and more preferably 200 to 700 g / m 2 In order to ensure that the absorbent article exhibits sufficient liquid absorption performance and, in particular, to suppress liquid leakage, the content is set to 100 g / m 2 From the viewpoints of suppressing the occurrence of the gel blocking phenomenon, exhibiting the liquid diffusion performance as an absorbent article, and further improving the liquid permeation rate, the above content is preferably 1000 g / m 2 It is preferable that:
[0073] The absorbent may further include fibrous material in addition to the water-absorbent resin particles. The absorbent may be, for example, a mixture containing water-absorbent resin particles and fibrous material. The mass ratio of the water-absorbent resin particles in the absorbent may be 2% by mass to 100% by mass, preferably 10% by mass to 80% by mass, and more preferably 20% by mass to 70% by mass, based on the total of the water-absorbent resin particles and the fibrous material. The absorbent may be configured, for example, in a form in which the water-absorbent resin particles and the fibrous material are uniformly mixed, in a form in which the water-absorbent resin particles are sandwiched between fibrous material formed in a sheet or layer, or in other forms.
[0074] Examples of fibrous materials include pulverized wood pulp, cellulosic fibers such as cotton, cotton linters, rayon, cellulose acetate, etc., and synthetic fibers such as polyamides, polyesters, polyolefins, etc. The fibrous materials may also be mixtures of the above-mentioned fibers.
[0075] In order to improve the shape retention of the absorbent body before and during use, the fibers may be bonded together by adding an adhesive binder to the fibrous material. Examples of the adhesive binder include heat-fusible synthetic fibers, hot melt adhesives, adhesive emulsions, etc.
[0076] Examples of heat-fusible synthetic fibers include fully melted binders such as polyethylene, polypropylene, and ethylene-propylene copolymers, and non-fully melted binders consisting of a side-by-side or core-sheath structure of polypropylene and polyethylene. In the above-mentioned non-fully melted binders, only the polyethylene portion is heat-fused. Examples of hot melt adhesives include blends of base polymers such as ethylene-vinyl acetate copolymer, styrene-isoprene-styrene block copolymer, styrene-butadiene-styrene block copolymer, styrene-ethylene-butylene-styrene block copolymer, styrene-ethylene-propylene-styrene block copolymer, and amorphous polypropylene with tackifiers, plasticizers, antioxidants, and the like.
[0077] The adhesive emulsion may be, for example, a polymer of at least one monomer selected from the group consisting of methyl methacrylate, styrene, acrylonitrile, 2-ethylhexyl acrylate, butyl acrylate, butadiene, ethylene, and vinyl acetate. These adhesive binders may be used alone or in combination of two or more.
[0078] The absorbent according to the present embodiment may further contain additives such as inorganic powder (e.g., amorphous silica), deodorant, pigment, dye, antibacterial agent, fragrance, adhesive, etc. These additives can impart various functions to the absorbent. When the water-absorbent resin particles contain inorganic particles, the absorbent may contain inorganic powder in addition to the inorganic particles in the water-absorbent resin particles. Examples of inorganic powder include silicon dioxide, zeolite, kaolin, clay, etc.
[0079] The shape of the absorbent body according to this embodiment is not particularly limited, and may be, for example, a sheet-like shape. The thickness of the absorbent body (for example, the thickness of a sheet-like absorbent body) may be, for example, 0.1 to 20 mm, or 0.3 to 15 mm.
[0080] The absorbent article according to the present embodiment may include, in addition to the absorbent body, a core wrap, a liquid-permeable top sheet, and a liquid-impermeable back sheet. The core wrap maintains the shape of the absorbent body. The liquid-permeable top sheet is disposed on the outermost side of the side into which the liquid to be absorbed penetrates. The liquid-impermeable back sheet is disposed on the outermost side of the side opposite to the side into which the liquid to be absorbed penetrates.
[0081] Examples of absorbent articles include diapers (e.g., paper diapers), toilet training pants, incontinence pads, sanitary products (sanitary napkins, tampons, etc.), sweat pads, pet sheets, parts for simple toilets, and animal waste treatment materials.
[0082] Fig. 1 is a cross-sectional view showing an example of an absorbent article. The absorbent article 100 shown in Fig. 1 includes an absorbent body 10, core wraps 20a and 20b, a liquid-permeable top sheet 30, and a liquid-impermeable back sheet 40. In the absorbent article 100, the liquid-impermeable back sheet 40, the core wrap 20b, the absorbent body 10, the core wrap 20a, and the liquid-permeable top sheet 30 are laminated in this order. In Fig. 1, there are some parts shown as having gaps between the members, but the members may be in close contact with each other without the presence of such gaps.
[0083] The absorbent body 10 includes water-absorbent resin particles 10a and a fiber layer 10b containing fibrous material. The water-absorbent resin particles 10a are dispersed in the fiber layer 10b.
[0084] The core wrap 20a is disposed on one side of the absorbent body 10 (the upper side of the absorbent body 10 in FIG. 1) in contact with the absorbent body 10. The core wrap 20b is disposed on the other side of the absorbent body 10 (the lower side of the absorbent body 10 in FIG. 1) in contact with the absorbent body 10. The absorbent body 10 is disposed between the core wrap 20a and the core wrap 20b.
[0085] The core wrap 20a and the core wrap 20b have, for example, a main surface of the same size as the absorbent 10. By using the core wrap, the shape retention of the absorbent can be maintained and the water-absorbent resin particles constituting the absorbent can be prevented from falling off or flowing. Examples of the core wrap include nonwoven fabric, woven fabric, tissue, synthetic resin film having liquid-permeable holes, and net-like sheet having mesh, and from the viewpoint of economy, tissue obtained by wet molding pulp is preferably used.
[0086] The liquid permeable top sheet 30 is disposed on the outermost side of the absorbent article 100, on the side into which the liquid to be absorbed penetrates. The liquid permeable top sheet 30 is disposed on the core wrap 20a in contact with the core wrap 20a. The liquid impermeable back sheet 40 is disposed on the outermost side of the absorbent article 100, on the side opposite the liquid permeable top sheet 30. The liquid impermeable back sheet 40 is disposed below the core wrap 20b in contact with the core wrap 20b. The liquid permeable top sheet 30 and the liquid impermeable back sheet 40 have, for example, a main surface that is wider than the main surface of the absorbent body 10, and the outer edges of the liquid permeable top sheet 30 and the liquid impermeable back sheet 40 extend around the absorbent body 10 and the core wraps 20a and 20b.
[0087] Examples of the liquid permeable top sheet 30 include nonwoven fabrics, porous sheets, etc. Examples of nonwoven fabrics include thermal bonded nonwoven fabrics, air-through nonwoven fabrics, resin bonded nonwoven fabrics, spunbonded nonwoven fabrics, melt-blown nonwoven fabrics, spunbonded / melt-blown / spunbonded nonwoven fabrics, air-laid nonwoven fabrics, spunlace nonwoven fabrics, and point-bonded nonwoven fabrics. Of these, thermal bonded nonwoven fabrics, air-through nonwoven fabrics, spunbonded nonwoven fabrics, and spunbonded / melt-blown / spunbonded nonwoven fabrics are preferably used.
[0088] The material of the liquid permeable top sheet 30 may be a resin or fiber known in the art, and may include polyolefins such as polyethylene (PE) and polypropylene (PP), polyesters such as polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polyethylene naphthalate (PEN), polyamides such as nylon, rayon, other synthetic resins or fibers, cotton, silk, hemp, and pulp (cellulose) fibers, from the viewpoint of increasing the strength of the liquid permeable top sheet 30. As the material of the liquid permeable top sheet 30, synthetic fibers are preferably used, and polyolefins and polyesters are particularly preferable. These materials may be used alone or in combination of two or more materials.
[0089] From the viewpoint of improving the liquid absorption performance of the absorbent article, it is desirable that the nonwoven fabric used in the liquid permeable top sheet 30 has a suitable hydrophilicity. From this viewpoint, the hydrophilicity measured according to "Hydrophilicity of Nonwoven Fabrics" (based on Paper Pulp Test Method No. 68 (2000)) described in WO 2011 / 086843 is preferably 5 to 200, and more preferably 10 to 150. Such a hydrophilic nonwoven fabric may be one of the above-mentioned nonwoven fabrics that uses a material that itself exhibits a suitable hydrophilicity, such as rayon fiber, or one that uses hydrophobic chemical fibers, such as polyolefin fibers and polyester fibers, that have been hydrophilized by a known method to impart a suitable hydrophilicity.
[0090] Examples of methods for hydrophilizing chemical fibers include a method of mixing hydrophobic chemical fibers with a hydrophilizing agent and then subjecting the mixture to a spunbonding process to obtain a nonwoven fabric, a method of adding a hydrophilizing agent when preparing a spunbonded nonwoven fabric from hydrophobic chemical fibers, or a method of impregnating a spunbonded nonwoven fabric from hydrophobic chemical fibers with a hydrophilizing agent after obtaining the nonwoven fabric from hydrophobic chemical fibers. Examples of hydrophilizing agents include anionic surfactants such as aliphatic sulfonates and higher alcohol sulfate salts, cationic surfactants such as quaternary ammonium salts, nonionic surfactants such as polyethylene glycol fatty acid esters, polyglycerin fatty acid esters, and sorbitan fatty acid esters, silicone surfactants such as polyoxyalkylene-modified silicones, and stain release agents made of polyester, polyamide, acrylic, and urethane resins.
[0091] The nonwoven fabric used in the liquid-permeable top sheet 30 is preferably appropriately bulky and has a large basis weight, from the viewpoints of imparting good liquid permeability, flexibility, strength, and cushioning properties to the absorbent article, and of increasing the liquid permeation rate of the absorbent article. The basis weight of the nonwoven fabric is preferably 5 to 200 g / m 2 and more preferably 8 to 150 g / m 2 and more preferably 10 to 100 g / m 2 The thickness of the nonwoven fabric is preferably from 20 to 1400 μm, more preferably from 50 to 1200 μm, and further preferably from 80 to 1000 μm.
[0092] The liquid-impermeable back sheet 40 prevents the liquid absorbed in the absorber 10 from leaking out from the back sheet 40 side to the outside. For the liquid-impermeable back sheet 40, a liquid-impermeable film mainly made of polyolefin resin such as polyethylene (PE) or polypropylene (PP), a breathable resin film, a composite film in which a breathable resin film is bonded to a nonwoven fabric such as spunbond or spunlace, or a spunbond / meltblown / spunbond (SMS) nonwoven fabric in which a water-resistant meltblown nonwoven fabric is sandwiched between high-strength spunbond nonwoven fabrics can be used. From the viewpoint of ensuring flexibility so as not to impair the wearing comfort of the absorbent article, the back sheet 40 is mainly made of low-density polyethylene (LDPE) resin and has a basis weight of 10 to 50 g / m 2 In addition, when a breathable material is used, stuffiness during wearing is reduced, and discomfort to the wearer can be alleviated.
[0093] The size relationship between the absorbent body 10, the core wraps 20a, 20b, the liquid permeable top sheet 30, and the liquid impermeable back sheet 40 is not particularly limited and is appropriately adjusted depending on the application of the absorbent article, etc. Furthermore, the method of retaining the shape of the absorbent body 10 using the core wraps 20a, 20b is not particularly limited, and the absorbent body may be sandwiched between multiple core wraps as shown in Fig. 1, or the absorbent body may be covered by one core wrap.
[0094] The absorbent 10 may be bonded to the liquid-permeable top sheet 30. By bonding the absorbent 10 and the liquid-permeable top sheet 30, the liquid is more smoothly guided to the absorbent, and an absorbent article with better liquid leakage prevention is easily obtained. When the absorbent 10 is sandwiched or covered by a core wrap, it is preferable that at least the core wrap and the liquid-permeable top sheet 30 are bonded, and it is more preferable that the core wrap and the absorbent 10 are bonded. Examples of bonding methods include a method of applying a hot melt adhesive to the liquid-permeable top sheet 30 in a longitudinal stripe shape, a spiral shape, or the like at a predetermined interval in the width direction, and a method of bonding using a water-soluble binder selected from starch, carboxymethyl cellulose, polyvinyl alcohol, polyvinylpyrrolidone, and other water-soluble polymers. In addition, when the absorbent 10 contains heat-fusible synthetic fibers, a method of bonding by heat fusion may be adopted.
[0095] The present invention also provides a method for measuring the gel outflow test force of water-absorbent resin particles. The method includes the steps of: making water-absorbent resin particles absorb physiological saline in an amount 29 times that of the water-absorbent resin particles under stirring to prepare a swollen gel; placing 20 g of the swollen gel evenly in a cylinder with an inner diameter of 5 cm and a hole with a diameter of 5 mm at the bottom; compressing the swollen gel in the cylinder at a speed of 10 mm / min using a tool with a diameter of 4.9 cm; and recording the test force at the time when a part of the swollen gel flows out from the hole at the bottom of the cylinder as the gel outflow test force. A more specific measurement method will be described in the examples below.
[0096] When the water-absorbent resin particles having a gel outflow test force of 5 to 14N are used in an absorbent article, the amount of backflow of the absorbent article can be reduced. Therefore, the present invention also provides a method for reducing the amount of backflow of an absorbent article, which includes setting the gel outflow test force of the water-absorbent resin particles measured by the above-mentioned measuring method to 5 to 14N. A more specific method for measuring the gel outflow test force is shown in the examples described later. The method for reducing the amount of backflow of an absorbent article may further include, for example, setting the saline water retention capacity to 30 to 60 g / g, setting the 2-hour saline water absorption value of the water-absorbent resin particles under a load of 4.14 kPa to 15 ml / g or more, etc. Specific examples of the manufacturing method of the water-absorbent resin particles having these predetermined properties are as described above. The gel outflow test force of the water-absorbent resin particles can be set to 5 to 14N, for example, by selecting the manufacturing conditions of the water-absorbent resin particles so that the uniformity of crosslinking in the water-absorbent resin particles is high. EXAMPLES
[0097] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0098] <Production of Water-Absorbent Resin Particles> [Example 1] A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and an internal volume of 2 L was prepared, equipped with a reflux condenser, a dropping funnel, a nitrogen gas introduction tube, and a stirrer. A stirring blade (flat blade) 200, the outline of which is shown in FIG. 2, was attached to the stirrer. The stirring blade 200 has a shaft 200a and a flat plate portion 200b. The flat plate portion 200b is welded to the shaft 200a and has a curved tip. The flat plate portion 200b has four slits S extending along the axial direction of the shaft 200a. The four slits S are arranged in the width direction of the flat plate portion 200b, with the width of the two inner slits S being 1 cm and the width of the two outer slits S being 0.5 cm. The length of the flat plate portion 200b is about 10 cm, and the width of the flat plate portion 200b is about 6 cm. Next, 293 g of n-heptane was added as a hydrocarbon dispersion medium to the separable flask, and 0.736 g of maleic anhydride-modified ethylene-propylene copolymer (Hiwax 1105A, manufactured by Mitsui Chemicals, Inc.) was added as a polymeric dispersant to obtain a mixture. The mixture was heated to 80°C while stirring to dissolve the dispersant, and then cooled to 50°C.
[0099] On the other hand, 92.0g (1.03 mol) of 80.5% by mass acrylic acid aqueous solution was placed in a 300mL beaker as an ethylenically unsaturated monomer, and 147.7g of 20.9% by mass sodium hydroxide aqueous solution was added dropwise while cooling from the outside to perform 75 mol% neutralization. Then, 0.092g of hydroxyethyl cellulose (Sumitomo Seika Chemicals Co., Ltd., HEC AW-15F) as a thickener, 0.092g (0.339 mmol) of 2,2'-azobis(2-amidinopropane) dihydrochloride as a radical polymerization initiator, and 0.018g (0.067 mmol) of potassium persulfate, and 0.0046g (0.026 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare the first stage aqueous liquid.
[0100] The prepared aqueous solution was added to the reaction solution in the separable flask and stirred for 10 minutes. Next, 0.736 g of sucrose stearate (Mitsubishi Chemical Foods Corporation, Ryoto Sugar Ester S-370, HLB: 3) was dissolved as a surfactant in 6.62 g of n-heptane under heating to prepare a surfactant solution. The surfactant solution was further added to the reaction solution, and the inside of the system was thoroughly replaced with nitrogen while stirring at a stirrer speed of 425 rpm. Then, the flask was immersed in a water bath at 70°C to raise the temperature, and polymerization was carried out for 60 minutes to obtain a first-stage polymerization slurry liquid.
[0101] On the other hand, 128.8g (1.44 mol) of 80.5% by mass acrylic acid aqueous solution was placed in another 500mL beaker as an ethylenically unsaturated monomer, and 159.0g of 27% by mass sodium hydroxide aqueous solution was added dropwise while cooling from the outside to perform 75 mol% neutralization. After that, 0.129g (0.476 mmol) of 2,2'-azobis(2-amidinopropane) dihydrochloride and 0.026g (0.096 mmol) of potassium persulfate as radical polymerization initiators, and 0.0117g (0.067 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare the second aqueous solution.
[0102] The separable flask system was cooled to 25° C. while stirring at a stirrer speed of 650 rpm. Then, the entire amount of the second-stage aqueous liquid was added to the first-stage polymerization slurry liquid, and the system was replaced with nitrogen for 30 minutes. Thereafter, the flask was again immersed in a 70° C. water bath to raise the temperature, and a polymerization reaction was carried out for 60 minutes to obtain a hydrous gel polymer.
[0103] 0.589g of 45% by mass of pentasodium diethylenetriamine pentacetate aqueous solution was added to the hydrous gel polymer after the second-stage polymerization under stirring. Then, the flask was immersed in an oil bath set at 125°C, and 234.6g of water was extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Then, 4.42g (0.507mmol) of 2% by mass of ethylene glycol diglycidyl ether aqueous solution was added to the flask as a surface crosslinking agent, and the mixture was kept at 83°C for 2 hours.
[0104] Thereafter, n-heptane was evaporated at 125°C to dry the mixture, thereby obtaining polymer particles (dried product). The polymer particles were passed through a sieve with an opening of 850 μm, and 0.2% by mass of amorphous silica (Oriental Silicas Corporation, Toxil NP-S) relative to the mass of the polymer particles was mixed with the polymer particles, thereby obtaining 232.1 g of water-absorbent resin particles containing amorphous silica. The median particle size of the water-absorbent resin particles was 355 μm.
[0105] [Example 2] Except for changing the amount of water extracted from the system by azeotropic distillation to 229.2 g, the same procedure as in Example 1 was carried out to obtain 233.0 g of water-absorbent resin particles. The median particle size of the water-absorbent resin particles was 368 μm.
[0106] [Example 3] Except for changing the amount of water extracted from the system by azeotropic distillation to 224.3 g, the same procedure as in Example 1 was carried out to obtain 231.0 g of water-absorbent resin particles. The median particle size of the water-absorbent resin particles was 342 μm.
[0107] [Example 4] Except for changing the amount of water extracted from the system by azeotropic distillation to 207.9 g, the same procedure as in Example 1 was carried out to obtain 232.3 g of water-absorbent resin particles. The median particle size of the water-absorbent resin particles was 361 μm.
[0108] [Comparative Example 1] A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and a volume of 2 L was prepared, equipped with a reflux condenser, a dropping funnel, a nitrogen gas inlet tube, and a stirrer with a stirring blade having four inclined paddle blades with a blade diameter of 5 cm in two stages. 293 g of n-heptane was added to the separable flask as a hydrocarbon dispersion medium, and 0.736 g of maleic anhydride-modified ethylene-propylene copolymer (Hiwax 1105A, Mitsui Chemicals, Inc.) was added as a polymeric dispersant to obtain a mixture. The mixture was heated to 80°C while stirring to dissolve the dispersant, and then cooled to 50°C.
[0109] On the other hand, 92.0g (1.03 mol) of 80.5% by mass acrylic acid aqueous solution was placed in a 300mL beaker as an ethylenically unsaturated monomer, and 147.7g of 20.9% by mass sodium hydroxide aqueous solution was added dropwise while cooling from the outside to neutralize 75 mol%. Then, 0.092g of hydroxyethyl cellulose (Sumitomo Seika Chemicals Co., Ltd., HEC AW-15F) as a thickener, 0.0736g (0.272 mmol) of potassium persulfate as a radical polymerization initiator, and 0.010g (0.057 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare the first stage aqueous liquid.
[0110] The prepared aqueous solution was added to the reaction solution in the separable flask and stirred for 10 minutes. Next, 0.736 g of sucrose stearate (Mitsubishi Chemical Foods Corporation, Ryoto Sugar Ester S-370, HLB: 3) was dissolved as a surfactant in 6.62 g of n-heptane under heating to prepare a surfactant solution. The surfactant solution was further added to the reaction solution, and the inside of the system was thoroughly replaced with nitrogen while stirring at a stirrer speed of 550 rpm. Then, the flask was immersed in a water bath at 70°C to raise the temperature, and polymerization was carried out for 60 minutes to obtain a first-stage polymerization slurry liquid.
[0111] On the other hand, 128.8g (1.44 mol) of 80.5% by mass acrylic acid aqueous solution was placed in another 500mL beaker as an ethylenically unsaturated monomer, and 159.0g of 27% by mass sodium hydroxide aqueous solution was added dropwise while cooling from the outside to perform 75 mol% neutralization. After that, 0.090g (0.333 mmol) of potassium persulfate as a radical polymerization initiator and 0.012g (0.067 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare the second aqueous solution.
[0112] The contents of the separable flask were cooled to 25° C. while stirring at a stirrer speed of 1000 rpm, and the entire amount of the second-stage aqueous liquid was added to the first-stage polymerization slurry liquid, and the system was purged with nitrogen for 30 minutes. Thereafter, the flask was again immersed in a 70° C. water bath to raise the temperature, and a polymerization reaction was carried out for 60 minutes to obtain a hydrous gel polymer.
[0113] 0.265g of 45% by mass of pentasodium diethylenetriamine pentacetate aqueous solution was added to the hydrous gel polymer after the second-stage polymerization under stirring. Then, the flask was immersed in an oil bath set at 125°C, and 271.4g of water was extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Then, 6.40g (0.735mmol) of 2% by mass of ethylene glycol diglycidyl ether aqueous solution was added to the flask as a surface crosslinking agent, and the mixture was kept at 83°C for 2 hours.
[0114] Thereafter, n-heptane was evaporated at 125°C to dry the mixture, thereby obtaining polymer particles (dried product). The polymer particles were passed through a sieve with an opening of 850 μm, and 0.5% by mass of amorphous silica (Toxil NP-S, Oriental Silicas Corporation) relative to the mass of the polymer particles was mixed with the polymer particles, thereby obtaining 230.6 g of water-absorbent resin particles containing amorphous silica. The median particle size of the water-absorbent resin particles was 355 μm.
[0115] [Comparative Example 2] The amount of water extracted from the system by azeotropic distillation was changed to 256.1 g, the amount of the aqueous ethylene glycol diglycidyl ether solution added as a surface crosslinking agent was changed to 4.42 g (0.507 mmol), and the amount of amorphous silica mixed with respect to the polymer particles was changed to 0.1 mass %. The same procedure as in Comparative Example 1 was repeated to obtain 230.8 g of water absorbent resin particles. The median particle diameter of the water absorbent resin particles was 349 μm.
[0116] [Comparative Example 3] Except for changing the amount of water extracted from the system by azeotropic distillation to 247.9 g and changing the amount of the ethylene glycol diglycidyl ether aqueous solution added as a surface crosslinking agent to 4.42 g (0.507 mmol), 231.0 g of water absorbent resin particles were obtained in the same manner as in Comparative Example 1. The median particle diameter of the water absorbent resin particles was 355 μm.
[0117] The obtained water-absorbent resin particles were evaluated for gel outflow test force, physiological saline water absorption amount under load, physiological saline water retention amount, median particle size, and backflow amount of absorbent articles by the following methods.
[0118] <Measurement of gel outflow test force> [Preparation of swollen gel] 2 g of water-absorbent resin particles were added to a 100 ml glass beaker containing 58 g of physiological saline at 25°C under stirring at 600 rpm (stirrer tip: length 3 cm, diameter 8 mm, no ring). After it was confirmed that the water-absorbent resin particles had swollen and the vortex on the liquid surface had converged, the stirring was stopped. After that, the mixture was left to stand for 10 minutes to obtain a swollen gel in which the water-absorbent resin particles had swelled 30 times.
[0119] [Test force measurement] For the measurement of the gel outflow test force, a small tabletop tester (EZtest, model number: EZ-SX) manufactured by Shimadzu Corporation and a measuring device shown in FIG. 3 were used. The measurement was performed in an environment of 25°C ± 2°C and humidity 50 ± 10% (RH). A transparent acrylic cylinder 51 has a hole with a diameter of 3.0 cm in the center of the bottom surface, and has an inner diameter of 5.0 cm and an outer diameter of 6.0 cm. A metal disk 52 with a thickness of 3.0 mm and a diameter of 4.9 cm is placed in the cylinder 51. A tapered hole with a diameter expanding toward both surfaces is provided in the center of the disk 52, and the minimum diameter of the hole is 5.0 mm and the maximum diameter is 8.0 mm. 20.0 g of the gel (swollen gel) of the swollen water-absorbent resin particles 10a was placed on the disk 52 in the cylinder 51, and the swollen gel was evenly distributed in the cylinder 51 while being loosened with a spatula.
[0120] The compression of the swollen gel was carried out as follows. A jig 53 having a disk with a diameter of 4.9 cm and a thickness of 1.2 cm at the tip of a handle with a length of 14 cm was attached to the load cell of a small tabletop tester (load cell capacity: 50 N, manufactured by Shimadzu Corporation). A type with a hole with a diameter of 3.0 cm in the center (manufactured by Shimadzu Corporation) was used as the measurement table of the tester. A cylinder 51 containing the swollen gel and the disk 52 on top of the hole on the measurement table was placed directly under the jig 53 so that the bottom of the cylinder 51 was horizontal. The jig 53 was attached so that the disk was parallel to the bottom of the cylinder 51. The jig 53 was manually lowered in the vertical direction until the tip of the jig 53 came into contact with the surface of the swollen gel and the test force slightly exceeded 0.01 N. Subsequent operations of the jig 53 attached to the tester were carried out using Shimadzu Autograph software Trapezium X (manufactured by Shimadzu Corporation). The jig 53 was further lowered in the vertical direction, and a load was applied to the swollen gel while increasing linearly. The gradient of the load increase was 4.9 N / min. The jig 53 was stopped when the load cell detected 4.9 N. In order to reduce the air gap, the jig 53 was maintained at 4.9 N for 30 seconds after it was stopped. Thereafter, the jig was pushed down at a speed of 10 mm / min to compress the swollen gel toward the bottom of the cylinder 51, and the test force was measured. The test force at the point when the start of the outflow of the swollen gel from the hole in the disk 52 was visually confirmed was taken as the gel outflow test force.
[0121] FIG. 4 shows an example of the gel outflow test force measurement result. When measuring the test force by pressing at a speed of 10 mm / min, as the displacement (travel distance) of the jig 53 increases, the test force increases smoothly while the swollen gel is compressed. When the swollen gel starts to flow out of the hole in the disk 52, the smoothly increasing test force starts to increase while repeatedly increasing and decreasing. The point at which the first decrease in the test force is observed coincides with the point at which it is visually confirmed that the swollen gel starts to flow out of the hole in the disk 52. That is, in the graph of FIG. 4, the gel outflow test force is the peak value of the test force immediately before the first decrease in the test force is observed, as indicated by the arrow in the figure. The results are shown in Table 1.
[0122] <Measurement of saline water absorption under a load of 4.14 kPa> The physiological saline water absorption amount under a load of 4.14 kPa (water absorption amount under load) was measured using a measuring device whose outline is shown in FIG. 5. The measurement was performed twice for one type of water absorbent resin particle, and the average value was calculated. The measuring device includes a burette part 1, a clamp 3, a conduit 5, a stand 11, a measurement table 13, and a measurement part 4 placed on the measurement table 13. The burette part 1 has a burette tube 21 with a scale, a rubber plug 23 that seals the opening at the top of the burette tube 21, a cock 22 connected to the tip at the bottom of the burette tube 21, and an air introduction tube 25 and a cock 24 connected to the bottom of the burette tube 21. The burette part 1 is fixed with a clamp 3. The flat measurement table 13 has a through hole 13a with a diameter of 2 mm formed in its center, and is supported by a stand 11 whose height is variable. The through hole 13a of the measurement table 13 and the cock 22 of the burette part 1 are connected by a conduit 5. The inner diameter of the conduit 5 is 6 mm.
[0123] The measurement unit 4 has a cylinder 31 made of acrylic resin, a polyamide mesh 32 bonded to one opening of the cylinder 31, and a weight 33 movable in the vertical direction within the cylinder 31. The cylinder 31 is placed on the measurement table 13 via the polyamide mesh 32. The inner diameter of the cylinder 31 is 20 mm. The opening of the polyamide mesh 32 is 75 μm (200 mesh). The weight 33 has a diameter of 19 mm and a mass of 119.6 g, and can apply a load of 4.14 kPa to the water-absorbent resin particles 10a uniformly arranged on the polyamide mesh 32 as described later.
[0124] The measurement of the physiological saline water absorption capacity under a load of 4.14 kPa using the measuring device shown in FIG. 5 was performed in a room at 25° C. and humidity of 50±10% (RH). First, the cocks 22 and 24 of the burette part 1 were closed, and 0.9% by mass physiological saline adjusted to 25° C. was poured into the burette tube 21 from the opening at the top of the burette tube 21. Next, the top opening of the burette tube 21 was sealed with a rubber stopper 23, and then the cocks 22 and 24 were opened. The inside of the conduit 5 was filled with 0.9% by mass saline 50 so that no air bubbles were introduced. The height of the measurement table 13 was adjusted so that the height of the water surface of the 0.9% by mass saline solution that reached the through hole 13a was the same as the height of the upper surface of the measurement table 13. After the adjustment, the height of the water surface of the 0.9% by mass saline solution 50 in the burette tube 21 was read on the scale of the burette tube 21, and that position was set as the zero point (the reading at 0 seconds).
[0125] In the measurement section 4, 0.10 g of water-absorbent resin particles 10a were uniformly arranged on the polyamide mesh 32 in the cylinder 31, a weight 33 was placed on the water-absorbent resin particles 10a, and the cylinder 31 was installed so that its center coincided with the conduit port at the center of the measurement table 13. The amount of reduction in the saline solution in the burette tube 21 (i.e., the amount of saline solution absorbed by the water-absorbent resin particles 10a) Wa (ml) was read two hours after the water-absorbent resin particles 10a started to absorb the saline solution from the conduit 5, and the saline solution absorption capacity of the water-absorbent resin particles 10a under a load of 4.14 kPa was calculated by the following formula. The results are shown in Table 1. Absorption capacity of physiological saline solution under a load of 4.14 kPa (ml / g) = Wa (ml) / mass of water-absorbent resin particles (g)
[0126] <Measurement of saline water retention> A cotton bag (membrane broad 60, 100 mm wide x 200 mm long) containing 2.0 g of absorbent resin particles was placed in a 500 ml beaker. 500 g of 0.9% by mass sodium chloride aqueous solution (physiological saline) was poured into the cotton bag containing the absorbent resin particles at once so as not to cause any lumps, the top of the cotton bag was tied with a rubber band, and the bag was left to stand for 30 minutes to swell the absorbent resin particles. After 30 minutes, the cotton bag was dehydrated for 1 minute using a dehydrator (manufactured by Kokusan Co., Ltd., product number: H-122) set to a centrifugal force of 167 G, and the mass Wb (g) of the cotton bag containing the swollen gel after dehydration was measured. The same operation was performed without adding the absorbent resin particles, and the empty mass Wc (g) of the cotton bag when wet was measured, and the physiological saline water retention was calculated from the following formula. The measurement of physiological saline water retention was performed in an environment of 25°C ± 2°C and humidity 50 ± 10% (RH). The results are shown in Table 1. Saline water retention (g / g) = [Wb-Wc] / 2.0
[0127] <Measurement of median particle size (particle size distribution)> 50 g of water-absorbent resin particles were used for measuring the median particle size (particle size distribution). JIS standard sieves were arranged in the following order from the top: a sieve with an opening of 850 μm, a sieve with an opening of 500 μm, a sieve with an opening of 425 μm, a sieve with an opening of 300 μm, a sieve with an opening of 250 μm, a sieve with an opening of 180 μm, a sieve with an opening of 150 μm, and a tray.
[0128] The water-absorbent resin particles were placed on the top sieve of the combination, and classified in accordance with JIS Z 8815 (1994) using a Rotap type shaker (manufactured by Iida Manufacturing Co., Ltd.). After classification, the mass of the water-absorbent resin particles remaining on each sieve was calculated as a mass percentage relative to the total amount to obtain a particle size distribution. By accumulating the particles on the sieves in order from the largest particle diameter with respect to this particle size distribution, the relationship between the sieve opening and the accumulated value of the mass percentage of the water-absorbent resin particles remaining on the sieves was plotted on a logarithmic probability paper. By connecting the plots on the probability paper with a straight line, the particle size corresponding to an accumulated mass percentage of 50 mass% was determined as the median particle size.
[0129] <Measurement of the amount of return of absorbent articles> [Production of absorbent articles] Using an airflow type mixer (Autech Co., Ltd., Pad Former), 10 g of water-absorbent resin particles and 6.8 g of crushed pulp were uniformly mixed by air papermaking to produce a sheet-shaped absorbent body of 40 cm x 12 cm in size. Next, a sheet of 16 g / m2 with the same size as the absorbent body was prepared. 2 The absorbent body was sandwiched between two tissue papers, and a load of 196 kPa was applied to the whole for 30 seconds to obtain a laminate. 2 An air-through type porous liquid-permeable sheet made of polyethylene-polypropylene was placed on the upper surface of the laminate to obtain an absorbent article for evaluation.
[0130] The absorbent article for evaluation was placed on a horizontal table so that the surface on which the liquid-permeable sheet was provided was the upper surface, and a 100 mL liquid-injection cylinder with an inlet having an inner diameter of 3 cm was placed in the center of the absorbent article for evaluation. 80 ml of physiological saline was injected into the cylinder at once. The cylinder was removed from the absorbent article, and the absorbent article was left as it was. 30 minutes (second time) and 60 minutes (third time) after the first test liquid injection, the same operation was performed using the measuring device at the same position as the first time. 60 minutes after the third injection, 40 sheets of 10 cm square filter paper whose mass (Wd (g)) had been measured in advance were placed near the test liquid injection position on the absorbent article, and a weight with a mass of 5 kg and a bottom surface of 10 cm x 10 cm was placed on top of them. After the load was applied for 5 minutes, the mass (We (g)) of the filter paper was measured, and the increased mass was taken as the backflow amount (g). The test for the amount of return was carried out in a room adjusted to 25°C and 50% humidity (RH). The smaller the amount of return, the more preferable the absorbent article. The results are shown in Table 1. It was shown that the absorbent article using the water-absorbent resin particles of the Example had a reduced amount of return. Backflow amount (g) = We - Wd
[0131] [Table 1] [Explanation of symbols]
[0132] 1...burette part, 3...clamp, 4...measuring part, 5...conduit, 10...absorbent body, 10a...water-absorbent resin particles, 10b...fiber layer, 11...frame, 13...measuring stand, 13a...through hole, 20a, 20b...core wrap, 21...burette tube, 22...cock, 23...rubber stopper, 24...cock, 25...air introduction tube, 30...liquid-permeable top sheet, 31...cylinder, 32...polyamide mesh, 33...weight, 40...liquid-impermeable back sheet, 51...cylinder, 52...disk, 53...jig, 100...absorbent article, 200...stirring blade, 200a...shaft, 200b...flat plate part, S...slit.
Claims
1. A water-absorbent resin particle comprising a crosslinked polymer having a monomer unit derived from an ethylenically unsaturated monomer, the ethylenically unsaturated monomer comprises at least one compound selected from the group consisting of (meth)acrylic acid and salts thereof, a ratio of the (meth)acrylic acid and a salt thereof to a total amount of monomers for obtaining the water-absorbing resin particles is 70 to 100 mol %, The gel outflow test force measured by the following method is 11.4 to 13.4 N, Water-absorbent resin particles having a saline water retention capacity of 45 to 55 g / g. Gel outflow test force measurement method: A swollen gel is prepared by making the water-absorbent resin particles absorb physiological saline in an amount 29 times that of the water-absorbent resin particles under stirring. 20 g of the swollen gel is evenly placed in a cylinder with an inner diameter of 5 cm and a hole with a diameter of 5 mm at the bottom. The swollen gel in the cylinder is compressed at a speed of 10 mm / min using a tool with a diameter of 4.9 cm, and the test force at the time when a part of the swollen gel flows out from the hole at the bottom of the cylinder is recorded as the gel outflow test force.
2. 2. The water-absorbent resin particles according to claim 1, which have a physiological saline water absorption value of 25 ml / g or less after 2 hours under a load of 4.14 kPa.
3. 3. The water-absorbent resin particles according to claim 1, which have a physiological saline water absorption value of 15 ml / g or more after 2 hours under a load of 4.14 kPa.
4. An absorbent comprising the water-absorbent resin particles according to any one of claims 1 to 3.
5. An absorbent article comprising the absorbent body according to claim 4.
6. 6. The absorbent article of claim 5 which is a diaper.
7. making the water-absorbent resin particles absorb physiological saline in an amount 29 times the amount of the water-absorbent resin particles under stirring to prepare a swollen gel; Putting 20 g of the swollen gel evenly into a cylinder having an inner diameter of 5 cm and a hole having a diameter of 5 mm at the bottom; A method for measuring a gel outflow test force, comprising: compressing the swollen gel in the cylinder at a speed of 10 mm / min using a tool having a diameter of 4.9 cm; and recording the test force at the time when a portion of the swollen gel flows out of the hole at the bottom of the cylinder as the gel outflow test force.
8. A method for producing water-absorbent resin particles comprising a crosslinked polymer having a monomer unit derived from an ethylenically unsaturated monomer, comprising: the ethylenically unsaturated monomer comprises at least one compound selected from the group consisting of (meth)acrylic acid and salts thereof, a ratio of the (meth)acrylic acid and a salt thereof to a total amount of monomers for obtaining the water-absorbing resin particles is 70 to 100 mol %, A method for producing water-absorbent resin particles, comprising selecting water-absorbent resin particles having a gel outflow test force of 5 to 14 N measured by the measurement method according to claim 7.
9. The gel outflow test force of the water absorbent resin particles measured by the measurement method according to claim 7 is set to 5 to 14 N, The water-absorbent resin particles contain a crosslinked polymer having a monomer unit derived from an ethylenically unsaturated monomer, the ethylenically unsaturated monomer contains at least one compound selected from the group consisting of (meth)acrylic acid and salts thereof, and a ratio of the (meth)acrylic acid and salts thereof is 70 to 100 mol % based on the total amount of monomers for obtaining the water-absorbent resin particles.
Citation Information
Patent Citations
Ammonium salt-containing water-absorbing resin and method for producing the same
JP2006199805A
Water-absorbent resin and water-absorbent resin production method
JP2016028113A
Process for producing water-absorbing resin, water-absorbing resin, water-absorbing agent, and absorptive article
JP2016028117A
Process for production of water-absorbing resin particles, water-absorbing resin particles made by the process, and absorbents and absorbent articles made by using the particles
WO2006123561A1
Water-absorbing resin, water-absorbing body, and water-absorbing product
WO2014038324A1